Method for producing oxide-containing ceramic sintered body and release sheet
By employing release sheets made from carbides or nitrides of specific periodic table elements, the reaction between oxide-containing ceramic samples and mold release materials is minimized, ensuring the integrity and characteristics of the ceramic sintered body are maintained during hot press firing.
Patent Information
- Application Number
- JP2021561263
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-11-28
- Filing Date
- 2020-11-09
- Publication Date
- 2024-09-26
- Estimated Expiration
- 2040-11-09
AI Technical Summary
The reaction between oxide-containing ceramic samples and graphite mold release materials during hot press firing leads to issues such as sample evaporation, melting, or carbide formation, causing the sample to stick to the spacer, which affects the sample's characteristics.
Using a release sheet formed from carbides or nitrides of Group 4, 5, and 6 elements of the periodic table, such as WC, TiC, TaC, and NbC, to minimize the reaction between the oxide-containing ceramic molded body and the mold release material during hot press firing.
The use of these release sheets suppresses the reaction with the ceramic samples, maintaining the properties of the oxide-containing ceramic sintered body and preventing issues like sticking and chemical changes, while allowing for efficient production with minimal impact on productivity.
Smart Images

Figure 0007556880000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing an oxide-containing ceramic sintered body and a release sheet. [Background technology]
[0002] As a method for firing ceramics, the hot press method is known, in which a sample (ceramic powder or ceramic molded body) is fired while being pressed at high temperature. When manufacturing ceramics by the hot press method, a spacer is generally placed between the sample and the pressing member to protect the sample and the pressing member. This spacer is often made of the same material as the other members to avoid stress concentration due to the difference in thermal expansion coefficient between the other members. For example, in an inert atmosphere, all members are generally made of graphite, and in an oxidizing atmosphere, all members are generally made of alumina or silicon carbide. However, in this method, the sample and the spacer come into direct contact with each other, which causes a problem of reaction between the sample and the spacer, resulting in adhesion or cracking of the spacer. For this reason, a method has been proposed in which a release agent is provided between the sample and the spacer (e.g., Patent Documents 1 to 3). [Prior art documents] [Patent documents]
[0003] [Patent Document 1] Japanese Patent Application Publication No. 10-194847 [Patent Document 2] Patent No. 5002087 [Patent Document 3] JP 2008-031020 A Summary of the Invention [Problem to be solved by the invention]
[0004] In an inert atmosphere or vacuum atmosphere, a graphite sheet is generally used as a release material. However, when a graphite sheet release material is used in hot press sintering at high temperatures, the sample and the release material may react, affecting the properties of the sample. In particular, when an oxide ceramic sample is sintered using a carbon sheet as a release material, the carbon may react with the sample, causing the sample to evaporate, melt, or become carbide. In addition, the reaction between the release material and the sample may progress, causing the release material to be lost, and the sample may come into direct contact with the spacer and stick to it.
[0005] The present invention has been made to solve such problems, and its main object is to suppress the reaction between an oxide-containing ceramic molded body and a release agent during hot-press sintering of an oxide-containing ceramic sintered body. [Means for solving the problem]
[0006] The method for producing an oxide-containing ceramic sintered body of the present invention comprises the steps of: (a) preparing an oxide-containing ceramic molded body prior to firing into an oxide-containing ceramic sintered body; (b) sandwiching the oxide-containing ceramic compact between a pair of release sheets and placing it in a hot press sintering furnace, and hot press sintering the oxide-containing ceramic compact while pressing it with a pair of punches through the pair of release sheets to obtain the oxide-containing ceramic sintered compact; A method for producing an oxide-containing ceramic sintered body, comprising: The release sheet is formed from a carbide or nitride of at least one element selected from the group consisting of elements of groups 4, 5, and 6 of the periodic table.
[0007] In this method for producing an oxide-containing ceramic sintered body, the release sheet is formed of a carbide or nitride of at least one element selected from the group consisting of elements of groups 4, 5, and 6 of the periodic table, so that the release sheet has low reactivity with the oxide-containing ceramic molded body and the reaction with the oxide-containing ceramic molded body is suppressed, thereby suppressing the influence on the properties of the obtained sintered body.
[0008] In the method for producing an oxide-containing ceramic sintered body of the present invention, the release sheet is preferably formed of at least one compound selected from the group consisting of WC, TiC, TaC, and NbC, which can sufficiently suppress the reaction between the release sheet and the oxide-containing ceramic compact, thereby sufficiently suppressing the effect on the properties of the resulting sintered body.
[0009] In the method for producing an oxide-containing ceramic sintered body of the present invention, the thickness of the release sheet is preferably 0.1 mm or more and 5 mm or less. If the thickness of the release sheet is too thin, the oxide-containing ceramic molded body may diffuse through the gaps in the release sheet, reach the punch, and react with the punch. On the other hand, if the thickness is 0.1 mm or more, the reaction between the oxide-containing ceramic molded body and the punch can be suppressed. If the thickness of the release sheet is too thick, the ratio of the release sheet in the hot press sintering furnace increases, and the productivity of the oxide-containing ceramic sintered body decreases. On the other hand, if the thickness of the release sheet is 5 mm or less, the decrease in productivity of the oxide-containing ceramic sintered body can be suppressed.
[0010] In the method for producing an oxide-containing ceramic sintered body of the present invention, in the step (b), a spacer may be interposed between the release sheet and the punch, thereby protecting the oxide-containing ceramic compact and the punch.
[0011] In the method for producing an oxide-containing ceramic sintered body of the present invention, the release sheet is preferably one obtained by forming a slurry containing a release sheet raw material powder, a binder, and a dispersion medium into a sheet shape and then degreasing the same. In this way, a release sheet having a large area can be obtained at low cost, and therefore an oxide-containing ceramic sintered body having a large area can be produced at low cost.
