Austenitic Stainless Steel
Austenitic stainless steel with a tailored chemical composition and dislocation cell structure enhances strength and embrittlement resistance, addressing hydrogen embrittlement issues in high-pressure hydrogen environments.
Patent Information
- Application Number
- JP2019102450
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2019-05-31
- Publication Date
- 2024-09-26
- Estimated Expiration
- 2039-05-31
AI Technical Summary
Existing austenitic stainless steels used in high-pressure hydrogen environments suffer from hydrogen embrittlement, limiting their strength and durability in applications like fuel cell vehicles and hydrogen stations, despite having good embrittlement resistance.
Austenitic stainless steel with a specific chemical composition (C: 0.100% or less, Si: 1.00% or less, Mn: 3.00% to less than 7.00%, Cr: 15.00% to 30.00%, Ni: 10.00% to 21.00%, Mo: 1.20% to 4.50%, P: 0.050% or less, S: 0.050% or less, Al: 0.100% or less, N: 0.150% to 0.500%, and Fe with a dislocation cell structure and austenite grain size number of 7.5 or more, and a dislocation cell organization ratio of 50% to 80%, minimizing coarse precipitates.
The solution provides high tensile strength and excellent hydrogen embrittlement resistance, ensuring durability in high-pressure hydrogen environments.
Smart Images

Figure 0007556675000004 
Figure 0007556675000009 
Figure 0007556675000008
Abstract
Description
[Technical field]
[0001] The present disclosure relates to austenitic stainless steel materials. [Background technology]
[0002] In recent years, there has been progress in the development of fuel cell vehicles that run on hydrogen fuel, and in the practical application of hydrogen stations that supply hydrogen to fuel cell vehicles. Stainless steel is one of the candidate materials for use in these applications. However, in a high-pressure hydrogen gas environment, even stainless steel can become embrittled by hydrogen gas (hydrogen embrittlement). The High Pressure Gas Safety Act stipulates that SUS316L be used as a stainless steel material with excellent resistance to hydrogen embrittlement.
[0003] However, in consideration of the need to reduce the weight of fuel cell vehicles, make hydrogen stations more compact, and operate at high pressures at hydrogen stations, it is desirable for the stainless steel materials used for containers, fittings, and piping to have excellent hydrogen embrittlement resistance in hydrogen gas environments and strength equal to or greater than that of the existing SUS316L.
[0004] International Publication No. 2016 / 068009 (Patent Document 1) proposes an austenitic stainless steel that has excellent hydrogen embrittlement resistance and high strength.
[0005] The austenitic stainless steel disclosed in Patent Document 1 has a chemical composition, in mass %, of C: 0.10% or less, Si: 1.0% or less, Mn: 3.0% or more and less than 7.0%, Cr: 15 to 30%, Ni: 12.0% or more and less than 17.0%, Al: 0.10% or less, N: 0.10 to 0.50%, P: 0.050% or less, S: 0.050% or less, V: 0.01 to 1.0%, and at least one of Nb: 0.01 to 0.50%, Mo: 0 to 3.0%, W: 0 to 6.0%, Ti: 0 to 0.5%, Zr: 0 to 0.5%, Hf: 0 to 0.05%, and the like. 0.3%, Ta: 0~0.6%, B: 0~0.020%, Cu: 0~5.0%, Co: 0~10.0%, Mg: 0~0.0050%, Ca: 0~0.0050%, La: 0~0.20%, Ce: 0~0.20%, Y: 0~0.40%, Sm: 0~0.40%, Pr: 0~0.40%, Nd: 0~0.50%, balance: Fe and impurities, the ratio of the minor axis to the major axis of the austenite grains is greater than 0.1, the grain size number of the austenite grains is 8.0 or more, and the tensile strength is 1000 MPa or more. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] International Publication No. 2016 / 068009 Summary of the Invention [Problem to be solved by the invention]
[0007] In the austenitic stainless steel disclosed in Patent Document 1, the Ni content is set to 12.0% or more to improve hydrogen embrittlement resistance. Furthermore, by finely precipitating carbonitrides, the deformation of crystal grains is suppressed by the pinning effect, and the crystal grains are refined. As a result, high tensile strength is obtained.
[0008] However, by means other than that disclosed in Patent Document 1, an austenitic stainless steel material having excellent hydrogen embrittlement resistance and high strength may be produced.
[0009] An object of the present disclosure is to provide an austenitic stainless steel material having high tensile strength and excellent resistance to hydrogen embrittlement. [Means for solving the problem]
[0010] The austenitic stainless steel material according to the present disclosure has Chemical composition, in mass%, C: 0.100% or less, Si: 1.00% or less, Mn: 3.00 to less than 7.00% Cr: 15.00~30.00%, Ni: 10.00~21.00%, Mo: 1.20-4.50%, P: 0.050% or less, S: 0.050% or less, Al: 0.100% or less, N: 0.150 to 0.500%, and the balance being Fe and impurities; The austenite grain size number according to ASTM E112 is 7.5 or more, In a cross section perpendicular to the longitudinal direction of the austenitic stainless steel material, the dislocation cell structure ratio is 50 to 80%, The number density of precipitates with a major axis of 1.0 μm or more is 5.0 / 0.2 mm 2 The following is the result. Effect of the Invention
[0011] The austenitic stainless steel material according to the present disclosure has high tensile strength and excellent resistance to hydrogen embrittlement. [Brief description of the drawings]
[0012] [Figure 1] FIG. 1 is a diagram showing an example of a bright-field image (TEM image) of an observation field in which a dislocation cell structure is formed, obtained by transmission electron microscope observation, in an austenitic stainless steel material having the chemical composition of this embodiment. [Diagram 2]FIG. 2 is a diagram showing an example of a TEM image in which no dislocation cell structure is formed in an austenitic stainless steel material having the chemical composition of this embodiment. [Diagram 3] FIG. 3 is an image in which the bright-field image in FIG. 1 has been binarized using the median value of the histogram of pixel values as the threshold value. [Figure 4] FIG. 4 is a diagram in which the outline of a low dislocation density region (dislocation cell) having an area of 0.20 μm 2 or more is drawn and extracted based on the binarized image of FIG. [Diagram 5] FIG. 5 is a schematic diagram for explaining sample collection positions when the austenitic stainless steel material of this embodiment is a steel pipe. [Figure 6] FIG. 6 is a schematic diagram for explaining sample collection positions when the austenitic stainless steel material of this embodiment is a steel bar. [Figure 7] FIG. 7 is a schematic diagram for explaining sample collection positions when the austenitic stainless steel material of this embodiment is a steel plate. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] The present inventors have studied an austenitic stainless steel material having sufficient hydrogen embrittlement resistance and high tensile strength. In order to improve hydrogen embrittlement resistance, the inclusion of Cr, Ni, and Mo is extremely effective. Therefore, the present inventors have studied the chemical composition of an austenitic stainless steel material having excellent hydrogen embrittlement resistance. As a result, it was considered that sufficient hydrogen embrittlement resistance can be obtained if the austenitic stainless steel material has a chemical composition, in mass%, of C: 0.100% or less, Si: 1.00% or less, Mn: 3.00 to less than 7.00%, Cr: 15.00 to 30.00%, Ni: 10.00 to 21.00%, Mo: 1.20 to 4.50%, P: 0.050% or less, S: 0.050% or less, Al: 0.100% or less, N: 0.150 to 0.500%, and the balance being Fe and impurities.
