Pellet manufacturing method
A method for producing acrylic resin pellets with specific size and physical properties, along with controlled cooling conditions, addresses the instability in metering and molding defects, achieving stable and defect-free production of acrylic resin products.
Patent Information
- Application Number
- JP2021045267
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-03-18
- Publication Date
- 2024-09-26
- Estimated Expiration
- 2041-03-18
AI Technical Summary
Existing methods for producing acrylic resin pellets, particularly those with ring structures, face challenges in stable metering and molding due to instability in the injection molding process, leading to defects such as silver streaks and uneven material distribution.
A method involving the production of acrylic resin pellets with specific size and physical properties, including a major axis of 4.5 mm or less, melt flow rate of 2 g/10 minutes at 230°C, weight average molecular weight of 100,000 or less, and molecular weight distribution of 2.5 or less, combined with controlled cooling conditions in the injection molding machine to stabilize metering and prevent defects.
The method stabilizes metering during molding and reduces defects like silver streaks in molded products, ensuring efficient and consistent production of high-quality acrylic resin products.
Smart Images

Figure 0007556809000007 
Figure 0007556809000004 
Figure 0007556809000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing novel pellets (resin pellets), etc. [Background technology]
[0002] Acrylic resins, such as polymethyl methacrylate (PMMA), are used as optical materials because of their high transparency. Among these acrylic resins, acrylic polymers having a ring structure in the main chain are being developed because of their heat resistance. For example, Patent Document 1 discloses a copolymer having methyl (meth)acrylate units, methacrylic acid units, and glutaric anhydride units. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] International Publication No. 2017 / 022393 Brochure Summary of the Invention [Problem to be solved by the invention]
[0004] An object of the present invention is to provide a novel method for producing pellets (resin pellets, resin composition) (and further, pellets themselves).
[0005] Another object of the present invention is to provide a novel molding method (a method for producing a molded product). [Means for solving the problem]
[0006] As described above, acrylic resins are widely used, and attempts are being made to introduce a ring structure into acrylic resins from the viewpoint of heat resistance, etc. It has been difficult to stably produce pellets of such acrylic resins by a strand method, etc. This tendency is particularly noticeable in acrylic resins having a ring structure, which are relatively hard and brittle.
[0007] Under these circumstances, the present inventors obtained pellets of acrylic resin (particularly, acrylic resin having a ring structure) by a hot-cut method or the like, but found that when such pellets (hot-cut pellets, etc.) are used for molding, the measurement in a molding machine (injection molding machine, etc.) may become unstable, and appearance / molding defects (for example, silver streaks in a molded product) may be easily caused.
[0008] That is, as shown in FIG. 1, a molding machine (such as an injection molding machine) typically includes a cylinder (cylinder portion) 2, a nozzle portion Hn equipped with a nozzle 1 connected to the front end of the cylinder 2, and a hopper 3 connected to the rear portion H3 of the cylinder 2 for feeding molding material (such as resin pellets) into the cylinder 2.
[0009] A screw consisting of a front section (metering section) S1, a middle section (compression section) S2, and a rear section (supply section) S3 is housed within cylinder 2, and these correspond to the front section (metering section) H1, the middle section (compression section) H2, and the rear section (supply section) H3 of cylinder 2 when the screw is pushed in (the screw is moved toward the nozzle).
[0010] Temperature measuring devices (thermocouples, etc.) 4 are installed in each part of the cylinder, and a cooling device (a cooling jacket such as a water-cooled jacket) H4 is installed around the rear part H3 of the cylinder (or the base end of H3, below the hopper 3) so as to surround the periphery (outer periphery). This cooling device H4 can also be called the cooling means (device) for the rear part H3 of the cylinder (or its base end, below the hopper).
[0011] The molding material is charged and transferred from a hopper 3 and melted in a cylinder 2. This molten molding material is supplied to a mold (not shown) through a nozzle 1 and becomes a desired molded body.
[0012] In such a molding machine, as described above, molding material such as pellets is fed from the hopper 3 to the supply section H3 (S3). However, it has been found that if the pellets (hot-cut pellets, etc.) are acrylic resin (especially acrylic resin having a ring structure) (or a material containing said resin), the weighing in the weighing section S1 (H1) may become unstable.
[0013] The reason for this instability is unclear, but one possible contributing factor is that for some reason (for example, the pellets cracking after being fed into the supply section (before melting)), it is difficult for the pellets to receive shear (by the screw) inside the cylinder, and the pellets are metered in the metering section in an insufficiently melted state.
[0014] On the other hand, according to the study by the present inventors, it was found that when acrylic resins (especially acrylic resins having a ring structure) are used in injection molding, the occurrence frequency of appearance and molding defects such as silver streaks, coloring or color tone (YI) varies depending on the injection molding conditions. The reason for this is also unclear, but some reason (for example, unstable weighing makes it difficult for gas to escape, or fluctuations in thermal history make it easier for gas to be generated by thermal decomposition, etc.) is thought to be one of the causes.
[0015] In the midst of this, the present inventor has found that a novel method for producing pellets can be provided by specifying the size of the pellets, and that pellets obtained by this method (for example, hot-cut pellets) can improve the above-mentioned unstable metering (and even silver streaks) even when an acrylic resin having a ring structure [particularly an acrylic resin having a relatively small Mw or a relatively large MFR and having a ring structure (for example, a cyclic ester structure)] is used (and even when hot-cut pellets, etc. are used), and that silver streaks (and even unstable metering, etc.) can be improved by specifying the cooling conditions of the supply section in an injection molding machine (injection device) in relation to the physical properties of the molding material (resin) used, and thus completed the present invention.
[0016] That is, the present invention relates to the following inventions, etc. [1] A method for producing resin pellets, comprising the steps of: The resin contains an acrylic resin (A), A method of cutting resin (so that the major axis is 4.5 mm or less) and producing pellets (resin pellets) with a major axis of 4.5 mm or less. [2] The method according to [1], wherein the acrylic resin (A) has a ring structure. [3] The method according to [1] or [2], wherein the acrylic resin (A) has a cyclic ester structure. [4] The method according to any one of [1] to [3], wherein the acrylic resin (A) (or the resin) has a melt flow rate of 2 g / 10 min or more at 230° C. under a load of 3.8 kg as determined in accordance with JIS K 7210. [5] The method according to any one of [1] to [4], wherein the acrylic resin (A) (or the resin) has a weight average molecular weight of 100,000 or less. [6] The method according to any one of [1] to [5], wherein the molecular weight distribution of the acrylic resin (A) (or the resin) is 2.5 or less. [7] The method according to any of [1] to [6], wherein the acrylic resin (A) satisfies at least one of the following properties selected from a melt flow rate of 2 g / 10 min or more at 230° C. under a load of 3.8 kg, in accordance with JIS K 7210, a weight average molecular weight of 100,000 or less, and a molecular weight distribution of 2.5 or less, and has a cyclic ester structure. [8] The method according to any one of [1] to [7], wherein a molten resin is cut (hot cut). [9] The method according to any one of [1] to [8], wherein a resin extruded from a die (extrusion die) of an extruder is cut in a molten state (hot cut).
[10] The method according to any one of [1] to [9], wherein the short diameter of the pellet is 4.5 mm or less.
[11] The method according to any one of [1] to
[10] , wherein the pellet has a major axis and a minor axis of 4.0 mm or less.
[12] The method according to any one of [1] to
[11] , wherein the pellet has a thickness of 3.5 mm or less.
[13] The method according to any one of [1] to
[12] , wherein the pellets are for injection molding [for use in an injection molding machine (injection device)].
[14] Pellets produced by any of the methods listed below: [1] -
[13] .
[15] A method for injection molding a resin (a method for producing a molded product by injection molding), comprising the steps of: The resin contains an acrylic resin (A), A method in which Tg-Tj (℃) is 80 or less, where Tj (℃) is the temperature of the cooling device installed in the supply section (or below the hopper) of the cylinder of an injection molding machine (injection unit) and Tg (℃) is the glass transition temperature of the resin.
[16] The method according to
[15] , wherein the acrylic resin (A) has a ring structure.
[17] The method according to
[15] or
[16] , wherein the acrylic resin (A) has a cyclic ester structure.
[18] The method according to any one of
[15] to
[17] , wherein the acrylic resin (A) (resin (A)) has a melt flow rate of 2 g / 10 min or more at 230° C. under a load of 3.8 kg in accordance with JIS K 7210.
[19] The method according to any one of
[15] to
[18] , wherein the acrylic resin (A) has a weight average molecular weight of 100,000 or less.
[20] The method according to any one of
[15] to
[19] , wherein the acrylic resin (A) (or the resin) has a molecular weight distribution of 2.5 or less. [twenty one] The method according to any one of
[15] to
[20] , wherein the acrylic resin (A) has a cyclic ester structure. [twenty two] The method according to any one of
[15] to
[21] , wherein pellets having a major axis of 4.5 mm or less are used as the resin. [twenty three] The method according to any one of
[15] to
[22] , wherein Tg-Tj (°C) is 70 or less. [twenty four] the acrylic resin (A) is an acrylic resin having a cyclic ester structure and satisfying at least one of the following: a melt flow rate of 2 g / 10 min or more at 230° C. under a load of 3.8 kg, a weight average molecular weight of 100,000 or less, and a molecular weight distribution of 2.5 or less, in accordance with JIS K 7210; The method according to any one of
[15] to
[23] , wherein pellets each having a major axis and a minor axis of 4.0 mm or less are used as the resin. [twenty five] The method according to any one of
[15] to
[24] further comprises a pellet production step of producing resin pellets by the method according to any one of [1] to
[13] , and uses the resin pellets obtained in the pellet production step as the resin. Effect of the Invention
[0017] According to one aspect of the present invention, a method for producing novel pellets (resin pellets, resin compositions) can be provided. In such a method, the pellet size is adjusted to a specific size, and even if the resin constituting the pellet is an acrylic resin such as an acrylic resin having a ring structure (particularly, an acrylic resin having a ring structure with a small Mw or a large MFR), the metering during molding can be efficiently stabilized (and silver streaks in the molded product can be efficiently prevented).
[0018] According to another aspect of the present invention, a novel molding method (a method for manufacturing a molded product) can be provided. In such a method, the cooling conditions during molding (in a molding machine) are adjusted to specific conditions in relation to the physical properties (glass transition temperature) of the resin used, and appearance or molding defects in molded products such as silver streaks (and even unstable weighing during molding) can be efficiently improved.
[0019] According to these aspects of the present invention, there are also provided pellets and molded products produced by the above-mentioned methods. [Brief description of the drawings]
[0020] [Figure 1] FIG. 1 is a diagram (cross-sectional view) showing a typical molding machine (injection molding machine, injection unit). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0021] <Pellet manufacturing method> In one aspect of the present invention, a method for producing resin pellets is provided.
[0022] [resin] The resin is not limited, but may usually contain at least an acrylic resin (sometimes referred to as acrylic resin (A) etc.). Such an acrylic resin may have a ring structure, as described later. The acrylic resin is usually a thermoplastic resin (resin, polymer). The method for producing such an acrylic resin is not particularly limited, but the acrylic resin may be produced by the method described below.
[0023] The acrylic resin (A) may usually have a (meth)acrylic acid ester unit [a unit (structural unit) derived from a (meth)acrylic acid ester].
[0024] The (meth)acrylic acid ester constituting the (meth)acrylic acid ester unit is not particularly limited, but examples thereof include aliphatic (meth)acrylates [e.g., (meth)acrylic acid alkyl esters (e.g., (meth)acrylic acid C such as methyl (meth)acrylate, ethyl (meth)acrylate, and butyl (meth)acrylate]. 1-18 alkyl), etc.], alicyclic (meth)acrylates [e.g., (meth)acrylic acid cycloalkyl esters (e.g., (meth)acrylic acid C such as cyclopropyl (meth)acrylate and cyclobutyl (meth)acrylate, etc. 3-20cycloalkyl), bridged cyclic (meth)acrylates (e.g., isobornyl (meth)acrylate), etc.], aromatic (meth)acrylates [e.g., aryl (meth)acrylate esters (e.g., phenyl (meth)acrylate, o-tolyl (meth)acrylate, etc. (meth)acrylic acid C 6-20 aryl), (meth)acrylic acid aralkyl esters (e.g., (meth)acrylic acid C such as benzyl (meth)acrylate, 6-10 Aryl C 1-4 alkyl), phenoxyalkyl (meth)acrylate (e.g., phenoxy (meth)acrylate C such as phenoxyethyl (meth)acrylate, 1-4 alkyl), etc.
[0025] The (meth)acrylic acid ester also includes a (meth)acrylic acid ester having a substituent (e.g., a hydroxy group, an alkoxy group, a glycidyl group, etc.). Such a (meth)acrylic acid ester includes, for example, a methacrylic acid ester having a hydroxy group [e.g., a (meth)acrylic acid hydroxyalkyl ester (e.g., a (meth)acrylic acid hydroxyalkyl ester such as 2-hydroxyethyl (meth)acrylate], 1-12 alkyl), etc.], (meth)acrylic acid esters having an alkoxy group [for example, (meth)acrylic acid alkoxyalkyl esters (for example, methacrylic acid C such as 2-methoxyethyl (meth)acrylate, etc. 1-12 Alkoxy C 1-12 alkyl)], and (meth)acrylic acid esters having a glycidyl group (for example, glycidyl (meth)acrylate, etc.).
[0026] The (meth)acrylic acid ester unit may be constituted by one type or a combination of two or more types of (meth)acrylic acid ester.
[0027] The (meth)acrylic acid ester unit preferably contains at least a methacrylic acid ester unit, although this depends on the desired physical properties.
[0028] Examples of the methacrylic acid ester constituting the (meth)acrylic acid ester unit include aliphatic methacrylates [e.g., methacrylic acid alkyl esters (e.g., methyl methacrylate, ethyl methacrylate, n-propyl methacrylate, isopropyl methacrylate, n-butyl methacrylate, isobutyl methacrylate, sec-butyl methacrylate, tert-butyl methacrylate, pentyl methacrylate, amyl methacrylate, isoamyl methacrylate, n-hexyl methacrylate, 2-ethylhexyl methacrylate, heptyl methacrylate, octyl methacrylate, decyl methacrylate, dodecyl methacrylate, pentadecyl methacrylate, hexadecyl methacrylate, heptadecyl methacrylate, octadecyl methacrylate, etc. 1-18 Alkyl, preferably methacrylic acid C 1-12 alkyl), etc.], alicyclic methacrylates [e.g., methacrylic acid cycloalkyl esters (e.g., methacrylic acid C such as cyclopropyl methacrylate, cyclobutyl methacrylate, cyclopentyl methacrylate, and cyclohexyl methacrylate, etc. 3-20 Cycloalkyl, preferably methacrylic acid C 3-12 cycloalkyl), bridged cyclic methacrylates (e.g., isobornyl methacrylate, etc.), etc.), aromatic methacrylates [e.g., methacrylic acid aryl esters (e.g., phenyl methacrylate, o-tolyl methacrylate, m-tolyl methacrylate, p-tolyl methacrylate, 2,3-xylyl methacrylate, 2,4-xylyl methacrylate, 2,5-xylyl methacrylate, 2,6-xylyl methacrylate, 3,4-xylyl methacrylate, 3,5-xylyl methacrylate, 1-naphthyl methacrylate, 2-naphthyl methacrylate, binaphthyl methacrylate, anthryl methacrylate, etc. 6-20 Aryl, preferably methacrylic acid C 6-10 aryl), methacrylic acid aralkyl esters (e.g., methacrylic acid C such as benzyl methacrylate, 6-10 Aryl C 1-4 alkyl), phenoxy alkyl methacrylate (e.g., phenoxy methacrylate C such as phenoxyethyl methacrylate, 1-4alkyl), etc.
[0029] Among the methacrylic acid ester units, from the viewpoint of improving transparency, etc., it is preferable to use a methacrylic acid alkyl ester unit (e.g., methacrylic acid C 1-18 It is preferable that the copolymer contains at least one alkyl unit, and more preferable that the copolymer contains at least one methyl methacrylate unit.
