Novel catalytic substance for producing polyester, process for producing polyester using the same, and polyester produced using the same
A catalyst with a specific formula optimizes polyester production by enhancing molecular weight and reducing thermal discoloration, addressing the trade-off issues in existing methods without the need for thermal stabilizers.
Patent Information
- Application Number
- JP2023516568
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-09-09
- Filing Date
- 2021-09-13
- Publication Date
- 2024-09-24
- Estimated Expiration
- 2041-09-13
AI Technical Summary
Existing polyester production methods face challenges in achieving high molecular weight while minimizing thermal discoloration, often requiring additional thermal stabilizers to manage color issues during processing.
A catalyst with a specific formula (C a H b O c P d Ti e ) is used to polymerize dicarboxylic acid aromatic heterocyclic compounds, optimizing conditions for esterification and polycondensation reactions to produce polyester with high molecular weight and reduced thermal discoloration without the need for thermal stabilizers.
The catalyst enables the production of polyester with improved molecular weight and minimized thermal discoloration, ensuring high-quality products suitable for various applications without the use of additional additives.
Smart Images

Figure 0007555485000028 
Figure 0007555485000039 
Figure 0007555485000042
Abstract
Description
[Technical field]
[0001] The present invention relates to novel catalytic materials used to prepare polyesters from dicarboxylic acid aromatic heterocyclic compounds or derivatives thereof, methods for producing polyesters therewith, and polyesters produced therewith. [Background technology]
[0002] In order to reduce greenhouse gases, developed countries such as the United States and Europe are strengthening regulations on carbon dioxide emissions. Therefore, there is an increasing demand for the biochemical industry, which can reduce greenhouse gases by reducing the dependence on existing fossil raw materials. In other words, the chemical industry is changing from being dependent on petroleum to being dependent on bio.
[0003] As an example, active research is being conducted into the replacement of polyethylene terephthalate (PET), which is primarily used in beverage bottles and food storage containers, with bio-based polyester.
[0004] In the production of polyesters, dicarboxylic acid aromatic heterocyclic compounds or derivatives useful as monomers are usually derivatives produced by oxidizing 5-hydroxymethylfurfural, a representative example being 2,5-furandicarboxylic acid. For reference, 5-hydroxymethylfurfural (HMF) is a derivative of a natural and widely available raw material, since it is obtained from sugar.
[0005] A technology has been developed for producing polyesters by esterifying the dicarboxylic acid aromatic heterocyclic compound or a derivative thereof with a diol and subjecting the oligomer thus obtained to a condensation polymerization reaction.
[0006] The esterification reaction is a bonding reaction between the carboxyl group of a dibasic acid and the OH group of a glycol, which occurs under an inert gas atmosphere at normal or elevated pressure, and produces water as a by-product (Equation 1).
[0007] (Formula 1) JPEG0007555485000001.jpg20150
[0008] The reaction is accelerated by removing the produced water with effluent water, and it can be inferred that the esterification reaction is completed when no effluent water is generated. The reaction can also be accelerated by adding a polymerization catalyst as necessary.
[0009] In addition, in the condensation polymerization reaction, the terminal glycol of one of the oligomers obtained by the esterification reaction described above is removed under a reduced pressure environment, and is bonded to the terminal glycol of the other oligomer. Glycol is generated as a by-product (Formula 2), and by draining and removing this, the reaction is promoted and the degree of polymerization is increased.
[0010] (Formula 2) JPEG0007555485000002.jpg30162
[0011] In the condensation polymerization process, coloring may occur due to the formation of double bonds between carbon atoms (Formula 3). Coloring of polyester can cause a loss of aesthetic appearance when processed into bottles, films, fibers, etc. In addition, it may be difficult to achieve appropriate color development when dyeing clothing.
[0012] (Formula 3) JPEG0007555485000003.jpg18151
[0013] If a polymer becomes discolored, it can cause a loss of aesthetic appeal when it is processed into bottles, films, fibers, etc. Therefore, in order to eliminate discoloration (hereinafter also referred to as thermal discoloration), a technology has been proposed in which additives such as heat stabilizers are added at an appropriate point during the condensation polymerization process, but a technology that satisfies all of the physical properties that are in a trade-off relationship between thermal discoloration and molecular weight has not yet been developed. [Prior art documents] [Patent documents]
[0014] [Patent Document 1] Chinese Patent No. 103483571 Summary of the Invention [Problem to be solved by the invention]
[0015] An object of the present invention is to provide a catalyst for producing polyester, which has a molecular weight that can withstand various molding processes and can suppress discoloration of the polyester during the production process, a method for producing polyester using the catalyst, and polyester produced using the catalyst. [Means for solving the problem]
[0016] According to a first aspect of the present invention, there is provided a catalyst for producing polyester, said catalyst having formula C a H b O c P d Ti e The present invention provides a catalyst for producing polyester, comprising a structure represented by the following formula: (a is an integer of 30 to 120, b is an integer of 50 to 250, c is an integer of 5 to 30, d is an integer of 0 to 4, e is an integer of 1 to 2, and c / e≧5).