[0012] In the method for producing an oxide-containing ceramic sintered body of the present invention, the particle size of the release sheet raw material powder is preferably 0.1 μm or more and 10 μm or less. If the particle size of the release sheet raw material powder is too small, the powder may not be uniformly dispersed in the slurry, resulting in a non-uniform release sheet. On the other hand, if the particle size of the release sheet raw material powder is 0.1 μm or more, the release sheet raw material powder is uniformly dispersed in the slurry, resulting in a homogeneous sheet. On the other hand, if the particle size of the release sheet raw material powder is too large, the components of the oxide-containing ceramic compact may diffuse into the gaps in the release sheet. On the other hand, if the particle size of the release sheet raw material powder is 10 μm or less, a release sheet having density is obtained, and the diffusion of sample components into the gaps in the release sheet can be suppressed.
[0013] The release sheet of the present invention is A release sheet used when hot-pressing an oxide-containing ceramic sintered body, The release sheet is formed from a carbide or nitride of at least one element selected from the group consisting of elements of groups 4, 5, and 6 of the periodic table.
[0014] Since this release sheet is formed from a carbide or nitride of at least one element selected from the group consisting of elements from groups 4, 5, and 6 of the periodic table, it is possible to obtain a release sheet that has low reactivity with the oxide-containing ceramic formed body and can suppress reaction with the oxide-containing ceramic formed body.
[0015] In the release sheet of the present invention, the release sheet is preferably formed of at least one compound selected from the group consisting of WC, TiC, TaC and NbC, thereby making it possible to obtain a release sheet that can sufficiently suppress the reaction with the oxide-containing ceramic molded body.
[0016] In the release sheet of the present invention, the thickness of the release sheet is preferably 0.1 mm or more and 5 mm or less. If the thickness of the release sheet is too thin, the oxide-containing ceramic molded body may diffuse through the gaps in the release sheet, reach the punch, and react with the punch. On the other hand, if the thickness is 0.1 mm or more, the reaction between the oxide-containing ceramic molded body and the punch can be suppressed. If the thickness of the release sheet is too thick, the ratio of the release sheet in the hot press sintering furnace increases, and the productivity of the oxide-containing ceramic sintered body decreases. On the other hand, if the thickness of the release sheet is 5 mm or less, the decrease in productivity of the oxide-containing ceramic molded body can be suppressed. [Brief description of the drawings]
[0017] [Figure 1] FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0018] The method for producing an oxide-containing ceramic sintered body of the present embodiment includes the steps of: (a) preparing an oxide-containing ceramic molded body prior to firing into an oxide-containing ceramic sintered body; (b) sandwiching the oxide-containing ceramic compact between a pair of release sheets and placing the compact in a hot press sintering furnace, and hot press sintering the oxide-containing ceramic compact while pressing it with a pair of punches through the pair of release sheets to obtain an oxide-containing ceramic sintered compact; It includes.
[0019] In step (a), an oxide-containing ceramic molded body is prepared before being fired into an oxide-containing ceramic sintered body. Examples of the oxide-containing ceramic sintered body include ceramic sintered bodies containing oxides such as alumina, yttria, samaria, magnesia, and zirconia. The oxide-containing ceramic sintered body may be a ceramic sintered body containing an oxide as a main component (a component that accounts for 50 mass% or more (including 100 mass%) of the total), or a ceramic sintered body containing an oxide as a secondary component (a component that accounts for less than 50 mass% of the total). Examples of the ceramic sintered body containing an oxide as a secondary component include ceramic sintered bodies containing an oxide as an auxiliary component (oxide ceramics, non-oxide ceramics such as AlN, Si3N4, and SiC, etc.) and ceramic sintered bodies having an oxide coating on the surface of the raw material powder (AlN, Si3N4, SiC, etc.).
[0020] In step (a), the raw powder of the oxide-containing ceramic sintered body may be filled into a mold, and then uniaxial press molding may be performed at a predetermined pressure to produce the oxide-containing ceramic molded body. Alternatively, the raw powder of the oxide-containing ceramic sintered body may be mixed with a binder and a dispersion medium to prepare a slurry, and the slurry may be molded to produce the oxide-containing ceramic molded body. Since such an oxide-containing ceramic molded body may contain carbon components, it is preferable to use it after degreasing. The degreasing temperature may be set to a temperature at which the organic matter contained in the oxide-containing ceramic molded body is removed by heat. Examples of the binder include ethyl cellulose-based or butyral-based organic compounds. Examples of the dispersion medium include alcohols such as 2-ethylhexanol, octanol, terpineol, and butyl carbitol, and aromatic compounds such as xylene, and the like, which may be used alone or in combination. In addition, plasticizers, dispersants, sintering aids, etc. may be added. Examples of the plasticizer include organic compounds such as phthalates and adipic esters, and examples of the dispersant include esters of polyhydric alcohols and fatty acids such as sorbitan trioleate. Examples of the sintering aids include AlF3, MgO, MgF2, V2O3, CaO, CuO, La2O3, etc., when the ceramic is alumina, and these can be added alone or in combination.
