Tin-silver plating solution and method for forming tin-silver solder bumps using the same

A tin-silver plating solution with controlled additives and ion ratios stabilizes the plating process, addressing whisker formation and composition issues, resulting in uniform and reliable solder bumps for flip chip packaging.

JP7557627B2Active Publication Date: 2024-09-27KOREA INSTITUTE OF INDUSTRIAL TECHNOLOGY +1
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2023530693
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-10-18
Filing Date
2021-11-17
Publication Date
2024-09-27
Estimated Expiration
2041-11-17

AI Technical Summary

Technical Problem

The generation of whiskers and non-uniformity of silver composition in tin-silver solder bumps during high-speed plating, along with the challenges of controlling silver ion precipitation and plating surface uniformity, hinder the reliability and efficiency of flip chip packaging.

Method used

A tin-silver plating solution containing specific organic additives, including a silver complexing agent, a tin carrier, and a grain refiner, along with controlled ratios of tin and silver ions, is used to stabilize the plating process and ensure uniform composition, reducing whisker formation and enabling high-speed plating.

Benefits of technology

The solution achieves uniform silver composition, reduces whisker generation, and maintains high throughput with improved surface roughness and solderability, ensuring reliable and efficient formation of tin-silver solder bumps.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007557627000047
    Figure 0007557627000047
  • Figure 0007557627000046
    Figure 0007557627000046
  • Figure 0007557627000044
    Figure 0007557627000044
Patent Text Reader

Abstract

A tin ion source and silver ions (Ag + A tin-silver plating solution is provided that contains a silver (Ag) complexing agent, a tin carrier, and an organic additive containing a grain refiner. When the plating solution is used for high speed plating, the generation of whiskers is reduced, and the silver ion (Ag) in the tin-silver plating solution is reduced. + Since the composition of the tin-silver solder bump is kept uniform, the silver composition in the resulting tin-silver solder bump can be made uniform.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a tin-silver plating solution, and more particularly to a tin-silver plating solution used to plate substrates of electronic components, including semiconductor devices. [Background technology]

[0002] As electronic products become smaller, thinner, larger in capacity, and more functional, the reduction in area of ​​circuit boards, which are core components of such electronic products, and the increase in the mounting area of ​​semiconductor devices are directly linked to the competitiveness of such electronic products. Research and development is therefore being conducted to increase the mounting area of ​​the semiconductor device, i.e., the mounting area of ​​the semiconductor device, which is mounted on the circuit board.

[0003] Therefore, in order to reduce the mounting area, a method of directly mounting a semiconductor device in the form of a bare chip has been used in recent years, and flip chip mounting is one of the most widely used bare chip mounting methods.

[0004] There are various types of flip chip packages, but flip chip packaging technology using solder bumps has the advantage of being able to apply fine pitch, increase speed, and implement products that are lightweight, thin, highly functional, and high performance by directly bonding solder bumps between circuit boards and drastically increasing the number of input / output terminals per unit area through an area array method that utilizes the entire surface area of ​​the chip.

[0005] Conventionally, the commonly used tin-lead solder bumps had the advantages of excellent soldering properties, a low melting point, and easy management of the plating solution, but the use of tin-lead solder bumps has been restricted by the enforcement of the RoHS Act, which regulates the use of hazardous substances including lead. In addition, after plating the solder bumps with tin plating solution, whiskers are frequently generated during the reflow process to create solder balls, and there has been a continuous need for research to improve this. Therefore, tin-based alloys such as tin-silver, tin-bismuth, tin-copper, and tin-zinc are being considered as alternatives to tin-lead alloys.

[0006] Among them, tin-silver alloys have attracted attention due to their advantages such as low resistivity, stability, ability to achieve a wide range of melting points, and elimination of alpha particle emission due to pure Sn source. However, in tin-silver solder bump manufacturing, the silver ions (Ag + ) tends to deposit on a specific UBM (under bump metal) layer or a tin anode plate, and silver ions (Ag + In addition, if the alloy composition ratio of the tin-silver solder bump is not appropriate, whiskers or nodules may appear, which may cause problems with the interconnection reliability in the flip chip.

