Composition for heat treatment jig and method for manufacturing heat treatment jig

A composition of alumina, silicon carbide, and spinel in a balanced ratio addresses the durability and reaction resistance issues of conventional heat treatment containers, ensuring high thermal shock resistance and reaction resistance for lithium battery active material production.

JP7555285B2Active Publication Date: 2024-09-24TYK CORP
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
JP2021024944
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-02-19
Publication Date
2024-09-24
Estimated Expiration
2041-02-19

AI Technical Summary

Technical Problem

Conventional heat treatment containers used in the production of lithium battery active materials face issues with reaction resistance and durability against thermal shock, as increasing spinel content compromises thermal shock resistance, leading to microcracks and potential damage.

Method used

A composition for a heat treatment jig comprising alumina (5-33% by weight), silicon carbide (2-20% by weight), and optionally mullite, cordierite, and spinel (35-65% by weight), with silicon carbide and alumina contents balanced to maintain thermal shock resistance and reaction resistance, and a manufacturing method involving molding and firing.

Benefits of technology

The composition and method produce a heat treatment jig with high durability against thermal shock and improved reaction resistance, suppressing microcrack formation and maintaining strength under repeated thermal stress, suitable for lithium battery active material production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007555285000005
    Figure 0007555285000005
  • Figure 0007555285000004
    Figure 0007555285000004
  • Figure 0007555285000003
    Figure 0007555285000003
Patent Text Reader

Abstract

To provide a composition for a heat processing tool suitable for manufacturing a heat processing tool and the like having high durability against thermal shock, and a method of manufacturing the heat processing tool using the composition for the heat processing tool.SOLUTION: A composition for a heat processing tool includes 5 wt.% or more and 33 wt.% or less of alumina and 2 wt.% or more and 20 wt.% or less of silicon carbide, and includes one or plural kinds selected from mullite, cordierite, and spinel in the remainder. The composition for the heat processing tool may preferably have an average particle diameter of 12 μm or larger and 45 μm or smaller. Further, the composition for the heat processing tool may preferably contain the spinel of 35 wt.% or more and 65 wt.% or less. The composition for the heat processing tool is suitably used to a method of manufacturing a heat processing tool like a heat processing container 10.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a composition for a heat treatment jig and a method for producing a heat treatment jig. [Background technology]

[0002] Conventionally, a heat treatment tool such as the heat treatment container disclosed in Patent Document 1 below has been used to perform heat treatment in, for example, the production of active materials for lithium batteries.

[0003] The heat treatment container disclosed in the following Patent Document 1 is characterized by having a base containing 60-95 mass% alumina and a surface portion containing 20-80 mass% spinel and formed integrally with the base. The manufacturing method disclosed in the following Patent Document 1 is characterized by having a step of arranging an alumina-based powder, a step of arranging a spinel-based powder above the alumina-based powder, a step of compressing and molding, and a step of firing. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Patent No. 5005100 Summary of the Invention [Problem to be solved by the invention]

[0005] The heat treatment container of the above Patent Document 1 is said to have improved reactivity resistance during the manufacture of a positive electrode active material for lithium batteries by containing spinel. However, with the change in the positive electrode active material for lithium batteries, a heat treatment container with better reactivity resistance than before is required, and the conventional amount of spinel is no longer sufficient for obtaining sufficient durability. However, if the amount of spinel is increased, there is a concern that the durability against thermal shock will decrease. Specifically, in a heat treatment container containing spinel, microcracks will occur due to the application of thermal shock, and if the thermal shock is repeatedly applied, there is a concern that the cracks will eventually connect and break. Therefore, in the prior art, in order to improve the manufacturing efficiency of, for example, active materials for lithium batteries, etc., there has been a demand for a heat treatment jig with high durability against thermal shock and a composition for a heat treatment jig for forming such a heat treatment jig.

[0006] Based on this knowledge, the present invention aims to provide a composition for a heat treatment jig suitable for producing a heat treatment jig or the like having high durability against thermal shock, and a method for producing a heat treatment jig using the composition for a heat treatment jig. [Means for solving the problem]

[0007] (1) The composition for a heat treatment jig of the present invention, provided to solve the above-mentioned problems, is characterized by containing alumina in a range of 5% to 33% by weight, silicon carbide in a range of 2% to 20% by weight, and one or more selected from mullite, cordierite, and spinel as the balance.