[0017] At this time, the above formula C a H b O c P d Ti e In the above formula, a is an integer of 44 to 100, b is an integer of 98 to 194, c is an integer of 8 to 18, d is an integer of 2 to 4, and e is an integer of 1 to 2, and 8≦c / e≦18.
[0018] The catalyst may contain at least one of -Ti-OP-, -Ti-PO- and -Ti-O- bonds.
[0019] The catalyst may include a structure represented by the following formulas 1 to 3.
[0020] [Chemical formula 1] JPEG0007555485000004.jpg40140
[0021] [Chemical formula 2] JPEG0007555485000005.jpg2977
[0022] [Chemical formula 3] JPEG0007555485000006.jpg983
[0023] The catalyst may have a specific gravity measured at 25° C. of 0.94 to 0.99.
[0024] The catalyst may be one that polymerizes a dicarboxylic acid aromatic heterocyclic compound having a structure represented by the following formula 4 or 5, or a derivative thereof, to produce a polyester.
[0025] [Chemical formula 4] JPEG0007555485000007.jpg2760
[0026] [Chemical formula 5] JPEG0007555485000008.jpg2859
[0027] According to a second aspect of the present invention, there is provided a method for producing a polyester, comprising subjecting a dicarboxylic acid aromatic heterocyclic compound or a derivative thereof to an ester reaction with an alkylene-providing raw material in the presence of a catalyst, followed by a condensation polymerization reaction, wherein the catalyst is the above-mentioned catalyst for producing a polyester, and the dicarboxylic acid aromatic heterocyclic compound or a derivative thereof comprises a structure represented by the following chemical formula 4 or chemical formula 5:
[0028] [Chemical formula 4] JPEG0007555485000009.jpg2760
[0029] [Chemical formula 5] JPEG0007555485000010.jpg2859
[0030] wherein the alkylene provider may be an aliphatic diol or an aromatic diol.
[0031] The alkylene-providing raw material can be used in a molar ratio of 1.2 to 3.6 based on 1 mole of the dicarboxylic acid aromatic heterocyclic compound represented by Chemical Formula 4 or Chemical Formula 5 or a derivative thereof.
[0032] The esterification reaction may be performed by treating the dicarboxylic acid aromatic heterocyclic compound and the alkylene-providing feedstock under a nitrogen atmosphere at 150-240° C. and 1-6 bar pressure to obtain an ester product of the dicarboxylic acid aromatic heterocyclic compound or a derivative thereof.
[0033] The condensation polymerization reaction may be a condensation polymerization treatment of the ester product at 230 to 285° C. under reduced pressure conditions.
[0034] The amount of the catalyst used may be more than 5 ppm and less than 300 ppm.
[0035] According to a third aspect of the present invention, there is provided a polyester comprising a repeating unit containing an ester bond of a dicarboxylic acid aromatic heterocyclic compound or a derivative thereof and an alkylene providing raw material, wherein the difference (ΔIV) between the intrinsic viscosity measured at 25° C. and the intrinsic viscosity measured at 35° C. is 0.06 or more, and the b value measured by a Lab color difference meter is 12 or less, and the dicarboxylic acid aromatic heterocyclic compound or derivative thereof comprises a structure represented by the following Chemical Formula 4 or Chemical Formula 5.
[0036] [Chemical formula 4] JPEG0007555485000011.jpg2760
[0037] [Chemical formula 5] JPEG0007555485000012.jpg2859
[0038] In this case, the alkylene source may be an aliphatic diol or an aromatic diol.
[0039] The polyester may have an intrinsic viscosity measured at 25° C. of 0.5 or more, and an intrinsic viscosity measured at 35° C. of 0.43 or more.
[0040] After dissolving 2 g of the polyester in 20 ml of hexafluoroisopropanol (HFIP) (0.1 g / ml in HFIP), the b value of the solution measured using a Lab colorimeter may be less than 7.12.
[0041] The polyester may have a value of the following mathematical formula 1 of 0.5 or more.
[0042] <Formula 1> JPEG0007555485000013.jpg2246
[0043] (In the above formula 1, ΔIV is the difference between the intrinsic viscosity values measured at 35° C. and 25° C., and the b value is the b value measured with a Lab color difference meter.)
[0044] The polyester may have a value of the following mathematical formula 2 of 0.4 or more.
[0045] <Formula 2> JPEG0007555485000014.jpg2941
[0046] (In the above formula 2, ΔIV is the difference between the intrinsic viscosity values measured at 35° C. and 25° C., respectively, the b value is the b value measured by a Lab color difference meter, and Tg is the glass transition temperature.) Effect of the Invention
[0047] The catalyst for producing polyester according to one aspect of the present invention has an effect of providing polyester with physical properties in a trade-off relationship between thermal discoloration and molecular weight without adding a heat stabilizer or antioxidant.
[0048] The polyester according to another aspect of the present invention is not only environmentally friendly in that it can be naturally decomposed by microorganisms present in the environment, but also has the effect of being suitable as a replacement for PET, which has been used conventionally.
[0049] Furthermore, the method for producing polyester according to another aspect of the present invention has the advantage that it does not require a separate reactor for producing PEF, and a reactor that has been used for conventional PET production can be used as is. BEST MODE FOR CARRYING OUT THEINVENTION
[0050] Hereinafter, a method for producing a polyester using the dicarboxylic acid aromatic heterocyclic compound or a derivative thereof of the present invention as a raw material and a catalyst used therein will be described in detail.
