Polyethylene terephthalate resin composition and molded article

A PET resin composition with alkali metal carboxylate, carbon black, glass fiber, and water repellent enhances weather resistance and mechanical properties, addressing the lack of durability in outdoor applications.

JP7556493B2Active Publication Date: 2024-09-26MITSUBISHI CHEM CORP
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2024506401
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2022-03-11
Filing Date
2023-03-09
Publication Date
2024-09-26
Estimated Expiration
2043-03-09

AI Technical Summary

Technical Problem

Existing polyethylene terephthalate (PET) resin compositions lack sufficient weather resistance, which is crucial for outdoor applications exposed to harsh environmental conditions.

Method used

A PET resin composition is developed by blending specific amounts of alkali metal carboxylate, carbon black, glass fiber, and a water repellent, along with a mold release agent and epoxy compound, to enhance weather resistance and mechanical properties.

Benefits of technology

The composition exhibits excellent weather resistance with minimal color change, improved impact resistance, and maintains appearance over time, making it suitable for outdoor use.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007556493000002
    Figure 0007556493000002
  • Figure 0007556493000006
    Figure 0007556493000006
  • Figure 0007556493000001
    Figure 0007556493000001
Patent Text Reader

Abstract

This polyethylene terephthalate resin composition has excellent weather resistance. The polyethylene terephthalate resin composition is characterized by comprising (A) 100 parts by mass of a polyethylene terephthalate resin, (B) 0.1-5 parts by mass of a carboxylic acid alkali metal salt, (C) 0.1-6 parts by mass of carbon black, (D) 55 parts by mass or more of glass fibers, and (E) 0.01-2 parts by mass of a water repellent.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a polyethylene terephthalate resin composition and a molded article, and more particularly to a polyethylene terephthalate resin composition and a molded article having excellent weather resistance. [Background technology]

[0002] Polyethylene terephthalate resin (hereinafter sometimes abbreviated as PET) has excellent mechanical and electrical properties, as well as excellent chemical and heat resistance, and is therefore widely used as a material for manufacturing various electrical and electronic equipment parts, interior and exterior parts for vehicles such as automobiles, trains, and electric trains, and other general industrial products. Furthermore, it is also used in parts that require a good appearance, such as unpainted exterior parts for vehicles, and the range of its use is expanding.

[0003] Exterior parts used outdoors are required to have weather resistance that lasts for a long period of time, such as excellent weather resistance, resistance to fading of the parts, resistance to loss of gloss of the product, resistance to protruding reinforcing fillers on the surface, resistance to changes in appearance, etc. In particular, there is a strong demand for parts using PET to maintain the above-mentioned excellent performance for a long period of time, even when used outdoors where they are exposed to strong sunlight, severe temperature changes, severe wind and rain, etc.

[0004] Patent Document 1 discloses a polyethylene terephthalate (PET) resin composition that has high fluidity and generates little burrs during molding, and is composed of 20 to 80% by weight of polyethylene terephthalate, 60% by weight or less of an inorganic filler, and (C) 0.05 to 10% by weight of a polytetrafluoroethylene resin produced by an emulsion polymerization method. However, the PET resin composition of Patent Document 1 does not fully consider the performance, such as weather resistance, that is strongly required for exterior parts for outdoor use. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Japanese Patent Application Publication No. 5-271521 Summary of the Invention [Problem to be solved by the invention]

[0006] An object of the present invention is to provide a polyethylene terephthalate resin composition having high weather resistance. [Means for solving the problem]

[0007] Means for Solving the Problems The present inventors have conducted intensive research to achieve the above object, and as a result have found that a polyethylene terephthalate resin composition in which a carboxylate alkali metal salt, carbon black, glass fiber, and a water repellent agent are blended with a polyethylene terephthalate resin in specific amounts each has excellent weather resistance over a long period of time, and have arrived at the present invention. The present invention is as follows.

[0008] 1. A polyethylene terephthalate resin composition comprising, relative to 100 parts by mass of (A) polyethylene terephthalate resin, (B) 0.1 to 5 parts by mass of an alkali metal salt of a carboxylate, (C) 0.1 to 6 parts by mass of carbon black, (D) 55 parts by mass or more of glass fiber, and (E) 0.01 to 2 parts by mass of a water repellent agent. 2. The polyethylene terephthalate resin composition according to the above item 1, wherein the mass ratio (E) / (B) of the content of the water repellent agent (E) to the alkali metal carboxylate (B) is 0.2 to 1.3. 3. A polyethylene terephthalate resin composition according to the above 1 or 2, wherein the water repellent (E) has a critical surface tension of 40 mN / m or less. 4. The polyethylene terephthalate resin composition according to any one of the above items 1 to 3, wherein (E) the water repellent is polytetrafluoroethylene. 5. The polyethylene terephthalate resin composition according to any one of the above 1 to 4, wherein (B) the alkali metal carboxylate is sodium carboxylate. 6. The polyethylene terephthalate resin composition according to any one of the above 1 to 4, wherein (B) the alkali metal carboxylate is an alkali metal montanate. 7. The polyethylene terephthalate resin composition according to 5 above, wherein (B) the sodium carboxylate is sodium montanate. 8. The polyethylene terephthalate resin composition according to 6 above, wherein (B) the alkali metal salt of montanic acid is sodium montanate. 9. The polyethylene terephthalate resin composition according to any one of 1 to 8 above, further comprising 0.1 to 3 parts by mass of a release agent per 100 parts by mass of the polyethylene terephthalate resin (A). 10. The polyethylene terephthalate resin composition according to the above item 9, wherein the release agent is a polyolefin compound or an aliphatic carboxylic acid amide. 11. The polyethylene terephthalate resin composition according to the above item 9, wherein the release agent is an aliphatic carboxylic acid amide. 12. (C) Carbon black has a DBP oil absorption of 40-80 cm 3 12. The polyethylene terephthalate resin composition according to any one of 1 to 11 above, wherein the resin composition has a molecular weight of 1 / 100 g. 13. The polyethylene terephthalate resin composition according to any one of 1 to 12 above, further comprising 0.1 to 4 parts by mass of an epoxy compound per 100 parts by mass of the polyethylene terephthalate resin (A). 14. The polyethylene terephthalate resin composition according to the above item 13, wherein the epoxy compound is a bisphenol A type epoxy compound. 15. A molded article of the polyethylene terephthalate resin composition according to any one of 1 to 14 above. 16. The molded article according to the above item 15, wherein the contact angle of the surface of the molded article with water is 80° or more. 17. The molded article according to claim 15 or 16, which is for use as a product for outdoor use. 18. A method for producing a polyethylene terephthalate resin composition according to any one of 1 to 14 above, comprising a step of blending a colorant composition containing (A) polyethylene terephthalate resin and (C) carbon black with (A) polyethylene terephthalate resin. 19. A method for producing a polyethylene terephthalate resin composition according to any one of 1 to 14 above, using an extruder, characterized in that the extruder has two or more vents. Effect of the Invention

[0009] The polyethylene terephthalate resin composition of the present invention has highly excellent weather resistance and exhibits little color change (color difference, ΔE * ) is extremely small, there is no deterioration in appearance due to glass fiber lifting, and the impact resistance is excellent. For these reasons, it is particularly suitable for use as exterior parts for outdoor use. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] The present invention will be described in detail below. The polyethylene terephthalate resin composition of the present invention is characterized by containing, relative to 100 parts by mass of (A) polyethylene terephthalate resin, (B) 0.1 to 5 parts by mass of an alkali metal salt of a carboxylate, (C) 0.1 to 6 parts by mass of carbon black, (D) 55 parts by mass or more of glass fiber, and (E) 0.01 to 2 parts by mass of a water repellent.

[0011] [(A) Polyethylene terephthalate resin] The polyethylene terephthalate resin is a polyethylene terephthalate resin in which the ratio of oxyethyleneoxyterephthaloyl units (hereinafter sometimes referred to as "ET units") consisting of terephthalic acid and ethylene glycol to all constituent repeating units (hereinafter sometimes referred to as "ET ratio") is preferably 90 equivalent % or more, and the polyethylene terephthalate resin in the present invention may contain constituent repeating units other than ET units in the range of less than 10 equivalent %. The polyethylene terephthalate resin is produced using terephthalic acid or its lower alkyl ester and ethylene glycol as the main raw materials, but other acid components and / or other glycol components may also be used together as raw materials.

