Cellulose acetate and cellulose acetate compositions
By optimizing the acetyl substitution and sulfuric acid content in cellulose acetate and incorporating biodegradable additives, the compositions achieve enhanced biodegradability in seawater, addressing the degradation challenges of conventional cellulose acetate.
Patent Information
- Application Number
- JP2022130695
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2022-08-18
- Publication Date
- 2024-09-27
- Estimated Expiration
- 2039-12-09
AI Technical Summary
Conventional cellulose acetate exhibits poor biodegradability in seawater due to the lower content of fungi and bacteria, making it difficult to degrade in this environment.
Cellulose acetate compositions with a total degree of acetyl substitution of 2.7 or less, a ratio τ of the sum of the degree of acetyl substitution at the 2nd and 3rd positions to the 6th position of 2.0 or more, and a sulfuric acid component between 20 ppm and 400 ppm, along with additives that enhance biodegradability, such as magnesium oxide and triacetin, are used to improve biodegradability in seawater.
The cellulose acetate compositions demonstrate excellent biodegradability in seawater, with improved degradation rates and reduced environmental impact.
Smart Images

Figure 0007557505000001
Abstract
Description
[Technical field]
[0001] The present invention relates to cellulose acetate and cellulose acetate compositions. [Background technology]
[0002] In recent years, various studies have been conducted on biodegradable resins that are easily decomposed in environments such as compost, rivers, oceans, and soil. A representative biodegradable resin is cellulose acetate. Cellulose acetate is advantageous in that it can be obtained from natural materials such as wood and cotton, which do not compete with food or feed.
[0003] In Non-Patent Document 1, the number of viable bacteria in PM medium under freshwater conditions of 0.5% (0.08M) NaCl and seawater conditions of 3% (0.5M) NaCl, and the identified bacterial phase of the isolated bacteria were investigated. As a result, the number of viable bacteria in freshwater conditions was 2.6 x 10 7 cells / ml, and 9.7×10 5 It has been reported that the viable cell count was 3.7% of that in freshwater.
[0004] Patent Document 1 states that "it has been found that polymer compositions containing at least one basic additive, wherein the at least one basic additive has a pH of 13 or less and 7 or more when measured in a 1 wt % aqueous solution at 20° C., exhibit improved biodegradability over compositions not containing the at least one additive," and discloses cellulose acetate as the polymer.
[0005] Patent Document 2 describes the following. In a cellulose acetate optical film that exhibits optical properties by being stretched, a cellulose acetate is obtained that has excellent stretchability and excellent optical properties after being stretched. The present invention provides a cellulose diacetate for retardation films, which has a total degree of acetyl group substitution of 2.27 to 2.56, a polydispersity Mw / Mn of more than 3.0 and not more than 7.5, a degree of substitution at the 6-position of 0.65 to 0.85, a half-width of the acetylation degree distribution of 1.0 to 2.3, and a viscosity-average degree of polymerization of 182 or more and 213 or less. The cellulose diacetate for retardation films of the present invention preferably has a 6% viscosity of 120 to 230 mPa·s, and a weight-average molecular weight Mw of 205,000 or more and 235,000 or less. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] International Publication No. 2016 / 092024 [Patent Document 2] International Publication No. 2011 / 093216 [Non-patent literature]
[0007] [Non-Patent Document 1] Eiji Ishii et al., Life Sciences, 1983, Vol. 27, No. 3, p. 111-118 Summary of the Invention [Problem to be solved by the invention]
[0008] However, conventional cellulose acetate did not have sufficient degradability in seawater. This is because, as can be seen from Non-Patent Document 1, seawater contains less fungi and bacteria than soil and freshwater such as river water, making it an environment in which biodegradation is difficult. In other words, the proportion of bacteria, fungi, etc. that contribute to biodegradation is low, and as a result, biodegradation in seawater is difficult.
[0009] An object of the present invention is to provide a cellulose acetate having excellent biodegradability in seawater. [Means for solving the problem]
[0010] A first aspect of the present disclosure relates to a cellulose acetate having a total degree of acetyl substitution of 2.7 or less, a ratio τ of the sum of the degrees of acetyl substitution at the 2-position and the 3-position to the degree of acetyl substitution at the 6-position in the total degree of acetyl substitution of 2.0 or more, and an amount of sulfuric acid component of more than 20 ppm to 400 ppm or less.
[0011] In the cellulose acetate, the amount of the sulfuric acid component is preferably 80 ppm or more and 380 ppm or less.
[0012] In the cellulose acetate, the amount of the sulfuric acid component is preferably 150 ppm or more and 350 pm or less.
[0013] In the cellulose acetate, it is preferable that the ratio τ of the sum of the degrees of acetyl substitution at the 2-position and the 3-position to the degree of acetyl substitution at the 6-position in the total degree of acetyl substitution is 2.5 or less.
[0014] A second aspect of the present disclosure relates to a cellulose acetate composition comprising cellulose acetate and an additive, wherein the cellulose acetate has a total degree of acetyl substitution of 2.7 or less, and a ratio τ of the sum of the degrees of acetyl substitution at the 2nd position and the 3rd position to the degree of acetyl substitution at the 6th position in the total degree of acetyl substitution of 2.0 or more, and the additive is one or more selected from the group consisting of substances having a pH of 8 or more in a 1 wt % aqueous solution at 20° C., substances soluble in water at 20° C. at 2 wt % or more, and substances having excellent biodegradability in the ocean.
[0015] In the cellulose acetate composition, the amount of sulfuric acid in the cellulose acetate is preferably more than 20 ppm and not more than 400 ppm.
[0016] In the cellulose acetate composition, the content of the additive is preferably 5 to 40% by weight.
[0017] In the cellulose acetate composition, the substance having a pH of 8 or more in a 1 wt % aqueous solution at 20° C. is preferably magnesium oxide.
[0018] In the cellulose acetate composition, the substance that dissolves in water at 20° C. to a concentration of 2% by weight or more is preferably triacetin.
[0019] In the cellulose acetate composition, a slurry obtained by mixing with water preferably has a pH of 7 to 13 at 20°C. Effect of the Invention
[0020] According to the present invention, it is possible to provide cellulose acetate having excellent biodegradability in seawater. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0021] [Cellulose acetate] The cellulose acetate of the present disclosure has a total acetyl substitution degree of 2.7 or less, a ratio τ of the sum of the acetyl substitution degrees at the 2-position and the acetyl substitution degrees at the 3-position to the acetyl substitution degree at the 6-position in the total acetyl substitution degree of 2.0 or more, and an amount of sulfuric acid component of more than 20 ppm to 400 ppm.
[0022] The cellulose acetate has a total acetyl substitution degree of 2.7 or less, preferably 2.6 or less, more preferably 2.5 or less, and even more preferably 2.2 or less. The total acetyl substitution degree may be 0.1 or more, and preferably 1.8 or more. If the total acetyl substitution degree of the cellulose acetate is too high, the biodegradability in seawater is poor, and if the total acetyl substitution degree is too low, the moldability is poor.
[0023] The total degree of acetyl substitution is the sum of the degrees of acetyl substitution at the 2-, 3- and 6-positions of the glucose ring of cellulose acetate measured as described below.
[0024] The degree of acetyl substitution at the 2-, 3-, and 6-positions of the glucose ring of cellulose acetate can be measured by NMR according to the method of Tezuka (Tezuka, Carbonydr. Res. 273, 83 (1995)). That is, the free hydroxyl groups of a cellulose acetate sample are propionylated with propionic anhydride in pyridine. The obtained sample is dissolved in deuterated chloroform and 13 The C-NMR spectrum is measured. The carbon signals of the acetyl group appear in the region from 169 ppm to 171 ppm in the order of 2nd, 3rd, and 6th positions from the high magnetic field, and the signals of the carbonyl carbon of the propionyl group appear in the same order in the region from 172 ppm to 174 ppm. From the abundance ratio of the acetyl group and the propionyl group at the corresponding positions (in other words, the area ratio of each signal), the degree of acetyl substitution at the 2nd, 3rd, and 6th positions of the glucose ring in the original cellulose acetate can be calculated. The degree of acetyl substitution is given by 13 In addition to C-NMR, 1 It can also be analyzed by H-NMR.