[0008] (2) The above-mentioned composition for a heat treatment jig is preferably characterized in that the average particle size of the silicon carbide is within the range of 12 μm or more and 45 μm or less.

[0009] (3) The composition for a heat treatment jig described above may be characterized in that it contains the spinel in a weight ratio ranging from 35% to 65%.

[0010] (4) The composition for heat treatment jig of the present invention, provided to solve the above-mentioned problems, is prepared to contain alumina in a range of 5% or more and 33% or less by weight, and silicon carbide in a range of 2% or more and 20% or less by weight, and the contents of silicon carbide and alumina are specified so that the sum of the contents of silicon carbide and alumina is a predetermined ratio by weight.

[0011] (5) The composition for heat treatment jig of the present invention, which is provided to solve the above-mentioned problems, is prepared to contain alumina in the range of 5% or more and 33% or less by weight, silicon carbide in the range of 2% or more and 20% or less by weight, and spinel in the range of 35% or more and 65% or less by weight, and the contents of silicon carbide, alumina, and spinel are specified so that the sum of the contents of silicon carbide, alumina, and spinel is a predetermined ratio by weight.

[0012] (6) The method for manufacturing a heat treatment jig of the present invention, provided to solve the above-mentioned problems, is characterized by molding and firing the composition for a heat treatment jig of the present invention described above, or a composition for a heat treatment jig prepared by the method for preparing a composition for a heat treatment jig of the present invention described above. Effect of the Invention

[0013] According to the present invention, it is possible to provide a composition for a heat treatment jig suitable for producing a heat treatment jig or the like having high durability against thermal shock, and a method for producing a heat treatment jig using the composition for a heat treatment jig. [Brief description of the drawings]

[0014] [Figure 1] 1 is a perspective view showing a heat treatment container manufactured by a method for manufacturing a heat treatment jig according to an embodiment of the present invention; [Diagram 2] 1 is a graph showing the rate of decrease in elastic modulus for Examples 1 and 6 and Comparative Examples 1 and 3, in which silicon carbide is contained at 5% by weight. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0015] Hereinafter, a composition for a heat treatment jig according to one embodiment of the present invention and a method for producing a heat treatment jig using the composition will be described.

[0016] The heat treatment jig composition exemplified in the present embodiment below can be suitably used in the manufacture of heat treatment jigs in general, such as heat treatment containers such as saggers and crucibles, shelves, setters, etc. In the heat treatment jig of this embodiment, the thinnest part of the wall preferably has a thickness of 9 to 12 mm. In the heat treatment jig of this embodiment, the thickness of the part other than the thinnest part of the wall is not particularly limited, but is preferably 16 mm or less.

[0017] The composition for heat treatment jig of this embodiment contains alumina and silicon carbide, and is prepared so as to contain one or more selected from mullite, cordierite, and spinel as the balance. More specifically, the composition for heat treatment jig of this embodiment contains alumina in a range of 5% to 33% by weight and silicon carbide in a range of 2% to 20% by weight. Also, the composition for heat treatment jig of this embodiment contains spinel in a range of 35% to 65% by weight. The composition for heat treatment jig of this embodiment contains mullite, cordierite, clay, etc. as the balance in addition to alumina, silicon carbide, and spinel.

[0018] The heat treatment jig of the present embodiment is produced by sintering a molded body obtained by molding the composition for the heat treatment jig described above. By producing the heat treatment container of the present invention from a mixture of these ceramic powders, the heat treatment container is formed of porous ceramics and has heat resistance.

[0019] In the composition for a heat treatment jig of this embodiment, alumina mainly exerts an effect of increasing the reactivity resistance to the compound to be heat-treated. Therefore, a heat treatment jig formed by firing the composition for a heat treatment jig of this embodiment exerts high reactivity resistance (also called corrosion resistance) to the compound to be heat-treated.

[0020] In the composition for heat treatment jig of this embodiment, alumina is mixed in a weight ratio of 5% to 33%. This allows the manufacture of a heat treatment jig that has high reactivity resistance to the compound to be heat treated. If the content of alumina powder is less than 5%, the effect of containing alumina powder in the heat treatment jig cannot be fully exhibited. If the content of alumina powder exceeds 33%, other components contained in the ceramic powder are relatively reduced, making it difficult for the heat treatment jig to exhibit the desired characteristics.

