Binder, solidified body, and method for producing solidified body
A binder with a carboxyl group-containing polymer and polyhydric alcohol improves impregnability and strength in heat-resistant molded products, addressing the limitations of conventional binders by enhancing both properties simultaneously.
Patent Information
- Application Number
- JP2022563620
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-11-17
- Filing Date
- 2021-10-07
- Publication Date
- 2024-09-24
- Estimated Expiration
- 2041-10-07
AI Technical Summary
Conventional binders used in heat-resistant molded products face challenges in achieving high impregnability and strength, leading to variations in product performance and reduced mechanical strength when impregnability is increased.
A binder comprising a carboxyl group-containing polymer with a molecular weight of 2000 to 6000 g/mol and a polyhydric alcohol, with a molar ratio of 79:21 to 35:65, and optionally including polyamine and silane coupling agents, enhances impregnation properties while maintaining strength.
The binder achieves excellent impregnation and high mechanical strength, producing solidified bodies with improved handling and reduced variability in performance.
Smart Images

Figure 0007555423000006 
Figure 0007555423000003 
Figure 0007555423000002
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a binder, a solidified body, and a method for producing a solidified body. [Background technology]
[0002] Heat-resistant molded bodies formed by attaching a binder to a filler such as glass fiber and molding it into a mat shape are widely used as insulation materials for houses, warehouses, devices, and equipment. Phenol-formaldehyde binders are widely used as the binder. However, the phenol-formaldehyde binder has a problem that unreacted formaldehyde remains in the molded body and formaldehyde is released after construction of the house, etc. Therefore, binders that do not release formaldehyde are being studied.
[0003] For example, Patent Documents 1 to 3 propose, as binders that do not emit formaldehyde, binders that harden by reacting a carboxyl group-containing polymer, such as a polyacrylic acid polymer, with a hydroxyl group contained in the polymer itself or in a crosslinking agent such as a polyhydric alcohol. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2016-44253 A [Patent Document 2] JP 2016-98285 A [Patent Document 3] Japanese Patent Application Publication No. 6-184285 Summary of the Invention [Problem to be solved by the invention]
[0005] Here, the inventors have conducted extensive research and found that there is still room for improvement in the impregnation of fillers with conventional binders. By increasing the impregnation of the binder, it is expected that the handleability of the binder during the production of heat-resistant molded bodies can be improved and that variations in product performance caused by insufficient impregnation can be suppressed. However, when the impregnation of the binder is increased, the strength of the product tends to decrease, and it has been difficult to increase the impregnation of the binder while maintaining the strength of the product.
[0006] In view of the above, an object of the present disclosure is to provide a binder that can realize sufficiently high strength and has excellent impregnation properties, as well as to provide a solidified body using the binder and a method for producing the solidified body. [Means for solving the problem]
[0007] The binder of the present disclosure comprises a carboxyl group-containing polymer having a weight average molecular weight of 2000 to 6000 g / mol and a polyhydric alcohol, wherein the molar ratio of carboxylic acid groups of the carboxyl group-containing polymer to the polyhydric alcohol is 79:21 to 35:65, and the polyhydric alcohol comprises a polyhydric alcohol having a viscosity of 900 mPa s or less at 20°C.
[0008] The binder of the present disclosure may contain a carboxyl group-containing polymer having a weight average molecular weight of 2000 to 6000 g / mol and a polyhydric alcohol, in which the molar ratio of the carboxylic acid groups of the carboxyl group-containing polymer to the polyhydric alcohol is 79:21 to 35:65, and the polyhydric alcohol may contain at least one compound selected from the group consisting of a hydrocarbon compound substituted with 2 to 10 hydroxyl groups and a polyalkylene glycol.
[0009] The hydroxyl-substituted hydrocarbon compound is preferably at least one selected from the group consisting of ethylene glycol, propylene glycol, 1,3-propanediol, 1,3-butylene glycol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, glycerin, trimethylolpropane, trimethylolethane, erythritol, xylitol, and sorbitol.
[0010] The carboxyl group-containing polymer preferably contains a phosphorus element.
[0011] The carboxyl group-containing polymer preferably contains a residue derived from a phosphorus oxoacid.
[0012] It is preferable that the binder further comprises a polyamine.
[0013] It is preferable that the binder further contains a silane coupling agent.
[0014] It is preferable that the binder further contains a polyamine and a silane coupling agent.
[0015] It is preferable that the binder has a viscosity of 200 mPa·s or less at 25°C.
[0016] The binder may be a fiber binder.
[0017] The solidified body of the present disclosure includes a solidified product of the binder and a filler bonded by the solidified product. The solidified body of the present disclosure is formed by solidifying a precursor containing a filler and a carboxyl group-containing polymer having a weight average molecular weight of 2000 to 6000 g / mol and a polyhydric alcohol in contact with the filler, the precursor having a molar ratio of carboxylic acid groups of the carboxyl group-containing polymer to the polyhydric alcohol being 79:21 to 35:65, and the polyhydric alcohol satisfies at least one of the following conditions (1) and (2): (1) The polyhydric alcohol includes a polyhydric alcohol having a viscosity of 900 mPa·s or less at 20°C. (2) The polyhydric alcohol contains at least one compound selected from the group consisting of a hydrocarbon compound substituted with 2 to 10 hydroxyl groups and a polyalkylene glycol.
[0018] The method for producing a solidified body of the present disclosure includes a step of contacting a carboxyl group-containing polymer having a weight-average molecular weight of 2000 to 6000 g / mol and a polyhydric alcohol with a filler to obtain a precursor, in which the molar ratio of carboxylic acid groups of the carboxyl group-containing polymer to the polyhydric alcohol in the precursor is 79:21 to 35:65, and a step of solidifying the precursor, in which the polyhydric alcohol satisfies at least one of the following conditions (1) and (2): (1) The polyhydric alcohol includes a polyhydric alcohol having a viscosity of 900 mPa·s or less at 20°C. (2) The polyhydric alcohol contains at least one compound selected from the group consisting of a hydrocarbon compound substituted with 2 to 10 hydroxyl groups and a polyalkylene glycol. Effect of the Invention
[0019] According to the present disclosure, it is possible to provide a binder that can realize sufficiently high strength and has excellent impregnation properties. In addition, according to the present disclosure, it is also possible to provide a solidified body using the binder and a method for manufacturing the solidified body. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0020] Hereinafter, one embodiment of the present disclosure will be described in detail, but the present disclosure is not limited thereto. In this specification, "(meth)acrylate" means "acrylate" or "methacrylate". The same applies to other similar expressions such as "(meth)acrylic acid".
