Polyvinyl Acetal Resin

A polyvinyl acetal resin with controlled diffuse transmittance and specific structural adjustments addresses the issue of undissolved particles in ceramic green sheets, resulting in tougher and more reliable ceramic capacitors with fewer defects.

JP7557568B2Active Publication Date: 2024-09-27SEKISUI CHEMICAL CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023044043
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-03-27
Filing Date
2023-03-20
Publication Date
2024-09-27
Estimated Expiration
2041-03-22

AI Technical Summary

Technical Problem

Conventional polyvinyl acetal resins used in ceramic green sheets for multilayer ceramic capacitors fail to sufficiently remove finer undissolved substances, leading to reduced toughness and increased sheet defects, which affects the reliability and quality of the capacitors.

Method used

A polyvinyl acetal resin with a maximum diffuse transmittance of 2.0% or less in the visible light region, adjusted by controlling the degree of crystallinity, saponification, acetalization conditions, and hydroxyl and acetal group content, is used to minimize undissolved particles, enhancing the toughness and reliability of ceramic green sheets.

Benefits of technology

The resin results in ceramic green sheets with fewer undissolved particles, improved toughness, and higher reliability, enabling the production of high-quality multilayer ceramic capacitors with reduced defects and enhanced productivity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007557568000005
    Figure 0007557568000005
  • Figure 0007557568000006
    Figure 0007557568000006
  • Figure 0007557568000001
    Figure 0007557568000001
Patent Text Reader

Abstract

Provided is a polyvinyl acetal resin which, when dissolved in an organic solvent, produces little fine undissolved matter, and when used as a binder for ceramic green sheets, can provide ceramic green sheets with excellent toughness, and can be used to produce ceramic capacitors with excellent reliability. [Solution] A polyvinyl acetal resin having a maximum diffuse transmittance of 2.0% or less in the visible light range measured using a D65 light source, a 10-degree field of view, and a thickness of 5 mm.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a polyvinyl acetal resin which, when dissolved in an organic solvent, produces little fine undissolved matter, and in particular, when used as a binder for ceramic green sheets, can give ceramic green sheets having excellent toughness, and can be used to fabricate ceramic capacitors having excellent reliability. [Background technology]

[0002] 2. Description of the Related Art In recent years, electronic components mounted in various electronic devices have become smaller and more laminated, and laminated electronic components such as multilayer circuit boards, laminated coils, and laminated ceramic capacitors are widely used. Among them, multilayer ceramic capacitors are generally manufactured through the following steps. First, a plasticizer, a dispersant, etc. are added to a solution in which a binder resin such as polyvinyl butyral resin or poly(meth)acrylic acid ester resin is dissolved in an organic solvent, and then a ceramic raw material powder is added and mixed uniformly with a mixing device such as a bead mill or a ball mill to obtain a ceramic slurry composition having a certain viscosity after defoaming. This slurry composition is cast onto a support surface such as a release-treated polyethylene terephthalate film or a SUS plate using a doctor blade, reverse roll coater, etc., and the volatile matter such as the solvent is distilled off by heating, etc., and then peeled off from the support to obtain a ceramic green sheet. Next, a conductive paste that will become the internal electrodes is applied to the obtained ceramic green sheets by screen printing, and multiple sheets are alternately stacked and heated and pressed to produce a laminate. After that, a process to thermally decompose and remove the binder resin components and the like contained in the laminate, that is, a so-called degreasing process, is performed, and external electrodes are sintered onto the end faces of the ceramic sintered body obtained by firing to obtain a multilayer ceramic capacitor.

[0003] Polyvinyl acetal resins used in the preparation of ceramic green sheets are generally used as solutions dissolved in organic solvents such as methyl ethyl ketone, toluene, alcohol, and mixtures thereof. However, when conventional polyvinyl acetal resins are dissolved in organic solvents, a small amount of undissolved matter is generated. When such undissolved matter is present, when the polyvinyl acetal resins are used in multilayer ceramic capacitors, voids tend to remain in the degreasing and firing processes, and the dispersibility of ceramic powders and the like is reduced, resulting in reduced electrical properties of the resulting products. For this reason, when using polyvinyl acetal resin for ceramic green sheets, it was necessary to mix it with organic or inorganic compounds, dissolve it in an organic solvent, and then perform a filtration process to remove any undissolved materials.

[0004] In response to this, Patent Document 1 proposes a polyvinyl acetal resin in which a reduction rate of the filtration flow rate is less than 10% when a polyvinyl acetal resin solution, which is prepared by dissolving the polyvinyl acetal resin in a 1:1 mixed solvent of methyl ethyl ketone and / or toluene and ethanol to prepare a 5 wt % solution, is filtered using a filter with a mesh size of 5 μm under conditions of a filtration temperature of 25° C. and a filtration pressure of 10 mmHg. It is also proposed that the use of such a polyvinyl acetal resin results in less undissolved matter when dissolved in an organic solvent, and the filtration time can be shortened, thereby improving productivity. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2005-325342 A Summary of the Invention [Problem to be solved by the invention]

[0006] Meanwhile, in recent years, with the increasing functionality and miniaturization of electronic devices, multilayer ceramic capacitors are being required to have larger capacitance and smaller size. In order to meet such demands, it is necessary to thoroughly remove finer undissolved matter, but even with the polyvinyl acetal resin described in Patent Document 1, it is not possible to thoroughly remove finer undissolved matter, resulting in problems such as a decrease in the toughness of the ceramic green sheet and an inability to sufficiently suppress sheet defects.

[0007] An object of the present invention is to provide a polyvinyl acetal resin which, when dissolved in an organic solvent, produces little fine undissolved matter, and, particularly, when used as a binder for ceramic green sheets, can give ceramic green sheets having excellent toughness, and can be used to fabricate ceramic capacitors having excellent reliability. [Means for solving the problem]

[0008] The present invention is a polyvinyl acetal resin having a maximum diffuse transmittance in the visible light region of 2.0% or less, measured using a D65 light source, a 10-degree visual field, and a thickness of 5 mm. The present invention will be described in detail below.

[0009] As a result of intensive research, the present inventors have found that a polyvinyl acetal resin having a maximum diffuse transmittance of 2.0% or less in the visible light region measured by a predetermined measuring method leaves little undissolved matter when dissolved in an organic solvent. They have also found that by using such a polyvinyl acetal resin as a binder resin for a ceramic green sheet, it is possible to produce a ceramic green sheet that is less likely to cause sheet defects and is capable of producing a highly reliable multilayer ceramic capacitor, and have completed the present invention.

