Crosslinked polymer gel and method for producing the same, monomer composition, and method for producing crosslinked polymer particles
By polymerizing (meth)acrylic acid compounds with benzaldehyde, crosslinked polymer gels with high water retention and easy cutting are produced, addressing liquid leakage and processing challenges in absorbent articles.
Patent Information
- Application Number
- JP2021530644
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-07-05
- Filing Date
- 2020-07-01
- Publication Date
- 2024-09-20
- Estimated Expiration
- 2040-07-01
AI Technical Summary
Existing absorbent articles face issues with liquid leakage due to insufficient absorption capacity of water-absorbing resins, and processing crosslinked polymer gels for particles is challenging, requiring improved methods for easy cutting and high water retention.
A method involving polymerization of a monomer composition containing (meth)acrylic acid compounds and benzaldehyde to produce crosslinked polymer gels with high centrifuge retention capacity, which can be easily cut and processed into particles.
The method enables the production of crosslinked polymer gels with enhanced water retention capacity and ease of cutting, reducing processing forces and minimizing liquid leakage in absorbent articles.
Smart Images

Figure 0007554748000002 
Figure 0007554748000003 
Figure 0007554748000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a crosslinked polymer gel and a method for producing the same, a monomer composition, and a method for producing crosslinked polymer particles. [Background technology]
[0002] Conventionally, absorbent articles for absorbing liquids mainly composed of water (e.g., urine) have used absorbents containing water-absorbent resins (see, for example, Patent Document 1 below). The water-absorbent resin can be obtained, for example, by polymerizing at least one (meth)acrylic acid compound selected from the group consisting of (meth)acrylic acid and its salts to obtain a crosslinked polymer gel, and then crushing, drying and pulverizing the crosslinked polymer gel to obtain crosslinked polymer particles. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] Japanese Patent Application Publication No. 06-345819 Summary of the Invention [Problem to be solved by the invention]
[0004] When a liquid mainly composed of water is applied to an absorbent article, if the liquid is not sufficiently absorbed by the absorbent body of the absorbent article, the excess liquid may flow over the surface of the absorbent article and leak out of the absorbent article. Therefore, the water-absorbing resin constituting the absorbent body is required to have an excellent water-retention capacity. By using crosslinked polymer particles having an excellent water-retention capacity, a water-absorbing resin having an excellent water-retention capacity is easily obtained. For example, the centrifuge retention capacity of the crosslinked polymer particles is preferably 60 g / g or more.
[0005] When the crosslinked polymer gel is subjected to processing such as crushing to obtain crosslinked polymer particles having such a centrifuge retention capacity, it is preferable to avoid malfunctions in the processing device. For example, as an index of the ease of processing the crosslinked polymer gel, it is preferable that the crosslinked polymer gel be easily cut when it is cut.
[0006] One aspect of the present invention is to provide a method for producing a crosslinked polymer gel that can be easily cut. Another aspect of the present invention is to provide a crosslinked polymer gel that can be easily cut. Another aspect of the present invention is to provide a monomer composition from which a crosslinked polymer gel that can be easily cut can be obtained. Another aspect of the present invention is to provide a method for producing crosslinked polymer particles using the crosslinked polymer gel. [Means for solving the problem]
[0007] One aspect of the present invention provides a method for producing a crosslinked polymer gel, comprising: a step of polymerizing a monomer composition containing at least one (meth)acrylic acid compound selected from the group consisting of (meth)acrylic acid and its salts, and benzaldehyde to obtain a crosslinked polymer gel; and crushing, drying and pulverizing the crosslinked polymer gel to obtain crosslinked polymer particles having a centrifuge retention capacity of 60 g / g or more.
[0008] Another aspect of the present invention provides a monomer composition for obtaining a crosslinked polymer gel, the monomer composition comprising at least one (meth)acrylic acid compound selected from the group consisting of (meth)acrylic acid and its salts, and benzaldehyde, the crosslinked polymer gel being crushed, dried and pulverized to give crosslinked polymer particles having a centrifuge retention capacity of 60 g / g or more.
[0009] According to the above-mentioned method for producing a crosslinked polymer gel and the monomer composition, a crosslinked polymer gel that can be easily cut can be obtained.
[0010] Another aspect of the present invention provides a method for producing crosslinked polymer particles, which comprises crushing, drying and pulverizing the crosslinked polymer gel obtained by the above-mentioned method for producing a crosslinked polymer gel to obtain crosslinked polymer particles.
[0011] Another aspect of the present invention provides a crosslinked polymer gel having structural units derived from the monomer composition described above. Effect of the Invention
[0012] According to one aspect of the present invention, a method for producing a crosslinked polymer gel that can be easily cut can be provided. According to another aspect of the present invention, a crosslinked polymer gel that can be easily cut can be provided. According to another aspect of the present invention, a monomer composition that can give a crosslinked polymer gel that can be easily cut can be provided. According to another aspect of the present invention, a method for producing crosslinked polymer particles using the crosslinked polymer gel can be provided. [Brief description of the drawings]
[0013] [Figure 1] FIG. 1 is a cross-sectional view showing an example of an absorbent article. [Diagram 2] FIG. 13 is a diagram for explaining the test contents of a cutting test. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] Hereinafter, the embodiments of the present invention will be described in detail. However, the present invention is not limited to the following embodiments, and various modifications can be made within the scope of the present invention.
[0015] In this specification, "acrylic" and "methacrylic" are collectively written as "(meth)acrylic". "Acrylate" and "methacrylate" are also collectively written as "(meth)acrylate". "Polyethylene glycol" and "ethylene glycol" are collectively written as "(poly)ethylene glycol". The same applies to other expressions including "(poly)". In the numerical ranges described in stages in this specification, the upper limit or lower limit of a numerical range in a certain stage can be arbitrarily combined with the upper limit or lower limit of a numerical range in another stage. In the numerical ranges described in this specification, the upper limit or lower limit of the numerical range may be replaced with a value shown in the Examples. "Water-soluble" means that the material has a solubility of 5% by mass or more in water at 25°C. The materials exemplified in this specification may be used alone or in combination of two or more types. When a plurality of substances corresponding to each component are present in the composition, the content of each component in the composition means the total amount of the plurality of substances present in the composition, unless otherwise specified. "Physiological saline" means a 0.9% by mass aqueous solution of sodium chloride. The terms "content of (meth)acrylic acid compounds" and "total mass of (meth)acrylic acid compounds" refer to the total amount of acrylic acid, acrylic acid salts, methacrylic acid, and methacrylic acid salts. "ppm" refers to ppm by mass.
[0016] The method for producing a crosslinked polymer gel (aqueous crosslinked polymer gel) according to the present embodiment includes a polymerization step of polymerizing a monomer composition containing at least one (meth)acrylic acid compound selected from the group consisting of (meth)acrylic acid and its salts, and benzaldehyde to obtain a crosslinked polymer gel. The monomer composition according to the present embodiment is a monomer composition for obtaining a crosslinked polymer gel, and contains at least one (meth)acrylic acid compound selected from the group consisting of (meth)acrylic acid and its salts, and benzaldehyde. The centrifuge retention capacity (hereinafter sometimes referred to as "CRC") of the crosslinked polymer particles obtained by crushing, drying and pulverizing the crosslinked polymer gel obtained by the method for producing a crosslinked polymer gel and the monomer composition according to the present embodiment is 60 g / g or more.
