Fire-resistant resin composition, fire-resistant material, and fittings
The fire-resistant resin composition addresses moldability and corrosion issues by neutralizing thermally expandable graphite with a sulfate salt, ensuring effective fire resistance and reduced equipment costs through improved moldability and expansion performance.
Patent Information
- Application Number
- JP2021167691
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-10-12
- Publication Date
- 2024-09-19
- Estimated Expiration
- 2040-09-24
AI Technical Summary
Existing fire-resistant resin compositions using thermally expandable graphite face issues with moldability due to acidic substances adhering to the graphite, leading to corrosion of molds and decreased expansion performance from excessive water washing, which increases equipment costs and reduces effectiveness.
A fire-resistant resin composition is developed by neutralizing thermally expandable graphite with a neutralizing agent to form a sulfate salt, which is then incorporated into the composition, preventing mold corrosion and maintaining expansion performance without water washing, thereby improving moldability and fire resistance.
The composition achieves excellent moldability and fire resistance by neutralizing thermally expandable graphite with a sulfate salt, enhancing the fire-resistant material's formability and reducing equipment costs while maintaining expansion performance.
Smart Images

Figure 0007554170000002 
Figure 0007554170000001 
Figure 0007554170000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a fire-resistant resin composition, a fire-resistant material, and a fitting including the fire-resistant material. [Background technology]
[0002] In the field of construction, fireproof materials are used for building materials such as fittings, pillars, and wall materials for fire prevention. Examples of fireproof materials include those made of resin mixed with inorganic fillers and thermally expandable graphite (see, for example, Patent Document 1). In general, thermally expandable graphite is a material in which the acid component inserted between the graphite layers is burned and gasified by rapid heating, and the gas released at that time explosively expands the gap between the layers, and it is widely used as a flame-retardant filler for resins and rubbers. Fire-resistant materials containing thermally expandable graphite have the above-mentioned characteristics of thermally expandable graphite and exhibit fire-resistant and insulating performance.
[0003] A fire-resistant material containing thermally expandable graphite is placed, for example, in the gap between fittings such as doors and windows installed in openings in buildings and the frames surrounding them, such as door frames and window frames; in the event of a fire, the sheet expands in the thickness direction to close the gap between the fittings and the frames and prevent the fire from spreading. Thermally expandable graphite is formed by inserting an acid component by a solid-liquid reaction between graphite and an acid such as sulfuric acid or nitric acid and an oxidizing agent, so that an acidic substance adheres to the graphite. Therefore, when used as a filler for a thermally expandable fire-resistant material, the resin is deteriorated by the acidic substance, the hardness of the residue after expansion is reduced, the viscosity of the fire-resistant resin composition is excessively increased by a chemical reaction, and a mold for forming the fire-resistant material from the fire-resistant resin composition is corroded, resulting in a deterioration in moldability (see, for example, Patent Document 2). As a means for solving this problem, the thermally expandable graphite is repeatedly washed with water and dried (see, for example, Patent Document 3). [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2017-141463 A [Patent Document 2] JP 2007-045676 A [Patent Document 3] JP 2019-215076 A Summary of the Invention [Problem to be solved by the invention]
[0005] However, when the step of washing the thermally expandable graphite with water is carried out several times, new problems arise, such as problems in terms of equipment costs due to the increase in the number of steps, and a decrease in expansion performance due to excessive washing with water.
[0006] Therefore, an object of the present invention is to provide a fire-resistant resin composition which has fire resistance and can be used to produce a fire-resistant material having excellent moldability. [Means for solving the problem]
[0007] As a result of intensive research, the present inventors have found that the above-mentioned problems can be solved by neutralizing the thermally expandable graphite with a neutralizing agent and incorporating a sulfate as the neutralized salt in a fire-resistant resin composition containing a matrix component and thermally expandable graphite, and have completed the present invention as described below. That is, the present invention provides the following [1] to [8]. [1] A fire-resistant resin composition comprising: a matrix component which is at least one selected from the group consisting of a resin component and an elastomer component; thermally expandable graphite; and a sulfate, the content of the sulfate being 1% by mass or more and 30% by mass or less. [2] The fire-resistant resin composition according to the above [1], wherein the sulfate is at least one selected from the group consisting of normal salts and acid salts. [3] The fire-resistant resin composition according to [1] or [2] above, which does not contain a phosphorus component. [4] The fire-resistant resin composition according to any one of the above [1] to [3], wherein the matrix component contains a component having at least one of a halogen atom, or a structural unit derived from styrene or vinyl acetate. [5] The fire-resistant resin composition according to any one of the above [1] to [4], wherein the thermally expandable graphite is contained in an amount of 20 to 200 parts by mass per 100 parts by mass of the matrix component. [6] The fire-resistant resin composition according to any one of the above [1] to [5], wherein the sulfate is attached to a surface of the thermally expandable graphite. [7] A fire-resistant material comprising the fire-resistant resin composition according to any one of [1] to [6] above. [8] Building materials equipped with the fire-resistant material described in [7] above. Effect of the Invention
[0008] According to the present invention, there is provided a fire-resistant resin composition which has fire resistance and can be used to produce a fire-resistant material having excellent moldability. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] Hereinafter, the present invention will be described with reference to an embodiment. [Fire-resistant resin composition] The fire-resistant resin composition of the present invention is a fire-resistant resin composition containing a matrix component, thermally expandable graphite, and a sulfate.
