Manufacturing method of molded product and molded product

By controlling temperature differences and employing extrusion molding, the method effectively reduces particle generation in molded articles made from tetrafluoroethylene/perfluoro(alkyl vinyl ether) copolymers, addressing contamination issues in semiconductor and chemical supply equipment.

JP7557155B2Active Publication Date: 2024-09-27DAIKIN INDUSTRIES LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2023142193
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2018-07-12
Filing Date
2023-09-01
Publication Date
2024-09-27
Estimated Expiration
2039-07-10

AI Technical Summary

Technical Problem

Existing methods for manufacturing molded articles using tetrafluoroethylene/perfluoro(alkyl vinyl ether) copolymers fail to adequately suppress the generation of particles, particularly in semiconductor devices and chemical supply equipment, where these particles contaminate high-purity chemical solutions and are difficult to remove.

Method used

A manufacturing method involving controlled temperature differences during the preparation and molding steps, where temperature T1 (molding material preparation) and temperature T2 (molding) satisfy the relationship 20≦T1-T2≦80, along with the use of extrusion molding and specific conditions to minimize low molecular weight substance volatilization, is employed to reduce particle generation.

Benefits of technology

The method significantly reduces particle generation in the final molded product, ensuring low particle counts even after cleaning with isopropyl alcohol, enhancing the suitability of the product for semiconductor and chemical supply applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007557155000006
    Figure 0007557155000006
  • Figure 0007557155000004
    Figure 0007557155000004
  • Figure 0007557155000005
    Figure 0007557155000005
Patent Text Reader

Abstract

To provide a method for producing a molding that makes it possible to produce a molding with reduced generation of particles.SOLUTION: A method for producing a molding has a preparation step for preparing a molding material by molding a tetrafluoroethylene / perfluoro (alkyl vinyl ether) copolymer at temperature T1(°C), and a molding step for extrusion molding the molding material at temperature T2(°C) to obtain a molding, where temperature T1 and temperature T2 satisfy the relation of 20≤T1-T2≤80.SELECTED DRAWING: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a method for producing a molded article and to a molded article. [Background technology]

[0002] Patent Document 1 describes a method for producing a stabilized fluoropolymer, characterized in that, prior to stabilization of a fluoropolymer by melt-kneading in a kneader including a stabilization treatment zone for stabilizing a melt-processable fluoropolymer having unstable groups in the presence of water and oxygen, a melting zone for melt-kneading the fluoropolymer at a temperature and for a time sufficient to decompose or volatilize low molecular weight substances in the fluoropolymer is disposed as a zone preceding the stabilization treatment zone, and the low molecular weight substances are decomposed and / or volatilized in the melting zone and released outside the kneader prior to the stabilization treatment zone. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] International Publication No. 2002 / 050135 Summary of the Invention [Problem to be solved by the invention]

[0004] An object of the present disclosure is to provide a method for producing a molded article that can produce a molded article with a reduced amount of particle generation. Another object of the present disclosure is to provide a molded product with reduced particle generation. [Means for solving the problem]

[0005] According to the present disclosure, there is provided a method for producing a molded product, which includes a preparation step of molding a tetrafluoroethylene / perfluoro(alkyl vinyl ether) copolymer at a temperature T1 (°C) to prepare a molding material, and a molding step of extrusion molding the molding material at a temperature T2 (°C) to obtain a molded product, wherein the temperatures T1 and T2 satisfy the relationship 20≦T1-T2≦80.

[0006] The temperature T1 (°C) in the preparation step is preferably 390°C or higher. The tetrafluoroethylene / perfluoro(alkyl vinyl ether) copolymer used in the preparation step preferably has a melting point of 295° C. or higher. The tetrafluoroethylene / perfluoro(alkyl vinyl ether) copolymer used in the preparation step preferably has a perfluoro(alkyl vinyl ether) unit content of 3.5 to 7.0 mass %. In the preparation step, the molding material is preferably prepared by extrusion molding. The molding material obtained in the preparation step is preferably in the form of pellets. The molded product obtained in the molding step is preferably a tube.

[0007] The present disclosure also provides a molded article that contains a tetrafluoroethylene / perfluoro(alkyl vinyl ether) copolymer having a melting point of 295°C or higher, and that, when contacted with isopropyl alcohol, disperses in isopropyl alcohol in an amount of 700 particles / ml or less having a size of 30 nm or larger.

[0008] The molded article of the present disclosure is preferably a tube. Effect of the Invention

[0009] According to the present disclosure, it is possible to provide a method for manufacturing a molded article that can produce a molded article with a reduced amount of particle generation. Furthermore, according to the present disclosure, it is possible to provide a molded product with reduced particle generation. [Brief description of the drawings]

[0010] [Figure 1] FIG. 1 is a diagram for explaining the mechanism by which particles adhere to a tube in a conventional tube molding process. [Diagram 2] FIG. 2 is a diagram illustrating an example of the preparation process. [Diagram 3] FIG. 3 is a diagram for explaining a method for measuring the number of particles. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] Specific embodiments of the present disclosure will be described in detail below, but the present disclosure is not limited to the following embodiments.

[0012] With the progress of semiconductor miniaturization processes, it is becoming important to reduce contaminants from molded products used in semiconductor devices and chemical supply equipment. For example, JP2014-222756A points out the problem of particles being generated from piping for supplying chemicals and getting into the chemicals.

[0013] Molded articles containing a copolymer containing tetrafluoroethylene units (TFE units) and perfluoro(alkyl vinyl ether) units (PAVE units) (hereinafter referred to as TFE / PAVE copolymer (or PFA)) are used in large numbers in semiconductor devices and chemical supply equipment because of their excellent chemical resistance, and the area in contact with high-purity chemicals is large. However, in the prior art including Patent Document 1, no method has been considered for suppressing particle generation from molded articles containing a TFE / PAVE copolymer, which can exhibit a very high melting point depending on the composition.

[0014] Therefore, the present inventors have conducted extensive research into particle reduction technology and have found that by strictly controlling the temperature at which the TFE / PAVE copolymer is heated in the series of processes for producing a molded article from raw materials, it is possible to suppress particle generation from the final molded article to an unprecedented level.