[0017] According to the method for producing a crosslinked polymer gel and the monomer composition of the present embodiment, a crosslinked polymer gel that can be easily cut can be obtained. With such a crosslinked polymer gel, the force required to cut the gel can be reduced. The reason why the effect of being able to easily cut the gel is obtained is not clear, but the present inventors speculate as follows. However, the cause is not limited to the contents below. That is, when the CRC of the crosslinked polymer particles is 60 g / g or more, the polymerization rate is suitably controlled due to the presence of benzaldehyde during polymerization of the monomer composition containing a (meth)acrylic acid compound, so that the force required to cut the gel is reduced.
[0018] The crosslinked polymer gel according to the present embodiment can be obtained by the method for producing the crosslinked polymer gel according to the present embodiment and the monomer composition. The crosslinked polymer gel according to the present embodiment has a structural unit derived from the monomer composition according to the present embodiment.
[0019] The CRC of the crosslinked polymer particles is an abbreviation for Centrifuge Retention Capacity. The CRC of the crosslinked polymer particles can be measured by the method described in the Examples below with reference to the EDANA method (NWSP 241.0.R2(15), pages 769-778). Specifically, a nonwoven bag containing 0.2 g of dry crosslinked polymer particles is immersed in 1000 g of physiological saline for 30 minutes, and then centrifuged using a centrifuge to remove water, and the water absorption capacity can be obtained. The CRC of the crosslinked polymer particles can be measured at room temperature (25±1°C).
[0020] The CRC of the crosslinked polymer particles is 60 g / g or more. The CRC of the crosslinked polymer particles may be 65 g / g or more, 70 g / g or more, 75 g / g or more, 78 g / g or more, 80 g / g or more, 82 g / g or more, 84 g / g or more, 85 g / g or more, or 86 g / g or more. The CRC of the crosslinked polymer particles may be 100 g / g or less, 95 g / g or less, 90 g / g or less, or 87 g / g or less. From these viewpoints, the CRC of the crosslinked polymer particles may be 60 to 100 g / g. The crosslinked polymer particles having a CRC of 60 g / g or more are crosslinked polymer particles obtained by crushing, drying and pulverizing a crosslinked polymer gel, and may be crosslinked polymer particles obtained by classifying after pulverization as necessary, and may be particles with a particle size of 180 to 850 μm. For example, the coarse crushing method uses circular holes with a diameter of 6.4 mm at a density of 40 holes / 36.30 cm. 2 Drying can be carried out, for example, at 180°C for 30 minutes. Crushing can be carried out, for example, under conditions of a trapezoidal screen opening of 1 mm. The shape of the crosslinked polymer particles can be, for example, crushed, granular, etc.
[0021] The crosslinked polymer gel and crosslinked polymer particles according to the present embodiment may contain, for example, a crosslinked polymer obtained by polymerizing the monomer composition according to the present embodiment. The crosslinked polymer gel and crosslinked polymer particles according to the present embodiment may further contain other components such as a gel stabilizer, a metal chelating agent (ethylenediaminetetraacetic acid and its salts, diethylenetriaminepentaacetic acid and its salts (e.g., pentasodium diethylenetriaminepentaacetate), etc.), a flow improver (lubricant), etc. The other components may be located inside the crosslinked polymer, on the surface, or both.
[0022] The crosslinked polymer gel and the crosslinked polymer particles may include inorganic particles disposed on the surface of the crosslinked polymer. For example, the inorganic particles can be disposed on the surface of the crosslinked polymer by mixing the crosslinked polymer with the inorganic particles. Examples of the inorganic particles include silica particles such as amorphous silica.
[0023] The monomer composition according to the present embodiment may contain water, an organic solvent, and the like. The monomer composition according to the present embodiment may be an aqueous monomer solution. Examples of the polymerization method of the monomer composition include an aqueous solution polymerization method, a bulk polymerization method, and a precipitation polymerization method. Among these, the aqueous solution polymerization method is preferred from the viewpoint of easily obtaining good water absorption performance (e.g., CRC) and from the viewpoint of easy control of the polymerization reaction. In the following, a case where the aqueous solution polymerization method is used as an example of the polymerization method will be described.
[0024] The monomer composition according to the present embodiment contains at least one (meth)acrylic acid compound selected from the group consisting of (meth)acrylic acid and its salts, and benzaldehyde. The monomer composition according to the present embodiment may contain both (meth)acrylic acid and a salt of (meth)acrylic acid. Examples of the salt of (meth)acrylic acid include alkali metal salts (sodium salt, potassium salt, etc.) and alkaline earth metal salts (calcium salt, etc.).
[0025] The monomer composition may contain an ethylenically unsaturated monomer different from the (meth)acrylic acid compound. As the ethylenically unsaturated monomer, a water-soluble ethylenically unsaturated monomer can be used. Examples of ethylenically unsaturated monomers other than (meth)acrylic acid compounds include carboxylic acid monomers such as α,β-unsaturated carboxylic acids such as maleic acid, maleic anhydride, and fumaric acid, and salts thereof; nonionic monomers such as (meth)acrylamide, N,N-dimethyl(meth)acrylamide, 2-hydroxyethyl(meth)acrylate, N-methylol(meth)acrylamide, and polyethylene glycol mono(meth)acrylate; amino group-containing unsaturated monomers such as N,N-diethylaminoethyl(meth)acrylate, N,N-diethylaminopropyl(meth)acrylate, and diethylaminopropyl(meth)acrylamide, and quaternized products thereof; and sulfonic acid monomers such as vinyl sulfonic acid, styrene sulfonic acid, 2-(meth)acrylamido-2-methylpropanesulfonic acid, 2-(meth)acryloylethanesulfonic acid, and salts thereof.
[0026] The acid group of an ethylenically unsaturated monomer having an acid group (e.g., (meth)acrylic acid) may be neutralized in advance with an alkaline neutralizing agent. Examples of the alkaline neutralizing agent include alkali metal salts such as sodium hydroxide, sodium carbonate, sodium hydrogencarbonate, potassium hydroxide, and potassium carbonate; and ammonia. The alkaline neutralizing agent may be used in the form of an aqueous solution in order to simplify the neutralization operation. The neutralization of the acid group may be carried out before, during, or after the polymerization of the ethylenically unsaturated monomer as a raw material.
[0027] The degree of neutralization of the ethylenically unsaturated monomer by the alkaline neutralizer is preferably 10 to 100 mol%, 30 to 90 mol%, 40 to 85 mol%, or 50 to 80 mol%, from the viewpoint of easily obtaining good water absorption performance (e.g., CRC) by increasing the osmotic pressure and from the viewpoint of suppressing defects caused by the presence of an excess alkaline neutralizer. The "degree of neutralization" refers to the degree of neutralization of all acid groups possessed by the ethylenically unsaturated monomer.