[0021] The binder according to this embodiment includes a carboxyl group-containing polymer (hereinafter also referred to as component (A)) having a weight average molecular weight of 2,000 to 6,000 g / mol and a polyhydric alcohol (hereinafter also referred to as component (B)), and the molar ratio of the carboxylic acid group of component (A) to component (B) is 79:21 to 40:60. The above-mentioned component (B) satisfies at least one of the following conditions (1) and (2). (1) The polyhydric alcohol has a viscosity of 900 mPa·s or less at 20°C. (2) The polyhydric alcohol contains at least one compound selected from the group consisting of a hydrocarbon compound substituted with 2 to 10 hydroxyl groups and a polyalkylene glycol. According to such a binder, the impregnation property with respect to the filler can be improved, and a solidified body excellent in strength can be obtained.
[0022] <Component A: Carboxyl group-containing polymer> The carboxyl group-containing polymer contained in the binder of this embodiment has a weight average molecular weight (Mw) of 2,000 to 6,000 g / mol. By including such a carboxyl group-containing polymer, a binder excellent in impregnation property can be obtained. The weight average molecular weight of the carboxyl group-containing polymer is preferably 2,500 to 6,000 g / mol, and more preferably 3,000 to 6,000 g / mol. In addition, the number average molecular weight (Mn) of the carboxyl group-containing polymer is preferably 1,000 to 4,000 g / mol, and more preferably 1,500 to 3,000 g / mol. The polydispersity (Mw / Mn) of the carboxyl group-containing polymer is preferably 1 to 3, and more preferably 1.4 to 2.5. The weight average molecular weight and number average molecular weight of the carboxyl group-containing polymer can be measured by gel permeation chromatography (GPC) under the conditions described in the examples, for example.
[0023] The carboxyl group-containing polymer of the present embodiment preferably contains a structural unit derived from a monomer having an ethylenically unsaturated group and a carboxyl group (hereinafter also referred to as an unsaturated carboxylic acid monomer). The unsaturated carboxylic acid monomer is not particularly limited, but may be, for example, a compound represented by the following general formula (I). In this specification, the term "carboxyl group" includes both a carboxylic acid group (-COOH) and a salt of a carboxylic acid group.
[0024] [ka] [In general formula (1), R 1 , R 2 , and R 3 are the same or different and each represents a hydrogen atom, a methyl group, or -(CH2) z COOM 1 represents a -(CH2) group; z COOM 1 The group is a -COOX group or another -(CH2) z COOM 1 may form an anhydride with the group, z is an integer of 0 to 2, and M 1 represents a hydrogen atom, an alkali metal, an alkaline earth metal, an ammonium ion, an organic ammonium ion, or an organic amine group, and X represents a hydrogen atom, a methyl group, an ethyl group, an alkali metal, an alkaline earth metal, an ammonium ion, an organic ammonium ion, or an organic amine group.
[0025] Examples of the unsaturated carboxylic acid monomer represented by the general formula (1) include monocarboxylic acid monomers such as (meth)acrylic acid and crotonic acid, or their salts; dicarboxylic acid monomers such as maleic acid, itaconic acid, and fumaric acid, or their salts; anhydrides of dicarboxylic acid monomers such as maleic acid, itaconic acid, and fumaric acid, or their salts; and the like. Examples of the salts mentioned here include alkali metal salts, alkaline earth metal salts, ammonium salts, organic ammonium salts, and organic amine salts. Examples of the alkali metal salts include lithium salts, sodium salts, and potassium salts. Examples of the alkaline earth metal salts include calcium salts and magnesium salts. Examples of the organic ammonium salts include methylammonium salts, ethylammonium salts, dimethylammonium salts, diethylammonium salts, trimethylammonium salts, and triethylammonium salts. Examples of the organic amine salts include alkanolamine salts such as ethanolamine salts, diethanolamine salts, and triethanolamine salts.
[0026] As the unsaturated carboxylic acid monomer represented by general formula (1), from the viewpoint of further exerting the effects of the present disclosure, preferably, (meth)acrylic acid or a salt thereof, maleic acid or a salt thereof, or maleic anhydride is used, more preferably, acrylic acid or a salt thereof, or maleic acid or a salt thereof, and even more preferably, acrylic acid.
[0027] The unsaturated carboxylic acid monomers may be used alone or in combination of two or more.
[0028] In the binder, the carboxyl groups of the carboxyl group-containing polymer may be neutralized or may not be neutralized. Of the carboxyl groups of the carboxyl group-containing polymer, 80 mol % or more may be carboxylic acid groups (i.e., unneutralized COOH groups), 90 mol % or more may be carboxylic acid groups, or 95 mol % or more may be carboxylic acid groups. The neutralization of the carboxyl group-containing polymer may be carried out by adding a neutralizing agent during or after the synthesis of the carboxyl group-containing polymer, and it is preferable to add the neutralizing agent after the synthesis. When the component (C) described below is added to the binder, it is preferable to add the neutralizing agent, the polyhydric alcohol (B), and the polyamine (C) in this order to the synthesized carboxyl group-containing polymer.
[0029] The carboxyl group-containing polymer may contain a structural unit derived from a monomer (hereinafter also referred to as "other monomer") other than the unsaturated carboxylic acid monomer. Examples of the other monomer include monomers having an ethylenically unsaturated group and a hydroxyl group (hereinafter also referred to as "unsaturated alcohol"); alkyl (meth)acrylates such as methyl (meth)acrylate, ethyl (meth)acrylate, butyl (meth)acrylate, cyclohexyl (meth)acrylate, and lauryl (meth)acrylate; amino group-containing acrylates such as dimethylaminoethyl (meth)acrylate or salts thereof; amide group-containing monomers such as (meth)acrylamide, dimethylacrylamide, and isopropylacrylamide; vinyl esters such as vinyl acetate; alkenes such as ethylene and propylene; aromatic vinyl monomers such as styrene; maleimide, phenylmaleimide, cyclohexylmaleimide, and the like. Examples of such monomers include maleimide derivatives such as maleimide, nitrile group-containing vinyl monomers such as (meth)acrylonitrile, monomers having sulfonic acid groups such as 3-allyloxy-2-hydroxypropanesulfonic acid, 2-acrylamido-2-methylpropanesulfonic acid, styrenesulfonic acid, vinylsulfonic acid, and salts thereof, phosphonic acid group-containing monomers such as vinylphosphonic acid, allylphosphonic acid, and methallylphosphonic acid, aldehyde group-containing vinyl monomers such as (meth)acrolein, alkyl vinyl ethers such as methyl vinyl ether, ethyl vinyl ether, and butyl vinyl ether, and other functional group-containing monomers such as vinyl chloride, vinylidene chloride, allyl alcohol, and vinylpyrrolidone. These monomers may be used alone or in combination of two or more.