[0015] In addition, according to the findings obtained by the present inventors, even if a molded product is washed with ultrapure water until particles are no longer detectable, if the washed molded product is further contacted with isopropyl alcohol, particles are detected in the isopropyl alcohol. In other words, the number of particles cannot be accurately evaluated by the conventional evaluation method of washing a molded product with ultrapure water, recovering the ultrapure water (washing water), and measuring the particles dispersed in the ultrapure water, but it has also been discovered that the number of particles can be accurately evaluated for the first time by a new evaluation method using isopropyl alcohol.

[0016] The manufacturing method disclosed herein has been completed based on these findings, and includes a preparation step of molding a TFE / PAVE copolymer at a temperature T1 (°C) to prepare a molding material, and a molding step of extrusion molding the molding material at a temperature T2 (°C) to obtain a molded product, and is characterized in that the temperatures T1 and T2 satisfy the relationship 20≦T1-T2≦80.

[0017] The temperature T1 (°C) in the preparation step is the molding temperature when the TFE / PAVE copolymer is molded to prepare the molding material. In the preparation step, the molding temperature may be set to be constant within a range that does not interfere with molding, or the molding temperature may be changed. When the molding temperature is changed, the molding temperature can be changed so that the temperature T1 and the temperature T2 satisfy the relationship 20≦T1-T2≦80, with the temperature at any point in the preparation step being T1. That is, the temperature T1 in the preparation step may be the temperature at any point in the preparation step, or may be the maximum temperature in the preparation step. The temperature T1 is not the copolymer temperature, but the set temperature of the molding machine used for molding.

[0018] The temperature T1 is preferably higher than the melting point or softening point of the TFE / PAVE copolymer, more preferably higher than the melting point of the TFE / PAVE copolymer, even more preferably higher than 350°C, even more preferably higher than 370°C, particularly preferably higher than 390°C, and most preferably higher than 400°C, because it is possible to obtain a molded product with a further reduced amount of particle generation without damaging the TFE / PAVE copolymer, and is also excellent in productivity. The temperature T1 is preferably lower than the thermal decomposition temperature of the TFE / PAVE copolymer, more preferably lower than 430°C, because it is possible to obtain a molded product with a further reduced amount of particle generation without damaging the TFE / PAVE copolymer, and is also excellent in productivity. In the conventional molding material preparation process, since the advantage of molding the TFE / PAVE copolymer at a relatively high temperature was not known, the molding temperature was set to a low temperature in consideration of the effect on the TFE / PAVE copolymer, production costs, safety, and the like. However, the present inventors have found that the conventional method of setting the molding temperature as low as possible tends to be unable to sufficiently suppress the amount of particle generation.

[0019] The temperature T2 (°C) in the molding process is the molding temperature when the molding material is molded. In the molding process, the molding temperature may be set to be constant within a range that does not interfere with molding, or the molding temperature may be changed. When changing the molding temperature, the molding temperature can be changed so that the temperature T1 and the temperature T2 satisfy the relationship 20≦T1-T2≦80, with the temperature at any point in the molding process being T2. That is, the temperature T2 in the molding process may be the temperature at any point in the molding process, or may be the maximum temperature in the molding process. The temperature T2 is not the copolymer temperature, but the set temperature of the molding machine used for molding.

[0020] The temperature T2 is set to a temperature lower than the temperature T1 so as to satisfy the inequality: 20≦T1-T2≦80. That is, in the manufacturing method of the present disclosure, the temperature difference between the temperature T1 and the temperature T2 is controlled within the range of 20 to 80° C., so that the generation of particles from the finally obtained molded product can be suppressed to a level not seen before. On the other hand, when molding into the molded product, if a conventional method is adopted in which the molding temperature is set as high as possible in order to increase the extrusion speed with an emphasis on productivity, the amount of particle generation cannot be sufficiently suppressed. Since a molded product with a further reduced amount of particle generation can be obtained, the temperatures T1 and T2 preferably satisfy the inequality: 30≦T1-T2, more preferably satisfy the inequality: 40≦T1-T2, and more preferably satisfy the inequality: T1-T2≦70. In addition, the larger the molded product to be manufactured, the greater the temperature difference between T1 and T2 is preferably.

[0021] The reason why a molded product with reduced particle generation can be manufactured by strictly controlling the temperatures T1 and T2 is not clear, but is presumed to be as follows. FIG. 1 is a diagram for explaining the mechanism by which particles adhere to a tube in a conventional tube molding process. As shown in FIG. 1, a TFE / PAVE copolymer 101 molten in a cylinder 111 passes through an adapter 112 and is extruded from a die 113 to form a cone 102 of the molten TFE / PAVE copolymer extending to a sizing die 114, and then passes through the sizing die 114 to form a tube 103. The outer shape of the tube 103 is determined by the sizing die 114, and the wall thickness of the tube 103 is determined by the extrusion amount controlled by the rotation speed of a screw 115. Outside air 121 is blown into the inside of the cone 102 and the tube 103 from a hole 116 provided in the die 113, and the molten TFE / PAVE copolymer is cooled and solidified. The outside air 121 is usually passed through a filter to remove environmentally derived contaminant particles. When the TFE / PAVE copolymer 101 heated to the die temperature is extruded from the die 113, low molecular weight substances 131 volatilize from the surface of the molten TFE / PAVE copolymer, and as the TFE / PAVE copolymer cools, they adhere to the inner surface of the cone 102 and the tube 103. In the conventional tube molding process, such a phenomenon occurs, and it is presumed that the adhered low molecular weight substances are dissolved as particles in the chemical solution. The low molecular weight substances have a chemical structure similar to that of the TFE / PAVE copolymer, and adhere to the inner surface of the tube due to strong hydrophobic interactions in water or in the chemical solution, making it extremely difficult to wash them off with water.

[0022] On the other hand, in the manufacturing method of the present disclosure, it is presumed that by strictly controlling temperatures T1 and T2, even if the TFE / PAVE copolymer is melted in the molding process, low molecular weight substances are unlikely to be generated, and a molded product with reduced particle generation can be produced.

