Compositions containing coloring agents, methods for preparing said compositions and their uses - Patents.com

A siloxane-polyoxamide copolymer-based method addresses pigment incorporation challenges in polymeric materials, achieving uniform color distribution and thermal stability in color masterbatches for various plastics.

JP7556052B2Active Publication Date: 2024-09-25WACKER CHEMIE AG
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2022567783
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-05-11
Publication Date
2024-09-25
Estimated Expiration
2040-05-11

AI Technical Summary

Technical Problem

The incorporation of pigments into polymeric materials during melt-mixing is challenging due to issues such as weak pigment agglomeration, uneven distribution, and thermal degradation of silicone copolymers at high processing temperatures, leading to inhomogeneous coloration and reduced mechanical properties in color masterbatches.

Method used

A method involving the reaction of siloxane-polyoxamide copolymers with colorants and optional additives, followed by pelletization, to create a homogeneous colorant-containing composition that can withstand high temperatures, ensuring uniform color distribution and improved thermal stability.

Benefits of technology

The method produces color masterbatches with excellent uniformity, high thermal stability, and improved rheological behavior, suitable for a wide range of polymeric materials, with enhanced compatibility and reduced thermal degradation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007556052000001
    Figure 0007556052000001
  • Figure 0007556052000002
    Figure 0007556052000002
  • Figure 0007556052000003
    Figure 0007556052000003
Patent Text Reader

Abstract

The present invention relates to colorant-containing compositions comprising (D) at least one colorant, (E) at least one siloxane-polyoxamide copolymer containing a component of general formula (IV), in which the residues and subscripts have the meanings as defined in claim 1, and optionally (F) additives. The present invention also relates to processes for their preparation and their use for coloring polymeric materials. TIFF2023526192000006.tif27166
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to colorant-containing compositions, processes for their preparation, and their use in coloring polymeric materials. [Background technology]

[0002] Essential to the individual coloring of plastic articles is what is now called a color masterbatch, which is typically made from plastic pellets and colorants. The required coloring is generally achieved by mixing and melting the colorant and plastic pellets in an extruder, while mixing with small amounts of additives.

[0003] The uniformity of the color shade in the final plastic article depends on the flow behavior achieved in the melt and / or the quality of the distribution of the masterbatch in the matrix. Therefore, there are specific types of masterbatches for each type of plastic. The fundamental problem in masterbatch production is that pigments, whose primary particles are in the size range of a few nanometers to a few micrometers, must be incorporated into the polymeric material in a melt-mixing process. However, the incorporation of pigment agglomerates and the homogeneous distribution of the pigment in the sometimes very viscous plastic melt can be quite problematic. Also, in this melt compounding procedure, the already melted and pelletized polymeric material must be melted and pelletized again, possibly several times depending on the process. Repeated heat loads as well as the associated high energy expenditure as a result of chain decomposition reactions can also damage the masterbatch carrier material, resulting in a reduction in the molar mass.

[0004] The mixing behavior of colorants in the respective plastics is unpredictable, especially at relatively high concentrations of pigments and / or dyes, and therefore the preparation of masterbatches in particular often presents difficulties, since the colorants, i.e., for example, pigments or dyes, to be incorporated into a particular plastic often undergo weak agglomeration, causing severe inhomogeneity, which leads to unfavorable properties on the part of the masterbatch, for example in terms of rheological or mechanical properties.

[0005] EP-A2113522 discloses a masterbatch that comprises a polysiloxane-polyurea copolymer, which is a particularly interesting plastic, and because of its advantageous physical properties, it covers a wide range of application areas and can be easily and finely distributed into many thermoplastic polymers.In addition, it is relatively easy to incorporate color pigments in finely divided and high concentrations into the reactants used to produce this silicone copolymer.The disadvantage of using the color masterbatch according to EP-A2113522 during the thermoplastic processing of polymers is the fact that the silicone copolymer used in EP-A2113522 has a tendency to chain decomposition at relatively high processing temperatures above about 220°C, so that due to its thermal decomposition, this silicone polymer cannot be used with certain thermoplastics that have relatively high processing temperatures, since a uniform supply of pigments into the thermoplastic matrix is ​​no longer guaranteed. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] European Patent Application Publication No. 2113522 Summary of the Invention

[0007] The subject of the present invention is a method for producing a colorant-containing composition, comprising the steps of: In a first step, at least one siloxane (A) of general formula (I),

[0008] [ka] [In the formula, R 1 are the same or different and are monovalent SiC-bonded optionally substituted hydrocarbon radicals, which may be interrupted by heteroatoms; R 2 are the same or different and are hydrogen atoms or monovalent optionally substituted hydrocarbon radicals, which may be interrupted by heteroatoms; Y are the same or different and represent a divalent optionally substituted hydrocarbon group having 1 to 40 carbon atoms, each of which may be substituted with an oxygen atom or -NR-; R is a hydrogen atom or a monovalent optionally substituted hydrocarbon group; n is 0 or a number from 1 to 1000; p is 0 or a number from 1 to 10. At least one compound (B) of the following general formula: R 4 NH-R 3 -NR 4 H (II) [In the formula, R 3 is a divalent optionally substituted hydrocarbon group having 1 to 40 carbon atoms, each of which may be substituted with an oxygen atom or -NR'-; R' is a hydrogen atom or a monovalent optionally substituted hydrocarbon group; R 4 may be the same or different and are hydrogen atoms or monovalent optionally substituted hydrocarbon radicals, which may be interrupted by heteroatoms. (D) at least one colorant; Optionally, a compound of the general formula (C): R 5 NH-Y 1 -SiR 6 2-[O-SiR 6 2] m -O-SiR 6 2-Y 1 -NHR5 (III) [In the formula, R 6 are the same or different and are monovalent SiC-bonded optionally substituted hydrocarbon radicals, which may be interrupted by heteroatoms; R 5 are the same or different and are hydrogen atoms or monovalent optionally substituted hydrocarbon radicals, which may be interrupted by heteroatoms; Y 1 are the same or different and are optionally substituted divalent hydrocarbon radicals having 1 to 40 carbon atoms, each of which may be optionally substituted by an oxygen atom or NR″-; R″ is a hydrogen atom or a monovalent optionally substituted hydrocarbon group; m is 0 or a number from 1 to 1000. and Optional Additives (F) are mixed together and reacted, Optionally, in a second step, the composition obtained in the first step is melted and then pelletized.

[0009] A further subject of the present invention is a colorant-containing composition comprising: (D) at least one colorant; (E) at least one siloxane-polyoxamide copolymer containing units of general formula (IV)

[0010] [ka] [In the formula, R 1 , R 3 , R 4 , Y, n and p in each case have the definitions given above for them; and Optionally, (F) additives. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] Preferably, n is a number between 20 and 400, more preferably a number between 30 and 250, and most preferably a number between 50 and 200.