[0021] Alternatively, in step (a), the oxide-containing ceramic molded body may be produced by mold casting. In this case, a ceramic slurry containing the raw powder of the oxide-containing ceramic sintered body, a solvent, a dispersant, and a gelling agent may be poured into a mold, and the gelling agent may be chemically reacted to gel the ceramic slurry, thereby producing the oxide-containing ceramic molded body. The solvent is not particularly limited as long as it dissolves the dispersant and the gelling agent, but it is preferable to use a solvent having two or more ester bonds, such as a polybasic acid ester (e.g., dimethyl glutarate, etc.) or an acid ester of a polyhydric alcohol (e.g., triacetin, etc.). The dispersant is not particularly limited as long as it uniformly disperses the raw powder of the oxide-containing ceramic sintered body in the solvent, but it is preferable to use a polycarboxylic acid copolymer, a polycarboxylate, etc. The gelling agent may include, for example, isocyanates, polyols, and a catalyst. Among these, the isocyanates are not particularly limited as long as they have an isocyanate group as a functional group, and examples thereof include tolylene diisocyanate (TDI), diphenylmethane diisocyanate (MDI), or modified forms thereof. The polyols are not particularly limited as long as they have two or more hydroxyl groups that can react with an isocyanate group, and examples thereof include ethylene glycol (EG), polyethylene glycol (PEG), propylene glycol (PG), and polypropylene glycol (PPG). The catalysts are not particularly limited as long as they promote the urethane reaction between isocyanates and polyols, and examples thereof include triethylenediamine, hexanediamine, and 6-dimethylamino-1-hexanol. Here, the gelling reaction is a reaction in which isocyanates and polyols undergo a urethane reaction to form a urethane resin (polyurethane). The ceramic slurry gels due to the reaction of the gelling agent, and the urethane resin functions as an organic binder.
[0022] The release sheet used in step (b) is a material that does not react with the components of the hot press sintering furnace and does not deteriorate the properties of the ceramic molded body, and is a sheet formed of at least one carbide or nitride of an element selected from the group consisting of Groups 4, 5, and 6 of the periodic table. Examples of Group 4 include Ti, Zr, and Hf, examples of Group 5 include V, Nb, and Ta, and examples of Group 6 include Cr, Mo, and W. The release sheet is preferably a sheet formed of at least one compound selected from the group consisting of WC, TiC, TaC, and NbC, and more preferably a sheet formed of at least one compound selected from the group consisting of TaC and NbC. It may also be a mixture of at least two or more compounds selected from the group consisting of WC, TiC, TaC, and NbC. The release sheet may be a molded sheet obtained by molding the raw material powder of the release sheet into a sheet shape, a sintered sheet obtained by sintering the molded sheet, or a single crystal sheet, but a molded sheet is preferable from the perspective of cost. When a molded sheet or a sintered sheet is used as the release sheet, it may contain impurities such as sintering aids as long as they do not affect the reactivity with the oxide-containing ceramic, the sinterability of the oxide-containing ceramic, or the properties of the sintered body. As the release sheet, a sheet with flat front and back surfaces (flat sheet) is preferable.
[0023] When a molded sheet obtained by molding the raw material powder of the release sheet into a sheet shape is used as the release sheet, examples of the molding method include uniaxial press molding, tape molding, extrusion molding, casting molding, and injection molding, among which uniaxial press molding or tape molding is preferred. The raw material powder of the release sheet may be molded as it is, or may be molded using a slurry prepared together with a binder and a dispersion medium. Specific examples of the binder and dispersion medium are as described above. In addition, plasticizers, dispersants, sintering aids, etc. may be added as appropriate, and specific examples thereof are also as described above. For example, when uniaxial press molding is adopted, the release sheet may be produced by filling the raw material powder of the release sheet into a mold and then performing uniaxial press molding at a predetermined pressure. When the release sheet contains carbon components, it is preferable to degrease the release sheet to remove the carbon components before use. In order to increase the density of the release sheet, the particle size of the raw material powder of the release sheet is preferably 10 μm or less, more preferably 5 μm or less. If the release sheet has high density, it is possible to prevent the oxide-containing ceramic formed body from diffusing into the release sheet when the oxide-containing ceramic formed body is sandwiched between a pair of release sheets and hot-press fired in step (b). The particle size of the raw material powder of the release sheet is preferably 0.1 μm or more, and more preferably 0.5 μm or more, in order to improve dispersibility when the release sheet is formed using a slurry of the raw material powder.
[0024] In step (b), the oxide-containing ceramic molded body is sandwiched between a pair of release sheets and placed in a hot press sintering furnace, and the ceramic molded body is hot press sintered while being pressed by a pair of punches through the pair of release sheets to obtain an oxide-containing ceramic sintered body. In this case, a spacer may be interposed between the release sheet and the punch. In addition, when a plurality of ceramic molded bodies are sintered, a spacer may be arranged so as to contact the release sheet at any position. The thickness of the release sheet is not particularly limited, but when a molded sheet is used as the release sheet, if the thickness is too thin, the oxide-containing ceramic molded body may diffuse through the gaps in the release sheet in step (b) to reach the punch and react with the punch. In addition, when a spacer is arranged between the release sheet and the punch, it may react with the spacer. In order to prevent the oxide-containing ceramic molded body from diffusing through the gaps in the release sheet to reach the punch or the spacer, the thickness of the release sheet is preferably 0.1 mm or more, more preferably 0.2 mm or more. On the other hand, if the thickness of the release sheet is too thick, the ratio of the release sheet in the hot press sintering furnace increases, and the productivity of the oxide-containing ceramic sintered body decreases. In order not to decrease the productivity of the oxide-containing ceramic sintered body, the thickness of the release sheet is preferably 5 mm or less, and more preferably 2 mm or less.