[0023] In the above preparation step, the molding method for preparing the molding material is not particularly limited, but a method capable of molding into a shape suitable for extrusion molding in the above molding step is preferred, and an extrusion molding method is more preferred. In the above preparation step, by preparing the molding material by extrusion molding, the molding material can be prepared with high productivity, and a molded product with further reduced particle generation can be obtained.

[0024] The shape of the TFE / PAVE copolymer used in the above preparation step is not particularly limited, but is preferably in the form of particles or powder, as this is easy to produce.

[0025] The shape of the molding material is not particularly limited, but is preferably a shape suitable for extrusion molding in the molding step. The molding material may be powder, pellets, crumbs, etc., but is preferably a pellet, since an extrusion molding method can be adopted as a molding method for preparing the molding material, the shape is suitable for extrusion molding in the molding step, the productivity is excellent, and a molded product with a further reduced amount of particle generation can be obtained.

[0026] The pellets are preferably approximately cylindrical pellets having a length of 1 to 3 mm and a diameter of 0.5 to 3 mm, because they are easy to produce and handle, and more preferably have a diameter of 1 to 2 mm.

[0027] In the above preparation step, it is particularly preferable to prepare pellets as the molding material by extrusion molding, since this allows the molding material to be prepared with high productivity and allows a molded product to be obtained with even reduced particle generation.

[0028] In the preparation step, when the molding material is prepared by extrusion molding, an extruder can be used. The extruder may be a single screw extruder or a twin screw extruder.

[0029] FIG. 2 is a diagram for explaining an example of the preparation process. In the preparation process shown in FIG. 2, an extruder 210 includes a cylinder 211, a screw 212 accommodated in the cylinder 211, a die 213 attached to the tip of the cylinder 211, a hopper 214 for supplying a raw material to the cylinder 211, and a drive unit 215 for rotating the cylinder 211. In this embodiment, first, a powder of a TFE / PAVE copolymer (not shown) as a raw material is supplied from the hopper 214 to the cylinder 211, and the TFE / PAVE copolymer is melted in the cylinder 211. Next, the melted TFE / PAVE copolymer 201 is extruded from the die 213 to form a strand 202. The strand 202 extruded from the die 213 travels a certain distance and is then introduced into a water tank 221 to be cooled. Finally, the cooled strand 202 is fed into a pelletizer 222, cut by a cutter (not shown) provided in the pelletizer 222, and discharged as pellets 231. At this time, it is presumed that low molecular weight substances are volatilized from the high-temperature strand 202 extruded from the die 213.

[0030] A vent hole (not shown) may be provided in the cylinder 211 of the extruder 210, and a vacuum pump (not shown) may be connected to the vent hole. By providing the vent hole, low molecular weight substances volatilized from the molten TFE / PAVE copolymer 201 can be discharged to the outside of the cylinder 211.

[0031] For example, when pellets are prepared by a hot cutting method in which a strand immediately after being extruded from a die is cut before being cooled, or an underwater cutting method in which a strand immediately after being extruded from a die is put into water and cut underwater, rather than a method in which a cooled strand is cut to prepare pellets as in the preparation process shown in Figure 2, it is preferable to provide a vent hole in the cylinder, since there is a possibility that low molecular weight components may not be sufficiently volatilized from the TFE / PAVE copolymer.

[0032] Since the low molecular weight material can be sufficiently volatilized to obtain a molded product with further reduced particle generation, when the cylinder of the extruder does not have a vent hole, it is usually easiest for the low molecular weight material to volatilize from the strand extruded from the die, so it is convenient to set the die temperature as temperature T1 so as to satisfy the relationship between temperatures T1 and T2 described above. When the cylinder of the extruder has a vent hole, it is preferable to set the temperature of the cylinder where the vent hole is located as temperature T1, since it is easiest for the low molecular weight material to volatilize from the vent hole. When a vacuum pump is connected to the vent hole, it is expected that the volatilization of the low molecular weight material will proceed smoothly, so the temperature T1 may be lowered than when the vacuum pump is not connected. From the above, in the above preparation process, it is preferable to provide a low molecular weight material volatilization region (a region where the low molecular weight material is easily volatilized) and control the temperature of the TFE / PAVE copolymer in the low molecular weight material volatilization region as temperature T1. In the preparation step, it is more preferable to use an extruder equipped with a die set at a temperature T1, or an extruder equipped with a cylinder set at a temperature T1 and a vent hole provided in the cylinder.

[0033] The extruder may be provided with a breaker plate for stabilizing extrusion of the strands. The number of strands extruded from the die is not particularly limited, but may be 5 to 350. The rotation speed of the screw provided in the extruder is not particularly limited, and is set in consideration of the extrusion amount and extrusion stability, and is, for example, in the range of 5 to 40 rpm.

[0034] From the viewpoint of producing a molded product with further reduced particle generation, it is preferable that the diameter of the strand extruded from the die is small, but if the strand is too thin, problems such as the strand being broken during the preparation process may occur. Therefore, the diameter of the strand is preferably 0.5 to 3 mm, more preferably 1 to 2 mm.

[0035] The molding material obtained in the preparation step may be molded again at a temperature T1 (° C.) to prepare a molding material. By repeating the preparation step, a molded product with even lower particle generation can be produced.

[0036] In the molding step, the molding material obtained in the preparation step is extrusion molded at a temperature T2 (°C) to obtain a molded product. The shape of the molded product is not particularly limited as long as it is a shape that can be molded by extrusion molding, and examples of the molded product include pellets, films, sheets, plates, rods, blocks, cylinders, containers, electric wires, tubes, bottles, and the like. The molded product is preferably a tube, a film, or a bottle, and more preferably a tube. As described above, according to the conventional molding method, low molecular weight substances are likely to adhere to the inner surface of the tube, which is presumed to be a source of particle generation, but according to the manufacturing method of the present disclosure, even when a tube is manufactured, a tube with reduced particle generation can be obtained.