[0028] The content of the (meth)acrylic acid compound is preferably in the following range based on the total mass of the monomer composition. The content of the (meth)acrylic acid compound is preferably 10% by mass or more, 15% by mass or more, 20% by mass or more, 25% by mass or more, 30% by mass or more, or 35% by mass or more from the viewpoint of easily obtaining a gel that can be easily cut and from the viewpoint of easily increasing the CRC. The content of the (meth)acrylic acid compound is preferably 60% by mass or less, 55% by mass or less, 50% by mass or less, less than 50% by mass, 45% by mass or less, or 40% by mass or less from the viewpoint of easily obtaining a gel that can be easily cut and from the viewpoint of easily increasing the CRC. From these viewpoints, the content of the (meth)acrylic acid compound is preferably 10 to 60% by mass. In the crosslinked polymer particles according to this embodiment, the content of the structural unit derived from the (meth)acrylic acid compound is preferably in the above-mentioned ranges regarding the content of the (meth)acrylic acid compound based on the total mass of the crosslinked polymer particles.
[0029] The content of the (meth)acrylic acid compound is preferably within the following range based on the total amount of the monomers contained in the monomer composition and / or the total amount of the ethylenically unsaturated monomers contained in the monomer composition. The content of the (meth)acrylic acid compound is preferably 50 mol% or more, 70 mol% or more, 90 mol% or more, 95 mol% or more, 97 mol% or more, or 99 mol% or more. The monomers contained in the monomer composition and / or the ethylenically unsaturated monomers contained in the monomer composition may be substantially composed of (meth)acrylic acid compounds (substantially 100 mol% of the monomers contained in the monomer composition and / or the ethylenically unsaturated monomers contained in the monomer composition are (meth)acrylic acid compounds).
[0030] Benzaldehyde may be contained in the (meth)acrylic acid compound, or may constitute the monomer composition independently of the (meth)acrylic acid compound.
[0031] The content of benzaldehyde is more than 0 mmol per mole of the (meth)acrylic acid compound, and is preferably in the following range: from the viewpoint of easily obtaining a gel that can be easily cut and from the viewpoint of easily increasing the CRC, the content of benzaldehyde is 0.0001 mmol or more, 0.0003 mmol or more, 0.0005 mmol or more, 0.001 mmol or more, 0.0025 mmol or more, 0.003 mmol or more, more than 0.003 mmol, 0.005 mmol or more, 0.01 mmol or more, 0.012 mmol or more, 0.02 mmol or more. More than 0.03 mmol, more than 0.05 mmol, more than 0.06 mmol, more than 0.08 mmol, more than 0.1 mmol, more than 0.1 mmol, more than 0.2 mmol, more than 0.25 mmol, more than 0.3 mmol, more than 0.3 mmol, more than 0.32 mmol, more than 0.4 mmol, more than 0.45 mmol, more than 0.5 mmol, more than 0.6 mmol, or more than 0.65 mmol. The content of benzaldehyde is preferably 10 mmol or less, 7 mmol or less, 6 mmol or less, 5 mmol or less, 4 mmol or less, 3 mmol or less, 2.5 mmol or less, 2 mmol or less, 1.5 mmol or less, 1 mmol or less, less than 1 mmol, less than 0.8 mmol or less, or less than 0.7 mmol, from the viewpoint of easily obtaining a gel that can be easily cut, easily increasing CRC, and easily suppressing the remaining of unreacted monomer. From these viewpoints, the content of benzaldehyde is preferably more than 0 mmol and not more than 10 mmol.
[0032] The benzaldehyde content exceeds 0 ppm based on the total mass of the monomer composition, and is preferably in the following range. From the viewpoint of easily obtaining a gel that can be easily cut and of easily increasing the CRC, the content of benzaldehyde is preferably 0.02 ppm or more, 0.1 ppm or more, 0.15 ppm or more, 0.2 ppm or more, 0.5 ppm or more, 1.0 ppm or more, 1.5 ppm or more, 2.0 ppm or more, 5.0 ppm or more, 7.5 ppm or more, 12 ppm or more, 12.5 ppm or more, 20 ppm or more, 25 ppm or more, 30 ppm or more, 35 ppm or more, 50 ppm or more, 60 ppm or more, 62.5 ppm or more, 75 ppm or more, 80 ppm or more, 90 ppm or more, 100 ppm or more, 125 ppm or more, 150 ppm or more, 175 ppm or more, 200 ppm or more, 250 ppm or more, 300 ppm or more, 350 ppm or more, or 360 ppm or more. From the viewpoint of easily obtaining a gel that can be easily cut and from the viewpoint of easily increasing the CRC, the content of benzaldehyde is preferably 3000 ppm or less, 2000 ppm or less, 1500 ppm or less, 1000 ppm or less, 800 ppm or less, 600 ppm or less, 500 ppm or less, 450 ppm or less, or 400 ppm or less. From these viewpoints, the content of benzaldehyde is preferably more than 0 ppm and 3000 ppm or less.
[0033] The monomer composition may contain a polymerization initiator. Polymerization of the monomer contained in the monomer composition may be initiated by adding a polymerization initiator to the monomer composition and, if necessary, heating, irradiating with light, or the like. Examples of the polymerization initiator include a photopolymerization initiator and a radical polymerization initiator, and a water-soluble radical polymerization initiator is preferred. From the viewpoint of easily obtaining a gel that can be easily cut and of easily increasing the CRC, the polymerization initiator preferably contains at least one selected from the group consisting of an azo compound and a peroxide.
[0034] Azo compounds include 2,2'-azobis[2-(N-phenylamidino)propane] dihydrochloride, 2,2'-azobis{2-[N-(4-chlorophenyl)amidino]propane} dihydrochloride, 2,2'-azobis{2-[N-(4-hydroxyphenyl)amidino]propane} dihydrochloride, and 2,2'-azobis[2-(N-benzylamidino)propane] dichloride. acid salt, 2,2'-azobis[2-(N-allylamidino)propane] dihydrochloride, 2,2'-azobis(2-amidinopropane) dihydrochloride, 2,2'-azobis{2-[N-(2-hydroxyethyl)amidino]propane} dihydrochloride, 2,2'-azobis[2-(5-methyl-2-imidazolin-2-yl)propane] dihydrochloride, 2,2'-azobis[2-( 2-imidazolin-2-yl)propane] dihydrochloride, 2,2'-azobis[2-(4,5,6,7-tetrahydro-1H-1,3-diazepin-2-yl)propane] dihydrochloride, 2,2'-azobis[2-(5-hydroxy-3,4,5,6-tetrahydropyrimidin-2-yl)propane] dihydrochloride, 2,2'-azobis{2-[1-(2-hydroxyethyl)-2-imidazolin-2-yl]propane} dihydrochloride, 2,2'-azobis[2-(2-imidazolin-2-yl)propane] disulfate dihydrate, 2,2'-azobis[N-(2-carboxyethyl)-2-methylpropionamidine] tetrahydrate, 2,2'-azobis[2-methyl-N-(2-hydroxyethyl)propionamide], and the like. From the viewpoint of easily obtaining a gel that can be easily cut and of easily obtaining good water absorption performance (e.g., CRC), the azo compound preferably contains at least one selected from the group consisting of 2,2'-azobis(2-methylpropionamide) dihydrochloride, 2,2'-azobis(2-amidinopropane) dihydrochloride, 2,2'-azobis{2-[1-(2-hydroxyethyl)-2-imidazolin-2-yl]propane} dihydrochloride, and 2,2'-azobis[N-(2-carboxyethyl)-2-methylpropionamidine] tetrahydrate.