[0025] A cross-sectional view of a graphite furnace 10, which is an example of a hot press sintering furnace, is shown in FIG. 1. The graphite furnace 10 is equipped with a graphite mold 12 having a heater function, and a graphite sleeve 14 that is arranged inside the graphite mold 12 and is vertically divided into two. When an oxide-containing ceramic molded body 16 is hot press sintered in this graphite furnace 10, the oxide-containing ceramic molded body 16 is sandwiched between a pair of release sheets 18, 18, and further sandwiched between a pair of graphite spacers 20, 20, and then placed inside the graphite sleeve 14, and the oxide-containing ceramic molded body 16 is heated while being pressed by a pair of graphite punches 22, 22. When the oxide-containing ceramic is alumina, the sintering atmosphere in the hot press sintering is not particularly limited, but an inert gas such as nitrogen or Ar, or a vacuum atmosphere is preferable. The pressure is 50 kgf / cm. 2 More than 200kgf / cm is preferable.2 The firing temperature (maximum temperature) is preferably 1700 to 2050°C, more preferably 1750 to 2000°C. When the temperature is lowered from the maximum temperature, the pressure is increased by 50 kgf / cm until the temperature reaches a predetermined temperature (a temperature set in the range of 1000 to 1400°C (preferably 1100 to 1300°C)). 2 It is preferable to apply a pressure of 50 kgf / cm or more in the temperature range below the predetermined temperature. 2 It is preferable to release the pressure to a pressure less than 1200° C. In this way, it is possible to prevent cracks from occurring in the sintered body. The timing for releasing the pressing pressure is preferably at 1200° C. during the temperature drop in order to prevent cracks from occurring.
[0026] In the method for producing an oxide-containing ceramic sintered body according to the present embodiment described above, the release sheet is formed of a carbide or nitride of at least one element selected from the group consisting of elements of groups 4, 5, and 6 of the periodic table. Therefore, the release sheet has low reactivity with the oxide-containing ceramic molded body, and the reaction with the oxide-containing ceramic molded body is suppressed. Therefore, the effect on the properties of the obtained sintered body can be suppressed.
[0027] The release sheet is preferably made of at least one compound selected from the group consisting of WC, TiC, TaC, and NbC, which can sufficiently suppress the reaction between the release sheet and the oxide-containing ceramic compact, and can sufficiently suppress the effect on the properties of the resulting sintered body.
[0028] Furthermore, the thickness of the release sheet is preferably 0.1 mm or more and 5 mm or less. If the thickness of the release sheet is too thin, the oxide-containing ceramic molded body may diffuse through the gaps in the release sheet, reach the spacer (punch if there is no spacer, same below), and react with the spacer. On the other hand, if the thickness is 0.1 mm or more, the reaction between the oxide-containing ceramic molded body and the spacer can be suppressed. If the thickness of the release sheet is too thick, the ratio of the release sheet in the hot press sintering furnace increases, and the productivity of the oxide-containing ceramic sintered body decreases. On the other hand, if the thickness of the release sheet is 5 mm or less, the decrease in productivity of the oxide-containing ceramic sintered body can be suppressed.
[0029] Furthermore, in the step (b), since a spacer is interposed between the release sheet and the punch, the oxide-containing ceramic formed body and the punch can be protected.
[0030] The release sheet is preferably one which is prepared by forming a slurry containing a release sheet raw material powder, a binder and a dispersion medium into a sheet shape and then degreasing the same, whereby a release sheet having a large area can be obtained at low cost, and therefore an oxide-containing ceramic sintered body having a large area can be produced at low cost.
[0031] The particle size of the release sheet raw material powder is preferably 0.1 μm or more and 10 μm or less. If the particle size of the release sheet raw material powder is too small, the powder may not be uniformly dispersed in the slurry, resulting in the production of a non-uniform release sheet. On the other hand, if the particle size of the release sheet raw material powder is 0.1 μm or more, the release sheet raw material powder is uniformly dispersed in the slurry, resulting in the production of a homogeneous sheet. On the other hand, if the particle size of the release sheet raw material powder is too large, the sample components may diffuse into the gaps in the release sheet. On the other hand, if the particle size of the release sheet raw material powder is 10 μm or less, a release sheet having a dense property is obtained, and the diffusion of the sample components into the gaps in the release sheet can be suppressed.
[0032] It goes without saying that the present invention is not limited to the above-described embodiment, and can be embodied in various forms within the technical scope of the present invention. EXAMPLES
[0033] Examples of concretely producing oxide-containing ceramic sintered bodies are described below as examples. Experimental Examples 1 to 4, 6 to 9, 11 to 14, and 16 to 19 correspond to examples of the present invention, and Experimental Examples 5, 10, 15, and 20 correspond to comparative examples. Note that the present invention is not limited to the following examples.
[0034] [Experimental Example 1] (1) Preparation of alumina compact Commercially available alumina powder with an average particle size (D50) of 0.6 μm was used as the raw material, and a pressed body with a diameter of 20 mm and a thickness of 8 mm was obtained by uniaxial press molding using a mold. The pressing pressure was 200 kgf / cm 2 The average particle size (D50) of each powder was measured using a particle size distribution analyzer (Nikkiso, MT3300II).
[0035] (2) Preparation of release sheet The raw material was a commercially available tantalum carbide (TaC) powder with an average particle size (D50) of 1.6 μm. Two pressed bodies with a diameter of 20 mm and a thickness of 2 mm were produced by uniaxial press molding using a metal mold, and these were used as TaC release sheets (flat sheets) to be used when hot-pressing the alumina compact. The pressing pressure was 200 kgf / cm. 2 It was decided.
[0036] (3) Hot press firing The three-layer structure (TaC release sheet / alumina compact / TaC release sheet) in which the TaC release sheet prepared in (2) was laminated on the top and bottom surfaces of the alumina compact prepared in (1) was then sintered in the graphite furnace 10 shown in Fig. 1 in argon at a sintering temperature (maximum temperature reached) of 1700°C for 4 hours with a surface pressure of 200 kgf / cm. 2After firing, the TaC release sheet and the alumina sintered body were separated, and no visible reaction between the TaC release sheet and the alumina sintered body was observed.
