Flame retardant mixtures for thermoplastic polymers
A combination of zinc phosphinate and melamine phosphoric acid reaction products in thermoplastic polymers addresses the limitations of existing halogen-free systems, achieving superior thermal stability and flammability standards with reduced corrosion and migration.
Patent Information
- Application Number
- JP2021545810
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-02-11
- Filing Date
- 2020-02-06
- Publication Date
- 2024-09-26
- Estimated Expiration
- 2040-02-06
AI Technical Summary
Existing halogen-free flame retardant systems for thermoplastic polymers, particularly polyamides and polyesters, fail to meet high thermal stability and international flammability standards such as UL94 V-0, glow wire flammability index (GWFI) requirements, and glow wire ignition temperature (GWIT), while also experiencing issues like corrosion, migration, and degradation during processing.
A flame retardant mixture comprising zinc phosphinate, reaction products of melamine and condensed phosphoric acid, and optional additives like zinc borate and melamine condensation products, in specific proportions, enhances thermal stability and maintains mechanical and electrical properties, achieving UL94 V-0, GWFI of 960°C, and GWIT of 775°C.
The mixture provides improved glow wire resistance, reduced corrosion, minimal migration, and maintains polymer integrity during processing, with enhanced mechanical properties and compliance with stringent flammability standards.
Smart Images

Figure 0007556867000011 
Figure 0007556867000007 
Figure 0007556867000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a flame retardant mixture for thermoplastic polymers and to polymers comprising said flame retardant mixture. [Background technology]
[0002] Many plastics are flammable due to their chemical composition.To be able to achieve the high flame retardancy requirements demanded by plastics processors and in some cases by legislators, plastics usually have to be modified with flame retardants.For this purpose, many different flame retardants and flame retardant synergists are known and commercially available.Because of their more favorable secondary combustion properties in terms of smoke gas density and small gas composition, and for environmental reasons, preferably non-halogenated flame retardant systems have been used for some time.
[0003] Among the non-halogenated flame retardants, the salts of phosphinic acids (phosphinates) have been found to be very effective, especially for thermoplastic polymers (DE-A-2252258 and DE-A-2447727). Here, some derivatives of this flame retardant class are appreciated and used accordingly, due to their less negative effect on the mechanical properties of thermoplastic molding compounds.
[0004] Furthermore, synergistic combinations of phosphinates with certain nitrogen-containing compounds, especially melamine derivatives, have been found and these have been found to be more effective as flame retardants than the phosphinates alone in a whole series of polymers (WO-A-2002 / 28953, WO-A-97 / 01664 and DE-A-19734437 and DE-A-19737727).
[0005] It has further been found that the flame retardant action of various phosphinates in thermoplastic polymers can also be significantly improved by the addition of small amounts of nitrogen-free inorganic or mineral compounds, and that said additives can also improve the flame retardant action of phosphinates in combination with nitrogen-containing synergists (EP-A-0024167, WO-A-2004 / 016684). In particular, the combination of phosphinates with melamine polyphosphates leads in polyamides to a V-0 classification according to the UL94 test.
[0006] The use of phosphinate-containing flame retardant systems initially led to partial polymer decomposition, discoloration of the polymer and smoke evolution during processing, especially at processing temperatures above 300° C. However, these difficulties could be alleviated by the addition of basic or amphoteric oxides, hydroxides, carbonates, silicates, borates or stannates (WO-A-2004 / 022640).
[0007] To further improve the thermal stability, WO-A-2012 / 045414 proposes the combination of phosphinate salts with salts of phosphorous acid. The flame retardant effect of phosphinate salts can be significantly improved, especially in aliphatic polyamides. Compared to the use of melamine polyphosphate as synergist, no exudation is observed after storage at high temperature and humidity.
[0008] WO-A-2014 / 135256 describes flame-retardant polyamides containing phosphinates and phosphites as synergists as well as reinforcements and further additives. The polyamide molding compounds thus obtained show good thermal stability and no tendency to migration. Flammability class UL94 V-0 and creep resistance (comparative tracking index, CTI) of 600 volts are achieved.
[0009] Halogen-free polyamide compositions often do not show sufficient glow-wire results in terms of glow-wire ignition temperature (GWIT) according to IEC 60335, meaning that there is undesirable ignition of the polyamide at the tip of the glow-wire at 750° C. The use of flame-retardant polyamide molding compounds in household appliances that are left standing requires a GWIT of 750° C. or higher.
[0010] US-A-2007 / 299171 (Patent Document 12) discloses thermoplastic, especially polyamides, comprising a phosphinate (F1), a reaction product of melamine and phosphoric acid (F2) and a condensation product of melamine (F3), F1+F2 being at least 13%, preferably at least 15%, based on the total composition. By using F1, F2 and F3 simultaneously, a GWIT of 775°C is reached. The disadvantage of such a preparation is that the use of the reaction product of melamine and phosphoric acid can cause migration effects. Furthermore, the thermal stability is limited to about 300°C; at even higher processing temperatures, polymer decomposition and destruction, and also corrosive effects (e.g. in the screw in compounding and injection molding) can occur.
[0011] WO-A-2009 / 109318A1 (reference 13) describes the corrosion effect of aluminum phosphinate in polyamides and polyesters. The addition of various additives can significantly reduce corrosion.
