Method for producing fiber-reinforced resin composition

Direct water introduction in the extruder for cellulose fiber and resin kneading addresses water absorption issues, ensuring uniform dispersion and mechanical properties in fiber-reinforced resin compositions.

JP7554026B2Active Publication Date: 2024-09-19TOYOTA SHATAI KK +1
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2020158344
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-09-23
Publication Date
2024-09-19
Estimated Expiration
2040-09-23

AI Technical Summary

Technical Problem

Existing methods for producing fiber-reinforced resin compositions using cellulose fibers and polyvinyl alcohol result in unintended dimensional changes due to water absorption and dew condensation, limiting uniform dispersion and mechanical properties.

Method used

A method involving direct water introduction into an extruder for kneading cellulose fibers and resin without a water-soluble polymer, adjusting cellulose fiber content to 25% by mass or more and water to 1% by mass or more, and incorporating a discharge section to remove excess water, ensuring uniform dispersion.

Benefits of technology

Achieves uniform kneading of cellulose fibers and resin without excessive water absorption or release, preventing dimensional changes and dew condensation, while maintaining excellent mechanical properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007554026000008
    Figure 0007554026000008
  • Figure 0007554026000004
    Figure 0007554026000004
  • Figure 0007554026000005
    Figure 0007554026000005
Patent Text Reader

Abstract

To blend cellulose fibers and a resin uniformly as much as possible while avoiding excessive ability of absorbing and releasing water.SOLUTION: A method for producing a fiber-reinforced resin composition 10 includes a step of blending cellulose fibers 12 and a resin 14 with an extruder 2. Water 18 is directly put into the extruder 2, and the cellulose fibers 12 and the resin 14 are blended in the absence of a water-absorbable, water-soluble polymer.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing a fiber-reinforced resin composition. [Background technology]

[0002] This type of fiber-reinforced resin composition has excellent strength and is therefore used in many fields such as automobiles. In producing the fiber-reinforced resin composition, it is desirable to knead the fibers and resin as uniformly as possible in an extruder in order to ensure excellent mechanical properties.

[0003] Here, in the field of fiber-reinforced resin compositions, cellulose-based fibers have been attracting attention as a material to replace inorganic materials. However, since cellulose-based fibers are hydrophilic, they are difficult to disperse well in hydrophobic resins such as polyolefin resins, and the types of resins that can be used may be limited. Therefore, in the manufacturing method disclosed in Patent Document 1, polyvinyl alcohol is added to the cellulose-based fibers and polyolefin resin when they are kneaded together. This polyvinyl alcohol is a type of water-soluble polymer with hydrophilic groups, and has water-absorbing properties that absorb and retain water. In the known technology, polyvinyl alcohol forms a coating on the surface of the cellulose-based fibers, making it possible to knead the cellulose-based fibers and polyolefin resin as uniformly as possible. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2019-218450 A Summary of the Invention [Problem to be solved by the invention]

[0005] However, when the manufacturing method of the known technology is used, the fiber reinforced resin composition contains polyvinyl alcohol, which has water absorption as described above. For this reason, in the fiber reinforced resin composition of the known technology, there was a concern that the water absorption of polyvinyl alcohol would cause unintended dimensional changes, and that the release of moisture would cause condensation on peripheral devices. The present invention was devised in view of the above-mentioned points, and the problem that the present invention aims to solve is to knead cellulosic fibers and resin as uniformly as possible without excessive water absorption and release. [Means for solving the problem]

[0006] As a means for solving the above problems, the method for producing a fiber-reinforced resin composition according to the first invention is a method for producing a fiber-reinforced resin composition comprising a step of kneading cellulose-based fibers and a resin in an extruder. In this type of production method, it is desirable to knead the cellulose-based fibers and the resin as uniformly as possible without excessive water absorption and release. Therefore, in the present invention, water is directly introduced into the extruder, and the cellulose-based fibers and the resin are kneaded in a state in which no water-soluble polymer with water absorption is contained. At the same time, cellulosic fibers having a fiber diameter on the order of millimeters to micrometers and having been dried are fed into the extruder. In the present invention, by directly feeding water into the extruder, a sufficient amount of water can be supplied to the kneaded product of the cellulose fiber and the resin. Therefore, in the present invention, the cellulose fiber can be well dispersed by a sufficient amount of water, and even if the water-soluble polymer is omitted, the cellulose fiber can be kneaded with the resin as uniformly as possible. Here, the kneaded product is a product formed from the cellulose fiber and the resin during kneading, and may contain additives as necessary. In addition, the fiber-reinforced resin composition is a product obtained after kneading the cellulose fiber and the resin (and additives as necessary), and contains each of these blending components at the content rate at the product stage. Furthermore, in the present invention, by using cellulosic fibers after drying treatment, it becomes possible to adjust the substantial amount of water in the extruder by the amount of water directly charged.