[0012] Preferably, m is a number between 20 and 400, more preferably between 30 and 250, and most preferably between 50 and 200.

[0013] Preferably, p is a number from 1 to 3, more preferably 1 or 2, and more specifically 1.

[0014] Hydrocarbon group R 1 Examples of the alkyl group include alkyl groups such as methyl, ethyl, n-propyl, isopropyl, 1-n-butyl, 2-n-butyl, isobutyl, tert-butyl, n-pentyl, isopentyl, neopentyl, and tert-pentyl groups; hexyl groups such as n-hexyl groups; octyl groups such as n-octyl groups; isooctyl groups such as 2,2,4-trimethylpentyl groups; nonyl groups such as n-nonyl groups; decyl groups such as n-decyl groups; dodecyl groups such as n-dodecyl groups; and n-octadecyl groups. which are cycloalkyl groups such as octadecyl, cyclopentyl, cyclohexyl, cycloheptyl and methylcyclohexyl groups; alkenyl groups such as vinyl, 1-propenyl and 2-propenyl groups; aryl groups such as phenyl, naphthyl, anthryl and penanthryl groups; alkaryl groups such as o-, m-, p-tolyl, xylyl and ethylphenyl groups; or aralkyl groups such as benzyl or α- and β-phenylethyl groups.

[0015] Preferably, the group R 1 comprises an aliphatic hydrocarbon group, more preferably a methyl group or an ethyl group, and more specifically a methyl group.

[0016] base R 2 Examples of the group R 1 is the group shown for

[0017] Preferably, the group R 2comprises an aliphatic hydrocarbon group, more preferably a methyl group or an ethyl group, and more specifically an ethyl group.

[0018] base R 3 Examples are a methylene group, an ethylene group, a propylene group or a hexylene group.

[0019] Preferably, the group R 3 comprises a divalent aliphatic hydrocarbon group, more preferably an ethylene group or a hexylene group, more specifically an ethylene group.

[0020] base R 4 Examples of the group R 1 or a hydrogen atom.

[0021] Preferably, the group R 4 contains a hydrogen atom or an aliphatic hydrocarbon group, more preferably a hydrogen atom or a methyl group, and more specifically a hydrogen atom.

[0022] base R 5 Examples of the group R 1 is the group shown for

[0023] Preferably, the group R 5 contains a hydrogen atom or an aliphatic hydrocarbon group, and more preferably, R 5 comprises a hydrogen atom or a methyl group, more specifically a hydrogen atom.

[0024] base R 6 Examples of the group R 1 is the group shown for

[0025] Preferably, the group R 6 comprises an aliphatic hydrocarbon group, more preferably a methyl group or an ethyl group, and more specifically a methyl group.

[0026] Examples of the group R are the groups R 1 or a hydrogen atom.

[0027] Preferably, the groups R, R' and R" in each case independently of one another are a methyl group or a hydrogen atom, more preferably a hydrogen atom.

[0028] Groups Y and Y 1 Examples of, independently of one another, are the methylene, ethylene, propylene and hexylene radicals.

[0029] Groups Y and Y 1 are each independently preferably a divalent aliphatic hydrocarbon group, more preferably a methylene group or a propylene group, more specifically a propylene group.

[0030] Component (A) preferably comprises a liquid that is colorless at 20° C. and 1013 hPa.

[0031] The component (A) used in the present invention preferably has a viscosity at 25°C of 10 mPas to 30,000 mPas, more preferably 30 mPas to 2,000 mPas.

[0032] Examples of siloxanes (A) that can be used in the process of the present invention are R 1 = methyl, R 2 =H3C-CH2-, Y=-(CH2)3-, p=1, n=140, R 1 = methyl, R 2 =H3C-, Y=-(CH2)3-, p=1, n=140, R 1 = methyl, R 2 =H3C-, Y=-(CH2)3-, p=1, n=50, R 1 = methyl, R 2 =H3C-CH2-, Y=-(CH2)3-, p=1, n=50, R 1 = methyl, R 2 =H3C-CH2-, Y=-(CH2)3-, p=1, n=140 and R 1 = methyl, R 2=H3C-CH2-, Y=-(CH2)3-, p=1, n=250, R 1 = methyl, R 2 =H3C-CH2-, Y=-(CH2)3-, p=1, n=140, R 1 = methyl, R 2 =H3C-, Y=-(CH2)3-, p=1, n=140 or R 1 = methyl, R 2 Preferred is the formula (I) with =H3C-CH2-, Y=-(CH2)3-, p=2 and n=140; R 1 = methyl, R 2 Particularly preferred is formula (I) where =H3C-CH2-, Y=-(CH2)3-, p=1 and n=140.

[0033] Component (A) includes commercially available products or products prepared by methods common in silicon chemistry.

[0034] The compound (B) used in the process of the present invention is preferably NH2-(CH2)2-NH2, NH2-(CH2)6-NH2, H2N-[(CHCH3-CH2-O)6(C2H4-O) 12 ]-(CH2-CHCH3)-NH2, H2N-[(CHCH3-CH2-O)6(C2H4-O) 39 ]-(CH2-CHCH3)-NH2, or H2N-[(CHCH3-CH2-O)4(C2H4-O)9]-(CH2-CHCH3)-NH2, with NH2-(CH2)2-NH2 being preferred.

[0035] Component (B) includes commercially available products or products prepared by methods common in chemistry.

[0036] In the process of the present invention, component (B) is preferably used in an amount of 0.2 to 40 parts by weight, more preferably 0.4 to 4 parts by weight, based on 100 parts by weight of component (A).

[0037] Component (C) preferably comprises a liquid that is colorless at 20° C. and 1013 hPa.

[0038] The component (C) optionally used in the present invention preferably has a viscosity at 25°C of between 10 mPas and 30000 mPas, more preferably between 30 mPas and 2000 mPas.

[0039] Examples of the optionally employed component (C) are NH2-(CH2)3-SiMe2-[O-SiMe2]2-O-SiMe2-(CH2)3-NH2, NH2-(CH2)3-SiMe2-[O-SiMe2] 50 -O-SiMe2-(CH2)3-NH2, NH2-(CH2)3-SiMe2-[O-SiMe2] 140 -O-SiMe2-(CH2)3-NH2, NH2-(CH2)3-SiMe2-[O-SiMe2] 250 -O-SiMe2-(CH2)3-NH2 and NH2-(CH2)-SiMe2-[O-SiMe2] 50 -O-SiMe2-(CH2)-NH2, NH2-(CH2)3-SiMe2-[O-SiMe2] 50 -O-SiMe2-(CH2)3-NH2 or NH2-(CH2)3-SiMe2-[O-SiMe2] 140 -O-SiMe2-(CH2)3-NH2 is preferred, and NH2-(CH2)3-SiMe2-[O-SiMe2] 140 Particularly preferred is --O--SiMe2--(CH2)3--NH2, where Me represents a methyl group.