[0035] Examples of the peroxide include persulfates such as potassium persulfate, ammonium persulfate, and sodium persulfate, and organic peroxides such as methyl ethyl ketone peroxide, methyl isobutyl ketone peroxide, di-t-butyl peroxide, t-butyl cumyl peroxide, t-butyl peroxyacetate, t-butyl peroxyisobutyrate, and t-butyl peroxypivalate. From the viewpoint of easily obtaining a gel that can be easily cut and of easily obtaining good water absorption performance (e.g., CRC), the peroxide preferably contains at least one selected from the group consisting of potassium persulfate, ammonium persulfate, and sodium persulfate.
[0036] The content of the polymerization initiator is preferably in the following range relative to 1 mole of the (meth)acrylic acid compound. The content of the polymerization initiator is preferably 0.001 mmol or more, 0.003 mmol or more, 0.015 mmol or more, 0.03 mmol or more, 0.06 mmol or more, 0.08 mmol or more, or 0.1 mmol or more from the viewpoint of easily obtaining a gel that can be easily cut, easily increasing the CRC, and easily avoiding a rapid polymerization reaction. The content of the polymerization initiator is preferably 5 mmol or less, 4 mmol or less, 2 mmol or less, 1 mmol or less, 0.5 mmol or less, 0.3 mmol or less, 0.25 mmol or less, 0.2 mmol or less, or 0.15 mmol or less from the viewpoint of easily obtaining a gel that can be easily cut, easily increasing the CRC, and easily avoiding a rapid polymerization reaction. From these viewpoints, the content of the polymerization initiator is preferably 0.001 to 5 mmol.
[0037] The monomer composition may contain a reducing agent. Examples of the reducing agent include sodium sulfite, sodium hydrogen sulfite, ferrous sulfate, L-ascorbic acid, etc. The polymerization initiator and the reducing agent may be used in combination.
[0038] The monomer composition may contain an oxidizing agent, such as hydrogen peroxide, sodium perborate, perphosphoric acid and its salts, potassium permanganate, and the like.
[0039] The monomer composition may contain an internal crosslinking agent. By using the internal crosslinking agent, the obtained crosslinked polymer can have a crosslinking structure caused by the internal crosslinking agent as its internal crosslinking structure in addition to the self-crosslinking structure caused by the polymerization reaction.
[0040] Examples of the internal crosslinking agent include compounds having two or more reactive functional groups (e.g., polymerizable unsaturated groups). Examples of the internal crosslinking agent include di- or tri(meth)acrylic acid esters of polyols such as (poly)ethylene glycol, (poly)propylene glycol, trimethylolpropane, glycerin polyoxyethylene glycol, polyoxypropylene glycol, and (poly)glycerin; unsaturated polyesters obtained by reacting the above polyols with unsaturated acids (maleic acid, fumaric acid, etc.); glycidyl group-containing compounds such as (poly)ethylene glycol diglycidyl ether, (poly)propylene glycol diglycidyl ether, (poly)glycerin diglycidyl ether, and glycidyl (meth)acrylate; bisacrylamides such as N,N'-methylenebis(meth)acrylamide; di- or tri(meth)acrylic acid esters obtained by reacting polyepoxides with (meth)acrylic acid. Examples of the internal crosslinking agent include esters; di(meth)acrylic acid carbamyl esters obtained by reacting a polyisocyanate (tolylene diisocyanate, hexamethylene diisocyanate, etc.) with hydroxyethyl (meth)acrylate; allylated starch; allylated cellulose; diallyl phthalate; N,N',N"-triallyl isocyanurate; divinylbenzene; pentaerythritol; ethylenediamine; and polyethyleneimine. From the viewpoints of easily obtaining a gel that can be easily cut, of easily increasing the CRC, and of excellent reactivity at low temperatures, it is preferable that the internal crosslinking agent contains at least one selected from the group consisting of (poly)ethylene glycol diglycidyl ether, (poly)propylene glycol diglycidyl ether, and (poly)glycerin diglycidyl ether.
[0041] The content of the internal crosslinking agent is preferably within the following range relative to 1 mole of the (meth)acrylic acid compound: From the viewpoint of easily obtaining a gel that can be easily cut and from the viewpoint of easily obtaining good water absorption performance (e.g., CRC), the content of the internal crosslinking agent is preferably 0.0005 mmol or more, 0.001 mmol or more, 0.002 mmol or more, 0.005 mmol or more, 0.01 mmol or more, 0.015 mmol or more, 0.02 mmol or more, or 0.025 mmol or more. The content of the internal crosslinking agent is preferably 0.3 mmol or less, 0.25 mmol or less, 0.2 mmol or less, 0.18 mmol or less, less than 0.18 mmol, 0.17 mmol or less, 0.16 mmol or less, 0.15 mmol or less, 0.1 mmol or less, 0.06 mmol or less, less than 0.06 mmol, 0.05 mmol or less, less than 0.05 mmol, 0.04 mmol or less, or 0.03 mmol or less, from the viewpoint of easily obtaining a gel that can be easily cut and from the viewpoint of easily obtaining good water absorption performance (for example, CRC). From these viewpoints, the content of the internal crosslinking agent is preferably 0.0005 to 0.3 mmol.
[0042] The monomer composition may contain additives such as chain transfer agents, thickeners, and inorganic fillers as components different from the above-mentioned components, as necessary. Examples of chain transfer agents include thiols, thiolic acids, secondary alcohols, hypophosphorous acid, phosphorous acid, and acrolein. Examples of thickeners include carboxymethyl cellulose, hydroxyethyl cellulose, hydroxypropyl cellulose, methyl cellulose, polyethylene glycol, polyacrylic acid, neutralized polyacrylic acid, and polyacrylamide. Examples of inorganic fillers include metal oxides, ceramics, and clay minerals.
[0043] Examples of the polymerization method of the aqueous solution polymerization include a static polymerization method in which the monomer composition is polymerized without stirring (for example, in a static state), and an agitation polymerization method in which the monomer composition is polymerized while being stirred in a reaction vessel, etc. In the static polymerization method, a single block-shaped gel is obtained at the completion of the polymerization, which has approximately the same volume as the monomer composition present in the reaction vessel.
[0044] The polymerization form may be batchwise, semi-continuous, continuous, etc. For example, when the stationary polymerization method is carried out as continuous polymerization, the polymerization reaction is carried out while continuously supplying the monomer composition to a continuous polymerization apparatus, and a gel can be obtained continuously.
[0045] The polymerization temperature varies depending on the polymerization initiator used, but from the viewpoints of rapidly progressing the polymerization, shortening the polymerization time to increase productivity, and facilitating the reaction by removing the heat of polymerization, it is preferably 0 to 130° C. or 10 to 110° C. The polymerization time is appropriately set depending on the type and amount of the polymerization initiator used, the reaction temperature, etc., but is preferably 1 to 200 minutes or 5 to 100 minutes.
[0046] In the method for producing crosslinked polymer particles according to the present embodiment, the crosslinked polymer gel obtained by the method for producing a crosslinked polymer gel according to the present embodiment is crushed, dried and pulverized to obtain crosslinked polymer particles. That is, the method for producing crosslinked polymer particles according to the present embodiment may include a gel preparation step for obtaining a crosslinked polymer gel by the method for producing a crosslinked polymer gel according to the present embodiment, a gel crushing step for crushing the crosslinked polymer gel to obtain a crushed product (gel crushed product), a drying step for drying the crushed product to obtain a dried product, and a dried product crushing step for pulverizing the dried product.