[0025] The ratio τ of the sum of the acetyl substitution degree at the 2-position and the acetyl substitution degree at the 3-position to the acetyl substitution degree at the 6-position in the total acetyl substitution degree is 2.0 or more, and the value of τ may be 2.1 or more, 2.2 or more, or 2.3 or more. There is no particular upper limit, but it may be 2.5 or less. If the value of τ is less than 2.0, the cellulose acetate is poor in biodegradability in seawater.
[0026] The cellulose acetate of the present disclosure has a sulfuric acid content of more than 20 ppm and not more than 400 ppm. The sulfuric acid content is preferably 50 ppm or more and not more than 380 ppm, more preferably 80 ppm or more and not more than 380 ppm, even more preferably 100 ppm or more and not more than 350 ppm, and particularly preferably 150 ppm or more and not more than 350 ppm. When the sulfuric acid content is within this range, the cellulose acetate has better biodegradability in seawater. The higher the sulfuric acid content, the higher the biodegradability in seawater. Also, if the sulfuric acid content is too high, it becomes difficult to produce the cellulose acetate.
[0027] The amount of sulfuric acid was calculated by the amount of sulfurous acid gas sublimated from dried cellulose acetate. 2- It is a conversion amount.
[0028] [Cellulose acetate composition] The cellulose acetate composition of the present disclosure may contain optional components in addition to cellulose acetate. The optional components of the cellulose acetate composition include additives and substances that are highly safe in the marine environment.
[0029] Examples of additives include one or more additives selected from the group consisting of substances having a pH of 8 or more in a 1 wt % aqueous solution at 20°C, substances that dissolve in water at 20°C at a concentration of 2 wt % or more, and substances that are highly biodegradable in the ocean.
[0030] The following cellulose acetate composition is preferred as a composition containing the cellulose acetate of the present disclosure: The cellulose acetate composition contains cellulose acetate and an additive, and the cellulose acetate has a total degree of acetyl substitution of 2.7 or less, and a ratio τ of the sum of the degrees of acetyl substitution at the 2nd position and the 3rd position to the degree of acetyl substitution at the 6th position in the total degree of acetyl substitution is 2.0 or more; and the additive is one or more selected from the group consisting of substances having a pH of 8 or more in a 1 wt % aqueous solution at 20° C., substances soluble in water at 20° C. at 2 wt % or more, and substances having excellent biodegradability in the ocean.
[0031] (Substances with a pH of 8 or higher in a 1% by weight aqueous solution at 20°C) In other words, a substance having a pH of 8 or more in a 1 wt % aqueous solution at 20° C. can be called a basic additive. The basic additive preferably has a pH of 8.5 or more in a 1 wt % aqueous solution at 20° C., and more preferably has a pH of 8.5 to 11.
[0032] The pH of a 1 wt % aqueous solution at 20° C. is measured according to standard procedures, for example with a glass pH electrode.
[0033] In the present disclosure, the "1 wt% aqueous solution at 20°C" does not necessarily mean that all of the solute is dissolved in water. In general, an aqueous solution refers to a liquid in which a solute is dissolved in water (H2O). In other words, it refers to a solution in which the solvent is water. Since water molecules are polar molecules, the solute of an aqueous solution is considered to be an ionic crystal or a polar molecular substance. However, in the present disclosure, the "aqueous solution" includes a suspension. In other words, it includes a slurry, which is a dispersion system in which solid particles are dispersed in a liquid, and a colloidal solution. In addition, in the present disclosure, the "1 wt% aqueous solution at 20°C" also includes a solution in which, when a basic additive is added to water at 1 wt%, a part of the basic additive dissolves to become an aqueous solution, and the remaining part of the basic additive becomes a suspension.
[0034] The solid particles may be colloidal particles (approximately 100 nm or less), but may also be larger particles. A suspension of colloidal particles is called a colloidal solution, while a suspension of particles larger than colloidal particles is sometimes simply called a suspension. Unlike colloidal solutions, a suspension of particles larger than colloidal particles will settle to a steady state over time. The solid particles may be visible under a microscope and will settle over time if placed in a quiet place.
[0035] When the basic additive in the aqueous solution is an inorganic substance that becomes ions in the aqueous solution, the surface of the basic additive is charged with ions due to the influence of the surface charge of the particle, which affects the ion distribution in the vicinity of the surface. This influence causes a distribution of ions called an electric double layer around the surface of the basic additive, which is different from that in the solution (solvent) outside the vicinity of the particle interface. The electric double layer is formed by a fixed layer where ions are most strongly adsorbed on the particle surface and a diffusion layer away from the fixed layer. Even if the basic additive of the present disclosure is not dissolved in water, the pH of the dispersion medium changes due to the surface charge of the basic additive as described above.
[0036] Substances (basic additives) having a pH of 8 or higher in a 1% by weight aqueous solution at 20°C include oxides, hydroxides, carbonates, acetates, ammonium salts, aluminates, silicates, or metasilicates of alkaline earth metals or alkali metals; ZnO; and basic Al2O3.
[0037] The basic additive is preferably one or more selected from the group consisting of an oxide, hydroxide, carbonate, ammonium salt, aluminate, silicate, or metasilicate of an alkaline earth metal or an alkali metal; ZnO; and basic Al2O3.
[0038] The basic additive is more preferably one or more selected from the group consisting of an oxide, hydroxide, aluminate, silicate, or metasilicate of an alkaline earth metal or an alkali metal; ZnO; and basic Al2O3.
[0039] More preferably, the basic additive is one or more selected from the group consisting of an oxide, aluminate, silicate, or metasilicate of an alkaline earth metal or an alkali metal; ZnO; and basic Al2O3.
[0040] As the basic additive, one or more selected from the group consisting of an oxide, an aluminate, a silicate, and a metasilicate of an alkaline earth metal or an alkali metal is even more preferable.
[0041] As the basic additive, an oxide of an alkaline earth metal is particularly preferred, with magnesium oxide (MgO) being one of the most preferred.
[0042] Examples of the oxides of alkaline earth metals or alkali metals include magnesium oxide (MgO) and calcium oxide (CaO).
[0043] Alkaline earth metal or alkali metal hydroxides include Mg(OH)2 and Ca(OH)2.
[0044] Alkaline earth metal or alkali metal carbonates include MgCO3, CaCO3, NaHCO3, Na2CO3, and K2CO3.
[0045] Alkaline earth metal or alkali metal acetates include magnesium acetate and calcium acetate.
[0046] Examples of aluminates of alkaline earth metals or alkali metals include sodium aluminate. Sodium aluminate is an inorganic compound containing sodium and aluminum. Compounds called sodium aluminate include sodium aluminum dioxide (NaAlO2), which is a double oxide, and sodium tetrahydroxide aluminate (Na[Al(OH)4], which is a hydroxy complex.
[0047] Examples of silicates of alkaline earth metals or alkali metals include sodium silicate (Na2SiO3). Silica is a compound represented by the general formula [SiO x (OH) 4-2x ] n It is a general term for compounds of silicon, oxygen, and hydrogen represented by the formula:
[0048] Examples of metasilicates of alkaline earth metals or alkali metals include magnesium aluminometasilicate, which is represented by the general formula Al2O3·MgO·2SiO2·xH2O (where x indicates the number of crystal waters, and 1≦x≦10). Magnesium aluminometasilicate itself is well known, and commercially available products can be used. For example, magnesium aluminometasilicate that meets the Japanese Pharmacopoeia non-medicinal drug standards can be suitably used. Magnesium aluminometasilicate is sold as an antacid under the name Neusilin (registered trademark).
