Halogen-free flame-retardant polyamide composite material and its manufacturing method

JP7557059B2Active Publication Date: 2024-09-26KINGFA SCI & TECH CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2023519582
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-09-29
Filing Date
2021-02-23
Publication Date
2024-09-26
Estimated Expiration
2041-02-23

Smart Images

  • Figure 0007557059000002
    Figure 0007557059000002
  • Figure 0007557059000003
    Figure 0007557059000003
  • Figure 0007557059000001
    Figure 0007557059000001
Patent Text Reader

Abstract

The present invention discloses a halogen-free flame-retardant polyamide composite containing 20-50 parts by weight of an aliphatic polyamide, 10-30 parts by weight of an aromatic polyamide, 20-30 parts by weight of a halogen-free flame retardant, 10-50 parts by weight of glass fiber, 1-5 parts by weight of a char-forming agent, and 0-5 parts by weight of an auxiliary agent, where the aromatic polyamide is at least one of PA66 / 6T, PA-MXD6, and PA6T / 6I, and the char-forming agent is at least one of dipentaerythritol and tripentaerythritol. In the halogen-free flame-retardant polyamide composite, the aromatic polyamide itself has heat aging resistance and exhibits a certain synergistic effect with the dense char layer formed by the char-forming agent during aging. This allows the halogen-free flame-retardant polyamide composite to have excellent weather resistance, aging resistance, and flame retardancy. The present invention also discloses a method for producing the halogen-free flame-retardant polyamide composite.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to the field of polymeric material modification, in particular to halogen-free flame retardant polyamide composite materials and methods for their preparation. [Background technology]

[0002] Halogen-free flame-retardant polyamide materials are widely used in the electronics, electrical and automotive industries, and have excellent comprehensive mechanical properties and heat resistance, but with the advancement of miniaturization and integration, the requirements for materials at the production end are increasing, while the existing related products are no longer able to meet these requirements in terms of aging resistance and weather resistance, which is one of the important factors limiting the application of such products. When optimization is performed using a conventional antioxidant system, the improvement effect is very limited, so it is necessary to effectively improve the performance of materials through the optimization of the entire formulation system. Summary of the Invention [Problem to be solved by the invention]

[0003] In view of the above, the present invention aims to solve the above-mentioned deficiencies of the prior art and provide a halogen-free flame-retardant polyamide composite material with high weather resistance and high aging resistance. [Means for solving the problem]

[0004] In order to achieve the above object, the technical solution adopted by the present invention is as follows: A halogen-free flame-retardant polyamide composite material is provided, comprising, as components, 20-50 parts by mass of an aliphatic polyamide, 10-30 parts by mass of an aromatic polyamide, 20-30 parts by mass of a halogen-free flame retardant, 10-50 parts by mass of glass fiber, 1-5 parts by mass of a char former, and 0-5 parts by mass of an auxiliary, wherein the aromatic polyamide is at least one of PA66 / 6T, PA MXD6, and PA6T / 6I, and the char former is at least one of dipentaerythritol and tripentaerythritol.

[0005] In the halogen-free flame-retardant polyamide composite material of the present application, a specific aromatic polyamide and a char-forming agent are blended, utilizing the heat aging resistance of the aromatic polyamide itself and the synergistic effect with the dense carbonized layer formed by the char-forming agent during aging, and the two exert a synergistic effect of improving the effects, thereby imparting excellent weather resistance, aging resistance and flame retardancy to the halogen-free flame-retardant polyamide composite material.

[0006] Preferably, the aromatic polyamide is at least one of PA66 / 6T, PA6T / 6I, and the char-forming agent is dipentaerythritol.

[0007] Preferably, the aliphatic polyamide is at least one of PA6, PA46, PA66, PA56, PA610.

[0008] More preferably, the aliphatic polyamide is PA66.

[0009] Preferably, the halogen-free flame retardant is a blend of aluminum diethylphosphinate, boehmite, and zinc borate, and the mass ratio of the aluminum diethylphosphinate, the boehmite, and the zinc borate is (15-16):(4-5):(2-3).

[0010] Preferably, the glass fiber is at least one selected from E glass fiber, H glass fiber, R, S glass fiber, D glass fiber, C glass fiber, and quartz glass fiber.

