Polyurethane system manufacturing

The use of a mixture of polyhydrazides and dispersion media in polyurethane production reduces aldehyde emissions and maintains foam integrity and storage stability, addressing the challenges of existing polyurethane production methods.

JP7554813B2Active Publication Date: 2024-09-20EVONIK OPERATIONS GMBH
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2022504240
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-07-24
Filing Date
2020-07-13
Publication Date
2024-09-20
Estimated Expiration
2040-07-13

AI Technical Summary

Technical Problem

Existing polyurethane production methods struggle to reduce aldehyde emissions without affecting processability, foam structure, and mold release properties, particularly in polyurethane foams, while maintaining storage stability of additives.

Method used

A reaction process involving a mixture of polyhydrazide, polysemicarbazide, polysulfonylhydrazide, and/or carbodihydrazide with a dispersion medium, such as phthalic acid alkyl esters, is used to catalyze isocyanate-polyol reactions, reducing aldehyde emissions by incorporating components like adipic acid dihydrazide and polyethylene glycol tridecyl ether phosphate.

Benefits of technology

The solution effectively minimizes aldehyde emissions, maintains foam structure and mold release properties, and ensures long-term storage stability of the additives, providing polyurethane foams with low formaldehyde and acetaldehyde emissions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007554813000002
    Figure 0007554813000002
  • Figure 0007554813000003
    Figure 0007554813000003
  • Figure 0007554813000001
    Figure 0007554813000001
Patent Text Reader

Abstract

The present invention relates to a method for producing polyurethanes using a component A comprising a polyhydrazide, polysemicarbazide, polysulfonylhydrazide and / or -carbodihydrazide, in particular a polyhydrazide, wherein component A is used in the form of a mixture C, which mixture C further comprises component B, which comprises a dispersion medium.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention is in the field of polyurethanes and in particular relates to a process for the preparation of polyurethane systems by reacting at least one polyol component with at least one isocyanate component in the presence of one or more catalysts which catalyze the isocyanate-polyol reaction and / or the isocyanate-water reaction and / or the isocyanate trimerization reaction, the reaction being carried out in the presence of component A which comprises a polyhydrazide, polysemicarbazide, polysulfonylhydrazide and / or -carbodihydrazide, in particular a polyhydrazide, as well as the polyurethane systems prepared accordingly.

[0002] A polyurethane system in the sense of the present invention is, for example, a polyurethane coating, a polyurethane adhesive, a polyurethane sealant, a polyurethane elastomer or especially a polyurethane foam / polyurethane foam material.

[0003] Polyurethanes are used in a variety of fields due to their excellent mechanical and physical properties. Particularly important markets for the various polyurethanes are the foam sector, such as traditional ether- and ester polyol-based flexible foams, cold foams (often also called HR foams), rigid foams, integral foams and microcellular foams, as well as foams with intermediate properties between these types, such as semi-rigid foams, in the automotive and furniture industries. For example, rigid foams are used as ceiling materials, ester foams for interior trims and punched sunshades with frame-laminated coverings, and cold and flexible foams for seating systems, instrument panels and mattresses. However, adhesives and coatings are also areas of use for polyurethanes, where their excellent properties make them convincing.

[0004] Aldehyde emissions are a problem during the manufacture and storage of polyurethane foams, and health concerns motivate many consumers to avoid aldehyde-emitting products whenever possible, whether or not these concerns are actually justified.

[0005] In addition, Chinese authorities in particular have been raising their standards in recent years, for example requiring very strict limits for interior emissions for cars sold in China. In addition to aromatic hydrocarbons, the focus here is again on aldehydes in particular. Overall, therefore, polyurethane foams that emit as few aldehydes as possible are desirable.

[0006] Various approaches have already been taken to meet this desire. For example, WO 2009 / 117479 assumes that formaldehyde originates from the raw materials and is contained in particular in the amine catalyst (tertiary amine) used. This document then proposes to achieve low formaldehyde emissions by adding a primary amine to the tertiary amine catalyst. Advantageously, dimethylaminopropylamine is used.

[0007] DE 10003156 A1 is not directly concerned with low-emission foam materials, but aims to develop polymers with good adsorption capacity for various compounds, in particular heavy metal ions. To solve this problem, polyurethane foam materials are proposed which contain ethyleneimine, polyethyleneimine, polyvinylamine, carboxymethylated polyethyleneimine, phosphonomethylated polyethyleneimine, quaternized polyethyleneimine and / or dithiocarbamated polyethyleneimine. These foam materials can also be used to adsorb organic substances, such as formaldehyde.

[0008] DE 10258046 A1 addresses the problem of producing polyurethane foams with reduced formaldehyde emissions. In contrast to DE 10003156 A1, the problem of DE 10258046 A1 thus consists in reducing the formaldehyde emissions from the PUR foam itself, and not in the adsorption of formaldehyde from the ambient air. To solve this problem, a method is proposed which provides for the addition of amino-group-containing polymers to the polyurethane foam, which addition can take place before and / or during the production of the polyurethane foam.

