Resin composition, method for producing said resin composition, and molded article using said resin composition
The resin composition with a dispersed water-soluble polymer addresses the challenge of achieving lightweight and strong resin moldings by using a thermoplastic resin and polyvinyl alcohol fibers, resulting in improved mechanical strength and reduced weight.
Patent Information
- Application Number
- JP2020094374
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-06-04
- Filing Date
- 2020-05-29
- Publication Date
- 2024-09-27
- Estimated Expiration
- 2040-05-29
AI Technical Summary
Conventional resin compositions containing fillers like glass fiber and talc result in high specific gravity and poor mechanical strength, making it difficult to achieve lightweight and strong resin moldings.
A resin composition comprising a thermoplastic resin and a water-soluble polymer, such as polyvinyl alcohol resin, dispersed in the form of fibers, is produced by dissolving the polymer in a solvent, melt-kneading with the resin, and removing the solvent, using a continuous melt-kneader to achieve a lightweight molded article with enhanced mechanical strength.
The composition achieves a lightweight molded article with mechanical strength comparable to or exceeding that of conventional fillers, while maintaining excellent mechanical properties.
Smart Images

Figure 0007557284000006 
Figure 0007557284000003 
Figure 0007557284000004
Abstract
Description
[Technical field]
[0001] The present invention relates to a resin composition, a method for producing the resin composition, and a molded article using the resin composition. [Background technology]
[0002] Conventionally, resin compositions containing fillers such as glass fiber and talc have been used to obtain resin molded articles having excellent mechanical strength. However, as there is an increasing demand for lighter resin molded articles used in various applications, the addition of glass fiber, talc, etc. causes the resin molded article to have a high specific gravity, and there is a demand for resin compositions capable of forming resin molded articles having both high mechanical strength and light weight. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2012-251036 A Summary of the Invention [Problem to be solved by the invention]
[0004] The present invention has been made to solve the above problems, and an object of the present invention is to provide a resin composition which has excellent mechanical strength and can form a lightweight molded article. [Means for solving the problem]
[0005] The resin composition of the present invention contains a thermoplastic resin and a water-soluble polymer, and the water-soluble polymer is dispersed in the form of fibers in the thermoplastic resin. In one embodiment, the water-soluble polymer is a polyvinyl alcohol resin. In one embodiment, the polyvinyl alcohol resin has a degree of polymerization of 200-2,500. In one embodiment, the polyvinyl alcohol resin has a degree of saponification of 90 mol % or more. In one embodiment, the thermoplastic resin is a polyolefin resin. In one embodiment, the thermoplastic resin is a polypropylene-based resin. According to another aspect of the present invention, there is provided a method for producing the resin composition, comprising: dissolving a water-soluble polymer in a solvent to prepare a solution; melt-kneading the solution with a thermoplastic resin; and removing the solvent after the melt-kneading. In one embodiment, the solvent is water. In one embodiment, the water-soluble polymer concentration in the solution is 5% by weight to 50% by weight. In one embodiment, the solution and the thermoplastic resin are melt-kneaded using a continuous melt-kneading device. According to yet another aspect of the present invention, there is provided a method for producing the above-mentioned resin composition. This method includes melt-kneading a water-soluble polymer and a thermoplastic resin, and subjecting the mixture obtained by the melt-kneading to a shear rate of 100 sec -1 and extruding the material in such a manner that the material is extruded in a desired shape. According to yet another aspect of the present invention, there is provided a molded article. The molded article is formed from the above-mentioned resin composition. Effect of the Invention
[0006] According to the present invention, it is possible to provide a resin composition which is excellent in mechanical strength and capable of forming a lightweight molded article. [Brief description of the drawings]
[0007] [Figure 1] 3A to 3C are optical microscope photographs of molded bodies obtained in Examples and Comparative Examples. [Diagram 2] FIG. 2 is a SEM photograph of a molded body obtained in an example. [Diagram 3] FIG. 2 is a SEM photograph of a molded body obtained in an example. [Figure 4]FIG. 2 is a micrograph showing the dispersion state of a water-soluble polymer in a resin composition obtained in an example. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0008] A. Resin Composition The resin composition of the present invention contains a thermoplastic resin and a water-soluble polymer. The water-soluble polymer is dispersed in the thermoplastic resin in the form of fibers.