[0010] The polyvinyl acetal resin of the present invention has a maximum diffuse transmittance of 2.0% or less in the visible light region measured with a D65 light source, a 10-degree visual field, and a thickness of 5 mm. In the present invention, the thickness of 5 mm is set to a long optical path, allowing minute differences to be detected. The resin having a maximum diffuse transmittance of 2.0% or less is assumed to have a uniform structure, and when dissolved in an organic solvent, it is possible to reduce fine undissolved matter. Furthermore, when used as a binder for ceramic green sheets, it is possible to obtain ceramic green sheets having excellent toughness, and it is possible to fabricate ceramic capacitors having excellent reliability. The maximum value of the above-mentioned diffuse transmittance is preferably 0.3% or more, and is preferably 1.7% or less, and more preferably 1.6% or less. The maximum value of the diffuse transmittance can be measured, for example, by the following method: Specifically, the polyvinyl acetal resin of the present invention is placed on a glass plate so that the thickness after heating and melting is 5 mm, and the resin is sandwiched between other glass plates and heated and melted to prepare a sample. The temperature and pressure during the heating and melting are not particularly limited, but a compression molding machine is used at a temperature of 140 to 160°C and a pressure of 1.0 to 8.0 kg / m 2 Under these conditions, the sample is selected when it is visually confirmed that there are no air bubbles remaining in the molten resin. The sample is prepared in an environment with a room temperature of 23°C and a humidity of 50%. The diffuse transmittance of the obtained sample is measured for each wavelength in the visible light range with a D65 light source and a 10-degree visual field using a spectrophotometer, and the maximum value is calculated. The above-mentioned diffuse transmittance means the ratio of the amount of light transmitted in a direction other than the straight-forward direction to the amount of light incident on the sample. In this specification, the visible light region is defined as a wavelength range of 360 to 740 nm. The glass plate may be, for example, clear float glass having a thickness of 2.5 mm, a width of 50 mm, a length of 50 mm, a maximum diffuse transmittance of 0.2% to 0.35% and an average diffuse transmittance of 0.2% to 0.3% in the visible light region measured with a 10-degree field of view using a D65 light source, and a lightness index L* of 2.0 to 2.5 against a black background. As the spectrophotometer, for example, a "CM-5" manufactured by Konica Minolta can be used. In the measurement using the "CM-5," ​​a sample is fixed using a "Transmittance Sample Holder: CM-A96" manufactured by Konica Minolta. The measurement environment is a room temperature of 23°C and a humidity of 50%.

[0011] The maximum value of the diffuse transmittance in the above-mentioned visible light region can be adjusted by appropriately setting the degree of crystallinity and degree of saponification of the raw material polyvinyl alcohol resin, the conditions of the acetalization reaction, the amount of acetal groups in the polyvinyl acetal resin, the amount of hydroxyl groups, etc.

[0012] Moreover, the average value of the diffuse transmittance in the visible light region is preferably 0.3% or more, preferably 1.0% or less, and more preferably 0.9% or less. Resins with an average diffuse transmittance of 1.0% or less are expected to have a uniform structure and have the advantage that when dissolved in an organic solvent, there is little fine undissolved matter, which can reduce defects in the green sheet. The average diffuse transmittance can be determined, for example, in the same manner as for the maximum diffuse transmittance, by measuring the diffuse transmittance at each wavelength and calculating the average value.

[0013] The average diffuse transmittance in the visible light region can be adjusted by appropriately setting, for example, the degree of crystallinity and degree of saponification of the raw material polyvinyl alcohol resin, the conditions of the acetalization reaction, the amount of acetal groups in the polyvinyl acetal resin, and the amount of hydroxyl groups.

[0014] The polyvinyl acetal resin of the present invention preferably has a ratio of the average value of the diffuse transmittance in the above-mentioned visible light region to the minimum value of the diffuse transmittance in the wavelength range of 550 to 740 nm of 1.2 or more. When the diffuse transmittance ratio is 1.2 or more, it can be considered that there are few impurities and that the disturbance in the spectral distribution of the light source is small, and therefore defects in the green sheet can be reduced. The above-mentioned diffuse transmittance ratio is more preferably 1.25 or more and is preferably 5 or less. The minimum value of diffuse transmittance in the wavelength range of 550 to 740 nm can be determined, for example, in the same manner as for the maximum value of diffuse transmittance, by preparing a sample, measuring the diffuse transmittance of each wavelength in the wavelength range of 550 to 740 nm at a 10-degree visual field using a spectrophotometer with a D65 light source, and taking the minimum value.

[0015] The minimum value of the diffuse transmittance in the wavelength range of 550 to 740 nm can be adjusted, for example, by appropriately setting the degree of crystallinity and degree of saponification of the raw material polyvinyl alcohol resin, the conditions of the acetalization reaction, the amount of acetal groups in the polyvinyl acetal resin, the amount of hydroxyl groups, etc.

[0016] The polyvinyl acetal resin of the present invention preferably has a lightness index L* of 10 or less on a black background. Resins having a lightness index L* of 10 or less have fewer impurities and a smaller proportion of diffused light, and therefore have the advantage of being able to reduce defects in the green sheet. The lightness index L* is preferably 2.5 or more, and more preferably 8 or less. The lightness index L* is an index that indicates the lightness or darkness of a color tone. When the lightness index L* value is large, the color tone becomes lighter, and when the lightness index L* value is small, the color tone becomes darker. The lightness index L* can be measured using a spectrophotometer in accordance with JIS Z 8722:2009.

[0017] The polyvinyl acetal resin of the present invention is dissolved in a 1:1 mixed solution of ethanol and toluene at a concentration of 0.2% by weight, and the particle size distribution of the solution is measured using a particle counter. The ratio of particles having a diameter of 0.5 to 1.0 μm is 4.42 × 10 per 100 volume percent of the resin solution. -8The particle volume is determined by counting the number of particles having a diameter of 0.5 to 1.0 μm using a particle counter, calculating the volume of the particles having a diameter of 0.5 to 1.0 μm assuming that the particles have a diameter of 0.75 μm and are true spheres, and then calculating the proportion (volume %) of particles having a diameter of 0.5 to 1.0 μm based on the number and volume of the particles. The above ratio is 4.42 x 10 -8 When the content is 50% by volume or less, the filtration time can be shortened, the uniformity of the slurry is improved, a smoother green sheet can be produced, and sheet defects such as cracks are less likely to occur, so that dielectric breakdown is less likely to occur, which is advantageous in that the reliability of the obtained multilayer ceramic capacitor is improved. The above ratio is 3.31 x 10 -8 The lower limit of the above ratio is not particularly limited, and the lower the ratio the better, with 0 volume % being preferred. As the particle counter, for example, "KS-42C" manufactured by Rion Co., Ltd. can be used.