[0007] The method for producing a fiber-reinforced resin composition of the second invention is the method for producing a fiber-reinforced resin composition of the first invention, except that water is added in a state in which the content of cellulosic fibers is adjusted to 25% by mass or more relative to the total mass of the kneaded product. The amount of water added is adjusted to 1% by mass or more relative to the total mass of the kneaded product and water. In the present invention, when the content of cellulosic fibers in the kneaded product is 25% by mass or more, the cellulosic fibers and the resin can be kneaded as uniformly as possible by adding water in an amount of 1% by mass or more relative to the total mass of the kneaded product and water.

[0009] No. 3 The method for producing a fiber-reinforced resin composition of the present invention is as follows: or No. 2 invention of In the method for producing a fiber-reinforced resin composition, the extruder is provided with a discharge section capable of discharging water to the outside after kneading the cellulose-based fiber and the resin. In the present invention, by providing the discharge section in the extruder, excess water in the extruder can be discharged to the outside at the end of the kneading process. Effect of the Invention

[0010] According to the first aspect of the present invention, the cellulosic fibers and the resin can be kneaded as uniformly as possible without causing excessive water absorption and release. Furthermore, according to the first aspect of the invention, the cellulosic fibers and the resin can be more reliably and uniformly kneaded together. According to the second aspect of the present invention, the cellulosic fibers and the resin can be more reliably and uniformly kneaded. 3 According to the invention, the cellulosic fibers and the resin can be kneaded as uniformly as possible and then taken out of the extruder in an appropriate state. [Brief description of the drawings]

[0011] [Figure 1] FIG. 2 is a schematic diagram of an extruder showing the feeding positions of each compounding ingredient. [Diagram 2] FIG. 2 is a schematic diagram showing the installation positions of each component of the extruder. [Diagram 3] 1 is an optical microscope photograph of the fiber-reinforced resin composition of Example 1. [Figure 4]FIG. 4 is a diagram showing the image of FIG. 3 after being binarized into aggregated and dispersed portions. [Diagram 5] FIG. 5 is a diagram showing the outline of the aggregated portion in FIG. [Figure 6] 2 is an optical microscope photograph of the fiber-reinforced resin composition of Comparative Example 1. [Figure 7] FIG. 7 is a diagram showing the image of FIG. 6 after being binarized into aggregated and dispersed portions. [Figure 8] FIG. 8 is a diagram showing the outline of an aggregated portion in FIG. [Figure 9] 3 is an optical microscope photograph of the fiber-reinforced resin composition of Comparative Example 2. [Figure 10] FIG. 10 is a diagram showing the image of FIG. 9 after being binarized into aggregated and dispersed portions. [Figure 11] FIG. 11 is a diagram showing the outline of the aggregated portion in FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] Hereinafter, an embodiment of the present invention will be described with reference to Fig. 1 to Fig. 11. In Fig. 1, for convenience, reference numeral 10 corresponds to the location where the fiber reinforced resin composition is taken out, reference numerals 12, 14, and 16 correspond to the locations where each compounding component is fed, and reference numeral 18 corresponds to the locations where water is fed and discharged. In Fig. 2, reference numerals 3 to 7 correspond to the positions of each component relative to the extruder.

[0013] As shown in FIG. 1, the fiber reinforced resin composition 10 of this embodiment is produced by kneading the cellulose fiber 12 and the resin 14 in an extruder 2. In this type of fiber reinforced resin composition 10, the cellulose fiber 12 and the resin 14 should be kneaded as uniformly as possible from the viewpoint of ensuring the desired mechanical properties, and care should be taken not to give the fiber reinforced resin composition 10 excessive water absorption and release. Therefore, in this embodiment, water 18 is directly fed into the extruder 2 during the production process described below, so that the cellulose fiber 12 and the resin 14 are kneaded as uniformly as possible without giving excessive water absorption and release. Hereinafter, each compounding component of the fiber reinforced resin composition 10, the configuration of the extruder 2, and the production method of the fiber reinforced resin composition 10 will be described in detail.

[0014] [Cellulosic fibers] As the cellulose-based fiber 12 shown in FIG. 1, various cellulose-based fibers such as natural plant fibers, regenerated fibers, refined fibers, and semi-synthetic fibers can be used. The raw material of the cellulose-based fiber 12 is not particularly limited, but considering the convenience of raw material procurement, it is preferable to use various pulps. Examples of this type of pulp include wood pulp (chemical pulp, mechanical pulp, waste paper pulp) obtained from softwood or hardwood trees, and non-wood pulp obtained from seed plants, etc., and these can be used alone or in combination of two or more. The fiber diameter of the cellulose-based fiber 12 in the raw material is not particularly limited, and the fiber diameter may be on the order of millimeters to micrometers, like the cellulose-based fiber 12 in pulp. The raw material may also contain cellulose-based fiber 12 (cellulose nanofiber) with a fiber diameter on the order of nanometers.

