Hardening composition
A curable composition using a block copolymer and specific acrylate monomers addresses flexibility issues in cured products, enhancing durability and insulation.
Patent Information
- Application Number
- JP2020101174
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-06-10
- Publication Date
- 2024-09-27
- Estimated Expiration
- 2040-06-10
AI Technical Summary
Cured products from conventional light-curable compositions lack sufficient flexibility, leading to potential cracking.
Incorporation of a block copolymer with polyolefin and polystyrene block structures, along with saturated cycloalkyl and saturated chain alkyl (meth)acrylate monomers, to enhance flexibility.
The composition achieves a cured product with improved flexibility and reduced moisture permeability, maintaining electrical insulation properties.
Smart Images

Figure 0007557288000001 
Figure 0007557288000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a curable composition that is cured, for example, by irradiation with light. [Background technology]
[0002] Conventionally, as a curable composition that is cured by irradiation with light, for example, a curable composition containing a urethane acrylate (A) synthesized from hydrogenated polybutadiene diol or hydrogenated polyisoprene diol and having a number average molecular weight of 1,000 to 20,000, a monofunctional (meth)acrylate monomer (B), and an initiator (C) having an absorption band at a wavelength of 380 nm or more, in which the content of the component (C) is 10 to 15 parts by weight per 100 parts by weight of the total of the components (A) and (B) is known (for example, Patent Document 1).
[0003] The curable composition described in Patent Document 1 is applied onto an electronic circuit and then cured by irradiation with light, and is used in electronic circuit coating applications. The curable composition described in Patent Document 1 can be cured even with light from an LED light source, and can have good moisture resistance, electrical insulation, and the like. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2018-024761 A Summary of the Invention [Problem to be solved by the invention]
[0005] However, the cured product obtained by curing the curable composition described in Patent Document 1 does not necessarily have sufficient flexibility, and for example, the cured product that has become a cured coating may crack, etc. Therefore, there is a demand for a curable composition that can provide a cured product with good flexibility after curing.
[0006] In view of the above problems, an object of the present invention is to provide a curable composition which can give a cured product having good flexibility after curing. [Means for solving the problem]
[0007] In order to solve the above problems, the curable composition according to the present invention comprises: a block copolymer having a polyolefin block structure and a polystyrene block structure in its molecule; A saturated cycloalkyl (meth)acrylate monomer having a saturated cyclic hydrocarbon structure and a (meth)acryloyl group in the molecule; a saturated chain alkyl (meth)acrylate monomer having a saturated chain hydrocarbon structure and a (meth)acryloyl group in the molecule; The present invention is characterized by comprising: According to the above-mentioned curable composition, the cured product after curing can have good flexibility.
[0008] In the curable composition according to the present invention, the block copolymer preferably has a hydroxy group at an end of the molecular chain, which can improve the flexibility of the cured product obtained after the curable composition is cured. Effect of the Invention
[0009] According to the curable composition of the present invention, a cured product having good flexibility can be obtained. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] Hereinafter, one embodiment of the curable composition according to the present invention will be described.
[0011] The curable composition of the present embodiment comprises a block copolymer having a polyolefin block structure and a polystyrene block structure in the molecule, A saturated cycloalkyl (meth)acrylate monomer having a saturated cyclic hydrocarbon structure and a (meth)acryloyl group in the molecule; and a saturated chain alkyl (meth)acrylate monomer having a saturated chain hydrocarbon structure and a (meth)acryloyl group in the molecule.
[0012] The block copolymer has a polyolefin block structure and a polystyrene block structure in the molecule, a polystyrene block structure at each end of the molecular chain, and a polyolefin block structure between the polystyrene block structures.
[0013] The polyolefin block structure does not contain polar groups such as ether groups or ester groups, and is composed only of hydrocarbon groups. Such hydrocarbon groups may be saturated or unsaturated. Such hydrocarbon groups may contain both saturated and unsaturated hydrocarbon groups. It is preferable that the majority of the polyolefin block structure is composed of saturated hydrocarbons. In order to further harden the curable composition of the present embodiment, the polyolefin block structure may contain an unsaturated hydrocarbon group, while in order to provide a cured product of the curable composition of the present embodiment with better heat resistance and weather resistance, it is preferable that the proportion of unsaturated hydrocarbon groups in the polyolefin block structure is small. For example, the proportion of unsaturated hydrocarbon groups in the polyolefin block structure may be 10 mass% or less, or 5 mass% or less, relative to the total mass of the curable composition.