[0018] The volume ratio of the particles having a diameter of 0.5 to 1.0 μm can be adjusted by appropriately setting, for example, the degree of crystallinity and degree of saponification of the raw material polyvinyl alcohol resin, the conditions of the acetalization reaction, the amount of acetal groups in the polyvinyl acetal resin, and the amount of hydroxyl groups.

[0019] With respect to the polyvinyl acetal resin of the present invention, from the viewpoint of maintaining mechanical strength when a thin film ceramic green sheet is produced, the average polymerization degree has a preferable lower limit of 300, more preferably 600, and from the viewpoint of solubility in organic solvents and dissolution viscosity, the average polymerization degree is preferably 8,000, more preferably 7,000. The average degree of polymerization can be measured in accordance with JIS K 6726.

[0020] The polyvinyl acetal resin of the present invention preferably has a structural unit having an acetal group represented by the following formula (1), a structural unit having a hydroxyl group represented by the following formula (2), and a structural unit having an acetyl group represented by the following formula (3).

[0021] [ka]

[0022] In the above formula (1), R 1 represents a hydrogen atom or an alkyl group having 1 to 20 carbon atoms.

[0023] In the above formula (1), R 1 When is an alkyl group having 1 to 20 carbon atoms, examples of the alkyl group include a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, an isobutyl group, a sec-butyl group, a tert-butyl group, a pentyl group, a hexyl group, a heptyl group, a 2-ethylhexyl group, an octyl group, a nonyl group, a decyl group, an undecyl group, a dodecyl group, a tridecyl group, a tetradecyl group, a pentadecyl group, an octadecyl group, etc. Among these, a methyl group and an n-propyl group are preferable.

[0024] In the polyvinyl acetal resin of the present invention, the content of the structural unit having the acetal group represented by the above formula (1) (hereinafter also referred to as the "acetal group amount") is preferably 45 mol % in lower limit and 78 mol % in upper limit. When the amount of acetal groups is 45 mol % or more, the solubility in organic solvents can be improved, and when the amount of acetal groups is 78 mol % or less, the polyvinyl acetal resin can have excellent toughness. The lower limit of the acetal group amount is more preferably 46 mol %, still more preferably 48 mol %, and the upper limit is more preferably 76 mol %, still more preferably 74 mol %. The amount of acetal groups can be measured, for example, by NMR. Regarding the method for calculating the amount of acetal groups, since the acetal groups of polyvinyl acetal resin are obtained by acetalizing two hydroxyl groups of polyvinyl alcohol, the method of counting the two acetalized hydroxyl groups is used.

[0025] In the polyvinyl acetal resin of the present invention, the content of the structural unit having a hydroxyl group represented by the above general formula (2) (hereinafter also referred to as the "hydroxyl group amount") is preferably 23 mol % in lower limit and 39 mol % in upper limit. When the amount of hydroxyl groups is 23 mol % or more, the polyvinyl acetal resin can have excellent toughness.When the amount of hydroxyl groups is 39 mol % or less, the solubility in organic solvents can be sufficiently improved. The lower limit of the hydroxyl group amount is more preferably 24 mol %, still more preferably 25 mol %, and the upper limit is more preferably 38 mol %, still more preferably 37 mol %. The amount of hydroxyl groups can be measured, for example, by NMR.

[0026] In the polyvinyl acetal resin of the present invention, the content of the structural unit having an acetyl group represented by the above general formula (3) (hereinafter also referred to as the "acetyl group amount") is preferably 0.6 mol % in lower limit and 18 mol % in upper limit. When the amount of acetyl groups is 0.6 mol% or more, the increase in viscosity of the composition for ceramic green sheets due to intramolecular and intermolecular hydrogen bonds of hydroxyl groups in the polyvinyl acetal resin can be suppressed.When the amount of acetyl groups is 18 mol% or less, the flexibility of the polyvinyl acetal resin is not excessively increased, and the handleability can be improved. The lower limit of the amount of acetyl groups is more preferably 1.0 mol %, and the upper limit thereof is more preferably 16 mol %. The amount of acetyl groups can be measured, for example, by NMR.

[0027] The polyvinyl acetal resin of the present invention has a weight average molecular weight (Mw) of preferably 40,000 at its lower limit, more preferably 70,000 at its lower limit, and preferably 1,400,000 at its upper limit, more preferably 1,200,000 at its upper limit. The polyvinyl acetal resin of the present invention has a number average molecular weight (Mn) of preferably 15,000 at its lower limit, more preferably 40,000 at its lower limit, and preferably 500,000 at its upper limit, more preferably 400,000 at its upper limit. The polyvinyl acetal resin of the present invention has a ratio (Mw / Mn) of the weight average molecular weight (Mw) to the number average molecular weight (Mn) of preferably 2.0 lower limit, more preferably 2.2 lower limit, preferably 4.0 upper limit, more preferably 3.7 upper limit. The Mw and Mn can be measured, for example, by gel permeation chromatography (GPC) using an appropriate standard (e.g., polystyrene standard). Columns used for measuring the Mw and Mn include, for example, TSKgel SuperHZM-H.

[0028] The polyvinyl acetal resin of the present invention can usually be produced by acetalizing a polyvinyl alcohol resin.

[0029] As the polyvinyl alcohol resin, for example, a conventionally known polyvinyl alcohol resin such as a resin produced by saponifying a polyvinyl acetate resin with an alkali, an acid, aqueous ammonia or the like can be used. The polyvinyl alcohol resin may be fully saponified, but it does not have to be fully saponified as long as there is at least one unit having two consecutive hydroxyl groups at the meso and racemo positions at at least one position in the main chain, and may be a partially saponified polyvinyl alcohol resin. In addition, as the polyvinyl alcohol resin, a copolymer of vinyl alcohol and a monomer copolymerizable with vinyl alcohol, such as an ethylene-vinyl alcohol copolymer resin or a partially saponified ethylene-vinyl alcohol copolymer resin, may also be used. The polyvinyl acetate resin may be, for example, an ethylene-vinyl acetate copolymer.

[0030] The polyvinyl alcohol resin preferably has a crystallinity of 37% or less, and more preferably 33% or less. By using the above polyvinyl alcohol resin, the number of undissolved matters measured by the above method can be kept within a predetermined range. The crystallinity can be measured by differential scanning calorimetry (DSC).

[0031] The polyvinyl alcohol resin preferably has a degree of saponification of 70 mol % or more and 99.4 mol % or less, and more preferably 78 mol % or more and 98 mol % or less. By using the above polyvinyl alcohol resin, the number of undissolved matters measured by the above method can be kept within a predetermined range.

