Ring-opening copolymer
Patent Information
- Application Number
- JP2021565618
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-12-17
- Filing Date
- 2020-12-16
- Publication Date
- 2024-09-26
- Estimated Expiration
- 2040-12-16
AI Technical Summary
【0016】 本発明によれば、ホットフロー性に優れ、これにより、クラムの互着を有効に防止することができ、しかも、耐摩耗性に優れたゴム架橋物を与えることができる開環共重合体および該開環共重合体の製造方法、ならびに、このような開環共重合体を用いて得られるゴム組成物、該ゴム組成物を用いて得られるゴム架橋物、および該ゴム組成物またはゴム架橋物を用いて得られる成形体を提供することができる。
Smart Images

Figure 0007556361000007 
Figure 0007556361000013 
Figure 0007556361000015
Abstract
Description
[Technical field]
[0001] The present invention relates to a ring-opened copolymer, more specifically, to a ring-opened copolymer capable of giving a cross-linked rubber product having excellent hot flow properties (resistance to adhesion of crumbs to each other) and excellent abrasion resistance, and a method for producing the ring-opened copolymer. The present invention also relates to a rubber composition obtained by using such a ring-opened copolymer, a cross-linked rubber product obtained by using the rubber composition, and a molded article obtained by using the rubber composition or the cross-linked rubber product. [Background technology]
[0002] It is generally known that cyclopentene and norbornene compounds undergo metathesis ring-opening polymerization in the presence of so-called Ziegler-Natta catalysts consisting of Group 6 transition metal compounds such as WCl6 and MoCl5 and organometallic activators such as triisobutylaluminum, diethylaluminum chloride, and tetrabutyltin to give unsaturated linear ring-opened polymers.
[0003] For example, Patent Document 1 discloses a ring-opening copolymer made of cyclopentene and a norbornene compound, in which the structural units derived from cyclopentene are 40 to 90% by weight, the structural units derived from the norbornene compound are 10 to 60% by weight, and the weight-average molecular weight (Mw) is 200,000 to 1,000,000, based on all repeating structural units in the copolymer. According to the technology of Patent Document 1, the wet grip property and low heat build-up of the obtained cross-linked rubber can be improved by ring-opening copolymerizing cyclopentene with a norbornene compound.
[0004] Also, for example, Patent Document 2 discloses a method for producing a cyclopentene ring-opening polymer by ring-opening polymerization of cyclopentene in the presence of a metathesis polymerization catalyst, characterized in that the cyclopentene is reacted with 0.001 to 1 mol % of a cyclic olefin having a vinyl group and / or a compound having three or more vinyl groups, based on the cyclopentene. According to the technology of Patent Document 2, the cyclopentene ring-opening copolymer has a branched structure, making it possible to easily produce a cyclopentene ring-opening copolymer having excellent hot flow properties.
[0005] However, Patent Documents 1 and 2 do not discuss the abrasion resistance of the resulting cross-linked rubber product. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] International Publication No. 2014 / 133028 [Patent Document 2] JP 2011-126966 A Summary of the Invention [Problem to be solved by the invention]
[0007] The present invention has been made in view of the above circumstances, and has an object to provide a ring-opening copolymer capable of giving a cross-linked rubber product having excellent hot flow properties (resistance to adhesion of crumbs to each other) and excellent abrasion resistance, a method for producing the ring-opening copolymer, a rubber composition obtained by using such a ring-opening copolymer, a cross-linked rubber product obtained by using the rubber composition, and a molded article obtained by using the rubber composition or the cross-linked rubber product. [Means for solving the problem]
[0008] Means for Solving the Problems The present inventors have conducted intensive research in order to achieve the above-mentioned object, and as a result have found that a ring-opening copolymer containing structural units derived from a norbornene compound having a specific structure, structural units derived from a specific monocyclic cyclic olefin, and a prescribed proportion of branched structural units, has excellent hot flow properties, can effectively prevent the occurrence of mutual adhesion of crumbs, and can give a cross-linked rubber product having excellent abrasion resistance, thereby completing the present invention.
[0009] That is, according to the present invention, there is provided a ring-opened copolymer comprising a structural unit derived from a norbornene compound represented by the following general formula (I), a structural unit derived from a monocyclic olefin, and a branched structural unit, wherein the content of the branched structural unit in all repeating structural units in the ring-opened copolymer is 0.005 to 0.08 mol %. [ka] (In the above general formula (I), R 1 ~R 4 each independently represents a hydrogen atom, a linear saturated hydrocarbon group having 1 to 20 carbon atoms, or a substituent containing a halogen atom, a silicon atom, an oxygen atom, or a nitrogen atom, and m is 0 or 1.
[0010] In the ring-opened copolymer of the present invention, the content of the structural units derived from the norbornene compound in all repeating structural units is preferably 5 mol % or more. In the ring-opening copolymer of the present invention, m is preferably 0 in the general formula (I). In the ring-opening copolymer of the present invention, in the general formula (I), R 1 ~R 4 are each preferably independently a hydrogen atom or an alkyl group having 1 to 3 carbon atoms. In the ring-opened copolymer of the present invention, the monocyclic olefin is preferably at least one selected from the group consisting of cyclopentene, cyclohexene, cycloheptene, and cyclooctene. In the ring-opened copolymer of the present invention, the branched structural unit is preferably a branched structural unit represented by any one of the following formulas (II) to (V). [ka] (In the above formula (II), the hydrogen atom may be substituted with an alkyl group having 1 to 6 carbon atoms.) [ka] (In the above formula (III), the hydrogen atom may be substituted with an alkyl group having 1 to 6 carbon atoms.) [ka] (In the above formula (IV), the hydrogen atom may be substituted with an alkyl group having 1 to 6 carbon atoms.) [ka] (In the above formula (V), the hydrogen atom may be substituted with an alkyl group having 1 to 6 carbon atoms.) The ring-opening copolymer of the present invention preferably has a weight average molecular weight of 150,000 or more and 400,000 or less.
[0011] According to the present invention, there is also provided a rubber composition containing the ring-opened copolymer. The rubber composition of the present invention preferably further contains a crosslinking agent.
[0012] According to the present invention, there is also provided a cross-linked rubber product obtained by cross-linking the above rubber composition.
[0013] According to the present invention, there is also provided a molded article obtained by molding the above rubber composition or the above cross-linked rubber product.
[0014] The present invention also provides a method for producing a ring-opened copolymer, which comprises ring-opening metathesis polymerization of a monomer mixture containing a norbornene compound represented by the following general formula (I), a monocyclic cyclic olefin, and a monomer capable of forming a branched structure, wherein the monomer capable of forming a branched structure is at least one selected from the group consisting of a polycyclic diolefin compound having at least two ring structures each having one double bond, a cyclic olefin compound having a ring structure having one double bond and a vinyl group, and a compound having three or more vinyl groups. [ka] (In the above general formula (I), R 1 ~R 4 each independently represents a hydrogen atom, a linear saturated hydrocarbon group having 1 to 20 carbon atoms, or a substituent containing a halogen atom, a silicon atom, an oxygen atom, or a nitrogen atom, and m is 0 or 1.
[0015] In the method for producing a ring-opened copolymer of the present invention, the content of the monomer capable of forming a branched structure in the monomer mixture is preferably 0.01 to 0.045 mol % based on the total amount of the monomer mixture. Effect of the Invention
[0016] According to the present invention, it is possible to provide a ring-opened copolymer which has excellent hot flow properties, and thereby can effectively prevent crumbs from adhering to each other, and which can give a cross-linked rubber product having excellent abrasion resistance, a method for producing the ring-opened copolymer, a rubber composition obtained by using such a ring-opened copolymer, a cross-linked rubber product obtained by using the rubber composition, and a molded article obtained by using the rubber composition or the cross-linked rubber product. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0017] <Ring-opening copolymer> The ring-opened copolymer of the present invention is a ring-opened copolymer containing a structural unit derived from a norbornene compound represented by the following general formula (1), a structural unit derived from a monocyclic cyclic olefin, and a branched structural unit, and the content of the branched structural unit in all repeating structural units in the ring-opened copolymer is 0.005 to 0.08 mol %. [ka] (In the above general formula (1), R 1 ~R 4 each independently represents a hydrogen atom, a linear saturated hydrocarbon group having 1 to 20 carbon atoms, or a substituent containing a halogen atom, a silicon atom, an oxygen atom, or a nitrogen atom, and m is 0 or 1.