[0047] As the crushing device in the gel crushing step, for example, a kneader (pressure kneader, double-arm kneader, etc.), a meat chopper, a cutter mill, a farmer mill, etc. can be used.
[0048] In the drying step, liquid components (water, etc.) in the crushed material are removed by heating and / or blowing air to obtain a dried material (gel-dried material). The drying method may be natural drying, heat drying, spray drying, freeze drying, etc. The drying temperature is, for example, 70 to 250°C.
[0049] Examples of the pulverizer used in the pulverization step include a roller mill, a stamp mill, a jet mill, a high-speed rotary pulverizer (hammer mill, pin mill, rotor beater mill, etc.), and a vessel-driven mill (rotary mill, vibration mill, planetary mill, etc.).
[0050] The method for producing crosslinked polymer particles according to the present embodiment may include a classification step of classifying the pulverized product (pulverized product of the dried product) after the dried product pulverization step. In the classification step, the pulverized product can be divided into two or more particle groups having different particle size distributions. In the method for producing crosslinked polymer particles according to the present embodiment, the classification step may be performed multiple times by repeating the dried product pulverization step and the classification step, and the classification step may be performed after the additional crosslinking step described below. Examples of classification methods include screen classification and air classification. Examples of screen classification include a vibrating sieve, a rotary sifter, a cylindrical stirring sieve, a blower sifter, and a rotary tap shaker. Screen classification is a method of classifying particles on a screen into particles that pass through the mesh of the screen and particles that do not pass through the mesh by vibrating the screen. Air classification is a method of classifying particles by utilizing air flow.
[0051] The water-absorbent resin according to the present embodiment can be obtained by crosslinking the polymer after the gel crushing step. The crosslinking may be performed at any time after the gel crushing step, and may be performed before or after the drying step, before or after the pulverizing step, or before or after the classification step. The crosslinking may be surface crosslinking of the polymer particles. The crosslinking may be performed, for example, by reacting a crosslinking agent (for example, a surface crosslinking agent) with the polymer. By performing the crosslinking using a crosslinking agent, the crosslinking density of the polymer (for example, the crosslinking density near the surface of the polymer particles) is increased, and therefore the water absorption performance of the polymer (CRC, water absorption amount under load, water absorption speed, etc.) is easily increased.
[0052] Examples of the crosslinking agent include compounds containing two or more functional groups (reactive functional groups) that are reactive with functional groups derived from ethylenically unsaturated monomers. Examples of the crosslinking agent include polyols such as ethylene glycol, propylene glycol, 1,4-butanediol, trimethylolpropane, glycerin, polyoxyethylene glycol, polyoxypropylene glycol, and polyglycerin; polyglycidyl compounds such as (poly)ethylene glycol diglycidyl ether, (poly)glycerin diglycidyl ether, (poly)glycerin triglycidyl ether, (poly)propylene glycol polyglycidyl ether, and (poly)glycerol polyglycidyl ether; haloepoxy compounds such as epichlorohydrin, epibromohydrin, and α-methylepichlorohydrin; isocyanated compounds having two or more reactive functional groups, such as aryloxyalkyl groups such as aryloxyalkyl groups (e.g., 2,4-tolylene diisocyanate, hexamethylene diisocyanate); oxetane compounds such as 3-methyl-3-oxetanemethanol, 3-ethyl-3-oxetanemethanol, 3-butyl-3-oxetanemethanol, 3-methyl-3-oxetaneethanol, 3-ethyl-3-oxetaneethanol, and 3-butyl-3-oxetaneethanol; oxazoline compounds such as 1,2-ethylenebisoxazoline; carbonate compounds such as ethylene carbonate; and hydroxyalkylamide compounds such as bis[N,N-di(β-hydroxyethyl)]adipamide.
[0053] The water-absorbent resin according to the present embodiment may contain, on its surface, inorganic particles of a gel stabilizer; a metal chelating agent (ethylenediaminetetraacetic acid and its salts, diethylenetriaminepentaacetic acid and its salts (e.g., pentasodium diethylenetriaminepentaacetate), etc.); a flowability improver (lubricant), etc. For example, by mixing the polymer after additional crosslinking with inorganic particles, the inorganic particles can be arranged on the surface of the polymer. Examples of inorganic particles include silica particles such as amorphous silica.
[0054] The water-absorbent resin according to the present embodiment can retain water and absorb body fluids such as urine, sweat, and blood (e.g., menstrual blood). The water-absorbent resin according to the present embodiment can be used as a constituent component of an absorbent. The present embodiment can be used in fields such as sanitary materials such as paper diapers and sanitary products; agricultural and horticultural materials such as water retention agents and soil conditioners; and industrial materials such as water-stopping agents and dew condensation prevention agents.
[0055] The absorbent body according to the present embodiment contains the water-absorbing resin according to the present embodiment (e.g., water-absorbing resin particles). The absorbent body according to the present embodiment may contain fibrous material, for example, a mixture containing the water-absorbing resin and the fibrous material. The absorbent body may have a configuration in which the water-absorbing resin and the fibrous material are uniformly mixed, a configuration in which the water-absorbing resin is sandwiched between fibrous material formed in a sheet or layer shape, or other configurations.
[0056] Examples of the fibrous material include finely ground wood pulp, cotton, cotton linters, rayon, cellulosic fibers such as cellulose acetate, synthetic fibers such as polyamide, polyester, polyolefin, and mixtures of these fibers. Hydrophilic fibers can be used as the fibrous material.
[0057] In order to improve the shape retention of the absorbent body before and during use, the fibers may be bonded together by adding an adhesive binder to the fibrous material. Examples of the adhesive binder include heat-fusible synthetic fibers, hot melt adhesives, adhesive emulsions, etc.
[0058] Examples of heat-fusible synthetic fibers include fully melted binders such as polyethylene, polypropylene, and ethylene-propylene copolymers; non-fully melted binders having a side-by-side or core-sheath structure of polypropylene and polyethylene, etc. In the above-mentioned non-fully melted binders, only the polyethylene portion can be heat-fusible.
[0059] Examples of hot melt adhesives include mixtures of base polymers such as ethylene-vinyl acetate copolymers, styrene-isoprene-styrene block copolymers, styrene-butadiene-styrene block copolymers, styrene-ethylene-butylene-styrene block copolymers, styrene-ethylene-propylene-styrene block copolymers, and amorphous polypropylene with tackifiers, plasticizers, antioxidants, and the like.
[0060] The adhesive emulsion may be, for example, a polymer of at least one monomer selected from the group consisting of methyl methacrylate, styrene, acrylonitrile, 2-ethylhexyl acrylate, butyl acrylate, butadiene, ethylene, and vinyl acetate.
[0061] The absorbent body according to the present embodiment may contain inorganic powder (e.g., amorphous silica), a deodorant, an antibacterial agent, a pigment, a dye, a fragrance, an adhesive, etc. When the water-absorbent resin contains inorganic particles, the absorbent body may contain inorganic powder in addition to the inorganic particles in the water-absorbent resin.