[0032] The acetalization can be carried out by a known method, and is preferably carried out in a water solvent, in a mixed solvent of water and an organic solvent compatible with water, or in an organic solvent. As the organic solvent compatible with water, for example, an alcohol-based organic solvent can be used. Examples of the organic solvent include alcohol-based organic solvents, aromatic organic solvents, aliphatic ester-based solvents, ketone-based solvents, lower paraffin-based solvents, ether-based solvents, amide-based solvents, and amine-based solvents. Examples of the alcohol-based organic solvent include methanol, ethanol, n-propanol, isopropanol, n-butanol, and tert-butanol. Examples of the aromatic organic solvent include xylene, toluene, ethylbenzene, and methyl benzoate. Examples of the aliphatic ester solvent include methyl acetate, ethyl acetate, butyl acetate, methyl propionate, ethyl propionate, methyl butyrate, ethyl butyrate, methyl acetoacetate, and ethyl acetoacetate. Examples of the ketone solvent include acetone, methyl ethyl ketone, methyl isobutyl ketone, cyclohexanone, methylcyclohexanone, benzophenone, and acetophenone. Examples of the lower paraffin solvent include hexane, pentane, octane, cyclohexane, and decane. Examples of the ether solvent include diethyl ether, tetrahydrofuran, ethylene glycol dimethyl ether, ethylene glycol diethyl ether, and propylene glycol diethyl ether. Examples of the amide solvent include N,N-dimethylformamide, N,N-dimethylacetamide, N-methylpyrrolidone, and acetanilide. Examples of the amine solvent include ammonia, trimethylamine, triethylamine, n-butylamine, di-n-butylamine, tri-n-butylamine, aniline, N-methylaniline, N,N-dimethylaniline, and pyridine. These solvents may be used alone or in combination of two or more. Among these, ethanol, n-propanol, isopropanol, and tetrahydrofuran are particularly preferred from the viewpoints of solubility in the resin and ease of purification.

[0033] The acetalization is preferably carried out in the presence of an acid catalyst. The acid catalyst is not particularly limited, and examples thereof include mineral acids such as sulfuric acid, hydrochloric acid, nitric acid, and phosphoric acid, carboxylic acids such as formic acid, acetic acid, and propionic acid, and sulfonic acids such as methanesulfonic acid, ethanesulfonic acid, benzenesulfonic acid, and paratoluenesulfonic acid. These acid catalysts may be used alone or in combination of two or more compounds. Among them, hydrochloric acid, nitric acid, and sulfuric acid are preferred, and hydrochloric acid is particularly preferred.

[0034] The aldehyde used in the acetalization reaction may be an aldehyde having a chain aliphatic group, a cyclic aliphatic group, or an aromatic group having 1 to 10 carbon atoms. Any known aldehyde may be used as the aldehyde. The aldehyde used in the acetalization reaction is not particularly limited, and may be, for example, an aliphatic aldehyde, an aromatic aldehyde, or the like. Examples of the aliphatic aldehyde include formaldehyde, acetaldehyde, propionaldehyde, n-butyraldehyde, isobutyraldehyde, n-valeraldehyde, n-hexylaldehyde, 2-ethylbutyraldehyde, 2-ethylhexylaldehyde, n-heptylaldehyde, n-octylaldehyde, n-nonylaldehyde, n-decylaldehyde, and amylaldehyde. Examples of the aromatic aldehyde include benzaldehyde, cinnamaldehyde, 2-methylbenzaldehyde, 3-methylbenzaldehyde, 4-methylbenzaldehyde, p-hydroxybenzaldehyde, m-hydroxybenzaldehyde, phenylacetaldehyde, and β-phenylpropionaldehyde. These aldehydes may be used alone or in combination of two or more. Among them, formaldehyde, acetaldehyde, butyl aldehyde, 2-ethylhexyl aldehyde, and n-nonyl aldehyde are preferable as aldehydes, because they have excellent acetalization reactivity, bring about sufficient internal plasticizing effect to the resin produced, and as a result, can impart good flexibility. In addition, formaldehyde, acetaldehyde, and butyl aldehyde are more preferable, because they can provide an adhesive composition that is particularly excellent in impact resistance and adhesion to metals.

[0035] The amount of the aldehyde to be added can be appropriately set according to the amount of acetal groups in the target polyvinyl acetal resin. In particular, it is preferable to add 55 mol% to 95 mol%, preferably 60 mol% to 90 mol%, based on 100 mol% of polyvinyl alcohol, because this allows the acetalization reaction to proceed efficiently and makes it easy to remove unreacted aldehyde.

[0036] The retention time after the reaction depends on other conditions, but is preferably 1.5 hours or more, and more preferably 2 hours or more. By setting the retention time in the above range, the acetalization reaction can be sufficiently progressed. The holding temperature after the reaction is preferably 15° C. or higher, and more preferably 20° C. or higher. By setting the holding temperature in the above range, the acetalization reaction can be sufficiently progressed. The holding temperature is preferably 70° C. or lower.

[0037] A composition for a ceramic green sheet can be prepared by mixing the polyvinyl acetal resin of the present invention and an organic solvent.

[0038] The organic solvent is not particularly limited, and may be any solvent capable of dissolving the polyvinyl acetal resin, such as ketones, including acetone, methyl ethyl ketone, dipropyl ketone, and diisobutyl ketone. Other examples include alcohols, such as methanol, ethanol, isopropanol, and butanol, and aromatic hydrocarbons, such as toluene and xylene. Other examples include esters, such as methyl propionate, ethyl propionate, butyl propionate, methyl butanoate, ethyl butanoate, butyl butanoate, methyl pentanoate, ethyl pentanoate, butyl pentanoate, methyl hexanoate, ethyl hexanoate, butyl hexanoate, 2-ethylhexyl acetate, and 2-ethylhexyl butyrate. Other examples include methyl cellosolve, ethyl cellosolve, butyl cellosolve, terpineol, dihydroterpineol, butyl cellosolve acetate, butyl carbitol acetate, terpineol acetate, and dihydroterpineol acetate. In particular, alcohols, ketones, aromatic hydrocarbons and mixed solvents thereof are preferred in terms of coating and drying properties, with a mixed solvent of ethanol and toluene and a mixed solvent of methyl ethyl ketone and toluene being more preferred.

[0039] The content of the organic solvent in the ceramic green sheet composition is set according to the type of polyvinyl acetal resin used, and is not particularly limited, but if it is too small, it is difficult to exhibit the solubility required for kneading. Also, if it is too large, the viscosity of the ceramic green sheet composition becomes too low, which may cause poor handling when producing a ceramic green sheet. For this reason, the content of the organic solvent is preferably 20% by weight or more and 80% by weight or less.

