Fiber-reinforced resin molding material, fiber-reinforced resin molded product, and method for manufacturing fiber-reinforced resin molded product

The fiber-reinforced resin molding material with amorphous thermoplastic resin, reinforcing fibers, and phosphorus flame retardant addresses the challenges of high mechanical properties and flame retardancy while maintaining product appearance, suitable for diverse applications.

JP7556291B2Active Publication Date: 2024-09-26TORAY INDUSTRIES INC
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
JP2020573374
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-12-20
Filing Date
2020-11-09
Publication Date
2024-09-26
Estimated Expiration
2040-11-09

AI Technical Summary

Technical Problem

Conventional fiber-reinforced resin molding materials face challenges in achieving high mechanical properties, flame retardancy, and maintaining product appearance due to the decomposition of low molecular weight flame retardants, which cause gas burns and defects in molded products.

Method used

A fiber-reinforced resin molding material comprising amorphous thermoplastic resin, reinforcing fibers, and a phosphorus flame retardant, with controlled thermal loss, is developed to suppress gas generation and oxidative decomposition during molding, ensuring excellent flame retardancy and mechanical properties.

Benefits of technology

The material produces molded products with improved flame retardancy, mechanical properties, and enhanced appearance by minimizing gas burns and oxidative decomposition, suitable for various applications including electrical and electronic equipment, automobile parts, and household appliances.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007556291000004
    Figure 0007556291000004
  • Figure 0007556291000006
    Figure 0007556291000006
  • Figure 0007556291000005
    Figure 0007556291000005
Patent Text Reader

Abstract

A fiber-reinforced resin molding material at least containing: 100 parts by mass of a component (A) which is an amorphous thermoplastic resin; 4-60 parts by mass of a component (B) which is a reinforced fiber; and 20-60 parts by mass of a component (C) which is a phosphorus-based flame retardant, wherein the thermal reduction of the molding material is 1.5% or less when being heated at 300°C for 10 minutes either in a nitrogen atmosphere or in an air atmosphere. A molded article using the molding material. A method for manufacturing a fiber-reinforced resin molded article. Use of the fiber-reinforced resin molding material according to the present invention can provide a molded article having excellent flame retardancy and mechanical properties while having good product appearance in which gas burning during molding is suppressed.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a fiber-reinforced resin molding material, a fiber-reinforced resin molded product, and a method for producing a fiber-reinforced resin molded product, and more specifically to a fiber-reinforced resin molding material that exhibits excellent flame retardancy and molded product appearance, a molded product using the molding material, and a method for producing the molded product. [Background technology]

[0002] Molded products made of reinforced fibers and thermoplastic resins are widely used in sporting goods, aerospace, and general industrial applications because they are lightweight and have excellent mechanical properties. The reinforced fibers used in these molded products are reinforced in various forms depending on the application. These reinforced fibers include metal fibers such as aluminum fibers and stainless steel fibers, organic fibers such as aramid fibers and PBO (polyphenylene benzoxazole) fibers, and inorganic fibers such as carbon fibers, glass fibers, and silicon carbide fibers.

[0003] Furthermore, a wide variety of molding materials (specifically, molding materials using continuous reinforcing fibers and a thermoplastic resin as a matrix) for obtaining such molded products are known, such as thermoplastic prepregs, yarns, and glass mats (GMTs). Such molding materials utilize the properties of thermoplastic resins to facilitate molding, do not require storage loads like thermosetting resins, and are characterized by the high toughness and excellent recyclability of the molded products obtained. In particular, molding materials processed into pellets can be applied to molding methods such as injection molding and stamping molding, which are economical and productive, and are useful as industrial materials.

[0004] In applications such as electronic device housings, there is a demand for even lighter and thinner materials, and molded articles made from these molding materials are required to have high mechanical properties, flame retardancy, and good appearance.

[0005] As for flame retardants, masterbatches using phosphazene flame retardants that do not contain halogen atoms have been proposed in consideration of environmental and safety aspects (see Patent Documents 1 and 2). In addition, a short fiber reinforced resin molding material that combines a phosphorus-based flame retardant that does not contain halogen atoms with reinforcing fibers to achieve both flame retardancy and mechanical properties has been described (see Patent Document 3). In addition, a fiber reinforced resin molding material that has excellent flame retardancy and mechanical properties has been proposed by coating a polycarbonate resin that contains a specific amount of flame retardant and / or liquid crystal resin on a resin-impregnated reinforcing fiber obtained by melt-impregnating a reinforcing fiber bundle with an epoxy resin (see Patent Document 4). [Prior art documents] [Patent documents]

[0006] [Patent Document 1] JP 2006-307178 A [Patent Document 2] JP 2008-101035 A [Patent Document 3] International Publication No. 2014 / 148641 [Patent Document 4] JP 2013-209629 A Summary of the Invention [Problem to be solved by the invention]

[0007] As described above, fiber-reinforced resin molding materials using flame retardants have been proposed in the past. However, as the required level of thinning of products increases, higher levels of mechanical properties and flame retardancy are required. In addition, problems that have not been a problem until now have become apparent. For example, in order to achieve a high level of flame retardancy, it is necessary to blend a large amount of flame retardant, but flame retardants, which are low molecular weight compounds, are more easily decomposed than thermoplastic resins, which are high molecular weight compounds, and cause poor appearance of molded products, such as gas burns at welds and molded product ends due to generated gas. For this reason, there was a problem that molded products using the conventional molding materials as described above could not be obtained that fully satisfied the flame retardancy, mechanical properties, and molded product appearance.

[0008] For example, in Patent Documents 1 and 2, the flame retardancy of the resin composition could not be effectively expressed because the polyester resin such as polyethylene terephthalate resin, polyester elastomer, and phenolic resin components contained in the flame retardant master batch reduce the flame retardancy. In addition, the techniques described in Patent Documents 1 to 3 could not effectively express the mechanical properties of the molded product because the reinforcing fibers in the resin molding material are short fibers with short fiber lengths. Patent Document 4 uses a resin composition containing a large amount of flame retardant, but there is no description of improving the appearance of the molded product.

[0009] Under these circumstances, there has been a demand for the development of a fiber-reinforced resin molding material which provides molded articles exhibiting excellent flame retardancy and mechanical properties and having good appearance, as well as molded articles made from the same.

[0010] In view of the problems of the prior art, the object of the present invention is to provide a fiber-reinforced resin molding material capable of producing a molded article having excellent flame retardancy and mechanical properties and excellent appearance, a molded article using the molding material, and a method for producing the molded article. [Means for solving the problem]

[0011] As a result of intensive research, the present inventors have come to invent the following fiber-reinforced resin molding material, a molded product using the molding material, and a method for producing the same, which are capable of solving the above-mentioned problems.

[0012] The fiber-reinforced resin molding material of the present invention is a molding material containing at least the following components (A) to (C), and is characterized in that the heat loss when heated at 300°C for 10 minutes under nitrogen and under air is 1.5% or less in both cases. (A) Amorphous thermoplastic resin: 100 parts by weight (B) Reinforcement fiber: 4 to 60 parts by weight (C) Phosphorus-based flame retardant: 20 to 60 parts by weight

[0013] The fiber-reinforced plastic molding of the present invention is a molding produced by using the fiber-reinforced plastic molding material described above.

[0014] Furthermore, the method for producing a fiber-reinforced resin molded product of the present invention is a method for producing a fiber-reinforced resin molded product using the above-mentioned fiber-reinforced resin molding material, and includes a step of drying the fiber-reinforced resin molding material at a temperature from the glass transition temperature of the fiber-reinforced resin molding material to the glass transition temperature + 20°C before molding. Effect of the Invention

[0015] By using the fiber-reinforced resin molding material of the present invention, it is possible to obtain molded products that have excellent product appearance with suppressed gas burning during molding, and that have excellent flame retardancy and mechanical properties. The molded products molded using the molding material of the present invention are extremely useful for various parts and members such as electric and electronic equipment, office automation equipment, home appliances, and automobile parts, internal members, and housings. [Brief description of the drawings]

[0016] [Figure 1] 1 is a schematic cross-sectional view of a fiber-reinforced resin molding material according to one embodiment of the present invention, taken in a direction perpendicular to a fiber axis or a pellet axis. [Diagram 2] FIG. 2 is a schematic cross-sectional view of a fiber-reinforced resin molding material according to another embodiment of the present invention, taken in a direction perpendicular to the fiber axis or pellet axis. [Diagram 3] 1 is a schematic cross-sectional view of a fiber-reinforced resin molding material according to one embodiment of the present invention, taken in a direction parallel to a fiber axis or a pellet axis. [Figure 4] FIG. 2 is a schematic cross-sectional view showing an example of the shape of a cross section perpendicular to the fiber axis of a composite fiber bundle made of (B) reinforcing fiber and (E) resin in the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0017] The present invention will be described in detail below with reference to the embodiments. The fiber-reinforced resin molding material of the present invention (hereinafter, sometimes simply referred to as "molding material") is a molding material that satisfies the following requirements. In the present invention, the molding material means a raw material used when molding a molded article by injection molding or the like.

[0018] The molding material of the present invention is a molding material containing at least the following components (A) to (C), and is characterized in that the heat loss when heated at 300°C for 10 minutes under nitrogen and under air is 1.5% or less. (A) Amorphous thermoplastic resin: 100 parts by weight (B) Reinforcement fiber: 4 to 60 parts by weight (C) Phosphorus-based flame retardant: 20 to 60 parts by weight

[0019] During molding, some of the heated molding material undergoes thermal decomposition and hydrolysis, generating decomposition gas. The generated decomposition gas is compressed when pressure is applied during molding, causing localized temperature increases at the edges of the molded product, welds, etc. At this time, the oxidative decomposition of the overheated molding material is accelerated, causing a defective appearance of the molded product accompanied by discoloration called gas burn.