[0051] Throughout the specification, when a part is said to "comprise" certain elements, this means that it may further include other elements, but not to the exclusion of other elements, unless specifically stated to the contrary.
[0052] <First aspect of the present invention> A first aspect of the present invention is a catalyst for producing polyester, comprising a compound of formula C a H b O c P d Ti e (a is an integer of 30 to 120, b is an integer of 50 to 250, c is an integer of 5 to 30, d is an integer of 0 to 4, e is an integer of 1 to 2, and c / e≧5).
[0053] Here, a can be an integer from 44 to 100.
[0054] Furthermore, b can be an integer from 98 to 194.
[0055] In addition, c can be an integer from 8 to 18.
[0056] In addition, d can be an integer of 2 to 4.
[0057] Also, 8≦c / e≦18.
[0058] As an example, a catalyst that satisfies the above-mentioned conditions a, b, c, d, e, and c / e and contains a -Ti-OP- bond, a catalyst that contains a -Ti-PO- bond, or a catalyst that contains a -Ti-O- bond can be used.
[0059] As a specific example, it is more preferable to use a catalyst which satisfies the above-mentioned conditions a, b, c, d, e, and c / e and contains a -Ti-OP- bond or a catalyst which contains a -Ti-PO- bond, since this can eliminate the trade-off relationship between thermal discoloration and molecular weight.
[0060] The catalyst may include structures represented by the following Formulas 1 to 3, but is not limited thereto.
[0061] [Chemical formula 1] JPEG0007555485000015.jpg40140
[0062] [Chemical formula 2] JPEG0007555485000016.jpg2977
[0063] [Chemical formula 3] JPEG0007555485000017.jpg983
[0064] According to an embodiment of the present invention, the specific gravity of the catalyst measured at 25° C. may be within a range of 0.94 to 0.99, or 0.94 to 0.97. Within the above range, an optimized specific gravity can be provided in the polymerization reaction, which is more preferable in terms of eliminating the trade-off relationship between thermal discoloration and molecular weight.
[0065] The amount of the catalyst used is not particularly limited, but may be, for example, within the range of a content of more than 5 ppm and less than 300 ppm.
[0066] The catalyst may be capable of polymerizing a dicarboxylic acid aromatic heterocyclic compound or a derivative thereof, including a structure represented by the following formula 4 or 5, to produce a polyester:
[0067] [Chemical formula 4] JPEG0007555485000018.jpg2760
[0068] [Chemical formula 5] JPEG0007555485000019.jpg2859
[0069] <Second aspect of the present invention> The method for producing polyester comprises esterifying the above-mentioned dicarboxylic acid aromatic heterocyclic compound or a derivative thereof with an alkylene-providing raw material in the presence of a catalyst for producing polyester to obtain an oligomer, and then producing polyester by condensation polymerization of the oligomers.
[0070] As described above, the raw material of the present invention may be a dicarboxylic acid aromatic heterocyclic compound or a derivative thereof, which includes the structure represented by Chemical Formula 4 or Chemical Formula 5.
[0071] [Chemical formula 4] JPEG0007555485000020.jpg2760
[0072] [Chemical formula 5] JPEG0007555485000021.jpg2859
[0073] The alkylene source may be an aliphatic diol or an aromatic diol, and specific examples include, but are not limited to, ethylene glycol, propanediol, butanediol, hexanediol, octanediol, and the like.
[0074] The alkylene-providing raw material is preferably used in a molar ratio of 1.2 to 3.6 or 1.2 to 2.4 based on 1 mole of the dicarboxylic acid aromatic heterocyclic compound or its derivative represented by Chemical Formula 4 or Chemical Formula 5, since this allows the production of a polyester with a high molecular weight and a low b value.
[0075] In addition, the method for producing polyester may include various copolymerization components as necessary, including, but not limited to, isosorbide, 1,4-cyclohexanedimethanol, 2,2,4,4-tetramethyl-1,3-cyclobutanediol, and glycerin.
[0076] According to an embodiment of the present invention, the esterification reaction is a step of treating the dicarboxylic acid aromatic heterocyclic compound and the alkylene source material under a nitrogen atmosphere to obtain an ester product of the dicarboxylic acid aromatic heterocyclic compound or a derivative thereof.
[0077] In this case, the reaction temperature may be within the range of 150 to 240° C., the reaction pressure may be 1 bar to 6 bar, and the reaction may be carried out for 1 hour to 6 hours.
[0078] The above-mentioned temperature and pressure conditions are preferable because they allow the esterification step of the dicarboxylic acid aromatic heterocyclic compound or its derivative to be carried out sufficiently.
[0079] The polycondensation step is a step of producing polyester as a polycondensation product by subjecting the product of the reaction step to reduced pressure and severe temperature conditions.
[0080] Here, reduced pressure conditions refer to vacuum conditions unless otherwise specified.
[0081] Furthermore, the temperature conditions for the condensation polymerization reaction are not limited as long as the reaction temperature is within a range in which glycol separation and glycol bonding between the produced oligomers can be sufficiently repeated. For example, the reaction can be carried out under conditions of 230 to 285°C.
