Carbon Fiber Reinforced Composites
A vinyl chloride resin composition with specific copolymers and additives addresses bleed-out and adhesion issues in carbon fiber composites, enhancing flexibility and mechanical properties.
Patent Information
- Application Number
- JP2020149957
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-09-07
- Publication Date
- 2024-09-27
- Estimated Expiration
- 2040-09-07
AI Technical Summary
Carbon fiber reinforced composite materials using vinyl chloride resin face issues such as bleed-out, adhesion to other members, reduced flexibility, and difficulty in impregnation due to high viscosity and proximity to thermal decomposition temperature, which affect impact resistance, productivity, and recyclability.
A carbon fiber reinforced composite material using a vinyl chloride resin composition comprising a copolymer of vinyl chloride monomer with ethylene-vinyl acetate or 2-ethylhexyl (meth)acrylate monomer, with specific weight ratios and additives to enhance flexibility, reduce adhesion, and improve impregnation.
The composite material exhibits increased flexibility, suppresses adhesion, and prevents bleed-out, while offering good impact resistance, productivity, recyclability, flame retardancy, durability, and mechanical strength.
Smart Images

Figure 0007557316000001
Abstract
Description
[Technical Field]
[0001] The present invention relates to a carbon fiber reinforced composite material comprising a vinyl chloride resin composition and a carbon fiber substrate. [Background technology]
[0002] Carbon fiber reinforced composite materials formed from a carbon fiber substrate and a matrix resin have excellent mechanical properties such as strength and elastic modulus, and also have excellent functional properties such as light resistance and chemical resistance. Therefore, carbon fiber reinforced composite materials are used in a variety of applications, such as aircraft structural components, wind turbine blades, and automobile exterior panels. Furthermore, carbon fiber reinforced composite materials formed from a carbon fiber substrate and a soft matrix resin have excellent tensile strength and scratch resistance, and also have excellent design properties, so their use in the automotive industry, such as for automobile instrument panels, and in general industrial fields, such as for belts and key cases, is being considered.
[0003] Known examples of the matrix resin include thermosetting resins such as epoxy resins, which have low viscosity when impregnated into carbon fiber substrates and have excellent adhesion to the carbon fiber substrates.
[0004] On the other hand, in recent years, from the viewpoints of improving impact resistance and productivity, and reducing environmental impact (for example, improving recyclability), development has progressed in which thermoplastic resins such as polyolefins and polyamide-based polymer alloys are used in carbon fiber reinforced composite materials. However, carbon fiber reinforced composite materials containing polyolefins and polyamide-based polymer alloys are inferior in chemical resistance and flame retardancy.
[0005] Thermoplastic resins other than polyolefins and polyamide-based polymer alloys include vinyl chloride resins, which have excellent properties such as flame retardancy, durability, oil resistance, chemical resistance, and mechanical strength, and also have the ability to suppress creep deformation compared to ethylene-based resins and propylene-based resins.
[0006] The following Patent Document 1 discloses a prepreg in which a matrix resin composition containing an epoxy resin, an epoxy resin curing agent, and a vinyl chloride copolymer is impregnated into a carbon fiber substrate. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] Japanese Patent Application Publication No. 2017-095537 Summary of the Invention [Problem to be solved by the invention]
[0008] Regarding vinyl chloride resins, impregnated carbon fiber substrates may bleed out or stick to other components. Furthermore, when vinyl chloride resins and plasticizers are used, the flexibility of the impregnated material may decrease over time due to migration of the plasticizer. Furthermore, the processing temperature when impregnating a carbon fiber substrate with vinyl chloride resin is close to the thermal decomposition temperature of the vinyl chloride resin, making it difficult to impregnate the carbon fiber substrate with vinyl chloride resin. For these reasons, there are various challenges in converting vinyl chloride resins into carbon fiber reinforced composite materials. In Patent Document 1, the thermosetting resin and its curing agent are the main components, and vinyl chloride resin is only included as a secondary component.
[0009] An object of the present invention is to provide a carbon fiber reinforced composite material that is capable of increasing flexibility, suppressing adhesion to other members, and suppressing the occurrence of bleed-out. [Means for solving the problem]
[0010] According to a broad aspect of the present invention, there is provided a carbon fiber reinforced composite material comprising a vinyl chloride resin composition and a carbon fiber substrate, wherein the vinyl chloride resin composition is impregnated into the carbon fiber substrate, and the vinyl chloride resin composition contains a copolymer of a vinyl chloride monomer and an ethylene-vinyl acetate polymer, or a copolymer of a vinyl chloride monomer and a 2-ethylhexyl (meth)acrylate monomer.
[0011] In a specific aspect of the carbon fiber reinforced composite material according to the present invention, in 100% by weight of the copolymer of vinyl chloride monomer and ethylene-vinyl acetate polymer, the content of structural units derived from the vinyl chloride monomer is 50% by weight or more and 80% by weight or less, and the content of structural units derived from the ethylene-vinyl acetate polymer is 20% by weight or more and 50% by weight or less; and in 100% by weight of the copolymer of vinyl chloride monomer and 2-ethylhexyl (meth)acrylate monomer, the content of structural units derived from the vinyl chloride monomer is 50% by weight or more and 80% by weight or less, and the content of structural units derived from the 2-ethylhexyl (meth)acrylate monomer is 20% by weight or more and 50% by weight or less.
[0012] In a specific aspect of the carbon fiber reinforced composite material according to the present invention, the carbon fiber reinforced composite material is a molded body. [Effects of the Invention]
[0013] The carbon fiber reinforced composite material according to the present invention comprises a vinyl chloride resin composition and a carbon fiber substrate, the carbon fiber substrate being impregnated with the vinyl chloride resin composition. In the carbon fiber reinforced composite material according to the present invention, the vinyl chloride resin composition comprises a copolymer of a vinyl chloride monomer and an ethylene-vinyl acetate polymer, or a copolymer of a vinyl chloride monomer and a 2-ethylhexyl (meth)acrylate monomer. Because the carbon fiber reinforced composite material according to the present invention has the above configuration, it is possible to increase flexibility, suppress adhesion to other members, and suppress the occurrence of bleed-out. DETAILED DESCRIPTION OF THE INVENTION
[0014] The present invention will be described in detail below.
