Thermoplastic resin composition, molded article and product
A thermoplastic resin composition with a hydrophilic copolymer and fatty acid metal salt addresses the adhesion of hydrophilic and hydrophobic dust stains, ensuring effective antifouling and improved mechanical strength while facilitating lower-temperature processing.
Patent Information
- Application Number
- JP2023532900
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-07-05
- Publication Date
- 2024-09-24
- Estimated Expiration
- 2041-07-05
AI Technical Summary
Conventional antistatic agents for thermoplastic resin molded products are ineffective in preventing the adhesion of hydrophobic dust stains such as soot and oil smoke, and materials with high melting points complicate processing and may lead to material decomposition.
A thermoplastic resin composition incorporating an aromatic polycarbonate resin, styrene resin, aromatic polyester resin, polyphenylene ether resin, methacrylic resin, polyarylene sulfide resin, olefin resin, or polyamide resin, combined with a hydrophilic copolymer having oxyethylene groups and a fatty acid metal salt, which suppresses the adhesion of both hydrophilic and hydrophobic dust stains while maintaining a lower melting point for easier processing.
The composition effectively prevents the adhesion of both hydrophilic and hydrophobic dust stains while allowing for lower processing temperatures and reduced material decomposition, enhancing mechanical strength such as impact resistance.
Smart Images

Figure 0007555492000032 
Figure 0007555492000029 
Figure 0007555492000033
Abstract
Description
[Technical field]
[0001] The present disclosure relates to thermoplastic resin compositions, molded articles and manufactured articles. [Background technology]
[0002] Thermoplastic resins are lighter than metals and easier to process, so their molded products are used in a variety of applications and environments, such as internal parts for home appliances and office equipment, housings, vehicle parts, and miscellaneous goods.
[0003] Depending on the environment and method of use, molded products of these thermoplastic resins may become contaminated with dust such as sand, dirt, soot, and oily smoke. When dust adheres to a molded product, it deteriorates its appearance and may cause a deterioration in the performance of the product.
[0004] Therefore, in order to suppress the adhesion of dust stains, attempts have been made to impart antistatic properties to molded articles of thermoplastic resins by using antistatic agents.
[0005] For example, there is a known method of imparting antistatic properties to a molded article by attaching an antistatic agent to the surface of the molded article by spraying, dipping, coating, etc. However, in the method of attaching an antistatic agent to the surface of a molded article, since most of the antistatic agents are water-soluble surfactants, the antistatic agent is removed by wiping, washing, etc., resulting in the loss of antistatic properties.
[0006] On the other hand, a method (kneading method) is also known in which antistatic properties are imparted to molded thermoplastic resin products by blending an antistatic agent as an additive to the thermoplastic resin. This kneading method has been attracting attention in recent years because of its long-lasting antistatic effect.
[0007] Various compounds are known as antistatic agents used in the kneading method. For example, Patent Document 1 (JP Patent Publication No. 2011-256293) discloses a fatty acid amide compound of aminoethylethanolamine. Patent Document 2 (JP Patent Publication No. 58-118838) and Patent Document 3 (JP Patent Publication No. 3-290464) disclose polyether ester amide. Patent Document 4 (JP Patent Publication No. 2001-278985), Patent Document 5 (WO 2014 / 115745) and Patent Document 6 (WO 2014 / 148454) disclose block copolymers composed of olefin blocks and hydrophilic polymer blocks, and Patent Documents 5 and 6 disclose polyether ester polymer-type antistatic agents.
[0008] Patent Document 1 discloses the use of an alkali metal compound, an alkaline earth metal compound (e.g., calcium stearate) in combination with an aminoethylethanolamine fatty acid amide compound to improve the antistatic effect. Patent Document 4 discloses the use of an alkali metal compound, such as lithium chloride, potassium acetate, or sodium dodecylbenzenesulfonate in combination with an olefin block and a hydrophilic polymer block to improve the antistatic effect of a block copolymer. Patent Documents 5 and 6 disclose the use of an alkali metal compound, such as potassium acetate or sodium dodecylbenzenesulfonate, in a polyetherester polymer-based antistatic agent.
[0009] However, although all of the above antistatic agents have a certain degree of effect in suppressing the adhesion of hydrophilic dust stains such as sand dust and dirt, almost no effect of suppressing the adhesion of hydrophobic dust stains such as soot and oily smoke was observed. Therefore, Patent Document 7 (International Publication No. 2021 / 006192) discloses a resin composition to which both hydrophilic dust stains and hydrophobic dust stains are difficult to adhere. [Prior art documents] [Patent documents]
[0010] [Patent Document 1] JP 2011-256293 A [Patent Document 2] Japanese Patent Application Publication No. 58-118838 [Patent Document 3] Japanese Patent Application Publication No. 3-290464 [Patent Document 4] JP 2001-278985 A [Patent Document 5] International Publication No. 2014 / 115745 [Patent Document 6] International Publication No. 2014 / 148454 [Patent Document 7] International Publication No. 2021 / 006192 Summary of the Invention [Problem to be solved by the invention]
[0011] However, in the resin composition of Patent Document 7, B1 (olefin skeleton, melting point: about 130 to 140°C) and B2 (polyamide skeleton, melting point: about 195 to 200°C), which are specifically disclosed as the hydrophilic copolymer (B) having a polyoxyethylene chain, have high melting points and are therefore not suitable for low-temperature processes. In addition, they may become difficult to process, or may require longer times for processing, kneading, etc. This may also lead to the decomposition of other materials.
[0012] Therefore, an object of the present disclosure is to provide a resin composition that is resistant to both hydrophilic and hydrophobic dust stains, by using a material that has a lower melting point than conventional materials. [Means for solving the problem]
[0013] As a result of their investigations, the inventors have found that even when using a hydrophilic copolymer (B) having a lower melting point than the "hydrophilic copolymer formed by repeatedly and alternately bonding a polyolefin and a hydrophilic polymer having a polyoxyethylene chain" (B1) and "polyether ester amide" (B2) disclosed in International Publication No. 2021 / 006192 (Patent Document 7) as such a hydrophilic copolymer, it is possible to provide a resin composition that is resistant to both hydrophilic dust stains and hydrophobic dust stains.
[0014] The thermoplastic resin composition of the present disclosure comprises: A thermoplastic resin (A) selected from the group consisting of an aromatic polycarbonate resin (A1), a styrene-based resin (A2), an aromatic polyester resin (A3), a polyphenylene ether-based resin (A4), a methacrylic resin (A5), a polyarylene sulfide resin (A6), an olefin-based resin (A7), a polyamide resin (A8), and mixtures thereof; a hydrophilic copolymer (B) having an oxyethylene group; and a fatty acid metal salt (C) represented by the following formula (1):
[0015] M(OH)y(R-COO)x (1) (In formula (1), R is an alkyl or alkenyl group having 6 to 40 carbon atoms. M is at least one metal element selected from the group consisting of aluminum, zinc, calcium, magnesium, lithium, and barium. x and y are each independent integers of 0 or more, and satisfy the relationship x+y=[valence of M].) The hydrophilic copolymer (B) is formed by bonding a plurality of alternating copolymers (a) of polyester (a1) and hydrophilic polymer (a2) having an oxyethylene group via ester bonds with at least one compound selected from the group consisting of polyhydric alcohol compounds (b1) having three or more hydroxyl groups, epoxy compounds (b2) having two or more epoxy groups, and polycarboxylic acid compounds (b3). Effect of the Invention
[0016] According to the present disclosure, by blending the above-mentioned hydrophilic copolymer (B) and fatty acid metal salt (C) with the thermoplastic resin (A), it is possible to suppress adhesion of both hydrophilic dust stains and hydrophobic dust stains to a molded article containing the thermoplastic resin composition. Therefore, it is possible to provide a resin composition that is difficult to attract both hydrophilic dust stains and hydrophobic dust stains by using a material with a lower melting point than conventional materials. [Brief description of the drawings]
[0017] [Figure 1] FIG. 6 is a schematic cross-sectional view showing an example of a molded product according to a second embodiment. [Diagram 2] 10 is a schematic graph showing a composition distribution in the depth direction for an example of a molded article according to the second embodiment. [Diagram 3] FIG. 1 is a conceptual diagram for explaining a thermoplastic resin composition according to an embodiment. [Figure 4] FIG. 1 is a conceptual diagram for explaining a thermoplastic resin composition according to an embodiment. [Diagram 5] FIG. 11 is a cross-sectional schematic diagram showing an example of an air conditioner according to embodiment 3. [Figure 6] FIG. 1 is a conceptual diagram for explaining a thermoplastic resin composition according to an embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0018] Hereinafter, embodiments of the present disclosure will be described. In the drawings, dimensional relationships such as length, width, thickness, and depth are appropriately changed for clarity and simplification of the drawings, and do not represent actual dimensional relationships.
[0019] Embodiment 1 The thermoplastic resin composition of the present embodiment is A thermoplastic resin (A) selected from the group consisting of an aromatic polycarbonate resin (A1), a styrene-based resin (A2), an aromatic polyester resin (A3), a polyphenylene ether-based resin (A4), a methacrylic resin (A5), a polyarylene sulfide resin (A6), an olefin-based resin (A7), a polyamide resin (A8), and mixtures thereof; a hydrophilic copolymer (B) having an oxyethylene group; and a fatty acid metal salt (C).
[0020] A molded article containing the thermoplastic resin composition of the present embodiment exhibits a remarkable antifouling effect in which adhesion of both hydrophilic and hydrophobic dust stains is suppressed. Note that this effect is exhibited by a thermoplastic resin composition containing all of the above components (A) to (C), and it is difficult to obtain such a remarkable antifouling effect with only component (A), only component (B), only component (C), only components (A) and (B), only components (A) and (C), or only components (B) and (C).
[0021] Furthermore, as the hydrophilic copolymer (B), a hydrophilic copolymer is used in which a plurality of alternating copolymers (a) of a polyester (a1) and a hydrophilic polymer (a2) having an oxyethylene group (which are repeatedly and alternately bonded together) are bonded via ester bonds to at least one compound selected from the group consisting of a polyhydric alcohol compound (b1) having three or more hydroxyl groups, an epoxy compound (b2) having two or more epoxy groups, and a polycarboxylic acid compound (b3).
[0022] This makes it possible to use a material having a lower melting point than conventional materials as the hydrophilic copolymer (B), thereby suppressing the production of a resin composition to which both hydrophilic and hydrophobic dust stains are resistant to adhesion.
[0023] In addition, a molded article containing the thermoplastic resin composition of the present embodiment can also have good mechanical strength such as impact resistance.
[0024] <Thermoplastic resin (A)> The thermoplastic resin (A) is selected from the group consisting of aromatic polycarbonate resins (A1), styrene-based resins (A2), aromatic polyester resins (A3), polyphenylene ether-based resins (A4), methacrylic resins (A5), polyarylene sulfide resins (A6), olefin-based resins (A7), polyamide resins (A8), and mixtures thereof.
[0025] Examples of the above mixture, that is, a mixture of at least two resins selected from the aromatic polycarbonate resin (A1), the styrene-based resin (A2), the aromatic polyester resin (A3), the polyphenylene ether-based resin (A4), the methacrylic resin (A5), the polyarylene sulfide resin (A6), the olefin-based resin (A7), and the polyamide resin (A8), are not particularly limited, but include, for example, a mixture of an aromatic polycarbonate resin (A1) and a styrene-based resin (A2), an aromatic polycarbonate resin (A1) and an aromatic polyester resin (A3), an aromatic polycarbonate resin (A4), a methacrylic resin (A5), a polyarylene sulfide resin (A6), an olefin-based resin (A7), and a polyamide resin (A8), Examples of combinations include combinations of a carbonate resin (A1) and an olefin resin (A7), an aromatic polycarbonate resin (A1) and a methacrylic resin (A5), a styrene resin (A2) and an aromatic polyester resin (A3), a styrene resin (A2) and a methacrylic resin (A5), a styrene resin (A2) and an olefin resin (A7), a styrene resin (A2) and a polyamide resin (A8), a polyphenylene ether resin (A4) and an olefin resin (A7), a methacrylic resin (A5) and an olefin resin (A7), and an olefin resin (A7) and a polyamide resin (A8).
[0026] The melting point of the thermoplastic resin (A) is, for example, 150 to 270°C, and preferably 160 to 230°C.
[0027] (Aromatic polycarbonate resin (A1)) The aromatic polycarbonate resin (A1) is usually obtained by reacting a dihydroxy compound with a carbonate precursor by an interfacial polycondensation method or a melt transesterification method, or by polymerizing a carbonate prepolymer by a solid-phase transesterification method, or by polymerizing a cyclic carbonate compound by a ring-opening polymerization method.
[0028] The dihydroxy component used here may be any dihydroxy component that is usually used as a dihydroxy component in aromatic polycarbonates, and may be a bisphenol or an aliphatic diol.
[0029] Examples of bisphenols include 4,4'-dihydroxybiphenyl, bis(4-hydroxyphenyl)methane, 1,1-bis(4-hydroxyphenyl)ethane, 1,1-bis(4-hydroxyphenyl)-1-phenylethane, 2,2-bis(4-hydroxyphenyl)propane, 2,2-bis(4-hydroxy-3-methylphenyl)propane, 1,1-bis(4-hydroxyphenyl)-3,3,5-trimethylcyclohexane, 2,2-bis(4-hydroxy-3,3'-biphenyl)propane, 2,2-bis(4-hydroxyphenyl)methane ... -3-isopropylphenyl)propane, 2,2-bis(3-t-butyl-4-hydroxyphenyl)propane, 2,2-bis(4-hydroxyphenyl)butane, 2,2-bis(4-hydroxyphenyl)octane, 2,2-bis(3-bromo-4-hydroxyphenyl)propane, 2,2-bis(3,5-dimethyl-4-hydroxyphenyl)propane, 2,2-bis(3-cyclohexyl-4-hydroxyphenyl)propane, 1,1-bis(3-cyclohexyl-4-hydroxyphenyl)cyclohexane, bis(4-hydroxyphenyl)propane, 4,4'-dihydroxydiphenyl ether, 4,4'-dihydroxy-3,3'-dimethyldiphenyl ether, 4,4'-sulfonyldiphenol, 4,4'-dihydroxydiphenyl sulfoxide, 4,4'-dihydroxydiphenyl sulfide, 2,2'-dimethyl 4,4'-dihydroxy-3,3'-dimethyldiphenyl sulfoxide, 4,4'-hydroxy-3,3'-dimethyldiphenyl sulfide, 2,2'-diphenyl-4,4'-sulfonyldiphenol, 4,4'-dihydroxy-3,3'-diphenyldiphenyl sulfoxide, 4,4'-dihydroxy-3,3'-diphenyldiphenyl sulfide, 1,3-bis{2-(4-hydroxyphenyl)propyl}benzene, 1,4-bis{2-(4-hydroxyphenyl)propyl}benzene, 1,Examples of the 4-bis(4-hydroxyphenyl)cyclohexane include 4,8-bis(4-hydroxyphenyl)tricyclo[5,2,1,02,6]decane, 4,4'-(1,3-adamantanediyl)diphenol, 1,3-bis(4-hydroxyphenyl)-5,7-dimethyladamantane, and the like.
[0030] Examples of aliphatic diols include 2,2-bis-(4-hydroxycyclohexyl)-propane, 1,1,4-tetradecanediol, octaethylene glycol, 1,1,6-hexadecanediol, 4,4'-bis(2-hydroxyethoxy)biphenyl, bis{(2-hydroxyethoxy)phenyl}methane, 1,1-bis{(2-hydroxyethoxy)phenyl}ethane, 1,1-bis{(2-hydroxyethoxy)phenyl}-1-phenylethane, 2,2-bis{(2-hydroxyethoxy)phenyl}propane, 2,2-bis{(2-hydroxy 2,2-bis{4-(2-hydroxyethoxy)-3-methylphenyl}propane, 1,1-bis{(2-hydroxyethoxy)phenyl}-3,3,5-trimethylcyclohexane, 2,2-bis{4-(2-hydroxyethoxy)-3,3'-biphenyl}propane, 2,2-bis{(2-hydroxyethoxy)-3-isopropylphenyl}propane, 2,2-bis{3-t-butyl-4-(2-hydroxyethoxy)phenyl}propane, 2,2-bis{(2-hydroxyethoxy)phenyl}butane, 2,2-bis{(2-hydroxyethoxy)phenyl}-4-methylpentane 2,2-bis{(2-hydroxyethoxy)phenyl}octane, 1,1-bis{(2-hydroxyethoxy)phenyl}decane, 2,2-bis{3-bromo-4-(2-hydroxyethoxy)phenyl}propane, 2,2-bis{3,5-dimethyl-4-(2-hydroxyethoxy)phenyl}propane, 2,2-bis{3-cyclohexyl-4-(2-hydroxyethoxyphenylpropane, 1,1-bis{3-cyclohexyl-4-(2-hydroxyethoxy)phenyl}cyclohexane, bis{(2-hydroxyethoxy)phenyl}diphenyl fluorene, 9,9-bis{(2-hydroxyethoxy)phenyl}fluorene, 9,9-bis{4-(2-hydroxyethoxy)-3-methylphenyl}fluorene, 1,1-bis{(2-hydroxyethoxy)phenyl}cyclohexane, 1,1-bis{(2-hydroxyethoxy)phenyl}cyclopentane, 4,4'-bis(2-hydroxyethoxy)diphenyl ether, 4,4'-bis(2-hydroxyethoxy)-3,3'-dimethyldiphenyl ether, 1,3-bis[2-{(2-hydroxyethoxy)phenyl}propyl]benzene, 1,Examples of such compounds include 4-bis[2-{(2-hydroxyethoxy)phenyl}propyl]benzene, 1,4-bis{(2-hydroxyethoxy)phenyl}cyclohexane, 1,3-bis{(2-hydroxyethoxy)phenyl}cyclohexane, 4,8-bis{(2-hydroxyethoxy)phenyl}tricyclo[5,2,1,02,6]decane, 1,3-bis{(2-hydroxyethoxy)phenyl}-5,7-dimethyladamantane, 3,9-bis(2-hydroxy-1,1-dimethylethyl)-2,4,8,10-tetraoxaspiro(5,5)undecane, 1,4:3,6-dianhydro-D-sorbitol (isosorbide), 1,4:3,6-dianhydro-D-mannitol (isomannide), and 1,4:3,6-dianhydro-L-iditol (isoidide).
[0031] Among these, aromatic bisphenols are preferred, and among these, 1,1-bis(4-hydroxyphenyl)-1-phenylethane, 2,2-bis(4-hydroxyphenyl)propane, 2,2-bis(4-hydroxy-3-methylphenyl)propane, 1,1-bis(4-hydroxyphenyl)cyclohexane, 1,1-bis(4-hydroxyphenyl)-3,3,5-trimethylcyclohexane, 4,4'-sulfonyldiphenol, 2,2'-dimethyl-4,4'-sulfonyldiphenol, 9,9-bis(4-hydroxy-3-methylphenyl)fluorene, 1,3-bis{2-(4-hydroxyphenyl)propyl}benzene, and 1,4-bis{2-(4-hydroxyphenyl)propyl}benzene are preferred, and 2,2-bis(4-hydroxyphenyl)propane, 1,1-bis(4-hydroxyphenyl)cyclohexane, 4,4'-sulfonyldiphenol, and 9,9-bis(4-hydroxy-3-methylphenyl)fluorene are particularly preferred. Among these, 2,2-bis(4-hydroxyphenyl)propane is the most suitable because of its excellent strength and good durability. These may be used alone or in combination of two or more kinds.
[0032] The aromatic polycarbonate resin (A1) may be a branched polycarbonate resin obtained by using a branching agent in combination with the above-mentioned dihydroxy compound.
[0033] Examples of the trifunctional or higher polyfunctional aromatic compound used in such a branched polycarbonate resin include phloroglucine, phloroglucide, 4,6-dimethyl-2,4,6-tris(4-hydroxyphenyl)heptene-2,2,4,6-trimethyl-2,4,6-tris(4-hydroxyphenyl)heptane, 1,3,5-tris(4-hydroxyphenyl)benzene, 1,1,1-tris(4-hydroxyphenyl)ethane, 1,1,1-tris(3,5-dimethyl-4-hydroxyphenyl)ethane, 2, Examples of the trisphenols include 6-bis(2-hydroxy-5-methylbenzyl)-4-methylphenol, 4-{4-[1,1-bis(4-hydroxyphenyl)ethyl]benzene}-α,α-dimethylbenzylphenol, tetra(4-hydroxyphenyl)methane, bis(2,4-dihydroxyphenyl)ketone, 1,4-bis(4,4-dihydroxytriphenylmethyl)benzene, trimellitic acid, pyromellitic acid, benzophenonetetracarboxylic acid, and acid chlorides thereof. Among these, 1,1,1-tris(4-hydroxyphenyl)ethane and 1,1,1-tris(3,5-dimethyl-4-hydroxyphenyl)ethane are preferred, and 1,1,1-tris(4-hydroxyphenyl)ethane is particularly preferred.
[0034] These aromatic polycarbonate resins are produced by a reaction means known per se for producing ordinary aromatic polycarbonate resins, for example, a method of reacting an aromatic dihydroxy component with a carbonate precursor such as phosgene or a carbonic acid diester. The basic means for the production method will be briefly described below.
[0035] In a reaction using, for example, phosgene as a carbonate precursor, the reaction is usually carried out in the presence of an acid binder and a solvent. As the acid binder, for example, an alkali metal hydroxide such as sodium hydroxide or potassium hydroxide, or an amine compound such as pyridine is used. As the solvent, for example, a halogenated hydrocarbon such as methylene chloride or chlorobenzene is used. In addition, a catalyst such as a tertiary amine or a quaternary ammonium salt can be used to promote the reaction. In this case, the reaction temperature is usually 0 to 40°C, and the reaction time is several minutes to 5 hours.
[0036] The transesterification reaction using a carbonic acid diester as a carbonate precursor is carried out by heating and stirring an aromatic dihydroxy component with a carbonic acid diester under an inert gas atmosphere, and distilling off the resulting alcohol or phenol. The reaction temperature varies depending on the boiling point of the resulting alcohol or phenol, but is usually in the range of 120 to 300°C. The reaction is completed by reducing the pressure from the beginning of the reaction to distill off the resulting alcohol or phenol. In addition, a catalyst usually used in transesterification reactions can be used to promote the reaction.