[0014] Therefore, the present inventors further investigated the strength of austenitic stainless steel having the above chemical composition. As described in Patent Document 1, it is believed that strength can be increased by forming fine precipitates such as carbonitrides and refining crystal grains by the pinning effect of the fine precipitates. However, the precipitates may become the starting points of hydrogen cracking.
[0015] Therefore, the inventors of the present invention did not adopt a method of increasing strength by the pinning effect of precipitates, but instead investigated a method of increasing strength by a method other than the pinning effect of precipitates. As a result, the inventors of the present invention discovered for the first time that high strength can be obtained by forming a dislocation cell structure instead of utilizing the pinning effect of precipitates in an austenitic stainless steel material having the above-mentioned chemical composition.
[0016] Fig. 1 shows a bright-field image (hereinafter referred to as TEM image) of a visual field (4.2 μm×4.2 μm) in which dislocation cell structures are formed, obtained by structural observation using a transmission electron microscope (TEM) in an austenitic stainless steel material having the above-mentioned chemical composition. Fig. 2 shows an example of a TEM image in which no dislocation cell structures are formed in an austenitic stainless steel material having the above-mentioned chemical composition. Fig. 1 corresponds to test number 1 in the examples described below. Fig. 2 corresponds to test number 14.
[0017] Both Fig. 1 and Fig. 2 show austenitic stainless steel materials having the above-mentioned chemical composition. In Fig. 2, a large number of dislocations 105 are present, but the dislocations 105 do not form cells.
[0018] In contrast, the TEM image shown in Fig. 1 shows a different state of dislocations compared to Fig. 2. Specifically, Fig. 1 shows the presence of cell wall regions 101 with high dislocation density and low-density dislocation regions 102, which are surrounded by the cell wall regions 101 and have low dislocation density. In Fig. 1, the cell wall regions 101 are formed in a mesh-like shape. In this specification, the structure in which the cell wall regions 101 and the low-density dislocation regions 102 exist is referred to as a "dislocation cell structure."
[0019] The present inventors have found that in an austenitic stainless steel material having the above-mentioned chemical composition, high strength can be obtained by making the austenite grains 7.5 or more in terms of grain size number according to ASTM E112 and forming a dislocation cell structure. More specifically, they have found that if the dislocation cell structure ratio, defined by the following method, is 50% or more, excellent hydrogen embrittlement resistance and high strength can be obtained.
[0020] Here, the dislocation cell structure ratio is defined by the following method.
[0021] In a cross section perpendicular to the longitudinal direction of the austenitic stainless steel material, 15 arbitrary fields of view, each with a size of 4.2 μm × 4.2 μm, are selected. In each selected field of view, a photographic image (bright-field image) is generated using a transmission electron microscope (TEM), and in the generated photographic image, cell wall regions 101 with high dislocation density and low-density dislocation regions 102 with low dislocation density are identified. Of the multiple low-density dislocation regions 102 identified in each field of view, 0.20 μm 2 A visual field in which nine or more low-density dislocation regions 102 having an area of 100 mm or more are present is recognized as a visual field in which a dislocation cell structure is formed. The ratio of visual fields in which a dislocation cell structure is formed to all visual fields (15 visual fields) is defined as the dislocation cell structure rate (%).
[0022] More specifically, the dislocation cell structure ratio is determined by the following method. Three samples are taken from a cross section perpendicular to the longitudinal direction of the austenitic stainless steel material. The test surface of each sample is a cross section perpendicular to the longitudinal direction of the austenitic stainless steel material. Wet polishing is performed on each sample until the thickness is 30 μm. After wet polishing, the samples are electrolytically polished using a mixture of perchloric acid (10 vol.%) and ethanol (90 vol.%) to prepare thin film samples. A structure observation is performed on the test surface of each thin film sample using a TEM. TEM observation is performed on five arbitrary fields of view on the test surface of each sample. The size of each field of view is a rectangle of 4.2 μm × 4.2 μm. The accelerating voltage during TEM observation is 200 kV. <110> The observation target is the crystal grains that can be observed by the incident electron beam. Bright-field images are acquired in each field of view.
[0023] Using the bright-field image of each field, whether each field has a dislocation cell structure or not is judged by the following method. In the following explanation, a method for judging a dislocation cell structure is explained by taking the bright-field image shown in FIG. 1 as an example. In the bright-field image, a histogram showing the frequency of pixel values (0 to 255) is generated, and the median of the histogram is obtained. The number of pixels in the bright-field image of each field is not particularly limited, but is, for example, 100,000 pixels or more and 150,000 pixels or less. The bright-field image is binarized using the median as a threshold value. FIG. 3 is an image in which the bright-field image of FIG. 1 is binarized using the median of the histogram of pixel values as a threshold value. In the binarized image, the black region is a region with high dislocation density. Therefore, the black region is recognized as the cell wall region 101. On the other hand, the white region is a region with low dislocation density. Therefore, the white closed region surrounded by the cell wall region 101 is recognized as the low-density dislocation region 102.
[0024] The boundary of the white closed region (low-density dislocation region 102) is defined, and the area of each low-density dislocation region 102 is calculated. 2 The above low-density dislocation region 102 is recognized as a "dislocation cell."
[0025] Figure 4 shows the results of the 0.20 μm thresholding based on the binarized image of Figure 3. 2This is a diagram obtained by drawing and extracting the boundaries of low-density dislocation regions 102 (dislocation cells) having the above areas. In Fig. 4, when the boundaries of the low-density dislocation regions 102 are in contact with each other, the areas of those low-density dislocation regions 102 are calculated as one low-density dislocation region 102. In the case of the field of view of Fig. 1, there are 13 low-density dislocation regions 102.
[0026] When the number of low-density dislocation regions 102 in FIG. 2 is calculated by the same method as described above, the number is five in FIG.
[0027] Using the above analytical techniques, the number of dislocation cells (0.20 μm) in each field of view (4.2 μm × 4.2 μm) was 2 The number of low dislocation density regions 102) having an area of 100 μm or more is determined. Then, when nine or more dislocation cells are present in each field of view, the microstructure of that field of view is recognized as a dislocation cell structure. Note that when three or more straight lines intersect with both of the two opposing sides (opposite sides) of the field of view (rectangular bright-field image of 4.2 μm × 4.2 μm), the field of view is recognized as having a planar structure and is not recognized as a dislocation cell structure. The number of fields of view with dislocation cell structures among the 15 fields of view observed is determined. Then, the dislocation cell structure rate (%) is defined by the following formula. Dislocation cell structure rate = number of fields of view recognized as having dislocation cell structure / total number of fields of view × 100
[0028] The above-mentioned calculation of the median of the histogram of pixel values of the TEM image, the binarization of the TEM image, the determination of the boundary of the low-density dislocation region 102, and the calculation of the area of the low-density dislocation region 102 can all be analyzed using well-known image processing software. An example of well-known image processing software is ImageJ (product name). Note that it is well-known to those skilled in the art that similar analyses can be performed using image processing software other than ImageJ.
[0029] If the austenitic stainless steel material has the above chemical composition and has a dislocation cell structure ratio of 50% or more based on the above definition, it will have high strength. The reason for this is unclear, but the following is thought to be the reason. In the cell wall region 101, which is a high-density dislocation region in the dislocation cell structure, dislocations are densely packed and entangled with each other. Therefore, the dislocations that make up the cell wall region 101 are difficult to move and are fixed. As a result, it is thought that the strength of the austenitic stainless steel material is increased.