[0030] The acrylic resin may contain units derived from other polymerizable monomers (monomers) than the (meth)acrylic acid ester units, if necessary. Examples of such other monomers include acid group-containing monomers (methacrylic acid, acrylic acid, etc.), styrene-based monomers [e.g., styrene, vinyl toluene, styrenes having substituents (e.g., halogen groups, alkoxy groups, alkyl groups, hydroxy groups, etc.) (e.g., α-methylstyrene, chlorostyrene, etc.), styrenesulfonic acid or salts thereof, etc.], vinyl esters (e.g., vinyl acetate, etc.), unsaturated nitriles (e.g., acrylonitrile, methacrylonitrile, etc.), olefin-based monomers (e.g., C olefins such as ethylene, propylene, 1-butene, isobutylene, 1-octene, etc.), and the like. 2-10 alkenes), amide group-containing vinyl monomers [for example, (meth)acrylamide, N-substituted (meth)acrylamides (for example, N-alkyl(meth)acrylamides such as N-methyl(meth)acrylamide; N-cycloalkyl(meth)acrylamides such as N-cyclohexyl(meth)acrylamide; N-aryl(meth)acrylamides such as N-phenyl(meth)acrylamide; N-aralkyl(meth)acrylamides such as N-benzyl(meth)acrylamide, etc.)], 2-(hydroxymethyl)acrylic acid esters (for example, alkyl esters such as ethyl 2-(hydroxymethyl)acrylate), etc.
[0031] The other monomers may be one type or two or more types may be combined to form units derived from the other monomers.
[0032] The content ratio of (meth)acrylic acid ester units in the acrylic resin (or the constituent units of the acrylic resin) can be selected from the range of, for example, 10 mass% or more (e.g., 20 mass% or more) and may be preferably 30 mass% or more (e.g., 35 mass% or more), more preferably 40 mass% or more (e.g., 45 mass% or more), and may be 50 mass% or more, 55 mass% or more, 60 mass% or more, 65 mass% or more, 70 mass% or more, 80 mass% or more, etc.
[0033] When the acrylic resin contains methacrylic acid ester units, the content of the methacrylic acid ester units in the acrylic resin (or the constituent units of the acrylic resin) can be selected from the range of, for example, 10% by mass or more, and may be 20% by mass or more, preferably 30% by mass or more (e.g., 35% by mass or more), and more preferably 40% by mass or more (e.g., 45% by mass or more), or may be 50% by mass or more, 55% by mass or more, 60% by mass or more, 65% by mass or more, 70% by mass or more, 80% by mass or more, etc.
[0034] When the acrylic resin contains methacrylic acid ester units, the content ratio of the methacrylic acid ester units in the (meth)acrylic acid ester units may be, for example, 10 mass% or more (e.g., 20 mass% or more), preferably 30 mass% or more (e.g., 40 mass% or more), more preferably 50 mass% or more (e.g., 60 mass% or more), and may be 70 mass% or more, 80 mass% or more, 90 mass% or more, etc.
[0035] When the acrylic resin contains methacrylic acid alkyl ester units, the content ratio of the methacrylic acid alkyl ester units in the (meth)acrylic acid ester units may be, for example, 10 mass% or more (e.g., 20 mass% or more), preferably 30 mass% or more (e.g., 40 mass% or more), more preferably 50 mass% or more (e.g., 60 mass% or more), and may be 70 mass% or more, 80 mass% or more, 90 mass% or more, etc.
[0036] In addition, when the acrylic resin contains methyl methacrylate units, the content ratio of methyl methacrylate units in the (meth)acrylic acid ester units may be, for example, 10 mass% or more (e.g., 20 mass% or more), preferably 30 mass% or more (e.g., 40 mass% or more), more preferably 50 mass% or more (e.g., 60 mass% or more), and may be 70 mass% or more, 80 mass% or more, 90 mass% or more, etc.
[0037] When the acrylic resin contains acrylic ester units, the content of the acrylic ester units in the acrylic resin may be relatively small from the viewpoint of heat resistance and refractive index, and may be selected, for example, from the range of less than 10 mass % (e.g., 8 mass % or less), preferably 5 mass % or less (e.g., 4 mass % or less), and more preferably 3 mass % or less (e.g., 2 mass % or less).
[0038] When the acrylic resin contains a unit derived from another polymerizable monomer, the content of the unit in the acrylic resin is not particularly limited and can be appropriately selected. In particular, when the acrylic resin contains an acid group-containing monomer as the other polymerizable monomer, the content of the acid group-containing monomer unit may be relatively low from the viewpoint of transparency, coloring, etc., and may be, for example, 10 mass% or less (e.g., 5 mass% or less), preferably 2 mass% or less (e.g., 1 mass% or less), more preferably 0.5 mass% or less, etc.
[0039] The acrylic resin (A) may have a ring structure. The ring structure is usually present in the main chain of the acrylic resin (polymer chain, acrylic polymer). Acrylic resins having a ring structure (and furthermore, acrylic resins having a relatively large MFR and / or a relatively small Mw) appear to be significantly affected by pellet size with respect to metering, and therefore the present invention can be suitably applied thereto.
[0040] In addition, by having a ring structure in the acrylic resin, various physical properties [e.g., heat resistance, moist heat resistance, yellowing resistance, hardness (strength), solvent resistance, surface hardness, barrier properties against oxygen and water vapor, optical properties, dimensional stability, shape stability, etc.] can be imparted, improved or enhanced in the acrylic resin. In addition, since the acrylic resin has a ring structure, it is possible to efficiently produce a molded article (for example, a lens) having a thinner film thickness than polymethyl methacrylate or the like.
[0041] Specific examples of the ring structure include a cyclic imide structure (e.g., a structure derived from an N-substituted maleimide monomer, a glutarimide structure, etc.), a cyclic amide structure (e.g., a lactam structure, etc.), a cyclic ester structure (e.g., a lactone ring structure, etc.), an acid anhydride structure (e.g., a structure derived from a maleic anhydride monomer, a glutaric anhydride structure), and the like.
[0042] The ring structure may in particular be a non-anhydride structure [for example, a ring structure that is not a structure derived from a maleic anhydride monomer, a glutaric anhydride structure, or the like (for example, a cyclic imide structure, a cyclic amide structure, a cyclic ester structure, etc.)].
[0043] The acrylic resin may have one or more ring structures. When the acrylic resin has two or more ring structures, the two or more ring structures may be ring structures of the same system (e.g., two or more cyclic imide structures, etc.) or ring structures of different systems (e.g., a combination of a cyclic imide structure and a lactone structure, etc.).
[0044] Examples of the glutarimide structure and glutaric anhydride structure include a structure represented by the following formula (1).
[0045] [ka] (In the formula, R 1 and R 2 are each independently a hydrogen atom or an alkyl group; R 3 is a hydrogen atom or a substituent, and X 1 is an oxygen atom or a nitrogen atom. 1 When is an oxygen atom, n=0, and X 1 is a nitrogen atom, n=1.)
[0046] R in Equation (1) 1 and R2 In the above, examples of the alkyl group include C 1-8 Examples of the alkyl group include methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, tert-butyl, n-pentyl, isopentyl, n-hexyl, isohexyl, n-heptyl, isoheptyl, n-octyl, and 2-ethylhexyl groups.
[0047] R 1 and R 2 is in particular a hydrogen atom or C 1-4 It is preferably an alkyl group.
[0048] R in Equation (1) 3 In the above formula, examples of the substituent include a hydrocarbon group. Examples of the hydrocarbon group include an aliphatic group, an alicyclic group, an aromatic group, etc. The hydrocarbon group may further have a substituent such as a halogen.
[0049] R in Equation (1) 3 In the above, examples of the aliphatic group include C 1-10 Examples of the alkyl groups include methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, tert-butyl, n-pentyl, isopentyl, n-hexyl, isohexyl, n-heptyl, isoheptyl, n-octyl, and 2-ethylhexyl groups. 1-4 Alkyl groups, particularly methyl groups, are preferred.
[0050] R in Equation (1) 3 In the above, the alicyclic group is, for example, 3-12 Cycloalkyl groups (e.g., cyclopropyl, cyclobutyl, cyclopentyl, cyclohexyl, etc.) are included. Among these cycloalkyl groups, 3-7 Cycloalkyl groups, particularly cyclohexyl groups, are preferred.
[0051] R in Equation (1) 3In the above, examples of the aromatic group include C 6-20 Aromatic groups [e.g., C 6-20 Aryl groups (e.g., phenyl, o-tolyl, m-tolyl, p-tolyl, 2,3-xylyl, 2,4-xylyl, 2,5-xylyl, 2,6-xylyl, 3,4-xylyl, 3,5-xylyl, 1-naphthyl, 2-naphthyl, binaphthyl, anthryl, etc.), C 7-20 aralkyl groups (for example, benzyl group, etc.) etc. Among these aromatic groups, phenyl group and tolyl group are preferred.
[0052] Typically, in formula (1), R 1 and R 2 are each independently a hydrogen atom or a methyl group, R 3 But, C 1-10 Alkyl group, C 3-12 Cycloalkyl group or C 6-20 It may be an aromatic group, preferably R 1 and R 2 are each independently a hydrogen atom or a methyl group, R 3 But, C 1-4 Alkyl group, C 3-7 Cycloalkyl groups, C 6-20 Aryl group or C 7-20 R may be an aralkyl group, and more preferably 1 and R 2 are each independently a hydrogen atom or a methyl group, R 3 is a methyl group, a cyclohexyl group, a phenyl group, or a tolyl group, and most preferably R 1 and R 2 are each independently a hydrogen atom or a methyl group, R 3 may be a cyclohexyl group or a phenyl group. From the viewpoint of suppressing coloration of the acrylic polymer, R 3 may be a hydrogen atom, a methyl group, or a cyclohexyl group, and from the viewpoint of improving the strength of the molded article, R 3 may be a hydrogen atom or a methyl group.
[0053] The ring structure may have one or more types of structures represented by formula (1).
[0054] In particular, when the ring structure has a structure represented by formula (1), a glutarimide structure which is a cyclic non-anhydride structure (i.e., in formula (1), X 1 is a nitrogen atom).
[0055] In addition, the glutaric anhydride structure (i.e., in formula (1), X 1 A ring structure in which is an oxygen atom) may be hydrolyzed or have an increased acid value, which may reduce water resistance or hot water resistance or cause fluctuations in optical properties. Therefore, it may be preferable that the ring structure does not substantially have a glutaric anhydride structure, or contains only a small amount of the glutaric anhydride structure.
[0056] Examples of structures derived from maleimide monomers (particularly N-substituted maleimide monomers) and maleic anhydride monomers include the structure represented by the following formula (2).
[0057] [ka] (In the formula, R 4 , R 5 are each independently a hydrogen atom or a methyl group, and R 6 is a hydrogen atom or a substituent, and X 2 is an oxygen atom or a nitrogen atom. X 2 When is an oxygen atom, n=0, and X 2 is a nitrogen atom, n=1.)
[0058] R in Equation (2) 6 In the above formula, examples of the substituent include a hydrocarbon group. The hydrocarbon group may be, for example, an aliphatic group {e.g., an alkyl group [e.g., C 1-6 Straight-chain alkyl groups (e.g., methyl, ethyl, etc.), C 1-6 Branched alkyl groups (e.g., isopropyl groups, etc.) 1-6 alkyl group, etc.}, alicyclic groups (e.g., cyclopentyl group, cyclohexyl group, etc. 3-20cycloalkyl groups, etc.), aromatic groups {e.g., C 6-20 Aromatic groups [e.g., C 7-20 Aralkyl groups (e.g., benzyl groups, etc.), C 6-20 aryl group (for example, phenyl group, etc.)}. The hydrocarbon group may further have a substituent such as a halogen.
[0059] X 2 When is an oxygen atom, the ring structure represented by formula (2) is a structure derived from maleic anhydride monomer.
[0060] On the other hand, X 2 When is a nitrogen atom, the ring structure represented by formula (2) is a structure derived from an N-substituted maleimide monomer.
[0061] In formula (2), X 2 When is a nitrogen atom, preferably, R 4 and R 5 are each independently a hydrogen atom, R 6 C 3-20 Cycloalkyl group or C 6-20 It may be an aromatic group, more preferably R 4 and R 5 are each independently a hydrogen atom, R 6 may be a cyclohexyl group, a benzyl group, or a phenyl group. From the viewpoint of suppressing coloration of the acrylic polymer, R 6 may be a hydrogen atom, a methyl group, or a cyclohexyl group, and from the viewpoint of improving the strength of the molded article, R 6 may be a hydrogen atom or a methyl group.
[0062] The ring structure may have one or more types of structures represented by formula (2).
[0063] In particular, when the ring structure has a structure represented by formula (2), a structure derived from a maleimide monomer which is a cyclic non-anhydride structure (i.e., in formula (2), X 2 is a nitrogen atom).
[0064] In the above formula (2), X 2 When n is an oxygen atom (and n=0), the above formula (2) is a structure derived from a maleic anhydride monomer. Such a structure derived from a maleic anhydride monomer may be hydrolyzed or have an increased acid value, which may reduce water resistance or hot water resistance or cause fluctuations in optical properties. Therefore, it may be preferable that the ring structure does not substantially have a structure derived from a maleic anhydride monomer, or contains only a small amount of such a structure.
[0065] The lactone ring (cyclic ester) structure is not particularly limited and may be, for example, a 4- to 8-membered ring. However, due to the excellent stability of the ring structure, a 5- or 6-membered ring is preferable, and a 6-membered ring is more preferable.
[0066] The lactone ring structure may be, for example, a structure disclosed in JP-A-2004-168882, and examples thereof include a structure represented by the following formula (3).
[0067] [ka] (In the formula, R 7 , R 8 and R 9 are each independently a hydrogen atom or a substituent.
[0068] In the formula (3), examples of the substituent include organic residues such as hydrocarbon groups. Examples of the hydrocarbon group include aliphatic groups (e.g., C groups such as methyl, ethyl, and propyl groups). 1-20 C such as alkyl group, ethenyl group, propenyl group, etc. 2-20 unsaturated aliphatic hydrocarbon groups, aromatic groups (e.g., phenyl groups, naphthyl groups, etc.) 6-20 Aromatic hydrocarbon groups, etc.
[0069] The hydrocarbon group may contain an oxygen atom, and one or more hydrogen atoms may be substituted with at least one type of group selected from a hydroxyl group, a carboxyl group, an ether group, and an ester group.
[0070] In formula (3), preferably, R 9 is a hydrogen atom or a methyl group, R 7 and R 8 are each independently a hydrogen atom or C 1-20 More preferably, R 9 is a hydrogen atom or a methyl group, R 7 and R 8 may each independently be a hydrogen atom or a methyl group.
[0071] The ring structure may contain one or more types of structures represented by formula (3).
[0072] The lactam ring structure is not particularly limited, and examples thereof include a pyrrolidinone ring structure represented by the following formula (4).
[0073] The pyrrolidinone ring structure has a five-membered amide ring structure (cyclic amide structure) as a basic skeleton. This cyclic amide structure is also a five-membered lactam structure (γ-lactam structure). Having a pyrrolidinone ring structure in the main chain means that at least one atom of the five atoms constituting the basic skeleton of the five-membered pyrrolidinone ring structure, typically three carbon atoms not constituting an amide bond (—N(R)CO—), is located in the main chain of the polymer and constitutes the main chain.
[0074] [ka] (In the formula, R 10 ~R 12 are each independently a hydrogen atom or a substituent.
[0075] R in Equation (4) 10 In the above, the substituents include, for example, a hydrocarbon group or -NHCOR 13 Group (R 13 is a hydrogen atom or a hydrocarbon group).
[0076] R 10 or R13 Examples of the hydrocarbon group in include an aliphatic group, an alicyclic group, and an aromatic group. Examples of the aliphatic group include C 1-18 Alkyl groups (e.g., methyl, ethyl, propyl, butyl, pentyl, hexyl, heptyl, octyl, and other C 1-18 Linear or branched alkyl groups, etc. Examples of the alicyclic group include C 3-18 Examples of the cycloalkyl group include a cyclopropyl group, a cyclobutyl group, a cyclopentyl group, and a cyclohexyl group. Examples of aromatic groups include C 6-20 Aromatic groups [e.g., C 6-20 Aryl groups (e.g., phenyl, tolyl, xylyl, naphthyl, anthryl, etc.), C 7-20 aralkyl groups (for example, benzyl groups, etc.).
[0077] R 10 In particular, hydrogen atom, C 1-18 Straight-chain alkyl groups (eg, methyl groups, etc.) are preferred. Also, R 13 In particular, hydrogen atom, C 1-18 A straight chain alkyl group (preferably C 1-12 A straight chain alkyl group, more preferably C 1-4 Straight chain alkyl groups, etc.), C 6-20 Aryl groups (e.g., phenyl groups, etc.), C 3-18 Cycloalkyl groups (preferably C 3-12 Cycloalkyl groups, more preferably C 3-6 Cycloalkyl groups and the like are preferred.