[0049] Other preferred basic substances include basic polymers and oligomers; basic amino acids and proteins; and basic sugars.
[0050] The basic additive of the present disclosure is not necessarily water soluble, but has a water solubility of 10 -5 The basic additive of the present disclosure may have a solubility of 10 to 70 g / 100 mL water at 20° C. -6 It is preferable that the solubility of the compound is 10 g or more / 100 mL of water at 20°C. -5 It is more preferable that the solubility of the compound is 10 g or more / 100 mL of water at 20° C. -4 The basic additive preferably has a solubility of 10 g or less / 100 mL water at 20° C., more preferably has a solubility of 1 g or less / 100 mL water at 20° C., and even more preferably has a solubility of 0.1 g or less / 100 mL water at 20° C.
[0051] Underwater approx. 10 -4 Examples of additives with a solubility of about 10 g / 100 mL (20°C) are MgO, ZnO, and Mg(OH)2 in water. -2 An example of an additive with a solubility of about 0.1 g / 100 mL (20° C.) in water is MgCO3. Examples of additives with a solubility of about 0.1 g / 100 mL (20° C.) in water are CaO and Ca(OH)2.
[0052] (Substances that dissolve at least 2% by weight in water at 20°C) The substance that dissolves at 2% by weight or more in water at 20° C. may be either a polymeric substance or a low molecular weight substance, so long as it is water-soluble.
[0053] Examples of the polymeric substance include hydrophilic polymers. Here, the hydrophilic polymer is a polymer having a hydrophilic functional group. The hydrophilic polymer is not particularly limited, and examples thereof include polymers having an OH group such as polyvinyl alcohol and partially saponified polyvinyl acetate; polymers having a COOH group such as polyacrylic acid, polymethacrylic acid, and copolymers of acrylic acid or methacrylic acid with other monomers; polymers having a polyether skeleton such as polyethylene glycol, 1,3-polypropylene glycol, and 1,4 polybutylene glycol; and polymers having a monomer having an amide skeleton in the molecule such as polyvinylpyrrolidone, polyacrylamide, poly-N-methylacrylamide, poly-N,N-dimethylacrylamide, polyacryloylmorpholine, poly-N-vinylmorpholine, and poly-N-vinylmorpholine-N-oxide. The hydrophilic polymer may be used alone or in combination of two or more kinds.
[0054] The polymer substance is a polymer having a repeating unit, and the number of atoms constituting the repeating unit is N2, and the number of OH groups, amide groups, amino groups, COOH groups, and NR3 groups contained in the repeating unit is N2. + When the total number of groups is N1, N1 / N2 is preferably 0.01 or more and 0.55 or less, and more preferably 0.1 or more and 0.5 or less. This is because high hydrophilicity can be imparted. + Examples of the group R include CH3, CH2CH3, and the like.
[0055] The polymeric substance is preferably an amide group-containing vinyl polymer. The amide group-containing vinyl polymer is obtained by polymerization of a vinyl monomer having an amide group. The amide group-containing vinyl polymer is more preferably polyvinylpyrrolidone or a vinylpyrrolidone copolymer, because it has excellent compatibility with cellulose acetate.
[0056] Examples of low molecular weight substances include polysaccharides and cellulose acetate plasticizers.
[0057] The polysaccharides include polysaccharides composed of at least one type of polysaccharide (A) selected from oligosaccharides (powdered oligosaccharides), reduced starch syrup, and cluster dextrin, and at least one type of crystalline sugar alcohol (B).
[0058] As the at least one type of polysaccharide selected from oligosaccharides (powdered oligosaccharides), reduced starch syrup, and cluster dextrin, the following can be used.
[0059] The oligosaccharide (A1) may be either a homooligosaccharide or a heterooligosaccharide. Examples of the oligosaccharide (A1) include disaccharides to decasaccharides and disaccharides to hexasaccharides. The oligosaccharide (A1) may be an anhydride. In the oligosaccharide (A1), a monosaccharide may be bonded to a sugar alcohol. Furthermore, the oligosaccharide (A1) may be an oligosaccharide composition composed of a plurality of sugar components, or may be an oligosaccharide composition produced by decomposition of a polysaccharide. Such an oligosaccharide composition may be simply called oligosaccharide (A1).
[0060] The oligosaccharide (A1) is usually solid at room temperature. The oligosaccharide (A1) (or oligosaccharide composition) can be used alone or in combination of two or more kinds. The oligosaccharide (A1) is generally derived from a natural product, so that the burden on the environment can be reduced.
[0061] Disaccharides include homo-oligosaccharides, such as trehalose, maltose, isomaltose, cellobiose, gentiobiose, and melibiose; and hetero-oligosaccharides, such as lactose, sucrose, and palatinose.
[0062] Trisaccharides include homo-oligosaccharides such as maltotriose, isomaltotriose, panose, and cellotriose; and hetero-oligosaccharides such as manninotriose, solatriose, melezitose, planteose, gentianose, umbelliferose, lactosucrose, and raffinose.
[0063] Examples of tetrasaccharides include homooligosaccharides such as maltotetraose and isomaltotetraose; and heterooligosaccharides such as stachyose, cellotetraose, scorodose, lyquinose, or tetraose in which a sugar or sugar alcohol is bound to the reducing end of panose. Among these tetrasaccharides, tetraose in which a monosaccharide or sugar alcohol is bound to the reducing end of panose is disclosed in, for example, JP-A-10-215892, and examples thereof include tetraose in which a monosaccharide such as glucose, fructose, mannose, xylose, or arabinose is bound to the reducing end of panose; or a sugar alcohol such as sorbitol, xylitol, or erythritol is bound to the reducing end of panose.
[0064] Examples of pentasaccharides include homooligosaccharides such as maltopentaose and isomaltopentaose, and heterooligosaccharides such as pentaose in which a disaccharide is bound to the reducing end of panose. Pentaose in which a disaccharide is bound to the reducing end of panose is disclosed in, for example, JP-A-10-215892, and examples thereof include pentaose in which a disaccharide such as sucrose, lactose, cellobiose, or trehalose is bound to the reducing end of panose.
[0065] Examples of hexasaccharides include homooligosaccharides such as maltohexaose and isomaltohexaose.
[0066] Among these oligosaccharides (or oligosaccharide compositions), oligosaccharides composed of at least tetrasaccharides are preferred from the viewpoints of melt viscosity characteristics and melt-mixing or kneading properties with a resin component.
[0067] Examples of such oligosaccharides or oligosaccharide compositions include starch sugars (starch saccharification products), galactooligosaccharides, coupling sugars, fructooligosaccharides, xylooligosaccharides, soybean oligosaccharides, chitin oligosaccharides, and chitosan oligosaccharides, and these components can be used alone or in combination of two or more. For example, starch sugars are oligosaccharide compositions obtained by reacting starch with acid or glucoamylase, and may be a mixture of oligosaccharides to which multiple glucose units are bound.
[0068] Examples of starch sugars include reduced starch saccharification products (product name: PO-10, tetrasaccharide content of 90% by weight or more) manufactured by Towa Chemical Industry Co., Ltd. Galactooligosaccharides are oligosaccharide compositions obtained by reacting lactose with β-galactosidase or the like, and are composed of galactosyllactose and galactose-(glucose) n (n is an integer from 1 to 4). Coupling sugar is an oligosaccharide composition obtained by the action of cyclodextrin synthase (CGTase) on starch and sucrose, and may be a mixture of (glucose) n -sucrose mixture (n is an integer from 1 to 4). Fructooligosaccharides are oligosaccharide compositions obtained by the action of fructofuranosidase on sugar, and may be a mixture of sucrose-(fructose) n (n is an integer of 1 to 4).
[0069] The above-mentioned substance that dissolves in water at 20° C. at a concentration of 2% by weight or more preferably contains a plasticizer for cellulose acetate.