[0030] Even if the content of each element in the chemical composition of an austenitic stainless steel material is within the above-mentioned range, the austenite grain size number according to ASTM E112 is 7.5 or more, and the dislocation cell structure ratio is 50% or more, if there are many coarse precipitates in the steel material, hydrogen is absorbed at the interface between the coarse precipitates and the parent phase (austenite), and the hydrogen embrittlement resistance decreases. Therefore, the present inventors have investigated and examined the relationship between coarse precipitates and hydrogen embrittlement resistance in austenitic stainless steel materials whose content of each element in the chemical composition is within the above-mentioned range, whose austenite grain size number according to ASTM E112 is 7.5 or more, and whose dislocation cell structure ratio is 50% or more. As a result, in austenitic stainless steel materials in which the content of each element in the chemical composition is within the above-mentioned range, the austenite grain size number according to ASTM E112 is 7.5 or more, and the dislocation cell structure ratio is 50% or more, the number density of precipitates with a major axis of 1.0 μm or more is 5.0 precipitates / 0.2 mm 2 It has been found that the following provides excellent hydrogen embrittlement resistance and high tensile strength.
[0031] The austenitic stainless steel material of this embodiment, which has been completed based on the above findings, has the following configuration.
[0032] [1] The austenitic stainless steel material is Chemical composition, in mass%, C: 0.100% or less, Si: 1.00% or less, Mn: 3.00 to less than 7.00% Cr: 15.00~30.00%, Ni: 10.00~21.00%, Mo: 1.20-4.50%, P: 0.050% or less, S: 0.050% or less, Al: 0.100% or less, N: 0.150 to 0.500%, and the balance being Fe and impurities; The austenite grain size number according to ASTM E112 is 7.5 or more, In a cross section perpendicular to the longitudinal direction of the austenitic stainless steel material, the dislocation cell structure ratio is 50 to 80%, The number density of precipitates with a major axis of 1.0 μm or more is 5.0 / 0.2 mm 2 The following is the result.
[0033] The austenitic stainless steel material according to [2] is the austenitic stainless steel material according to [1], The austenite grain size number is greater than or equal to 8.0.
[0034] The austenitic stainless steel material according to [3] is an austenitic stainless steel material according to [1] or [2], The dislocation cell structure rate is 55% or more.
[0035] The austenitic stainless steel material according to [4] is an austenitic stainless steel material according to any one of [1] to [3], The number density of the precipitates having a major axis of 1.0 μm or more is 4.8 precipitates / 0.2 mm 2 The following is the result.
[0036] The austenitic stainless steel material of this embodiment will be described in detail below. "%" for elements means mass % unless otherwise specified.
[0037] [Chemical composition] The chemical composition of the austenitic stainless steel material of this embodiment contains the following elements.
[0038] C: 0.100% or less Carbon (C) is an unavoidable impurity. That is, the C content is more than 0%. C forms carbides at the austenite grain boundaries, which reduces the hydrogen embrittlement resistance of the steel material. If the C content exceeds 0.100%, the hydrogen embrittlement resistance of the steel material will decrease even if the contents of other elements are within the range of this embodiment. Therefore, the C content is 0.100% or less. The preferred upper limit of the C content is 0.080%, more preferably 0.060%, more preferably 0.040%, and even more preferably 0.030%. The C content is preferably as low as possible. However, if the C content is reduced excessively, the manufacturing cost will increase. Therefore, in consideration of normal industrial production, the preferred lower limit of the C content is 0.001%, more preferably 0.002%, and even more preferably 0.005%.
[0039] Si: 1.00% or less Silicon (Si) is inevitably contained. That is, the Si content is more than 0%. Si deoxidizes steel. However, if the Si content is too high, Si bonds with Ni, Cr, etc., and promotes the formation of sigma (σ) phase. If the Si content exceeds 1.00%, even if the contents of other elements are within the range of this embodiment, the hot workability and toughness of the steel material will decrease due to the formation of σ phase. Therefore, the Si content is 1.00% or less. The preferred upper limit of the Si content is 0.90%, more preferably 0.70%, and even more preferably 0.50%. If the Si content is excessively reduced, the manufacturing cost will increase. Therefore, taking into consideration normal industrial production, the preferred lower limit of the Si content is 0.01%, and even more preferably 0.02%. The preferred lower limit of the Si content for more effectively enhancing the deoxidizing effect of steel is 0.10%, and even more preferably 0.20%.
[0040] Mn: 3.00 to less than 7.00% Manganese (Mn) stabilizes austenite and enhances hydrogen embrittlement resistance. Mn also promotes the formation of dislocation cell structures. If the Mn content is less than 3.00%, this effect cannot be sufficiently obtained even if the contents of other elements are within the range of this embodiment. On the other hand, if the Mn content is 7.00% or more, even if the contents of other elements are within the range of this embodiment, δ ferrite is formed, and the hydrogen embrittlement resistance of the steel material decreases. Therefore, the Mn content is less than 3.00 to 7.00%. The preferred lower limit of the Mn content is 3.10%, more preferably 3.20%, and more preferably 3.30%. The preferred upper limit of the Mn content is 6.50%, more preferably 6.00%, more preferably 5.50%, more preferably 5.00%, and more preferably 4.90%.
[0041] Cr: 15.00~30.00% Chromium (Cr) enhances the hydrogen embrittlement resistance of steel. Cr also promotes the formation of dislocation cell structures. If the Cr content is less than 15.00%, these effects cannot be sufficiently obtained even if the contents of other elements are within the ranges of this embodiment. On the other hand, if the Cr content exceeds 30.00%, coarse M grains are formed even if the contents of other elements are within the ranges of this embodiment. 23 Carbides such as C6 are formed, which reduces the workability and toughness of the steel material and reduces hydrogen embrittlement resistance. Therefore, the Cr content is 15.00 to 30.00%. The preferred lower limit of the Cr content is 15.50%, more preferably 16.00%, and even more preferably 16.30%. The preferred upper limit of the Cr content is 27.00%, more preferably 25.00%, and even more preferably 22.00%.
[0042] Ni: 10.00~21.00% Nickel (Ni) stabilizes austenite, inhibits the formation of processing-induced martensite, and enhances the hydrogen embrittlement resistance of steel. Ni also makes it easier to form dislocation cell structures. If the Ni content is less than 10.00%, the above effects cannot be sufficiently obtained even if the contents of other elements are within the ranges of this embodiment. On the other hand, if the Ni content exceeds 21.00%, the above effects are saturated and the manufacturing cost increases even if the contents of other elements are within the ranges of this embodiment. Therefore, the Ni content is 10.00 to 21.00%. The preferred lower limit of the Ni content is 10.50%, more preferably 11.00%, more preferably 11.50%, more preferably 12.00%, and more preferably 13.20%. The preferred upper limit of the Ni content is 17.50%, more preferably 17.00%, and more preferably 16.50%.
[0043] Mo: 1.20~4.50% Molybdenum (Mo) enhances the hydrogen embrittlement resistance and strength of steel. Mo also refines crystal grains and makes it easier to generate dislocation cell structures. If the Mo content is less than 1.20%, this effect cannot be obtained even if the contents of other elements are within the range of this embodiment. On the other hand, if the Mo content exceeds 4.50%, the effect is saturated and the manufacturing cost increases even if the contents of other elements are within the range of this embodiment. Therefore, the Mo content is 1.20 to 4.50%. The preferred lower limit of the Mo content is 1.30%, more preferably 1.40%, and more preferably 1.60%. The preferred upper limit of the Mo content is 3.50%, more preferably 3.00%, and more preferably 2.50%.