[0020] The present inventors have found that by making the thermal loss of the molding material under nitrogen below a certain level, the amount of gas generated from the molten molding material during molding can be reduced. They also found that by making the thermal loss under air below a certain level, the oxidative decomposition of the components during molding and pressure application can be suppressed. They further found that by using a molding material that has a thermal loss under both nitrogen and air below a certain level, the effect of suppressing gas burning during molding can be dramatically improved, and thus the present invention was arrived at.

[0021] First, each of the above components will be described. <(A) Amorphous thermoplastic resin> The molding material in the present invention includes (A) an amorphous thermoplastic resin. An amorphous thermoplastic resin is a thermoplastic resin that does not actively form a crystalline state among thermoplastic resins. More specifically, a thermoplastic resin that has good molecular stereoregularity, small side chains, no branching, and high intermolecular cohesive force is a crystalline resin, but an amorphous thermoplastic resin is a resin that does not have some or all of the above. In general, an amorphous thermoplastic resin has good compatibility with a flame retardant compared to a crystalline thermoplastic resin, and therefore has improved flame retardancy and flowability.

[0022] The glass transition temperature of the (A) amorphous thermoplastic resin itself is preferably 100°C or higher and 250°C or lower. A glass transition temperature of 100°C or higher is preferable because it provides excellent heat resistance and suppresses gas generation due to resin decomposition. 120°C or higher is more preferable. A glass transition temperature of 250°C or lower is preferable because it provides excellent fluidity during molding. 200°C or lower is more preferable, and 150°C or lower is even more preferable. Here, the glass transition temperature refers to a value measured by DSC at a heating rate of 20°C / min according to JIS K7121.

[0023] The (A) amorphous thermoplastic resin is not particularly limited, but is preferably at least one resin selected from the group consisting of polyarylate resins, polysulfone resins, polyethersulfone resins, polyimide resins, polyetherimide resins, acrylic resins, methacrylic resins, styrene resins, vinyl resins, polyphenylene ether resins, and polycarbonate resins. These amorphous thermoplastic resins have the advantage of being highly flexible and having good compatibility with flame retardants. It is particularly preferable to include a polycarbonate resin from the viewpoint of compatibility with flame retardants.

[0024] Polycarbonate resins are resins with a good balance of mechanical properties, thermal stability, and flame retardancy, and are preferably used because the reinforcing effect of reinforcing fibers and the flame retardancy improvement effect of flame retardants and / or liquid crystal resins work more effectively. In the present invention, the polycarbonate resin is a polymer having a carbonate ester structure in the main chain, and examples of such polymers include aliphatic polycarbonates, aliphatic-aromatic polycarbonates, and aromatic polycarbonates. These may be used alone or in combination of two or more. From the viewpoint of excellent impact resistance, aromatic polycarbonates having a carbonate ester structure of 4,4'-dihydroxydiphenyl-2,2-propane (bisphenol A) are particularly preferably used.

[0025] The viscosity average molecular weight (Mv) of the polycarbonate resin is preferably 10,000 to 50,000, more preferably 15,000 to 40,000, and even more preferably 18,000 to 35,000. A viscosity average molecular weight (Mv) of 10,000 or more is preferable because it provides better mechanical properties such as impact resistance. A viscosity average molecular weight (Mv) of 50,000 or less is preferable because it provides better flowability during molding and high moldability.

[0026] Here, the viscosity average molecular weight (Mv) can be determined by the following method. First, a solution in which 0.7 g of polycarbonate resin is dissolved in 100 ml of methylene chloride at 20° C. is subjected to the specific viscosity (η SP ) is measured at 20°C using an Ostwald viscometer. Specific viscosity (η SP )=(t-t0) / t0 [t0 is the number of seconds that methylene chloride falls, and t is the number of seconds that the sample solution falls]

[0027] Next, the specific viscosity (η SP ) the viscosity average molecular weight Mv can be calculated from the following formula: η SP / c=[η]+0.45×[η] 2 c (where [η] is the intrinsic viscosity) [η]=1.23×10-4 Mv 0.83 c=0.7

[0028] The method for obtaining the polycarbonate resin is not particularly limited, and a known manufacturing method can be used, for example, the phosgene method, the ester exchange method, the solid-phase polymerization method, etc. In addition, commercially available products such as "Iupilon" and "Novarex" (product names) manufactured by Mitsubishi Engineering Plastics Corporation, "Panlite" (product name) manufactured by Teijin Chemical Co., Ltd., and "Toughlon" (product name) manufactured by Idemitsu Petrochemical Co., Ltd. can also be obtained and used.

[0029] <(B) Reinforced fiber> The (B) reinforcing fiber in the present invention can improve the mechanical properties by the fiber reinforcing effect on the (A) amorphous thermoplastic resin. Furthermore, when the reinforcing fiber has inherent properties such as electrical conductivity and thermal conductivity, it can also impart these properties that cannot be achieved by the (A) amorphous thermoplastic resin alone. From this viewpoint, among the reinforcing fibers, PAN (polyacrylonitrile), pitch, rayon, and other carbon fibers are preferred from the viewpoint of further improving the mechanical properties and reducing the weight of the molded product, and PAN-based carbon fibers are even more preferred from the viewpoint of the balance between the strength and elastic modulus of the obtained molded product. In addition, glass fibers are also preferably used for the purpose of balancing the flame retardancy and the mechanical properties.

[0030] The content of the (B) reinforcing fiber in the molding material of the present invention is 4 to 60 parts by weight (4 parts by weight or more and 60 parts by weight or less) relative to 100 parts by weight of the (A) amorphous thermoplastic resin. If the content of the reinforcing fiber is less than 4 parts by weight, the mechanical properties such as bending strength of the molded product are difficult to exhibit. In addition, the amount of gas generated increases, so the probability of gas burning increases. The content of the reinforcing fiber is more preferably 10 parts by weight or more, and even more preferably 20 parts by weight or more. On the other hand, if the content of the reinforcing fiber exceeds 60 parts by weight, the fluidity and flame retardancy of the molding material may decrease during molding processing. The content of the reinforcing fiber is preferably 30 parts by weight or less.

[0031] Furthermore, when carbon fibers are used as reinforcing fibers, the surface oxygen concentration ratio [O / C], which is the ratio of the number of oxygen (O) and carbon (C) atoms on the fiber surface measured by X-ray photoelectron spectroscopy, is preferably 0.05 to 0.5, more preferably 0.08 to 0.4, and even more preferably 0.15 to 0.3. By having a surface oxygen concentration ratio of 0.05 or more, the amount of functional groups on the carbon fiber surface can be secured, and stronger adhesion with the thermoplastic resin can be obtained. In addition, there is no particular limit to the upper limit of the surface oxygen concentration ratio, but in terms of the balance between the handleability and productivity of the carbon fiber, it can be exemplified to generally be 0.5 or less.

[0032] The surface oxygen concentration ratio of carbon fibers is determined by X-ray photoelectron spectroscopy according to the following procedure. First, a carbon fiber bundle from which sizing agents and other substances adhering to the carbon fiber surface have been removed with a solvent is cut into 20 mm pieces and spread out on a copper sample support. Then, A1Kα1 and 2 are used as X-ray sources, and the sample chamber is heated to 1×10 -8 Torr. The kinetic energy (KE) of the main C1s peak is set to 1202 eV as a correction value for the peak due to charging during measurement. The C1s peak area is determined by drawing a straight baseline in the range of 1191 to 1205 eV as the KE. The O1s peak area is determined by drawing a straight baseline in the range of 947 to 959 eV as the KE.

[0033] Here, the surface oxygen concentration ratio is calculated as an atomic ratio from the ratio of the O1s peak area to the C1s peak area using a sensitivity correction value specific to the device. When using an ES-200 model manufactured by Kokusai Electric Co., Ltd. as the X-ray photoelectron spectroscopy device, the sensitivity correction value is set to 1.74.

[0034] The means for controlling the surface oxygen concentration ratio [O / C] to 0.05 to 0.5 is not particularly limited, but may be, for example, electrolytic oxidation treatment, chemical oxidation treatment, or gas phase oxidation treatment, with electrolytic oxidation treatment being preferred.

[0035] The average fiber diameter of the carbon fibers is not particularly limited, but from the viewpoint of the mechanical properties and surface appearance of the resulting molded article, it is preferably within the range of 1 to 20 μm, and more preferably within the range of 3 to 15 μm.

[0036] In addition, it is preferable that the (B) reinforcing fiber is provided with a sizing agent, since this improves the bundling property, bending resistance, and abrasion resistance, and suppresses the occurrence of fluff and thread breakage in the advanced processing step. Furthermore, the sizing agent is preferable because it interacts with the functional groups on the carbon fiber surface and can improve the adhesiveness and mechanical properties of the composite.

[0037] The amount of the sizing agent applied is not particularly limited, but is preferably 0.1 to 3 parts by weight or less, more preferably 0.2 to 1.2 parts by weight or less, and even more preferably 0.5 to 1 part by weight or less, relative to 100 parts by weight of the carbon fibers. When the amount is 0.1 part by weight or more, the adhesion is improved and the mechanical properties of the molded product are improved. When the amount is 3 parts by weight or less, the dispersibility of the carbon fibers in the molded product is improved. Furthermore, this is preferable because it suppresses the deterioration of the physical properties of the matrix resin.