[0040] The ceramic green sheet composition may contain a plasticizer. By adding a plasticizer, the mechanical strength and flexibility of the resulting ceramic green sheet can be significantly improved. Examples of the plasticizer include phthalic acid diesters such as dioctyl phthalate (DOP) and dibutyl phthalate (DBP), adipic acid diesters such as dioctyl adipate, and alkylene glycol diesters such as triethylene glycol-di-2-ethylhexanoate, tetraethylene glycol-di-2-ethylhexanoate, triethylene glycol-di-2-ethylbutyrate, tetraethylene glycol-di-2-ethylbutyrate, tetraethylene glycol-di-heptanoate, and triethylene glycol-di-heptanoate.

[0041] In the composition for ceramic green sheet, the content of the plasticizer relative to 100 parts by weight of the polyvinyl acetal resin is preferably 7 parts by weight in lower limit, more preferably 8.5 parts by weight in lower limit, preferably 18 parts by weight in upper limit, more preferably 13.5 parts by weight in upper limit.

[0042] The ceramic green sheet composition may contain other resins such as polyvinyl acetal resins other than the polyvinyl acetal resin of the present invention, acrylic resins, ethyl cellulose, etc., within the range that does not impair the effects of the present invention. In such a case, the content of the polyvinyl acetal resin of the present invention relative to the total binder resins is preferably 50% by weight or more.

[0043] To the composition for ceramic green sheet, ceramic powder, dispersing agent, antioxidant, ultraviolet absorber, surfactant, filler, etc. may be appropriately added as needed, and in some cases, a small amount of other resin such as acrylic resin or urethane resin may be added.

[0044] The ceramic powder includes powders of oxides or non-oxides of metals or non-metals used in the manufacture of ceramics. The composition of these powders may be a single composition, a compound state, or a mixture. The constituent elements of the metal oxide or non-oxide may be a single element or a plurality of elements, both as cations and anions, and may further include additives added to improve the properties of the oxide or non-oxide. Specific examples of the oxides or non-oxides include oxides, carbides, nitrides, borides, and sulfides of Li, K, Mg, B, Al, Si, Cu, Ca, Sr, Ba, Zn, Cd, Ga, In, Y, lanthanides, actinides, Ti, Zr, Hf, Bi, V, Nb, Ta, W, Mn, Fe, Co, Ni, and the like. In addition, specific oxide powders containing multiple metal elements, usually called double oxides, can be classified based on their crystal structure as follows: those with a perovskite structure include NaNbO3, SrZrO3, PbZrO3, SrTiO3, BaZrO3, PbTiO3, BaTiO3, etc.; those with a spinel structure include MgAl2O4, ZnAl2O4, CoAl2O4, NiAl2O4, MgFe2O4, etc.; those with an ilmenite structure include MgTiO3, MnTiO3, FeTiO3, etc.; and those with a garnet structure include GdGa5O4, GdGa5O5, etc. 12 , Y6Fe5O 12 Among these, the modified polyvinyl acetal resin of the present invention exhibits high properties when mixed with BaTiO3 powder in a ceramic green sheet.

[0045] The average particle size of the ceramic powder is not particularly limited, but for example, for producing a thin ceramic green sheet (thickness 5 μm or less), it is preferably 0.5 μm or less.

[0046] The method for producing the composition for ceramic green sheets is not particularly limited, and examples thereof include a method in which the polyvinyl acetal resin of the present invention, an organic solvent, and various additives added as necessary are mixed using various mixers such as a ball mill, a blender mill, and a three-roll mill.

[0047] After the ceramic green sheet composition is applied, it is heated and dried to obtain a resin sheet.

[0048] The method for applying the composition for a ceramic green sheet is not particularly limited, and examples thereof include a method using a roll coater, a die coater, a curtain coater, etc. As for other specific methods, conventionally known methods can be used.

[0049] The resin sheet containing the ceramic powder can be used as a ceramic green sheet. The ceramic green sheets can be used to manufacture ceramic electronic components. For example, the ceramic electronic components can be manufactured by carrying out a step of applying a paste for electrode layers to the surfaces of the ceramic green sheets, and a step of stacking the ceramic green sheets on which the electrode layers have been formed, and heat-pressing the stack to obtain a laminate, followed by degreasing and firing the laminate.

[0050] The ceramic electronic components are not particularly limited, and examples thereof include multilayer ceramic capacitors, multilayer ceramic inductors, capacitors, piezoelectric actuators, multilayer varistors, multilayer thermistors, EMI filters, aluminum nitride multilayer substrates, alumina multilayer substrates, etc. Such multilayer ceramic capacitors also constitute the present invention.

[0051] The method for producing a ceramic electronic component includes a step of applying a paste for electrode layers to the surfaces of the ceramic green sheets. The electrode layer paste can be obtained by dissolving, for example, polyvinyl acetal resin, ethyl cellulose, acrylic resin, etc. as a binder resin in an organic solvent and dispersing conductive powder, etc. These resins may be used alone or in combination of two or more. The electrode layer paste containing polyvinyl acetal resin is preferred because it exhibits excellent adhesion to the ceramic green sheet in the heat-pressing step.

[0052] In the method for producing a ceramic electronic component, the above-mentioned ceramic green sheets having electrode layers formed thereon are produced, and then similarly produced ceramic green sheets having electrode layers formed thereon are stacked and heated and pressed to obtain a laminate, which is then degreased and fired, thereby obtaining a multilayer ceramic electronic component in which problems such as sheet attack and cracks are solved. The above-mentioned heat-pressure bonding step, and the steps of degreasing and firing the laminate are not particularly limited, and conventionally known methods can be used. Effect of the Invention

[0053] According to the present invention, it is possible to provide a polyvinyl acetal resin which, when dissolved in an organic solvent, produces little fine undissolved matter, and can improve productivity particularly when used as a binder for ceramic green sheets. It is also possible to obtain ceramic green sheets having excellent toughness, and which can be used to fabricate ceramic capacitors having excellent reliability. [Brief description of the drawings]

[0054] [Figure 1] FIG. 1 is a schematic diagram of a DSC curve. [Diagram 2] FIG. 2 is a graph showing the measurement results of the diffuse transmittance of the polyvinyl acetal resin obtained in Example 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0055] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.