[0082] The condensation polymerization reaction can be carried out for 1 to 24 hours.
[0083] In particular, in the present invention, the catalyst used in the production of the oligomer contains -Ti-PO- or -Ti-OP- bonds, so that it is possible to produce a polyester having stability against thermal discoloration by increasing the molecular weight even when the reaction time is shortened under the severe high temperature conditions of the condensation polymerization reaction.
[0084] <Third aspect of the present invention> A third aspect of the present invention is a polyester produced by the production method according to the second aspect using the catalyst for producing a polyester according to the first aspect.
[0085] The polyester may include a repeating unit derived from a dicarboxylic acid aromatic heterocyclic compound or a derivative thereof, and specifically may include a repeating unit including an ester bond between a dicarboxylic acid aromatic heterocyclic compound or a derivative thereof and an alkylene providing material.
[0086] The dicarboxylic acid aromatic heterocyclic compound or a derivative thereof may include a structure represented by the following Chemical Formula 4 or Chemical Formula 5.
[0087] [Chemical formula 4] JPEG0007555485000022.jpg2760
[0088] [Chemical formula 5] JPEG0007555485000023.jpg2859
[0089] The alkylene source may be an aliphatic diol or an aromatic diol, examples of which include, but are not limited to, ethylene glycol, propanediol, butanediol, hexanediol, octanediol, and the like.
[0090] The polyester may have a difference (ΔIV) between an intrinsic viscosity measured at 25° C. and an intrinsic viscosity measured at 35° C. of 0.06 or more, for example, 0.59 or more and 0.68 or less.
[0091] At the same time, the polyester may have a b value of 12 or less on a Lab colorimeter, for example less than 14.5.
[0092] That is, the polyester has a higher ΔIV value relative to the b value than general polyesters. Generally, the higher the molecular weight of a polyester obtained by a condensation polymerization process, the higher the color value (b value) due to thermal discoloration tends to be. However, since the polyester is produced using the catalyst, even if the ΔIV is high, the color value (b value) is low and there is no thermal discoloration, and a polymer with a high molecular weight can be obtained.
[0093] Here, the polyester may have an intrinsic viscosity measured at 25° C. of 0.5 or more, for example, 0.59 or more and 0.68 or less, and may have an intrinsic viscosity measured at 35° C. of 0.43 or more, for example, 0.476 or more and 0.512 or less.
[0094] In addition, the polyester may have a b value of less than 7.12 in a solution state as measured by a Lab colorimeter, for example, less than 6.12 and greater than or equal to 0.501. As an example, the b value of the solution state as measured by a Lab colorimeter may be measured by dissolving 2 g of the polyester in 20 ml of hexafluoroisopropanol (HFIP) (0.1 g / ml in HFIP) and then measuring the b value of the solution state as measured by a Lab colorimeter using a quartz cell designed specifically for solution colorimeter measurement, using a Konica Minolta CM-3700A product.
[0095] The polyester may have a value of the following Formula 1 of 0.5 or more, for example, 1.0 or more and 1.5 or less.
[0096] <Formula 1> JPEG0007555485000024.jpg2246
[0097] In the above formula 1, ΔIV is the difference between the intrinsic viscosity values measured at 35° C. and 25° C., and the b value is the b value measured with a Lab color difference meter.
[0098] In addition, the polyester may have a value of the following mathematical formula 2 of 0.4 or more, for example, 0.6 or more and 1.21 or less.
[0099] <Formula 2> JPEG0007555485000025.jpg2941
[0100] In the above formula 2, ΔIV is the difference between the intrinsic viscosity values measured at 35° C. and 25° C., respectively, the b value is the b value measured by a Lab color difference meter, and Tg is the glass transition temperature.
[0101] That is, the polyester has a calculated correlation value (Equation 2) between the difference (ΔIV) between the intrinsic viscosity measured at normal pressure and 25°C and the intrinsic viscosity measured at normal pressure and 35°C, the color purity b value in a chip state, and the glass transition temperature, which is 0.4 or more, and the ΔIV and Tg values relative to the b value are higher than those of general polyesters. Generally, the higher the molecular weight of a polyester obtained by a condensation polymerization process, the higher the color value (b value) due to thermal discoloration tends to be, but the polyester is produced using the catalyst, so that a polymer with a high molecular weight and a low color value (b value) can be obtained even if the ΔIV is high, and there is no thermal discoloration.
[0102] Additionally, the COOH end groups of the polyester may be in the range of 10 to 12 meq / kg.
[0103] Additionally, the moisture content of the polyester may be within the range of 7067 to 7947 ppm.
[0104] The glass transition temperature (Tg) of the polyester may be within the range of 84.7 to 86°C.
[0105] <Fourth aspect of the present invention> A fourth aspect of the present invention is an apparatus for producing a polyester by polymerizing a dicarboxylic acid aromatic heterocyclic compound or a derivative thereof using an alkylene starting material in the presence of a catalyst.
[0106] The fourth aspect of the production apparatus includes a reactor, a storage tank for the dicarboxylic acid aromatic heterocyclic compound or its derivative raw material, and an alkylene raw material supply device, where the reactor may be, but is not limited to, a cylindrical column reactor filled with a support carrying an active catalyst.