[0007] Another problem in manufacturing the tin-silver solder bumps is that the current density at which plating can be performed is limited. High current density during plating increases the bump plating speed and has a positive effect on high throughput, but it is difficult to control the plating surface and excessive hydrogen gas is generated at the plating electrode, which may have adverse effects such as the generation of voids in the bump due to non-dense plating.

[0008] Therefore, there is a need for the development of a tin-silver plating solution that has a stable plating rate and stable silver content under high-speed plating conditions and has a smooth plating surface. [Prior art documents] [Patent documents]

[0009] [Patent Document 1] Korean Patent No. 10-1175062 Summary of the Invention [Problem to be solved by the invention]

[0010] An object of the present invention is to provide a tin-silver plating solution for reducing the generation of whiskers under high speed plating and improving the non-uniformity of the silver composition in the solder.

[0011] The technical problems that the present invention aims to solve are not limited to the above-mentioned technical problems, and other technical problems not mentioned will be clearly understood by a person having ordinary skill in the art to which the present invention pertains from the following description. [Means for solving the problem]

[0012] In order to solve the above problems, one embodiment of the present invention is a tin ion source and a silver ion (Ag + and an organic additive, the organic additive comprising a silver (Ag) complexing agent represented by the following Chemical Formula 1, a tin carrier represented by the following Chemical Formula 2, and a grain refiner represented by the following Chemical Formula 3:

[0013] [ka]

[0014] Here, A1 is an alkylene having a linear structure and having 1 to 10 carbons, and R1 and R2 are each independently a functional group containing at least one of carbon, oxygen, nitrogen, sulfur, and silicon.

[0015] [ka]

[0016] Here, A2 is a substituted or unsubstituted C6 to C 30 an aryl group or a heteroaryl having 6 to 30 ring atoms, in which at least one ring carbon contains at least one heteroatom selected from the group consisting of nitrogen, oxygen, and sulfur; The R3 is hydrogen or a substituted or unsubstituted C1-C 30 Alkyl groups, substituted or unsubstituted, C3-C 30 Cycloalkyl groups, substituted or unsubstituted C2-C 30 Alkenyl groups, substituted or unsubstituted C2-C 30 Alkynyl groups, substituted or unsubstituted C1-C 30 one of an alkoxy group, a hydroxy group, a sulfonate group ionically bonded to an alkali metal cation, a phosphonate group ionically bonded to an alkali metal cation, a nitronate group ionically bonded to an alkali metal cation, and a carboxylate group ionically bonded to an alkali metal cation; The n1 to n4 each independently represents an integer of 0 to 26, and the sum of n1 to n4 is 10 to 26.

[0017] [ka]

[0018] Here, R4 is hydrogen, an alkyl having a linear structure having 1 to 20 carbons, an alkyl having a branched structure having 5 to 20 carbons, or an alkyl having a linear structure having 1 to 7 carbons and including a hydroxyl group; R5 is hydrogen, an alkyl having a linear structure having 1 to 20 carbons, an alkyl having a branched structure having 5 to 20 carbons, or an alkyl having a linear structure having 1 to 7 carbons and including a hydroxyl group; R6 is hydrogen, an alkyl having a linear structure having 1 to 20 carbons, or an alkyl having a branched structure having 5 to 20 carbons; R7 is hydrogen, an alkyl having a linear structure having 1 to 20 carbons, or an alkyl having a branched structure having 5 to 20 carbons; and X is any one selected from the group of ions consisting of chlorine (Cl), bromine (Br), iodine (I), nitrate (NO3), sulfate (SO4), carbonate (CO3), and hydroxyl (OH).

[0019] In one embodiment of the present invention, the tin ion source may be a tin-silver plating solution containing at least one water-soluble tin compound selected from the group consisting of tin sulfate, tin chloride, tin sulfamate, tin acetate, tin phosphate, tin methanesulfonate, tin gluconate, and tin carboxylate.

[0020] In one embodiment of the present invention, the silver ions (Ag + ) source may be a tin-silver plating solution characterized in that it contains at least one water-soluble silver (Ag) compound selected from the group consisting of silver sulfate, silver chloride, silver sulfamate, acetate, silver phosphate, silver methanesulfonate, silver gluconate, and silver carboxylate.

