Method for producing hardened hydraulic composition

The method addresses the challenge of high-temperature steam curing-induced cracking by using cement clinker, silica fume, and metakaolin to enhance salt penetration resistance in concrete, ensuring efficient production and reduced cracking.

JP7554571B2Active Publication Date: 2024-09-20TAIHEIYO CEMENT CORP
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
JP2020059730
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-03-30
Publication Date
2024-09-20
Estimated Expiration
2040-03-30

AI Technical Summary

Technical Problem

Existing methods for improving salt penetration resistance in secondary products like concrete through pozzolanic reaction promotion face challenges, particularly high-temperature steam curing leading to potential cracking due to delayed ettringite formation.

Method used

A method involving the use of cement clinker powder, silica fume, gypsum, and metakaolin, mixed at specific ratios, followed by steam curing at 70°C or higher for at least one hour, and subsequent curing to produce a cured product with enhanced salt penetration resistance.

Benefits of technology

The method efficiently produces a cured product with improved salt penetration resistance while minimizing cracking risks, achieving better strength and production efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007554571000001
    Figure 0007554571000001
  • Figure 0007554571000002
    Figure 0007554571000002
Patent Text Reader

Abstract

To provide a method enabling efficient production of a hydraulic composition hardened body excellent in salt penetration resistance.SOLUTION: There is provided a production method of a hydraulic composition hardened body including cement clinker powder, silica fume in an amount of 1 to 30 pts.mass relative to 100 pts.mass of the cement clinker powder, water, and plaster in an amount of 0 to 0.5 pt.mass in terms of SO3 relative to 100 pts.mass of the cement clinker powder. The production method of the hydraulic composition hardened body comprises: a composition preparing step of mixing each material constituting the hydraulic composition to obtain uncured hydraulic composition; a steam aging step of performing on the uncured hydraulic composition, steam aging for 1 hour or longer at a temperature of 70°C or higher to obtain a steam-aged hydraulic composition; and a hardening step of performing on the steam-aged hydraulic composition, aging for curing to obtain the hydraulic composition hardened body.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing a hardened product of a hydraulic composition. [Background technology]

[0002] A method using a pozzolanic admixture such as silica fume for the purpose of improving the salt penetration resistance of hardened bodies such as mortar and concrete is known. Patent Document 1 describes a highly durable mortar that can achieve sufficiently high levels of chloride penetration resistance, drying shrinkage suppression, frost damage resistance, and compressive strength while maintaining sufficient resistance to carbonation. The highly durable mortar contains a binder, silica fume, metakaolin, water, fine aggregate, and a chemical admixture, in which the binder contains cement, 1 to 15 parts by mass of the silica fume and 1 to 15 parts by mass of the metakaolin per 100 parts by mass of the binder, and the ratio (B / A) of the mass B of the water to the total mass A of the binder, the silica fume, and the metakaolin is 0.20 to 0.65. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2016-88777 A Summary of the Invention [Problem to be solved by the invention]

[0004] In order to improve resistance to salt penetration in secondary products such as concrete that use admixtures having pozzolanic reaction and are steam-cured, it is necessary to accelerate the pozzolanic reaction of the admixture. From the viewpoint of improving production efficiency, it is desirable for the pozzolanic reaction to occur early. As a method for accelerating and causing the pozzolanic reaction to occur early, a method of performing steam curing at high temperatures is known. However, when steam curing is performed at high temperatures, cracks may occur in the hardened body due to expansion caused by DEF (Delayed Ettringite Formation). For this reason, steam curing at temperatures above 65°C is not usually performed. An object of the present invention is to provide a method for efficiently producing a set product of a hydraulic composition having excellent resistance to salt penetration. [Means for solving the problem]

[0005] As a result of intensive research to solve the above problems, the present inventors have found that the above objects can be achieved by a method for producing a hardened product of a hydraulic composition, the method including the steps of: mixing cement clinker powder, silica fume in an amount of 1 to 30 parts by mass relative to 100 parts by mass of the cement clinker powder, and water, and the amount of gypsum is 0 to 0.5 parts by mass in terms of SO3 relative to 100 parts by mass of the cement clinker powder, to obtain an unhardened hydraulic composition; steam curing the unhardened hydraulic composition at a temperature of 70°C or higher for 1 hour or more to obtain a hydraulic composition after steam curing; and curing the hydraulic composition after steam curing to harden it, to obtain a hardened product of the hydraulic composition, and have completed the present invention. That is, the present invention provides the following [1] to [4].