[0012] Examples of acid components other than terephthalic acid include phthalic acid, isophthalic acid, naphthalenedicarboxylic acid, 4,4'-diphenylsulfonedicarboxylic acid, 4,4'-biphenyldicarboxylic acid, 1,4-cyclohexanedicarboxylic acid, 1,3-phenylenedioxydiacetic acid and structural isomers thereof, dicarboxylic acids such as malonic acid, succinic acid, and adipic acid and derivatives thereof, and oxyacids such as p-hydroxybenzoic acid and glycolic acid and derivatives thereof.

[0013] Examples of diol components other than ethylene glycol include aliphatic glycols such as 1,2-propanediol, 1,3-propanediol, 1,4-butanediol, pentamethylene glycol, hexamethylene glycol, and neopentyl glycol; alicyclic diols such as 1,3-cyclohexanedimethanol, 1,4-cyclohexanedimethanol, 1,2-decahydronaphthalenedimethanol, 1,3-decahydronaphthalenedimethanol, 1,4-decahydronaphthalenedimethanol, 1,5-decahydronaphthalenedimethanol, 1,6-decahydronaphthalenedimethanol, 2,7-decahydronaphthalenedimethanol, tetralin dimethanol, norbornane dimethanol, tricyclodecane dimethanol, and pentacyclododecane dimethanol; and aromatic dihydroxy compound derivatives such as bisphenol A and bisphenol S.

[0014] Examples of copolymerized polyethylene terephthalate resins include ethylene glycol / isophthalic acid / terephthalic acid copolymers (isophthalic acid-copolymerized polyethylene terephthalate).

[0015] The raw material containing the above-mentioned terephthalic acid or its ester-forming derivative and ethylene glycol is subjected to an esterification reaction or an ester exchange reaction in the presence of an esterification catalyst or an ester exchange catalyst to form bis(β-hydroxyethyl) terephthalate and / or an oligomer thereof, which is then subjected to melt polycondensation at high temperature and reduced pressure in the presence of a polycondensation catalyst and a stabilizer to form a polymer.

[0016] The esterification catalyst is not particularly required because terephthalic acid acts as a self-catalyst for the esterification reaction. The esterification reaction can be carried out in the presence of the esterification catalyst and a polycondensation catalyst described later, or in the presence of a small amount of inorganic acid. As the transesterification catalyst, alkali metal salts such as sodium and lithium, alkaline earth metal salts such as magnesium and calcium, and metal compounds such as zinc and manganese are preferably used, and among them, manganese compounds are particularly preferred in terms of the appearance of the resulting polyethylene terephthalate.

[0017] As the polycondensation catalyst, a compound soluble in the reaction system, such as a germanium compound, an antimony compound, a titanium compound, a cobalt compound, a tin compound, or an aluminum compound, is used alone or in combination. As the polycondensation catalyst, an antimony catalyst or an aluminum catalyst is particularly preferred from the viewpoint of color tone and transparency. These polycondensation catalysts may be used in combination with a stabilizer to suppress decomposition reaction during polymerization, and as the stabilizer, one or more of phosphoric acid esters such as trimethyl phosphate, triethyl phosphate, and triphenyl phosphate, phosphoric acid esters such as triphenyl phosphite and trisdodecyl phosphite, methyl acid phosphate, dibutyl phosphate, monobutyl phosphate acid phosphate ester, phosphoric acid, phosphorous acid, hypophosphorous acid, and polyphosphoric acid are preferred.

[0018] The proportion of the catalyst used is usually 1 to 2000 ppm, preferably 3 to 500 ppm, in terms of the mass of the metal in the catalyst in the total polymerization raw materials, and the proportion of the stabilizer used is usually 10 to 1000 ppm, preferably 20 to 200 ppm, in terms of the mass of the phosphorus atom in the stabilizer in the total polymerization raw materials. The catalyst and stabilizer can be supplied at any stage of the esterification reaction or the ester exchange reaction, in addition to when preparing the raw material slurry. They can also be supplied at the beginning of the polycondensation reaction process.

[0019] The intrinsic viscosity (IV) of polyethylene terephthalate resin is usually in the range of 0.3 to 1.5 dl / g, but the polyethylene terephthalate resin (A) used in the present invention preferably has an IV of 0.4 to 1.2 dl / g. If the IV is less than 0.4 dl / g, the strength is likely to decrease, and if it exceeds 1.2 dl / g, the fluidity is likely to be insufficient. The IV is more preferably 0.45 to 1.0 dl / g, and even more preferably 0.5 to 0.9 dl / g. The intrinsic viscosity of the polyethylene terephthalate resin is a value measured at 30° C. in a mixed solvent of tetrachloroethane and phenol in a 1:1 (mass ratio).

[0020] [(B) Alkali metal carboxylate] Examples of the carboxylic acid of the alkali metal carboxylate include saturated aliphatic carboxylic acid, unsaturated aliphatic carboxylic acid, aromatic carboxylic acid, chain carboxylic acid, cyclic carboxylic acid, etc. Among them, saturated aliphatic carboxylic acid or aromatic carboxylic acid is preferred because it has a high effect as a crystal nucleating agent. Examples of the saturated aliphatic carboxylic acid or aromatic carboxylic acid include montanic acid, behenic acid, stearic acid, benzoic acid, etc. Among them, montanic acid is preferred because it has a high effect as a crystal nucleating agent, and the molded product made of the polyethylene terephthalate resin composition has a good appearance and high impact strength. Examples of the alkali metal include sodium, lithium, potassium, etc. Among them, sodium is preferred because it is highly effective as a crystal nucleating agent. As the alkali metal carboxylate, sodium carboxylate is preferred because it has a high effect of increasing the crystallization temperature and tends to improve basic physical properties, and sodium montanate is further preferred because it improves the appearance of the molded product and also increases the impact strength.

[0021] The crystallization temperature of the alkali metal carboxylate of the present invention is preferably 100°C or higher, more preferably 130°C or higher, even more preferably 170°C or higher, and particularly preferably 210°C or higher since the effect as a crystal nucleating agent is enhanced. The crystallization temperature is preferably 300°C or lower, more preferably 250°C or lower, and is preferably 230°C or lower since the appearance of the molded product is good. The crystallization temperature can be measured using a differential scanning calorimeter (DSC) based on JIS K7121. Specifically, the temperature is raised from 40°C to 300°C at a heating rate of 20°C / min in a nitrogen atmosphere, and then held at 300°C for 3 minutes, and then cooled to 40°C at a cooling rate of -20°C / min, and the temperature of the maximum peak due to crystallization during heating can be determined as the crystallization temperature Tc. The differential scanning calorimeter "DSC7020" manufactured by Hitachi High-Tech Science Corporation can be used.

[0022] The content of (B) alkali metal carboxylate is 0.1 to 5 parts by mass relative to 100 parts by mass of (A) polyethylene terephthalate resin. By including it in such a range, the strength can be improved. The content is preferably 0.2 parts by mass or more, more preferably 0.3 parts by mass or more, and preferably 4 parts by mass or less, further preferably 3 parts by mass or less, among which 2 parts by mass or less, among which 1.5 parts by mass or less, 1 part by mass or less, 0.8 parts by mass or less, 0.6 parts by mass or less, and particularly preferably 0.5 parts by mass or less.

[0023] [(C) Carbon Black] The polyethylene terephthalate resin composition of the present invention contains carbon black. By containing carbon black, the weather resistance and appearance of the polyethylene terephthalate resin composition and the molded article are improved.