[0037] Examples of the carbonic acid diester used in the above-mentioned transesterification reaction include diphenyl carbonate, dinaphthyl carbonate, bis(diphenyl) carbonate, dimethyl carbonate, diethyl carbonate, dibutyl carbonate, etc. Among these, diphenyl carbonate is particularly preferred.
[0038] In the present disclosure, a terminal terminator can be used in the polymerization reaction. The terminal terminator is used to adjust the molecular weight, and the obtained aromatic polycarbonate resin has excellent thermal stability compared to those not having the terminals blocked, since the terminals are blocked. Examples of such terminal terminators include monofunctional phenols represented by the following formulas (2) to (4).
[0039] [ka]
[0040] [In formula (2), A is a hydrogen atom, an alkyl group having 1 to 9 carbon atoms, an alkylphenyl group (the alkyl portion has 1 to 9 carbon atoms), a phenyl group, or a phenylalkyl group (the alkyl portion has 1 to 9 carbon atoms), and r is an integer of 1 to 5 (preferably 1 to 3)].
[0041] [ka]
[0042] [ka]
[0043] [In formula (3) and formula (4), X is -RO-, -R-CO-O- or -RO-CO-, where R represents a single bond or a divalent aliphatic hydrocarbon group having 1 to 10 carbon atoms (preferably 1 to 5), and n represents an integer of 10 to 50.] Specific examples of the monofunctional phenols represented by the above formula (2) include phenol, isopropylphenol, p-tert-butylphenol, p-cresol, p-cumylphenol, 2-phenylphenol, 4-phenylphenol, and isooctylphenol.
[0044] Moreover, the monofunctional phenols represented by the above formulas (3) to (4) are phenols having a long-chain alkyl group or an aliphatic ester group as a substituent. When the terminals of an aromatic polycarbonate resin are blocked with these phenols, they not only function as a terminal terminator or a molecular weight regulator, but also improve the melt flowability of the resin, facilitating molding, and have the effect of lowering the water absorption rate of the resin, so that these phenols are preferably used.
[0045] As the substituted phenols of the above formula (3), those in which n is 10 to 30, particularly 10 to 26, are preferred, and specific examples thereof include decylphenol, dodecylphenol, tetradecylphenol, hexadecylphenol, octadecylphenol, eicosylphenol, docosylphenol, and triacontylphenol.
[0046] As the substituted phenol of the above formula (4), a compound in which X is -R-CO-O- and R is a single bond is suitable, and n is preferably 10 to 30, particularly preferably 10 to 26. Specific examples thereof include decyl hydroxybenzoate, dodecyl hydroxybenzoate, tetradecyl hydroxybenzoate, hexadecyl hydroxybenzoate, eicosyl hydroxybenzoate, docosyl hydroxybenzoate, and tricontyl hydroxybenzoate.
[0047] Among these monofunctional phenols, the monofunctional phenols represented by the above formula (2) are preferred, alkyl- or phenylalkyl-substituted phenols are more preferred, and p-tert-butylphenol, p-cumylphenol or 2-phenylphenol is particularly preferred.
[0048] It is desirable that the terminal terminator of these monofunctional phenols is introduced into the terminals in an amount of at least 5 mol %, and preferably at least 10 mol %, based on the total terminals of the obtained aromatic polycarbonate resin. The terminal terminator may be used alone or in combination of two or more kinds.
[0049] The aromatic polycarbonate resin (A1) may be a polyester carbonate copolymerized with an aromatic dicarboxylic acid, such as terephthalic acid, isophthalic acid, naphthalenedicarboxylic acid, or a derivative thereof, within the scope of the present disclosure.
[0050] The viscosity average molecular weight of the aromatic polycarbonate resin (A1) is not limited. However, if the viscosity average molecular weight is less than 10,000, the strength and the like decrease, and if it exceeds 50,000, the molding processability decreases, so the range of 10,000 to 50,000 is preferable, the range of 12,000 to 30,000 is more preferable, and the range of 15,000 to 28,000 is even more preferable. In addition, the viscosity average molecular weight in the present disclosure is calculated by first calculating the specific viscosity calculated by the following formula using an Ostwald viscometer from a solution in which 0.7 g of the aromatic polycarbonate resin is dissolved in 100 mL of methylene chloride at 20°C, and then inserting the calculated specific viscosity into the following formula to calculate the viscosity average molecular weight Mv.
[0051] Specific viscosity (η SP )=(t-t0) / t0 [t0 is the number of seconds that methylene chloride falls, and t is the number of seconds that the sample solution falls] η SP / c=[η]+0.45×[η] 2c (where [η] is the intrinsic viscosity) [η]=1.23×10 -4 Mv 0.83 c=0.7 The aromatic polycarbonate resin (A1) has a total chlorine content of preferably 0 to 200 ppm, more preferably 0 to 150 ppm. If the total chlorine content in the aromatic polycarbonate resin exceeds 200 ppm, the color and thermal stability are undesirably deteriorated.
[0052] (Styrene-based resin (A2)) Examples of the main component of the styrene-based resin (A2) in this embodiment include polystyrene resin (PS), high impact polystyrene resin (HIPS), copolymers of alkyl (meth)acrylate monomers and aromatic vinyl monomers (MS), copolymers of cyanide vinyl compounds and aromatic vinyl compounds (AS), copolymers of cyanide vinyl compounds and aromatic vinyl compounds containing diene rubber components (ABS), copolymers of cyanide vinyl compounds and aromatic vinyl compounds containing ethylene-α-olefin rubber components (AES), copolymers of cyanide vinyl compounds and aromatic vinyl compounds containing acrylic rubber components (ASA), copolymers of alkyl (meth)acrylate monomers and aromatic vinyl compounds containing diene rubber components (MBS), copolymers of alkyl (meth)acrylate monomers and cyanide vinyl compounds containing diene rubber components (MABS), and copolymers of alkyl (meth)acrylate monomers and aromatic vinyl compounds containing acrylic rubber components (MAS).
[0053] The main component is the component that occupies the largest portion by mass, and the content of the main component in the styrene-based resin (A2) is preferably 90% by mass or more, and more preferably 95% by mass or more.
[0054] The styrene resin (A2) may be a resin having high stereoregularity, such as syndiotactic polystyrene, obtained by using a catalyst such as a metallocene catalyst during its production. The styrene resin (A2) may also be a polymer, copolymer, or block copolymer having a narrow molecular weight distribution, or a polymer or copolymer having high stereoregularity, obtained by a method such as anionic living polymerization or radical living polymerization.
[0055] Polystyrene resin (PS) is a polymer obtained by polymerizing at least one type of aromatic vinyl compound by a polymerization method such as solution polymerization, bulk polymerization, suspension polymerization, or bulk-suspension polymerization. Preferred aromatic vinyl compounds include, for example, styrene, α-methylstyrene, methylstyrene, ethylstyrene, isopropylstyrene, tertiary butylstyrene, and other alkylstyrenes, phenylstyrene, vinylstyrene, chlorostyrene, bromostyrene, fluorostyrene, chloromethylstyrene, methoxystyrene, and ethoxystyrene. These compounds may be used alone or in combination. Particularly preferred aromatic vinyl compounds among these are styrene, p-methylstyrene, m-methylstyrene, p-tertiary butylstyrene, p-chlorostyrene, m-chlorostyrene, and p-fluorostyrene, with styrene being particularly preferred.
[0056] The molecular weight of the polystyrene resin (PS) is not particularly limited, but the polystyrene-equivalent mass average molecular weight measured by GPC (gel permeation chromatography) at 135° C. using trichlorobenzene as a solvent is preferably 100,000 or more, more preferably 150,000 or more. There is no limitation on the width of the molecular weight distribution.
[0057] High impact polystyrene resin (HIPS) is a polymer in which a rubber-like polymer made of butadiene rubber or the like is dispersed in the form of particles in a matrix made of an aromatic vinyl polymer such as PS. HIPS can be obtained, for example, by dissolving a rubber-like polymer in a mixture of an aromatic vinyl monomer and an inert solvent, and stirring the mixture to carry out bulk polymerization, suspension polymerization, solution polymerization, or the like. HIPS may also be a mixture in which a polymer obtained by dissolving a rubber-like polymer in a mixture of an aromatic vinyl monomer and an inert solvent is mixed with an aromatic vinyl polymer obtained separately.
[0058] In the HIPS, the matrix portion made of an aromatic vinyl polymer is not particularly limited, but the mass average molecular weight in terms of polystyrene measured by GPC (gel permeation chromatography) at 135° C. using trichlorobenzene as a solvent is preferably 100,000 or more, more preferably 150,000 or more. The average particle size of the rubber-like polymer is not particularly limited, but is generally 0.4 to 6.0 μm.
[0059] As the aromatic vinyl monomer, styrene and its derivatives (e.g., o-methylstyrene, m-methylstyrene, p-methylstyrene, 2,4-dimethylstyrene, etc.) can be used, with styrene being the most suitable. Two or more of these monomers may be used in combination.
[0060] The rubber-like polymer may be polybutadiene, polyisoprene, styrene-butadiene copolymer, etc. Examples of polybutadiene include high-cis polybutadiene having a high content of cis bonds and low-cis polybutadiene having a low content of cis bonds.
[0061] Among these, polybutadiene containing 70% by mass or more of high cis polybutadiene rubber having 90% by mole or more of cis-1,4 bonds in 100% by mass of the rubber-like polymer is preferably used.
[0062] Specifically, in any of the rubber-modified styrene-based resin obtained by using only high-cis polybutadiene rubber, the rubber-modified styrene-based resin obtained by mixing high-cis polybutadiene rubber and low-cis polybutadiene rubber, or the mixture of the rubber-modified styrene-based resin obtained by using high-cis polybutadiene rubber and the rubber-modified styrene-based resin obtained by using low-cis polybutadiene rubber, it is preferable that the high-cis polybutadiene rubber is contained in 70% by mass or more of the rubber-like polymer present in the rubber-modified styrene-based resin in 100% by mass. Here, the high-cis polybutadiene rubber means, for example, a polybutadiene rubber containing cis-1,4 bonds at a ratio of 90 mol % or more. The low-cis polybutadiene rubber means, for example, a polybutadiene rubber having a 1,4-cis bond content of 10 to 40 mol %.
[0063] In the copolymer (MS) of an alkyl (meth)acrylate monomer and an aromatic vinyl monomer, the alkyl (meth)acrylate monomer is, for example, at least one monomer selected from methyl (meth)acrylate and phenyl (meth)acrylate. In particular, it is preferable to use methyl (meth)acrylate. The term "(meth)acrylate" includes both methacrylate and acrylate.
[0064] Examples of the aromatic vinyl monomer that can be used include styrene, α-methylstyrene, o-methylstyrene, p-methylstyrene, vinylxylene, ethylstyrene, dimethylstyrene, p-tert-butylstyrene, vinylnaphthalene, and methoxystyrene, and styrene is particularly preferred. These can be used alone or in combination.
[0065] There are no particular limitations on the mass average molecular weight of the MS and the composition ratio of methyl (meth)acrylate / styrene, but the mass average molecular weight is preferably 80,000 to 300,000, more preferably 100,000 to 200,000, and the composition ratio of methyl (meth)acrylate / styrene is preferably 80 / 20 to 40 / 60, more preferably 70 / 30 to 50 / 50.
[0066] In the copolymer (AS) of a vinyl cyanide compound and an aromatic vinyl compound, acrylonitrile is particularly preferred as the vinyl cyanide compound, and styrene and α-methylstyrene are particularly preferred as the aromatic vinyl compound.
[0067] With regard to the proportion of each component in AS, when the whole is taken as 100 mass%, the proportion of the vinyl cyanide compound is preferably 5 to 50 mass%, more preferably 15 to 35 mass%, and the proportion of the aromatic vinyl compound is preferably 95 to 50 mass%, more preferably 85 to 65 mass%.
[0068] Furthermore, these vinyl compounds may be mixed with the other copolymerizable vinyl compounds described above. In this case, the content of the other vinyl compounds in AS is preferably 15% by mass or less.
[0069] The AS may be produced by any method such as bulk polymerization, suspension polymerization, emulsion polymerization, etc., but is preferably produced by bulk polymerization, and the copolymerization method may be either one-stage copolymerization or multi-stage copolymerization.
[0070] The reduced viscosity of AS is preferably 0.2 to 1.0 dL / g (20 to 100 mL / g), more preferably 0.3 to 0.5 dL / g (30 to 50 mL / g). If the reduced viscosity is less than 0.2 dL / g (20 mL / g), the impact resistance is reduced, and if it exceeds 1.0 dL / g (100 mL / g), the processability is deteriorated.
[0071] The reduced viscosity was measured by precisely weighing 0.25 g of copolymer (AS) of vinyl cyanide compound and aromatic vinyl compound, dissolving it in 50 mL of dimethylformamide for 2 hours, and measuring the solution in an environment of 30°C using an Ubbelohde viscometer. The viscometer used had a solvent flow time of 20 to 100 seconds. The reduced viscosity was calculated from the number of seconds the solvent flowed (t0) and the number of seconds the solution flowed (t) using the following formula.
[0072] Reduced viscosity (η sp / C)={(t / t0)-1} / 0.5 In addition, the copolymers of vinyl cyanide compounds and aromatic vinyl compounds containing a diene rubber component (ABS), vinyl cyanide compounds and aromatic vinyl compounds containing an ethylene-α-olefin rubber component (AES), vinyl cyanide compounds and aromatic vinyl compounds containing an acrylic rubber component (ASA), alkyl (meth)acrylate monomers and aromatic vinyl compounds containing a diene rubber component (MBS), alkyl (meth)acrylate monomers and aromatic vinyl compounds containing a diene rubber component (MABS), and alkyl (meth)acrylate monomers and aromatic vinyl compounds containing an acrylic rubber component (MAS) are thermoplastic copolymers.
[0073] In the present embodiment, the ratio of each of the rubber components contained in ABS, AES, ASA, MBS, MABS and MAS is preferably 5 to 80 mass %, more preferably 8 to 50 mass %, and particularly preferably 10 to 30 mass %.
[0074] As the vinyl cyanide compound to be grafted onto the rubber component, acrylonitrile is particularly preferred, and as the aromatic vinyl compound to be grafted onto the rubber component, styrene and α-methylstyrene are particularly preferred.
[0075] Furthermore, as the alkyl (meth)acrylate monomer, methyl (meth)acrylate and ethyl (meth)acrylate can be particularly preferably used.
[0076] The ratio of the component grafted to the rubber component is preferably 20 to 95% by mass, more preferably 50 to 90% by mass, based on 100% by mass of the styrene-based resin (A2). Furthermore, maleic anhydride, N-substituted maleimide, etc. may be mixed as part of the component grafted to the rubber component, and the content of these in the styrene-based resin (A2) is preferably 15% by mass or less.
[0077] In ABS, AES, ASA, MBS, MABS and MAS, the rubber component exists in the form of particles. The particle size of the rubber component is preferably 0.1 to 5.0 μm, more preferably 0.15 to 1.5 μm, and particularly preferably 0.2 to 0.8 μm. Here, the distribution of the particle size of the rubber component may be a single distribution or may have two or more peaks. In addition, in the morphology of the particle size of the rubber component, the rubber particles may form a single phase, or may have a salami structure by containing an occluded phase around the rubber particles.
[0078] Incidentally, ABS, AES, ASA, MBS, MABS and MAS may contain free polymer components (such as aromatic vinyl compounds) generated during polymerization.
[0079] The reduced viscosity (reduced viscosity at 30°C determined by the method described above) of ABS, AES, ASA, MBS, MABS and MAS is preferably 0.2 to 1.0 dL / g (20 to 100 mL / g), more preferably 0.3 to 0.7 dL / g (30 to 70 mL / g).
[0080] The ratio (graft ratio) of the aromatic vinyl compound grafted to the rubber component is preferably 20 to 200 mass %, and more preferably 20 to 70 mass %, based on the rubber component.
[0081] ABS, AES, ASA, MBS, MABS and MAS may be produced by any of bulk polymerization, suspension polymerization and emulsion polymerization. In particular, ABS is preferably produced by bulk polymerization. Representative bulk polymerization methods include the continuous bulk polymerization method (so-called Toray method) described in Chemical Engineering, Vol. 48, No. 6, p. 415 (1984) and the continuous bulk polymerization method (so-called Mitsui Toatsu method) described in Chemical Engineering, Vol. 53, No. 6, p. 423 (1989).
[0082] In the present embodiment, ABS, AES, ASA, MBS, MABS and MAS can all be suitably used as the styrene resin (A2). The copolymerization method may be a single-stage copolymerization or a multi-stage copolymerization. Resins obtained by blending ABS, AES, ASA, MBS, MABS and MAS obtained by such a production method with a vinyl compound polymer obtained by separately copolymerizing an aromatic vinyl compound and a vinyl cyanide component or the like can also be suitably used as the styrene resin (A2).
[0083] For AS, ABS, AES, ASA, MBS, MABS and MAS, the content of alkaline (earth) metal is preferably small from the viewpoint of good thermal stability and hydrolysis resistance. The content of alkaline (earth) metal in the styrene-based resin (A2) is preferably less than 100 ppm, more preferably less than 80 ppm, further preferably less than 50 ppm, and particularly preferably less than 10 ppm. Thus, from the viewpoint of reducing the content of alkaline (earth) metal, the bulk polymerization method is preferably used.
[0084] In relation to such good thermal stability and hydrolysis resistance, when an emulsifier is used in AS, ABS, etc., the emulsifier is preferably a sulfonate, more preferably an alkylsulfonate, and when a coagulant is used, the coagulant is preferably sulfuric acid or an alkaline earth metal salt of sulfuric acid.
[0085] Examples of rubber components contained in ABS, AES, ASA, MBS, MABS, and MAS include polybutadiene, polyisoprene, diene copolymers, copolymers of ethylene and α-olefins, copolymers of ethylene and unsaturated carboxylic acid esters, copolymers of ethylene and aliphatic vinyls (e.g., ethylene-vinyl acetate copolymers), non-conjugated diene terpolymers of ethylene and propylene, acrylic rubbers, and silicone rubbers.
[0086] Examples of diene copolymers include random and block copolymers of styrene-butadiene, acrylonitrile-butadiene copolymers, and copolymers of alkyl (meth)acrylates and butadiene.
[0087] Examples of the copolymer of ethylene and an α-olefin include ethylene-propylene random copolymers and block copolymers, and ethylene-butene random copolymers and block copolymers.
[0088] Examples of the copolymer of ethylene and an unsaturated carboxylate include an ethylene-methacrylate copolymer and an ethylene-butyl acrylate copolymer.
[0089] An example of the non-conjugated diene terpolymer of ethylene and propylene is an ethylene-propylene-hexadiene copolymer.
[0090] Examples of the acrylic rubber include polybutyl acrylate, poly(2-ethylhexyl acrylate), and copolymers of butyl acrylate and 2-ethylhexyl acrylate.
[0091] Examples of silicone-based rubbers include polyorganosiloxane rubber, IPN type rubber consisting of a polyorganosiloxane rubber component and a polyalkyl (meth)acrylate rubber component (i.e., a rubber having a structure in which the two rubber components are intertwined with each other so that they cannot be separated), and IPN type rubber consisting of a polyorganosiloxane rubber component and a polyisobutylene rubber component.
[0092] The rubber component is preferably selected from the group consisting of polydiene rubber (such as polybutadiene), acrylic rubber, and ethylene-propylene rubber. The glass transition temperature of the rubber component is, for example, typically −10° C. to −20° C. for acrylic rubber, −50° C. to −58° C. for ethylene-propylene rubber, and about −100° C. for butadiene rubber.
[0093] The rubber content in the ABS, AES, ASA, MBS, MABS and MAS used in the present embodiment is preferably 4% by mass to 25% by mass. The rubber content can be adjusted, for example, by adjusting the amount of the rubber component during copolymerization. It is also possible to adjust the rubber content by, for example, mixing an aromatic vinyl copolymer containing a rubber component with an aromatic vinyl polymer or copolymer not containing a rubber component.
[0094] (Aromatic polyester resin (A3)) The aromatic polyester resin (A3) is a polymer or copolymer obtained by a condensation reaction of aromatic dicarboxylic acid or a reactive derivative thereof and diol or an ester derivative thereof as main components.
[0095] Examples of aromatic dicarboxylic acids include terephthalic acid, isophthalic acid, orthophthalic acid, 1,5-naphthalenedicarboxylic acid, 2,6-naphthalenedicarboxylic acid, 4,4'-biphenyldicarboxylic acid, 4,4'-biphenyletherdicarboxylic acid, 4,4'-biphenylmethanedicarboxylic acid, 4,4'-biphenylsulfonedicarboxylic acid, 4,4'-biphenylisopropylidenedicarboxylic acid, 1,2-bis(phenoxy)ethane-4,4'-dicarboxylic acid, 2,5-anthracenedicarboxylic acid, 2,6-anthracenedicarboxylic acid, 4,4'-p-terphenylenedicarboxylic acid, and 2,5-pyridinedicarboxylic acid. Other examples include diphenylmethanedicarboxylic acid, diphenyletherdicarboxylic acid, and β-hydroxyethoxybenzoic acid. Terephthalic acid and 2,6-naphthalenedicarboxylic acid are particularly preferred. Two or more aromatic dicarboxylic acids may be used in combination. It is also possible to use a small amount of aliphatic dicarboxylic acids such as adipic acid, azelaic acid, sebacic acid, dodecanedioic acid, and alicyclic dicarboxylic acids such as cyclohexanedicarboxylic acid in combination with the dicarboxylic acid.
[0096] Examples of the diol include aliphatic diols such as ethylene glycol, propylene glycol, butylene glycol, hexylene glycol, neopentyl glycol, pentamethylene glycol, hexamethylene glycol, decamethylene glycol, 2-methyl-1,3-propanediol, diethylene glycol, and triethylene glycol.
[0097] Other examples include alicyclic diols such as 1,4-cyclohexanedimethanol, etc. Other examples include diols containing aromatic rings such as 2,2-bis(β-hydroxyethoxyphenyl)propane, etc., and mixtures thereof, etc. Furthermore, one or more long-chain diols having a molecular weight of 400 to 6000, such as polyethylene glycol, poly-1,3-propylene glycol, polytetramethylene glycol, etc., may be copolymerized in small amounts.