[0015] It is also preferable that the hydroxyl groups of the cellulosic fibers 12 in the raw material are chemically modified to be hydrophobic, and that a hydrophobic treatment is performed using a compatibilizer. For example, by substituting the hydroxyl groups of the cellulosic fibers 12 with hydrophobic groups via ester bonds or the like, the defibrability of the cellulosic fibers 12 is improved, which contributes to uniform kneading with the resin 14 described below.

[0016] [resin] As the resin 14 shown in Fig. 1, various thermoplastic resins (including elastomers) capable of bonding the cellulose-based fibers 12 together can be used. The type of resin contained in the fiber-reinforced resin composition 10 is not limited. Examples of the resin include thermoplastic resins such as polyolefin resins such as polypropylene and polyethylene, ABS (acrylonitrile-butadiene-styrene) resin, acrylic resin, polyester resin, polyurethane resin, polystyrene resin, polyamide resin, polyvinyl chloride resin, and polycarbonate resin, and thermoplastic elastomers such as olefin-based elastomers, styrene-based elastomers, polyamide-based elastomers, polyester-based elastomers, and polyurethane-based elastomers. Among these, polyolefin resins are preferred.

[0017] [Content of each compounding component in fiber reinforced resin composition] In the fiber reinforced resin composition 10 shown in FIG. 1, the contents of the cellulose fiber 12 and the resin 14 can be set in consideration of the intended use and the like. For example, the content of the resin 14 may be selected from the range of 30% by mass to 99% by mass, or from the range of 55% by mass to 95% by mass, with respect to the total mass of the fiber reinforced resin composition 10. The content of the cellulose fiber 12 may be selected from the range of 1% by mass to 70% by mass, or from the range of 5% by mass to 45% by mass, with respect to the total mass of the fiber reinforced resin composition 10. If the content of the cellulose fiber 12 is less than 1% by mass, no significant improvement in mechanical properties due to the cellulose fiber 12 is observed, and the predetermined strength of the fiber reinforced resin composition 10 may not be ensured. If the content of the cellulose fiber 12 exceeds 70% by mass, the binding of the cellulose fiber 12 by the resin 14 may be weakened, and the fiber reinforced resin composition 10 may become brittle. For example, when the fiber-reinforced resin composition 10 is used as a component of a vehicle, in order to ensure the desired strength and shape retention, it is desirable for the composition to contain 5% to 45% by mass of cellulosic fibers 12, 55% to 95% by mass of resin 14, and, if necessary, additives (described later).

[0018] The fiber reinforced resin composition 10 may contain various components as additives 16 that contribute to improving the quality and performance of the fiber reinforced resin composition 10. The content of each additive 16 is not particularly limited, but can be set to 10% by mass or less, typically 5% by mass or less, based on the total mass of the fiber reinforced resin composition 10. Examples of this type of additive 16 include acid-modified polypropylene, light resistance agents, antioxidants, heat stabilizers, flame retardants, metal deactivators, antistatic agents, and lubricants. In particular, acid-modified polypropylene improves the defibration property of the cellulose-based fibers 12 and contributes to ensuring strength, so it is desirable to include 1% by mass to 5% by mass of the acid-modified polypropylene based on the total mass of the fiber reinforced resin composition 10. When pulp is used as the raw material for the cellulose-based fibers 12, the pulp may be added with a sizing agent, a paper strength enhancer such as a dry strength agent or a wet strength agent, a pH adjuster, a drainage improver, an antifoaming agent, a bulking agent, a retention agent, an antibacterial agent, an antifungal agent, a filler, or a dye.

[0019] [Extruder] As the extruder 2 shown in FIG. 1 and FIG. 2, an extruder that can be used for kneading a general resin composition can be used, and can be selected from various twin-screw extruders (co-rotating or counter-rotating) and various single-screw extruders. For example, the extruder 2 of this embodiment is a co-rotating twin-screw extruder, and is equipped with a cylinder 2a having a temperature raising (heat retention) function and two screws 2b rotatably installed in the cylinder 2a. Here, the screw length L / screw diameter D (L / D) of the extruder 2 is not particularly limited, but can typically be set in the range of 36 to 120, and can also be set to less than 36 (for example, less than 36 and 25 or more). The screw length L of the extruder 2 is not particularly limited, and can be set in the range of 600 mm to 16,000 mm in consideration of the above-mentioned value of L / D. The screw diameter D of the extruder 2 is also not particularly limited, and can be set in the range of, for example, 15 mm to 400 mm, and when the screw diameter is not constant, the minimum value can be set as the screw diameter D. The cylinder temperature during kneading may be selected from the range of 150°C to 250°C.