[0010] <Thermal expandable graphite> The fire-resistant resin composition of the present invention contains thermally expandable graphite. Thermally expandable graphite expands when heated, and is obtained by treating graphite powder such as natural scaly graphite, pyrolytic graphite, and kish graphite with an inorganic acid and a strong oxidizing agent to generate a graphite intercalation compound, which is a type of crystalline compound that maintains the layered structure of carbon. Examples of the inorganic acid include concentrated sulfuric acid. Examples of the strong oxidizing agent include concentrated nitric acid, perchloric acid, perchlorates, permanganates, dichromates, and hydrogen peroxide. Examples of the inorganic acid include nitric acid, selenic acid, and the like, in addition to concentrated sulfuric acid.
[0011] The thermally expandable graphite obtained by the acid treatment as described above may be subjected to a neutralization treatment. In the present invention, by neutralizing the thermally expandable graphite, sulfate as a neutralized salt adheres to the surface of the thermally expandable graphite, and the sulfate adhered to the surface is used as it is as the sulfate to be contained in the fire-resistant resin composition. The sulfate is obtained by a neutralization reaction between sulfuric acid, which is an inorganic acid, and a neutralizing agent.
[0012] The neutralizing agent is not particularly limited as long as it can generate sulfates, which will be described later, by neutralizing thermally expandable graphite, but metal compounds such as alkali metal compounds, alkaline earth metal compounds, amphoteric metal compounds, ammonia, amines, etc. Alkaline earth metals are metal elements belonging to Group 2, and magnesium and beryllium are also considered to be types of alkaline earth metals.
[0013] Examples of the alkali metal compound used as a neutralizing agent include oxides, hydroxides, carbonates, and hydrogen carbonates of alkali metals. Examples of the oxides of alkali metals include lithium oxide, sodium oxide, and potassium oxide. Examples of the hydroxides of alkali metals include lithium hydroxide, sodium hydroxide, and potassium hydroxide. Examples of the carbonates of alkali metals include lithium carbonate, sodium carbonate, and potassium carbonate. Examples of the hydrogen carbonates of alkali metals include sodium hydrogen carbonate and potassium hydrogen carbonate.
[0014] Examples of alkaline earth metal compounds include oxides, hydroxides, carbonates, and hydrogen carbonates of alkaline earth metals. Examples of alkaline earth metal oxides include beryllium oxide, magnesium oxide, and calcium oxide. Examples of alkaline earth metal hydroxides include beryllium hydroxide, magnesium hydroxide, and calcium hydroxide. Examples of alkaline earth metal carbonates include beryllium carbonate, magnesium carbonate, and calcium carbonate. Examples of alkaline earth metal hydrogen carbonates include calcium hydrogen carbonate.
[0015] Examples of amphoteric metal compounds include oxides, hydroxides, and carbonates of aluminum. Examples of amines include monomethylamine, dimethylamine, trimethylamine, monoethylamine, diethylamine, triethylamine, and ethanolamine. The neutralizing agent may be used alone or in combination of two or more kinds. Of these, sodium hydroxide, calcium hydroxide, potassium hydroxide, and magnesium hydroxide are preferred, and sodium hydroxide is more preferred.
[0016] As a specific method for the neutralization treatment, a wet method may be used in which the thermally expandable graphite is brought into contact with a solution containing a neutralizing agent (hereinafter also referred to as a "neutralizing agent-containing solution") to perform the neutralization treatment, or the neutralizing agent may be dry-blended in the form of a solid such as a powder or granules with the thermally expandable graphite, but a wet method is preferred. In the wet method, the thermally expandable graphite is immersed in a solution containing a neutralizing agent, the solution containing the neutralizing agent is stirred as necessary, and then the thermally expandable graphite is separated from the solution containing the neutralizing agent. The separation may be performed, for example, by filtration. After separation, the thermally expandable graphite may be appropriately dried. The solution containing the neutralizing agent may be, for example, an aqueous solution of the neutralizing agent.
[0017] The conditions of the neutralization treatment are not particularly limited as long as the sulfate salt can be obtained by neutralization. In addition, the amount of sulfate salt attached to the thermally expandable graphite and whether a normal salt or an acid salt is obtained can be appropriately adjusted by appropriately changing the conditions of the neutralization treatment. For example, in the wet method, normal salts can be easily generated by increasing the concentration of the neutralizing agent in the neutralizing agent-containing solution or increasing the temperature of the neutralizing agent-containing solution during the treatment with the neutralizing agent.
[0018] By carrying out the neutralization treatment as described above, it is possible to neutralize acidic substances such as sulfuric acid attached to the surface of the thermally expandable graphite. Therefore, even without going through a process of washing the thermally expandable graphite with water, it is possible to prevent the deterioration of the matrix component of the fire-resistant resin composition due to the acidic substances, and to prevent the corrosion of the mold for forming the fire-resistant material from the fire-resistant resin composition, and to improve the moldability of the fire-resistant material formed from the composition. In addition, by carrying out the removal of the acidic substances by the neutralization treatment as described above without going through a process of washing with water, it is possible to prevent the deterioration of the expansion performance of the thermally expandable graphite, ensure the fire resistance of the fire-resistant material, and keep the equipment costs for producing the fire-resistant resin composition and the fire-resistant material low.