[0006] [1] A method for producing a hardened hydraulic composition comprising cement clinker powder, silica fume in an amount of 1-30 parts by mass relative to 100 parts by mass of the cement clinker powder, and water, and the amount of gypsum is 0-0.5 parts by mass in terms of SO3 relative to 100 parts by mass of the cement clinker powder, the method comprising the steps of: mixing each material constituting the hydraulic composition to obtain an unhardened hydraulic composition; steam curing the unhardened hydraulic composition at a temperature of 70°C or higher for 1 hour or more to obtain a steam-cured hydraulic composition; and curing the steam-cured hydraulic composition to harden it, to obtain a hardened hydraulic composition. [2] A method for producing a hardened product of the hydraulic composition according to [1], wherein the hydraulic composition contains metakaolin in an amount of 30 parts by mass or less per 100 parts by mass of cement clinker powder. [3] The method for producing a hardened product of a hydraulic composition according to the above [1] or [2], wherein the steam curing in the steam curing step is normal pressure steam curing. [4] A method for producing a hardened product of the hydraulic composition according to any one of [1] to [3], wherein the hydraulic composition contains a hardening accelerator. Effect of the Invention

[0007] According to the method for producing a set product of a hydraulic composition of the present invention, a set product of a hydraulic composition having excellent resistance to salt penetration can be efficiently produced. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0008] The method for producing a hardened hydraulic composition of the present invention is a method for producing a hardened hydraulic composition containing cement clinker powder, silica fume in an amount of 1 to 30 parts by mass relative to 100 parts by mass of the cement clinker powder, and water, and the amount of gypsum is 0 to 0.5 parts by mass in terms of SO3 relative to 100 parts by mass of the cement clinker powder, and includes a composition preparation step of mixing each material constituting the hydraulic composition to obtain an unhardened hydraulic composition, a steam curing step of steam curing the unhardened hydraulic composition at a temperature of 70°C or higher for 1 hour or more to obtain a hydraulic composition after steam curing, and a hardening step of curing the hydraulic composition after steam curing to harden it, to obtain a hardened hydraulic composition.

[0009] Examples of the cement clinker used in the present invention include various types of Portland cement clinker such as ordinary Portland cement clinker, high early strength Portland cement clinker, moderate heat Portland cement clinker, and low heat Portland cement clinker. The Blaine specific surface area of ​​the cement clinker powder is preferably 2,000 to 10,000 cm 2 / g, more preferably 2,500 to 8,000 cm 2 / g, and particularly preferably 3,000 to 6,000 cm 2 / g. The above Blaine specific surface area is 2,000 cm 2 / g or more, the compressive strength (hereinafter sometimes abbreviated as "strength") of the set body of the hydraulic composition becomes larger. 2 When the viscosity is 100 / g or less, the fluidity of the hydraulic composition before hardening is further improved.

[0010] The amount of silica fume is 1 to 30 parts by mass, preferably 2 to 25 parts by mass, more preferably 3 to 20 parts by mass, and particularly preferably 4 to 18 parts by mass, based on 100 parts by mass of cement clinker powder. If the amount is less than 1 part by mass, the salt penetration resistance of the hardened body decreases. If the amount is more than 30 parts by mass, the strength of the hardened body decreases. The BET specific surface area of ​​the silica fume is preferably 10 to 25 m 2 / g, more preferably 12 to 20m 2 / g, particularly preferably 14 to 18m 2 / g. The specific surface area is 10m 2 If the specific surface area is 25 m / g or more, the strength of the set body of the hydraulic composition will be greater. 2 When the viscosity is 100 / g or less, the fluidity of the hydraulic composition before hardening is further improved.

[0011] The hydraulic composition may contain metakaolin in addition to silica fume. The amount of metakaolin is preferably 30 parts by mass or less, more preferably 4 to 25 parts by mass, even more preferably 6 to 22 parts by mass, still more preferably 8 to 17 parts by mass, and particularly preferably 9 to 12 parts by mass, based on 100 parts by mass of the cement clinker powder. If the amount is 30 parts by mass or less, the strength of the hardened body of the hydraulic composition becomes greater. The BET specific surface area of ​​metakaolin is preferably 8 to 20 m 2 / g, more preferably 9 to 15m 2 / g, particularly preferably 10 to 14m 2 / g. The specific surface area is 8m 2 If the specific surface area is 20m / g or more, the strength of the set body of the hydraulic composition will be greater. 2 When the viscosity is 100 / g or less, the fluidity of the hydraulic composition before hardening is further improved.