[0014] The polyolefin block structure has as its constituent units ethylene, propylene, 1,3-butadiene (and its hydrogenated derivatives), isoprene (and its hydrogenated derivatives), and the like. The polyolefin block structure is usually composed of saturated bonds, but may have some unsaturated bonds. The constituent units are preferably ethylene, propylene, and butylene (-CH2CH(CH2CH3)-). In other words, the polyolefin block structure preferably has at least one of ethylene, propylene, and butylene as a constituent unit.
[0015] In the polyolefin block structure, the constituent units may be arranged randomly, in other words, the constituent units may be formed by incorporating different types of monomers into the molecular chain through random polymerization. For example, the polyolefin block structure may include a random arrangement of ethylene and propylene building blocks.
[0016] The degree of polymerization in the polyolefin block structure is, for example, 100 or more and 1,000 or less.
[0017] Each polystyrene block structure has, as a structural unit, a structural unit such as styrene, α-methylstyrene, o-methylstyrene, m-methylstyrene, p-methylstyrene, t-butylstyrene, 2,4-dimethylstyrene, or 2,4-diethylstyrene. The structural unit includes one or more of these. As the structural unit, styrene or α-methylstyrene structural units are preferred. In other words, each polystyrene block structure preferably has at least one of styrene and α-methylstyrene as a structural unit.
[0018] The degree of polymerization of each polystyrene block structure is, for example, 50 or more and 100 or less.
[0019] Examples of the block copolymer include styrene-butadiene-styrene block copolymer (SBS), styrene-isoprene-styrene block copolymer (SIS), styrene-ethylene-butene-styrene block copolymer (SEBS), styrene-ethylene-propylene-styrene block copolymer (SEPS), styrene-ethylene-ethylene-propylene-styrene block copolymer (SEEPS), etc. As the block copolymer, styrene-ethylene-ethylene-propylene-styrene block copolymer (SEEPS) is preferable.
[0020] The proportion of the polystyrene block structure in the block copolymer may be from 10% by mass to 50% by mass, and is preferably from 20% by mass to 40% by mass.
[0021] The block copolymer preferably has a hydroxy group at an end of the molecular chain. The block copolymer may have a hydroxy group at each of both ends of the molecular chain, or may have a hydroxy group at either one end (one end). By having a hydroxy group at the end of the molecular chain, the compatibility of the block copolymer with the saturated cycloalkyl (meth)acrylate monomer and the saturated chain alkyl (meth)acrylate monomer is improved, and therefore the cured product obtained by curing the curable composition has better flexibility and low moisture permeability. The other end may be a residue of a polymerization initiator, or the like.
[0022] The block copolymer does not contain reactive groups such as isocyanate groups or glycidyl groups in the molecule, and the main chain of the block copolymer does not contain nitrogen (N) that forms urethane bonds or amide bonds, or sulfur (S) that forms sulfonyl groups. The above block copolymer generally does not have a crosslinked structure and is not modified.
[0023] A preferred molecular structure of the block copolymer having a hydroxy group at one end of the molecular chain as described above is represented by the following formula (1). Formula (1) represents a structure having a hydroxy group at one end of SEEPS. In the following formula (1), p may be 50 or more and 100 or less, q may be 100 or more and 500 or less, r may be 400 or more and 1,000 or less, s may be 50 or more and 100 or less, and m may be 500 or more and 1,500 or less.
[0024] [ka]
[0025] The block copolymer may have a number average molecular weight of, for example, 10,000 or more and 100,000 or less.
[0026] The block copolymer may be a commercially available product, such as Kraton G1650 (Kraton) or Septon HG252 (Kuraray, having an -OH group at one end of the molecular chain).
[0027] As described above, the curable composition of the present embodiment contains a saturated cycloalkyl (meth)acrylate monomer and a saturated chain alkyl (meth)acrylate monomer.
[0028] The saturated cycloalkyl (meth)acrylate monomer is preferably an esterified compound of a monohydric alcohol containing a saturated cyclic hydrocarbon structure (a cyclic moiety structure formed only of carbon atoms) and (meth)acrylic acid. The number of carbon atoms of the monohydric alcohol containing a saturated cyclic hydrocarbon structure is preferably 8 to 15. The saturated cycloalkyl (meth)acrylate monomer preferably does not contain a benzene ring or a polar group such as an ether bond (-CH2-O-CH2-), an -OH group, or a -COOH group in the molecule.