[0019] The content of thermally expandable graphite in the fire-resistant resin composition is preferably 20 parts by mass or more, more preferably 30 parts by mass or more, even more preferably 70 parts by mass or more, and preferably 200 parts by mass or less, more preferably 150 parts by mass or less, and even more preferably 130 parts by mass or less, relative to 100 parts by mass of the matrix component. If the content of thermally expandable graphite is equal to or more than these lower limits, it becomes easier to obtain an expansion suitable for preventing the passage of flames, and if it is equal to or less than these upper limits, the strength of the thermally expanded residue of the fire-resistant material tends to be high, and the moldability of the fire-resistant material is improved. Note that, although sulfates may adhere to the surface of the thermally expandable graphite as described above, the content referred to here does not include sulfates.
[0020] <Sulfates> The fire-resistant resin composition of the present invention contains a sulfate. The sulfate is preferably at least one selected from the group consisting of normal salts and acid salts. Among them, normal salts are more preferable from the viewpoint of increasing the water resistance of the fire-resistant material formed from the fire-resistant resin composition. Examples of normal salts of sulfates include aluminum sulfate, ammonium sulfate, potassium sulfate, calcium sulfate, sodium sulfate, beryllium sulfate, magnesium sulfate, lithium sulfate, and rubidium sulfate. Examples of acid salts of sulfates include ammonium hydrogen sulfate, potassium hydrogen sulfate, and sodium hydrogen sulfate. These may be used alone or in combination of two or more.
[0021] Of the above-mentioned sulfates, from the viewpoints of fire resistance, moldability, and ease of production, at least one selected from the group consisting of calcium sulfate, sodium sulfate, and sodium hydrogen sulfate is preferable, at least one selected from the group consisting of calcium sulfate and sodium sulfate is more preferable, and from the viewpoint of water resistance, calcium sulfate is particularly preferable.
[0022] As described above, the sulfate is obtained by neutralizing the thermally expandable graphite, and may be present by adhering to the surface of the thermally expandable graphite, although a part of the sulfate may be separated from the thermally expandable graphite and be present in the matrix component of the fire-resistant resin composition. The sulfate can increase the expansion start temperature by coexisting with the thermally expandable graphite, and also acts as an aggregate to improve the residual hardness of the fireproof material, thereby improving the fire resistance. In addition, since the sulfate is poorly water-soluble, the water resistance is improved. Furthermore, since the sulfate plays a role of binding the layers of the thermally expandable graphite, the fracture of the thermally expandable graphite can be prevented when the fireproof resin composition is kneaded, and it becomes possible to form a fireproof material that is excellent in both fire resistance and moldability.
[0023] The content of sulfate in the fire-resistant resin composition is 1% by mass or more and 30% by mass or less with respect to the total amount of the fire-resistant resin composition. If the content of sulfate is less than 1% by mass, the expansion ratio and residual hardness of the fire-resistant material are reduced, resulting in a decrease in fire resistance and moldability. From the viewpoint of improving the fire resistance of the fire-resistant material, the content of sulfate is preferably 1.5% by mass or more, more preferably 3.0% by mass or more. On the other hand, if the content of sulfate exceeds 30% by mass, the viscosity of the fire-resistant resin composition is excessively increased, and the moldability of the fire-resistant material is deteriorated. From the viewpoint of improving the moldability of the fire-resistant material, the content of sulfate is preferably 15% by mass or less, more preferably 10% by mass or less.
[0024] <Matrix components> The fire-resistant resin composition of the present invention contains a matrix component, which is at least one component selected from the group consisting of a resin component and an elastomer component. From the viewpoint of increasing the strength of the thermal expansion residue of the fireproof material and improving the fire resistance, the matrix component of the present invention preferably contains a component having at least one of a halogen atom, or a structural unit derived from styrene or vinyl acetate. The component having at least one of a halogen atom, or a structural unit derived from styrene or vinyl acetate may be a resin component or an elastomer component.
[0025] (Resin component) The resin component in the matrix component may be a thermoplastic resin or a thermosetting resin, but is preferably a thermoplastic resin. Examples of the thermoplastic resin include polyolefin resins such as polypropylene resin, polyethylene resin, poly(1-)butene resin, and polypentene resin, polyester resins such as polyethylene terephthalate, polystyrene resin, acrylonitrile-butadiene-styrene (ABS) resin, ethylene-vinyl acetate copolymer resin (EVA), polycarbonate resin, polyphenylene ether resin, (meth)acrylic resin, polyamide resin, polyvinyl chloride resin (PVC), novolac resin, polyurethane resin, and polyisobutylene. From the viewpoint of fire resistance, the thermoplastic resin preferably contains at least one of a halogen atom and a structural unit derived from styrene or vinyl acetate. From such a viewpoint, among the thermoplastic resins, polyvinyl chloride resin (PVC) and ethylene-vinyl acetate copolymer resin (EVA) are preferred, and polyvinyl chloride resin (PVC) is more preferred.
[0026] Examples of polyvinyl chloride resins (PVC) include homopolymers of vinyl chloride monomers, copolymers of vinyl chloride monomers and monomers having unsaturated bonds copolymerizable with vinyl chloride monomers, and graft copolymers in which vinyl chloride monomers are graft-copolymerized onto polymers or copolymers other than vinyl chloride monomers. These may be used alone or in combination of two or more. In the present invention, chlorinated polyvinyl chloride resins, which are chlorinated polyvinyl chloride resins, are also included in the polyvinyl chloride resins. The degree of polymerization of the polyvinyl chloride resin is preferably from 500 to 2000, more preferably from 800 to 1500. Within such a range, the fluidity of the resin component is increased, making it easier to adjust the expansion ratio to a desired range.