[0018] Specific examples of the norbornene compound represented by the above general formula (1) for forming the norbornene-compound-derived structural unit in the present invention include the following compounds.
[0019] Bicyclo[2.2.1]hept-2-enes having unsubstituted or linear saturated hydrocarbon substituents, such as 2-norbornene, 5-methyl-2-norbornene, 5-ethyl-2-norbornene, 5-butyl-2-norbornene, 5-hexyl-2-norbornene, and 5-decyl-2-norbornene;
[0020] Bicyclo[2.2.1]hept-2-enes having an alkoxycarbonyl group, such as methyl 5-norbornene-2-carboxylate, ethyl 5-norbornene-2-carboxylate, methyl 2-methyl-5-norbornene-2-carboxylate, and ethyl 2-methyl-5-norbornene-2-carboxylate;
[0021] Bicyclo[2.2.1]hept-2-enes having a hydroxycarbonyl group, such as 5-norbornene-2-carboxylic acid and 5-norbornene-2,3-dicarboxylic acid;
[0022] Bicyclo[2.2.1]hept-2-enes having a hydroxyl group, such as 5-hydroxy-2-norbornene, 5-hydroxymethyl-2-norbornene, 5,6-di(hydroxymethyl)-2-norbornene, 5,5-di(hydroxymethyl)-2-norbornene, 5-(2-hydroxyethoxycarbonyl)-2-norbornene, and 5-methyl-5-(2-hydroxyethoxycarbonyl)-2-norbornene;
[0023] Bicyclo[2.2.1]hept-2-enes having a hydrocarbonyl group, such as 5-norbornene-2-carbaldehyde;
[0024] Bicyclo[2.2.1]hept-2-enes having an alkoxycarbonyl group and a hydroxycarbonyl group, such as 3-methoxycarbonyl-5-norbornene-2-carboxylic acid;
[0025] bicyclo[2.2.1]hept-2-enes having a carbonyloxy group, such as 5-norbornen-2-yl acetate and 2-methyl-5-norbornen-2-yl acetate;
[0026] Bicyclo[2.2.1]hept-2-enes having functional groups containing nitrogen atoms, such as 5-norbornene-2-carbonitrile and 5-norbornene-2-carboxamide;
[0027] Bicyclo[2.2.1]hept-2-enes containing halogen atoms, such as 5-chloro-2-norbornene;
[0028] Bicyclo[2.2.1]hept-2-enes having a functional group containing a silicon atom, such as 5-trimethoxysilyl-2-norbornene and 5-triethoxysilyl-2-norbornene;
[0029] The norbornene compound represented by the above general formula (1) may be used alone or in combination of two or more. The norbornene compound represented by the above general formula (1) is preferably a norbornene compound represented by the above general formula (1) in which m is 0. In addition, in the above general formula (1), R 1 ~R 4 R are preferably groups that do not have an olefinic carbon-carbon double bond and do not bond to each other to form a ring, and may be the same or different. 1 ~R 4 is more preferably a hydrogen atom or an alkyl group having 1 to 3 carbon atoms. As the norbornene compound represented by the above general formula (1), 2-norbornene, 5-methyl-2-norbornene, and 5-ethyl-2-norbornene are more preferable, and 2-norbornene is even more preferable from the viewpoint of easier achievement of the effects of the present invention.
[0030] The content ratio of the structural units derived from norbornene compounds to all repeating structural units in the ring-opened copolymer of the present invention is not particularly limited, but is preferably 5 to 95 mol%, more preferably 10 to 90 mol%, even more preferably 15 to 85 mol%, more preferably 20 to 80 mol%, and particularly preferably 20 to 50 mol%. By setting the content ratio of the structural units derived from norbornene compounds in the above range, the abrasion resistance of the cross-linked rubber can be further improved.
[0031] The monocyclic olefin for forming the monocyclic olefin-derived structural unit in the present invention is not particularly limited as long as it is an olefin having no substituent having a carbon-carbon unsaturated bond and only one cyclic structure, and examples thereof include cyclic monoolefins such as cyclopropene, cyclobutene, cyclopentene, methylcyclopentene, cyclohexene, methylcyclohexene, cycloheptene, and cyclooctene; cyclic diolefins such as cyclohexadiene, methylcyclohexadiene, cyclooctadiene, and methylcyclooctadiene; and the like.
[0032] The monocyclic olefin may be used alone or in combination of two or more. As the monocyclic olefin, cyclopentene, cyclohexene, cycloheptene and cyclooctene are preferred, and from the viewpoint of more easily obtaining the effects of the present invention, cyclopentene and cyclooctene are more preferred, and cyclopentene is particularly preferred.
[0033] The content ratio of the structural units derived from monocyclic olefins to the total repeating structural units in the ring-opening copolymer of the present invention is not particularly limited, but is preferably 4.92 to 94.995 mol%, more preferably 9.925 to 89.99 mol%, further preferably 14.93 to 84.98 mol%, and particularly preferably 19.935 to 79.97 mol%. By setting the content ratio of the structural units derived from monocyclic olefins within the above range, the abrasion resistance of the cross-linked rubber can be further improved.
[0034] The monomer capable of forming a branched structure for forming the branched structural unit in the present invention is preferably at least one selected from the group consisting of a polycyclic diolefin compound having at least two ring structures each having one double bond, a cyclic olefin compound having a ring structure having one double bond and a vinyl group, and a compound having three or more vinyl groups.
[0035] By introducing a structural unit derived from a polycyclic diolefin compound having at least two ring structures each having one double bond (hereinafter, appropriately referred to as a "polycyclic diolefin compound") as a branched structural unit, a four-branched structure originating from such a structural unit can be introduced into the polymer chain. Also, by introducing a structural unit derived from a cyclic olefin compound having a ring structure each having one double bond and a vinyl group (hereinafter, appropriately referred to as a "vinyl group-containing cyclic olefin compound") as a branched structural unit, a three-branched structure originating from such a structural unit can be introduced into the polymer chain. Also, by introducing a structural unit derived from a compound having three or more vinyl groups as a branched structural unit, a three or more branched structure originating from such a structural unit can be introduced into the polymer chain.
[0036] The polycyclic diolefin compound for forming the structural unit derived from the polycyclic diolefin compound is not particularly limited, but includes a compound represented by the following general formula (2) and compounds represented by the following formulas (3) to (6). [ka] In the above general formula (2), R 5 , R 6 is an alkylene group having 1 to 6 carbon atoms, n is an integer of 0 to 2, and in the above general formula (2), a hydrogen atom may be substituted with an alkyl group having 1 to 6 carbon atoms. Furthermore, the compound represented by the above general formula (2) gives a branched structural unit represented by the above general formula (2a) when it is subjected to ring-opening copolymerization with a norbornene compound or a monocyclic olefin. In the above general formula (2a), R 5 , R 6 n is the same as in the above general formula (2), and in the above general formula (2a), the hydrogen atom may be substituted with an alkyl group having 1 to 6 carbon atoms. [ka] In the above formulas (3) to (6), the hydrogen atoms may be substituted with an alkyl group having 1 to 6 carbon atoms. Furthermore, when the compounds represented by the above formulas (3) to (6) are ring-opening copolymerized with a norbornene compound or a monocyclic olefin, they give branched structural units represented by the above formulas (3a) to (6a), respectively, and in the above formulas (3a) to (6a), the hydrogen atoms may be substituted with an alkyl group having 1 to 6 carbon atoms.