[0009] Typically, the resin composition is solid, and in one embodiment, it is provided as pellets. The resin composition of the present invention can form a molded body having excellent mechanical strength by containing a water-soluble polymer dispersed in a fibrous form. In addition, since the mechanical strength can be improved by the water-soluble polymer, the resin composition of the present invention can be used to form a molded body that is lighter than a resin composition having high strength achieved by using a conventional filler (e.g., glass fiber, talc, etc.). That is, the resin composition of the present invention can form a molded body that is equivalent to or more excellent in mechanical strength than a molded body obtained from a resin composition containing a conventional filler (e.g., glass fiber, talc, etc.) and is lighter in weight.
[0010] A-1. Thermoplastic resin The thermoplastic resin may be any suitable thermoplastic resin as long as the effect of the present invention can be obtained. Examples of the thermoplastic resin include polyolefin resin, acrylic resin, polyester resin, styrene resin, polyamide resin, polyacetal resin, polyvinyl resin, polyvinyl chloride resin, polycarbonate resin, etc. Among them, polyolefin resin is preferable. If polyolefin resin is used, a molded body having better mechanical strength can be obtained.
[0011] Examples of the polyolefin resin include homopolymers of α-olefins, copolymers containing structural units derived from α-olefins, etc. As the polyolefin resin, two or more kinds of resins may be used in combination.
[0012] The α-olefin constituting the polyolefin resin is preferably an α-olefin having 2 to 10 carbon atoms, more preferably an α-olefin having 2 to 8 carbon atoms, further preferably ethylene, propylene or 1-butene, and particularly preferably propylene.
[0013] In one embodiment, a polypropylene resin is used as the polyolefin resin. By using a polypropylene resin, it is possible to disperse the water-soluble polymer in the resin, and the effect of including a fibrous water-soluble polymer becomes significant, and a resin composition capable of forming a molded body having particularly excellent mechanical strength can be obtained. Examples of the polypropylene resin include a homopolymer of propylene and a copolymer of propylene and other monomers copolymerizable with propylene. A homopolymer of propylene is preferable. Examples of other monomers copolymerizable with propylene include, for example, ethylene, 1-butene, isobutene, 1-pentene, 2-methyl-1-butene, 3-methyl-1-butene, 1-hexene, 3-methyl-1-pentene, 4-methyl-1-pentene, 1-heptene, 1-octene, 1-decene, 1-dodecene, 1-tetradecene, 1-hexadecene, 1-octadecene, and 1-icosene. The content of propylene-derived structural units in the polypropylene-based resin is preferably 50 mol % or more, more preferably 80 mol % or more, more preferably 90 mol % or more, and even more preferably 95 mol % or more.
[0014] The melt flow rate of the thermoplastic resin at 230° C. and 2.16 kgf is preferably 0.1 g / 10 min to 100 g / min, more preferably 0.5 g / 10 min to 80 g / min, and further preferably 1 g / 10 min to 50 g / min. If it is within such a range, a resin composition having particularly excellent moldability can be obtained.
[0015] The content of the thermoplastic resin is preferably 70 to 97 parts by weight, more preferably 80 to 95 parts by weight, and even more preferably 85 to 95 parts by weight, based on 100 parts by weight of the resin composition.
[0016] A-2. Water-soluble polymer The water-soluble polymer is a polymeric compound that dissolves at least 1 g in 100 g of water at 25° C. Any suitable water-soluble polymer can be used as the water-soluble polymer as long as the effects of the present invention can be obtained. Examples of the water-soluble polymer include polymers having polar functional groups capable of hydrogen bonding, such as hydroxyl groups, carboxyl groups, amino groups, and amide groups. Specific examples of the water-soluble polymer include polyvinyl alcohol resins, polyalkylene glycol resins, polyacrylamide resins, polymaleic acid resins, and cellulose resins.
[0017] In one embodiment, a polyvinyl alcohol-based resin is used as the water-soluble polymer. Typically, the polyvinyl alcohol-based resin is obtained by saponifying a polyvinyl acetate-based polymer.