[0030] Examples of the monomer having an ethylenically unsaturated group and a hydroxyl group include unsaturated alcohols such as allyl alcohol, β-methallyl alcohol, isoprenol, 3-methyl-3-buten-1-ol, 3-methyl-2-buten-1-ol, 2-methyl-3-buten-2-ol, and compounds represented by the following general formula (2).
[0031] [ka] [In the above general formula (2), R 4 represents a hydrogen atom or a methyl group, R 5 represents an organic group having 2 to 20 carbon atoms.
[0032] In the above general formula (2), R 5 Specific examples of the alkylene group include alkylene groups such as -CH2CH2- group, -CH(CH3)CH2- group, -CH2CH(CH3)- group, -C(CH3)2- group, -CH2CH2CH2- group, -CH(C2H5)CH2- group, -C(C2H5)(CH3)- group, -CH2CH2CH2CH2- group, and -CH(C4H9)CH2- group; arylene groups such as phenylene group and naphthyl group; ether groups such as -CH2CH2OCH2CH2- group, -CH2CH2OCH2CH2OCH2CH2- group, -CH2CH2OCH2CH2OCH2CH2OCH2CH2- group, -CH(CH3)CHOCH2OCH(CH3)CH2- group, and -CH(CH3)CHOCH2OCH(CH3)CHOCH2OCH(CH3)CH2- group; and the like.
[0033] The content of the structural unit derived from the unsaturated alcohol in the carboxyl group-containing polymer is preferably 15 mol % or less, more preferably 10 mol % or less, and even more preferably 5 mol % or less, based on 100 mol % of all structural units contained in the carboxyl group-containing polymer. The carboxyl group-containing polymer may not contain a structural unit derived from an unsaturated alcohol.
[0034] The content of the structural units derived from the unsaturated carboxylic acid monomer in the carboxyl group-containing polymer is preferably 85 mol% or more, more preferably 90 mol% or more, and even more preferably 95 mol% or more, based on 100 mol% of all structural units contained in the carboxyl group-containing polymer. The carboxyl group-containing polymer may not contain any structural units other than the structural units derived from the unsaturated carboxylic acid monomer.
[0035] The carboxyl group-containing polymer of the present embodiment may be a homopolymer containing only structural units derived from one type of monomer, or may be a copolymer containing structural units derived from two or more types of monomers. When it is a copolymer, the carboxyl group-containing polymer may be a random copolymer or a block copolymer.
[0036] The structural unit derived from the unsaturated carboxylic acid monomer and the structural unit derived from the other monomer are structural units formed by radical polymerization of the unsaturated carboxylic acid monomer and the other monomer, respectively. However, they do not necessarily have to be formed by radical polymerization of the monomers, and may be formed by another method as long as they have the same chemical structure as the structural unit formed by radical polymerization.
[0037] The carboxyl group-containing polymer of the present embodiment may contain a phosphorus element. The phosphorus element may be derived from a phosphorus-containing compound used as, for example, a chain transfer agent when synthesizing the carboxyl group-containing polymer. That is, in this case, the phosphorus element is contained in the residue of the phosphorus-containing compound bonded to the carboxyl group-containing polymer. When the carboxyl group-containing polymer contains a phosphorus element, it is preferable because the curing reaction of the binder is promoted.
[0038] Examples of the phosphorus-containing compound include phosphorus oxoacids or salts such as hypophosphorous acid (salt), phosphorous acid (salt), phosphoric acid (salt), pyrophosphoric acid (salt), polyphosphoric acid (salt), and organic phosphoric acid (salt). The content of phosphorus element in the carboxyl group-containing polymer is preferably 0 to 20 mass%, more preferably 0.1 to 15 mass%, and even more preferably 0.5 to 10 mass%, calculated as the phosphorus-containing compound, relative to 100 mass% of component (A). The phosphorus-containing compound contained as a residue in the carboxyl group-containing polymer may be one or more kinds.
[0039] The content of the component (A) in the binder of the present embodiment is preferably 10 to 90 mass %, and more preferably 20 to 80 mass %, relative to 100 mass % of the total amount of the binder.
[0040] The polymer of this embodiment can be obtained by polymerizing the above-mentioned unsaturated carboxylic acid monomer and other monomers by a conventionally known method. For example, it is preferable to use a polymer produced by a solution polymerization method in which the above-mentioned unsaturated carboxylic acid monomer and other monomers are polymerized in water in the presence of a polymerization initiator and a chain transfer agent under heating and refluxing conditions. As the polymerization initiator, sodium persulfate is preferable. As the chain transfer agent, the above-mentioned phosphorus oxoacid or salt, sodium bisulfate, etc. are preferable.
[0041] <(B) Component: Polyhydric alcohol> The polyhydric alcohol of the present embodiment satisfies at least one of the following conditions (1) and (2). The polyhydric alcohol may satisfy both of the following conditions (1) and (2). (1) Has a viscosity of 900 mPa s or less at 20°C. (2) Contains at least one compound selected from the group consisting of a hydrocarbon compound substituted with 2 to 10 hydroxyl groups (hereinafter also referred to as component (B1)) and a polyalkylene glycol (hereinafter also referred to as component (B2)). The polyhydric alcohol mainly functions as a crosslinking agent that crosslinks the carboxyl group-containing polymer in the curing reaction of the binder.
[0042] The use of such polyhydric alcohols in the binder can prevent the viscosity of the binder from increasing and improve the impregnation ability. Also, unlike the amino group-containing polyhydric alcohols such as diethanolamine and triethanolamine that have been used in the past, the protonation of the amino groups increases the pH in the binder, and there is little concern about the reduction in strength of the solidified body due to the inhibition of the hardening reaction.