[0037] Specific examples of the compound represented by the above general formula (2) include compounds represented by the following formulas (7) to (10). [ka] In the above formulas (7) to (10), the hydrogen atoms may be substituted with an alkyl group having 1 to 6 carbon atoms. Furthermore, the compounds represented by the above formulas (7) to (10), when subjected to ring-opening copolymerization with a norbornene compound or a monocyclic olefin, give branched structural units represented by the above formulas (7a) to (10a), respectively, and in the above formulas (7a) to (10a), the hydrogen atoms may be substituted with an alkyl group having 1 to 6 carbon atoms.
[0038] Among the above compounds, it is preferable to use the compound represented by the above formula (4), (7) or (8) because it is possible to form a branched structure more appropriately. That is, it is preferable that the ring-opening copolymer of the present invention has, as a branched structural unit, a branched structural unit represented by the above formula (4a), (7a) or (8a).
[0039] In addition, the vinyl group-containing cyclic olefin compound for forming the structural unit derived from the vinyl group-containing cyclic olefin compound is not particularly limited, but includes monocyclic olefins having a vinyl group such as 4-vinylcyclopentene and 5-vinylcyclooctene; norbornenes having a vinyl group such as 5-vinyl-2-norbornene, 5-propenyl-2-norbornene, and 5-styryl-2-norbornene; and the like. These compounds may have hydrogen atoms substituted with alkyl groups having 1 to 6 carbon atoms. Among these, 5-vinyl-2-norbornene (including those having hydrogen atoms substituted with alkyl groups having 1 to 6 carbon atoms) represented by the following formula (11) is preferred from the viewpoint of more appropriately forming a branched structure. [ka] In the above formula (11), the hydrogen atom may be substituted with an alkyl group having 1 to 6 carbon atoms. Furthermore, the compound represented by the above formula (11) gives a branched structural unit represented by the above formula (11a) when it is subjected to ring-opening copolymerization with a norbornene compound or a monocyclic olefin, and in the above formula (11a), the hydrogen atom may be substituted with an alkyl group having 1 to 6 carbon atoms.
[0040] In addition, examples of compounds having three or more vinyl groups for forming a structural unit derived from a compound having three or more vinyl groups include compounds having three vinyl groups, such as 1,2,4-trivinylcyclohexane and 1,3,5-trivinylcyclohexane, and compounds having four or more vinyl groups, such as divinylbenzene oligomer and 1,2-polybutadiene oligomer.
[0041] The content ratio of the branched structural unit in the ring-opening copolymer of the present invention is 0.005 mol% or more, preferably 0.01 mol% or more, more preferably 0.02 mol% or more, even more preferably 0.03 mol% or more, and even more preferably 0.034 mol% or more, with the upper limit being 0.08 mol% or less, preferably 0.075 mol% or less, more preferably 0.07 mol% or less, and even more preferably 0.065 mol% or less. If the content ratio of the branched structural unit is too high, the obtained ring-opening copolymer will gel significantly, and it will be difficult to compound various compounding agents to make a rubber composition. If the content ratio of the branched structural unit is too low, the obtained ring-opening copolymer will have poor wear resistance when made into a rubber cross-linked product.
[0042] The ring-opened copolymer of the present invention may be a copolymer of the norbornene compound represented by the above general formula (1), the monocyclic olefin, and the monomer capable of forming a branched structure, as well as other monomers copolymerizable therewith. Examples of such other monomers include polycyclic cycloolefins having aromatic rings. Examples of polycyclic cycloolefins having aromatic rings include phenylcyclooctene, 5-phenyl-1,5-cyclooctadiene, and phenylcyclopentene. The content ratio of structural units derived from other monomers to the total repeating structural units in the ring-opened copolymer of the present invention is preferably 10 mol% or less, more preferably 5 mol% or less, and in the present invention, it is particularly preferable that the copolymer does not substantially contain structural units derived from other monomers.
[0043] The weight average molecular weight (Mw) of the ring-opening copolymer of the present invention is not particularly limited, but is preferably 100,000 to 1,000,000, more preferably 120,000 to 800,000, even more preferably 120,000 to 600,000, and particularly preferably 150,000 to 400,000, as a value of the weight average molecular weight (Mw) in terms of polystyrene measured by gel permeation chromatography. When the ring-opening copolymer of the present invention has such a molecular weight, the abrasion resistance of the cross-linked rubber can be made more excellent. In addition, the ratio (Mw / Mn) of the weight average molecular weight (Mw) to the number average molecular weight (Mn) in terms of polystyrene measured by gel permeation chromatography of the ring-opening copolymer of the present invention is not particularly limited, but is preferably 1.0 to 5.0, more preferably 1.5 to 3.0.
[0044] The ring-opening copolymer of the present invention may also have a modified group at the polymer chain end. By having such a modified end group, it is possible to further increase the affinity for silica, which may increase the dispersibility of silica in the rubber composition when silica is blended, and as a result, it may be possible to further increase the abrasion resistance when the rubber is cross-linked. The modified group to be introduced at the polymer chain end is not particularly limited, but is preferably a modified group containing an atom selected from the group consisting of an atom of Group 15 of the periodic table, an atom of Group 16 of the periodic table, and a silicon atom.
[0045] As the modifying group for forming the terminal modified group, from the viewpoint of being able to increase the affinity for silica and thereby to improve the abrasion resistance when made into a cross-linked rubber product, a modifying group containing an atom selected from the group consisting of a nitrogen atom, an oxygen atom, a phosphorus atom, a sulfur atom, and a silicon atom is more preferable, and among these, a modifying group containing an atom selected from the group consisting of a nitrogen atom, an oxygen atom, and a silicon atom is even more preferable.
[0046] Examples of the modified group containing a nitrogen atom include an amino group, a pyridyl group, an imino group, an amide group, a nitro group, a urethane bond group, or a hydrocarbon group containing any of these groups. Examples of the modified group containing an oxygen atom include a hydroxyl group, a carboxylic acid group, an ether group, an ester group, a carbonyl group, an aldehyde group, an epoxy group, or a hydrocarbon group containing any of these groups. Examples of the modified group containing a silicon atom include an alkylsilyl group, an oxysilyl group, or a hydrocarbon group containing any of these groups. Examples of the modified group containing a phosphorus atom include a phosphoric acid group, a phosphino group, or a hydrocarbon group containing any of these groups. Examples of the modified group containing a sulfur atom include a sulfonyl group, a thiol group, a thioether group, or a hydrocarbon group containing any of these groups. In addition, the modified group may be a modified group containing a plurality of the above groups. Among these, specific examples of particularly suitable modified groups from the viewpoint of further improving the abrasion resistance when made into a cross-linked rubber product include amino groups, pyridyl groups, imino groups, amide groups, hydroxyl groups, carboxylic acid groups, aldehyde groups, epoxy groups, oxysilyl groups, and hydrocarbon groups containing any of these groups, with oxysilyl groups being particularly preferred from the viewpoint of affinity for silica. Note that the oxysilyl group refers to a group having a silicon-oxygen bond.
[0047] Specific examples of the oxysilyl group include an alkoxysilyl group, an aryloxysilyl group, an acyloxy group, an alkylsiloxysilyl group, and an arylsiloxysilyl group. In addition, a hydroxysilyl group obtained by hydrolyzing an alkoxysilyl group, an aryloxysilyl group, or an acyloxy group can be mentioned. Among these, an alkoxysilyl group is preferred from the viewpoint of affinity to silica.
[0048] An alkoxysilyl group is a group in which one or more alkoxy groups are bonded to a silicon atom, and specific examples include a trimethoxysilyl group, a (dimethoxy)(methyl)silyl group, a (methoxy)(dimethyl)silyl group, a (methoxy)(dichloro)silyl group, a triethoxysilyl group, a (diethoxy)(methyl)silyl group, a (ethoxy)(dimethyl)silyl group, a (dimethoxy)(ethoxy)silyl group, a (methoxy)(diethoxy)silyl group, and a tripropoxysilyl group.
