Poly(ether ketone ketone) (PEKK) polymers and composites
By controlling reactant ratios and using low metal monomers, PEKK polymers with enhanced melt stability are produced, addressing processing challenges and enabling cost-effective production of thick composites with improved mechanical properties.
Patent Information
- Application Number
- JP2020571418
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-01-22
- Filing Date
- 2019-06-19
- Publication Date
- 2024-09-25
- Estimated Expiration
- 2039-06-19
AI Technical Summary
Existing PEKK polymers face challenges in processing due to high crystallinity and melting temperature, leading to poor consolidation and degradation during the production of thick composites using vacuum bag-only technology, requiring expensive equipment and long residence times.
The production of PEKK polymers with improved melt stability is achieved by using low metal monomers and controlling the relative amounts of reactants, particularly bis(hydroxybenzoyl)benzene and bis(halobenzoyl)benzene monomers in specific molar ratios, along with the use of sodium and potassium carbonate, to enhance melt stability and allow for cost-effective production of thick composites.
The resulting PEKK polymers exhibit significantly improved melt stability, enabling the production of thick composite products using vacuum bag-only technology without compromising toughness, and can be processed into high-quality composite materials with reduced void content and enhanced mechanical properties.
Smart Images

Figure 0007555828000018 
Figure 0007555828000001 
Figure 0007555828000002
Abstract
Description
[Technical field]
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS This application claims priority to U.S. Provisional Application No. 62 / 688047, filed June 21, 2018; European Patent Application No. 18184038.0, filed July 17, 2018; U.S. Provisional Application No. 62 / 782725, filed December 20, 2018; and European Patent Application No. 19153019.5, filed January 22, 2019, the entire contents of each of which are incorporated herein by reference for all purposes.
[0002] The present invention relates to poly(ether ketone ketone) (PEKK) polymers, their manufacture, articles and composites made therefrom, methods of making composites, and composite products comprising PEKK composites. [Background technology]
[0003] Poly(ether ketone ketone) polymers (hereinafter referred to as "PEKK polymers") are well suited for use in relatively extreme conditions. Due in part to the high crystallinity and high melting temperature of PEKK polymers, they have excellent thermal, physical and mechanical properties that make them well suited for use as the polymer matrix in continuous fiber reinforced composites. Such properties make PEKK polymers and their composites desirable in a wide range of demanding application contexts, including, but not limited to, aerospace and oil and gas drilling.
[0004] Nevertheless, the same high crystallinity and high melt temperature that provide many of the benefits of PEKK polymers also present problems in processing such polymers. For example, WO 2018 / 115035 (Solvay Specialty Polymers USA, LLC.) discloses that selective control of the relative amounts of reactants during synthesis can result in PEKK polymers with lower melt viscosities and therefore improved processability.
[0005] Also, it is not currently possible to produce thick PEKK composites (e.g., 60 plies or more) without compromising toughness without the use of large, expensive equipment, such as industrial-sized autoclaves, to limit the exposure of the molten resin to long residence times at high temperatures. Composites can be produced, for example, using the simpler, smaller-scale, and more cost-effective VBO (vacuum bag only) technique, in which layers of composite are applied sequentially to form the final composite product. However, this technique requires long residence times at high temperature levels as each new layer fuses to the layer that precedes it. If the polymer matrix does not have sufficient melt stability, poorly consolidated areas and degradation can occur when producing thick PEKK composites using this method. Summary of the Invention [Means for solving the problem]
[0006] The Applicant has now discovered that not all PEKK polymers obtained by the process disclosed in WO 2018 / 115035 exhibit a high degree of crystallinity, which makes the PEKK polymers useful for the production of composite materials in the form of a mixture with reinforcing fibres such as glass fibres or carbon fibres.
[0007] In addition, Applicants have recognized that there remains a need for PEKK polymers that have improved melt stability.
[0008] In another aspect, Applicants have recognized that there is a need for PEKK composites that have improved melt stability and are suitable for manufacturing thick composites using cost-effective techniques without compromising toughness.
[0009] The Applicant therefore faced the problem of providing a PEKK polymer characterized by an improved melt stability compared to the PEKK polymers obtained from processes already known in the art.
[0010] Applicants have surprisingly discovered that by using low metal monomers and selectively controlling the relative amounts of reactants during synthesis, they can produce PEKK polymers that have unexpectedly improved melt stability compared to PEKK polymers synthesized by conventional methods.
[0011] Additionally, applicants have surprisingly found that controlling the amount of fluorine in the end groups of the PEKK polymer affects, and therefore can control, the melt stability of the PEKK polymer.Applicants have surprisingly found that PEKK polymers having a desired amount of fluorine in the end groups can be prepared by a process that includes reacting bis(halobenzoyl)benzene monomers with bis(hydroxybenzoyl)benzene monomers in a molar ratio of 1.007:1 or greater.
[0012] Due to the unexpectedly improved melt stability of the PEKK polymers, PEKK composites comprising the PEKK polymers described herein are particularly well suited for the manufacture of thick composite products (i.e., products having at least a portion at least 4 mm thick). Furthermore, composite products comprising the PEKK composites of the present invention can be manufactured using the more cost-effective vacuum bag only ("VBO") technique.
[0013] In view of the above, in a first aspect, the present invention provides a poly(ether ketone ketone) polymer [PEKK S Polymer] manufacturing method [Method (M S ), the method comprises the steps of: (I) reacting at least one low metal bis(hydroxybenzoyl)benzene monomer [monomer (HB)] with at least one low metal bis(halobenzoyl)benzene monomer [monomer (FB)] in the presence of Na2CO3, K2CO3, and a solvent in a reaction mixture, · General formula-[M m At least one repeating unit (R M*PEKK )and, · General formula-[M p At least one repeating unit (R P* PEKK )and, (In these formulas, M m and M p are expressed by the following equations (3) and (4), respectively. At least one PEKK containing S Obtaining a mixture containing a polymer, comprising: the monomer (FB) and the monomer (HB) are in a molar ratio of at least 1.007:1; The relative amounts of the component reactants in step (I) are determined according to the following formula: (EQ1)Σ=(%Na2CO3-105)+6*|%K2CO3-1|+0.25*|37-%Monomers|-(%XS DFDK ) and (EQ2) 0%≦K2CO3<5 and (EQ3) 0.7%<%XS DFDK and (EQ4) 25%≦Monomers≦44% is selected according to the formula: (a) Σ<6; (b) %Na2CO3 is the concentration of Na2CO3 in mole % relative to the number of moles of said monomer (HB); (c) %K2CO3 is the concentration of K2CO3 in mole % relative to the number of moles of said monomer (HB), and %K2CO3 is in the range of 0 mole % to less than 5 mole %; (d) %Monomers is the total concentration of the monomer (HB) and the monomer (FB) in weight percent relative to the weight of the monomer (HB), the monomer (FB), and the solvent, and %Monomers is 25% by weight to 44% by weight; (e)%XS DFDK is the concentration in mole % of said monomer (FB) over an equimolar concentration of said monomer (HB); The monomer (HB) and the monomer (FB) have the following formula: X 5 -Mm -X 5 (13) X 6 -M p -X 6 (14) and During the ceremony, X 5 and X 6 is -OH for said monomer (HB) and is a halogen, preferably Cl or F, more preferably F, for said monomer (FB), M m and M p are expressed by the following formulas, respectively. Represented by TIFF0007555828000001.tif104170, During the ceremony, Each of R1 and R2 is independently selected from the group consisting of alkyl, alkenyl, alkynyl, aryl, ether, thioether, carboxylic acid, ester, amide, imide, alkali or alkaline earth metal sulfonate, alkyl sulfonate, alkali or alkaline earth metal phosphonate, alkyl phosphonate, amine, and quaternary ammonium; each of i and j is independently selected from 0 or an integer from 1 to 4; PEKK S Polymer: %[F]>45(μeq / g) / (g / 10min) 0.29 and a T / I ratio of more than 61 / 39, more preferably at least 65 / 35, and most preferably at least 68 / 32; Where: %[F] is [F] i.e. 19 The concentration of fluorine end groups in PEKK polymers measured by F-NMR and the MFI, i.e., the PEKK polymer concentration measured at 360 °C under a load of 8.4 kg according to ASTM D1238. S is the ratio between the melt flow index of the polymer to the power of 0.29; The T / I ratio is determined by the number of repeat units (R P* PEKK ) and repeating unit (R M* PEKK ) is the ratio between; process; (II) contacting the mixture containing at least one PEKK polymer obtained in step (I) with a solution containing sodium dihydrogen phosphate (NaH2PO4) and disodium hydrogen phosphate (Na2HPO4) to form the at least one PEKK polymer; S Isolating the polymer.
[0014] The applicant was also faced with the problem of providing a crystalline PEKK polymer that could be used to provide a composite material in the form of a blend with reinforcing fibers, and in fact, the applicant found that the quasi-amorphous PEKK polymers, despite having been obtained by a controlled manufacturing process, were not suitable for end use in composite materials.
[0015] Thus, in a second aspect, the present invention provides a method for producing a medicament for the treatment of a cancer, comprising: · General formula-[M m At least one repeating unit (R M* PEKK ); and · General formula-[M p At least one repeating unit (R P* PEKK ); (M in these formulas m and M p are expressed by the above formulas (3) and (4), respectively. Poly(ether ketone ketone) polymers [PEKK S Regarding the polymer, The PEKK polymer is %[F]>45(μeq / g) / (g / 10min) 0.29 , and characterized by a T / I ratio of more than 61 / 39, more preferably at least 65 / 35, and most preferably at least 68 / 32; Where: %[F] is [F] i.e. 19is the 0.29th power of the ratio between the concentration of fluorine end groups of the PEKK polymer measured by F-NMR and the MFI, or melt flow index, of the PEKK polymer measured at 360°C under a load of 8.4 Kg according to ASTM D1238; The T / I ratio is determined by the number of repeat units (R P* PEKK ) and repeating unit (R M* PEKK ) is the ratio between
[0016] In a third aspect, the present invention provides a poly(ether ketone ketone) polymer [PEKK C A method for producing a composite material comprising a polymer matrix comprising a polymer C ), the method comprising the steps of: (I * ) poly(ether ether ketone) (PEKK) is prepared by reacting at least one low metal bis(hydroxybenzoyl)benzene monomer [monomer (HB)] with at least one low metal bis(halobenzoyl)benzene monomer [monomer (FB)] in the presence of Na2CO3, K2CO3, and a solvent in a reaction mixture. C ) polymer is prepared, · General formula-[M m At least one repeating unit (R M* PEKK )and, · General formula-[M p At least one repeating unit (R P* PEKK )and, (In these formulas, M m and M p are expressed by the following equations (3) and (4), respectively. At least one PEKK containing C Obtaining a polymer matrix comprising a polymer, The relative amounts of the component reactants in step (I) are determined according to the following formula: (EQ1)Σ=(%Na2CO3-105)+6*|%K2CO3-1|+0.25*|37-%Monomers|-(%XSDFDK ) and (EQ2) 0%≦K2CO3<5 and (EQ3)0%<%XS DFDK and (EQ4) 25%≦Monomers≦44% is selected according to the formula: (a) Σ<6; (b) %Na2CO3 is the concentration of Na2CO3 in mole % relative to the number of moles of said monomer (HB); (c) %K2CO3 is the concentration of K2CO3 in mole % relative to the number of moles of said monomer (HB), and %K2CO3 is in the range of 0 mole % to less than 5 mole %; (d) %Monomers is the total concentration of the monomer (HB) and the monomer (FB) in weight percent relative to the weight of the monomer (HB), the monomer (FB), and the solvent, and %Monomers is 25% by weight to 44% by weight; (e)%XS DFDK is the concentration in mole % of said monomer (FB) over an equimolar concentration of said monomer (HB); The monomer (HB) and the monomer (FB) have the following formula: X 5 -M m -X 5 (13) X 6 -M p -X 6 (14) and During the ceremony, X 5 and X 6 is -OH for said monomer (HB) and is a halogen, preferably Cl or F, more preferably F, for said monomer (FB), M m and M p are expressed as follows: Represented by TIFF0007555828000002.tif106170, During the ceremony, Each of R1 and R2 is independently selected from the group consisting of alkyl, alkenyl, alkynyl, aryl, ether, thioether, carboxylic acid, ester, amide, imide, alkali or alkaline earth metal sulfonate, alkyl sulfonate, alkali or alkaline earth metal phosphonate, alkyl phosphonate, amine, and quaternary ammonium; Each of i and j is independently selected from 0 or an integer from 1 to 4; Process; (II * ) on the process (I * ) impregnating reinforcing fibers with the polymer matrix obtained in (a) to form a composite material.