[0024] The carbon black is not limited in type, raw material type, or manufacturing method, and any of furnace black, channel black, acetylene black, ketjen black, etc. can be used. There is no particular limit to the number average particle size, but it is preferably 5 to 60 nm. By using carbon black having a number average particle size in a predetermined range, a composition that is less likely to cause blisters at high temperatures can be obtained. The number average particle size can be determined by obtaining a magnified image of an aggregate according to the procedure described in the ASTM D3849 standard (Standard Test Method for Carbon Black - Morphological Characterization by Electron Microscopy), measuring the particle sizes of 3,000 unit constituent particles from this aggregate image, and taking the arithmetic average.

[0025] The nitrogen adsorption specific surface area of ​​carbon black (unit: m 2 / g) is usually 1000m 2 / g or less is preferable, and 50 to 400m 2 / g. The nitrogen adsorption specific surface area is preferably 1000 m 2 By making the molecular weight less than 1 / g, the flowability of the polyethylene terephthalate resin composition and the appearance of the molded article tend to be improved, which is preferable. The nitrogen adsorption specific surface area can be measured in accordance with JIS K6217. In addition, the DBP (dibutyl phthalate) oil absorption of carbon black is 300 cm 3 / 100g or less is preferable, and 30 to 200cm 3 / 100g is preferable, and 40 to 80cm 3 More preferably, the DBP absorption is 300 cm 3 By adjusting the molecular weight to less than 100 g / 100 g, the flowability of the polyethylene terephthalate resin composition of the present invention and the appearance of the molded article tend to be improved, which is preferable. The DBP absorption amount (unit: cm 3 / 100g) can be measured in accordance with JIS K6217. The pH of the carbon black used is not particularly limited, but is usually 2-10, preferably 3-9, and more preferably 4-8.

[0026] Carbon black can be used alone or in combination of two or more kinds. Carbon black can also be granulated using a binder, and can also be used as a masterbatch in which carbon black is melt-kneaded at a high concentration in other resins. By using a melt-kneaded masterbatch, it is possible to achieve improved handling during extrusion, improved dispersibility in the resin composition, improved weather resistance, and improved basic physical properties. Examples of the resin include polystyrene resins, polyester resins, acrylic resins, and polyolefin resins, among which polyester resins are preferred, and polyethylene terephthalate resins are the most preferred. The content of carbon black in the masterbatch is preferably from 10 to 80% by mass, more preferably from 20 to 70% by mass, and further preferably from 25 to 50% by mass.

[0027] The carbon black content is 0.01 to 6 parts by mass relative to 100 parts by mass of the polyethylene terephthalate resin (A). By including the carbon black in such an amount, discoloration after a weathering test is suppressed and the appearance is improved. The content is preferably 0.1 parts by mass or more, more preferably 0.3 parts by mass or more, of which 0.5 parts by mass or more, and particularly preferably 0.7 parts by mass or more, and is preferably 5 parts by mass or less, more preferably 3 parts by mass or less, of which 1.5 parts by mass or less, and particularly preferably 1 part by mass or less.

[0028] [(D) Glass fiber] The polyethylene terephthalate resin composition of the present invention contains glass fibers. Any known glass fiber can be used as the glass fiber, regardless of the form of the glass fiber when blended, such as A glass, E glass, alkali-resistant glass composition containing a zirconia component, chopped strand, roving glass, (long fiber) master batch of thermoplastic resin and glass fiber, etc. Among them, alkali-free glass (E glass) is preferable as the glass fiber used in the present invention, for the purpose of improving the thermal stability of the polyethylene terephthalate resin composition of the present invention.

[0029] The number average fiber length of the glass fibers is preferably 1 mm or more and 10 mm or less, more preferably 1.5 to 6 mm, and even more preferably 2 to 5 mm. If the number average fiber length exceeds 10 mm, the glass fibers are likely to fall off from the surface of the molded product, which tends to reduce productivity.If the number average fiber length is less than 1 mm, the aspect ratio of the glass fibers is small, which tends to result in insufficient improvement in mechanical strength.

[0030] The diameter of the glass fiber is preferably 3 to 20 μm. These can be produced by grinding a strand of glass fiber according to any conventionally known method, specifically, for example, with a hammer mill or a ball mill. When the diameter of the glass fiber is less than 3 μm, the improvement in mechanical strength is similarly insufficient, and when it exceeds 20 μm, the appearance is likely to deteriorate. The diameter of the glass fiber is more preferably 5 to 15 μm, and further preferably 6 to 14 μm.

[0031] The glass fibers may be surface-treated with a silane coupling agent such as aminosilane or epoxysilane in order to improve adhesion to the polyethylene terephthalate resin.

[0032] In addition, glass fibers are preferably used as chopped strands (chopped glass fibers) made by bundling a large number of these fibers and cutting them to a specified length, and the glass fibers used in this case are preferably blended with a sizing agent. Blending with a sizing agent has the advantage of increasing the production stability of molded products, as well as providing good mechanical properties. The sizing agent is not particularly limited, and examples thereof include urethane-based, epoxy-based, acrylic-based, etc. Among them, urethane-based and epoxy-based sizing agents are more preferable, and epoxy-based sizing agents are even more preferable.

[0033] The cut length of the chopped strands (chopped glass fibers) is not particularly limited, but is usually 1 to 10 mm, preferably 1.5 to 6 mm, and more preferably 2 to 5 mm.

[0034] The glass fibers may have a cross section that is substantially circular, specifically, a nearly circular cross section with a flattening ratio (major axis / minor axis) of the cross section of the fiber of 1 or more and less than 1.5. In this case, the flattening ratio is preferably 1 to 1.4, more preferably 1 to 1.2, and particularly preferably 1 to 1.1.

[0035] In addition, from the viewpoint of fluidity, it is also preferable that the glass fiber has a flat cross-sectional shape. Specifically, there can be mentioned flat cross-sectional glass fibers having an average major axis value of 10 to 50 μm and an average ratio of major axis to minor axis (major axis / minor axis) of 1.5 or more and 8 or less.

[0036] As the glass fiber, milled glass fiber is also preferable, and more specifically, milled glass fiber is a glass fiber strand in which several tens to several thousands of single glass fibers (filaments) are bundled, and the strand is cut to a predetermined length to produce chopped glass fiber strands, which are then crushed. In this case, the chopped glass fiber strands are preferably surface-treated with a sizing agent as described above.

[0037] The milled glass fiber is preferably a short fiber having a ratio of the average fiber length to the average fiber diameter (aspect ratio) of 10 or less. The aspect ratio of the milled glass fiber is preferably 8 or less, more preferably 7 or less, and preferably 2.5 or more, more preferably 3 or more. When the aspect ratio exceeds 10, warping and anisotropy become large, and the appearance of the molded product tends to deteriorate. The milled glass fiber has a number average fiber diameter of preferably 1 to 25 μm, more preferably 5 to 17 μm, and an average length of preferably 1 to 500 μm, more preferably 10 to 300 μm, and even more preferably 20 to 200 μm. Short milled glass fibers having an average fiber diameter of less than 1 μm tend to impair moldability, while those having an average fiber diameter of more than 25 μm tend to impair appearance and have insufficient reinforcing effect.

[0038] The preferred content of glass fiber is 55 parts by mass or more relative to 100 parts by mass of (A) polyethylene terephthalate resin. By including 55 parts by mass or more, strength can be improved. The content of glass fiber is preferably 60 parts by mass or more, more preferably 70 parts by mass or more, and particularly preferably 80 parts by mass or more, and is preferably 150 parts by mass or less, particularly preferably 140 parts by mass or less, 130 parts by mass or less, 120 parts by mass or less, 110 parts by mass or less, and particularly preferably 100 parts by mass or less.

[0039] [(E) Water repellent] The polyethylene terephthalate resin composition of the present invention contains a water repellent (E). The inclusion of a water repellent having a critical surface tension of 40 mN / m or less as the water repellent is preferable because it further improves weather resistance. It has been found that the lower the critical surface tension, the better the water repellency of the water repellent, and the better the weather resistance of the polyethylene terephthalate resin composition containing it.