[0029] The saturated cycloalkyl (meth)acrylate monomer is preferably a monofunctional monomer having one (meth)acrylate group in the molecule. In the saturated cycloalkyl (meth)acrylate monomer, the saturated cyclic hydrocarbon structure may be a structure in which each carbon ring is formed by 4 to 8 carbon atoms without containing a heteroatom. The saturated cycloalkyl (meth)acrylate monomer may be a monocyclic, bicyclic, or polycyclic. The bicyclic or polycyclic saturated cyclic hydrocarbon structure may share two or more carbon atoms. In the bicyclic or polycyclic saturated cycloalkyl (meth)acrylate monomer, at least one ring structure may be a saturated alkyl structure, and for example, all ring structures may be saturated alkyl structures. In the saturated cycloalkyl (meth)acrylate monomer, a methyl group or an ethyl group may be further bonded to the carbon of the saturated cyclic hydrocarbon structure.
[0030] Examples of saturated cycloalkyl (meth)acrylate monomers include isobornyl (meth)acrylate (containing a norbornane structure), dicyclopentadieneoxyethyl (meth)acrylate (containing a norbornane structure), dicyclopentanyl (meth)acrylate (containing a norbornane structure), dicyclopentenyloxyethyl (meth)acrylate (containing a norbornane structure), and adamantyl (meth)acrylate.
[0031] As the saturated cycloalkyl(meth)acrylate monomer, among the above-mentioned monomers, a monomer containing a norbornane structure is preferable, and at least one of isobornyl(meth)acrylate and dicyclopentanyloxyethyl(meth)acrylate is more preferable.
[0032] By including a saturated cycloalkyl (meth)acrylate monomer in the curable composition, the saturated cycloalkyl (meth)acrylate monomer can dissolve the block copolymer more thoroughly in the curable composition.
[0033] The saturated chain alkyl (meth)acrylate monomer is preferably a (meth)acrylate monomer having a saturated chain hydrocarbon with 8 to 15 carbon atoms in the molecule, and is preferably a (meth)acrylate monomer having a saturated chain hydrocarbon with 8 to 12 carbon atoms in the molecule. The saturated chain alkyl (meth)acrylate monomer preferably does not contain any of a benzene ring and a polar group such as an ether bond (-CH2-O-CH2-), an -OH group, or a -COOH group in the molecule. The saturated chain alkyl (meth)acrylate monomer is preferably a monofunctional monomer having one (meth)acrylate group in the molecule. In the saturated chain alkyl (meth)acrylate monomer, the saturated chain hydrocarbon structure may be a saturated chain hydrocarbon structure containing no atoms other than C and H and composed of 7 to 11 carbon atoms. When the curable composition contains a saturated chain alkyl (meth)acrylate monomer, the flexibility of the cured product obtained by curing the curable composition can be further improved.
[0034] In the saturated chain alkyl (meth)acrylate monomer, the saturated chain hydrocarbon structure may be linear or branched. In other words, the saturated chain hydrocarbon structure may be a saturated linear hydrocarbon structure or a saturated branched hydrocarbon structure. In other words, the saturated chain alkyl (meth)acrylate monomer may be a saturated linear alkyl (meth)acrylate monomer or a saturated branched alkyl (meth)acrylate monomer. As the saturated chain alkyl (meth)acrylate monomer, a saturated branched chain alkyl (meth)acrylate monomer is preferred in that it can dissolve the block copolymer more sufficiently in the curable composition, which allows a more uniform cured film to be obtained without being affected by the substrate supporting the cured product, the thickness of the cured product, or the curing reaction conditions.
[0035] In the curable composition of this embodiment, the ratio of the saturated cycloalkyl (meth)acrylate monomer to the total mass of the saturated cycloalkyl (meth)acrylate monomer and the saturated chain alkyl (meth)acrylate monomer (100 parts by mass) is preferably 30 parts by mass or more and 95 parts by mass or less. This makes it possible to obtain a cured product that has a better balance between electrical insulation performance and flexibility (elongation performance).
[0036] The hydrocarbon structure of the saturated linear alkyl (meth)acrylate monomer may be any structure as long as it is a saturated linear alkyl structure. Specifically, examples of the saturated linear alkyl(meth)acrylate monomer include n-heptyl(meth)acrylate, n-octyl(meth)acrylate, n-nonyl(meth)acrylate, and n-decyl(meth)acrylate.
[0037] The hydrocarbon structure of the saturated branched alkyl (meth)acrylate monomer may be a saturated branched alkyl structure, and may be an iso structure, a sec structure, a neo structure, or a tert structure. Specifically, examples of the saturated branched alkyl (meth)acrylate monomer include isoheptyl (meth)acrylate, isooctyl (meth)acrylate, isononyl (meth)acrylate, isodecyl (meth)acrylate, and 2-ethylhexyl (meth)acrylate. As the saturated branched alkyl (meth)acrylate monomer, at least one of isononyl (meth)acrylate and isodecyl (meth)acrylate is preferred, since it has better solubility in the block copolymer and is more likely to produce a more uniform cured coating.