[0043] The viscosity of the polyhydric alcohol at 20°C is preferably 500 mPa·s or less, more preferably 250 mPa·s or less, even more preferably 100 mPa·s or less, and particularly preferably 50 mPa·s or less. Note that the viscosity of the polyhydric alcohol refers to the viscosity of each polyhydric alcohol as a pure substance (i.e., as a single-component liquid). Examples of polyhydric alcohols having such a viscosity include dihydric alcohols such as ethylene glycol (20 mPa·s), diethylene glycol (36 mPa·s), 1,2-propanediol (56 mPa·s), 1,4-butanediol (98 mPa·s), tetraethylene glycol (55 mPa·s), 1,2-pentanediol (180 mPa·s (20°C), 2-methyl-2,4-pentanediol (34 mPa·s), and 3-methyl-1,5-pentanediol (173 mPa·s) (the numbers in parentheses are the viscosity of each compound at 20°C). The viscosity can be measured using, for example, a B-type viscometer.
[0044] The component (B1) is a compound obtained by substituting 2 to 10 hydrogen atoms of a hydrocarbon compound with hydroxyl groups. In this specification, "obtained by substitution" is a term that formally indicates a chemical structure, and does not refer only to a compound obtained by actually substituting hydrogen atoms and hydroxyl groups. Therefore, as long as the compound has a chemical structure obtained by substituting 2 to 10 hydrogen atoms of a hydrocarbon compound with hydroxyl groups, it may be a compound obtained by a chemical reaction other than direct substitution of hydrogen atoms and hydroxyl groups, or it may be a natural product.
[0045] The number of hydroxyl groups contained in the component (B1) may be 2 to 8, 2 to 5, or 2 or 3. The component (B1) may have 2 to 20, 2 to 10, or 2 to 5 carbon atoms. The above-mentioned hydrocarbon compound may be an aliphatic hydrocarbon compound or an aromatic hydrocarbon compound. The aliphatic hydrocarbon compound may be a saturated hydrocarbon compound or an unsaturated hydrocarbon compound, but is preferably a saturated hydrocarbon compound. The aliphatic hydrocarbon compound may be a chain-like aliphatic hydrocarbon compound or an aliphatic hydrocarbon compound containing a cyclic structure.
[0046] Examples of the component (B1) include alkanediols such as ethylene glycol, propylene glycol, 1,3-propanediol, 1,3-butylene glycol, 1,4-butanediol, 1,5-pentanediol, and 1,6-hexanediol; and trihydric or higher alcohols such as glycerin, trimethylolpropane, trimethylolethane, erythritol, xylitol, and sorbitol.
[0047] An example of the component (B2) is a compound represented by the following general formula (3).
[0048] [ka] (In general formula (3), A 1 is a divalent hydrocarbon group having 2 to 5 carbon atoms, n is 2 to 20, and in one molecule, A 1 may be one type or two or more types.)
[0049] In the general formula (3), examples of the divalent hydrocarbon group include an ethylene group, a 1,3-propylene group, a 1,2-propyl group, a 1,4-butylene group, and a 1,3-butylene group, and may include one or more of these groups. n may be an average value based on the number of molecules throughout the entire component (B2) (i.e., a rational number), but may also be an integer. n is preferably 2 to 10, and may be 2 to 5.
[0050] Examples of the component (B2) include polyalkylene glycols such as diethylene glycol, triethylene glycol, and tetraethylene glycol.
[0051] From the viewpoint of further increasing the impregnation ability of the binder, the molecular weight of the polyhydric alcohol is preferably 1000 g / mol or less, more preferably 500 g / mol or less, and even more preferably 200 g / mol or less.
[0052] From the viewpoint of improving the impregnation property of the binder and the mechanical strength of the obtained solidified body, the molar ratio of the carboxylic acid groups of the (A) component to the (B) component in the binder (molar amount of the carboxylic acid groups of the (A) component:molar amount of the (B) component) is 79:21 to 35:65, preferably 75:25 to 40:60, and more preferably 70:30 to 40:60.
[0053] The content of the component (B) in the binder of the present embodiment is preferably 5 to 60 mass %, and more preferably 7 to 50 mass %, relative to 100 mass % of the total amount of the binder.
[0054] <Other ingredients> The binder of the present embodiment may contain a component other than the components (A) and (B). For example, the binder may further contain at least one of a polyamine (hereinafter also referred to as the component (C)) and a silane coupling agent (hereinafter also referred to as the component (D)).
[0055] The polyamine (C) may be any compound having two or more amino groups in the molecule, but is preferably an amine compound having four or more nitrogen atoms per molecule. Examples of the polyamine (C) include polyalkylene polyamines, polyamide polyamines, polyalkylene imine alkylene oxides, and polyvinyl amines, with polyalkylene polyamines being preferred. Examples of the polyalkylene polyamines include polymers or copolymers having one or more alkylene imines as monomers (i.e., polyalkylene imines), and alkylene imine adducts of aliphatic polyvalent amines. The polyalkyleneimine is preferably a polymer or copolymer of an alkyleneimine having 2 to 8 carbon atoms (more preferably 2 to 6 carbon atoms), more preferably a polymer or copolymer of one or more alkyleneimines selected from the group consisting of ethyleneimine, propyleneimine, 1,2-butyleneimine, 2,3-butyleneimine and 1,1-dimethylethyleneimine, and even more preferably an ethyleneimine polymer (polyethyleneimine). The alkyleneimine adduct of an aliphatic polyamine is preferably one obtained by adding (ring-opening-adding) an alkyleneimine to 2 to 6 alkylenediamines (e.g., ethylenediamine, etc.). As the alkyleneimine of the adduct, those exemplified as the monomer of polyalkyleneimine are preferred. The polyalkyleneimine and adduct may not be produced by directly polymerizing or subjecting an alkyleneimine to an addition reaction, but may be synthesized by another chemical reaction as long as it has the same chemical structure as the polyalkyleneimine and adduct. The number average molecular weight of the polyamine may be 200 to 500000g / mol, 250 to 100000g / mol, 250 to 80000g / mol, 300 to 50000g / mol, 400 to 10000g / mol, or 500 to 5000g / mol. The polyamine may be used alone or in combination of two or more kinds. It is preferable that the (C) polyamine does not contain a hydroxyl group.