[0021] In one embodiment of the present invention, the tin-silver plating solution contains tin ions and silver ions (Ag + ) may be provided in a weight ratio of 75:25 to 99.9:0.1.

[0022] In one embodiment of the present invention, the silver ions (Ag +The tin-silver plating solution may be characterized in that the silver (Ag) complexing agent to the tin (Ti) source is provided in a molar ratio of 1:1 to 1:10.

[0023] Furthermore, in one embodiment of the present invention, the tin-silver plating solution may further include at least one of a conductive salt, an antioxidant, and a leveling agent.

[0024] Here, the conductive salt may be any one of a hydroxycarboxylic acid and an alkane sulfonic acid.

[0025] In addition, in this case, the tin-silver plating solution may be characterized in that the antioxidant is at least one selected from the group consisting of catechol, hydroquinone, resorcinol, cresol, phloroglucinol, oxyhydroquinone, and pyrogallol.

[0026] Furthermore, at that time, the tin-silver plating solution may be characterized in that the leveling agent is at least one selected from the group consisting of a nonionic surfactant, a cationic surfactant, an anionic surfactant, and a synthetic polymer.

[0027] In order to solve the above problems, another embodiment of the present invention is a method for producing a tin ion source and a silver ion (Ag + and an organic additive, the organic additive comprising a silver (Ag) complexing agent represented by the following formula 1, a tin carrier represented by the following formula 2, and a grain refiner represented by the following formula 3; and applying a current to plate a tin-silver alloy onto the lower bump metallurgy.

[0028] [ka]

[0029] Here, A1 is an alkylene having a linear structure and having 1 to 10 carbons, and R1 and R2 are each a functional group containing at least one of carbon, oxygen, nitrogen, sulfur, and silicon.

[0030] [ka]

[0031] Here, A2 is a substituted or unsubstituted C6 to C 30 an aryl group or a heteroaryl having 6 to 30 ring atoms, at least one of which is a nitrogen, oxygen, or sulfur heteroatom, and R3 is a hydrogen or a substituted or unsubstituted C1 to C 30 Alkyl groups, substituted or unsubstituted, C3-C 30 Cycloalkyl groups, substituted or unsubstituted C2-C 30 Alkenyl groups, substituted or unsubstituted C2-C 30 Alkynyl groups, substituted or unsubstituted C1-C 30 n1 is any one of an alkoxy group, a hydroxy group, a sulfonate group ionically bonded to an alkali metal cation, a phosphonate group ionically bonded to an alkali metal cation, a nitronate group ionically bonded to an alkali metal cation, and a carboxylate group ionically bonded to an alkali metal cation, and n1 to n4 are each independently an integer of 0 to 26, with the sum of n1 to n4 being 10 to 26.

[0032] [ka]

[0033] Here, R4 is hydrogen, an alkyl having a linear structure having 1 to 20 carbons, an alkyl having a branched structure having 5 to 20 carbons, or an alkyl having a linear structure having 1 to 7 carbons and a hydroxyl group; R5 is hydrogen, an alkyl having a linear structure having 1 to 20 carbons, an alkyl having a branched structure having 5 to 20 carbons, or an alkyl having a linear structure having 1 to 7 carbons and a hydroxyl group; R6 is hydrogen, an alkyl having a linear structure having 1 to 20 carbons, or an alkyl having a branched structure having 5 to 20 carbons; R7 is hydrogen, an alkyl having a linear structure having 1 to 20 carbons, or an alkyl having a branched structure having 5 to 20 carbons; and X is any one selected from the group of ions consisting of chlorine (Cl), bromine (Br), iodine (I), nitrate (NO3), sulfate (SO4), carbonate (CO3), and hydroxyl (OH).

[0034] In one embodiment of the present invention, the method for forming a tin-silver solder bump may be characterized in that in the step of plating the tin-silver alloy, the applied current has a current density of 1 to 10 ASD.