[0015] <Carbon fiber reinforced composite materials> The carbon fiber reinforced composite material according to the present invention comprises a vinyl chloride resin composition (A) and a carbon fiber substrate (B). In the carbon fiber reinforced composite material according to the present invention, the carbon fiber substrate (B) is impregnated with the vinyl chloride resin composition (A). In the carbon fiber reinforced composite material according to the present invention, the vinyl chloride resin composition (A) contains a copolymer of a vinyl chloride monomer and an ethylene-vinyl acetate polymer, or a copolymer of a vinyl chloride monomer and a 2-ethylhexyl (meth)acrylate monomer. The carbon fiber reinforced composite material according to the present invention is a carbon fiber reinforced plastic (CFRP).
[0016] Carbon fiber reinforced composite materials using epoxy resins as the matrix resin are inferior in terms of impact resistance, productivity, and recyclability. Carbon fiber reinforced composite materials using polyolefins, polyamide polymer alloys, etc. are inferior in terms of chemical resistance and flame retardancy. Furthermore, when vinyl chloride resins are used as the matrix resin, bleeding and cracking may occur, and adhesion to other components may occur due to high viscosity. Adding a plasticizer to vinyl chloride resins to reduce the viscosity of vinyl chloride resins presents a problem of poor adhesion between the resin composition and the carbon fiber substrate. Furthermore, migration of the plasticizer may result in reduced flexibility. Furthermore, the processing temperature during impregnation of vinyl chloride resins into carbon fiber substrates is close to the thermal decomposition temperature of vinyl chloride resins, making it difficult to impregnate vinyl chloride resins into carbon fiber substrates. For these reasons, there are various challenges associated with converting vinyl chloride resins into carbon fiber reinforced composite materials.
[0017] As a result of extensive research, the present inventors have found that a carbon fiber reinforced composite material having the above-mentioned configuration can solve various problems. Because the carbon fiber reinforced composite material according to the present invention has the above-mentioned configuration, it is possible to increase flexibility, suppress adhesion to other members, and suppress the occurrence of bleed-out. Furthermore, because the carbon fiber reinforced composite material according to the present invention contains the vinyl chloride resin composition (A), it is excellent in impact resistance, productivity, recyclability, flame retardancy, durability, oil resistance, chemical resistance, and mechanical strength, and furthermore, it is possible to suppress creep deformation compared to when an ethylene-based resin or a propylene-based resin is used.
[0018] The carbon fiber reinforced composite material will be described in detail below. In this specification, "(meth)acrylate" means either or both of "acrylate" and "methacrylate," and "(meth)acrylic" means either or both of "acrylic" and "methacrylic."
[0019] (Vinyl chloride resin composition (A)) In the carbon fiber reinforced composite material, the vinyl chloride resin composition (A) contains a copolymer (A-1) of a vinyl chloride monomer and an ethylene-vinyl acetate polymer (hereinafter sometimes referred to as component (A-1)), or a copolymer (A-2) of a vinyl chloride monomer and a 2-ethylhexyl (meth)acrylate monomer (hereinafter sometimes referred to as component (A-2)). The vinyl chloride resin composition (A) contains the component (A-1) or the component (A-2) as a vinyl chloride resin. The vinyl chloride resin composition (A) may contain either the component (A-1) or the component (A-2). The vinyl chloride resin composition (A) may contain both the component (A-1) and the component (A-2).
[0020] The component (A-1) may or may not contain a monomer other than vinyl chloride monomer and ethylene-vinyl acetate polymer as a constituent monomer of the component (A-1). The component (A-1) may have a structural unit different from both the structural unit derived from vinyl chloride monomer and the structural unit derived from ethylene-vinyl acetate polymer. The component (A-2) may or may not contain a monomer other than vinyl chloride monomer and 2-ethylhexyl (meth)acrylate monomer as a constituent monomer of the component (A-2). The component (A-2) may have a structural unit different from both the structural unit derived from vinyl chloride monomer and the structural unit derived from 2-ethylhexyl (meth)acrylate monomer.
[0021] The average degrees of polymerization of the components (A-1) and (A-2) are each preferably 400 or higher, more preferably greater than 400, and even more preferably 500 or higher. The average degrees of polymerization of the components (A-1) and (A-2) are each preferably 1500 or lower, more preferably 800 or lower, and even more preferably 700 or lower. When the average degrees of polymerization of the components (A-1) and (A-2) are equal to or higher than the lower limit, the effects of using a vinyl chloride resin (for example, improved mechanical strength) are more effectively exhibited. When the average degrees of polymerization of the components (A-1) and (A-2) are equal to or lower than the upper limit, the flexibility of the carbon fiber reinforced composite material is further improved.
[0022] The average degree of polymerization is measured as follows: Component (A-1) or (A-2) is dissolved in tetrahydrofuran (THF), and insoluble components are removed by filtration. The THF in the resulting filtrate is removed by drying to obtain a resin. The resulting resin is used as a sample to measure the average degree of polymerization in accordance with JIS K6721, a vinyl chloride resin testing method.