[0040] Although not preferred, when component (C) is used in the process of the present invention, the amount in question is preferably from 1 to 50 parts by weight, more preferably from 2 to 20 parts by weight, in each case based on 100 parts by weight of component (A).

[0041] Component (C) includes commercially available products and products which can be prepared by methods common in silicon chemistry.

[0042] The colorant (D) used in the present invention may be any colorant known up to now.

[0043] By colorants is meant all substances which have an optical effect. Examples of colorants (D) are those given in DIN ISO 18451.

[0044] The colorant (D) is preferably an inorganic or organic colorant or a precursor thereof, more preferably one selected from inorganic dyes, organic dyes, inorganic and organic pigments, and precursors or mixtures thereof.

[0045] Examples of inorganic pigments are oxides such as iron oxide (brown, red, black), chromium oxide (green), titanium dioxide, or carbon, such as carbon black, chromates, such as lead chromate yellow, molybdate orange, or complexes of inorganic chromatic pigments, such as chrome titanium yellow, chrome iron brown, cobalt blue, nickel titanium yellow, zinc iron brown, bismuth vanadate yellow, or from the group of the sulphides, such as cadmium sulphide (yellow, orange, red), cerium sulphide (yellow, orange, red), ultramarine blue (purple, blue) and zinc sulphide (white).

[0046] Organic pigments include azo pigments such as lake azo pigments (yellow, green), disazo pigments (yellow, orange, red), and disazo condensation pigments (yellow, red), benzimidazole pigments (yellow, orange), metal complex pigments (yellow), isoindoline pigments (yellow), isoindolinone pigments (yellow), and polycyclic pigments such as quinacridone (purple, blue), quinophthalone (yellow), diketopyrrolopyrrole (orange, red, purple), dioxazine dyes (purple), indanthrone (blue), perylene (red, purple), and phthalocyanine (blue, green).

[0047] Examples of dyes are anthraquinone dyes, dioxazine dyes, indigoid dyes, formazan dyes, methine dyes, nitro and nitroso dyes, sulfur dyes, and metal complex dyes.

[0048] The colorant (D) is more preferably an inorganic or organic pigment, more particularly an inorganic pigment.

[0049] In the method of the present invention, the colorant (D) is preferably used in an amount of 2 to 400 parts by weight, more preferably 20 to 300 parts by weight, and more specifically 25 to 200 parts by weight, based in each case on 100 parts by weight of component (A).

[0050] If desired, additives (F) may also be used, such as, for example, additives selected from nanofillers, stabilizers, antistatic agents, flame retardants, adhesion promoters, nucleating agents, foaming agents and antibacterial agents.

[0051] When additive (F) is used, the amount involved is preferably 0.1 to 50 parts by weight, more preferably 0.5 to 30 parts by weight, based in each case on 100 parts by weight of component (A). The composition of the present invention preferably does not contain additive (F).

[0052] The individual components of the method of the invention may in each case be one type of such component or may be a mixture of at least two different types of such components.

[0053] In the process of the present invention, preferably no further components other than components (A), (B), (C), (D) and (F) are used.

[0054] Since some of the reactants used may be sensitive to moisture and / or air, it is advantageous if the first step of the process is carried out in the absence of moisture and under a protective gas, preferably nitrogen or argon.

[0055] In the first step of the process of the present invention, colorant (D) is preferably mixed with one or more of components (A), (B) or (C), more preferably with component (A). The uniform dispersion of high concentrations of colorant (D) in these relatively low viscosity systems has the advantage that it is easily manageable and can be easily achieved by techniques well established in the paint and varnish industry.

[0056] The first step of the process of the present invention preferably involves a solid-liquid dispersion of the colorant (D) in components (A), (B) and / or (C), with optimal incorporation being achieved, for example, by grinding of the pigment (D).

[0057] It is therefore also easily possible to produce pastes with the base shade on the basis of liquid precursors. These pastes can be mixed to give the final shade, preferably before the final polymer synthesis in a first step. The subsequent complete reaction of the components to form the finished colorant-containing composition gives the desired shade of the target product in only one further processing step. Thus, preferably, the carrier material of the color masterbatch is subjected to a thermal load only once before its final development. The influence of possible pyrolysis reactions on the matrix is ​​correspondingly smaller.

[0058] The first step of the process according to the invention is preferably carried out at a temperature of at least 0° C., more preferably between 20 and 250° C., although in principle it is also possible to operate at lower or higher temperatures.

[0059] The first step of the invention is preferably carried out under the pressure of the surrounding atmosphere, in other words 900-1100 hPa, although in principle it is also possible to operate at lower or higher pressures.

[0060] The composition obtained in the first step is preferably solid at 20° C. and 1013 hPa.

[0061] If desired, the composition obtained in the first step can be melted in a second step and subsequently pelletized, which can be done continuously, semi-batch or batchwise.

[0062] The melting in the second step is in any case carried out under a pressure of preferably 100 to 30000 hPa, more preferably 1000 to 15000 hPa, at a temperature of 50 to 250°C, more preferably 100 to 200°C.

[0063] The pelletizing in the second step can be carried out entirely in existing equipment, preferably a twin strand pelletizing equipment or an underwater pelletizing equipment.

[0064] The pelletization in the second step is preferably carried out under a pressure of 900 to 1100 hPa at a temperature of 5 to 250°C, more preferably 10 to 150°C in any case.

[0065] As a result of the second step of the present invention, pellets of any desired shape can be obtained. The pellets obtained according to the present invention preferably have a spherical or cylindrical shape, preferably with a side length / diameter of 1 mm to 10 mm.

[0066] The polysiloxane-polyoxamide copolymer (E) of the composition of the present invention, preferably formed by polycondensation reaction from components (A), (B) and optionally (C) with elimination of low molecular weight components such as alcohols, is preferably an alternating block copolymer of (AB)n type (consisting of at least two block sequences) or ABA type (consisting of three blocks).When component (C) is used to prepare the copolymer (E), the dispersibility of certain dyes and / or pigments can be optionally optimized by improved wetting behavior.