[0017] In a further aspect, the present invention relates to a method as described above (M C ) The present invention relates to a composite material obtained by
[0018] According to this aspect, the present invention relates to a PEKK polymer. C The present invention relates to a composite material [Composite material (C)] comprising reinforcing fibers in said polymer matrix comprising a polymer, and further characterized by a complex viscosity ratio of 120 / 10 (parallel plate) in the range of 1.0 to 3.5, measured according to ASTM D4440 at 410°C, under nitrogen, 10 rad / s, 10 min and 120 min at 1% strain.
[0019] In another aspect, the present invention relates to a PEKK copolymer as defined above. S A composite material comprising a polymer and at least one reinforcing fiber, preferably selected from glass fibers or carbon fibers [composite material (C S )]. [Brief description of the drawings]
[0020] [Figure 1] 1 is a plot showing complex viscosity versus time for the PEKK polymer of Comparative Example 2 and the PEKK polymer of Example 5. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0021] For purposes of this specification: - the use of parentheses around symbols or numbers identifying compounds, chemical formulae or parts of formulae has the sole purpose of making those symbols or numbers easier to distinguish from the rest of the text, and therefore said parentheses may also be omitted; - the expression "low metal monomer" is intended to denote a monomer having a concentration of sodium and potassium less than 25 ppm by weight in sum and a concentration of calcium less than 10 ppm by weight, the metal concentrations being determined by inductively coupled plasma optical emission spectroscopy ("ICP-OES") as described in the examples. Low metal monomers can be prepared by methods known to those skilled in the art, for example by the methods described in International Application EP 2017 / 083672, filed December 19, 2017, which is incorporated herein by reference in its entirety; - the expression "crystalline PEKK polymer" is intended to refer to a PEKK polymer having a heat of fusion of at least 5 J / g, determined as the net (i.e. taking into account cold crystallization) area under the melting endotherm in the second heating scan in a differential scanning calorimeter (DSC) according to ASTM D3418-03 and E793-06 using heating and cooling rates of 20°C / min; - The expression "PEKK polymer" refers to said PEKK polymer, unless otherwise specified. S Polymer and PEKK C The term "polymer" is intended to refer to both polymers and non-polymers.
[0022] The polymer matrix was prepared according to the method described above (M C At least one PEKK obtained from C The polymer matrix may be prepared by methods well known in the art, including, for example, dry blending a PEKK polymer and any additional additives.
[0023] In some embodiments, the PEKK polymer is ground to a fine powder having an average particle size of less than 50 μm, preferably less than 30 μm.
[0024] Preferably, the PEKK polymer comprises at least one repeat unit (R M PEKK ) and at least one repeating unit (R P PEKK ).
[0025] Each repeating unit (R M PEKK ) is represented by the general formula (1): -[-M m -O-]- (1) It is expressed by the formula: Each repeating unit (R P PEKK ) is represented by the following general formula (2): -[-M p -O-]- (2) It is expressed by the formula: In these formulas, M m and M p are represented by the following general formulas (3) and (4): Represented by TIFF0007555828000003.tif102170, During the ceremony, R 1 and R 2 is independently selected in each occurrence from the group consisting of alkyl, alkenyl, alkynyl, aryl, ether, thioether, carboxylic acid, ester, amide, imide, alkali or alkaline earth metal sulfonate, alkyl sulfonate, alkali or alkaline earth metal phosphonate, alkyl phosphonate, amine, and quaternary ammonium; i and j, in each occurrence, are independently selected integers ranging from 0 to 4.
[0026] As used herein, dashed bonds indicate bonds to atoms outside the drawn structure. The subscripts "p" and "m" on the chemical species "M" reflect the respective para (Formula (4)) and meta (Formula (3)) benzoyl substitutions on the central benzene ring.
[0027] In some embodiments, each i and j is zero.
[0028] For clarity, in some embodiments, the PEKK polymer may be made up of multiple repeat units (R M PEKK ), multiple repeat units (R P PEKK ), or both. Therefore, M PEKK ) refers to all types of repeat units in PEKK according to general formula (1), and the repeat unit (R P PEKK ) refers to all types of repeat units in PEKK according to general formula (2).
[0029] As used herein, a PEKK polymer is a polymer that is made up of repeating units (R M PEKK ) and repeating unit (R P PEKK ) is at least 50 mole % relative to the total moles of repeat units in the PEKK polymer. M PEKK ) and repeating unit (R P PEKK ) is at least 60 mol%, at least 70 mol%, at least 80 mol%, at least 90 mol%, at least 95 mol%, or at least 99 mol%, based on the total moles of repeat units in the PEKK polymer.
[0030] Advantageously, said PEKK C In a polymer, the repeating unit (R M PEKK The number of moles of repeating units (R P PEKK The ratio of the total number of moles of (R P PEKK ) / (R M PEKK The "T / I ratio" or "T / I ratio" is in the range of 55 / 45 to 75 / 25, preferably 60 / 40 to 80 / 20, and more preferably 62 / 38 to 75 / 25.
[0031] Advantageously, said PEKK S In a polymer, the repeating unit (R P PEKK ) versus the total number of moles of repeat units (R M PEKK The ratio of the total number of moles of (R P PEKK ) / (R M PEKK ) ratio is at least about 1:1, at least about 1.2:1, at least about 1.3:1, at least about 1.4:1. Additionally or alternatively, P PEKK ) / (R M PEKK ) ratio is about 5.7:1 or less, about 5:1 or less, about 4:1 or less, about 3.5:1 or less, or about 3:1 or less, or about 2.7:1 or less.
[0032] In some embodiments, the repeating unit (R M PEKK ) is a repeating unit (R M1 PEKK ) and contains a repeating unit (R P PEKK ) is a repeating unit (R P1 PEKK ), (R P2 PEKK ), and (R P3 PEKK ).
[0033] Preferably, the repeating unit (R M1 PEKK ), (R P1 PEKK ), (R P2 PEKK ) and (R P3 PEKK ) are expressed by the following formulas (5) to (8): -[-M 1* m -O-]- (5) -[-M 1* p -O-]- (6) -[-M 2* p -O-]- (7) -[-M 3* p -O-]- (8) It is expressed as In these formulas: M 1* m , M 1* p , M 2* p , and M 3* p are expressed by the following equations (9) to (12): Represented by TIFF0007555828000004.tif197170, In these formulas: R 1* , R 2* , R 3* and R 4* is independently selected at each occurrence from the group consisting of alkyl, alkenyl, alkynyl, aryl, ether, thioether, carboxylic acid, ester, amide, imide, alkali or alkaline earth metal sulfonate, alkyl sulfonate, alkali or alkaline earth metal phosphonate, alkyl phosphonate, amine, and quaternary ammonium; i * , j * , k * and L * is an independently selected integer ranging from 0 to 4, in each occurrence.
[0034] In some embodiments, each i * , j * , k * and L * is zero.
[0035] In some embodiments, the repeating unit (R M1 PEKK ) and repeating units (R P1 PEKK ), (R P2 PEKK ) and (R P3 PEKK The total concentration of the repeating unit (R M PEKK ) and repeating unit (RP PEKK In some embodiments, the repeat unit (R P1 PEKK ), (R P2 PEKK ), and (R P3 PEKK ) versus the total number of moles of repeat units (R M1 PEKK The ratio of the number of moles of repeating units (R M PEKK ) and (R P PEKK ) are within the ranges set forth above.
[0036] As mentioned above, the PEKK of interest C The polymers unexpectedly exhibit improved melt stability compared to PEKK polymers produced by conventional methods. Thus, in some embodiments, the PEKK polymers exhibit complex viscosity ratios 120 / 10 (parallel plate) in the ranges of 1.0-3.0, 1.0-2.5, and 1.0-2.4, measured at 410° C. under nitrogen, 10 rad / s, 10 minutes, and 120 minutes at 1% strain, according to ASTM D4440. Further, in some embodiments, the PEKK C The polymers exhibit a melt stability (VR40) in the range of 1.0 to 1.3, preferably 1.0 to 1.25, measured according to ASTM D3835 as described in the Examples below.
[0037] As mentioned above, PEKK S The polymer is inh For example, they exhibit lower melt viscosity at the same mechanical properties. S The polymer can have a ΔMV that is −2 Pa s or less, where: ΔMV = MV (e) -MV (E1) TIFF0007555828000005.tif11170 during the ceremony, MV (e) is the expected melt viscosity in Pascal seconds ("Pa s"), and η inh is the intrinsic viscosity of the PEKK polymer in deciliters per gram ("dL / g").
[0038] Parameter m in Eq. mv and n are plots of MV vs. ηinh for various traditional PEKK polymers, and the curves This can be experimentally determined by fitting to TIFF0007555828000006.tif10170.
[0039] 61:39~65:35 (R P PEKK ) / (R M PEKK For PEKK polymers having a MV of 410° C., as described in the Examples below, m mv =1006(Pa·s)(g / dL) 3.90 And n=3.90.
[0040] (R P PEKK ) / (R M PEKK For preferred PEKK polymers having a m ) ratio of greater than 65:35 (1.86:1) to 75:25 (3.00:1), MV is measured at 380° C. as described in the Examples below, and m ) is measured at 380° C. as described in the Examples below, and m ) is measured at 380° C. as described in the Examples below, and mv =1490(Pa·s)(g / dL) 3.98 And n=3.98. MV and η inh is measured as described in the Examples below. In some embodiments, the PEKK polymer can have a ΔMV that is about -3 Pa s or less, about -5 or less, about -10 or less, about -12 or less, about -30 or less, -40 or less, -50 or less, or -60 or less.