[0012] When the hydraulic composition contains metakaolin, the amount of silica fume is preferably 5 to 20 parts by mass, more preferably 6 to 18 parts by mass, and particularly preferably 8 to 12 parts by mass, per 100 parts by mass of cement clinker powder, from the viewpoint of increasing the strength of the hardened body of the hydraulic composition and further improving salt penetration resistance. In addition, from the viewpoint of increasing the strength of the hardened body of the hydraulic composition, the total amount of silica fume and metakaolin is preferably 50 parts by mass or less, more preferably 40 parts by mass or less, and particularly preferably 35 parts by mass or less, per 100 parts by mass of cement clinker powder.

[0013] The amount of water is not particularly limited and may be a general amount used in mortar, concrete, etc. For example, the amount of water is preferably an amount such that the mass ratio of water to cement clinker powder (water / cement clinker powder) is 0.2 to 0.6. The amount of gypsum, in terms of SO3, relative to 100 parts by mass of cement clinker powder is 0 to 0.5 parts by mass, preferably 0 to 0.3 parts by mass, more preferably 0 to 0.2 parts by mass, further preferably 0 to 0.1 parts by mass, and particularly preferably 0 part by mass. If the amount exceeds 0.5 parts by mass, when steam curing is performed at a high temperature exceeding 65°C, cracks are likely to occur in the hardened body of the hydraulic composition due to expansion caused by delayed formation of ettringite, so steam curing at 70°C or higher cannot be performed, and therefore the production efficiency of the hardened body of the hydraulic composition cannot be improved.

[0014] The hydraulic composition may further contain a hardening accelerator from the viewpoint of promoting hydration and shortening the curing time. The hardening accelerator may be any hardening accelerator that is generally used as an admixture for mortar or concrete, and examples of such hardening accelerators include nitrite-based, thiocyanate-based, sulfate-based, thiosulfate-based, chloride-based, carbonate-based, and alumina-based hardening accelerators. Among these, from the viewpoint of being able to hasten the initial setting time without decreasing the fluidity of the hydraulic composition before hardening, nitrite-based hardening accelerators are preferred, and calcium nitrite-based hardening accelerators are more preferred. The amount of the hardening accelerator is preferably 0.2 to 1.2 parts by mass, more preferably 0.4 to 1.0 parts by mass, and particularly preferably 0.6 to 0.9 parts by mass, calculated as a solid content based on 100 parts by mass of cement clinker powder. If the amount is 0.2 parts by mass or more, the setting start time of the hydraulic composition before hardening can be accelerated, so that a hardened product of the hydraulic composition with a desired strength can be obtained in a pre-curing time of about 1 to 4 hours (the time required for general pre-curing). If the amount is 1.2 parts by mass or less, the cost can be reduced.

[0015] The hydraulic composition may further contain at least one of a high-range water reducing agent and a high-range air-entraining water reducing agent from the viewpoint of reducing the amount of water relative to the cement clinker powder, thereby achieving high strength after hardening while maintaining the fluidity before hardening and obtaining better workability. The high-performance water-reducing agent or high-performance AE water-reducing agent may be any that is generally used as an admixture for mortar or concrete, and examples thereof include naphthalenesulfonic acid-based, melamine-based, polycarboxylic acid-based, etc. Among them, from the viewpoint of further improving the fluidity of the hydraulic composition before hardening, a polycarboxylic acid-based high-performance water-reducing agent or high-performance AE water-reducing agent is preferred, and a polycarboxylic acid ether-based high-performance water-reducing agent or high-performance AE water-reducing agent is more preferred. The amount of at least one of the high performance water reducing agent and the high performance AE water reducing agent (when the cement composition contains both the high performance water reducing agent and the above-mentioned high performance AE water reducing agent, the total amount) is preferably 0.1 to 1.0 part by mass, more preferably 0.2 to 0.8 part by mass, and particularly preferably 0.3 to 0.7 part by mass, in terms of solid content, relative to 100 parts by mass of cement clinker powder. If the amount is 0.1 part by mass or more, the fluidity of the hydraulic composition before hardening is improved. If the amount exceeds 1.0 part by mass, the cost becomes excessively high.