[0021] Silicon carbide exerts an effect of suppressing the occurrence of microcracks when a thermal shock is applied to a heat treatment jig formed using the composition for heat treatment jig of this embodiment. By including silicon carbide in the composition for heat treatment jig, it is possible to suppress the decrease in elastic modulus when a thermal shock is applied to a heat treatment jig formed from the composition for heat treatment jig. Therefore, in the composition for heat treatment jig of this embodiment, silicon carbide exerts an effect of mainly improving thermal shock resistance.

[0022] In the composition for heat treatment jig of this embodiment, silicon carbide is blended in a range of 2% or more and 20% or less by weight. This allows the manufacture of a heat treatment jig that has high thermal shock resistance and can exhibit sufficient performance in terms of moldability into a heat treatment jig. Even when the content of silicon carbide is less than 2%, the effect of improving thermal shock resistance can be expected. However, in order to form a heat treatment jig that exhibits sufficient durability against thermal shock, the content of silicon carbide is preferably 2% or more. In addition, the effect of improving thermal shock resistance can be expected by blending silicon carbide in an amount of more than 20% by weight. However, from the viewpoint of moldability, the blending amount of silicon carbide is preferably 20% or less by weight.

[0023] In addition, in the composition for heat treatment jig of this embodiment, silicon carbide is blended with an average particle size in the range of 12 μm or more and 45 μm or less. If the average particle size of silicon carbide is less than 12 μm, there is a concern that when the heat treatment jig is exposed to an oxidizing atmosphere during the firing of the compound to be heat treated, the silicon carbide will be oxidized, and the effect of improving thermal shock resistance will not be fully exhibited. In addition, if the average particle size of silicon carbide is larger than 45 μm, there is a concern that the strength of the heat treatment jig will be significantly reduced.

[0024] In the composition for heat treatment jig of this embodiment, cordierite mainly exerts an effect of improving thermal shock resistance. In the composition for heat treatment jig of this embodiment, the above-mentioned silicon carbide also contributes to improving thermal shock resistance. Therefore, cordierite exerts an effect of further enhancing the effect of improving thermal shock resistance obtained by silicon carbide. Therefore, by blending cordierite in addition to silicon carbide, the thermal shock resistance of the heat treatment jig formed by firing the composition for heat treatment jig can be further improved.

[0025] In the composition for heat treatment jig of this embodiment, cordierite is blended within the range of the remainder of alumina and silicon carbide described above. If the content ratio of cordierite is reduced, the effect of improving the thermal shock resistance of the heat treatment jig is reduced. In addition, if the content ratio of cordierite is greater than the range of the remainder of alumina and silicon carbide described above, contamination by the heat-treated compound in the heat treatment jig is likely to occur. In particular, when a lithium-containing compound containing lithium is used as a non-heat-treated compound, such as a ceramic material for active material containing lithium, contamination by the lithium-containing compound is likely to occur.

[0026] In the composition for heat treatment jig of this embodiment, mullite, like cordierite, mainly exerts an effect of increasing thermal shock resistance. Also, like cordierite, mullite is blended within the range of the balance of alumina and silicon carbide described above. By blending mullite in such a blending amount, the thermal shock resistance of the heat treatment jig can be further improved.

[0027] In the composition for heat treatment jig of this embodiment, if the content of mullite is reduced, the effect of improving the thermal shock resistance of the heat treatment jig is reduced. Also, if the content of mullite is increased beyond the range of the remainder of alumina and silicon carbide described above, other components contained in the composition for heat treatment jig are relatively reduced, making it difficult for the heat treatment container itself to exhibit the desired properties.

[0028] In the composition for a heat treatment jig of this embodiment, the spinel mainly exerts an effect of increasing reactivity resistance. Therefore, a heat treatment jig formed by firing the composition for a heat treatment jig of this embodiment containing a spinel exhibits high reactivity resistance. The improvement in reactivity resistance by the spinel powder is particularly effective when the compound to be heat-treated in the heat treatment container is a compound containing lithium, and is particularly effective when it is a positive electrode active material for a lithium-ion secondary battery.