[0037] (4) Evaluation of sintered alumina In order to evaluate the reactivity of the alumina sintered body with the TaC release sheet, an EDS analysis was performed on the surface of the alumina sintered body that had been in contact with the TaC release sheet using a SEM / EDS device (JEOL, JSM-6390). As a result, Ta and C components were not detected on the surface of the alumina sintered body. In addition, to check whether or not there was a reaction between the TaC release sheet and the alumina sintered body, the obtained alumina sintered body was cut so as to pass through the center of the substrate in a direction perpendicular to the plate surface. The cross section of the cut sample was smoothed by lapping using diamond abrasive grains, and was mirror-finished by chemical mechanical polishing (CMP) using colloidal silica. A cross-section of the alumina sintered body was observed using a SEM / EDS device (JEOL, JSM-6390). As a result, Ta and C components were not detected inside the alumina sintered body, indicating that the alumina did not react with the TaC release sheet during sintering.
[0038] [Experimental Example 2] Alumina sintered bodies were produced using the same method as in Experimental Example 1, except that commercially available niobium carbide (NbC) powder with an average particle size (D50) of 2.3 μm was used as the raw material for the release sheet, and the reactivity was evaluated. As a result, after sintering, the NbC release sheet and the alumina sintered body were separated, and no visible reaction was observed between the NbC release sheet and the alumina sintered body. In addition, Nb and C components were not detected in SEM / EDS observation of the surface and cross section of the alumina sintered body, indicating that the alumina and the NbC release sheet did not react during sintering.
[0039] [Experimental Example 3] Alumina sintered bodies were produced using the same method as in Experimental Example 1, except that commercially available tungsten carbide (WC) powder with an average particle size (D50) of 2.2 μm was used as the raw material for the release sheet, and the reactivity was evaluated. As a result, after firing, the WC release sheet and the alumina sintered body were separated, and no visible reaction was observed between the WC release sheet and the alumina sintered body. In addition, W and C components were not detected in SEM / EDS observation of the surface and cross section of the alumina sintered body, indicating that the alumina and the WC release sheet did not react during firing.
[0040] [Experimental Example 4] Alumina sintered bodies were produced in the same manner as in Experimental Example 1, except that commercially available titanium carbide (TiC) powder with an average particle size (D50) of 2.1 μm was used as the raw material for the release sheet, and the reactivity was evaluated. As a result, after firing, the TiC release sheet and the alumina sintered body were separated, and no visible reaction was observed between the TiC release sheet and the alumina sintered body. In addition, Ti and C components were not detected in SEM / EDS observation of the surface and cross section of the alumina sintered body, indicating that the alumina and the TiC release sheet did not react during firing.
[0041] [Experimental Example 5] An alumina sintered body was produced in the same manner as in Experimental Example 1, except that an expanded graphite sheet (Nikafilm FL-400, manufactured by Nippon Carbon Co., Ltd.), a commercially available graphite sheet, was used as the release sheet, and the reactivity was evaluated. As a result, after sintering, the expanded graphite sheet disappeared due to a reaction with the alumina sintered body. In addition, the alumina sintered body was thinned, and the formation of a reaction product between C (carbon) and the alumina component was confirmed. SEM / EDS observation of the deposits suggested that the deposits were metallic aluminum and aluminum carbide produced by the reduction of the alumina component by C.
[0042] [Experimental Example 6] (1) Preparation of Y2O3 compact Commercially available Y2O3 powder with an average particle size (D50) of 0.4 μm was used as the raw material, and a press molded body with a diameter of 20 mm and a thickness of 8 mm was obtained by uniaxial press molding using a mold. The pressing pressure was 200 kgf / cm 2It was decided.
[0043] (2) Preparation of release sheet A TaC release sheet (flat sheet) was produced in the same manner as in Experimental Example 1.
[0044] (3) Hot press firing The TaC release sheet prepared in (2) was laminated on the top and bottom surfaces of the Y2O3 compact prepared in (1) to form a three-layer structure (TaC release sheet / Y2O3 compact / TaC release sheet). The structure was then sintered in N2 in the graphite furnace 10 shown in Fig. 1 at a sintering temperature (maximum temperature reached) of 1950°C for 4 hours with a surface pressure of 200 kgf / cm. 2 After sintering, the TaC release sheet and the Y2O3 sintered compact were separated, and no visible reaction between the TaC release sheet and the Y2O3 sintered compact was observed.
[0045] (4) Evaluation of Y2O3 sintered body In order to evaluate the reactivity between the Y2O3 sintered compact and the TaC release sheet, SEM / EDS observations of the surface and cross section of the Y2O3 sintered compact were carried out in the same manner as in Experimental Example 1. As a result, Ta and C components were not detected on the surface or inside of the Y2O3 sintered compact, indicating that Y2O3 did not react with the TaC release sheet during sintering.
[0046] [Experimental Example 7] A Y2O3 sintered body was prepared using the same method as in Experimental Example 6, except that a commercially available niobium carbide (NbC) powder with an average particle size (D50) of 2.3 μm was used as the raw material for the release sheet, and the reactivity was evaluated. As a result, after sintering, the NbC release sheet and the Y2O3 sintered body were separated, and no visible reaction was observed between the NbC release sheet and the Y2O3 sintered body. In addition, SEM / EDS observation of the surface and cross section of the Y2O3 sintered body did not detect Nb or C components on the surface or inside the sintered body, indicating that Y2O3 and the NbC release sheet did not react during sintering.