[0049] An aryloxysilyl group is a group in which one or more aryloxy groups are bonded to a silicon atom, and specific examples thereof include a triphenoxysilyl group, a (diphenoxy)(methyl)silyl group, a (phenoxy)(dimethyl)silyl group, a (diphenoxy)(ethoxy)silyl group, a (phenoxy)(diethoxy)silyl group, etc. Among these, the (diphenoxy)(ethoxy)silyl group and the (phenoxy)(diethoxy)silyl group have an alkoxy group in addition to an aryloxy group, and therefore are also classified as alkoxysilyl groups.
[0050] The acyloxysilyl group is a group in which one or more acyloxy groups are bonded to a silicon atom, and specific examples thereof include a triacyloxysilyl group, a (diacyloxy)(methyl)silyl group, and an (acyloxy)(dimethyl)silyl group.
[0051] An alkylsiloxysilyl group is a group in which one or more alkylsiloxy groups are bonded to a silicon atom, and specific examples include a tris(trimethylsiloxy)silyl group, a trimethylsiloxy(dimethyl)silyl group, a triethylsiloxy(diethyl)silyl group, and a tris(dimethylsiloxy)silyl group.
[0052] The arylsiloxysilyl group is a group in which one or more arylsiloxy groups are bonded to a silicon atom, and specific examples include a tris(triphenylsiloxy)silyl group, a triphenylsiloxy(dimethyl)silyl group, and a tris(diphenylsiloxy)silyl group.
[0053] A hydroxysilyl group is a group in which one or more hydroxy groups are bonded to a silicon atom, and specific examples include a trihydroxysilyl group, a (dihydroxy)(methyl)silyl group, a (hydroxy)(dimethyl)silyl group, a (dihydroxy)(ethoxy)silyl group, and a (hydroxy)(diethoxy)silyl group. Of these, the (dihydroxy)(ethoxy)silyl group and the (hydroxy)(diethoxy)silyl group have an alkoxy group in addition to a hydroxy group, and therefore are also classified as alkoxysilyl groups.
[0054] The ratio of modified groups introduced into the polymer chain terminals of the ring-opened copolymer of the present invention is not particularly limited, but is preferably 10% or more, more preferably 20% or more, even more preferably 30% or more, and particularly preferably 40% or more, as a percentage of the number of ring-opened copolymer chain terminals into which modified groups have been introduced / the total number of ring-opened copolymer chain terminals. The higher the ratio of modified terminal groups introduced, the higher the affinity for silica can be, and thus the better the abrasion resistance can be obtained when the resulting cross-linked rubber is obtained, which is preferable. The method for measuring the ratio of modified groups introduced into the polymer chain terminals is not particularly limited, but an example of the case where an oxysilyl group is introduced as a modified terminal group is as follows: 1 It can be determined from the peak area ratio corresponding to the oxysilyl group determined by H-NMR spectrum measurement and the number average molecular weight determined by gel permeation chromatography.
[0055] The Mooney viscosity (ML1+4, 100°C) of the ring-opening copolymer of the present invention is preferably 20 to 150, more preferably 22 to 120, and further preferably 25 to 90. By setting the Mooney viscosity within the above range, kneading at room temperature and high temperature can be facilitated, thereby improving processability.
[0056] <Method of producing ring-opened copolymer> The method for producing the ring-opened copolymer of the present invention is not particularly limited, and examples thereof include a method of copolymerizing a norbornene compound represented by the above general formula (1), a monocyclic olefin, and a monomer capable of forming a branched structure in the presence of a ring-opening polymerization catalyst. Among these, a method of ring-opening metathesis polymerization of a norbornene compound represented by the above general formula (1), a monocyclic olefin, and a monomer capable of forming a branched structure is preferred.
[0057] The amount of each monomer in the monomer mixture containing the norbornene compound represented by the above general formula (1), the monocyclic olefin, and the monomer capable of forming a branched structure used in the polymerization may be an amount corresponding to the above-mentioned content ratio. From the viewpoint of more effectively suppressing gelation of the resulting ring-opening copolymer, however, the content ratio of the monomer capable of forming a branched structure in the monomer mixture is preferably 0.01 to 0.045 mol %.
[0058] The ring-opening polymerization catalyst may be any catalyst capable of ring-opening copolymerization of the norbornene compound represented by the above general formula (1), a monocyclic olefin, and a monomer capable of forming a branched structure, and among these, a ruthenium carbene complex is preferred.
[0059] Specific examples of ruthenium carbene complexes include bis(tricyclohexylphosphine)benzylidene ruthenium dichloride, bis(triphenylphosphine)-3,3-diphenylpropenylidene ruthenium dichloride, bis(tricyclohexylphosphine)t-butylvinylidene ruthenium dichloride, dichloro-(3-phenyl-1H-inden-1-ylidene)bis(tricyclohexylphosphine)ruthenium, bis(1,3-diisopropylimidazolin-2-ylidene)benzylidene ruthenium dichloride, and bis(1,3-dicyclohexyl Examples of the ring-opening polymerization catalyst include benzylidene ruthenium dichloride, (1,3-dimesitylimidazolin-2-ylidene) (tricyclohexylphosphine) benzylidene ruthenium dichloride, (1,3-dimesitylimidazolin-2-ylidene) (tricyclohexylphosphine) benzylidene ruthenium dichloride, bis(tricyclohexylphosphine) ethoxymethylidene ruthenium dichloride, and (1,3-dimesitylimidazolin-2-ylidene) (tricyclohexylphosphine) ethoxymethylidene ruthenium dichloride. The ring-opening polymerization catalyst may be used alone or in combination of two or more.
[0060] The amount of the ring-opening polymerization catalyst used, in terms of the molar ratio of (ring-opening polymerization catalyst:monomer used for copolymerization), is usually within the range of 1:500 to 1:2,000,000, preferably 1:700 to 1:1,500,000, and more preferably 1:1,000 to 1:1,000,000.
[0061] The polymerization reaction may be carried out without a solvent or in a solution. When copolymerization is carried out in a solution, the solvent used is not particularly limited as long as it is inert in the polymerization reaction and can dissolve the norbornene compound represented by the above general formula (1), the monocyclic olefin, the polymerization catalyst, etc. used in the copolymerization, but it is preferable to use a hydrocarbon solvent or a halogen-based solvent. Examples of the hydrocarbon solvent include aromatic hydrocarbons such as benzene, toluene, xylene, and ethylbenzene; aliphatic hydrocarbons such as hexane, n-heptane, and n-octane; alicyclic hydrocarbons such as cyclohexane, cyclopentane, and methylcyclohexane; and the like. Examples of the halogen-based solvent include haloalkanes such as dichloromethane and chloroform; aromatic halogens such as chlorobenzene and dichlorobenzene; and the like. These solvents may be used alone or in combination of two or more.
[0062] When the norbornene compound represented by the above general formula (1), a monocyclic olefin, and a monomer capable of forming a branched structure are ring-opening copolymerized, an olefin compound or a diolefin compound may be added to the polymerization reaction system as a molecular weight regulator, if necessary, in order to adjust the molecular weight of the resulting ring-opening copolymer.
[0063] The olefin compound is not particularly limited as long as it is an organic compound having an ethylenically unsaturated bond, and examples thereof include α-olefins such as 1-butene, 1-pentene, 1-hexene, and 1-octene; styrenes such as styrene and vinyl toluene; halogen-containing vinyl compounds such as allyl chloride; vinyl ethers such as ethyl vinyl ether and i-butyl vinyl ether; silicon-containing vinyl compounds such as allyltrimethoxysilane, allyltriethoxysilane, allyltrichlorosilane, and styryltrimethoxysilane; and di-substituted olefins such as 2-butene and 3-hexene.
[0064] Diolefin compounds include non-conjugated diolefins such as 1,4-pentadiene, 1,4-hexadiene, 1,5-hexadiene, 1,6-heptadiene, 2-methyl-1,4-pentadiene, and 2,5-dimethyl-1,5-hexadiene.
[0065] The amount of the olefin compound and diolefin compound used as the molecular weight regulator may be appropriately selected depending on the molecular weight of the ring-opening copolymer to be produced, but is usually in the range of 1 / 100 to 1 / 100,000, preferably 1 / 200 to 1 / 50,000, and more preferably 1 / 500 to 1 / 10,000 in terms of molar ratio to the monomer used in the copolymerization.