[0020] Kneading discs can be placed at appropriate positions on the extruder 2, and the number of kneading discs is not particularly limited and can be set to any number. The angle between the major axes of adjacent kneading discs (shift angle) is not particularly limited and may be selected, for example, from the range of 30° to 90°. The aspect ratio of the main surface of the kneading disc (length of major axis / length of minor axis) is not particularly limited and may be selected, for example, from the range of 1.2 to 2.0.

[0021] [Water inlet and outlet] In addition, the extruder 2 shown in FIG. 1 and FIG. 2 has an inlet 3 for the cellulose fiber 12, the resin 14 (in a solid state), and the additive 16 at the most upstream position in the extrusion direction, and an outlet 4 for the fiber-reinforced resin composition 10 at the most downstream position. The extruder 2 is provided with an inlet 5 for water and an outlet 6 for discharge, and further includes an inlet device 7 for the resin, which will be described later, as necessary. Here, the inlet 5 may be any of various water injection devices such as a liquid addition pump, and the structure is not particularly limited as long as the water 18 (mainly in a liquid state) can be directly injected into the cylinder 2a. The outlet 6 may be any of various discharge devices such as a vacuum pump or an outlet hole, and the structure is not particularly limited as long as the water 18 (mainly water vapor) in the cylinder 2a can be discharged to the outside. Here, the positions of the inlet 5 and the outlet 6 are not particularly limited as long as the cellulose fiber 12 and the resin 14 can be uniformly mixed. For example, the inside of the extruder 2 with an L / D of 77 is divided into ten equal parts in the extrusion direction, and divided into sections C1 to C10 from the upstream to the downstream as shown in FIG. 2. The input section 5 can be provided in any one of the upstream sections C2, C3, C4, and C5, and the discharge section 6 can be provided in any one of the downstream sections C8, C9, and C10.

[0022] As described above, the extruder 2 shown in Figures 1 and 2 can be provided with an input device 7 for inputting the resin 14, and it is preferable that the resin 14 is in a molten state. As this type of input device 7, various devices capable of inputting the resin 14 can be adopted, for example, a single-screw extruder equipped with a temperature raising function can be used. The input device 7 can be provided, for example, in any of the downstream sections C6, C7, and C8. It is also possible to input the resin 14 in a molten state, not in a solid state, upstream of the extruder 2, and in this case, another input device (not shown) can be provided, for example, in any of the upstream sections C1, C2, and C3.

[0023] [Method of producing fiber-reinforced resin composition] Referring to FIG. 1, the method for producing the fiber-reinforced resin composition 10 includes a step of kneading the cellulose-based fibers 12 and the resin 14 (and the additive 16 as necessary), and the fiber-reinforced resin composition 10 in the form of pellets can be obtained by the step. In this type of production method, it is desirable to knead the cellulose-based fibers 12 and the resin 14 as uniformly as possible in the extruder 2 while taking care not to give the fiber-reinforced resin composition 10 excessive water absorption and release. Therefore, in this embodiment, as shown in FIG. 1, water 18 is directly fed into the extruder 2 to knead the cellulose-based fibers 12 and the resin 14 in a state in which a water-soluble polymer (described in detail later) having water absorption properties is not included. By feeding the water 18 directly into the extruder in this way, it becomes possible for the cellulose-based fibers 12 to have a good dispersion state even without using a water-soluble polymer. Therefore, the step of kneading the cellulose-based fibers 12 and the resin 14 will be specifically described below together with the feeding procedure and the amount of water 18.

[0024] [Water-soluble polymer] The water-soluble polymer with water absorption properties means a polymer that causes excessive water absorption and release in the fiber-reinforced resin composition 10, and various polymers having hydrophilic groups can be envisaged. For example, typical water-soluble polymers include polyvinyl alcohol (including crosslinked products and derivatives thereof), polyalkylene oxides such as polyethylene oxide and polypropylene oxide, polyvinyl ether, polyvinylpyrrolidone, water-soluble nylon, polyacrylamide, chitins, chitosans, starch, and copolymers thereof.

[0025] [Drying process] In addition, it is desirable to dehydrate the raw material (e.g., pulp) of the cellulosic fiber 12 shown in FIG. 1 so as not to contain excess moisture, and it is particularly desirable to subject it to a drying treatment. That is, if the pulp contains an excessive amount of water 18, when the pulp is charged, steam may flow back from the charging port 3, which may increase the labor required for charging or make the charging itself difficult. As this type of drying treatment, various methods such as vacuum drying, hot air drying, and suction drying can be used, and among them, suction drying (vacuum drying) at a high temperature of 75°C to 105°C is desirable. By using the pulp raw material (cellulosic fiber 12) after the drying treatment, the labor required for charging is reduced, and it is possible to adjust the actual amount of water in the extruder 2 by the amount of water 18 directly charged into the extruder 2, which will be described later. There is also a technique for intentionally making the cellulosic fiber 12 retain water (moisture), but the amount of water at this time must be small considering the labor required for charging, and is at most about 5% by mass with respect to the total mass of the kneaded material and water.