[0056] Example 1 3000g of polyvinyl alcohol resin (average polymerization degree 1,800, saponification degree 98.7 mol%, crystallinity degree 34%) was added to 300g of pure water and dissolved by stirring at 90°C for about 2 hours. The solution was cooled to 40°C, and 200g of hydrochloric acid with a concentration of 35% by weight and 160g of n-butyl aldehyde were added to carry out an acetalization reaction, and the reaction product was precipitated. The reaction was then completed by holding at 40°C for 3 hours, and neutralization, washing with water and drying were carried out by the usual method to obtain a white powder of polyvinyl acetal resin. The crystallinity of the polyvinyl alcohol resin was measured by the following method. Specifically, the polyvinyl alcohol resin was subjected to differential scanning calorimetry under the following measurement conditions using a thermal analyzer (DSC6200R, manufactured by Hitachi High-Tech Science Corporation), and the heat of fusion during the second heating was measured to determine the degree of crystallinity. <Measurement conditions> 0℃ (5 min hold) → (1st heating at 10℃ / min heating rate) → 250℃ → (10℃ / min cooling rate) → 0℃ (5 min hold) → (2nd heating at 10℃ / min heating rate) → 250℃ The heat of fusion was calculated from the area of ​​the peak appearing between 100°C and 250°C during the second heating. The peak area was defined as the area of ​​the region surrounded by the straight line connecting points A and B and the DSC curve, as shown in Figure 1. Here, point A was defined as the point at which the DSC curve was separated from the straight line drawn along the linear approximation of the DSC curve from 170°C to the higher temperature side. Point B was defined as the point on the DSC curve that indicated the end temperature of melting. The degree of crystallinity was calculated assuming that the heat of fusion of a polyvinyl alcohol resin with a degree of crystallinity of 100% was 156 J / g.

[0057] Example 2 3100g of pure water was added to 300g of polyvinyl alcohol resin (average polymerization degree 1,800, saponification degree 84.5 mol%, crystallinity degree 13%), and the mixture was stirred at 90°C for about 2 hours to dissolve. The solution was cooled to 40°C, and 200g of hydrochloric acid with a concentration of 35% by weight and 140g of n-butyl aldehyde were added to carry out an acetalization reaction, and the reaction product was precipitated. The mixture was then held at 40°C for 3 hours to complete the reaction, and neutralized, washed with water, and dried in the usual manner to obtain a white powder of polyvinyl acetal resin.

[0058] Example 3 3100g of pure water was added to 300g of polyvinyl alcohol resin (average polymerization degree 700, saponification degree 98.4 mol%, crystallinity degree 28%), and the mixture was stirred at 90°C for about 2 hours to dissolve. The solution was cooled to 40°C, and 200g of hydrochloric acid with a concentration of 35% by weight and 160g of n-butyl aldehyde were added to carry out an acetalization reaction, and the reaction product was precipitated. The mixture was then held at 40°C for 3 hours to complete the reaction, and neutralized, washed with water, and dried in a conventional manner to obtain a white powder of polyvinyl acetal resin.

[0059] Example 4 300g of polyvinyl alcohol resin (average polymerization degree 3,100, saponification degree 98.8 mol%, crystallinity degree 32%) was added to 3100g of pure water and dissolved by stirring at 90°C for about 2 hours. The solution was cooled to 40°C, and 200g of hydrochloric acid with a concentration of 35% by weight and 170g of n-butyl aldehyde were added to carry out an acetalization reaction, and the reaction product was precipitated. The reaction was then completed by holding at 40°C for 3 hours, and neutralization, washing with water and drying were carried out by the usual method to obtain a white powder of polyvinyl acetal resin.

[0060] Example 5 300g of polyvinyl alcohol resin (average polymerization degree 4,800, saponification degree 98.5 mol%, crystallinity degree 32%) was added to 3100g of pure water and stirred at 90°C for about 2 hours to dissolve. This solution was cooled to 40°C, and 200g of hydrochloric acid with a concentration of 35% by weight and 180g of n-butyl aldehyde were added to carry out an acetalization reaction to precipitate the reaction product. The reaction was then completed by holding at 40°C for 3 hours, and neutralization, washing with water and drying were carried out by the usual method to obtain a white powder of polyvinyl acetal resin.

[0061] Example 6 300g of polyvinyl alcohol resin (average polymerization degree 2,000, saponification degree 89.0 mol%, crystallinity degree 17%) was added to 3100g of pure water and stirred at 90°C for about 2 hours to dissolve. This solution was cooled to 40°C, and 200g of hydrochloric acid with a concentration of 35% by weight and 140g of n-butyl aldehyde were added to carry out an acetalization reaction to precipitate the reaction product. The reaction was then completed by holding at 40°C for 3 hours, and neutralization, washing with water and drying were carried out by the usual method to obtain a white powder of polyvinyl acetal resin.

[0062] Example 7 3100g of pure water was added to 150g of polyvinyl alcohol resin (average polymerization degree 6,800, saponification degree 88.0 mol%, crystallinity degree 16%), and the mixture was stirred at 90°C for about 2 hours to dissolve. The solution was cooled to 40°C, and 200g of hydrochloric acid with a concentration of 35% by weight and 120g of n-butyl aldehyde were added to carry out an acetalization reaction to precipitate the reaction product. The mixture was then held at 40°C for 3 hours to complete the reaction, and neutralized, washed with water, and dried in the usual manner to obtain a white powder of polyvinyl acetal resin.

[0063] Example 8 300g of polyvinyl alcohol resin (average polymerization degree 1,800, saponification degree 98.7 mol%, crystallinity degree 34%) was added to 3100g of pure water and dissolved by stirring at 90°C for about 2 hours. The solution was cooled to 40°C, and 200g of hydrochloric acid with a concentration of 35% by weight and 160g of n-butyl aldehyde were added thereto to carry out an acetalization reaction, and the reaction product was precipitated. The reaction was then completed by holding at 35°C for 3 hours, and neutralization, washing with water and drying were carried out by the usual method to obtain a white powder of polyvinyl acetal resin.

[0064] Example 9 3100g of pure water was added to 300g of polyvinyl acetal resin (average polymerization degree 1,800, saponification degree 98.7 mol%, crystallinity degree 34%), and the mixture was stirred at 90°C for about 2 hours to dissolve. The solution was cooled to 40°C, and 200g of hydrochloric acid with a concentration of 35% by weight and 160g of n-butyl aldehyde were added to carry out an acetalization reaction, and the reaction product was precipitated. The mixture was then held at 40°C for 4 hours to complete the reaction, and neutralized, washed with water, and dried in the usual manner to obtain a white powder of polyvinyl acetal resin.

[0065] Comparative Example 1 3000g of pure water was added to 300g of polyvinyl alcohol resin (average polymerization degree 1,800, saponification degree 99.5 mol%, crystallinity degree 41%), and the mixture was stirred at 90°C for about 2 hours to dissolve. The solution was cooled to 40°C, and 200g of hydrochloric acid with a concentration of 35% by weight and 160g of n-butyl aldehyde were added to carry out an acetalization reaction, and the reaction product was precipitated. The mixture was then held at 40°C for 3 hours to complete the reaction, and neutralized, washed with water, and dried in the usual manner to obtain a white powder of polyvinyl acetal resin.