[0037] An extruder can be used for the extrusion molding in the molding step. The extruder may be a single-screw extruder or a twin-screw extruder. The extruder is usually equipped with a cylinder, a screw housed in the cylinder, a die attached to the tip of the cylinder, an adapter for connecting the die to the cylinder, a hopper for supplying raw materials to the cylinder, and a drive device for rotating the cylinder. As described above, pellets are preferable as the molding material prepared in the preparation step because they are easy to charge from the hopper. The molding material charged into the cylinder is melted in the cylinder and extruded from the die to be molded into a tube. The temperatures of the cylinder, adapter, die, etc. can be set according to the size and shape of the molded product, and are preferably set so that the die temperature is the highest. As described above, in the tube molding step, it is presumed that low molecular weight substances volatilize from the molten TFE / PAVE copolymer extruded from the die and tend to adhere to the inner surface of the tube, so it is preferable to control the die temperature to a temperature T2.

[0038] A particularly preferred embodiment of the manufacturing method of the present disclosure includes a preparation step of extruding a TFE / PAVE copolymer to prepare pellets using an extruder equipped with a die set to temperature T1, or an extruder equipped with a cylinder set to temperature T1 and a vent hole provided in the cylinder, and a molding step of extruding the pellets to obtain a tube using an extruder equipped with a die set to temperature T2 (°C), wherein temperatures T1 and T2 satisfy the above-mentioned relationship.

[0039] Next, the tetrafluoroethylene / perfluoro(alkyl vinyl ether) copolymer used in the above preparation step will be described.

[0040] The TFE / PAVE copolymer is preferably a melt-processable fluororesin. In the present disclosure, melt-processable means that the polymer can be melted and processed using conventional processing equipment such as an extruder and an injection molding machine. Therefore, the melt-processable fluororesin usually has a melt flow rate of 0.01 to 500 g / 10 min, as measured by the measurement method described below.

[0041] The content of the PAVE-based monomer units in the TFE / PAVE copolymer is preferably 1.0 to 10% by mass, more preferably 2.0% by mass or more, even more preferably 3.5% by mass or more, particularly preferably 4.0% by mass or more, most preferably 5.0% by mass or more, more preferably 8.0% by mass or less, even more preferably 7.0% by mass or less, particularly preferably 6.5% by mass or less, and most preferably 6.0% by mass or less, based on the total amount of the PAVE-based monomer units. 19 Measured by F-NMR.

[0042] The PAVE constituting the above PAVE unit is represented by the general formula (1): CF2=CFO(CF2CFY 1 O) p -(CF2CF2CF2O)q -R f (1) (In the formula, Y 1 represents F or CF3, and R f represents a perfluoroalkyl group having 1 to 5 carbon atoms, p represents an integer of 0 to 5, and q represents an integer of 0 to 5.) and a monomer represented by general formula (2): CFX=CXOCF2OR 1 (2) (wherein X is the same or different and represents H, F or CF3; R 1 represents a linear or branched fluoroalkyl group having 1 to 6 carbon atoms which may contain 1 to 2 atoms of at least one type selected from the group consisting of H, Cl, Br and I, or a cyclic fluoroalkyl group having 5 or 6 carbon atoms which may contain 1 to 2 atoms of at least one type selected from the group consisting of H, Cl, Br and I.

[0043] Among them, the above-mentioned PAVE is preferably a monomer represented by general formula (1), more preferably at least one selected from the group consisting of perfluoro(methyl vinyl ether), perfluoro(ethyl vinyl ether) and perfluoro(propyl vinyl ether) (PPVE), and even more preferably PPVE.

[0044] The TFE / PAVE copolymer is not particularly limited, but is preferably a copolymer having a molar ratio of TFE units to PAVE units (TFE units / PAVE units) of 70 / 30 or more and less than 99 / 1. A more preferred molar ratio is 70 / 30 or more and 98.9 / 1.1 or less, and an even more preferred molar ratio is 80 / 20 or more and 98.9 / 1.1 or less. If the TFE units are too few, the mechanical properties tend to decrease, and if the TFE units are too many, the melting point tends to become too high and the moldability tends to decrease.

[0045] The above TFE / PAVE copolymer is also preferably a copolymer containing 0.1 to 10 mol % of monomer units derived from monomers copolymerizable with TFE and PAVE, and containing 90 to 99.9 mol % of TFE units and PAVE units in total.

[0046] Monomers that can be copolymerized with TFE and PAVE include HFP, CZ 3 Z 4 =CZ 5 (CF2) n Z 6 (In the formula, Z 3 , Z 4 and Z 5 are the same or different and represent H or F; Z 6 represents H, F or Cl, and n represents an integer of 2 to 10. 7 (In the formula, Rf 7 represents a perfluoroalkyl group having 1 to 5 carbon atoms.) Among these, HFP is preferred.

[0047] The above-mentioned TFE / PAVE copolymer is preferably at least one selected from the group consisting of copolymers consisting only of TFE units and PAVE units, and the above-mentioned TFE / HFP / PAVE copolymers, and more preferably a copolymer consisting only of TFE units and PAVE units.

[0048] The melting point of the TFE / PAVE copolymer is preferably 280 to 322°C, more preferably 290°C or higher, even more preferably 295°C or higher, particularly preferably 300°C or higher, and more preferably 315°C or lower. In order to mold a copolymer with a high melting point, it is necessary to heat the copolymer to a high temperature and mold it, so that low molecular weight substances are particularly likely to adhere to the surface of the molded product, and particles are likely to be generated. This is considered to be because the higher the molding temperature, the more easily low molecular weight substances are volatilized from the copolymer during molding. According to the manufacturing method of the present disclosure, even when a TFE / PAVE copolymer with a high melting point is used, a molded product with reduced particle generation can be manufactured. The melting point can be measured using a differential scanning calorimeter [DSC].

[0049] The glass transition temperature (Tg) of the TFE / PAVE copolymer is preferably 70 to 110° C., more preferably 80° C. or higher, and more preferably 100° C. or lower. The glass transition temperature can be measured by dynamic viscoelasticity measurement.