[0012] US-A-2014 / 0371357 describes a thermoplastic polyamide having 10-40% by weight of glass fibers, 10-40% by weight of melam and 0-15% of a halogen-free flame retardant, the polyamide containing up to 10 mol% of aromatic monomer units. A GWIT of at least 800°C is achieved; the halogen-free flame retardant can be a metal phosphinate. A drawback in using melam is the high loading level of 30-35% to achieve UL94 V-0 and a GWIT>750°C, which reduces the flow and mechanical properties of the polyamide compound. [Prior art documents] [Patent documents]
[0013] [Patent Document 1] DE-A-2252258 [Patent Document 2] DE-A-2447727 [Patent Document 3] WO-A-2002 / 28953 [Patent Document 4] WO-A-97 / 01664 [Patent Document 5] DE-A-19734437 [Patent Document 6] DE-A-19737727 [Patent Document 7] EP-A-0024167 [Patent Document 8] WO-A-2004 / 016684 [Patent Document 9] WO-A-2004 / 022640 [Patent Document 10] WO-A-2012 / 045414 [Patent Document 11] WO-A-2014 / 135256 [Patent Document 12] US-A-2007 / 299171 [Patent Document 13] WO-A-2009 / 109318A1 [Patent Document 14] US-A-2014 / 0371357 Summary of the Invention [Problem to be solved by the invention]
[0014] It was therefore an object of the present invention to provide a halogen-free flame retardant mixture for thermoplastic polymers, in particular polyamides and polyesters, based on phosphorus- and nitrogen-containing flame retardant systems, which has high thermal stability and good mechanical properties, reliably achieves both UL94 V-0 up to a wall thickness of 0.4 mm on test specimens as well as the glow-wire requirements of a Glow Wire Flammability Index (GWFI) of 960°C and a GWIT of 775°C for all tested wall thicknesses, is low in corrosion, shows only slight migration effects, shows good flowability and high electrical values (Comparative Tracking Index (CTI) >550V). [Means for solving the problem]
[0015] It has now surprisingly been found that the glow-wire resistance of thermoplastic polyamides and polyesters can be significantly improved when the molding compound comprises a combination of zinc phosphinate with a reaction product of melamine and condensed phosphoric acid in a specific ratio. In the case of said specific combination, the harmonious property profile of the electrical and mechanical properties of the polyamide is fully preserved. The molding compound thus obtained surprisingly shows only very little corrosion and almost no migration of the flame retardant used. Optionally, said flame retardant mixture further comprises further additives.
[0016] Thermoplastic polymers are mainly processed in the melt. The structural and state changes involved are hardly tolerated by the polymer without changing its chemical structure. Crosslinking, oxidation, molecular weight changes and therefore also changes in physical and technical properties can occur. To reduce the load on the polymer during processing, various additives are used depending on the polymer.
[0017] In many cases, various additives are used simultaneously, each of which has a specific task. For example, antioxidants and stabilizers are used so that the polymer can withstand processing without chemical damage and then have a sufficient time to be stable against external influences such as heat, UV light, weather and oxygen (air). In addition to improving flow properties, lubricants prevent excessive adhesion of the polymer melt to hot machine parts and act as dispersants for pigments, fillers and reinforcing materials.
[0018] The use of flame retardants can affect the stability of polymers during processing in the melt. In order to ensure sufficient flame retardancy of plastics according to international standards, flame retardants often have to be added in high doses. Due to their chemical reactivity required for flame retardant action at high temperatures, flame retardants can impair the processing stability of polymers. This can result, for example, in increased polymer degradation, crosslinking reactions, degassing or discoloration.
[0019] For example, polyamides are stabilized by small amounts of copper halides as well as aromatic amines and sterically hindered phenols, where achieving long-term stability at high continuous use temperatures is of great importance (H. Zweifel (Ed.): “Plastics Additives Handbook”, 5th edition, Carl Hanser Verlag, Munich, 2000, pages 80-84).
[0020] The present invention therefore provides a flame retardant mixture for thermoplastic polymers comprising: As component A), 30 to 55% by weight of a zinc salt of a dialkylphosphinic acid of the formula (I)
[0021] [ka] (In the formula, R 1 and R 2 are the same or different and may be linear, branched or cyclic C1-C 18 -Alkyl, C6-C 18 -Aryl, C7-C 18 -Arylalkyl and / or C7-C 18 -alkylaryl, and M is zinc, and m=1-2; as component B) 45% to 70% by weight of one or more reaction products of melamine with polyphosphoric acids and / or condensed melamine with polyphosphoric acids, As component C), 0% to 10% of one further inorganic flame retardant which is zinc borate, zinc stannate, zinc phosphate, zinc pyrophosphate, magnesium borate and / or calcium stannate, as component D) 0% to 20% by weight of one or more condensation products of melamine, As component E), 0% to 2% by weight of a phosphite or phosphonite or a mixture thereof, and As component F), 0% to 2% by weight, typically C 14 ~C 40 Esters or salts of long-chain aliphatic carboxylic acids (fatty acids) having a chain length of (wherein the sum of said components is always 100% by weight).
[0022] Preferably, the flame retardant mixture for thermoplastic polymers comprises: 35% to 55% by weight of component A), 45% to 65% by weight of component B), 0% to 10% by weight of component C), 0% to 20% by weight of component D), 0% to 2% by weight of component E), and 0% to 2% by weight of component F).
[0023] More preferably, said flame retardant mixture for thermoplastic polymers comprises: 38% to 45% by weight of component A), 45% to 60% by weight of component B), 2% by weight to 10% by weight of component C), 0% to 20% by weight of component D), 0% to 2% by weight of component E), and 0% to 2% by weight of component F).
[0024] Particularly preferably, said flame retardant mixture for thermoplastic polymers comprises: 37% to 45% by weight of component A), 53% to 60% by weight of component B), 2% to 7% by weight of component C), 0% to 20% by weight of component D), 1% to 2% by weight of component E), and 0% to 2% by weight of component F).
[0025] More preferably, said flame retardant mixture for thermoplastic polymers comprises: 30% by weight to 54.7% by weight of component A), 45% to 70% by weight of component B), 0.1% to 10% by weight of component C), 0% to 20% by weight of component D), 0.1% to 2% by weight of component E), and 0.1% to 2% by weight of component F).
[0026] Preferably, said flame retardant mixture for thermoplastic polymers alternatively comprises: 30% by weight to 54.6% by weight of component A), 45% to 70% by weight of component B), 0.1% to 10% by weight of component C), 0.1% to 20% by weight of component D), 0.1% to 2% by weight of component E), and 0.1% to 2% by weight of component F).
[0027] Preferably, in the flame retardant for thermoplastic polymers, R 1 and R 2 are the same or different and are methyl, ethyl, n-propyl, isopropyl, n-butyl, tert-butyl, n-pentyl and / or phenyl.
[0028] Preferably, component D) is melam, melem and / or melon.
[0029] Preferably, component D) is melem.