[0009] However, EP 3 459 983 A1 states that, depending on the polyurethane formulation used, the use of aldehyde scavengers may lead to foam interference and may also affect the efficiency of aldehyde absorption.

[0010] There is therefore still a need for further solutions in the provision of polyurethanes, in particular polyurethane foams, which allow a reduction in aldehyde emissions, without loss in terms of processability and without adversely affecting the foam structure, in particular the cell structure, as well as the demolding properties.

[0011] Against this background, a specific object of the present invention was to make it possible to provide polyurethanes, in particular polyurethane foams, with reduced aldehyde emissions, without losses in terms of processability and without adverse effects on the foam structure, in particular the cell structure and also on the demoldability. In particular, the interest of the customer is also taken into account here that additives can be used which have a particularly good storage stability of at least 3 months, during which time these additives do not undergo any changes in terms of visual appearance or effect.

[0012] Surprisingly, it has now been found that this problem is solved if the reaction is carried out in the presence of a component A which comprises a polyhydrazide, a polysemicarbazide, a polysulfonylhydrazide and / or a -carbodihydrazide, in particular a polyhydrazide, and in which component A is used in the form of a mixture C, which mixture C further comprises a component B which comprises a dispersion medium.

[0013] The subject of the present invention is therefore a process for the preparation of polyurethane systems by reacting at least one polyol component with at least one isocyanate component in the presence of one or more catalysts which catalyze the isocyanate-polyol reaction and / or the isocyanate-water reaction and / or the isocyanate trimerization reaction, the reaction being carried out in the presence of a component A which comprises a polyhydrazide, a polysemicarbazide, a polysulfonylhydrazide and / or a carbodihydrazide, in particular a polyhydrazide, said component A being used in the form of a mixture C, which mixture C further comprises a component B which comprises an alkyl phthalate ester. The method further comprises the step of preparing a dispersion medium comprising a dispersion medium from the group of esters, dicarboxylic acid alkyl esters, adipic acid alkyl esters, sebacic acid alkyl esters, dodecanoic acid alkyl esters, polyesters, phosphate esters, fatty acid esters, linear and modified natural or mineral oils, sulfonated oils, ethoxylated oils, epoxidized oils, fatty acids, sulfonamides, glycols, polyglycols, 1,2,4-benzenetricarboxylic acid alkyl esters and / or lecithins, in particular butyl diglycol, 1,2,4-benzenetricarboxylic acid tris(decyl) ester, or 1,2-cyclohexanedicarboxylic acid diisononyl ester.

[0014] The subject matter according to the invention makes it possible to provide polyurethanes, in particular polyurethane foams, with reduced aldehyde emissions, without losses in terms of processability and without adverse effects on the foam structure, in particular the cell structure and also on the demoldability. The mixture C used according to the invention comprises components A and B and has a particularly good storage stability of more than 3 months, without any changes in terms of visual appearance or effect on longer storage.

[0015] According to a particularly preferred embodiment of the invention, component A comprises a polyhydrazide, advantageously oxalic dihydrazide, malonic dihydrazide, succinic dihydrazide, adipic dihydrazide, sebacic dihydrazide, dodecanoic dihydrazide, isophthalic dihydrazide, piperazine-N,N'-dihydrazide, m-benzenedihydrazide and / or p-benzenedihydrazide, in particular adipic dihydrazide and / or carbodihydrazide. Adipic dihydrazide is the most preferred and gives particularly good results in the sense of the invention.

[0016] According to a further preferred embodiment of the invention, in addition to components A and B, mixture C further comprises polyethylene glycol tridecyl ether phosphate, phosphoric ester, organic phosphate and / or polyether (mono)ol, for example 2-ethylhexanol EO-PO polyether.

[0017] Further preferred embodiments of the present invention exist when the mixing ratio of component A to component B is 3:1 to 1:3, preferably 2:1 to 1:2, more preferably 1.5:1 to 1:1.5, in particular 1.1:1 to 1:1.1. These are parts by weight.

[0018] As already explained, the subject of the present invention is to ensure that the emissions of aldehydes are minimized.However, a further special advantage of the present invention is also that the mixture C used in the process according to the invention is very storage-stable, i.e. does not lose its appearance or quality, thus ensuring that the emissions of aldehydes are minimized even after longer storage periods, thus offering important advantages to the user.

[0019] In this context, it has proven to be particularly advantageous if component A is present as a ground product dispersed in component B, which corresponds to a preferred embodiment. Grinding is understood to mean, in particular, the grinding of solids with or in a mill or grinder. Possible equipment can be ball mills, for example planetary ball mills, which are used wherever great fineness is required. Planetary ball mills release very high grinding energy due to the very high centrifugal forces, which results in very short process times. The basic principle of grinding is based on impact or friction.

[0020] In process engineering, a dispersion is a heterogeneous mixture of at least two substances that are insoluble or poorly soluble in each other or do not chemically bond. Here, one or more substances (dispersed phase) are finely dispersed in another continuous substance (dispersion medium). The individual phases can be clearly separated from each other and can usually be separated from each other again by physical methods (e.g. filtration, centrifugation).