[0023] The complex viscosity (η) of the vinyl chloride resin composition (A) at 200°C and a frequency of 10 Hz is preferably 1 Pa·s or more, more preferably 10 Pa·s or more, even more preferably 20 Pa·s or more, and preferably 1500 Pa·s or less, more preferably 1000 Pa·s or less, and even more preferably 800 Pa·s or less. When the complex viscosity (η) is 1 Pa·s or more, the mechanical strength of the carbon fiber reinforced composite material and the vinyl chloride resin composition (A) can be increased. Furthermore, when the complex viscosity (η) is 1500 Pa·s or less, the vinyl chloride resin composition (A) can be easily impregnated into the interior of the carbon fiber substrate (B), thereby increasing the mechanical strength.
[0024] In 100% by weight of the copolymer (A-1) of the vinyl chloride monomer and ethylene-vinyl acetate polymer, the content of structural units derived from the vinyl chloride monomer is preferably 50% by weight or more, more preferably 55% by weight or more, even more preferably 60% by weight or more, and is preferably 80% by weight or less, more preferably 75% by weight or less, even more preferably 70% by weight or less.
[0025] In 100% by weight of the copolymer (A-1) of vinyl chloride monomer and ethylene-vinyl acetate polymer, the content of structural units derived from the ethylene-vinyl acetate polymer is preferably 20% by weight or more, more preferably 25% by weight or more, even more preferably 30% by weight or more, and preferably 50% by weight or less, more preferably 45% by weight or less, even more preferably 40% by weight or less. When the content of structural units derived from the ethylene-vinyl acetate polymer is equal to or more than the above lower limit and equal to or less than the above upper limit, the flexibility of the carbon fiber reinforced composite material is further improved.
[0026] In 100% by weight of the copolymer (A-2) of the vinyl chloride monomer and the 2-ethylhexyl (meth)acrylate monomer, the content of structural units derived from the vinyl chloride monomer is preferably 50% by weight or more, more preferably 55% by weight or more, even more preferably 60% by weight or more, and is preferably 80% by weight or less, more preferably 75% by weight or less, even more preferably 70% by weight or less.
[0027] In 100% by weight of the copolymer (A-2) of vinyl chloride monomer and 2-ethylhexyl (meth)acrylate monomer, the content of structural units derived from the 2-ethylhexyl (meth)acrylate monomer is preferably 20% by weight or more, more preferably 25% by weight or more, even more preferably 30% by weight or more, and preferably 50% by weight or less, more preferably 45% by weight or less, even more preferably 40% by weight or less. When the content of structural units derived from the 2-ethylhexyl (meth)acrylate monomer is equal to or more than the above lower limit and equal to or less than the above upper limit, the flexibility of the carbon fiber reinforced composite material is further improved.
[0028] The vinyl chloride resin composition (A) impregnated into the carbon fiber substrate (B) may be in a film form or a paste form at 23°C. The paste form includes a liquid form. From the viewpoint of easily impregnating the vinyl chloride resin composition (A) into the carbon fiber substrate (B), the vinyl chloride resin composition (A) is preferably in a paste form. From the viewpoint of improving the handleability of the vinyl chloride resin composition (A), the vinyl chloride resin composition (A) is preferably in a film form. The film-like vinyl chloride resin composition (A) can be melted by heating and impregnated into the carbon fiber substrate (B).
[0029] To effectively achieve the effects of the present invention, the total content of the components (A-1) and (A-2) in 100% by weight of the vinyl chloride resin composition (A) is preferably 20% by weight or more, more preferably 25% by weight or more, even more preferably 30% by weight or more, and preferably 50% by weight or less, more preferably 45% by weight or less, and even more preferably 40% by weight or less. When the vinyl chloride resin composition (A) contains the component (A-1) but does not contain the component (A-2), the total content of the components (A-1) and (A-2) refers to the content of the component (A-1). When the vinyl chloride resin composition (A) does not contain the component (A-1) but does contain the component (A-2), the total content of the components (A-1) and (A-2) refers to the content of the component (A-2).
[0030] From the viewpoint of effectively exerting the effects of the present invention, the content of the vinyl chloride resin composition (A) in 100% by weight of the carbon fiber reinforced composite material is preferably 50% by weight or more, more preferably 55% by weight or more, even more preferably 60% by weight or more, and is preferably 80% by weight or less, more preferably 75% by weight or less, even more preferably 70% by weight or less.
[0031] (additives) The vinyl chloride resin composition (A) may contain additives. Examples of the additives include heat stabilizers, heat stabilization aids, lubricants, processing aids, impact modifiers, heat resistance improvers, antioxidants, ultraviolet absorbers, antistatic agents, light stabilizers, fillers, pigments, plasticizers, and flame retardants. The additives may be used alone or in combination of two or more. From the viewpoints of further suppressing deterioration in physical properties due to bleed-out and further suppressing adhesion to other components, it is preferable that the vinyl chloride resin composition (A) does not contain a plasticizer.
[0032] The heat stabilizer is not particularly limited. Examples of the heat stabilizer include organotin-based stabilizers, lead-based stabilizers, calcium-zinc-based stabilizers, barium-zinc-based stabilizers, and barium-cadmium-based stabilizers. Examples of the organotin-based stabilizers include methyltin mercapto, dibutyltin mercapto, dioctyltin mercapto, dimethyltin mercapto, dibutyltin mercapto, dibutyltin maleate, dibutyltin maleate polymer, dioctyltin maleate, dioctyltin maleate polymer, dibutyltin laurate, and dibutyltin laurate polymer. The heat stabilizers may be used alone or in combination of two or more.
[0033] The heat stabilization aid is not particularly limited. Examples of the heat stabilization aid include epoxidized soybean oil, phosphate ester, polyol, hydrotalcite, and zeolite. The heat stabilization aid may be used alone or in combination of two or more.
[0034] The lubricant is not particularly limited. Examples of the lubricant include internal lubricants and external lubricants. The internal lubricant is used to reduce the flow viscosity of the molten resin during molding and prevent frictional heat generation. Examples of the internal lubricant include butyl stearate, lauryl alcohol, stearyl alcohol, epoxy soybean oil, glycerin monostearate, stearic acid, and bisamide. The external lubricant is used to improve the sliding effect between the molten resin and the metal surface during molding. Examples of the external lubricant include paraffin wax, polyolefin wax, ester wax, and montanic acid wax. The lubricant may be used alone or in combination of two or more. An internal lubricant and an external lubricant may be used in combination.