[0016] The hydraulic composition may contain other materials as necessary, such as aggregate, cement dispersant (excluding high performance water reducing agent and high performance AE water reducing agent), expansive material, shrinkage reducing agent, air content adjuster, etc. The aggregate may be fine aggregate alone or a combination of fine and coarse aggregate. The fine aggregate may be one or more selected from river sand, mountain sand, land sand, sea sand, crushed sand, silica sand, slag fine aggregate, lightweight fine aggregate, etc. In addition to natural aggregate, recycled aggregate may be used as the fine aggregate. The coarse aggregate may be one or more selected from river gravel, mountain gravel, land gravel, sea gravel, crushed stone, slag coarse aggregate, lightweight coarse aggregate, etc. As with the fine aggregate, the coarse aggregate may be natural or recycled. The amount of aggregate (the total amount when fine aggregate and coarse aggregate are used in combination) is not particularly limited, and may be a general amount used in mortar, concrete, etc. For example, the amount of aggregate is an amount such that the mass ratio of aggregate to cement clinker powder (aggregate / cement clinker powder) is preferably 1 to 7, more preferably 2 to 5.

[0017] Hereinafter, each step of the method for producing the hardened product of the hydraulic composition of the present invention will be described in detail. [Composition preparation process] This step is a step of mixing the above-mentioned materials constituting the hydraulic composition to obtain an unhardened hydraulic composition. The mixer used for mixing the materials is not particularly limited, and a conventional mixer such as a pan mixer or a twin-shaft mixer can be used. The mixing method is not particularly limited, and all of the materials may be put into a mixer at once and mixed, or the cement clinker powder, silica fume, and metakaolin and aggregate that are mixed as necessary may be put into a mixer and mixed dry, and then water and other materials that are mixed as necessary, etc. may be put in and mixed. After the composition preparation step, the resulting unhardened hydraulic composition is usually poured (cast) into a formwork, followed by a pre-curing step (described below) and a steam curing step.

[0018] [Pre-curing process] This step is an optional step between the composition preparation step and the steam curing step, and is a step of curing the uncured hydraulic composition obtained in the composition preparation step in air for 1 hour or more (preferably 1.5 to 6 hours, more preferably 2 to 5 hours). The temperature during air curing is usually room temperature (e.g., 5°C or more and less than 40°C, preferably 10 to 30°C). When the air curing time is 1 hour or more, the strength of the cured product of the hydraulic composition is further improved.

[0019] [Steam curing process] This process is a process in which the unhardened hydraulic composition obtained in the previous process (composition preparation process or pre-curing process) is steam-cured at a temperature of 70°C or higher for 1 hour or more to obtain a steam-cured hydraulic composition. In this process, steam curing is performed at a temperature of 70°C or higher for at least one hour, which promotes the pozzolanic reaction of silica fume and metakaolin, making the resulting hardened body denser and improving its resistance to salt penetration. In addition, since the hydraulic composition does not contain gypsum or contains a small amount of gypsum (0.5 parts by mass or less in terms of SO3 per 100 parts by mass of cement clinker powder), even when steam curing is performed at high temperatures (70°C or higher), a hardened body that is less likely to crack due to expansion caused by DEF (delayed formation of ettringite) can be obtained. The steam curing may be normal pressure steam curing carried out under atmospheric pressure, or high temperature / high pressure steam curing carried out under a pressure higher than normal pressure using an autoclave. Among these, normal pressure steam curing is preferred from the viewpoint of ease of production, etc.

[0020] In the steam curing, the temperature is raised for 1 hour or more (preferably 2 to 5 hours, more preferably 2 to 4 hours) until the desired maximum temperature is reached. The rate of temperature rise (range of temperature rise per unit time) until the desired maximum temperature is reached is preferably 10 to 30°C / hour. The time of steam curing in an atmosphere of 70°C or higher (preferably 80 to 100°C) is preferably 2 hours or more, more preferably 2 hours and 30 minutes or more, particularly preferably 3 hours or more, from the viewpoint of increasing the strength of the set body of the hydraulic composition. Moreover, the above time is preferably 10 hours or less, more preferably 8 hours or less, from the viewpoint of shortening the time required for producing the set body of the hydraulic composition. The maximum temperature in the steam curing is 70°C or higher, preferably 80 to 90°C, from the viewpoint of increasing the strength of the set body of the hydraulic composition and shortening the time required for the steam curing.