[0041] PEKK polymers have a T of 280°C to 370°C, 285°C to 360°C, or 290°C to 350°C. mT m is measured by DSC at 20° C. / min as described in the Examples.
[0042] The PEKK polymer may have an η of at least 0.40 dL / g, at least 0.50 dL / g, or at least 0.60 dL / g. inh Additionally or alternatively, the PEKK polymer may have an η inh of 1.50 dL / g or less, 1.40 dL / g or less, or 1.2 dL / g or less. inh is measured as described in the Examples below.
[0043] Advantageously, the PEKK of the present invention C The polymer should have a molecular weight of at least 45 (μeq / g) / (g / 10 min). 0.29 , or preferably 50 (μeq / g) / (g / 10 min) 0.29 , more preferably at least 60 (μeq / g) / (g / 10 min) 0.29 , %[F]([F] i.e. 19 The ratio between the concentration of fluorine end groups of the PEKK polymer, as determined by F-NMR, and the MFI, i.e., the melt flow index of the PEKK polymer, as determined at 360°C under a load of 8.4 Kg according to ASTM D1238, is 0.29.
[0044] Advantageously, the PEKK of the present invention C The polymer has a phosphorus content of at least 30 ppm, more preferably at least 40 ppm, and most preferably at least 60 ppm, as measured in the examples by ICP-OES.
[0045] As noted above, the polymer synthesis methods described herein have been found to produce PEKK polymers with unexpectedly improved melt viscosities. The synthesis approach includes the use of low metal monomers, selective control of reactants, and other elements of the synthesis scheme. More specifically, the synthesis approach involves reacting a blend of low metal bis(hydroxybenzoyl)benzene monomers and bis(halobenzoyl)benzene monomers in the presence of sodium carbonate, Na2CO3, and a solvent, where the relative amounts of the aforementioned components are selected to achieve a PEKK polymer with unexpectedly increased melt stability.
[0046] Generally, the PEKK polymers of interest herein each have the following general formula: X 5 -M m -X 5 (13) X 6 -M p -X 6 (14) The repeat unit is formed from the polycondensation of a low metal 1,3-bis(benzoyl) monomer and a 1,4-bis(benzoyl) monomer having the formula: In these formulas: X 5 is -OH or halogen, and X 6 is -OH or a halogen.
[0047] As used herein, halogen refers to any one of F, Cl, Br, and I. Preferably, the halogen is F or Cl, and more preferably, the halogen is F.
[0048] In this specification, 1,3-bis(benzoyl)benzene monomer refers to a monomer represented by formula (13), and 1,4-bis(benzoyl)benzene monomer refers to a monomer represented by formula (14). Furthermore, bis(hydroxybenzoyl)benzene monomer refers to a monomer represented by formula (15). 5 Or X 6 and each X is —OH.5 Or X 6 is a halogen. For example, 1,3-bis(hydroxybenzoyl)benzene monomer (1,3BHBB) is 5 As another example, a 1,4-bis(halobenzoyl)benzene monomer refers to a monomer of formula (13) where X is -OH, such as 1,4-bis(4'-fluorobenzoyl)benzene (1,4-DFDK). 6 refers to a monomer of formula (14) in which
[0049] For ease of reference, the method described above (M S ), Na2CO3, K2CO3, monomer (HB), monomer (FB), and solvent are collectively referred to as the "reactants."
[0050] Preferably, for PEKK polymers according to the present invention, Σ is <5.5, more preferably Σ<5.0, even more preferably <4.0, <3.0, <2.0, and most preferably <1.5.
[0051] Ratio of 65 / 35 (1.86:1) to 75 / 25 (3.00:1) P PEKK ) / (R M PEKK For PEKK polymers having a ratio of Σ<6.0, preferably Σ<5.5, and more preferably Σ<5.0.
[0052] With respect to %Na2CO3 and %K2CO3, in some embodiments, %Na2CO3+%K2CO3≦106.0%. %Na2CO3+%K2CO3 is preferably at least 95%, more preferably at least 100%, more preferably at least 102%, and even more preferably at least 103.5%. Preferably, Na2CO3 meets the particle size distribution requirements detailed in U.S. Patent No. 9,175,136, filed October 23, 2009, to Louis, which is incorporated herein by reference in its entirety.
[0053] As described above, each repeating unit (R M PEKK ) and (R P PEKK ) is formed by polycondensation of monomer (HB) and monomer (FB) such that the number of moles of monomer (HB) and monomer (FB) are equimolar.
[0054] Therefore, %XS DFDK In embodiments where %XS is >0, the monomer blend contains more moles of monomer (FB) compared to the moles of monomer (HB). In some such embodiments, %XS DFDK is in the range of 0.1 mol % to 10.0 mol %, preferably 0.3 mol % to 5.0 mol %, more preferably 0.5 to 3.0 mol %, and most preferably 0.8 to 2.5 mol %.
[0055] Said PEEK S For polymers, preferably, the %XS DFDK % is from 0.7 mol % to 10.0 mol %, preferably from 0.75 mol % to 5.0 mol %, and more preferably from 0.8 to 3.0 mol %.
[0056] With respect to the solvent, it can include, but is not limited to, diphenylsulfone, dibenzothiophene dioxide, benzophenone, or any combination of one or more thereof. Preferably, the solvent includes diphenylsulfone. More preferably, the solvent includes at least 90% by weight, at least 95% by weight, at least 98% by weight, or at least 99% by weight of diphenylsulfone. In some embodiments, the diphenylsulfone includes limited amounts of impurities, as detailed in U.S. Patent No. 9,133,111, issued April 7, 2014 to Louis, which is incorporated herein by reference.
[0057] With respect to the relative concentration of monomer (HB) and monomer (FB), the repeat unit (R M PEKK ) and repeating unit (R PPEKK It should be noted that each of the above copolymers is formed by polycondensation of a monomer (HB) selected from 1,3 bis(hydroxybenzoyl)benzene monomers or 1,4-bis(hydroxybenzoyl)benzene monomers with a monomer (FB) selected from 1,3-bis(halobenzoyl)benzene monomers or 1,4-bis(halobenzoyl)benzene monomers.
[0058] More specifically, each repeating unit (R M PEKK ) is formed from the polycondensation of two separate 1,3-bis(benzoyl)benzene monomers; or from the polycondensation of a 1,3-bis(benzoyl)benzene monomer and a 1,4-bis(benzoyl)benzene monomer. Similarly, each repeat unit (R P PEKK ) is formed from the polycondensation of two separate 1,4-bis(benzoyl)benzene monomers; or from the polycondensation of a 1,3-bis(benzoyl)benzene monomer and a 1,4-bis(benzoyl)benzene monomer. For example, 5 -M m -X 5 and a monomer (1,3-bis(benzoyl)benzene) according to formula X 6 -M p -X 6 The polycondensation with the monomer (1,4-bis(benzoyl)benzene) according to P PEKK ) and (R M PEKK ), where X 5 is -OH or halogen, and X 5 If is -OH, then X 6 is a halogen, and X 5 If is a halogen, X 6 is -OH. As another example, 5 -M m -X 5 and a monomer (1,3-bis(benzoyl)benzene) according to formula X 7 -M * m -X 7The polycondensation with the monomer (1,3-bis(benzoyl)benzene) according to M PEKK ), where M * m is expressed by equation (13), and M m and where X is the same as or distinct from 5 is -OH or halogen, and X 5 If is -OH, then X 7 is a halogen, and X 5 If is a halogen, X 7 is -OH. As another example, 6 -M p -X 6 and a monomer (1,4-bis(benzoyl)benzene) according to formula X 8 -M * p -X 8 The polycondensation with the monomer (1,4-bis(benzoyl)benzene) according to P PEKK ), where M * p is expressed by equation (14), and M p and where X is the same as or distinct from 6 is -OH or halogen, and X 6 If is -OH, then X 8 is a halogen, and X 6 If is a halogen, X 8 is -OH.
[0059] Preferably, the PEKK of interest herein C The polymer is in the range of 55 / 45 to 75 / 25 (R P PEKK ) / (R M PEKK ) ratio.
[0060] In a preferred embodiment, the PEKK S The polymer has an R of greater than 61 / 39, preferably at least 65 / 35, most preferably at least 68 / 32 and up to 75 / 25. PPEKK ) / (R M PEKK ) ratio.
[0061] Thus, the ratio of moles of 1,4-bis(benzoyl)benzene monomer to moles of 1,3-bis(benzoyl)benzene monomer in a blend of monomer (HB) and monomer (FB) (the "1,4 / 1,3 ratio") is C For polymers, the range is 55 / 45 to 75 / 25, while the PEKK S For the polymer, it is greater than 61 / 39, preferably at least 65 / 35, most preferably at least 68 / 32 and up to 75 / 25. The relative amounts of 1,4-bis(benzoyl)benzene and 1,3-bis(benzoyl)benzene monomers, monomer (HB) and monomer (FB), are not particularly limited, so long as the aforementioned 1,4 / 1,3 ratio is met. In some embodiments, the repeating units (R M PEKK ), at least 90 mol %, at least 95 mol %, or at least 99 mol % of the 1,3-bis(benzoyl)benzene monomers are 1,3-bis(hydroxybenzoyl)benzene monomers or 1,3-bis(halobenzoyl)benzene monomers.
[0062] Importantly, the stated concentrations of the reactants, as well as other concentrations of the reactants described herein, are determined by the repeat unit (R M PEKK ) and (R P PEKK) is related to the amount of reactants used to form the reaction mixture. In other words, one or more of the reactants can be independently incorporated into the reaction mixture at separate times during the reaction. In some embodiments, the reaction mixture contains each of the reactants in an amount ("defined amount") defined in formulas (EQ1)-(EQ4), and the defined amounts of bis(hydroxybenzoyl)benzene monomer and bis(halobenzoyl)benzene monomer are reacted simultaneously. For example, in one such embodiment, the reaction mixture contains Na2CO3, K2CO3, bis(hydroxybenzoyl)benzene monomer, bis(halobenzoyl)benzene monomer, and solvent simultaneously in their defined amounts prior to the reaction, and the corresponding monomers are reacted therein.
[0063] In alternative embodiments, one or more of the reaction components can be added to the reaction mixture before or at different times during the reaction, hi some such embodiments, a portion of a defined amount of one or more of the reaction components is added to the reaction mixture before the reaction, and the remainder of a defined amount of one or more of the components is added to the reaction mixture during the reaction.
[0064] In a preferred embodiment, each repeat unit (R M PEKK At least 90 mol %, at least 95, or at least 99 mol % of the 1,3-bis(benzoyl)benzene monomers forming the repeat units (R P PEKK At least 90 mol %, at least 95, or at least 99 mol % of the 1,4-bis(benzoyl)benzene monomers forming 1,4-bis(benzoyl)benzene are added to the reaction mixture during or prior to the reaction.