[0070] (Plasticizer for cellulose acetate) Detailed examples of plasticizers are given in "Handbook of Plasticizers," Ed. Wypych, George, ChemTec Publishing (2004). Examples of plasticizers include dimethyl phthalate, diethyl phthalate, dibutyl phthalate, dioctyl phthalate, diisononyl phthalate, butyl benzyl phthalate, butyl phthalyl butyl glycolate, tris(2-ethylhexyl) trimellitate, triethyl phosphate, triphenyl phosphate, tricresyl phosphate, p-phenylene bis(diphenyl phosphate), and other phosphate derivatives, diisobutyl adipate, bis(2-ethylhexyl) adipate, triethyl citrate, acetyl triethyl citrate, plasticizers containing citric acid (e.g., Citroflex (registered trademark)), monoacetin, diacetin, triacetin, tripropycin, and the like. onin; tributyrin; sucrose acetate isobutyrate; glucose pentapropionate; triethylene glycol-2-ethylhexanoate; polyethylene glycol; polypropylene glycol; polypropylene glycol dibenzoate; polyethylene glutarate; polyethylene succinate; polyalkyl glycosides; 2,2,4-trimethyl-1,3-pentanediol isobutyrate; diisobutyrate; phthalic acid copolymers; 1,3-butanediol; 1,4-butanediol end-capped with aliphatic epoxides; bis(2-ethylhexyl) adipate; epoxidized soybean oil; and mixtures thereof.
[0071] As the plasticizer, a glycerin ester plasticizer can be used. As the glycerin ester plasticizer, a lower fatty acid ester of glycerin, in other words, an ester compound of glycerin and a fatty acid having 2 to 4 carbon atoms can be used. The fatty acid having 2 carbon atoms is acetic acid, the fatty acid having 3 carbon atoms is propionic acid, and the fatty acid having 4 carbon atoms is butyric acid. The glycerin ester plasticizer may be one in which all three hydroxyl groups of glycerin are esterified with the same fatty acid, one in which two hydroxyl groups are esterified with the same fatty acid, or one in which all three hydroxyl groups of glycerin are esterified with different fatty acids.
[0072] Glycerin ester plasticizers are non-toxic and easily biodegradable, so they have a low environmental impact. In addition, by adding a glycerin ester plasticizer to cellulose acetate, the glass transition temperature of the resulting cellulose acetate composition can be lowered. This allows the raw material to have excellent thermoformability.
[0073] When the fatty acid is acetic acid, examples of glycerin ester plasticizers include triacetin, in which three hydroxyl groups of glycerin are esterified with acetic acid, and diacetin, in which two hydroxyl groups of glycerin are esterified with acetic acid.
[0074] Among the above glycerin ester-based plasticizers, triacetin (glycerol trisacetate) in which all three hydroxyl groups of glycerin are esterified with acetic acid (in other words, acetylated) is particularly preferred. Triacetin is a component that is recognized as safe for human ingestion, and is easily biodegradable, so it places a small burden on the environment. In addition, the cellulose acetate composition obtained by adding triacetin to cellulose acetate has improved biodegradability compared to the case where cellulose acetate is used alone. Furthermore, by adding triacetin to cellulose acetate, the glass transition temperature of cellulose acetate can be efficiently lowered. Therefore, excellent thermoformability can be imparted to the raw material.
[0075] In addition, triacetin is preferably one that is pure in terms of chemical structure and has a high purity. In addition, for example, a plasticizer containing 80% by weight or more or 90% by weight or more of triacetin, with the remainder being monoacetin and / or diacetin, may be used.
[0076] (Materials with excellent biodegradability in the ocean) The biodegradability of cellulose acetate can be promoted by adding a substance having excellent marine biodegradability. Examples of the substance having excellent marine biodegradability include compounds having excellent marine biodegradability. The substance having excellent marine biodegradability may be insoluble in water. Examples of the compound having excellent marine biodegradability include a substance that decomposes 50% or more, preferably 70% or more, and more preferably 90% or more, of a comparable cellulose after 180 days according to the method specified in ASTM D6691. Examples include polyhydroxyalkanoates such as poly[hydroxybutyrate-co-hydroxyhexanoate] (PHBH) and polyhydroxybutyrate, and thermoplastic starch resins (including acetylated starch).
[0077] The process of biodegradation of the cellulose acetate and cellulose acetate composition of the present disclosure is as follows. Generally, the mechanism of biodegradation of cellulose acetate is considered to be that when each acetyl group of cellulose acetate is hydrolyzed to reduce the degree of substitution, the cellulose is decomposed by the action of an enzyme that decomposes cellulose (e.g., β-glucosidase (EC 3.2.1.21)). β-glucosidase (EC 3.2.1.21) is an enzyme that catalyzes the reaction of hydrolyzing the β-glycosidic bond of sugar, and is also called β-D-glucoside glucohydrolase or amygdase. After the β-glycosidic bond that constitutes the polymer chain of cellulose acetate is hydrolyzed to become monosaccharides or low molecular weight polysaccharides, it is decomposed by the metabolism of normal microorganisms. Therefore, in order to promote biodegradation, it is effective to promote the elimination of the acetyl group.
[0078] Ocean water is weakly alkaline, and this basicity also promotes the deacetylation of cellulose acetate. As a result of the investigation, it was found that deacetylation (hydrolysis) under basic conditions is faster at the 2nd and 3rd positions in the glucose ring than at the 6th position. Therefore, for example, for cellulose acetate with the same total substitution degree, it was found that the total substitution degree decreases faster and biodegradation proceeds faster when the substitution degree of the 2nd and 3rd positions is higher than that of the 6th position. It was also found that biodegradability is excellent when the sulfuric acid component is more than 20 ppm and is 400 pp. If the sulfuric acid component is too high, there is a concern that it will decompose during use as a product before being immersed in the ocean. It is believed that these actions will show similar trends regardless of the total substitution degree when comparing products with the same total substitution degree. However, the degree of biodegradability is excellent when the total acetyl substitution degree is 2.7 or less.
[0079] In the total degree of acetyl substitution, the ratio τ of the sum of the degrees of acetyl substitution at the 2-position and the 3-position to the degree of acetyl substitution at the 6-position is 2.0 or more, particularly 2.1 or more, further preferably 2.15 or more, and further preferably 2.2 or more.
[0080] The decomposition mechanism of the cellulose acetate composition of the present disclosure is as follows. Although this mechanism is speculation, it is believed that in weakly alkaline seawater, a substance (basic additive) having a pH of 8 or more in a 1% by weight aqueous solution at 20°C promotes hydrolysis (deacetylation) of cellulose acetate. The deacetylation effect of this basic substance is more prominent in cellulose acetate having more acetyl groups at the 2nd and 3rd positions than at the 6th position, and further in cellulose acetate having more sulfuric acid components. As a result, it is believed that the degree of substitution of the cellulose acetate constituting the cellulose acetate composition decreases, which may contribute to improving biodegradability. It is preferable that these properties are not expressed during use as a product, but are quickly expressed after contact with seawater. Therefore, it is dispersed in the cellulose acetate composition as solid particles, and the particle size of the basic substance is preferably as small as possible, and the specific surface area is preferably large.
[0081] As a substance (basic additive) having a pH of 8 or more in a 1% by weight aqueous solution at 20° C., magnesium aluminometasilicate, magnesium oxide, etc. can be preferably used since they are highly safe and are used as pharmaceuticals.
[0082] The cellulose acetate composition of the present disclosure may also contain a substance that dissolves in water at 20°C at 2% by weight or more. Such a substance can dissolve in seawater when the cellulose acetate composition is put into seawater. Then, the substance leaves the cellulose acetate composition and forms structural voids in the molded article made of the cellulose acetate composition. Then, microorganisms can easily enter the voids, and the surface area of the molded article made of the cellulose acetate composition increases. As a result, it can contribute to improving biodegradability. Examples of such substances include triacetin and diacetin. These substances can also contribute to improving thermoformability because triacetin and diacetin act as plasticizers for cellulose acetate.