[0038] The above-mentioned curable composition may contain one type of saturated cycloalkyl (meth)acrylate monomer alone or two or more types of saturated chain alkyl (meth)acrylate monomers in combination. As the saturated cycloalkyl (meth)acrylate monomer and the saturated chain alkyl (meth)acrylate monomer, commercially available products can be used.
[0039] In the curable composition of the present embodiment, the proportion of the block copolymer is preferably 10 parts by mass or more and 25 parts by mass or less relative to 100 parts by mass in total of the above-mentioned block copolymer, saturated cycloalkyl (meth)acrylate monomer, and saturated chain alkyl (meth)acrylate monomer.
[0040] The curable composition of the present embodiment contains a photopolymerization initiator that initiates a polymerization reaction by irradiation with light.
[0041] The photopolymerization initiator is not particularly limited as long as it is a compound that generates radicals when irradiated with light (such as ultraviolet light). Examples of the photopolymerization initiator include acetophenone-based photoinitiators, benzoin-based photoinitiators, benzophenone-based photoinitiators, thioxanthone-based photoinitiators, and acylphosphine oxide-based photoinitiators. As the photopolymerization initiator, commercially available products can be used.
[0042] The curable composition of the present embodiment may contain a photosensitizer, a polymerization inhibitor, an antioxidant, a dye, a pigment, a fluorescent material, and the like, as necessary. The curable composition of the present embodiment preferably does not contain powder such as an inorganic powder or a resin powder.
[0043] The curable composition can be produced by a general method, for example, by mixing and stirring the block copolymer, a saturated cycloalkyl (meth)acrylate monomer, a saturated chain alkyl (meth)acrylate monomer, and a photopolymerization initiator.
[0044] The curable composition of the present embodiment is used as a cured product cured by irradiation with light such as ultraviolet light. For example, the curable composition is applied to an electronic circuit to be covered, and then the composition is cured by irradiation with light such as ultraviolet light to form a coating film of the cured product.
[0045] The light to be irradiated to promote the curing reaction can be ultraviolet light. The light source can be a high-pressure mercury lamp, a metal halide lamp, a xenon lamp, a chemical lamp, an LED lamp, or the like. The irradiation intensity can be, for example, 10 to 10,000 mW / cm. 2 can be adopted.
[0046] Examples of objects to be coated with the curable composition include electronic circuits and terminals on mounting boards used in precision instruments, electronic circuits and terminals on mounting boards installed in automobiles, bicycles, trains, aircraft, ships, etc., electronic circuits and terminals on mounting boards used in mobile devices (mobile phones, digital cameras, digital video cameras, etc.), electronic circuits and terminals on boards used in outdoor equipment (water heaters, air conditioner outdoor units, etc.), and electronic circuits and terminals on mounting boards used in wet equipment such as washing machines, warm-water cleaning toilet seats, and dishwashers and dryers.
[0047] The curable composition of the present embodiment is as exemplified above, but the present invention is not limited to the curable composition exemplified above. That is, various forms used in general curable compositions can be adopted as long as they do not impair the effects of the present invention. EXAMPLES
[0048] The present invention will now be described in more detail with reference to experimental examples, but the present invention is not limited to these.
[0049] The raw materials were mixed to prepare a curable composition as follows.
[0050] <Raw materials> (A) Block copolymer (A-1) Styrene-ethylene-butylene-styrene block copolymer (SEBS) Product name: Kraton G1650 (Kraton Corporation) (styrene content: 30% by mass, number average molecular weight: 67,000) (A-2) Styrene-ethylene / ethylene-propylene-styrene block copolymer (SEEPS) Product name: "Septon HG252" (manufactured by Kuraray Co., Ltd.) (styrene content 28% by mass, number average molecular weight 55,000) : Has an -OH group at one end of the molecular chain (denoted as SEEPS-OH) (B) Saturated cycloalkyl (meth)acrylate monomer (B-1) Isobornyl acrylate (IBXA commercial product) (B-2) Dicyclopentanyl acrylate Product name: "Fancryl FA-513AS" manufactured by Hitachi Chemical Co., Ltd. (C) Saturated chain alkyl (meth)acrylate monomer (C-1) Isononyl acrylate (INAA, commercially available product) Branched chain (C-2) Isodecyl acrylate (IDAA commercial product) Branched chain (others) Photopolymerization initiator Product name: "IRGACURE 907" Manufactured by IGM Resins Photosensitizer (2,4-diethylthioxanthone) Product name: "KAYACURE DETX-S" manufactured by Nippon Kayaku Co., Ltd.