[0066] Comparative Example 2 3100g of pure water was added to 300g of polyvinyl alcohol resin (average polymerization degree 1,800, saponification degree 80.0 mol%, crystallinity degree 10%), and the mixture was stirred at 90°C for about 2 hours to dissolve. The solution was cooled to 40°C, and 200g of hydrochloric acid with a concentration of 35% by weight and 100g of n-butyl aldehyde were added to carry out an acetalization reaction to precipitate the reaction product. The mixture was then held at 40°C for 3 hours to complete the reaction, and neutralized, washed with water, and dried in the usual manner to obtain a white powder of polyvinyl acetal resin.

[0067] Comparative Example 3 3100g of pure water was added to 150g of polyvinyl alcohol resin (average polymerization degree 8,200, saponification degree 99.0 mol%, crystallinity degree 39%), and the mixture was stirred at 90°C for about 2 hours to dissolve. The solution was cooled to 40°C, and 200g of hydrochloric acid with a concentration of 35% by weight and 100g of n-butyl aldehyde were added to carry out an acetalization reaction, and the reaction product was precipitated. The mixture was then held at 40°C for 3 hours to complete the reaction, and neutralized, washed with water, and dried in the usual manner to obtain a white powder of polyvinyl acetal resin.

[0068] Comparative Example 4 3100g of pure water was added to 300g of polyvinyl alcohol resin (average polymerization degree 800, saponification degree 99.5 mol%, crystallinity degree 39%), and the mixture was stirred at 90°C for about 2 hours to dissolve. The solution was cooled to 40°C, and 200g of hydrochloric acid with a concentration of 35% by weight and 130g of n-butyl aldehyde were added to carry out an acetalization reaction to precipitate the reaction product. The mixture was then held at 40°C for 3 hours to complete the reaction, and neutralized, washed with water, and dried in the usual manner to obtain a white powder of polyvinyl acetal resin.

[0069] Comparative Example 5 300g of polyvinyl alcohol resin (average polymerization degree 1,800, saponification degree 98.5 mol%, crystallinity degree 35%) was added to 3100g of pure water and stirred at 90°C for about 2 hours to dissolve. This solution was cooled to 40°C, and 200g of hydrochloric acid with a concentration of 35% by weight and 180g of n-butyl aldehyde were added to carry out an acetalization reaction to precipitate the reaction product. The reaction was then completed by holding at 40°C for 3 hours, and neutralization, washing with water and drying were carried out by the usual method to obtain a white powder of polyvinyl acetal resin.

[0070] Comparative Example 6 3100g of pure water was added to 300g of polyvinyl alcohol resin (average polymerization degree 1,800, saponification degree 98.7 mol%, crystallinity degree 34%), and the mixture was stirred at 90°C for about 2 hours to dissolve. The solution was cooled to 40°C, and 200g of hydrochloric acid with a concentration of 35% by weight and 160g of n-butyl aldehyde were added to carry out an acetalization reaction, and the reaction product was precipitated. The mixture was then held at 10°C for 2 hours to complete the reaction, and neutralized, washed with water, and dried in the usual manner to obtain a white powder of polyvinyl acetal resin.

[0071] Comparative Example 7 3100g of pure water was added to 300g of polyvinyl acetal resin (average polymerization degree 1,800, saponification degree 98.7 mol%, crystallinity degree 34%), and the mixture was stirred at 90°C for about 2 hours to dissolve. The solution was cooled to 40°C, and 200g of hydrochloric acid with a concentration of 35% by weight and 160g of n-butyl aldehyde were added to carry out an acetalization reaction, and the reaction product was precipitated. The mixture was then held at 20°C for 0.5 hours to complete the reaction, and neutralized, washed with water, and dried in a conventional manner to obtain a white powder of polyvinyl acetal resin.

[0072] (evaluation) The polyvinyl acetal resins obtained in Examples 1 to 9 and Comparative Examples 1 to 7 were evaluated as follows. The results are shown in Tables 1 and 2.

[0073] (1) Evaluation of polyvinyl acetal resin (1-1) Amount of acetal groups, hydroxyl groups, and acetyl groups The obtained polyvinyl acetal resin was dissolved in DMSO-D6 at a concentration of 10% by weight. 13 The amounts of acetal groups, hydroxyl groups, and acetyl groups were measured using C-NMR.

[0074] (1-2) Diffuse transmittance in the visible light range Two glass plates (thickness 2.5 mm, width 50 mm, length 50 mm) were prepared, and the obtained white powder of polyvinyl acetal resin was sandwiched between the two glass plates so that the thickness after heating and melting would be 5 mm, and then heated and melted to prepare a sample. The sample was prepared in an environment of room temperature 23°C and humidity 50%. The diffuse transmittance of the obtained samples in the visible light region was measured with a spectrophotometer (Konica Minolta's "CM-5") using a D65 light source at a 10-degree field of view, and the maximum and average values ​​were calculated. The samples were fixed using a Konica Minolta's "Transmittance Sample Holder CM-A96". The measurement results of the diffuse transmittance of the polyvinyl acetal resin obtained in Example 1 are shown in FIG.

[0075] (1-3) Diffuse transmittance in the range of 550 to 740 nm In the same manner as in "(1-2) Diffuse transmittance in the visible light region", the diffuse transmittance was measured in the wavelength range of 550 to 740 nm, and the minimum value was determined.

[0076] (1-4) Lightness index L* The lightness index L* was measured against a black background using a spectrophotometer (Konica Minolta's "CM-5") according to a method in accordance with JIS Z 8722:2009.

[0077] (1-5) Number of particles with a diameter of 0.5 to 1.0 μm and volume concentration of undissolved matter (volume%) The obtained polyvinyl acetal resin was dissolved in a 1:1 ethanol-toluene mixed solution to a concentration of 0.2% by weight. The particle size distribution of 10 ml of the obtained solution was measured using a particle counter (KS-42C, manufactured by Rion Co., Ltd.) to count the number of particles with diameters of 0.5 to 1.0 μm per ml. The volume of the particles with diameters of 0.5 to 1.0 μm was calculated assuming that the particles were true spheres with diameters of 0.75 μm, and the proportion (volume %) of particles with diameters of 0.5 to 1.0 μm was calculated based on the measurement results obtained.