[0030] Preferably, the flame retardant mixture for thermoplastic polymers according to one or more of claims 1 to 9 further comprises a telomer as component G), which is ethylbutylphosphinic acid, dibutylphosphinic acid, ethylhexylphosphinic acid, butylhexylphosphinic acid, ethyloctylphosphinic acid, sec-butylethylphosphinic acid, 1-ethylbutyl-butyl-phosphinic acid, ethyl-1-methylpentyl-phosphinic acid, di-sec-butylphosphinic acid (di-1-methyl-propylphosphinic acid), propylhexylphosphinic acid, dihexylphosphinic acid, hexylnonylphosphinic acid, dinonylphosphinic acid and / or their zinc salts; with the proviso that components A) and G) are different.
[0031] The present invention also relates to a polymer composition comprising a flame retardant mixture according to at least one of claims 1 to 10 and a thermoplastic and / or thermosetting polymer as component H).
[0032] Preferably, the thermoplastic polymer comprises a polyamide and / or a polyester.
[0033] Preferably, said flame retardant mixture is used for polyamides. The polyamides (PA) are preferably selected from the group consisting of PA6, PA6,6, PA4,6, PA12, PA 6,10, PA4,10, PA10,10, PA11, PA6T / 66, PA6T / 6, PA4T, PA9T, PA10T, polyamide copolymers, polyamide blends and combinations thereof.
[0034] Nylon-6,6 or copolymers or polymer blends of nylon-6,6 and nylon-6 are particularly preferred.
[0035] Preferably, said flame retardant mixture is also used for polyesters, which are preferably polybutylene terephthalate (PBT) or polyethylene terephthalate (PET), or blends of PBT and PET, or polyester elastomers.
[0036] Preferably, the polymer composition according to one or more of claims 11 to 15 comprises: 1% to 96% by weight of polymer 0% to 50% by weight of fillers and / or reinforcing materials, and 3% to 35% by weight of the flame retardant mixture according to at least one of claims 1 to 10. (wherein the percentages are based on the total amount of the polymer composition).
[0037] Preferably, the polymer composition comprises: 15% to 75% by weight of polymer 15% to 45% by weight of fillers and / or reinforcing materials, and 10% to 25% by weight of the flame retardant mixture according to at least one of claims 1 to 10. (wherein the percentages are based on the total amount of the polymer composition).
[0038] More preferably, the polymer composition comprises: 35% to 65% by weight of polymer 25% to 35% by weight of fillers and / or reinforcing materials, and 15% to 25% by weight of the flame retardant mixture according to at least one of claims 1 to 10. (wherein the percentages are based on the total amount of the polymer composition).
[0039] Preferably, the polymer composition according to at least one of claims 11 to 18 has a Comparative Tracking Index (CTI) of 500 volts or more, measured according to the International Electrotechnical Commission standard IEC-60112 / 3.
[0040] Preferably, the polymer composition achieves a rating of V-0 according to UL-94, especially when measured on a moulded article having a thickness of 3.2 mm to 0.4 mm.
[0041] Preferably, said polymer composition has a glow wire flammability index according to IEC 60695-2-12 of 960° C. or higher, in particular measured on a moulded article with a thickness of 0.75 to 3 mm.
[0042] Preferably, the polymer composition has a Glow Wire Ignition Temperature (GWIT) according to IEC-60695-2-13 of at least 775°C.
[0043] Preferably, the polymer composition comprises further additives which are antioxidants, UV stabilizers, gamma radiation stabilizers, hydrolysis stabilizers, co-stabilizers for the antioxidants, antistatic agents, emulsifiers, nucleating agents, plasticizers, processing aids, impact modifiers, dyes, pigments, fillers, reinforcing agents and / or further flame retardants.
[0044] Preferably, the polymer composition comprises glass fibers.
[0045] The invention also relates to the use of the above-mentioned polymer compositions in the electrical, electronics and automotive industries, in packaging in the food sector or in the games and toys sector, as moulding compounds, semi-finished or finished products, as label motifs, in medical technology or as plastic tags for the individual labelling of animals.
[0046] The invention also relates to the use of the polymer composition of the invention for the manufacture of parts in the form of large-area components, in particular large-area components of housing parts of switchgear, of printed circuit boards, housings, foils, wires, switches, distributors, relays, resistors, capacitors, coils, lamps, diodes, LEDs, transistors, connectors, controllers, memory devices and sensors, and in the form of components of complex shapes with demanding geometries.
[0047] More preferably, said flame retardant mixture for thermoplastic polymers comprises zinc borate or zinc stannate as component C) and melam or melem as component D).
[0048] Preferably, the polyamide contains 15% to 45% by weight of glass fibers.
[0049] Preferably, component A) is zinc diethylphosphinate.
[0050] Preferably, component B) is melamine polyphosphate or zinc melamine phosphate or calcium melamine phosphate.
[0051] Preferably, component C) is zinc borate.
[0052] As component E it is preferred to use phosphites of the formula (II) P(OR1)3(II) (R1 is a linear, branched or cyclic C1-C 18 -Alkyl, C6-C 18 -Aryl, C7-C18 -Arylalkyl and / or C7-C 18 -alkylaryl).
[0053] Preferably, the phosphonites (component E)) are components as described by H. Zweifel (Ed.): “Plastics Additives Handbook”, 5th edition, Carl Hanser Verlag, Munich, 2000, pages 108 to 122, in particular those described by Sandostab (登録商標) P-EPQ, Irganox (登録商標) 5057 and L118, Irgafos (登録商標) These include those with names 168, 12 and 38, as well as other compounds.
[0054] These often have the general structure R-[P(OR 5 )2] m (III) [In the formula, R is a mono- or polyvalent aliphatic, aromatic or heteroaromatic organic group; R 5 is a compound of structure (IV)
[0055] [ka] Or, two R's 5 The group forms a bridging group of formula (V)
[0056] [ka] Where: A is a direct bond, O, S, C 1-18 -Alkylene (linear or branched), C 1-18 - alkylidene (linear or branched), R 6 are independently 1-12 -Alkyl (linear or branched), C 1-12 -Alkoxy and / or C 5-12 -cycloalkyl, n is 0 to 5, and m is 1 to 4].