[0078] R in Equation (4) 11 In the above, examples of the substituent include -COOR 14 Group (R 14 is a hydrogen atom or a hydrocarbon group).
[0079] R 14 Examples of the hydrocarbon group in 10 or R13 Examples of the hydrocarbon groups include those exemplified by Also, R 14 Particularly preferred embodiments of the invention are also 13 This is the same as the particularly preferred embodiment of the above.
[0080] R in Equation (4) 12 In the above, examples of the substituent include -COR 15 Group (R 15 is a hydrogen atom or a hydrocarbon group).
[0081] R 15 Examples of the hydrocarbon group in 10 or R 13 Examples of the hydrocarbon groups include those exemplified by Also, R 15 Particularly preferred embodiments of the invention are also 13 This is the same as the particularly preferred embodiment of the above.
[0082] The ring structure of the acrylic resin may be appropriately selected depending on the desired physical properties (e.g., heat resistance, hardness (strength), solvent resistance, surface hardness, oxygen or water vapor barrier properties, optical properties, dimensional stability, shape stability, etc.). For example, from the viewpoint of heat resistance, etc., the ring structure may suitably contain a lactone ring structure or a cyclic imide structure (e.g., a structure derived from an N-substituted maleimide monomer, a glutarimide structure, etc.).
[0083] From the viewpoint of water resistance, hot water resistance, and the like, the ring structure may suitably contain a cyclic non-anhydride structure [for example, a lactone ring structure, a cyclic imide structure (particularly, a glutarimide structure, or a structure derived from an N-substituted maleimide monomer)].
[0084] Furthermore, from the viewpoints of surface hardness, solvent resistance, barrier properties, optical properties, and the like, the ring structure may suitably contain a lactone ring structure, a glutarimide structure, or the like.
[0085] In particular, the ring structure may contain at least one ring structure selected from a cyclic imide structure (particularly, a glutarimide structure or a structure derived from an N-substituted maleimide monomer) and a lactone ring structure, and among these, may contain at least a lactone ring structure. Acrylic resins having a lactone ring (cyclic ester) structure appear to be prone to unstable weighing (for example, the pellet size has a large effect on weighing), and the present invention can be suitably applied thereto.
[0086] The content of the ring structure can be selected depending on the application, desired physical properties, and the like, and is not particularly limited. For example, it can be selected from a range of about 0.1% by mass or more (e.g., 0.5% by mass or more) in the acrylic resin, and may be 1% by mass or more, preferably 3% by mass or more, more preferably 5% by mass or more, 10% by mass or more, 15% by mass or more, 20% by mass or more, 22% by mass or more, 25% by mass or more, etc.
[0087] The content ratio of the ring structure (or its upper limit) is not particularly limited, and may be, for example, 90 mass% or less, 80 mass% or less, 70 mass% or less, 60 mass% or less, 55 mass% or less, 50 mass% or less, 45 mass% or less, 40 mass% or less, 35 mass% or less, etc., in the acrylic resin.
[0088] A larger content of the ring structure is preferable in terms of heat resistance, hardness (strength), solvent resistance, surface hardness, dimensional stability, and the like.
[0089] In addition, these upper and lower limits may be appropriately combined to set an appropriate range (for example, 1 to 70 mass%, 3 to 60 mass%, 5 to 60 mass%, 5 to 50 mass, etc.) (the same applies to other ranges).
[0090] In particular, when the acrylic resin has a glutarimide structure, the content of the glutarimide structure may be preferably 5% by mass or more, more preferably 10% by mass or more, and even more preferably 15% by mass or more, and may be 90% by mass or less, preferably 60% by mass or less, more preferably 50% by mass or less, and even more preferably 40% by mass or less.
[0091] When the acrylic resin has a structure derived from an N-substituted maleimide monomer, the content of the structure derived from the N-substituted maleimide monomer may be, for example, 5 to 90 mass%, preferably 5 to 60 mass%, more preferably 10 to 50 mass%, and even more preferably 10 to 30 mass%.
[0092] When the acrylic resin has a lactone ring structure, the content of the lactone ring structure may be, for example, 1 to 80 mass%, preferably 3 to 70 mass%, and more preferably 5 to 60 mass% (e.g., 10 to 50 mass%), and can also be 15 mass% or more (e.g., 18 to 55 mass%), 20 mass% or more (e.g., 23 to 50 mass%), 25 mass% or more (e.g., 26 to 45 mass%, 28 to 40 mass%, etc.), and the like.
[0093] When the acrylic resin has a lactam ring structure, the content of the lactam ring structure may be, for example, about 1 to 80 mass %, preferably about 5 to 70 mass %, and more preferably about 10 to 50 mass %.
[0094] The content of the ring structure may be, for example, 1 to 80 mass%, preferably 3 to 70 mass%, and more preferably 5 to 60 mass% (e.g., 10 to 50 mass%), and can also be a relatively high content, for example, 10 mass% or more [for example, 13 to 60 mass%, 15 mass% or more (e.g., 18 to 55 mass%), 20 mass% or more (e.g., 23 to 50 mass%), 25 mass% or more (e.g., 26 to 45 mass%, 28 to 40 mass%, etc.)].
[0095] By introducing a ring structure into the acrylic resin at a relatively high content, it is possible to efficiently obtain a resin (molded product) having extremely excellent heat resistance (for example, high glass transition temperature) and moist heat resistance. On the other hand, as the content of ring structures increases, it may easily lead to unstable weighing (for example, the effect of pellet size on weighing becomes greater), and from this viewpoint, an acrylic resin having a relatively large number of ring structures (for example, having ring structures in a proportion of 10 mass % or more, 15 mass % or more, 20 mass % or more, etc.) may be preferably used.
[0096] In the present invention, even when the acrylic resin contains a high proportion of a ring structure (for example, a ring structure including at least a lactone ring structure), coloring (yellowing) can be efficiently suppressed.
[0097] The proportion of ring structures in the acrylic resin can be determined by a conventional method depending on the type of ring structure, etc. For example, the proportion of cyclic ester structures (lactone ring structures) may be determined based on the dealcoholization reaction rate, and the proportion of non-cyclic ester structures (e.g., cyclic imide structures, cyclic amide structures, acid anhydride structures, etc.) may be determined by NMR (e.g., 1 H-NMR, 13 The NMR analysis (NMR measurement) may be performed based on an analysis (measurement) condition, which may be appropriately selected, for example, using a predetermined measurement solvent (e.g., CDCl3, DMSO-d6) and at a predetermined measurement temperature (e.g., 40°C).
[0098] As an example, a method based on the dealcoholization reaction rate will be described.
[0099] First, the weight loss that occurs when all hydroxyl groups from the polymer composition obtained by polymerization are dealcoholized as methanol was used as the basis, and the dealcoholization reaction rate was calculated from the weight loss due to the dealcoholization reaction from 150°C, before weight loss began, to 300°C, before polymer decomposition began, in dynamic TG measurements. That is, in dynamic TG measurement of a polymer having a lactone ring structure, the weight loss rate is measured between 150°C and 300°C, and the actual weight loss rate obtained is designated as (X). On the other hand, based on the composition of the polymer, it is assumed that all hydroxyl groups contained in the polymer composition are involved in the formation of lactone rings and become alcohols, which are then dealcoholized, and the theoretical weight loss rate (i.e., the weight loss rate calculated on the assumption that a 100% dealcoholization reaction occurs in that composition) is designated as (Y). More specifically, the theoretical weight reduction rate (Y) can be calculated from the molar ratio of the raw material monomer having a structure (hydroxyl group) involved in the dealcoholization reaction in the polymer, i.e., the content of the raw material monomer in the polymer composition. These values (X) and (Y) are used to calculate dealcoholization: 1-(Actual weight reduction rate (X) / Theoretical weight reduction rate (Y)) Substituting the value into the above equation and expressing it as a percentage gives the dealcoholization reaction rate.
[0100] The acrylic resin may contain atoms or groups derived from components used during polymerization.
[0101] For example, the acrylic resin may contain a sulfur atom. In a more specific embodiment, the acrylic resin may have a sulfur-containing group (sulfur-containing skeleton) at least at the molecular terminal.
[0102] Such an acrylic resin having a sulfur atom or a sulfur-containing group can be obtained, for example, by using a thiol compound (such as the thiol compound described below) as a chain transfer agent.
[0103] When the acrylic resin is a copolymer, the form of the copolymerization is not particularly limited, and it may be a random copolymer, a block copolymer, an alternating copolymer, a graft copolymer, or the like.
[0104] For example, since an acrylic resin has a ring structure, it can usually be called a copolymer, but the manner in which the ring structure is introduced is not particularly limited, and the ring structure may be introduced randomly, or may be introduced in a block, alternating, graft, or other manner.
[0105] The melt flow rate (MFR) of the acrylic resin (A) (or resin) at a temperature of 230° C. and a load of 3.8 kg is, for example, 0.1 g / 10 min or more (e.g., 0.2 g / 10 min or more), preferably 0.3 g / 10 min or more (e.g., 0.4 g / 10 min or more), and more preferably 0.5 g / 10 min or more (e.g., 0.6 g / 10 min or more, 0.7 g / 10 min or more, 0.8 g / 10 min or more). / 10 min or more, 1 g / 10 min or more, 1.5 g / 10 min or more, 1.6 g / 10 min or more), or may be 1.8 g / 10 min or more (for example, 2 g / 10 min or more, 2.2 g / 10 min or more, 2.5 g / 10 min or more, 2.8 g / 10 min or more, 3 g / 10 min or more, 3.2 g / 10 min or more, 3.5 g / 10 min or more, 3.8 g / 10 min or more, 4 g / 10 min or more).
[0106] The upper limit of the melt flow rate of the acrylic resin (A) (or resin) at a temperature of 230° C. and a load of 3.8 kg may be, for example, 10 g / 10 min or less, 9.8 g / 10 min or less, 9.6 g / 10 min or less, 9.4 g / 10 min or less, 9.2 g / 10 min or less, 9 g / 10 min or less, 8.8 g / 10 min or less, 8.6 g / 10 min or less, 8.4 g / 10 min or less, 8.2 g / 10 min or less, 8 g / 10 min or less, 7.8 g / 10 min or less, 7.6 g / 10 min or less, 7.4 g / 10 min or less, 7.2 g / 10 min or less, 7 g / 10 min or less, 6.5 g / 10 min or less, 6 g / 10 min or less, 5.5 g / 10 min or less, 5.2 g / 10 min or less, or 5 g / 10 min or less.
[0107] Specific ranges of the melt flow rate of the acrylic resin (A) (or resin) include combinations of the above ranges, and may be, for example, 0.1 to 10 g / 10 min, 1.8 to 9 g / 10 min, or 2 to 8 g / 10 min at a temperature of 230° C. and a load of 3.8 kg.
[0108] The melt flow rate of the acrylic resin (or resin) may be measured in accordance with JIS K 7210.
[0109] By having excellent melt fluidity (high melt fluidity), coloring during molding (for example, melt molding such as injection molding) is reduced, and molded products (melt molded products such as injection molded products) with low yellowness can be easily obtained efficiently.
[0110] In addition, the high melt fluidity enables molding processing at lower temperatures, and by suppressing the thermal history during the molding process, discoloration of the molded product can be reduced. In addition, the time required for the heating and cooling processes of the injection device can be shortened, so that improved productivity can be expected.
[0111] On the other hand, acrylic resins (particularly acrylic resins having a ring structure) with high melt fluidity (e.g., MFR of 1.8 g / 10 min or more, 2 g / 10 min or more) tend to make the metering unstable (and are prone to producing silver streaks and the like). However, according to the method of the present invention, even with such resins, the metering can be efficiently stabilized (and silver streaks and the like can be reduced).
[0112] The weight average molecular weight (Mw) of the acrylic resin (A) (or resin) may be selected from a range of 5000 or more (for example, about 7000 or more, for example, 10000 or more (for example, 12000 or more), preferably 15000 or more (for example, 18000 or more), more preferably 20000 or more (for example, 25000 or more), or 30000 or more (for example, 35000 or more, 38000 or more, 40000 or more, 42000 or more, 45000 or more, 48000 or more, 50000 or more, 52000 or more, 55000 or more, 58000 or more, 60000 or more, 62000 or more, 65000 or more, etc.).
[0113] The weight average molecular weight (Mw) of the acrylic resin (A) (or resin) may be, for example, 500,000 or less, 400,000 or less, 300,000 or less, 250,000 or less, 200,000 or less, 180,000 or less, 150,000 or less, 120,000 or less, or may be 110,000 or less (for example, 105,000 or less, 100,000 or less, less than 100,000, 98,000 or less, 95,000 or less, 90,000 or less, etc.).
[0114] A specific range of the weight average molecular weight (Mw) of the acrylic resin (A) (or resin) may be, for example, 20,000 to 200,000, 30,000 to 150,000, or 50,000 to 100,000, from the viewpoint of moldability and the like.
[0115] Acrylic resins (particularly acrylic resins having a ring structure) with a relatively low Mw (for example, 110,000 or less, 100,000 or less, 95,000 or less, etc.) tend to have unstable metering (and are prone to silver streaks and the like); however, according to the method of the present invention, even with such resins, it is possible to efficiently stabilize the metering (and reduce silver streaks and the like).
[0116] The molecular weight distribution (Mw / Mn) of the acrylic resin (A) may be, for example, from 1 to 10 (e.g., 1.1 to 7.0), preferably from about 1.2 to 5.0 (e.g., 1.5 to 4.0), or may be from about 1.5 to 3.0, or may be 2.8 or less, 2.7 or less, 2.6 or less, particularly 2.5 or less (e.g., 2.4 or less, 2.3 or less, 2.2 or less), etc.
[0117] The acrylic resin (A) (or resin) may have a relatively narrow molecular weight distribution (Mw / Mn) from the viewpoints of melt flowability, strength of a molded product, and the like. On the other hand, acrylic resins (particularly acrylic resins having a ring structure) with narrow molecular weight distributions (e.g., 2.5 or less, 2.3 or less, etc.) tend to have unstable metering (and are prone to silver streaks and the like), possibly due to their relationship with melt fluidity. However, according to the method of the present invention, even with such resins, it is possible to efficiently stabilize the metering (and reduce silver streaks and the like).
[0118] The molecular weight (and molecular weight distribution) may be measured, for example, using GPC and converted into polystyrene.
[0119] The acid value of the acrylic resin (A) (or resin) varies depending on the application, etc., but a small acid value may be suitably used, and may be, for example, about 10 mmol / g or less, preferably 5 mmol / g or less, and more preferably 3 mmol / g or less (e.g., 1.5 mmol / g or less), or may be 1.2 mmol / g or less (e.g., 1 mmol / g or less, 0.8 mmol / g or less, 0.7 mmol / g or less, 0.6 mmol / g or less, 0.5 mmol / g or less, 0.4 mmol / g or less, 0.35 mmol / g or less, etc.). An acrylic resin (A) with a low acid value may easily lead to unstable metering (for example, the strength is low and the pellets are easily broken, resulting in a large effect of pellet size). However, according to the present invention, even with such an acrylic resin (A) with a low acid value, metering can be efficiently stabilized (and silver streaks and the like can be reduced).
[0120] The acid value can be measured by a conventional method. For example, it may be measured or calculated based on the amount of acid groups (including acid groups generated by hydrolysis (neutralization) of an acid anhydride) contained in the acrylic resin and the amount of base (e.g., sodium hydroxide) used for neutralization. Specifically, it may be measured or calculated by the method described below.
[0121] The glass transition temperature (Tg) of the acrylic resin (A) may be, for example, 70°C or higher (e.g., 80 to 200°C), preferably 90°C or higher (e.g., 100 to 180°C), and more preferably about 110°C or higher (e.g., 112 to 170°C), or about 115°C or higher (e.g., 118 to 160°C), or can be 120°C or higher [e.g., 120 to 160°C, 125°C or higher (e.g., 126 to 155°C), 128°C or higher (e.g., 129 to 150°C)], etc. The glass transition temperature can be efficiently adjusted, for example, by the type and ratio of the (meth)acrylic monomer, and when the acrylic resin contains a ring structure, the type and ratio of the ring structure, etc. Usually, an acrylic resin having a ring structure often has a relatively high glass transition temperature, and among acrylic resins having a ring structure, an acrylic resin having a larger ratio of the ring structure often has a higher glass transition temperature.