[0035] The processing aid is not particularly limited. Examples of the processing aid include homopolymers or copolymers of alkyl methacrylates such as methyl methacrylate, ethyl methacrylate, and butyl methacrylate; copolymers of alkyl methacrylates and alkyl acrylates such as methyl acrylate, ethyl acrylate, and butyl acrylate; copolymers of alkyl methacrylates and aromatic vinyl compounds such as styrene, α-methylstyrene, and vinyltoluene; and copolymers of alkyl methacrylates and vinyl cyan compounds such as acrylonitrile and methacrylonitrile. Only one type of processing aid may be used, or two or more types may be used in combination. From the viewpoint of further improving processability, the processing aid is preferably a copolymer of alkyl methacrylate and alkyl acrylate, and more preferably a copolymer of alkyl methacrylate and alkyl acrylate having a weight average molecular weight of 100,000 to 2,000,000. Examples of the copolymer of alkyl methacrylate and alkyl acrylate having a weight average molecular weight of 100,000 or more and 2,000,000 or less include an n-butyl acrylate-methyl methacrylate copolymer and a 2-ethylhexyl acrylate-methyl methacrylate-butyl methacrylate copolymer.
[0036] The impact modifier is not particularly limited. Examples of the impact modifier include polybutadiene, polyisoprene, polychloroprene, chlorinated polyethylene, fluororubber, styrene-butadiene copolymer rubber, methyl methacrylate-butadiene-styrene copolymer, methyl methacrylate-butadiene-styrene graft copolymer, acrylonitrile-styrene-butadiene copolymer rubber, acrylonitrile-styrene-butadiene graft copolymer, styrene-butadiene-styrene block copolymer rubber, styrene-isoprene-styrene copolymer rubber, styrene-ethylene-butylene-styrene copolymer rubber, ethylene-propylene copolymer rubber, ethylene-propylene-diene copolymer rubber (EPDM), silicone-containing acrylic rubber, silicone / acrylic composite rubber graft copolymer, and silicone rubber. The impact modifier may be used alone or in combination of two or more.
[0037] The heat resistance improver is not particularly limited. Examples of the heat resistance improver include α-methylstyrene-based and N-phenylmaleimide-based resins. The heat resistance improver may be used alone or in combination of two or more.
[0038] The antioxidant is not particularly limited. Examples of the antioxidant include phenolic antioxidants such as 4,4'-butylidenebis-(6-t-butyl-3-methylphenol), phosphite antioxidants such as tris(mixed mono- and di-nonylphenyl)phosphite, and thioether antioxidants such as distearyl thiodipropionate. As the antioxidant, phenolic antioxidants such as 4,4'-butylidenebis-(6-t-butyl-3-methylphenol) are particularly preferred because they have a low high-temperature decomposition inhibitory function. The antioxidants may be used alone or in combination of two or more.
[0039] The ultraviolet absorber is not particularly limited. Examples of the ultraviolet absorber include salicylic acid ester-based ultraviolet absorbers, benzophenone-based ultraviolet absorbers, benzotriazole-based ultraviolet absorbers, and cyanoacrylate-based ultraviolet absorbers. The ultraviolet absorbers may be used alone or in combination of two or more.
[0040] The antistatic agent is not particularly limited. Examples of the antistatic agent include anionic surfactants, cationic surfactants, nonionic surfactants, and amphoteric surfactants. Examples of the anionic surfactants include fatty acid salts, higher alcohol sulfate ester salts, liquid fatty oil sulfate ester salts, fatty amine and amide sulfate salts, dibasic fatty acid ester sulfonic acid salts, fatty acid amide sulfonic acid salts, alkylaryl sulfonic acid salts, formalin condensation naphthalene sulfonic acid salts, and mixtures thereof. Examples of the cationic surfactants include fatty amine salts, quaternary ammonium salts, alkylpyridinium salts, and mixtures thereof. Examples of the nonionic surfactants include polyoxyethylene alkyl ethers, polyoxyethylene alkylphenol esters, polyoxyethylene alkyl esters, sorbitan alkyl esters, polyoxyethylene sorbitan alkyl esters, and mixtures thereof. Mixtures of the nonionic surfactants with anionic surfactants or cationic surfactants are also acceptable. Examples of the amphoteric surfactant include imidazoline type, higher alkylamino type (betaine type), sulfate ester type, phosphate ester type, sulfonic acid type, etc. The antistatic agent may be used alone or in combination of two or more types.
[0041] The light stabilizer is not particularly limited. Examples of the light stabilizer include hindered amine light stabilizers. The light stabilizers may be used alone or in combination of two or more.
[0042] The filler is not particularly limited. Examples of the filler include carbonates such as talc, heavy calcium carbonate, precipitated calcium carbonate, and colloidal calcium carbonate, inorganic substances such as aluminum hydroxide, magnesium hydroxide, titanium oxide, clay, mica, wollastonite, zeolite, silica, zinc oxide, magnesium oxide, carbon black, graphite, glass beads, glass fiber, carbon fiber, and metal fiber, and organic fibers such as polyamide. The fillers may be used alone or in combination of two or more.
[0043] The pigment is not particularly limited. Examples of the pigment include organic pigments and inorganic pigments. Examples of the organic pigments include azo-based organic pigments, phthalocyanine-based organic pigments, threne-based organic pigments, and dye lake-based organic pigments. Examples of the inorganic pigments include oxide-based inorganic pigments, molybdenum chromate-based inorganic pigments, sulfide-selenide-based inorganic pigments, and ferrocyanide-based inorganic pigments. The pigments may be used alone or in combination of two or more.