[0066] In addition, when the ring-opening copolymer of the present invention has a modifying group at the polymer chain end, it is preferable to use a modifying group-containing olefinically unsaturated hydrocarbon compound as a molecular weight regulator instead of the above-mentioned olefin compound or diolefin compound. By using such a modifying group-containing olefinically unsaturated hydrocarbon compound, the modifying group can be suitably introduced into the polymer chain end of the ring-opening copolymer obtained by copolymerization.
[0067] The olefinic unsaturated hydrocarbon compound containing a modifying group is not particularly limited as long as it is a compound having a modifying group and one olefinic carbon-carbon double bond having metathesis reactivity. For example, when it is desired to introduce an oxysilyl group into the polymer chain end of a ring-opening copolymer, an olefinic unsaturated hydrocarbon containing an oxysilyl group may be present in the polymerization reaction system.
[0068] Examples of such oxysilyl group-containing olefinically unsaturated hydrocarbons include alkoxysilane compounds such as vinyl(trimethoxy)silane, vinyl(triethoxy)silane, allyl(trimethoxy)silane, allyl(methoxy)(dimethyl)silane, allyl(triethoxy)silane, allyl(ethoxy)(dimethyl)silane, styryl(trimethoxy)silane, styryl(triethoxy)silane, styrylethyl(triethoxy)silane, allyl(triethoxysilylmethyl)ether, and allyl(triethoxysilylmethyl)(ethyl)amine, which introduce a modifying group only at one end (single end) of the polymer chain of the ring-opening copolymer; aryloxysilane compounds such as allyl(phenoxy)silane and allyl(dimethyl)silane; acyloxysilane compounds such as vinyl(triacetoxy)silane, allyl(triacetoxy)silane, allyl(diacetoxy)methylsilane and allyl(acetoxy)(dimethyl)silane; alkylsiloxysilane compounds such as allyltris(trimethylsiloxy)silane; arylsiloxysilane compounds such as allyltris(triphenylsiloxy)silane; polysiloxane compounds such as 1-allylheptamethyltrisiloxane, 1-allylnonamethyltetrasiloxane, 1-allylnonamethylcyclopentasiloxane and 1-allylundecamethylcyclohexasiloxane; and the like.
[0069] In addition, examples of compounds for introducing modifying groups into both ends (both ends) of the polymer chain of the ring-opening copolymer include alkoxysilane compounds such as bis(trimethoxysilyl)ethylene, bis(triethoxysilyl)ethylene, 2-butene-1,4-di(trimethoxysilane), 2-butene-1,4-di(triethoxysilane), and 1,4-di(trimethoxysilylmethoxy)-2-butene; aryloxysilane compounds such as 2-butene-1,4-di(triphenoxysilane); and 2-butene-1,4-di(triphenylsilane). ,4-di(triacetoxysilane); alkylsiloxysilane compounds such as 2-butene-1,4-di[tris(trimethylsiloxy)silane]; arylsiloxysilane compounds such as 2-butene-1,4-di[tris(triphenylsiloxy)silane]; polysiloxane compounds such as 2-butene-1,4-di(heptamethyltrisiloxane) and 2-butene-1,4-di(undecamethylcyclohexasiloxane); and the like.
[0070] The modifying group-containing olefinically unsaturated hydrocarbon compound, such as an oxysilyl group-containing olefinically unsaturated hydrocarbon compound, acts as a molecular weight regulator in addition to the function of introducing a modifying group into the polymer chain terminal of the ring-opening copolymer, so the amount of the modifying group-containing olefinically unsaturated hydrocarbon compound used may be appropriately selected depending on the molecular weight of the ring-opening copolymer to be produced, but is usually in the range of 1 / 100 to 1 / 100,000, preferably 1 / 200 to 1 / 50,000, and more preferably 1 / 500 to 1 / 10,000 in terms of molar ratio to the monomer used in copolymerization.
[0071] The polymerization reaction temperature is not particularly limited, but is preferably -100°C or higher, more preferably -50°C or higher, even more preferably 0°C or higher, and particularly preferably 15°C or higher. The upper limit of the polymerization reaction temperature is not particularly limited, but is preferably less than 120°C, more preferably less than 100°C, even more preferably less than 90°C, and particularly preferably less than 80°C. The polymerization reaction time is also not particularly limited, but is preferably 1 minute to 72 hours, and more preferably 10 minutes to 20 hours.
[0072] If desired, an antiaging agent such as a phenol-based stabilizer, a phosphorus-based stabilizer, or a sulfur-based stabilizer may be added to the ring-opening copolymer obtained by the polymerization reaction. The amount of the antiaging agent to be added may be appropriately determined depending on the type of the agent. Furthermore, if desired, an extender oil may be added. When the ring-opening copolymer is obtained as a polymerization solution, a known recovery method may be adopted to recover the ring-opening copolymer from the polymerization solution. For example, a method of separating the solvent by steam stripping or the like, filtering off the solid, and drying the solid to obtain a solid ring-opening copolymer may be adopted.
[0073] <Rubber composition> In the rubber composition of the present invention, the above-mentioned ring-opened copolymer of the present invention can be blended with required amounts of compounding agents such as a crosslinking agent, a crosslinking accelerator, a crosslinking activator, a filler other than silica, an antiaging agent, an activator, a process oil, a plasticizer, and a lubricant according to a conventional method.
[0074] Examples of the crosslinking agent include powdered sulfur, precipitated sulfur, colloidal sulfur, insoluble sulfur, and highly dispersible sulfur; halogenated sulfur such as sulfur monochloride and sulfur dichloride; organic peroxides such as dicumyl peroxide and ditertiary butyl peroxide; quinone dioximes such as p-quinone dioxime and p,p'-dibenzoylquinone dioxime; organic polyamine compounds such as triethylenetetramine, hexamethylenediamine carbamate, and 4,4'-methylenebis-o-chloroaniline; and alkylphenol resins having methylol groups. Among these, sulfur is preferred, and powdered sulfur is more preferred. These crosslinking agents are used alone or in combination of two or more. The amount of the crosslinking agent is preferably 0.1 to 15 parts by weight, more preferably 0.5 to 5 parts by weight, based on 100 parts by weight of the rubber component in the rubber composition.
[0075] Examples of the crosslinking accelerator include sulfenamide-based crosslinking accelerators such as N-cyclohexyl-2-benzothiazolylsulfenamide, Nt-butyl-2-benzothiazolylsulfenamide, N-oxyethylene-2-benzothiazolylsulfenamide, N-oxyethylene-2-benzothiazolylsulfenamide, and N,N'-diisopropyl-2-benzothiazolylsulfenamide; guanidine-based crosslinking accelerators such as 1,3-diphenylguanidine, 1,3-diorthotolylguanidine, and 1-orthotolylbiguanidine; and thiourea, etc. Examples of the crosslinking accelerator include urea-based crosslinking accelerators; thiazole-based crosslinking accelerators such as 2-mercaptobenzothiazole, di-2-benzothiazyl disulfide, and zinc salt of 2-mercaptobenzothiazole; thiuram-based crosslinking accelerators such as tetramethylthiuram monosulfide and tetramethylthiuram disulfide; dithiocarbamic acid-based crosslinking accelerators such as sodium dimethyldithiocarbamate and zinc diethyldithiocarbamate; xanthic acid-based crosslinking accelerators such as sodium isopropylxanthate, zinc isopropylxanthate, and zinc butylxanthate. Among these, those containing a guanidine-based crosslinking accelerator and / or a thiazole-based crosslinking accelerator are preferred, and those containing a guanidine-based crosslinking accelerator and a thiazole-based crosslinking accelerator are particularly preferred. These crosslinking accelerators are used alone or in combination of two or more kinds. The amount of the crosslinking accelerator is preferably 0.1 to 15 parts by weight, more preferably 0.5 to 5 parts by weight, based on 100 parts by weight of the rubber component in the rubber composition.