[0038] Examples of sizing agents include epoxy resins, polyethylene glycol, polyurethane, polyester, emulsifiers, surfactants, etc. These may be applied alone or in combination of two or more.

[0039] As a sizing agent component, an epoxy resin is preferred from the viewpoint of adhesiveness. When an epoxy resin is present between the reinforcing fiber and the matrix resin, it makes the fiber flexible and difficult to peel off, which is preferable because it makes it easier to improve the strength of the molded product.

[0040] Examples of epoxy resins include bisphenol A type epoxy resins, bisphenol F type epoxy resins, aliphatic epoxy resins, and phenol novolac type epoxy resins. Among them, aliphatic epoxy resins are preferred as epoxy resins because they are more likely to exhibit adhesion to matrix resins. Normally, when an epoxy resin has many epoxy groups, the crosslink density after the crosslinking reaction increases, so it tends to have a structure with low toughness. Even if it is present between the carbon fiber and the matrix resin, it is brittle and easily peels off, and the strength of the molded product may not be expressed. On the other hand, aliphatic epoxy resins have a flexible skeleton, so they tend to have a structure with high toughness even if the crosslink density is high, and they are soft at the interface and difficult to peel off, so they are preferred because they can easily improve the strength of the molded product.

[0041] Aliphatic epoxy resins are epoxy resins that do not contain aromatic rings in the molecule. Aromatic rings are cyclic chemical skeletons that have electronic conjugation and exhibit aromaticity.

[0042] Specific examples of aliphatic epoxy resins include, for example, diglycidyl ether compounds such as ethylene glycol diglycidyl ether, polyethylene glycol diglycidyl ethers, propylene glycol diglycidyl ether, polypropylene glycol diglycidyl ethers, 1,4-butanediol diglycidyl ether, neopentyl glycol diglycidyl ether, polytetramethylene glycol diglycidyl ether, polyalkylene glycol diglycidyl ethers, etc. Also, examples of polyglycidyl ether compounds such as glycerol polyglycidyl ether, diglycerol polyglycidyl ether, polyglycerol polyglycidyl ethers, sorbitol polyglycidyl ethers, arabitol polyglycidyl ethers, trimethylolpropane polyglycidyl ethers, trimethylolpropane glycidyl ethers, pentaerythritol polyglycidyl ethers, and polyglycidyl ethers of aliphatic polyhydric alcohols.

[0043] Among aliphatic epoxy resins, it is preferable to use a polyfunctional aliphatic epoxy resin having three or more functional groups, and more preferably to use an aliphatic polyglycidyl ether compound having three or more highly reactive glycidyl groups. Among these, glycerol polyglycidyl ether, diglycerol polyglycidyl ether, polyethylene glycol glycidyl ethers, and polypropylene glycol glycidyl ethers are more preferable. Aliphatic polyglycidyl ether compounds are preferable because they have a good balance of flexibility, crosslinking density, and compatibility with the matrix resin, and effectively improve the mechanical properties of the molded product.

[0044] The means for applying the sizing agent is not particularly limited, but may be, for example, a method of immersing the fiber in the sizing liquid via a roller, a method of contacting the fiber with a roller on which the sizing liquid is applied, or a method of spraying the fiber with the sizing liquid in a mist form. Either a batch method or a continuous method may be used, but a continuous method is preferred because it has good productivity and small variation. In this case, it is preferable to control the concentration of the sizing liquid, temperature, thread tension, etc. so that the amount of the effective component of the sizing agent attached to the carbon fiber is uniformly attached within an appropriate range. It is more preferable to vibrate the reinforcing fiber with ultrasonic waves when applying the sizing agent.

[0045] Examples of the solvent used for the sizing agent include water, methanol, ethanol, dimethylformamide, dimerylacetamide, acetone, etc., but water is preferred from the viewpoint of easy handling and disaster prevention. Therefore, when a compound that is insoluble or poorly soluble in water is used as a sizing agent, it is better to add an emulsifier and a surfactant and disperse it in water. Specifically, the emulsifier and surfactant can be an anionic emulsifier such as styrene-maleic anhydride copolymer, olefin-maleic anhydride copolymer, formalin condensate of naphthalene sulfonate, polyacrylic acid sodium, etc., a cationic emulsifier such as polyethyleneimine, polyvinylimidazoline, etc., a nonionic emulsifier such as nonylphenol ethylene oxide adduct, polyvinyl alcohol, polyoxyethylene ether ester copolymer, sorbitan ester ethyl oxide adduct, etc., but a nonionic emulsifier with small interactions is preferred because it is less likely to inhibit the adhesive effect of the multifunctional compound.

[0046] <(C) Phosphorus-based flame retardants> The molding material of the present invention contains a phosphorus-based flame retardant, which has high compatibility with thermoplastic resins, and the mixture exhibits excellent flame retardancy and flowability.

[0047] In addition, it is preferable that the phosphorus-based flame retardant is compatible with the amorphous thermoplastic resin (A). The higher the compatibility, the higher the flame retardancy, which is preferable. The compatibility can be confirmed by the change in the glass transition temperature of the amorphous thermoplastic resin (A). The glass transition temperature of the mixture can be measured at a heating rate of 20°C / min using a differential scanning calorimeter (DSC) in accordance with JIS K7121.

[0048] The content of the phosphorus-based flame retardant (C) in the molding material of the present invention is 20 to 60 parts by weight (20 parts by weight or more and 60 parts by weight or less) relative to 100 parts by weight of the amorphous thermoplastic resin (A). If the content of the phosphorus-based flame retardant is less than 20 parts by weight, the flame retardancy and fluidity of the molded article will decrease. The content of the phosphorus-based flame retardant is more preferably 40 parts by weight or more. On the other hand, if the content of the phosphorus-based flame retardant exceeds 60 parts by weight, the mechanical properties of the molded article will decrease. The content of the phosphorus-based flame retardant is preferably 50 parts by weight or less.

[0049] The phosphorus-based flame retardant used in the present invention preferably has a heat loss of 5% or less when heated at 300° C. for 10 minutes under nitrogen. When the heat loss is 5% or less, the amount of gas generated during melting of the resin during molding is reduced, which is preferable because gas burning can be suppressed.

[0050] The phosphorus-based flame retardant (C) used in the present invention is not particularly limited, and any known flame retardant can be used, such as a phosphorus compound-based flame retardant or a red phosphorus-based flame retardant.

[0051] Representative examples of phosphorus compound-based flame retardants include phosphate ester compounds such as triphenyl phosphate, tricresyl phosphate, trimethyl phosphate, triethyl phosphate, cresyl diphenyl phosphate, xylenyl diphenyl phosphate, 2-ethylhexyl diphenyl phosphate, and other aromatic phosphate esters, halogen-containing phosphate ester compounds such as trisdichloropropyl phosphate, trischloroethyl phosphate, and trischloropropyl phosphate, as well as condensed phosphate ester compounds, polyphosphates, red phosphorus compounds, etc. These may be used alone or in combination of two or more.

[0052] Phosphorus compound flame retardants and red phosphorus compounds accelerate dehydration and carbonization, forming dense char on the surface of molded products, blocking heat and oxygen and preventing the spread of flames. In addition, they exert flame retardancy by stabilizing active H and OH radicals in the combustion field through their radical trapping effect against the radical chain reaction in thermal decomposition.

[0053] In the present invention, among the various flame retardants described above, from the viewpoints of the expression of flame retardancy, the presence or absence of concerns about the generation of toxic gases, the increase in specific gravity due to the addition of the flame retardant, and compatibility with the (A) amorphous thermoplastic resin, it is preferable to use a phosphorus compound-based flame retardant, and it is particularly preferable to use a condensed phosphate ester compound.

[0054] The phosphorus content of the phosphorus-based flame retardant is preferably 5 to 50%. The phosphorus content is the weight of phosphorus in the weight of the phosphorus-based flame retardant, and if it is 5% or more, dense char is easily formed and flame retardancy is improved. It is preferably 7% or more, and more preferably 9% or more. If the phosphorus content is 50% or less, compatibility with the (A) amorphous thermoplastic resin is improved, and thus flame retardancy is high, which is preferable.

[0055] In the present invention, the phosphorus-based flame retardant (C) may be contained in any of the raw materials used during molding as a molding material. In the present invention, preferred examples of the phosphorus-based flame retardant contained in any of the raw materials include, for example, a resin composition obtained by melt-kneading an amorphous thermoplastic resin and a phosphorus-based flame retardant, which may be contained in the resin coating the reinforcing fiber, or may be impregnated in the reinforcing fiber bundle in advance in the process of obtaining the reinforcing fiber. In addition, a molding material mixture obtained by dry-blending a reinforcing fiber coated with a thermoplastic resin and a resin composition obtained by melt-kneading a thermoplastic resin and a phosphorus-based flame retardant is also preferred because the amount of the reinforcing fiber and the flame retardant contained in the molded product before molding can be easily adjusted. Here, the dry blend in the present invention is different from melt-kneading, and refers to stirring and mixing two types of materials at a temperature at which the resin component does not melt, to make them substantially uniform, and is preferably used when a pellet-shaped material is used mainly during injection molding or extrusion molding.

[0056] <(D) Antioxidants> The molding material of the present invention preferably contains an antioxidant (D). As the antioxidant, it is preferable to use an antioxidant such as a hindered phenol type, a hydroquinone type, a phosphorus type, a phosphite type, an amine type, a sulfur type, or a substituted product thereof.