[0065] In another preferred embodiment, a defined amount of solvent is present in the reaction mixture prior to the reaction.
[0066] In some embodiments, defined amounts of Na2CO3 and K2CO3 can be added to the reaction mixture either before the reaction or during the first reaction.
[0067] Based on the description herein, one of skill in the art will recognize additional methods of adding the individual reaction components to the reaction mixture.
[0068] The reaction can include a first heat, in which the reaction mixture is heated to maintain its temperature within a first temperature range of 180° C. to 270° C. In some embodiments, the first heat can include maintaining the temperature of the reaction mixture within a first temperature range for a first period of time. The first period of time can be 5 minutes ("min") to 300 minutes, 7 minutes to 240 minutes, or 10 minutes to 180 minutes, or 15 minutes to 120 minutes. As noted above, one or more of the reaction components can be added independently to the reaction mixture at separate times during the reaction. In some embodiments, each of the reaction components in their defined amounts is added to the reaction mixture prior to the first heat. In alternative embodiments, at least one or more of the reaction components is added to the reaction mixture during the first heat, and the remainder of the reaction components are added to the reaction mixture prior to the first heat. In some such embodiments, a defined amount of one or more reaction components (e.g., the entire amount of one or more reaction components) is added to the reaction mixture during the first heat.
[0069] In alternative such embodiments, only a portion of the defined amount of one or more reactants is added to the reaction mixture during the first heat, with the remaining portion being added to the reaction mixture prior to the first heat. Generally, each reactant is present in the reaction mixture in its defined amount prior to the end of the first heat. In such embodiments, the first period of time relates to the time when the defined amount of each reactant has been added to the reaction mixture. In a preferred embodiment, the repeating unit (R M PEKK at least 90 mol %, at least 95, or at least 99 mol % of the 1,3-bis(benzoyl)benzene monomers forming the 1,3-bis(benzoyl)benzene monomers are added before or during the first heat, and wherein at least 90 mol %, at least 95, or at least 99 mol % of the 1,4-bis(benzoyl)benzene monomers forming the remaining 1,4-bis(benzoyl)benzene monomers are added during or before the first heat, respectively.
[0070] In some embodiments, the reaction further comprises a second heat following the first heat, where the reaction mixture is heated to maintain its temperature within a second temperature range of 300° C. to 340° C.
[0071] In some such embodiments, the reaction mixture can be maintained within the second temperature range for a second period of time. The second period of time can be from 0 to 240 minutes, from 0 to 180 minutes, or from 0 to 120 minutes.
[0072] In some embodiments, the second heating further comprises adding an endcapping agent to the reaction mixture.
[0073] The endcapping agent controls the molecular weight of the PEKK polymer by terminating the polymerization reaction at a selected point during the polymerization. In such an embodiment, the second heat comprises a second addition.
[0074] Preferred endcapping agents include those having the formula: TIFF0007555828000007.tif27170 (wherein G is -C(O)-Ar or S(O2)-Ar, and Ar is an arylene group) This includes those represented by:
[0075] In some embodiments, the endcapping agent is a repeat unit of the PEKK polymer (R M PEKK ) or repeating unit (R P PEKK ), an excess of bis(halobenzoyl)benzene monomer (1,3-bis(halobenzoyl)benzene monomer or 1,4-bis(halobenzoyl)benzene monomer) is used to form
[0076] The PEKK of the present invention CFor polymers, excess means an amount of 1,3-bis(halobenzoyl)benzene monomer or 1,4-bis(halobenzoyl)benzene monomer in excess of the amount that causes the total amount of each monomer added to the reaction mixture to be at least 1.03 times, preferably at least 1.04 times, and more preferably at least 1.05 times the molar equivalent of the bis(hydroxybenzoyl)benzene monomer. For clarity, it is noted that the endcapping agent is preferably an endcapping agent that is .... M PEKK ) or repeating unit (R P PEKK In embodiments where the endcapping agent is a bis(halobenzoyl)benzene monomer used to form the endcapping agent, the amount of endcapping agent is %XS DFDK is not included.
[0077] In some embodiments, the PEKK C The polymer comprises more than 50 mol%, preferably more than 55 mol%, more than 60 mol%, more than 65 mol%, more than 70 mol%, more than 75 mol%, more than 80 mol%, more than 85 mol%, more than 90 mol%, more than 95 mol%, more than 99 mol% of non-reactive end groups as determined by nuclear magnetic resonance spectroscopy (NMR). A "non-reactive end group" herein is a group that is not an -OH group that forms the end of a polymer chain. Preferably, the non-reactive group is a 1,4-bis(halobenzoyl)benzene group. Most preferably, the non-reactive group comprises a terminal fluorine.
[0078] The PEKK of the present invention S For polymers, excess means an amount of 1,3-bis(halobenzoyl)benzene monomer or 1,4-bis(halobenzoyl)benzene monomer in excess of the amount that causes the total amount of each monomer added to the reaction mixture to be at least 1.08 times, preferably at least 1.10 times, and more preferably at least 1.12 times the molar equivalent of the bis(hydroxybenzoyl)benzene monomer. For clarity, it is noted that the endcapping agent is an endcapping agent that .... M PEKK ) or repeating unit (R P PEKKIn embodiments where the endcapping agent is a bis(halobenzoyl)benzene monomer used to form the endcapping agent, the amount of endcapping agent is %XS DFDK is not included.
[0079] In some embodiments of the method of forming a PEKK polymer, monomer (HB) and monomer (FB) collectively comprise at least one first 1,3-bis(benzoyl)benzene monomer, at least one first 1,4-bis(benzoyl)benzene monomer, at least one second 1,4-bis(benzoyl)benzene monomer, and at least one third 1,4-bis(benzoyl)benzene monomer, where each 1,3-bis(benzoyl)benzene monomer has a formula according to formula (13) and each 1,4-bis(benzoyl)benzene monomer has a formula according to formula (14). In some such embodiments, one of the at least one first 1,3-bis(benzoyl)benzene monomer, one of the at least one first 1,4-bis(benzoyl)benzene monomer, one of the at least one second 1,4-bis(benzoyl)benzene monomer, and one of the at least one third 1,4-bis(benzoyl)benzene monomer are each represented by the following formula: X 1 -M 1* m -X 1 (16) X 2 -M 1* p -X 2 (17) X 3 -M 2* p -X 3 (18) X 4 -M 3* p -X 4 (19) In these formulas, X 1 is -OH or a halogen; X 1 When is -OH, X 2 is a halogen, and X 1If is a halogen, X 2 is -OH, X 3 is -OH or a halogen; X 3 When is -OH, X 4 is a halogen, and X 3 If is a halogen, X 4 is -OH.
[0080] In some such embodiments, monomer X 1 -M *1 m -X 1 and X 2 -M *1 p -X 2 are polycondensed to form the repeating units (R M1 PEKK ) and (R P1 PEKK ) to form monomer X 3 -M * p -X 3 and X 4 -M * p -X 4 are polycondensed to form the repeating units (R P2 PEKK ), and (R P3 PEKK ) is formed.
[0081] In some embodiments, X 1 and X 3 is -OH. In some embodiments, each i * , j * , k * and L * is the repeating unit (R P1 PEKK ), (R P2 PEKK ) and (R P3 PEKK ) are identical, so that they are zero.
[0082] The method (M C ) is the above-mentioned step (I* ) and after the step (II * (I) isolating the composition containing at least one PEKK polymer by extracting the solvent (e.g., diphenylsulfone) and residual salts with acetone and water at a pH in the range of 1 to 12. * b) may further be included.
[0083] In addition, the method (M C ) is the above-mentioned step (I * After the step (I * b) or the step (II * ) before the at least one PEKK C The method may further include a step of isolating the composition containing the polymer. Preferably, the step includes the steps of: * At least one PEKK obtained after b) C This is done by washing the polymer matrix containing the polymer with a solution of at least one of sodium dihydrogen phosphate (NaH2PO4·2H2O) and disodium hydrogen phosphate (Na2HPO4).
[0084] Preferably, step (I * At least one PEKK obtained after b) C The polymer matrix containing the polymer is contacted with a solution, for example an aqueous solution containing both NaH2PO4·2H2O and Na2HPO4. The concentration of NaH2PO4·2H2O in the solution is preferably in the range of 0.01-0.20% by weight, preferably 0.02-0.15% by weight, most preferably 0.03-0.10% by weight, and the concentration of Na2HPO4 is preferably in the range of 0.01-0.20% by weight, preferably 0.02-0.15% by weight, most preferably 0.03-0.10% by weight.
[0085] As described above, the at least one PEKK S The step (II) of isolating the polymer-containing composition is carried out by washing the composition with a solution containing NaH2PO4 and Na2HPO4.
[0086] Preferably, in the step (II), the concentration of NaH2PO4 in the solution is preferably in the range of 0.01 to 0.20% by weight, preferably 0.02 to 0.15% by weight, and most preferably 0.03 to 0.10% by weight, and the concentration of Na2HPO4 is preferably in the range of 0.01 to 0.20% by weight, preferably 0.02 to 0.15% by weight, and most preferably 0.03 to 0.10% by weight.
[0087] Preferably, the above mentioned polymer matrix can comprise one or more additional components selected from the group consisting of: (i) colorants (e.g., dyes); (ii) pigments (e.g., titanium dioxide, zinc sulfide, and zinc oxide); (iii) light stabilizers (e.g., UV stabilizers); (iv) heat stabilizers; (v) antioxidants (e.g., organic phosphites and phosphonites); (vi) acid scavengers (vii) processing aids (viii) nucleating agents (ix) plasticizers, internal lubricants, and external lubricants; (x) flame retardants (xi) smoke suppressants (x) antistatic agents (xi) antiblocking agents (xii) conductive additives (e.g., carbon black and carbon nanofibrils); (xiii) plasticizers; (xiv) flow improvers; (xv) extenders; (xvi) metal deactivators, and any combination of one or more thereof.
[0088] Preferably, the total concentration of the additional components is less than 20%, preferably less than 10%, more preferably less than 5%, and even more preferably less than 2%, based on the total weight of the polymer matrix. The PEKK polymers described herein can be desirably used in polymer compositions and can be incorporated into molded articles, such as, but not limited to, mobile electronic devices, medical devices, and composites. Additionally, the PEKK polymers, or compositions thereof, can be desirably used in the context of additive manufacturing applications.
[0089] A polymer composition including a PEKK polymer ("PEKK polymer composition") can include a reinforcing filler.
[0090] The reinforcing fibers may be organic or inorganic.
[0091] Fibers suitable for use as the reinforcing fiber component include, for example, carbon fibers, graphite fibers, glass fibers such as E-glass fibers, ceramic fibers such as silicon carbide fibers, synthetic polymer fibers such as aromatic polyamide fibers, polyimide fibers, and polybenzoxazole fibers. The weight of a single layer or cross section of such fibers is, for example, 50 to 600 g / m 2 may vary.
[0092] In some embodiments, the fibers include carbon fibers, glass fibers, or both carbon and glass fibers.