[0029] In the composition for heat treatment jig of this embodiment, spinel is blended in a range of 35% to 65% by weight. As a result, the heat treatment jig formed by firing the composition for heat treatment jig of this embodiment blended with spinel exhibits the characteristic of high reactivity resistance to the compound to be heat treated. Here, when spinel is blended in the composition for heat treatment jig, there is generally a concern that durability against thermal shock may decrease. However, blending spinel in the presence of silicon carbide suppresses the decrease in durability against thermal shock. Therefore, according to the composition for heat treatment jig of this embodiment, a heat treatment jig with high reactivity resistance can be formed while ensuring sufficient thermal shock resistance.

[0030] The above-mentioned composition for heat treatment jig can specify the contents of silicon carbide and alumina so that the sum of the contents of silicon carbide and alumina is a predetermined ratio by weight. That is, the above-mentioned composition for heat treatment jig can adjust the content of silicon carbide so that a part of the content occupied by alumina in a state in which silicon carbide is not contained is replaced by silicon carbide. Therefore, the above-mentioned composition for heat treatment jig can specify the contents of alumina and silicon carbide so that the content of alumina decreases with an increase in the content of silicon carbide. In addition, the above-mentioned composition for heat treatment jig can specify the contents of silicon carbide, alumina, and spinel so that the sum of the contents of silicon carbide, alumina, and spinel is a predetermined ratio by weight. That is, the above-mentioned composition for heat treatment jig can adjust the content of silicon carbide so that a part of the content occupied by alumina and spinel in a state in which silicon carbide is not contained is replaced by silicon carbide. Therefore, the contents of alumina, spinel, and silicon carbide in the composition for heat treatment jig described above can be specified so that a correlation is established in which the content of either or both of alumina and spinel decreases with an increase in the content of silicon carbide.

[0031] The composition for heat treatment jig of this embodiment contains clay in addition to the above-mentioned alumina, silicon carbide, spinel, mullite, and cordierite. The composition for heat treatment jig of this embodiment may contain, for example, a conventionally known additive. The additive to be added to the composition for heat treatment jig of this embodiment may be, for example, a compound that disappears with firing of the molded body, a binder, or the like, which is used in conventional heat treatment containers and does not cause a change in the characteristics of the heat treatment container. For example, by making the composition for heat treatment jig of this embodiment contain a binder, it is possible to improve the moldability of the heat treatment jig, suppress the manufacturing cost of the heat treatment jig, improve the yield, and other effects.

[0032] The manufacturing method of the heat treatment jig of this embodiment can be realized by molding the composition for heat treatment jig described above into a predetermined shape and then firing it under predetermined conditions. The firing conditions can be appropriately set, but for example, the maximum temperature is set to 1250°C to 1400°C, preferably 1280°C to 1350°C, and firing is performed for a predetermined time. In order to prevent decomposition of cordierite due to sintering, the firing temperature is preferably 1400°C or less.

[0033] According to the composition for a heat treatment jig of the present embodiment and the method for producing a heat treatment jig using the composition, for example, the following effects (1) to (7) can be obtained.

[0034] (1) The composition for a heat treatment jig of the present embodiment is characterized by containing alumina in a range of 5% to 33% by weight, silicon carbide in a range of 2% to 20% by weight, and one or more selected from mullite, cordierite, and spinel as the balance.

[0035] In this way, when a heat treatment jig is formed using a composition for heat treatment jig containing silicon carbide, the occurrence of microcracks due to thermal shock can be suppressed. This makes it possible to form a heat treatment jig in which microcracks are unlikely to grow and the heat treatment jig is unlikely to break even when thermal shock is repeatedly applied. Therefore, the composition for heat treatment jig of this embodiment is suitable for manufacturing a heat treatment jig or the like that has high durability against thermal shock.

[0036] (2) The composition for heat treatment jigs of this embodiment is characterized in that the average particle size of silicon carbide is in the range of 12 μm or more and 45 μm or less. In this way, by containing silicon carbide having a size of 12 μm or more, the possibility that the effect of suppressing the occurrence of microcracks can be maintained by continuing to exist as silicon carbide when the heat treatment jig is used in an oxidizing atmosphere is increased compared to the case where silicon carbide smaller than 12 μm is contained. In addition, by using silicon carbide having an average particle size of 45 μm or less, the decrease in strength of the heat treatment jig due to the inclusion of silicon carbide can be suppressed. Therefore, by setting the average particle size of silicon carbide in the range of 12 μm or more and 45 μm or less, it is possible to provide a composition for heat treatment jigs that can suppress the decrease in strength due to the inclusion of silicon carbide while sufficiently ensuring the effect of suppressing the occurrence of microcracks in the heat treatment jig. Note that the average particle size in this specification and the like is the D50 value of the material powder measured by a particle size distribution measuring device (MT3300II manufactured by Microtrack Bell Co., Ltd.).