[0050] The melt flow rate (MFR) of the TFE / PAVE copolymer at 372° C. is preferably 0.1 to 100 g / 10 min, more preferably 0.5 g / 10 min or more, even more preferably 1 g / 10 min or more, more preferably 80 g / 10 min or less, even more preferably 40 g / 10 min or less, and particularly preferably 30 g / 10 min or less. The MFR is a value obtained according to ASTM D1238 as the mass (g / 10 min) of polymer flowing out of a nozzle with an inner diameter of 2 mm and a length of 8 mm under a load of 5 kg at 372° C. from a melt indexer (manufactured by Yasuda Seiki Seisakusho Co., Ltd.) per 10 minutes.

[0051] As the TFE / PAVE copolymer, a copolymer having a small number of functional groups is preferred because it allows the production of molded products with even lower particle generation. 6 It is preferable that each of the 10 carbon atoms has 0 to 50 carbon atoms. 6The number of functional groups per unit is more preferably 0 to 30, and further preferably 0 to 15.

[0052] The functional group is a functional group present at the end of the main chain or the end of the side chain of the TFE / PAVE copolymer, or a functional group present in the main chain or the side chain. The functional group is preferably at least one selected from the group consisting of -CF=CF2, -CF2H, -COF, -COOH, -COOCH3, -CONH2 and -CH2OH.

[0053] The type of functional group and the number of functional groups can be identified by infrared spectroscopy.

[0054] Specifically, the number of functional groups is measured by the following method. First, the TFE / PAVE copolymer is melted at 330 to 340°C for 30 minutes and compression molded to prepare a film having a thickness of 0.25 to 0.3 mm. This film is analyzed by Fourier transform infrared spectroscopy to obtain an infrared absorption spectrum of the TFE / PAVE copolymer, and a difference spectrum with a base spectrum that is completely fluorinated and has no functional groups is obtained. From the absorption peaks of specific functional groups that appear in this difference spectrum, the number of carbon atoms in the TFE / PAVE copolymer is calculated according to the following formula (A): 6 Calculate the number of functional groups per unit, N. N=I×K / t (A) I: Absorbance K: Correction coefficient t: film thickness (mm)

[0055] For reference, the absorption frequencies, molar absorption coefficients, and correction coefficients for the functional groups in this disclosure are shown in Table 1. The molar absorption coefficients were determined from FT-IR measurement data of low molecular weight model compounds.

[0056] [Table 1]

[0057] The absorption frequencies of -CH2CF2H, -CH2COF, -CH2COOH, -CH2COOCH3, and -CH2CONH2 are shown in the table, and are several tens of Kaiser (cm) from the absorption frequencies of -CF2H, -COF, -COOH free, -COOH bonded, -COOCH3, and -CONH2. -1 ) lower. Therefore, for example, the functional group number of -COF is the absorption frequency of 1883 cm due to -CF2COF. -1 The number of functional groups determined from the absorption peak of -CH2COF and the absorption frequency of 1840 cm -1 The number of functional groups is the sum of the number of functional groups determined from the absorption peaks of

[0058] The number of functional groups may be the total number of -CF=CF2, -CF2H, -COF, -COOH, -COOCH3, -CONH2 and -CH2OH.

[0059] The functional group is introduced into the TFE / PAVE copolymer by, for example, a chain transfer agent or a polymerization initiator used in producing the TFE / PAVE copolymer. For example, when an alcohol is used as a chain transfer agent or a peroxide having a -CH2OH structure is used as a polymerization initiator, -CH2OH is introduced into the main chain end of the TFE / PAVE copolymer. In addition, the functional group is introduced into the side chain end of the TFE / PAVE copolymer by polymerizing a monomer having a functional group.

[0060] The TFE / PAVE copolymer having such functional groups can be fluorinated to obtain the TFE / PAVE copolymer having the number of functional groups within the above range. That is, the TFE / PAVE copolymer used in the manufacturing method of the present disclosure is preferably fluorinated. In addition, the TFE / PAVE copolymer used in the manufacturing method of the present disclosure also preferably has a -CF3 end group.

[0061] The above fluorination treatment can be carried out by contacting a non-fluorination-treated TFE / PAVE copolymer with a fluorine-containing compound.

[0062] The fluorine-containing compound is not particularly limited, but may be a fluorine radical source that generates fluorine radicals under fluorination treatment conditions, such as F2 gas, CoF3, AgF2, UF6, OF2, N2F2, CF3OF, halogen fluorides (e.g., IF5, ClF3), etc.

[0063] The fluorine radical source such as F2 gas may be of 100% concentration, but from the viewpoint of safety, it is preferable to mix it with an inert gas and dilute it to 5 to 50% by mass, more preferably to dilute it to 15 to 30% by mass. Examples of the inert gas include nitrogen gas, helium gas, argon gas, etc., and nitrogen gas is preferable from the viewpoint of economy.

[0064] The conditions for the fluorination treatment are not particularly limited, and the molten TFE / PAVE copolymer may be contacted with a fluorine-containing compound, but the treatment is usually carried out at a temperature below the melting point of the TFE / PAVE copolymer, preferably 20 to 220°C, more preferably 100 to 200°C. The fluorination treatment is generally carried out for 1 to 30 hours, preferably 5 to 25 hours. The fluorination treatment is preferably carried out by contacting a non-fluorinated TFE / PAVE copolymer with fluorine gas (F2 gas).

[0065] The TFE / PAVE copolymer can be produced by a conventional method such as emulsion polymerization or suspension polymerization by appropriately mixing monomers that form the constituent units thereof and additives such as a polymerization initiator.

[0066] Next, the molded article of the present disclosure will be described. The molded article of the present disclosure contains a TFE / PAVE copolymer having a melting point of 295° C. or higher, and when it comes into contact with isopropyl alcohol, the number of particles having a size of 30 nm or more dispersed in isopropyl alcohol is 700 pieces / ml or less.

[0067] The TFE / PAVE copolymer contained in the molded article of the present disclosure may be the same as the TFE / PAVE copolymer used in the manufacturing method of the present disclosure, and is preferably the same as the TFE / PAVE copolymer used in the manufacturing method of the present disclosure.