[0051] Example 1 ·3、Reference Example 2·4 , Comparative Example) The above raw materials were stirred at 80° C. for 3 hours in the amounts shown in Table 1 to produce a curable composition.
[0052] [Table 1]
[0053] As shown below, the embodiment 、Reference example、 Specifically, the viscosity of each of the curable compositions produced, and the tensile elongation, tensile modulus, moisture permeability, and volume resistivity of the cured products were examined. Generally, a higher volume resistivity indicates more complete curing.
[0054] <Viscosity of Composition> Measurements were performed under the following conditions using a Toki Sangyo Co., Ltd. E-type rotational viscometer: RE-85R. Measurement temperature: 25℃, rotor: 1.34°, R24
[0055] <Curing> Each composition was applied to a tin plate measuring 0.3 × 130 × 180 mm so that the thickness of the cured product after curing was 100 μm. For samples cured by light, a 500 W UV lamp was used to apply an integrated light dose of 1,000 mJ / cm 2 The sample was irradiated with ultraviolet light so as to have a light intensity of 100 nm.
[0056] <Tensile elongation of the cured product (cured coating film)> A cured product (cured coating film) was formed on the release-treated PET film in the same manner as in the above curing treatment. Next, the PET film was peeled off from the cured coating film, and the cured coating film was cut into a JIS dumbbell No. 2 shape. Then, the tensile elongation was measured under the measurement conditions of chuck distance: 20 mm, crosshead speed: 300 mm / min. The elongation rate (%) was calculated by the following formula. Elongation rate (%) = (breaking elongation (mm) - 20) / 20 x 100
[0057] <Tensile modulus of cured product (cured coating film)> For the cured product (cured coating film) formed by the above-mentioned curing treatment, the slope S at which the tensile strength (N) / displacement elongation (mm) was maximized was determined, and the tensile modulus was calculated by the following formula. Tensile modulus (MPa) = S (tensile strength (N) / variable elongation (mm)) / (thickness (mm) x width (mm) x 20
[0058] <Moisture permeability of cured product (cured coating film)> Measurements were carried out using the cup method at 40°C under moisture absorption conditions in accordance with JIS K8123.
[0059] <Volume resistivity of the cured product (cured coating film)> A paste-like silver conductive paint was applied in a circle (diameter 30 mm) on each of the cured products (cured coating films) cured on the tin plate as described above. The upper electrode was formed by drying at 60°C for 30 minutes. Meanwhile, the tin plate used as the substrate was used as the lower electrode. A voltage of DC 100V was applied and the resistance value was calculated 60 seconds later. The electrode area was multiplied by the resistance value and divided by the thickness of the cured product (cured film) to calculate the volume resistivity.
[0060] The results of the evaluation by the above tests are shown in Table 1. As can be seen from the evaluation results shown in Table 1, the curable compositions of the Examples had sufficiently high tensile elongation percentages of the cured products and good flexibility after curing. In the cured products obtained by curing the curable compositions of the respective Examples, the acrylate monomers are polymerized with each other to form polymers, but the block copolymer is believed to exist in a state in which it does not react with the acrylate monomers, which is believed to give the cured products good flexibility. [Industrial Applicability]
[0061] The curable composition of the present invention is preferably used, for example, as a curable composition for insulating coating, by applying it to an electronic circuit, curing it by light irradiation, and forming a cured product, for example, to cover the electronic circuit with the cured product.
Claims
1. A styrene-ethylene, ethylene, propylene-styrene block copolymer having a hydroxy group at one end of the molecular chain; isobornyl (meth)acrylate, a monofunctional saturated branched alkyl (meth)acrylate monomer having a saturated branched hydrocarbon structure and one (meth)acryloyl group in the molecule; 1. A curable composition comprising:
2. The curable composition described in claim 1, wherein the monofunctional saturated branched alkyl (meth)acrylate monomer is at least one of isononyl (meth)acrylate or isodecyl (meth)acrylate.
Citation Information
Patent Citations
Solid curable polymer composition
JP2005506430A
Photocurable primer for ethylenic resin
JP2007002167A
Adhesive composition, adhesive layer and its manufacturing method, and optical member with adhesive attached thereto
JP2008233653A
Curable composition, and film laminate
JP2010077384A
Composition for peeling and peeling method
JP2016011361A