[0122] The Tg may be measured, for example, by the method described below.
[0123] The acrylic resin may be a commercially available product or may be manufactured. A method for manufacturing the acrylic resin will be described below.
[0124] (Method of manufacturing acrylic resin)
[0125] The acrylic resin (acrylic polymer) can be produced through at least a step of polymerizing a polymerization component (polymerization step).
[0126] The polymerization components are monomers that are raw materials for acrylic resins, and correspond to the above-exemplified (meth)acrylic acid esters and other monomers. The types and preferred embodiments of the monomers are the same as those described above.
[0127] The acrylic resin may have a ring structure, and depending on the type of ring structure, the polymerization components may contain a monomer that constitutes the ring structure or a monomer that is a raw material for the ring structure.
[0128] For example, in the case of producing an acrylic resin having a structure derived from a maleimide monomer or a maleic anhydride monomer, the polymerization components include, for example, maleic anhydride, maleimide-based monomers [e.g., maleimide; N-alkylmaleimide (e.g., N-methylmaleimide, N-ethylmaleimide, etc.); 1-10 N-alkylmaleimides, N-cycloalkylmaleimides (e.g., cyclohexylmaleimide, etc.) 3-20 cycloalkylmaleimides), N-arylmaleimides (e.g., N-phenylmaleimide, etc. 6-10 N-arylmaleimides, N-aralkylmaleimides (e.g., N-benzylmaleimide, etc. 7-10 The compound may include N-substituted maleimides such as aralkylmaleimides.
[0129] When producing an acrylic resin having a lactone ring structure, the polymerization components may contain a monomer that serves as a raw material for the lactone ring, such as a 2-(hydroxymethyl)acrylic acid ester (for example, an alkyl ester such as ethyl 2-(hydroxymethyl)acrylate).
[0130] In the case of producing an acrylic resin having a lactam ring structure, the polymerization components may contain lactam monomers [for example, N-vinylpyrrolidone monomers (for example, N-vinylpyrrolidone, N-vinyl-4-butylpyrrolidone, N-vinyl-4-propylpyrrolidone, N-vinyl-4-ethylpyrrolidone, N-vinyl-4-methylpyrrolidone, N-vinyl-4-methyl-5-ethylpyrrolidone, N-vinyl-4-methyl-5-propylpyrrolidone, N-vinyl-5-methyl-5-ethylpyrrolidone, N-vinyl-5-propylpyrrolidone, N-vinyl-5-butylpyrrolidone, etc.), N-vinylcaprolactam monomers (for example, N-vinylcaprolactam, N-vinyl-6-methylcaprolactam, N-vinyl-6-propylcaprolactam, N-vinyl-7-butylcaprolactam, etc.)], etc.
[0131] The polymerization may generally be a radical polymerization.
[0132] The polymerization may be carried out in the presence of a polymerization initiator (particularly a radical polymerization initiator).
[0133] The polymerization initiator (radical polymerization initiator) is not particularly limited, but examples thereof include organic peroxides [e.g., peroxides (dialkyl peroxides, diacyl peroxides, etc.), peroxy monocarbonates, peroxy esters, peroxy ketals, etc.], azo compounds, and the like.
[0134] Specific examples of the polymerization initiator include organic peroxides [e.g., tert-amylperoxyisononanoate, t-amylperoxy-2-ethylhexanoate, tert-butylperoxy-3,5,5-trimethylhexanate, tert-butylperoxylaurate, tert-butylperoxyisopropyl monocarbonate, tert-hexylperoxyisopropyl monocarbonate, tert-butylperoxyacetate, 1,1-bis(tert-butylperoxy)3,3,5-trimethylcyclohexane, 1,1-bis(tert-butylperoxy)cyclohexane, tert-butylperoxy2-ethylhexanoate, tert-butyl ...cyclohexane, tert-butylperoxy2-ethylhexanoate, tert-butylperoxyisopropyl monocarbonate, tert-butylperoxyisopropyl monocarbonate, tert-butylperoxyacetate, 1,1-bis(tert-butylperoxy)cyclohexane, tert-butylperoxy2-ethylhexanoate, xanate, tert-butylperoxyisobutyrate, tert-hexylperoxy 2-ethylhexanate, di-tert-butyl peroxide, 2,5-dimethyl-2,5-bis(tert-butylperoxy)hexane, etc.], azo compounds [for example, 2-(carbamoylazo)-isobutyronitrile, 1,1'-azobis(1-cyclohexanecarbonitrile), 2,2'-azobisisobutyronitrile, 2,2'-azobis(2-methylbutyronitrile), dimethyl 2,2'-azobisisobutyrate, 2,2'-azobis(2,4,4-trimethylpentane), 2,2'-azobis(2-methylpropane), etc.], etc.
[0135] The polymerization initiators may be used alone or in combination of two or more kinds.
[0136] In particular, at least an organic peroxide (such as a peroxy ester) may be suitably used as the polymerization initiator.
[0137] The amount (usage ratio) of the polymerization initiator used will vary depending on the type of polymerization initiator, and may be, for example, 0.01 part by mass or more, preferably 0.05 parts by mass or more, more preferably 0.1 part by mass or more, and particularly 0.15 parts by mass or more, relative to 100 parts by mass of the polymerization components, or may be 0.2 parts by mass or more (e.g., 0.25 parts by mass or more, 0.28 parts by mass or more, 0.3 parts by mass or more, 0.32 parts by mass or more, 0.35 parts by mass or more, 0.38 parts by mass or more, 0.4 parts by mass or more, 0.42 parts by mass or more, 0.45 parts by mass or more, 0.48 parts by mass or more, 0.5 parts by mass or more, 0.52 parts by mass or more).
[0138] The upper limit of the amount of the polymerization initiator used is not particularly limited, and may be, for example, 10 parts by mass, 9 parts by mass, 8 parts by mass, 7 parts by mass, 6 parts by mass, 5 parts by mass, 4.5 parts by mass, 4 parts by mass, 3.5 parts by mass, 3.2 parts by mass, 3 parts by mass, 2.8 parts by mass, 2.5 parts by mass, 2.2 parts by mass, 2 parts by mass, 1.8 parts by mass, 1.5 parts by mass, 1.2 parts by mass, 1 part by mass, 0.9 parts by mass, 0.8 parts by mass, 0.7 parts by mass, or the like, relative to 100 parts by mass of the polymerization components.
[0139] In particular, the proportion of the polymerization initiator used relative to 100 parts by mass of the polymerization components may be relatively large [for example, 0.2 parts by mass or more, 0.3 parts by mass or more, 0.4 parts by mass or more (for example, 0.4 to 0.8 parts by mass)].
[0140] By using a relatively large amount of the polymerization initiator in this way, it is easy to efficiently obtain an acrylic resin that is advantageous in terms of melt fluidity, etc. Even when a chain transfer agent is used, it is easy to ensure a sufficient polymerization reaction rate, and an acrylic resin with good melt fluidity can be efficiently obtained.
[0141] The polymerization may be carried out in the presence of a chain transfer agent.
[0142] The chain transfer agent is not particularly limited, but examples thereof include thiol compounds {e.g., primary thiols [e.g., aliphatic primary thiols (e.g., primary alkyl mercaptans such as butanethiol, octanethiol, decanethiol, dodecanethiol (n-dodecyl mercaptan), hexadecanethiol, octadecanethiol, and decanetrithiol, preferably primary C 3―30 alkyl mercaptans), etc.], secondary thiols [for example, aliphatic secondary thiols (e.g., secondary alkyl mercaptans such as 2-propanethiol, 2-butanethiol, 2-methyl-1-propanethiol, 3-methyl-2-butanethiol, 3-pentanethiol, 2-decanethiol, 3-decanethiol, 4-decanethiol, 5-decanethiol, 2-hexadecanethiol, 5-hexadecanethiol, and 8-octadecanethiol, preferably secondary C 3―30 alkyl mercaptans), alicyclic secondary thiols (e.g., cycloalkyl mercaptans such as cyclohexanethiol and cyclopentanethiol, preferably C 3―20 Cycloalkyl mercaptans), aromatic secondary thiols (e.g., aryl mercaptans such as thiophenol, preferably C 6-20 aryl mercaptans), etc.], tertiary thiols [for example, aliphatic tertiary thiols (for example, tert-alkyl mercaptans such as tert-butyl mercaptan, tert-dodecyl mercaptan, tert-nonyl mercaptan, tert-hexyl mercaptan, etc., preferably C 3―30 tert-alkyl mercaptans, etc.}
[0143] In addition, when the chain transfer agent contains a polyfunctional thiol, the proportion of the polyfunctional thiol in the chain transfer agent may be small. The amount (proportion) of the polyfunctional thiol used in the chain transfer agent may be, for example, 20% by mass or less (e.g., 15% by mass or less), preferably 10% by mass or less (e.g., 5% by mass or less), more preferably 3% by mass or less, 1% by mass or less, 0.5% by mass or less, etc.
[0144] The chain transfer agent may be used alone or in combination.
[0145] The amount (usage ratio) of the chain transfer agent used may be, for example, 0.001 part by mass or more, preferably 0.005 part by mass or more, more preferably 0.01 part by mass or more, particularly preferably 0.015 part by mass or more, or may be 0.02 part by mass or more, relative to 100 parts by mass of the polymerization components.
[0146] The upper limit of the amount of the chain transfer agent used is not particularly limited, and may be, for example, 5 parts by mass, 4 parts by mass, 3 parts by mass, 2 parts by mass, 1.5 parts by mass, 1 part by mass, 0.5 parts by mass, 0.25 parts by mass, 0.2 parts by mass, 0.15 parts by mass, 0.1 parts by mass, 0.08 parts by mass, 0.07 parts by mass, or the like, relative to 100 parts by mass of the polymerization components.
[0147] In particular, even when a chain transfer agent is used, the proportion of the chain transfer agent used relative to 100 parts by mass of the polymerization components may be relatively small [for example, 0.5 parts by mass or less, 0.1 parts by mass or less (for example, 0.001 to 0.1 parts by mass)] from the viewpoint of reducing coloration, and it is not necessary to use a chain transfer agent.
[0148] In this way, even if no chain transfer agent is used or even if a relatively small amount of chain transfer agent is used, an acrylic resin which is advantageous in terms of melt flowability and the like can be easily and efficiently obtained.
[0149] The mass ratio of the chain transfer agent and the polymerization initiator may be preferably 1 / 2 or less, more preferably 1 / 3 or less, 1 / 4 or less, or 1 / 5 or less, from the viewpoints of suppressing coloration of the acrylic resin, melt fluidity, etc. The mass ratio of the chain transfer agent and the polymerization initiator is calculated by (mass of the chain transfer agent) / (mass of the polymerization initiator).
[0150] The polymerization may be carried out in the presence of a polymerization initiator, a chain transfer agent, and other components (eg, a pH adjuster, various catalysts, etc.) as necessary.
[0151] The polymerization may be any of bulk polymerization, solution polymerization, suspension polymerization, emulsion polymerization, etc., and may be solution polymerization from the viewpoint of obtaining a polymer that does not contain impurities and has stable fluidity. In solution polymerization, since it can polymerize relatively uniformly, it seems that the generation of a polymer with a significantly high molecular weight is suppressed compared to bulk polymerization, and it is easy to efficiently obtain a polymer with stable fluidity. In addition, since it does not contain impurities such as emulsifiers compared to suspension polymerization and emulsion polymerization, it is easy to efficiently obtain a polymer with high transparency.
[0152] When the polymerization is carried out in a solvent (for example, in the case of solution polymerization), the solvent can be appropriately selected depending on the types of polymerization components and the like, and is not particularly limited. For example, organic solvents [aromatic hydrocarbons (for example, benzene, toluene, xylene, ethylbenzene, etc.), aliphatic or alicyclic hydrocarbons (for example, cyclohexane, methylcyclohexane, etc.), halogenated solvents (for example, chloroform, methylene chloride, carbon tetrachloride, etc.)], ketones (for example, acetone, methyl ethyl ketone, etc.), esters (for example, ethyl acetate, butyl acetate, etc.), ethers [for example, chain ethers (for example, diethyl ether, etc.), cyclic ethers (e.g., tetrahydrofuran, dioxane, etc.), amides [e.g., N-substituted amides (N-alkyl-substituted alkanamides such as N,N-dimethylformamide)], alcohols (e.g., alkanols such as methanol, ethanol, isopropanol), glycol ethers (e.g., monoalkyl ethers of alkanediols or polyalkanediols such as ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, propylene glycol monomethyl ether, diethylene glycol monoethyl ether, etc.)], and the like.
[0153] The solvents may be used alone or in combination of two or more kinds.
[0154] In the polymerization, the concentration of the polymerization components in the entire polymerization system may be, for example, 20% by mass or more (e.g., 20 to 70% by mass), preferably 35% by mass or more (e.g., 35 to 65% by mass), more preferably 40% by mass or more (e.g., 40 to 60% by mass), and particularly preferably 45% by mass or more (e.g., 45 to 55% by mass), from the viewpoints of suppressing an increase in molecular weight and productivity.
[0155] Each component (e.g., polymerization components, polymerization initiator, chain transfer agent, other components, solvent, etc.) may be present (charged) in the reaction system (reactor) at the start of polymerization, may be added (or mixed) as the polymerization progresses, or may be a combination of these. In such cases, the addition speed and addition time of each component can be appropriately selected.
[0156] Each component may be added to the reaction system in multiple portions (two or more portions, for example, 2 to 5 portions). In particular, the polymerization components (monomers) may be added to the reaction system as the polymerization proceeds, in which case the polymerization components may be added in multiple portions or may be added dropwise. When the polymerization components are added dropwise to the reaction system, an acrylic resin having a relatively narrow molecular weight distribution is easily obtained. Also, a polymerization initiator may be added to the reaction system as the polymerization proceeds. In particular, when the polymerization components are added to the reaction system by dropping, it is preferable to add the polymerization initiator to the reaction system by dropping. By adding the polymerization initiator to the reaction system as the polymerization proceeds, it is expected that safety can be ensured or a polymer having a relatively narrow molecular weight distribution can be obtained. When the polymerization components and the polymerization initiator are added dropwise, the dropping speed is not particularly limited. However, from the viewpoint of easily obtaining an acrylic resin having a relatively small molecular weight, it is preferable to add them slowly, and they may be added over one hour or more (for example, 1 to 10 hours).
[0157] The polymerization is usually carried out at a predetermined temperature (or under heating). The polymerization temperature (reaction temperature) can be appropriately selected depending on the types of polymerization components, polymerization initiator, solvent, etc., and may be, for example, 20°C or higher, preferably 30°C or higher (e.g., 35 to 180°C), more preferably 40°C or higher (e.g., 45 to 170°C), particularly preferably 50°C or higher (e.g., 55 to 160°C), particularly preferably 60°C or higher (e.g., 65 to 150°C), and may usually be about 70 to 140°C (e.g., 80 to 130°C).
[0158] The polymerization temperature may be changed as the polymerization proceeds. Even in such a case, the polymerization is usually carried out within the above-mentioned temperature range.
[0159] The polymerization may be carried out under stirring, in air, or in an inert atmosphere (such as nitrogen, helium, or argon).
[0160] The polymerization time (when maturation is performed) can be appropriately selected depending on the amount of polymerization components, polymerization temperature, etc., and is not particularly limited, but may be, for example, 30 minutes or more (e.g., 40 minutes to 24 hours), preferably 1 hour or more (e.g., 1.5 to 16 hours), and more preferably 2 hours or more (e.g., 2.5 to 12 hours).
[0161] When the acrylic resin has a ring structure, such a ring structure may be formed during the above-mentioned polymerization depending on the type of ring structure (for example, in the case of a structure derived from a maleimide monomer or maleic anhydride monomer, a lactam ring structure, etc.), and can be formed or introduced into the acrylic resin through a step of forming or introducing a ring structure after polymerization. The method of forming or introducing the ring structure is not particularly limited and can follow a known method.
[0162] For example, the lactone ring structure can be formed or introduced by cyclizing (cyclization condensation, cyclization treatment) an acrylic resin containing a unit derived from a monomer that is a raw material for the lactone ring [e.g., 2-(hydroxymethyl)acrylic acid ester] as described above. The cyclization may be carried out in the presence of a cyclization catalyst [e.g., a phosphorus-based catalyst (e.g., a phosphoric acid ester such as stearyl phosphate)].