[0011] Preferably, the halogen-free flame-retardant polyamide composite material contains, as components, 20 to 50 parts by mass of an aliphatic polyamide, 15 to 25 parts by mass of an aromatic polyamide, 20 to 30 parts by mass of a halogen-free flame retardant, 10 to 50 parts by mass of glass fiber, 1.5 to 3 parts by mass of a char-forming agent, and 0 to 5 parts by mass of an auxiliary.

[0012] Preferably, the auxiliary agent is at least one selected from an antioxidant and a lubricant, the antioxidant is a hindered phenol-based antioxidant, and the lubricant is at least one selected from a higher fatty acid, a higher fatty acid metal salt, a higher fatty acid ester, and a higher fatty acid amide.

[0013] Examples of the hindered phenol-based antioxidant include octadecyl-3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate, n-octadecyl-3-(3'-methyl-5-tert-butyl-4'-hydroxyphenyl)propionate, n-tetradecyl-3-(3',5'-di-tert-butyl-4'-hydroxyphenyl)propionate, 1,6-hexanediol bis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate, ester], tetrakis(methylene-3-(3',5'-di-tert-butyl-4'-hydroxyphenyl)propionate)methane, 3,9-bis{2-[3-(3-tert-butyl-4-hydroxy-5-methylphenyl)propionyloxy]-1,1-dimethylethyl}-2,4,8,10-tetraoxaspiro[5,5]undecane, N,N'-bis-[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionyl]hexamethylenediamine, and the like.

[0014] The present invention further provides a method for producing the halogen-free flame-retardant polyamide composite material, which includes premixing each component other than the glass fiber in a high-speed mixer to obtain a premix, feeding the premix into a twin-screw extruder to melt and mix with the glass fiber and extrude to granulate, and injection molding the extruded and granulated polyamide material to obtain the halogen-free flame-retardant polyamide composite material, wherein the major axis ratio of the screws of the twin-screw extruder is 40:1 to 48:1, the glass fiber is fed at the 5th to 6th stage side of the screws, the barrel temperature is 240 to 300°C, and the screw rotation speed is 300 to 500 rpm.

[0015] The present invention further discloses the use of the halogen-free flame-retardant polyamide composite material in vehicle materials. Effect of the Invention

[0016] Compared with the prior art, the beneficial effects of the present invention are as follows:

[0017] In the halogen-free flame-retardant polyamide composite material of the present application, by blending a specific aromatic polyamide and a char-forming agent, the aromatic polyamide itself has the ability to resist heat aging, and has a synergistic effect with the dense carbonized layer formed by the char-forming agent during aging, and the two exert a synergistic effect of improving the effects, thereby imparting excellent weather resistance, aging resistance and flame retardancy to the halogen-free flame-retardant polyamide composite material. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0018] In order to make the objectives, technical solutions and advantages of the present invention clearer, the present invention will be further described below with reference to specific examples. The following examples are merely representative examples of the present invention, and the scope of the present invention is not limited thereto.

[0019] In the following examples and comparative examples, the test methods for each performance are as follows. (1) Flame retardancy: The flame retardancy test was carried out on a sample with a thickness of 0.8 mm according to the relevant standard of UL 94 2018. Flame retardancy has an important significance for electrical safety, and in order to meet the application needs, the flame retardancy grade according to UL94 2018 needs to reach V-0. (2) Aging resistance: The aging resistance test is evaluated according to the relevant rules and methods of UL 746B 2018. The ISO 527-2 1BA sample with an aging temperature of 230°C and a thickness of 0.8 mm is used as the test sample. The time required for the tensile strength to decrease to 50% of the initial performance is recorded, and this is used as the evaluation index of aging resistance. (3) Weather resistance: Weather resistance is tested and evaluated in accordance with the relevant standards of Cycle 4892-2. The test samples are flat plates, and the color difference ΔE before and after deterioration by a xenon lamp is recorded as the evaluation index.