[0040] In general, the surface tension of a liquid that, when dropped onto the surface of an object, results in a contact angle θ (the angle that a droplet makes at the interface with the surface of the object) of θ = 0° is called the critical surface tension of the object. Therefore, the critical surface tension of a water repellent is the surface tension of a liquid that, when dropped onto the surface of a molded product made from the water repellent, results in a contact angle θ of 0°. The molded product may be in the form of a film. For example, the molded body is allowed to stand for 24 hours in a temperature-controlled room at a temperature of 23°C and a humidity of 60% RH to adjust its condition, and then the contact angle θ is measured with a contact angle meter (DropMaster DM500, manufactured by Kyowa Interface Science Co., Ltd.) for multiple liquids with different surface tensions, a Zisman plot is created, and the value at which cosθ = 1 (θ = 0°), i.e., the critical surface tension, can be determined. (E) When the critical surface tension of the water repellent is 40 mN / m or less, the contact angle θ of the water repellent is large, and the water repellent effect is large, which is thought to be the reason for improved weather resistance.

[0041] A preferred example of the (E) water repellent is a silicone-based water repellent, and particularly preferred is a composition containing a silicone resin in a base resin. Examples of silicone resins include organopolysiloxane, dimethylpolysiloxane, methylphenylpolysiloxane, methylhydrogenpolysiloxane, etc., and among these, dimethylpolysiloxane is preferably used. Examples of base resins include thermoplastic resins, such as low-density polyethylene, high-density polyethylene, polypropylene, and various polyolefin resins.

[0042] As the (E) water repellent agent, polytetrafluoroethylene is particularly preferred. The polytetrafluoroethylene is preferably one having fibril-forming ability. Fibrillated polytetrafluoroethylene has a large effect of improving weather resistance, and its reinforcing effect can improve impact resistance.

[0043] Polytetrafluoroethylene can use, as a copolymerization component, hexafluoropropylene, chlorotrifluoroethylene, fluoroalkylethylene, fluorine-containing olefins such as perfluoroalkyl vinyl ether, fluorine-containing alkyl (meth)acrylates such as perfluoroalkyl (meth)acrylates, etc. The content of such copolymerization components is preferably 10 mass% or less based on the total tetrafluoroethylene in the polytetrafluoroethylene.

[0044] Polytetrafluoroethylene can be produced by two methods: suspension polymerization and emulsion polymerization. Between suspension polymerization products and emulsion polymerization products, suspension polymerization products are preferable because polytetrafluoroethylene is less likely to aggregate during extrusion and is less likely to experience a decrease in impact resistance due to aggregation.

[0045] Also, polytetrafluoroethylene coated with organic polymer can be used as polytetrafluoroethylene. Organic polymer-coated polytetrafluoroethylene (or also called polytetrafluoroethylene-organic polymer composite) can be produced by various known methods, such as (i) a method of mixing polytetrafluoroethylene particle aqueous dispersion and organic polymer particle aqueous dispersion, and powdering by coagulation or spray drying to produce, (ii) a method of polymerizing the monomer that constitutes organic polymer in the presence of polytetrafluoroethylene particle aqueous dispersion, and then powdering by coagulation or spray drying to produce, (iii) a method of emulsion-polymerizing a monomer that has an ethylenic unsaturated bond in a dispersion that mixes polytetrafluoroethylene particle aqueous dispersion and organic polymer particle aqueous dispersion, and then powdering by coagulation or spray drying to produce, etc. Examples of the organic polymer that coats the polytetrafluoroethylene include polymers made of one or more monomers such as styrene, (meth)alkyl acrylate, and acrylonitrile, and elastomers.

[0046] However, polytetrafluoroethylene that is not coated with an organic polymer is preferred because it has a greater effect of improving impact resistance.

[0047] Polytetrafluoroethylene is D [3,2]A particle size in the range of 0.01 to 300 μm is preferable from the viewpoint of increasing the dispersibility of polytetrafluoroethylene and suppressing a decrease in impact resistance due to aggregation of polytetrafluoroethylene, and is more preferably 0.1 μm or more, even more preferably 1 μm or more, still more preferably 10 μm or more, and still more preferably 12 μm or more, and is preferably 200 μm or less, even more preferably 100 μm or less, of which 40 μm or less, particularly 30 μm or less, and even more preferably 20 μm or less. Polytetrafluoroethylene D [3,2] In the present invention, the particle size is the D [3,2] is the particle size.

[0048] The polytetrafluoroethylene may be used alone or in any combination of two or more kinds in any ratio.

[0049] The content of the (E) water repellent agent is 0.01 to 2 parts by mass relative to 100 parts by mass of the (A) polyethylene terephthalate resin, and is preferably 0.03 part by mass or more, more preferably 0.05 part by mass or more, and particularly preferably 0.08 part by mass or more, and is preferably 1.5 parts by mass or less, especially preferably 1 part by mass or less, 0.8 part by mass or less, 0.5 part by mass or less, and particularly preferably 0.4 part by mass or less. In addition, the ratio of the content of the (E) water repellent to the content of the (B) alkali metal carboxylate, (E) water repellent / (B) alkali metal carboxylate, is 0.01 or more, preferably 0.1 or more, and more preferably 0.2 or more in order to improve hydrolysis resistance, and is 5 or less, preferably 2 or less, and even more preferably 1.3 or less in order to improve the appearance of the molded article.

[0050] [Stabilizer] The polyethylene terephthalate resin composition of the present invention preferably contains a stabilizer, which can prevent deterioration of color, further improve thermal stability, or prevent a decrease in mechanical strength. As the stabilizer, a phosphorus-based stabilizer and a phenol-based stabilizer are preferred.

[0051] Examples of phosphorus-based stabilizers include phosphorous acid, phosphoric acid, phosphite esters, and phosphate esters, and among these, organic phosphate compounds, organic phosphite compounds, and organic phosphonite compounds are preferred.

[0052] The organic phosphate compound is preferably a compound represented by the following general formula: (R 1 O) 3-n P(=O)OH n (In the formula, R 1 are alkyl groups or aryl groups, which may be the same or different, and n is an integer of 0 to 2. More preferably, the compound represented by R 1 Examples of the alkyl group having 8 to 30 carbon atoms include a long-chain alkyl acid phosphate compound having 8 to 30 carbon atoms. Specific examples of the alkyl group having 8 to 30 carbon atoms include an octyl group, a 2-ethylhexyl group, an isooctyl group, a nonyl group, an isononyl group, a decyl group, an isodecyl group, a dodecyl group, a tridecyl group, an isotridecyl group, a tetradecyl group, a hexadecyl group, an octadecyl group, an eicosyl group, and a triacontyl group. Examples of the metal salt include salts of alkaline earth metals, zinc, lead, and tin, and particularly zinc salts.

[0053] Examples of long-chain alkyl acid phosphate compounds include octyl acid phosphate, 2-ethylhexyl acid phosphate, decyl acid phosphate, lauryl acid phosphate, octadecyl acid phosphate, oleyl acid phosphate, behenyl acid phosphate, phenyl acid phosphate, nonylphenyl acid phosphate, cyclohexyl acid phosphate, phenoxyethyl acid phosphate, and alkoxypolyethylene glycol acid phosphate. , bisphenol A acid phosphate, dimethyl acid phosphate, diethyl acid phosphate, dipropyl acid phosphate, diisopropyl acid phosphate, dibutyl acid phosphate, dioctyl acid phosphate, di-2-ethylhexyl acid phosphate, dioctyl acid phosphate, dilauryl acid phosphate, distearyl acid phosphate, diphenyl acid phosphate, bisnonylphenyl acid phosphate, and the like, or metal salts thereof. Among these, octadecyl acid phosphate is preferred, and this is commercially available, for example, under the trade name "ADEKA STAB AX-71" (octadecyl acid phosphate) manufactured by ADEKA Corporation, or under the trade name "JP-518Zn" (octadecyl acid phosphate Zn salt) manufactured by Johoku Chemical Industry Co., Ltd.