[0163] The glutarimide structure can be formed or introduced into the acrylic polymer by known methods such as imidizing (meth)acrylic acid ester units (for example, the methods described in JP-A-2006-309033, JP-A-2006-317560, JP-A-2006-328329, JP-A-2006-328334, JP-A-2006-337491, JP-A-2006-337492, JP-A-2006-337493, JP-A-2007-009182, etc.).
[0164] The glutaric anhydride structure can be formed or introduced into an acrylic polymer, for example, by a method of intramolecular dealcoholization reaction between adjacent (meth)acrylic acid ester units and (meth)acrylic acid units (for example, the methods described in JP-A-2006-283013, JP-A-2006-335902, and JP-A-2006-274118).
[0165] Through such a polymerization step (and a cyclization step, if necessary), an acrylic resin is obtained.
[0166] The resin obtained through the polymerization step may be appropriately purified and separated by a conventional method.
[0167] [Other resins] The resin (or pellets) may contain other resins (resins other than acrylic resins) as necessary [the resin composition (or pellets thereof) may be constituted together with the other resins].
[0168] The other resins can be appropriately selected depending on the desired physical properties, applications, etc., and are not particularly limited. They may be thermoplastic resins, curable resins, or combinations of these. The other resins may be used alone or in combination of two or more kinds.
[0169] Specific examples of other resins include olefin-based polymers (e.g., polyethylene, polypropylene, ethylene-propylene copolymers, poly(4-methyl-1-pentene), etc.), halogen-based polymers (e.g., vinyl halide polymers such as polyvinyl chloride, polyvinylidene chloride, polyvinyl chloride, etc.), styrene-based polymers [e.g., polystyrene, styrene-based copolymers (e.g., styrene-methyl methacrylate copolymers, styrene-acrylonitrile copolymers, acrylonitrile-butadiene-styrene block copolymers (ABS resins), etc.)], polyester-based polymers (e.g., Examples of the resin include aromatic polyesters such as polyethylene terephthalate, polybutylene terephthalate, and polyethylene naphthalate), polyamide resins (for example, aliphatic polyamide resins such as polyamide 6, polyamide 66, and polyamide 610), polyacetal resins, polyphenylene oxide resins, polyphenylene sulfide resins, polyether ether ketone resins, polysulfone resins, polyethersulfone resins, and rubber polymers [for example, styrene resins (for example, styrene copolymers such as ABS resin) blended with rubber (polybutadiene rubber, acrylic rubber, and the like)].
[0170] The other resins include cellulose-based resins. Examples of cellulose-based resins (cellulose derivatives) include cellulose esters [e.g., cellulose acetate (cellulose diacetate, cellulose triacetate), cellulose propionate, cellulose butyrate, cellulose acetate propionate, cellulose acetate butyrate, and other cellulose acylates], cellulose ethers [e.g., alkyl celluloses (e.g., methyl cellulose, ethyl cellulose, and other), hydroxyalkyl celluloses (e.g., hydroxyethyl cellulose, hydroxyalkyl cellulose, and other), carboxyalkyl celluloses (e.g., carboxymethyl cellulose, and other)], and cyanoethyl cellulose.
[0171] The other resins include thermoplastic elastomers. The thermoplastic elastomers are not particularly limited, and examples thereof include styrene-based elastomers, olefin-based elastomers, urethane-based elastomers, and amide-based elastomers.
[0172] [Other ingredients] The resin (or pellets) may contain other components as necessary (the resin composition (or pellets thereof) may be constituted together with the other components). Such other components can be selected according to the desired application, physical properties, etc. The other components are not particularly limited, and examples thereof include ultraviolet absorbers, colorants, antioxidants (e.g., phenol-based antioxidants, thioether-based antioxidants, phosphoric acid-based antioxidants, etc.), stabilizers, reinforcing materials, flame retardants, antistatic agents, organic fillers, inorganic fillers, antiblocking agents, resin modifiers, organic fillers, inorganic fillers, plasticizers, lubricants, retardation reducing agents, etc.
[0173] The other components may be used alone or in combination of two or more.
[0174] The ultraviolet absorbing ability of the ultraviolet absorber (UVA) may be within the wavelength range of 300 to 380 nm, and the molar extinction coefficient (chloroform solution) for the light of the wavelength at which the absorption by UVA is maximum is 10,000 (L mol-1 ·cm -1 ) or more.
[0175] The ultraviolet absorbing agent (UVA) is not particularly limited, but examples thereof include benzophenone-based compounds, salicylate-based compounds, benzoate-based compounds, triazole-based compounds, and triazine-based compounds.
[0176] Examples of triazole compounds include 2,2'-methylenebis[4-(1,1,3,3-tetramethylbutyl)-6-(2H-benzotriazol-2-yl)phenol], 2-(3,5-di-t-butyl-2-hydroxyphenyl)-5-chlorobenzotriazole, 2-(2H-benzotriazol-2-yl)-p-cresol, 2-(2H-benzotriazol-2-yl)-4,6-bis(1-methyl-1-phenylethyl)phenol, 2-benzotriazol-2-yl-4,6-di-t-butylphenol, 2-[5-chloro(2H)-benzotriazol-2-yl]-4-methyl-6-(t-butyl)phenol, 2-(2H-benzotriazol-2-yl)-4,6-di-t-butylphenol, 2-(2H-benzotriazol-2-yl)-4,6-di-t-butylphenol, )-4-(1,1,3,3-tetramethylbutyl)phenol, 2-(2H-benzotriazol-2-yl)-4-methyl-6-(3,4,5,6-tetrahydrophthalimidylmethyl)phenol, reaction products of methyl-3-(3-(2H-benzotriazol-2-yl)-5-t-butyl-4-hydroxyphenyl)propionate / polyethylene glycol 300, 2-(2H-benzotriazol-2-yl)-6-(linear and branched chain dodecyl)-4-methylphenol, 2-(5-methyl-2-hydroxyphenyl)benzotriazole, 2-[2-hydroxy-3,5-bis(α,α-dimethylbenzyl)phenyl]-2H-benzotriazole, 3-(2H-benzotriazol-2-yl)-5-(1,1-dimethylethyl)-4-hydroxy-C 7-9 Side chain and straight chain alkyl esters, etc. Triazole compounds having a halogen atom, for example a chlorine atom, are preferred because of their high ultraviolet absorbing ability.
[0177] Examples of the triazine compounds include 2,4-diphenyl-6-(2-hydroxy-4-methoxyphenyl)-1,3,5-triazine, 2,4-diphenyl-6-(2-hydroxy-4-ethoxyphenyl)-1,3,5-triazine, 2,4-diphenyl-(2-hydroxy-4-propoxyphenyl)-1,3,5-triazine, 2,4-diphenyl-(2-hydroxy-4-butoxyphenyl)-1,3,5-triazine, 2,4-diphenyl-6-(2-hydroxy-4-butoxyphenyl)-1,3,5-triazine, 2,4-diphenyl-6-(2-hydroxy-4-hexyloxyphenyl)-1,3,5-triazine, 2,4-diphenyl-6-(2-hydroxy-4-octyloxyphenyl)-1,3,5-triazine, and 2,4-diphenyl-6-(2-hydroxy-4-dodecyloxyphenyl). 2,4-bis(2-hydroxy-4-butoxyphenyl)-6-(2,4-dibutoxyphenyl)-1,3,5-triazine, 2,4-bis(2-hydroxy-4-butoxyphenyl)-6-(2,4-dibutoxyphenyl)-1,3-5-triazine, 2,4,6-tris(2-hydroxy-4-hexyloxy-3-methylphenyl)-1,3,5-triazine, 2,4-bis(2,4-dimethylphenyl)-6-[2-hydroxy-4-(3-alkyloxy-2-hydroxypropyloxy)-5-α-cumylphenyl]-s-triazine skeleton (alkyloxy; long-chain alkyloxy groups such as octyloxy, nonyloxy, and decyloxy) UVAs. Among these, UVAs having a 2,4-bis(2,4-dimethylphenyl)-6-[2-hydroxy-4-(3-alkyloxy-2-hydroxypropyloxy)-5-α-cumylphenyl]-s-triazine skeleton (alkyloxy; long-chain alkyloxy groups such as octyloxy, nonyloxy, and decyloxy) are preferred because of their excellent ultraviolet absorbing performance.
[0178] The molecular weight of the UVA is not particularly limited, but is preferably at least 600. The upper limit of the molecular weight of the UVA may be, for example, 10,000, 8,000, 5,000, or the like.
[0179] The ultraviolet absorbents may be used alone or in combination of two or more kinds.
[0180] The colorant is not particularly limited and can be appropriately selected depending on the application of the composition, and may be, for example, a pigment (eg, inorganic pigment, organic pigment), a dye, or the like.
[0181] The colorant may also have bluing properties (the property of compensating (countering) and reducing the color (eg, yellow) of the acrylic resin or composition). Such a colorant may be a colorant (compound) having a maximum absorption wavelength in the range of 520 to 600 nm, 540 to 580 nm, or the like, depending on the color to be corrected.
[0182] Such a colorant can be appropriately selected depending on the type (wavelength) of the color to be corrected, and examples thereof include compounds having an anthraquinone skeleton (anthraquitone-based compounds), compounds having a phthalocyanine skeleton (phthalocyanine-based compounds), compounds having an azo skeleton (azo-based compounds), and compounds having a triarylmethane skeleton (triarylmethane-based compounds). Among these, compounds having an anthraquinone skeleton may be preferably used from the viewpoint of heat resistance and the like.
[0183] Specific examples of colorants (colorants having bluing properties, bluing agents) include anthraquinone dyes [e.g., Solvent Violet 13 (CA. No. (Color Index Number) 60725), Solvent Violet 14, Solvent Violet 31 (CA. No. 68210), Solvent Violet 33 (CA. No. 60725), Solvent Violet 36 (CA. No. 68210), Solvent Blue 45 (CA. No. 61110), Solvent Blue 94 (CA. No. 61500), Solvent Blue 87, Solvent Blue 97, Disperse Violet 28, etc.], phthalocyanine dyes [e.g., Solvent Blue 25 (CA. No. 74350), etc.], monoazo dyes [e.g., Solvent Violet 21, etc.], triarylmethane dyes [e.g., Solvent Blue 2 (CA.No.42563), etc.
[0184] As such colorants, commercially available products such as "Macrolex (registered trademark) Violet B", "Macrolex (registered trademark) Violet 3R", "Macrolex (registered trademark) Blue RR" (manufactured by LANXESS KK), "Sumiplast (registered trademark) Violet B", "Sumiplast (registered trademark) Green G" (manufactured by Sumika Chemtex Co., Ltd.), "Polysynthren (registered trademark) Blue RLS" (manufactured by Clariant), "Diaresin Violet D", "Diaresin Blue G", "Diaresin Blue N" (manufactured by Mitsubishi Chemical Corporation) and the like may be used.
[0185] In addition, a black dye may be used as the colorant from the viewpoint of obtaining an excellent jet black (piano black-like) appearance.
[0186] As such a black dye, for example, organic dyes such as compounds having an anthraquinone skeleton (anthraquinone-based compounds), compounds having a perinone skeleton (perinone-based compounds), compounds having a perylene skeleton (perylene-based compounds), compounds having an azo skeleton (azo-based compounds), compounds having a methine skeleton (methine-based compounds), and compounds having a quinone skeleton (quinone-based compounds) are preferably used. As the anthraquinone-based compounds, organic dyes such as blue, purple, and green may be preferably used, and as the perinone-based compounds, organic dyes such as red and orange may be preferably used.
[0187] The black dye is commercially available. For example, "Oplus (registered trademark) Black 838", "Nubian (registered trademark) Black PC-0870", "Nubian (registered trademark) Black PC-5856", "Nubian (registered trademark) Black PC-5857", "Nubian (registered trademark) Black PC-8550" (manufactured by Orient Chemical Industries Co., Ltd.), "Sumiplast (registered trademark) Black H3B", "Sumiplast (registered trademark) Black HLG", "Sumiplast (registered trademark) Black HB" (manufactured by Sumika Chemtex Co., Ltd.), etc. may be used.
[0188] The colorants may be used alone or in combination of two or more kinds.
[0189] [Proportion of each ingredient] In the resin (or pellets), the proportion of the acrylic resin (A) (or the proportion of the acrylic resin (A) in the resin components) may be selected from the range of, for example, 10 mass % or more (e.g., 20 mass %) and may be 30 mass % or more (e.g., 40 mass % or more), preferably 50 mass % or more (e.g., 60 mass % or more), and more preferably 70 mass % or more (e.g., 80 mass % or more, 90 mass % or more).
[0190] When the resin (or pellets) contains other resins, the content of the other resins relative to the entire resin (pellets) [or resin components (total amount of acrylic resin (A) and other resins)] can be selected from the range of, for example, about 70 mass % or less (e.g., 0.1 to 60 mass %), and may be 50 mass % or less (e.g., 0.5 to 40 mass %), preferably about 30 mass % or less (e.g., 1 to 25 mass %), or may be 20 mass % or less (e.g., 15 mass % or less, 10 mass % or less, 5 mass % or less, 3 mass % or less, 1 to 10 mass %, etc.).
[0191] From the viewpoint of efficiently exhibiting the physical properties of the acrylic resin (A), even when other resins are contained, it is preferable that the proportion of the other resins is not too large.
[0192] When the resin (pellet) contains other components (additives), the proportion of the other components may be, for example, about 0.01 to 10 mass % (eg, 0.05 to 5 mass %) with respect to the entire resin (pellet).
[0193] [Pellet manufacturing method] In one aspect of the present invention, pellets of the resin described above are produced in a particular manner.
[0194] That is, in such a method, a resin is cut (for example, hot cut) to produce pellets, and at this time, the pellets are cut so that the pellets (pellets after cooling or in a solidified state) have a specific size.
[0195] The shape of the pellets may vary depending on the melting and cutting method, but may be, for example, columnar (cylindrical), flat, circular (disc-shaped), or the like. In the present invention, among these shapes, circular pellets and the like may be preferably used. By using pellets of such a shape, it is possible to more efficiently stabilize the metering (and further reduce silver streaks and the like).
[0196] The size of the pellets (hot-cut pellets, etc.) may be selected from a range of about 5 mm or less in terms of major axis (major axis of the cut surface, maximum width of the cut surface), and may be 4.5 mm or less, preferably 4.2 mm or less, and more preferably 4.0 mm or less (e.g., 3.9 mm or less, 3.8 mm or less).
[0197] The short diameter of the pellet (short diameter of the cut surface, minimum width of the cut surface) may be selected from a range of about 5 mm or less, and may be 4.5 mm or less, preferably 4.2 mm or less, and more preferably 4.0 mm or less (for example, 3.9 mm or less, 3.8 mm or less).
[0198] When the long axis of the pellet is L (mm) and the short axis of the pellet is S (mm), the value of LS may be 0 mm or more (e.g., 0 to 4 mm, 0 to 3.5 mm), and may preferably be 2 mm or less (e.g., less than 2 mm, 1.8 mm or less, 1.5 mm or less, 1.2 mm or less, 1.0 mm or less). In the present invention, such pellets having a small LS value may be preferably used. By using such pellets, it is possible to more efficiently stabilize the metering (and further reduce silver streaks, etc.).
[0199] The thickness (or length) of the pellets depends on the cutting method, etc., but may be selected from a range of, for example, about 10 mm or less (e.g., 8 mm or less, 7 mm or less, 6 mm or less), and may be 5 mm or less (e.g., 4.5 mm or less), preferably 4.2 mm or less (e.g., 4.0 mm or less), and more preferably 3.5 mm or less (e.g., 3.2 mm or less, 3.0 mm or less).
[0200] The major axis, minor axis, and thickness may be average values (arithmetic mean values, etc.) of a plurality of pellets.
[0201] The major axis, minor axis and thickness can be measured by a conventional method, for example, by the method described below.
[0202] The thickness of the pellet may be equal to or smaller than the major axis of the pellet (particularly smaller than the major axis of the pellet), or may be equal to or smaller than the minor axis of the pellet (particularly smaller than the minor axis of the pellet).
[0203] In such a case, when the major axis of the pellet is L (mm), the minor axis of the pellet is S (mm), and the thickness of the pellet is T (mm), the value of LT or the value of ST may be 0 mm or more (e.g., 0 to 4 mm, 0 to 3.5 mm), 0.1 mm or more (e.g., 0.2 to 3.5 mm), 0.3 mm or more (e.g., 0.4 to 3.2 mm), or 0.5 mm or more (e.g., 0.5 to 3 mm). In the present invention, pellets having such LT or ST values (for example, pellets having a relatively similar major axis (or minor axis) and thickness) may be preferably used. By using such pellets, it is possible to more efficiently stabilize the metering (and further reduce silver streaks, etc.).