[0044] Examples of the flame retardant include metal hydroxides, bromine compounds, triazine ring-containing compounds, zinc compounds, phosphorus compounds, halogen-based flame retardants, silicone-based flame retardants, intumescent flame retardants, antimony oxide, etc. The flame retardants may be used alone or in combination of two or more.
[0045] The content of additives (components other than vinyl chloride resin) in 100% by weight of the vinyl chloride resin composition (A) is preferably 5% by weight or less, more preferably 3% by weight or less. When the content of the additives in the vinyl chloride resin composition (A) is not more than the above upper limit, the additives in the vinyl chloride resin composition (A) can be prevented from seeping out near the interface between the vinyl chloride resin composition (A) and the carbon fiber substrate (B), resulting in further improved flexibility. The lower limit of the content of the additives in the vinyl chloride resin composition (A) is not particularly limited. The content of the additives in the vinyl chloride resin composition (A) may be 0% by weight (unused), may exceed 0% by weight, or may be 1% by weight or more.
[0046] (Carbon fiber substrate (B)) In the carbon fiber reinforced composite material according to the present invention, the vinyl chloride resin composition (A) is impregnated into the carbon fiber substrate (B). The carbon fiber substrate refers to, for example, a carbon fiber material in which carbon fiber bundles (filaments) made of a plurality of carbon fibers are incorporated as warp bundles and weft bundles.
[0047] Examples of the carbon fiber include PAN (polyacrylonitrile)-based carbon fiber and PITCH-based carbon fiber. From the viewpoint of effectively increasing mechanical strength, the carbon fiber is preferably PAN (polyacrylonitrile)-based carbon fiber. In the carbon fiber substrate (B), the carbon fiber may be used in combination with fibers other than carbon fiber. The material of the carbon fiber substrate (B) may contain fibers other than carbon fiber. Examples of the fibers other than carbon fiber include metal fibers, inorganic fibers, organic fibers, and natural fibers. Examples of the metal fibers include steel fibers. Examples of the inorganic fibers include glass fibers, ceramic fibers, and boron fibers. Examples of the organic fibers include aramid fibers, polyester fibers, polyethylene fibers, nylon fibers, vinylon fibers, polyacetal fibers, polyparaphenylenebenzoxazole fibers, and polypropylene fibers. Examples of the natural fibers include cotton fibers, hemp fibers, wool fibers, and silk fibers. From the viewpoint of increasing mechanical strength, the material of the carbon fiber bundle is preferably carbon fiber only. From the viewpoint of increasing the mechanical strength, the material of the carbon fiber base material (B) is preferably carbon fiber alone.
[0048] The carbon fiber substrate (B) is preferably a woven carbon fiber fabric, a knitted carbon fiber fabric, or a nonwoven carbon fiber fabric. As the carbon fiber substrate (B), only one of the woven carbon fiber fabric, the knitted carbon fiber fabric, and the nonwoven carbon fiber fabric may be used, or two or more of them may be used in combination. From the viewpoint of effectively increasing the mechanical strength, the carbon fiber substrate (B) is preferably a woven carbon fiber fabric or a knitted carbon fiber fabric, and more preferably a woven carbon fiber fabric. The woven fiber substrate is preferably a plain weave or twill weave fabric.
[0049] The carbon fiber substrate (B) is preferably in the form of a flat sheet. The carbon fiber substrate (B) is preferably a carbon fiber sheet. The surface of the carbon fiber substrate (B) may have a pattern, or may have a design drawn thereon by dyeing or the like.
[0050] The carbon fibers are further classified into continuous carbon fibers and discontinuous carbon fibers based on the fiber morphology. The discontinuous carbon fibers are classified, for example, into short carbon fibers having a fiber length of 1 mm or less and long carbon fibers having a fiber length of more than 1 mm and 5 cm or less. From the viewpoint of improving the functional properties of the carbon fiber reinforced composite material, such as light resistance and chemical resistance, the carbon fibers are preferably continuous carbon fibers.
[0051] Examples of the form of continuous carbon fiber include: A form in which continuous carbon fibers are aligned in one direction; A form in which continuous carbon fibers are woven in the warp and weft directions (cross); A form in which carbon fiber bundles (filaments) are bundled to form a tow; A form in which the tows are aligned in one direction and held together with auxiliary weft threads; A form in which multiple carbon fiber sheets in which continuous carbon fibers are aligned in one direction are stacked so that the carbon fibers are oriented in different directions and stitched together with auxiliary threads (multiaxial warp knit). The carbon fiber substrate (B) is preferably formed from carbon fiber bundles (filaments) made of continuous carbon fibers in the above forms.
[0052] From the viewpoint of improving the impregnation of the vinyl chloride resin composition (A) into the carbon fiber substrate (B), the material of the carbon fiber substrate (B) is preferably a carbon fiber bundle that has been subjected to an opening treatment (hereinafter, sometimes referred to as an opened carbon fiber bundle). Examples of the opening treatment method include a method of incorporating spacer particles, a method of squeezing the carbon fibers with a round rod, a method using an airflow, and a method of vibrating the carbon fibers with ultrasound or the like. The method of opening the carbon fiber bundle is preferably a method of incorporating spacer particles. If the carbon fiber bundle is opened by the method of incorporating spacer particles and the interfiber distance is increased in advance, the interfiber distance will not narrow even if high tension is applied to the carbon fibers during the production stage, and the impregnation of the vinyl chloride resin composition (A) into the carbon fiber substrate (B) will be improved.