[0098] The aromatic polyester resin (A3) can be branched by introducing a small amount of a branching agent. There is no limitation on the type of branching agent, but examples of the branching agent include trimesic acid, trimellitic acid, trimethylolethane, trimethylolpropane, and pentaerythritol.
[0099] Examples of the aromatic polyester resin (A3) include polyethylene terephthalate (PET), polytrimethylene terephthalate, polybutylene terephthalate (PBT), polyhexylene terephthalate, polyethylene naphthalate (PEN), polybutylene naphthalate (PBN), and polyethylene-1,2-bis(phenoxy)ethane-4,4'-dicarboxylate. Examples of copolymer polyester resins include polyethylene isophthalate / terephthalate and polybutylene terephthalate / isophthalate. Among these, polyethylene terephthalate, polybutylene terephthalate, polyethylene naphthalate, polybutylene naphthalate, and mixtures thereof, which have well-balanced mechanical properties, can be preferably used.
[0100] The terminal group structure of the aromatic polyester resin (A3) is not particularly limited, and the ratio of hydroxyl groups and carboxyl groups in the terminal groups may be approximately equal, or one may be more. Furthermore, the terminal groups may be blocked by reacting with a compound having reactivity with the terminal groups.
[0101] There is no limitation on the method for producing the alkylene glycol ester of aromatic dicarboxylic acid and / or its low polymer, but it is usually produced by reacting an aromatic dicarboxylic acid or its ester-forming derivative with an alkylene glycol or its ester-forming derivative under heating. For example, the ethylene glycol ester of terephthalic acid and / or its low polymer, which is used as a raw material for polyethylene terephthalate, is produced by a method of directly esterifying terephthalic acid with ethylene glycol, or by transesterifying a lower alkyl ester of terephthalic acid with ethylene glycol, or by adding ethylene oxide to terephthalic acid.
[0102] The alkylene glycol ester of aromatic dicarboxylic acid and / or its oligomer may contain other dicarboxylic acid ester copolymerizable therewith as an additional component in an amount within a range that does not substantially impair the effect of the method of the present disclosure. Specifically, the other dicarboxylic acid ester may be contained in an amount within a range of 10 mol % or less, preferably 5 mol % or less based on the total molar amount of the acid components.
[0103] The copolymerizable additional component is selected from esters of an acid component and a glycol component, or anhydrides thereof. The acid component may include, for example, one or more of aliphatic and alicyclic dicarboxylic acids such as adipic acid, sebacic acid, 1,4-cyclohexanedicarboxylic acid, and hydroxycarboxylic acids such as β-hydroxyethoxybenzoic acid, p-oxybenzoic acid, and the like.
[0104] Examples of glycol components include alkylene glycols having two or more carbon atoms, 1,4-cyclohexanedimethanol, neopentyl glycol, bisphenol A, bisphenol S, aliphatic, alicyclic, aromatic diol compounds, and polyoxyalkylene glycols. The above-mentioned additional component esters may be used alone or in combination of two or more. However, it is preferable that the copolymerization amount is within the above range.
[0105] When terephthalic acid and / or dimethyl terephthalate is used as the starting material, recovered dimethyl terephthalate obtained by depolymerizing polyalkylene terephthalate, or recovered terephthalic acid obtained by hydrolyzing it, can be used in an amount of 70 mass% or more based on the mass of the total acid components constituting the polyester. In this case, the target polyalkylene terephthalate is preferably polyethylene terephthalate, and in particular, it is preferable from the viewpoint of effective utilization of resources to use recovered PET bottles, recovered fiber products, recovered polyester film products, and furthermore, polymer waste generated in the manufacturing process of these products as a raw material source for polyester production.
[0106] Here, the method for obtaining dimethyl terephthalate by depolymerizing the recovered polyalkylene terephthalate is not particularly limited, and any conventionally known method can be adopted. For example, the recovered polyalkylene terephthalate is depolymerized using ethylene glycol, and then the depolymerized product is subjected to an ester exchange reaction with a lower alcohol, for example, methanol, and the reaction mixture is purified to recover a lower alkyl ester of terephthalic acid, which is subjected to an ester exchange reaction with alkylene glycol, and the obtained phthalic acid / alkylene glycol ester is polycondensed to obtain a polyester resin.
[0107] In addition, the method for recovering terephthalic acid from the recovered dimethyl terephthalate is not particularly limited, and any conventional method may be used. For example, dimethyl terephthalate can be recovered from the reaction mixture obtained by the transesterification reaction by recrystallization and / or distillation, and then heated with water under high temperature and high pressure to hydrolyze and recover terephthalic acid. In the impurities contained in the terephthalic acid obtained by this method, the total content of 4-carboxybenzaldehyde, paratoluic acid, benzoic acid, and dimethyl hydroxyterephthalate is preferably 1 ppm or less. In addition, the content of monomethyl terephthalate is preferably in the range of 1 to 5000 ppm.
[0108] The terephthalic acid recovered by the above-mentioned method can be directly esterified with an alkylene glycol, and the resulting ester can be polycondensed to produce a polyester resin.
[0109] There is no particular limitation on the reaction conditions for producing the aromatic polyester resin (A3). In general, the polycondensation reaction is preferably carried out at a temperature of 230 to 320° C. under normal pressure or reduced pressure (0.1 Pa to 0.1 MPa), or a combination of these conditions, for 15 to 300 minutes.
[0110] In the aromatic polyester resin (A3), a reaction stabilizer, such as trimethyl phosphate, may be added to the reaction system at any stage in the polyester production, if necessary. Furthermore, if necessary, one or more of antioxidants, ultraviolet absorbers, flame retardants, fluorescent whitening agents, matting agents, tinting agents, defoamers, and other additives may be blended into the reaction system. In particular, it is preferable that the polyester resin contains an antioxidant containing at least one hindered phenol compound. The content of the antioxidant is preferably 1% by mass or less relative to the mass of the polyester resin. If the content exceeds 1% by mass, the antioxidant itself may thermally deteriorate, causing the inconvenience of deteriorating the quality of the obtained product.
[0111] Examples of the hindered phenol compound include pentaerythritol tetraacetate [3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], 3,9-bis{2-[3-(3-tert-butyl-4-hydroxy-5-methylphenyl)propionyloxy]-1,1-dimethylethyl}-2,4,8,10-tetraoxaspiro[5,5]undecane, etc. It is also preferable to use these hindered phenol antioxidants in combination with thioether secondary antioxidants.
[0112] The method of adding the above hindered phenol-based antioxidant to the polyester resin is not particularly limited, but it is preferably added at any stage after the end of the transesterification reaction or esterification reaction and before the completion of the polymerization reaction.
[0113] The intrinsic viscosity of the aromatic polyester resin (A3) is not limited, but is preferably in the range of 0.30 to 1.5. When the intrinsic viscosity is within this range, melt molding is easy, and the strength of the molded product obtained therefrom is also high. The intrinsic viscosity is more preferably in the range of 0.40 to 1.2, and particularly preferably 0.50 to 1.0. The intrinsic viscosity of the aromatic polyester resin is measured at a temperature of 35°C by dissolving the aromatic polyester resin in orthochlorophenol. The polyester resin obtained by solid phase polycondensation is generally used for bottles and the like, and often has an intrinsic viscosity of 0.70 to 0.90.
[0114] It is preferable that the content of the cyclic trimer of the ester of the aromatic dicarboxylic acid and the alkylene glycol is 0.5% by mass or less, and the content of acetaldehyde is 5 ppm or less.
[0115] The cyclic trimers include alkylene terephthalates (eg, ethylene terephthalate, trimethylene terephthalate, tetramethylene terephthalate, hexamethylene terephthalate, etc.) and alkylene naphthalates (eg, ethylene naphthalate, trimethylene naphthalate, tetramethylene naphthalate, hexamethylene naphthalate, etc.).
[0116] (Polyphenylene ether resin (A4)) The polyphenylene ether resin (A4) may be a mixed resin in which a polystyrene resin is previously mixed with a polyphenylene ether resin, or may consist solely of a polyphenylene ether resin.
[0117] Examples of the polyphenylene ether resin include a homopolymer having a repeating unit structure represented by the following formula (5) and a copolymer having a repeating unit structure represented by the following formula (5).
[0118] [ka]
[0119] In the above formula (5), R 1 , R 2 , R 3 and R 4 are each independently a monovalent group selected from the group consisting of a hydrogen atom, a halogen atom, a primary alkyl group having 1 to 7 carbon atoms, a secondary alkyl group having 1 to 7 carbon atoms, a phenyl group, a haloalkyl group, an aminoalkyl group, a hydrocarbyloxy group, and a halohydrocarbyloxy group in which at least two carbon atoms separate the halogen atom and the oxygen atom.
[0120] From the viewpoints of fluidity, toughness, and chemical resistance during processing, the polyphenylene ether resin preferably has a reduced viscosity of 0.15 to 2.0 dL / g, more preferably 0.20 to 1.0 dL / g, and even more preferably 0.30 to 0.70 dL / g, as measured using a chloroform solution having a concentration of 0.5 g / dL at 30° C. using an Ubbelohde viscometer.
[0121] Examples of the polyphenylene ether resin include, but are not limited to, homopolymers such as poly(2,6-dimethyl-1,4-phenylene ether), poly(2-methyl-6-ethyl-1,4-phenylene ether), poly(2-methyl-6-phenyl-1,4-phenylene ether), and poly(2,6-dichloro-1,4-phenylene ether), and copolymers such as copolymers of 2,6-dimethylphenol and other phenols (for example, 2,3,6-trimethylphenol and 2-methyl-6-butylphenol). Among them, from the viewpoint of the balance between toughness and rigidity when made into a resin composition and the ease of availability of raw materials, poly(2,6-dimethyl-1,4-phenylene ether) and copolymers of 2,6-dimethylphenol and 2,3,6-trimethylphenol are preferred, and poly(2,6-dimethyl-1,4-phenylene ether) is more preferred.
[0122] The polyphenylene ether resin can be produced by a known method. The method for producing the polyphenylene ether resin is not limited to the following, but includes, for example, the method of oxidatively polymerizing 2,6-xylenol using a complex of cuprous salt and amine as a catalyst by Hay described in U.S. Pat. No. 3,306,874, the methods described in U.S. Pat. No. 3,306,875, U.S. Pat. No. 3,257,357, U.S. Pat. No. 3,257,358, JP-B-17880, JP-A-50-51197, JP-A-63-152628, etc.
[0123] Examples of the polystyrene resin already contained in the polyphenylene ether resin (A4) include atactic polystyrene, rubber-reinforced polystyrene (high impact polystyrene, HIPS), styrene-acrylonitrile copolymer (AS) having a styrene content of 50 mass% or more, and ABS resin in which the styrene-acrylonitrile copolymer is rubber-reinforced, and the like. Atactic polystyrene and / or high impact polystyrene are preferred.
[0124] The polystyrene resins may be used alone or in combination of two or more kinds.
[0125] The polyphenylene ether resin (A4) is preferably a polyphenylene ether resin (A4) consisting of a polyphenylene ether resin and a polystyrene resin, the mass ratio of the polyphenylene ether resin to the polystyrene resin being 97 / 3 to 5 / 95. From the viewpoint of achieving even better fluidity, the mass ratio of the polyphenylene ether resin to the polystyrene resin is more preferably 90 / 10 to 10 / 90, and even more preferably 80 / 20 to 10 / 90.
[0126] (Methacrylic resin (A5)) The methacrylic resin (A5) used in the present disclosure is substantially a copolymer of an alkyl methacrylate and an alkyl acrylate, and may be copolymerized with other vinyl monomers not including aromatic vinyl monomers, as long as the object of the present disclosure is not impaired.
[0127] The methacrylic resin is, for example, a polymer obtained by polymerization of monomers consisting of 30 to 100 mass% alkyl methacrylate, 0 to 70 mass% acrylic acid ester, and 0 to 49 mass% other vinyl monomers not including aromatic vinyl monomers copolymerizable therewith. When the methacrylic resin is a copolymer of alkyl methacrylate and alkyl acrylate, the mass ratio of the alkyl methacrylate to the alkyl acrylate is preferably 40 to 90 mass%, more preferably 10 to 60 mass%, and the alkyl methacrylate is preferably 50 to 85 mass%, more preferably 50 to 15 mass%, based on 100 mass% in total of the alkyl methacrylate and the alkyl acrylate.
[0128] The alkyl methacrylate may have an alkyl group with about 1 to 8 carbon atoms, such as methyl methacrylate, ethyl methacrylate, n-butyl methacrylate, t-butyl methacrylate, 2-ethylhexyl methacrylate, etc., and among these, methyl methacrylate is preferred. Two or more types of alkyl methacrylate may be used as necessary.
[0129] The alkyl acrylate may have an alkyl group having about 1 to 8 carbon atoms, such as methyl acrylate, ethyl acrylate, n-butyl acrylate, t-butyl acrylate, and 2-ethylhexyl acrylate, among which methyl acrylate and n-butyl acrylate are preferred. The alkyl acrylate may be used in combination with two or more of them as required, in which case it is preferred to use n-butyl acrylate as the main component and further use one or more alkyl acrylates other than n-butyl acrylate, and it is more preferred to use n-butyl acrylate and methyl acrylate, with n-butyl acrylate being the main component. Here, n-butyl acrylate being the main component means that the mass ratio of n-butyl acrylate exceeds 50 mass% based on the total of two or more alkyl acrylates being 100 mass%.
[0130] The other monomers not including alkyl methacrylates, alkyl acrylates, and aromatic vinyl monomers may be, for example, monofunctional monomers, i.e., compounds having one polymerizable carbon-carbon double bond in the molecule, or polyfunctional monomers, i.e., compounds having at least two polymerizable carbon-carbon double bonds in the molecule.
[0131] Examples of the monofunctional monomer include alkenyl cyanides such as acrylonitrile and methacrylonitrile, acrylic acid, methacrylic acid, maleic anhydride, and N-substituted maleimides.
[0132] Examples of polyfunctional monomers include polyunsaturated carboxylic acid esters of polyhydric alcohols such as ethylene glycol dimethacrylate, butanediol dimethacrylate, and trimethylolpropane triacrylate, alkenyl esters of unsaturated carboxylic acids such as allyl acrylate, allyl methacrylate, and allyl cinnamate, and polyalkenyl esters of polybasic acids such as diallyl phthalate, diallyl maleate, triallyl cyanurate, and triallyl isocyanurate. Two or more types of monomers other than alkyl methacrylate, alkyl acrylate, and aromatic vinyl may be used as necessary.
[0133] The methacrylic resin may be one type or two or more types. The two or more types of methacrylic resin may be different in the types of monomers constituting the methacrylic resin, or may be the same in the types of monomers but different in the mass ratio of each monomer.
[0134] The polymerization method for the methacrylic resin is not particularly limited, and can be carried out by a method such as ordinary bulk polymerization, suspension polymerization, or emulsion polymerization.
[0135] Also, so-called high-impact methacrylic resins, which are methacrylic resins previously blended with rubber particles, can be used. Generally, these high-impact methacrylic resins contain 5 to 40% by mass of a rubber component.
[0136] The rubber component to be compounded is not particularly limited, but one having a refractive index close to that of the methacrylic resin is preferable. Examples of such rubber components include diene graft copolymers mainly composed of butadiene, rubber-like polymers having a core-shell type graft structure mainly composed of acrylic esters and methacrylic esters, and rubber-like polymers grafted to enlarged particles.
[0137] The MFR value (230° C., 3.8 kg load) of the methacrylic resin (B) is preferably from 5 to 25 g / 10 minutes, and more preferably from 10 to 20 g / 10 minutes.
[0138] (Polyarylene sulfide resin (A6)) The polyarylene sulfide resin (A6) has a resin structure having a repeating unit in which an arylene and a sulfur atom are bonded together. The polyarylene sulfide resin contains a repeating unit represented by the following formula (6).
[0139] [ka]
[0140] In the above formula (6), Ar is a substituted or unsubstituted arylene. The arylene is not particularly limited, but examples thereof include phenylene, naphthylene, biphenylene, and terphenylene.
[0141] When the above Ar has a substituent, the substituent includes, but is not limited to, alkyl groups such as a methyl group, an ethyl group, a propyl group, an isopropyl group, a butyl group, an isobutyl group, a sec-butyl group, a tert-butyl group, etc.; alkoxy groups such as a methoxy group, an ethoxy group, a propyloxy group, an isopropyloxy group, a butoxy group, an isobutyloxy group, a sec-butyloxy group, a tert-butyloxy group, etc.; a nitro group; an amino group; a cyano group, etc.
[0142] The above Ar may have one substituent or two or more substituents. When it has two or more substituents, the substituents may be the same or different from each other.
[0143] Among the above-mentioned polyarylene sulfide resins, polyphenylene sulfide resins (PPS resins) in which Ar is substituted or unsubstituted phenylene are preferred. The PPS resins contain at least one repeating unit represented by the following formulae (7) and (8).
[0144] [ka]
[0145] In the above formulas (7) and (8), R each independently represents an alkyl group such as a methyl group, ethyl group, propyl group, isopropyl group, butyl group, isobutyl group, sec-butyl group, or tert-butyl group; an alkoxy group such as a methoxy group, ethoxy group, propyloxy group, isopropyloxy group, butoxy group, isobutyloxy group, sec-butyloxy group, or tert-butyloxy group; a nitro group; an amino group; or a cyano group.
[0146] Furthermore, n is an integer of 0 to 4, preferably an integer of 0 to 2, more preferably 0 or 1, and even more preferably 0. When n is 0, the mechanical strength can be increased.
[0147] Of the above, the PPS resin preferably contains a repeating unit represented by formula (7) from the viewpoints of heat resistance, crystallinity, and the like.
[0148] The PPS resin may also contain a trifunctional structural unit represented by the following formula (9).
[0149] [ka]
[0150] In the above formula (9), R is the same as in the above formulas (7) and (8). Furthermore, m is an integer of 0 to 3, preferably an integer of 0 to 2, more preferably 0 or 1, and even more preferably 0.
[0151] When the PPS resin contains a trifunctional structural unit represented by the above formula (9), the content thereof in the PPS resin is preferably 0.001 to 3 mol %, and more preferably 0.01 to 1 mol %, based on the total moles of all structural units.
[0152] Furthermore, the PPS resin may contain structural units represented by the following formulas (10) to (14).
[0153] [ka]
[0154] [ka]
[0155] [ka]
[0156] In the above formulas (10) to (14), R and n are the same as in the above formula (7), etc. Furthermore, p is an integer of 0 to 6, preferably an integer of 0 to 3, more preferably 0 or 1, and even more preferably 0.
[0157] When the PPS resin contains structural units represented by the above formulae (10) to (14), the content thereof in the PPS resin is preferably 10 mol % or less, more preferably 5 mol % or less, and even more preferably 3 mol % or less, based on all structural units, from the viewpoint of mechanical strength, etc. In this case, when the PPS resin contains two or more structural units represented by the above formulae (10) to (14), the total of the structural units is preferably the above content.
[0158] The above-mentioned polyarylene sulfide resins may be used alone or in combination of two or more kinds.
[0159] The polyarylene sulfide resin may be either linear or branched. In one embodiment, the branched type can be obtained by heating a linear PAS resin in the presence of oxygen.
[0160] The weight average molecular weight of the polyarylene sulfide resin is preferably 25,000 to 80,000, and more preferably 25,000 to 50,000. A weight average molecular weight of 25,000 or more is preferable because the material strength can be maintained. On the other hand, a weight average molecular weight of 80,000 or less is preferable from the viewpoint of moldability.
[0161] In this specification, the value of "weight average molecular weight" is a value measured by gel permeation chromatography. In this case, the measurement conditions of the gel permeation chromatography are as follows: A high-speed GPC HLC-8220 (manufactured by Tosoh Corporation) and a column (TSK-GELGMHX L x 2) are used, 200 mL of a solution in which 5 mg of sample is dissolved in 10 g of tetrahydrofuran (THF) is injected into the device, and the measurement is performed with a flow rate of 1 mL / min (THF), a thermostatic bath temperature of 40°C, and a differential refractive index (RI) detector.
[0162] The melt viscosity of the polyarylene sulfide resin measured at 300°C is preferably 2 to 1000 Pa·s, more preferably 10 to 500 Pa·s, and even more preferably 60 to 200 Pa·s. A melt viscosity of 2 Pa·s or more is preferable because the material strength can be maintained. On the other hand, a melt viscosity of 1000 Pa·s or less is preferable from the viewpoint of moldability.
[0163] The non-Newtonian index of the polyarylene sulfide resin is preferably 0.90 to 2.00, more preferably 0.90 to 1.50, and even more preferably 0.95 to 1.20. A non-Newtonian index value of 0.90 or more is preferable because the material strength can be maintained. On the other hand, a non-Newtonian index value of 2.00 or less is preferable from the viewpoint of moldability.
[0164] The polyarylene sulfide resin can be produced by known methods, such as (1) a method of polymerizing a dihalogenoaromatic compound in the presence of sulfur and sodium carbonate, and, if necessary, a polyhalogenoaromatic compound or other copolymerization components, (2) a method of polymerizing a dihalogenoaromatic compound in the presence of a sulfidizing agent or the like in a polar solvent, and, if necessary, a polyhalogenoaromatic compound or other copolymerization components, (3) a method of adding p-chlorothiophenol and, if necessary, other copolymerization components, and performing self-condensation.
[0165] Among these methods, method (2) is preferred because it is versatile. During the reaction, an alkali metal salt of a carboxylic acid or sulfonic acid or an alkali hydroxide may be added to adjust the degree of polymerization.
[0166] Among the above methods (2), (a) A method for producing a PAS resin by introducing a water-containing sulfidizing agent into a mixture containing a heated organic polar solvent and a dihalogeno-aromatic compound at a rate at which water can be removed from the reaction mixture, and reacting the dihalogeno-aromatic compound with the sulfidizing agent, and optionally a polyhalogeno-aromatic compound, in the organic polar solvent, and controlling the amount of water in the reaction system to within a range of 0.02 to 0.5 mol per mol of the organic polar solvent (see JP-A-07-228699), or (b) A method in which a dihalogenoaromatic compound and, if necessary, a polyhalogenoaromatic compound or other copolymerization components are added in the presence of a solid alkali metal sulfide and an aprotic polar organic solvent, and an alkali metal hydrosulfide and an organic acid alkali metal salt are reacted while controlling the amount of organic acid alkali metal salt to 0.01 to 0.9 moles per mole of the sulfur source and the amount of water in the reaction system to within the range of 0.02 moles per mole of the aprotic polar organic solvent (see International Publication No. WO 2010 / 058713). is particularly preferred.