[0037] (3) The composition for heat treatment jig of this embodiment is characterized by containing spinel in a range of 35% to 65% by weight. Generally, when a composition for heat treatment jig contains spinel, it is possible to improve reactivity resistance, but there is a concern that the thermal shock resistance may decrease. However, by containing silicon carbide as in the composition for heat treatment jig of this embodiment, it is possible to suppress the decrease in thermal shock resistance caused by the inclusion of spinel. Therefore, according to the composition for heat treatment jig of this embodiment, the synergistic effect of silicon carbide and spinel can be used to improve thermal shock resistance while also improving reactivity resistance.

[0038] (4) The composition for heat treatment jig of this embodiment is prepared to contain alumina in a range of 5% to 33% by weight and silicon carbide in a range of 2% to 20% by weight, and the contents of silicon carbide and alumina are specified so that the sum of the contents of silicon carbide and alumina is a predetermined ratio by weight. In this way, the composition for heat treatment jig of this embodiment has a balanced content of alumina and silicon carbide. Therefore, according to the composition for heat treatment jig of this embodiment, it is possible to form a heat treatment jig that can exhibit both the effect of improving reactivity resistance by alumina and the effect of improving thermal shock resistance by silicon carbide in a well-balanced manner.

[0039] (5) The composition for heat treatment jig of this embodiment is prepared to contain alumina in the range of 5% to 33% by weight, silicon carbide in the range of 2% to 20% by weight, and spinel in the range of 35% to 65% by weight, and the contents of silicon carbide, alumina, and spinel are specified so that the sum of the contents of silicon carbide, alumina, and spinel is a predetermined ratio by weight. In this way, the composition for heat treatment jig of this embodiment has a balanced content of alumina, spinel, and silicon carbide. Also, as described above, by containing spinel together with silicon carbide, it is possible to suppress the decrease in thermal shock resistance caused by containing spinel. Therefore, according to the composition for heat treatment jig of this embodiment, it is possible to form a heat treatment jig that can exhibit both the effect of improving reactivity resistance by alumina and spinel and the effect of improving thermal shock resistance by silicon carbide in a well-balanced manner.

[0040] (6) The method for producing a heat treatment jig of the present embodiment involves molding and firing the composition for a heat treatment jig of the present embodiment described above, or the composition for a heat treatment jig prepared by the method for preparing a composition for a heat treatment jig of the present embodiment described above. Therefore, according to the production method of the present embodiment, a heat treatment jig having high durability against thermal shock can be produced. EXAMPLES

[0041] The composition for heat treatment jig and the manufacturing method of the heat treatment jig of the present invention will be specifically described below using examples. In this example, as an example of the heat treatment jig, a sagger having a tank-like external shape with an opening on the top side was produced as the heat treatment container 10 as shown in Figure 1. The heat treatment container 10 can be used for purposes such as firing a compound to be heat-treated, for example, a ceramic material for active material containing lithium.

[0042] The heat treatment vessel 10 shown in FIG. 1 has a bottom 12 and an upright wall 14. The bottom 12 is plate-like and can be rectangular, circular, or the like in plan view (rectangle in the illustrated example). The upright wall 14 is a portion formed so as to stand upright around the entire periphery of the bottom 12 at the peripheral portion of the bottom 12. The heat treatment vessel 10 in FIG. 1 was manufactured such that the thinnest portions of the bottom 12 and the upright wall 14 had a thickness of 9 to 12 mm, and the thicknesses of the portions other than the thinnest portions were 16 mm or less.

[0043] Alumina, silicon carbide, spinel, mullite, cordierite, and clay were prepared, and then weighed and mixed to obtain the weight ratios shown in Tables 1 to 3 below to prepare a plurality of compositions for heat treatment jigs as samples. Each sample was subjected to an evaluation test using the test method described below, and the results are shown in Tables 1 to 3. In Tables 1 to 3 below, compositions for heat treatment jigs that are indicated by the same sample name each contain the same components in the same weight ratio.