[0047] [Experimental Example 8] A Y2O3 sintered body was prepared using the same method as in Experimental Example 6, except that a commercially available tungsten carbide (WC) powder with an average particle size (D50) of 2.2 μm was used as the raw material for the release sheet, and the reactivity was evaluated. As a result, it was found that the Y2O3 sintered body and the WC release sheet were adhered to each other after firing. The obtained three-layer structure (WC release sheet / Y2O3 sintered body / WC release sheet) was cut so as to pass through the center of the substrate in a direction perpendicular to the plate surface. The cut sample was smoothed on the cross section by lapping using diamond abrasive grains, and was mirror-finished by chemical mechanical polishing (CMP) using colloidal silica. The obtained cross-sectional sample was observed around the WC release sheet / Y2O3 sintered body interface using a SEM / EDS device (JSM-6390, manufactured by JEOL Ltd.). As a result, trace amounts of W and C components were detected within a range of about 7 μm in the thickness direction inside the Y2O3 sintered body from the Y2O3 sintered body / WC release sheet interface. These results show that there is almost no reaction between Y2O3 and the WC release sheet during firing, and that the WC release sheet can be used as a release material. However, it was also shown that processing is required to separate the WC release sheet after firing, and that the WC component is slightly diffused inside the Y2O3, and that the diffused area must be removed by grinding or other methods.
[0048] [Experimental Example 9] A Y2O3 sintered body was prepared using the same method as in Experimental Example 6, except that a commercially available titanium carbide (TiC) powder with an average particle size (D50) of 2.1 μm was used as the raw material for the release sheet, and the reactivity was evaluated. As a result, it was found that the Y2O3 sintered body and the TiC release sheet were adhered to each other after sintering. The obtained three-layer structure (TiC release sheet / Y2O3 sintered body / TiC release sheet) was cut so as to pass through the center of the substrate in a direction perpendicular to the plate surface. The cut sample was smoothed on the cross section by lapping using diamond abrasive grains, and was mirror-finished by chemical mechanical polishing (CMP) using colloidal silica. The obtained cross-sectional sample was observed around the TiC release sheet / Y2O3 sintered body interface using a SEM / EDS device (JSM-6390, manufactured by JEOL Ltd.). As a result, trace amounts of Ti and C components were detected within a range of about 9 μm in the thickness direction inside the Y2O3 sintered body from the Y2O3 sintered body / TiC release sheet interface. These results show that Y2O3 hardly reacts with the TiC release sheet during firing, and that the TiC release sheet can be used as a release material. However, it was also shown that processing is required to separate the TiC release sheet after firing, that the TiC component is slightly diffused inside the Y2O3, and that the diffused area must be removed by grinding or other methods.
[0049] [Experimental Example 10] A Y2O3 sintered body was prepared in the same manner as in Experimental Example 6, except that a commercially available graphite sheet (Nikafilm FL-400, manufactured by Nippon Carbon) was used as the release sheet, and the reactivity was evaluated. As a result, after sintering, the expanded graphite sheet disappeared due to a reaction with the Y2O3 sintered body. In addition, the Y2O3 sintered body was thinned, and the formation of reaction products between C and the Y2O3 component was confirmed. SEM / EDS observation of the reaction products suggested that the reaction products were metallic yttrium, yttrium carbide, and yttrium nitride, which were generated by the reduction and reductive nitridation of the Y2O3 component by C.
[0050] [Experimental Example 11] (1) Preparation of Si3N4 compact To 100 parts by mass of commercially available Si3N4 powder with an average particle size (D50) of 0.7 μm, 3 parts by mass of commercially available Al2O3 powder with an average particle size (D50) of 0.6 μm and 5 parts by mass of commercially available Y2O3 powder with an average particle size (D50) of 0.4 μm were added as sintering aids, and then the mixture was mixed in ethanol for 24 hours using a pot mill. The resulting slurry was dried, sieved through a #100 sieve, and uniaxially pressed using a mold to obtain a pressed compact with a diameter of 20 mm and a thickness of 8 mm. The pressing pressure was 200 kgf / cm 2 It was decided.
[0051] (2) Preparation of release sheet 100 parts by mass of commercially available tantalum carbide (TaC) powder with an average particle size (D50) of 1.6 μm was mixed with 3.2 parts by mass of acrylic binder (Orikox #2434T, Kyoeisha Chemical Co., Ltd.), 1.3 parts by mass of bis(2-ethylhexyl) phthalate (DOP, J-Plus Co., Ltd.) as a plasticizer, 0.2 parts by mass of polyether ester acid amine (DA-234, Kusumoto Chemical Co., Ltd.) as a dispersant, and xylene and 1-butanol as a dispersion medium. The amount of the dispersion medium was adjusted so that the slurry viscosity was 20000 cP. The slurry prepared in this way was tape-cast onto a PET film by the doctor blade method so that the thickness after drying was 200 μm, and a molded sheet was obtained. This molded sheet was sandwiched between alumina setters and placed in a degreasing furnace, where it was degreased in nitrogen at 500°C for 6 hours to produce a TaC release sheet (flat sheet) to be used when hot-pressing the Si3N4 molded body.
[0052] (3) Hot press firing The three-layer structure (TaC release sheet / Si3N4 compact / TaC release sheet) in which the TaC release sheet prepared in (2) was laminated on the top and bottom surfaces of the Si3N4 compact prepared in (1) was then sintered in the graphite furnace 10 in Fig. 1 at a sintering temperature (maximum temperature reached) of 1800°C for 4 hours under nitrogen and a surface pressure of 200 kgf / cm. 2 After sintering, the TaC release sheet and the Si3N4 sintered body were separated, and no visible reaction between the TaC release sheet and the Si3N4 sintered body was observed.