[0167] The dihalogeno aromatic compound is not particularly limited, but examples thereof include p-dihalobenzene, m-dihalobenzene, o-dihalobenzene, 2,5-dihalotoluene, 1,4-dihalonaphthalene, 1-methoxy-2,5-dihalobenzene, 4,4'-dihalobiphenyl, 3,5-dihalobenzoic acid, 2,4-dihalobenzoic acid, 2,5-dihalonitrobenzene, 2,4-dihalonitrobenzene, 2,4-dihaloanisole, p,p'-dihalodiphenyl ether, 4,4'-dihalobenzophenone, 4,4'-dihalodiphenyl sulfone, 4,4'-dihalodiphenyl sulfoxide, 4,4'-dihalodiphenyl sulfide, and compounds having an alkyl group having 1 to 18 carbon atoms on the aromatic ring of each of the above compounds. The above dihalogeno aromatic compounds may be used alone or in combination of two or more.
[0168] The polyhalogenoaromatic compound is not particularly limited, but may be 1,2,3-trihalobenzene, 1,2,4-trihalobenzene, 1,3,5-trihalobenzene, 1,2,3,5-tetrahalobenzene, 1,2,4,5-tetrahalobenzene, 1,4,6-trihalonaphthalene, etc. The above-mentioned polyhalogenoaromatic compounds may be used alone or in combination of two or more kinds.
[0169] The halogen atom contained in each of the above compounds is preferably a chlorine atom or a bromine atom.
[0170] The method for post-treating the reaction mixture containing the polyarylene sulfide resin obtained by the polymerization step is not particularly limited, but may be, for example, (1) After the polymerization reaction is completed, the solvent is first distilled off under reduced pressure or normal pressure, either directly or after adding an acid or a base to the reaction mixture, and then the solid matter remaining after the solvent distillation is washed once or twice or more times with a solvent such as water, the reaction solvent (or an organic solvent having a similar solubility to the low molecular weight polymer), acetone, methyl ethyl ketone, or alcohols, and then neutralized, washed with water, filtered, and dried; (2) After the polymerization reaction is completed, a solvent such as water, acetone, methyl ethyl ketone, alcohols, ethers, halogenated hydrocarbons, aromatic hydrocarbons, aliphatic hydrocarbons, etc. (a solvent which is soluble in the polymerization solvent used and is a poor solvent for at least polyarylene sulfide) is added as a precipitating agent to the reaction mixture to precipitate solid products such as polyarylene sulfide and inorganic salts, which are then filtered, washed, and dried; (3) After the polymerization reaction is completed, a reaction solvent (or an organic solvent having a similar solubility to the low molecular weight polymer) is added to the reaction mixture, followed by stirring, filtering to remove the low molecular weight polymer, washing once or twice or more times with a solvent such as water, acetone, methyl ethyl ketone, or alcohols, followed by neutralization, washing with water, filtering, and drying; (4) After the polymerization reaction is completed, water is added to the reaction mixture, followed by washing with water, filtering, and if necessary, adding acid during the water washing step for acid treatment, and then drying. (5) After the polymerization reaction is completed, the reaction mixture is filtered, and if necessary, washed once or twice or more times with the reaction solvent, and then washed with water, filtered, and dried. etc.
[0171] In the post-treatment methods exemplified above in (1) to (5), the polyarylene sulfide resin may be dried in vacuum, in air, or in an atmosphere of an inert gas such as nitrogen.
[0172] (Olefin resin (A7)) The olefin resin (A) is a synthetic resin obtained by polymerizing or copolymerizing an olefin monomer having a radically polymerizable double bond.
[0173] The olefin monomer is not particularly limited, and examples thereof include α-olefins and conjugated dienes. Examples of α-olefins include ethylene, propylene, 1-butene, 1-pentene, 1-hexene, 1-heptene, 1-octene, and 4-methyl-1-pentene. Examples of conjugated dienes include butadiene and isoprene. The olefin monomers may be used alone or in combination of two or more.
[0174] The olefin resin (A7) is not particularly limited, and examples thereof include homopolymers of ethylene, copolymers of ethylene and α-olefins other than ethylene, homopolymers of propylene, copolymers of propylene and α-olefins other than propylene, homopolymers of butene, homopolymers or copolymers of conjugated dienes such as butadiene and isoprene, etc. As the olefin resin (A7), homopolymers of propylene or copolymers of propylene and α-olefins other than propylene are preferred.
[0175] When the olefin resin (A7) is a copolymer of propylene and other monomers (polypropylene copolymer), linear α-olefins, branched α-olefins, etc. can be suitably used as the copolymerization α-olefins other than propylene. Examples of linear olefins include ethylene, butene-1, pentene-1, hexene-1, heptene-1, and octene-1. Examples of branched α-olefins include 2-methylpropene-1, 3-methylpentene-1, 4-methylpentene-1, 5-methylhexene-1, 4-methylhexene-1, and 4,4-dimethylpentene-1. These copolymerization α-olefins may be used alone or in combination of two or more.
[0176] The blending amount of these copolymerization α-olefins (copolymerization components) in the olefin resin (A) is preferably 30% by mass or less, more preferably 20% by mass or less. When these are copolymerized, the type of copolymer is not particularly limited, and may be, for example, any of random type, block type, graft type, and mixtures thereof. The polypropylene copolymer (copolymer of propylene and other monomers) may be any of the commonly used random copolymers, block copolymers, etc. Preferred examples of the polypropylene copolymer include propylene-ethylene copolymer, propylene-butene-1 copolymer, and propylene-ethylene-butene-1 copolymer.
[0177] Furthermore, as the olefin resin (A7), for example, a functional group-containing olefin resin obtained by introducing at least one functional group selected from the group consisting of an acid anhydride group, a carboxyl group, a hydroxyl group, an amino group, and an isocyanate group into the above-mentioned polypropylene polymer (polymer of a propylene monomer) or polypropylene copolymer can be used.
[0178] (Polyamide resin (A8)) The polyamide resin (A8) is a thermoplastic polymer having an amide bond, the main constituent materials of which are amino acids, lactams, diamines and dicarboxylic acids or their amide-forming derivatives. A polycondensate obtained by condensing diamines and dicarboxylic acids or their acyl activated derivatives can be used. A polymer obtained by polycondensing aminocarboxylic acids, lactams or amino acids can also be used. A copolymer of these can also be used.
[0179] The diamine includes an aliphatic diamine and an aromatic diamine. Examples of aliphatic diamines include tetramethylenediamine, hexamethylenediamine, undecamethylenediamine, dodecamethylenediamine, 2,2,4-trimethylhexamethylenediamine, 2,4,4-trimethylhexamethylenediamine, 5-methylnonamethylenediamine, 2,4-dimethyloctamethylenediamine, metaxylylenediamine, paraxylylenediamine, 1,3-bis(aminomethyl)cyclohexane, 1-amino-3-aminomethyl-3,5,5-trimethylcyclohexane, 3,8-bis(aminomethyl)tricyclodecane, bis(4-aminocyclohexyl)methane, bis(3-methyl-4-aminocyclohexyl)methane, 2,2-bis(4-aminocyclohexyl)propane, bis(aminopropyl)piperazine, and aminoethylpiperazine.
[0180] Examples of aromatic diamines include p-phenylenediamine, m-phenylenediamine, 2,6-naphthalenediamine, 4,4'-diphenyldiamine, 3,4'-diphenyldiamine, 4,4'-diaminodiphenyl ether, 3,4'-diaminodiphenyl ether, 4,4'-sulfone, 3,4'-diaminodiphenyl sulfone, 4,4'-diaminodiphenyl ketone, 3,4'-diaminodiphenyl ketone, and 2,2-bis(4-aminophenyl)propane.
[0181] Examples of dicarboxylic acids include adipic acid, suberic acid, azelaic acid, sebacic acid, dodecanoic acid, terephthalic acid, isophthalic acid, naphthalenedicarboxylic acid, 2-chloroterephthalic acid, 2-methylterephthalic acid, 5-methylisophthalic acid, 5-sodium sulfoisophthalic acid, hexahydroterephthalic acid, hexahydroisophthalic acid, and diglycolic acid.
[0182] Specific examples of polyamide resins include aliphatic polyamides such as polycaproamide (nylon 6), polytetramethylene adipamide (nylon 46), polyhexamethylene adipamide (nylon 66), polyhexamethylene sebacamide (nylon 610), polyhexamethylene dodecamide (nylon 612), polyundecamethylene adipamide (nylon 116), polyundecaneamide (nylon 11), and polydodecanamide (nylon 12). Also included are aliphatic-aromatic polyamides such as polytrimethylhexamethylene terephthalamide, polyhexamethylene isophthalamide (nylon 6I), polyhexamethylene terephthalic / isophthalamide (nylon 6T / 6I), polybis(4-aminocyclohexyl)methandodecamide (nylon PACM12), polybis(3-methyl-4-aminocyclohexyl)methandodecamide (nylon dimethyl PACM12), polymetaxylylene adipamide (nylon MXD6), polyundecamethylene terephthalamide (nylon 11T), polyundecamethylene hexahydroterephthalamide (nylon 11T(H)), and copolymerized polyamides thereof. Also included are copolymers and mixtures thereof, and poly(p-phenylene terephthalamide), poly(p-phenylene terephthalamide-co-isophthalamide), and the like.
[0183] <Hydrophilic copolymer (B)> The hydrophilic copolymer (B) has an oxyethylene group (preferably a polyoxyethylene chain). Since the oxyethylene group functions as a hydrophilic segment, the presence of the oxyethylene group provides antistatic performance and an effect of suppressing adhesion of hydrophilic dust stains.
[0184] The hydrophilic copolymer (B) having an oxyethylene group has a characteristic that, when mixed with the thermoplastic resin (A), it tends to gather on the surface of a molded article containing a thermoplastic resin composition, compared to other hydrophilic polymers and antistatic agents. That is, the hydrophilic copolymer (B) having an oxyethylene group is present on the surface of a molded article in a large amount, not buried inside the molded article, compared to other hydrophilic polymers and antistatic agents. Therefore, the antifouling effect is efficiently exerted with respect to the amount of hydrophilic copolymer (B) having an oxyethylene group added. Therefore, the amount of hydrophilic copolymer (B) added required to obtain the same antifouling performance may be less than that of other hydrophilic polymers.
[0185] In this embodiment, as such a hydrophilic copolymer (B), a hydrophilic copolymer is used in which a plurality of alternating copolymers (a) of a polyester (a1) and a hydrophilic polymer (a2) having an oxyethylene group are bonded via an ester bond to at least one compound selected from the group consisting of a polyhydric alcohol compound (b1) having three or more hydroxyl groups, an epoxy compound (b2) having two or more epoxy groups, and a polycarboxylic acid compound (b3).
[0186] This hydrophilic copolymer (B) has a melting point of approximately 90 to 100°C, which is lower than the melting points of the "hydrophilic copolymer formed by repeatedly and alternately bonding polyolefins and hydrophilic polymers having polyoxyethylene chains" (B1) (melting point: approximately 135°C) and "polyether ester amide" (B2) (melting point: approximately 195 to 200°C) disclosed in International Publication No. 2021 / 006192 (Patent Document 7).
[0187] By using such a hydrophilic copolymer (B) having a melting point lower than that of the conventional one, the thermoplastic resin composition according to the present embodiment can be manufactured by a low-temperature process and is easy to process. In addition, even when the processing time, kneading time, etc. are relatively short, the hydrophilic copolymer (B) is easily dispersed in the thermoplastic resin composition. In addition, the materials constituting the thermoplastic resin composition (particularly materials other than the hydrophilic copolymer (B)) are less likely to decompose. These effects are effects that cannot be obtained when B1 or B2 disclosed in International Publication No. 2021 / 006192 (Patent Document 7) is used.
[0188] [Alternating copolymer (a)] The alternating copolymer (a) is a copolymer in which a polyester (a1) and a hydrophilic polymer (a2) having an oxyethylene group are repeatedly and alternately bonded through ester bonds. In other words, the alternating copolymer (a) is a copolymer having a plurality of blocks derived from the polyester (a1) and a plurality of blocks derived from the hydrophilic polymer (a2) having an oxyethylene group, alternately.
[0189] The terminal of the alternating copolymer (a) may be a block derived from the polyester (a1) or a block derived from the hydrophilic polymer (a2). When the terminal of the alternating copolymer (a) is a block derived from the polyester (a1), the terminal has a carboxyl group. When the terminal of the alternating copolymer (a) is a block derived from the hydrophilic polymer (a2), the terminal has a hydroxyl group. The functional groups at the terminals of the alternating copolymer (a) may be the same or different.
[0190] The alternating copolymer (a) is represented, for example, by the following formula (15) or formula (16). The alternating copolymer (a) represented by formula (15) has carboxyl groups at both ends. The alternating copolymer (a) represented by formula (16) has hydroxyl groups at both ends. It is preferable that the alternating copolymer (a) has carboxyl groups at both ends as shown in formula (15).
[0191] [ka]
[0192] [ka]
[0193] In the above formulas (15) and (16), "a1" represents a residue obtained by removing a carboxyl group from polyester (a1), and "a2" represents a residue obtained by removing a hydroxyl group from hydrophilic polymer (a2) diol. n is a natural number, preferably an integer of 1 to 10, more preferably an integer of 1 to 7, and most preferably an integer of 1 to 5.
[0194] [Polyester (a1)] The polyester (a1) is not particularly limited as long as it is a polyester having carboxyl groups at both ends, but preferably has a structure represented by the following formula (17), in which a residue obtained by removing the carboxyl group of a dicarboxylic acid and a residue obtained by removing the hydroxyl group of a diol are repeatedly bonded alternately via ester bonds.
[0195] [ka]
[0196] In the above formula (17), X represents a residue obtained by removing a carboxyl group from a dicarboxylic acid, and Y represents a residue obtained by removing a hydroxyl group from a diol. n is preferably an integer of 1 to 50, more preferably an integer of 5 to 40, and even more preferably an integer of 10 to 30.
[0197] The polyester (a1) represented by the above formula (17) can be obtained, for example, by subjecting a dicarboxylic acid and a diol to a polycondensation reaction.
[0198] (Dicarboxylic acid) The dicarboxylic acids include aliphatic dicarboxylic acids and aromatic dicarboxylic acids, and may be mixtures of aliphatic and aromatic dicarboxylic acids.
[0199] The aliphatic dicarboxylic acid preferably includes an aliphatic dicarboxylic acid having 2 to 20 carbon atoms, such as oxalic acid, malonic acid, succinic acid, fumaric acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, 2,5-furandicarboxylic acid, itaconic acid, 1,10-decanedicarboxylic acid, 1,4-cyclohexanedicarboxylic acid, dimer acid, maleic acid, fumaric acid, etc. Among these aliphatic dicarboxylic acids, dicarboxylic acids having 4 to 16 carbon atoms are preferred, and dicarboxylic acids having 6 to 12 carbon atoms are more preferred, from the viewpoints of melting point and heat resistance.
[0200] The aromatic dicarboxylic acid may be a derivative of the aromatic dicarboxylic acid (for example, an acid anhydride, an alkyl ester, an alkali metal salt, an acid halide, etc.). The aromatic dicarboxylic acid and its derivative may be a mixture of two or more kinds.
[0201] The aromatic dicarboxylic acid preferably includes aromatic dicarboxylic acids having 8 to 20 carbon atoms, such as terephthalic acid, isophthalic acid, phthalic acid, phenylmalonic acid, homophthalic acid, phenylsuccinic acid, β-phenylglutaric acid, α-phenyladipic acid, β-phenyladipic acid, biphenyl-2,2'-dicarboxylic acid, biphenyl-4,4'-dicarboxylic acid, naphthalenedicarboxylic acid, sodium 3-sulfoisophthalate, and potassium 3-sulfoisophthalate.
[0202] The dicarboxylic acid used in obtaining polyester (a1) by polycondensation reaction may be a derivative of dicarboxylic acid (e.g., acid anhydride, alkyl ester, alkali metal salt, acid halide, etc.). In this case, after the reaction of the dicarboxylic acid derivative with the diol, the obtained polyester may be treated to have both ends converted to carboxyl groups, or the polyester obtained by the reaction of the dicarboxylic acid derivative with the diol may be used in the next reaction to obtain alternating copolymer (a) without such treatment. The dicarboxylic acid (including its derivative) may be a mixture of two or more kinds.
[0203] (Diol) The diol is not particularly limited as long as it is a compound having two hydroxyl groups, and examples thereof include aliphatic diols, aromatic group-containing diols, etc. The diol may be a mixture of two or more kinds.
[0204] Examples of aliphatic diols include 1,2-ethanediol (ethylene glycol), 1,2-propanediol (propylene glycol), 1,3-propanediol, 1,2-butanediol, 1,3-butanediol, 2-methyl-1,3-propanediol, 1,4-butanediol, 1,5-pentanediol, 2,2-dimethyl-1,3-propanediol (neopentyl glycol), 2,2-diethyl-1,3-propanediol (3,3-dimethylol pentane), 2-n-butyl-2-ethyl-1,3propanediol (3,3-dimethylol heptane), 3-methyl-1,5-pentanediol, and the like. Examples of the aliphatic diol include 1,6-hexanediol, 2,2,4-trimethyl-1,3-pentanediol, 2-ethyl-1,3-hexanediol, 2-methyl-1,8-octanediol, 1,9-nonanediol, 1,10-decanediol, 1,12-octadecanediol, 1,4-cyclohexanedimethanol, hydrogenated bisphenol A, 1,2-, 1,3- or 1,4-cyclohexanediol, cyclododecanediol, dimer diol, isosorbide, hydrogenated dimer diol, diethylene glycol, dipropylene glycol, triethylene glycol, polyethylene glycol, etc. Among these aliphatic diols, 1,4-cyclohexanedimethanol and hydrogenated bisphenol A are preferred from the viewpoint of dust adhesion suppression effect.
[0205] In addition, since the polyester having carboxyl groups at both ends represented by the above formula (17) is preferably hydrophobic, among the aliphatic diols, hydrophilic polyethylene glycol is not preferred, although when used together with a hydrophobic diol other than polyethylene glycol, hydrophilic polyethylene glycol can also be used.
[0206] Examples of aromatic group-containing diols include bisphenol A, 1,2-hydroxybenzene, 1,3-hydroxybenzene, 1,4-hydroxybenzene, 1,4-benzenedimethanol, ethylene oxide adduct of bisphenol A, propylene oxide adduct of bisphenol A, 1,4-bis(2-hydroxyethoxy)benzene, resorcin, polyhydroxyethyl adduct of mononuclear dihydric phenol compound (pyrocatechol, etc.), etc. Among these diols having aromatic groups, ethylene oxide adduct of bisphenol A and 1,4-bis(β-hydroxyethoxy)benzene are preferred.
[0207] The polyester (a1) can be obtained, for example, by subjecting the above dicarboxylic acid or a derivative thereof to a polycondensation reaction with the above diol.
[0208] When obtaining a polyester (a1) having carboxyl groups at both ends, it is preferable to use an excess of dicarboxylic acid or a derivative thereof relative to the diol, and the molar ratio of dicarboxylic acid or a derivative thereof to diol is preferably 2 or more.
[0209] In the polycondensation reaction for obtaining polyester (a1), a catalyst for promoting the esterification reaction may be used. As the catalyst, a conventionally known catalyst such as dibutyltin oxide, tetraalkyl titanate, zirconium acetate, zinc acetate, etc. may be used. In the polycondensation reaction for obtaining polyester (a1), an antioxidant such as a phenol-based antioxidant may be added to the reaction system in order to suppress oxidation of the product.
[0210] The polyester (a1) having carboxyl groups at both ends is not particularly limited as long as it can form an ester bond by reacting with the hydrophilic polymer (a2) having hydroxyl groups at both ends to form the alternating copolymer (a). The carboxyl groups at both ends of the polyester (a1) may be protected or modified, or may be in the form of a precursor.
[0211] [Hydrophilic polymer (a2) having an oxyethylene group] The hydrophilic polymer (a2) having an oxyethylene group is a hydrophilic polymer having an oxyethylene group (preferably a polyoxyethylene chain) and has hydroxyl groups at both ends.
[0212] The hydrophilic polymer (a2) has one or more groups (oxyethylene groups) represented by the following formula (18), and preferably has a plurality of groups (oxyethylene groups) represented by the following formula (18). The hydrophilic polymer (a2) is more preferably a polyethylene glycol (having a polyoxyethylene chain) represented by the following formula (19).
[0213] [ka]
[0214] [ka]
[0215] In the above formula (19), m represents an integer of 5 to 250. From the viewpoints of heat resistance and dust adhesion suppression effect, m is preferably 20 to 150.
[0216] Examples of the polymer having hydroxyl groups at both ends and one or more groups represented by the above formula (18) include polyethylene glycol obtained by addition reaction of ethylene oxide, and polyether obtained by addition reaction of ethylene oxide with at least one other alkylene oxide (e.g., propylene oxide, 1,2-, 1,4-, 2,3- or 1,3-butylene oxide, etc.). This polyether may be a random copolymer or a block copolymer.
[0217] Other examples of the compound having hydroxyl groups at both ends and one or more groups represented by the above formula (18) include compounds having a structure in which ethylene oxide is added to an active hydrogen atom-containing compound, and compounds having a structure in which ethylene oxide and one or more other alkylene oxides (e.g., propylene oxide, 1,2-butylene oxide, 1,4-butylene oxide, 2,3-butylene oxide, 1,3-butylene oxide, etc.) are added to an active hydrogen atom-containing compound. The addition in these compounds may be either random addition or block addition.
[0218] Examples of the active hydrogen atom-containing compound include glycols, dihydric phenols, primary monoamines, secondary diamines, and dicarboxylic acids.
[0219] Examples of the glycol include aliphatic glycols having 2 to 20 carbon atoms, alicyclic glycols having 5 to 12 carbon atoms, and aromatic aliphatic glycols having 8 to 26 carbon atoms.