[0093] In some embodiments, the fibers comprise carbon fibers, such as, for example, carbon fibers exhibiting a tensile strength of 3.5 gigapascals ("GPa") or greater and a tensile modulus of 200 GPa or greater as measured by ASTM D638.
[0094] The fibers may be in the form of whiskers, staple fibers, continuous fibers, sheets, plies, and combinations thereof. The continuous fibers may further be in any of unidirectional, multidirectional, non-woven, woven, knitted, stitched, wrapped, and netted configurations, as well as swirl mat, felt mat, and chopped mat structures. The fiber tows may be fixed in place in such configurations by a cross tow stitch, a weft insertion knit stitch, or a small amount of resin, such as sizing. A "continuous fiber" in this specification is a fiber having a length greater than 10 mm.
[0095] The weight of the reinforcing filler is preferably less than 80% by weight, more preferably less than 70% by weight, even more preferably less than 65% by weight, based on the total weight of the composition.
[0096] In some embodiments, the composition comprises a PEKK polymer in combination with one or more additional polymeric components, such as polyarylether polymers different from the PEKK polymer, sulfone polymers, and polyarylsulfide polymers, including, but not limited to, poly(etheretherketone) ("PEEK") polymers, poly(etherketone) ("PEK") polymers. According to other embodiments, the PEKK polymer, as detailed above, is the only polymeric component in the PEKK polymer composition. The expression "polymeric component" should be understood according to its ordinary meaning, i.e., to encompass compounds characterized by repeating linking units, typically having a molecular weight of 2,000 g / mol or greater.
[0097] The PEKK polymer compositions can be prepared by a variety of methods including intimately combining a PEKK polymer, optionally a reinforcing filler, and optionally any additional ingredients desired in the PEKK polymer composition, such as by dry blending, suspension or slurry mixing, solution mixing, melt mixing, or a combination of dry blending and melt mixing.
[0098] It is also possible to manufacture the composition of the present invention by further melt kneading the powder mixture described above.As described above, melt kneading can be achieved with the powder mixture as detailed above, or directly with the PEKK polymer as detailed above, the reinforcing filler as detailed above, and optionally other raw materials.Conventional melt kneading equipment can be used, such as co-rotating and counter-rotating extruders, single screw extruders, co-kneaders, disk-pack processors, and various other types of extrusion equipment.Preferably, extruders, more preferably twin screw extruders, can be used.
[0099] The present invention further relates to a method for producing a PEKK composite material, comprising impregnating the above-mentioned reinforcing fibers with a PEKK polymer as defined above.
[0100] The polymer matrix comprising said PEKK polymer and, optionally, one or more additional components as defined above, may be advantageously prepared by methods known in the art.
[0101] Such methods include, for example, dry blending the PEKK polymer with any additional ingredients.
[0102] In some embodiments, the PEKK polymer is ground to a fine powder having an average particle size of less than 50 μm, preferably less than 35 μm, and less than 30 μm.
[0103] For example, to form plies in the form of sheets or tapes of fibers at least partially impregnated with a polymeric matrix, various methods can be used that can impregnate the fibers with a polymeric matrix, where the matrix is either in molten or particulate form, such as, for example, powder coating, film lamination, extrusion, pultrusion, aqueous slurries, and melt impregnation.
[0104] As used herein, "tape" means a strip of material having longitudinally extending reinforcing fibers aligned along a single axis of the strip of material.
[0105] Plies of matrix-impregnated fibers can be placed adjacent to one another to form unconsolidated composite laminates, such as prepregs. The fiber reinforced layers of the laminate can be oriented with the respective fiber reinforcements in a selected direction relative to one another.
[0106] The plies can be laid up manually or automatically, for example, by automated tape layup using "pick-and-place" robotics, or by advanced fiber placement (AFP), in which tows of pre-impregnated fibers are heated and compressed in a mold or on a mandrel, to form a composite laminate with the desired physical dimensions and fiber orientation.
[0107] The layers of an unconsolidated laminate are typically not completely fused together, and an unconsolidated composite laminate may exhibit significant void content, e.g., greater than 20% by volume, as measured by X-ray microtomography. As an intermediate step to allow handling of the composite laminate prior to its consolidation, heat and / or pressure may be applied or sonic vibration welding may be used to stabilize the laminate and prevent the layers from moving relative to one another, e.g., to form a composite "blank."
[0108] The composite laminate so formed is then typically consolidated, for example in a mold, by subjecting the composite laminate to heat and pressure to form a molded fiber reinforced thermoplastic matrix composite article.
[0109] As used herein, "consolidation" refers to a process in which the matrix material is softened, the layers of the composite laminate are pressed together, air, moisture, solvents, and other volatiles are forced out of the laminate, and adjacent plies of the composite laminate are fused together to form a solid, coherent article. Ideally, a consolidated composite product will exhibit a minimal void content, e.g., less than 5% by volume, more typically less than 2% by volume, as measured by x-ray microtomography.
[0110] The PEKK composite preferably comprises 20-80% reinforcing fibers and 80-20% polymer matrix by weight of the PEKK composite.
[0111] The PEKK composites described herein can be incorporated into composite products such as, but not limited to, components for aerospace applications.
[0112] In some embodiments, the composite product is in the form of a substantially two-dimensional article.
[0113] Two-dimensional products include parts, such as films and sheets, in which one dimension (thickness or height) is significantly smaller than the other two characteristic dimensions (width and length). In some embodiments, the composite product is a three-dimensional part. Three-dimensional parts include parts that extend substantially in all three spatial dimensions in the same way, including part forms with complex shapes (e.g., concave or convex sections, possibly including undercuts, insets, etc.).
[0114] In some embodiments, the composite product includes at least one portion having a thickness of at least 4 mm, preferably at least 5 mm.
[0115] Due to the unexpectedly improved melt stability of the polymer matrix, composite products including the polymer matrix can exhibit less than 2% voids in parts having a thickness greater than 5 mm.
[0116] In some embodiments, the toughness of a PEKK composite material is greater than 75% of its initial toughness after being heated for 20 minutes at a temperature in the range of 290°C to 370°C, as measured as compressive strength after impact using an impact energy of 30 J according to ASTM test method D7137 / 7136.
[0117] In some embodiments, the toughness of a PEKK composite material is greater than 75% of its initial toughness after being heated for 20 minutes at a temperature in the range of 290°C to 370°C, where this toughness is measured as Mode 1 fracture toughness according to ASTM 5228.
[0118] The PEKK polymer composition (or PEKK polymer) can be desirably incorporated into a shaped article. The shaped article can be produced from the PEKK polymer composition using any suitable melt processing technique, including, but not limited to, extrusion, injection molding, and compression molding. In some embodiments, the shaped article is in the form of a substantially two-dimensional article. Two-dimensional products include parts, such as films and sheets, in which one dimension (thickness or height) is significantly smaller than the other two characteristic dimensions (width and length). In some embodiments, the molded article can be a coating. In some embodiments, the molded article is a three-dimensional part. Three-dimensional parts include parts that extend substantially in the same way in three dimensions of space, such as in the form of complex shaped parts (e.g., concave or convex sections, possibly including undercuts, inserts, etc.).
[0119] In some embodiments, the shaped article is a component of a portable electronic device. As used herein, "portable electronic device" refers to an electronic device that can be transported to various locations and used in various locations. Portable electronic devices can include, but are not limited to, mobile phones, personal digital assistants ("PDAs"), laptop computers, tablet computers, wearable computing devices (e.g., smart watches and smart glasses), cameras, portable audio players, portable radios, satellite positioning system receivers, and portable game consoles.
[0120] Moreover, due to the improved processability (e.g., lower MV) and higher thermal stability, the PEKK polymers described herein can be desirably used in 3D printing (also known as additive manufacturing) fabrication techniques such as fused filament fabrication (FFF) or selective laser sintering (SLS). Additive manufacturing involves the process of joining materials from 3D model data to produce articles. Articles are generally formed using layer-by-layer deposition. Commercially available 3D printing manufacturing equipment of the FFF type includes, by way of example, equipment manufactured by Stratasys, Inc. and sold under the trademark Fortus®. Examples of SLS-based 3D printing equipment are available from EOS corporation, such as that sold under the trade name EOSINT®. In such embodiments, the article can be formed by 3D printing the PEKK polymer (or PEKK polymer composition).
[0121] In some embodiments, the articles described herein are medical devices or components of medical devices. As used herein, a "medical device" is a product, apparatus, equipment, or machine used in the prevention, diagnosis, or treatment of disease or disorder, or to detect, measure, restore, correct, or modify a structure or function of the human or animal body.
[0122] Material selection is extremely important for medical devices, especially when the materials are implanted within or in contact with the body. There is a continuing need for medical device materials that meet the specific requirements of the medical device in its application setting (e.g., wear resistance) and also reduce or prevent undesirable interactions with the body, such as, for example, leaching of chemicals from the medical device into the body.
[0123] The PEKK polymers described herein may be particularly suitable for use in medical devices due to their higher purity as reflected, for example, in their reduced chlorine and metals content.
[0124] Medical devices may generally include surgical devices, non-surgical devices, prosthetics, implants, and the like.
[0125] In some embodiments, the medical device comprising the PEKK polymers described herein is an implantable medical device (IMD). IMDs are medical devices designed to replace lost biological structures, support damaged biological structures, or reinforce existing biological structures in the body. Examples of IMGs include cranial implants such as craniomaxillofacial implants, spinal implants such as spinal cages and spinal discs, finger and toe implants, knee replacements, hip replacements such as acetabular caps, stents, heart valves, pacemakers, and hardware such as bone screws and plates. Medical devices may also include dental appliances such as removable full and partial denture frames, crowns, bridges, dentures, and implant bars.
[0126] To the extent that the disclosure of any patents, patent applications, and publications incorporated herein by reference conflicts with the statements of this application to the extent that it may render a term unclear, the statements of this application shall control.
[0127] To the extent that the disclosure of any patents, patent applications, and publications incorporated herein by reference conflicts with the statements of this application to the extent that it may render a term unclear, the statements of this application shall control. EXAMPLES
[0128] raw materials 1,4-bis(4-phenoxybenzoyl)benzene was prepared according to Russian Patent Application Publication No. 445643A1, which is incorporated herein by reference. 1,2-Dichlorobenzene, terephthaloyl chloride, isophthaloyl chloride, 3,5-dichlorobenzoyl chloride, aluminum chloride (AlCl3), methanol, NaH2PO4·2H2O, and Na2HPO4 were purchased from Sigma Aldrich. Methanol was obtained from Sigma-Aldrich. Diphenylsulfone (polymer grade) (99.8% purity) was obtained from Proviron. Sodium carbonate, light soda ash (d 90 Particle size = 130 μm) was obtained from Solvay SA, France and dried before use. Potassium carbonate (d 90 <45 μm) were obtained from Armand products and dried before use. Lithium chloride (anhydrous powder) was obtained from Acros.