[0021] Overall, it has proven to be advantageous for the grain size of the mill or dispersion to be between 0.5 and 200 μm, advantageously between 0.5 and 60 μm, most preferably between 0.5 and 30 μm, which corresponds to a preferred embodiment.

[0022] Furthermore, it has proven advantageous if the process according to the invention is characterized in that mixture C is used in a weight proportion of 0.01 to 20 parts in total, advantageously 0.05 to 5 parts, in particular 0.1 to 3 parts, based on 100 parts of the polyol component.

[0023] In particular, it is preferred to produce polyurethane foams as polyurethane systems, particularly preferably rigid polyurethane foams, flexible polyurethane foams, viscoelastic PU foams, polyurethane HR foams, semi-rigid polyurethane foams, thermoformable polyurethane foams or PU integral foams.

[0024] The compounds used according to the invention, their preparation, their use for producing polyurethane systems or polyurethane foams, and polyurethane systems or polyurethane foams themselves are described below by way of example, without the invention being limited to these exemplary embodiments. Where ranges, general formulae or classes of compounds are given below, these are intended to include not only the corresponding ranges or compound groups explicitly stated, but also all subranges and subcompound groups that are obtained by excluding individual values ​​(ranges) or compounds. Where documents are cited in this specification, their contents are intended to form part of the disclosure of the present invention in their entirety, with particular reference to the matter to which they are referred. Where data are given below as percentages, data are given as weight % unless otherwise stated. Where average values ​​are given below, these are numerical averages, unless otherwise stated. Where physical properties, such as viscosity, are given below, these are physical property values ​​at 25°C, unless otherwise stated. Where chemical (general) formulae are used in the present invention, the indicated subscripts can represent not only absolute numbers but also average values. In the case of polymeric compounds, the subscripts advantageously represent average values.

[0025] The preparation of polyurethane systems can be carried out in a manner generally known and described in the prior art.This is well known to those skilled in the art, and a basic overview is described, for example, in G. Oertel, Polyurethane Handbook, 2nd Edition, Hanser / Gardner Publications Inc., Cincinnati, Ohio, 1994, p.177-247.When preparing polyurethane systems according to the invention, mixture C is advantageously used in a weight proportion of 0.01-20 parts, preferably 0.05-5 parts, particularly preferably 0.1-3 parts, based on 100 parts of polyol component.

[0026] When carrying out the process for the preparation of polyurethane systems according to the invention, it may be advantageous to additionally add water, physical blowing agents, flame retardants and / or further additives.

[0027] As isocyanate component in the process according to the invention, all isocyanates can be used, in particular aliphatic, cycloaliphatic, araliphatic, advantageously aromatic polyfunctional isocyanates known per se. Suitable isocyanates within the meaning of the invention are advantageously all polyfunctional organic isocyanates, such as, for example, 4,4'-diphenylmethane diisocyanate (MDI), toluene diisocyanate (TDI), hexamethylene diisocyanate (HMDI) and isophorone diisocyanate (IPDI). Particularly suitable are mixtures of MDI with higher condensation analogues having an average functionality of 2 to 4, known as "polymeric MDI" ("crude MDI"), and the various isomers of TDI in pure form or as isomer mixtures. Particularly preferred isocyanates are mixtures of TDI and MDI. Also particularly suitable are two-nuclear products, called "pure MDI", which consist mainly of mixtures of the 2,4'- and 4,4'-isomers or prepolymers thereof. Particularly suitable are MDI prepolymers.Examples of particularly suitable isocyanates are given, for example, in EP 1 712 578 A, EP 1 161 474 A, WO 00 / 58383 A, US 2007 / 0072951 A, EP 1 678 232 A and WO 2005 / 085310 A, which are hereby incorporated by reference in their entirety.

[0028] As polyols suitable for the polyol component in the sense of the present invention, advantageously, all organic substances having a plurality of groups reactive with isocyanates and their preparations can be used.Preferred polyols are all polyether polyols and polyester polyols commonly used in the manufacture of polyurethane systems, in particular polyurethane foam materials.Advantageously, polyols are not compounds having at least one 5- or 6-membered ring consisting of one or two oxygen and carbon atoms.

[0029] Polyether polyols can be obtained, for example, by reaction of polyhydric alcohols or amines with alkylene oxides. Polyester polyols are advantageously based on esters of polycarboxylic acids (which can be either aliphatic, for example adipic acid, or aromatic, for example phthalic or terephthalic acid) with polyhydric alcohols (usually glycols). It is also possible to use natural oil-based polyethers (natural oil-based polyols, NOP). These polyols are obtained, for example, from natural oils, such as soybean oil or palm oil, and can be used in modified or unmodified form.

[0030] Another class of polyols are those obtained as prepolymers by reacting a polyol with an isocyanate in a molar ratio of from 100:1 to 5:1, preferably from 50:1 to 10:1.