[0053] (4) Evaluation of Si3N4 sintered body In order to evaluate the reactivity of the Si3N4 sintered compact with the TaC release sheet, the surface and cross section of the Si3N4 sintered compact were observed by SEM / EDS in the same manner as in Experimental Example 1. As a result, Ta and C components were not detected on the surface or inside of the Si3N4 sintered compact, indicating that Si3N4 and the auxiliary components Al2O3 and Y2O3 did not react with the TaC release sheet during sintering.
[0054] [Experimental Example 12] A Si3N4 sintered body was prepared using the same method as in Experimental Example 11, except that a commercially available niobium carbide (NbC) powder with an average particle size (D50) of 2.3 μm was used as the raw material for the release sheet, and the reactivity was evaluated. As a result, after sintering, the NbC release sheet and the Si3N4 sintered body were separated, and no visible reaction was observed between the NbC release sheet and the Si3N4 sintered body. In addition, Nb and C components were not detected in the SEM / EDS observation of the surface and cross section of the Si3N4 sintered body, indicating that Si3N4 and the auxiliary components Al2O3 and Y2O3 did not react with the NbC release sheet during sintering.
[0055] [Experimental Example 13] A Si3N4 sintered body was prepared using the same method as in Experimental Example 11, except that a commercially available tungsten carbide (WC) powder with an average particle size (D50) of 2.2 μm was used as the raw material for the release sheet, and the reactivity was evaluated. As a result, after firing, the WC release sheet and the Si3N4 sintered body were separated, and no visible reaction was observed between the WC release sheet and the Si3N4 sintered body. In addition, W and C components were not detected in the SEM / EDS observation of the surface and cross section of the Si3N4 sintered body, indicating that Si3N4 and the auxiliary components Al2O3 and Y2O3 did not react with the WC release sheet during firing.
[0056] [Experimental Example 14] A Si3N4 sintered body was prepared using the same method as in Experimental Example 11, except that a commercially available titanium carbide (TiC) powder with an average particle size (D50) of 2.1 μm was used as the raw material for the release sheet, and the reactivity was evaluated. As a result, after sintering, the TiC release sheet and the Si3N4 sintered body were separated, and no visible reaction was observed between the TiC release sheet and the Si3N4 sintered body. In addition, Ti and C components were not detected in the SEM / EDS observation of the surface and cross section of the Si3N4 sintered body, indicating that Si3N4 and the auxiliary components Al2O3 and Y2O3 did not react with the TiC release sheet during sintering.
[0057] [Experimental Example 15] A Si3N4 sintered body was prepared using the same method as in Experimental Example 11, except that a commercially available graphite sheet (Nikafilm FL-400, manufactured by Nippon Carbon) was used as the release sheet, and the reactivity was evaluated. As a result, the expanded graphite sheet and the Si3N4 sintered body did not separate after sintering. Part of the expanded graphite sheet disappeared due to the reaction with Al2O3 and Y2O3, which are sintering aids in the Si3N4 sintered body, and the formation of reaction products between C and the Al2O3 and Y2O3 components was confirmed. SEM / EDS observation of the reaction products suggested that the reaction products were metallic aluminum, aluminum carbide, metallic yttrium, and yttrium carbide.
[0058] [Experimental Example 16] (1) Preparation of SiC compact To 100 parts by mass of commercially available SiC powder with an average particle size (D50) of 0.7 μm, 18 parts by mass of commercially available AlN powder with an average particle size (D50) of 0.5 μm and 12 parts by mass of commercially available Y2O3 powder with an average particle size (D50) of 0.4 μm were added as sintering aids, and then mixed in ethanol for 24 hours using a pot mill. The resulting slurry was dried, sieved through a #100 sieve, and uniaxially pressed using a mold to obtain a pressed compact with a diameter of 20 mm and a thickness of 8 mm. The pressing pressure was 200 kgf / cm 2 It was decided.
[0059] (2) Preparation of release sheet 100 parts by mass of commercially available tantalum carbide (TaC) powder with an average particle size (D50) of 1.6 μm was mixed with 3.2 parts by mass of acrylic binder (Orikox #2434T, Kyoeisha Chemical Co., Ltd.), 1.3 parts by mass of bis(2-ethylhexyl) phthalate (DOP, J-Plus Co., Ltd.) as a plasticizer, 0.2 parts by mass of polyether ester acid amine (DA-234, Kusumoto Chemical Co., Ltd.) as a dispersant, and xylene and 1-butanol as a dispersion medium. The amount of the dispersion medium was adjusted so that the slurry viscosity was 20000 cP. The slurry thus prepared was tape-cast onto a PET film by the doctor blade method so that the thickness after drying was 200 μm, and a molded sheet was obtained. This molded sheet was sandwiched between alumina setters and placed in a degreasing furnace, and degreased in nitrogen at 500 °C for 6 hours to obtain a TaC release sheet (flat sheet) to be used when hot-pressing and sintering a SiC molded body.
[0060] (3) Hot press firing The three-layer structure (TaC release sheet / SiC compact / TaC release sheet) in which the TaC release sheets prepared in (2) were laminated on the top and bottom surfaces of the SiC compact prepared in (1) was then sintered in the graphite furnace 10 shown in Fig. 1 in argon at a sintering temperature (maximum temperature reached) of 2000°C for 4 hours with a surface pressure of 200 kgf / cm. 2 After firing, the TaC release sheet and the SiC sintered body were separated, and no visible reaction was observed between the TaC release sheet and the SiC sintered body.