[0054] The organic phosphite compound is preferably a compound represented by the following general formula: R 2 OP(OR 3 )(OR 4 ) (In the formula, R 2 , R 3 and R 4 are each a hydrogen atom, an alkyl group having 1 to 30 carbon atoms, or an aryl group having 6 to 30 carbon atoms, and R 2 , R 3 and R 4 At least one of the groups is an aryl group having 6 to 30 carbon atoms.) Examples of the compound include compounds represented by the following formula:

[0055] Examples of the organic phosphite compound include triphenyl phosphite, tris(nonylphenyl)phosphite, dilauryl hydrogen phosphite, triethyl phosphite, tridecyl phosphite, tris(2-ethylhexyl)phosphite, tris(tridecyl)phosphite, tristearyl phosphite, diphenyl monodecyl phosphite, monophenyl didecyl phosphite, diphenyl mono(tridecyl)phosphite, tetraphenyl dipropylene glycol diphosphite, tetraphenyl tetra(tridecyl)pentaerythritol tetraphosphite, hydrogenated bisphenol A phenol phosphite polymer, diphenyl hydrogen phosphite, 4,4'-butylidene-bis(3-methyl-6-tert-butylphenyl di(tridecyl)phosphite), tetra(tridecyl) 4,4'-isopropyl phosphite, tetraphenyl di ... Examples of the phosphite include propylidenediphenyl diphosphite, bis(tridecyl)pentaerythritol diphosphite, bis(nonylphenyl)pentaerythritol diphosphite, dilauryl pentaerythritol diphosphite, distearyl pentaerythritol diphosphite, tris(4-tert-butylphenyl)phosphite, tris(2,4-di-tert-butylphenyl)phosphite, hydrogenated bisphenol A pentaerythritol phosphite polymer, bis(2,4-di-tert-butylphenyl)pentaerythritol diphosphite, bis(2,6-di-tert-butyl-4-methylphenyl)pentaerythritol diphosphite, 2,2'-methylenebis(4,6-di-tert-butylphenyl)octyl phosphite, and bis(2,4-dicumylphenyl)pentaerythritol diphosphite. Among these, bis(2,6-di-tert-butyl-4-methylphenyl)pentaerythritol diphosphite is preferred, and this is commercially available, for example, from ADEKA Corporation under the trade name "PEP-36."

[0056] The organic phosphonite compound is preferably a compound represented by the following general formula: R 5 -P(OR 6 )(OR 7 ) (In the formula, R5 , R 6 and R 7 are each a hydrogen atom, an alkyl group having 1 to 30 carbon atoms, or an aryl group having 6 to 30 carbon atoms, and R 5 , R 6 and R 7 At least one of the groups is an aryl group having 6 to 30 carbon atoms.) Examples of the compound include compounds represented by the following formula:

[0057] The organic phosphonite compounds include tetrakis(2,4-di-isopropylphenyl)-4,4'-biphenylene diphosphonite, tetrakis(2,4-di-n-butylphenyl)-4,4'-biphenylene diphosphonite, tetrakis(2,4-di-tert-butylphenyl)-4,4'-biphenylene diphosphonite, tetrakis(2,4-di-tert-butylphenyl)-4,3'-biphenylene diphosphonite, and tetrakis(2,4-di-tert-butylphenyl)-3,3'-biphenylene diphosphonite. tetrakis(2,6-di-iso-propylphenyl)-4,4'-biphenylene diphosphonite, tetrakis(2,6-di-n-butylphenyl)-4,4'-biphenylene diphosphonite, tetrakis(2,6-di-tert-butylphenyl)-4,4'-biphenylene diphosphonite, tetrakis(2,6-di-tert-butylphenyl)-4,3'-biphenylene diphosphonite, and tetrakis(2,6-di-tert-butylphenyl)-3,3'-biphenylene diphosphonite.

[0058] Examples of phenol-based stabilizers include pentaerythritol tetrakis(3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate), octadecyl-3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate, thiodiethylene bis(3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate), pentaerythritol tetrakis(3-(3,5-di-neopentyl-4-hydroxyphenyl)propionate), and the like.

[0059] Among them, pentaerythritol tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate] and octadecyl-3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate are preferred.Specific examples of such phenol-based antioxidants include "Irganox 1010" and "Irganox 1076" manufactured by BASF (trade names, the same applies below), and "Adeka STAB AO-50" and "Adeka STAB AO-60" manufactured by ADEKA.

[0060] The stabilizer may be contained alone or in any combination and ratio of two or more kinds.

[0061] The content of the stabilizer is preferably 0.001 to 1 part by mass relative to 100 parts by mass of the polyethylene terephthalate resin (A). If the content of the stabilizer is less than 0.001 part by mass, it is difficult to expect improvement in the thermal stability and compatibility of the resin composition, and a decrease in molecular weight and deterioration in hue during molding are likely to occur, while if it exceeds 1 part by mass, the amount becomes excessive, and the occurrence of silver streaks and deterioration in hue tend to occur more easily. The content of the stabilizer is more preferably 0.001 to 0.7 parts by mass, and even more preferably 0.005 to 0.6 parts by mass.

[0062] [Release agent] The polyethylene terephthalate resin composition of the present invention preferably contains a release agent. As the release agent, known release agents that are usually used for polyester resins can be used, among which aliphatic carboxylic acid amides, polyolefin compounds, fatty acid ester compounds, etc. Among these release agents, polyolefin compounds or aliphatic carboxylic acid amide compounds are preferred, and aliphatic carboxylic acid amides are particularly preferred because they have good releasability and cause little discoloration after weathering tests.

[0063] The polyolefin-based compound may be a compound selected from paraffin wax and polyethylene wax, and among them, those having a weight average molecular weight of 700 to 10,000, more preferably 900 to 8,000, are preferred.

[0064] Examples of fatty acid ester compounds include fatty acid esters such as saturated or unsaturated monovalent or divalent aliphatic carboxylic acid esters, glycerin fatty acid esters, sorbitan fatty acid esters, and partially saponified products thereof, etc. Among these, mono- or di-fatty acid esters composed of a fatty acid having 11 to 28 carbon atoms, preferably 17 to 21 carbon atoms, and an alcohol are preferred.

[0065] Examples of fatty acids include palmitic acid, stearic acid, caproic acid, capric acid, lauric acid, arachic acid, behenic acid, lignoceric acid, cerotic acid, melissic acid, tetralinic acid, montanic acid, adipic acid, azelaic acid, etc. The fatty acid may also be alicyclic.

[0066] Examples of the alcohol include saturated or unsaturated monohydric or polyhydric alcohols. These alcohols may have a substituent such as a fluorine atom or an aryl group. Among these, monohydric or polyhydric saturated alcohols having 30 or less carbon atoms are preferred, and aliphatic saturated monohydric or polyhydric alcohols having 30 or less carbon atoms are more preferred. Here, the term "aliphatic" also includes alicyclic compounds. Specific examples of such alcohols include octanol, decanol, dodecanol, stearyl alcohol, behenyl alcohol, ethylene glycol, diethylene glycol, glycerin, pentaerythritol, 2,2-dihydroxyperfluoropropanol, neopentylene glycol, ditrimethylolpropane, and dipentaerythritol.

[0067] The above ester compound may contain an aliphatic carboxylic acid and / or an alcohol as an impurity, and may be a mixture of a plurality of compounds.

[0068] Specific examples of fatty acid ester compounds include glycerin monostearate, glycerin monobehenate, glycerin dibehenate, glycerin-12-hydroxymonostearate, sorbitan monobehenate, pentaerythritol monostearate, pentaerythritol distearate, stearyl stearate, and ethylene glycol montanic acid ester.

[0069] Examples of the aliphatic carboxylic acid amide include compounds obtained by a dehydration reaction between a higher aliphatic monocarboxylic acid and / or a polybasic acid and a diamine.

[0070] As the higher aliphatic monocarboxylic acid, saturated aliphatic monocarboxylic acids and hydroxycarboxylic acids having 16 or more carbon atoms are preferred, and examples thereof include palmitic acid, stearic acid, behenic acid, montanic acid, and 12-hydroxystearic acid.