[0083] The total content of the additives in the cellulose acetate composition is preferably 40% by weight or less, more preferably 30% by weight or less, and even more preferably 20% by weight or less, and is preferably 5% by weight or more, and more preferably 10% by weight or more.
[0084] The content of the basic additive (a substance having a pH of 8 or more in a 1 wt % aqueous solution at 20° C.) in the cellulose acetate composition is preferably 1 to 30 wt %, more preferably 2 to 20 wt %, further preferably 3 to 15 wt %, particularly preferably 5 to 10 wt %. If the amount of the basic additive is too large, problems such as moldability may occur, such as difficulty in molding the cellulose acetate or the cellulose acetate composition.
[0085] The content of the water-soluble additive (a substance that dissolves in water at 20°C at 2% by weight or more) in the cellulose acetate composition is preferably 5 to 30% by weight, more preferably 7.5 to 28% by weight, and even more preferably 10 to 25% by weight. If the amount of the water-soluble additive is too large, the strength of the cellulose acetate composition decreases.
[0086] The content of the substance having excellent marine biodegradability in the cellulose acetate composition is preferably 5 to 40% by weight.
[0087] The cellulose acetate composition of the present disclosure can be used in combination with other substances to improve the biodegradability of the mixture as a whole.
[0088] Even if the above-mentioned basic substance is added to cellulose acetate or a composition containing cellulose acetate, if the composition contains, for example, an acidic substance and a neutralization reaction occurs when immersed in water, causing the composition to change from neutral to acidic, the effect of adding the basic substance may not be obtained.
[0089] Therefore, the cellulose acetate composition of the present disclosure preferably has a pH of 7 to 13, and more preferably a pH of 8 to 12, at 20° C. when mixed with water to obtain a slurry.
[0090] It is believed that the biodegradation of the cellulose acetate of the present disclosure is first performed by the elimination of the acetyl group, the degree of acetyl substitution decreases, and the cellulose acetate becomes closer to cellulose, and is then decomposed by the action of microorganisms. Therefore, the additive is preferably an additive that promotes the decomposition of the cellulose acetate.
[0091] Cellulose acetate has a cellulose type II crystal structure (more precisely, a cellulose acetate type II crystal structure). It can be converted from cellulose type I to cellulose type II by acetylation of raw cellulose. The cellulose type II crystal structure has an antiparallel chain structure in which the reducing ends are alternately positioned, and is not as strong as the cellulose type I crystal structure. Such a crystal structure of cellulose acetate also contributes to the excellent biodegradability of the cellulose acetate composition of the present disclosure in seawater. It is said that once the cellulose type I crystal structure is changed to the cellulose acetate type II crystal structure, it will not change to the type I crystal structure.
[0092] The cellulose acetate composition of the present disclosure has excellent thermoformability, and is therefore suitable for thermoforming.The shape of the molded product obtained by molding the cellulose acetate composition of the present disclosure is not particularly limited, and includes, for example, one-dimensional molded products such as fibers; two-dimensional molded products such as films; and three-dimensional molded products such as particles including pellets, tubes and hollow cylinders.
[0093] In the case of particulate matter, the ratio of particles with a diameter of 2 mm or less is preferably 50% by weight or less, since this provides better biodegradability.
[0094] The ratio (weight %) of particles with a particle size of 2 mm or less can be determined using a sieve specified in JIS Z 8801. That is, a sieve with an opening of 2 mm and a tray are attached to a low tap machine (manufactured by Iida Seisakusho Co., Ltd., tapping: 156 times / min, rolling: 290 times / min), and 100 g of a sample is vibrated for 5 minutes, after which the ratio of the total weight of the particles on each sieve to the total weight (100 g of sample) is calculated.
[0095] The cellulose acetate or cellulose acetate composition disclosed herein has excellent biodegradability in seawater, and is therefore suitable for products that are easily disposable, such as containers such as straws and cups, packaging materials, binders, and cigarette filters; clothing fibers; nonwoven fabrics; cosmetic beads and scrubs, and other products that are likely to be washed away, even if only partially, into the natural environment with water when used; and sanitary products (diapers, sanitary products), and other products that are expected to be flushed down the toilet.
[0096] [Method of producing cellulose acetate] The method for producing cellulose acetate of the present disclosure is not particularly limited, and examples thereof include the following method: A production method comprising the steps of: (a) reacting cellulose with acetic anhydride in the presence of an acid catalyst and an acetic acid solvent to produce a cellulose acetate dope; (b) hydrolyzing the produced cellulose acetate to adjust the total acetyl substitution degree to 2.7 or less; and (c) precipitating the hydrolyzed cellulose acetate with a precipitating agent.
[0097] (Step (a) of Producing a Dope of Cellulose Acetate) In the process of producing a cellulose acetate dope, cellulose is reacted with acetic anhydride in the presence of an acid catalyst and an acetic acid solvent, in other words, an acetylation reaction of cellulose. This cellulose is preferably subjected to an activation process. The activation process may include pretreatment and activation of the raw cellulose by adding acetic acid or acetic acid containing 1 to 10% by weight of sulfuric acid (sulfur-containing acetic acid) to the raw cellulose in one or two stages.
[0098] The cellulose (pulp) used as the raw material may be wood pulp (softwood pulp, hardwood pulp), cotton linters, etc. These celluloses may be used alone or in combination of two or more kinds, for example, softwood pulp may be used in combination with cotton linters or hardwood pulp.
[0099] Regarding linter pulp, linter pulp is preferred because it has high cellulose purity and a small amount of coloring components, resulting in high transparency of molded products.
[0100] Next, wood pulp will be described. Wood pulp is preferred because it can be stably supplied as a raw material and is more cost-effective than linters. Examples of wood pulp include hardwood prehydrolyzed kraft pulp. Also, as the wood pulp, crushed pulp obtained by crushing hardwood prehydrolyzed kraft pulp into a cotton-like form can be used. Crushing can be performed, for example, using a disc refiner.
[0101] Furthermore, in order to reduce insoluble residues and not impair the transparency of the molded product, the α-cellulose content of the raw cellulose is preferably 90% by weight or more, more preferably 92% by weight or more, even more preferably 95% by weight or more, and most preferably 97% by weight or more.
[0102] When the starting cellulose is supplied in a sheet-like form that makes it difficult to handle in the subsequent steps, for example, the starting cellulose is preferably subjected to a step of dry crushing treatment.
[0103] In the activation step of pre-activating raw cellulose by adding acetic acid or acetic acid containing 1 to 10% by weight of sulfuric acid (sulfur-containing acetic acid), acetic acid and / or sulfur-containing acetic acid can be added in an amount of preferably 10 to 500 parts by weight per 100 parts by weight of raw cellulose. Examples of the method of adding acetic acid and / or sulfur-containing acetic acid to cellulose include a method of adding acetic acid or sulfur-containing acetic acid in one step, a method of adding acetic acid and then adding sulfur-containing acetic acid after a certain time has elapsed, and a method of adding acetic acid or sulfur-containing acetic acid in two or more steps in separate steps, such as a method of adding acetic acid and then adding sulfur-containing acetic acid after a certain time has elapsed, and a method of adding acetic acid and then adding sulfur-containing acetic acid after a certain time has elapsed. Specific means of addition include a method of spraying and stirring.
[0104] The pretreatment activation can be carried out by adding acetic acid and / or sulfur-containing acetic acid to cellulose, followed by leaving the mixture at rest at 17 to 40° C. for 0.2 to 48 hours, or by sealing and stirring the mixture at 17 to 40° C. for 0.1 to 24 hours.