[0026] Then, pulp (cellulosic fibers 12) and solid resin 14 are fed from the feed port 3 of the extruder 2 shown in FIG. 1, and additives 16 (e.g., acid-modified polypropylene) are further fed as necessary. At this time, it is preferable to adjust the content of the cellulosic fibers 12 to 25% by mass or more, more preferably 30% by mass or more, and even more preferably 40% by mass or more, based on the total mass of the kneaded products (12, 14, 16). As the content of the cellulosic fibers 12 increases (becomes more concentrated), the shear force of the screw 2b is more likely to act appropriately on the cellulosic fibers 12, and the defibration of the cellulosic fibers 12 can be promoted. By setting the content of the cellulosic fibers 12 to 30% by mass or more, preferably 40% by mass or more, it is possible to more reliably improve the defibration of the cellulosic fibers 12. There is no particular upper limit to the content of cellulosic fibers 12 in the kneaded material. However, for example, if the content of cellulosic fibers 12 is 70 mass% or less, deterioration of the fibers (for example, deterioration due to friction with the screw) can be effectively suppressed by the action of resin 14.

[0027] [Direct addition of water] Next, water 18 is directly fed into the extruder 2 from the feeding section 5 shown in FIG. 1 and is supplied to the kneaded product of the cellulose fiber 12, the resin 14, and the additive 16. In this embodiment, a sufficient amount of water 18 is directly fed into the extruder 2 to make the cellulose fiber 12 well dispersed, thereby making it possible to knead it with the resin 14 as uniformly as possible. The amount of water 18 fed can be set according to the mass of the kneaded product (particularly the content of the cellulose fiber 12). For example, when the content of the cellulose fiber in the kneaded product is 25% by mass or more, the amount of water 18 fed can be adjusted to 1% by mass or more, preferably 6% by mass or more, more preferably 6.5% by mass to 18% by mass, and even more preferably 6.7% by mass to 11% by mass. Here, when the amount of water 18 is less than 1% by mass, the aggregation of the cellulose fiber 12 is not appropriately suppressed, making it difficult to make a good dispersed state. By adding the above-mentioned predetermined amount of water 18, it becomes possible to suppress the aggregation of the cellulose fibers 12, and to promote the dispersion of the cellulose fibers 12. Here, the upper limit of the content of the cellulose fibers 12 in the kneaded product is not particularly limited as long as the dispersion can be ensured, but it can be set to 45 mass % assuming the use as a component of a vehicle. Note that the upper limit of the amount of water 18 added is set in consideration of the performance of a general-purpose input unit 5, and can be further increased depending on the performance of the input unit 5 used.

[0028] In this embodiment, the amount of water 18 added can be greater than the above setting in order to more reliably ensure the dispersion of the cellulose-based fibers 12. For example, the amount of water 18 added is adjusted to 8% by mass or more, preferably 8% by mass to 18% by mass, and more preferably 9% by mass to 11% by mass, based on the total mass of the kneaded material and water. This can further promote the dispersion of the cellulose-based fibers when the content of the cellulose-based fibers is 25% by mass or more, and can also more reliably promote the dispersion of the cellulose-based fibers when the content of the cellulose-based fibers 12 is high (30% by mass or more or 40% by mass or more).

[0029] In the extruder 2 shown in Fig. 1, the content of the cellulose-based fibers 12 in the kneaded product can also be adjusted by adding resin 14. That is, when the content of the cellulose-based fibers 12 in the kneaded product is high, the content of the cellulose-based fibers 12 can be adjusted (diluted) to the content at the stage of the fiber-reinforced resin composition 10 (product) by adding resin 14 from the input device 7. In this case, by directly inputting the molten resin 14 into the extruder 2, it is not necessary to melt the resin 14 in the extruder 2, and the content of the cellulose-based fibers 12 can be quickly diluted.