[0031] Yet another class of polyols that can be used advantageously are the so-called filler polyols (polymer polyols). These are characterized in that they contain solid organic fillers in a dispersed distribution up to a solids content of 40% by weight or more. For example, the following can be used, among others: SAN Polyol: This is a highly reactive polyol containing dispersed styrene / acrylonitrile (SAN) based copolymers. PHD Polyol: This is a highly reactive polyol that also contains polyurea in dispersed form. PIPA Polyol: This is a highly reactive polyol that contains polyurethane in dispersed form, formed, for example, by reacting alkanolamines and isocyanates in a conventional polyol in situ.

[0032] The solid content, which can be preferably 5->40% by weight of the polyol depending on the application, is responsible for improving the open cell, which allows the polyol to be expanded in a controlled manner, especially with TDI, and does not cause foam shrinkage. Thus, the solids act as essential process aids. They also function to control hardness, since the higher the solid content, the harder the foam will be.

[0033] Formulations using solid-containing polyols have significantly lower intrinsic stability and therefore require physical stabilization in addition to chemical stabilization via crosslinking reactions.

[0034] Depending on the solids content of the polyol, it can be used, for example, alone or mixed, for example, with unfilled polyols as mentioned above.

[0035] Polyols which can be preferably used are the so-called cell-opener polyols, which are polyether polyols having a high ethylene oxide content, preferably of at least 40% by weight, in particular 50 to 100% by weight, based on the alkylene oxide content.

[0036] The ratio of the isocyanate component to the polyol component preferred in the present invention is expressed as an index, and is in the range of 10 to 1000, preferably 40 to 350. This index represents the ratio of the isocyanate actually used to the calculated isocyanate (in the stoichiometric reaction with the polyol). An index of 100 represents a molar ratio of reactive groups of 1:1.

[0037] Suitable catalysts that can be used in the process according to the invention are preferably substances that catalyze the gelling reaction (isocyanate-polyol), the blowing reaction (isocyanate-water) or the dimerization or trimerization of isocyanates. Typical examples are amines such as triethylamine, dimethylcyclohexylamine, tetramethylethylenediamine, tetramethylhexanediamine, pentamethyldiethylenetriamine, pentamethyldipropylenetriamine, triethylenediamine, dimethylpiperazine, 1,2-dimethylimidazole, N-ethylmorpholine, tris(dimethylaminopropyl)hexahydro-1,3,5-triazine, dimethylaminoethanol, dimethylaminoethoxyethanol, and bis(dimethylaminoethyl)ether, tin salts of organic carboxylic acids, tin compounds such as dibutyltin dilaurate, potassium salts such as potassium acetate. Advantageously, as further catalysts, those that do not contain organotin compounds are used, in particular those that do not contain dibutyltin dilaurate.

[0038] The appropriate amount of these catalysts used in the method according to the present invention varies depending on the type of catalyst, and is usually in the range of 0.01 to 5 pphp (= parts by weight per 100 parts by weight of polyol), and in the case of potassium salts, in the range of 0.1 to 10 pphp.

[0039] The suitable water content in the process according to the invention depends on whether or not further physical blowing agents are used in addition to water. In the case of foams blown purely with water, these values ​​are usually advantageously between 1 and 20 pphp, and if further blowing agents are used, the amount used is usually reduced, for example to 0 or, for example, to 0.1 to 5 pphp. In order to obtain a high foam weight per unit volume, it is advantageous to use neither water nor other blowing agents.

[0040] Suitable physical blowing agents in the sense of the present invention are gases, such as liquefied CO2, and easily volatile liquids, such as hydrocarbons with 4 or 5 carbon atoms, preferably cyclo, iso and n-pentane, hydrofluorocarbons, preferably HFC 245fa, HFC 134a and HFC 365mfc, as well as olefinic hydrofluorocarbons, such as HHO 1233zd or HHO 1336mzzZ, hydrochlorofluorocarbons, preferably HCFC 141b, oxygenates, such as methyl formate and dimethoxymethane, or hydrochlorocarbons, preferably dichloromethane and 1,2-dichloroethane.Furthermore, ketones (such as acetone) or aldehydes (such as methylal) are suitable as blowing agents.

[0041] As stabilizer, the substances mentioned in the prior art can be used.Advantageously, the composition according to the present invention can contain one or more stabilizers.This is in particular a silicon compound that contains carbon atoms, and is advantageously selected from polysiloxane, polydimethylsiloxane, organic modified polysiloxane, polyether modified polysiloxane, and polyether-polysiloxane copolymer.

[0042] As silicon compounds containing one or more carbon atoms, the substances mentioned in the prior art can be used. Advantageously, Si compounds are used which are particularly suitable for the respective foam type. Suitable siloxanes are described, for example, in the following publications: EP 0839852, EP 1544235, DE 102004001408, WO 2005 / 118668, US 2007 / 0072951, DE 2533074, EP 1537159, EP 533202, US 3933695, EP 0780414, DE 4239054, DE 4229402, EP 867465. The Si compounds can be prepared according to the prior art. Suitable examples are described, for example, in US Pat. No. 4,147,847, EP-A-0 493,836, and US Pat. No. 4,855,379.