[0021] Then, the temperature is lowered to room temperature (about 20° C.) for 2 to 12 hours (preferably 3 to 11 hours). The rate of temperature drop (temperature drop per unit time) to room temperature (about 20° C.) is preferably 3 to 40° C. / hour, more preferably 5 to 20° C. / hour, and particularly preferably 6 to 10° C. / hour. The time required for the steam curing step (the time from the start of temperature increase to the end of temperature decrease) is preferably 16 hours or less, more preferably 15 hours or less, from the viewpoint of shortening the time required for manufacturing a product.

[0022] [Curing process] This step is a step of curing the hydraulic composition after the steam curing for hardening to obtain a hardened body of the hydraulic composition. The above-mentioned curing is usually performed by leaving it at rest at room temperature. EXAMPLES

[0023] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples. [Materials used] (1) Cement clinker powder; ordinary Portland cement clinker powder, manufactured by Taiheiyo Cement Corporation, Blaine specific surface area: 3,370 cm 2 / g, density: 3.15g / cm 3 (2) Cement: ordinary Portland cement, Blaine specific surface area: 3,000 cm, manufactured by Taiheiyo Cement Corporation 2 / g, density: 3.16g / cm 3 The amount of gypsum per 100 parts by mass of ordinary Portland cement clinker powder (SO3 equivalent value): 2.1 parts by mass (3) Silica fume; BET specific surface area: 15.6 m 2 / g, density: 2.25g / cm 3 (4) Metakaolin A; BET specific surface area: 13.6 m 2 / g, density: 2.64g / cm 3 , average particle size: 1.00μm (5) Metakaolin B; BET specific surface area: 11.4 m 2 / g, density: 2.73g / cm 3 , average particle size: 1.50μm (6) Fine aggregate; mountain sand, surface dry density 2.57g / cm 3 (7) High-performance water reducing agent; polycarboxylate ether-based high-performance water reducing agent, manufactured by BASF Japan Ltd., trade name "Masterglenium 8000S, Type M", solid content: 30% by mass (8) Air volume regulator: polyalkylene glycol derivative, BASF Japan Ltd., product name "Master Air 404" diluted 100 times (9) Hardening accelerator: calcium nitrite hardening accelerator, manufactured by Manol Corporation, trade name "Antifreezing material NAC-M", solid content 20% by mass

[0024] [Examples 1 to 7] The hydraulic compositions shown in Tables 1 and 2 were prepared. Specifically, cement clinker powder and the admixtures and fine aggregates shown in Tables 1 and 2 were charged into a 5-liter Hobart mixer, and dry-mixed at low speed for 15 seconds. Next, a liquid mixture of a high-performance water-reducing agent, an air content regulator, a hardening accelerator, and water was charged into the mixer and mixed at low speed for 60 seconds. After scraping off the materials adhering to the inner wall of the mixer, the mixture was mixed at high speed for 60 seconds. The mixture was left to stand in the mixer for 180 seconds, and then further mixed at low speed for 60 seconds to prepare mortar. The reason for leaving the mixture in the mixer for 180 seconds was to intentionally cause stiffness due to the lack of gypsum, and then to mix it again to minimize changes in the fluidity of the mortar. The flow value of the mortar immediately after mixing was measured by dropping it 15 times in accordance with JIS R 5201:2015 (Physical testing method for cement). In addition, the air content of the mortar was measured in accordance with JIS A 1116:2014 (Test method for unit volume mass of fresh concrete and test method for air content by mass (mass method)). In addition, the temperature of the mortar immediately after mixing was measured.

[0025] Furthermore, 30 minutes after pouring, the mortar was poured into a φ5×10cm steel formwork, sealed, and pre-cured at 20°C for 3 hours. After pre-curing, the temperature was raised to 90°C over 3 hours and 30 minutes (heating rate: 20°C / hour), held at 90°C (maximum temperature) for 3 hours, and then cooled to 20°C over 10 hours (cooling rate: 7°C / hour), for steam curing. After steam curing, the mortar was left to stand for 14 days in a sealed state at 20°C, and then demolded to obtain a hardened body. The hardened body obtained was cut horizontally to the casting surface to obtain a cylindrical specimen of φ5×5 cm. After applying epoxy resin to the side of the specimen to prevent salt from penetrating from the side, the specimen was immersed in a 10% by mass sodium chloride (NaCl) solution with the cut surface facing up. After 7 and 14 days of immersion, the specimens were removed, split in the axial direction, and a 0.1 mol / L silver nitrate solution was sprayed on the split surface. The depth from the cut surface to the part emitting fluorescence was measured with an electronic caliper, and this was taken as the salt penetration depth. In addition, the compressive strength of the obtained mortar at an age of 14 days was measured in accordance with "JIS R 5201:2015 (Physical testing method for cement)". The results are shown in Table 2.