[0030] Then, the cellulosic fiber 12, the resin 14, and the additive 16 are mixed as uniformly as possible by the extruder 2 shown in FIG. 1, and the excess water 18 in the extruder 2 is discharged from the discharge section 6 to the outside. The fiber-reinforced resin composition 10 thus produced is cut into pellets after being discharged from the outlet 4 to the outside. Since the fiber-reinforced resin composition 10 does not contain a water-soluble polymer, it is unlikely to undergo unintended dimensional changes and is unlikely to cause condensation on peripheral devices. Furthermore, since the fiber-reinforced resin composition 10 is mixed with the cellulosic fiber 12, the resin 14, and the additive 16 as uniformly as possible, it has excellent mechanical properties. Furthermore, since the fiber-reinforced resin composition 10 is mixed in the presence of sufficient water 18, it is less colored by heat and has a good appearance.

[0031] As described above, in this embodiment, by directly feeding the water 18 into the extruder 2, a sufficient amount of water 18 can be supplied to the kneaded product of the cellulosic fiber 12 and the resin 14. Therefore, in the present invention, the cellulosic fiber 12 can be well dispersed by a sufficient amount of water 18, and even if the water-soluble polymer is omitted, the cellulosic fiber 12 can be kneaded with the resin 14 as uniformly as possible. In this embodiment, when the content of the cellulosic fiber 12 in the kneaded product is 25% by mass or more, the cellulosic fiber 12 and the resin 14 can be kneaded as uniformly as possible by feeding 1% by mass or more of water 18 with respect to the total mass of the kneaded product and water. In this embodiment, by using the cellulosic fiber 12 after the drying treatment, the substantial amount of water in the extruder 2 can be adjusted by the amount of water 18 directly fed. In this embodiment, the discharge section 6 is provided in the extruder 2, so that the excess water 18 in the extruder 2 can be discharged to the outside at the end of the kneading process. Therefore, according to this embodiment, the cellulosic fibers 12 and the resin 14 can be kneaded as uniformly as possible without causing excessive water absorption and release.

[0032] [Test example] Hereinafter, the present embodiment will be described based on test examples, but the present invention is not limited to the test examples. [Table 1] below shows the mechanical properties of the fiber reinforced resin composition of Example 1 and the fiber reinforced resin compositions of Comparative Examples 1 and 2, and [Table 2] shows the mechanical properties of the fiber reinforced resin composition of Example 2 and the fiber reinforced resin composition of Comparative Example 3. In addition, Figs. 3 to 5 are diagrams showing the calculation procedure of the aggregation rate of the fiber reinforced resin composition of Example 1. Figs. 6 to 8 are diagrams showing the calculation procedure of the aggregation rate of the fiber reinforced resin composition of Comparative Example 1, and Figs. 9 to 11 are diagrams showing the calculation procedure of the aggregation rate of the fiber reinforced resin composition of Comparative Example 2.

[0033] [Extruder] As the extruder, a twin-screw extruder (manufactured by Japan Steel Works, Ltd., product name: TEX30, L / D=77, D=30 mm) was used. Also, referring to FIG. 2, a liquid addition pump (manufactured by Takumina Corporation, product name: SXP2-006-STS-UWX, feeding conditions: 370 ml / h) was installed in section C4 of the extruder 2 as the feeding section 5. Also, a water-sealed vacuum pump (manufactured by Shinko Seiki Co., Ltd., product name: SW-25S) was installed in section C10 of the extruder 2 as the discharge section 6. Also, a single-screw extruder (manufactured by Cosmotec Co., Ltd., product name: CT31N-1) was installed in section C6 of the extruder as the feeding device 7. And the kneading conditions were set to a temperature of 170° C., a rotation speed of 140 rpm, and a discharge rate of 5 kg / h.

[0034] [Example 1] In Example 1, a fiber-reinforced composition was produced using the above-mentioned extruder, which consisted of 66.7% by mass of polypropylene (manufactured by Prime Polymer Co., Ltd., product name: J108M, MFR: 40g / 10min), 30% by mass of softwood pulp, and 3.3% by mass of maleic anhydride-modified polypropylene (manufactured by Addivant, product name: Polybond 3200). The softwood pulp was dried (temperature: 80°C, time: 24 hours) using a vacuum dryer (manufactured by Yamato Scientific Co., Ltd., product name: DP610) before kneading.

[0035] In Example 1, the entire amount of softwood pulp, 33.35% by mass of solid polypropylene, and the entire amount of maleic anhydride-modified polypropylene were fed from the inlet of the extruder. Then, water was fed from the feeding section, and the amount of water fed was adjusted to be approximately 10% by mass with respect to the total mass of the kneaded product and water (the amount of water fed was 7.4% by mass when the fiber-reinforced resin composition was taken as 100% by mass (standard)). Then, 33.35% by mass of molten polypropylene was additionally fed from the feeding device, and the content of cellulose-based fibers in the kneaded product was adjusted to be 30% by mass, and excess water was discharged from the discharge section to prepare the fiber-reinforced resin composition of Example 1.