[0105] The process of reacting cellulose with acetic anhydride in the presence of an acid catalyst and an acetic acid solvent to produce a cellulose acetate dope (acetylation reaction process) will be described. Sulfuric acid is preferable as the acid catalyst. For example, the acetylation can be started by adding cellulose to a mixture of acetic acid, acetic anhydride, and sulfuric acid, or by adding a mixture of acetic acid and acetic anhydride and sulfuric acid to cellulose. Here, the cellulose acetate dope refers to a solution obtained by dissolving cellulose acetate or a mixture containing cellulose acetate in a solvent.
[0106] Furthermore, these mixtures are not particularly limited as long as they contain acetic acid and acetic anhydride, but the ratio of acetic acid to acetic anhydride is preferably 300 to 600 parts by weight of acetic acid and 200 to 400 parts by weight of acetic anhydride, and more preferably 350 to 530 parts by weight of acetic acid and 240 to 280 parts by weight of acetic anhydride.
[0107] The ratio of cellulose, the mixture of acetic acid and acetic anhydride, and sulfuric acid in the acetylation reaction is preferably 500 to 1,000 parts by weight of the mixture of acetic acid and acetic anhydride, and preferably 0.5 to 15 parts by weight of concentrated sulfuric acid, more preferably 5 to 14 parts by weight, and even more preferably 7 to 11 parts by weight, per 100 parts by weight of cellulose. Increasing the amount of concentrated sulfuric acid increases the amount of sulfuric acid component.
[0108] In the acetylation reaction step, the acetylation reaction of cellulose can be carried out at 20 to 55° C. with stirring for 30 minutes to 36 hours from the start of acetylation.
[0109] The acetylation reaction of cellulose can be carried out, for example, by raising the temperature to 20 to 55°C over 5 minutes to 36 hours from the start of acetylation under stirring conditions, or by not adding any heat to the inside or outside of the reaction system under stirring conditions. The initial stage of the acetylation reaction is a solid-liquid heterogeneous reaction, and it is preferable to raise the temperature as long as possible in order to suppress the depolymerization reaction while promoting the acetylation reaction and reducing unreacted materials, but from the viewpoint of productivity, it is preferable to raise the temperature within 2 hours, more preferably within 1 hour.
[0110] The time required for the acetylation reaction (hereinafter also referred to as the acetylation time) is preferably 30 to 200 minutes. Here, the acetylation time refers to the time from when the raw material cellulose is introduced into the reaction system and the reaction with acetic anhydride starts until the neutralizing agent is introduced.
[0111] (Step (b) of hydrolyzing cellulose acetate) In step (b) of hydrolyzing the produced cellulose acetate to make the total degree of acetyl substitution 2.7 or less, for example, a neutralizing agent containing water (including water vapor), dilute acetic acid, or carbonates, acetates, hydroxides, or oxides of calcium, magnesium, iron, aluminum, zinc, etc., is added to terminate the acetylation reaction during hydrolysis (saponification). Note that dilute acetic acid refers to an aqueous solution of acetic acid with a concentration of 1 to 50% by weight.
[0112] As the neutralizing agent, magnesium acetate and calcium acetate are preferable. Since calcium and the like combine with sulfuric acid, the sulfate ion concentration in the cellulose acetate dope can be increased. As a result, the amount of sulfuric acid in the obtained cellulose acetate can be adjusted to more than 20 ppm and less than 400 ppm. In addition, by increasing the amount of water added during hydrolysis, the ratio (τ) of the 2,3-position substitution degree to the 6-position substitution degree can be increased.
[0113] The time of the hydrolysis (saponification) reaction (hereinafter also referred to as the maturation time) is not particularly limited, and the time may be appropriately adjusted depending on the target total degree of acetyl substitution. Here, the maturation time refers to the time from the start of the addition of the neutralizing agent to the end of the hydrolysis (saponification) reaction. The total degree of substitution can be reduced by increasing the maturation time.
[0114] The hydrolysis (saponification) reaction is carried out by maintaining the mixture for 20 to 120 minutes at an aging temperature of preferably 50 to 100° C., particularly preferably 70 to 90° C. Here, the aging temperature refers to the temperature in the reaction system during the aging time.
[0115] (Step (c) of precipitating the hydrolyzed cellulose acetate with a precipitant) The step of precipitating the prepared cellulose acetate with a precipitating agent will now be described. The precipitating agent may be appropriately selected depending on the desired total degree of acetyl substitution.
[0116] The precipitated cellulose acetate may be washed with a precipitating agent to remove free metal components, sulfuric acid components, etc. In order to enhance the thermal stability of the cellulose acetate, in addition to washing with the precipitating agent, an alkali metal compound and / or an alkaline earth metal compound, particularly a calcium compound such as calcium hydroxide, may be added as a stabilizer as necessary. A stabilizer may also be used during washing with the precipitating agent.
[0117] (Optional process) After the step (c) of precipitating the hydrolyzed cellulose acetate with a precipitant, the obtained cellulose acetate may be separated and dried as necessary. The cellulose acetate is preferably separated by dehydration using filtration or centrifugation. The drying method is not particularly limited, and a known method can be used, for example, drying can be performed under conditions such as blowing air or reduced pressure. An example of the drying method is hot air drying.
[0118] Furthermore, when the cellulose acetate composition of the present disclosure contains an additive, the additive can be incorporated in the composition by the following method.
[0119] The cellulose acetate composition can be obtained by mixing cellulose acetate and additives with a solvent such as acetone and then removing the solvent, or by melting cellulose acetate and kneading the additives therewith. EXAMPLES
[0120] The present invention will be described in detail below with reference to examples, but the technical scope of the present invention is not limited to these examples.
[0121] The physical properties described in the following Examples and Comparative Examples were evaluated by the following methods.
[0122] <Acetyl substitution degree at each of 2, 3, and 6 positions, and total acetyl substitution degree> The degree of acetyl substitution at the 2-, 3-, and 6-positions was measured according to the method of Tezuka (Carbonydr. Res. 273, 83 (1995)) as described above. The free hydroxyl groups of a cellulose acetate sample were propionylated with propionic anhydride in pyridine, the sample was dissolved in deuterated chloroform, and the resulting solution was dissolved in deuterated chloroform. 13 The C-NMR spectrum was measured by the NMR method. The degree of acetyl substitution at the 2nd, 3rd, and 6th positions (DS2, DS3, DS6) was calculated from the area ratio of each carbon signal of the acetyl group appearing in the order of 2nd, 3rd, and 6th positions from the high magnetic field in the region from 169 ppm to 171 ppm. The total degree of acetyl substitution is the sum of the degrees of acetyl substitution at the 2nd, 3rd, and 6th positions. In addition, the sum of the degree of acetyl substitution at the 2nd position and the degree of acetyl substitution at the 3rd position (DS2+3) and the ratio τ of the sum of the degree of acetyl substitution at the 2nd position and the degree of acetyl substitution at the 3rd position to the degree of acetyl substitution at the 6th position were calculated.
[0123] <Amount of sulfuric acid component> The dried cellulose acetate or cellulose acetate composition is baked in an electric furnace at 1300°C, and the sublimated sulfurous acid gas is trapped in 10% hydrogen peroxide solution and titrated with a normal aqueous sodium hydroxide solution to obtain SO4 2-The converted amount was measured as the amount of sulfuric acid component, which is expressed in ppm as the amount of sulfuric acid component per gram of bone-dry cellulose acetate or cellulose acetate composition.