[0053] The carbon fiber bundle (filament) is a bundle of a plurality of carbon fibers. The carbon fiber is generally a single fiber. The number of carbon fibers constituting the carbon fiber bundle (filament) is preferably 1,000 or more, more preferably 2,000 or more, and even more preferably 5,000 or more, and is preferably 50,000 or less, more preferably 40,000 or less, and even more preferably 25,000 or less. When the number of carbon fibers constituting the carbon fiber bundle (filament) is equal to or more than the above lower limit and equal to or less than the above upper limit, the mechanical strength and impregnation property can be effectively improved.
[0054] The fiber diameter of the carbon fiber bundle (filament) is preferably 3 μm or more, and preferably 12 μm or less. When the fiber diameter of the carbon fiber bundle (filament) is equal to or more than the lower limit, the mechanical strength and impregnation property can be effectively improved. Specifically, for example, when the carbon fiber bundle (filament) moves laterally on the surface of a roll, spool, or the like in various processing processes, the occurrence of breakage and accumulation of fluff can be suppressed. When the fiber diameter of the carbon fiber bundle (filament) is equal to or less than the upper limit, the production of the carbon fiber base material (B) becomes easy.
[0055] Although not particularly limited, the plurality of carbon fiber bundles (filaments) are preferably formed into a sheet. The basis weight of the sheet-shaped carbon fiber bundles (filaments) is preferably 100 g / m 2 More preferably, 150 g / m 2 More than 600g / m 2 Less than 500 g / m 2 When the basis weight is equal to or greater than the lower limit, the work efficiency can be improved when the obtained carbon fiber reinforced composite material is laminated and subjected to secondary processing. When the basis weight is equal to or less than the upper limit, the impregnation of the vinyl chloride resin composition (A) into the carbon fiber base material (B) becomes good.
[0056] From the viewpoint of effectively increasing the mechanical strength and impregnation property, the density of the carbon fibers is preferably 1 fiber / inch or more, more preferably 2 fibers / inch or more, and is preferably 50 fibers / inch or less, more preferably 20 fibers / inch or less.
[0057] From the viewpoint of effectively increasing the mechanical strength and impregnation property, the thickness of the carbon fiber base material (B) is preferably 0.2 mm or less, more preferably 0.15 mm or less, even more preferably 0.1 mm or less, and particularly preferably 0.05 mm or less.
[0058] From the viewpoint of effectively exerting the effects of the present invention, the content of the carbon fiber base material (B) in 100% by weight of the carbon fiber reinforced composite material is preferably 20% by weight or more, more preferably 25% by weight or more, even more preferably 30% by weight or more, and is preferably 60% by weight or less, more preferably 55% by weight or less, even more preferably 50% by weight or less.
[0059] (Other details of carbon fiber reinforced composite materials) The carbon fiber reinforced composite material according to the present invention may be a molded body. The molded body can be obtained by molding the carbon fiber reinforced composite material before molding. Furthermore, when obtaining the carbon fiber reinforced composite material, the carbon fiber reinforced composite material may be made into a molded body. When obtaining the carbon fiber reinforced composite material, a molded body having a predetermined shape may be obtained.
[0060] The shape of the molded body is not particularly limited, and can be any shape appropriate for the application.
[0061] When the carbon fiber reinforced composite material according to the present invention is heated at 150° C. for 4 hours, the weight change rate is preferably 2% by weight or less.
[0062] In the molded article, the carbon fiber substrate (B) impregnated with the vinyl chloride resin composition (A) may be laminated in a plurality of layers. In this case, by laminating the carbon fiber substrates (B) so that the carbon fiber directions of the carbon fiber substrates (B) are different at a certain angle, a molded article having the above-mentioned multiaxial warp knit form can be obtained.
[0063] (Method of manufacturing carbon fiber reinforced composite materials) The carbon fiber reinforced composite material according to the present invention can be produced, for example, by the following method.
[0064] The vinyl chloride resin composition (A) is prepared. The vinyl chloride resin composition (A) is preferably in the form of a film. The vinyl chloride resin composition (A) may contain the additives described above.
[0065] Next, the carbon fiber base material (B) is prepared. It is preferable to use a carbon fiber bundle that has been subjected to an opening treatment (opened carbon fiber bundle) as a material for the carbon fiber base material (B). The manufacturing method for the carbon fiber base material (B) preferably comprises a step of opening the carbon fiber bundle. The method of opening the carbon fiber bundle is preferably a method of impregnating the carbon fiber bundle with spacer particles. Examples of the method of impregnating the spacer particles include a method of contacting the carbon fiber bundle with an opening impregnation liquid containing spacer particles. It is preferable that the step of opening the carbon fiber bundle comprises a step of contacting the carbon fiber bundle with an opening impregnation liquid and a step of heating the carbon fiber bundle that has been contacted with the opening impregnation liquid.
[0066] The fiber-opening impregnation liquid preferably contains spacer particles and a monomer capable of forming a resin. The fiber-opening impregnation liquid may be prepared by mixing the monomer and the spacer particles, or by dissolving the monomer in a solvent and then mixing it with the spacer particles. The fiber-opening impregnation liquid is preferably prepared by dissolving the monomer in a solvent and then mixing it with the spacer particles.
[0067] The monomers react to form a resin, which is preferably an oxazine-based resin or an acrylic-based resin.
[0068] The spacer particles may be organic particles or inorganic particles, but from the viewpoint of further enhancing flexibility, the spacer particles are preferably organic particles.
[0069] By using the fiber-opening impregnation liquid, the carbon fiber bundles are sufficiently opened by the spacer particles. Therefore, the compatibility between the vinyl chloride resin composition (A) and the carbon fiber substrate (B) is improved, and the vinyl chloride resin composition (A) is impregnated into the carbon fiber substrate (B) in an appropriate amount, resulting in good resin impregnation. Furthermore, when the carbon fibers are bridged by the spacer particles and the spacer particles are adhered to the carbon fibers, the opened state of the carbon fiber bundles is maintained even when pressure or the like is applied. Therefore, even when the carbon fiber substrate (B) is impregnated with the vinyl chloride resin composition (A) by applying heat and pressure, for example, the opened state of the carbon fiber bundles of the carbon fiber substrate (B) is sufficiently maintained, resulting in good resin impregnation. Furthermore, the resulting carbon fiber-reinforced composite material has excellent mechanical strength due to the appropriate impregnation with the vinyl chloride resin composition (A).