[0020] The materials used in the examples and comparative examples are as follows. Aliphatic polyamide: Polyamide resin A1: Product name PA66 EP-158, manufactured by Huafeng Group Co., Ltd. Aliphatic polyamide: Polyamide resin A2: Product name PA56, manufactured by Shandong Kaisai Co., Ltd. Aliphatic polyamide: Polyamide resin A3: Product name PA610 F150, manufactured by Shandong Guangyin Co., Ltd. Aromatic polyamide: Polyamide resin B: PA 6T / 6I, product name Selar PA 3462R, manufactured by DuPont Aromatic polyamide: Polyamide resin C: PA66 / 6T, product name C1504T, manufactured by Shandong Guangyin Co., Ltd. Aromatic polyamide: Polyamide resin D: PAMXD6, manufactured by Shanghai Yingli Chemical Co., Ltd. Aromatic polyamide: Polyamide resin E: PA6I, manufactured by Shandong Xianglong New Materials Co., Ltd. Halogen-free flame retardants: Aluminum diethylphosphinate, product name OP1230, phosphorus content 23-24% by mass, manufactured by Clariant Boehmite, product name BG-613SO, manufactured by Isseki Tsushin Co., Ltd. Zinc borate, product name ZB-500, manufactured by Chengdu Kaifei High-Performance Chemical Co., Ltd. Antioxidant: Hindered phenol antioxidant, N,N'-bis-[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionyl]hexamethylenediamine, product name IRGANOX 1098, manufactured by BASF Lubricant: Higher fatty acid ester, product name LOXIOL G 32, manufactured by Emery Glass fiber: ECS11-4.5-560A, E-glass fiber, manufactured by China Megashi Co., Ltd., diameter 11 μm Char formers: Dipentaerythritol, product name CHARMOR DP40, manufactured by Perstorp Tripentaerythritol, product name Sigma-Aldrich, manufactured by Merck Pentaerythritol, manufactured by Hubei Yihua Group Co., Ltd.

[0021] In the manufacturing method of the halogen-free flame-retardant polyamide composite material according to the embodiment of the present invention, each component other than the glass fiber is premixed in a high-speed mixer to obtain a premix, which is then fed into a twin-screw extruder to melt, mix, and extrude to form granules (here, the screw major axis ratio of the twin-screw extruder is 40:1 (glass fiber is fed at the 5th to 6th stage side of the screw), the barrel temperature is 240 to 300°C, and the screw rotation speed is 300 rpm). The extruded and granulated polyamide composite material is injection molded at an injection temperature of 280°C and an injection pressure of 70 MPa.

[0022] In the present application, Examples 1 to 14 and Comparative Examples 1 to 8 were designed, and the content and performance data of each component in Examples 1 to 7 are shown in Table 1, the content and performance data of each component in Examples 8 to 14 are shown in Table 2, and the content and performance data of each component in Comparative Examples 1 to 8 are shown in Table 3.

[0023] Table 1: Content and performance data of each component in Examples 1 to 7 [Table 1]

[0024] Table 2: Content and performance data of each component in Examples 8 to 14 [Table 2]

[0025] Table 3: Content and performance data of each component in Comparative Examples 1 to 8 [Table 3]

[0026] From a comparison of Examples 1 to 3, it was found that the aliphatic polyamide in Example 1 was PA66, and Example 1 was superior to Examples 2 and 3 in aging resistance and weather resistance.

[0027] From a comparison of Examples 4 to 6, it was found that the aromatic polyamide in Example 4 was PA 6T / 6I, the aromatic polyamide in Example 5 was PA66 / 6T, and the aromatic polyamide in Example 6 was PA MXD6, and that the aging resistance and weather resistance of Examples 4 and 5 were superior to that of Example 6.

[0028] Comparison of Example 4 and Example 7 shows that the char former in Example 4 is dipentaerythritol, and the char former in Example 7 is tripentaerythritol, and the aging resistance and weather resistance of Example 4 are superior to those of Example 7.

[0029] From a comparison between Examples 4 and 8 and Examples 9 to 10, it was found that in Examples 4 and 8, the mass ratio of aluminum diethylphosphinate, boehmite, and zinc borate was (15-16):(4-5):(2-3), while in Examples 9 to 10, the mass ratio of aluminum diethylphosphinate, boehmite, and zinc borate was not within the range of (15-16):(4-5):(2-3), and therefore Examples 4 and 8 were superior in aging resistance and weather resistance to Examples 9 and 10.

[0030] Comparing Examples 4, 13, and 14 with Example 12, it was found that in Examples 4, 13, and 14, the aromatic polyamide was in the range of 15 to 25 parts by mass, and the char-forming agent was in the range of 1.5 to 3 parts by mass, while in Example 12, the aromatic polyamide was not in the range of 15 to 25 parts by mass, and the char-forming agent was not in the range of 1.5 to 3 parts by mass. It was found that Examples 4, 13, and 14 had better aging resistance and weather resistance than Example 12.