[0056] The content of the (C) component in the binder is preferably 0.01 to 5 parts by mass, and more preferably 0.1 to 3 parts by mass, per 100 parts by mass of the combined amount of the (A) and (B) components.
[0057] When the binder contains component (D), component (D) acts at the interface between the filler and the binder, tending to increase the impregnation of the binder and the strength of the resulting solidified body. Examples of silane coupling agents include aminosilane coupling agents such as γ-aminopropyltriethoxysilane, γ-(2-aminoethyl)aminopropyltrimethoxysilane, and γ-(2-aminoethyl)aminopropylmethyldimethoxysilane, and epoxysilane coupling agents such as γ-glycidoxypropyltrimethoxysilane and γ-glycidoxypropylmethyldimethoxysilane. These can be used alone or in combination of two or more.
[0058] The content of the silane coupling agent in the binder is preferably 0.01 to 5 parts by mass, and more preferably 0.1 to 3 parts by mass, per 100 parts by mass of the combined amount of the components (A) and (B).
[0059] The binder may further contain a free phosphorus-containing compound. The phosphorus compound is preferable because it is considered to have an effect of promoting crosslinking of the (A) component. Examples of the free phosphorus-containing compound include phosphorus oxoacids such as hypophosphorous acid (salt), phosphorous acid (salt), phosphoric acid (salt), pyrophosphoric acid (salt), polyphosphoric acid (salt), and organic phosphoric acid (salt), or salts or esters thereof (including hydrates thereof); and organic phosphorus compounds such as trimethylphosphine, triphenylphosphine, and triphenylphosphine oxide. When the binder contains a phosphorus-containing compound, it may contain one or more of these. Examples of salts include those mentioned above. The content of the phosphorus-containing compound in the binder can be preferably 20% by mass or less, more preferably 0.1 to 10% by mass, and even more preferably 0.5 to 7% by mass, based on 100% by mass of the (A) component. In addition, when component (A) contains phosphorus element, the content of the phosphorus-containing compound may be the total amount of the content of the phosphorus element contained in component (A) (converted into the amount of free phosphorus-containing compound) and the content of the free phosphorus-containing compound.
[0060] The binder may further contain a hardening accelerator other than the phosphorus-containing compound. Examples of such hardening accelerators include protonic acids (sulfuric acid, carboxylic acid, carbonic acid, etc.) and their salts (metal (alkali metal, alkaline earth metal, transition metal, 2B group, 4A group, 4B group, 5B group, etc.) salts, ammonium salts, etc.), oxides, chlorides, hydroxides, alkoxides, etc. of metals (mentioned above). These may be used alone or in combination of two or more.
[0061] The binder may contain a solvent. The solvent may be an organic solvent, but is preferably water. That is, the binder may be an aqueous solution. The content of water in the binder (aqueous solution) is preferably 10 to 80% by mass, more preferably 20 to 70% by mass, and even more preferably 25 to 60% by mass, relative to 100% by mass of the total amount of the binder.
[0062] The binder may be in a form that does not contain water or contains only a small amount of water. In this case, the content of water in the binder may be less than 10% by mass, 5% by mass or less, or 1% by mass or less, relative to 100% by mass of the total amount of the binder. Such a binder may be used as it is depending on the application, or may be diluted by adding a solvent such as water before use.
[0063] The binder may further contain additives such as rust inhibitors, colorants, dust inhibitors such as heavy oil water dispersions, and inorganic sulfates (neutralizers). Inorganic sulfates have the function of neutralizing alkaline components eluted from inorganic fibers such as glass, and examples thereof include ammonium sulfate. The content of the (A) component and the (B) component in the binder may be 90% by mass or more, or may be 95% by mass or more, based on 100% by mass of the total amount of the binder excluding the solvent.
[0064] From the viewpoint of further improving the impregnation property, the viscosity of the binder is preferably 200 mPa·s or less at 25°C, more preferably 180 mPa·s or less, even more preferably 160 mPa·s or less, even more preferably 120 mPa·s or less, and particularly preferably 100 mPa·s or less. The viscosity of the binder can be appropriately adjusted by adjusting the blending ratio of components (A) and (B) and the water content. The viscosity can be measured, for example, using a B-type viscometer.
[0065] The pH of the binder is preferably 1 to 4.0, more preferably 1.5 to 3.7, and further preferably 2 to 3.5.
[0066] <Filling material> The binder of the present embodiment can be suitably used for binding fillers (materials to be bound). There is no particular limitation on the filler, and it may be an inorganic filler or an organic filler. There is also no particular limitation on the shape of the filler, and any shape of filler, such as fibrous or particulate, may be used. The fibrous filler may be either woven fabric or nonwoven fabric. The binder of the present embodiment has excellent impregnation properties, and is therefore useful as a binder for fibers, and is particularly useful when used in nonwoven fabrics.
[0067] Examples of inorganic fillers include inorganic fibers such as glass fiber, rock wool, and carbon fiber (either woven or nonwoven, with nonwoven being preferred); inorganic particles (inorganic powders) such as powdered glass, glass particles (glass beads), and mineral particles. Among these, glass fiber or powdered glass is preferred, since the solidified body can be widely applied as a heat insulating material or the like. The binder of the present embodiment is particularly useful when binding glass nonwoven fibers (e.g., glass wool).
[0068] Examples of the organic filler include organic fibers such as wool, cellulose, hemp, nylon, and polyester; organic particles (organic powders) such as nylon fine particles and polyester fine particles; and the like.
[0069] <Solidified body> The solidified body of the present embodiment includes a solidified product of the binder and a filler material bound by the solidified product. In other words, the solidified body of the present embodiment can be said to be a composite material including a solidified product of the binder and a filler material.
[0070] <Manufacturing method of solidified body> There is no particular restriction on the method for producing the solidified body, as long as it includes a step of contacting the above-mentioned (A) component and (B) component with a filler and solidifying the precursor obtained. The (A) component and (B) component may be mixed in advance in a predetermined molar ratio with other components as necessary to prepare a binder, and the binder may be contacted with the filler (for example, impregnated into the filler or mixed with the filler) to produce the precursor, but the step of preparing the binder in advance may not be provided. When the step of preparing the binder is not provided, for example, the (A) component and (B) component, as well as other components as necessary, may be added to the filler all at once or successively and mixed or impregnated to produce the precursor. The precursor may be molded into a desired shape before the solidification step described below.