[0062] The absorbent body according to this embodiment may be, for example, in a sheet shape. The thickness of the absorbent body (for example, the thickness of the sheet-shaped absorbent body) may be 0.1 to 20 mm or 0.3 to 15 mm.
[0063] The content of the water-absorbent resin in the absorbent body may be 2 to 95 mass %, 10 to 80 mass %, or 20 to 60 mass % based on the total of the water-absorbent resin and the fibrous material, from the viewpoint of easily obtaining sufficient absorption properties.
[0064] The content of the water-absorbent resin in the absorbent body is set at 1 / m 2 The content of the fibrous material in the absorbent body is preferably 100 to 1000 g, 150 to 800 g, or 200 to 700 g per m of the absorbent body from the viewpoint of easily obtaining sufficient absorption properties. 2 Preferably, the serving size is 50 to 800 g, 100 to 600 g, or 150 to 500 g.
[0065] The absorbent article according to the present embodiment includes the absorbent body according to the present embodiment. Other components of the absorbent article according to the present embodiment include a core wrap that maintains the shape of the absorbent body and prevents the components of the absorbent body from falling off or flowing; a liquid-permeable sheet that is disposed on the outermost side of the side into which the liquid to be absorbed penetrates; and a liquid-impermeable sheet that is disposed on the outermost side of the side opposite to the side into which the liquid to be absorbed penetrates. Examples of absorbent articles include diapers (e.g., paper diapers), toilet training pants, incontinence pads, sanitary materials (sanitary napkins, tampons, etc.), sweat pads, pet sheets, parts for simple toilets, and animal waste treatment materials.
[0066] Fig. 1 is a cross-sectional view showing an example of an absorbent article. The absorbent article 100 shown in Fig. 1 includes an absorbent body 10, core wraps 20a and 20b, a liquid-permeable sheet 30, and a liquid-impermeable sheet 40. In the absorbent article 100, the liquid-impermeable sheet 40, the core wrap 20b, the absorbent body 10, the core wrap 20a, and the liquid-permeable sheet 30 are laminated in this order. In Fig. 1, there are some parts shown as having gaps between the members, but the members may be in close contact with each other without the presence of such gaps.
[0067] The absorbent body 10 includes water-absorbent resin particles 10a containing the water-absorbent resin according to this embodiment, and a fiber layer 10b containing fibrous material. The water-absorbent resin particles 10a are dispersed in the fiber layer 10b.
[0068] The core wrap 20a is disposed on one side of the absorbent body 10 (upper side of the absorbent body 10 in FIG. 1) in contact with the absorbent body 10. The core wrap 20b is disposed on the other side of the absorbent body 10 (lower side of the absorbent body 10 in FIG. 1) in contact with the absorbent body 10. The absorbent body 10 is disposed between the core wrap 20a and the core wrap 20b. Examples of the core wraps 20a and 20b include tissue, nonwoven fabric, woven fabric, synthetic resin film having liquid permeable holes, and net-like sheet having mesh. The core wrap 20a and the core wrap 20b have a main surface of the same size as that of the absorbent body 10, for example.
[0069] The liquid-permeable sheet 30 is disposed on the outermost side of the absorbent article 100, on which the liquid to be absorbed penetrates. The liquid-permeable sheet 30 is disposed on the core wrap 20a in a state of contact with the core wrap 20a. Examples of the liquid-permeable sheet 30 include nonwoven fabrics and porous sheets made of synthetic resins such as polyethylene, polypropylene, polyester, and polyamide. The liquid-impermeable sheet 40 is disposed on the outermost side of the absorbent article 100, on the opposite side to the liquid-permeable sheet 30. The liquid-impermeable sheet 40 is disposed below the core wrap 20b in a state of contact with the core wrap 20b. Examples of the liquid-impermeable sheet 40 include sheets made of synthetic resins such as polyethylene, polypropylene, and polyvinyl chloride, and sheets made of composite materials of these synthetic resins and nonwoven fabrics. The liquid-permeable sheet 30 and the liquid-impermeable sheet 40 have, for example, a main surface that is wider than the main surface of the absorbent body 10, and the outer edges of the liquid-permeable sheet 30 and the liquid-impermeable sheet 40 extend around the absorbent body 10 and the core wraps 20a, 20b.
[0070] The size relationship between the absorbent body 10, the core wraps 20a, 20b, the liquid permeable sheet 30, and the liquid impermeable sheet 40 is not particularly limited and is adjusted as appropriate depending on the application of the absorbent article, etc. Furthermore, the method of maintaining the shape of the absorbent body 10 using the core wraps 20a, 20b is not particularly limited, and the absorbent body may be wrapped with multiple core wraps as shown in Fig. 1, or may be wrapped with one core wrap.
[0071] The absorbent may be bonded to the top sheet. When the absorbent is sandwiched or covered by a core wrap, it is preferable that at least the core wrap and the top sheet are bonded, and it is more preferable that the core wrap and the top sheet are bonded and the core wrap and the absorbent are bonded. Examples of the method of bonding the absorbent include a method of applying a hot melt adhesive to the top sheet in a stripe or spiral pattern at a predetermined interval in the width direction and bonding it; a method of bonding using a water-soluble binder such as starch, carboxymethyl cellulose, polyvinyl alcohol, polyvinylpyrrolidone, or other water-soluble polymer. In addition, when the absorbent contains a heat-fusible synthetic fiber, a method of bonding by heat fusion of the heat-fusible synthetic fiber may be adopted.
[0072] According to the present embodiment, a method for absorbing liquid using the water-absorbent resin, absorbent body, or absorbent article according to the present embodiment can be provided. The method for absorbing liquid according to the present embodiment includes a step of contacting the water-absorbent resin, absorbent body, or absorbent article according to the present embodiment with a liquid to be absorbed.
[0073] According to the present embodiment, it is possible to provide a method for manufacturing an absorbent body using the above-mentioned water-absorbent resin. The method for manufacturing an absorbent body according to the present embodiment includes a water-absorbent resin manufacturing step for obtaining the above-mentioned water-absorbent resin. The method for manufacturing an absorbent body according to the present embodiment may include a step of mixing the water-absorbent resin and a fibrous material after the water-absorbent resin manufacturing step. According to the present embodiment, it is possible to provide a method for manufacturing an absorbent article using an absorbent body obtained by the above-mentioned method for manufacturing an absorbent body. The method for manufacturing an absorbent article according to the present embodiment includes an absorbent body manufacturing step for obtaining an absorbent body by the above-mentioned method for manufacturing an absorbent body. The method for manufacturing an absorbent article according to the present embodiment may include a step for obtaining an absorbent article using the absorbent body and other components of the absorbent article after the absorbent body manufacturing step, and in this step, for example, the absorbent article is obtained by stacking the absorbent body and other components of the absorbent article on each other.
[0074] According to this embodiment, it is possible to provide the application of a water-absorbent resin, an absorbent body, and an absorbent article to liquid absorption. According to this embodiment, it is possible to provide the application of a crosslinked polymer gel to the adjustment of the force required when cutting the crosslinked polymer gel. According to this embodiment, it is possible to provide a method for adjusting the force required when cutting the crosslinked polymer gel, the method being based on the amount of benzaldehyde in the monomer composition for obtaining the crosslinked polymer gel, for adjusting the force required when cutting the crosslinked polymer gel. EXAMPLES
[0075] The present invention will be described in more detail below using examples and comparative examples, but the present invention is not limited to the following examples.