[0018] The polyvinyl alcohol resin may be a copolymer containing a structural unit derived from vinyl alcohol in addition to polyvinyl alcohol. The structural units (hereinafter also referred to as "other structural units") other than the structural units derived from vinyl alcohol (and the structural units derived from vinyl acetate) contained in the copolymer include units having a dihydroxyalkyl group, an acetoacetyl group, an oxyalkylene group, a carboxy group, an alkoxycarbonyl group, etc., and units derived from olefins such as ethylene. Specific examples of polyvinyl alcohol resins as copolymers include butenediol-vinyl alcohol copolymers (BVOH), ethylene-vinyl alcohol copolymers (EVOH), etc.
[0019] In the polyvinyl alcohol-based resin as a copolymer, the content of other structural units is preferably 2 mol % to 30 mol %, and more preferably 5 mol % to 20 mol %, based on all structural units constituting the polyvinyl alcohol-based resin.
[0020] The saponification degree of the polyvinyl alcohol resin is preferably 90 mol% or more, more preferably 95 mol% or more, and even more preferably 98 mol% or more. In this range, the strength of the fibrous polyvinyl alcohol resin is increased, and a resin composition that can contribute to improving mechanical strength can be obtained. The saponification degree can be measured according to JIS K6726.
[0021] The degree of polymerization of the polyvinyl alcohol resin is preferably 200 to 2500, more preferably 200 to 1000. Within this range, the polyvinyl alcohol resin can be easily dissolved. The polyvinyl alcohol resin is easily dispersed in a fibrous form, and the use of the polyvinyl alcohol resin can provide a resin composition that can contribute to improving mechanical strength. The degree of polymerization can be measured in accordance with JIS K 6726.
[0022] The weight average molecular weight of the water-soluble polymer is preferably 8000 to 100000, and more preferably 8000 to 45000. The weight average molecular weight of the water-soluble polymer can be measured by gel permeation chromatography.
[0023] The melting point of the water-soluble polymer is preferably higher than that of the thermoplastic resin. The melting point of the water-soluble polymer is preferably at least 20° C. higher than that of the thermoplastic resin, and more preferably at least 35° C. higher. The melting point of the water-soluble polymer is preferably 180° C. to 250° C., and more preferably 190° C. to 230° C.
[0024] As described above, the water-soluble polymer is fibrous. By using a water-soluble polymer in a fibrous form, a resin composition capable of forming a molded article having excellent mechanical strength can be obtained. In the resin composition, the fiber diameter (number average diameter) of the water-soluble polymer is preferably 100 μm or less, more preferably 50 μm or less, and even more preferably 10 μm or less. The lower limit of the fiber diameter (number average diameter) of the water-soluble polymer is, for example, 0.1 μm. In addition, the fiber length (number average length) of the water-soluble polymer is preferably 50 μm or more, more preferably 100 μm or more, and even more preferably 200 μm or more. The upper limit of the fiber length (number average length) of the water-soluble polymer is, for example, 2000 μm. In addition, the aspect ratio (fiber length / fiber diameter) of the water-soluble polymer is preferably 5 or more and 2000 or less, more preferably 8 or more and 1000 or less, and even more preferably 10 or more and 500 or less. By dispersing the water-soluble polymer having such a shape in the resin composition, a resin composition capable of forming a molded article having excellent mechanical strength can be obtained.
[0025] The content of the water-soluble polymer is preferably 3 to 20 parts by weight, more preferably 5 to 15 parts by weight, based on 100 parts by weight of the resin composition. If the content is within this range, a resin composition capable of forming a molded product having particularly excellent mechanical strength can be obtained.
[0026] The resin composition of the present invention may further contain any suitable additives as necessary, such as a flow modifier, a smear inhibitor, a heat stabilizer, a weathering agent, or other stabilizers, a pigment, a dye, or other colorants, a lubricant, a crosslinking agent, a crosslinking assistant, an antiblocking agent, an antistatic agent, an antifogging agent, an organic filler, an inorganic filler, or the like.
[0027] B. Method for producing resin composition In one embodiment, the method for producing the resin composition of the present invention comprises: dissolving a water-soluble polymer in a solvent to prepare a solution; melt-kneading the solution with a thermoplastic resin; and removing the solvent after melt-kneading.By this method, the resin composition, that is, the resin composition containing the water-soluble polymer dispersed in a fibrous form, can be obtained.In addition, in this specification, melt-kneading means kneading performed under the condition that the thermoplastic resin melts.