[0220] Examples of aliphatic glycols include ethylene glycol, 1,2-propylene glycol, 1,3-propanediol, 1,2-butanediol, 1,3-butanediol, 1,4-butanediol, 1,3-hexanediol, 1,4-hexanediol, 1,6-hexanediol, 2,5-hexanediol, 1,2-octanediol, 1,8-octanediol, 1,10-decanediol, 1,18-octadecanediol, 1,20-eicosanediol, diethylene glycol, triethylene glycol, and thiodiethylene glycol.
[0221] Examples of alicyclic glycols include 1-hydroxymethyl-1-cyclobutanol, 1,2-cyclohexanediol, 1,3-cyclohexanediol, 1,4-cyclohexanediol, 1-methyl-3,4-cyclohexanediol, 2-hydroxymethylcyclohexanol, 4-hydroxymethylcyclohexanol, 1,4-cyclohexanedimethanol, and 1,1'-dihydroxy-1,1'-dicyclohexyl.
[0222] Examples of aromatic glycols include dihydroxymethylbenzene, 1,4-bis(β-hydroxyethoxy)benzene, 2-phenyl 1,3-propanediol, 2-phenyl 1,4-butanediol, 2-benzyl 1,3-propanediol, triphenylethylene glycol, tetraphenylethylene glycol, and benzopinacol.
[0223] As the dihydric phenol, a phenol having 6 to 30 carbon atoms can be used, and examples thereof include catechol, resorcinol, 1,4-dihydroxybenzene, hydroquinone, bisphenol A, bisphenol F, bisphenol S, dihydroxydiphenyl ether, dihydroxydiphenyl thioether, binaphthol, and alkyl (having 1 to 10 carbon atoms) or halogen-substituted derivatives thereof.
[0224] Examples of the primary monoamine include aliphatic primary monoamines having 1 to 20 carbon atoms, such as methylamine, ethylamine, n-propylamine, isopropylamine, n-butylamine, s-butylamine, isobutylamine, n-pentylamine, isopentylamine, n-hexylamine, n-heptylamine, n-octylamine, n-decylamine, n-octadecylamine, and n-icosylamine.
[0225] Examples of secondary diamines include aliphatic secondary diamines having 4 to 18 carbon atoms, heterocyclic secondary diamines having 4 to 13 carbon atoms, alicyclic secondary diamines having 6 to 14 carbon atoms, aromatic secondary diamines having 8 to 14 carbon atoms, and secondary alkanol diamines having 3 to 22 carbon atoms.
[0226] Examples of the aliphatic secondary diamine include N,N'-dimethylethylenediamine, N,N'-diethylethylenediamine, N,N'-dibutylethylenediamine, N,N'-dimethylpropylenediamine, N,N'-diethylpropylenediamine, N,N'-dibutylpropylenediamine, N,N'-dimethyltetramethylenediamine, N,N'-diethyltetramethylenediamine, N,N'-dibutyltetramethylenediamine, N,N'-dimethylhexamethylenediamine, N,N'-diethylhexamethylenediamine, N,N'-dibutylhexamethylenediamine, N,N'-dimethyldecamethylenediamine, N,N'-diethyldecamethylenediamine, and N,N'-dibutyldecamethylenediamine.
[0227] Examples of the heterocyclic secondary diamine include piperazine and 1-aminopiperidine.
[0228] Examples of alicyclic secondary diamines include N,N'-dimethyl-1,2-cyclobutanediamine, N,N'-diethyl-1,2-cyclobutanediamine, N,N'-dibutyl-1,2-cyclobutanediamine, N,N'-dimethyl-1,4-cyclohexanediamine, N,N'-diethyl-1,4-cyclohexanediamine, N,N'-dibutyl-1,4-cyclohexanediamine, N,N'-dimethyl-1,3-cyclohexanediamine, N,N'-diethyl-1,3-cyclohexanediamine, and N,N'-dibutyl-1,3-cyclohexanediamine.
[0229] Examples of aromatic secondary diamines include N,N'-dimethyl-phenylenediamine, N,N'-dimethyl-xylylenediamine, N,N'-dimethyl-diphenylmethanediamine, N,N'-dimethyl-diphenyletherdiamine, N,N-dimethyl-benzidine, and N,N'-dimethyl-1,4-naphthalenediamine.
[0230] Examples of secondary alkanol diamines include N-methyldiethanolamine, N-octyldiethanolamine, N-stearyldiethanolamine, and N-methyldipropanolamine.
[0231] The dicarboxylic acid may be a dicarboxylic acid having 2 to 20 carbon atoms. Examples of the dicarboxylic acid having 2 to 20 carbon atoms include aliphatic dicarboxylic acids, aromatic dicarboxylic acids, and alicyclic dicarboxylic acids.
[0232] Examples of aliphatic dicarboxylic acids include oxalic acid, malonic acid, succinic acid, glutaric acid, methylsuccinic acid, dimethylmalonic acid, β-methylglutaric acid, ethylsuccinic acid, isopropylmalonic acid, adipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, undecanedicarboxylic acid, dodecanedicarboxylic acid, tridecanedicarboxylic acid, tetradecanedicarboxylic acid, hexadecanedicarboxylic acid, octadecanedicarboxylic acid, and icosanedicarboxylic acid.
[0233] Examples of aromatic dicarboxylic acids include terephthalic acid, isophthalic acid, phthalic acid, phenylmalonic acid, homophthalic acid, phenylsuccinic acid, β-phenylglutaric acid, α-phenyladipic acid, β-phenyladipic acid, biphenyl-2,2'-dicarboxylic acid, biphenyl-4,4'-dicarboxylic acid, naphthalenedicarboxylic acid, sodium 3-sulfoisophthalate, and potassium 3-sulfoisophthalate.
[0234] Examples of alicyclic dicarboxylic acids include 1,3-cyclopentanedicarboxylic acid, 1,2-cyclopentanedicarboxylic acid, 1,4-cyclohexanedicarboxylic acid, 1,2-cyclohexanedicarboxylic acid, 1,3-cyclohexanedicarboxylic acid, 1,4-cyclohexanediacetic acid, 1,3-cyclohexanediacetic acid, 1,2-cyclohexanediacetic acid, and dicyclohexyl-4,4-dicarboxylic acid.
[0235] These active hydrogen atom-containing compounds may be used alone or in mixtures of two or more of them.
[0236] The hydrophilic polymer (a2) used to obtain the alternating copolymer (a) may be any compound capable of forming an ester bond by reacting with the polyester (a1) component to form the alternating copolymer (a), and the hydroxyl groups at both ends of the hydrophilic polymer (a2) may be protected or modified, or may be in the form of a precursor.
[0237] The alternating copolymer (a) can be obtained by polycondensation reaction of a polyester (a1) having carboxyl groups at both ends and a hydrophilic polymer (a2) having hydroxyl groups at both ends.
[0238] In addition, as long as the polyester (a1) and the hydrophilic polymer (a2) have a structure in which they are repeatedly and alternately bonded via ester bonds formed by a carboxyl group and a hydroxyl group, it is not necessarily necessary to synthesize the alternating copolymer (a) from the specific polyester (a1) and the specific hydrophilic polymer (a2) described above.
[0239] Both ends of the alternating copolymer (a) become either carboxyl groups or hydroxyl groups depending on the ratio of the amounts of the polyester (a1) and the hydrophilic polymer (a2) used during polymerization.
[0240] For example, by adjusting the reaction ratio between polyester (a1) and hydrophilic polymer (a2) so that the amount of polyester (a1) is 2 molar parts per 1 molar part of hydrophilic polymer (a2), an alternating copolymer (a) having carboxyl groups at both ends can be obtained. Also, by adjusting the reaction ratio between polyester (a1) and hydrophilic polymer (a2) so that the amount of hydrophilic polymer (a2) is 2 molar parts per 1 molar part of polyester (a1), an alternating copolymer (c2) having hydroxyl groups at both ends can be obtained.
[0241] After completion of the synthesis reaction of the polyester (a1), the polyester (a1) may be subjected to a polycondensation reaction with the hydrophilic polymer (a2) to obtain the alternating copolymer (a) without isolating the polyester (a1).
[0242] In the polycondensation reaction for obtaining the alternating copolymer (a), a catalyst for promoting the esterification reaction may be used. As the catalyst, a conventionally known catalyst such as dibutyltin oxide, tetraalkyl titanate, zirconium acetate, zinc acetate, etc. may be used. In addition, in the polycondensation reaction for obtaining the alternating copolymer (a), an antioxidant such as a phenol-based antioxidant may be added to the reaction system in order to suppress oxidation of the product.
[0243] [Compounds (b1)~(b3)] The hydrophilic copolymer (B) is a copolymer in which the alternating copolymer (a) is bonded via an ester bond to one compound selected from the group consisting of a polyhydric alcohol compound (b1) having three or more hydroxyl groups, an epoxy compound (b2) having two or more epoxy groups, and a polycarboxylic acid compound (b3).
[0244] In this embodiment, the polyester (a1) has carboxyl groups at both ends. The hydrophilic polymer (a2) having an oxyethylene group has hydroxyl groups at both ends. The alternating copolymer (a) is obtained by an ester bond between the carboxyl groups of the polyester (a1) and the hydroxyl groups of the hydrophilic polymer (a2).
[0245] Specifically, for example, when both ends of the alternating copolymer (a) are carboxyl groups, a hydrophilic copolymer (B) is obtained by bonding multiple alternating copolymers (a) via ester bonds with at least one of a polyhydric alcohol compound (b1) or an epoxy compound (b2) having two or more epoxy groups.
[0246] When both ends of the alternating copolymer (a) are hydroxyl groups, a hydrophilic copolymer (B) is obtained by bonding a plurality of alternating copolymers (a) to the polycarboxylic acid compound (b3) via ester bonds.
[0247] The amount of alternating copolymer (a) per hydrophilic copolymer (B) used to obtain hydrophilic copolymer (B) (i.e., the average number of blocks derived from alternating copolymer (a) contained in hydrophilic copolymer (B)) is preferably 1 to 50 molar parts, more preferably 1 to 30 molar parts, and even more preferably 1 to 10 molar parts per molar part of hydrophilic copolymer (B).
[0248] The hydrophilic copolymer (B) may further contain an ester bond formed between a carboxyl group other than those at both ends of the polyester (a1) and a polyhydric alcohol compound (b1) or an epoxy compound (b2), or may contain an ester bond formed between a hydroxyl group other than those at both ends of the hydrophilic polymer (a2) and a polycarboxylic acid (b3).
[0249] (b1) Polyhydric alcohol compounds having three or more hydroxyl groups The polyhydric alcohol compound (b1) is not particularly limited as long as it is a compound having three or more hydroxyl groups, and examples thereof include trihydric alcohols such as glycerin, 1,2,3-butanetriol, 1,2,4-butanetriol, 2-methyl-1,2,3-propanetriol, 1,2,3-pentanetriol, 1,2,4-pentanetriol, 1,3,5-pentanetriol, 2,3,4-pentanetriol, 2-methyl-2,3,4-butanetriol, trimethylolethane, 2,3,4-hexanetriol, 2-ethyl-1,2,3-butanetriol, trimethylolpropane, 4-propyl-3,4,5-heptanetriol, 2,4-dimethyl-2,3,4-pentanetriol, triethanolamine, triisopropanolamine, and 1,3,5-tris(2-hydroxyethyl)isocyanurate; tetrahydric alcohols such as pentaerythritol, 1,2,3,4-pentanetetrol, 2,3,4,5-hexanetetrol, 1,2,4,5-pentanetetrol, 1,3,4,5-hexanetetrol, diglycerin, ditrimethylolpropane, sorbitan, N,N,N',N'-tetrakis(2-hydroxypropyl)ethylenediamine, and N,N,N',N'-tetrakis(2-hydroxyethyl)ethylenediamine; Pentahydric alcohols such as adonitol, arabitol, xylitol, and triglycerin; hexahydric alcohols such as dipentaerythritol, sorbitol, mannitol, iditol, inositol, dulcitol, talose, and allose; Examples include tripentaerythritol and polypentaerythritol.
[0250] Two or more kinds of such polyhydric alcohol compounds (b1) may be used. (b2) Epoxy compounds The epoxy compound (b2) is not particularly limited as long as it is a compound having two or more epoxy groups, and examples thereof include polyglycidyl ether compounds of mononuclear polyhydric phenol compounds such as hydroquinone, resorcin, pyrocatechol, and phloroglucinol; Polyglycyl ether compounds of polynuclear polyhydric phenol compounds such as dihydroxynaphthalene, biphenol, methylene bisphenol (bisphenol F), methylene bis(ortho-cresol), ethylidene bisphenol, isopropylidene bisphenol (bisphenol A), isopropylidene bis(ortho-cresol), tetrabromo bisphenol A, 1,3-bis(4-hydroxycumylbenzene), 1,4-bis(4-hydroxycumylbenzene), 1,1,3-tris(4-hydroxyphenyl)butane, 1,1,2,2-tetra(4-hydroxyphenyl)ethane, thiobisphenol, sulfobisphenol, oxybisphenol, phenol novolac, orthocresol novolac, ethylphenol novolac, butylphenol novolac, octylphenol novolac, resorcinol novolac, and terpene phenol; Polyglycidyl ethers of polyhydric alcohols such as ethylene glycol, propylene glycol, butylene glycol, hexanediol, polyethylene glycol, polyglycol, thiodiglycol, glycerin, trimethylolpropane, pentaerythritol, sorbitol, and bisphenol A-ethylene oxide adduct; Homopolymers or copolymers of glycidyl esters of aliphatic, aromatic or alicyclic polybasic acids, such as maleic acid, fumaric acid, itaconic acid, succinic acid, glutaric acid, suberic acid, adipic acid, azelaic acid, sebacic acid, dimer acid, trimer acid, phthalic acid, isophthalic acid, terephthalic acid, trimellitic acid, trimesic acid, pyromellitic acid, tetrahydrophthalic acid, hexahydrophthalic acid, endomethylenetetrahydrophthalic acid, and the like, and glycidyl methacrylate; Epoxy compounds having a glycidylamino group, such as N,N-diglycidylaniline, bis(4-(N-methyl-N-glycidylamino)phenyl)methane, and diglycidyl orthotoluidine; Epoxidized products of cyclic olefin compounds such as vinylcyclohexene diepoxide, dicyclopentadiene diepoxide, 3,4-epoxycyclohexylmethyl-3,4-epoxycyclohexanecarboxylate, 3,4-epoxy-6-methylcyclohexylmethyl-6-methylcyclohexanecarboxylate, and bis(3,4-epoxy-6-methylcyclohexylmethyl)adipate; Examples of the epoxy resin include epoxidized conjugated diene polymers such as epoxidized polybutadiene and epoxidized styrene-butadiene copolymers; heterocyclic compounds such as triglycidyl isocyanurate; and epoxidized soybean oil.
[0251] These epoxy compounds may be internally crosslinked with a prepolymer of terminal isocyanate, or may be polymerized with a polyvalent active hydrogen compound (polyhydric phenol, polyamine, carbonyl group-containing compound, polyphosphate ester, etc.). Two or more kinds of such epoxy compounds (b2) may be used.
[0252] (b3) Polycarboxylic acid compounds The polycarboxylic acid compound (b3) may be a carboxylic acid having three or more carboxyl groups, or a carboxylic acid having two or more carboxyl groups and one or more hydroxyl groups. From the viewpoint of dust adhesion suppression effect, a carboxylic acid having three or more carboxyl groups is preferred. The polycarboxylic acid compound (b3) may be a mixture of these.
[0253] The carboxylic acid having three or more carboxyl groups may be a derivative thereof (for example, an acid anhydride, an alkyl ester, an alkali metal salt, an acid halide, etc.) The carboxylic acid having three or more carboxyl groups and its derivative may be a mixture of two or more kinds.
[0254] Examples of carboxylic acids having three or more carboxyl groups include aconitic acid, 1,2,3-propanetricarboxylic acid, butane-1,2,3,4-tetracarboxylic acid, 3-butene-1,2,3-tricarboxylic acid, trimellitic acid, pyromellitic acid, mellitic acid, cyclohexanetricarboxylic acid, naphthalene-1,2,5-tricarboxylic acid, naphthalene-2,6,7-tricarboxylic acid, 1,3,5-pentanetricarboxylic acid, trimesic acid, 3,3',4-diphenyltricarboxylic acid, benzophenone-3,3',4-tricarboxylic acid, and diphenyltricarboxylic acid. Examples of the carboxylic acid include phenylsulfone-3,3',4-tricarboxylic acid, diphenylether-3,3',4-tricarboxylic acid, diphenyl-2,2',3,3'-tetracarboxylic acid, benzophenone-2,2',3,3'-tetracarboxylic acid, diphenylsulfone-2,2',3,3'-tetracarboxylic acid, diphenyl-2,2',3,3'-tetracarboxylic acid, benzophenone-2,2',3,3'-tetracarboxylic acid, diphenylsulfone-2,2',3,3'-tetracarboxylic acid, diphenylether-2,2',3,3'-tetracarboxylic acid, etc. Furthermore, acid-modified polyethylene wax having three or more carboxyl groups, polyacrylic acid, etc. can also be used.
[0255] The carboxylic acid having two or more carboxyl groups and one or more hydroxyl groups may be a derivative thereof (e.g., acid anhydride, alkyl ester, alkali metal salt, acid halide, etc.). The carboxylic acid having two or more carboxyl groups and one or more hydroxyl groups and the derivative thereof may be a mixture of two or more kinds.
[0256] Examples of carboxylic acids having two or more carboxyl groups and one or more hydroxyl groups include tartaric acid, malic acid, citric acid, isocitric acid, citramalic acid, and tartronic acid.
[0257] The total amount of hydroxyl groups of the polyhydric alcohol compound (b1) used to obtain the alternating copolymer (a) (not the number of hydroxyl groups per polyhydric alcohol compound (b1); the same applies below) or the total amount of epoxy groups of the epoxy compound (b2) is preferably 0.1 to 4.0 equivalents, more preferably 0.5 to 3.0 equivalents, based on the total amount of carboxyl groups of the alternating copolymer (a) to be reacted therewith.
[0258] The total amount of carboxyl groups in the polycarboxylic acid (b3) used to obtain the alternating copolymer (a) is preferably 0.1 to 4.0 equivalents, more preferably 0.5 to 3.0 equivalents, based on the total amount of hydroxyl groups in the alternating copolymer (a) to be reacted therewith.
[0259] The reaction for obtaining the alternating copolymer (a) may be carried out in various solvents or in a molten state.
[0260] After the completion of the reaction (synthesis reaction) for obtaining the alternating copolymer (a), the alternating copolymer (a) may not be isolated, but a polyhydric alcohol compound (b1), an epoxy compound (b2) or a polycarboxylic acid (b3) may be added to the reaction system, and the reaction for obtaining the hydrophilic copolymer (B) may be performed as it is. In this case, the carboxyl group of the unreacted polyester (a1) used in excess when synthesizing the alternating copolymer (a) may react with some of the hydroxyl groups of the polyhydric alcohol compound (b1) or the epoxy group of the epoxy compound (b2) to form an ester bond. Also, the hydroxyl group of the unreacted hydrophilic polymer (a2) used in excess when synthesizing the alternating copolymer (a) may react with some of the carboxyl groups of the polycarboxylic acid (b3) to form an ester bond.
[0261] The hydrophilic copolymer (B) does not necessarily have to be synthesized from the specific alternating copolymer (a) and the specific polyhydric alcohol compound (b1), epoxy compound (b2) or polycarboxylic acid (b3) described above, so long as the alternating copolymer (a) has a structure in which the alternating copolymer (a) and the polyhydric alcohol compound (b1), epoxy compound (b2) or polycarboxylic acid (b3) are bonded via an ester bond.
[0262] In the hydrophilic copolymer (B), the block derived from the polyester (a1) has a polystyrene-equivalent number average molecular weight of preferably 800 to 8,000, more preferably 1,000 to 6,000, and further preferably 2,000 to 4,000.
[0263] In the hydrophilic copolymer (B), the block derived from the hydrophilic polymer (a2) has a polystyrene-equivalent number average molecular weight of preferably 400 to 6,000, more preferably 1,000 to 5,000, and further preferably 2,000 to 4,000.
[0264] In the hydrophilic copolymer (B), the block derived from the alternating copolymer (a) has a polystyrene-equivalent number average molecular weight of preferably 5,000 to 25,000, more preferably 7,000 to 17,000, and more preferably 9,000 to 13,000.
[0265] The hydrophilic copolymer (B) of the present embodiment exerts an adhesion suppressing effect against hydrophilic dust stains by being dispersed in a thermoplastic resin composition, so that the surface resistivity of the hydrophilic copolymer (B) itself is usually preferably as low as possible. The surface resistivity of the hydrophilic copolymer (B) is preferably 1×10 4 ~1×10 10 Ω, and more preferably 1×10 4 ~1×10 7 It is Omega.
[0266] In order to improve the adhesion suppression effect against hydrophilic dust stains, the thermoplastic resin composition may further contain an antistatic agent other than the hydrophilic polymer described above. Examples of the other antistatic agent include surfactants (anionic surfactants, cationic surfactants, nonionic surfactants, amphoteric surfactants, etc.) and ionic liquids.
[0267] The hydrophilic copolymer (B) having an oxyethylene group also has another special effect.
[0268] To obtain amphoteric (hydrophilic and hydrophobic) antifouling properties, both the hydrophilic copolymer (B) and the fatty acid metal salt (C) described later are necessary, but the fatty acid metal salt (C) has a smaller molecular weight than the hydrophilic copolymer (B) and is less entangled with the thermoplastic resin (A), so it may fall off from the surface of the molded product or deteriorate. However, when the hydrophilic copolymer (B) is present in large amounts on the surface of the molded product, and the hydrophilic groups of the hydrophilic copolymer (B), which prevents the adhesion of hydrophilic dust stains due to its antistatic effect, adhere to the hydrophilic groups of the fatty acid metal salt (C), the fatty acid metal salt (C) can remain stably present on the surface without falling off.
[0269] On the opposite side of the hydrophilic group of the fatty acid metal salt (C) is the non-polar hydrophobic group R of the fatty acid metal salt (C), which provides a new effect that cannot be obtained by the hydrophilic copolymer (B) alone: a high adhesion inhibition effect against hydrophobic dust stains.