[0107] In addition, the alkylene-providing raw material supply device has a structure connected to a piping that connects a storage tank for the dicarboxylic acid aromatic heterocyclic compound or its derivative raw material with the reactor, and can supply the raw material into the reactor in a pressurized state.
[0108] The layout structure of these alkylene-providing raw material supply devices is preferable because the raw materials are transferred into the reactor under pressure, eliminating the need for separate or additional control of the pressurization conditions in the reactor, and the raw materials can increase the degree of reaction activation.
[0109] The reactor pressure may be controlled within a range of 1 to 6 atmospheres by the alkylene source material supplied through the alkylene source material supply device, and the reactor temperature may be controlled within a range of 40°C to 260°C.
[0110] The alkylene raw material is the same as that described above, and therefore a detailed description thereof will be omitted.
[0111] In this case, the dicarboxylic acid aromatic heterocyclic compound or a derivative thereof may include a structure represented by Formula 4 or Formula 5.
[0112] The cylindrical column reactor may be filled with the above-mentioned catalyst. The catalyst is the same as that described above, so a detailed description thereof will be omitted.
[0113] The gas phase polyester discharged from the reactor is separated from the purification reactor or the crystallization reactor, and a polyester collection section may be included below the purification reactor or the crystallization reactor.
[0114] The reactor may include a first polymerization reactor and a second polymerization reactor, in which case the first polymerization reactor may be used as an esterification reactor and the second oxidation reactor may be used as a polycondensation reactor.
[0115] If necessary, the reactors may be configured such that the first polymerization reactor is used as a reactor for the first esterification reaction and the second esterification reaction, and the second polymerization reactor is used as a reactor for the condensation polymerization reaction.
[0116] As an example, the solution in which the dicarboxylic acid aromatic heterocyclic compound or its derivative is dissolved in the alkylene source material is supplied by the pressure difference between the reactor and the storage tank of the dicarboxylic acid aromatic heterocyclic compound or its derivative raw material, and the flow rate is adjusted using a valve to adjust the reaction time (residence time).
[0117] In addition, the solution that has passed through a column (e.g., a cylindrical column) in which the catalyst is fixedly packed as a reactor and has completed the reaction is transferred to a post-treatment reactor and stored in a collection vessel for purification and / or crystallization processes.
[0118] The polyester conversion solution stored in the collection vessel is discharged from the bottom, and the catalyst and polyester are separated to recover the polyester as a reaction product.
[0119] The starting material, dicarboxylic acid aromatic heterocyclic compound or its derivative, can be fed to the upper end of the reactor to maximize the reaction rate, but is not limited thereto.
[0120] In the reactor, the raw material, a solution of a dicarboxylic acid aromatic heterocyclic compound or its derivative, is contacted with a fixed phase catalyst in an inert atmosphere to cause an esterification reaction. At this time, the content of the raw material, a solution of a dicarboxylic acid aromatic heterocyclic compound or its derivative, which is automatically or semi-automatically fed into the reactor, can be controlled through a liquid mass feeder and a control valve provided at the upper end of the reactor.
[0121] In addition, the storage tank for the raw material dicarboxylic acid aromatic heterocyclic compound or its derivative is filled with the dicarboxylic acid aromatic heterocyclic compound or its derivative dissolved in the alkylene-providing raw material described above, or the dicarboxylic acid aromatic heterocyclic compound or its derivative alone, at a concentration of, for example, 0.5 to 10.0% by weight or 0.5 to 5.0% by weight.
[0122] In the case where the dicarboxylic acid aromatic heterocyclic compound or its derivative is charged alone, the alkylene providing material supplied from the alkylene providing material supply tank may be supplied to a pipe connecting the storage tank for the dicarboxylic acid aromatic heterocyclic compound or its derivative with the reactor to adjust the concentration to the above-mentioned range.
[0123] The catalyst to be filled in the reactor is prepared to include the catalyst according to the first aspect described above.
[0124] In a specific example, the catalyst is packed in a vertically installed tubular reactor. In this case, when an esterification reactor and a polycondensation reactor are present, the catalyst is packed in the tubular reactor for the esterification reactor.
[0125] After loading, the reactor temperature is kept at 100 to 500°C and a vacuum is maintained, adsorbed impurities are removed, and the catalyst is loaded into the reactor.
[0126] The reactor (corresponding to a tower filled with a catalyst) is adjusted to a range of 1 to 10 bar, and below 1 bar the reaction rate decreases, and above 10 bar the reaction rate increases only slightly. Therefore, the optimum pressure is 2 to 4 bar.
[0127] The reaction temperature in the reactor is in the range of 40 to 260°C. Below 40°C, the reaction rate is slow, and above 260°C, adsorption on the catalyst surface decreases, decreasing reactivity. The optimal condition is 40 to 250°C.
[0128] A solution of a dicarboxylic acid aromatic heterocyclic compound or its derivative is supplied to the top of the reactor (a catalyst packed tower) using a liquid mass supply device. The supplied solution of a dicarboxylic acid aromatic heterocyclic compound or its derivative flows to the bottom of the reactor by gravity and reacts with the catalyst to carry out an esterification reaction.