[0044] [Table 1]

[0045] [Table 2]

[0046] [Table 3]

[0047] <About the test method>

[0048] (a) Bending stress

[0049] Each of the above-mentioned samples was prepared by molding into a size of 10×10×60 mm. The three-point bending strength of each sample was measured at room temperature with a support distance of 40 mm in accordance with JIS R1604.

[0050] (b) Elastic modulus Each of the above-mentioned samples was prepared by molding into a plate of 100×50×10 mm, and the elastic modulus at room temperature was measured with an elastic modulus meter.

[0051] (c) Thermal shock deterioration test

[0052] A thermal shock degradation test was conducted on each of the above-mentioned samples to evaluate the degree of degradation caused by repeated application of thermal shock. Specifically, each of the above-mentioned samples was prepared by molding into a 100 x 50 x 10 plate, and a test was conducted in which the sample was subjected to a series of steps of (1) heating at 1000°C for 30 minutes, (2) immersion in water, and (3) elastic modulus measurement, repeated six times. The degree of degradation caused by repeated application of thermal shock was evaluated by expressing the rate of change (degradation rate) from the initial elastic modulus of each sample to the elastic modulus after six sets as a percentage.

[0053] (d) Formability The above-mentioned samples were evaluated for moldability when molded into the heat treatment container 10, with those that were easy to mold being marked with ◯ and those that were difficult to mold being marked with ×.

[0054] <About the test results> The results of each of the above-mentioned tests will be explained below with reference to Tables 1 to 3 above.

[0055] [Regarding the test results shown in Table 1] Table 1 summarizes the test results of the above-mentioned tests for Examples 1 to 6 and Comparative Examples 1 to 4, which contain alumina in the range of 15% to 35% by weight, silicon carbide in the range of 0% to 20% by weight, mullite in the range of 5% by weight, cordierite in the range of 15% by weight, and the remainder containing 35% by weight of spinel and 10% by weight of clay.

[0056] In the test examples summarized in Table 1, the presence or absence and weight ratio of silicon carbide contained in the composition for heat treatment jig are different between Examples 1 to 6 and Comparative Examples 1 to 4. Therefore, according to Table 1, knowledge can be obtained about the influence of the presence or absence and weight ratio of silicon carbide in the composition for heat treatment jig on the properties required for the heat treatment jig. In the test examples summarized in Table 1, the contents of silicon carbide and alumina are specified so that the sum of the contents of silicon carbide and alumina is a predetermined ratio (35%) in weight ratio, and the content of alumina is decreased or increased according to an increase or decrease in the content of silicon carbide. In addition, in the test examples summarized in Table 1, the particle size of silicon carbide is changed. Therefore, according to Table 1, knowledge can be obtained about the influence of the particle size of silicon carbide on the properties required for the heat treatment jig. Below, the test results summarized in Table 1 are examined for each test.

[0057] First, when the test results on bending stress for each of the Examples and Comparative Examples listed in Table 1 were confirmed, it was found that, among Examples 1 to 6 and Comparative Examples 1 to 4, Comparative Example 3, which used silicon carbide with an average particle size of 150 μm, which is larger than 45 μm, had a bending stress significantly lower than the other Examples and Comparative Examples. This led to the finding that the bending stress (strength) is significantly reduced when silicon carbide having an average particle size of more than 45 μm is used.

[0058] Furthermore, when the test results regarding the initial elastic modulus were examined, it was found that all of Examples 1 to 6 and Comparative Examples 1 to 4 exhibited a strength of 4.0 [GPa] or more.

[0059] Next, a thermal shock degradation test was carried out for each of the examples and comparative examples listed in Table 1, and the degree of thermal shock degradation was derived. As a result, it was found that in Examples 1 to 6 and Comparative Example 3, even when six sets of thermal shocks were applied, the elastic modulus was 50% or more of the initial elastic modulus. However, in Comparative Example 1, which does not contain silicon carbide, the elastic modulus after six sets of thermal shocks was only 31.7% of the initial elastic modulus, resulting in a significant deterioration. In addition, in Comparative Example 2, which contained 1% silicon carbide by weight, the value was sufficiently higher (47.3%) than Comparative Example 1, which did not contain any silicon carbide, but the result was slightly below 50%.