[0027] The ethylene-vinyl acetate copolymer resin (EVA) may be a non-crosslinked ethylene-vinyl acetate copolymer resin or a high-temperature crosslinked ethylene-vinyl acetate copolymer resin. In addition, the ethylene-vinyl acetate copolymer resin may be a modified ethylene-vinyl acetate resin such as a saponified ethylene-vinyl acetate copolymer or a hydrolyzed ethylene-vinyl acetate. The ethylene-vinyl acetate copolymer resin preferably has a vinyl acetate content of 5 to 90 mass %, more preferably 8 to 50 mass %, and even more preferably 12 to 35 mass %, as measured in accordance with JIS K 6730 "Testing methods for ethylene-vinyl acetate resins". The melt flow rate (MFR) of the ethylene-vinyl acetate copolymer resin at 190° C. is preferably 0.5 to 15 g / 10 min, and more preferably 1 to 8 g / 10 min. The melt flow rate of the ethylene-vinyl acetate copolymer at 190° C. is a value measured under a load of 2.16 kg in accordance with JIS K7210:1999.
[0028] The thermosetting resin is not particularly limited, but examples thereof include epoxy resins, polyurethane resins, phenolic resins, melamine resins, urea resins, unsaturated polyester resins, alkyd resins, and thermosetting polyimides. Among these, epoxy resins are preferred from the viewpoint of improving fire resistance.
[0029] The epoxy resin may be an epoxy resin having an aromatic ring or an epoxy resin not having an aromatic ring, but from the viewpoint of enhancing non-flammability, an epoxy resin having an aromatic ring is preferable. The epoxy resin is obtained, for example, by reacting an epoxy resin compound having an epoxy group with a curing agent. Examples of the epoxy resin compound used to obtain the epoxy resin having an aromatic ring include bisphenol A type epoxy resin compounds, bisphenol F type epoxy resin compounds, biphenyl type epoxy resin compounds, naphthalene type epoxy resin compounds, phenol novolac type epoxy resin compounds, bisphenol A novolac type epoxy resin compounds, tetraphenolethane type epoxy resin compounds, tetraglycidyldiaminodiphenylmethane type epoxy resin compounds, aminophenol type epoxy resin compounds, aniline type epoxy resin compounds, xylylenediamine type epoxy resin compounds, etc. Among these, bisphenol A type epoxy resin compounds and bisphenol F type epoxy resin compounds are preferred.
[0030] The curing agent used may be of polyaddition type or catalyst type. Examples of polyaddition type curing agents include polyamines, acid anhydrides, polyphenols, and polymercaptans. Examples of catalyst type curing agents include tertiary amines, imidazoles, and Lewis acid complexes. The method for curing the epoxy resin compound is not particularly limited, and may be performed by a known method. The content of the curing agent is preferably within a range of 50 to 150 parts by mass relative to 100 parts by mass of the epoxy resin compound. When the content is 50 parts by mass or more, the epoxy resin compound is easily cured, and when the content is 150 parts by mass or less, an effect according to the amount of the curing agent is obtained.
[0031] (Elastomer component) The elastomer component in the matrix component is not particularly limited, and examples thereof include diene rubbers such as isoprene rubber (IR), butadiene rubber (BR), styrene-butadiene rubber (SBR), hydrogenated styrene-butadiene copolymer rubber (HSBR), chloroprene rubber (CR), and acrylonitrile-butadiene rubber (NBR); ethylene-propylene rubber (EPM), ethylene-propylene-diene rubber (EPDM), natural rubber, butyl rubber, chlorinated butyl rubber, chlorosulfonated polyethylene, acrylic rubber, epichlorohydrin rubber, multi-vulcanized rubber, non-vulcanized rubber, silicone rubber, fluororubber, and urethane rubber.
[0032] The elastomer component may be a thermoplastic elastomer, and specific examples thereof include olefin-based thermoplastic elastomers (TPO), styrene-based thermoplastic elastomers, ester-based thermoplastic elastomers, amide-based thermoplastic elastomers, vinyl chloride-based thermoplastic elastomers, and combinations thereof.
[0033] TPO is a thermoplastic elastomer that consists of polyolefins such as polyethylene and polypropylene as hard segments and rubbers such as ethylene-propylene rubber and ethylene-propylene-diene rubber as soft segments. Among these, from the viewpoint of improving the moldability and fire resistance of the fire-resistant material, it is preferable to contain an olefin-based thermoplastic elastomer (TPO). Styrene-based thermoplastic elastomers include block copolymers with polystyrene blocks as the hard segments, such as styrene-butadiene-styrene block copolymer (SBS), styrene-ethylene-styrene block copolymer (SES), styrene-ethylene-butylene-styrene block copolymer (SEBS), and styrene-ethylene-propylene-styrene block copolymer (SEPS).
[0034] From the viewpoint of fire resistance, it is preferable that the elastomer component contains a component having at least one of a halogen atom or a structural unit derived from styrene or vinyl acetate. From such a viewpoint, the elastomer component is preferably at least one selected from styrene-butadiene rubber (SBR), styrene-butadiene-styrene block copolymer (SBS), and chloroprene rubber (CR), and more preferably at least one selected from styrene-butadiene rubber (SBR) and chloroprene rubber (CR). Also, from the viewpoint of moldability, it is preferable to use EPDM, TPO, etc. as the elastomer component.