[0124] <Slurry pH> 2.0 g of finely powdered dried cellulose or cellulose acetate composition was accurately weighed, 80 ml of boiled distilled water was added, stirred, sealed and left overnight, and then further stirred to allow the sample to settle. Approximately 10 ml of the supernatant was used as the sample solution, and the pH was measured using a calibrated pH meter. As a blank, the pH of boiled distilled water was also measured, and the pH was calculated using the formula [H + ]=10 -(pH) (pH indicates the measured pH value) is the hydrogen ion concentration of the sample solution and the blank solution, [H + ] s and [H + ] b (s indicates sample, b indicates blank) were calculated. [H + ] s ≧[H + ] b Then, the slurry pH can be calculated by the following formula:
[0125] Slurry pH = -LOG([H + ] S -[H + ] b ) [H + ] S <[H + ] b In this case, the formula [OH - ]=10 -14 / [H + ] to determine the hydroxyl ion concentration [OH - ] S , [OH - ] b Then, the slurry pH can be calculated using the following formula: Slurry pH = 14 + LOG([OH - ] S -[OH - ] b +10 -7 )
[0126] <Biodegradable> Biodegradability was evaluated using a method of evaluating biodegradability by immersion in seawater. First, a film was prepared by a general solvent casting method. 10 to 15 parts by weight of the cellulose or cellulose acetate composition obtained in the examples and comparative examples was dissolved in 85 to 90 parts by weight of acetone, and a predetermined amount of MgO was added to prepare a dope. The dope was poured onto a glass plate and cast with a bar coater. The film was dried at 40°C for 30 minutes, peeled off from the glass plate, and dried at 80°C for another 30 minutes to obtain an evaluation film with a thickness of 30 μm.
[0127] The film (10cm x 10cm x 50μm) prepared by the above method was placed in a stainless steel container and biodegraded according to ASTM D6691. Seawater collected from Hakata Bay in Kitakyushu was used. However, biodegradability was evaluated by weight measurement. That is, 90 days and 180 days after the start of immersion, the entire content of the stainless steel container was filtered through a filter with a mesh size of 10μm, and the film and the residue of the decomposed film were collected on the filter. After rinsing the filter with 50mL of distilled water, the residue and the filter were dried under vacuum at 80℃ for 4 hours.
[0128] The increase in filter weight before and after filtration of the film residue was designated as W1 (g), and the weight of the film before immersion was designated as W2 (g), and the weight retention was calculated using the following formula. Weight retention rate (weight%)=100×W1 / W2
[0129] Comparative Example 1 Hardwood prehydrolyzed kraft pulp with an α-cellulose content of 98.4 wt% was crushed into a cotton-like state using a disc refiner. 26.8 parts by weight of acetic acid was sprayed onto 100 parts by weight of the crushed pulp (water content 8%), and after thorough mixing, the mixture was left to stand for 60 hours as a pretreatment for activation (activation step). The activated pulp was added to a mixture of 323 parts by weight of acetic acid, 245 parts by weight of acetic anhydride, and 13.1 parts by weight of sulfuric acid, and the mixture was adjusted to a maximum temperature of 5°C to 40°C over 40 minutes, and acetylated for 90 minutes. A neutralizing agent (24% magnesium acetate aqueous solution) was added over 3 minutes so that the amount of sulfuric acid (amount of aged sulfuric acid) was adjusted to 2.5 parts by weight. Furthermore, after the reaction bath was heated to 75°C, water was added to adjust the reaction bath moisture (aging moisture) to a concentration of 52 mol%. The aging moisture concentration was expressed in mol% by multiplying the ratio of the reaction bath moisture to acetic acid expressed in molar ratio by 100. The mixture was then aged at 85°C for 130 minutes, and the aging was stopped by neutralizing the sulfuric acid with magnesium acetate to obtain a reaction mixture containing cellulose acetate. A dilute aqueous solution of acetic acid was added to the reaction mixture, and the cellulose acetate was separated. It was then washed with water, dried, and stabilized with calcium hydroxide to obtain cellulose acetate. The results of evaluating each physical property are shown in Table 1.
[0130] Comparative Example 2 Except for changing the maturation time to 100 minutes, the same procedure as in Comparative Example 1 was carried out to obtain cellulose acetate. The results of evaluation of each physical property are shown in Table 1.
[0131] Comparative Example 3 Hardwood prehydrolyzed kraft pulp with an α-cellulose content of 98.4% by weight was crushed into a cotton-like state using a disc refiner. In the pretreatment process, 100 parts by weight of the crushed pulp (moisture content 7.0%) was sprayed with 33 parts by weight of acetic acid maintained at 25°C, mixed well, and then left to stand for 2 hours for activation. In the esterification process, the pretreated activated pulp was added to a mixed solution consisting of 364 parts by weight of acetic acid, 244 parts by weight of acetic anhydride, and 6.6 parts by weight of concentrated sulfuric acid. The mixed solution was cooled to -8.9°C in advance. Based on the time point when the pulp was added to the mixed solution, it took 48 minutes to adjust the temperature from -8.9°C to a peak temperature of 50.9°C, and after 65 minutes, it was lowered by 5°C from the peak temperature. The neutralizing agent (24% by weight magnesium acetate) was added 152 minutes after the pulp was added to the mixed solution, and the amount of sulfuric acid (amount of aged sulfuric acid) was adjusted to 3.7 parts by weight, and the esterification process was completed. Furthermore, as the hydrolysis process, the reaction bath was heated to 50.9°C and hydrolysis was performed for 50 minutes. The hydrolysis reaction was stopped by neutralizing the sulfuric acid with magnesium acetate, and a reaction mixture containing cellulose acetate was obtained. The time from the time the pulp was added to the mixed solution to the time the neutralizing agent was added was defined as the esterification time. The cellulose acetate-containing reaction mixture was precipitated with about 300 parts by weight of a 10% dilute acetic acid aqueous solution per 100 parts by weight of the reaction mixture. After washing with water, calcium hydroxide was added as a stabilizer, and the cellulose acetate was obtained by filtering and drying. The results of evaluating each physical property are shown in Table 1.
[0132] Comparative Example 4 Cotton linters with an α-cellulose content of 98.4% by weight and a carboxyl group content of 0.8 meq / 100 g were used. In the pretreatment process, 100 parts by weight of disintegrated pulp (moisture content 7.0%) was sprayed with 43 acetic acid maintained at 25°C, mixed well, and then left to stand for 2 hours for activation. In the esterification process, the pretreated activated pulp was added to a mixed solution consisting of 386 parts by weight of acetic acid, 279 parts by weight of acetic anhydride, and 9.9 parts by weight of concentrated sulfuric acid. The mixed solution was cooled to -12.7°C in advance. Based on the time point when the pulp was added to the mixed solution, it took 62 minutes to adjust the peak temperature from -8.9°C to 38°C. 126 minutes after the time point when the pulp was added to the mixed solution, the addition of a neutralizer (24% by weight magnesium acetate) was started, and the amount of sulfuric acid (amount of aged sulfuric acid) was adjusted to 3.7 parts by weight, and the esterification process was completed. Furthermore, in the hydrolysis step, the reaction bath was heated to 50.9°C and hydrolysis was carried out for 50 minutes. The hydrolysis reaction was stopped by neutralizing the sulfuric acid with magnesium acetate, and a reaction mixture containing cellulose acetate was obtained. The time from the time when the pulp was added to the mixed solution until the neutralizing agent was added was defined as the esterification time. The cellulose acetate-containing reaction mixture was precipitated with about 300 parts by weight of a 10% dilute acetic acid aqueous solution per 100 parts by weight of the reaction mixture containing cellulose acetate. After washing with water, calcium hydroxide was added as a stabilizer, and the mixture was filtered and dried to obtain cellulose acetate. The results of evaluating each physical property are shown in Table 1.