[0270] In other words, the hydrophilic copolymer (B) having an oxyethylene group and the fatty acid metal salt (C) are both present on the surface of the molded article, and exert a synergistic effect with each other, thereby exerting a high adhesion inhibitory effect (anti-fouling property) against amphoteric dust stains.
[0271] <Fatty acid metal salts (C)> The fatty acid metal salt (C) is a compound represented by the following formula (1).
[0272] M(OH)y(R-COO)x (1) (In formula (1), R is an alkyl or alkenyl group having 6 to 40 carbon atoms. M is at least one metal element selected from the group consisting of aluminum, zinc, calcium, magnesium, lithium, and barium. x and y are each independent integers of 0 or more, and satisfy the relationship x+y=[valence of M].) Simply using the above-mentioned hydrophilic polymers and antistatic agents as additives can provide the effect of inhibiting the adhesion of hydrophilic dust stains, but the effect of inhibiting the adhesion of hydrophobic dust stains is low. In the comparative example described below, the amount of hydrophobic dust stains that adheres is not even reduced by half, so a new measure is needed.
[0273] In addition, additives that generally provide water- and oil-repellent effects include silicone oil, fluororesins such as PTFE, and hydrophobic silica such as fumed silica, but none of these additives were effective in suppressing the adhesion of hydrophobic dust stains. This is because when added to resin, the additives are buried inside the resin and do not come to the surface. The problem can be solved by blending fatty acid metal salt (C) with thermoplastic resin (A) and hydrophilic copolymer (B) as a material that can exist at a high concentration on the surface and has hydrophobic and water- and oil-repellent properties.
[0274] The fatty acid metal salt used in this embodiment is a fatty acid metal salt represented by formula (1). M(OH)y(R-COO)x (1) (In formula (1), R is an alkyl or alkenyl group having 6 to 40 carbon atoms. M is at least one metal element selected from the group consisting of aluminum, zinc, calcium, magnesium, lithium, and barium. x and y are each independent integers of 0 or more, and satisfy the relationship x+y=[valence of M].) In formula (1), the carbon number of R is 6 to 40, preferably 11 to 27, and more preferably 15 to 20. If the carbon number of R is less than 6, or if the carbon number is more than 40, the effect of preventing dust adhesion decreases, which is not preferable. R is an alkyl group or an alkenyl group, and is preferably an alkyl group.
[0275] Generally speaking, if the contact angle with water is higher than that of petroleum or mineral oil, it is said to be water- and oil-repellent, and if the contact angle with water is higher than 90 degrees, it is said to be hydrophobic. Fatty acid metal salts (C) fall into this category.
[0276] The melting point of the fatty acid metal salt (C) is, for example, 130 to 180°C, preferably 140 to 170°C, and more preferably 150 to 160°C.
[0277] (Metal element M) In the formula (1), M is at least one metal element selected from the group consisting of aluminum, zinc, calcium, magnesium, lithium and barium.
[0278] M is preferably at least one metal element selected from aluminum and zinc. In this case, the thermoplastic resin composition can exhibit higher antifouling performance. M is more preferably aluminum. In this case, the thermoplastic resin composition can exhibit even higher antifouling performance.
[0279] With reference to FIG. 3, when the ionic radius of M is small (FIGS. 3(a1), (a2)), the non-polar groups (hydrophobic groups) of the fatty acid metal salt can be arranged more densely on the surface of the molded article containing the thermoplastic resin composition than when the ionic radius of M is large (FIGS. 3(b1), (b2)). When the hydrophobic groups are denser, the effect of inhibiting adhesion of hydrophobic dust stains is enhanced. The ionic radii of M are 54 for aluminum, 74 for zinc, 100 for calcium, and 135 for barium, respectively, with aluminum being the smallest and zinc being the next smallest. For this reason, in order to enhance the antifouling effect, aluminum is the most suitable metal element M, followed by zinc.
[0280] (fatty acid) Examples of fatty acids constituting the fatty acid metal salt (C) of the present embodiment include caproic acid, capric acid, lauric acid, palmitic acid, stearic acid, behenic acid, lignoceric acid, montanic acid, oleic acid, linoleic acid, etc. The fatty acid is preferably a long-chain fatty acid (fatty acid having 12 or more carbon atoms) such as stearic acid, behenic acid, montanic acid, etc. In particular, stearic acid is more preferable for production because it is easily available and inexpensive.
[0281] Examples of fatty acid metal salts (C) include zinc stearate, zinc 12-hydroxystearate, zinc laurate, zinc oleate, zinc 2-ethylhexanoate, aluminum tristearate, (dihydroxy)aluminum monostearate, (hydroxy)aluminum distearate, aluminum 12-hydroxystearate, aluminum laurate, aluminum oleate, and aluminum 2-ethylhexanoate. Fatty acid metal salts (C) are preferably zinc stearate, aluminum tristearate, (dihydroxy)aluminum monostearate, and (hydroxy)aluminum distearate, and more preferably (hydroxy)aluminum distearate. The fatty acid metal salts (C) may be used alone or in combination of two or more.
[0282] Aluminum stearate, zinc stearate, calcium stearate, and barium stearate are characterized by their smoothness, high water repellency, and low surface free energy (about 21.2 mN / m). Materials with low surface free energy, such as fluororesin (surface free energy: about 21.5 mN / m), have a stable surface state and are therefore less susceptible to adhesion of dirt. The formation of a layer of aluminum stearate with low surface free energy on the surface of a molded article containing a thermoplastic resin composition exhibits an effect of preventing adhesion of hydrophobic dust stains such as carbon black, soot, and oily smoke. In addition, the lower surface free energy makes it more difficult for hydrophilic dust stains such as dust, sand, and soil to adhere. Therefore, in addition to the static elimination effect of the hydrophilic copolymer (B) blended in the thermoplastic resin composition, the antifouling properties against hydrophobic dust stains and hydrophilic dust stains are further improved.
[0283] (Valence) In formula (1), x and y are each independently an integer of 0 or more, and satisfy the relationship x+y=[the valence of M].
[0284] When the valence of M is 1, y is 0, but when the valence of M is 2 or more, y is 0 or an integer of 1 or more. When the valence of M is 3 or more, y is preferably 1. In this case, the thermoplastic resin composition can exhibit higher antifouling performance.
[0285] As an example, aluminum stearate, which is an aluminum salt of a long-chain fatty acid and in which the valence of M is 3, will be described.
[0286] Aluminum stearate is a mono-type aluminum monostearate that contains one stearic acid [Al(C 17 H 35 COO)(OH)2], and aluminum distearate (Al(C 17 H 35 COO)2(OH)] and tri-type aluminum tristearate, which contains three stearic acids [Al(C 17 H 35 Chief Operating Officer (COO)3.
[0287] Referring to Figure 4, aluminum tristearate is less likely to migrate to the surface of a molded article due to the large amount of non-polar groups (Figure 4(a)), and is an unstable substance that is prone to hydrolysis by moisture in the air to form a mixture with aluminum monostearate or aluminum distearate. Therefore, aluminum distearate is more likely to migrate to the surface of a molded article (Figure 4(b)), and has a higher amphoteric dust suppression effect than aluminum tristearate. Note that even when the valence of M is greater than 3, ditype fatty acid metal salts, which have fewer fatty acids than tritype, similarly have a higher amphoteric dust suppression effect.
[0288] On the other hand, aluminum monostearate has a smaller number of R, which is a non-polar group (hydrophobic group), when the number of aluminum groups is the same, compared to aluminum distearate (Figure 4(c)). Therefore, aluminum distearate has a higher amphoteric dust suppression effect than aluminum monostearate.
[0289] In fact, when the surface area of a molded product was measured using time-of-flight secondary ion mass spectrometry (TOF-SIMS), C derived from stearic acid was 18 H 35 O2 - was detected as a secondary ion. Since the detection depth of TOF-SIMS is generally considered to be 1 to 2 nm, it was possible to confirm the presence of stearic acid on the outermost surface of the molded product.
[0290] CH, the main peak in polystyrene analysis - C when the ionic strength of 18 H 35 O2 - The secondary ion intensity ratio of the molded product using aluminum distearate was 0.341, which was two to four times higher than those of the molded product using aluminum monostearate (0.0687) and the molded product using aluminum tristearate (0.172). Therefore, the molded product using aluminum distearate (y=1) has many non-polar groups (hydrophobic groups) on the surface and is most likely to exhibit a dust suppression effect.
[0291] For the same reason as in the case where the valence of M is 3 or more, di-type fatty acid metal salts have a higher amphoteric dust suppression effect than mono-type fatty acid metal salts even when the valence of M is 2. Therefore, when the valence of M is 2, it is preferable that y is 0 (x is 2).
[0292] <Content of each ingredient> In the thermoplastic resin composition of the present embodiment, the blending amount of the hydrophilic copolymer (B) is preferably 1 to 20 parts by mass, and more preferably 1 to 17 parts by mass, based on 100 parts by mass of the thermoplastic resin (A).
[0293] The amount of the fatty acid metal salt (C) is preferably 0.5 to 10 parts by mass, and more preferably 1 to 8 parts by mass, based on 100 parts by mass of the thermoplastic resin (A).
[0294] The thermoplastic resin composition of the present embodiment particularly preferably contains 100 parts by mass of a thermoplastic resin (A), 1 to 20 parts by mass of a hydrophilic copolymer (B), and 0.5 to 10 parts by mass of a fatty acid metal salt (C).
[0295] The fatty acid metal salt (C) may be blended into the thermoplastic resin composition generally at 0.5 mass % or less (particularly, about 0.1%) as a lubricant, mold release agent, or the like for improving moldability. However, blending more than 0.5 mass % of the fatty acid metal salt (C) exerts the effect of causing both the hydrophilic copolymer (B) and the fatty acid metal salt (C) to be present at high concentrations on the surface of the molded article, and further improves the antifouling effect of both.
[0296] If the amount of hydrophilic copolymer (B) exceeds 20 parts by mass, the mechanical strength such as elastic modulus will decrease, and if it is less than 1 part by mass, the effect of suppressing dust adhesion will decrease.
[0297] If the amount of fatty acid metal salt (C) exceeds 10 parts by mass, the heat resistance and impact resistance decrease, whereas if it is less than 0.5 parts by mass, the effect of inhibiting adhesion of dust decreases.
[0298] As mentioned above, fatty acid metal salt (C) may be generally used for purposes other than the purpose of the present embodiment, which is to inhibit adhesion of both hydrophilic and hydrophobic dust stains. For example, as disclosed in JP-A-2004-168055 and JP-A-2003-183529, fatty acid metal salt (C) is used as a lubricant, molding improver, mold release agent, antifogging agent, etc. In this case, the amount of fatty acid metal salt (C) is less than 0.5 parts by mass per 100 parts by mass of thermoplastic resin (A). Furthermore, in general manufacturing applications, the amount is 0.1 parts by mass or less. In addition, the effect of fatty acid metal salt (C) in inhibiting adhesion of dust has not been known so far.
[0299] In this embodiment, in order to obtain an effect of suppressing adhesion of both hydrophilic and hydrophobic dust stains, the amount of fatty acid metal salt (C) is sufficiently larger than the amount generally used, and it has been found that a remarkable effect of suppressing adhesion of amphoteric dust stains can be obtained for the first time. Therefore, the amount of fatty acid metal salt (C) is preferably 0.5 parts by mass or more, more preferably 1 to 8 parts by mass, per 100 parts by mass of thermoplastic resin (A). In this case, a dust suppression effect equal to or better than that of a molded article having a dust suppression coating on the surface thereof can be obtained. There has been no known example of compounding 1 part by mass or more of fatty acid metal salt (C) per 100 parts by mass of thermoplastic resin for the purpose of dust suppression.
[0300] The non-polar hydrophobic group R of the fatty acid metal salt facing the air provides a new effect of inhibiting the adhesion of hydrophobic dust stains. By adding 0.5 mass% or more of the fatty acid metal salt (C) to the thermoplastic resin (A), many hydrophobic groups can be densely arranged on the surface of the molded article containing the thermoplastic resin composition, enhancing the effect of inhibiting the adhesion of hydrophobic dust stains.
[0301] As described later, the antistatic effect of the hydrophilic copolymer (B) having oxyethylene groups enhances the effect of inhibiting the adhesion of hydrophilic dust stains, and the addition of a fatty acid metal salt (C) enhances the effect of inhibiting the adhesion of hydrophobic dust stains, resulting in a new effect of being resistant to amphoteric stains.
[0302] <Optional ingredients> The thermoplastic resin composition of the present embodiment may contain, as optional components, components such as, for example, a heat stabilizer, an ultraviolet absorber, a light stabilizer, an antibacterial agent, an antifungal agent, and an inorganic filler, within a range that does not impair the object of the present embodiment.
[0303] (Heat stabilizer) The thermoplastic resin composition of the present embodiment may contain a heat stabilizer in order to improve the thermal stability during production and the like.
[0304] As the heat stabilizer, it is preferable to use a phosphorus-based stabilizer and / or a hindered phenol-based antioxidant, and it is more preferable to use these in combination.
[0305] The amount of the phosphorus-based stabilizer and / or the hindered phenol-based antioxidant added to the thermoplastic resin composition of the present embodiment is not particularly limited.
[0306] Since the effect of improving thermal stability can be effectively obtained without affecting the blending amounts of each of the above essential components, the amount is preferably 0.01 to 1 part by mass, and more preferably 0.01 to 0.6 parts by mass, per 100 parts by mass of the thermoplastic resin composition.
[0307] Examples of phosphorus-based stabilizers include phosphorous acid, phosphoric acid, phosphonous acid, phosphonic acid, and their esters, phosphonite compounds, and tertiary phosphines.
[0308] Examples of phosphorous esters (phosphite compounds) include triphenyl phosphite, tris(nonylphenyl)phosphite, tridecyl phosphite, distearyl pentaerythritol diphosphite, bis(2,4-di-tert-butylphenyl)pentaerythritol diphosphite, bis(2,6-di-tert-butyl-4-methylphenyl)pentaerythritol diphosphite, bis{2,4-bis(1-methyl-1-phenylethyl)phenyl}pentaerythritol diphosphite, phenyl bisphenol A pentaerythritol diphosphite, bis(nonylphenyl)pentaerythritol diphosphite, and dicyclohexyl pentaerythritol diphosphite.
[0309] As the phosphorous ester (phosphite compound), in addition to the above, those having a cyclic structure upon reaction with a dihydric phenol can also be used.
[0310] For example, 2,2'-methylenebis(4,6-di-tert-butylphenyl)(2,4-di-tert-butylphenyl)phosphite, 2,2'-methylenebis(4,6-di-tert-butylphenyl)(2-tert-butyl-4-methylphenyl)phosphite, and 2,2-methylenebis(4,6-di-tert-butylphenyl)octylphosphite can be mentioned.
[0311] Examples of phosphoric acid esters (phosphate compounds) include triphenyl phosphate and trimethyl phosphate.
[0312] Examples of the phosphonite compound include tetrakis(di-tert-butylphenyl)-biphenylene diphosphonite, and bis(di-tert-butylphenyl)-phenyl-phenyl phosphonite.
[0313] The phosphonite compound can be used in combination with the above-mentioned phosphite compound having an aryl group substituted with two or more alkyl groups, and is preferred.
[0314] Examples of phosphonic acid esters (phosphonate compounds) include dimethyl benzenephosphonate, diethyl benzenephosphonate, and dipropyl benzenephosphonate.
[0315] Tertiary phosphines include triphenylphosphine and the like. Among the above phosphorus-based stabilizers, phosphonite compounds or phosphite compounds represented by the following formula (20) are preferred.
[0316] [ka]
[0317] (In formula (20), R and R' represent an alkyl group having 6 to 30 carbon atoms or an aryl group having 6 to 30 carbon atoms, and may be the same or different.) As mentioned above, the phosphonite compound is preferably tetrakis(2,4-di-tert-butylphenyl)-biphenylene diphosphonite.
[0318] Among the above formula (15), more preferred phosphite compounds are distearyl pentaerythritol diphosphite, bis(2,4-di-tert-butylphenyl)pentaerythritol diphosphite, bis(2,6-di-tert-butyl-4-methylphenyl)pentaerythritol diphosphite, and bis{2,4-bis(1-methyl-1-phenylethyl)phenyl}pentaerythritol diphosphite.
[0319] Examples of the hindered phenol compound include tetrakis[methylene-3-(3-tert-butyl-4-hydroxy-5-methylphenyl)propionate]methane, octadecyl-3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate, and 3,9-bis[2-{3-(3-t-butyl-4-hydroxy-5-methylphenyl)propionyloxy}-1,1-dimethylethyl]-2,4,8,10-tetraoxaspiro[5,5]undecane.
[0320] The thermoplastic resin composition of the present embodiment may contain other heat stabilizers in addition to the phosphorus-based stabilizer and the hindered phenol-based antioxidant, as necessary.
[0321] The other heat stabilizer is preferably used in combination with at least one of a phosphorus-based stabilizer and a hindered phenol-based antioxidant, and is particularly preferably used in combination with both.
[0322] Other examples of the heat stabilizer include lactone-based stabilizers such as the reaction product of 3-hydroxy-5,7-di-tert-butyl-furan-2-one and o-xylene (for details of this stabilizer, see JP-A-7-233160).
[0323] As for the lactone-based stabilizer, Irganox HP-136 (registered trademark, manufactured by CIBA SPECIALTY CHEMICALS) and the like are commercially available.
[0324] Irganox HP-2921 (registered trademark, manufactured by CIBA SPECIALTY CHEMICALS) and the like are commercially available as stabilizers comprising a mixture of the above-mentioned lactone-based stabilizer, a phosphite compound, and a hindered phenol compound.
[0325] The amount of the lactone-based stabilizer added is preferably 0.0005 to 0.05 parts by mass, and more preferably 0.001 to 0.03 parts by mass, based on 100 parts by mass of the thermoplastic resin composition.
[0326] Other stabilizers include sulfur-containing stabilizers such as pentaerythritol tetrakis(3-mercaptopropionate), pentaerythritol tetrakis(3-laurylthiopropionate), and glycerol-3-stearylthiopropionate.
[0327] The amount of stabilizer other than the phosphorus-based stabilizer and / or the hindered phenol-based antioxidant added to the thermoplastic resin composition of the present embodiment is not particularly limited, and is preferably 0.0005 to 0.1 parts by mass, more preferably 0.001 to 0.08 parts by mass, and particularly preferably 0.001 to 0.05 parts by mass, relative to 100 parts by mass of the thermoplastic resin composition.
[0328] (UV absorber) The thermoplastic resin composition of the present embodiment may contain an ultraviolet absorber. Since the thermoplastic resin composition of the present embodiment may have poor weather resistance due to the influence of the rubber component, etc., blending an ultraviolet absorber is effective in improving weather resistance.
[0329] Examples of the ultraviolet absorbent of the present embodiment include a benzophenone-based ultraviolet absorbent, a benzotriazole-based ultraviolet absorbent, a hydroxyphenyltriazine-based ultraviolet absorbent, a cyclic iminoester-based ultraviolet absorbent, and a cyanoacrylate-based ultraviolet absorbent.
[0330] Examples of benzophenone-based ultraviolet absorbers include 2,4-dihydroxybenzophenone, 2-hydroxy-4-methoxybenzophenone, 2-hydroxy-4-octoxybenzophenone, 2-hydroxy-4-benzyloxybenzophenone, 2-hydroxy-4-methoxy-5-sulfoxybenzophenone, 2-hydroxy-4-methoxy-5-sulfoxytrihydridolate benzophenone, 2,2'-dihydroxy-4-methoxybenzophenone, 2,2',4,4'-tetrahydroxybenzophenone, 2,2'-dihydroxy-4,4'-dimethoxybenzophenone, 2,2'-dihydroxy-4,4'-dimethoxy-5-sodium sulfoxybenzophenone, bis(5-benzoyl-4-hydroxy-2-methoxyphenyl)methane, 2-hydroxy-4-n-dodecyloxybenzophenone, and 2-hydroxy-4-methoxy-2'-carboxybenzophenone.
[0331] Examples of benzotriazole-based ultraviolet absorbers include 2-(2-hydroxy-5-methylphenyl)benzotriazole, 2-(2-hydroxy-5-tert-octylphenyl)benzotriazole, 2-(2-hydroxy-3,5-dicumylphenyl)phenylbenzotriazole, 2-(2-hydroxy-3-tert-butyl-5-methylphenyl)-5-chlorobenzotriazole, 2,2'-methylenebis[4-(1,1,3,3-tetramethylbutyl)-6-(2H-benzotriazol-2-yl)phenol], 2-(2-hydroxy-3,5-di-tert-butylphenyl)benzotriazole, 2-(2-hydroxy-3,5-di-tert-butylphenyl)benzotriazole, Examples of the benzotriazole-based ultraviolet absorbers include 2-(2-hydroxy-3,5-di-tert-amylphenyl)-5-chlorobenzotriazole, 2-(2-hydroxy-5-tert-octylphenyl)benzotriazole, 2-(2-hydroxy-5-tert-butylphenyl)benzotriazole, 2-(2-hydroxy-4-octoxyphenyl)benzotriazole, 2,2'-methylenebis(4-cumyl-6-benzotriazolephenyl), 2,2'-p-phenylenebis(1,3-benzoxazin-4-one), and 2-[2-hydroxy-3-(3,4,5,6-tetrahydrophthalimidomethyl)-5-methylphenyl]benzotriazole. Examples of other benzotriazole-based ultraviolet absorbers include polymers having a 2-hydroxyphenyl-2H-benzotriazole skeleton. Examples of polymers having a 2-hydroxyphenyl-2H-benzotriazole skeleton include copolymers of 2-(2'-hydroxy-5-methacryloxyethylphenyl)-2H-benzotriazole and vinyl monomers copolymerizable with the monomer, and copolymers of 2-(2'-hydroxy-5-acryloxyethylphenyl)-2H-benzotriazole and vinyl monomers copolymerizable with the monomer.
[0332] Examples of hydroxyphenyltriazine-based ultraviolet absorbents include 2-(4,6-diphenyl-1,3,5-triazin-2-yl)-5-hexyloxyphenol, 2-(4,6-diphenyl-1,3,5-triazin-2-yl)-5-methyloxyphenol, 2-(4,6-diphenyl-1,3,5-triazin-2-yl)-5-ethyloxyphenol, 2-(4,6-diphenyl-1,3,5-triazin-2-yl)-5-propyloxyphenol, and 2-(4,6-diphenyl-1,3,5-triazin-2-yl)-5-butyloxyphenol.Furthermore, examples include compounds in which the phenyl group of the above-mentioned compounds is replaced with a 2,4-dimethylphenyl group, such as 2-(4,6-bis(2,4-dimethylphenyl)-1,3,5-triazin-2-yl)-5-hexyloxyphenol.