[0129] 19 Determination of F end groups by F NMR The concentration of F end groups was determined using hexafluoroacetone trihydrate as an external standard. 19 Determined by F-NMR.
[0130] The F terminal group is It is of type TIFF0007555828000008.tif30170. The sample (approximately 10 mg) was dissolved in 0.5 ml of CD2Cl2 and 0.5 ml of CH3SO3H. After multiple attempts, a clear solution was finally obtained. All NMR spectra were recorded at 30° C. on a 400 MHz NMR Bruker AVANCE spectrometer. 19 F 1D NMR spectra were obtained as follows: a precisely known amount of hexafluoroacetone trihydrate was dissolved in 0.5 mL of CD2Cl2 (or C2D2Cl4) and 0.5 mL of CH3SO3H. 19 F-NMR spectra were recorded as an external standard. The F end group concentration [F] of the polymer was calculated using the following formula: TIFF0007555828000009.tif15170In formula, All weights are in grams. [F] is in μeq / g, I Arylfluoride is -94 to -96 ppm 19is the integral of the F NMR signal (spectrum of the polymer sample), I HFA.3H2O is -82.5ppm 19 The integrals of the F NMR signals (external standard spectrum-signals are for 6F).
[0131] Determination of Melt Flow Index The melt flow index was determined according to ASTM D1238 at 360° C. with a load of 3.8 kg. The final MFI shown in the table for a load of 8.4 kg was obtained by multiplying the obtained value by 2.35.
[0132] Determination of melt stability by capillary rheology (VR40) Melt viscosity was measured using a capillary rheometer according to ASTM D3835. The melt viscosity was measured at 410°C and 46.3s using a die with the following characteristics: diameter = 1.016 mm, length = 20.32 mm, cone angle = 120°. -1 Readings were taken after 10 and 40 minutes residence time at a shear rate of 100 rpm.
[0133] Melt stability was evaluated by the ratio of viscosity at 40 minutes to that at 10 minutes (VR40). The closer the value is to 1, the more melt stable it is.
[0134] Determination of complex melt viscosity with parallel plates. Test plates measuring 7.62 cm in diameter x 3 mm were prepared by compression molding under the following conditions: 1. Preheat to 368℃. 2. 368℃ / 15 minutes at 2000 kgf 3. 368℃ / 2 minutes at 2700 kgf 4. Cool to 30°C over 40 minutes at 2000 kg-f. Disks of 25 mm diameter were drilled out from the test plates and analyzed by parallel plate rheology according to ASTM D4440 on a TA ARESR DA3 rheometer. The complex viscosity was measured at 410°C under nitrogen at 10 rad / s and 1% strain for 120 min.
[0135] Determination of elemental impurities in monomers and PEKK polymers by ICP-OES A clean, dry platinum crucible was placed on an analytical balance and the balance was zeroed. 0.5-3 grams of monomer / polymer sample was weighed into a pan boat and the weight was recorded to the nearest 0.0001 g. The crucible with the sample was placed in a muffle furnace (Thermo Scientific Thermolyne F6000 Programmable Furnace). The furnace was gradually heated to 525°C and held at that temperature for 10 hours to dry ash the sample.
[0136] After ashing, the furnace was cooled to room temperature and the crucible was removed from the furnace and placed in a fume hood. The ash was dissolved in dilute hydrochloric acid. Using a polyethylene pipette, this solution was transferred to a 25 mL volumetric flask. The crucible was rinsed twice with approximately 5 mL of ultrapure water (R<18 MΩcm) and the rinses were added to the volumetric flask to perform a quantitative transfer. Ultrapure water was added to the flask until a total of 25 mL was reached. The flask was stoppered on the top and shaken to ensure the contents were mixed.
[0137] ICP-OES analysis was performed using an inductively coupled plasma optical emission spectrometer Perkin-Elmer Optima 8300 Dual View. The optical emission spectrometer was calibrated using a set of NIST-traceable multi-element mixed standards with analyte concentrations from 0.0 to 10.0 mg / L. Linear calibration curves were obtained over the concentration range with correlation coefficients better than 0.9999 for each of the 48 analytes. Standards were run before and after every 10 samples to ensure instrument stability. Results were reported as the average of triplicate experiments. The concentrations of elemental impurities in the samples were calculated using the following equation: A=(B*C) / (D) (In the formula, A = concentration of the element in the sample, mg / kg (=wt.ppm), B = elements in solution analyzed by ICP-OES, mg / L; C = volume of solution analyzed by ICP-OES, mL D=weight of sample used in this procedure).
[0138] Glass transition temperature (T g ) Determination Glass transition temperature (T g ) was measured by differential scanning calorimetry (DSC) according to ASTM D3418-03 and E1356-03 and recorded from the second heat using the half-height method.
[0139] Determination of heat of fusion (ΔH) The heat of fusion (ΔH) of the polymer powders was determined as the area under the melting endotherm in the second heating scan in a differential scanning calorimeter (DSC) according to ASTM D3418-03 and E793-06 using heating and cooling rates of 20° C. / min. The heat of fusion (ΔH) was measured in the second heating scan and was taken as the area under a linear baseline drawn from above the glass transition temperature (Tg) to beyond the end of the endotherm.
[0140] The heat of fusion (ΔH) of the molded parts was determined as the area under the melting endotherm in the first heating scan in a differential scanning calorimeter (DSC) according to ASTM D3418-03 and E793-06 using heating and cooling rates of 20° C. / min.
[0141] For filled compositions, the measured heat of fusion (ΔH) was corrected for the filler content and represents the heat of fusion (ΔH) for only the polymer component excluding the filler.
[0142] Preparation of monomers 1,4-Bis(4'-fluorobenzoyl)benzene (1,4-DFDK) and 1,3 bis(4'-fluorobenzoyl)benzene (1,3-DFDK) were prepared by Friedel-Crafts acylation of fluorobenzene according to Example 1 of Gilb et al., U.S. Patent No. 5,300,693, filed November 25, 1992, which is incorporated herein by reference in its entirety. A portion of the 1,4-DFDK was purified by recrystallization in chlorobenzene as described in U.S. Patent No. 5,300,693, and a portion of the 1,4-DFDK was purified by recrystallization in DMSO / ethanol. 1,4-DFDK purified by recrystallization in DMSO / ethanol was used as the 1,4-DFDK in the polymerization reaction to produce the PEKK described below, and 1,4-DFDK recrystallized in chlorobenzene was used as the precursor to 1,4-bis(4'-hydroxybenzoyl)benzene (1,4-BHBB). 1,4-BHBB and 1,3-bis(4'-hydroxybenzoyl)benzene (1,3-BHBB) were prepared by hydrolysis of 1,4-DFDK and 1,3-DFDK, respectively, according to the procedure described in Example 1 of U.S. Pat. No. 5,250,738 to Hackenbruch et al., filed Feb. 24, 1992, which is incorporated herein by reference in its entirety. The 1,4-BHBB used in Comparative Example 2 below was purified using the procedure of U.S. Pat. No. 5,250,738 to give a "high metal monomer" hereafter referred to as "Monomer A." The 1,4-BHBB used in Comparative Example 3 and Examples 4 and 5 below was purified by recrystallization in DMF / ethanol to give "Monomer B" (the "low metal monomer"). The amounts of various metals in the 1,4-BHBB monomer were determined by ICP-OES analysis as described below, and the analytical results are shown in Table 1.
[0143] TIFF0007555828000010.tif77170
[0144] Comparative Example 1: PEKK made by an electrophilic process. Polycondensation Into a 2000 mL 4-necked reaction flask equipped with an agitator, dry N2 inlet tube, thermocouple inserted into the reaction medium, and condenser, 1000 g of 1,2-dichlorobenzene and 40.63 g of 1,4-bis(4-phenoxybenzoyl)benzene were introduced. Then, under a sweep of dry nitrogen, 7.539 g of terephthaloyl chloride, 9.716 g of isophthaloyl chloride, and 0.238 g of benzoyl chloride were added to the reaction mixture. The reactor was then cooled to 5°C and 71.88 g of aluminum chloride (AlCl3) was added slowly while keeping the temperature below 5°C. The reaction was held at 5°C for 10 minutes and then the temperature of the mixture was increased to 90°C at 5°C / min. The reaction mixture was held at 90°C for 30 minutes and then cooled to 30°C. At 30°C, 250 g of methanol was added slowly to keep the temperature below 60°C. After the addition was complete, the reaction mixture was left stirring for 2 hours and then cooled to 30°C.
[0145] Filtration and washing The solids were then removed by filtration on a Buchner. The wet cake was rinsed on the filter with an additional 188 g of methanol. The wet cake was then reslurried in a beaker with 440 g of methanol for 2 hours. The polymer solids were filtered again on a Buchner funnel and the wet cake was rinsed on the fitler with 188 g of methanol. The solids were slurried with 470 g of aqueous hydrochloric acid (3.5 wt%) for 2 hours. The solids were then removed by filtration on a Buchner. The wet cake was rinsed on the filter with an additional 280 g of water. The wet cake was then reslurried in a beaker with 250 g of 0.5 N aqueous sodium hydroxide for 2 hours. The wet cake was then reslurried in a beaker with 475 g of water and filtered on a Buchner funnel. The final water wash step was repeated three more times. The polymer is then slurried with 0.75 g of an aqueous solution containing 6.6 wt % NaH2PO4·2H2O and 3.3 wt % Na2HPO4, and then dried in a vacuum oven at 180 °C for 12 h.
[0146] Comparative Example 2: Synthesis of PEKK using Monomer A The 1,4-BHBB used in this example was Monomer A with a total metal concentration of 146 ppm.
[0147] Into a 500 mL 4-neck reaction flask equipped with a stirrer, a Claisen adapter with a thermocouple placed in the reaction medium, and a Dean-Stark trap with a condenser and a dry ice trap, 127.50 g of diphenylsulfone, 26.130 g of 1,3-BHBB, 18.921 g of 1,4-BHBB (monomer A), and 46.525 g of 1,4-DFDK were introduced. The flask contents were evacuated under vacuum and then filled with high purity nitrogen (containing less than 10 ppm O). The reaction mixture was then placed under a constant nitrogen purge (60 mL / min).
[0148] The reaction mixture was slowly heated to 270°C. At 270°C, 15.555g Na2CO3 and 0.098g K2CO3 were added to the reaction mixture from a powder dispenser over 60 minutes. At the end of the additions, the reaction mixture was heated to 320°C at 1°C / min. After 14 minutes at 320°C, 1.368g 1,4-DFDK was added to the reaction mixture while maintaining a nitrogen purge in the reactor. After 5 minutes, 0.600g lithium chloride was added to the reaction mixture. After 10 minutes, another 0.456g 1,4-DFDK was added to the reactor and the reaction mixture was held at temperature for 15 minutes.
[0149] The reactor contents were then poured from the reactor into a stainless steel pan and allowed to cool. The solids were crushed and ground in an attrition mill through a 2 mm screen. The diphenyl sulfone and salts were extracted from a mixture of acetone and water at pH 1-12. For the final wash, 0.67 g of NaH2PO4·2H2O and 0.62 g of Na2HPO4 were dissolved in 1200 mL of DI water. The powder was then removed from the reactor and dried at 120 °C under vacuum for 12 hours, yielding 72 g of a yellow powder.