[0057] Mixtures of phosphites and phosphonites may also be used.
[0058] Preferably, component F) comprises alkali metal, alkaline earth metal, aluminium and / or zinc salts of long-chain fatty acids having 14 to 40 carbon atoms and / or reaction products of long-chain fatty acids having 14 to 40 carbon atoms with polyhydric alcohols, such as ethylene glycol, glycerol, trimethylolpropane and / or pentaerythritol.
[0059] The invention further relates to the use of the flame retardant mixtures of the invention in flame retardant polyamide compositions in or for plug connectors, current contact parts in power distribution equipment (residual current protection), circuit boards, potting compounds, plug connectors, circuit breakers, lamp housings, LED housings, capacitor housings, coil components in or on printed circuit boards, ventilators, ground contacts, plugs; housings for plugs, for cables, for flexible circuit boards, for mobile phone charging cables, engine covers, textile coatings and other products.
[0060] Surprisingly, it has been found that the use of the flame retardant mixture of the present invention in polyamide compositions results in a good flame retardant effect (V-0, GWFI and especially GWIT) in combination with improved flowability, low corrosion, high thermal stability and high impact resistance. Polymer degradation is prevented or greatly reduced, and mold adhesion and exudation are not observed. Furthermore, the flame retardant polyamide compositions of the present invention show only slight (if any) discoloration during processing in the melt.
[0061] Thermoplastic polyamides are polyamides whose molecular chains have no or a variable number of side chains of a certain length, which soften when heated and can be molded in virtually infinite ways, according to Hans Domininghaus's "Die Kunststoffe und ihre Eigenschaften [Polymers and their Properties]", 5th edition (1998), p. 14.
[0062] Preferably, the aliphatic polyamides and copolyamides are nylon-12, nylon-4, nylon-4,6, nylon-6, nylon-6,6, nylon-6,9, nylon-6,10, nylon-6,12, nylon-6,66, nylon-7,7, nylon-8,8, nylon-9,9, nylon-10,9, nylon-10,10, nylon-11, nylon-12, etc. These are available, for example, under the tradename Nylon from DuPont. (登録商標) , Ultramid from BASF (登録商標) , Akulon from DSM (登録商標) , Zytel from DuPont (登録商標) , Durethan from Bayer (登録商標) Grillamid from Ems Chemie (登録商標) It is known by the trade name.
[0063] Also suitable are aromatic polyamides, preferably derived from m-xylene, diamines and adipic acid; polyamides made from hexamethylenediamine and iso- and / or terephthalic acid and, optionally, elastomers as modifiers, such as poly-2,4,4-trimethylhexamethylene-terephthalamide or poly-m-phenyleneisophthalamide, block copolymers of the above polyamides with polyolefins, olefin copolymers, ionomers or chemically bonded or grafted elastomers or polyethers, such as polyethylene glycol, polypropylene glycol or polytetramethylene glycol. In addition, there are also polyamides or copolyamides modified with EPDM or ABS; as well as polyamides condensed during processing ("RIM-polyamide systems").
[0064] Also preferred are blends of nylon-6,6 and one or more semi-aromatic amorphous polyamides.
[0065] Other flame retardants or flame retardant synergists not specifically mentioned here can also be used. In particular, nitrogen-containing flame retardants, such as melamine cyanurate, or further phosphorus-based flame retardants, such as aryl phosphates or red phosphorus, can be used. In addition, salts of aliphatic and aromatic sulfonic acids and mineral flame retardant additives, such as aluminum hydroxide and / or magnesium hydroxide, calcium magnesium carbonate hydrate (e.g. DE-A-4236122), can also be used. Also useful are flame retardant synergists from the group of oxygen-, nitrogen- or sulfur-containing metal compounds, preferably zinc oxide, zinc hydroxystannate, zinc sulfide, molybdenum oxide, titanium dioxide, magnesium oxide, magnesium carbonate, calcium carbonate, calcium oxide, titanium nitride, boron nitride, magnesium nitride, zinc nitride, calcium phosphate, calcium borate, magnesium borate or mixtures thereof.
[0066] Suitable further flame retardant additives are preferably charcoal formers, more preferably polyalcohols such as pentaerythritol and dipentaerythritol, phenol-formaldehyde resins, polycarbonates, polyimides, polysulfones, polyethersulfones or polyetherketones, and anti-dripping agents, in particular tetrafluoroethylene polymers.
[0067] The flame retardants may be added in pure form or via a masterbatch or compact.
[0068] Preferably, said condensed melamine compound (component C) is melam or melem.
[0069] [ka] The flame retardant polyamide composition comprising the flame retardant mixture of the present invention may, in a further preferred embodiment, comprise at least one filler or reinforcing material.
[0070] Here, mixtures of two or more different fillers and / or reinforcing materials can also be used, preferably based on talc, mica, silicates, quartz, titanium dioxide, wollastonite, kaolin, amorphous silicas, nanoscale minerals, more preferably based on montmorillonites or nanoboehmite, magnesium carbonate, chalk, feldspar, barium sulfate, glass beads, and / or fibrous fillers and / or reinforcing materials based on carbon fibres and / or glass fibres. Preference is given to using mineral particulate fillers based on talc, mica, silicates, quartz, titanium dioxide, wollastonite, kaolin, amorphous silicas, magnesium carbonate, chalk, feldspar, barium sulfate and / or glass fibres.
[0071] Particular preference is given to using mineral particulate fillers based on talc, wollastonite, kaolin and / or glass fibres.
[0072] Furthermore, it is particularly preferred to use acicular mineral fillers. Acicular mineral fillers are understood in the present invention to mean mineral fillers with very pronounced acicular properties. An example is acicular wollastonite. Preferably, the above minerals have a length to diameter ratio of 2:1 to 35:1, more preferably 3:1 to 19:1, particularly preferably 4:1 to 12:1. The average grain size of the acicular minerals usable in the present invention, as measured with a CILAS grain sizer, is preferably less than 20 μm, more preferably less than 15 μm, particularly preferably less than 10 μm.