[0068] The melting point of the TFE / PAVE copolymer contained in the molded article of the present disclosure is 295°C or higher. In order to mold a copolymer with a high melting point, it is necessary to heat the copolymer to a high temperature and mold it, so that low molecular weight substances in particular tend to adhere to the surface of the molded article, and particles are easily generated. Although the molded article of the present disclosure contains a TFE / PAVE copolymer with a melting point of 295°C or higher, the amount of particles generated is small. The melting point of the TFE / PAVE copolymer is more preferably 300°C or higher, preferably 322°C or lower, and more preferably 315°C or lower.

[0069] When the molded article of the present disclosure comes into contact with isopropyl alcohol (the number of particles having a size of 30 nm or more is 30 / ml or less), the number of particles dispersed in the isopropyl alcohol is 700 / ml or less, preferably 600 / ml or less, more preferably 500 / ml or less, and although there is no particular lower limit, it is preferably 50 / ml or more. A method for measuring the number of particles dispersed in isopropyl alcohol will be described later.

[0070] The shape of the molded article of the present disclosure is not particularly limited, and examples thereof include pellets, films, sheets, plates, rods, blocks, cylinders, containers, electric wires, tubes, bottles, etc. The molded article of the present disclosure is preferably a tube, a film, or a bottle, and more preferably a tube. As described above, according to the conventional molding method, low molecular weight substances tend to adhere to the inner surface of the tube, which is presumed to be a source of particle generation, but the molded article of the present disclosure generates a small amount of particles even when it is a tube.

[0071] The above tube is filled with isopropyl alcohol (the number of particles of 30 nmφ or more is 30 / ml or less) in an amount equivalent to the content of the tube, left at room temperature for one day, and then the isopropyl alcohol is collected. The number of particles of 30 nmφ or more dispersed in the collected isopropyl alcohol is preferably 700 / ml or less, more preferably 600 / ml or less, and even more preferably 500 / ml or less, and although there is no particular lower limit, is preferably 50 / ml or more. A method for measuring the number of particles dispersed in isopropyl alcohol will be described later.

[0072] The outer diameter of the tube is not particularly limited, but may be 2 to 100 mm, or 5 to 50 mm. The thickness of the tube may be 0.1 to 10 mm, or 0.3 to 5 mm. According to the manufacturing method of the present disclosure, even if a relatively large tube having an outer diameter of 20 mm or more and a thickness of 1 mm or more is manufactured, the number of particles dispersed in isopropyl alcohol can be within the above range. Therefore, the tube of the present disclosure may be a tube having an outer diameter of 20 mm or more and a thickness of 1 mm or more.

[0073] The molded article of the present disclosure and the molded article obtained by the manufacturing method of the present disclosure can be used for, but is not limited to, the following applications: Diaphragm parts of diaphragm pumps, bellows molded products, wire coating products, semiconductor parts, packing and seals, thin-walled tubes for copy rolls, monofilaments, belts, gaskets, optical lens parts, tubes for oil drilling, tubes for geothermal power generation, electric wires for oil drilling, electric wires for satellites, electric wires for nuclear power generation, electric wires for aircraft, solar panel film, gaskets for secondary batteries and electric double-layer capacitors, OA rolls, etc.

[0074] The above molded articles can also be suitably used as tubes for passing gases or liquid medicines, bottles for storing medicines, gas bags, liquid medicine bags, liquid medicine containers, bags for freezing and storing medicines, and the like.

[0075] The above-mentioned molded products can also be suitably used for bodies and parts of on-off valves, sleeves used when connecting fittings and tubes, screw caps for chemical bottles and containers, gears, screws, frying pans, pots, rice cookers, products with a fluororesin coating on a metal base or the like, release films, etc.

[0076] Particularly suitable applications of the above molded articles include perfluoro-based fluororesin components such as piping for chemical supply facilities in semiconductor manufacturing, tubes for semiconductor manufacturing equipment, joints, valves, tanks, containers, chemical bags, and wafer carriers.

[0077] In one preferred embodiment, the molded article of the present disclosure and the molded article obtained by the manufacturing method of the present disclosure are tubes.

[0078] In semiconductor factories, tubes are widely used to distribute ultrapure water and high-purity chemicals used in semiconductor manufacturing. Fine particles generated from molded products containing TFE / PAVE copolymers are hydrophobic. Therefore, particularly when aqueous chemicals are distributed inside the tubes, the fine particles tend to adhere to the inner surface of the tubes due to the interaction between the fine particles and the tubes, and the adhered fine particles are difficult to remove with cleaning water such as pure water. Therefore, when new tubes are used in semiconductor factories, problems arise such as the need for a large amount of ultrapure water or chemicals to flush the inside of the tubes, and the need for long cleaning times.

[0079] Since the tube has the above-mentioned configuration, almost no particles adhere to the inner surface, and particles are unlikely to be generated. Since the tube has such an effect, it is preferable that the tube is a tube for piping a chemical liquid for circulating the chemical liquid. The chemical liquid may be a chemical liquid used in semiconductor manufacturing, such as ammonia water, ozone water, hydrogen peroxide water, hydrochloric acid, sulfuric acid, resist liquid, thinner liquid, developer, etc.

[0080] Although the embodiments have been described above, it will be understood that various changes in form and details are possible without departing from the spirit and scope of the claims. EXAMPLES

[0081] Next, embodiments of the present disclosure will be described with reference to examples, but the present disclosure is not limited to these examples.

[0082] The values ​​in the examples were measured by the following methods.

[0083] (Melting Point) It was determined as the temperature corresponding to the maximum value on the heat of fusion curve when the temperature was raised at a rate of 10°C / min using a differential scanning calorimeter (DSC).

[0084] (MFR) For the copolymer powders and pellets used in the examples and comparative examples, the mass of polymer flowing out per 10 minutes (g / 10 minutes) from a nozzle with an inner diameter of 2 mm and a length of 8 mm under a load of 5 kg at 372°C was determined using a melt indexer (manufactured by Yasuda Seiki Seisakusho) in accordance with ASTM D1238.

[0085] (Monomer unit content) The content of each monomer unit is: 19 Measurement was performed by F-NMR.