[0057] Specific examples of the phosphorus-based and phosphite-based antioxidants include tetrakis(2,4-di-t-butylphenyl)-4,4'-biphenylene phosphonite, bis(2,6-di-t-butyl-4-methylphenyl)pentaerythritol diphosphite, 2,2-methylenebis(4,6-di-t-butylphenyl)octyl phosphite, triphenyl phosphite, tris(2,4-di-t-butylphenyl)phosphite, diphenyl isodecyl phosphite, phenyl diisodecyl phosphite, 4,4-butylidene-bis(3-methyl-6-t-butylphenyl-di-tridecyl)phosphite, cyclic ne Examples of such phosphite include neopentanetetraylbis(octadecylphosphite), cyclic neopentanetetraylbis(2,6-di-t-butyl-4-methylphenyl)phosphite, tris(nonyl phenyl)phosphite, diisodecylpentaerythritol diphosphite, 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide, 10-(3,5-di-t-butyl-4-hydroxybenzyl)-9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide, 10-decyloxy-9,10-dihydro-9-oxa-10-phosphaphenanthrene, and mixtures thereof.

[0058] Examples of the hindered phenol-based antioxidants include triethylene glycol-bis[3-(3-t-butyl-5-methyl-4-hydroxyphenyl)propionate, 4,4'-butylidenebis(3-methyl-6-t-butylphenol), 1,6-hexanediol-bis[3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate, 2,4-bis-(n-octylthio)-6-(4-hydroxy-3,5-di-t-butylanilino)-1,3,5-triazine, pentaerythrityl-tetrakis[3-(3,5-di-t-butyl 2,2-thio-diethylenebis[3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate], octadecyl-3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate, 2,2-thiobis(4-methyl-6-t-butylphenol), N,N'-hexamethylenebis(3,5-di-t-butyl-4-hydroxy-hydrocinnamamide), 3,5-di-t-butyl-4-hydroxy-benzylphosphonate-diethyl ester, 1,3,5-trimethyl-2, 4,6-Tris(3,5-di-t-butyl-4-hydroxybenzyl)benzene, bis(3,5-di-t-butyl-4-hydroxybenzylsulfonate calcium ethyl, tris-(3,5-di-t-butyl-4-hydroxybenzyl)isocyanurate, 2,6-di-t-butyl-p-cresol, butylated hydroxyanisole, 2,6-di-t-butyl-4-ethylphenol, stearyl-β-(3,5-di-t-butyl-4-hydroxyphenyl)propionate, 2,2'-methylenebis-(4-methyl-6-t-butylphenol), 2 ,2'-methylene-bis-(4-ethyl-6-t-butylphenol), 4,4'-thiobis-(3-methyl-6-t-butylphenol), octylated diphenylamine, 2,4-bis[(octylthio)methyl]-o-cresol, isooctyl-3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate, 4,4'-butylidenebis(3-methyl-6-t-butylphenol, 3,9-bis[1,1-dimethyl-2-[β-(3-t-butyl-4-hydroxy-5-methylphenyl)propionyloxy]ethyl]2,4,8,10-Tetraoxaspiro[5,5]undecane, benzenepropanoic acid, 3-(1,1-dimethylethyl)-4-hydroxy-5-methyl-2,4,8,10-tetraoxaspiro[5.5]undecane-3,9-diylbis(2,2-dimethyl-2,1-ethanediyl)ester, 1,1,3-tris(2-methyl-4-hydroxy-5-t-butylphenyl)butane, 1,3,5-trimethyl-2,4,6-tris(3,5-di-t-butyl-4-hydroxybenzyl)benzene, bis[3,3'-bis-(4'-hydr Examples of the tertiary ester include 1,3,5-tris(3',5'-di-t-butyl-4'-hydroxybenzyl)-sec-triazine-2,4,6-(1H,3H,5H)trione, d-α-tocopherol, 3,9-bis(2-(3-(3-tertiary butyl-4-hydroxy-5-methylphenyl)propionyloxy)-1,1-dimethylethyl)-2,4,8,10-tetraoxaspiro[5.5]undecane, and mixtures thereof.

[0059] Examples of the amine-based antioxidant include dimethyl succinate-1-(2-hydroxyethyl)-4-hydroxy-2,2,6,6-tetramethylpiperidine polycondensate, poly[{6-(1,1,3,3-tetramethylbutyl)amino-1,3,5-triazine-2,4-diyl}{(2,2,6,6-tetramethyl-4-piperidyl)imino}hexamethylene{(2,2,6,6-tetramethyl-4-piperidyl)imino}], 2-(3,5-di-t-butyl-4-hydroxybenzyl)-2-n-butylmalonate bis(1,2,2,6,6-pentamethyl-4-piperidyl), tetrakis(2,2,6,6-tetramethyl-4-piperidyl), bis(1,2,3,4-butanetetracarboxylate), bis-2,2,6,6-tetramethyl-4-piperidyl-sebacate, bis(1,2,2,6,6-pentamethyl-4-piperidyl)sebacate, methyl(1,2,2,6,6-pentamethyl-4-piperidyl)sebacate, 1-[2-[3-(3.5-di-t-butyl-4-hydroxyphenyl)propionyloxy]ethyl]-4-[3-(3,5-t-butyl-hydroxyphenyl)propionyloxy]2,2,6,6-tetramethylpiperidine, 4-benzoyloxy-2,2,6,6-tetramethylpiperidine, and the like, or a mixture thereof, can be exemplified.

[0060] Examples of sulfur-based antioxidants include 4,4'-thiobis(6-t-butyl-3-methylphenol), dialkyl (C12-18) 3,3'-thiodipropionate, pentaerythrityl tetrakis(3-laurylthiopropionate), and mixtures thereof.

[0061] Among the various antioxidants mentioned above, from the viewpoint of inhibiting decomposition, sulfur-based antioxidants, hindered phenol-based antioxidants, or mixtures thereof are preferably used.

[0062] The content of the antioxidant is preferably 1.0% by weight or more relative to the total amount of the molding material (100% by weight). When the antioxidant is contained in an amount of 1.0% by weight or more, decomposition of the components of the molding material during molding and heating is suppressed, and gas burning is less likely to occur. The upper limit of the antioxidant content is preferably 2.0% by weight or less. When the antioxidant content is 2.0% by weight or less, gas burning due to the decomposition of the antioxidant itself is suppressed, and the appearance of the molded product is improved.

[0063] Next, the molding material of the present invention will be described. The molding material of the present invention has a heat loss of 1.5% or less when heated at 300°C for 10 minutes under nitrogen and air. If the heat loss under nitrogen exceeds 1.5%, the amount of gas generated during resin melting during molding increases, so that the temperature rise due to gas compression becomes significant during pressurization during molding, and poor appearance due to gas burning is likely to occur. It is more preferable that the heat loss is 1.3% or less, and even more preferable that the heat loss is 1.1% or less. Furthermore, if the heat loss under air exceeds 1.5%, oxidative decomposition is likely to occur at the ends and welds that are locally heated due to gas compression during pressurization in the molding process, so that poor appearance due to gas burning is likely to occur. It is more preferable that the heat loss is 1.3% or less, and even more preferable that the heat loss is 1.1% or less. Furthermore, the small heat loss under both nitrogen and air can synergistically suppress gas burning.

[0064] In the present invention, the "thermal weight loss" refers to the weight loss rate of the molding material after heating under the above heating conditions, with the weight of the molding material being 100%, and can be calculated by the following formula. (Heat loss) [Weight%] = {(Weight before heating - Weight after heating) / Weight before heating} x 100

[0065] In addition, the molding material of the present invention preferably has a moisture content of 0.02% or less. When the resin is melted during molding, thermal decomposition and hydrolysis of the molding material components are likely to occur, and if the moisture content is 0.02% or less, hydrolysis of the flame retardant in particular is suppressed, and poor appearance due to gas burns is suppressed, which is preferable. This moisture content is more preferably 0.01% or less. The moisture content contained in the molding material can be controlled by drying at high temperatures. The drying temperature is preferably from the glass transition temperature of the molding material to the glass transition temperature + 20°C. The drying time is preferably 4 hours or more. The moisture content of the molding material can be measured using the Karl Fischer method.

[0066] The molding material of the present invention preferably has a glass transition temperature of 100° C. or less. A glass transition temperature of 100° C. or less is preferable because the fluidity at the molding temperature is improved. A glass transition temperature of 90° C. or less is more preferable, and a glass transition temperature of 80° C. or less is even more preferable. The glass transition temperature can be measured by using a differential scanning calorimeter (DSC) at a heating rate of 20° C. / min according to JIS K7121.

[0067] In the molding material of the present invention, it is preferable that the reinforcing fibers (particularly the reinforcing fiber bundles) are impregnated with the (E) resin. Here, "the reinforcing fibers are impregnated with the resin" particularly refers to a state in which the (B) reinforcing fiber bundles are impregnated with the (E) resin.

[0068] The (E) resin has a melt viscosity lower than that of the (A) amorphous thermoplastic resin. The (E) resin forms an impregnated reinforcing fiber bundle together with the (B) reinforcing fiber, and serves as a so-called impregnation aid and dispersion aid, helping the (A) amorphous thermoplastic resin to impregnate the (B) reinforcing fiber during molding and also helping the (B) reinforcing fiber to disperse in the (A) amorphous thermoplastic resin.