[0028] The concentration of the water-soluble polymer in the solution is preferably 5% by weight to 50% by weight, more preferably 10% by weight to 40% by weight, and further preferably 15% by weight to 25% by weight. Within such a range, a resin composition can be obtained in which the water-soluble polymer that has been preferably fiberized is well dispersed in the thermoplastic resin.
[0029] As the solvent, any appropriate solvent can be used as long as it can dissolve the water-soluble polymer at a concentration of 1% by weight or more at 25° C. Examples of the solvent include water, alcohol, ethylene glycol, triethylene glycol, glycerin, acetamide, dimethylacetamide, dimethylsulfoxide, etc., and two or more types of solvents can be mixed and used. Of these, water is preferred.
[0030] The water-soluble polymer solution may further contain any suitable additive, as necessary, such as a dispersant, an antifoaming agent, a flow modifier, a surfactant, a salt, an organic filler, or an inorganic filler.
[0031] Examples of the melt kneading method include a method using a kneading device such as a single screw extruder, a multi-screw extruder, a tandem extruder, or a Banbury mixer.
[0032] In one embodiment, the solution and the thermoplastic resin are melt-kneaded using a continuous melt-kneading device (for example, a twin-screw extruder).
[0033] In one embodiment, the solution and the thermoplastic resin are separately charged into the kneading device. Preferably, the solution and the thermoplastic resin are charged into the kneading device in a procedure in which the thermoplastic resin is melted and then the solution is added to the thermoplastic resin. For example, a continuous melt kneading device is used that includes a main throat that is an inlet for materials, an outlet for discharging the resin composition obtained after kneading, and a side feeder (liquid addition nozzle) provided between the main throat and the outlet, and the thermoplastic resin is charged from the main throat, the thermoplastic resin is melted, and then the solution is charged from the side feeder. In one embodiment, the solution is added by injecting the solution at a pressure higher than the internal pressure of the melt kneading device.
[0034] As the processing conditions for melt-kneading, any appropriate conditions can be adopted as long as the effects of the present invention can be obtained.
[0035] The melting temperature during the melt kneading is a temperature at which the thermoplastic resin can be melted, and is, for example, 100° C. to 300° C. When a polypropylene resin is used as the thermoplastic resin, the melting temperature during the melt kneading is preferably 160° C. to 230° C., and more preferably 180° C. to 210° C.
[0036] The screw rotation speed during the melt kneading is preferably 50 rpm to 500 rpm, and more preferably 100 rpm to 300 rpm. Within such a range, the water-soluble polymer can be particularly preferably turned into fibers.
[0037] The solvent removal after melt-kneading can be performed by any appropriate method. In one embodiment, a vacuum vent is provided in a continuous melt-kneading apparatus, and the inside of the melt-kneading apparatus is depressurized by the vacuum vent, thereby removing the solvent from the mixture containing the solution and the thermoplastic resin after melt-kneading.
[0038] In another embodiment, the resin composition can be obtained by melt-kneading a water-soluble polymer (e.g., a powdered water-soluble polymer) with a thermoplastic resin, and extruding the mixture to obtain pellets, thereby providing a sufficient flow rate (shear rate) at the die outlet. This production method can also provide a resin composition containing a water-soluble polymer dispersed in a fibrous form.
[0039] Preferably, the shear rate is 100 sec -1 The mixture of the water-soluble polymer and the thermoplastic resin (the mixture after melt kneading) is extruded in such a manner that the shear rate is more preferably 1000 sec -1 The upper limit of the shear rate of the resin composition during melt molding is, for example, 10,000 sec -1 Within such a range, as described above, the orientation of the water-soluble polymer is increased, and a resin composition capable of forming a molded article having superior mechanical strength can be obtained.
[0040] In one embodiment, the resin composition is provided in the form of pellets. The pelletization of the resin composition can be carried out by any suitable method.
[0041] C. Molded object The resin composition of the present invention can be melt molded to obtain films, fibers, and other molded articles of various shapes. Examples of melt molding methods include injection molding, extrusion molding (sheet molding, film molding), and blow molding. Among them, injection molding is preferred.