[0070] The fiber-opening impregnation liquid preferably contains a solvent. The solvent is preferably one that can dissolve the monomer. The solvent is not particularly limited, but examples thereof include alcohol, water, tetrahydrofuran, dioxane, and dimethylformamide. Examples of the alcohol include methanol and ethanol. The solvent may be used alone or in combination of two or more.
[0071] Next, the carbon fiber bundles are brought into contact with the obtained fiber-opening impregnation liquid. By bringing the carbon fiber bundles into contact with the fiber-opening impregnation liquid, the spacer particles enter the gaps between the carbon fibers of the carbon fiber bundles, opening the carbon fiber bundles.
[0072] Next, the carbon fiber bundles that have been brought into contact with the fiber-opening impregnation liquid are heated. The heating polymerizes the monomer to produce a resin such as naphthoxazine resin or acrylic resin, which coats the spacer particles. The spacer particles can be bonded to and cross-linked between the carbon fibers by the resin. Thereafter, the resin may be carbonized by further heating to obtain spacer particles coated with a carbon allotrope. The spacer particles coated with a carbon allotrope (coated particles) preferably form a structure that bridges between the carbon fibers. Furthermore, the carbon allotrope coating the spacer particles may be adhered to the carbon fibers. Furthermore, the carbon allotrope may coat the surface of the carbon fibers, or a structure may be formed in which the carbon allotrope on the surface of the coating particle and the carbon allotrope coating the carbon fibers are connected to each other.
[0073] The obtained carbon fiber substrate (B) is impregnated with the vinyl chloride resin composition (A), thereby obtaining a carbon fiber reinforced composite material. The method for impregnating the vinyl chloride resin composition (A) is not particularly limited, and any conventionally known method can be used as this method. Specific examples include the following methods: A method in which the film-like vinyl chloride resin composition (A) is superimposed on the carbon fiber substrate (B) and hot press molded; and A method in which the vinyl chloride resin composition (A) is melt extrusion molded onto the carbon fiber substrate (B).
[0074] For the hot press molding, extrusion molding or press molding can be used. By using a molding die, a carbon fiber reinforced composite material of a desired shape can be obtained. The hot press molding is preferably carried out at a temperature equal to or higher than the thermal decomposition temperature of the vinyl chloride resin composition (A) used.
[0075] Next, the present invention will be clarified by showing specific examples and comparative examples of the present invention, but the present invention is not limited to the following examples.
[0076] The following materials were prepared:
[0077] PVC resin: Vinyl chloride resin (1) (Tokuyama Sekisui Kogyo Co., Ltd. "TG40", degree of polymerization: 640, copolymer of vinyl chloride monomer and ethylene-vinyl acetate polymer, content of structural units derived from vinyl chloride monomer: 60% by weight, content of structural units derived from ethylene-vinyl acetate polymer: 40% by weight) Vinyl chloride resin (2) (a copolymer of "TS640M" (polymerization degree: 640) manufactured by Tokuyama Sekisui Kogyo Co., Ltd.) and 2-ethylhexyl acrylate monomer, the content of structural units derived from vinyl chloride monomer: 70% by weight, the content of structural units derived from 2-ethylhexyl acrylate monomer: 30% by weight) Vinyl chloride resin A (Tokuyama Sekisui Kogyo Co., Ltd. "SLP40", polymerization degree: 400)
[0078] Plasticizer: Dioctyl phthalate ("DOP" manufactured by J-Plus)
[0079] Heat stabilizer: Methyltin mercapto (Nitto Kasei "AT5300", liquid at 23°C)
[0080] Example 1 (Preparation of vinyl chloride resin composition (A)) A blend was obtained by adding 0.5 parts by weight of methyltin mercapto to 100 parts by weight of vinyl chloride resin (1). The blend was completely dissolved in tetrahydrofuran (THF) to a concentration of 10% by weight to obtain a solution. The resulting solution was spread on a glass plate using a coater, and the THF was removed by drying to obtain a resin film (vinyl chloride resin composition (A)) with a thickness of 80 μm to 100 μm.
[0081] (Preparation of carbon fiber substrate (B)) A monomer solution was prepared by uniformly mixing monomer components containing 10 parts by weight of 1,5-dihydroxynaphthalene, 4 parts by weight of 40% methylamine aqueous solution, and 8 parts by weight of formalin (formaldehyde content: 37% by weight) with 800 parts by weight of an ethanol aqueous solution (ethanol content: 50% by weight) as a solvent. 10 parts by weight of divinylbenzene cross-linked polymer particles (Micropearl SP, manufactured by Sekisui Chemical Co., Ltd., average particle size: 10 μm) were added to the above monomer solution as spacer particles to prepare a fiber-opening impregnation solution.
[0082] In addition, a carbon fiber fabric consisting of PAN-based carbon fiber bundles (number of carbon fibers: 3000, average fiber diameter of carbon fiber bundles: 7 μm, basis weight: 200 g / m) 2 A carbon fiber woven fabric (thickness: 0.19 mm, plain weave) was prepared. The carbon fiber woven fabric was immersed in the above-mentioned fiber-spreading impregnation solution, then pulled out, and then heated at 200°C for 2 minutes. This heating caused the polymerization reaction of the naphthoxazine resin to proceed, resulting in carbonization and the generation of amorphous carbon (carbon allotrope) derived from the naphthoxazine resin, and a woven fabric of spread carbon fiber bundles was obtained. The obtained woven fabric of spread carbon fiber bundles was used as carbon fiber substrate (B). The amount of spacer particles (coated particles) coated with the carbon allotrope in the carbon fiber substrate (B) was 1% by weight.