[0073] In a preferred embodiment, the filler and / or reinforcing material may be surface-modified, preferably with an adhesion promoter or adhesion promoter system, more preferably with a silane-based adhesion promoter system. However, pretreatment is not necessary. In addition to silanes, polymer dispersions, film formers, branching agents and / or glass fiber processing aids may also be used, especially when glass fibers are used.
[0074] Glass fibres for particular use (generally having a fibre diameter of 7 to 18 μm, preferably 9 to 15 μm) are added in the form of continuous fibres or in the form of chopped or ground glass fibres, which may be modified with suitable size systems and adhesion promoters or adhesion promoter systems, preferably based on silanes.
[0075] The flame-retardant polyamide composition comprising the flame retardant mixture of the present invention can also contain further additives. In the context of the present invention, preferred additives are antioxidants, UV stabilizers, gamma radiation stabilizers, hydrolysis stabilizers, antistatic agents, emulsifiers, nucleating agents, plasticizers, processing aids, impact modifiers, dyes and pigments. The additives can be used alone or in mixtures or in the form of masterbatches.
[0076] Suitable antioxidants are, for example, alkylated monophenols, such as 2,6-di-tert-butyl-4-methylphenol; alkylthiomethylphenols, such as 2,4-dioctylthiomethyl-6-tert-butylphenol; hydroquinones and alkylated hydroquinones, such as 2,6-di-tert-butyl-4-methoxyphenol; tocopherols, such as α-tocopherol, β-tocopherol, γ-tocopherol, δ-tocopherol and mixtures thereof (vitamin E); hydroxylated thiodiphenyl ethers, such as 2,2'-thiobis(6-tert-butyl-4-methylphenol), 2,2'-thiobis(4-octylphenol), 4,4'-thiobis(6-tert-butyl-3-methylphenol), 4,4'-thiobis(6-tert-butyl-2-methylphenol), 4,4'-thiobis(3,6-di-sec-amylphenol), 4,4'-bis-(2,6-di-methyl-4-hydroxyphenyl)-disulfide; alkylidene bisphenols, such as 2,2'-methylenebis(6-tert-butyl-4-methylphenol; O-, N- and S-benzyl compounds, such as 3,5,3',5'-tetra-tert-butyl-4,4'-dihydroxydibenzyl ether; hydroxybenzylated malonates, such as dioctadecyl-2,2-bis(3,5-di-tert-butyl-2-hydroxybenzyl)malonate; hydroxybenzyl aromatics, such as 1,3,5-tris-(3,5-di-tert-butyl)-4-hydroxybenzyl)-2,4,6- trimethylbenzene, 1,4-bis(3,5-di-tert-butyl-4-hydroxybenzyl)-2,3,5,6-tetramethylbenzene, 2,4,6-tris-(3,5-di-tert-butyl-4-hydroxybenzyl)phenol; triazine compounds such as 2,4-bisoctylmercapto-6(3,5-di-tert-butyl-4-hydroxyanilino)-1,3,5-triazine; benzylphosphonates such as dimethyl-2,5-di-tert-butyl-4-hydroxybenzylphosphonate;Acylaminophenols, 4-hydroxylauramide, 4-hydroxystearanilide, N-(3,5-di-tert-butyl-4-hydroxyphenyl)carbamic acid octyl ester; β-(3.5-di-tert-butyl-4-hydroxyphenyl)propionic acid and mono- or polyhydric alcohol esters; β-(5-tert-butyl-4-hydroxy-3-methylphenyl)propionic acid and mono- or polyhydric alcohol esters; β-(3,5-dicyclohexyl-4-hydroxyphenyl)propionic acid and mono- or polyhydric alcohol esters Esters of pionic acid with monohydric or polyhydric alcohols; esters of 3,5-di-tert-butyl-4-hydroxyphenylacetic acid with monohydric or polyhydric alcohols; amides of β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionic acid, such as N,N'-bis(3,5-di-tert-butyl-4-hydroxyphenylpropionyl)hexamethylenediamine, N,N'-bis(3,5-di-tert-butyl-4-hydroxyphenylpropionyl)trimethylenediamine, N,N'-bis-(3,5-di-tert-butyl-4-hydroxyphenylpropionyl)hydrazine;
[0077] Particularly preferably, sterically hindered phenols are used alone or in combination with phosphites, where N,N'-bis[3-(3',5'-di-tert-butyl-4'-hydroxyphenyl)propionyl]hexamethylenediamine (e.g. Irganox, BASF SE, Ludwigshafen, Germany) is preferred. (登録商標) 1098) is particularly preferred.
[0078] Suitable UV absorbers and light stabilizers are, for example, 2-(2'-hydroxyphenyl)benzotriazoles, such as 2-(2'-hydroxy-5'-methylphenyl)benzotriazole; 2-hydroxybenzophenones, such as 4-hydroxy, 4-methoxy, 4-octoxy, 4-decyloxy, 4-dodecyloxy, 4-benzyloxy, 4,2',4-trihydroxy, 2'-hydroxy-4,4'-dimethoxy derivatives; optionally substituted esters of benzoic acid, such as 4-tert-butylphenyl salicylate, phenyl salicylate, octylphenyl salicylate, dibenzoylresorcinol, bis-(4-tert-butylbenzoyl)resorcinol, benzoylresorcinol, 2,4-di-tert-butylphenyl 3,5-di-tert-butyl-4-hydroxybenzoate, hexadecyl 3,5-di-tert-butyl-4-hydroxybenzoate, octadecyl 3,5-di-tert-butyl-4-hydroxybenzoate, 2-methyl-4,6-di-tert-butylphenyl 3,5-di-tert-butyl-4-hydroxybenzoate; acrylates such as ethyl or isooctyl α-cyano-β,β-diphenylacrylate, methyl α-carbomethoxycinnamate, methyl or butyl α-cyano-β-methyl-p-methoxycinnamate, methyl α-carbomethoxy-p-methoxycinnamate, N-(β-carbomethoxy-β-cyanovinyl)-2-methyl-indoline.
[0079] The colorants used are preferably inorganic pigments, in particular titanium dioxide, ultramarine blue, iron oxide, zinc sulfide or carbon black, and also organic pigments, preferably phthalocyanines, quinacridones, perylenes, and dyes, preferably nigrosine and anthraquinones.