[0042] During melt molding, the flow rate of the molten resin composition is preferably high within a range in which a molded article with the desired properties can be molded. For example, during the above molding, by providing a sufficient flow rate (shear rate) at the die outlet and inside the mold, the orientation of the water-soluble polymer is increased, and a molded article with superior mechanical strength can be obtained. The shear rate of the resin composition during melt molding is preferably 100 sec -1 More preferably, 1000 sec -1The upper limit of the shear rate of the resin composition during melt molding is, for example, 10,000 sec -1 Within such a range, the orientation of the water-soluble polymer is increased, as described above, and a molded article having superior mechanical strength can be obtained.
[0043] The melting temperature during melt molding is preferably a temperature at which the thermoplastic resin in the resin composition can melt and at which the water-soluble polymer can maintain its fibrous form.
[0044] The molded article can be molded into, for example, a sheet, a film, a rod, a tube, a block, an irregular shape, etc., depending on the application. Examples of the shape of the molded article include containers, freezer bags, blown bottles, trays, packaging materials, tapes, lids, etc. The molded article can also be used as a covering material. Furthermore, by using the resin composition of the present invention, molded articles of mechanical parts, electrical parts, electronic parts, and automobile parts can also be obtained. EXAMPLES
[0045] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these examples. The evaluation methods in the examples are as follows. Note that parts and % are based on weight unless otherwise specified.
[0046] (1) Tensile yield stress and elastic modulus of molded body The measurement was performed in accordance with JIS K 7162, with a sample thickness of 4.0 mm, a test speed of 50 mm / min, and a temperature of 23° C. The tensile direction was parallel to the injection direction of the resin composition.
[0047] (2) Specific gravity of the molded body The measurements were performed by the immersion method using test pieces of appropriate shape in accordance with JIS K7112.
[0048] [Example 1] (Preparation of Water-Soluble Polymer Aqueous Solution) 20 parts by weight of water-soluble polymer A1 (butenediol-vinyl alcohol copolymer, manufactured by Nippon Synthetic Chemical Industry Co., Ltd., product name "G-Polymer OKS-1011", fully saponified, degree of polymerization: 300) was added to 80 parts by weight of purified water, and the mixture was stirred at 90°C for 1 hour to obtain an aqueous water-soluble polymer solution. (Formation of resin composition) A polyolefin resin (polypropylene, Japan Polypropylene, product name "Novatec MA1B") was put into a twin-screw extruder (Toshiba Machine, product name "TEM37SS") and heated to 200°C to melt the polyolefin resin. The water-soluble polymer aqueous solution was then injected at a pressure higher than the extruder internal pressure so that the amount of water-soluble polymer was 10 parts by weight per 90 parts by weight of the polyolefin resin. The polyolefin resin and the water-soluble polymer were then thoroughly kneaded at a temperature of 200°C while maintaining a pressure at which purified water would not vaporize. Next, the contained water was forcibly removed by volatilization through the vacuum vent of the twin-screw extruder, to obtain a pellet-like resin composition containing 10 parts by weight of the water-soluble polymer in 90 parts by weight of the polyolefin resin. (injection molding) The resin composition was molded at a molding temperature of 200°C using an injection molding machine (manufactured by Toyo Machinery & Metals, product name "SI-80IV-D150B" 200t) to obtain a test piece conforming to JIS K 7141. The obtained test piece was conditioned in a constant temperature and humidity room for 24 hours and then subjected to the above evaluations (1) and (2). The results are shown in Table 1.
[0049] [Example 2] Test specimens were molded in the same manner as in Example 1, except that water-soluble polymer A2 (polyvinyl alcohol, manufactured by Kuraray Co., Ltd., trade name "Kuraray Poval PVA-110", fully saponified, degree of polymerization: 1000) was used instead of water-soluble polymer A1. The test specimens obtained were conditioned in a constant temperature and humidity chamber for 24 hours and then subjected to the above evaluations (1) and (2). The results are shown in Table 1.