[0076] As the crosslinking activator, for example, higher fatty acid such as stearic acid, zinc oxide, etc. can be used. The compounding amount of the crosslinking activator is appropriately selected, but the compounding amount of the higher fatty acid is preferably 0.05 to 15 parts by weight, more preferably 0.5 to 5 parts by weight, based on 100 parts by weight of the rubber component in the rubber composition, and the compounding amount of the zinc oxide is preferably 0.05 to 10 parts by weight, more preferably 0.5 to 3 parts by weight, based on 100 parts by weight of the rubber component in the rubber composition.
[0077] As the process oil, mineral oil or synthetic oil may be used. As the mineral oil, aromatic oil, naphthenic oil, paraffin oil, etc. are usually used. Other compounding agents include activators such as diethylene glycol, polyethylene glycol, silicone oil, etc.; fillers other than silica such as carbon black, calcium carbonate, talc, clay, etc.; tackifiers such as petroleum resin, coumarone resin, etc.; wax, etc.
[0078] The rubber composition of the present invention may also contain silica. Examples of silica include, but are not limited to, dry process white carbon, wet process white carbon, colloidal silica, and precipitated silica. Carbon-silica dual phase filler in which silica is supported on the surface of carbon black may also be used. Among these, wet process white carbon containing hydrated silicic acid as the main component is preferred. These may be used alone or in combination of two or more.
[0079] Silica has a nitrogen adsorption specific surface area of 50 to 300 m 2 / g is preferable, and 80 to 220m 2 / g is more preferable, and 100 to 170m 2 / g is particularly preferred. When the specific surface area is in this range, the affinity between the ring-opening copolymer and silica is particularly good. The pH of the silica is preferably less than 7, more preferably 5 to 6.9. The nitrogen adsorption specific surface area can be measured by the BET method in accordance with ASTM D3037-81.
[0080] The amount of silica in the rubber composition of the present invention is preferably 1 to 150 parts by weight, more preferably 10 to 120 parts by weight, further preferably 15 to 100 parts by weight, and particularly preferably 20 to 80 parts by weight, based on 100 parts by weight of the rubber component containing the ring-opened copolymer of the present invention in the rubber composition. By setting the amount of silica in the above range, the abrasion resistance of the obtained cross-linked rubber product can be more appropriately improved.
[0081] In the rubber composition of the present invention, it is preferable to further compound a silane coupling agent for the purpose of further improving the affinity between the ring-opening copolymer and silica. Examples of the silane coupling agent include vinyltriethoxysilane, β-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, N-(β-aminoethyl)-γ-aminopropyltrimethoxysilane, bis(3-(triethoxysilyl)propyl)tetrasulfide, bis(3-(triethoxysilyl)propyl)disulfide, and tetrasulfides such as γ-trimethoxysilylpropyldimethylthiocarbamyltetrasulfide and γ-trimethoxysilylpropylbenzothiazyltetrasulfide described in JP-A-6-248116. Among them, tetrasulfides are preferable. These silane coupling agents can be used alone or in combination of two or more kinds. The amount of the silane coupling agent is preferably 0.1 to 30 parts by weight, more preferably 1 to 15 parts by weight, based on 100 parts by weight of silica.
[0082] The rubber composition of the present invention may contain, as a rubber component, a rubber other than the above-mentioned ring-opened copolymer of the present invention. Examples of rubbers other than the ring-opening copolymer of the present invention include natural rubber (NR), polyisoprene rubber (IR), emulsion polymerization SBR (styrene-butadiene copolymer rubber), solution polymerization random SBR (bound styrene 5 to 50% by weight, 1,2-bond content of butadiene portion 10 to 80%), high trans SBR (trans bond content of butadiene portion 70 to 95%), low cis BR (polybutadiene rubber), high cis BR, high trans BR (trans bond content of butadiene portion 70 to 95%), styrene-isoprene copolymer rubber, butadiene-isoprene copolymer rubber, emulsion polymerization styrene-acrylonitrile-butadiene copolymer rubber, acrylonitrile-butadiene copolymer rubber, high vinyl SBR-low vinyl SBR block copolymer rubber, polyisoprene-SBR block copolymer rubber, polystyrene-polybutadiene-polystyrene block copolymer, acrylic rubber, epichlorohydrin rubber, fluororubber, silicone rubber, ethylene-propylene rubber, and urethane rubber. Of these, NR, BR, IR and SBR are preferably used. These rubbers may be used alone or in combination of two or more.
[0083] The content of the ring-opening copolymer in the rubber composition of the present invention is preferably 5% by weight or more, more preferably 10% by weight or more, and particularly preferably 20% by weight or more, based on the total amount of the rubber components. If this content is too low, the effect of improving the abrasion resistance may not be obtained.
[0084] The rubber composition of the present invention can be obtained by kneading each component according to a conventional method. For example, the compounding ingredients other than the crosslinking agent and the crosslinking accelerator are kneaded with a rubber component such as a ring-opening copolymer, and then the kneaded mixture is mixed with the crosslinking agent and the crosslinking accelerator to obtain a rubber composition. The kneading temperature of the compounding ingredients other than the crosslinking agent and the crosslinking accelerator with the rubber component such as a ring-opening copolymer is preferably 80 to 200°C, more preferably 120 to 180°C, and the kneading time is preferably 30 seconds to 30 minutes. The mixing of the crosslinking agent and the crosslinking accelerator is usually performed after cooling to 100°C or less, preferably 80°C or less.
[0085] <Rubber cross-linked products> The cross-linked rubber product of the present invention is obtained by cross-linking the above-mentioned rubber composition of the present invention. The cross-linked rubber product of the present invention can be produced by using the rubber composition of the present invention, for example, molding the rubber composition into a desired shape using a molding machine such as an extruder, an injection molding machine, a compressor, or a roll, and then heating the composition to cause a cross-linking reaction and fix the shape as a cross-linked product. In this case, the cross-linking may be carried out after molding in advance or simultaneously with molding. The molding temperature is usually 10 to 200°C, preferably 25 to 120°C. The cross-linking temperature is usually 100 to 200°C, preferably 130 to 190°C, and the cross-linking time is usually 1 minute to 24 hours, preferably 2 minutes to 12 hours, and particularly preferably 3 minutes to 6 hours.
[0086] Depending on the shape, size, etc. of the cross-linked rubber product, even if the surface is cross-linked, the inside may not be sufficiently cross-linked, so secondary cross-linking may be performed by further heating.
[0087] The heating method may be appropriately selected from among methods commonly used for crosslinking rubber, such as press heating, steam heating, oven heating, and hot air heating.
[0088] The cross-linked rubber product of the present invention thus obtained is excellent in abrasion resistance. The molded article of the present invention made of the cross-linked rubber product of the present invention can be used for various applications, such as materials for various tire parts such as cap tread, base tread, carcass, sidewall, and bead parts in tires, materials for hoses, belts, mats, anti-vibration rubber, and various other industrial products, impact resistance improvers for resins, resin film cushioning agents, shoe soles, rubber shoes, golf balls, and toys, by making use of such properties. The molded article made of the cross-linked rubber product of the present invention can be suitably used for various tire parts such as tread, carcass, sidewall, and bead parts in various tires such as all-season tires, high-performance tires, and studless tires. EXAMPLES
[0089] The present invention will be described below in more detail with reference to examples, but the present invention is not limited to these examples. In the following, "parts" are by weight unless otherwise specified. The test methods used in the present examples and comparative examples are as follows. [Weight average molecular weight of ring-opened copolymer] The weight average molecular weight (Mw) of the ring-opening copolymer was determined based on a chart obtained by gel permeation chromatography (GPC) based on the molecular weight in terms of polystyrene. The specific measurement conditions for gel permeation chromatography are as follows: Measuring instrument: HLC-8320 EcoSCE (Tosoh Corporation) Column: Two GMH-HR-H columns (manufactured by Tosoh Corporation) were connected in series. Detector: Differential refractometer RI-8020 (Tosoh Corporation) Eluent: Tetrahydrofuran Column temperature: 40℃
[0090] [Proportion of 2-norbornene-derived structural units and 5-vinyl-2-norbornene-derived structural units in ring-opened copolymer] 1The monomer structure composition ratio in the ring-opened copolymer was determined by H-NMR spectroscopy.