[0044] P:0.050% or less Phosphorus (P) is an unavoidably contained impurity. That is, the P content is more than 0%. If the P content exceeds 0.050%, the hot workability and toughness of the steel material will decrease even if the contents of other elements are within the range of this embodiment. Therefore, the P content is 0.050% or less. A preferable upper limit of the P content is 0.030%, and more preferably 0.025%. It is preferable that the P content is as low as possible. However, excessive reduction of the P content increases the manufacturing cost. Therefore, in consideration of normal industrial production, a preferable lower limit of the P content is 0.001%, and more preferably 0.005%.
[0045] S: 0.050% or less Sulfur (S) is an unavoidably contained impurity. That is, the S content is more than 0%. If the S content exceeds 0.050%, the hot workability and toughness of the steel material will decrease even if the contents of other elements are within the range of this embodiment. Therefore, the S content is 0.050% or less. A preferable upper limit of the S content is 0.030%, more preferably 0.025%. The S content is preferably as low as possible. However, excessive reduction of the S content increases the manufacturing cost. Therefore, in consideration of normal industrial production, a preferable lower limit of the S content is 0.001%, more preferably 0.002%.
[0046] Al: 0.100% or less Aluminum (Al) is inevitably contained. That is, the Al content is more than 0%. Al deoxidizes steel. Even if even a small amount of Al is contained, this effect can be obtained to some extent. However, if the Al content exceeds 0.100%, oxides and intermetallic compounds are likely to be generated in the steel material even if the contents of other elements are within the range of this embodiment, and the toughness of the steel material decreases. Therefore, the Al content is 0.100% or less. The preferred lower limit of the Al content for more effectively deoxidizing the steel material is 0.001%, and more preferably 0.002%. The preferred upper limit of the Al content is 0.050%, and more preferably 0.040%. In this specification, the Al content means the content of sol.Al (acid-soluble Al).
[0047] N: 0.150~0.500% Nitrogen (N) enhances the strength of steel material. If the N content is less than 0.150%, the above effect cannot be sufficiently obtained even if the contents of other elements are within the range of this embodiment. On the other hand, if the N content exceeds 0.500%, coarse nitrides are likely to be formed even if the contents of other elements are within the range of this embodiment. Therefore, the N content is 0.150 to 0.500%. The preferred lower limit of the N content is 0.180%, more preferably 0.190%, and more preferably 0.200%. The preferred upper limit of the N content is 0.450%, more preferably 0.400%, more preferably 0.350%, and more preferably 0.300%.
[0048] The balance of the chemical composition of the austenitic stainless steel material according to the present embodiment is composed of Fe and impurities. Here, the impurities refer to substances that are mixed in from raw materials such as ore and scrap, or the manufacturing environment, during industrial production of the austenitic stainless steel material according to the present embodiment, and are permissible within a range that does not adversely affect the austenitic stainless steel material according to the present embodiment.
[0049] [Austenite grain size number] In the austenitic stainless steel material of this embodiment, the austenite grain size number according to ASTM E112 is 7.5 or more, where ASTM is the abbreviation for American Society for Testing and Material.
[0050] If the austenite grain size number is less than 7.5, the dislocation cell structure described below is unlikely to form. If the dislocation cell structure is not formed, the strength of the austenitic stainless steel material having the above-mentioned chemical composition will be low.
[0051] If the austenite grain size number is 7.5 or more, dislocation cell structures are formed in the austenitic stainless steel material having the above-mentioned chemical composition. Specifically, if the austenite grain size number is 7.5 or more, the crystal grains become fine. Therefore, the dislocations formed within the crystal grains are short. Short dislocations are easy to move and tend to become entangled with each other, which results in the formation of dislocation cell structures.
[0052] In the steel material having the above-mentioned chemical composition, if the austenite grain size number is 7.5 or more and the dislocation cell structure ratio in the microstructure is 50 to 80%, not only excellent hydrogen embrittlement resistance is obtained, but also high strength is obtained due to the synergistic effect of the refinement of the grain size and the dislocation cell structure. The preferable lower limit of the grain size number is 7.8, more preferably 7.9, and even more preferably 8.0.
[0053] The upper limit of the austenitic grain size number is not particularly limited. However, when an austenitic stainless steel material is manufactured by the manufacturing method described below, the austenitic grain size number is 11.0 or less. Therefore, in this embodiment, a preferred upper limit of the grain size number of the austenitic stainless steel material is 11.0. A more preferred upper limit of the grain size number of the austenitic stainless steel material is 10.5, more preferably 10.0, more preferably 9.8, and even more preferably 9.6.
[0054] The austenite grain size number is obtained by the following method. The austenitic stainless steel material is cut perpendicular to the longitudinal direction. When the austenitic stainless steel material is a steel pipe, as shown in FIG. 5, the thickness is defined as t (mm) in the cross section perpendicular to the longitudinal direction of the austenitic stainless steel material (hereinafter also referred to as the test surface). The t / 2 position in the thickness direction from the outer surface is defined as sampling position P1. The t / 4 position in the thickness direction from the outer surface is defined as sampling position P2. The t / 4 position in the thickness direction from the inner surface is defined as sampling position P3. The sample taken from sampling position P1 is called sample P1. The sample taken from sampling position P2 is called sample P2. The sample taken from sampling position P3 is called sample P3. Sample P1 is taken so that the center position of the test surface corresponds to approximately the t / 2 position. Sample P2 is taken so that the center position of the test surface corresponds to approximately the t / 4 position. The sample P3 is collected so that the center position of the test surface corresponds to the t / 4 position.
[0055] When the austenitic stainless steel material is a steel bar, as shown in FIG. 6, the radius is defined as R (mm) in the cross section (test surface) perpendicular to the longitudinal direction of the austenitic stainless steel material. The position R in the radial direction from the surface, that is, the center position of the test surface, is defined as the sampling position P1. In the diameter including the center position of the test surface, the position R / 2 in the radial direction from the surface at one end of the diameter is defined as the sampling position P2. The position R / 2 in the radial direction from the surface at the other end of the diameter is defined as the sampling position P3. Samples P1 to P3 are sampled from the sampling positions P1 to P3. Sample P1 is sampled so that the center position of the test surface corresponds to approximately the center position of the cross section of the steel bar. Sample P2 is sampled so that the center position of the test surface corresponds to approximately the R / 2 position. Sample P3 is sampled so that the center position of the test surface corresponds to approximately the R / 2 position.
[0056] When the austenitic stainless steel material is a steel plate, as shown in FIG. 7, the plate thickness is defined as t (mm) in a cross section (test surface) perpendicular to the longitudinal direction of the austenitic stainless steel material. The t / 2 position in the plate thickness direction from the top surface is defined as sampling position P1. The t / 4 position in the plate thickness direction from the top surface is defined as sampling position P2. The t / 4 position in the plate thickness direction from the bottom surface is defined as sampling position P3. Samples P1 to P3 are sampled from sampling positions P1 to P3. Sample P1 is sampled so that the center position of the test surface corresponds to approximately the t / 2 position. Sample P2 is sampled so that the center position of the test surface corresponds to approximately the t / 4 position. Sample P3 is sampled so that the center position of the test surface corresponds to approximately the t / 4 position.