[0080] Suitable polyamide stabilizers are, for example, copper salts in combination with iodides and / or phosphorus compounds, and salts of divalent manganese.
[0081] Suitable basic costabilizers are melamine, polyvinylpyrrolidone, dicyandiamide, triallyl cyanurate, urea derivatives, hydrazine derivatives, amines, polyamides, polyurethanes, alkali metal and alkaline earth metal salts of higher fatty acids, such as calcium stearate, zinc stearate, magnesium behenate, magnesium stearate, sodium ricinoleate, potassium palmitate, antimony catecholate or stannous catecholate.
[0082] Suitable nucleating agents are, for example, 4-tert-butylbenzoic acid, adipic acid and diphenylacetic acid, aluminum oxide or silicon dioxide, most preferably talc, but this list is not limiting.
[0083] The flow aids used are preferably copolymers of at least one α-olefin and at least one methacrylic or acrylic ester of an aliphatic alcohol. Particular preference is given here to copolymers in which the α-olefin is composed of ethene and / or propene and the methacrylic or acrylic ester contains, as the alcohol component, a linear or branched alkyl group having 6 to 20 carbon atoms. Very particular preference is given to (2-ethyl)-hexyl acrylate.
[0084] Copolymers suitable in the present invention as flow aids are notable not only for their composition but also for their low molecular weight. Thus, suitable copolymers for compositions to be protected from thermal decomposition according to the present invention are in particular copolymers having a melt flow index (MFI) of at least 100g / 10min, preferably at least 150g / 10min, more preferably at least 300g / 10min at 190°C and a load of 2.16kg. MFI serves to characterize the flow of melts of thermoplastics and is in accordance with ISO1133 or ASTM D1238 standards. In the context of the present invention, MFI and all MFI values are uniformly measured / determined according to ISO1133 with a test weight of 2.16kg at 190°C.
[0085] The plasticizer to be used is preferably dioctyl phthalate, dibenzyl phthalate, butyl benzyl phthalate, hydrocarbon oil or N-(n-butyl)benzenesulfonamide.
[0086] The invention also relates to products, preferably fibres, films or mouldings, obtainable from the compositions according to the invention by injection moulding or extrusion.
[0087] Zinc phosphinates (component A)) are described in PCT / WO97 / 39053, which is expressly incorporated by reference. Particularly preferred phosphinates are zinc dimethylphosphinate, zinc diethylphosphinate, zinc ethylbutylphosphinate and zinc dibutylphosphinate.
[0088] Component F) preferably comprises aluminum stearate, calcium stearate, zinc stearate and / or calcium montanate.
[0089] Suitable components F) are typically 14 ~C 40 The esters are the reaction products of the above carboxylic acids with standard polyhydric alcohols, such as ethylene glycol, glycerol, trimethylolpropane or pentaerythritol. Useful salts of the above carboxylic acids are in particular the alkali metal or alkaline earth metal salts or the aluminum and zinc salts.
[0090] Preferred components F) are esters or salts of stearic acid, such as glyceryl monostearate or calcium stearate.
[0091] Component F) also preferably includes the reaction product of montan wax acid with ethylene glycol.
[0092] Preferably, the reaction product is a mixture of ethylene glycol-mono-montan wax acid ester, ethylene glycol-dimontan wax acid ester, montan wax acid and ethylene glycol.
[0093] Preferably, component F) also includes the reaction product of a montan wax acid and a calcium salt.
[0094] More preferably, the reaction product is a mixture of 1,3-butanediol-mono-montan wax ester, 1,3-butanediol-di-montan wax ester, montan wax acid, 1,3-butanediol, calcium montanate and a calcium salt.
[0095] The inventive polyamide composition comprising the inventive flame retardant mixture according to any one of claims 1 to 10 preferably has a glow wire ignition temperature (GWFI) according to IEC-60695-2-13 of 775°C or higher at a test specimen thickness of 0.4 to 3 mm.
[0096] The additives can be introduced into the polymer in various different process steps. For example, in the case of polyamides, the additives can be mixed into the polymer melt at the beginning or end of the polymerization / polycondensation or in a subsequent compounding operation. Furthermore, there are processing operations in which the additives are not added until a later stage. This is especially the case in the case of the use of pigment or additive masterbatches. It is also possible to apply the additives (especially in powder form) to the polymer pellets, which may be warm as a result of the drying operation, using a drum.
[0097] The invention finally also relates to a process for the production of flame-retardant polymer moldings, in which the flame-retardant polymer molding compositions of the invention are processed at elevated temperature by injection molding (e.g. in an Aarburg Allrounder type injection molding machine) and compression, foam injection molding, internal gas injection molding, blow molding, film casting, calendaring, laminating or coating to give flame-retardant polymer moldings. In addition, the present application relates to the invention described in the claims, but may also include the following as other aspects. 1. The following: As component A), 30 to 55% by weight of a zinc salt of a dialkylphosphinic acid of the formula (I)
change
[0098] example 1. Ingredients used Commercially available polyamides: Nylon-6,6 (PA 6,6-GR): Ultramid (登録商標) A27 (from BASF SE (Germany)) Nylon-6: Ultramid (登録商標) B27 (from BASF SE (Germany)) Nylon-6T / 6,6:Vestamid (登録商標) HTplus M1000 (from Evonik, Germany) Nylon-10T:Vestamid (登録商標) HTplus M3000 (from Evonik, Germany) PPG HP3610 glass fiber (from PPG, The Netherlands) with a diameter of 10 μm and a length of 4.5 mm Flame retardant (component A): Zinc salt of diethylphosphinic acid (hereinafter referred to as DEPZN) For comparison: Aluminum salt of diethylphosphinic acid (hereinafter referred to as DEPAL) Flame retardant (component B): B1: Melamine polyphosphate, Melapur (登録商標) 200 / 70 (from BASF AG(D)) (called MPP) B2: Zinc melamine phosphate, Safire (登録商標) 400 (from Huber (USA)) Flame retardant (component C): C1: Firebrake (登録商標) 500 Zinc Borate (from Rio Tinto (USA)) C2: Zinc stannate, Flamtard (登録商標) S (from William Blythe (UK)) Flame retardant (component D): Delflam (登録商標) NFR (Melem) Phosphonite (Component E): Sandostab (登録商標) P-EPQ (from Clariant GmbH (Germany)) Wax Ingredients (Component F): Licowax (登録商標) E (from Clariant Produkte (Deutschland) GmbH (Germany) (Ester of montan wax acid)
[0099] 2. Production, processing and testing of flame-retardant polyamide molding compounds The flame retardant components were mixed with the phosphonite, lubricant and stabilizer in the ratios given in the table and compounded via the side feeder of a twin-screw extruder (Leistritz ZSE 27 / 44D) into PA6,6 at temperatures between 260 and 310°C or into PA6 at 250 and 275°C. Glass fibres were added via a second side feeder. The homogenised polymer strands were withdrawn, cooled in a water bath and subsequently pelletised.