[0086] (Number of functional groups) The sample is melted at 330-340°C for 30 minutes and compression molded to produce a film with a thickness of 0.25-0.3 mm. This film is scanned 40 times using a Fourier transform infrared spectrometer [FT-IR (trade name: Model 1760X, manufactured by PerkinElmer) to analyze it and obtain an infrared absorption spectrum, and a difference spectrum with a base spectrum where the sample is completely fluorinated and has no functional groups is obtained. From the absorption peaks of specific functional groups that appear in this difference spectrum, the ratio of carbon atoms in the sample to carbon atoms in the range of 1×10 is calculated according to the following formula (A). 6 Calculate the number of functional groups per unit, N.

[0087] N=I×K / t (A) I: Absorbance K: Correction coefficient t: film thickness (mm)

[0088] For reference, the absorption frequencies, molar absorption coefficients, and correction coefficients for the functional groups in this disclosure are shown in Table 2. The molar absorption coefficients were determined from FT-IR measurement data of low molecular weight model compounds.

[0089] [Table 2]

[0090] (Number of particles) (1) Preparation of isopropyl alcohol Commercially available high-purity isopropyl alcohol (IPA) was filtered using a 5 nmφ filter. The filtered IPA was left for one day, and it was confirmed that the number of particles with a size of 30 nmφ or more was 30 pieces / ml or less. The filtered IPA was used to wash the tube and measure the number of particles.

[0091] (2) Preparation of sample tubes In a clean bench in a clean room, the tubes prepared in the examples and comparative examples were cut to a length of 3 m. The inner surface of the obtained sample tube was washed with ultrapure water in an amount five times the content volume of the sample tube to remove environmentally derived contaminant particles. Next, filtered IPA was supplied into the sample tube, and the same amount of high-purity IPA as the content volume of the tube was sealed, and then the liquid was immediately drained and the ultrapure water was replaced with IPA.

[0092] (3) Measuring the number of particles The sample tube obtained in (2) above was filled with high-purity IPA in an amount equal to the content of the tube, and left at room temperature for one day. In the case of a sample tube with an outer diameter of 10 mm, an inner diameter of 8 mm, and a length of 3 m, 150 mL of IPA was sealed inside. In the case of a sample with an outer diameter of 25.4 mm, an inner diameter of 22.2 mm, and a length of 3 m, 1160 mL of IPA was sealed inside. In addition, in the case of a sample with an outer diameter of 6.0 mm, an inner diameter of 4.0 mm, and a length of 3 m, 37 mL of IPA was sealed inside.

[0093] Next, the IPA sealed in the sample tube was introduced into a particle counter (KS-19F, light scattering type liquid-borne particle detector, manufactured by Rion Co., Ltd.) using a syringe pump to measure the number of particles.

[0094] The maximum number of particles was measured immediately after introducing IPA into the particle counter, and the number of particles measured then showed a gradual decrease. The maximum value of the total number of particles with a size of 30 nm or more after the start of measurement was compared as the number of particles eluted from the sample tube.

[0095] FIG. 3 is a diagram for explaining a method for measuring the number of particles.

[0096] First, nitrogen gas 331 is supplied into first chemical liquid container 321 to pressurize isopropyl alcohol (IPA) 311 stored in chemical liquid container 321. Pressurized IPA 311 passes through filter 322 and is stored in second chemical liquid container 323. IPA 312 in second chemical liquid container 323 is left for one day and then used for measurement.

[0097] A valve 324 is connected to the lower part of second chemical liquid container 323, and sample tube 301 is connected to second chemical liquid container 323 via valve 324. The other end of sample tube 301 is connected to particle counter 341 via valve 326. Furthermore, a syringe pump 342 is provided downstream of particle counter 341 so that IPA in sample tube 301 can be introduced into particle counter 341.

[0098] In addition, another line is provided for supplying ultrapure water 332 to the sample tube 301 , and the sample tube 301 is also connected to this line via a filter 328 and a valve 325 .

[0099] In order to prevent particles from being mixed into the IPA 312 and the ultrapure water 332 by opening and closing the valves 324 to 326 connected to the sample tube 301, it is necessary to use diaphragm valves as the valves 324 to 326.

[0100] Once a system for measuring the number of particles has been configured in this manner, ultrapure water 332 that has passed through filter 328 is supplied to sample tube 301 to clean the inside of sample tube 301 and discharged as waste liquid 333. Next, IPA 312 is supplied from second chemical liquid container 323 to sample tube 301 to replace the ultrapure water with IPA, and then a predetermined amount of IPA is sealed in sample tube 301.

[0101] After a predetermined time has elapsed since the IPA was sealed, the syringe pump 342 is operated to introduce the IPA in the sample tube 301 into the particle counter 341. In this disclosure, the number of particles is measured in this manner.

[0102] In the above-described measurement method, the IPA sealed in the sample tube was directly introduced into the particle counter using a syringe pump, but it is also possible to recover the IPA sealed in the sample tube in a container that has been thoroughly washed with IPA, and then introduce the recovered IPA into the particle counter.

[0103] The above-mentioned measurement method is a method for measuring the number of particles generated from the inner surface of a tube, but the number of particles generated from the surface of a molded product other than a tube can also be measured by the same method. That is, after thoroughly washing the surface of the molded product with ultrapure water, the ultrapure water attached to the surface is replaced with IPA. The obtained molded product is placed in high-purity IPA and left at room temperature for one day. The IPA after the molded product is immersed is introduced into a particle counter and the number of particles is measured. If the molded product is too large to be immersed in IPA, a measurement sample prepared by cutting it to an appropriate size may be used, but in order to accurately measure the number of particles generated from the molded product surface, it is preferable that the cut surface is as small as possible.