[0060] In addition, even when silicon carbide is contained at 5% by weight, in the case of Comparative Example 4 in which the particle size of silicon carbide is smaller than 12 μm (2 μm), it was found that the degree of thermal shock degradation is improved compared to the case in which silicon carbide is not contained. On the other hand, since the degree of thermal shock degradation in Comparative Example 4 was 40.8%, it was found that the particle size of silicon carbide is 12 μm or more, which is a more suitable condition for improving the degree of thermal shock degradation. It is presumed that the reason why the degree of thermal shock degradation is lower when the particle size of silicon carbide is smaller than 12 μm compared to when the particle size is larger than this is because silicon carbide is oxidized in an oxidizing atmosphere, thereby reducing the effect of including silicon carbide.

[0061] Furthermore, among Examples 1 to 6 and Comparative Examples 1 to 4, those containing 5% by weight of silicon carbide (Experimental Examples 1, 6, and Comparative Example 3) were examined for the rate of decrease in elastic modulus when thermal shock was applied multiple times. As a result, as shown in FIG. 2, in Comparative Example 1 not containing silicon carbide, it was found that the elastic modulus significantly decreased with each application of the second or subsequent thermal shock. In contrast, it was found that in samples containing silicon carbide, such as Experimental Examples 1 and 6 and Comparative Example 3, the elastic modulus did not significantly decrease even when the second or subsequent thermal shock was applied. Based on these test results, it was found that the decrease in elastic modulus caused by repeated application of thermal shock can be suppressed by including silicon carbide in the composition for heat treatment jig.

[0062] Based on the test results shown in Table 1, it was found that the initial elastic modulus and the degree of thermal shock deterioration can be improved by making the composition for heat treatment jigs contain silicon carbide at a weight ratio of 2% or more compared to those that do not contain silicon carbide. In addition, when silicon carbide is contained, it was found that the effect of improving the degree of thermal shock deterioration can be enhanced by making the particle size of silicon carbide 12 μm or more. Furthermore, it was found that the effect of improving bending stress can be enhanced compared to those that do not contain silicon carbide by making the particle size of silicon carbide 45 μm or less.

[0063] [Regarding the test results shown in Table 2] Table 2 summarizes the test results of the above-mentioned tests for Examples 1 to 6, which contain alumina in the range of 10% to 35% by weight, silicon carbide in the range of 0% to 25% by weight, mullite in the range of 5% by weight, cordierite in the range of 15% by weight, and the remainder containing 35% by weight of spinel and 10% by weight of clay, as well as Comparative Examples 1, 2, and 5.

[0064] Table 2 summarizes the test results of investigating the effect of silicon carbide in the composition for heat treatment jig on moldability. As shown in Table 2, the compositions for heat treatment jig containing silicon carbide in the range of 1% to 20% by weight (Examples 1 to 5 and Comparative Example 2) had good moldability, similar to Comparative Example 1, which did not contain silicon carbide. However, when the content of silicon carbide was increased to 25% by weight, the moldability decreased. Therefore, it was found that in order to use the composition for heat treatment jig for molding, it is preferable to set the content of silicon carbide in the composition for heat treatment jig to a range of 25% or less by weight.

[0065] [Regarding the test results shown in Table 3] Table 3 summarizes the test results for the above-mentioned experimental examples 1, 7 to 11, and comparative example 6, in which the alumina content was varied within the range of 5% or more and 30% or less by weight, and the spinel content was varied within the range of 35% or more and 65% or less by weight, under the condition that the silicon carbide content was 5% by weight and the particle size of the silicon carbide was 12 μm.

[0066] First, by checking the test results on bending stress for each of the Examples and Comparative Examples listed in Table 3, it was found that the bending stress required for use as a heat treatment jig can be exerted in all of Experimental Examples 1, 7 to 11, and Comparative Example 6. In addition, as for the test results on the initial elastic modulus, it was found that a strength of 4.0 [GPa] or more can be exerted in all of Experimental Examples 1, 7 to 11, and Comparative Example 6, and sufficient performance can be obtained for use as a heat treatment jig.

[0067] Next, a thermal shock degradation test was carried out for each of the Examples and Comparative Examples listed in Table 3, and the thermal shock degradation degree was derived. As a result, it was found that, for Experimental Examples 1, 7 to 11 in which silicon carbide was contained, even if the content of spinel, which is concerned about a decrease in thermal shock resistance, was increased to 65% by weight, a sufficient value of the thermal shock degradation degree for use as a heat treatment jig was obtained. In contrast, it was found that, for Comparative Example 6 in which silicon carbide was not contained, the degradation due to thermal shock was greater than that of the other Experimental Examples 1, 7 to 11, and the performance was inferior in terms of thermal shock resistance for use as a heat treatment jig. Therefore, it was found that, when spinel is contained in the composition for heat treatment jig together with silicon carbide, a heat treatment jig capable of exhibiting performance suitable for heat treatment can be formed by containing spinel at least in the range of 35% to 65% by weight.