[0061] (4) Evaluation of sintered SiC In order to evaluate the reactivity of the SiC sintered compact with the TaC release sheet, the surface and cross section of the SiC sintered compact were observed by SEM / EDS in the same manner as in Experimental Example 1. As a result, Ta and C components were not detected on the surface or inside of the SiC sintered compact, indicating that SiC and the auxiliary components AlN and Y2O3 did not react with the TaC release sheet during sintering.
[0062] [Experimental Example 17] A SiC sintered body was produced using the same method as in Experimental Example 16, except that a commercially available niobium carbide (NbC) powder with an average particle size (D50) of 2.3 μm was used as the raw material for the release sheet, and the reactivity was evaluated. As a result, after sintering, the NbC release sheet and the SiC sintered body were separated, and no visible reaction was observed between the NbC release sheet and the SiC sintered body. In addition, Nb and C components were not detected in the SEM / EDS observation of the surface and cross section of the SiC sintered body, indicating that SiC and the auxiliary components AlN and Y2O3 did not react with the NbC release sheet during sintering.
[0063] [Experimental Example 18] A SiC sintered body was produced using the same method as in Experimental Example 16, except that commercially available tungsten carbide (WC) powder with an average particle size (D50) of 2.2 μm was used as the raw material for the release sheet, and the reactivity was evaluated. As a result, after firing, the WC release sheet and the SiC sintered body were separated, and no visible reaction was observed between the WC release sheet and the SiC sintered body. In addition, W and C components were not detected in SEM / EDS observation of the surface and cross section of the SiC sintered body, indicating that SiC and the auxiliary components AlN and Y2O3 did not react with the WC release sheet during firing.
[0064] [Experimental Example 19] A SiC sintered body was produced using the same method as in Experimental Example 16, except that commercially available titanium carbide (TiC) powder with an average particle size (D50) of 2.1 μm was used as the raw material for the release sheet, and the reactivity was evaluated. As a result, after firing, the TiC release sheet and the SiC sintered body were separated, and no visible reaction was observed between the TiC release sheet and the SiC sintered body. In addition, Ti and C components were not detected in SEM / EDS observation of the surface and cross section of the SiC sintered body, indicating that SiC and the auxiliary components AlN and Y2O3 did not react with the TiC release sheet during firing.
[0065] [Experimental Example 20] A SiC sintered body was produced using the same method as in Experimental Example 16, except that a commercially available graphite sheet (Nikafilm FL-400, manufactured by Nippon Carbon) was used as the release sheet, and the reactivity was evaluated. As a result, the expanded graphite sheet and the SiC sintered body did not separate after sintering. Part of the expanded graphite sheet disappeared due to a reaction with Y2O3, a sintering aid in the SiC sintered body, and the formation of a reaction product between C and the Y2O3 component was confirmed. SEM / EDS observation of the reaction product suggested that the reaction product was metallic yttrium and yttrium carbide.
[0066] This application claims priority from Japanese Patent Application No. 2019-215374, filed on November 28, 2019, the entire contents of which are incorporated herein by reference. [Industrial Applicability]
[0067] The present invention can be used in the case of hot press firing an oxide-containing ceramic sintered body. [Explanation of symbols]
[0068] 10 graphite furnace, 12 graphite mold, 14 graphite sleeve, 16 ceramic molding body, 18 release sheet, 20 graphite spacer, 22 graphite punch.
Claims
1. (a) preparing an oxide-containing ceramic molded body before being fired into an oxide-containing ceramic sintered body; (b) sandwiching the oxide-containing ceramic compact between a pair of release sheets and placing the oxide-containing ceramic compact in a hot press sintering furnace, and hot press sintering the oxide-containing ceramic compact while pressing it with a pair of punches through the pair of release sheets to obtain the oxide-containing ceramic sintered compact; A method for producing a ceramic sintered body comprising: The release sheet is formed of a carbide of at least one element selected from the group consisting of elements of Groups 4, 5, and 6 of the periodic table. Method for producing oxide-containing ceramic sintered bodies.
2. The release sheet is formed of at least one compound selected from the group consisting of WC, TiC, TaC and NbC, A method for producing the oxide-containing ceramic sintered body according to claim 1.
3. The thickness of the release sheet is 0.1 mm or more and 5 mm or less. A method for producing the oxide-containing ceramic sintered body according to claim 1 or 2.
4. In the step (b), a spacer is interposed between the release sheet and the punch. A method for producing the oxide-containing ceramic sintered body according to any one of claims 1 to 3.
5. The release sheet is obtained by forming a slurry containing a release sheet raw material powder, a binder, and a dispersion medium into a sheet shape and then degreasing the same. A method for producing the oxide-containing ceramic sintered body according to any one of claims 1 to 4.
6. The particle size of the release sheet raw material powder is 0.1 μm or more and 10 μm or less. A method for producing the oxide-containing ceramic sintered body according to claim 5.
7. A release sheet used when hot-pressing an oxide-containing ceramic sintered body, The release sheet is formed of a carbide of at least one element selected from the group consisting of elements of Groups 4, 5, and 6 of the periodic table. Release sheet.
8. The release sheet is formed of at least one compound selected from the group consisting of WC, TiC, TaC and NbC, The release sheet according to claim 7.
9. The thickness of the release sheet is 0.1 mm or more and 5 mm or less. The release sheet according to claim 7 or 8.
Citation Information
Patent Citations
JP1975002087A
Non-oxide ceramics hot press method
JP1983079872A
Boron nitride sheet
JP1990279569A
Production of ceramic compact
JP1998194847A
Sintering mold of pressurized sintering device
JP2002338370A