[0050] [Comparative Example 1] A polyolefin resin (polypropylene, Japan Polypropylene Corporation, product name "Novatec MA1B") and a powdered water-soluble polymer (butenediol vinyl alcohol copolymer, Nippon Synthetic Chemical Industry Co., Ltd., product name "G-Polymer OKS-1011", fully saponified, degree of polymerization: 300) were placed into a twin-screw extruder (Toshiba Machine Corporation, product name "TEM37SS") and heated to 200°C to obtain a resin composition. Except for using this resin composition, a test specimen was molded in the same manner as in Example 1. The obtained test specimen was conditioned in a temperature-constant humidity chamber for 24 hours and then subjected to the above evaluations (1) and (2). The results are shown in Table 1.
[0051] [Comparative Example 2] Test pieces were molded in the same manner as in Example 2, except that the aqueous water-soluble polymer solution was not prepared, and a water-soluble polymer (polyvinyl alcohol, manufactured by Kuraray Co., Ltd., trade name "Kuraray Poval PVA-110", fully saponified, polymerization degree: 1000) was added in powder form when melt-kneading in the twin-screw extruder. The test pieces obtained were conditioned in a constant temperature and humidity chamber for 24 hours, and then subjected to the above evaluations (1) and (2). The results are shown in Table 1.
[0052] [Comparative Example 3] Except for not adding the water-soluble polymer aqueous solution, the polyolefin resin was passed through a twin-screw extruder to mold a test piece in the same manner as in Example 1. The obtained test piece was conditioned in a constant temperature and humidity chamber for 24 hours and then subjected to the above evaluations (1) and (2). The results are shown in Table 1.
[0053] [Comparative Example 4] Test pieces were molded in the same manner as in Example 1, except that an inorganic filler (manufactured by Nippon Talc Co., Ltd., product name "PC-25") was added to the polyolefin resin instead of the water-soluble polymer aqueous solution. The amount of inorganic filler was 10 parts by weight relative to 90 parts by weight of the polyolefin resin. The obtained test pieces were conditioned in a constant temperature and humidity chamber for 24 hours, and then subjected to the above evaluations (1) and (2). The results are shown in Table 1.
[0054] [Table 1]
[0055] <Observation of Dispersion State> From the test pieces obtained in Example 1 and Comparative Example 1, thin sections were taken using a microtome and immersed in boiling water at 90°C for 4 hours. The water-soluble polymer was completely dissolved and desorbed from the thin sections, and the specimens were used for observation. In other words, the water-soluble polymer was present in the voids in the thin sections after immersion, and the dispersion state of the water-soluble polymer could be observed by observing the specimens with an optical microscope (300x), as shown in Figure 1. In Figure 1, the dark areas are the areas where the water-soluble polymer was present. The direction of the arrow corresponds to the injection direction during molding. The surface of the test piece obtained in Example 1 was observed by SEM. The SEM photograph is shown in Figure 2. Furthermore, an SEM photograph of a cross section of the test piece cut perpendicular to the resin flow direction is shown in Figure 3. The number average particle size and number average fiber length of Example 1 were determined by measuring the fiber diameter and fiber length in a 1000 μm×1000 μm area of a SEM photograph. The number average particle size of Example 1 was 18 μm, and the number average fiber length was 200 μm.
[0056] [Example 3] A polyolefin resin (polypropylene, Japan Polypropylene, product name "Novatec MA1B") and a powdered water-soluble polymer (butenediol vinyl alcohol copolymer, Nippon Synthetic Chemical Industry Co., Ltd., product name "G-Polymer OKS-1011", fully saponified, degree of polymerization: 300) were put into a twin-screw extruder (Toshiba Machine, product name "TEM37SS") and heated to 200°C to obtain a mixture of the water-soluble polymer and the thermoplastic resin, which was made into a pellet-shaped composition. This composition was measured using a capillary viscometer (Yasuda Seiki Seisakusho, product name "140SAS-2002") at a temperature of 200°C, a cylindrical die L / D = 40 / 1 (land 40 mm, diameter 1 mm), and a shear rate of 1000 S. -1 The mixture was extruded under the above conditions and cut to obtain a pellet-shaped resin composition. The obtained resin composition was placed on a hot stage (manufactured by Mettler Toledo, product name "Mettler FP90") and observed at an observation temperature of 180°C using a polarizing microscope (manufactured by Leica, product name "Leica DMLP"), and the results are shown in Figure 4. (injection molding) The resin composition was molded at a molding temperature of 200°C using an injection molding machine (manufactured by Toyo Machinery & Metals, product name "SI-80IV-D150B" 200t) to obtain a test piece conforming to JIS K 7141. The obtained test piece was conditioned in a constant temperature and humidity room for 24 hours and then subjected to the above evaluations (1) and (2). The results are shown in Table 2.