[0076] <Preparation of gel> Example 1 A stirrer (diameter: 8 mm, length: 40 mm, no ring) was placed in the center of a stainless steel tray (external dimensions of opening: 210 mm x 170 mm, internal dimensions of bottom: 170 x 130 mm, height: 30 mm) with a fluororesin-coated inner surface. 340.0 g of sodium acrylate partially neutralized solution (monomer used in polymerization, monomer concentration: 45 mass%, neutralization rate of sodium acrylate: 75 mol%), 0.0077 g of ethylene glycol diglycidyl ether (internal crosslinking agent, 0.044 mmol), 0.374 mg (0.0035 mmol) of benzaldehyde, and 59.0 g of ion-exchanged water were added, and the mixture was mixed uniformly by rotating the stirrer to obtain a mixture (concentration of sodium acrylate partially neutralized solution: 38 mass%). The stainless steel tray was then sealed by sealing the top of the tray with a polyethylene film. After adjusting the temperature of the mixture in the stainless steel bath to 25°C, the mixture was replaced with nitrogen to adjust the dissolved oxygen content to 0.1 ppm or less. Next, under stirring at 300 rpm, 3.09 g of 2 mass% potassium persulfate aqueous solution (potassium persulfate: 0.229 mmol) and 0.65 g of 0.5 mass% L-ascorbic acid aqueous solution were dropped in order to prepare a monomer aqueous solution. Polymerization started 2 minutes after the dropwise addition of the 0.5 mass% L-ascorbic acid aqueous solution. 22 minutes after the start of polymerization, the obtained product was immersed in a water bath at 75°C while still in the container and aged for 20 minutes to obtain a gel (gel after polymerization). The thickness of the gel was 1.3 cm. Two gels, Gel A for producing crosslinked polymer particles and Gel B for performing a cutting test, were obtained by performing the same operation.
[0077] Example 2 A gel was obtained by carrying out the same procedure as in Example 1, except that the amount of benzaldehyde used was changed to 1.245 mg (0.0117 mmol).
[0078] Example 3 A gel was obtained by carrying out the same procedure as in Example 1, except that the amount of benzaldehyde used was changed to 2.490 mg (0.0234 mmol).
[0079] Example 4 A gel was obtained by carrying out the same procedure as in Example 1, except that the amount of benzaldehyde used was changed to 87.15 mg (0.819 mmol).
[0080] Example 5 A gel was obtained by carrying out the same procedure as in Example 1, except that the amount of benzaldehyde used was changed to 124.5 mg (1.173 mmol).
[0081] Example 6 A gel was obtained by carrying out the same procedure as in Example 1, except that the amount of ethylene glycol diglycidyl ether used was changed to 0.0154 g (0.088 mmol) and the amount of benzaldehyde used was changed to 1.245 mg (0.0117 mmol).
[0082] Example 7 A stirrer (diameter: 8 mm, length: 40 mm, no ring) was placed in the center of a stainless steel tray (external dimensions of opening: 210 mm x 170 mm, internal dimensions of bottom: 170 x 130 mm, height: 30 mm) with a fluororesin-coated inner surface. 340.0 g of sodium acrylate partially neutralized solution (monomer used in polymerization, monomer concentration: 45 mass%, neutralization rate of sodium acrylate: 75 mol%), 0.0541 g of ethylene glycol diglycidyl ether (internal crosslinking agent, 0.311 mmol), 1.245 mg (0.0117 mmol) of benzaldehyde, and 59.0 g of ion-exchanged water were added, and the mixture was mixed uniformly by rotating the stirrer to obtain a mixture (concentration of sodium acrylate partially neutralized solution: 38 mass%). The stainless steel tray was then sealed by sealing the top of the stainless steel tray with a polyethylene film. After adjusting the temperature of the mixture in the stainless steel bath to 25°C, the mixture was replaced with nitrogen to adjust the dissolved oxygen content to 0.1 ppm or less. Next, under stirring at 300 rpm, 3.09 g of 2 mass% V-50 aqueous solution (2,2'-azobis(2-amidinopropane) dihydrochloride, 0.228 mmol, manufactured by Wako Pure Chemical Industries, Ltd.), 0.65 g of 0.5 mass% L-ascorbic acid aqueous solution, and 0.72 g of 0.35 mass% hydrogen peroxide solution were dropped in order to prepare an aqueous monomer solution. Polymerization started immediately after the 0.35 mass% hydrogen peroxide solution was dropped. 12 minutes after the start of polymerization, the obtained product was immersed in a water bath at 75°C while still in the container and aged for 20 minutes to obtain a gel (gel after polymerization). The thickness of the gel was 1.3 cm. Two gels, Gel A for producing crosslinked polymer particles and Gel B for performing a cutting test, were obtained by performing the same operation.
[0083] Comparative Example 1 A gel was obtained by carrying out the same procedure as in Example 1 except that benzaldehyde was not used.
[0084] Comparative Example 2 A gel was obtained by carrying out the same procedure as in Example 1, except that the amount of ethylene glycol diglycidyl ether used was changed to 0.0154 g (0.088 mmol) and no benzaldehyde was added.
[0085] (Comparative Example 3) A gel was obtained by performing the same operations as in Example 7 except that benzaldehyde was not used.
[0086] <Production of Crosslinked Polymer Particles> The gel A of each Example and Comparative Example was processed as follows to obtain respective crosslinked polymer particles. Eight rectangular parallelepiped gels with a width of 2 cm, a length of 13 cm, and a thickness of 1.3 cm were obtained from gel A using scissors. The rectangular parallelepiped gels were sequentially put into a meat chopper (Model No.: 12VR - 750SDX, manufactured by Kiren Royal Co., Ltd.). The diameter of the holes (circular) in the plate located at the discharge port of the meat chopper was 6.4 mm, and the hole density was 40 holes / 36.30 cm 2 and the crushing was carried out until no more crushed material (crushed gel) came out from the plate of the meat chopper. After spreading the crushed material on a net, a dried product was obtained by drying it in a hot air dryer (Model No.: FV - 320, manufactured by ADVANTEC) set at 180 °C for 30 minutes. The dried product was crushed using a crusher (Retsch, Rotabeater Mill, SR300) under the condition of a trapezoidal hole of the screen of 1 mm. The particles after crushing were classified with a sieve having an aperture of 850 μm and a sieve of 180 μm, and the crosslinked polymer particles that passed through the 850 - μm sieve and remained on the 180 - μm sieve were collected.
[0087] <CRC Measurement> With reference to the EDANA method (NWSP 241.0.R2(15), pages 769 - 778), the CRC of the crosslinked polymer particles was measured according to the following procedure.
[0088] A nonwoven fabric (product name: Heat Pack MWA-18, manufactured by Nippon Paper Papylia Co., Ltd.) measuring 60 mm x 170 mm was folded in half in the longitudinal direction to adjust the size to 60 mm x 85 mm. A nonwoven fabric bag measuring 60 mm x 85 mm was produced by heat-sealing the nonwoven fabric together on both sides extending in the longitudinal direction (a 5 mm-wide bonded portion was formed on both sides along the longitudinal direction). 0.2 g of the above-mentioned crosslinked polymer particles was placed inside the nonwoven fabric bag. The remaining side extending in the transverse direction was then heat-sealed to close the nonwoven fabric bag.