[0091] [Crumb mutual adhesion rate] The ring-opened copolymer as a sample was put into a mixer containing hot water. The ring-opened copolymer as a sample was then cut into pieces by the mixer to form crumbs. Next, the obtained crumb-like ring-opened copolymer and water were put into a container equipped with a stirrer, and stirred at 60°C for 4 hours at a rotation speed of 40 rpm. Next, the crumb-like ring-opened copolymer was sieved using a wire mesh with 20 mm openings, and the crumb mutual adhesion ratio was calculated by the following formula. The lower the value of the crumb mutual adhesion ratio, the less mutual adhesion occurs when the ring-opened copolymer is made into crumbs, and the hot flow property is excellent. Crumb adhesion rate (%) = (weight (g) of crumb-like ring-opening copolymer remaining on the wire mesh) / (total weight (g) of crumb-like ring-opening copolymer) × 100
[0092] [Wear resistance] Test pieces were prepared by press-crosslinking the rubber composition at 160° C. for 20 minutes. The abrasion resistance of the test pieces was measured at 23° C. under a load of 10 N using a DIN abrasion tester (manufactured by Ueshima Seisakusho Co., Ltd.) in accordance with JIS K6264. The measurement results are shown as an index with Comparative Example 1 set at 100, and a larger index value indicates better abrasion resistance.
[0093] Example 1 In a nitrogen atmosphere, 500 g of cyclohexane, 1.49 mol of cyclopentene as a monocyclic olefin, 0.600 mol of 2-norbornene as a norbornene compound, 1.25 mmol of 1-hexene, and 0.428 mmol of 5-vinyl-2-norbornene as a monomer capable of forming a branched structural unit were added to a glass reaction vessel equipped with a stirrer. The content of 5-vinyl-2-norbornene in the monomer mixture was 0.020 mol%. Next, 0.0209 mmol of dichloro-(3-phenyl-1H-inden-1-ylidene)bis(tricyclohexylphosphine)ruthenium(II) dissolved in 5 mL of toluene was added, and the polymerization reaction was carried out at room temperature for 2 hours. After the polymerization reaction, the polymerization was stopped by adding an excess of vinyl ethyl ether.
[0094] The polymerization solution obtained by the polymerization reaction was poured into a large excess of methanol containing 2,6-di-t-butyl-p-cresol (BHT), and the precipitated polymer was collected and washed with methanol, and then vacuum dried at 50°C for 24 hours to obtain a ring-opened copolymer (1). The weight average molecular weight (Mw), the proportion of structural units derived from 2-norbornene, the proportion of structural units derived from 5-vinyl-2-norbornene, and the crumb mutual adhesion rate of this ring-opened copolymer (1) were determined according to the above-mentioned method. The results are shown in Table 1. The obtained ring-opened copolymer (1) did not generate insoluble matter (gel) even when dissolved in tetrahydrofuran. In addition, the ring-opened copolymers obtained in Examples 2 to 6 and Comparative Examples 1, 2, and 4 described later did not generate gel even when dissolved in tetrahydrofuran, similar to the ring-opened copolymer (1) obtained in Example 1.
[0095] 50 parts of the ring-opening copolymer (1) obtained above and 50 parts of natural rubber were masticated in a Banbury mixer having a volume of 250 ml. The masticated mixture of the ring-opening copolymer (1) and natural rubber was mixed with silica (trade name "Zeosil 1165MP", manufactured by Rhodia, nitrogen adsorption specific surface area (BET method): 163 m 260 parts of sucrose (100% sucrose / g), 10 parts of process oil (trade name "Aromax T-DAE", manufactured by JX Nippon Oil & Energy Corporation), and 4.8 parts of a silane coupling agent (bis(3-(triethoxysilyl)propyl)tetrasulfide, trade name "Si69", manufactured by Degussa Co., Ltd.) were added, and the mixture was kneaded for 1.5 minutes at a starting temperature of 110°C. 3.0 parts of zinc oxide (zinc oxide No. 1), 1.0 part of stearic acid (trade name "SA-300", manufactured by ADEKA Co., Ltd.), and 2.0 parts of an antioxidant (N-phenyl-N'-(1,3-dimethylbutyl)-p-phenylenediamine, trade name "Nocrac 6C", manufactured by Ouchi Shinko Chemical Industry Co., Ltd.) were added to the kneaded mixture, and the mixture was kneaded for 2.5 minutes, and the rubber composition was discharged from the Banbury mixer. The temperature of the rubber composition at the end of kneading was 150°C. After cooling to room temperature, the rubber composition was mixed again in a Banbury mixer for 3 minutes, and then discharged from the Banbury mixer. Next, the obtained rubber composition was mixed with 1.1 parts of sulfur, 1.4 parts of a crosslinking accelerator: di-2-benzothiazolyl disulfide (manufactured by Ouchi Shinko Chemical Industry Co., Ltd., product name "Noccela DM"), and 1.4 parts of a crosslinking accelerator: 1,3-di-o-tolyl guanidine (manufactured by Ouchi Shinko Chemical Industry Co., Ltd., product name "Noccela DT") in an open roll at 50°C, and a sheet-shaped rubber composition was obtained. The abrasion resistance of the obtained rubber composition was evaluated according to the above method. The results are shown in Table 1.
[0096] Example 2 Except for changing the amount of 1-hexene used from 1.25 mmol to 1.99 mmol, the same procedure as in Example 1 was carried out to obtain a ring-opened copolymer (2) and evaluate it in the same manner. The results are shown in Table 1.
[0097] Moreover, except that the ring-opened copolymer (2) obtained above was used, a rubber composition was obtained and evaluated in the same manner as in Example 1. The results are shown in Table 1.
[0098] Example 3 A ring-opened copolymer (3) was obtained in the same manner as in Example 1, except that the amount of 5-vinyl-2-norbornene used was changed from 0.428 mmol to 0.266 mmol. The content of 5-vinyl-2-norbornene in the monomer mixture was 0.013 mol%. The obtained ring-opened copolymer (3) was evaluated in the same manner as in Example 1. The results are shown in Table 1.
[0099] Moreover, except for using the ring-opened copolymer (3) obtained above, a rubber composition was obtained in the same manner as in Example 1, and the rubber composition was evaluated in the same manner. The results are shown in Table 1.
[0100] Example 4 A ring-opened copolymer (4) was obtained in the same manner as in Example 1, except that the amount of 5-vinyl-2-norbornene used was changed from 0.428 mmol to 0.759 mmol. The content of 5-vinyl-2-norbornene in the monomer mixture was 0.036 mol%. The obtained ring-opened copolymer (4) was evaluated in the same manner as in Example 1. The results are shown in Table 1.
[0101] Moreover, except for using the ring-opened copolymer (4) obtained above, a rubber composition was obtained in the same manner as in Example 1, and the rubber composition was evaluated in the same manner. The results are shown in Table 1.
[0102] Example 5 The ring-opened copolymer (5) was obtained in the same manner as in Example 1, except that the amount of cyclopentene used was changed to 2.54 mol, the amount of 2-norbornene used to 0.271 mol, and the amount of 1-hexene used to 1.69 mmol. The content of 5-vinyl-2-norbornene in the monomer mixture was 0.015 mol%. The obtained ring-opened copolymer (5) was evaluated in the same manner as in Example 1. The results are shown in Table 1.
[0103] Moreover, except for using the ring-opened copolymer (5) obtained above, a rubber composition was obtained in the same manner as in Example 1, and the rubber composition was evaluated in the same manner. The results are shown in Table 1.
[0104] Example 6 A ring-opened copolymer (6) was obtained in the same manner as in Example 1, except that the amount of cyclopentene used was changed to 0.92 mol, the amount of 2-norbornene used was changed to 0.775 mol, and the amount of 1-hexene used was changed to 1.02 mmol. The content of 5-vinyl-2-norbornene in the monomer mixture was 0.025 mol%. The obtained ring-opened copolymer (6) was evaluated in the same manner as in Example 1. The results are shown in Table 1.