[0067] The siloxane structure of component (A) is highly apolar in copolymer (E), whereas organic component (B) introduces polar groups into copolymer (E). The variation of apolar and polar units allows polysiloxane copolymer (E) to be adapted to a wide variety of different polymeric materials in terms of compatibility. As a result, color masterbatches for virtually all polymeric materials can be produced from one or a few basic materials. Thus, based on these polysiloxane copolymers (E), it is possible to produce universal masterbatches for virtually all polymeric materials, but at least for a large group of polymeric materials in any case, such as polyolefins, polyesters, polyamides, styrene-based polymers, etc.

[0068] Examples of units of formula (IV) in the copolymer (E) are R 1 = methyl, R 3 =-(CH2)2-, R 4 =H, Y=-(CH2)3-, p=1, n=140, R 1 = methyl, R 3 =-(CH2)6-, R 4 =H, Y=-(CH2)3-, p=1, n=140, R 1 = methyl, R 3 =-(CH2)2-, R 4 =H, Y=-(CH2)3-, p=1, n=50, R 1 = methyl, R 3 =-(CH2)6-, R 4 =H, Y=-(CH2)3-, p=1, n=50, R 1 = methyl, R 3 =-(CH2)6-, R 4 =H, Y=-(CH2)3-, p=2, n=140 and R 1 = methyl, R 3 =-(CH2)2-, R 4 =H, Y=-(CH2)3-, p=1, n=250, R 1 = methyl, R 3=-(CH2)2-, R 4 =H, Y=-(CH2)3-, p=1, n=140, R 1 = methyl, R 3 =-(CH2)6-, R 4 =H, Y=-(CH2)3-, p=1, n=140, or R 1 = methyl, R 3 =-(CH2)2-, R 4 =H, Y=-(CH2)3-, p=1, n=50 It is preferred that the polymer is composed of units of formula (IV) R 1 = methyl, R 3 =-(CH2)2-, R 4 =H, Y=-(CH2)3-, p=1, n=140, or R 1 = methyl, R 3 =-(CH2)2-, R 4 =H, Y=-(CH2)3-, p=1, n=50 Particularly preferred is one composed of units of formula (IV):

[0069] The end groups of copolymer (E) are preferably alternating unreacted amino end groups of components (B) or (C) or unreacted oxamido ester groups of component (A), with the preferred end groups being unreacted oxamido ester end groups of component (A), since unreacted amino end groups can potentially lead to instances of discoloration at relatively high operating temperatures, resulting in adverse changes in the color of the compositions of the present invention.

[0070] A typical example of the copolymer (E) is R 1 = methyl, R 2 siloxane (A) of formula (I) used in the process of the present invention having =H3C-CH2-, Y=-(CH2)3-, p=1, n=140, and R 3 =-(CH2)2-, R 4 the reaction product of compound (B) of formula (II) having =H, or R 1 = methyl, R 2siloxane (A) of formula (I) having =H3C-CH2-, Y=-(CH2)3-, p=1, n=50; and R 3 =-(CH2)2-, R 4 a reaction product with a compound (B) of formula (II) having =H, or R 1 = methyl, R 2 siloxane (A) of formula (I) having =H3C-CH2-, Y=-(CH2)3-, p=1, n=250, and R 3 =-(CH2)2-, R 4 a reaction product with a compound (B) of formula (II) having =H, or R 1 = methyl, R 2 siloxane (A) of formula (I) having =H3C-CH2-, Y=-(CH2)3-, p=1, n=140, and R 3 =-(CH2)6-, R 4 a reaction product with a compound (B) of formula (II) having =H, or R 1 = methyl, R 2 siloxane (A) of formula (I) having =H3C-CH2-, Y=-(CH2)3-, p=1, n=140, and R 3 =-(CH2)2-, R 4 Compound (B) of formula (II) having =H and R 6 = methyl, R 5 =H, Y 1 = -(CH2)3-, m = 140, or R 1 = methyl, R 2 siloxane (A) of formula (I) having =H3C-CH2-, Y=-(CH2)3-, p=1, n=50; and R 3 =-(CH2)6-, R 4 Compound (B) of formula (II) having =H and R 6 = methyl, R 5 =H, Y 1 = -(CH2)3-, m = 140, or R 1 = methyl, R 2siloxane (A) of formula (I) having =H3C-, Y=-(CH2)3-, p=1, n=200, and R 3 =-(CH2)2-, R 4 Compound (B) of formula (II) having =H and R 6 = methyl, R 5 =H, Y 1 = -(CH2)3-, m = 140, or R 1 = methyl, R 2 siloxane (A) of formula (I) having =H3C-CH2-, Y=-(CH2)3-, p=1, n=140, and R 3 =-(CH2)2-, R 4 Compound (B) of formula (II) having =H and R 3 =-[(CHCH3-CH2-O)6(C2H4-O) 12 ]-(CH2-CHCH3)-, R 4 a reaction product with a compound (B) of formula (II) having =H, or R 1 = methyl, R 2 siloxane (A) of formula (I) having =H3C-CH2-, Y=-(CH2)3-, p=1, n=50; and R 3 =-(CH2)6-, R 4 Compound (B) of formula (II) having =H and R 3 =-[(CHCH3-CH2-O)6(C2H4-O) 39 ]-(CH2-CHCH3)-, R 4 a reaction product with a compound (B) of formula (II) having =H, or R 1 = methyl, R 2 siloxane (A) of formula (I) having =H3C-, Y=-(CH2)3-, p=1, n=200, and R 3 =-(CH2)2-, R 4 Compound (B) of formula (II) having =H and R 3 =-[(CHCH3-CH2-O)4(C2H4-O)9]-(CH2-CHCH3)-, R 4 It is the reaction product with a compound (B) of formula (II) having =H.

[0071] The copolymer (E) in the composition of the invention preferably has a molecular weight (number average) of from 20 000 g / mol to 1 000 000 g / mol, more preferably from 40 000 g / mol to 200 000 g / mol, in each case measured by size exclusion chromatography (SEC) in THF at 45° C.

[0072] The composition of the present invention is preferably a composition comprising: (E) a copolymer comprising units of formula (IV) (D) Pigments and Optionally, (F) additives.