[0035] From the viewpoint of moldability, the matrix component is preferably a thermoplastic resin or an elastomer component. The matrix component may be composed of a component having at least one of a halogen atom, or a structural unit derived from styrene or vinyl acetate, but may also contain other components other than the above components. From the viewpoint of moldability, the other components are preferably elastomer components such as EPDM and TPO. From the viewpoint of fire resistance, the component having at least one of a halogen atom and a structural unit derived from styrene or vinyl acetate is preferably 50 to 100 mass %, more preferably 60 to 100 mass %, and even more preferably 70 to 100 mass %, based on the total amount of the matrix components.
[0036] From the viewpoint of increasing the dispersibility of the thermally expandable graphite and improving the fire resistance and moldability of the fire-resistant material, it is also preferable to use styrene-butadiene rubber (SBR) and chloroprene rubber (CR) in combination. When styrene-butadiene rubber (SBR) and chloroprene rubber (CR) are used in combination, the content ratio thereof (SBR / CR) is preferably from 90 / 10 to 10 / 90, and more preferably from 80 / 20 to 20 / 80, in mass ratio.
[0037] The bound styrene content of the styrene-butadiene rubber (SBR) used in the present invention is not particularly limited, but from the viewpoint of improving the moldability of the fire-resistant material, it is, for example, 10 to 60 mass%, preferably 15 to 55 mass%, and more preferably 20 to 50 mass%. 1 It can be measured by H-NMR. The Mooney viscosity [ML(1+4)100°C] of the styrene-butadiene rubber is not particularly limited, but is, for example, 30 to 150, preferably 35 to 70, and more preferably 40 to 60, from the viewpoint of improving the moldability of the fire-resistant material.
[0038] The Mooney viscosity [ML(1+4)100°C] of the chloroprene rubber (CR) is not particularly limited, but from the viewpoint of improving the moldability of the fire-resistant material, it is, for example, 25 to 150, preferably 30 to 100, and more preferably 35 to 75. In this specification, the Mooney viscosity is a value measured in accordance with JIS K6300.
[0039] The matrix component contains an elastomer component, and the content of the elastomer component is preferably 15% by mass or more based on the total amount of the matrix component. When the content of the elastomer component is 15% by mass or more, the fire-resistant sheet formed from the fire-resistant resin composition is prevented from becoming brittle, and defects such as cracks on the surface are less likely to occur even in cold regions. The content of the elastomer component is preferably 25% by mass or more, more preferably 50% by mass or more, even more preferably 80% by mass or more, and even more preferably 100% by mass based on the total amount of the matrix component.
[0040] The content of the matrix component in the fire-resistant resin composition is preferably 65% by mass or less, more preferably 60% by mass or less, and also preferably 20% by mass or more, more preferably 25% by mass or more. By making the content of the matrix component equal to or less than the upper limit, the fire-resistant resin composition can contain a certain amount or more of thermally expandable graphite, sulfate, and inorganic filler. Also, by making the content equal to or less than the lower limit, it is easy to improve moldability, etc.
[0041] <Inorganic filler> The fire-resistant resin composition of the present invention may contain an inorganic filler other than the above-mentioned thermally expandable graphite and sulfate. In the following description, when simply referring to "inorganic filler", it means an inorganic filler other than the above-mentioned thermally expandable graphite and sulfate. When heated to form an expansion insulation layer, the inorganic filler increases the heat capacity and suppresses heat transfer, while acting as an aggregate to improve the residual hardness of the fire-resistant material.
[0042] From the viewpoint of improving the moldability of the refractory material, it is preferable that the inorganic filler contains an inorganic filler A having a specific gravity of 2.5 or more. By including the inorganic filler A, the amount of matrix components per unit volume can be increased, which improves the brittleness of the refractory material and makes it easier to improve the moldability. From this viewpoint, the specific gravity of the inorganic filler A is preferably 3 or more, more preferably 4 or more. For example, metal oxides and metal carbonates described later can be used as the inorganic filler A having a specific gravity of 2.5 or more. The inorganic filler A may be used alone or in combination. The content of the inorganic filler A based on the total amount of the inorganic fillers is preferably 50% by mass or more, more preferably 80% by mass or more, and even more preferably 100% by mass.
[0043] As the inorganic filler, it is preferable to use the above-mentioned inorganic filler A having a specific gravity of 2.5 or more, but it is also possible to use an inorganic filler having a specific gravity of less than 2.5. The inorganic filler that can be used in the present invention is not particularly limited, and examples thereof include metal oxides such as alumina, zinc oxide, titanium oxide, calcium oxide, magnesium oxide, iron oxide, tin oxide, antimony oxide, and ferrite; metal carbonates such as calcium carbonate, zinc carbonate, strontium carbonate, and barium carbonate; metal hydroxides such as calcium hydroxide, magnesium hydroxide, aluminum hydroxide, and hydrotalcite; gypsum fiber; calcium salts such as calcium silicate; silica, diatomaceous earth, dawsonite, talc, clay, mica, montmorillonite, bentonite, activated clay, sepiolite, imogolite, sericite, glass fiber, glass beads, and silica. balloons, aluminum nitride, boron nitride, silicon nitride, carbon black, graphite, carbon fiber, carbon balloons, various metal powders, potassium titanate, lead zirconate titanate, aluminum borate, molybdenum sulfide, silicon carbide, stainless steel fiber, zinc borate, various magnetic powders, slag fiber, fly ash, metal phosphates such as sodium phosphate, potassium phosphate, magnesium phosphate, and aluminum phosphate, metal phosphite such as sodium phosphite, potassium phosphite, magnesium phosphite, and aluminum phosphite, ammonium polyphosphate, metal orthophosphate, metal metaphosphate, and metal tripolyphosphate. The inorganic fillers may be used alone or in combination of two or more.