[0035] To achieve the above object, another embodiment of the present invention provides a Sn-Ag solder bump formed by the above method. Effect of the Invention

[0036] Even when high-speed plating is performed using the tin-silver plating solution according to one embodiment of the present invention, the generation of whiskers is reduced, and the silver ions (Ag + By maintaining a uniform composition of the tin-silver solder, the silver composition in the resulting tin-silver solder bumps can be made uniform.

[0037] Furthermore, the method for forming tin-silver solder bumps of the present invention allows plating to be performed at a high current density and high speed, thereby achieving a high throughput.

[0038] In addition, the Sn-Ag solder bumps formed using the Sn-Ag solder bump forming method of the present invention have uniform bump height, improved surface roughness and solderability, uniform silver (Ag) content and distribution in the bump, reduced whisker generation, and good reflow characteristics. Furthermore, there is an effect that the excellent processability and reliability of ultra-fine bumps can be maintained.

[0039] It should be understood that the effects of the present invention are not limited to these, but include all effects that can be inferred from the configuration of the invention described in the detailed description of the present invention or the claims. [Brief description of the drawings]

[0040] [Figure 1] 2 is a flow chart illustrating a method for forming a tin-silver solder bump of the present invention. [Diagram 2] 1A and 1B are surface scanning electron microscope images of tin-silver solder bumps according to an embodiment of the present invention and a comparative example. [Diagram 3] 4 is a scanning electron microscope image of a soldering result of an embodiment of the present invention and a comparative example. [Figure 4] 4 is a scanning electron microscope image of the surface of the tin-silver solder bump and the soldering result of Example 2a of the present invention. [Diagram 5] 1 is a scanning electron microscope image of the surface and soldering result of a tin-silver solder bump of Example 2b of the present invention. [Figure 6] 4 is a scanning electron microscope image of the surface of the tin-silver solder bump and the soldering result of Example 3a of the present invention. [Figure 7] 1 is a scanning electron microscope image of the surface and soldering result of a tin-silver solder bump of Example 3b of the present invention. [Figure 8] 4A-4C are scanning electron microscope images of the surface and soldering result of the tin-silver solder bump of Example 4a of the present invention. [Figure 9] 4 is a scanning electron microscope image of the surface and soldering result of the tin-silver solder bump of Example 4b of the present invention. [Figure 10]4 is a scanning electron microscope image of the surface of the tin-silver solder bump and the soldering result of Example 4c of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0041] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS The present invention may, however, be embodied in many different forms and should not be construed as limited to the embodiments set forth herein.

[0042] The terms used in this specification are merely used to describe specific embodiments and are not intended to limit the present invention. Unless otherwise specified, singular expressions include plural expressions. In this specification, terms such as "include" and "have" indicate the presence of features, numbers, steps, operations, components, parts, or combinations thereof described in the specification, unless otherwise specified to the contrary, and do not preclude the presence or additional possibility of one or more other features, numbers, steps, operations, components, parts, or combinations thereof.

[0043] One aspect of the present invention is a method for producing a tin ion source using a silver ion (Ag + and an organic additive, the organic additive comprising a silver (Ag) complexing agent represented by the following Chemical Formula 1, a tin support represented by the following Chemical Formula 2, and a grain refiner represented by the following Chemical Formula 3:

[0044] [ka]

[0045] Here, A1 is an alkylene having a linear structure and having 1 to 10 carbons, and R1 and R2 are each a functional group containing at least one of carbon, oxygen, nitrogen, sulfur, and silicon.

[0046] [ka]

[0047] Here, A2 is a substituted or unsubstituted C6 to C 30 an aryl group or a heteroaryl having 6 to 30 ring atoms, at least one of which is a nitrogen, oxygen, or sulfur heteroatom, and R3 is a hydrogen or a substituted or unsubstituted C1 to C 30 Alkyl groups, substituted or unsubstituted, C3-C 30 Cycloalkyl groups, substituted or unsubstituted C2-C 30 Alkenyl groups, substituted or unsubstituted C2-C 30 Alkynyl groups, substituted or unsubstituted C1-C 30 n1 is any one of an alkoxy group, a hydroxy group, a sulfonate group ionically bonded to an alkali metal cation, a phosphonate group ionically bonded to an alkali metal cation, a nitronate group ionically bonded to an alkali metal cation, and a carboxylate group ionically bonded to an alkali metal cation, and n1 to n4 are each independently an integer of 0 to 26, with the sum of n1 to n4 being 10 to 26.