[0071] Examples of polybasic acids include aliphatic dicarboxylic acids such as malonic acid, succinic acid, adipic acid, sebacic acid, pimelic acid, and azelaic acid; aromatic dicarboxylic acids such as phthalic acid and terephthalic acid; and alicyclic dicarboxylic acids such as cyclohexanedicarboxylic acid and cyclohexylsuccinic acid.

[0072] Examples of diamines include ethylenediamine, 1,3-diaminopropane, 1,4-diaminobutane, hexamethylenediamine, metaxylylenediamine, tolylenediamine, paraxylylenediamine, phenylenediamine, and isophoronediamine.

[0073] As the carboxylic acid amide compound, a compound obtained by polycondensation of stearic acid, sebacic acid, and ethylenediamine is preferred, and a compound obtained by polycondensation of 2 moles of stearic acid, 1 mole of sebacic acid, and 2 moles of ethylenediamine is more preferred. In addition to bisamide compounds obtained by reacting diamines and aliphatic carboxylic acids, such as N,N'-methylenebisstearamide and N,N'-ethylenebisstearamide, dicarboxylic acid amide compounds, such as N,N'-dioctadecylterephthalamide, can also be suitably used.

[0074] The content of the release agent is preferably 0.1 to 3 parts by mass, more preferably 0.2 to 2.5 parts by mass, and even more preferably 0.5 to 2 parts by mass, relative to 100 parts by mass of the polyethylene terephthalate resin (A). If it is less than 0.1 part by mass, the surface properties tend to deteriorate due to poor release during melt molding, while if it exceeds 3 parts by mass, the workability of kneading the resin composition tends to decrease and the appearance of the molded product tends to deteriorate.

[0075] [Epoxy compounds] The polyethylene terephthalate resin composition of the present invention preferably contains an epoxy compound. The epoxy compound may be any compound having one or more epoxy groups in one molecule, and typically, a glycidyl compound which is a reaction product of epichlorohydrin with an alcohol, a phenol, or a carboxylic acid, or a compound in which an olefinic double bond has been epoxidized may be used. As the epoxy compound, known compounds that are usually used in polyester resins can be used, among which bisphenol A type epoxy compounds, novolac type epoxy compounds, bisphenol F type epoxy compounds, alicyclic epoxy compounds, glycidyl ethers, glycidyl esters, epoxidized butadiene polymers, resorcinol type epoxy compounds, etc. Among these epoxy compounds, bisphenol A type epoxy compounds are particularly preferred.

[0076] Examples of the bisphenol A type epoxy compound include bisphenol A diglycidyl ether and hydrogenated bisphenol A diglycidyl ether, and examples of the bisphenol F type epoxy compound include bisphenol F diglycidyl ether and hydrogenated bisphenol F diglycidyl ether. Examples of the novolac type epoxy compound include a phenol novolac type epoxy compound and a cresol novolac type epoxy compound.

[0077] Examples of the alicyclic epoxy compounds include vinylcyclohexene dioxide, dicyclopentadiene oxide, 3,4-epoxycyclohexyl-3,4-cyclohexylcarboxylate, bis(3,4-epoxycyclohexylmethyl)adipate, vinylcyclohexene diepoxide, 3,4-epoxycyclohexyl glycidyl ether, and the like.

[0078] Specific examples of glycidyl ethers include monoglycidyl ethers such as methyl glycidyl ether, butyl glycidyl ether, 2-ethylhexyl glycidyl ether, decyl glycidyl ether, stearyl glycidyl ether, phenyl glycidyl ether, butylphenyl glycidyl ether, and allyl glycidyl ether; and diglycidyl ethers such as neopentyl glycol diglycidyl ether, ethylene glycol diglycidyl ether, glycerin diglycidyl ether, propylene glycol diglycidyl ether, and bisphenol A diglycidyl ether.

[0079] Examples of the glycidyl esters include monoglycidyl esters such as glycidyl benzoate and glycidyl sorbate; and diglycidyl esters such as diglycidyl adipic acid, diglycidyl terephthalate and diglycidyl orthophthalate.

[0080] Examples of the epoxidized butadiene polymer include epoxidized polybutadiene, epoxidized styrene-butadiene copolymers, and epoxidized hydrogenated styrene-butadiene copolymers. An example of the resorcin type epoxy compound is resorcin diglycidyl ether.

[0081] The epoxy compound may also be a copolymer containing a glycidyl group-containing compound as one component, such as a copolymer of a glycidyl ester of an α,β-unsaturated acid and one or more monomers selected from the group consisting of an α-olefin, acrylic acid, an acrylic acid ester, a methacrylic acid, and a methacrylic acid ester.

[0082] In addition, the epoxy compound is preferably an epoxy compound having an epoxy equivalent of 50 to 10,000 g / eq and a weight average molecular weight of 8,000 or less. If the epoxy equivalent is less than 50 g / eq, the amount of epoxy groups is too large, so the viscosity of the resin composition is high, and conversely, if the epoxy equivalent is more than 10,000 g / eq, the amount of epoxy groups is small, so the effect of improving the hydrolysis resistance of the polyethylene terephthalate resin composition tends to be difficult to fully manifest. The epoxy equivalent is preferably 100 g / eq or more, more preferably 120 g / eq or more, more preferably 150 g / eq or more, and most preferably 170 g / eq or more. It is preferably 7000 g / eq or less, more preferably 5000 g / eq or less, more preferably 1000 g / eq or less, more preferably 500 g / eq or less, more preferably 300 g / eq or less, and most preferably 200 g / eq or less. Moreover, those having a weight average molecular weight exceeding 8000 tend to have a lower compatibility with polyethylene terephthalate resin and a lower mechanical strength of the molded product. The weight average molecular weight is more preferably 7000 or less, further preferably 6000 or less, further preferably 3000 or less, further preferably 1000 or less, further preferably 500 or less, and most preferably 400 or less.

[0083] As the epoxy compound, bisphenol A type epoxy compounds and novolac type epoxy compounds obtained by reacting bisphenol A or novolac with epichlorohydrin are preferred. Among them, bisphenol A type epoxy compounds are particularly preferred from the viewpoints of hydrolysis resistance, discoloration after weathering test, and surface appearance of molded products.

[0084] The content of the epoxy compound when contained is preferably 0.1 to 4 parts by mass, more preferably 0.2 parts by mass or more, among which 0.3 parts by mass or more, 0.4 parts by mass or more, 0.5 parts by mass or more, and most preferably 0.6 parts by mass or more, based on 100 parts by mass of the polyethylene terephthalate resin (A). Also, 3.5 parts by mass or less is more preferable, 3 parts by mass or less is even more preferable, among which 2.0 parts by mass or less, particularly 1.0 parts by mass or less is preferable. If the epoxy compound is 0.1 parts by mass or more, it is preferable because the mechanical strength of the molded product is improved. If the epoxy compound content is more than 4 parts by mass, crosslinking proceeds and the flowability during molding tends to deteriorate.

[0085] Furthermore, the equivalent ratio of the epoxy group of the epoxy compound to the terminal COOH group of the polyethylene terephthalate resin (epoxy group / COOH group) is preferably in the range of 0.2 to 2.7. If the equivalent ratio is less than 0.2, hydrolysis resistance is likely to deteriorate, and if it exceeds 2.7, moldability is likely to become unstable. The epoxy group / COOH group ratio is more preferably 0.3 or more and 2.5 or less.

[0086] [Other ingredients] The polyethylene terephthalate resin composition of the present invention may contain other resin additives other than those described above, as necessary, within the range that does not impair the effects of the present invention. Examples of other resin additives include ultraviolet absorbers, pigments other than carbon black, lubricants, catalyst deactivators, antistatic agents, foaming agents, plasticizers, flame retardants, flame retardant assistants, etc.

[0087] In the present invention, the polyethylene terephthalate resin composition may contain other thermoplastic resins, etc., other than the above-mentioned resins, as necessary, within the range that does not impair the effects of the present invention. Examples of other thermoplastic resins include polybutylene terephthalate resin, polyamide resin, polyacetal resin, polyphenylene oxide resin, polyphenylene sulfide resin, liquid crystal polyester resin, acrylic resin, etc. These may be used alone or in combination of two or more kinds.