[0043] In particular, organically modified Si compounds can be used. Particularly preferred organically modified Si compounds that can be used are, for example, those represented by the following formula (IV): M k D m D' n T o Q p (IV) where: M=[R 2 R 1 2SiO 1 / 2 ] D=[R 1 R 1 SiO 2 / 2 ] D'=[R 3 R 1 SiO 2 / 2 ] T=[R 1 SiO 3 / 2 ] Q = [SiO 4 / 2 ] k=0 to 22, preferably 2 to 10, particularly preferably 2 m=0 to 400, preferably 0 to 200, particularly preferably 2 to 100 n=0 to 50, preferably 0.5 to 20, particularly preferably 0.7 to 9 o=0 to 10, preferably 0 to 5, particularly preferably 0 p=0 to 10, preferably 0 to 5, particularly preferably 0 R 2 =R 1 or R 3 R 1 = independently of one another an alkyl or aryl group or H, advantageously methyl, ethyl, propyl or phenyl, preferably methyl or phenyl R 3 = organic modification, for example polyether or monovalent radicals having 1 to 30 carbon atoms and at least one heteroatom selected from the group N, S, O, P, F, Cl, Br.

[0044] R in formula (IV) 3 is preferably -CH2CH2CH2O[CH2CH2O] a [CH2CH(CH3)O] b [CHR 4 CHR 4 O] c R 5 -CH2CH2CH2CN -CH2CH2CF3 -CH2CH2CH2Cl is a radical from the group R 5 = alkyl, aryl, urethane, carboxyl, silyl, or H, preferably H, -Me, or -C(O)Me R 4 = alkyl, aryl, optionally interrupted by oxygen, particularly preferably H, Me, Et or Ph a=0 to 100, preferably 0.5 to 70, particularly preferably 1 to 40 b=0 to 100, preferably 0.5 to 70, particularly preferably 0 to 40 c=0 to 50, preferably 0 to 15, particularly preferably 0 a+b+c>3.

[0045] In particular, unmodified Si compounds can be used. Particularly preferred unmodified Si compounds that can be used are, for example, those represented by the following formula (V): M q D r (V) where: M and D are as defined in formula (IV) above; q=2 r=0 to 50, preferably 1 to 40, and particularly preferably 2 to 30.

[0046] Particularly preferably, the above-mentioned Si compounds, in particular the compounds of formula (IV) and / or (V), can be used alone or in combination with each other. In the case of mixtures, furthermore, a compatibilizer can be used. This can be selected from the group of aliphatic or aromatic hydrocarbons, particularly preferably aliphatic polyethers or polyesters.

[0047] In the siloxane compound of formula (IV), (the group R 2 (total number of groups R 2 It may be advantageous for at least 10 equivalent % (and at most 50 equivalent %) of the alkyl groups having 8 to 22 carbon atoms.

[0048] Advantageously, from 0.00001 to 20 parts by weight of the silicon compound per 100 parts by weight of the polyol component can be used.

[0049] In particular, the use of the aforementioned silicon compounds in combination with the mixture C to be used according to the invention gives very good results in terms of the polyurethanes required according to the invention.

[0050] In addition to or instead of water and optionally a physical blowing agent, other chemical blowing agents that react with isocyanates with gas evolution, such as, for example, formic acid, carbamates or carbonates, can also be present in the additive composition according to the invention.

[0051] Suitable optional flame retardants in the sense of the present invention are preferably liquid organic phosphorus compounds, such as halogen-free organic phosphates, such as triethyl phosphate (TEP), halogenated phosphates, such as tris(1-chloro-2-propyl)phosphate (TCPP) and tris(2-chloroethyl)phosphate (TCEP), and organic phosphonates, such as dimethylmethane phosphonate (DMMP), dimethylpropane phosphonate (DMPP), or solids, such as ammonium polyphosphate (APP) or red phosphorus.Furthermore, halogenated compounds, such as halogenated polyols, as well as solids, such as expandable graphite or melamine, are suitable as flame retardants.

[0052] The process according to the invention makes it possible to produce polyurethane systems, especially polyurethane foams, which have good processability and particularly low aldehyde emissions.

[0053] The term polyurethane within the meaning of the present invention is understood to be a general term for polymers prepared in particular from di- or polyisocyanates and polyols or other species reactive towards isocyanates, such as amines, in which the urethane bond does not necessarily represent the exclusive or predominant bond type, and also explicitly includes polyisocyanurates and polyureas.

[0054] The preparation of polyurethane systems, in particular polyurethane foam materials, or the preparation of polyurethane systems / polyurethane foam materials according to the invention can be carried out according to all methods known to those skilled in the art, for example by hand mixing or preferably using high-pressure or low-pressure foaming machines. The process according to the invention can be carried out continuously or discontinuously. When producing molded foams, refrigerators, shoe soles or panels, it is preferred to carry out the process discontinuously. When producing insulation boards, metal composite elements, blocks and in spraying processes, it is preferred to carry out the process continuously.