[0044] Among these, from the viewpoint of improving fire resistance, the inorganic filler is preferably a metal oxide, a metal hydroxide, a metal carbonate, etc., and more preferably at least one selected from iron oxide, aluminum hydroxide, and calcium carbonate. More specifically, the inorganic filler is more preferably one that contains at least iron oxide, and a combination of iron oxide and calcium carbonate is also preferred. By using iron oxide, even when the expansion ratio of the fireproof material is relatively large, the strength of the thermal expansion residue is easily maintained, and therefore the fire resistance is easily improved. When iron oxide is contained, the content of iron oxide is preferably 15 mass % or more, more preferably 25 mass % or more, and even more preferably 40 mass % or more, based on the total amount of the inorganic filler.
[0045] The total content of the thermally expandable graphite, sulfate, and inorganic filler in the fire-resistant resin composition is preferably 35% by mass or more. When the total content is 35% by mass or more, the expansion ratio of the fire-resistant sheet and the strength of the thermal expansion residue become good, and excellent fire resistance can be imparted to the fire-resistant resin composition. From the viewpoint of improving fire resistance, the total content of the thermally expandable graphite and the inorganic filler is more preferably 40% by mass or more. From the viewpoint of increasing the blending amount of the matrix component and improving moldability, the above total content is preferably 80% by mass or less, more preferably 75% by mass or less.
[0046] <Plasticizer> The fire-resistant resin composition of the present invention may contain a plasticizer. When the fire-resistant resin composition contains a plasticizer, the matrix component becomes more fluid, and the fire-resistant material becomes more expandable. When a polyvinyl chloride resin is used as the matrix component, it is preferable to use a plasticizer in combination. Furthermore, the moldability is improved by using a plasticizer.
[0047] The plasticizer is not particularly limited, but examples thereof include phthalate ester plasticizers such as di-2-ethylhexyl phthalate (DOP), dibutyl phthalate (DBP), diheptyl phthalate (DHP), and diisodecyl phthalate (DIDP), fatty acid ester plasticizers such as di-2-ethylhexyl adipate (DOA), diisobutyl adipate (DIBA), and dibutyl adipate (DBA), epoxidized ester plasticizers such as epoxidized soybean oil, adipic acid ester plasticizers such as adipic acid ester and adipic acid polyester, trimellitic acid ester plasticizers such as tri-2-ethylhexyl trimellitate (TOTM) and triisononyl trimellitate (TINTM), and process oils such as mineral oil. The plasticizers may be used alone or in combination of two or more.
[0048] When the fire-resistant resin composition of the present invention contains a plasticizer, the content thereof is preferably 10 to 80 parts by mass, more preferably 20 to 60 parts by mass, per 100 parts by mass of the matrix component. When the content of the plasticizer is within the above range, extrusion moldability tends to be improved, and the molded body can be prevented from becoming too soft.
[0049] <Other ingredients> In addition to the above, the fire-resistant resin composition may appropriately contain various additives such as various organic flame retardants such as bromine-containing flame retardants, nitrogen-containing flame retardants, and phosphoric ester compounds, colorants, and antioxidants.
[0050] <Phosphorus component> The fire-resistant resin composition of the present invention preferably does not contain a phosphorus component. By not containing a phosphorus component, the water resistance of the fire-resistant material formed from the fire-resistant composition is improved. Therefore, even after long-term exposure to water, it is possible to ensure excellent expansion ratio, residual hardness, and shape retention after expansion. Here, the phosphorus component is a compound containing a phosphorus atom, and it is preferable not to use a compound containing a phosphorus atom as the above-mentioned matrix component, inorganic filler, and additives such as organic flame retardants, colorants, and antioxidants that are blended as necessary.
[0051] [Fireproof material] The fire-resistant resin composition of the present invention can be used to form a fire-resistant material made of the fire-resistant resin composition. The expansion ratio of the fireproof material in the thickness direction is not particularly limited, but from the viewpoint of fire resistance and water resistance, it is preferably 5 to 70 times, more preferably 10 to 60 times, and further preferably 15 to 55 times. It is preferable that the fireproof material of the present invention shows an expansion ratio in the above range even after being immersed in water for a long time. The expansion ratio is measured by the method described in the examples.
[0052] The thickness of the fireproof material is not particularly limited, but from the viewpoints of fire resistance and ease of handling, it is preferably 0.2 to 10 mm, more preferably 0.5 to 3.0 mm.
[0053] As described above, the fire-resistant material of the present invention has excellent formability and is unlikely to break or develop surface cracks during use, making it easy to handle even when the sheet is long, and can be used as a long product, for example, 1 m or more in length.
[0054] The fire-resistant resin composition and fire-resistant material of the present invention can be produced, for example, as follows. First, a predetermined amount of matrix component, thermally expandable graphite, and additives such as plasticizer, inorganic filler, organic flame retardant, colorant, and antioxidant, which are blended as necessary, are mixed in a mixer such as a kneading roll to obtain a fire-resistant resin composition. Note that, as described above, the sulfate is attached to the thermally expandable graphite, and is preferably blended into the fire-resistant resin composition together with the thermally expandable graphite. Next, the obtained fire-resistant resin composition is molded into a sheet by a known molding method such as press molding, calendar molding, extrusion molding, etc., to obtain a fire-resistant material.