[0057] The test surface of each of the samples P1 to P3 is mirror-polished. The mirror-polished test surface is corroded using a mixed acid (a solution of hydrochloric acid and nitric acid mixed in a ratio of 1:1) to reveal the austenite grain boundaries. The test surface of each of the samples P1 to P3 is subjected to a structural observation using an optical microscope. The magnification of the optical microscope for structural observation is 100 times. Three fields of view are selected arbitrarily on the test surface of each of the samples P1 to P3. The size of each field of view is 1000 μm × 1000 μm. The austenite grain size number is measured in each field in accordance with ASTM E112. The arithmetic mean value of the austenite grain size numbers obtained in the nine fields of view (three fields of view for each of the samples P1 to P3) is defined as the austenite grain size number of the austenitic stainless steel material.
[0058] [Dislocation cell structure] The austenitic stainless steel material of this embodiment further has a dislocation cell structure ratio of 50 to 80% in the microstructure, where the dislocation cell structure ratio is defined by the following method.
[0059] [Definition of dislocation cell structure ratio] In a cross section perpendicular to the longitudinal direction of the austenitic stainless steel material of this embodiment, 15 arbitrary fields of view, each with a size of 4.2 μm × 4.2 μm, are selected. A TEM image (bright field image) is generated for each selected field of view. In the generated TEM image, cell wall regions 101 with high dislocation density and low-density dislocation regions 102 with low dislocation density are identified. Of the multiple low-density dislocation regions 102 identified in each field of view, those with an area of 0.20 μm 2 A visual field in which nine or more low-density dislocation regions 102 exist is recognized as a visual field in which a dislocation cell structure is formed. The ratio of the number of visual fields in which a dislocation cell structure is formed to the total number of visual fields (15 visual fields) is defined as the dislocation cell structure ratio (%).
[0060] More specifically, the dislocation cell structure ratio is determined by the following method.
[0061] [Method for measuring dislocation cell structure ratio] Samples P1 to P3 for dislocation cell structure observation are taken from the above-mentioned sample taking positions P1 to P3 in a cross section perpendicular to the longitudinal direction of the austenitic stainless steel material. The test surface of each sample P1 to P3 is a cross section perpendicular to the longitudinal direction of the austenitic stainless steel material. Wet polishing is performed until the thickness of the samples P1 to P3 is 30 μm. After wet polishing, electrolytic polishing is performed on each sample P1 to P3 using a mixture of perchloric acid (10 vol.%) and ethanol (90 vol.%) to obtain thin film samples P1 to P3. A transmission electron microscope (TEM) is used to observe the structure of the test surface of each thin film sample P1 to P3. Specifically, TEM observation is performed on any five fields of view of the test surface of each sample. The size of each field of view is a rectangle of 4.2 μm × 4.2 μm. The acceleration voltage during TEM observation is 200 kV. <110> The observation target is the crystal grains that can be observed by the incident electron beam. A bright-field image is generated in each field of view.
[0062] Using the bright-field image of each field, whether each field has a dislocation cell structure or not is judged by the following method. In each bright-field image, a histogram showing the frequency of pixel values (0 to 255) is generated, and the median of the histogram is obtained. The number of pixels in the bright-field image of each field is not particularly limited, but may be, for example, 100,000 pixels or more and 150,000 pixels or less. The bright-field image is binarized using the median as a threshold value. In FIG. 3, which is an example of a binarized image, the black regions are regions with high dislocation density. Therefore, the black regions are recognized as cell wall regions 101. On the other hand, the white regions are regions with low dislocation density. Therefore, the white closed regions surrounded by the cell wall regions are recognized as low-density dislocation regions 102. The outer periphery of the white closed regions (low-density dislocation regions 102) is defined, and the area of each low-density dislocation region 102 is obtained. Then, when the area is less than 0.20 μm 2 The above low-density dislocation region 102 is recognized as a "dislocation cell."
[0063] In each field of view (4.2 μm × 4.2 μm), the dislocation cells (0.20 μm 2 The number of low dislocation density regions 102) having an area of 100 μm or more is determined. Then, when nine or more dislocation cells are present in each field of view, the microstructure of that field of view is recognized as a dislocation cell structure. Note that when three or more straight lines intersect with both of the two opposing sides (opposite sides) of the field of view (rectangular bright-field image of 4.2 μm × 4.2 μm), the field of view is recognized as having a planar structure and is not recognized as a dislocation cell structure. The number of fields of view with dislocation cell structures among the 15 fields of view observed is determined. Then, the dislocation cell structure rate (%) is defined by the following formula. Dislocation cell structure rate = number of fields of view recognized as having dislocation cell structure / total number of fields of view × 100
[0064] In the austenitic stainless steel material according to this embodiment, the dislocation cell structure ratio determined by the above definition is 50% or more. Therefore, the austenitic stainless steel material according to this embodiment not only has excellent hydrogen embrittlement resistance, but also has high strength. In the cell wall region 101, dislocations are densely packed and entangled with each other. Therefore, the dislocations that make up the dislocation cell structure are unlikely to move. As a result, it is believed that the strength of the austenitic stainless steel material is increased.
[0065] The upper limit of the dislocation cell structure ratio is not particularly limited, and a higher dislocation cell structure ratio is preferable. However, if the dislocation cell structure ratio is 50 to 80%, excellent hydrogen embrittlement resistance and sufficiently high strength can be obtained. The preferred lower limit of the dislocation cell structure ratio is 51%, more preferably 52%, more preferably 55%, more preferably 57%, more preferably 58%, more preferably 59%, and more preferably 60%.
[0066] [Number density of coarse precipitates in steel] In the austenitic stainless steel material of this embodiment, the number density of precipitates with a major axis of 1.0 μm or more is 5.0 precipitates / 0.2 mm 2 The following is the result.
[0067] In the austenitic stainless steel material having the above-mentioned chemical composition, precipitates with a major axis of 1.0 μm or more are defined as "coarse precipitates". The precipitates are carbides, nitrides, carbonitrides, etc., and examples thereof include M 23 It is a C6 type carbide. The coarse precipitates are likely to adsorb hydrogen at the interface with the parent phase (austenite). Therefore, if there are a large number of coarse precipitates, the hydrogen embrittlement resistance of the austenitic stainless steel material decreases. Note that precipitates with a major axis of less than 1.0 μm are less likely to adsorb hydrogen than coarse precipitates. Therefore, compared to coarse precipitates, the effect on hydrogen embrittlement resistance is extremely small. Therefore, in this embodiment, attention is focused on the coarse precipitates.
[0068] The number of coarse precipitates was 5.0 / 0.2 mm. 2 If the number of coarse precipitates is more than 5.0 / 0.2 mm, sufficient hydrogen embrittlement resistance cannot be obtained even if the content of each element in the chemical composition of the austenitic stainless steel material is within the range of this embodiment, the austenite grain size number according to ASTM E112 is 7.5 or more, and the dislocation cell structure ratio is 50 to 80%. 2If the content of each element in the chemical composition of the austenitic stainless steel material is within the range of this embodiment, the austenite grain size number in accordance with ASTM E112 is 7.5 or more, and the dislocation cell structure ratio is 50 to 80%, excellent hydrogen embrittlement resistance can be obtained.