[0129] The esterification reaction product can be separated from the unreacted alkylene-providing raw material by a method commonly used in the production process of ordinary chemical products.
[0130] In addition, the reaction product can be subjected to a vacuum treatment while heating it under specific temperature conditions to volatilize an excess amount of unreacted alkylene-providing raw material, thereby recovering a high-purity product.
[0131] According to the method of the present invention, the reaction can be carried out under appropriate conditions using the optimal raw materials and catalyst to provide the desired product, so that the trade-off between thermal discoloration and molecular weight can be effectively eliminated without the need for separate additives such as heat stabilizers or antioxidants, and the desired reaction product can be produced. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0132] The present invention will be described below with reference to examples. However, the following examples were carried out under limited reaction times and conditions in order to illustrate the present invention, and the scope of the present invention is not limited thereto.
[0133] <Example> <Examples 1-1 to 1-6, Comparative Example 1-1> A catalyst (Sigma Aldrich product) having the structure shown in Table 1 below was added in a 2L Autoclave reactor according to the amount, and an esterification reaction was carried out with 428 g of a dicarboxylic acid aromatic heterocyclic compound or its derivative (Sigma Aldrich product) represented by the following chemical formula 4 and 283 g of ethylene glycol (Sigma Aldrich product) in a nitrogen atmosphere at a temperature of 150 to 240°C and a pressure of 1 to 6 bar.
[0134] [Chemical formula 4] JPEG0007555485000026.jpg2760
[0135] The required time and theoretical effluent water content as a function of catalyst content were ascertained.
[0136] Next, pressure was applied to the mixture to complete the reaction, and then condensation polymerization reaction was started at a temperature of 230 to 285° C. under vacuum for 5 hours to obtain polyester.
[0137] [Table 1]
[0138] <Comparative Examples 1-2 and 1-3> As Comparative Example 1-2, a catalyst (Sigma Aldrich product) having the structure shown in Table 2 below was added to a 2L Autoclave reactor in the respective amounts, and an esterification reaction was carried out with 428 g of the dicarboxylic acid aromatic heterocyclic compound represented by the chemical formula 4 or its derivative and 283 g of ethylene glycol in a nitrogen atmosphere at a temperature of 150 to 240°C and a pressure of 1 to 6 bar.
[0139] In addition, as Comparative Example 1-3, a catalyst (Sigma Aldrich product) having the structure shown in Table 2 below was added to a 2L size Autoclave reactor in the respective amounts, and an esterification reaction was carried out with 428 g of a dicarboxylic acid aromatic heterocyclic compound or its derivative represented by the following chemical formula 4 and 283 g of ethylene glycol under a nitrogen atmosphere at a temperature of 150 to 240°C and a pressure of 1 to 6 bar.
[0140] The required time and theoretical effluent water content as a function of catalyst content were ascertained.
[0141] Next, pressure was increased to normal pressure to terminate the reaction, and then a thermal stabilizer (TEP, triethylphosphate, Sigma-Aldrich product) shown in Table 2 below was added, and a condensation polymerization reaction was started at a temperature of 230 to 285°C under vacuum for 5 hours to obtain polyester.
[0142] The required time and theoretical effluent water content as a function of catalyst content were ascertained.
[0143] Next, pressure was increased to normal pressure to terminate the reaction, and then condensation polymerization reaction was started at a temperature of 230 to 285° C. under vacuum for 5 hours to obtain polyester.
[0144] [Table 2]
[0145] <Physical property evaluation> 1) Tg measurement: Tg was measured using a TA Instruments DSC under conditions of N2, 20 psi, room temperature to 300°C at 20°C / min.
[0146] 2) L / a / b measurement: The L / a / b values were measured using a chip color difference meter made by Nippon Denshoku (sa-4000).
[0147] 3) IV measurement: 2 g of a sample was dissolved in 25 ml of a solvent, phenol / tetrachloroethane, and the IV was measured using an Oswald viscometer.
[0148] 4) DEG content measurement: The DEG content was measured using an Agilent GC-MS with a column Rtx-5MS (0.25 μm×0.25 mm×30 m) and expressed in % units.
[0149] 5) Measurement of terminal COOH group content: After pretreatment at 100°C using a Metrohm product, the content was analyzed at room temperature and expressed in meq / kg units.
[0150] 6) Moisture content measurement: The moisture content was measured by heating to 160°C using a Metrohm product and expressed in ppm units.
[0151] <Experimental Example 1> The polyesters obtained in Examples 1-1 to 1-6 and Comparative Examples 1-1 to 1-3 were measured for Tg, L / a / b, IV, DEG content, terminal COOH group content, and water content, and the results are shown in Table 3 below.
[0152] [Table 3]
[0153] As shown in Table 3, in Examples 1-1 to 1-4, in which a catalyst represented by Chemical Formula 1, c / e of 18, and viscosity measured at 25°C of 0.97, a catalyst represented by Chemical Formula 2, c / e of 11, and viscosity measured at 25°C of 0.94, or a catalyst represented by Chemical Formula 3, c / e of 8, and viscosity measured at 25°C of 0.94 were used in an appropriate amount range of more than 5 ppm to less than 300 ppm, the obtained polyester had an intrinsic viscosity (IV) of 0.591 to 0.680, an L value of 45.1 to 47.5, an a value of 1.7 to 1.8, and a b value of 10.7 to 11.8 measured by a color difference meter, and thus the trade-off problem between molecular weight and thermal discoloration was solved.