[0055] In the process according to the invention, the mixture C used according to the invention can advantageously be mixed in immediately before the (urethane bond formation) reaction or even during the reaction. Preferably, the combination / addition takes place in a mixhead or, for the finished polyol system, also in a batch process.

[0056] A further subject of the invention is a polyurethane system, preferably a polyurethane foam, which is produced by the process according to the invention as described above.

[0057] The polyurethane system according to the invention may contain a total amount of mixture C of advantageously 0.001 to 20% by weight, advantageously 0.005 to 5% by weight and in particular 0.01 to 3% by weight, relative to the total composition of the polyurethane system.

[0058] The polyurethane system according to the invention can advantageously be a polyurethane foam, in particular, for example, a rigid polyurethane foam, a flexible polyurethane foam, a viscoelastic foam, an HR foam, a semi-rigid polyurethane foam, a thermoformable polyurethane foam or an integral foam, preferably a polyurethane HR foam.

[0059] The polyurethane systems according to the invention, preferably polyurethane foams, can be used, for example, for the production of corresponding products such as refrigerator insulation, insulation boards, sandwich elements, pipe insulation, spray foams, 1- and 1.5-part can foams (1.5-part can foams are foams produced by breaking the container in a can), imitation wood, modelling foams, packaging foams, mattresses, furniture cushions, car seat cushions, head rests, instrument panels, car interior trim, car ceilings, sound absorbers, steering wheels, shoe soles, carpet backing foams, filter foams, sealing foams, sealants, and also as adhesives, binders or paints.

[0060] A further subject of the present invention is a composition for producing polyurethane foams, comprising at least one urethane and / or isocyanurate catalyst, at least one blowing agent, at least one isocyanate component and at least one polyol component, which comprises as additive a mixture C as described above. With regard in particular to mixture C, reference is made in full to what has already been said, in order to avoid repetition.

[0061] The term composition in this context also includes multi-component compositions in which two or more components are mixed to effect a chemical reaction that results in the production of a polyurethane foam. In particular, the term composition in this context includes a mixture (blend) of at least one urethane and / or isocyanurate catalyst, at least one blowing agent, at least one isocyanate component, and mixture C as described above.

[0062] A preferred composition for producing polyurethane foams according to the present invention may comprise polyol in an amount of, for example, 25 to 75 wt%, water in an amount of, for example, 1 to 7 wt%, catalyst in an amount of, for example, 0.05 to 3 wt%, physical blowing agent in an amount of, for example, 0 to 25 wt% (for example, 0.1 to 25 wt%), stabilizer in an amount of, for example, 0.3 to 5 wt%, such as Si-containing and non-Si-containing, in particular Si-containing and non-Si-containing organic stabilizers and surfactants, isocyanate in an amount of, for example, 20 to 50 wt%, and mixture C to be used according to the present invention in an amount of, for example, 0.001 to 20 wt% (advantageously 0.005 to 5 wt%).

[0063] With regard to preferred embodiments of these aforementioned compositions, and in particular with regard to mixture C, reference is made to the preceding explanations.

[0064] A further subject of the present invention is a method for reducing the total emissions of aldehydes, in particular the emissions of aldehydes including formaldehyde and acetaldehyde, from a polyurethane system, in particular a polyurethane foam material, by adding mixture C (mixture C as defined above) to a polyurethane system, in particular a polyurethane foam material, advantageously in an amount of 0.001 to 20% by weight, advantageously 0.005 to 5% by weight, in particular 0.01 to 3% by weight, based on the total weight of the polyurethane system, in particular a polyurethane foam material, which addition can take place before and / or during the production of the polyurethane system, in particular a polyurethane foam material.

[0065] A further subject of the present invention is a polyurethane system, in particular a polyurethane foam material, which comprises mixture C as defined above, advantageously in an amount of 0.001 to 20% by weight, advantageously 0.005 to 5% by weight and in particular 0.01 to 3% by weight, relative to the total weight of the polyurethane system, in particular a polyurethane foam material, and in particular is obtainable by adding mixture C before and / or during the production of the polyurethane system, in particular the polyurethane foam material.

[0066] A further subject of the invention is the use of mixture C as described above for producing a polyurethane foam material having low emissions with respect to aldehydes, advantageously including formaldehyde and acetaldehyde.A further subject of the invention is the use of mixture C as described above for reducing the emissions of aldehydes, advantageously including formaldehyde and acetaldehyde, from a polyurethane foam material compared to a polyurethane foam material produced otherwise similarly but without mixture C.

[0067] A further subject of the invention is the use of mixture C, in particular as described above, for reducing emissions of aldehydes, including in particular formaldehyde and acetaldehyde, from polyurethane systems, in particular polyurethane foam materials.

[0068] The present invention will be described illustratively in the following examples, but it is not intended that the present invention, the scope of which is clear from the entire specification and the claims, be limited to the embodiments shown in the examples.