[0069] The melt viscosity of the (E) resin at 200°C is preferably 0.01 to 10 Pa·s. If the melt viscosity at 200°C is 0.01 Pa·s or more, the fracture originating from the (E) resin can be further suppressed, and the impact strength of the molded product can be further improved. The melt viscosity is more preferably 0.05 Pa·s or more, and even more preferably 0.1 Pa·s or more. On the other hand, if the melt viscosity at 200°C is 10 Pa·s or less, the (E) resin can be easily impregnated into the (B) reinforcing fibers. Therefore, when the molding material is molded, the dispersibility of the (B) reinforcing fibers can be further improved. The melt viscosity is more preferably 5 Pa·s or less, and even more preferably 2 Pa·s or less. Here, the melt viscosity of the (E) resin at 200°C can be measured by a viscoelasticity measuring instrument at 0.5 Hz using a 40 mm parallel plate.

[0070] The (E) resin is preferably one having a high affinity with the (A) amorphous thermoplastic resin. By selecting an (E) resin having a high affinity with the (A) amorphous thermoplastic resin, the (E) resin is efficiently compatible with the (A) amorphous thermoplastic resin during the production of the molding material and during molding, and therefore the dispersibility of the (B) reinforcing fibers can be further improved.

[0071] The resin (E) is appropriately selected depending on the combination with the amorphous thermoplastic resin (A) which is the matrix resin. For example, a terpene resin is preferably used when the molding temperature is in the range of 150 to 270°C, and an epoxy resin is preferably used when the molding temperature is in the range of 270 to 320°C.

[0072] (E) resin preferably has a carboxyl group, a hydroxyl group, or an epoxy group. These functional groups interact with the sizing agent on the surface of the reinforcing fiber and with the (A) amorphous thermoplastic resin, improving adhesion and improving the mechanical properties of the molded product. To improve adhesion, a highly reactive epoxy resin is preferred.

[0073] In addition, the (E) resin preferably has a heat loss of 5% by weight or less at the molding temperature measured under the condition of a temperature rise of 20°C / min (in air). If the heat loss is 5% by weight or less, the generation of decomposition gas during molding can be suppressed, and gas burning can be suppressed. More preferably, it is 3% by weight or less.

[0074] The term "heat loss" used herein refers to the weight loss rate of the (E) resin after heating under the above heating conditions, with the weight of the (E) resin before heating being taken as 100%, and can be calculated by the following formula. (Heating loss) [weight%] = {(weight before heating - weight after heating) / weight before heating} x 100

[0075] In addition, the molding material of the present invention preferably has a structure in which the impregnated reinforcing fiber (resin-impregnated reinforcing fiber) is coated with (A) amorphous thermoplastic resin. The term "coated structure" refers to a structure in which (A) amorphous thermoplastic resin is disposed on the surface of the resin-impregnated reinforcing fiber and is bonded to (E) resin.

[0076] 1 and 2 are schematic diagrams showing examples of cross-sectional forms of the molding material of the present invention in the axial direction (for example, the direction perpendicular to the pellet axis). In the present invention, the axial direction means a cross section on a plane perpendicular to the axial direction. As shown in FIG. 1, a core-sheath structure in which a composite fiber bundle (1) having (B) reinforcing fiber and (E) resin is used as a core structure and is surrounded by (A) amorphous thermoplastic resin (2) is preferably arranged. In addition, a plurality of composite fiber bundles (1) as shown in FIG. 2 can be arranged so as to be covered by (A) amorphous thermoplastic resin (2), and in this case, the number of composite fiber bundles (1) is preferably about 2 to 6.

[0077] Fig. 3 is a schematic diagram showing an example of a preferred cross-sectional form of the molding material of the present invention in a direction parallel to the axis (for example, a direction parallel to the pellet axis). As shown in Fig. 3, the molding material of the present invention is preferably such that the (B) reinforcing fibers are arranged almost parallel to the axial direction of the molding material, and the length of the (B) reinforcing fibers is substantially the same as the length of the molding material.

[0078] Here, "arranged almost parallel" refers to a state in which the axis of the long axis of the (B) reinforcing fiber and the axis of the long axis of the molding material are oriented in the same direction, and the angular deviation between the axes is preferably 20° or less, more preferably 10° or less, and even more preferably 5° or less. In addition, "substantially the same length" means that, for example, in a pellet-shaped molding material, the (B) reinforcing fiber is not cut in the middle of the inside of the pellet, and the (B) reinforcing fiber significantly shorter than the entire length of the pellet is not substantially included. In particular, although the amount of the (B) reinforcing fiber shorter than the entire length of the pellet is not specified, when the content of the (B) reinforcing fiber of a length of 50% or less of the entire length of the pellet is 30 parts by weight or less, it is evaluated that the (B) reinforcing fiber significantly shorter than the entire length of the pellet is not substantially included. Furthermore, the content of the (B) reinforcing fiber of a length of 50% or less of the entire length of the pellet is preferably 20 parts by weight or less. The entire length of the pellet is the length in the reinforcing fiber orientation direction in the pellet. (B) Since the reinforcing fibers have the same length as the molding material, the length of the reinforcing fibers in the molded product can be increased, resulting in excellent mechanical properties.

[0079] In addition, the boundary between the reinforcing fiber bundles and the (A) amorphous thermoplastic resin may be bonded, and the (A) amorphous thermoplastic resin may partially penetrate into a part of the composite near the boundary, and may be in a state where it is compatible with the (E) resin constituting the composite, or in a state where it is impregnated into the reinforcing fibers.

[0080] The molding material of the present invention is kneaded by, for example, injection molding to become a final molded product. From the viewpoint of the handling of the molding material, it is preferable that the reinforcing fiber bundle and the (A) amorphous thermoplastic resin remain bonded and do not separate until molding is performed, and maintain the shape as described above. Otherwise, the reinforcing fiber bundle and the (A) amorphous thermoplastic resin are completely different in shape (size, aspect ratio), specific gravity, and weight, so that they may be classified during transportation and handling of the material until molding, and during material transfer in the molding process, and the mechanical properties of the molded product may vary when molded, or the fluidity of the molding material during molding may decrease, causing mold clogging, or blocking during the molding process.

[0081] From this viewpoint, it is preferable to use a configuration in which the reinforcing fibers are arranged in a core-sheath structure as exemplified in Fig. 1. With such an arrangement, the (A) amorphous thermoplastic resin restrains the reinforcing fiber bundles, and a stronger composite can be obtained.

[0082] The content of the (E) resin in the molding material of the present invention is preferably 0.1 parts by weight or more and 20 parts by weight or less, more preferably 3 parts by weight or more and 10 parts by weight or less, relative to 100 parts by weight of the (A) amorphous thermoplastic resin. By setting it in such a range, the dispersibility of the (B) reinforcing fiber can be further improved when molding the molding material. If the content of the impregnating resin is less than 0.1 parts by weight, the impregnation into the (B) reinforcing fiber becomes insufficient, and the mechanical properties may be reduced due to insufficient dispersibility of the (B) reinforcing fiber, which is not preferable. On the other hand, if it exceeds 20 parts by weight, the low viscosity components in the molding material become relatively large, so the physical properties of the matrix resin are reduced, and as a result, the mechanical properties of the molded product obtained by molding the molding material are reduced, which is not preferable.

[0083] Next, a method for producing the molding material of the present invention will be described. Here, the molding material of the present invention is preferably a molding material obtained by cutting a molding material in which a fiber bundle in which (B) reinforcing fibers are impregnated with (E) resin is coated with (A) amorphous thermoplastic resin into a length of 1 to 50 mm. By preparing the molding material to this length, the fluidity and handleability during molding can be sufficiently improved. An example of a particularly preferred embodiment of the molding material cut to an appropriate length in this way is long fiber pellets for injection molding.

[0084] Here, the method for producing a fiber bundle includes a step (I) of supplying an (E) resin to the (B) reinforcing fibers and contacting the (E) resin with the (B) reinforcing fibers in a molten state at 100 to 300°C, and a step (II) of heating the (B) reinforcing fibers in contact with the (E) resin to impregnate the (B) reinforcing fibers with the (E) resin.

[0085] The process (I) is not particularly limited, and a known method such as applying an oil, a sizing agent, or a matrix resin to the fiber bundle can be used. Among these, dipping or coating is preferred, and specifically, a reverse roll, a forward rotation roll, a kiss roll, a spray, or a curtain is preferably used as the coating method.

[0086] Here, dipping refers to a method in which the (E) resin is supplied to a molten bath by a pump and the (B) reinforcing fiber is passed through the molten bath. By immersing the (B) reinforcing fiber in a molten bath of the (E) resin, the (E) resin can be reliably attached to the (B) reinforcing fiber. In addition, the reverse roll, the forward rotation roll, and the kiss roll refer to a method in which the (E) resin melted by a pump is supplied to a roll and the molten (E) resin is applied to the (B) reinforcing fiber. Furthermore, the reverse roll is a method in which two rolls rotate in opposite directions to each other and apply the molten (E) resin onto the roll, and the forward rotation roll is a method in which two rolls rotate in the same direction and apply the molten (E) resin onto the roll. Usually, in the reverse roll and the forward rotation roll, the (B) reinforcing fiber is sandwiched and another roll is installed to reliably attach the (E) resin. On the other hand, the kiss roll is a method in which the (E) resin is attached simply by contacting the (B) reinforcing fiber with the roll. For this reason, kiss rolls are preferable when the viscosity is relatively low, but whichever roll method is used, a specified amount of heated and melted (E) resin is applied and then run while adhering the (B) reinforcing fibers, allowing a specified amount of (E) resin to adhere per unit length of fiber bundle. Spraying utilizes the principle of an atomizer, and is a method in which molten (E) resin is atomized and sprayed onto the (B) reinforcing fibers, while curtain is a method in which molten (E) resin is applied by allowing it to fall naturally from small holes, or by overflowing from a melting tank. The amount required for application is easy to adjust, which reduces loss of (E) resin.