[0150] The final PEKK polymer had a T / I ratio of 71 / 29.
[0151] Comparative Example 3: Preparation of PEKK according to Chinese Patent Publication No. CN1974631 using Monomer B Into a 500 mL 4-neck reaction flask equipped with a stirrer, a N2 inlet tube, a Claisen adapter with a thermocouple inserted into the reaction medium, and a Dean-Stark trap with a condenser and a dry ice trap, 249.93 g of diphenylsulfone, 39.790 g of 1,4-BHBB (monomer B), 17.726 g of 1,4-DFDK, 22.561 g of 1,3-DFDK, and 13.646 g of Na2CO3 were introduced. The flask contents were evacuated under vacuum and then filled with high purity nitrogen (containing less than 10 ppm O2). The reaction mixture was then placed under a constant nitrogen purge (60 mL / min).
[0152] The reaction mixture was heated to 120°C and then from 120°C to 160°C at 2°C / min. The mixture was then held at 160°C for 1 h, heated at 5°C / min to 210°C and held at 210°C for 1 h. The mixture was then heated to 250°C at 5°C / min and held at 250°C for 1 h. The mixture was then heated to 290°C at 10°C / min and held at 290°C for 2 h. The mixture was heated to 310°C at 10°C / min and held at 310°C for 3 h. The reactor contents were then poured from the reactor into a stainless steel pan and allowed to cool. The solids were crushed and ground in an attrition mill through a 2 mm screen. Diphenyl sulfone and salts were extracted from a mixture of acetone and water at pH 1-12. For the final wash, 0.67 g of NaH2PO4·2H2O and 0.62 g of Na2HPO4 were dissolved in 1200 mL of DI water. The powder was then removed from the reactor and dried at 120 °C under vacuum for 12 h to yield 68 g of an off-white / yellow powder.
[0153] The final polymer had a T / I ratio of 70 / 30.
[0154] Example 4: Initial synthesis of PEKK using monomer B The procedure of Comparative Example 2 was followed except that the 1,4-BHBB monomer was Monomer B and the total metals concentration was 9.7 ppm.
[0155] The final polymer had a T / I ratio of 71 / 29.
[0156] Example 5: Second synthesis of PEKK using monomer B The procedure of Example 4 was followed except that the weights of NaH2PO4·2H2O and Na2HPO4 were doubled to 1.34 g and 1.24 g, respectively.
[0157] The final polymer had a T / I ratio of 71 / 29.
[0158] Comparative Example 6: Preparation of PEKK according to Chinese Patent Publication No. 1974631 using the same monomers as in the examples according to the present invention Into a 500 mL 4-neck reaction flask equipped with a stirrer, N2 inlet tube, Claisen adapter with thermocouple inserted into the reaction medium, and Dean-Stark trap with condenser and dry ice trap, 219.94 g of diphenylsulfone, 14.706 g of 1,4-bis(4'-hydroxybenzoyl)benzene (14BHBB B, clean), 35.453 g of 1,4-bis(4'-fluorobenzoyl)benzene, 20.309 g of 1,3-bis(4'-fluorobenzoyl)benzene, and 12.009 g of Na2CO3 were introduced. The flask contents were evacuated under vacuum and then filled with high purity nitrogen (containing less than 10 ppm O2). The reaction mixture was then placed under a constant nitrogen purge (60 mL / min).
[0159] The reaction mixture was heated to 120°C and then from 120°C to 160°C at 2°C / min. The mixture was then held at 160°C for 1 h, heated at 5°C / min to 210°C and held at 210°C for 1 h. The mixture was then heated to 250°C at 5°C / min and held at 250°C for 1 h. The mixture was then heated to 290°C at 10°C / min and held at 290°C for 2 h. The mixture was then heated to 310°C at 10°C / min and held at 310°C for 26 minutes to target a molecular weight consistent with other examples. The reactor contents were then poured from the reactor into a SS pan to cool. The solids were crushed and ground in an attrition mill through a 2 mm screen. Diphenyl sulfone and salts were extracted from a mixture of acetone and water at pH 1-12. For the final wash, 0.67 g of NaH2PO4·2H2O and 0.62 g of Na2HPO4 were dissolved in 1200 mL of DI water. The powder was then removed from the reactor and dried under vacuum at 120 °C for 12 h to yield 60 g of an off-white / yellow powder.
[0160] The final polymer had a T / I ratio of 71 / 29.
[0161] Comparative Example 7: Synthesis and Analysis of PEKK Using Monomers with High Levels of Residual Metals and Low Na2CO3 The 1,4-BHBB used in this example was Monomer A with a total metal concentration of 146 ppm.
[0162] Into a 500 mL 4-neck reaction flask equipped with a stirrer, a Claisen adapter with a thermocouple placed in the reaction medium, and a Dean-Stark trap with a condenser and a dry ice trap, 112.50 g of diphenylsulfone, 23.056 g of 1,3-BHBB, 16.695 g of 1,4-BHBB, and 41.051 g of 1,4-DFDK were introduced. The flask contents were evacuated under vacuum and then filled with high purity nitrogen (containing less than 10 ppm O). The reaction mixture was then placed under a constant nitrogen purge (60 mL / min).
[0163] The reaction mixture was slowly heated to 260°C. At 260°C, 13.566g Na2CO3 and 0.086g K2CO3 were added to the reaction mixture from a powder dispenser over 60 minutes. At the end of the additions, the reaction mixture was heated to 320°C at 1°C / min. After 14 minutes at 320°C, 1.409g 1,4-DFDK was added to the reaction mixture while maintaining a nitrogen purge in the reactor. After 5 minutes, 0.529g lithium chloride was added to the reaction mixture. After 10 minutes, another 0.402g 1,4-DFDK was added to the reactor and the reaction mixture was held at temperature for 15 minutes.
[0164] The reactor contents were then poured from the reactor into a stainless steel pan and allowed to cool. The solids were crushed and ground in an attrition mill through a 2 mm screen. The diphenyl sulfone and salts were extracted from a mixture of acetone and water at pH 1-12. For the final wash, 2.03 g of NaH2PO4·2H2O and 1.86 g of Na2HPO4 were dissolved in 1200 mL of DI water. The powder was then removed from the reactor and dried at 120 °C under vacuum for 12 hours, yielding 72 g of a yellow powder.
[0165] The final PEKK polymer had a T / I ratio of 71 / 29.
[0166] TIFF0007555828000011.tif195170
[0167] As shown above, the PEKK of Examples 4 and 5 surprisingly exhibited improved melt stability (see, for example, VR40 and complex viscosity ratio of 120 / 10) compared to Comparative Example 1, which was produced using an electrophilic process.
[0168] Additionally, despite the relatively low level of metal in the PEKK of Comparative Example 2, the PEKK of Examples 4 and 5 (Σ=0.9 and low metal monomer B) unexpectedly exhibited improved melt stability (see, e.g., VR40 and complex viscosity ratio of 120 / 10) compared to Comparative Example 2 (Σ=0.9 and high metal monomer A). In this regard, parallel plate complex viscosity profiles over time for the PEKK polymers of Comparative Example 2 and Example 5 are shown in Figure 1. Figure 1 further demonstrates the unexpectedly improved stability over time of the PEKK of Example 5 compared to the PEKK of Comparative Example 2.
[0169] In addition, the PEKK of Inventive Example 5, with the amount of reactants meeting the requirement of Σ<6.0, surprisingly exhibited significantly improved melt stability (VR40) compared to the PEKK of Comparative Example 3, where the amount of reactants did not meet the requirement of Σ<6.0.
[0170] Finally, the time at which the shear storage modulus (G') and shear loss modulus (G") cross over ("crossover time"), i.e., the time it takes for the polymer to begin to behave more like a solid than a liquid at 410°C, was also recorded, showing that the PEKK of Examples 4 and 5 unexpectedly did not cross over under the test conditions to the same extent as the PEKK of Comparative Examples 1 and 2.
[0171] Impact Strength Test The PEKK polymer of Comparative Example 1 (CE1) and the PEKK polymer of Example 5 were converted into continuous carbon fiber unitape prepregs by a melt impregnation process.
[0172] The Uni-Tape prepreg has a nominal resin content of 34% by weight and a stiffness of 145 g / m 2 The prepreg tape was cut and laid up into a 32-ply quasi-isotropic layup ([+45 / 90 / -45 / 0]4s) (panel size 350mm x 350mm) in preparation for consolidation in an autoclave.
[0173] The layups were vacuum bagged using a high temperature polyimide film for the bagging film. A continuous ascending consolidation autoclave cycle was employed, using a vacuum of 685-760 mmHg on the layups at the beginning of the cycle, then heating at a heating rate of 3-7°C / min to the consolidation temperature. After reaching the maximum consolidation temperature, a pressure of 6.8 bar was applied and held for a specified time before cooling. The cooling rate, also performed at the same vacuum level, was 3-5°C / min. The test panels were removed from the autoclave and then ultrasonically scanned to ensure excellent consolidation (void content less than 2%) before the laminates were machined into test coupons for compression after impact testing.
[0174] The compression after impact test method used was ASTM D7137 using an impact energy level of 6.7 J / mm.
[0175] Five test coupons were tested for each of CE1 and Example 5. The results as Compressive After Impact (CAI) strength for both polymers were measured at different autoclave hold times at maximum temperature and are shown in Table 3 below.
[0176] TIFF0007555828000012.tif35170
[0177] The polymer of Example 5, which had fewer impurities, showed a 14% increase in toughness, in contrast to the polymer of Comparative Example 1, which had a limited amount of washing to reduce impurities, which showed a 5% decrease.