[0100] After thorough drying, the molding compounds were processed into test specimens in an injection molding machine (Arburg 320 C Allrounder) at a melt temperature of 250-300°C and tested and classified for flame retardancy using the UL94 test (Underwriter Laboratories).
[0101] The UL94 fire classifications are as follows: V-0: Afterflame time does not exceed 10 seconds, total afterflame time after 10 exposures is 50 seconds or less, no burning drips, no complete consumption of the test piece, after flame exposure the afterflame time of the test piece does not exceed 30 seconds. V-1: The afterflame time after the flame is removed does not exceed 30 seconds, the total afterflame time after 10 flame exposures is 250 seconds or less, and the afterflame time of the test piece after the flame is removed does not exceed 60 seconds. Other criteria are as for V-0. V-2: Cotton indicator is ignited by burning droplets. Other criteria are as for V-1. Not classifiable (ncl): Does not meet fire resistance classification V-2.
[0102] The glow-wire resistance was determined using the glow-wire test GWFI (glow-wire flammability index) according to IEC 60695-2-12, and the glow-wire ignition test GWIT (glow-wire ignition temperature) according to IEC 60695-2-13. In the GWFI test, a glow-wire is used at temperatures between 550 and 960 °C on three test specimens (for example, using plates with the shape 60X60X1.5 mm) to determine the highest temperature at which the afterflame time does not exceed 30 seconds and the sample does not burn and fall off. In the GWIT test, by means of a comparable measurement, the glow-wire ignition temperature is recorded, which is 25 K higher (30 K between 900 °C and 960 °C) than the highest glow-wire temperature that does not cause ignition during the contact time of the glow-wire in three consecutive tests. Ignition is considered here as a flame with a burning time of more than 5 seconds.
[0103] The flowability of the molding compositions was measured by determining the melt volume flow rate (MVR) at 275°C / 2.16 kg. A higher MVR value means better flowability in the injection molding process. However, a significant increase in the MVR value may also indicate polymer degradation.
[0104] Corrosion was examined using the plaque method. [Brief description of the drawings]
[0105] The plaque method, developed at the DKI (German Society for Plastics, Darmstadt), provides a model test for the comparative evaluation of metallic materials or for the comparative evaluation of the corrosion and abrasion resistance of plasticized moulding compounds. In this test, two test specimens are placed in pairs in a nozzle so that a rectangular gap with a length of 12 mm, a width of 10 mm and an adjustable height from 0.1 to a maximum of 1 mm is formed for the passage of the plastic melt (Figure 1). Through this gap, the plastic melt is extruded (or injection moulded) from the plasticizing unit, resulting in high local shear stresses and shear rates in the gap.
[0106] The wear measurement parameter was the weight loss determined by weighing the specimens with an analytical A&D Electronic Balance to the nearest 0.1 mg. The mass of the specimens was measured before and after the corrosion test, with a polymer throughput of 25 kg or 50 kg.
[0107] After a defined throughput (typically 25 or 50 kg), the sample plaques are removed and the adhering plastic is washed off by physical / chemical means. Physical cleaning is performed by removing the hot plastic mass by wiping with a soft material (cotton). Chemical cleaning is performed by heating the specimens to 60°C for 20 minutes in m-cresol. Plastic mass still adhering after boiling is removed by wiping with a soft cotton pad.
[0108] All tests in each series were carried out under identical conditions (temperature program, screw configuration, injection molding parameters, etc.) for comparability, unless otherwise stated.
[0109] The results of using the flame retardant-stabilizer mixtures according to the invention are shown in Examples I1 to I3. All amounts are expressed as weight percent and are based on the polymer molding compound including flame retardant, additives and reinforcements.
[0110] [Table 1]
[0111] Only the inventive combination of zinc phosphinate, melamine polyphosphate and zinc borate achieves flammability class UL94 V-0 at 0.4mm while achieving GWIT above 775°C and CTI 600 volts, low corrosion, mild exudation and 65kJ / m 2 Impact strength of over 10kJ / m 2 This results in a polyamide molding compound having a notched impact strength of .
[0112] In contrast, the combination of aluminum phosphinate with melamine polyphosphate and zinc borate shows clear corrosion and significant exudation, as well as lower impact strength and notched impact strength.
[0113] Furthermore, the polyamides with the inventive combination do not show any adhesion to the mould in injection moulding, whereas in the comparative examples adhesion to the mould occurs even after 200 shots, which requires cleaning of the mould.
[0114] [Table 2]
[0115] Overall, only the combination of the present invention achieves all the required parameters.
[0116] [Table 3]
[0117] Only the combination according to the invention achieves all the required parameters even in nylon-6 containing glass fibers: here, even in the injection molding of the preparation according to the invention, no adhesion to the mold is observed.