[0087] The melting temperature when the (E) resin is supplied is preferably 100 to 300°C. For more stable adhesion, the temperature is preferably 180 to 230°C. If the temperature is less than 100°C, the viscosity of the (E) resin increases, and uneven adhesion may occur when the resin is supplied. If the temperature exceeds 300°C, the (E) resin may be thermally decomposed if the resin is produced over a long period of time. The (E) resin can be supplied stably by contacting the (B) reinforcing fibers in a molten state of 100 to 300°C.

[0088] Next, in step (II), the (B) reinforcing fibers in contact with the (E) resin obtained in step (I) are heated to impregnate the (B) reinforcing fibers with the (E) resin. Specifically, this is a step in which the (B) reinforcing fibers in contact with the (E) resin are tensioned with a roll or bar, repeatedly widened and bundled, and pressure or vibration is applied at a temperature at which the (E) resin melts, so that the (E) resin is impregnated into the (B) reinforcing fibers. A more specific example is a method in which the reinforcing fiber bundle is passed through the surfaces of multiple heated rolls or bars so as to come into contact with the bundle and widened, and among these, a method of impregnation using a squeeze die, squeeze roll, roll press, or double belt press is preferably used. Here, the squeeze die refers to a die whose diameter narrows in the direction of travel, and is a die that bundles the reinforcing fiber bundle while scraping off excess (E) resin attached thereto and at the same time promoting impregnation. A squeeze roll is a roller that applies tension to the reinforcing fiber bundle to scrape off excess (E) resin while promoting impregnation. A roll press is a device that uses pressure between two rolls to continuously remove air from inside the reinforcing fiber bundle while promoting impregnation, and a double belt press is a device that presses the reinforcing fiber bundle from above and below with belts to promote impregnation.

[0089] In addition, in the step (II), it is preferable that the (E) resin is impregnated into the (B) reinforcing fiber.

[0090] In step (II), the maximum temperature of the (E) resin is preferably 150 to 300° C., more preferably 180 to 300° C., and even more preferably 180 to 250° C. If the temperature is less than 150° C., the (E) resin may not be sufficiently melted, resulting in an insufficiently impregnated reinforcing fiber bundle, whereas if the temperature is 400° C. or higher, undesirable side reactions such as a decomposition reaction of the (E) resin may occur.

[0091] The heating method in step (II) is not particularly limited, but specific examples include a method using a heated chamber and a method using a hot roller to simultaneously apply heat and pressure.

[0092] In addition, from the viewpoint of suppressing the occurrence of undesirable side reactions such as crosslinking and decomposition of the (E) resin, it is preferable to heat in a non-oxidizing atmosphere. Here, the non-oxidizing atmosphere refers to an atmosphere having an oxygen concentration of 5% by volume or less, preferably 2% by volume or less, and more preferably an atmosphere containing no oxygen, that is, an inert gas atmosphere such as nitrogen, helium, or argon, and among these, a nitrogen atmosphere is particularly preferable from the viewpoints of economy and ease of handling.

[0093] In addition, the take-up speed of the composite fiber bundle directly affects the process speed, so the higher the speed, the more preferable it is from the viewpoints of economy and productivity. Specifically, the take-up speed is preferably 10 to 100 m / min. More preferably, it is 20 to 100 m / min, and even more preferably, it is 30 to 100 m / min. Examples of the take-up method include a method of drawing out the composite fiber bundle with a nip roller, a method of winding it up with a drum winder, and a method of directly cutting the composite fiber bundle to a fixed length with a strand cutter or the like.

[0094] Furthermore, the molding material of the present invention is constituted by bonding the (A) amorphous thermoplastic resin to the composite fiber bundle obtained as described above. The method for bonding the (A) amorphous thermoplastic resin to the composite fiber bundle is not particularly limited, but more specifically, there can be mentioned a method of continuously arranging the (A) amorphous thermoplastic resin so as to coat the periphery of the composite fiber bundle using an extruder and a coating die for an electric wire coating method, or a method of arranging a molten film-like (A) amorphous thermoplastic resin on one or both sides of a composite flattened by a roll or the like using an extruder and a T-die, and integrating the resin with a roll or the like.

[0095] Fig. 4 is a schematic diagram showing an example of the shape of the composite fiber bundle (1) obtained in the present invention in the axial direction perpendicular thereto. In Fig. 4, the black circles (3) represent the single yarns of the (B) reinforcing fiber, and the white areas (4) represent the (E) resin. The (E) resin (4) fills the spaces between the single yarns (3). In other words, the (B) reinforcing fiber single yarns (3) are dispersed like islands in a sea of ​​the (E) resin (4).

[0096] Next, a method for producing the fiber-reinforced resin molded article (hereinafter, sometimes simply referred to as "molded article") of the present invention will be described.

[0097] A molded product can be obtained by molding the molding material of the present invention described above. The molding method is not particularly limited, but molding methods with excellent productivity such as injection molding, autoclave molding, press molding, filament winding molding, and stamping molding can be applied, and these can also be used in combination. In addition, integrated molding such as insert molding and outsert molding can also be easily performed. Furthermore, even after molding, correction treatment by heating, and bonding methods with excellent productivity such as heat welding, vibration welding, and ultrasonic welding can also be utilized.

[0098] Among these, a molding method using a mold is preferred, and a molding method using an injection molding machine in particular can continuously produce a stable molded product. There are no particular restrictions on the conditions for injection molding, but the following conditions are preferred: injection time: 0.5 to 10 seconds, more preferably 2 to 10 seconds, back pressure: 0.1 MPa to 10 MPa, more preferably 2 MPa to 8 MPa, dwell pressure: 1 MPa to 50 MPa, more preferably 1 MPa to 30 MPa, dwell time: 1 to 20 seconds, more preferably 5 to 20 seconds, cylinder temperature: 250°C to 320°C, mold temperature: 20°C to 100°C. Here, the cylinder temperature refers to the temperature of the part of the injection molding machine where the molding material is heated and melted, and the mold temperature refers to the temperature of the mold into which the resin is injected to form a predetermined shape. By appropriately selecting these conditions, particularly the injection time, back pressure, and mold temperature, the fiber length of the reinforcing fiber in the molded product can be easily adjusted. The cylinder temperature is preferably 250°C or higher. A temperature of 250° C. or higher is preferable because it increases the fluidity of the molding material when molding large parts such as automobile exterior parts, enables molding in a short time, and allows the molding material to reach the edges.

[0099] The method for producing a molded product of the present invention preferably includes a step of drying the molding material before molding. The drying temperature is preferably in the range of the glass transition temperature to the glass transition temperature + 20°C. If the temperature is above the glass transition temperature, moisture is easily removed from the molecular chain, and the moisture content of the molding material decreases, which is preferable because gas burning during molding can be suppressed. Also, if the temperature is below the glass transition temperature + 20°C, it is preferable because heat fusion between molding materials can be suppressed. The drying time is preferably 4 hours or more. If the drying time is 4 hours or more, it is preferable because the moisture content of the molding material decreases, which is preferable because gas burning during molding can be suppressed. Also, although there is no particular upper limit, the moisture content becomes constant at 24 hours or more, and the effect may be reduced. Thus, it is particularly preferable that the moisture content of the molding material of the present invention used for producing a molded product is 0.02% or less as described above, which can particularly suppress gas burning during molding.

[0100] Examples of molded products obtained by the above molding method include automobile parts, components and outer panels such as instrument panels, door beams, under covers, lamp housings, pedal housings, radiator supports, spare tire covers, various modules such as front ends, cylinder head covers, bearing retainers, intake manifolds, pedals, etc.; aircraft-related parts, components and outer panels such as landing gear pods, winglets, spoilers, edges, rudder, fairings, ribs, etc.; tools such as monkey bars and wrenches; and household and office electrical appliance parts such as telephones, facsimiles, VTRs, copy machines, televisions, microwave ovens, audio equipment, toiletries, laser discs (registered trademark), refrigerators, and air conditioners. Other examples include electrical and electronic equipment parts such as casings used in personal computers and mobile phones, and keyboard supports that are members that support keyboards inside personal computers. In the present invention, when conductive carbon fibers are used as the (B) reinforcing fibers, such electrical and electronic equipment parts are more preferably given electromagnetic wave shielding properties.

[0101] The molded article of the present invention is also particularly suitable for use as large automobile exterior molded articles such as charger covers, battery AC adapter cases, capacitor cases, power meters, and door parts. EXAMPLES

[0102] The present invention will be described in more detail with reference to the following examples, but the present invention is not limited to the descriptions of these examples. First, the methods for evaluating various properties used in the examples and comparative examples will be described.

[0103] (1) Heat loss measurement The thermal loss of molding materials or flame retardants under nitrogen or air was measured by thermogravimetric analysis (TGA). Using a platinum sample pan, the temperature was raised to 300°C at a rate of 50°C / min while flowing nitrogen or air at 20ml / min into the measurement chamber, and the thermal loss was measured after holding for 10 minutes. The test machine used was a TG / DTA7200 (Hitachi High-Tech Science).

[0104] (2) Bending strength measurement of molded products The bending strength of the ISO dumbbell test pieces obtained in each of the Examples and Comparative Examples was measured using a three-point bending test jig (indenter radius 5 mm) with a support distance set to 64 mm and a test speed of 2 mm / min in accordance with ISO 178. The test machine used was an "Instron (registered trademark)" universal testing machine Model 5566 (manufactured by Instron Corporation).