[0071] The content of the binder in the precursor is preferably 1 to 40 parts by mass, more preferably 1 to 30 parts by mass, and even more preferably 1 to 15 parts by mass, in terms of solid content, relative to 100 parts by mass of the filler. When the amount of the binder attached is within the above range, the mechanical strength of the produced solidified body tends to be improved.
[0072] After preparing the precursor, the binder contained in the precursor is solidified to solidify the precursor as a whole. As a method for solidifying the precursor, a method of heating the precursor (heating step) can be mentioned. The heating temperature and heating time in the heating step can be, for example, 100 to 300°C and 1 to 120 minutes, but from the viewpoint of operability, it is preferable to perform the heating step at a low temperature for a short time. For example, the heating temperature is preferably 120 to 250°C, more preferably 140 to 230°C, and even more preferably 150 to 200°C. In addition, the heating time is preferably 1 to 60 minutes, more preferably 1 to 45 minutes, and even more preferably 1 to 30 minutes.
[0073] In addition, the binder of the present embodiment tends to have low-temperature curing properties and fast curing properties, which is advantageous from the viewpoint of saving energy during the curing reaction and shortening the curing time. For example, the complete curing temperature can be used as an index of the low-temperature curing properties and fast curing properties of the binder. The complete curing temperature of the binder is preferably 195°C or less, more preferably 185°C or less, even more preferably 180°C or less, even more preferably 175°C or less, and particularly preferably 165°C or less. The complete curing temperature of the binder can be determined by measuring using a dynamic viscoelasticity measuring device from 30° C. to 250° C. at a heating rate of 4° C. / min, and determining the temperature at which the storage modulus becomes constant. EXAMPLES
[0074] The present disclosure will be described in more detail below with reference to examples, but the present disclosure is not limited to these examples. In addition, unless otherwise specified, "%" means "% by mass".
[0075] As component (A), carboxyl group-containing polymers having various weight average molecular weights were prepared as follows: The weight average molecular weight and solid content of component (A) were measured under the following conditions.
[0076] <Conditions for measuring weight average molecular weight (Mw)> The weight average molecular weight (Mw) was measured under the following conditions. Equipment: Tosoh HLC-8320GPC Detector: RI Column: Tosoh TSK-GEL G3000PWXL Column temperature: 35℃ Flow rate: 0.5ml / min Calibration curve: Poly Sodium Acrylate Standard manufactured by Sowa Science Co., Ltd. Eluent: A mixture of sodium dihydrogen phosphate dodecahydrate / disodium hydrogen phosphate dihydrate (34.5 g / 46.2 g) diluted to 5,000 g with pure water.
[0077] <Method for measuring the solid content of the polymer aqueous solution after completion of polymerization> The aqueous polymer solution was dried for 60 minutes in an oven heated to 130° C. The solid content (%) of the aqueous polymer solution after the completion of polymerization was calculated from the change in weight before and after drying.
[0078] <Production Example 1> 316.3g of pure water was charged (initial charge) into a 2.5-liter SUS separable flask equipped with a reflux condenser, a stirrer (paddle blade), and a thermometer, and the temperature was raised to the boiling point under stirring. Next, 900.0g (i.e., 10.0mol) of 80% by mass acrylic acid aqueous solution (hereinafter referred to as "80% AA") was dripped into the polymerization reaction system in a boiling point reflux state under stirring for 180 minutes, 71.0g of 15% by mass sodium persulfate aqueous solution (hereinafter referred to as "15% NaPS") was dripped into the polymerization reaction system in a boiling point reflux state for 195 minutes, 25.7g of 45% by mass sodium hypophosphite aqueous solution (hereinafter referred to as "45% SHP") was dripped into the polymerization reaction system in a boiling point reflux state for 18 minutes, and 101.7g of 45% by mass sodium hypophosphite aqueous solution (hereinafter referred to as "45% SHP") was dripped into the polymerization reaction system in a two-stage feed rate for 18 minutes, and then 101.7g of 45% by mass sodium hypophosphite aqueous solution (hereinafter referred to as "45% SHP") was dripped into the polymerization reaction system in a two-stage feed rate for 162 minutes, and each of the components was dripped into the polymerization reaction system through a separate feed route from the tip nozzle. Each component was dripped continuously at a constant drip rate except for 45% SHP. After the dropwise addition of 80% AA was completed, the reaction solution was kept at boiling point reflux for another 30 minutes (aging) to complete the polymerization. After the polymerization was completed, 417.8 g of pure water was added to the reaction solution, and the resulting aqueous solution had a solid content of 44.3%, a number average molecular weight of 1920, and a weight average molecular weight of 3080 (polydispersity index: 1.60). Hereinafter, the obtained polymer is also referred to as PAA3000.
[0079] <Production Example 2> 329.0g of pure water was charged (initial charge) into a 2.5-liter SUS separable flask equipped with a reflux condenser, a stirrer (paddle blade), and a thermometer, and the temperature was raised to the boiling point under stirring. Next, 900.0g (i.e., 10.0mol) of 80% by mass acrylic acid aqueous solution (hereinafter referred to as "80% AA") was dripped into the polymerization reaction system in a boiling point reflux state under stirring for 180 minutes, 59.2g of 15% by mass sodium persulfate aqueous solution (hereinafter referred to as "15% NaPS") was dripped into the polymerization reaction system in a boiling point reflux state for 195 minutes, 21.4g of 45% by mass sodium hypophosphite aqueous solution (hereinafter referred to as "45% SHP") was dripped into the polymerization reaction system in a boiling point reflux state for 18 minutes, and 84.8g of 45% by mass sodium hypophosphite aqueous solution (hereinafter referred to as "45% SHP") was dripped into the polymerization reaction system in a two-stage feed rate for 18 minutes, and then 84.8g of 45% by mass sodium hypophosphite aqueous solution (hereinafter referred to as "45% SHP") was dripped into the polymerization reaction system in a two-stage feed rate for 162 ... After the dropwise addition of 80% AA was completed, the reaction solution was kept at boiling point reflux for another 30 minutes (aging) to complete the polymerization. After the polymerization was completed, 411.8 g of pure water was added to the reaction solution, and the resulting aqueous solution had a solid content of 44.7%, a number average molecular weight of 2260, and a weight average molecular weight of 4080 (polydispersity index: 1.81). Hereinafter, the obtained polymer is also referred to as PAA4000.