[0069] [Method for measuring the number density of coarse precipitates] The number density of the coarse precipitates can be measured by the following method. Samples for measuring the number density of the coarse precipitates are collected from the above-mentioned sample collection positions P1 to P3. Hereinafter, the sample collected from position P1 will be referred to as sample P1. The sample collected from position P2 will be referred to as sample P2. The sample collected from position P3 will be referred to as sample P3.
[0070] The test surface of each of samples P1 to P3 is a cross section perpendicular to the longitudinal direction of the austenitic stainless steel material. The test surface is mirror-polished. After mirror-polishing, samples P1 to P3 are etched using a mixed acid (a solution of hydrochloric acid and nitric acid mixed in a ratio of 1:1) to reveal the austenite grain boundaries and precipitates. The test surface after etching is observed in one field of view using a SEM as a backscattered electron image. The field of view size is 400 μm x 500 μm. The precipitates in the field of view can be identified by their contrast.
[0071] The major axis of the precipitate is measured. Specifically, the longest straight line among the straight lines connecting any two points at the interface between the precipitate and the parent phase (austenite) is defined as the major axis (μm). Precipitates with a major axis of 1.0 μm or more are identified as "coarse precipitates". The number of identified coarse precipitates is counted. The number of coarse precipitates obtained and the visual field area (0.2 mm2) are then recorded. 2 ) and the number density (pieces / 0.2 mm) of coarse precipitates in each sample P1 to P3. 2 The arithmetic average of the three particle densities is then calculated as the particle density of the coarse precipitates (particles / 0.2 mm 2 ) is defined as
[0072] As described above, the austenitic stainless steel material of this embodiment has each element in the chemical composition within the above-mentioned range, an austenite grain size number according to ASTM E112 of 7.5 or more, a dislocation cell structure ratio of 50 to 80%, and a number density of precipitates with a major axis of 1.0 μm or more of 5.0 precipitates / 0.2 mm 2 Therefore, the austenitic stainless steel material of this embodiment not only has excellent hydrogen embrittlement resistance, but also has high tensile strength.
[0073] [Shape of the austenitic stainless steel material according to this embodiment] The shape of the austenitic stainless steel material of this embodiment is not particularly limited. The austenitic stainless steel material of this embodiment may be a steel pipe. The austenitic stainless steel material of this embodiment may be a steel bar. The austenitic stainless steel material of this embodiment may be a steel plate. The austenitic stainless steel material of this embodiment may be in a shape other than a steel pipe, a steel bar, or a steel plate.
[0074] [Applications of the austenitic stainless steel material according to this embodiment] The austenitic stainless steel material of this embodiment is widely applicable to applications requiring hydrogen embrittlement resistance and high strength. The austenitic stainless steel material of this embodiment is particularly applicable to components for high-pressure hydrogen gas environment applications. High-pressure hydrogen gas environment applications include, for example, components for high-pressure hydrogen containers mounted on fuel cell vehicles and components for high-pressure hydrogen containers installed at hydrogen stations that supply hydrogen to fuel cell vehicles. However, the austenitic stainless steel material of this embodiment is not limited to high-pressure hydrogen gas environment applications. As described above, the austenitic stainless steel material of this embodiment is widely applicable to applications requiring hydrogen embrittlement resistance and high strength.
[0075] [Manufacturing method] A method for producing an austenitic stainless steel material according to this embodiment will be described below. The method for producing an austenitic stainless steel material described below is one example of the method for producing an austenitic stainless steel material according to this embodiment. Therefore, an austenitic stainless steel material having the above-mentioned configuration may be produced by a production method other than the production method described below. However, the production method described below is a preferred example of the method for producing an austenitic stainless steel material according to this embodiment.
[0076] The manufacturing method of the austenitic stainless steel material according to the present embodiment includes a preparation step, a heat treatment step, and a cold working step. Each step will be described in detail.
[0077] [Preparation process] In the preparation step, an intermediate steel material having the above-mentioned chemical composition is prepared. The intermediate steel material having the above-mentioned chemical composition may be purchased from a third party. Alternatively, the intermediate steel material may be manufactured. When the intermediate steel material is manufactured, it is manufactured, for example, by the following method.
[0078] Molten steel having the above-mentioned chemical composition is produced by a known method. The produced molten steel is used to produce a material by a known casting method. For example, an ingot is produced by an ingot casting method. A cast piece (slab, bloom, billet, etc.) may be produced by a continuous casting method. The ingot may be subjected to hot processing such as blooming and hot forging to produce a slab, bloom, or billet. The material is produced by the above-mentioned steps.
[0079] The prepared material is subjected to hot working (hot working process). Examples of hot working include hot forging, hot extrusion, and hot rolling. Examples of hot forging include stretch forging. Examples of hot rolling include tandem rolling using a tandem rolling mill including a plurality of rolling stands arranged in a row (each rolling stand has a pair of work rolls) to perform rolling in multiple passes, or reverse rolling using a reverse rolling mill having a pair of work rolls to perform rolling in multiple passes. Examples of hot extrusion include hot extrusion using the Eugène-Sejournet method. An intermediate steel material may be manufactured by the above manufacturing process. A preferred heating temperature before hot working is 950 to 1200°C. A preferred area reduction rate in hot working is 50% or more. Here, the area reduction rate (%) is defined by the following formula. Reduction of area = (1 - cross-sectional area perpendicular to the longitudinal direction of intermediate steel material after hot working / cross-sectional area perpendicular to the longitudinal direction of material before hot working) x 100
[0080] The lower limit of the area reduction rate is preferably 55%, and more preferably 60%. The upper limit of the area reduction rate is not particularly limited. When the equipment load is taken into consideration, the upper limit of the area reduction rate is preferably, for example, 90%.
[0081] [Heat treatment process] In the heat treatment process, the intermediate steel material having the above-mentioned chemical composition is subjected to heat treatment. Specifically, it is held at a heat treatment temperature T1 (°C). After the holding time has elapsed, the intermediate steel material is quenched. The quenching is, for example, water cooling or oil cooling. The cooling rate is, for example, 100°C / sec or more. The heat treatment temperature T1 (°C) is as follows. Heat treatment temperature T1: 1000~1150(℃)
[0082] [About heat treatment temperature T1] If the heat treatment temperature T1 is less than 1000°C, the precipitates in the intermediate steel material do not dissolve sufficiently and remain in the steel material. In this case, the number density of the coarse precipitates is 5.0 precipitates / 0.2 mm 2On the other hand, if the heat treatment temperature T1 exceeds 1150°C, the austenite grains will become coarse, and the austenite grain size number of the produced austenitic stainless steel material will be less than 7.5. Therefore, the heat treatment temperature T1 is 1000 to 1150°C. The preferred lower limit of the heat treatment temperature T1 is 1020°C, and more preferably 1040°C. The preferred upper limit of the heat treatment temperature T1 is 1130°C. The holding time at the heat treatment temperature T1 is not particularly limited. The holding time is, for example, 2 to 30 minutes.
[0083] As described above, the intermediate steel material is quenched after being heat-treated at the heat treatment temperature T1. This prevents the alloying elements that have been solid-dissolved by the heat treatment from precipitating during cooling. The quenching is, for example, water cooling or oil cooling. As a water cooling method, the steel material may be immersed in a water tank for cooling, or the steel material may be quenched by shower water cooling or mist cooling.