[0078] (2) Evaluation of resin sheets The obtained polyvinyl acetal resin was added to 90 parts by weight of an ethanol / toluene mixed solvent (weight ratio 1:1) and dissolved with stirring to obtain a composition for a resin sheet. The amount of polyvinyl acetal resin added was 10 parts by weight when the polyvinyl acetal resins (average polymerization degree 2000 or less) obtained in Examples 1 to 3, 6, 8, and 9 and Comparative Examples 1, 2, and 4 to 7 were used. When the polyvinyl acetal resins (average polymerization degree 2000 or more and 4000 or less) obtained in Example 4 were used, the amount was 5 parts by weight. When the polyvinyl acetal resins (average polymerization degree 4000 or more) obtained in Examples 5 and 7 and Comparative Example 3 were used, the amount was 2.5 parts by weight. The obtained composition for resin sheets was applied onto a release-treated PET film using a coater so that the thickness after drying would be 20 μm, and the film was dried by heating to prepare a measurement sample (resin sheet).

[0079] (2-1) Elastic modulus The obtained measurement samples were subjected to measurement of tensile modulus (MPa) in accordance with JIS K 7113 using a tensile tester (manufactured by Shimadzu Corporation, AUTOGRAPH AGS-J) at a tension speed of 20 mm / min.

[0080] (2-2) Upper yield stress, breaking stress, breaking strain The obtained measurement sample was cut into a test piece in the shape of a dumbbell No. 1 (based on JIS K 6771), and pulled at a pulling speed of 500% / min using a tensile testing machine (Shimadzu Corporation, AUTOGRAPH AGS-J). The breaking tensile strength (kg / cm) was measured at a measurement temperature of 20°C. 2 ) was measured. From the obtained values, a stress σ (MPa)-strain ε (%) curve was obtained. Note that 500% / min means a speed at which the test piece is moved a distance five times the distance between the chucks in one minute. The upper yield stress, breaking stress, and breaking strain were obtained from the obtained stress-strain curve.

[0081] (3) Evaluation of ceramic green sheets (Preparation of inorganic dispersion) One part by weight of polyvinyl acetal resin (BL-1, manufactured by Sekisui Chemical Co., Ltd.) was added to a mixed solvent of 20 parts by weight of toluene and 20 parts by weight of ethanol, and dissolved by stirring. Next, 100 parts by weight of barium titanate powder (BT01, manufactured by Sakai Chemical Industry Co., Ltd.) was added to the obtained solution, and the mixture was stirred for 180 minutes with a bead mill (Ready Mill, manufactured by Imex Co., Ltd.) to prepare an inorganic dispersion.

[0082] (Preparation of resin solution) The obtained polyvinyl acetal resin and 2 parts by weight of DOP were added to a mixed solvent of 45 parts by weight of ethanol and 45 parts by weight of toluene, and dissolved with stirring to prepare a resin solution. The amount of polyvinyl acetal resin added was 8 parts by weight when the polyvinyl acetal resins (average polymerization degree less than 4000) obtained in Examples 1 to 4, 6, 8, and 9 and Comparative Examples 1, 2, and 4 to 7 were used, and 4 parts by weight when the polyvinyl acetal resins (average polymerization degree 4000 or more) obtained in Examples 5 and 7 and Comparative Example 3 were used.

[0083] (Preparation of ceramic green sheets) The resin solution was added to the obtained inorganic dispersion liquid, and the mixture was stirred for 90 minutes in a bead mill to obtain a composition for ceramic green sheets. The obtained ceramic green sheet composition was applied onto a release-treated PET film using a coater so that the thickness after drying would be 20 μm, and then the film was dried by heating to prepare a ceramic green sheet.

[0084] (3-1) Presence or absence of peeling The resulting ceramic green sheet was cut into 10 cm squares, and three sheets were stacked together and heated at a temperature of 80°C and a pressure of 180 kg / cm. 2 The laminate was laminated under heat and pressure bonding conditions for 5 minutes. The presence or absence of peeling between the layers was visually observed and evaluated according to the following criteria. ◯: No delamination was observed at all, and the layers were firmly bonded. △: Partial delamination was observed. ×: A considerable amount of delamination was observed.

[0085] (3-2) Cross-sectional area 1 μm 2 More than 100 defects On the surface of the obtained ceramic green sheet, 2 Ten fields of view were randomly selected, and the cross-sectional area per field was measured using a shape analysis laser microscope (Keyence Corporation, "VK-X100") to determine the area of ​​the cross section. 2 The average number of defects above that was counted.

[0086] (3-3) Arithmetic mean height (Sa), maximum height (Sz) The arithmetic mean height Sa of the obtained ceramic green sheet was evaluated in accordance with ISO25178 using a three-dimensional surface roughness meter (VertScan2.0 manufactured by Ryoka Systems Co., Ltd.).

[0087] [Table 1]

[0088] [Table 2] [Industrial Applicability]

[0089] According to the present invention, it is possible to provide a polyvinyl acetal resin which, when dissolved in an organic solvent, produces little fine undissolved matter, and which, particularly when used as a binder for ceramic green sheets, can give ceramic green sheets having excellent toughness, and which can be used to fabricate ceramic capacitors having excellent reliability.

Claims

1. The maximum diffuse transmittance in the visible light region measured using a D65 light source, a 10-degree visual field, and a thickness of 5 mm is 2.0% or less; The copolymer comprises a structural unit having an acetal group represented by the following formula (1), a structural unit having a hydroxyl group represented by the following formula (2), and a structural unit having an acetyl group represented by the following formula (3), A polyvinyl acetal resin having a hydroxyl group content of 23 mol % or more. [Formula 1] In the above formula (1), R 1 represents a hydrogen atom or an alkyl group having 1 to 20 carbon atoms.

2. When the particle size distribution of a polyvinyl acetal resin solution dissolved in a 1:1 ethanol / toluene mixed solution to a concentration of 0.2% by weight was measured using a particle counter, the ratio of particles with diameters of 0.5 to 1.0 μm was 4.42 × 10 per 100 volume percent of the resin solution. -8 2. The polyvinyl acetal resin according to claim 1, wherein the polyvinyl acetal resin has a volume percent or less.

3. 3. The polyvinyl acetal resin according to claim 1, which has a lightness index L* of 10 or less on a black background.

4. The polyvinyl acetal resin according to any one of claims 1 to 3, wherein the average diffuse transmittance in the visible light region is 1.0% or less.

5. The polyvinyl acetal resin according to any one of claims 1 to 4, wherein the ratio of the average value of the diffuse transmittance in the visible light region to the minimum value of the diffuse transmittance in the wavelength range of 550 to 740 nm is 1.2 or more.

Citation Information

Patent Citations

  • Polyvinyl acetal resin and method for producing polyvinyl acetal resin

    JP2005325342A