[0055] The fireproofing material can be used in various buildings such as detached houses, apartment buildings, high-rise houses, high-rise buildings, commercial facilities, public facilities, etc., various vehicles such as automobiles and trains, and various vehicles such as ships and aircraft. When a fire breaks out in a building or vehicle, the fireproofing material expands by heating, blocking the flow of air and exerting fire-extinguishing properties. The fireproof material is attached to components constituting the above-mentioned buildings, vehicles, ships, aircraft, etc., and is used. For example, in buildings, the fireproof material is attached to fittings such as windows, shoji screens, doors, doors, and sliding doors, pillars, walls made of steel concrete, floors, roofs, etc., to reduce or prevent the intrusion of fire and smoke. Among these, it is preferable to use the fireproof material in fittings. That is, one embodiment of the present invention also provides fittings equipped with the fireproof material.
[0056] The fireproof material may be used alone, or may be used with other members attached as appropriate. For example, the fireproof material may be laminated with members other than the fireproof material, and a substrate may be provided on at least one surface of the fireproof material. The substrate may be a combustible material layer, or a quasi-noncombustible material layer or a noncombustible material layer. The thickness of the substrate is not particularly limited, but is, for example, 5 μm to 1 mm. Examples of materials used for the combustible material layer include one or more of cloth materials, paper materials, wood materials, and resin films. When the substrate is a quasi-noncombustible material layer or a noncombustible material layer, examples of the materials used include metals, inorganic materials, and the like, and more specifically, woven or nonwoven fabrics made of glass fibers, ceramic fibers, carbon fibers, and graphite fibers. In addition, composite materials of these fibers and metals may be used, and for example, aluminum glass cloth is preferable. In addition, an adhesive layer may be laminated on the sheet-shaped fireproof material. The adhesive layer may be provided on the substrate, or may be directly formed on the surface of the fireproof material. EXAMPLES
[0057] The present invention will be described in more detail below using examples, but the present invention is not limited to these examples.
[0058] [Evaluation method] (1) Expansion ratio A test piece (length 100 mm, width 100 mm, thickness 1.5 mm) made from the obtained refractory material was immersed in 500 mL of pure water in a sealed container at 60°C for one week, and then the sample was taken out. The sample was evaporated and dried at 60°C for 96 hours to prepare a test piece, which was placed on the bottom of a stainless steel holder (101 mm square, height 80 mm), fed into an electric furnace, and heated at 600°C for 30 minutes. The width, length, and thickness of the thickest part of the test piece were then measured, and the expansion ratio was calculated by ((thickness of test piece after heating) / (thickness of test piece before heating)).
[0059] (2) Residual hardness The heated test piece after measuring the expansion ratio was fed into a compression tester (Kato Tech Co., Ltd., "Finger Feeling Tester") and compressed at a speed of 0.1 cm / sec with a three-point indenter with a diameter of 1 mm. The maximum stress up to 10 mm compression from the top surface of the residue was measured, and the compressive strength (kgf / cm) of the test piece after combustion was calculated. 2 ) was measured.
[0060] (3) Shape retention The above-mentioned residue hardness is an index of the hardness of the residue after expansion, but since the measurement is limited to the surface portion of the residue, it may not be an index of the hardness of the entire residue. Therefore, shape retention was measured as an index of the hardness of the entire residue. The test piece for measuring the expansion ratio was lifted by holding both ends with hands, and the ease with which the residue crumbled was visually observed. The evaluation criteria were as follows: PASS: If the specimen is lifted without collapsing. FAIL: If the specimen collapses and cannot be lifted.
[0061] (4) Elution rate Five test pieces (length 50 mm, width 50 mm, thickness 1.5 mm) made from the obtained fireproof materials of each Example and Comparative Example were immersed in 200 g of pure water and left to soak in a sealed container at 60° C. for one week, after which the samples were taken out, the pure water in which they were immersed was evaporated and dried at 60° C. for 96 hours, and the mass of the precipitate that formed was measured. The elution rate was calculated using the following formula and used as an index of water resistance. Dissolution rate (%) = [(mass of precipitate) / (mass of refractory material before immersion in pure water)] × 100
[0062] (5) Formability The appearance of the obtained sheet was visually observed and rated as follows. A: No cracks, etc., and a smooth surface B: No cracks, but the surface is slightly rough. C: Cracks, wrinkles, or cracks are present.
[0063] [Examples 1 to 19, Comparative Examples 1 to 4] A matrix component, thermally expandable graphite, an inorganic filler, and a plasticizer were put into a roll and kneaded at 150°C for 5 minutes according to the formulation shown in Tables 1 to 3 below to obtain a fire-resistant resin composition. The obtained fire-resistant resin composition was press-molded at 150°C for 3 minutes to obtain a fire-resistant material having a thickness of 1.5 mm. The components used in each of the examples and comparative examples are as follows.
[0064] (1) Matrix components (i) Elastomer Component <Chloroprene rubber: CR> CR: Product name "Denka Chloroprene S-41", manufactured by Denka Co., Ltd., Mooney viscosity [ML(1+4)100℃]: 48
[0065] <Styrene-butadiene rubber: SBR> SBR: Product name "Nipol 1502", manufactured by Zeon Corporation, weight average molecular weight 500,000, bound styrene content: 23.5% by mass, Mooney viscosity [ML(1+4)100℃]: 52 <Styrene-butadiene-styrene copolymer: SBS> ·“TR1086” manufactured by SBS JSR Co., Ltd., amount of bound styrene: 45% by mass <Ethylene-propylene-diene rubber: EPDM> -EPDM "ENB-EPT X-3012P" manufactured by Mitsui Chemicals, Inc. <Olefin-based thermoplastic elastomer: TPO> -TPO "Milastomer 5020BS" manufactured by Mitsui Chemicals, Inc.