[0073] More preferably, the composition of the invention is a composition comprising: (E)R 1 = methyl, R 3 =-(CH2)2-, R 4 Copolymers comprising units of formula (IV) with =H, Y=-(CH2)3-, p=1 and n=140; (D) inorganic pigments from the group of oxides, or (E)R 1 = methyl, R 3 =-(CH2)6-, R 4 Copolymers comprising units of formula (IV) with =H, Y=-(CH2)3-, p=1 and n=140; (D) inorganic pigments from the group of oxides, or (E)R 1 = methyl, R 3 =-(CH2)2-, R 4 Copolymers comprising units of formula (IV) with =H, Y=-(CH2)3-, p=1 and n=250; (D) inorganic pigments from the group of oxides, or (E)R 1 = methyl, R 3 =-(CH2)2-, R 4 Copolymers comprising units of formula (IV) with =H, Y=-(CH2)3-, p=1 and n=50; (D) inorganic pigments from the group of oxides, or (E)R 1 = methyl, R 3=-(CH2)2-, R 4 Copolymers comprising units of formula (IV) with =H, Y=-(CH2)3-, p=1 and n=140; (D) an organic pigment, or (E)R 1 = methyl, R 3 =-(CH2)6-, R 4 Copolymers comprising units of formula (IV) with =H, Y=-(CH2)3-, p=1 and n=140; (D) an organic pigment, or (E)R 1 = methyl, R 3 =-(CH2)2-, R 4 Copolymers comprising units of formula (IV) with =H, Y=-(CH2)3-, p=1 and n=250; (D) an organic pigment, or (E)R 1 = methyl, R 3 =-(CH2)2-, R 4 Copolymers comprising units of formula (IV) with =H, Y=-(CH2)3-, p=1 and n=50; (D) an organic pigment, or (E)R 1 = methyl, R 3 =-(CH2)2-, R 4 Copolymers comprising units of formula (IV) with =H, Y=-(CH2)3-, p=1 and n=140; (D) inorganic pigments from the group of carbon blacks, or (E)R 1 = methyl, R 3 =-(CH2)6-, R 4 Copolymers comprising units of formula (IV) with =H, Y=-(CH2)3-, p=1 and n=140; (D) inorganic pigments from the group of carbon blacks, or (E)R 1 = methyl, R 3 =-(CH2)2-, R 4 Copolymers comprising units of formula (IV) with =H, Y=-(CH2)3-, p=1 and n=250; (D) inorganic pigments from the group of carbon blacks, or (E)R 1 = methyl, R3 =-(CH2)2-, R 4 Copolymers comprising units of formula (IV) with =H, Y=-(CH2)3-, p=1 and n=50; (D) Inorganic pigments from the group of carbon blacks.

[0074] Further preferred is a composition comprising: (E)R 1 = methyl, R 3 =-(CH2)2-, R 4 Copolymers comprising units of formula (IV) with =H, Y=-(CH2)3-, p=1 and n=140; (D) inorganic pigments from the group of carbon blacks, or (E)R 1 = methyl, R 3 =-(CH2)6-, R 4 Copolymers comprising units of formula (IV) with =H, Y=-(CH2)3-, p=1 and n=140; (D) inorganic pigments from the group of carbon blacks, or (E)R 1 = methyl, R 3 =-(CH2)2-, R 4 Copolymers comprising units of formula (IV) with =H, Y=-(CH2)3-, p=1 and n=140; (D) inorganic pigments from the group of oxides, or (E)R 1 = methyl, R 3 =-(CH2)6-, R 4 Copolymers comprising units of formula (IV) with =H, Y=-(CH2)3-, p=1 and n=140; (D) inorganic pigments from the group of oxides, or (E)R 1 = methyl, R 3 =-(CH2)2-, R 4 Copolymers comprising units of formula (IV) with =H, Y=-(CH2)3-, p=1 and n=140; (D) an organic pigment, or (E)R 1 = methyl, R 3 =-(CH2)6-, R 4Copolymers comprising units of formula (IV) with =H, Y=-(CH2)3-, p=1 and n=140; (D) Organic pigments.

[0075] Particularly preferred is a composition comprising: (E)R 1 = methyl, R 3 =-(CH2)2-, R 4 Copolymers comprising units of formula (IV) with =H, Y=-(CH2)3-, p=1 and n=140; (D) inorganic pigments from the group of carbon blacks, or (E)R 1 = methyl, R 3 =-(CH2)2-, R 4 Copolymers comprising units of formula (IV) with =H, Y=-(CH2)3-, p=1 and n=140; (D) inorganic pigments from the group of oxides, or (E)R 1 = methyl, R 3 =-(CH2)2-, R 4 Copolymers comprising units of formula (IV) with =H, Y=-(CH2)3-, p=1 and n=140; (D) Organic pigments.

[0076] The individual components of the composition of the invention may in any case be one type of such component or may be a mixture of at least two different types of such components.

[0077] The compositions of the invention or compositions produced according to the invention can be used for all purposes for which colorant-containing compositions have been used up to now, preferably as color additives in the production of plastics, plastic profiles or plastic fibers.

[0078] A further subject of the invention is a method for producing colored molded articles by mixing a polymeric material with the colorant-containing composition of the invention or with a colorant-containing composition produced according to the invention, melting and homogenizing the resulting mixture, followed by shapingly cooling the mixture.

[0079] The process of the present invention for producing colored molded articles can be carried out continuously, semi-batch, or batchwise.

[0080] The process of the present invention for producing a colored molded article can be carried out according to different operating modes known up to now, depending on the polymeric material employed, for example using the pressures, temperatures and equipment etc. specified for the second step of the process of the present invention for producing the composition of the present invention.

[0081] Preferred examples of polymeric materials for use in the present invention are polyethylene, polypropylene, polyamide, polyethylene terephthalate, polybutylene terephthalate, thermoplastic elastomers based on crosslinked rubber, ethylene-vinyl acetate, polyhydroxybutyrate and / or copolymers or mixtures thereof, as well as polystyrene, impact-modified polystyrene, styrene-acrylonitrile copolymers, acrylonitrile-butadiene-styrene copolymers, polyvinyl chloride, polyvinylidene fluoride, ethylene-tetrafluoroethylene (ETFE), polymethyl methacrylate, polycarbonate, polyaryletherketones, polyacrylonitrile, polyetherimides, polyethylene naphthalate, polyethersulfones, polyimides, polyketones, polyoxymethylene, polyphenylene sulfide, polyphenylene sulfone, polysulfone, styrene-butadiene rubber, acrylonitrile-butadiene rubber, natural rubber, and copolymers or mixtures thereof, with polyethylene, polypropylene, polyamide, polyethylene terephthalate or polybutylene terephthalate being particularly preferred.

[0082] These polymeric materials pigmented according to the invention may more particularly be produced by mixing at least one polymeric material in the molten state with a composition according to the invention or with a composition produced according to the invention and cooling the mixture obtained. The polymeric materials pigmented according to the invention preferably take the form of a molded article obtained by a molding operation selected from the group consisting of injection molding, extrusion, compression molding, rolling, rotational molding, laser sintering, fused deposition modeling (FDM), pelletizing and / or casting.

[0083] In particular, it has proven advantageous that the colorant-containing compositions of the present invention or produced according to the present invention are highly tolerant to a wide variety of plastics and therefore exhibit high compatibility with a wide variety of polymeric materials or polymer mixtures at the use concentrations customary for the processing and modification of plastics.