[0068] Based on the test results of each of the examples and comparative examples shown in Tables 1 to 3, it has been found that the composition for heat treatment jig contains alumina in a range of 5% to 33% by weight, silicon carbide in a range of 2% to 20% by weight, and one or more selected from mullite, cordierite, and spinel as the balance. In addition, it has been found that when spinel is contained in the composition for heat treatment jig, it is preferable that the spinel is contained in a range of 35% to 65% by weight. Furthermore, it has been found that the silicon carbide contained in the composition for heat treatment jig preferably has an average particle size in the range of 12 μm to 45 μm.

[0069] Furthermore, based on the test results for each of the examples and comparative examples shown in Tables 1 to 3, it was discovered that by molding and firing a composition for a heat treatment jig containing each component in the preferred composition ratio as described above, a heat treatment jig with high durability against temperature changes can be provided.

[0070] Furthermore, based on the test results for each of the above-mentioned Examples and Comparative Examples, it was found that a heat treatment jig manufactured from a composition for a heat treatment jig containing each component in the above-mentioned preferred composition ratio is optimal for firing and manufacturing a ceramic material for an active material of a lithium-ion secondary battery containing lithium. Specifically, the heat treatment jig manufactured by the above-mentioned manufacturing method is unlikely to be damaged, for example, even if it is subjected to a process such as forced air cooling while still at a high temperature (for example, a high temperature of about 500 degrees) while containing an active material for a lithium-ion secondary battery. In addition, the heat treatment jig manufactured by the above-mentioned manufacturing method has high corrosion resistance against lithium contained in the lithium-containing compound. Therefore, the heat treatment jig manufactured by the above-mentioned manufacturing method is suitable for manufacturing an active material for a lithium-ion secondary battery. [Industrial Applicability]

[0071] The composition for a heat treatment jig and the method for manufacturing a heat treatment jig of the present invention can be suitably used as a material for and a manufacturing method of jigs in general for use in heat treatment. In addition, the heat treatment jig formed by the composition for a heat treatment jig and the method for manufacturing a heat treatment jig of the present invention can be suitably used in, for example, the manufacture of active materials for lithium ion secondary batteries. [Explanation of symbols]

[0072] 10: Heat treatment container (heat treatment jig) 12: Bottom 14: Standing wall

Claims

1. Alumina in an amount of 5% or more and 33% or less by weight, Contains silicon carbide in a weight ratio of 2% to 20%; The balance includes one or more selected from mullite, cordierite, and spinel, A composition for use in a heat treatment jig, characterized in that the average particle size of the silicon carbide is within the range of 12 μm or more and 45 μm or less.

2. 2. The composition for use in a heat treatment jig according to claim 1, comprising the spinel in a weight ratio ranging from 35% to 65%.

3. Alumina is 5% or more and 33% or less by weight, The silicon carbide content is adjusted to be in the range of 2% to 20% by weight, A method for preparing a composition for a heat treatment jig, comprising specifying the contents of silicon carbide and alumina so that the sum of the contents of silicon carbide and alumina is a predetermined ratio by weight.

4. Alumina is 5% or more and 33% or less by weight, Silicon carbide: 2% or more and 20% or less by weight; The spinel content is adjusted to be in the range of 35% to 65% by weight, a method for preparing a composition for a heat treatment jig, the content of each of the silicon carbide, the alumina, and the spinel being specified so that the sum of the contents of the silicon carbide, the alumina, and the spinel is a predetermined ratio by weight.

5. A method for producing a heat treatment jig, comprising molding and firing a composition for a heat treatment jig prepared by the composition for a heat treatment jig described in claim 1 or 2, or the method for preparing a composition for a heat treatment jig described in claim 3 or 4.

Citation Information

Patent Citations

  • JP1975005100A

  • Refractories for lining

    JP1987197360A

  • Unshaped refractory and stainless hot metal ladle lined inside therewith

    JP1992325466A

  • Jig for baking electronic component

    JP1996159671A

  • Kiln tool

    JP1996283073A