[0133] Comparative Example 5 Sheet-like cellulose (cotton linter pulp) with an α-cellulose content of 97 wt% was processed with a disc refiner to obtain a cotton-like cellulose. Acetic acid was sprayed onto 100 parts by weight of the cotton-like cellulose (water content 8.0 wt%) in the ratio shown, stirred thoroughly, and allowed to stand at a temperature of 24°C for 60 minutes (first activation step). Furthermore, 30.24 parts of acetic acid containing 0.94 parts of sulfuric acid was added to the cellulose that had been subjected to the first activation step, and allowed to stand at 24°C for 45 minutes (second activation step). Then, 417.85 parts of acetic acid, 282.98 parts of acetic anhydride, and 8.72 parts of sulfuric acid were mixed with the cellulose that had been activated through the second activation step, and the mixture was kept at 15°C or less for 20 minutes, after which the temperature of the reaction system was raised to 35°C at a temperature rise rate of 0.31°C / min and held for 80 minutes to perform acetylation. Then, 0.15 parts by weight of acetic acid, 22.98 parts by weight of water, and 7.30 parts by weight of magnesium acetate were mixed and kept at a temperature of 61° C. for 95 minutes, and then 7.48 parts by weight of magnesium acetate, 20.94 parts by weight of acetic acid, and 21.44 parts of water were added to stop the aging reaction. The reaction bath was poured into dilute acetic acid with stirring to precipitate the product, which was then immersed in a dilute aqueous calcium hydroxide solution, filtered, and dried to obtain cellulose acetate.
[0134] (Examples 1 to 8, Comparative Examples 6 to 11) Sheet-like cellulose (hardwood pulp) was processed with a disc refiner to make it cotton-like. 100 parts by weight of cotton-like cellulose (water content 8.0% by weight) was sprayed with 32.71 parts by weight of acetic acid, thoroughly stirred, and allowed to stand at a temperature of 24°C for 60 minutes (activation step). 358.51 parts by weight of acetic acid, 214.99 parts by weight of acetic anhydride, and parts by weight of sulfuric acid A were mixed with the activated cellulose, and after holding at 15°C for 20 minutes, the temperature of the reaction system was raised to 45°C at a temperature rise rate of 0.31°C / min and held for 70 minutes to perform acetylation, producing cellulose triacetate. Next, 0.28 parts by weight of acetic acid, 89.55 parts by weight of water, and 13.60 parts by weight of magnesium acetate were added to stop the acetylation reaction. The amount of sulfuric acid A was appropriately adjusted within the range of 0.1 to 15 parts by weight to adjust the amount of sulfuric acid in the cellulose acetate to be synthesized. To the resulting reaction mixture, 0.06 parts by weight of acetic acid, parts by weight of water B, and 2.90 parts by weight of magnesium acetate were added, and the maturation reaction was carried out for C minutes at 85°C. The amount of water B added to the maturation reaction was in the range of 1 to 50 parts by weight, and the degree of substitution at the 2-, 3-, and 6-positions was adjusted. The maturation reaction time C was in the range of 5 to 120 minutes, and the degree of substitution of the cellulose acetate to be synthesized was adjusted. Cellulose acetate was obtained in this manner. The results of evaluating each physical property are shown in Table 1.
[0135] Example 9 9.5 parts by weight of cellulose acetate having a degree of substitution of 2.46 synthesized in Example 1 was heated at 110°C for 2 hours and dried, then added to 90 parts by weight of acetone and stirred at 25°C for 6 hours to dissolve the cellulose acetate. 0.5 parts by weight of magnesium aluminometasilicate powder, which is a basic additive, was added thereto as an additive, and further stirred at 25°C for 6 hours to prepare a dope for film production. This dope was poured onto a glass plate, cast with a bar coater, dried at 40°C for 30 minutes, and then peeled off the film from the glass plate and dried at 80°C for another 30 minutes to obtain a cellulose acetate composition film having a thickness of 30 μm. The results of evaluating each physical property are shown in Table 1.
[0136] Example 10 A cellulose acetate composition film having a thickness of 30 μm was obtained in the same manner as in Example 9, except that magnesium oxide was used as a basic additive, and the amount of cellulose acetate was 9.6 parts by weight and 0.4 parts by weight. The results of evaluating each physical property are shown in Table 1.
[0137] Example 11 A cellulose acetate composition film having a thickness of 30 μm was obtained in the same manner as in Example 9, except that 2.5 parts by weight of triacetin and 7.5 parts by weight of cellulose acetate were used as water-soluble additives instead of the basic additive. The results of evaluating each physical property are shown in Table 1.
[0138] Example 12 A cellulose acetate composition film having a thickness of 30 μm was obtained in the same manner as in Example 9, except that 0.5 parts by weight of magnesium oxide, which is a basic additive, 2.0 parts by weight of triacetin, which is a water-soluble additive, and 7.5 parts by weight of cellulose acetate were used as additives. The results of evaluating each physical property are shown in Table 1.
[0139] (Example 13) As an additive, 0.8 parts by weight of PHBH, which is a substance with excellent biodegradability in the ocean, and 9.2 parts by weight of cellulose acetate were used, melt-kneaded at 240°C using a twin-screw kneader, and a cellulose acetate composition film with a thickness of about 30 μm was obtained using a T-die mold of a Labo Plastomill. The results of evaluating each physical property are shown in Table 1.
[0140] [Table 1]
[0141] As shown in Table 1, the cellulose acetate compositions of the comparative examples, which have a high total degree of acetyl substitution, a low ratio τ of the sum of the degrees of acetyl substitution at the 2-position and the 3-position to the degree of acetyl substitution at the 6-position, or a low amount of sulfuric acid, are all poor in biodegradability. On the other hand, the cellulose acetate compositions of the examples are excellent in biodegradability in seawater.
Claims
1. A cellulose acetate having a total degree of acetyl substitution of 2.7 or less, and a ratio τ of the sum of the degrees of acetyl substitution at the 2-position and the 3-position to the degree of acetyl substitution at the 6-position in the total degree of acetyl substitution of 2.0 or more, The cellulose acetate composition further comprises, as an additive, 1 to 30% by weight of a substance having a pH of 8 or more in a 1% by weight aqueous solution at 20°C, and / or 5 to 30% by weight of a substance soluble in water at 20°C at a concentration of 2% by weight or more.
2. 2. The cellulose acetate composition according to claim 1, wherein the amount of sulfuric acid in the cellulose acetate is more than 20 ppm and not more than 400 ppm.
3. 3. The cellulose acetate composition according to claim 1, wherein the total content of the additives is 5 to 40% by weight.
4. 3. The cellulose acetate composition according to claim 1, wherein the substance having a pH of 8 or more in a 1% by weight aqueous solution at 20°C is magnesium oxide.
5. 3. The cellulose acetate composition according to claim 1, wherein the substance soluble in water at 20°C in an amount of 2% by weight or more is triacetin.
6. 3. The cellulose acetate composition according to claim 1, wherein the cellulose acetate composition is mixed with water to give a slurry having a pH of 7 to 13 at 20°C.
7. 3. The cellulose acetate composition according to claim 1, wherein the amount of sulfuric acid in the cellulose acetate is 150 ppm or more.
8. The cellulose acetate composition according to claim 1 or 2, wherein the cellulose acetate has a cellulose acetate type II crystal structure.
9. 2. The cellulose acetate composition according to claim 1, wherein the ratio τ of the sum of the acetyl substitution degrees at the 2-position and the acetyl substitution degrees at the 3-position to the acetyl substitution degree at the 6-position in the total acetyl substitution degree is 2.0 or more and 2.5 or less.
10. the substance that dissolves in water at 20° C. at 2% by weight or more is selected from the group consisting of amide group-containing vinyl polymers, polysaccharides, and plasticizers for cellulose acetate; 2. The cellulose acetate composition according to claim 1, wherein the plasticizer for the cellulose acetate is an ester compound of glycerin and a fatty acid having 2 to 4 carbon atoms.
Citation Information
Patent Citations
Biodegradable cellulose ester composition and molded product therefrom
JP1995076632A
Biodegradable film or sheet and processed product of the same film or sheet
JP1997241425A
Cellulose ester excellent in solubility
JP1997286801A
Acetyl cellulose resin composition and its production method
JP2002030182A
Cellulose ester film, long size optical retardation film, optical film and method for manufacturing them and polarizing plate and display device using them
JP2002062430A