[0204] In cutting the resin, the state of the resin (the resin to be cut) is not limited, but typically, the resin in a molten state may be cut (particularly, the molten resin is cut in a molten state (hot cut)). Hot-cutting is susceptible to the effects of unstable weighing, etc., but according to the present invention, such unstable weighing, etc. can be suppressed, and stable (efficient) production of hot-cut pellets can be achieved.
[0205] The method for melting the resin (melting means) is not particularly limited, and for example, an extruder or the like can be used.
[0206] In addition, when producing pellets containing other resins and other components in addition to the acrylic resin, the other resins and other components may be melted in advance in the acrylic resin, or may be melted (melt-kneaded) while being mixed with the acrylic resin in the melting means (extruder).
[0207] The cutting method (cutting means) is not particularly limited, but for example, a cutter (a cutter used in a hot-cut method) can be used. Specific cutting means (pelletizers) include, for example, a hot-cut pelletizer, a watering pelletizer, a mist-cut pelletizer, an underwater pelletizer, a rotary knife pelletizer, a centrifugal pelletizer, and a strand-cut pelletizer.
[0208] In a representative method, from the viewpoint of stable production of pellets, a resin extruded from a melting means (such as an extruder) through a die (such as an extrusion die) may be cut in a molten state (hot cut).
[0209] The die may usually have a number of holes.
[0210] The resin may be cooled at an appropriate stage depending on the cutting method, etc. For example, when cutting by hot cutting, the resin after cutting (for example, in a molten state) may be cooled. The cooling method (solidification method) of the resin (for example, in hot cutting, the cut resin, or the molten resin) is not particularly limited, and may be natural cooling (air cooling), water cooling, etc., depending on the type of pelletizer, etc.
[0211] The resin (e.g., the cut resin) may be cooled, but in many cases the resin is cooled so as to immediately solidify. For example, the resin (e.g., the cut resin, the molten resin) may be cooled so as to solidify within 1 minute (e.g., within 30 seconds, within 20 seconds, within 10 seconds, within 5 seconds, etc.) after cutting.
[0212] [pellet] Pellets are obtained in the manner described above. The size and other details of such pellets are as described above.
[0213] The use of the pellets is not particularly limited, but they may be suitably used for melt molding, particularly injection molding.
[0214] Although acrylic resin pellets can be unstable in the metering of injection molding machines (injection devices), pellets obtained as described above can achieve relatively stable metering even when used for injection molding. Furthermore, by using such pellets, molded products (injection molded products) with fewer appearance and molding defects such as silver streaks can be efficiently manufactured.
[0215] In particular, such pellets (or the method for producing pellets) may be combined (applied) with the method of another aspect of the present invention described below. By combining in this manner, it may be possible to more efficiently produce molded products with stable weighing and fewer appearance and molding defects such as silver streaks, although this may depend on the type of acrylic resin.
[0216] <Resin molding method> In another aspect of the present invention, a method for molding a resin (a method for manufacturing a molded product) is provided.
[0217] In such a method, the resin may be the same as the resin described above (the resin described in one embodiment of the present invention). That is, the resin may usually contain an acrylic resin (A), and the preferred embodiment of the acrylic resin (A), other resins, other components, etc. may be the same as those described above.
[0218] For example, the acrylic resin (A) may be an acrylic resin having a ring structure (e.g., a cyclic ester structure), or may be an acrylic resin having the above-mentioned MFR (e.g., MFR of 2 g / 10 min or more), Mw (e.g., Mw of 100,000 or less), Mw / Mn (e.g., Mw / Mn of 2.5 or less), or the like.
[0219] Such an acrylic resin is also suitable for the production of molded articles (injection molded articles) that have relatively stable weighing and few appearance and molding defects such as silver streaks, in the methods of other aspects of the present invention.
[0220] The resin may be in the form of pellets. Such pellets may be similar to the pellets in one embodiment of the present invention (e.g., similar in major axis, minor axis, thickness, and the difference between them (e.g., major axis 4.5 mm or less, minor axis 4.5 mm or less, thickness 3.5 mm or less, etc.)) or different, but similar pellets may be preferably used.
[0221] Furthermore, when pellets are used as the resin, the pellets may be a resin obtained in the same manner as in one embodiment of the present invention (e.g., hot-cut pellets obtained by cutting a molten resin), and typically, pellets obtained by the method of one embodiment of the present invention (e.g., hot-cut pellets) may be used.
[0222] The use of such pellets may be incorporated into the method of the other aspect of the present invention, i.e., the method of the other aspect of the present invention includes a pellet production step of producing pellets by the method of the one aspect of the present invention, and the pellets of the resin obtained in this production step may be used as the resin.
[0223] In another embodiment of the present invention, the resin is injection molded (or the resin is injection molded to produce a molded article (injection molded article)).
[0224] The molding machine (injection molding machine, injection unit) used in injection molding has the structure explained above with reference to FIG.
[0225] That is, as shown in FIG. 1, a molding machine (such as an injection molding machine) typically includes a cylinder (cylinder portion) 2, a nozzle portion Hn having a nozzle 1 connected to the front end of the cylinder 2, and a hopper (feeding port) 3 connected to the rear portion H3 of the cylinder 2.
[0226] A screw consisting of a front section (metering section) S1, a middle section (compression section) S2, and a rear section (supply section) S3 is housed within cylinder 2, and these correspond to the front section (metering section) H1, the middle section (compression section) H2, and the rear section (supply section) H3 of cylinder 2 when the screw is pushed in (the screw is moved toward the nozzle).
[0227] Temperature measuring devices (such as thermocouples) 4 may be installed in each part of the cylinder.
[0228] A cooling device (a cooling jacket such as a water-cooled jacket) H4 is installed at the rear part H3 of the cylinder (or at the base end of H3, below the hopper 3). Such a cooling device is usually installed so as to surround the periphery (outer periphery) of H3.
[0229] Resin (pellets, etc.) is fed from a hopper 3 into a supply section H3 (S3) and melted in the cylinder 2 (melted by the shearing force of the screw). This molten resin is measured in a metering section S1 (H1) and fed through a nozzle 1 into a mold (not shown) to become a desired molded body.
[0230] Here, in the method according to another embodiment of the present invention, the temperature (set temperature) of the cooling device (H4) is adjusted in relation to the glass transition temperature of the resin.
[0231] That is, when the temperature of the cooling device is Tj (°C) and the glass transition temperature of the resin is Tg (°C), Tg-Tj may be 80 or less (e.g., 75 or less), preferably 70 or less, more preferably 65 or less (e.g., 62 or less), and particularly preferably 60 or less (e.g., 58 or less), or may be 55 or less (e.g., 52 or less, 50 or less, 48 or less, etc.).
[0232] The lower limit of Tg-Tj (°C) may be, for example, 3, 5, 8, 10, 12, 15, 18, 20, 22, 25, 28, 30, 32, 35, 38, 40, 42, 45, etc., and may typically be 20 or more (for example, 20, 25, 30, etc.).
[0233] Although the reason why such a temperature makes it easier to realize metering stability and improvement of silver streaks is unclear, it is thought that one of the reasons is that, for example, moisture and remaining volatile components in the pellets are more likely to escape. Furthermore, when the above-mentioned pellets are used, it is thought that the pellets are less likely to crack, which further makes it easier to realize the above-mentioned improvements.
[0234] As described above, in the injection molding machine, the resin (molten resin) is metered in the metering section, and such metering can be stabilized by adjusting the temperature of the cooling device.
[0235] Therefore, the method of the present invention can also be said to be a method (or a method of stabilizing the metering) of measuring resin (molten resin) [metering the molten resin to be discharged (injected) into a mold (through a nozzle)] by setting Tg-Tj (°C) to a specific temperature (e.g., 80 or less, 70 or less, etc.) in injection molding or an injection molding machine (or a method of injection molding and producing a molded article).
[0236] Other molding (injection molding) conditions (conditions other than the temperature of the cooling device, for example, the set temperatures of the supply section, compression section, metering section and nozzle section, compression conditions, etc.) are not particularly limited and can be appropriately selected according to conventional methods.
[0237] <Molded products, etc.> Through at least the above-mentioned method (the method of one aspect of the present invention and / or the method of another aspect of the present invention), pellets (resin pellets, resin composition) or molded articles (molded bodies) can be obtained.
[0238] The yellowness index (YI) of such a molded article (or resin pellets) may be relatively small, depending on the constituent components, and may be, for example, 4 or less, preferably 3.5 or less, more preferably 3 or less, or may be 2.8 or less, 2.6 or less, 2.5 or less, 2.4 or less, 2.3 or less, 2.2 or less, 2.1 or less, 2.0 or less, 1.9 or less, 1.8 or less, etc.
[0239] The lower limit of the yellowness index may be 0 (or the detection limit) or a finite value (e.g., 0.01, 0.02, 0.05, 0.1, 0.15, 0.2, 0.25, 0.3, 0.35, 0.4, 0.45, 0.5, etc.).
[0240] The yellowness index may be, for example, a value in a thickness of 3 mm {e.g., a sheet [sheet-shaped molded product (injection molded product)] having a thickness of 3 mm} [e.g., a value measured in accordance with the provisions of JIS K7373 using a spectrophotometer (Shimadzu Corporation, UV-3600) with a C2 light source and a wavelength range of 380 nm to 780 nm], or in detail, a value measured by the method described below.
[0241] The shape of the molded product is not particularly limited, and may be any of a two-dimensional shape [for example, a film (or sheet)] and a three-dimensional shape (for example, a block shape).
[0242] The molded article can be used for various purposes. Since the molded article often has excellent transparency (and low colorability) and excellent optical properties due to the acrylic resin (A), it may be preferably used for optical purposes (for example, as an optical component).
[0243] Specific examples of applications include light guiding components, film applications [for example, protective films (optical protective films, etc.), optical films (optical sheets), etc.], lenses (optical lenses, etc.), covers (lens covers, etc.), foam (foam molded products) applications (for example, cushioning materials, heat retention / insulation materials, vibration damping materials, soundproofing materials, sealing materials, packing materials, etc.), and interior material applications [for example, interior material applications for vehicles (automobiles, etc.) such as front panels of in-vehicle displays and meter covers]. Examples of lenses (optical lenses, etc.) include Fresnel lenses, linear Fresnel lenses, lenticular lenses, flat prisms, fly's eye lenses, aspheric lenses, condenser lenses, microlenses, collimator lenses, concave lenses, convex lenses, and diffractive lenses. Examples of applications of lenses (lens components) include head-up displays, cameras (e.g., in-vehicle cameras), LIDAR devices, etc. Examples of lenses for such applications include Fresnel lenses and condenser lenses used in head-up displays, and Fresnel lenses, condenser lenses, collimator lenses, convex lenses, etc. used in LIDAR devices.
[0244] Examples of light guide members include light guides [or lighting devices, such as lamps or lights]. The light guides may be for automobiles, motorcycles, etc. The location (or application) where the light guide is provided is not particularly limited, and examples of light guides for automobiles include headlamps, tail lamps, brake lamps, side mirror lamps, and daytime running lights (DRLs).
[0245] Specific examples of the member (light guide member) include a light cover and a light guide {a light guide for a vehicle lamp [for example, a light guide for an automobile headlamp (for example, a light guide for a DRL)]}.
[0246] Examples of the protective film include protective films for substrates of various optical disks (VD, CD, DVD, MD, LD, etc.) and polarizer protective films used in polarizing plates for liquid crystal displays.
[0247] Examples of optical films (optical sheets) include retardation films, zero retardation films (in-plane and thickness direction retardation is infinitesimally small), viewing angle compensation films, light diffusion films, reflective films, anti-reflection films, anti-glare films, brightness enhancement films, conductive films for touch panels, diffusion plates, light guides, retardation plates, zero retardation plates, and prism sheets.
[0248] Among these, in the present invention, since a melt molding method such as injection molding can be applied as described above, the molded article may be a molded article having a three-dimensional shape.
[0249] In particular, molded articles for optical applications (optical components) may require high transparency (and further low colorability, high surface hardness, etc.), and the method of the present invention is useful for producing such molded articles. It can be suitably used.
[0250] The present invention is not limited to the above-described embodiments, and various modifications are possible. The present invention also includes embodiments obtained by appropriately combining the technical means disclosed in the different embodiments. EXAMPLES
[0251] The present invention will be described in more detail below with reference to examples, but the present invention is not limited thereto.
[0252] In the following description, unless otherwise specified, "%" means "% by mass (by weight)" and "parts" means "parts by mass (by weight)".
[0253] The measurement and evaluation of various physical properties were carried out by the following methods.
[0254] [Weight average molecular weight (Mw) and molecular weight distribution (Mw / Mn)] The weight average molecular weight and molecular weight distribution of the resin were determined in terms of polystyrene using gel permeation chromatography (GPC) using the following apparatus and conditions: System: Tosoh GPC system HLC-8320 Measurement column configuration Guard column: Tosoh, TSKguardcolumn SuperHZ-L Separation column: Tosoh TSKgel SuperHZM-M, 2 columns connected in series Reference column configuration Reference column: Tosoh, TSKgel SuperH-RC Developing solvent: Chloroform (Wako Pure Chemical Industries, special grade) Flow rate of developing solvent: 0.6mL / min Standard sample: TSK standard polystyrene (Tosoh, PS-oligomer kit) Column temperature: 40℃
[0255] [Glass transition temperature (Tg)] The glass transition temperature was measured in accordance with the provisions of JIS K7121-1987. Specifically, a differential scanning calorimeter (Rigaku's "Thermo plus EVO DSC-8230") was used to measure the glass transition temperature by the starting point method from a DSC curve obtained by heating about 10 mg of a sample from room temperature to 200°C (heating rate 20°C / min) under a nitrogen gas atmosphere. α-alumina was used as a reference.
[0256] [Melt flow rate (MFR)] The melt flow rate was measured in accordance with JIS K 7210-1:2014 Method A at a temperature of 230°C and a load of 3.8 kg (37 N).
[0257] [Ratio of lactone ring structure contained in acrylic resin] First, the weight loss that occurs when all hydroxyl groups from the polymer composition obtained by polymerization are dealcoholized as methanol was used as the basis, and the dealcoholization reaction rate was calculated from the weight loss due to the dealcoholization reaction from 150°C, before weight loss began, to 300°C, before polymer decomposition began, in dynamic TG measurements. That is, in dynamic TG measurement of a polymer having a lactone ring structure, the weight loss rate is measured between 150°C and 300°C, and the actual weight loss rate obtained is designated as (X). On the other hand, based on the composition of the polymer, it is assumed that all hydroxyl groups contained in the polymer composition are involved in the formation of lactone rings and become alcohols, which are then dealcoholized, and the theoretical weight loss rate (i.e., the weight loss rate calculated on the assumption that a 100% dealcoholization reaction occurs in that composition) is designated as (Y). More specifically, the theoretical weight reduction rate (Y) can be calculated from the molar ratio of the raw material monomer having a structure (hydroxyl group) involved in the dealcoholization reaction in the polymer, i.e., the content of the raw material monomer in the polymer composition. These values (X) and (Y) are used to calculate dealcoholization: 1-(Actual weight reduction rate (X) / Theoretical weight reduction rate (Y)) Substituting the value into the above equation and expressing it as a percentage gives the dealcoholization reaction rate. The ratio of lactone ring structures in the pellets obtained in Production Example 6 (Production Example 7) described later is calculated. The theoretical weight loss rate (Y) of this polymer is calculated as follows: the molecular weight of methanol is 32, the molecular weight of methyl 2-(hydroxymethyl)acrylate is 116, and the content (mass ratio) of methyl 2-(hydroxymethyl)acrylate in the polymer is 13 mass% in the composition, so that it is (32 / 116)×13≒3.59 mass%. On the other hand, the actual weight loss rate (X) measured by dynamic TG measurement was 0.08 mass%. By applying these values to the above dealcoholization calculation formula, it becomes 1-(0.08 / 3.59)≒0.978, so the dealcoholization reaction rate is 97.8%. In the case of Production Example 1, the content of methyl 2-(hydroxymethyl)acrylate in the copolymer was 13.0% by mass, the calculated dealcoholization reaction rate was 97.8% by mass, and the formula weight of the lactone cyclized structural unit produced when methyl 2-(hydroxymethyl)acrylate having a molecular weight of 116 is condensed with methyl methacrylate is 170, so the content of lactone rings in the copolymer was 8.6 (13.0 × 0.978 × 170 / 116)% by mass.