[0105] Moreover, except for using the ring-opened copolymer (6) obtained above, a rubber composition was obtained in the same manner as in Example 1, and the rubber composition was evaluated in the same manner. The results are shown in Table 1.
[0106] Comparative Example 1 Except for not using 5-vinyl-2-norbornene, the same procedure as in Example 1 was repeated to obtain a ring-opened copolymer (7), which was then evaluated in the same manner. The results are shown in Table 1.
[0107] Moreover, except for using the ring-opened copolymer (7) obtained above, a rubber composition was obtained in the same manner as in Example 1, and the rubber composition was evaluated in the same manner. The results are shown in Table 1.
[0108] Comparative Example 2 A ring-opened copolymer (8) was obtained in the same manner as in Comparative Example 1, except that the amount of cyclopentene used was changed to 1.30 mol, the amount of 2-norbornene used was changed to 0.659 mol, and the amount of 1-hexene used was changed to 1.17 mmol. The ring-opened copolymer (8) obtained was evaluated in the same manner as in Example 1. The results are shown in Table 1.
[0109] Moreover, except for using the ring-opened copolymer (8) obtained above, a rubber composition was obtained in the same manner as in Example 1, and the rubber composition was evaluated in the same manner. The results are shown in Table 1.
[0110] Comparative Example 3 A ring-opened copolymer (9) was obtained in the same manner as in Example 1, except that the amount of 5-vinyl-2-norbornene used was changed from 0.428 mmol to 1.042 mmol. The content of 5-vinyl-2-norbornene in the monomer mixture was 0.050 mol %. The obtained ring-opened copolymer (9) was evaluated in the same manner as in Example 1. The results are shown in Table 1.
[0111] When the obtained ring-opened copolymer (9) was dissolved in tetrahydrofuran, an insoluble matter (gel matter) was observed. The gelled ring-opened copolymer (9) could not be cut into small pieces, and could not be made into a crumb-like form. It also could not be mixed uniformly with other components, and therefore a rubber composition could not be formed. Therefore, it was not possible to measure the crumb mutual adhesion rate and the abrasion resistance of the cross-linked rubber of the ring-opened copolymer (9).
[0112] Comparative Example 4 The amount of cyclopentene used was changed to 3.41 mol, the amount of 1-hexene used to 2.05 mmol, the amount of 5-vinyl-2-norbornene used to 0.693 mmol, and the ring-opened copolymer (10) was obtained in the same manner as in Example 1, except that 2-norbornene was not used. The content of 5-vinyl-2-norbornene in the monomer mixture was 0.020 mol%. The obtained ring-opened copolymer (10) was evaluated in the same manner as in Example 1. The results are shown in Table 1.
[0113] Moreover, except for using the ring-opened copolymer (10) obtained above, a rubber composition was obtained in the same manner as in Example 1, and the rubber composition was evaluated in the same manner. The results are shown in Table 1.
[0114] [Table 1]
[0115] From the results shown in Table 1, it was found that the ring-opening copolymers containing structural units derived from the norbornene compound represented by the above general formula (I), structural units derived from a monocyclic olefin, and branched structural units, and having a content ratio of the branched structural units of 0.005 to 0.08 mol % in all repeating structural units in the ring-opening copolymer, were capable of preventing the occurrence of mutual adhesion when made into crumbs, had excellent hot flow properties, and gave cross-linked rubber products with excellent abrasion resistance (Examples 1 to 6). On the other hand, the ring-opening copolymer not containing a branched structural unit was poor in hot flow properties because it was subject to adhesion to each other when it was made into crumbs, and the cross-linked rubber obtained using it was poor in abrasion resistance (Comparative Examples 1 and 2). Furthermore, a ring-opening copolymer having a branched structural unit content of more than 0.08 mol % relative to the total repeating structural units in the ring-opening copolymer is obtained as an insoluble component (gel component) in the polymerization solution, and therefore cannot be uniformly mixed with other components to form a rubber composition (Comparative Example 3). Furthermore, the cross-linked rubber obtained using a ring-opening copolymer not containing a structural unit derived from a norbornene compound represented by the above general formula (I) was inferior in abrasion resistance (Comparative Example 4).
Claims
1. A ring-opening copolymer comprising a structural unit derived from a norbornene compound represented by the following general formula (I), a structural unit derived from a monocyclic cyclic olefin, and a branched structural unit, The ring-opened copolymer has a content of the branched structural unit of 0.005 to 0.08 mol % in all repeating structural units in the ring-opened copolymer. 【Chemistry 12】 (In the above general formula (I), R 1 ~R 4 each independently represents a hydrogen atom, a linear saturated hydrocarbon group having 1 to 20 carbon atoms, or a substituent containing a halogen atom, a silicon atom, an oxygen atom, or a nitrogen atom, and m is 0 or 1.
2. 2. The ring-opened copolymer according to claim 1, wherein the content of the structural unit derived from the norbornene compound in all repeating structural units in the ring-opened copolymer is 5 mol % or more.
3. 3. The ring-opening copolymer according to claim 1, wherein in the general formula (I), m is 0.
4. In the general formula (I), R 1 ~R 4 The ring-opening copolymer according to any one of claims 1 to 3, wherein each of the is independently a hydrogen atom or an alkyl group having 1 to 3 carbon atoms.
5. 5. The ring-opened copolymer according to claim 1, wherein the monocyclic olefin is at least one selected from the group consisting of cyclopentene, cyclohexene, cycloheptene, and cyclooctene.
6. The ring-opening copolymer according to any one of claims 1 to 5, wherein the branched structural unit is a branched structural unit represented by any one of the following formulas (II) to (V): 【Chemistry 13】 (In the above formula (II), the hydrogen atom may be substituted with an alkyl group having 1 to 6 carbon atoms.) 【Chemistry 14】 (In the above formula (III), the hydrogen atom may be substituted with an alkyl group having 1 to 6 carbon atoms.) 【Chemistry 15】 (In the above formula (IV), the hydrogen atom may be substituted with an alkyl group having 1 to 6 carbon atoms.) 【Chemistry 16】 (In the above formula (V), the hydrogen atom may be substituted with an alkyl group having 1 to 6 carbon atoms.)
7. 7. The ring-opening copolymer according to claim 1, having a weight average molecular weight of 150,000 or more and 400,000 or less.
8. A rubber composition comprising the ring-opening copolymer according to any one of claims 1 to 7.
9. The rubber composition according to claim 8, further comprising a crosslinking agent.
10. A cross-linked rubber product obtained by cross-linking the rubber composition according to claim 9.
11. A molded article obtained by molding the rubber composition according to claim 8 or the cross-linked rubber product according to claim 10.
12. A method for producing a ring-opening copolymer by ring-opening metathesis polymerization of a monomer mixture containing a norbornene compound represented by the following general formula (I), a monocyclic olefin, and a monomer capable of forming a branched structure, The method for producing a ring-opening copolymer, wherein the monomer capable of forming a branched structure is at least one selected from the group consisting of a polycyclic diolefin compound having at least two ring structures each having one double bond, a cyclic olefin compound having a ring structure having one double bond and a vinyl group, and a compound having three or more vinyl groups. 【Chemistry 17】 (In the above general formula (I), R 1 ~R 4 each independently represents a hydrogen atom, a linear saturated hydrocarbon group having 1 to 20 carbon atoms, or a substituent containing a halogen atom, a silicon atom, an oxygen atom, or a nitrogen atom, and m is 0 or 1.
13. The method for producing a ring-opening copolymer according to claim 12, wherein the content of the monomer capable of forming a branched structure in the monomer mixture is 0.01 to 0.045 mol %.
Citation Information
Patent Citations
Method for producing cyclopentene ring-opened polymer
JP2011126966A
High-resilience material
JP2019081840A
Cyclopentene ring-opening copolymer, method for producing same, and rubber composition
WO2014133028A1
Rubber composition and rubber crosslinked product
WO2018079602A1