[0084] When steel is manufactured by hot working, the heat treatment process may be performed on the steel immediately after the completion of the hot working. For example, the steel temperature (finishing temperature) immediately after the completion of the hot working may be set to 1000 to 1150°C, and then rapidly cooled. In this case, the same effect as the heat treatment using the heat treatment furnace described above can be obtained. When the steel immediately after the completion of the hot working is rapidly cooled, the heat treatment temperature T1 of the heat treatment process corresponds to the temperature (°C) of the intermediate steel immediately after the hot working.
[0085] [Cold working process] In the cold working process, cold working is performed on the intermediate steel material after the heat treatment process. Cold working includes, for example, cold drawing, cold forging, cold rolling, etc. For example, when the steel material is a steel pipe or a steel bar, cold drawing is performed. When the steel material is a steel plate, cold rolling is performed.
[0086] The area reduction rate RR in the cold working process is 15.0% or more. The area reduction rate RR (%) in the cold working process is defined by the following formula. Area reduction rate RR = (1-(Cross-sectional area of intermediate steel after completion of cold working process / Cross-sectional area of intermediate steel before cold working process)) x 100 Here, the cross-sectional area of the intermediate steel material is the area (mm 2 )
[0087] If the area reduction rate RR in the cold working process is less than 15.0%, the dislocation cell structure rate will be less than 50%. Therefore, a sufficiently high strength cannot be obtained. Therefore, the area reduction rate RR in the cold working process is 15.0% or more. The preferable lower limit of the area reduction rate RR is 18.0%, more preferably 19.0%, and even more preferably 20.0%.
[0088] The upper limit of the area reduction rate RR is not particularly limited. However, if the area reduction rate RR exceeds 80.0%, the effect of improving the strength is saturated. Therefore, the upper limit of the area reduction rate RR is preferably 80.0%. The upper limit of the area reduction rate RR is more preferably 75.0%, and even more preferably 70.0%.
[0089] The above manufacturing process provides a steel sheet having the above-mentioned chemical composition, an austenite grain size number according to ASTM E112 of 7.5 or more, a dislocation cell structure ratio of 50 to 80%, and a number density of precipitates with a major axis of 1.0 μm or more of 5.0 precipitates / 0.2 mm 2 It is possible to produce an austenitic stainless steel material having the following properties:
[0090] The above-mentioned manufacturing method is one example of a method for manufacturing the austenitic stainless steel material of this embodiment. Therefore, the austenitic stainless steel material of this embodiment has the above-mentioned chemical composition, an austenite grain size number according to ASTM E112 of 7.5 or more, a dislocation cell structure ratio of 50 to 80%, and a number density of precipitates with a major axis of 1.0 μm or more of 5.0 precipitates / 0.2 mm 2 The austenitic stainless steel material of the present embodiment may be manufactured by other manufacturing methods as long as the manufacturing method is as follows. The manufacturing method described above is a suitable example for manufacturing the austenitic stainless steel material of the present embodiment. EXAMPLES
[0091] The effects of the austenitic stainless steel material of this embodiment will be described more specifically with reference to examples. The conditions in the following examples are one example of conditions adopted to confirm the feasibility and effects of the austenitic stainless steel material of this embodiment. Therefore, the austenitic stainless steel material of this embodiment is not limited to this one example of conditions.
[0092] An ingot was produced by vacuum melting 180 kg of austenitic stainless steel having the chemical composition shown in Table 1. The ingot was subjected to hot forging and hot rolling to produce a steel plate (intermediate steel material) having a width of 200 mm and a thickness of 20 mm. In all test numbers (see Table 2), the heating temperature during hot forging was 950 to 1100°C, and the reduction in area during hot forging was 65% in all cases.
[0093] [Table 1]
[0094] A heat treatment process was carried out on the intermediate steel materials of each test number thus produced. The heat treatment temperature T1 in the heat treatment process was as shown in Table 2. The holding time at the heat treatment temperature T1 was 10 to 30 minutes. The steel plates held at the heat treatment temperature T1 were water-cooled immediately after being removed from the heat treatment furnace.
[0095] [Table 2]
[0096] A cold working process was carried out on the intermediate steel material after the heat treatment process. Cold rolling was carried out as the cold working process. The area reduction rate RR in the cold working process was as shown in Table 2. Note that the cold working process was not carried out in test number 16. Therefore, the area reduction rate RR in the cold working process of test number 16 was 0%. An austenitic stainless steel material (steel plate) was produced by the above manufacturing process.
[0097] [Evaluation test] [Grain size number measurement test] As shown in Figure 7, in a cross section (test surface) perpendicular to the longitudinal direction of an austenitic stainless steel material, where the thickness is t (mm), sample P1 was taken from the top surface in the thickness direction at t / 2 position, sample P2 was taken from the top surface in the thickness direction at t / 4 position, and sample P3 was taken from the bottom surface in the thickness direction at t / 4 position. Sample P1 was taken so that the center position of the test surface approximately corresponds to the t / 2 position, sample P2 was taken so that the center position of the test surface approximately corresponds to the t / 4 position, and sample P3 was taken so that the center position of the test surface approximately corresponds to the t / 4 position.
[0098] The test surface of each of the samples P1 to P3 was mirror-polished. The mirror-polished test surface was etched using a mixed acid (a solution of hydrochloric acid and nitric acid mixed at a ratio of 1:1) to reveal the austenite grain boundaries. The test surface of each of the samples P1 to P3 was subjected to microstructural observation using an optical microscope. The magnification of the optical microscope for the microstructural observation was 100 times. Three fields of view were selected arbitrarily on the test surface of each of the samples P1 to P3. The size of each field of view was 1000 μm × 1000 μm. The austenite grain size number was measured in each field in accordance with ASTM E112. The arithmetic mean value of the austenite grain size numbers obtained in nine fields of view (three fields of view for each of the samples P1 to P3) was defined as the austenite grain size number. The obtained austenite grain size numbers are shown in Table 2.
[0099] [Dislocation cell structure rate calculation test] As shown in FIG. 7, samples P1 to P3 for dislocation cell structure observation were taken from a cross section (test surface) perpendicular to the longitudinal direction of the austenitic stainless steel material, with the thickness being t (mm), at a sampling position P1 at t / 2 in the thickness direction from the top surface, a sampling position P2 at t / 4 in the thickness direction from the top surface, and a sampling position P3 at t / 4 in the thickness direction from the bottom surface. The test surface of each sample P1 to P3 was a cross section perpendicular to the longitudinal direction of the austenitic stainless steel material. Wet polishing was performed until the sample thickness was 30 μm. After wet polishing, each sample P1 to P3 was electrolytically polished using a mixture of perchloric acid (10 vol.%) and ethanol (90 vol.%) to prepare thin film samples P1 to P3. The test surface of each thin film sample P1 to P3 was subjected to structure observation using a TEM. Specifically, TEM observation was performed on five arbitrary fields of view (five fields for thin film sample P1, five fields for thin film sample P2, and five fields for thin film sample P3) on the test surface of each thin film sample P1 to P3. The size of each field of view was 4.2 μm × 4.2 μm. The accelerating voltage during TEM observation was 200 kV. <110> The observation targets were crystal grains that could be observed with an incident electron beam of 1000 nm. Bright-field images were generated in each field of view.