[0105] (3) Charpy impact strength measurement of molded products A parallel portion of the Type A1 multipurpose test piece according to JIS K7139 obtained in each Example and Comparative Example was cut out, and a V-notch Charpy impact test was carried out in accordance with ISO179 using a C1-4-01 model testing machine manufactured by Tokyo Test Instruments Co., Ltd., to measure the impact strength (kJ / m 2 ) was calculated.

[0106] (4) Moisture content measurement of molding materials Measurements were performed using a Karl Fischer measurement device (vaporizer: SE-24, electrolytic cell: AQ-6) manufactured by Hiranuma Sangyo Co., Ltd. The sample was 3 g, and the nitrogen used for moisture vaporization was 220°C and 200 ml / min.

[0107] (5) Glass transition temperature of molding material The glass transition temperature was measured using 10±2 mg of the molding material at a heating rate of 20° C. / min using a differential scanning calorimeter (DSC) in accordance with JIS K7121.

[0108] (6) Evaluation of gas burns The ends of the dumbbell test pieces are prone to gas burning because gas does not easily escape. Therefore, to evaluate the appearance of the molded product, 20 dumbbell-shaped multipurpose test pieces of type A1 described in JIS K7139 were molded in succession, and the percentage of dumbbell pieces that showed discoloration of 2 mm or more at the ends was measured. The molding conditions were as described in each of the examples and comparative examples described later.

[0109] (7) Flame retardancy A molded product (test piece) of 125mm x 13mm (0.5mmt [thickness]) was molded and flame retardancy evaluation was carried out in accordance with UL-94. Specifically, a burner flame was applied to the lower end of the vertically supported test piece and held for 10 seconds, after which the burner flame was removed from the test piece. After the flame went out, the burner flame was applied again and the same operation was carried out. Then, a judgment was made based on the duration of flaming combustion after the end of the first flame application, the total duration of flaming combustion and flameless combustion after the second application, and the presence or absence of burning debris. The criteria for each grade in UL94 are roughly as follows: V-0: The first and second flaming combustion durations were within 10 seconds each, the total of the first and second flaming combustion durations of the five test specimens was within 50 seconds, the total of the second flaming combustion duration and flameless combustion duration was within 30 seconds, and there was no burning debris. V-1: The duration of the first and second flaming combustion was more than 10 seconds and less than 30 seconds each, the total duration of the first and second flaming combustion for the five test specimens was less than 250 seconds, the total duration of the second flaming combustion and flameless combustion was more than 30 seconds and less than 60 seconds, and there was no burning debris. V-2: The duration of the first and second flaming combustion was more than 10 seconds but less than 30 seconds, the total duration of the first and second flaming combustion for the five test specimens was less than 250 seconds, the total duration of the second flaming combustion and flameless combustion was more than 30 seconds but less than 60 seconds, and burning debris was present. V-out: The duration of the first flaming combustion was more than 30 seconds, or the combined duration of the second flaming combustion and the duration of flameless combustion was more than 60 seconds.

[0110] (8) Fluidity test Using a mold with a cavity extending in the longitudinal direction with a width of 13 mm and a thickness of 0.5 mm, injection molding was performed in the longitudinal direction of the mold cavity under the following conditions with a constant injection speed, and evaluation test pieces with a length equivalent to the flow distance that the injected resin could reach in the cavity were molded. The length to the tip (longest part) of the test piece was measured, and the average of the lengths of the five test pieces was taken as the flow length. Molding materials with good flowability fill the mold in a short time, so the distance they flow before cooling and solidifying is long, and so the flowability improves in the following order: C, B, A. A: Maximum length 100mm or more B: Maximum length 80mm or more and less than 100mm C: Maximum length 60mm or more and less than 80mm [Injection molding conditions] Cylinder temperature / mold temperature: 300℃ / 70℃ Injection speed: 30mm / s

[0111] (9) Measurement of mold shrinkage A molded product of 80mm x 80mm (2mmt [thickness]) was molded, and the distance between the gauge lines of the resin test piece in the resin flow direction (MD) and perpendicular to the resin flow direction (TD) was measured. The shrinkage rate was measured relative to the gauge line distance engraved on the mold. The measured value was the average value of the shrinkage rates in the MD and TD directions. The molding shrinkage rates are best in the following order: D, C, B, A. A: Less than 0.2% B: 0.2% or more but less than 0.3% C: 0.3% or more and less than 0.5% D: 0.5% or more [Molding conditions] Cylinder temperature / mold temperature: 300℃ / 70℃ Cooling time: 20s (cooling time by mold) Holding pressure: Half of the peak injection pressure

[0112] Next, each component used in the examples and comparative examples will be described. (A) Amorphous thermoplastic resin (A-1) Teijin Chemical Co., Ltd. An aromatic polycarbonate resin having a bisphenol A carbonate structure, "Panlite (registered trademark) L-1225L" (viscosity average molecular weight: 19,500, glass transition temperature: 145°C), was used.

[0113] (B) Reinforced fiber For (B-1) and (B-2), carbon fibers were produced by the production method of Reference Example 1 described below. (B-1) Carbon fiber with glycerol polyglycidyl ether (aliphatic epoxy compound: epoxy group number 3) (B-2) Carbon fiber with bisphenol A type epoxy resin (aromatic epoxy compound: epoxy group number 2, jER828 manufactured by Japan Epoxy Resin Co., Ltd.) (B-3) Glass fiber (JER2400 T-423N manufactured by Nippon Electric Glass Co., Ltd.)

[0114] (C) Phosphorus-based flame retardants (C-1) Condensed phosphate ester flame retardant "PX-200" manufactured by Daihachi Chemical Industry Co., Ltd. (phosphorus concentration 9%, heat loss in air at 300℃ for 10 minutes 7%) (C-2) Condensed phosphate ester flame retardant "CR-741" manufactured by Daihachi Chemical Industry Co., Ltd. (phosphorus concentration 9%, heat loss at 300℃ for 10 minutes in air 12%) (C-3) Condensed phosphate ester flame retardant "SR-3000" manufactured by Daihachi Chemical Industry Co., Ltd. (phosphorus concentration 7%, heat loss in air at 300℃ for 10 minutes 3%) (C-4) Melam polyphosphate "PHOSMEL (registered trademark) 100" manufactured by Nissan Chemical Co., Ltd.

[0115] (D) Antioxidants (D-1) Hindered phenol "Irganox (registered trademark) 1010" manufactured by BASF Japan Ltd. (D-2) Thioether (Adeka Corporation) "Adeka STAB (registered trademark) AO-412S" (D-3) A 1 / 1 mixture of (D-1) / (D-2) (D-4) A 2 / 1 mixture of (D-1) / (D-2)

[0116] (E) Resin (E-1) Mitsubishi Chemical Corporation Bisphenol A type epoxy resin "jER1003" (melt viscosity: 0.5 Pa·s, heat loss rate: 2%) (E-2) Mitsubishi Chemical Corporation Bisphenol A type epoxy resin "jER1004AF" (melt viscosity: 1 Pa·s, heat loss rate: 1%) (E-3) Hydrogenated terpene polymer “Clearon P125” (melt viscosity: 400 Pa·s, heat loss rate: 18%) manufactured by Yasuhara Chemical Co., Ltd. was used.

[0117] (Reference Example 1) Preparation of carbon fiber The copolymer, whose main component is polyacrylonitrile, is spun, calcined, and electrolytically oxidized to produce a total of 24,000 single fibers, with a single fiber diameter of 7 μm, a mass per unit length of 1.6 g / m, and a specific gravity of 1.8 g / cm. 3 The continuous carbon fiber was obtained. The strand tensile strength of this continuous carbon fiber was 4,880 MPa, and the strand tensile modulus was 225 GPa. The surface oxygen concentration ratio (O / C) was controlled by the current density in the electrolytic oxidation treatment, and was O / C = 0.10.

[0118] As a sizing agent, a sizing agent mother liquid was prepared by dissolving epoxy resin in water or dispersing it with a surfactant, and the sizing agent was applied to the carbon fibers by immersion and dried at 220° C. The amount of the sizing agent applied was controlled to 1.0 part by weight per 100 parts by weight of carbon fiber by adjusting the concentration of the mother liquid.

[0119] (Reference Example 2) Preparation of resin-impregnated reinforcing fiber A liquid coating of the (E) resin was formed by heating and melting it on a roll heated to the application temperature. A reverse roll was used to form a coating of a constant thickness on the roll. Continuous (B) reinforcing fibers were passed over this roll while in contact with the fibers, and the (E) resin was adhered to the fibers. Next, the fibers were passed between five sets of roll presses with a diameter of 50 mm in a chamber heated to the impregnation temperature. This operation allowed the (E) resin to be impregnated into the interior of the reinforcing fiber bundle, forming resin-impregnated reinforcing fibers with the specified blending amount.

[0120] (Reference Example 3) Preparation of resin composition A JSW TEX-30α type twin-screw extruder (screw diameter 30 mm, die diameter 5 mm, barrel temperature 290°C, screw rotation speed 150 rpm) was used, and a dry blend of (A) amorphous thermoplastic resin and (B) reinforcing fiber and / or (C) phosphorus-based flame retardant and / or (D) antioxidant was fed from the main hopper. The molten resin was discharged from the die opening while degassing was performed through a downstream vacuum vent, and the resulting strand was cooled and then cut with a cutter to obtain molten kneaded pellets of the resin composition.

[0121] Example 1 (Step X) (A-1), (C-1) and (D-1) were dry-blended according to the formulation shown in Table 1, and the same was used to obtain a resin composition according to Reference Example 3.