Claims
1. below: As component A), 30 to 55% by weight of a zinc salt of a dialkylphosphinic acid of the formula (I) [Formula 1] [In the formula, R 1 and R 2 are the same or different and are linear, branched or cyclic C 1 -C 18 -Alkyl, C 6 -C 18 -Aryl, C 7 -C 18 -arylalkyl and / or C 7 -C 18 -alkylaryl, M is zinc, and m=1-2; as component B), 45 to 70% by weight of one or more reaction products of melamine with polyphosphoric acid and / or condensed melamine with polyphosphoric acid, as component C) 0% to 10% of at least one further inorganic flame retardant which is zinc borate, zinc stannate, zinc phosphate, zinc pyrophosphate, magnesium borate and / or calcium stannate, as component D) 0% to 20% by weight of one or more condensation products of melamine, As component E), 0% to 2% by weight of at least one phosphite or phosphinite or a mixture thereof, and As component F) 0% to 2% by weight of at least one, typically C 14 ~C 40 esters and / or salts of long chain aliphatic carboxylic acids (fatty acids) having a chain length of The sum of said components is always 100% by weight, However, the flame retardant mixtures for thermoplastic polymers mentioned above, which contain an aluminum salt of dialkylphosphinic acid, are excluded.
2. below: 30 to 55% by weight of a zinc salt of a dialkylphosphinic acid of the formula (I) as component A) [Case 2] [In the formula, R 1 and R 2 are the same or different and are linear, branched or cyclic C 1 -C 18 -Alkyl, C 6 -C 18 -Aryl, C 7 -C 18 -arylalkyl and / or C 7 -C 18 -alkylaryl, M is zinc, and m=1-2; 45 to 70% by weight of one or more reaction products of melamine with polyphosphoric acid and / or condensed melamine with polyphosphoric acid as component B), as component C) from 0% to 10% of at least one further inorganic flame retardant which is zinc borate, zinc stannate, zinc phosphate, zinc pyrophosphate, magnesium borate and / or calcium stannate, 0% to 20% by weight of one or more condensation products of melamine as component D), 0% to 2% by weight of at least one phosphite or phosphinite or a mixture thereof as component E), and As component F), 0% to 2% by weight of at least one, typically C 14 ~C 40 esters and / or salts of long chain aliphatic carboxylic acids (fatty acids) having a chain length of wherein the sum of said components is always 100% by weight.
3. below: 35% to 55% by weight of component A; 45% to 65% by weight of component B; 0% to 10% by weight of component C), 0% to 20% by weight of component D), 0% to 2% by weight of component E), and 0% to 2% by weight of component F) 3. The flame retardant mixture according to claim 1 or 2, comprising:
4. R in component A) 1 and R 2 4. The flame retardant mixture according to claim 1, wherein are identical or different and are methyl, ethyl, n-propyl, isopropyl, n-butyl, tert-butyl, n-pentyl and / or phenyl.
5. 5. The flame retardant mixture according to claim 1, wherein component D) is melam, melem and / or melon.
6. 6. The flame retardant mixture according to claim 1, wherein component D) is melem.
7. A polymer composition comprising the flame retardant mixture according to any one of claims 1 to 6 and a thermoplastic polymer as component H).
8. 8. The polymer composition of claim 7, wherein the thermoplastic polymer comprises a polyamide and / or a polyester.
9. 9. The polymer composition of claim 8, wherein the polyamide (PA) is selected from the group consisting of PA6, PA6,6, PA4,6, PA12, PA6,10, PA6T / 66, PA6T / 6, PA4T, PA9T, PA10T, polyamide copolymers, polyamide blends and combinations thereof.
10. 10. The polymer composition according to claim 8 or 9, wherein the polyamide is PA6,6 or a copolymer or polymer blend of PA6,6 and PA6.
11. 9. The polymer composition of claim 8, wherein the polyester is polybutylene terephthalate (PBT), or polyethylene terephthalate (PET), or a blend of PBT and PET, or a polyester elastomer.
12. below: 1% to 96% by weight of a thermoplastic polymer 0% to 50% by weight of fillers and / or reinforcing materials, and 3% to 35% by weight of the flame retardant mixture according to any one of claims 1 to 6.
12. The polymer composition according to any one of claims 7 to 11, comprising:
13. below: 15% to 75% by weight of a thermoplastic polymer 15% to 45% by weight of fillers and / or reinforcing materials, and 10% to 25% by weight of the flame retardant mixture according to any one of claims 1 to 6.
13. The polymer composition according to any one of claims 7 to 12, comprising:
14. A polymer composition according to any one of claims 7 to 13, having a comparative tracking index of 500 volts or greater, measured according to International Electrotechnical Commission standard IEC-60112 / 3.
15. A polymer composition according to any one of claims 7 to 14, which achieves a rating of V-0 according to UL-94, measured on moulded articles having a thickness of 3.2 mm to 0.4 mm.
16. A polymer composition according to any one of claims 7 to 15, having a glow wire flammability index according to IEC 60695-2-12 of 960°C or higher, measured on a moulded body of 0.75 to 3 mm thickness.
17. A polymer composition according to any one of claims 7 to 16, having a glow wire ignition temperature (GWIT) according to IEC 60695-2-13 of at least 775°C.
18. 18. The polymer composition according to any one of claims 7 to 17, comprising further additives which are antioxidants, UV stabilizers, gamma radiation stabilizers, hydrolysis stabilizers, co-stabilizers for the antioxidants, antistatic agents, emulsifiers, nucleating agents, plasticizers, processing aids, impact modifiers, dyes, pigments, fillers, reinforcing agents and / or further flame retardants.
19. The polymer composition according to any one of claims 7 to 18, comprising glass fibres.
20. Use of the polymer composition according to any one of claims 7 to 19 in the electrical, electronics and automotive industry, in the food sector, in packaging or in the games and toys sector, as moulding compounds or final products, as label motifs, in medical technology or as plastic tags for the individual labelling of animals.
21. Use of the polymer composition according to any one of claims 7 to 19 for the manufacture of parts of printed circuit boards, housings, foils, wires, switches, distributors, relays, resistors, capacitors, coils, lamps, diodes, LEDs, transistors, connectors, controllers, memory devices and sensors.
Citation Information
Patent Citations
synergistic flame retardant combination for polymers
DE19734437A1
synergistic flame retardant combination for plastics
DE19737727A1
flame retardant THERMOPLASTIC POLYESTER
DE2252258A1
Flame-retardant polyamide molding compounds
DE2447727A1
Method and apparatus for speckle pattern interferometric determination of point displacements
EP0024167A2