[0084] The process of the present invention has the notable advantage of being highly efficient with respect to the process regime.

[0085] The color masterbatch of the present invention, which can be produced according to the method regime of the present invention, has been found to have excellent uniformity, i.e., no concentration gradient of the colorant in the masterbatch. Further advantageous properties of the color masterbatch include an unusually high thermal stability, extremely good rheological behavior and good stress-strain behavior.

[0086] The compositions of the present invention are furthermore notable for their high compatibility with regard to the colorants added and their amounts used, and have the advantage of exhibiting very high thermal stability, especially in the relatively high temperature range exceeding 250°C.

[0087] An additional advantage of the method of the present invention is that following dispersion of the colorant in the fluid polymer precursor, the colorant is further dispersed and homogenized in the fully reacted polymer matrix in the mixer or extruder, which further improves the distribution of the colorant in the color masterbatch.

[0088] The process of the present invention has the advantage that the reactants used are very controllable and can be processed using conventional equipment. EXAMPLES

[0089] The examples described below are carried out, unless otherwise specified, under ambient atmospheric pressure, i.e. around 1000 hPa, at room temperature, i.e. around 23° C. or the temperature which occurs when the reactants are combined at room temperature without additional heating or cooling, and at a relative atmospheric humidity of about 50%. Furthermore, unless otherwise indicated, all parts and percentages reported are by weight.

[0090] For the purposes of the present invention, the number average molecular weight Mn is determined by size exclusion chromatography (SEC) against polystyrene standards in THF at 45° C. with a flow rate of 1.0 ml / min and detection by ELSD (Evaporative Light Scattering Detector) on a triple PLGel MixC column set from Agilent Technologies with an injection volume of 100 μL after acetylation with acetic anhydride.

[0091] Silicone 1: an ethyloxalamidopropyl-terminated polydimethylsiloxane of the following formula having an average molecular weight Mn of 11457 g / mol H5C2O-CO-CO-NH-C3H6-Si(CH3)2-[OSi(CH3)2] n -OSi(CH3)2-C3H6-NH-CO-CO-OC2H5

[0092] Diamine 1: Ethylenediamine NH2-(CH2)2-NH2

[0093] Diamine 2: an aliphatic polyether diamine with an amine number of 3.3 meq / g (commercially available under the name "Jeffamine ED 600" from Huntsman, Everberg, Belgium).

[0094] Centrifugal mixer: ARE 250 from C3-Analysentechnik, Haar, Germany, manufactured by Shinki Corporation, Tokyo, Japan

[0095] [Example 1] 114.5 g of Silicone 1 was weighed into a 250 ml polypropylene beaker, and then 45 g of TiO2 (commercially available under the name Kronos 2225 titanium dioxide from Kronos Titan GmbH, Leverkusen, Germany) was added as an inorganic pigment. The mixture was homogenized in a centrifugal mixer at a speed of 2000 rpm for a total of 5 minutes to obtain a liquid color paste. Then, 0.6 g of Diamine 1 was added to the mixture, and the mixture was homogenized in a centrifugal mixer at 2000 rpm for another 120 seconds. After an additional 20 minutes of isothermal reaction time without further stirring, the mixture was polymerized. The solid color masterbatch formed was then removed from the PP beaker and cut into pieces less than 5 mm.

[0096] [Example 2] 114.5g of Silicone 1 was weighed into a 250ml polypropylene beaker, and then 45g of phthalocyanine green organic pigment (available under the name Heliogen® Green from Kremer Pigmente, Eichstetten, Germany) was added. The mixture was homogenized in a centrifugal mixer (Thinky) at a speed of 2000 rpm for a total of 5 minutes. Then, 0.6g of ethylenediamine was added to the mixture, and the mixture was homogenized in a centrifugal mixer at 2000 rpm for an additional 120 seconds. After an additional 20 minutes of isothermal reaction time without further stirring, the mixture was polymerized. The formed color masterbatch matrix was then removed from the PP beaker and cut into pieces less than 5mm.

[0097] [Example 3] 114.5g of silicone 1 was weighed into a 250ml polypropylene beaker, and then 90g of TiO2 (available under the name Kronos 2225 titanium dioxide from Kronos Titan GmbH, Leverkusen, Germany) was added as an inorganic pigment. The mixture was homogenized in a centrifugal mixer (Thinky) at a speed of 2000 rpm for a total of 5 minutes. Then, 0.6g of ethylenediamine was added to the mixture, and the mixture was homogenized in a centrifugal mixer at 2000 rpm for another 120 seconds. After an additional 20 minutes of isothermal reaction time without further stirring, the mixture was polymerized. The formed color masterbatch matrix was then removed from the PP beaker and cut into pieces less than 5mm.

[0098] [Example 4] 114.5 g of Silicone 1 was weighed into a 250 ml polypropylene beaker, and then 45 g of an organic yellow pigment (commercially available under the name Pigment Yellow 83 from Kremer Pigmente, Eichstetten, Germany) was added. The mixture was homogenized in a centrifugal mixer (Thinky) at a speed of 2000 rpm for a total of 5 minutes. Then, 0.6 g of ethylenediamine was added to the mixture, and the mixture was homogenized in a centrifugal mixer at 2000 rpm for an additional 120 seconds. After an additional 20 minutes of isothermal reaction time without further stirring, the mixture was polymerized. The formed color masterbatch matrix was then removed from the PP beaker and cut into pieces less than 5 mm.

[0099] [Example 5] 114.5g of Silicone 1 was weighed into a 250ml polypropylene beaker, and then 45g of pigment carbon black (available under the name Printex 60A from Orion, Frankfurt am Main, Germany) was added. The mixture was homogenized in a centrifugal mixer (ThinkY) at a speed of 2000 rpm for a total of 5 minutes. Then, 0.6g of ethylenediamine was added to the mixture, and the mixture was homogenized in a centrifugal mixer at 2000 rpm for another 120 seconds. After an additional 20 minutes of isothermal reaction time without further stirring, the mixture was polymerized. The formed black masterbatch matrix was then removed from the PP beaker and cut into pieces less than 5mm.

[0100] [Example 6] 114.5 g of Silicone 1 was weighed into a 250 ml polypropylene beaker, then 45.5 g of pigmented carbon black (commercially available under the name Printex 60A from Orion, Frankfurt am Main, Germany) was added. The mixture was homogenized in a centrifugal mixer (ThinkY) at a speed of 2000 rpm for a total of 5 minutes.