[0154] Additionally, the Tg of the polyester was measured to be 84.9-85.7°C, the DEG to be 1.47%-2.23%, the COOH end groups to be 10-12 meq / kg, and the moisture content to be 7123-7486 ppm.
[0155] Meanwhile, in Comparative Example 1-1, where the catalyst was not added at 0 ppm, condensation polymerization did not occur, and the molecular weight was at the level of oligomer, and it was confirmed that thermal discoloration occurred during the condensation polymerization process due to the low molecular weight.In addition, in Example 1-5 or Example 1-6, where the catalyst was added in an excess amount of 300 ppm, the intrinsic viscosity (IV) was improved to 0.665 and 0.692, respectively, but the results were poor in terms of color such as L value, a value, and b value.
[0156] As a result, it was confirmed that when the catalyst having the structure of Chemical Formula 1 is used in a content range of more than 5 ppm to less than 300 ppm, it is suitable for solving the trade-off problem between molecular weight and thermal discoloration.
[0157] Furthermore, in Comparative Example 1-2, in which a catalyst represented by chemical formula 4, having a c / e of 4 and a specific gravity of 1.0 measured at 25°C, was used in an appropriate amount of more than 5 ppm to less than 300 ppm, the obtained polyester had an intrinsic viscosity (IV) of 0.62, which was relatively low compared to the Examples, and also showed poor results in terms of color such as L value, a value, and b value.
[0158] As a result, it was confirmed that in the case of a catalyst including the structure of Chemical Formula 4, the use of the appropriate range is inappropriate.
[0159] In addition, in Comparative Example 1-3, a heat stabilizer was added to the condensation polymerization process in Comparative Example 1-2, which used a catalyst represented by Chemical Formula 4, with a c / e of 4 and a specific gravity of 1.0 measured at 25°C, in an appropriate amount of more than 5 ppm to less than 300 ppm. The intrinsic viscosity (IV) of the resulting polyester was 0.50, which was relatively low compared to the Examples, but the color value was greatly improved by adding the heat stabilizer.
[0160] As a result, it was confirmed that in the case of a catalyst having the structure of Chemical Formula 4, thermal discoloration can be prevented only by adding an additive such as a heat stabilizer to the polycondensation process.
[0161] <Experimental Example 2> The polyesters obtained in Examples 1-1 to 1-6 and Comparative Examples 1-1 to 1-3 were measured for IV (25°C), IV (35°C), color difference meter in chip state (L / a / b), color difference meter in solution state (L / a / b), and Tg, and the results are shown in Table 4 below.
[0162] Table 4 also shows the difference (ΔIV) in intrinsic viscosity measured at 25° C. and 35° C., and the values calculated according to the following Equations 1 and 2.
[0163] <Formula 1> JPEG0007555485000030.jpg2246
[0164] <Formula 2> JPEG0007555485000031.jpg2941
[0165] [Table 4]
[0166] 1) Solution colorimeter measurement method: 2 g of the synthesized polyester was dissolved in 20 ml of hexafluoroisopropanol (HFIP) (0.1 g / ml in HFIP), and then the solution was measured using a Konica Minolta CM-3700A product in a Tuartz cell designed specifically for solution colorimeter measurements.
[0167] From the results in Table 4, it was confirmed that the polyester according to the embodiment has a correlation calculation value (Equation 1) between the difference (ΔIV) between the intrinsic viscosity measured at normal pressure and 25°C and the intrinsic viscosity measured at normal pressure and 35°C, and the color purity (b value) in a chip state is 0.06 or more, the b value in a chip state is 12 or less, and the b value in a solution state is less than 7.12, and the ΔIV value relative to the b value is higher than that of the comparative example. Generally, the higher the molecular weight of the polyester obtained by the condensation polymerization process, the higher the color value (b value) due to thermal discoloration tends to be. However, in the case of the embodiment, it was confirmed that the color value (b value) was lower even though the ΔIV was higher than that of the comparative example, thereby resolving the trade-off relationship and confirming that a polymer without thermal discoloration and with a high molecular weight can be obtained.
[0168] On the other hand, for the polyester according to the comparative example, the calculated correlation value (Equation 1) between the difference (ΔIV) between the intrinsic viscosity measured at 25°C and the intrinsic viscosity measured at 35°C and the color purity (b value) in the chip state was calculated to be less than 0.5, indicating that the higher the molecular weight of the polyester obtained by the condensation polymerization process, the higher the color numerical value (b value).
[0169] In addition, from the results of Table 4, it was confirmed that the calculated correlation value (Equation 2) between the difference (ΔIV) between the intrinsic viscosity measured at normal pressure and 25°C and the intrinsic viscosity measured at normal pressure and 35°C, the color purity b value in the chip state, and the glass transition temperature of the polyester according to the embodiment was calculated to be 0.4 or more, and the ΔIV and Tg values relative to the b value were higher than those of the comparative example. This is because, generally, the higher the molecular weight (ΔIV) of the polyester due to the condensation polymerization process, the higher the color numerical value (b value) due to thermal discoloration tends to be, but in the case of the embodiment, a polyester with a higher ΔIV but lower color purity (b value) than the comparative example can be obtained, thereby eliminating the trade-off relationship.