[0333] Examples of cyclic imino ester-based ultraviolet absorbers include 2,2'-p-phenylene bis(3,1-benzoxazin-4-one), 2,2'-(4,4'-diphenylene) bis(3,1-benzoxazin-4-one), and 2,2'-(2,6-naphthalene) bis(3,1-benzoxazin-4-one).
[0334] Examples of cyanoacrylate-based ultraviolet absorbers include 1,3-bis-[(2'-cyano-3',3'-diphenylacryloyl)oxy]-2,2-bis[(2-cyano-3,3-diphenylacryloyl)oxy]methyl)propane and 1,3-bis-[(2-cyano-3,3-diphenylacryloyl)oxy]benzene.
[0335] Furthermore, the ultraviolet absorber may be a polymer-type ultraviolet absorber obtained by copolymerizing an ultraviolet absorbing monomer and / or a light stable monomer having a hindered amine structure with a monomer such as an alkyl (meth)acrylate. Suitable examples of the ultraviolet absorbing monomer include (meth)acrylic acid esters, and compounds containing a benzotriazole skeleton, a benzophenone skeleton, a triazine skeleton, a cyclic imino ester skeleton, and a cyanoacrylate skeleton in the ester substituent.
[0336] Among the above, in terms of ultraviolet absorbing ability, benzotriazole-based and hydroxyphenyltriazine-based ultraviolet absorbents are preferred, and in terms of heat resistance and hue (transparency), cyclic iminoester-based and cyanoacrylate-based ultraviolet absorbents are preferred. The above ultraviolet absorbents may be used alone or in a mixture of two or more kinds.
[0337] The content of the ultraviolet absorber is preferably 0.01 to 2 parts by mass, more preferably 0.02 to 2 parts by mass, still more preferably 0.03 to 1 part by mass, and particularly preferably 0.05 to 0.5 parts by mass, based on 100 parts by mass of the thermoplastic resin composition.
[0338] (Light stabilizer) The thermoplastic resin composition of the present embodiment may contain a light stabilizer. Since the thermoplastic resin composition of the present embodiment may cause yellowing in the dark, the incorporation of a light stabilizer is effective in preventing such deterioration.
[0339] As such a light stabilizer, a hindered amine light stabilizer (HALS) can be suitably used. HALS is, for example, a compound represented by the following formulas (21) to (24), or a combination of two or more of these compounds.
[0340] [ka]
[0341] [ka]
[0342] [ka]
[0343] [ka]
[0344] In the formulas (21) to (24), R1 to R3 are independent substituents. Examples of the substituent include hydrogen, an ether group, an ester group, an amine group, an amide group, an alkyl group, an alkenyl group, an alkynyl group, an aralkyl group, a cycloalkyl group, and an aryl group.
[0345] These substituents may contain functional groups, such as alcohols, ketones, anhydrides, imines, siloxanes, ethers, carboxyls, aldehydes, esters, amides, imides, amines, nitriles, ethers, urethanes, and combinations thereof.
[0346] As the hindered amine light stabilizer (HALS), compounds derived from substituted piperidine compounds are preferred, and compounds derived from alkyl-substituted piperidyl, piperidinyl or piperazinone compounds, and substituted alkoxypiperidinyl compounds are more preferred.
[0347] Examples of the hindered amine light stabilizer include, but are not limited to, 2,2,6,6-tetramethyl-4-piperidone; 2,2,6,6-tetramethyl-4-piperidinol; bis-(1,2,2,6,6-pentamethylpiperidyl)-(3',5'-di-t-butyl-4'-hydroxybenzyl)butylmalonate; di-(2,2,6,6-tetramethyl-4-piperidyl)sebacate; N-(2-hydroxyethyl)-2,2,6,6- Oligomer of tetramethyl-4-piperidinol and succinic acid;Oligomer of cyanuric acid and N,N-di(2,2,6,6-tetramethyl-4-piperidyl)-hexamethylenediamine;Bis-(2,2,6,6-tetramethyl-4-piperidinyl) succinate;Bis-(1-octyloxy-2,2,6,6-tetramethyl-4-piperidinyl) sebacate;Bis-(1,2,2,6,6-pentamethyl-4-piperidinyl) sebacate;Tetrakis-(2 ,2,6,6-tetramethyl-4-piperidyl)-1,2,3,4-butanetetracarboxylate;N,N'-bis-(2,2,6,6-tetramethyl-4-piperidyl)-hexane-1,6-diamine;N-butyl-2,2,6,6-tetramethyl-4-piperidinamine;2,2'-[(2,2,6,6-tetramethyl-piperidinyl)-imino]-bis-[ethanol];Poly((6-morpholine-S-triazine-2,4-diyl)(2,2, 6,6-Tetramethyl-4-piperidinyl)-iminohexamethylene-(2,2,6,6-tetramethyl-4-piperidinyl)-imino;5-(2,2,6,6-tetramethyl-4-piperidinyl)-2-cyclo-undecyl-oxazole;1,1'-(1,2-ethane-di-yl)-bis-(3,3',5,5'-tetramethyl-piperazinone);8-Acetyl-3-dodecyl-7,7,9,9-tetramethyl-1,3,8-triazaspiro(4.5) Decane-2,4-dione; Polymethylpropyl-3-oxy-[4(2,2,6,6-tetramethyl)-piperidinyl]siloxane; 1,2,3,4-butanetetracarboxylic acid-1,2,3-tris(1,2,2,6,6-pentamethyl-4-piperidinyl)-4-tridecyl ester; α-Methylstyrene-N-(2,2,6,6-tetramethyl-4-piperidinyl)maleimide and N-stearylmaleimide copolymer; 1,2,3,4-butanetetracarboxylic acid-β,β,β',β'-tetramethyl-2,4,8,10-tetraoctanoic acid Copolymer of oxaspiro[5.5]undecane-3,9-diethanol with 1,2,2,6,6-pentamethyl-4-piperidinyl ester;β,β,β',β'-tetramethyl-polymer of 2,4,8,10-tetraoxaspiro[5.5]undecane-3,9-diethanol with 1,2,3,4-butanetetracarboxylic acid, 2,2,6,6-tetramethyl-4-piperidinyl ester;D-glucitol, 1,3:2,4-bis-o-(2,2,6,6-tetramethyl-4-piperidinylidene)-;7-oxa-3,20-diazadispiro[ 5.1.11.2]-Henneicosan-21-one-2,2,4,4-tetramethyl-20-(oxiranylmethyl) oligomer;Propanedioic acid, [(4-methoxyphenyl)methylene]-, bis(1,2,2,6,6-pentamethyl-4-piperidinyl) ester;Formamide, N,N'-1,6-hexanediylbis[N-(2,2,6,6-tetramethyl-4-piperidinyl;1,3,5-triazine-2,4,6-triamine, N,N'''-[1,2-ethanediylbis[[[4,6-bis[butyl(1,2,2,6,6-pentamethoxy)methyl] 1,5-Dimethyl-4-piperidinyl)amino]-1,3,5-triazin-2-yl]imino]-3,1-propanediyl]]-bis[N',N''-dibutyl-N',N''-bis(1,2,2,6,6-pentamethyl-4-piperidinyl);Poly[[6-[(1,1,3,33-tetramethylbutyl)amino]-1,3,5-triazine-2,4-diyl][(2,2,6,6-tetramethyl-4-piperidinyl)-imino]-1,6-hexanediyl[(2,2,6,6-tetramethyl-4-piperidinyl)imino]];1,5-Dioxaspiro(5.5)Undecane 3,3-dicarboxylic acid, bis(2,2,6,6-tetramethyl-4-piperidinyl) ester;1,5-Dioxaspiro(5.5)Undecane 3,3-dicarboxylic acid, bis(1,2,2,6,6-pentamethyl-4-piperidinyl) ester;N-2,2,6,6-tetramethyl-4-piperidinyl-N-amino-oxamide;4-Acryloyloxy-1,2,2,6,6-pentamethyl-4-piperidine;1,5,8,12-Tetrakis[2',4'-bis(1'',2'',2'',6'',6''-pentamethyl-4''-piperidinyl(butyl)amino)-1',3',5'-triazin-6'-yl]-1,5,8,1 2-Tetraazadodecane; 3-Dodecyl-1-(2,2,6,6-tetramethyl-4-piperidyl)-pyrrolidine-2,5-dione; 1,1'-(1,2-ethane-di-yl)-bis-(3,3',5,5'-tetra-methyl-piperazinone); 1,1'1''-(1,3,5-triazine-2,4,6-triyltris((cyclohexylimino)-2,1-ethanediyl)tris(3,3,5,5-tetramethylpiperazinone); 1,1',1''-(1,3,5-triazine-2,4,6-triyltris((cyclohexylimino)-2,1-ethanediyl)tris(3,3,4,5,5-tetramethylpiperazinone).
[0348] The amount of such a hindered amine light stabilizer (HALS) added is preferably 0.01 to 5 parts by mass, more preferably 0.05 to 3 parts by mass, and further preferably 0.1 to 1 part by mass, based on 100 parts by mass of the thermoplastic resin composition.
[0349] (Antibacterial agent) The thermoplastic resin composition of the present embodiment may contain an antibacterial agent. The antibacterial agent is not particularly limited, but examples thereof include inorganic antibacterial agents in which antibacterial metals such as zinc oxide, silver, copper, and zinc are supported on crystalline aluminosilicate, amorphous aluminosilicate, silica gel, activated alumina, diatomaceous earth, activated carbon, zirconium phosphate, hydroxyapatite, magnesium oxide, magnesium perchlorate, glass, and the like. As the antibacterial metal, zinc oxide is preferred.
[0350] The zinc oxide is not particularly limited, and may be a commercially available product, for example, a product obtained by heating and vaporizing metallic zinc and burning it in air, or a product prepared by heating zinc sulfate or zinc nitrate. In addition, the zinc oxide may have various shapes, such as a fiber shape, a plate shape, a particle shape, or a tetrapod shape. The zinc oxide used in the present embodiment may be surface-treated with silicon oxide, silicone oil, an organic silicon compound, an organic titanium compound, or the like.
[0351] Examples of commercially available zinc oxide include "type 1 zinc oxide," "type 2 zinc oxide," and "type 3 zinc oxide" classified by JIS K-1410, official zinc oxide specified in the Japanese Pharmacopoeia, and anisotropic (columnar, plate-like, tetrapod-like) zinc oxide (zinc oxide having shape anisotropy) prepared through a hydrothermal synthesis process. Among these zinc oxides, particulate zinc oxide having an average particle size of 50 to 200 nm is preferred, and particulate zinc oxide having an average particle size of 100 to 150 nm is particularly preferred. The average particle size referred to here is the particle size at which the cumulative mass distribution is 50% in the particle size distribution obtained by measurement using a laser diffraction / scattering type particle size distribution measuring device.
[0352] The amount of zinc oxide added is preferably 0.01 to 1 part by mass, more preferably 0.05 to 0.5 parts by mass, and even more preferably 0.1 to 0.3 parts by mass, based on 100 parts by mass of the thermoplastic resin composition.
[0353] (Inorganic filler) The thermoplastic resin composition of the present embodiment may contain an inorganic filler as a reinforcing filler for the purpose of imparting rigidity and improving strength.
[0354] Examples of inorganic fillers include talc, wollastonite, mica, clay, monmonrilonite, smectite, kaolin, calcium carbonate, glass fiber, glass beads, glass balloons, glass milled fiber, glass flakes, carbon fiber, carbon flakes, carbon beads, carbon milled fiber, metal flakes, metal fibers, metal-coated glass fiber, metal-coated carbon fiber, metal-coated glass flakes, silica, ceramic particles, ceramic fibers, ceramic balloons, aramid particles, aramid fibers, polyarylate fibers, graphite, potassium titanate whiskers, aluminum borate whiskers, basic magnesium sulfate, and various other whiskers. Among these, silicate-based fillers such as talc, wollastonite, mica, glass fiber, and glass milled fiber are preferably used. Among these, talc, wollastonite, and mica are particularly preferred.
[0355] When an inorganic filler is blended, the thermoplastic resin composition of the present embodiment may contain an additive containing an acidic group such as a carboxylic anhydride group or a sulfonic acid group in order to improve the wettability of the inorganic filler.
[0356] The content of the inorganic filler in the present embodiment is preferably 0.1 to 30 parts by mass, more preferably 0.5 to 20 parts by mass, and even more preferably 1 to 10 parts by mass, relative to 100 parts by mass of the thermoplastic resin composition. If the blending amount is less than 0.1 part by mass, the reinforcing effect of the filler is not obtained, and if it exceeds 30 parts by mass, the impact strength is significantly reduced, which is not preferable.
[0357] (Other optional ingredients) Other optional components that can be used in this embodiment include dyes for coloring, pigments, defoamers, plasticizers, lubricants, release agents, flame retardants, etc. Furthermore, it is also possible to blend thermoplastic resins other than the thermoplastic resin (A) and the hydrophilic copolymer (B) within a range that does not impair the object of this embodiment.
[0358] As such a thermoplastic resin, a thermoplastic resin used as a general-purpose resin in home appliances and office automation equipment can be used.
[0359] Examples of such thermoplastic resins include: Olefin-based resins include polyolefin-based resins (high-density polyethylene, low-density polyethylene, polypropylene, etc.), cyclic olefin-based resins, and polyester-based resins (polylactic acid, polyethylene terephthalate, polybutylene terephthalate, etc.); Styrene-based resins include polystyrene (PS resin), acrylonitrile butadiene styrene (ABS resin), and acrylonitrile styrene (AS resin). ASA resin is made by polymerizing acrylic rubber instead of butadiene in ABS resin. AES resin is made by polymerizing ethylene rubber instead of butadiene in ABS resin. Examples include methyl methacrylate butadiene styrene (MBS resin).
[0360] Other examples of general-purpose resins include polyvinyl chloride resins (polyvinyl chloride, polyvinylidene chloride, etc.), polymethyl methacrylate resins, polyvinyl alcohol, polyethylene terephthalate (PET resin), and polybutylene terephthalate (PBT resin).
[0361] Furthermore, examples of engineering plastics that are particularly strong and have enhanced functions such as heat resistance include polycarbonate resins (BPA-type polycarbonate, aliphatic polycarbonate, etc.), polyamide resins, polyphenylene ether resins (PPE resins), polyoxymethylene resins (polyacetal, etc.), polyphenylene sulfide resins, polyetherimide resins, aromatic polyether ketone resins, polysulfone resins, and polyamideimide resins.
[0362] These resins may be used alone or in combination as the raw material of the thermoplastic resin composition of the present embodiment. Examples of the resins include polymer alloys such as PC / ABS and PC / AS. Such polymer alloys have the characteristics of both polycarbonate (PC resin) and styrene-based resins (ABS resin, AS resin, etc.), and are used in a wide range of fields such as electrical and electronic equipment, office automation equipment, lighting equipment, precision machinery, automotive parts, and household goods.
[0363] Compared with the above-mentioned thermoplastic resin (A) and the hydrophilic copolymer (B) having an oxyethylene group (preferably a polyoxyethylene chain), the fatty acid metal salt (C) has a lower molecular weight. Therefore, regardless of which resin is used as a raw material, the fatty acid metal salt (C) is likely to be exposed on the surface of a molded article, and therefore it is possible to blend various resins into the thermoplastic resin composition.
[0364] Referring to FIG. 6, the fatty acid metal salt (C) and the hydrophilic copolymer (B) have different melt viscosities during molding. During molding, the thermoplastic resin (A) injected into the mold solidifies first, then the hydrophilic copolymer (B), and then the fatty acid metal salt (C) with a lower molecular weight. In other words, compared to the thermoplastic resin (A), the hydrophilic copolymer (B) and the fatty acid metal salt (C) have a slower solidification rate and therefore tend to be more easily exposed on the surface of the molded product. In this way, the hydrophilic copolymer (B) and the fatty acid metal salt (C) have different melt viscosities during molding from the thermoplastic resin (A), and therefore can be blended with the thermoplastic resin (A).
[0365] On the other hand, for example, a resin raw material having a high melting point (e.g., about 320°C or higher) and extremely high polarity is difficult to disperse, and therefore the desired dust suppression effect is difficult to obtain. In other words, the hydrophilic copolymer (B) and the fatty acid metal salt (C) are more likely to collect near the surface layer of the molded article than the above-mentioned thermoplastic resin (A), and therefore the dust suppression effect is more likely to be obtained.
[0366] Furthermore, the polar group of the low molecular weight fatty acid metal salt (C) has an affinity with the hydrophilic copolymer (B) having an oxyethylene group. Therefore, by the hydrophilic copolymer (B) adhering to the fatty acid metal salt (C), the hydrophilic copolymer (B) and the fatty acid metal salt (C) are prevented from being detached, and can be present in large quantities near the surface layer of the molded article. Therefore, the adhesion suppression effect is easily exerted against both hydrophilic and hydrophobic dust stains.
[0367] <Production of Thermoplastic Resin Composition> Any method may be adopted for producing the thermoplastic resin composition of the present embodiment. For example, the thermoplastic resin (A), the hydrophilic copolymer (B), the fatty acid metal salt (C) and optionally other additives may be thoroughly mixed using a premixing means such as a V-type blender, a Henschel mixer, a mechanochemical device, or an extrusion mixer, and then the premix is granulated as necessary using an extrusion granulator or a briquetting machine, and then melt-kneaded in a melt kneader such as a vented twin-screw extruder, and then pelletized using a pelletizer.
[0368] Other examples include a method of independently supplying each component to a melt kneader such as a vented twin-screw extruder, or a method of premixing a portion of each component and then supplying the remaining components to a melt kneader independently. Examples of a method of premixing a portion of each component include a method of premixing components other than the thermoplastic resin (A) in advance and then mixing them with the thermoplastic resin (A) or directly supplying them to the extruder.
[0369] The extruder preferably has a vent capable of degassing moisture in the raw materials and volatile gases generated from the melt-kneaded resin. A vacuum pump is preferably installed from the vent to efficiently discharge the generated moisture and volatile gases to the outside of the extruder. It is also possible to install a screen in a zone before the extruder die section to remove foreign matter mixed in the extrusion raw materials, thereby removing the foreign matter from the resin composition. Examples of such a screen include a wire mesh, a screen changer, and a sintered metal plate (such as a disk filter).
[0370] Examples of the melt kneader include a twin-screw extruder, a Banbury mixer, a kneading roll, a single-screw extruder, and a multi-screw extruder having three or more screws.
[0371] The thermoplastic resin composition extruded as described above is directly cut and pelletized, or formed into strands, which are then cut by a pelletizer and pelletized. The shape of the pellets is preferably cylindrical. The diameter of the cylinder is preferably 1 to 5 mm, more preferably 1.5 to 4 mm, and even more preferably 2 to 3.3 mm. Meanwhile, the length of the cylinder is preferably 1 to 30 mm, more preferably 2 to 5 mm, and even more preferably 2.5 to 3.5 mm.
[0372] The thermoplastic resin composition of the present embodiment can be used to produce various products by injection molding the pellets produced as described above to obtain molded products. In such injection molding, not only normal molding methods but also injection compression molding, injection press molding, gas-assisted injection molding, foam molding (including a method of injecting a supercritical fluid), insert molding, in-mold coating molding, heat-insulating mold molding, rapid heating and cooling mold molding, two-color molding, sandwich molding, and ultra-high speed injection molding can be used. In addition, molding can be performed using either a cold runner system or a hot runner system.
[0373] The thermoplastic resin composition of the present embodiment can also be used in the form of various profile extrusion molded products, sheets, films, etc. by extrusion molding. For molding sheets and films, inflation methods, calendaring methods, casting methods, etc. can also be used. Furthermore, it is possible to mold it into a heat shrinkable tube by applying a stretching operation. The thermoplastic resin composition of the present embodiment can also be made into a molded product by rotational molding, blow molding, etc.
[0374] Embodiment 2 The molded article according to the present embodiment is made of the above-mentioned thermoplastic resin composition. Since the molded article according to the present embodiment is made of the above-mentioned thermoplastic resin composition, it has an effect of suppressing adhesion of both hydrophilic dust stains and hydrophobic dust stains.
[0375] In the molded article according to the present embodiment, the concentration of fatty acid metal salt (C) (content in the thermoplastic resin composition) near the surface of the molded article (a portion up to a certain depth from the surface) is preferably higher than the concentration of fatty acid metal salt (C) inside the molded article (a portion deeper than a certain depth from the surface). Specifically, for example, the concentration of fatty acid metal salt (C) within 10 nm from the surface of the molded article is preferably higher than the concentration of fatty acid metal salt (C) in a portion deeper than 10 nm from the surface of the molded article.
[0376] The "surface of a molded article" referred to here means at least a portion of the surface of the molded article, and does not necessarily mean the entire surface of the molded article, but may be a portion of the surface of the molded article.
[0377] Such a difference in the concentration of the fatty acid metal salt (C) in the depth direction of the molded article can be confirmed, for example, by scraping the surface of the molded article with Ar ions and performing elemental analysis of the metal element M (measurement of the area ratio of the metal element M) using X-ray photoelectron spectroscopy (XPS) on the surface of the molded article that has been scraped to each depth (see Figure 2).
[0378] For example, as shown in Figure 1, the concentration of fatty acid metal salt (C) (area ratio of metal element M) is measured at each depth within 10 nm from the surface of the molded article (measurement depth A), and the highest concentration is determined. Meanwhile, the concentration of fatty acid metal salt (C) is measured at a depth half the thickness L of the molded article (L / 2: measurement depth B), as indicated by the dotted line in Figure 1. By comparing these concentration measurements, the difference in the concentration of fatty acid metal salt (C) in the depth direction of the molded article can be confirmed.