[0100] Using the bright-field image of each field, it was judged whether each field had a dislocation cell structure or not by the following method. In the obtained bright-field image, a histogram showing the frequency of pixel values (0 to 255) was generated, and the median of the histogram was calculated. The number of pixels in the bright-field image of each field was 117,306 pixels. The bright-field image was binarized using the median as a threshold value. In the binarized image, low-density dislocation regions 102, which are white regions, were identified. The outer limits of the low-density dislocation regions 102 were defined, and the area of each low-density dislocation region 102 was calculated. If the area was less than 0.20 μm 2 The above low-density dislocation regions 102 were recognized as "dislocation cells." 2The number of low dislocation density regions102) with an area of 100 μm or more was counted. When nine or more dislocation cells were present in each field of view, the microstructure in that field of view was determined to be a dislocation cell structure. The number of fields of view with dislocation cell structures was counted out of the 15 fields of view observed. The dislocation cell structure rate (%) was then defined by the following formula. Dislocation cell structure rate = number of fields of view recognized as having dislocation cell structure / total number of fields of view × 100 The dislocation cell structure rates obtained are shown in Table 2.
[0101] [Slow strain rate tensile test] A slow strain rate tensile test (SSRT) was conducted on the steel plates with each test number. Specifically, multiple round bar tensile test pieces were prepared from the center of the thickness of the steel plate. The diameter of the parallel part of the round bar tensile test piece was 3.0 mm, and the parallel part was parallel to the longitudinal direction of the steel plate (corresponding to the rolling direction). The central axis of the parallel part was approximately the same as the center of the thickness of the steel plate. The surface of the parallel part of the round bar tensile test piece was polished with #150, #400, and #600 Emily paper in that order, and then degreased with acetone. Using the obtained round bar test piece, a strain rate of 3.0 × 10 was applied in air at room temperature. -5 A tensile test was carried out at 1000 rpm / sec to obtain the reduction in area at break (elongation at break, unit: %) and the tensile strength (MPa). The obtained tensile strengths are shown in Table 2.
[0102] In addition, a different round bar tensile test piece was used and subjected to strain rate of 3.0×10 in hydrogen gas at 90 MPa. -5 A tensile test was carried out at 1000 / sec to obtain the reduction in area at break (elongation at break, unit: %). The relative reduction in area at break (%) for each test number was calculated using the following formula. Relative reduction of area at break = reduction of area at break in hydrogen gas at 90 MPa / reduction of area at break in air at room temperature x 100 If the relative reduction in area at fracture was 90.0% or more, it was determined that the hydrogen embrittlement resistance was excellent (marked with "○" in the "Relative reduction in area at fracture evaluation" column in Table 2). On the other hand, if the relative reduction in area at fracture was less than 90.0%, it was determined that the hydrogen embrittlement resistance was low (marked with "×" in the "Relative reduction in area at fracture evaluation" column in Table 2).
[0103] [Test Results] The test results are shown in Table 2. The chemical compositions of test numbers 1 to 7 were appropriate, and the manufacturing methods were also appropriate. Therefore, the austenitic stainless steel materials had an austenite grain size number of 7.5 or more according to ASTM E112. Furthermore, the dislocation cell structure ratio was 50 to 80% in all cases. Furthermore, the number density of coarse precipitates was 5.0 pieces / 0.2 mm 2 As a result, in test numbers 1 to 7, the tensile strength was 1000 MPa or more, and high tensile strength was obtained. Furthermore, the relative reduction in area at break was 90.0% or more, and excellent hydrogen embrittlement resistance was demonstrated.
[0104] On the other hand, in test number 8, the Ni content was too low, so the relative reduction in area at fracture was less than 90.0%, and the hydrogen embrittlement resistance was low.
[0105] In test number 9, the Cr content was too low, so the relative reduction in area at fracture was less than 90.0%, and the hydrogen embrittlement resistance was low.
[0106] In test number 10, the Cr content was too high. As a result, the number density of coarse precipitates was 5.0 pieces / 0.2 mm. 2 As a result, the relative reduction in area was less than 90.0%, and the hydrogen embrittlement resistance was low. This is thought to be due to the excessive formation of Cr carbides, which became the starting point for hydrogen cracking.
[0107] In test number 11, the Mn content was too low. Therefore, the dislocation cell structure ratio was less than 50%. As a result, the relative reduction in area at fracture was less than 90.0%, and the hydrogen embrittlement resistance was low.
[0108] In test number 12, the Mo content was too low. Therefore, the austenite grain size number was low at less than 7.5. Furthermore, the dislocation cell structure ratio was less than 50%. As a result, the tensile strength was less than 1000 MPa. Furthermore, the relative reduction in area at fracture was less than 90.0%, and the hydrogen embrittlement resistance was low.
[0109] In test number 13, the chemical composition was appropriate, but the heat treatment temperature T1 in the heat treatment process was too high. Therefore, the austenite grain size number was low at less than 7.5. Furthermore, the dislocation cell structure rate was less than 50%. As a result, the tensile strength was less than 1000 MPa.
[0110] In test number 14, the chemical composition was appropriate, but the heat treatment temperature T1 in the heat treatment process was too low. As a result, the number density of coarse precipitates was 5.0 pieces / 0.2 mm 2 As a result, the relative reduction in area at fracture was less than 90.0%, and the hydrogen embrittlement resistance was low.
[0111] In test number 15, the area reduction rate RR in the cold working process was too low. In test number 16, the cold working process was not performed. Therefore, in test numbers 15 and 16, the dislocation cell structure rate was less than 50%. Therefore, the tensile strength was less than 1000 MPa.
[0112] The above describes the embodiments of the present invention. However, the above-described embodiments are merely examples for carrying out the present invention. Therefore, the present invention is not limited to the above-described embodiments, and the above-described embodiments can be appropriately modified and carried out without departing from the spirit of the present invention. [Explanation of symbols]
[0113] 101 Cell wall region 102 Low density dislocation region
Claims
1. An austenitic stainless steel material, The chemical composition, in mass%, is C: 0.100% or less, Si: 1.00% or less, Mn: 3.00 to less than 7.00%; Cr: 15.00-27.00%, Ni: 10.00-21.00%, Mo: 1.20-4.50%, P: 0.050% or less, S: 0.050% or less, Al: 0.100% or less, N: 0.150 to 0.500%, and The balance is Fe and impurities, The austenite grain size number according to ASTM E112 is 7.5 or more, In a cross section perpendicular to the longitudinal direction of the austenitic stainless steel material, a dislocation cell structure ratio is 50 to 80%, The number density of precipitates with a major axis of 1.0 μm or more is 5.0 / 0.2 mm 2 Below is the Austenitic stainless steel material.
2. 2. The austenitic stainless steel material according to claim 1, The austenite grain size number is 8.0 or more. Austenitic stainless steel material.
3. The austenitic stainless steel material according to claim 1 or 2, The dislocation cell structure rate is 55% or more. Austenitic stainless steel material.
4. The austenitic stainless steel material according to any one of claims 1 to 3, The number density of the precipitates having a major axis of 1.0 μm or more is 4.8 precipitates / 0.2 mm 2 Below is the Austenitic stainless steel material.
Citation Information
Patent Citations
Corrosion-resistant, high-strength austenitic stainless steel
JP1995188863A
Austenitic stainless steel and method for producing same
WO2015159554A1
Austenitic stainless steel and manufacturing method therefor
WO2016068009A1
Austenitic stainless steel material
WO2017175739A1