[0069] Working Example [Table 1] * A freshly prepared solution was used. To produce an aqueous solution containing 10% adipic dihydrazide, the solution had to be heated to 40-45°C for about 30 minutes. However, even at 60°C, 100% dissolution of the active substance was not obtained. When the solution was stored at room temperature, precipitation of a precipitate was observed. Therefore, a freshly prepared solution was used. ** Adipic acid dihydrazide and 1,2,4-benzenetricarboxylic acid tris(decyl) ester were mixed in a 1:1 ratio in the presence of 0.5% polyethylene glycol tridecyl ether phosphate and sheared in a Dispermat ball mill at 5000 rpm for approximately 1.5 hours.

[0070] [Table 2]

[0071] Example 1: Preparation of the dispersion Adipic acid dihydrazide and 1,2,4-benzenetricarboxylic acid tris(decyl) ester were mixed in a 1:1 ratio in the presence of 0.5% polyethylene glycol tridecyl ether phosphate and sheared in a Dispermat ball mill (planetary ball mill) (manufacturer: Retsch, name: PM 100) at 5000 rpm for approximately 1.5 hours.

[0072] Polyurethane foam manufacturing Foaming was carried out by hand mixing. For this, polyol, crosslinker, catalyst, additives, water and silicone stabilizer were weighed into a beaker (see Table 3) and premixed with a paddle mixer at 1000 rpm for 60 seconds. The isocyanate was then added and stirred in for 7 seconds at a stirrer speed of 2500 rpm. The reaction mixture was poured into a mold (dimensions 40 x 40 x 10 cm) thermostated at 57°C and sealed. The finished foam was demolded after 3.5 minutes. The amounts of feed and reactants used can be taken from Table 3.

[0073] The molded foam produced according to the above procedure was then analyzed for its formaldehyde and acetaldehyde content in accordance with VDA 275 (VDA 275 “Formteile fur den Fahrzeuginnenraum - Bestimmung der Formaldehydabgabe”. Messverfahren nach der modifizierten Flaschen-Methode; source: VDA 275, 07 / 1994, www.vda.de).

[0074] Foam spikes The polyurethane formulation feedstock used emits relatively low acetaldehyde emissions after foaming, so by mixing it with 30 ppm acetaldehyde, it is possible to measure increased initial values ​​and obtain convincing data on the reduction of aldehyde emissions, demonstrating the effectiveness of the active. Furthermore, the results for Form V1 in Table 3 serve as reference values ​​for formaldehyde and acetaldehyde.

[0075] Measurement principle In this method, samples of a given weight and dimension are fixed over distilled water in closed 1 L glass bottles and stored at a constant temperature for a given time. The bottles are then cooled and the formaldehyde and acetaldehyde absorbed in the distilled water are measured. The measured amounts of formaldehyde and acetaldehyde are relative to the dry weight (mg / kg) of the molded part.

[0076] analysis Specimens: Sample preparation, sample collection, and sample dimensions After the foam was demolded, it was stored for 24 hours at 21° C. and about 50% relative humidity. Afterwards, samples were taken evenly at suitable and representative positions across the width of the (cooled) molded part. The foam was then wrapped in aluminum foil and sealed in a polyethylene bag.

[0077] The size of each sample was 100×40×40 mm (approximately 9 g). For each molded part, three samples were taken for measuring aldehydes.

[0078] Testing: Formaldehyde / acetaldehyde emissions Immediately after obtaining the encapsulated samples, they were subjected to the determination directly. The samples were weighed to the nearest 0.001 g on an analytical balance before the start of the analysis. 50 ml of distilled water were pipetted into each glass bottle used. After the samples were placed in the glass bottles, the containers were closed and stored in a heating chamber at a constant temperature of 60 ° C for 3 hours. After the end of the test time, the containers were removed from the heating chamber. After 60 minutes at room temperature, the samples were removed from the test bottles. Derivatization was then carried out according to the DNPH method (dinitrophenylhydrazine). For this, 900 μl of the aqueous phase are mixed with 100 μl of DNPH solution. The DNPH solution is prepared as follows: 50 mg of DNPH in 40 mL of MeCN (acetonitrile) is acidified with 250 μL of HCl (1:10 dilution) and filled up to 50 mL with MeCN. After derivatization, the samples are analyzed by HPLC. Separation into the individual aldehyde homologues is carried out.

[0079] Instrument parameters HPLC The following instruments were used for the analysis: Agilent Technologies 1260 Chromatography column: Phenomenex Luna 250*4.6mm C18, 5μ particle size Eluent: Water acetonitrile gradient Detection: UV 365nm [Table 3]

[0080] The numerical data of the ingredients are in grams.

[0081] Explanation of results From Table 3 it can be seen that when Dispersion 1 is used in the foam formulations, both in aqueous solution 1 (V2) and in Dispersion 1 (E1), at the same active substance content, a relatively good effect in the foam is obtained in terms of reducing the formaldehyde and acetaldehyde emissions. In both formulations, the processability in the foam is very good. The structure of the foam, especially the cell structure, as well as the demolding properties, are not adversely affected. With an increased active substance concentration in the foam of Dispersion 1 (E2), even lower formaldehyde and acetaldehyde values ​​were measured, while the process properties remained good.