[0104] The contact area between the surface of the molded article and IPA measured in this way is different from the contact area between the inner surface of the tube and IPA measured using the tube measurement method described above. However, the particle count measured above can be converted to the particle count measured over the same contact area as the tube (outer diameter 25.4 mm × inner diameter 22.2 mm × length 3 m) using the following formula (referred to as the "converted value of the particle count of the molded article" in the following formula). Conversion value of number of particles in molded product (pieces / ml) = C x A / B x 0.56 A: Surface area of ​​molded product immersed in IPA (cm 2 ) B: Amount of IPA in which the molded product was immersed (ml) C: Particle count measurements (particles / ml)

[0105] In the present disclosure, the number of particles dispersed in isopropyl alcohol when a molded product other than a tube comes into contact with isopropyl alcohol is determined by such measurement and conversion methods.

[0106] Comparative Example 1 (1) Preparation process TFE / PPVE copolymer 1 (composition ratio of TFE and PPVE (mass%): TFE / PPVE = 94.5 / 5.5, melting point: 304°C, MFR: 2.1g / 10min, number of functional groups: 6 / C10 6 The powder (100g) was charged into a screw extruder (shaft diameter 32 mm, L / D=52.5), melted in the cylinder, and then extruded from the die. At this time, the cylinder temperature of the screw extruder was set to 320-350°C, the adapter temperature to 340-350°C, and the die temperature to 350°C. The cylinder of the screw extruder did not have a vent hole. Therefore, in the preparation process of Comparative Example 1, it was assumed that low molecular weight substances would volatilize most easily from the strand extruded from the die, so the die temperature was controlled to a temperature T1. In fact, it was possible to visually observe the state in which volatile matter (polymer fumes) volatilized from the strand extruded from the die. The strand extruded from the die was then cooled in a water tank placed at a certain distance from the die, and then fed to a pelletizer where it was cut into pellets by a cutter. The pellets obtained were cylindrical with a length of 3.0 mm and a diameter of 2.0 mm, and had an MFR of 2.0 g / 10 mm.

[0107] (2) Molding process The pellets obtained above were extruded at a take-up speed of 85 cm / min using a tube extrusion molding machine (cylinder shaft diameter 50 mm, L / D=22) to obtain a tube with an outer diameter of 10.0 mm and an inner diameter of 8.0 mm. At this time, the cylinder temperature of the tube extrusion molding machine was set to 330 to 360 ° C., the adapter temperature was set to 370 ° C., and the die temperature was set to 370 ° C. In the molding process of Comparative Example 1, it is considered that low molecular weight substances volatilized from the copolymer 1 in a molten state extruded from the die tend to adhere to the inner surface of the obtained tube, and since 370 ° C. is the maximum temperature, the die temperature was controlled at temperature T2. The obtained tube had an outer diameter of 10.0 mm and an inner diameter of 8.0 mm. The number of particles generated from the obtained tube was determined by the above-mentioned method. The results are shown in Table 3.

[0108] Examples 1 to 3 Pellets were prepared in the same manner as in Comparative Example 1, except that the temperature T1 was changed to the temperature shown in Table 3 by changing the cylinder temperature, adapter temperature, and die temperature. Using each of the obtained pellets, tubes were obtained in the same manner as in Comparative Example 1, except that the temperature T2 was changed to the temperature shown in Table 3 by changing the cylinder temperature, adapter temperature, and die temperature, and the tube size was changed to the size shown in Table 3. The results are shown in Table 3.

[0109] Comparative Examples 2-3, Examples 4-5 TFE / PPVE copolymer 2 (composition ratio of TFE and PPVE (mass%): TFE / PPVE = 94.3 / 5.7, melting point: 303°C, MFR: 14.0g / 10min, number of functional groups: 4 / C10 6 Pellets were prepared in the same manner as in Comparative Example 1, except that a temperature T1 was changed to the temperatures shown in Table 3 by changing the cylinder temperature, adapter temperature, and die temperature. Using each of the obtained pellets, tubes were obtained in the same manner as in Comparative Example 1, except that the temperature T2 was changed to the temperature shown in Table 3 by changing the cylinder temperature, adapter temperature, and die temperature, and the tube size was changed to the size shown in Table 3. The results are shown in Table 3.

[0110] Comparative Example 4, Example 6 TFE / PPVE copolymer 3 (composition ratio of TFE and PPVE (mass%): TFE / PPVE = 96.7 / 3.3, melting point: 307°C, MFR: 10.4g / 10min, functional group number: 10 / C10 6 Pellets were prepared in the same manner as in Comparative Example 1, except that a temperature T1 was changed to the temperatures shown in Table 3 by changing the cylinder temperature, adapter temperature, and die temperature. Using each of the obtained pellets, tubes were obtained in the same manner as in Comparative Example 1, except that the temperature T2 was changed to the temperature shown in Table 3 by changing the cylinder temperature, adapter temperature, and die temperature, and the tube size was changed to the size shown in Table 3. The results are shown in Table 3.

[0111] [Table 3] [Explanation of symbols]

[0112] 101,201 TFE / PAVE copolymer 102 Corn 103 Tube 111,211 cylinders 112 Adapter 113,213 Die 114 Sizing Die 115,212 Screw 116 holes 121 Outside Air 131 Low molecular weight substance 202 Strand 210 Extruder 214 Hopper 215 Drive unit 221 Aquarium 222 Pelletizer 231 Pellets 301 Sample tube 311,312 Isopropyl alcohol (IPA) 313,333 Drainage 321,323 Liquid medicine container 322,328 Filters 324,325,326,327 Valve 331 Nitrogen Gas 332 Ultrapure water 341 Particle Counter 342 Syringe Pump

Claims

[Claim 1] A tube containing a tetrafluoroethylene / perfluoro(alkyl vinyl ether) copolymer having a melting point of 295°C or higher, wherein when the tube is filled with an amount of isopropyl alcohol equivalent to the tube's content and left at room temperature for one day, the number of particles having a diameter of 30 nm or more dispersed in the isopropyl alcohol is 700 particles / ml or less.

Citation Information

Patent Citations

  • Fluorocopolymer and its production

    JP1994080733A

  • Fine powder of meltable high-molecular-weight fluororesin, molded product and production thereof

    JP1996034820A

  • Manufacture of fluororesin tube with reduced particle

    JP2000233435A

  • Tetrafluoroethylene copolymer and method for production thereof

    JP2005320497A

  • Office automation equipment material and image fixing member therefor

    JP2009042478A