[0379] For example, in a sample (test piece) of a molded article having an amphoteric antifouling effect described later in the Examples, the concentration of fatty acid metal salt (C) within 10 nm from the surface was more than twice as high as the concentration of fatty acid metal salt (C) within 10 nm from the surface of the molded article. In a specific example, the concentration of fatty acid metal salt (C) within 10 nm from the surface was up to 3.2 mass%, and the concentration of fatty acid metal salt (C) within 10 nm from the surface of the molded article was about 0.3 mass% to 0.6 mass%, the former being about 5 to 10 times the latter.
[0380] In the fatty acid metal salt (C), the R portion is a non-polar group, and the remaining portion is a polar group. During molding, the polar group adheres to the mold, and the fatty acid metal salt (C) is thought to be aligned with the non-polar group facing the inside of the thermoplastic resin composition. Furthermore, after molding, other fatty acid metal salts (C) that were melted inside the thermoplastic resin composition migrate to the surface.
[0381] In addition, since the fatty acid metal salt (C) has low compatibility with thermoplastic resins, when it is blended in an amount equal to or greater than the critical solubility (concentration), it is diffused to the surface of the thermoplastic resin composition (molded article). In the vicinity of the surface of the thermoplastic resin composition, it is believed that the polar groups of the fatty acid metal salts (C) are bonded to each other and arranged with the hydrophobic group R, which is a non-polar group, facing the outside (air side) of the molded article.
[0382] Therefore, the concentration of the fatty acid metal salt (C) in the thermoplastic resin composition is higher near the surface of the molded article than inside the molded article, and the surface energy can be efficiently reduced and a water- and oil-repellent effect can be obtained on the surface of the molded article to which dust stains adhere. As a result, unlike the case where the fatty acid metal salt (C) is used as a lubricant, mold release agent, etc., which are general applications, a new effect of suppressing the adhesion of hydrophobic dust stains on the surface of the molded article can be obtained.
[0383] In addition, when a resin material is liquefied once and then molded into an arbitrary shape when forming a molded product, the above-mentioned effect can be obtained if the component ratio of the thermoplastic resin composition according to embodiment 1 is achieved at the liquefaction stage. For example, at the stage of liquefying the resin material, the thermoplastic resin composition of this embodiment can contain the optional components described in embodiment 1.
[0384] Embodiment 3 The product of the present embodiment includes the molded product described above. That is, the molded product described above is used as a resin part (internal part, housing, etc.) for products such as home appliances and office automation equipment. By including the molded product of the present embodiment, the product can achieve the effects of improving cleanliness and reducing the frequency of maintenance.
[0385] Examples of products include personal computers, laptop computers, CRT displays, printers, mobile terminals, mobile phones, copy machines, fax machines, recording media (CD, CD-ROM, DVD, PD, FDD, etc.), drives, parabolic antennas, power tools, VTRs, televisions, irons, hair dryers, rice cookers, microwave ovens, audio equipment, audio equipment (audio, LaserDisc (registered trademark), compact discs, etc.), lighting equipment (LED), remote controls, ventilation fans, range hoods, refrigerators, air conditioners (air conditioners, dehumidifiers, humidifiers, etc.), air purifiers, vacuum cleaners, rice cookers, cooking heaters, bath products, washroom products, jet towels, electric fans, typewriters, word processors, automobiles, vehicle equipment (car navigation, car stereos, etc.), and miscellaneous goods.
[0386] Furthermore, if the above-mentioned molded article is applied to resin parts such as air conditioners, doors, display devices, insulators, mirrors, measuring instruments, and operation parts of various devices, adhesion of dust and dirt is reduced, cleanliness is improved, and the frequency of maintenance can be reduced. The above-mentioned molded article is particularly useful as a resin part for products that cannot be maintained for long periods by users or contractors.
[0387] The molded article containing the thermoplastic resin composition of the present embodiment can be applied to any product having a resin part, and can be widely used in applications other than those mentioned above.
[0388] In addition, since the antifouling effect can be easily obtained by molding alone, there is an advantage that the number of complicated steps such as moving the molded product and applying work is overwhelmingly fewer than in painting or coating with an antifouling effect. Therefore, the molded product containing the above-mentioned thermoplastic resin composition is suitable for mass production of products and has extremely high practicality. In addition, compared to painting or coating with an antifouling effect, the molded product containing the above-mentioned thermoplastic resin composition has the advantage that it is easily applied as an exterior member without having to worry about uneven coating on the surface, rainbow patterns, glossiness, etc., and is suitable for mass production of products and has extremely high practicality.
[0389] Fig. 5 is a schematic cross-sectional view of an air conditioner according to this embodiment. As shown in Fig. 5, a main body case 10 of the indoor unit of the air conditioner is formed in a horizontally elongated, substantially rectangular parallelepiped shape, with an air intake port 11 provided on the top surface and an air outlet port 12 provided on the lower front surface. A pre-filter 17 is provided from the downstream side of the air intake port 11 to the front surface of the main body case 10. In addition, a front panel 14 is provided to cover the front surface of the main body case 10.
[0390] A fan 13 is provided inside the main body case 10 to draw indoor air drawn in through the air inlet 11 into the room through the air outlet 12. A heat exchanger 22 is provided upstream of the fan 13, and an air passage 21 is provided downstream of the fan 13, through which the air passes. A drain pan 18 is provided below the heat exchanger 22.
[0391] Although not shown, a fan motor for driving the fan 13, a control unit for controlling the operation of the air conditioner, etc. are provided within the main body case 10.
[0392] The up-down air deflectors 15, 16 adjust the up-down blowing angle of the air blown out from the air outlet 12. The left-right air deflector 19 adjusts the left-right blowing angle of the air blown out from the air outlet 12. A support shaft is provided at the end of each of the up-down air deflectors 15, 16, and the shaft is rotatably and detachably supported by a bearing provided on the side wall of the air outlet 12. The left-right air deflector 19 may be fixed, the direction may be manually set, or it may be driven by a motor to automatically rotate left-right.
[0393] When the fan 13 is driven, indoor air is sucked in through the air inlet 11, passes through the pre-filter 17, the heat exchanger 22, the fan 13, the air passage 21, the air outlet 12, the left and right air deflectors 19, and the top and bottom air deflectors 15, 16 in this order, and is blown out into the room. Hydrophilic dust dirt such as dust, sand, and fibers, and hydrophobic dust dirt such as oily smoke, soot, sebum, and tobacco come into contact with various air conditioner components together with the air, so the air inlet 11, the pre-filter 17, the heat exchanger 22, the fan 13, the air passage 21, the air outlet 12, the left and right air deflectors 19, and the top and bottom air deflectors 15, 16 are constantly soiled. In addition, the sucked-in air also comes into contact with the rear wall 20 facing the pre-filter 17 of the front panel 14, so the rear wall 20 also continues to be soiled.
[0394] Styrene-based resins such as PS or ABS are often used as materials for the front panel 14, air outlet 12, left and right air deflectors 19, top and bottom air deflectors 15, 16, air passage 21, and rear wall 20. An olefin-based resin such as polypropylene (PP) is often used as a material for the frame of the prefilter 17. An olefin-based resin such as PP or a styrene-based resin such as AS is often used as a material for the fan 13.
[0395] The molded article containing the above thermoplastic resin composition can be suitably used for products that are constantly subject to soiling, such as air conditioners.
[0396] When a molded article containing the above thermoplastic resin composition is applied to an air conditioner, the dirt on the components can be reduced, so that improved cleanliness and reduced maintenance frequency can be expected. In addition, since the dirt does not scatter again, the discomfort caused by the odor caused by the dirt that arrives with the wind can be reduced. In addition, the growth of mold that uses the attached dirt as nutrients can be suppressed. In addition, products installed high on the ceiling such as air conditioners require users to clean them using a stepladder or the like, making cleaning difficult, but the application of the above molded article can reduce the frequency of cleaning, which is particularly preferable for the elderly and the like.
[0397] Furthermore, if dirt accumulates in the gaps of fan 13 and fills them, or if dirt accumulates on the surfaces of the various air passages, narrowing the air passage, problems can occur such as a decrease in airflow, which reduces the heating / cooling capacity, and an increase in power consumption by the fan; however, by applying the above-mentioned molded product, dirt can be suppressed, making it possible to maintain the initial airflow volume and suppress an increase in power consumption.
[0398] In addition, for example, vegetable trays in refrigerators often use styrene-based resins such as ABS and PS, or olefin-based resins such as PP. Dust boxes in vacuum cleaners often use styrene-based resins such as ABS and PS, or olefin-based resins such as PP. Olefin-based resins such as PP are often used for the sirocco fans of various types of ventilation fans and the fans of electric fans. In all cases, the reduction in dirt can reduce the effort required for maintenance. EXAMPLES
[0399] <Evaluation method> (1) Tensile strength Tensile strength (tensile yield strength) was measured according to ISO 527-1, 2. The measured value was compared with the tensile strength of the styrene-based resin (component A) alone and evaluated according to the following criteria.
[0400] [Evaluation criteria for tensile strength] A: Retention rate is 95% or more, B: Retention rate is less than 95%, 90% or more, C: Retention rate is less than 90%, 85% or more, D: Retention rate is less than 85% (2) Flexural modulus The flexural modulus was measured in accordance with ISO 178 (test piece dimensions: length 80 mm x width 10 mm x thickness 4 mm). The measured value was compared with the flexural modulus of the styrene-based resin (component A) used, and evaluated based on the following criteria.
[0401] [Evaluation criteria for bending modulus] A: Retention rate is 95% or more, B: Retention rate is less than 95%, 90% or more, C: Retention rate is less than 90%, 85% or more, D: Retention rate is less than 85% (3) Charpy impact strength The notched Charpy impact strength measurements were carried out according to ISO 179. (4) Surface impact strength Square plates of 150mm x 150mm x 2mm (thickness) were molded using an injection molding machine, and high-speed surface impact tests were carried out with N = 5 to measure the surface impact strength (fracture energy) and calculate the average value for N = 5. In addition, the fracture mode was evaluated based on the following criteria.
[0402] [Evaluation criteria for destruction mode] A: Ductile fracture, B: Mixture of ductile and brittle fractures (ductile fractures: number of fractures > number of brittle fractures), C: Mixture of ductile and brittle fractures (brittle fractures: number of fractures > number of ductile fractures), D: Brittle fracture The fracture morphology was evaluated as follows: a test piece that did not break or scatter after the impact test, and the impact core penetration part remained uniformly protruding, was rated as a ductile fracture; a test piece that broke into the impact core or the shape of a pedestal, and the impact core penetration part remained flat with a sharp end face, was rated as a brittle fracture. A ductile fracture morphology is more preferable than a brittle fracture morphology.
[0403] The test machine used was a high-speed surface impact tester, Hydroshot HTM-1 (manufactured by Shimadzu Corporation). The test conditions were a core impact speed of 7 m / s, a core with a semicircular tip and a radius of 6.35 mm, and a receiving hole diameter of 25.4 mm. (5) Deflection temperature under load The deflection temperature under load was measured according to ISO 75-1 and 75-2. The measurement load was 1.80 MPa. (6) Evaluation of dust adhesion A square plate measuring 150 mm x 150 mm x 2 mm (thickness) was prepared and left for one week in an environment of 23°C and 50% humidity, after which a dust adhesion test was carried out on the square plate. Kanto loam (JIS test powder type 11) was used to evaluate hydrophilic dust adhesion, and carbon black (JIS test powder type 12) was used to evaluate hydrophobic dust adhesion.
[0404] Dust adhesion was evaluated by blowing a certain amount of dust (5g) onto the surface of the molded product with air, then observing the surface of the molded product at 100x magnification using a KEYENCE VHX-5000 digital microscope, determining the percentage of the dust-adhered area through image processing, and evaluating it based on the following criteria.
[0405] [Evaluation criteria for dust adhesion] A: Dust adhesion area ratio is less than 3%, B: Dust adhesion area ratio is 3-6%, C: Dust adhesion area ratio is 6-9%, D: Dust adhesion area ratio is 9% or more <Examples 1 to 20 and Comparative Examples 1 to 20> 100 parts by mass of components A to C shown in Tables 1 to 8 (total amount of components A to C), 0.3 parts by mass of a release agent [product name: Likester EW400 (manufactured by Riken Vitamin Co., Ltd.)], 0.1 parts by mass of a phosphorus-based heat stabilizer [product name: IRGAFOS168 (manufactured by BASF)], 0.1 parts by mass of a phenol-based heat stabilizer [product name: IRGANOX1076 (manufactured by BASF)], 0.2 parts by mass of a hindered amine-based light stabilizer [product name: Adeka STAB LA-57 (manufactured by ADEKA Corporation)], and 0.1 parts by mass of a bendtriazole-based ultraviolet absorber [product name: SEESORB701 (manufactured by Shipro Kasei Co., Ltd.)] were mixed in a V-type blender to obtain a mixture.
[0406] The obtained mixture was fed from the first feed port of the extruder. The feed rate of the raw material (mixture) was precisely measured by a weighing scale [CWF manufactured by Kubota Corporation]. For the extrusion of the raw material, a vented twin screw extruder (TEX30α-38.5BW-3V manufactured by Japan Steel Works, Ltd.) with a diameter of 30 mm was used, and the raw material was melt-kneaded under the conditions of a screw rotation speed of 200 rpm, a discharge rate of 20 kg / h, and a vent vacuum of 3 kPa to obtain pellets of a thermoplastic resin composition. As for the extrusion temperature, the temperature from the first feed port to the die portion was set to the temperature shown in the table.
[0407] A part of the obtained pellets was dried in a hot air circulation dryer at the temperature shown in the table for 4 hours, and then molded into evaluation test pieces (Examples 1 to 20 and Comparative Examples 1 to 20) using an injection molding machine (FANUC Corporation T-150D). The basic conditions for injection molding were the cylinder temperature and mold temperature shown in the table, and the injection speed was 20 mm / s.
[0408] Components A to C (each component represented by a symbol) shown in Tables 1 to 8 are as follows. [Component A] (PC:A1 component-1) Aromatic polycarbonate resin [Teijin Ltd. Panlite L-1225WX bisphenol A polycarbonate resin, viscosity average molecular weight = 19700] (ABS:A2 component-1) ABS resin [Clarastic SXH-330 (product name), manufactured by Japan A&L Co., Ltd., weight average molecular weight converted to standard polystyrene by GPC measurement: 90,000, butadiene rubber component: approx. 17.5% by weight, weight average rubber particle diameter: 0.40 μm] (PET:A3 component-1) Polyethylene terephthalate resin [Teijin Limited PET resin TR-8580H using Ge catalyst, IV=0.83] (PBT:A3 component-2) Polybutylene terephthalate resin (Polyplastics Co., Ltd., Duranex 500FP EF202X, IV=0.85) (m-PPE:A4 component-1) Modified polyphenylene ether resin [Polyphenylene ether obtained by oxidative polymerization of 2,6-xylenol (reduced viscosity measured at 30°C in a chloroform solution with a concentration of 0.5 g / dL = 0.42 dL / g) and HIPS (H8672 manufactured by PS Japan Co., Ltd.) were melt-kneaded in a weight ratio of 40 / 60 using a vented twin-screw extruder with a diameter of 30 mm (TEX30α-38.5BW-3V manufactured by Japan Steel Works, Ltd.) at a cylinder temperature of 300°C, a screw rotation speed of 200 rpm, a discharge rate of 20 kg / h, and a vent vacuum of 3 kPa.] (PMMA:A5 component-1) Polymethyl methacrylate resin [High impact methacrylic resin: Mitsubishi Rayon Co., Ltd., ACRYPET IRS204, acrylic resin consisting of acrylic resin matrix component and acrylic rubber component, MFR = 13g / 10min (230℃ / 3.8kgf)] (PPS:A6 component-1) Polyphenylene sulfide resin [16.5 kg of sodium sulfide (containing 49% water of crystallization), 6.5 kg of sodium hydroxide, 5.2 kg of sodium acetate, and 22.0 kg of N-methyl-2-pyrrolidone were charged and dehydrated at 210°C, after which 20.5 kg of 1,4-dichlorobenzene and 20.0 kg of N-methyl-2-pyrrolidone were added and reacted at 265°C for 5 hours. The reaction product was washed with water and then dried to obtain the product. The glass transition temperature was 90°C, the melting point was 280°C, and the number average molecular weight was 11,500.] (PA6:A8 component-1) Polyamide 6 resin [Amilan CM1017, manufactured by Toray Industries, Inc., melting point = 225°C] (PA66:A8 component-2) Polyamide 66 resin [Amilan CM3001-N, manufactured by Toray Industries, Inc., melting point = 260°C] [B component] A hydrophilic copolymer (surface resistance: 8×10 8 Ω) (Production of component B) 1,4-Cyclohexanedimethanol (544 g), adipic acid (558 g), and isophthalic acid (33 g) were polymerized in the presence of an antioxidant using a titanate catalyst at 210°C under reduced pressure for 3 hours to obtain a polyester having carboxyl groups at both ends.
[0409] The polyester (600 g) and polyethylene glycol (300 g) having hydroxyl groups at both ends were polymerized at 210°C under reduced pressure for 7 hours in the presence of an antioxidant using a zirconium catalyst to obtain an alternating copolymer having carboxyl groups at both ends.
[0410] The obtained alternating copolymer (300 g) and trimethylolpropane (2.3 g) were polymerized at 240° C. under reduced pressure for 6 hours to obtain a hydrophilic copolymer (component B: PEPO) having a structure in which blocks derived from the alternating copolymer are bonded via blocks derived from trimethylolpropane. The surface resistance value of the obtained component B was 8×10 8 The melting point of component B was about 90 to 100°C.
[0411] [C component] (StAl) Aluminum (hydroxy) distearate [NOF Corporation, Aluminum Stearate 600 (product name), metal content = 8.5-10.0%, free fatty acid = 12.0% or less, melting point: 150-160°C] The evaluation results of the above items (1) to (6) for the obtained test pieces for evaluation (Examples 1 to 20 and Comparative Examples 1 to 20) are shown in Tables 1 to 8. However, not all of the above items (1) to (6) were evaluated for all of the Examples and Comparative Examples.
[0412] [Table 1]
[0413] [Table 2]
[0414] [Table 3]
[0415] [Table 4]
[0416] [Table 5]
[0417] [Table 6]
[0418] [Table 7]
[0419] [Table 8]
[0420] From the evaluation results shown in Tables 1 to 8, it can be confirmed that the examples, which are molded articles containing a thermoplastic resin composition containing a thermoplastic resin (A), a hydrophilic copolymer having an oxyethylene group (B), and a fatty acid metal salt (C), provide an excellent adhesion inhibition effect (anti-fouling effect) against hydrophilic and hydrophobic dust stains.
[0421] Furthermore, it was confirmed that by adjusting the blending amount of each component, good mechanical strength of the molded product could be obtained.
[0422] Furthermore, when (hydroxy)aluminum distearate is used as the fatty acid metal salt (C) (i.e., when a metal salt containing two fatty acids is used when the valence of the metal element M is 3), there is a tendency for the adhesion inhibitory effect (anti-fouling effect) against both hydrophilic and hydrophobic dust stains to be superior compared to when zinc stearate, aluminum monostearate or aluminum tristearate is used.
[0423] The embodiments and examples disclosed herein should be considered to be illustrative and not restrictive in all respects. The scope of the present disclosure is defined by the claims, not the above description, and is intended to include all modifications within the meaning and scope of the claims. [Explanation of symbols]
[0424] 10 main body case, 11 air intake, 12 air outlet, 13 fan, 14 front panel, 15, 16 upper and lower air deflectors, 17 pre-filter, 18 drain pan, 19 left and right air deflectors, 20 rear wall, 21 air duct, 22 heat exchanger.
Claims
1. A thermoplastic resin (A) selected from the group consisting of aromatic polycarbonate resins (A1), styrene-based resins (A2), aromatic polyester resins (A3), polyphenylene ether-based resins (A4), methacrylic resins (A5), polyarylene sulfide resins (A6), olefin-based resins (A7), polyamide resins (A8), and mixtures thereof; a hydrophilic copolymer (B) having an oxyethylene group; and a fatty acid metal salt (C) represented by the following formula (1), The hydrophilic copolymer (B) is a thermoplastic resin composition in which a plurality of alternating copolymers (a) of a polyester (a1) and a hydrophilic polymer (a2) having an oxyethylene group are bonded via ester bonds to at least one compound selected from the group consisting of a polyhydric alcohol compound (b1) having three or more hydroxyl groups, an epoxy compound (b2) having two or more epoxy groups, and a polycarboxylic acid compound (b3). M(OH)y(R-COO)x...(1) (In formula (1), R is an alkyl group or alkenyl group having 6 to 40 carbon atoms. M is at least one metal element selected from the group consisting of aluminum and zinc. x and y are each independent integers of 0 or more, and satisfy the relationship x + y = [valence of M].)
2. The thermoplastic resin composition according to claim 1, comprising: 100 parts by mass of the thermoplastic resin (A); 1 to 20 parts by mass of the hydrophilic copolymer (B); and 0.5 to 10 parts by mass of the fatty acid metal salt (C).
3. The thermoplastic resin composition according to claim 1 or 2, wherein, in formula (1), M is aluminum.
4. The thermoplastic resin composition according to any one of claims 1 to 3, wherein in the formula (1), the valence of M is 3 or more and y is 1.
5. The thermoplastic resin composition according to any one of claims 1 to 4, wherein the styrene-based resin (A2) is selected from the group consisting of PS resin, HIPS resin, MS resin, ABS resin, AS resin, AES resin, ASA resin, MBS resin, MABS resin, MAS resin, and mixtures thereof.
6. The thermoplastic resin composition according to any one of claims 1 to 5, wherein the aromatic polyester resin (A3) is selected from the group consisting of polybutylene terephthalate resin, polyethylene terephthalate resin, and mixtures thereof.
7. A molded article comprising the thermoplastic resin composition according to any one of claims 1 to 6.
8. 8. The molded article according to claim 7, wherein the concentration of the fatty acid metal salt (C) in a portion from the surface of the molded article to a certain depth is higher than the concentration of the fatty acid metal salt (C) in a portion deeper than the certain depth from the surface of the molded article.
9. A product comprising the molded article according to claim 7 or 8.
Citation Information
Patent Citations
Novel polyolefinic composition
JP1983118838A
Thermoplastic resin composition
JP1991290464A
Block polymer and antistatic agent from the same
JP2001278985A
Antistatic polyolefin-based resin composition
JP2011256293A
Antistatic thermoplastic resin composition and molded body formed by molding the same
JP2017128676A