[0082] However, the use of aqueous solution 1 (V2) proved to be highly disadvantageous in terms of handling, reproducibility, and storage stability.

[0083] To produce an aqueous solution containing 10% adipic dihydrazide, it was necessary to heat the solution to 40-45°C for about 30 minutes. However, even at 60°C, 100% dissolution of the active substance was not achieved. When the solution was stored at room temperature, precipitation of a precipitate was observed after about 10 days at the latest. Even if the same procedure was used to minimize the precipitation of the precipitate, for example by reducing the content of active substance (increasing the water content), the observation remained that a precipitate of fine white crystals formed after about 10 days at the latest. Thus, it was found that adipic dihydrazide does not show any storage stability in aqueous solution, and reproducible results could not be obtained unless the aqueous solution was completely freshly prepared each time and used immediately.

[0084] Apart from this, the amount of 0.99 parts of water included in this further test is too high when using an aqueous solution in the product, making it impossible to adhere to the amount of water used in the formulation set out in Table 3 above (see total of 3.51 parts of water) because the aldehyde scavenger would introduce too much water into the system, resulting in less than the desired foam density, which would also lead to instability.

[0085] Moreover, such products cannot be delivered to customers with very low water usage, such as, for example here, steering wheel systems for microcellular polyurethane applications, which usually contain less than 1% water. To avoid this problem, the active substance concentrations were increased, which resulted in even more severe and faster formation of fine crystal precipitates, and therefore even less stable storage and reproducibility.

[0086] In contrast, dispersion 1 according to the invention proved to be extremely storage-stable and did not undergo any visual or effect-related changes even after storage, giving consistently particularly reproducible results.

Claims

1. 1. A method for producing a polyurethane system by reacting at least one polyol component with at least one isocyanate component in the presence of one or more catalysts which catalyze an isocyanate-polyol reaction and / or an isocyanate-water reaction and / or an isocyanate trimerization reaction, comprising:

1. A process according to claim 1 , characterized in that the reaction is carried out in the presence of a component A comprising a polyhydrazide, a polysulfonylhydrazide and / or a carbodihydrazide, said component A being used in the form of a mixture C, said mixture C further comprising a component B, said component B comprising a dispersion medium from the group of alkyl phthalates, alkyl dicarboxylates, alkyl adipates, alkyl sebacates, alkyl dodecanoates, polyesters, phosphates, fatty acid esters, linear and modified natural or mineral oils, sulfonated oils, ethoxylated oils, epoxidized oils, fatty acids, sulfonamides, glycols, polyglycols, alkyl 1,2,4-benzenetricarboxylates and / or lecithins.

2. The method of claim 1 , wherein component A comprises a polyhydrazide.

3. 3. The method of claim 1 or 2, wherein the mixture C further comprises polyethylene glycol tridecyl ether phosphate, a phosphoric acid ester, an organic phosphate and / or a polyether (mono)ol.

4. 4. The process according to claim 1, wherein the mixing ratio of component A to component B is from 3:1 to 1:

3.

5. 5. The process according to claim 1, wherein component A is present as a dispersed grind in component B.

6. The method according to claim 5, wherein the dispersed ground product has a particle size of 0.01 to 200 μm.

7. The process according to any one of claims 1 to 6, wherein the mixture C is used in a total weight proportion of 0.01 to 20 parts per 100 parts of the polyol component.

8. 8. The process according to claim 1, wherein a polyurethane foam is produced as the polyurethane system.

9. 9. A polyurethane system produced by the process of any one of claims 1 to 8.

10. 10. The polyurethane system according to claim 9, comprising from 0.001 to 20% by weight of mixture C as defined in any one of claims 1 to 9.

11. 11. The polyurethane system of claim 9 or 10, wherein the polyurethane system is a rigid polyurethane foam, a flexible polyurethane foam, a viscoelastic PU foam, a polyurethane HR foam, a semi-rigid polyurethane foam, a thermoformable polyurethane foam, or a PU integral foam.

12. 12. Use of the polyurethane system according to any one of claims 9 to 11 as refrigerator insulation, insulation boards, sandwich elements, pipe insulation, spray foam, 1- and 1.5-component can foam, imitation wood, modelling foam, packaging foam, mattresses, furniture cushions, car seat cushions, head rests, instrument panels, car interior trim, car ceilings, sound absorbers, steering wheels, shoe soles, carpet backing foams, filter foams, sealing foams, sealants and adhesives, coatings or for the production of corresponding products.

13. 13. A method for reducing the total emissions of aldehydes from a polyurethane system by adding to the polyurethane system a mixture C as defined in any one of claims 1 to 12, said addition being capable of taking place before and / or during the production of the polyurethane system.

14. The use of mixture C as defined in any one of claims 1 to 13 for the production of polyurethane systems having low emissions with respect to aldehydes.

15. 15. Use of mixture C as defined in any one of claims 1 to 14 for reducing aldehyde emissions from polyurethane systems.

Citation Information

Patent Citations

  • Deodorant resin composition

    JP1998036681A

  • Method for reducing the amount of material released from polyurethane foam

    JP2013506722A