[0057] [Example 4] Shear rate 138S -1 Except for changing the temperature, the observation was performed in the same manner as in Example 3, and the results are shown in Fig. 4. Also, a test piece was obtained in the same manner as in Example 3, and was subjected to the same evaluation as in Example 3. The results are shown in Table 2.
[0058] [Comparative Example 5] Shear rate 22S -1 Except for changing the temperature, the observation was performed in the same manner as in Example 3, and the results are shown in Fig. 4. Also, a test piece was obtained in the same manner as in Example 3, and was subjected to the same evaluation as in Example 3. The results are shown in Table 2.
[0059] As shown in Figure 4, the dispersion state of the unmelted water-soluble polymer A1 was observed at a temperature (180°C) above the melting point of the polyolefin resin and below the melting point (206°C) of the water-soluble polymer A1. It was observed that the amount of fibrous water-soluble polymer A1 increased as the shear rate increased. From the above, it is clear that the water-soluble polymer can be oriented in a fibrous form by controlling the shear rate when producing a pellet-shaped resin composition or a molded product.
[0060] [Table 2] [Industrial Applicability]
[0061] The resin composition of the present invention can be suitably used as a material for various molded articles such as containers, freezer bags, blown bottles, trays, packaging materials, tapes, lids, and automobile parts.
Claims
1. A method for producing a resin composition comprising a thermoplastic resin and a water-soluble polymer, comprising: dissolving a water-soluble polymer in a solvent to prepare a solution; Melting and kneading the solution with a thermoplastic resin; and removing the solvent after melt-kneading; the thermoplastic resin is a polyolefin resin, an acrylic resin, a polyester resin, a styrene resin, a polyamide resin, a polyacetal resin, a polyvinyl resin, a polyvinyl chloride resin, or a polycarbonate resin; The water-soluble polymer is a polyvinyl alcohol-based resin, a polyalkylene glycol-based resin, a polyacrylamide-based resin, a polymaleic acid-based resin, or a cellulose-based resin. A method for producing a resin composition.
2. The method for producing a resin composition according to claim 1 , wherein the water-soluble polymer is a polyvinyl alcohol-based resin.
3. The method for producing a resin composition according to claim 2, wherein the degree of polymerization of the polyvinyl alcohol-based resin is 200 to 2500.
4. The method for producing a resin composition according to claim 2 or 3, wherein the polyvinyl alcohol-based resin has a degree of saponification of 90 mol % or more.
5. The method for producing a resin composition according to claim 1 , wherein the thermoplastic resin is a polyolefin-based resin.
6. The method for producing a resin composition according to claim 1 , wherein the solvent is water.
7. The method for producing a resin composition according to any one of claims 1 to 6, wherein the water-soluble polymer concentration in the solution is 5% by weight to 50% by weight.
8. The method for producing a resin composition according to claim 1 , wherein the solution and the thermoplastic resin are melt-kneaded using a continuous melt-kneading device.
9. Melting and kneading a water-soluble polymer and a thermoplastic resin; The mixture obtained by the melt kneading was subjected to a shear rate of 100 sec. -1 and extruding the mixture so as to obtain the above-mentioned. A method for producing the resin composition according to any one of claims 1 to 8.
10. A resin composition obtained by a method for producing a resin composition described in any one of claims 1 to 9.
11. A molded article formed from the resin composition according to claim 10.
Citation Information
Patent Citations
Resin composition and its application
JP2005298697A
Polypropylene resin composition, method of manufacturing the same, and molded article produced by molding the same
JP2012149246A
Organic fiber for resin reinforcement, and fiber reinforced thermoplastic resin
JP2012251036A
Method for producing biomass nanofibers and method for producing biomass nanofiber-polymeric resin composite