Claims
1. (I) In the reaction mixture, Na 2 CO 3 , K 2 CO 3 and reacting, in the presence of a solvent, at least one bis(hydroxybenzoyl)benzene monomer [monomer (HB)] having a sum of sodium and potassium concentrations of less than 25 ppm by weight and a calcium concentration of less than 10 ppm by weight with at least one bis(halobenzoyl)benzene monomer [monomer (FB)] having a sum of sodium and potassium concentrations of less than 25 ppm by weight and a calcium concentration of less than 10 ppm by weight, ・ General formula - [M m At least one repeating unit (R M* PEKK )and, ・ General formula - [M p At least one repeating unit (R P* PEKK )and, (In these formulas, M m and M. p are expressed by the following formulas (3) and (4), respectively. Obtaining a mixture containing at least one PEKK polymer comprising: said monomer (FB) and said monomer (HB) are in a molar ratio of at least 1.007:1; The relative amounts of the component reactants in step (I) are determined according to the following formula: (EQ1)Σ=(%Na 2 CO 3 -105)+6*|%K 2 CO 3 -1|+0.25*|37-% Monomers|-(%XS DFDK ) and (EQ2) 0%≦K 2 CO 3 <5 and (EQ3) 0.7%<%XS DFDK and (EQ4) 25%≦Monomers≦44% is selected according to the formula: (a) Σ<6; (b) % Na 2 CO 3 is the Na mole percent unit relative to the number of moles of the monomer (HB) 2 CO 3 is the concentration of (c) %K 2 CO 3 is K in mole percent relative to the number of moles of the monomer (HB) 2 CO 3 is the concentration of %K 2 CO 3 is in the range of 0 mol % to less than 5 mol %; (d) % Monomers is the combined concentration of the monomer (HB) and the monomer (FB) in weight percent relative to the weight of the monomer (HB), the monomer (FB), and the solvent, and % Monomers is 25% by weight to 44% by weight; (e) % XS DFDK is the concentration in mole % of said monomer (FB) over an equimolar concentration of said monomer (HB); The monomer (HB) and the monomer (FB) have the following formula: X 5 -M m -X 5 (13) X 6 -M p -X 6 (14) and During the ceremony, X 5 and X 6 is —OH for the monomer (HB) and is a halogen for the monomer (FB), M m and M. p are expressed as follows: It is expressed as During the ceremony, Each of R1 and R2 is independently selected from the group consisting of alkyl, alkenyl, alkynyl, aryl, ether, thioether, carboxylic acid, ester, amide, imide, alkali or alkaline earth metal sulfonate, alkyl sulfonate, alkali or alkaline earth metal phosphonate, alkyl phosphonate, amine, and quaternary ammonium; each i and j is independently selected from 0 or an integer from 1 to 4; The PEKK polymer has a %[F]>45(μeq / g) / (g / 10min) 0.29 and a T / I ratio of greater than 61 / 39; Where: %[F] is [F], i.e. 19 is the 0.29th power of the ratio between the concentration of fluorine end groups of a PEKK polymer measured by F-NMR and the MFI, i.e., the melt flow index of said PEKK polymer measured at 360° C. under a load of 8.4 Kg according to ASTM D1238; The T / I ratio is determined by the repeat unit (R P* PEKK ) and repeating unit (R M* PEKK ) is the ratio between Process; (II) contacting the mixture containing at least one PEKK polymer obtained in step (I) with a solution comprising sodium dihydrogen phosphate and disodium hydrogen phosphate to isolate the at least one PEKK polymer; A method for producing a poly(ether ketone ketone) polymer [PEKK polymer] [Method (M S ) .
2. In the step (II), the NaH 2 P.O. 4 The method of claim 1, wherein the concentration of is in the range of 0.01 to 0.20% by weight.
3. The PEKK polymer comprises: ・ General formula - [M m At least one repeating unit (R M* PEKK ); and ・ General formula - [M p At least one repeating unit (R P* PEKK ). Including, In these formulas, M m and M. p are represented by formulas (3) and (4) according to claim 1, respectively; The PEKK polymer %[F]>45 (μeq / g) / (g / 10 min) 0.29 , and characterized by a T / I ratio of greater than 61 / 39, Where: %[F] is [F], i.e. 19 is the 0.29th power of the ratio between the concentration of fluorine end groups of the PEKK polymer measured by F-NMR and the MFI, i.e., the melt flow index of the PEKK polymer measured at 360° C. under a load of 8.4 Kg according to ASTM D1238; The T / I ratio is determined by the repeat unit (R P* PEKK ) and repeating unit (R M* PEKK ) is the ratio between The method according to claim 1 or 2.
4. The above (R P PEKK ) / (R M PEKK ) is at least 65:35 (1.86:1), and / or % Na 2 CO 3 +K 2 CO 3 The method according to any one of claims 1 to 3, wherein the σ is at least 103.5%.
5. ・ General formula - [M m At least one repeating unit (R M* PEKK ); and ・ General formula - [M pAt least one repeating unit (R P* PEKK ). (M in these formulas m and M. p are expressed as follows: It is expressed as During the ceremony, Each of R1 and R2 is independently selected from the group consisting of alkyl, alkenyl, alkynyl, aryl, ether, thioether, carboxylic acid, ester, amide, imide, alkali or alkaline earth metal sulfonate, alkyl sulfonate, alkali or alkaline earth metal phosphonate, alkyl phosphonate, amine, and quaternary ammonium; Each of i and j is independently selected from 0 or an integer from 1 to 4. A poly(ether ketone ketone) polymer [PEKK polymer] comprising: %[F]>45 (μeq / g) / (g / 10 min) 0.29 , and characterized by a T / I ratio of greater than 61 / 39, %[F] is [F], i.e. 19 is the 0.29th power of the ratio between the concentration of fluorine end groups of the PEKK polymer measured by F-NMR and the MFI, i.e., the melt flow index of the PEKK polymer measured at 360° C. under a load of 8.4 Kg according to ASTM D1238; The T / I ratio is determined by the repeat unit (R P* PEKK ) and repeating unit (R M* PEKK ) is the ratio between PEKK polymer.
6. The T / I ratio is at least 65 / 35, and / or the %[F] is 50 (μeq / g) / (g / 10min). 0.29 6. The PEKK polymer of claim 5, wherein the PEKK polymer has a viscosity of 100:1 or more.
7. 7. The PEKK polymer of claim 5 or 6 having a phosphorus content of at least 30 ppm as measured by ICP-OES.
8. %[F]>45 (μeq / g) / (g / 10 min) 0.29 where: %[F] is the 0.29th power of the ratio between [F], i.e., the concentration of fluorine end groups of the PEKK polymer as measured by 19F-NMR, and MFI, i.e., the melt flow index of said PEKK polymer as measured at 360° C. under a load of 8.4 Kg according to ASTM D1238. C A method for producing a composite material comprising a polymer matrix containing a polymer C )], (I * ) in the reaction mixture, Na 2 CO 3 , K 2 CO 3 and at least one bis(hydroxybenzoyl)benzene monomer [monomer (HB)] having a sum of sodium and potassium of less than 25 ppm by weight and a calcium concentration of less than 10 ppm by weight, and at least one bis(halobenzoyl)benzene monomer [monomer (FB)] having a sum of sodium and potassium of less than 25 ppm by weight and a calcium concentration of less than 10 ppm by weight, in the presence of a solvent, to produce poly(ether ketone ketone) (PEKK). C ) polymer by preparing ・ General formula - [M m At least one repeating unit (R M* PEKK )and, ・ General formula - [M p At least one repeating unit (R P* PEKK )and, (In these formulas, M m and M. p are expressed by the following formulas (3) and (4), respectively. At least one PEKK comprising C Obtaining a polymer matrix comprising a polymer, The relative amounts of the component reactants in step (I) are determined according to the following formula: (EQ1)Σ=(%Na 2 CO 3 -105)+6*|%K 2 CO 3 -1|+0.25*|37-% Monomers|-(%XS DFDK ) and (EQ2) 0%≦K 2 CO 3 <5 and (EQ3) 0%<%XS DFDK and (EQ4) 25%≦Monomers≦44% is selected according to the formula: (a) Σ<6; (b) % Na 2 CO 3 is the Na mole percent unit relative to the number of moles of the monomer (HB) 2 CO 3 is the concentration of (c) %K 2 CO 3 is K in mole percent relative to the number of moles of the monomer (HB) 2 CO 3 is the concentration of %K 2 CO 3 is in the range of 0 mol % to less than 5 mol %; (d) % Monomers is the combined concentration of the monomer (HB) and the monomer (FB) in weight percent relative to the weight of the monomer (HB), the monomer (FB), and the solvent, and % Monomers is 25% by weight to 44% by weight; (e) % XS DFDK is the concentration in mole % of said monomer (FB) over an equimolar concentration of said monomer (HB); The monomer (HB) and the monomer (FB) have the following formula: X 5 -M m -X 5 (13) X 6 -M p -X 6 (14) and During the ceremony, X 5 and X 6 is —OH for the monomer (HB) and is a halogen for the monomer (FB), M m and M. p are expressed as follows: It is expressed as During the ceremony, Each of R1 and R2 is independently selected from the group consisting of alkyl, alkenyl, alkynyl, aryl, ether, thioether, carboxylic acid, ester, amide, imide, alkali or alkaline earth metal sulfonate, alkyl sulfonate, alkali or alkaline earth metal phosphonate, alkyl phosphonate, amine, and quaternary ammonium; Each of i and j is independently selected from 0 or an integer from 1 to 4; Process; (II * ) above step (I * impregnating reinforcing fibers with the polymer matrix obtained in step (a) to form a composite material; The method (M C ).
9. The PEKK polymer or PEKK C The polymer comprises at least one repeating unit (R M PEKK ) and at least one repeating unit (R P PEKK ) and each of the repeating units (R M PEKK ) is represented by the general formula (1): - [-M m -O-]- (1) It is expressed by the formula: Each repeating unit (R P PEKK ) is represented by the following general formula (2): - [-M p -O-]- (2) In these formulas, M m and M. p are expressed as follows: It is expressed as During the ceremony, R 1 and R 2 is independently selected in each occurrence from the group consisting of alkyl, alkenyl, alkynyl, aryl, ether, thioether, carboxylic acid, ester, amide, imide, alkali or alkaline earth metal sulfonate, alkyl sulfonate, alkali or alkaline earth metal phosphonate, alkyl phosphonate, amine, and quaternary ammonium; i and j, in each occurrence, are independently selected integers ranging from 0 to 4; The method according to claim 1 or 8.
10. Repeating unit (R P PEKK ) / (R M PEKK ) molar ratio is in the range of 55 / 45 to 75 / 25, and / or % Na 2 CO 3 +%K 2 CO 3 10. The method of claim 8 or 9, wherein the solubility of the carboxylic acid is ≦106.0 mol%.
11. 9. The method of claim 8, wherein the reinforcing fibers are continuous and are carbon fibers, graphite fibers, glass fibers (such as E-glass fibers), ceramic fibers (such as silicon carbide fibers), synthetic polymer fibers (such as aromatic polyamide fibers, polyimide fibers, and polybenzoxazole fibers), or combinations thereof.
12. The PEKK polymer or PEKK C The step of preparing the polymer comprises adding an endcapping agent to the reaction mixture, the endcapping agent comprising: an excess of one or more bis(halobenzoyl)benzene monomers, and combinations thereof; The method of claim 1 or 8, wherein G is -C(O)-Ar, where Ar is an arylene group.
13. A composite material [Composite Material (C )] comprising at least one PEKK polymer according to any one of claims 5 to 7 and at least one reinforcing fiber. S ) .
14. 14. The composite material according to claim 13, comprising 20 to 80 wt. % reinforcing fibers and 80 to 20 wt. % of the PEKK polymer, based on the weight of the PEKK composite material. S ).
Citation Information
Patent Citations
Prepn process of poly (ether-ketone-ketone) as high performance polymer
CN1974631A
Stabilized modifier and thermoplastic material with modifiedimpact resistance
JP1995286087A
Molding material, manufacturing method of molded article using the same, and molded article
JP2015193812A
Poly(ether ketone ketone) polymers, corresponding synthesis methods and polymer compositions and articles made therefrom
JP2020502337A