[0089] The nonwoven bag was floated on 1000 g of physiological saline contained in a stainless steel tray (240 mm x 320 mm x 45 mm) without being folded over, so that the entire nonwoven bag was completely wetted. One minute after the nonwoven bag was placed in the physiological saline, the nonwoven bag was immersed in the physiological saline with a spatula to obtain a nonwoven bag containing gel.
[0090] Thirty minutes after the nonwoven fabric bag was placed in the saline solution (a total of 1 minute of floating time and 29 minutes of immersion time), the nonwoven fabric bag was removed from the saline solution. The nonwoven fabric bag was then placed in a centrifuge (manufactured by Kokusan Co., Ltd., model number: H-122). After the centrifugal force in the centrifuge reached 250G, the nonwoven fabric bag was dehydrated for 3 minutes. After dehydration, the mass M of the nonwoven fabric bag including the mass of the gel was a The same operation as above was carried out on the nonwoven fabric bag without containing the crosslinked polymer particles, and the mass M b The CRC was calculated based on the following formula: c is the mass of the crosslinked polymer particles used in the measurement, 0.2 g. The results are shown in Table 1. CRC[g / g] = {(M a -M b )-M c} / M c
[0091] <Cutting test> Gel B of each of the Examples and Comparative Examples was treated as follows, and each was subjected to a cutting test.
[0092] Using scissors, six rectangular parallelepiped test pieces measuring 2 cm wide, 13 cm long, and 1.3 cm thick were obtained from Gel B. Since voids tend to form in the area where the stirrer was present in Gel B (near the center of the gel), test pieces were obtained from an area where no voids were formed.
[0093] A cutting test was performed using EZtest (product name: EZtest, model number: EZ-SX, manufactured by Shimadzu Corporation). A blade (long cutting blade, catalog name: 45° cut end surface t3mm) used for cutting gel was attached to a load cell with a capacity of 500N (upper limit of measurement set to 450N) with the tip of the blade facing downward in the vertical direction, and a jig was assembled. The blade has a cutting edge (length in the tip direction: 3mm, cutting edge narrowed toward the tip direction and having a sharp tip) and a plate-shaped support part that supports the cutting edge. The length of the cutting blade in the longitudinal direction including the cutting edge is 7cm. The cutting edge is formed over the entire one side of the support part, and the base end of the cutting edge and the support part have a width of 3mm. The cutting edge has a first cutting surface that is inclined from one side of the support part toward the tip direction, and a second cutting surface that is inclined from the other side of the support part toward the tip direction. The first blade surface and the second blade surface are inclined at 22.5° each relative to the tip direction, and the angle (inner angle) between the first blade surface and the second blade surface is 45°. The shape of a cross section perpendicular to the longitudinal direction at the cutting edge is an isosceles triangle.
[0094] Using Shimadzu Autograph Software Trapezium X (Shimadzu Corporation), the blade attached to the EZtest was operated to cut the test pieces according to the following procedure. Cutting was performed at room temperature (25±1°C).
[0095] The test piece was placed on the measurement table with the 2 cm x 13 cm surface of the test piece in contact with the measurement table and the longitudinal direction of the test piece perpendicular to the longitudinal direction of the blade. The blade was lowered manually and stopped when the load cell detected a load of 0.01 N. The blade was then raised 0.01 mm and this position was set as the measurement start point.
[0096] From the measurement start point, the blade was pushed against the surface of the test piece at a speed of 20 mm / min (set to move automatically using the Trapezium X's program function), and the load applied to the jig when the gel was cut was measured. Figure 2 is a diagram to explain the contents of the cutting test, and is a load-displacement curve showing the dependency of the load applied to the jig on the displacement of the jig. As the blade was pushed into the gel, the load increased, and when the gel was cut, the load rose sharply and then suddenly fell, forming a peak (see Figure 2(a)), and the load at the peak top P was obtained. When the test piece was not cut, the load reached the upper limit of measurement, 450 N (see Figure 2(b)).
[0097] The load (peak top load) at the time of cutting of each of the six test pieces was measured, and the average load (cutting force) was calculated. The results of the cutting test (average load) are shown in Table 1. In the examples and comparative examples, none of the loads (six peak top loads) reached 450 N.
[0098] [Table 1]
[0099] According to Table 1, when the CRC of the crosslinked polymer particles is 60 g / g or more, it is confirmed that using a monomer composition containing a (meth)acrylic acid compound and benzaldehyde is effective in obtaining a crosslinked polymer gel that can be easily cut. [Explanation of symbols]
[0100] Reference Signs List 10: absorbent body, 10a: water-absorbent resin particles, 10b: fiber layer, 20a, 20b: core wrap, 30: liquid-permeable sheet, 40: liquid-impermeable sheet, 100: absorbent article.
Claims
1. The method includes a step of polymerizing a monomer composition containing at least one (meth)acrylic acid compound selected from the group consisting of (meth)acrylic acid and salts thereof, and benzaldehyde to obtain a crosslinked polymer gel, the content of the benzaldehyde is 0.0001 millimol or more relative to 1 mole of the (meth)acrylic acid compound, A method for producing a crosslinked polymer gel, wherein the crosslinked polymer gel is crushed, dried and pulverized to give crosslinked polymer particles having a centrifuge retention capacity of 60 g / g or more.
2. The method for producing a crosslinked polymer gel according to claim 1, wherein the content of said benzaldehyde is 0.1 millimol or more per mole of said (meth)acrylic acid compound.
3. A method for producing crosslinked polymer particles, comprising crushing, drying and pulverizing the crosslinked polymer gel obtained by the method for producing a crosslinked polymer gel according to claim 1 or 2 to obtain crosslinked polymer particles.
4. A monomer composition for obtaining a crosslinked polymer gel, comprising: The composition contains at least one (meth)acrylic acid compound selected from the group consisting of (meth)acrylic acid and salts thereof, and benzaldehyde, the content of the benzaldehyde is 0.0001 millimol or more relative to 1 mole of the (meth)acrylic acid compound, A monomer composition, wherein the crosslinked polymer gel is crushed, dried and pulverized to give crosslinked polymer particles having a centrifuge retention capacity of 60 g / g or more.
5. 5. The monomer composition according to claim 4, wherein the content of the benzaldehyde is 0.1 millimol or more per mole of the (meth)acrylic acid compound.
6. A crosslinked polymer gel having structural units derived from the monomer composition according to claim 4 or 5.
Citation Information
Patent Citations
Production of neutralized acrylic acid solution suitable for superabsorber production, e.g. for hygiene articles, involves dissolution of crude acrylic acid in aqueous alkali and extraction of impurities with solvent
DE10221203A1
Method for crystallizing (METH)acrylic acid and method for regulating content of polymerization inhibitor in (METH)acrylic acid product
EP2439186A1
Production of highly water absorbing resin
JP1994345819A
Hydrophilic resin, absorbent article and acrylic acid for polymerization
JP2009173942A
Water-absorbent resin and production prcess therefor
US20040110913A1