[0258] [Acid value] The acid value was measured by the following method. First, 0.15 g of the polymer was dissolved in 24.94 g of methylene chloride. 14.85 g of methanol was added to the obtained solution and stirred for 3 hours. Next, 2 drops of a 1 wt% phenolphthalein ethanol solution were added to the solution. While stirring the obtained solution, a 0.1 N aqueous sodium hydroxide solution was added, and stirring was continued for 1 hour at room temperature. At this time, the amount of the 0.1 N aqueous sodium hydroxide solution added was defined as A ml. Next, 0.1 N hydrochloric acid was dropped into the solution. The amount of 0.1 N hydrochloric acid added until the color of the solution (red purple) disappeared was defined as B ml. Next, a mixed solution of 24.94 g of methylene chloride and 14.85 g of methanol was prepared. Two drops of a 1 wt% phenolphthalein ethanol solution were added to this mixed solution. Next, while stirring this mixed solution, a 0.1 N aqueous sodium hydroxide solution was added, and stirring was continued for one hour at room temperature. At this time, the amount of the 0.1 N aqueous sodium hydroxide solution added is defined as C ml. Next, 0.1 N hydrochloric acid was dropped into this mixed solution. The amount of 0.1 N hydrochloric acid added until the color of the mixed solution (reddish purple) disappeared is defined as D ml. The acid value (mmol / g) of the polymer was calculated from the following formula. The acid value represents the amount of sodium hydroxide required to neutralize the acid groups contained in 1 g of the polymer and the acid groups generated by hydrolysis of the acid anhydride groups. [Acid value (mmol / g)]=0.1×[(AB)-(CD)] / 0.15
[0259] [Yellowness (YI)] The yellowness index was measured on a 3 mm thick molded body using a spectrophotometer (Shimadzu Corporation, UV-3600) with a C2 light source and a wavelength range of 380 nm to 780 nm in accordance with the regulations of JIS K7373: 2006. The molded body was prepared by drying the obtained pellets at 100°C for 12 hours or more, and then using an injection molding machine (Nissei Plastics, NS40-5A) to prepare a molded body (100 mm x 100 mm x 3 mm thick) at a mold temperature of 100°C under the injection molding machine temperature setting conditions described below.
[0260] [Three-point bending test] The three-point bending test was performed in accordance with the JIS K7171: 2016 standard using a bending tester (Instron universal testing machine model 185). The pellets were dried at 100°C for 12 hours or more, and then molded using a manual heat press molding machine (Imoto Manufacturing Co., Ltd.) at a molding temperature of 220°C with a mold size of 127 mm x 12.7 mm x thickness of 3.2 mm. The bending test was performed under the measurement conditions of a span of 60 mm and a test speed of 2 mm / min, and the maximum bending stress (bending strength) and bending modulus were measured.
[0261] [Pellet size] The pellet size was measured using a digital caliper. 20 of the obtained pellets were fixed with double-sided tape so that the cross-sectional direction of each pellet was horizontal to the flat plate. The average values of the long and short diameters of the pellet cross-sections of these arranged pellets were calculated. Furthermore, the average maximum height of the pellet cross-section was calculated as the thickness of the pellet.
[0262] [Weighing time and weighing variation] The pellets were dried at 100°C for 12 hours or more, and then molded using an injection molding machine (NS40-5A, manufactured by Nissei Plastics Co., Ltd.) under the temperature setting conditions of the injection molding machine described below. The weighing time during 20 continuous shots was measured, and the average value and standard deviation were calculated. The average value was taken as the weighing time, and the standard deviation was taken as the weighing variation. The shorter the weighing time, the better the weighing stability.
[0263] [Silver Streak Occurrence Rate] The obtained pellets were dried at 100°C for 12 hours or more, and then molded bodies (injection molded bodies with dimensions of 100 mm x 100 mm x 3 mm thickness) were produced using an injection molding machine (NS40-5A, manufactured by Nissei Plastics Co., Ltd.) at a mold temperature of 100°C using a mold with dimensions of 100 mm x 100 mm x 3 mm thickness under the injection molding machine setting temperature conditions described below. The number of molded products with silver streaks among the 20 molded products was visually confirmed, and the result was calculated as the silver streak occurrence rate according to the following formula. Silver streak occurrence rate (%) = [number of silver streaks / 20] x 100
[0264] (Production Example 1 [Production of Acrylic Resin Pellets (B1)] A reaction vessel equipped with a stirrer, a temperature sensor, a cooling tube, a nitrogen inlet tube, and a dropping pump was charged with 11.5 parts by mass of methyl 2-(hydroxymethyl)acrylate (RHMA), 38.5 parts by mass of methyl methacrylate (MMA), 90.7 parts by mass of toluene, and 0.05 parts by mass of tris(2,4-di-tert-butylphenyl)phosphite, and the temperature was raised to 105°C while passing nitrogen through. As an initial initiator, a solution consisting of 4.3 parts by mass of toluene and 0.29 parts by mass of t-amyl peroxy isononanoate (manufactured by Arkema Yoshitomi Co., Ltd., Luperox (registered trademark) 570) was dropped over 8 minutes, while solution polymerization was performed at 105 ° C. to 110 ° C. Then, 22 minutes later, a solution consisting of 5.0 parts by mass of toluene and 0.30 parts by mass of t-amyl peroxy isononanoate (manufactured by Arkema Yoshitomi Co., Ltd., Luperox (registered trademark) 570) was dropped over 170 minutes as a dropping initiator. In addition, 25 minutes after the initial initiator was added, a solution consisting of 11.5 parts by mass of 2-(hydroxymethyl) methyl acrylate (RHMA) and 38.5 parts by mass of methyl methacrylate (MMA) was dropped over 180 minutes, while solution polymerization was performed at 105 ° C. to 110 ° C., and further aging was performed over 1.5 hours. To the obtained polymerization solution, a solution consisting of 1.25 parts by mass of toluene and 0.30 parts by mass of stearyl phosphate (Phoslex A-18, manufactured by Sakai Chemical Industry Co., Ltd.) was added as a catalyst for the cyclization condensation reaction (cyclization catalyst), and the cyclization condensation reaction to form a lactone ring structure was allowed to proceed for 2 hours under reflux at approximately 90°C to 110°C. Next, the obtained polymerization solution was passed through a multi-tube heat exchanger maintained at 240°C to complete the cyclization condensation reaction, and then introduced into a vent-type screw twin-screw extruder (L / D=52) with a leaf disk-type polymer filter (filtration accuracy 5μm) at the tip at a processing rate of 90 parts by weight / hour in terms of resin amount, and the polymerization solution was devolatilized to obtain resin pellets (B1). The number of rear vents of the vent-type screw twin-screw extruder used was 1, and the number of fore vents was 4 (referred to as the first, second, third, and fourth vents from the upstream side), the barrel temperature was 240°C, and the degree of vacuum was 13.3 to 400hPa (10 to 300mmHg). During devolatilization, ion-exchanged water was introduced from behind the first and third vents at a rate of 1.3 parts by weight / hour, and a mixed solution of a bluing agent and an antioxidant that had been prepared separately was introduced from behind the second vent at a rate of 0.30 parts by weight / hour. As a mixed solution of bluing agent and antioxidant, a solution consisting of 0.27 parts by weight of a solution in which 1.0 part by weight of bluing agent (Sumiplast (registered trademark) Violet B manufactured by Sumika Chemtex Corporation) was dissolved in 99 parts by weight of toluene, 3.6 parts by weight of two types of antioxidants (Irganox 1010 manufactured by BASF Japan Ltd. and Adeka STAB AO-412S manufactured by ADEKA Corporation), and 112.5 parts by weight of toluene was used.
[0265] (Production Example 2 [Production of acrylic resin pellets (A1)] The resin pellets (B1) obtained in Production Example 1 were melt-kneaded using an extruder (φ=40 mm, L / D=16) equipped with a small hot-cut pelletizer (Tanabe Plastics Machinery Co., Ltd., RP40) at the tip at a cylinder temperature of 225°C and a screw rotation speed of 25 rpm, and the molten acrylic resin was extruded at 2.3 kg / h from a die (narrow hole) with a diameter of 1.5 mmφ in the extrusion die. The molten acrylic resin extruded from the extrusion die was cut into approximately 0.012 g pieces by rotating (1600 rpm) a cutter blade attached to the tip of the extruder, to obtain disk-shaped resin pellets (A1) with a major axis of 3 mm, a minor axis of 3 mm, and a thickness of 2.4 mm.
[0266] The resulting resin pellets (A1) had a weight average molecular weight of 80,000, a molecular weight distribution of 2.1, a glass transition temperature of 132° C., a melt flow rate of 4.0, a proportion of ring structures of 28.8% by mass, and an acid value of 0.3 mmol / g or less.
[0267] (Production Example 3 [Production of acrylic resin pellets (A2)] The resin pellets (B1) obtained in Production Example 1 were melt-kneaded using an extruder (φ=40 mm, L / D=16) equipped with a small hot-cut pelletizer (Tanabe Plastics Machinery Co., Ltd., RP40) at the tip at a cylinder temperature of 225°C and a screw rotation speed of 25 rpm, and the molten acrylic resin was extruded at 3 kg / h from a die (narrow hole) with a diameter of 2 mmφ in the extrusion die. The molten acrylic resin extruded from the extrusion die was cut into approximately 0.016 g pellets by rotating (1600 rpm) a cutter blade attached to the tip of the extruder, to obtain disk-shaped resin pellets (A2) with a major axis of 3.5 mm, a minor axis of 3.5 mm, and a thickness of 2.4 mm.
[0268] The resulting resin pellets (A2) had a weight average molecular weight of 80,000, a molecular weight distribution of 2.1, a glass transition temperature of 132° C., a melt flow rate of 4.0, a proportion of ring structures of 28.8% by mass, and an acid value of 0.3 mmol / g or less.
[0269] (Production Example 4 [Production of acrylic resin pellets (A3)] The resin pellets (B1) obtained in Production Example 1 were melt-kneaded using an extruder (φ=40 mm, L / D=16) equipped with a small hot-cut pelletizer (Tanabe Plastics Machinery Co., Ltd., RP40) at the tip at a cylinder temperature of 225°C and a screw rotation speed of 25 rpm, and the molten acrylic resin was extruded at 3.6 kg / h from a die (narrow hole) with a diameter of 2.5 mmφ in the extrusion die. The molten acrylic resin extruded from the extrusion die was cut into approximately 0.021 g pellets by rotating (1750 rpm) a cutter blade attached to the tip of the extruder, to obtain disk-shaped resin pellets (A3) with a major axis of 3.8 mm, a minor axis of 3.8 mm, and a thickness of 2.7 mm.
[0270] The resulting resin pellets (A3) had a weight average molecular weight of 80,000, a molecular weight distribution of 2.1, a glass transition temperature of 132° C., a melt flow rate of 4.0, a proportion of ring structures of 28.8% by mass, and an acid value of 0.3 mmol / g or less.
[0271] (Production Example 5 [Production of acrylic resin pellets (A4)] The resin pellets (B1) obtained in Production Example 1 were melt-kneaded using an extruder (φ=40 mm, L / D=16) equipped with a small hot-cut pelletizer (Tanabe Plastics Machinery Co., Ltd., RP40) at the tip at a cylinder temperature of 225°C and a screw rotation speed of 25 rpm, and the molten acrylic resin was extruded at 3.6 kg / h from a die (narrow hole) with a diameter of 3 mmφ in the extrusion die. The molten acrylic resin extruded from the extrusion die was cut into approximately 0.03 g pellets by rotating (1250 rpm) a cutter blade attached to the tip of the extruder, obtaining disk-shaped resin pellets (A4) with a major axis of 4.6 mm, a minor axis of 4.6 mm, and a thickness of 2.7 mm.
[0272] The resulting resin pellets (A4) had a weight average molecular weight of 80,000, a molecular weight distribution of 2.1, a glass transition temperature of 132° C., a melt flow rate of 4.0, a proportion of ring structures of 28.8% by mass, and an acid value of 0.3 mmol / g or less.
[0273] (Production Example 6 [Production of acrylic resin pellets (B2)] A reaction vessel equipped with a stirrer, a temperature sensor, a cooling tube, a nitrogen inlet tube, and a dropping pump was charged with 6.5 parts by mass of methyl 2-(hydroxymethyl)acrylate (RHMA), 43.5 parts by mass of methyl methacrylate (MMA), 90.7 parts by mass of toluene, and 0.05 parts by mass of tris(2,4-di-tert-butylphenyl)phosphite, and the temperature was raised to 105°C while passing nitrogen through. As an initial initiator, a solution consisting of 4.3 parts by mass of toluene and 0.22 parts by mass of t-amyl peroxy isononanoate (manufactured by Arkema Yoshitomi Co., Ltd., Luperox (registered trademark) 570) was dropped over 8 minutes, while solution polymerization was performed at 105 ° C. to 110 ° C. Then, 22 minutes later, a solution consisting of 5.0 parts by mass of toluene and 0.28 parts by mass of t-amyl peroxy isononanoate (manufactured by Arkema Yoshitomi Co., Ltd., Luperox (registered trademark) 570) was dropped over 180 minutes as a dropping initiator. In addition, 25 minutes after the initial initiator was added, a solution consisting of 6.5 parts by mass of 2-(hydroxymethyl) methyl acrylate (RHMA) and 43.5 parts by mass of methyl methacrylate (MMA) was dropped over 180 minutes, while solution polymerization was performed at 105 ° C. to 110 ° C., and further aging was performed for 1.5 hours. To the obtained polymerization solution, a solution consisting of 1.25 parts by mass of toluene and 0.075 parts by mass of stearyl phosphate (Phoslex A-18, manufactured by Sakai Chemical Industry Co., Ltd.) was added as a catalyst for the cyclization condensation reaction (cyclization catalyst), and the cyclization condensation reaction to form a lactone ring structure was allowed to proceed for 1.5 hours under reflux at approximately 90°C to 110°C. Next, the obtained polymerization solution was passed through a multi-tube heat exchanger maintained at 220°C to complete the cyclization condensation reaction, and then introduced into a vent-type screw twin-screw extruder (L / D=52) equipped with a leaf disk-type polymer filter (filtration accuracy 5μm) at the tip at a processing rate of 90 parts by weight / hour in terms of resin amount, and the polymerization solution was devolatilized to obtain resin pellets (B2). The number of rear vents of the vent-type screw twin-screw extruder used was 1, and the number of fore vents was 4 (referred to as the first, second, third, and fourth vents from the upstream side), the barrel temperature was 220°C, and the degree of vacuum was 13.3 to 400hPa (10 to 300mmHg). During devolatilization, ion-exchanged water was introduced from behind the first, second, and third vents at an introduction rate of 1.3 parts by weight / hour.
[0274] (Production Example 7 [Production of acrylic resin pellets (A5)] The resin pellets (B2) obtained in Production Example 6 were melt-kneaded using an extruder (φ=40 mm, L / D=16) equipped with a small hot-cut pelletizer (Tanabe Plastics Machinery Co., Ltd., RP40) at the tip at a cylinder temperature of 225°C and a screw rotation speed of 25 rpm, and the molten acrylic resin was extruded at 2.3 kg / h from a die (narrow hole) with a diameter of 1.5 mmφ in the extrusion die. The molten acrylic resin extruded from the extrusion die was cut into approximately 0.012 g pieces by rotating (1600 rpm) a cutter blade attached to the tip of the extruder, obtaining disk-shaped resin pellets (A5) with a major axis of 3 mm, a minor axis of 3 mm, and a thickness of 2.4 mm.
[0275] The resulting resin pellets (A5) had a weight average molecular weight of 88,000, a molecular weight distribution of 2.2, a glass transition temperature of 123° C., a melt flow rate of 4.5, a proportion of ring structures of 18.6% by mass, and an acid value of 0.2 mmol / g or less.