[0170] The features, structures, effects, etc. exemplified in each of the above-described embodiments may be combined or modified in other embodiments by a person having ordinary skill in the art to which the embodiments pertain, and therefore such combinations and modifications should be interpreted as being included in the scope of the present invention. [Industrial Applicability]
[0171] The present invention relates to a novel catalyst material used for producing polyesters from dicarboxylic acid aromatic heterocyclic compounds or derivatives thereof, a method for producing polyesters using the same, and polyesters produced using the same. The catalyst for producing polyesters has the effect of providing physical properties in a trade-off relationship between thermal discoloration and molecular weight in polyesters without the addition of a heat stabilizer or antioxidant.
Claims
1. A catalyst for producing polyester, comprising: The catalyst has any one of the following structures of Formula 1 to Formula 3: The catalyst is a catalyst for producing polyester, which produces polyester by polymerizing a dicarboxylic acid aromatic heterocyclic compound having a structure represented by the following chemical formula 4 or 5, or a derivative thereof. [Chemical formula 1] [Chemical formula 2] [Chemical formula 3] [Chemical formula 4] [Chemical formula 5]
2. The catalyst for producing polyester according to claim 1, wherein the catalyst has a specific gravity measured at 25° C. of 0.94 to 0.
99.
3. 1. A process for producing a polyester by esterifying a dicarboxylic acid aromatic heterocyclic compound or a derivative thereof with an alkylene-providing feedstock in the presence of a catalyst to produce an ester product, followed by a condensation polymerization reaction, comprising the steps of: The catalyst is a catalyst for producing polyester according to claim 1 or 2, The dicarboxylic acid aromatic heterocyclic compound or its derivative includes a structure represented by the following Chemical Formula 4 or Chemical Formula 5. [Chemical formula 4] [Chemical formula 5]
4. The method of claim 3 , wherein the alkylene providing feedstock is an aliphatic diol or an aromatic diol.
5. The method for producing a polyester according to claim 3, wherein the alkylene-providing raw material is used in a molar ratio of 1.2 to 3.6 based on 1 mole of the dicarboxylic acid aromatic heterocyclic compound or its derivative represented by Chemical Formula 4 or Chemical Formula 5.
6. The method for producing polyester according to claim 3, wherein the esterification reaction is carried out by treating the dicarboxylic acid aromatic heterocyclic compound and the alkylene providing material under a nitrogen atmosphere at 150 to 240° C. and a pressure of 1 to 6 bar to obtain an ester product of the dicarboxylic acid aromatic heterocyclic compound or a derivative thereof.
7. The method for producing a polyester according to claim 3, wherein the condensation polymerization reaction is performed by condensing the ester product at 230 to 285° C. under reduced pressure conditions.
8. The method for producing polyester according to claim 3, wherein the amount of the catalyst used is more than 5 ppm and less than 300 ppm.
9. The repeat unit includes an ester bond between a dicarboxylic acid aromatic heterocyclic compound or a derivative thereof and an alkylene source material, The difference (ΔIV) between the intrinsic viscosity measured at 25° C. and the intrinsic viscosity measured at 35° C. is 0.06 or more, The b value is 12 or less in a Lab color difference meter. The dicarboxylic acid aromatic heterocyclic compound or its derivative is a polyester having a structure represented by the following formula 4 or 5: [Chemical formula 4] [Chemical formula 5]
10. 10. The polyester of claim 9, wherein the alkylene donor is an aliphatic diol or an aromatic diol.
11. The intrinsic viscosity measured at 25° C. is 0.5 or more, 10. The polyester according to claim 9, wherein the intrinsic viscosity measured at 35°C is 0.43 or more.
12. The polyester according to claim 9, which has a b value of less than 7.12 when measured in a solution state using a Lab color difference meter after dissolving 2 g of the polyester in 20 ml of hexafluoroisopropanol (HFIP) (0.1 g / ml in HFIP).
13. The polyester according to claim 9, wherein the value of the following mathematical formula 1 is 0.5 or more. <Formula 1> (In the above formula 1, ΔIV is the difference between the intrinsic viscosity values measured at 35° C. and 25° C., and the b value is the b value measured by a Lab color difference meter.)
14. The polyester according to claim 9, wherein the value of the following mathematical formula 2 is 0.4 or more. <Formula 2> (In the above formula 2, ΔIV is the difference between the intrinsic viscosity values measured at 35° C. and 25° C., the b value is the b value measured by a Lab color difference meter, and Tg is the glass transition temperature.)
Citation Information
Patent Citations
Double-bond-containing all-bio-based polyesters, and preparation method and application thereof
CN103483571A
Manufacture of polyester
JP1992234428A
Polyester composition and method for producing the same
JP2015160871A
Process for preparing poly(trimethylene furan dicarboxylate)
JP2019530787A
Method for the preparation of polyester by use of composite catalyst
US5714570A