[0122] (Step Y) The resin-impregnated reinforcing fiber (B-1) was passed through a coating die for electric wire coating installed at the tip of a Japan Steel Works, Ltd. TEX-30α type twin-screw extruder (screw diameter 30 mm, L / D = 32), and the resin composition was extruded from the extruder in a molten state into the die, and was continuously arranged so as to coat the circumference of the resin-impregnated reinforcing fiber. Here, in the process of coating the circumference of the resin-impregnated reinforcing fiber with the resin composition, the extrusion amount of the (A) amorphous thermoplastic resin was adjusted so that the blending amount of the resin-impregnated reinforcing fiber in the resin molding material and the weight content of the reinforcing fiber in the molded product were the predetermined values ​​shown in Table 1. After cooling the obtained continuous molding material, it was cut with a cutter to obtain a molding material in the form of long fiber pellets of 7 mm.

[0123] (Step Z) The obtained long fiber pellet-like molding material was dried with hot air at 80°C and normal pressure for 4 hours, and then a test piece (molded product) for property evaluation was molded using a Sumitomo Heavy Industries SE75DUZ-C250 injection molding machine at the following conditions: injection time: 10 seconds, dwell pressure: molding lower limit pressure + 10 MPa, dwell time: 10 seconds, cylinder temperature: 300°C, mold temperature: 70°C.

[0124] The obtained test pieces were left in a constant temperature and humidity room adjusted to a temperature of 23°C and a relative humidity of 50% for 24 hours, and then subjected to a characteristic evaluation test. Next, the obtained test pieces for characteristic evaluation (molded products) were evaluated according to the evaluation methods described above. The evaluation results are summarized in Table 1.

[0125] Example 2 (Step X) A resin composition was obtained in the same manner as in Example 1. (Step Y) A molding material was obtained in the same manner as in Example 1. (Step Z) The obtained molding material in the form of long fiber pellets was vacuum-dried under reduced pressure at 80° C. for 24 hours to obtain a molded product in the same manner as in Example 1. The evaluation results are shown in Table 1.

[0126] Comparative Example 1 (Step X) A resin composition was obtained in the same manner as in Example 1, except that (D-1) was omitted. (Step Y) A molding material was obtained in the same manner as in Example 1. (Step Z) A molded article was obtained in the same manner as in Example 1. The evaluation results are shown in Table 1.

[0127] Comparative Example 2 (Step X) A resin composition was obtained in the same manner as in Example 1. (Step Y) A molding material was obtained in the same manner as in Example 1. (Process Z) The long fiber pellet-like molding material obtained in Process Y was left for 24 hours in a temperature and humidity controlled room at a temperature of 23°C and 50% RH, and then a test piece (molded product) for property evaluation was molded using an SE75DUZ-C250 injection molding machine manufactured by Sumitomo Heavy Industries, Ltd., with an injection time of 10 seconds, dwell pressure of lower limit molding pressure + 10 MPa, dwell time of 10 seconds, cylinder temperature of 300°C, and mold temperature of 80°C. The evaluation results are summarized in Table 1.

[0128] Comparative Example 3 (Step X) A resin composition was obtained in the same manner as in Comparative Example 1. (Step Y) A molding material was obtained in the same manner as in Example 1. (Step Z) A molding material was obtained in the same manner as in Comparative Example 2. The evaluation results are shown in Table 1.

[0129] Examples 3 to 16, 18 to 20, Comparative Example 4, Comparative Examples 6 to 12 (Step X) Resin compositions were obtained in the same manner as in Example 1, except that the raw material compositions were changed to those shown in Tables 1 to 3. (Step Y) A molding material was obtained in the same manner as in Example 1, except that the raw material compositions were changed to those shown in Tables 1 to 3. (Step Z) A molded article was obtained in the same manner as in Example 1. The evaluation results are summarized in Tables 1 to 3.

[0130] Comparative Example 5 (Step X) A resin composition was obtained in the same manner as in Example 1, except that the raw material composition was changed to that shown in Table 1. (Step Y) When an attempt was made to obtain a molding material by adjusting (B-1) to 80 parts by weight per 100 parts by weight of (A-1), the resin-impregnated reinforcing fiber was not sufficiently covered with (A-1), and poor cutting occurred during cutting with a cutter, making it impossible to obtain a molding material.

[0131] On the other hand, Comparative Examples 1 to 4 and 7 to 12 showed a large amount of heat loss under nitrogen or air, and scorching was observed during molding. Comparative Example 5 contained a large amount of reinforcing fibers, which caused clogging of the mold during molding processing, making molding impossible. Comparative Example 6 did not use a phosphorus-based flame retardant, and the flame retardancy was insufficient.

[0132] Example 17 (Step X) A resin composition was obtained by dry blending (A-1), (C-1) and (D-1) according to the formulation shown in Table 2 and using 3 mm chopped fibers of (B-1) according to Reference Example 3. The average fiber length of (B-1) contained in the resin composition was 0.3 mm. (Step Y) omitted. The resin composition obtained in (Step Z) and (Step X) was used as a molding material and dried with hot air at 80°C and normal pressure for 4 hours. Then, a test piece (molded product) for property evaluation was molded using a SE75DUZ-C250 injection molding machine manufactured by Sumitomo Heavy Industries, Ltd. with an injection time of 10 seconds, a dwell pressure of lower limit molding pressure + 10 MPa, a dwell time of 10 seconds, a cylinder temperature of 300°C, and a mold temperature of 70°C.

[0133] The obtained test pieces were left in a constant temperature and humidity room adjusted to a temperature of 23°C and a relative humidity of 50% for 24 hours, and then subjected to a characteristic evaluation test. Next, the obtained test pieces for characteristic evaluation (molded products) were evaluated according to the evaluation methods described above. The evaluation results are summarized in Table 2.

[0134] [Table 1]

[0135] [Table 2]

[0136] [Table 3]

[0137] All of the molding materials in Examples 1 to 20 contained (A) an amorphous thermoplastic resin, and contained 4 to 60 parts by weight of (B) reinforcing fiber and 20 to 60 parts by weight of (C) a phosphorus-based flame retardant per 100 parts by weight of the amorphous thermoplastic resin (A). Furthermore, when heated at 300°C for 10 minutes under nitrogen and air, the heat loss was 1.5% or less, and the molded articles exhibited excellent flame retardancy, molded article appearance, fluidity, molding shrinkage, and mechanical properties. [Industrial Applicability]

[0138] The fiber-reinforced resin molding material of the present invention can be applied to the production of any molded article that requires excellent flame retardancy, mechanical properties, appearance, etc. [Explanation of symbols]

[0139] 1: (B) Reinforced fiber and (E) Resin composite fiber bundle 2:(A) Amorphous thermoplastic resin 3: (B) Single yarn of reinforcing fiber 4: (E) Resin

Claims

1. A fiber-reinforced resin molding material comprising at least the following components (A) to (C), characterized in that the heat loss when heated at 300°C for 10 minutes under nitrogen and under air is 1.5% or less, and (D) an antioxidant is added in an amount of 1.0% by weight or more. (A) Amorphous thermoplastic resin: 100 parts by weight (B) Reinforcing fiber: 4 to 60 parts by weight (C) Phosphorus-based flame retardant: 20 to 60 parts by weight

2. The fiber-reinforced resin molding material according to claim 1, having a moisture content of 0.02% or less.

3. 3. The fiber-reinforced resin molding material according to claim 1, wherein the antioxidant (D) is a mixture of a sulfur-based antioxidant and a hindered phenol-based antioxidant.

4. The fiber-reinforced resin molding material according to any one of claims 1 to 3, wherein the phosphorus-based flame retardant (C) has a heat loss of 5% or less when heated at 300 ° C. for 10 minutes in air.

5. The fiber reinforced resin molding material according to any one of claims 1 to 4, having a glass transition temperature of 100 ° C. or less.

6. The fiber-reinforced resin molding material according to any one of claims 1 to 5, wherein the phosphorus-based flame retardant (C) is a condensed phosphoric acid ester.

7. The fiber-reinforced resin molding material according to any one of claims 1 to 6, wherein the reinforcing fiber (B) is a carbon fiber.

8. The fiber reinforced resin molding material according to any one of claims 1 to 7, wherein the fiber length of the reinforcing fiber (B) is 3 to 50 mm.

9. The fiber reinforced resin molding material according to any one of claims 1 to 8, wherein the reinforcing fiber (B) is coated with the amorphous thermoplastic resin (A).

10. The fiber reinforced resin molding material according to any one of claims 1 to 9, wherein the reinforcing fiber (B) is impregnated with the resin (E).

11. The fiber-reinforced resin molding material according to any one of claims 1 to 10, which is formed into a pellet shape.

12. A fiber-reinforced resin molded product produced using the fiber-reinforced resin molding material according to any one of claims 1 to 11.

13. A method for producing a fiber-reinforced resin molded product using the fiber-reinforced resin molding material according to any one of claims 1 to 11, comprising drying the fiber-reinforced resin molding material at a temperature from the glass transition temperature of the fiber-reinforced resin molding material to the glass transition temperature + 20 ° C. before molding. A method for producing a fiber-reinforced resin molded product.

Citation Information

Patent Citations

  • Phosphoric ester flame retardant

    JP1998168227A

  • Flame-retardant master batch and molded article using the same

    JP2006307178A

  • Flame retardant masterbatch

    JP2008101035A

  • Composite reinforcement fiber bundle, method for producing the same, and molding material

    JP2013011050A

  • Polycarbonate resin molding material and molding

    JP2013209629A