[0036] [Example 2] In the fiber reinforced resin composition of Example 2, the same blending components as those of Example 1 were used, but the difference from Example 1 was that the polypropylene was 71.7 mass% and the softwood pulp was 25 mass%. In Example 2, the entire softwood pulp, the entire solid polypropylene, and the entire maleic anhydride-modified polypropylene were fed from the inlet of the extruder. Then, water was fed from the feed section, and the amount of water fed was adjusted to 6.7 mass% with respect to the total mass of the kneaded product and water (the amount of water fed was 7.2 mass% when the fiber reinforced resin composition was taken as 100 mass% (standard)). After each blending component was kneaded, excess water was discharged from the discharge section to produce the fiber reinforced resin composition of Example 2.

[0037] [Comparative Example 1] In Comparative Example 1, a fiber-reinforced resin composition having the same blending components as in Example 1 was produced, but differed from Example 1 in that no water was fed into the extruder. That is, in Comparative Example 1, the entire amount of softwood pulp, 33.35 mass% of solid polypropylene, and the entire amount of maleic anhydride-modified polypropylene were fed into the inlet of the extruder and kneaded as they were. Then, 33.35 mass% of molten polypropylene was additionally fed from the feeding device, and the content of cellulose-based fibers in the kneaded product was adjusted to 30 mass%, thereby producing the fiber-reinforced resin composition of Comparative Example 1.

[0038] [Comparative Example 2] In Comparative Example 2, a fiber-reinforced resin composition having the same composition as that in Example 1 was produced, but it differed from Example 1 in that the softwood pulp was previously watered and water was not directly added to the extruder. That is, in Comparative Example 2, 33.7% by mass of water-impregnated softwood pulp (30% by mass of softwood pulp and 3.7% by mass of water based on the fiber-reinforced resin composition) was used. Then, the entire amount of water-impregnated softwood pulp, 33.35% by mass of solid polypropylene, and the entire amount of maleic anhydride-modified polypropylene were fed from the inlet of the extruder. The amount of water at this time (the amount of water impregnated in the softwood pulp) was 5.3% by mass with respect to the total mass of the kneaded product and water. Then, 33.35% by mass of molten polypropylene was additionally fed from the feeding device to adjust the content of cellulose-based fibers in the kneaded product to 30% by mass, and excess water was discharged from the discharge section to produce the fiber-reinforced resin composition of Comparative Example 2.

[0039] [Comparative Example 3] In Comparative Example 3, a fiber-reinforced resin composition was produced with the same blending components as in Example 2, but was different from Example 2 in that no water was fed into the extruder. That is, in Comparative Example 3, the entire amount of softwood pulp, the entire amount of solid polypropylene, and the entire amount of maleic anhydride-modified polypropylene were fed into the inlet of the extruder. Then, the respective blending components were kneaded to produce the fiber-reinforced resin composition of Comparative Example 3.

[0040] [Mechanical property measurement test] The flexural modulus of the fiber reinforced resin compositions of each Example and Comparative Example was measured in accordance with "ISO178". The tensile strength of the fiber reinforced resin compositions of each Example and Comparative Example was measured in accordance with "ISO527-1,2". The breaking elongation of the fiber reinforced resin compositions of each Example and Comparative Example was measured in accordance with "ISO527-1,2". And the impact strength of the fiber reinforced resin compositions of Example 1 and Comparative Examples 1 and 2 was measured in accordance with "ISO179-1".

[0041] [Agglutination rate measurement test] In this test, a flat plate-shaped sample with a thickness of 0.5 mm was molded from the fiber reinforced resin composition of Example 1 using a small press. A 16 mm x 20 mm area of ​​this sample was magnified and observed using an optical microscope, and an image of the area was obtained (see FIG. 3). The obtained image was imported into the image processing software ImageJ, and then the image was binarized using the "Threshold" function so that it was divided into an aggregated part and a dispersed part (see FIG. 4). Next, the aggregated part was specified using the "Analyze Particle" function (see FIG. 5), and the area ratio of the aggregated part to the area of ​​the entire image was calculated as the aggregation rate. In addition, the aggregation rate of the fiber reinforced resin composition of Comparative Example 1 was calculated from the images shown in FIGS. 6 to 8, and the aggregation rate of the fiber reinforced resin composition of Comparative Example 2 was calculated from the images shown in FIGS. 9 to 11 by the same procedure.