[0276] (Production Example 8 [Production of acrylic resin pellets (B3)] In a reaction vessel equipped with a stirrer, a temperature sensor, a cooling tube and a nitrogen inlet tube, 10 parts by weight of 2-(hydroxymethyl)methyl acrylate (RHMA), 40 parts by weight of methyl methacrylate (MMA), 0.025 parts by weight of tris(2,4-di-tert-butylphenyl)phosphite and 50 parts by weight of toluene as a polymerization solvent were charged. Next, the temperature was raised to 105°C while introducing nitrogen gas into the reaction vessel, and when refluxing accompanying the temperature rise began, 0.05 parts by weight of tertiary amyl peroxy isononanoate (manufactured by Arkema Yoshitomi Co., Ltd., Luperox (registered trademark) 570) was added as a polymerization initiator. At the same time, the drop of 0.10 parts by weight of the above tertiary amyl peroxy isononanoate was started, and while dropping this over 2 hours, solution polymerization was allowed to proceed under reflux at about 105 to 110°C. After the dropwise addition was completed, the reaction vessel was heated for 4 hours and aged.
[0277] Next, 0.05 parts by weight of stearyl phosphate (Phoslex A-18, manufactured by Sakai Chemical Industry Co., Ltd.) was added as a catalyst for the cyclization reaction to the polymerization solution thus obtained, and the cyclization condensation reaction to form a lactone ring structure was carried out under reflux at approximately 90°C to 110°C for 2 hours.
[0278] Next, the obtained polymerization solution was passed through a multi-tube heat exchanger maintained at 240 ° C. to complete the cyclization condensation reaction, and then introduced into a vent-type screw twin-screw extruder (L / D = 52) with a leaf disk-type polymer filter (filtration accuracy 5 μm) at the tip at a processing speed of 90 parts by weight / hour in terms of resin amount, and the polymerization solution was devolatilized to obtain resin pellets (B3). The number of rear vents of the vent-type screw twin-screw extruder used was 1, and the number of fore vents was 4 (referred to as the 1st, 2nd, 3rd, and 4th vents from the upstream side), and a side feeder was placed between the 3rd and 4th vents, the barrel temperature was 240 ° C., and the degree of vacuum was 13.3 to 400 hPa (10 to 300 mmHg). During devolatilization, ion-exchanged water was fed at a rate of 1.3 parts by weight / hour from behind the second vent, and a separately prepared solution of a cyclization catalyst deactivator was fed at a rate of 0.6 parts by weight / hour from behind the third vent. As the solution of the cyclization catalyst deactivator, a solution in which 1.0 part by weight of zinc octylate (manufactured by Nippon Kagaku Sangyo Co., Ltd., product name: Nikka Octyx Zinc 10% by weight) was dissolved in 0.3 parts by weight of toluene was used.
[0279] (Production Example 9 [Production of acrylic resin pellets (A6)] The resin pellets (B3) obtained in Production Example 8 were melt-kneaded using an extruder (φ=40 mm, L / D=16) equipped with a small hot-cut pelletizer (Tanabe Plastics Machinery Co., Ltd., RP40) at the tip at a cylinder temperature of 250°C and a screw rotation speed of 25 rpm, and the molten acrylic resin was extruded at 3.6 kg / h from a die (narrow hole) with a diameter of 3 mm in the extrusion die. The molten acrylic resin extruded from the extrusion die was cut into approximately 0.03 g pieces by rotating (1250 rpm) a cutter blade attached to the tip of the extruder, to obtain disk-shaped resin pellets (A6) with a major axis of 4.6 mm, a minor axis of 4.6 mm, and a thickness of 2.7 mm.
[0280] The resulting resin pellets (A6) had a weight average molecular weight of 116,000, a molecular weight distribution of 2.6, a glass transition temperature of 130° C., a melt flow rate of 0.8, a proportion of ring structures of 28.6% by mass, and an acid value of 0.3 mmol / g or less.
[0281] (Production Example 10 [Production of acrylic resin pellets (B4)] A reaction vessel equipped with a stirrer, a temperature sensor, a cooling tube, a nitrogen inlet tube, and a dropping pump was charged with 12 parts by mass of methyl 2-(hydroxymethyl)acrylate (RHMA), 83.5 parts by mass of methyl methacrylate, 90.4 parts by mass of toluene, 0.05 part by mass of tris(2,4-di-tert-butylphenyl)phosphite, and 0.07 part by mass of n-dodecyl mercaptan as a chain transfer agent, and the temperature was raised to 105°C while passing nitrogen through. 0.09 parts by mass of t-amyl peroxy isononanoate (Arkema Yoshitomi Co., Ltd., Luperox (registered trademark) 570) was added as an initial initiator, and 5 minutes later, a solution consisting of 4.5 parts by mass of styrene (St), 8.14 parts by mass of toluene, and 0.179 parts by mass of the dropping initiator t-amyl peroxy isononanoate (Arkema Yoshitomi Co., Ltd., Luperox (registered trademark) 570) was added dropwise over 2 hours while carrying out solution polymerization at 100°C to 110°C, and then aging was carried out for a further 4 hours. To the obtained polymerization solution, 0.075 parts by mass of stearyl phosphate (Phoslex A-18, manufactured by Sakai Chemical Industry Co., Ltd.) was added as a catalyst for the cyclization condensation reaction (cyclization catalyst), and the cyclization condensation reaction for forming a lactone ring structure was allowed to proceed for 1.5 hours under reflux at approximately 90°C to 110°C. Next, the obtained polymerization solution was passed through a multi-tube heat exchanger maintained at 240°C to complete the cyclization condensation reaction, and then introduced into a vent-type screw twin-screw extruder (L / D=52) with a leaf disk-type polymer filter (filtration accuracy 5μm) at the tip at a processing rate of 90 parts by weight / hour in terms of resin amount, and the polymerization solution was devolatilized to obtain resin pellets (B4). The number of rear vents in the vent-type screw twin-screw extruder used was 1, and the number of fore vents was 4 (referred to as the first, second, third, and fourth vents from the upstream side), the barrel temperature was 240°C, and the degree of vacuum was 13.3 to 400hPa (10 to 300mmHg). During devolatilization, ion-exchanged water was introduced from behind the first and second vents at a rate of 1.3 parts by weight / hour, and a solution of a cyclization catalyst deactivator that had been separately prepared was introduced from behind the third vent at a rate of 0.3 parts by weight / hour. As the solution of the cyclization catalyst deactivator, a solution in which 1.0 part by weight of zinc octylate (manufactured by Nippon Kagaku Sangyo Co., Ltd., trade name: Nikka Octyx Zinc 10% by weight) was dissolved in 0.3 parts by weight of toluene was used.
[0282] (Production Example 11 [Production of acrylic resin pellets (A7)] The resin pellets (B4) obtained in Production Example 10 were melt-kneaded using an extruder (φ=40 mm, L / D=16) equipped with a small hot-cut pelletizer (Tanabe Plastics Machinery Co., Ltd., RP40) at the tip at a cylinder temperature of 240°C and a screw rotation speed of 25 rpm, and the molten acrylic resin was extruded at 3.6 kg / h from a die (narrow hole) with a diameter of 3 mm in the extrusion die. The molten acrylic resin extruded from the extrusion die was cut into approximately 0.03 g pieces by rotating (1250 rpm) a cutter blade attached to the tip of the extruder, to obtain disk-shaped resin pellets (A7) with a major axis of 4.6 mm, a minor axis of 4.6 mm, and a thickness of 2.7 mm.
[0283] The resulting resin pellets (A7) had a weight average molecular weight of 130,000, a molecular weight distribution of 2.7, a glass transition temperature of 123° C., a melt flow rate of 1.6, a proportion of ring structures of 16.9% by mass, and an acid value of 0.2 mmol / g or less.
[0284] (Production Example 12 [Production of acrylic resin pellets (A8)] Pellets of a commercially available acrylic resin (Sumipex MH, manufactured by Sumitomo Chemical Co., Ltd., an acrylic resin with no ring structure and composed mainly of methyl methacrylate) were melt-kneaded at a cylinder temperature of 225°C and a screw rotation speed of 25 rpm using an extruder (φ=40 mm, L / D=16) equipped with a small hot-cut pelletizer (RP40, manufactured by Tanabe Plastics Machinery Co., Ltd.) at the tip, and the molten acrylic resin was extruded at 2.8 kg / h from a die (narrow hole) with a diameter of 3 mm in the extrusion die. The molten acrylic resin extruded from the extrusion die was cut into approximately 0.023 g pellets by rotating (1250 rpm) a cutter blade attached to the tip of the extruder, to obtain disk-shaped resin pellets (A8) with a major axis of 4.8 mm, a minor axis of 4.7 mm, and a thickness of 2.1 mm.
[0285] The resulting resin pellets (A8) had a weight average molecular weight of 93,000, a molecular weight distribution of 2.0, a glass transition temperature of 110° C., and a melt flow rate of 2.0.
[0286] Table 1 shows the evaluation results of the acrylic resin pellets (A) obtained in each production example.
[0287] [Table 1]
[0288] Example 1 The acrylic resin pellets (A1) obtained in Production Example 2 were dried at 100°C for 12 hours or more, and then a molded body (size 100mm×100mm×thickness 3mm injection molded body) was produced at a mold temperature of 100°C using an injection molding machine (manufactured by Nissei Plastics Co., Ltd., NS40-5A) having the same injection device as in FIG. 1 and the set temperatures of the injection molding machine shown in Table 2 in a mold of size 100mm×100mm×thickness 3mm.
[0289] Example 2 A molded article was produced in the same manner as in Example 1, except that the pellets of the acrylic resin (A2) obtained in Production Example 3 were used.
[0290] Example 3 A molded article was produced in the same manner as in Example 1, except that the pellets of the acrylic resin (A3) obtained in Production Example 4 were used.
[0291] Example 4 A molded body was produced in the same manner as in Example 1, except that the pellets of the acrylic resin (A3) obtained in Production Example 4 were used and the set temperature of the injection molding machine was changed.
[0292] Example 5 A molded body was produced in the same manner as in Example 1, except that the pellets of the acrylic resin (A5) obtained in Production Example 7 were used, the temperature setting of the injection molding machine was changed, and the mold temperature was set to 90°C.
[0293] Example 6 A molded article was produced in the same manner as in Example 1, except that the pellets of the acrylic resin (A4) obtained in Production Example 5 were used.
[0294] Example 7 A molded body was produced in the same manner as in Example 1, except that the pellets of the acrylic resin (A6) obtained in Production Example 9 were used and the set temperature of the injection molding machine was changed.
[0295] Example 8 A molded body was produced in the same manner as in Example 1, except that the pellets of the acrylic resin (A7) obtained in Production Example 11 were used, the temperature setting of the injection molding machine was changed, and the mold temperature was set to 90°C.
[0296] Example 9 A molded body was produced in the same manner as in Example 1, except that the pellets of the acrylic resin (A8) obtained in Production Example 12 were used, the temperature setting of the injection molding machine was changed, and the mold temperature was set to 80°C.
[0297] Example 10 A molded body was produced in the same manner as in Example 1, except that the pellets of the acrylic resin (A4) obtained in Production Example 5 were used and the set temperature of the injection molding machine was changed.
[0298] Table 2 shows the set temperatures of the injection molding machine and the evaluation results for each example.
[0299] [Table 2]
[0300] As is clear from the above table, by adjusting the pellet size or the temperature of the cooling device to a specific value, it was possible to relatively reduce the occurrence of measurement variations and silver streaks.
[0301] In detail, the results of Examples 6, 10, and 7 show that in an acrylic resin having a ring structure with a relatively small MFR or a relatively large Mw, or in an acrylic resin having no ring structure, the occurrence of measurement variations and silver streaks could be reduced simply by adjusting the temperature of the cooling device to a specific value.
[0302] On the other hand, based on the results of Examples 1 to 5 and Examples 6 and 10, in the case of an acrylic resin having a ring structure with a relatively large MFR or a relatively small Mw, the variation in measurement and the occurrence of silver streaks could be efficiently reduced to a higher level by combining adjustment of the pellet size and adjustment of the temperature of the cooling device.
[0303] In addition, from the results of Examples 6 and 10, by setting the difference in the temperature (Tg-Tj) of the cooling device defined in the present invention to a predetermined range (for example, Tg-Tj of 70°C or less), it was possible to further efficiently reduce the variation in measurement (and coloration). [Industrial Applicability]
[0304] According to the present invention, a novel pellet production method and the like can be provided. [Explanation of symbols]
[0305] 1 nozzle Hn Nozzle section 2 Cylinder H1 Cylinder front (measuring section) H2 Cylinder middle section (compression section) H3 Cylinder rear (supply section) S1 Front of the screw (metering section) S2 Screw middle section (compression section) S3 Rear of the screw (supply section) H4 Cooling device (cooling means) 3. Hopper 4 Temperature measuring device
Claims
1. A method for injection molding a resin, comprising the steps of: The resin comprises an acrylic resin (A), As the resin, pellets with a major axis of 4.0 mm or less are used. When Tj (°C) is the temperature of the cooling device installed in the supply section of the cylinder of the injection molding machine and Tg (°C) is the glass transition temperature of the resin, this method ensures that Tg - Tj (°C) is 72 or less.
2. 2. The method according to claim 1, wherein the acrylic resin (A) has a ring structure.
3. The method according to claim 1 or 2, wherein the acrylic resin (A) has a cyclic ester structure.
4. The method according to any one of claims 1 to 3, wherein the acrylic resin (A) has a melt flow rate of 2 g / 10 min or more at 230°C under a load of 3.8 kg as determined in accordance with JIS K 7210.
5. The method according to any one of claims 1 to 4, wherein the weight average molecular weight of the acrylic resin (A) is 100,000 or less.
6. The method according to any one of claims 1 to 5, wherein the molecular weight distribution of the acrylic resin (A) is 2.5 or less.
7. The method according to any one of claims 1 to 6, wherein the acrylic resin (A) has a cyclic ester structure.
8. The method according to any one of claims 1 to 7, wherein pellets having a major axis of 3.8 mm or less are used as the resin.
9. The method according to any one of claims 1 to 8, wherein Tg-Tj (°C) is 50 or less.
10. the acrylic resin (A) is an acrylic resin having a cyclic ester structure and satisfying at least one of the following characteristics: a melt flow rate of 2 g / 10 min or more at 230° C. under a load of 3.8 kg, a weight average molecular weight of 100,000 or less, and a molecular weight distribution of 2.5 or less, all of which are in accordance with JIS K 7210; The method according to any one of claims 1 to 9, wherein pellets having a major axis and a minor axis of 3.8 mm or less are used as the resin.
11. As the resin, pellets having a major axis of 3.8 mm or less are used, The method according to any one of claims 1 to 10, wherein Tg-Tj (°C) is 50 or less.
12. A method according to any one of claims 1 to 11, wherein the thickness of the pellet is 3.5 mm or less.
13. A method according to any one of claims 1 to 12, wherein pellets having a major axis of 3.8 mm or less and a thickness of 3.5 mm or less are used as the resin, and Tg-Tj (°C) is 50 or less.
14. A method according to any one of claims 1 to 13, wherein pellets having a major axis of 3.8 mm or less and a thickness of 2.7 mm or less are used as the resin, and Tg-Tj (°C) is 50 or less.
15. The acrylic resin (A) is an acrylic resin having a cyclic ester structure and a melt flow rate of 3.5 g / 10 min or more at 230° C. and a load of 3.8 kg, which is in accordance with JIS K 7210; The method according to any one of claims 1 to 14, wherein the resin is in the form of pellets having a major axis of 3.8 mm or less and a thickness of 2.7 mm or less, and Tg-Tj (°C) is 50 or less.
16. An injection molding machine comprising: a cylinder; a nozzle section having a nozzle connected to a front end of the cylinder; and a hopper connected to a rear end of the cylinder; A screw composed of a metering section, a compression section, and a supply section is housed in the cylinder, and these sections correspond to the metering section, the compression section, and the supply section of the cylinder when the screw is pushed in, respectively; A cooling device is installed under the hopper at the base end of the cylinder supply section, The method according to any one of claims 1 to 15, wherein the pellets are fed from a hopper into a supply section of the cylinder.
17. The method according to any one of claims 1 to 16, further comprising a pellet production step of cutting the resin to produce resin pellets, and using the resin pellets obtained in the pellet production step as the resin.
18. The method of claim 17, wherein the molten resin is cut during the pellet production process.
19. The method according to claim 17 or 18, wherein in the pellet production process, the resin extruded from a die of an extruder is cut in a molten state.
Citation Information
Patent Citations
Method for manufacturing optical film
JP2010082990A
Method for preparing thermoplastic resin composition
JP2013007060A
Copolymer, process for producing copolymer, resin composition, molded object, and motor vehicle
WO2017022393A1
Laminate production method
WO2020050184A1