[0101] Subsequently, 114.5 g of Silicone 1 was weighed into a second 250 ml PP beaker, after which 45.5 g of TiO2 (commercially available under the name Kronos 2225 titanium dioxide from Kronos Titan GmbH, Leverkusen, Germany) was added. This mixture was likewise homogenized in a centrifugal mixer (Thinky) at a speed of 2000 rpm for a total of 5 minutes.

[0102] Subsequently, 80 g of each of these mixtures was placed in a third 250 ml polypropylene beaker, after which 0.6 g of ethylenediamine was added to the mixture, and the mixture was homogenized in a centrifugal mixer at 2000 rpm for an additional 120 seconds. After an additional 20 minutes of isothermal reaction time without further stirring, the mixture was polymerized. The formed gray masterbatch matrix was then removed from the PP beaker and cut into pieces less than 5 mm.

[0103] [Example 7] 114.5g of silicone 1 and 3g of diamine 2 were weighed into a 250ml polypropylene beaker, then 60g of blue pigment (available under the name Ultramarine Blue, Extra Dark from Kremer Pigmente, Eichstetten, Germany) was added. The mixture was homogenized in a centrifugal mixer (Thinky) at a speed of 2000 rpm for a total of 5 minutes. Then, 0.3g of ethylenediamine was added to the mixture, and the mixture was homogenized in a centrifugal mixer at 2000 rpm for an additional 120 seconds. After an additional 20 minutes of isothermal reaction time without further stirring, the mixture was polymerized. The formed blue masterbatch matrix was then removed from the PP beaker and cut into pieces less than 5mm.

[0104] [Example 8] 114.5 g of Silicone 1 was weighed into a 250 ml polypropylene beaker, then 45.5 g of an organic yellow pigment (commercially available from Kremer Pigmente, Eichstetten, Germany under the name Pigment Yellow 83) was added. The mixture was homogenized in a centrifugal mixer (Thinky) at a speed of 2000 rpm for a total of 5 minutes.

[0105] Subsequently, 114.5 g of Silicone 1 was weighed into a second 250 ml PP beaker, after which 45.5 g of blue pigment (commercially available under the name Ultramarine Blue, Extra Dark from Kremer Pigmente, Eichstetten, Germany) was added. This mixture was likewise homogenized in a centrifugal mixer (Thinky) at a speed of 2000 rpm for a total of 5 minutes.

[0106] The two base pastes prepared above were then placed in separate 250 ml polypropylene beakers in the ratios 120 g yellow paste:40 g blue paste, 80 g yellow paste:80 g blue paste, and 40 g yellow paste:120 g blue paste, after which 0.6 g ethylenediamine was added in each case to the mixture, which was continuously homogenized in a centrifugal mixer at 2000 rpm for another 120 seconds. After a further 20 minutes of isothermal reaction time without further stirring, the mixture was polymerized. The formed color masterbatch matrix had different green tones depending on the mixing ratio of the base pastes (yellow and blue), and was cut into small pieces less than 5 mm after being removed from the PP beaker.

[0107] Subsequent pelletization at 20° C. and 1013 hPa gave a free-flowing, non-tacky color masterbatch.

[0108] [Example 9] 2.5 kg of TPU1 (thermoplastic polyurethane available under the name Elastollan® SP 9264 from BASF SE, Ludwigshafen, Germany) were mixed with 0.05 kg of the color masterbatch of Example 3, in each case in the form of pellets, at room temperature and added by hopper to zone 1 of a ZK25 counter-rotating twin-screw extruder from Collin (Ebelsberg, Germany), where the temperature in the intake area (zone 1) was 100° C., increasing to 160° C. in zone 2 and 165° C. in zone 3. Zones 4 and 5 were at 170° C. and the die was heated at 165° C. The rotation speed of the screw was 60 revolutions per minute. The resulting homogeneous melt was continuously extruded through a die with a diameter of 4 mm in the form of an extrudate, which was cooled. This resulted in 2.5 kg of homogeneously colored white TPU extrudate with a thickness of 5 mm.

[0109] [Example 10] 3.5 kg of thermoplastic copolymer amide (copolymer of polyamide 12 and polytetramethylene glycol, with a Shore A hardness of 81, commercially available under the name PEBAX® 3533 from Arkema SA, Columbus, France) were mixed with 0.07 kg of the color masterbatch of Example 7, in each case in the form of pellets, and the mixture was added continuously by means of a hopper into zone 1 of a ZK25 counter-rotating twin-screw extruder from Collin (Ebelsberg, Germany), where the temperature in the intake area (zone 1) was 100° C., increasing to 180° C. in zone 2 and 195° C. in zone 3. Zones 4 and 5 were at 190° C., the die was heated at 190° C. The rotation speed of the screw was 60 revolutions per minute. The resulting homogeneous melt was continuously extruded in the form of extrudates through a die with a diameter of 4 mm and cooled to 30° C. in a water bath. This gave 3.5 kg of uniformly blue coloured thermoplastic polyamide extrudate having a thickness of 5 mm.

[0110] [Example 11] 3.5 kg of thermoplastic polyamide 6 (commercially available under the name Akulon K122 from DMS, Geleen, The Netherlands) were mixed with 0.1 kg of the color masterbatch of Example 5, in each case in the form of pellets, and the mixture was continuously added by means of a hopper into zone 1 of a ZK25 counter-rotating twin-screw extruder from Collin (Ebersberg, Germany) and compounded, where the temperature in the intake area (zone 1) was 140° C., increasing to 220° C. in zone 2 and 235° C. in zone 3. Zones 4 and 5 were at 230° C. and the die was heated at 220° C. The rotation speed of the screw was 60 revolutions per minute. The resulting homogeneous melt was continuously extruded in the form of extrudates through a die with a diameter of 4 mm and cooled to 30° C. in a water bath. This resulted in 3.5 kg of homogeneously black-colored thermoplastic polyamide extrudates having a thickness of 4.5 mm.

[0111] [Example 12] 3.5 kg of thermoplastic polyamide 6 (commercially available under the name Akulon K122 from DMS, Geleen, The Netherlands) were mixed with 0.1 kg of the color masterbatch of Example 5, in each case in the form of pellets, and the mixture was processed continuously through a hopper in an Engel ES600 / 125 injection molding machine manufactured by Engel (Schwerkberg, Austria), where the temperature in the intake area (zone 1) was 213°C, increasing to 220°C in zone 2 and 235°C in zone 3. The die temperature was 235°C, the gate and ejector were heated at 50°C. The internal mold pressure was 370 bar. With a cooling time of 35 seconds, test plates were molded cylically, all with a uniform black coloration and a modulus of elasticity of 2.3 GPa, comparable to the uncolored material.