[0026] [Comparative Example 1] A hardened body was obtained in the same manner as in Example 1, except that no admixture was used. The flow value of the mortar was measured in the same manner as in Example 1. [Comparative Example 2] After pre-curing, the temperature was increased to 65°C over 2 hours and 15 minutes (temperature increase rate: 20°C / hour), kept at 65°C (maximum temperature) for 3 hours, and then decreased to 20°C over 5 hours (temperature decrease rate: 7.5°C / hour). Except for this, steam curing was performed in the same manner as in Example 1 to obtain a hardened body. The flow value of the mortar was measured in the same manner as in Example 1. [Comparative Example 3] A hardened body was obtained in the same manner as in Example 1, except that hydraulic composition I shown in Table 1 was used instead of hydraulic composition A. The flow value of the mortar was measured in the same manner as in Example 1.

[0027] [Comparative Example 4] A hardened body was obtained in the same manner as in Example 1, except that ordinary Portland cement was used instead of the clinker powder and no hardening accelerator was used. The flow value of the mortar was measured in the same manner as in Example 1.

[0028] [Table 1]

[0029] [Table 2]

[0030] From Table 2, it can be seen that the salt penetration depths of Examples 1 to 7 (7 days: 2.76 to 3.84 mm, 14 days: 3.22 to 4.59 mm) are smaller than the salt penetration depths of Comparative Example 1 (not containing silica fume and metakaolin) (7 days: 12.42 mm, 14 days: 15.69 mm), Comparative Example 2 (similar to Example 1 except that the maximum temperature of steam curing is 65°C) (7 days: 7.31 mm, 14 days: 9.20 mm), Comparative Example 3 (not containing silica fume but containing metakaolin) (7 days: 5.50 mm, 14 days: 9.14 mm), and Comparative Example 4 (using ordinary Portland cement instead of cement clinker powder) (7 days: 6.61 mm, 14 days: 8.32 mm). In addition, since the hardened bodies of the hydraulic compositions of Examples 1 to 7 do not contain gypsum, it is considered that there is little possibility of cracks occurring in the hardened bodies due to expansion caused by DEF, even though they were subjected to steam curing at high temperatures (70°C or higher for 1 hour or more). On the other hand, since the hydraulic composition of Comparative Example 4 contains gypsum, the risk of cracks occurring in the hardened body due to expansion caused by DEF is considered to be higher than in Examples 1 to 7 and Comparative Examples 1 to 3, which do not contain gypsum.

Claims

1. A cement clinker powder, silica fume in an amount of 4 to 25 parts by mass per 100 parts by mass of the cement clinker powder, water, no metakaolin, and an amount of gypsum in the amount of SO 3 A method for producing a hardened body of a hydraulic composition having a converted value of 0 to 0.5 parts by mass, comprising the steps of: a composition preparation step of mixing the materials constituting the hydraulic composition to obtain an uncured hydraulic composition; a steam curing step of steam curing the uncured hydraulic composition at a temperature of 70° C. or higher for 1 hour or more to obtain a steam-cured hydraulic composition; a hardening step of hardening the hydraulic composition after the steam curing to obtain a hardened body of the hydraulic composition; A method for producing a hardened product of a hydraulic composition, comprising:

2. The method for producing a hardened product of a hydraulic composition according to claim 1, wherein the steam curing in the steam curing step is normal pressure steam curing.

3. The method for producing a hardened product of the hydraulic composition according to claim 1 or 2, wherein the hydraulic composition contains a hardening accelerator.

Citation Information

Patent Citations

  • Sprayed cement or dry-sprayed cement

    DE3340681A1

  • Use of a binder mixture to formulate a cementitious mortar system

    EP1614670A2

  • Cement of low porosity and method of manufacturing thereof

    JP1976138715A

  • Cement

    JP1981063851A

  • High iron-oxide cement composition

    JP2006306664A