[0080] <Production Example 3> In a 2.5-liter SUS separable flask equipped with a reflux condenser, a stirrer (paddle blade), and a thermometer, 437.4 g of pure water was charged (initial charge), and the temperature was raised to the boiling point under stirring. Next, 1560.0 g (i.e., 17.3 mol) of 80 mass% acrylic acid aqueous solution (hereinafter referred to as "80% AA") was dropped into the polymerization reaction system in a boiling point reflux state under stirring for 180 minutes, 55.0 g of 15 mass% sodium persulfate aqueous solution (hereinafter referred to as "15% NaPS") was dropped for 195 minutes, and 26.9 g of 45 mass% sodium hypophosphite aqueous solution (hereinafter referred to as "45% SHP") was dropped for 18 minutes, followed by 107.7 g for 162 minutes, at two-stage supply rates, from the tip nozzle through separate supply paths. Each component was continuously dropped at a constant drip rate except for 45% SHP. After the dropwise addition of 80% AA was completed, the reaction solution was kept at boiling point reflux for another 30 minutes (aging) to complete the polymerization. After the polymerization was completed, 207.2 g of pure water was added to the reaction solution, and the resulting aqueous solution had a solid content of 56.3%, a number average molecular weight of 2890, and a weight average molecular weight of 5980 (polydispersity index: 2.07). Hereinafter, the obtained polymer is also referred to as PAA6000.
[0081] <Production Example 4> In a 2.5-liter SUS separable flask equipped with a reflux condenser, a stirrer (paddle blade), and a thermometer, 401.8 g of pure water was charged (initial charge), and the temperature was raised to the boiling point under stirring. Next, 1200.0 g (i.e., 13.3 mol) of 80 mass% acrylic acid aqueous solution (hereinafter referred to as "80% AA") was dropped into the polymerization reaction system in a boiling point reflux state under stirring for 180 minutes, 42.3 g of 15 mass% sodium persulfate aqueous solution (hereinafter referred to as "15% NaPS") was dropped for 195 minutes, and 15.9 g of 45 mass% sodium hypophosphite aqueous solution (hereinafter referred to as "45% SHP") was dropped for 18 minutes and then 63.8 g for 162 minutes, at two-stage supply rates, from the tip nozzle through separate supply paths. Each component was continuously dropped at a constant drip rate except for 45% SHP. After the dropwise addition of 80% AA was completed, the reaction solution was kept at boiling point reflux for another 30 minutes (aging) to complete the polymerization. After the polymerization was completed, 269.9 g of pure water was added to the reaction solution to obtain an aqueous solution (PAA8000) with a solid content of 51.5%, a number average molecular weight of 3570, and a weight average molecular weight of 8070 (polydispersity index: 2.26). Hereinafter, the obtained polymer is also referred to as PAA8000.
[0082] <Production Example 5> In a 2.5-liter SUS separable flask equipped with a reflux condenser, a stirrer (paddle blade), and a thermometer, 400.0 g of pure water was charged (initial charge), and the temperature was raised to the boiling point under stirring. Next, 1051.8 g (i.e., 11.7 mol) of 80 mass% acrylic acid aqueous solution (hereinafter referred to as "80% AA") was dropped into the polymerization reaction system in a boiling point reflux state under stirring for 180 minutes, 35.4 g of 15 mass% sodium persulfate aqueous solution (hereinafter referred to as "15% NaPS") was dropped for 195 minutes, and 5.5 g of 45 mass% sodium hypophosphite aqueous solution (hereinafter referred to as "45% SHP") was dropped for 18 minutes and then 22.0 g for 162 minutes, at two-stage supply rates, from the tip nozzle through separate supply paths. Each component was continuously dropped at a constant drip rate except for 45% SHP. After the dropwise addition of 80% AA was completed, the reaction solution was kept at boiling point reflux for another 30 minutes (aging) to complete the polymerization. After the polymerization was completed, 165.8 g of pure water was added to the reaction solution, and the resulting aqueous solution had a solid content of 52.4%, a number average molecular weight of 7410, and a weight average molecular weight of 29290 (polydispersity index: 3.95). Hereinafter, the obtained polymer is also referred to as PAA30000.
[0083] The binders of Examples 1 to 20 and Comparative Examples 1 to 11 were produced by mixing (A) a carboxyl group-containing polymer, (B) a polyhydric alcohol, (C) a polyamine, and (D) a silane coupling agent in the mixing ratios shown in Tables 1 to 3. For each of the obtained binders, various performance evaluations were carried out by adding an appropriate amount of water as shown below. The results are shown in Tables 1 to 3.
[0084] The viscosity of the polyhydric alcohol, component (B), at 20°C is as follows. Ethylene glycol: 20 mPa·s Diethylene glycol: 36 mPa·s Tetraethylene glycol: 55 mPa·s 1,4-Butanediol: 98mPa·s Diethanolamine: 1000mPa·s Triethanolamine: 1013 mPa·s In Tables 1 to 3, the content of component (A) is the amount (mol) of structural units derived from acrylic acid, and the unit of the content of component (B) is mol.
[0085] The abbreviations or abbreviations of the components in Tables 1 to 3 are as follows. <Component (C): Polyamine> PEI (1): Polyethyleneimine (product name: Epomin (registered trademark) SP-006, manufactured by Nippon Shokubai Co., Ltd., number average molecular weight 600 (measured by boiling point elevation method)) PEI (2): Polyethyleneimine (product name: Epomin (registered trademark) P-1000, manufactured by Nippon Shokubai Co., Ltd., number average molecular weight 70,000 (measured by viscosity method)) <Component (D): Silane coupling agent> Silane I: γ-glycidoxypropyltrimethoxysilane (Shin-Etsu Chemical Co., Ltd.) Aminosilane: γ-(2-aminoethyl)aminopropyltrimethoxysilane (Tokyo Chemical Industry Co., Ltd.) In Tables 1 to 3, the contents of the component (C) and the component (D) are in parts by mass relative to 100 parts by mass of the total content of the components (A) and (B).