Claims

1. A colorant-containing composition comprising: (D) at least one colorant; (E) at least one siloxane-polyoxamide copolymer containing units of general formula (IV) 【Chemistry 1】 [In the formula, R 1 are the same or different and are monovalent SiC-bonded optionally substituted hydrocarbon radicals, Y may be the same or different and represent a divalent optionally substituted hydrocarbon group having 1 to 40 carbon atoms; R 3 is a divalent optionally substituted hydrocarbon radical having 1 to 40 carbon atoms, each of which may be substituted with an oxygen atom; R 4 may be the same or different and are a hydrogen atom or a monovalent optionally substituted hydrocarbon group, n is 0 or a number from 1 to 1000; p is a number from 1 to 10; and optionally (F) additives; And, In a first step, at least one siloxane (A) of general formula (I), 【Chemistry 2】 [In the formula, R 1 are the same or different and are monovalent SiC-bonded optionally substituted hydrocarbon radicals, R 2 may be the same or different and are a hydrogen atom or a monovalent optionally substituted hydrocarbon group, Y may be the same or different and represent a divalent optionally substituted hydrocarbon group having 1 to 40 carbon atoms; n is 0 or a number from 1 to 1000; p is a number from 1 to 10. At least one compound (B) of the following general formula: R 4 NH-R 3 -NR 4 H (II) [In the formula, R 3 is a divalent optionally substituted hydrocarbon radical having 1 to 40 carbon atoms, each of which may be substituted with an oxygen atom; R 4 may be the same or different and are a hydrogen atom or a monovalent optionally substituted hydrocarbon group. (D) at least one colorant; Optionally, a compound of the general formula (C): ( 5 \Y 1 )) 6 2 ____) 6 2 ] m ____) 6 2  1 !R 5 (_=) [In the formula, R 6 are the same or different and are monovalent SiC-bonded optionally substituted hydrocarbon radicals, R 5 may be the same or different and are a hydrogen atom or a monovalent optionally substituted hydrocarbon group, Y 1 are the same or different and are divalent optionally substituted hydrocarbon radicals having 1 to 40 carbon atoms, each of which may be substituted by an oxygen atom or -NR"-; R″ is a hydrogen atom or a monovalent optionally substituted hydrocarbon group; m is 0 or a number from 1 to 1000. and Optional Additives (F) are mixed together and reacted, Optionally, in a second step, the composition obtained in the first step is melted and then pelletized, The colorant (D) is used in an amount of 2 to 400 parts by weight based on 100 parts by weight of component (A).

2. 2. The composition of claim 1, comprising: (E) a copolymer comprising units of formula (IV), (D) pigments, and also Optionally, (F) additives.

3. 3. The composition according to claim 1 or 2, characterized in that the copolymer (E) has a molecular weight (number average) of 20,000 g / mol to 1,000,000 g / mol, measured by size exclusion chromatography (SEC) in THF at 45° C.

4. 1. A method for producing a colorant-containing composition, comprising: In a first step, at least one siloxane (A) of general formula (I), 【Chemistry 3】 [In the formula, R 1 are the same or different and are monovalent SiC-bonded optionally substituted hydrocarbon radicals, R 2 may be the same or different and are a hydrogen atom or a monovalent optionally substituted hydrocarbon group, Y may be the same or different and represent a divalent optionally substituted hydrocarbon group having 1 to 40 carbon atoms; n is 0 or a number from 1 to 1000; p is a number from 1 to 10. At least one compound (B) of the following general formula: R 4 NH-R 3 -NR 4 H (II) [In the formula, R 3 is a divalent optionally substituted hydrocarbon radical having 1 to 40 carbon atoms, each of which may be substituted with an oxygen atom; R 4 may be the same or different and are a hydrogen atom or a monovalent optionally substituted hydrocarbon group. (D) at least one colorant; Optionally, a compound of the general formula (C): ( 5 \Y 1 )) 6 2 ____) 6 2 ] m ____) 6 2  1 !R 5 (_=) [In the formula, R 6 are the same or different and are monovalent SiC-bonded optionally substituted hydrocarbon radicals, R 5 may be the same or different and are a hydrogen atom or a monovalent optionally substituted hydrocarbon group, Y 1 are the same or different and are divalent optionally substituted hydrocarbon radicals having 1 to 40 carbon atoms, each of which may be substituted by an oxygen atom or -NR"-; R″ is a hydrogen atom or a monovalent optionally substituted hydrocarbon group; m is 0 or a number from 1 to 1000. and Optional Additives (F) are mixed together and reacted, Optionally, in a second step, the composition obtained in the first step is melted and then pelletized, The method wherein the colorant (D) is used in an amount of 2 to 400 parts by weight, based on 100 parts by weight of component (A).

5. The method of claim 4, wherein the colorant (D) comprises a pigment.

6. 6. The method according to claim 4 or 5, characterized in that in a first step said colorant (D) is mixed with one or more of components (A), (B) or (C).

7. 7. The method according to claim 4, wherein the melting in the second step is carried out at a temperature of from 50 to 250° C. under a pressure of from 100 to 30,000 hPa.

8. A method for producing a coloured moulded article by mixing a polymeric material with a colourant-containing composition according to any one of claims 1 to 3 or a colourant-containing composition produced as claimed in any one of claims 4 to 7, melting and homogenising the resulting mixture, and then moulding and cooling the mixture.

9. 9. The method according to claim 8, characterized in that the polymeric materials used are polyethylene, polypropylene, polyamide, polyethylene terephthalate, polybutylene terephthalate, thermoplastic elastomers based on crosslinked rubber, ethylene-vinyl acetate, polyhydroxybutyrate and / or their copolymers or mixtures thereof, as well as polystyrene, impact-modified polystyrene, styrene-acrylonitrile copolymers, acrylonitrile-butadiene-styrene copolymers, polyvinyl chloride, polyvinylidene fluoride, ethylene-tetrafluoroethylene (ETFE), polymethyl methacrylate, polycarbonate, polyaryletherketone, polyacrylonitrile, polyetherimide, polyethylene naphthalate, polyethersulfone, polyimide, polyketone, polyoxymethylene, polyphenylene sulfide, polyphenylene sulfone, polysulfone, styrene-butadiene rubber, acrylonitrile-butadiene rubber, natural rubber, and their copolymers or mixtures.

Citation Information

Patent Citations

  • Method for creating a colour master batch, colour master batch and polymer material coloured with same

    EP2113522A1

  • Composition formed into rigid shape and consisting essentially of silicone oil, especially for cosmetic use

    JP2002370919A

  • Films containing thermoplastic silicone block copolymers

    JP2009521346A

  • Polydiorganosiloxane polyoxamide copolymer

    JP2009521545A

  • adhesive composition

    JP2009521569A