[0042] [Table 1]

[0043] [Table 2]

[0044] [Results and Discussion] Referring to [Table 1], the fiber reinforced resin composition of Example 1 had a significantly lower coagulation rate than the fiber reinforced resin compositions of Comparative Examples 1 and 2, and had excellent mechanical properties (flexural modulus, tensile strength, elongation at break, and impact strength). Also, referring to [Table 2], the fiber reinforced resin composition of Example 2 also had excellent mechanical properties (flexural modulus, tensile strength, and elongation at break) compared to the fiber reinforced resin composition of Comparative Example 3. The results of each of these Examples are considered to be due to the fact that the cellulose-based fibers were able to be in a good dispersion state by directly feeding water into the extruder, and were able to be kneaded as uniformly as possible with the resin (see Figs. 3 to 5). And by comparing Example 1 with Comparative Example 1, the action of water on the cellulose fibers during kneading can be easily inferred (see Figs. 5 and 8). Furthermore, by comparing Example 1 with Comparative Example 2, it can be easily inferred that the direct feeding of water into the extruder contributes to good dispersion of the cellulose-based fibers (see Figs. 5 and 11). The method of Comparative Example 2 (containing water) could hardly improve the mechanical properties of the fiber reinforced resin composition.

[0045] Thus, according to each example, it was found that the cellulose-based fiber and the resin can be kneaded as uniformly as possible without excessive water absorption and release. Since the fiber-reinforced resin composition of each example does not contain a water-soluble polymer, it is easily presumed that the composition is unlikely to cause unintended dimensional changes and unlikely to cause condensation on peripheral devices. Furthermore, from the results of each example and Comparative Example 2, it was found that when the content of cellulose-based fiber in the kneaded material is 25% by mass or more, the amount of water directly input into the extruder can be set to 1% by mass or more, preferably 6% by mass or more, and more preferably 8% by mass or more, based on the total mass of the kneaded material and water.

[0046] The method for producing a fiber-reinforced resin composition according to the present embodiment is not limited to the above-mentioned embodiment, and may take various other embodiments. For example, in the present embodiment, an example in which the step of kneading the cellulose-based fiber and the resin is performed once has been described, but the same step can also be performed multiple times. For example, after kneading the cellulose-based fiber and the resin using a twin-screw extruder, excess water is discharged to obtain a pellet-shaped intermediate molded product. Then, this intermediate molded product is again fed into the twin-screw extruder to knead the cellulose-based fiber and the resin, thereby obtaining a fiber-reinforced resin composition. By performing kneading multiple times in this manner, it is possible to sufficiently defibrate the cellulose-based fiber, which contributes to improving the mechanical properties of the fiber-reinforced resin composition. In addition, in the present embodiment, each compounding component and water are fed into the extruder in this order, but the positions of the feed port and the feed section can be changed to feed the water first, and it is also possible to feed them into the extruder from the same section.

[0047] The pelletized fiber-reinforced resin composition can be molded into a predetermined shape by various molding methods such as injection molding, extrusion molding, compression molding, blow molding, transfer molding, cast molding, and inflation molding. After kneading the cellulose-based fiber and the resin with an extruder, the mixture can be directly put into an injection molding machine or the like without pelletizing. The fiber-reinforced resin composition of the present embodiment can be used for various applications, and can be used for various structures such as houses, as well as vehicle components such as interior and exterior materials for vehicles. The shape and dimensions of the fiber-reinforced resin composition can also be set according to the application, and can take various shapes such as a plate, a column, a cylinder, or a block. [Explanation of symbols]

[0048] 2. Extruder 2a Cylinder 2b Screw 3 Inlet 4 Outlet 5 Input section 6 Discharge section 7 Feeding device Sections C1 to C10 10 Fiber-reinforced resin composition 12 Cellulosic fibers 14 Resin 16 Additives 18 water

Claims

1. A method for producing a fiber-reinforced resin composition comprising a step of kneading cellulosic fibers and a resin in an extruder, Water is directly charged into the extruder to knead the cellulose-based fibers and the resin in a state in which the water-soluble polymer having water absorption properties is not contained, and A method for producing a fiber-reinforced resin composition, in which the cellulose-based fibers have a fiber diameter on the order of millimeters to micrometers and have been dried, are fed into the extruder.

2. The water is added in a state where the content of the cellulose-based fiber is adjusted to be 25% by mass or more based on the total mass of the kneaded product, and The method for producing a fiber-reinforced resin composition according to claim 1 , wherein the amount of water added is adjusted to be 1% by mass or more with respect to the total mass of the kneaded mixture and the water.

3. A method for producing a fiber-reinforced resin composition as described in claim 1 or 2, wherein the extruder is provided with a discharge section capable of discharging the water to the outside after kneading the cellulose-based fibers and the resin.

Citation Information

Patent Citations

  • Method of producing foamed plastics

    JP2002138157A

  • Method for producing aliphatic polyester composition, pulp used for the same, and cellulosic fiber, and method for microfibrillating the same

    JP2005042283A

  • Production apparatus and production method for microfibrillated cellulose composite resin material

    JP2015150838A

  • Production method of plated compact and plated compact

    JP2018104725A

  • Method for producing cellulosic resin composite

    JP2019218450A