[0031] A comparison of Example 4 with Comparative Examples 1 to 8 reveals that when no aromatic polyamide and no char-forming agent are blended, or when either an aromatic polyamide or a char-forming agent is blended alone, or when both are blended but the blending amounts or components are not within the preferred ranges, the anti-aging properties, weather resistance, and flame retardancy of the entire material are all clearly inferior to those of Example 4 of the present application.

[0032] It should be noted that the above embodiments are merely for illustrating the technical solutions of the present invention, and are not intended to limit the scope of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, it is obvious to those skilled in the art that the technical solutions of the present invention can be modified or equivalently substituted without departing from the spirit and scope of the technical solutions of the present invention.

Claims

1. 1. A halogen-free, flame-retardant polyamide composite material, comprising:

1. A halogen-free flame-retardant polyamide composite material comprising, as components, 20 to 50 parts by mass of an aliphatic polyamide, 10 to 30 parts by mass of an aromatic polyamide, 20 to 30 parts by mass of a halogen-free flame retardant, 10 to 50 parts by mass of glass fiber, 1 to 5 parts by mass of a char-forming agent, and 0 to 5 parts by mass of an auxiliary, relative to 100 parts by mass of the halogen-free flame-retardant polyamide composite material, wherein the aromatic polyamide is at least one of PA66 / 6T, PA MXD6, and PA6T / 6I, the char-forming agent is at least one of dipentaerythritol and tripentaerythritol, the halogen-free flame retardant is a blend of aluminum diethylphosphinate, boehmite, and zinc borate, and the mass ratio of the aluminum diethylphosphinate, the boehmite, and the zinc borate is (15 to 16):(4 to 5):(2 to 3).

2. 2. The halogen-free flame-retardant polyamide composite material according to claim 1, wherein the aromatic polyamide is at least one of PA66 / 6T, PA6T / 6I, and the char former is dipentaerythritol.

3. 2. The halogen-free flame-retardant polyamide composite material according to claim 1, wherein the aliphatic polyamide is at least one of PA6, PA46, PA66, PA56, and PA610.

4. 4. The halogen-free flame retardant polyamide composite material according to claim 3, characterized in that the aliphatic polyamide is PA66.

5. 2. The halogen-free flame-retardant polyamide composite material according to claim 1, wherein the glass fiber is at least one selected from the group consisting of E glass fiber, H glass fiber, R, S glass fiber, D glass fiber, C glass fiber, and quartz glass fiber.

6. The halogen-free flame-retardant polyamide composite material according to claim 1, characterized in that it comprises, as components, 20 to 50 parts by mass of an aliphatic polyamide, 15 to 25 parts by mass of an aromatic polyamide, 20 to 30 parts by mass of a halogen-free flame retardant, 10 to 50 parts by mass of glass fiber, 1.5 to 3 parts by mass of a char-forming agent, and 0 to 5 parts by mass of an auxiliary.

7. 2. The halogen-free flame-retardant polyamide composite material according to claim 1, characterized in that the auxiliary is at least one selected from an antioxidant and a lubricant, the antioxidant is a hindered phenol-based antioxidant, and the lubricant is at least one selected from a higher fatty acid, a higher fatty acid metal salt, a higher fatty acid ester, and a higher fatty acid amide.

8. A method for producing the halogen-free flame-retardant polyamide composite material according to any one of claims 1 to 7, comprising the steps of: Each component other than the glass fiber is premixed in a high-speed mixer to obtain a premix, and then the premix is ​​fed into a twin-screw extruder to melt and mix with the glass fiber, and then extruded to form granules; and performing injection molding on the extruded and granulated polyamide material to obtain a halogen-free flame-retardant polyamide composite material; The method for producing a halogen-free flame-retardant polyamide composite material is characterized in that the screw length ratio of the twin-screw extruder is 40:1 to 48:1, the glass fiber is fed at the 5th to 6th stage side of the screw, the barrel temperature is 240 to 300°C, and the screw rotation speed is 300 to 500 rpm.

9. Use of the halogen-free flame-retardant polyamide composite material according to any one of claims 1 to 7 in a vehicle material.

Citation Information

Patent Citations

  • Flame-retardant resin composition

    JP2005336473A

  • Flame-retardant polyamide molding compound and its use

    JP2007507566A

  • Flame-retardant polyamide resin composition and articles containing the same

    JP2013523958A

  • Halogen-free flame-retardant polyamide composition

    JP2013542311A

  • Polyamide compositions

    JP2016117898A