[0066] (ii) Resin component <Ethylene-vinyl acetate copolymer resin: EVA> EVA Mitsui DuPont Polychemicals Co., Ltd. "EV460" Vinyl acetate content: 19% by mass, MFR (190°C): 2.5g / 10min <Polyvinyl chloride resin: PVC> PVC Shin-Etsu Chemical Co., Ltd. "TK-1000", average degree of polymerization 1030
[0067] (2) Plasticizers DOP Di-2-ethylhexyl phthalate, "DOP" manufactured by JPlus Corporation
[0068] (3) Thermally expandable graphite Thermally expandable graphite A: 200g of 98% concentrated sulfuric acid was placed in a 500ml beaker, and 50g of 60% hydrogen peroxide was mixed into the concentrated sulfuric acid while cooling to below 20℃. 100g of flake natural graphite was added to this while stirring, and reacted at 30℃. After about 30 minutes, the slurry after the reaction was gradually added to a 1mol / L calcium hydroxide solution and neutralized at below 30℃, and this was collected by suction filtration using a Buchner funnel to obtain thermally expandable graphite A. In thermally expandable graphite A, calcium sulfate was attached to the surface of the thermally expandable graphite, and the mass ratio of thermally expandable graphite to calcium sulfate is as shown in Tables 1 and 2.
[0069] Thermally expandable graphite B: As with thermally expandable graphite A, flake natural graphite was reacted with concentrated sulfuric acid and hydrogen peroxide. After the reaction was completed, the mixture was gradually poured into a 1 mol / L sodium hydroxide solution and neutralized at 30°C, and the graphite intercalation compound produced by the reaction was collected by suction filtration using a Buchner funnel. This was then dried at 60-80°C to obtain thermally expandable graphite B. In thermally expandable graphite B, sodium sulfate was attached to the surface of the thermally expandable graphite, and the mass ratio of thermally expandable graphite to sodium sulfate is as shown in Tables 1 and 2.
[0070] Thermally expandable graphite C: As with thermally expandable graphite A, flake natural graphite was mixed with concentrated sulfuric acid and hydrogen peroxide to cause a reaction. After the reaction was completed, the mixture was gradually poured into a 0.01 mol / L sodium hydroxide solution and neutralized by stirring at 30°C for 5 minutes, and the graphite intercalation compound produced by the reaction was collected by suction filtration using a Buchner funnel. This was then dried at 60-80°C to obtain thermally expandable graphite C. In thermally expandable graphite C, sodium hydrogen sulfate was attached to the surface of the thermally expandable graphite, and the mass ratio of the thermally expandable graphite to sodium hydrogen sulfate is as shown in Tables 1 and 2. Thermally expandable graphite D: Air Water "CA-60N"
[0071] (4) Inorganic filler Iron oxide: Titanium Industries Co., Ltd. "BL-100", specific gravity 5.1 Calcium carbonate: "Whiten BF-300" manufactured by Bihoku Powder Industry Co., Ltd.
[0072] [Table 1]
[0073] [Table 2]
[0074] [Table 3]
[0075] As is clear from Tables 1 to 3, the fire-resistant materials formed from the fire-resistant resin compositions satisfying the present invention are excellent in both fire resistance and moldability. In addition, in Examples 3 and 4, which contain a large amount of thermally expandable graphite, some surface roughness is observed, but the expansion ratio is extremely high due to the large content of thermally expandable graphite. On the other hand, the fire-resistant materials formed from the fire-resistant resin compositions obtained in the Comparative Examples were impaired in at least one of fire resistance and moldability.
Claims
1. A matrix component including at least one selected from the group consisting of resin components, thermally expandable graphite, and a sulfate, the resin component is a polyvinyl chloride resin and / or an ethylene-vinyl acetate copolymer resin, the sulfate is at least one selected from the group consisting of aluminum sulfate, ammonium sulfate, potassium sulfate, calcium sulfate, sodium sulfate, beryllium sulfate, magnesium sulfate, lithium sulfate, rubidium sulfate, ammonium hydrogen sulfate, potassium hydrogen sulfate, and sodium hydrogen sulfate; The fire-resistant resin composition has a sulfate content of 1% by mass or more and 30% by mass or less.
2. The fire-resistant resin composition according to claim 1, which does not contain a phosphorus component.
3. 3. The fire-resistant resin composition according to claim 1, wherein the thermally expandable graphite is contained in an amount of 20 to 200 parts by mass per 100 parts by mass of the matrix component.
4. The fire-resistant resin composition according to any one of claims 1 to 3, wherein the sulfate is adhered to a surface of the thermally expandable graphite.
5. A fire-resistant material comprising the fire-resistant resin composition according to any one of claims 1 to 4.
6. A building fixture comprising the fireproof material according to claim 5.
Citation Information
Patent Citations
Flame retardation
JP1990206685A
Composite flame-retardant for rigid polyurethane foam
JP2001206978A
Thermally expansible graphite and its manufacturing method
JP2007045676A
Fireproof covering sheet for steel frame
JP2007162318A
Fire-resistant resin composition
JP2017141463A