[0088] However, when resins other than the above-mentioned essential component resins are contained, the content thereof is preferably 30 parts by mass or less, more preferably 25 parts by mass or less, and even more preferably 20 parts by mass or less, of which 10 parts by mass or less, particularly preferably 5 parts by mass or less, and most preferably 2 parts by mass or less, per 100 parts by mass of (A) polyethylene terephthalate resin.

[0089] [Production of polyethylene terephthalate resin composition] The method for producing the polyethylene terephthalate resin composition is not limited to a particular method, but the above-mentioned essential components and other components that are added as necessary are mixed, and then melted and kneaded. From the viewpoints of dispersibility of carbon black, discoloration of a molded body after a weathering test, and mechanical properties such as tensile strength, flexural strength, and Charpy impact strength, when blending (C) carbon black, it is preferable to blend it into (A) polyethylene terephthalate resin as a colorant composition containing (A) polyethylene terephthalate resin and (C) carbon black, i.e., as a master batch.

[0090] Examples of the melting and kneading method include a method in which the above-mentioned essential components and other components that are added as necessary are uniformly mixed using a Henschel mixer, ribbon blender, V-type blender, tumbler, etc., and then melting and kneading using a single-screw or multi-screw kneading extruder, roll, Banbury mixer, Labo Plastomill (Brabender), etc. The temperature during melting and kneading is preferably in the range of 200 to 300°C, more preferably in the range of 220 to 290°C. When the production is carried out using an extruder, it is preferable that the extruder has two or more vents from the viewpoint of mechanical properties such as tensile strength, bending strength, and Charpy impact strength of the molded article. The crystallization temperature of the polyethylene terephthalate resin composition of the present invention is preferably 200 to 230° C. in terms of improving the appearance and mechanical properties of the molded article, and is particularly preferably 207 to 210° C.

[0091] [Molded body] As a method for producing a molded article using the above-mentioned polyethylene terephthalate resin composition, any molding method generally used for polyethylene terephthalate resin compositions can be adopted, and examples thereof include injection molding, ultra-high speed injection molding, injection compression molding, two-color molding, gas-assisted or other hollow molding methods, molding methods using a heat-insulating mold, molding methods using a rapidly heated mold, insert molding, IMC (in-mold coating molding) molding, extrusion molding, sheet molding, and the like, with the injection molding method being particularly preferred.

[0092] Examples of the molded article include injection molded articles, extrusion molded articles, sheets, pipes, various films, etc. The shape, size, thickness, etc. of these molded articles are arbitrary. The surface of the molded article preferably has a contact angle with water of at least 80°. When the contact angle is at least 80°, the water repellency is greater and the weather resistance is improved.

[0093] The molded article can be used as an electric / electronic part, an automobile part, other electric equipment part, a machine part, a part of a home appliance, etc. The polyethylene terephthalate resin composition of the present invention has excellent weather resistance, impact resistance and appearance, and therefore can be suitably used for products used outdoors, particularly for automobile exterior parts, such as glazing, outer handles, door mirror stays, fenders, garnishes, bumpers, roof rails, etc. EXAMPLES

[0094] The present invention will be described in more detail below based on examples and comparative examples, but the present invention should not be construed as being limited to the following described examples.

[0095] The raw materials used in the following Examples and Comparative Examples are as shown in Tables 1 and 2 below.

[0096] [Table 1]

[0097] [Table 2]

[0098] (Examples 1 to 21, Comparative Examples 1 to 9) [Production of polyethylene terephthalate resin composition pellets] Of the components listed in Tables 1 and 2 above, the components other than glass fiber were blended in the ratios (mass ratios) listed in Tables 3 to 6, and after uniformly mixing for 20 minutes in a tumbler mixer, the mixture was fed into a twin-screw extruder "TEX30α" manufactured by Japan Steel Works, Ltd., and glass fiber was fed into the molten resin by side feeding from the middle of the twin-screw extruder in the ratios listed in Tables 3 to 6. In addition, one vacuum vent was installed upstream and one downstream of the side feeder in the extruder, and each was vented at a vacuum degree of -0.08 MPa (gauge pressure). The mixture was kneaded at a screw rotation speed of 300 rpm and a barrel temperature of 280° C., and the molten resin extruded in the form of strands was quenched in a water tank and pelletized using a pelletizer to obtain pellets of a polyethylene terephthalate resin composition.

[0099] Example 22 [Production of polyethylene terephthalate resin composition pellets] Of the components listed in Tables 1 and 2, the components other than the glass fiber were blended in the ratios (mass ratios) listed in Table 5, and after uniformly mixing for 20 minutes in a tumbler mixer, the components were fed into a twin-screw extruder "TEX30α" manufactured by Japan Steel Works, Ltd., and the glass fiber was fed into the molten resin by side feeding from the middle of the twin-screw extruder in the ratios listed in Table 5. In addition, vacuum vents were installed on both the upstream and downstream sides of the side feeder in the extruder, with the upstream bend open (gauge pressure: 0 MPa) and the downstream vent vented at a vacuum degree of -0.08 MPa (gauge pressure). The mixture was kneaded at a screw rotation speed of 300 rpm and a barrel temperature of 280° C., and the molten resin extruded in the form of strands was quenched in a water tank and pelletized using a pelletizer to obtain pellets of a polyethylene terephthalate resin composition.

[0100] [Box mold release: Maximum release resistance] The pellets obtained above were dried at 130°C for 5 hours, and then a Japan Steel Works injection molding machine (clamping force 50T) was used to mold a box-shaped molded product with a thickness of 1.5 mmt, outer dimensions of 30 x 50 x 15 mm, and a textured surface (textured to a height of 15 μm) under the conditions of a cylinder temperature of 290°C, a mold temperature of 143°C, and a cooling time of 20 seconds. The maximum mold release resistance value (unit: MPa) when the product was released from the mold by protruding the ejector pin was evaluated as the mold release resistance. If the maximum mold release resistance value is 10 MPa or less, it can be determined that there is no problem when it is used as an actual product.

[0101] [Tensile strength] The resin composition pellets obtained above were dried at 130°C for 5 hours, and then injection molded into ISO multipurpose test pieces (4 mm thick) using an injection molding machine (Nissei Plastic Industrial Co., Ltd., "J-85AD-60H") under conditions of a cylinder temperature of 280°C and a mold temperature of 140°C. The tensile strength (unit: MPa) of the ISO multipurpose test pieces obtained above was measured in accordance with ISO standards 527-1 and ISO 527-2.

[0102] [Tensile strength after hydrolysis treatment] The multipurpose test piece (4 mm thick) obtained above was treated for 25 hours at 121°C, 2 atm, and 100% RH using a highly accelerated life tester (Hirayama PC-R8D), and the tensile strength (unit: MPa) after the wet heat test was measured based on the JIS K7161 standard. The evaluation was based on two levels: A and B. A: Tensile strength after hydrolysis is 67 MPa or more B: Tensile strength after hydrolysis is less than 67 MPa

[0103] [Notched Charpy impact strength (unit: kJ / m 2 )] The pellets obtained were dried at 130°C for 5 hours, and then molded into ISO multipurpose test pieces (4 mm thick) using an injection molding machine "J-85AD-60H" manufactured by Japan Steel Works, Ltd., under conditions of a cylinder temperature of 280°C and a mold temperature of 140°C. Then, in accordance with ISO179, test pieces for a notched Charpy impact test were prepared using the multipurpose test pieces obtained, and the notched Charpy impact strength at room temperature (23°C) was measured. Notched Charpy impact strength is 9kJ / m 2 The higher one is "A". 9kJ / m 2 The evaluation was based on a two-level scale, with anything less than this being rated as "B" and anything less being rated as "C."