[0083] (Production of carbon fiber reinforced composite materials) The obtained carbon fiber substrate (B) was placed between two of the above-mentioned resin films, sandwiched between the above-mentioned resin films from above and below, and pressed for a total of about 10 minutes at 200°C under stepwise pressures of 0 MPa to 6 MPa. In this way, a carbon fiber reinforced composite material (molded product) including the vinyl chloride resin composition (A) and the carbon fiber substrate (B) impregnated with the vinyl chloride resin composition (A) was obtained.
[0084] Example 2 A carbon fiber reinforced composite material was produced in the same manner as in Example 1, except that the vinyl chloride resin (2) was used instead of the vinyl chloride resin (1).
[0085] (Comparative Examples 1 and 2) Carbon fiber reinforced composite materials were produced in the same manner as in Example 1, except that vinyl chloride resin A was used instead of vinyl chloride resin (1) and dioctyl phthalate was added in the amounts shown in Table 1 below.
[0086] (evaluation) (1) Adhesion (tack test) The obtained carbon fiber reinforced composite material was cut into a size of 50 mm length x 50 mm width to prepare two test samples A.
[0087] A polypropylene film (hereinafter sometimes referred to as PP film) measuring 60 mm in length and 80 mm in width was placed on one of the test samples A, and a 50 g weight (pressure 43 Pa) was placed on the PP film (test piece 1).
[0088] A PP film measuring 60 mm in length and 80 mm in width was placed on the other test sample A, and a weight of 800 g (pressure 694 Pa) was placed on the PP film (test piece 2).
[0089] For each of specimens 1 and 2, a weight was placed on the specimen, and the specimen was left to stand for 10 seconds before the weight was removed. After the weight was removed, both ends of the PP film on each of specimens 1 and 2 were slowly lifted upward to observe whether test sample A was lifted up along with the PP film. For both specimens with a weight of 50 g (pressure 43 Pa) and 800 g (pressure 694 Pa), the adhesion of the carbon fiber reinforced composite material was evaluated according to the following criteria.
[0090] [Criteria for determining adhesiveness] ○: Test sample A does not lift up together with the PP film ×: Test sample A is lifted up together with the PP film
[0091] (2) Flexibility (shore test) The obtained carbon fiber reinforced composite material was cut into a size of 20 mm length x 20 mm width, and 10 to 15 pieces were stacked together to prepare a test sample B with a thickness of approximately 60 mm. The Shore hardness was measured using a durometer (type A indenter, pressing load 10 N). The lower of the Shore hardnesses of Comparative Examples 1 and 2 was designated as the standard hardness, and the flexibility of the Examples was evaluated according to the following criteria.
[0092] [Flexibility criteria] ○: Shore hardness is less than STD ×: Shore hardness is equal to or greater than STD
[0093] (3) Bleed-out resistance (bleed test) The obtained carbon fiber reinforced composite material was cut into a size of 50 mm length x 50 mm width to prepare a test sample C.
[0094] Immediately after preparation, the test sample C was heated in an oven at 100°C for 2 hours, and the weight (1) of the test sample C after pre-drying was measured. It was then heated at 150°C for 4 hours, and the weight (2) of the test sample C after heating was measured. The weight change rate was calculated using the following formula, and the bleed-out resistance was evaluated according to the following criteria. Note that the lower the weight change rate (wt%), the higher the bleed-out resistance and the more the occurrence of bleed-out is suppressed.
[0095] Weight change rate (weight%) = ((weight (1) - weight (2)) / weight (1)) x 100
[0096] [Criteria for bleed-out resistance] ○: The weight change rate is 2% by weight or less ×: Weight change rate exceeds 2% by weight
[0097] The results are shown in Table 1 below.
[0098] [Table 1]
Claims
1. A vinyl chloride resin composition and a carbon fiber substrate, The vinyl chloride resin composition is impregnated into the carbon fiber substrate, The vinyl chloride resin composition contains a copolymer of a vinyl chloride monomer and an ethylene-vinyl acetate polymer, or a copolymer of a vinyl chloride monomer and a 2-ethylhexyl (meth)acrylate monomer; A carbon fiber reinforced composite material, wherein the carbon fiber substrate is a carbon fiber bundle opened by spacer particles.
2. A carbon fiber reinforced composite material as described in claim 1, wherein the spacer particles are spacer particles coated with a carbon allotrope.
3. a content of structural units derived from the vinyl chloride monomer is 50% by weight or more and 80% by weight or less, and a content of structural units derived from the ethylene-vinyl acetate polymer is 20% by weight or more and 50% by weight or less, based on 100% by weight of the copolymer of the vinyl chloride monomer and the ethylene-vinyl acetate polymer; 3. The carbon fiber reinforced composite material according to claim 1, wherein, in 100% by weight of the copolymer of the vinyl chloride monomer and the 2-ethylhexyl (meth)acrylate monomer, the content of structural units derived from the vinyl chloride monomer is 50% by weight or more and 80% by weight or less, and the content of structural units derived from the 2-ethylhexyl (meth)acrylate monomer is 20% by weight or more and 50% by weight or less.
4. The carbon fiber reinforced composite material according to any one of claims 1 to 3, which is a molded product.
Citation Information
Patent Citations
Reinforced fiber resin composite and method for producing structure reinforced using the same
JP2016030822A
Prepreg, method for producing prepreg and carbon fiber-reinforced composite material
JP2017095537A
Polyvinyl chloride resin composition and polyvinyl chloride resin sheet
JP2017132999A
Fiber-reinforced composite material, and method for manufacturing the same
JP2020055310A
Fiber reinforced polyvinyl chloride and copolyester compositions and articles made using these compositions
US20180371225A1