[0086] <Preparation of test specimen> Test pieces for measuring mechanical strength were prepared as follows. (i) Pure water was added to the binder to dilute it to 35% by mass, thereby preparing an aqueous binder solution. (ii) The aqueous binder solution obtained in (i) was added to glass beads having a particle size of 0.50 to 0.150 mm so that the aqueous binder solution was 5.0% of the mass of the glass beads, and mixed thoroughly to obtain a mixture. (iii) The mixture obtained in (ii) was pressed into a release-treated mold of 120 mm x 20 mm x 5 mm to mold it, and then it was dried in an oven at 210°C for 30 minutes and cooled at room temperature for 30 minutes to obtain a test piece.
[0087] <Mechanical strength of test specimen> Regarding the above test pieces, the flexural strength was measured at a test speed of 2 mm / min in accordance with JIS K7171. The flexural strengths of three test pieces were measured, and the average value was calculated.
[0088] <Evaluation Method for Impregnation Property against Glass Beads> In a petri dish with a diameter of 120 mm, 30 g of glass beads with a particle size of 0.50 to 0.150 mm were spread evenly in height, and 3 g of the above binder aqueous solution was slowly dropped onto the center of the petri dish. After the dropping was completed, the spreading area of the binder on the glass beads 10 seconds after the elapse of time was calculated. The area was classified according to the following criteria, and the impregnation property was evaluated. A: 25 cm 2 above B: 20 cm 2 above 25 cm 2 less than C: 20 cm 2 less than
[0089] <Evaluation Method for Complete Curing Temperature> Using a dynamic viscoelasticity measuring device (DMA), the measurement was carried out at a temperature rising rate of 4 °C / min from 30 °C to 250 °C, and the temperature at which the storage elastic modulus became constant was defined as the complete curing temperature.
[0090] <Measurement Method for pH> At 25 °C, for the binder aqueous solution obtained by adding pure water to the binder and diluting it to 50%, the pH value was measured using a pH meter (product name "D-51" manufactured by HORIBA). The results are shown in Tables 1 to 3.
[0091] <Measurement Method for Viscosity> At 25 °C, for the binder aqueous solution obtained by adding pure water to the binder and diluting it to 50%, the viscosity was measured using a B-type viscometer (manufactured by Tokyo Keiki Inc.) at a rotational speed of 30 rpm. The appropriate spindle was used according to the range of the viscosity to be measured. The results are shown in Tables 1 to 3.
[0092]
Table 1
[0093]
Table 2
[0094]
Table 3
Claims
1. a carboxyl group-containing polymer having a weight average molecular weight of 2000 to 6000 g / mol; and a polyhydric alcohol, the molar ratio of the carboxylic acid group of the carboxyl group-containing polymer to the polyhydric alcohol is 60:40 to 35:65; The binder, wherein the polyhydric alcohol comprises a polyhydric alcohol having a viscosity of 900 mPa·s or less at 20°C.
2. 2. The binder according to claim 1, wherein the polyhydric alcohol comprises at least one compound selected from the group consisting of a hydrocarbon compound substituted with 2 to 10 hydroxyl groups and a polyalkylene glycol.
3. a carboxyl group-containing polymer having a weight average molecular weight of 2000 to 6000 g / mol; and a polyhydric alcohol, the molar ratio of the carboxylic acid group of the carboxyl group-containing polymer to the polyhydric alcohol is 60:40 to 35:65; The binder, wherein the polyhydric alcohol comprises at least one compound selected from the group consisting of a hydrocarbon compound substituted with 2 to 10 hydroxyl groups and a polyalkylene glycol.
4. The binder according to claim 3, wherein the hydrocarbon compound substituted with a hydroxyl group is at least one selected from the group consisting of ethylene glycol, propylene glycol, 1,3-propanediol, 1,3-butylene glycol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, glycerin, trimethylolpropane, trimethylolethane, erythritol, xylitol, and sorbitol.
5. The binder according to any one of claims 1 to 4, wherein the carboxyl group-containing polymer contains a phosphorus element.
6. 6. The binder of claim 5, wherein the carboxyl-containing polymer contains residues derived from phosphorus oxoacids.
7. The binder according to any one of claims 1 to 6, further comprising a polyamine.
8. The binder according to any one of claims 1 to 7, further comprising a silane coupling agent.
9. The binder of any one of claims 1 to 6, further comprising a polyamine and a silane coupling agent.
10. The binder according to any one of claims 1 to 9, having a viscosity of 200 mPa·s or less at 25°C.
11. The binder according to any one of claims 1 to 10, which is a binder for fibers.
12. A solidified product of the binder according to any one of claims 1 to 11; and a filler bound by the solidified material.
13. a step of contacting a carboxyl group-containing polymer having a weight average molecular weight of 2000 to 6000 g / mol and a polyhydric alcohol with a filler to obtain a precursor, the molar ratio of the carboxylic acid group of the carboxyl group-containing polymer to the polyhydric alcohol in the precursor being 60:40 to 35:65; solidifying the precursor; The method for producing a solidified body, wherein the polyhydric alcohol satisfies at least one of the following conditions (1) and (2): (1) The polyhydric alcohol includes a polyhydric alcohol having a viscosity of 900 mPa·s or less at 20° C. (2) The polyhydric alcohol contains at least one compound selected from the group consisting of a hydrocarbon compound substituted with 2 to 10 hydroxyl groups and a polyalkylene glycol.
14. A solidified body formed by solidifying a precursor containing a filler, a carboxyl group-containing polymer having a weight average molecular weight of 2000 to 6000 g / mol, and a polyhydric alcohol, the precursor being in contact with the filler, a molar ratio of a carboxylic acid group of the carboxyl group-containing polymer in the precursor to the polyhydric alcohol is 60:40 to 35:65; A solidified body, wherein the polyhydric alcohol satisfies at least one of the following conditions (1) and (2): (1) The polyhydric alcohol includes a polyhydric alcohol having a viscosity of 900 mPa·s or less at 20° C. (2) The polyhydric alcohol contains at least one compound selected from the group consisting of a hydrocarbon compound substituted with 2 to 10 hydroxyl groups and a polyalkylene glycol.
Citation Information
Patent Citations
Hardenable water-base composition and method for hardening same
JP1994184285A
Fiber-finishing agent, finish liquid, finishing method and finished fiber
JP2001200480A
Thermosetting aqueous composition and processed paper products and processed fiber products using the composition
JP2006143933A
Aqueous binder for inorganic fiber heat-insulating / sound-absorbing material, and inorganic fiber heat-insulating / sound-absorbing material
JP2007211161A
Nonionic polyhydric alcohol-containing binder
JP2016044253A