[0104] [Unnotched Charpy impact strength (unit: kJ / m 2 )] The pellets obtained were dried at 130°C for 5 hours, and then molded into ISO multipurpose test pieces (thickness 4 mm) using an injection molding machine "J-85AD-60H" manufactured by Japan Steel Works, Ltd., under conditions of a cylinder temperature of 280°C and a mold temperature of 140°C. Then, in accordance with ISO179, test pieces for a notched Charpy impact test were prepared using the multipurpose test pieces obtained, and the unnotched Charpy impact strength at room temperature (23°C) was measured. Unnotched Charpy impact strength is 44kJ / m 2 The higher one is "A". 44kJ / m 2 The evaluation was based on a two-level scale, with anything less than this being rated as "B" and anything less being rated as "C."

[0105] [Discoloration after weathering test (ΔE * )] The pellets obtained were dried at 130°C for 5 hours, and then injection molded into textured test pieces (sheets measuring 60 mm long x 60 mm wide x 2 mm thick and 15 μm texture height) using a Japan Steel Works injection molding machine "J-100AD-60H" at a cylinder temperature of 280°C. Using a "Sunshine Weather Tester" manufactured by Suga Test Instruments Co., Ltd., rain was poured continuously for 18 minutes over a 120-minute period at a black panel temperature of 63°C for one cycle (2 hours). The textured surface was set as the front and removed at a specified time. A spectrophotometric color difference meter (Konica Minolta "CM-3600d") was used to measure the color difference (ΔE * ) was evaluated using the following formula: ΔE * =((ΔL * ) 2 +(Δa * ) 2 +(Δb * ) 2 ) 1 / 2 ΔE * The smaller the value, the less discoloration and the more excellent the resistance to heat discoloration. The evaluation was based on the following criteria. The evaluation was based on the following three AC levels. A: ΔE after weather resistance test * is 8.5 or less B: ΔE * is over 8.5 and under 9.0 C: ΔE * 9 or more

[0106] [Surface condition after weather resistance test] The surface condition of the test piece after the weather resistance test was visually observed and compared with that of the test piece before the weather resistance test, and evaluated according to the following criteria. The evaluation was based on the following three AC levels. A: There is little color change and no floating of glass fibers. B: The color change is small, but the amount of glass fiber floating has increased compared to before the weather resistance test. C: Large color change

[0107] [Crystallization temperature measurement using DSC] The crystallization temperature of the polyethylene terephthalate resin composition was measured using a differential scanning calorimeter (DSC) based on JIS K7121. The temperature was raised from 40°C to 300°C at a heating rate of 20°C / min under a nitrogen atmosphere, and after holding at 300°C for 3 minutes, the temperature was lowered to 40°C at a heating rate of -20°C / min. The temperature of the maximum peak due to crystallization during heating was determined as the crystallization temperature Tc. The melting point Tm was determined from the peak during melting. The differential scanning calorimeter used was "DSC7020" manufactured by Hitachi High-Tech Science Corporation.

[0108] [Water repellency] The pellets obtained were dried at 130°C for 5 hours, and then a test piece (60mm length x 60mm width x 2mm thickness, with a smooth surface) was injection molded using a Japan Steel Works injection molding machine "J-100AD-60H" at a cylinder temperature of 280°C. The molded product was left to stand for 24 hours in a thermostatic chamber at a temperature of 23°C and a humidity of 60% RH to adjust its condition, and then 1μL of pure water was dropped onto the product using a contact angle meter (Kyowa Interface Science Co., Ltd.'s "DropMaster DM500") to measure the contact angle.

[0109] [Appearance of molded product] The pellets obtained were dried at 130°C for 5 hours, and then injection molded into textured test pieces (sheets measuring 60mm length x 60mm width x 2mm thickness and 15μm texture height) using a Japan Steel Works injection molding machine "J-100AD-60H" at a cylinder temperature of 280°C. The textured surface of the molded product was checked to confirm the texture transferability. The evaluation was based on the following three AC levels. A: All the grain has been transferred and there are no ejector pin marks. B: All the grain has been transferred, but there are ejector pin marks. C: Some of the grain is crushed and the surface is glossy, or there are ejector pin marks.

[0110] [comprehensive evaluation] Based on the evaluation results of the three items, namely, the notched Charpy impact strength, discoloration after weathering test, and surface condition after weathering test, an overall evaluation was made on a five-level scale from A to E as follows. A: Three As B: Both discoloration after weathering test and surface condition after weathering test are rated A, and the notched Charpy impact strength is rated B. C: Either the evaluation of discoloration after weathering test or the evaluation of surface condition after weathering test is A and the other is B. D: 1 A, 2 C There is no E:A The above results are shown in Table 3 below.

[0111] [Table 3]

[0112] [Table 4]

[0113] [Table 5]

[0114] [Table 6] [Industrial Applicability]

[0115] Since the polyethylene terephthalate resin composition of the present invention has excellent weather resistance, it can be suitably used for parts to be used outdoors, particularly exterior parts for vehicles.

Claims

1. A polyethylene terephthalate resin composition comprising, relative to 100 parts by mass of (A) polyethylene terephthalate resin, (B) 0.1 to 5 parts by mass of an alkali metal salt of a carboxylate, (C) 0.1 to 6 parts by mass of carbon black, (D) 55 parts by mass or more of glass fiber, and (E) 0.01 to 2 parts by mass of a water repellent, wherein the critical surface tension of the water repellent is 40 mN / m or less.

2. The polyethylene terephthalate resin composition according to claim 1, wherein the mass ratio (E) / (B) of the content of the water repellent (E) to the alkali metal carboxylate (B) is 0.2 to 1.

3.

3. 3. The polyethylene terephthalate resin composition according to claim 1 or 2, wherein the water repellent (E) is polytetrafluoroethylene.

4. 3. The polyethylene terephthalate resin composition according to claim 1, wherein the alkali metal carboxylate (B) is a sodium carboxylate.

5. 3. The polyethylene terephthalate resin composition according to claim 1, wherein the carboxylate (B) is an alkali metal salt of montanic acid.

6. The polyethylene terephthalate resin composition according to claim 4, wherein the sodium carboxylate (B) is sodium montanate.

7. 6. The polyethylene terephthalate resin composition according to claim 5, wherein the alkali metal salt of montanic acid (B) is sodium montanate.

8. The polyethylene terephthalate resin composition according to claim 1 or 2, further comprising a release agent in an amount of 0.1 to 3 parts by mass per 100 parts by mass of the polyethylene terephthalate resin (A).

9. 9. The polyethylene terephthalate resin composition according to claim 8, wherein the release agent is a polyolefin compound or an aliphatic carboxylic acid amide.

10. 9. The polyethylene terephthalate resin composition according to claim 8, wherein the release agent is an aliphatic carboxylic acid amide.

11. (C) Carbon black has a DBP oil absorption of 40 to 80 cm 3 The polyethylene terephthalate resin composition according to claim 1 or 2, wherein the composition is a polyvinyl chloride resin.

12. The polyethylene terephthalate resin composition according to claim 1 or 2, further comprising an epoxy compound in an amount of 0.1 to 4 parts by mass per 100 parts by mass of the polyethylene terephthalate resin (A).

13. The polyethylene terephthalate resin composition according to claim 12, wherein the epoxy compound is a bisphenol A type epoxy compound.

14. A molded article of the polyethylene terephthalate resin composition according to claim 1 or 2.

15. 15. The molded article according to claim 14, wherein the contact angle of the surface of the molded article with water is 80° or more.

16. The molded article according to claim 14, which is for a product to be used outdoors.

17. 3. A method for producing a polyethylene terephthalate resin composition according to claim 1, further comprising a step of blending a colorant composition containing the polyethylene terephthalate resin (A) and carbon black (C) with the polyethylene terephthalate resin (A).

18. 3. A method for producing the polyethylene terephthalate resin composition according to claim 1 or 2, using an extruder, wherein the extruder has two or more vents.

Citation Information

Patent Citations

  • Polyethylene terephthalate resin composition

    JP1980052341A

  • resin composition

    JP1993271521A

  • Polyethylene terephthalate-based resin composition

    JP1999029696A

  • ANTISTATIC POLYMER COMPOSITION AND MOLDED PRODUCT THEREOF

    JP2002500237A

  • Flame-retardant polybutylene terephthalate resin composition and insulation component