[0048] [ka]

[0049] Here, R4 is hydrogen, an alkyl having a linear structure having 1 to 20 carbons, an alkyl having a branched structure having 5 to 20 carbons, or an alkyl having a linear structure having 1 to 7 carbons and including a hydroxyl group; R5 is hydrogen, an alkyl having a linear structure having 1 to 20 carbons, an alkyl having a branched structure having 5 to 20 carbons, or an alkyl having a linear structure having 1 to 7 carbons and including a hydroxyl group; R6 is hydrogen, an alkyl having a linear structure having 1 to 20 carbons, or an alkyl having a branched structure having 5 to 20 carbons; R7 is hydrogen, an alkyl having a linear structure having 1 to 20 carbons, or an alkyl having a branched structure having 5 to 20 carbons; and X is any one selected from the group of ions consisting of chlorine (Cl), bromine (Br), iodine (I), nitrate (NO3), sulfate (SO4), carbonate (CO3), and hydroxyl (OH).

[0050] In recent years, interest in lead-free solders has increased due to the tightening of regulations regarding environmental issues caused by lead, and pure tin, tin-copper, tin-silver, and ternary tin alloys have been considered as potential alternatives to the traditionally used tin-lead alloys.

[0051] Among these, tin-silver alloys in particular have advantages such as low resistance, stability, and a wide melting point range, and compared to tin-lead alloys, they have superior mechanical properties such as tensile strength, thermal fatigue, and creep, and are particularly advantageous in terms of joint strength.

[0052] The tin-silver plating solution of the present invention is for producing solder bumps containing the above-mentioned tin-silver alloy, and contains a tin ion source and silver ions (Ag + ) sources.

[0053] In one embodiment of the present invention, the tin ion source is a source of tin ions (Sn 2+), which may be a water-soluble tin compound, and the water-soluble tin compound may be, for example, at least one selected from the group consisting of tin sulfate, tin hydrochloride, tin sulfamate, tin acetate, tin phosphate, tin methanesulfonate, tin gluconate, and tin carboxylate, for example, tin methanesulfonate having high solubility.

[0054] In one embodiment of the present invention, the silver ions (Ag + The silver ion (Ag) source is added to the tin-silver plating solution of the present invention. + ), which may be a water-soluble silver compound, and the water-soluble silver compound may include, for example, at least one selected from the group consisting of silver sulfate, silver hydrochloride, silver sulfamate, acetate, silver phosphate, silver methanesulfonate, silver gluconate, and silver carboxylate, for example, silver methanesulfonate.

[0055] In one embodiment of the present invention, the tin ions and silver ions (Ag + ) may be provided in a weight ratio of 75:25 to 99.9:0.1, and the tin ion source and silver ion (Ag + The tin ion and silver ion (Ag + ) may be provided in the weight ratios set forth above.

[0056] The above-mentioned range of tin ions and silver ions (Ag + When a tin-silver solder bump is formed using a tin-silver plating solution having a weight ratio of tin ions and silver ions (Ag + If the weight ratio of ) is out of the above range, problems may occur when forming tin-silver solder bumps, such as the probability of whisker generation in the plating process and high melting temperature in the reflow process.

[0057] Next, the tin-silver plating solution of the present invention contains an organic additive.

[0058] The organic additives are added to reduce whisker generation in tin-silver solder bumps produced using the tin-silver plating solution of the present invention and to improve unevenness in the silver (Ag) composition, and include a silver (Ag) complexing agent, a tin carrier, and a crystal grain refining agent.

[0059] In one embodiment of the present invention, the silver (Ag) complexing agent contained in the organic additive may be a compound represented by the following Chemical Formula 1:

[0060] [ka]

[0061] Here, A1 is an alkylene having a linear structure and having 1 to 10 carbons, and R1 and R2 are each a functional group containing at least one of carbon, oxygen, nitrogen, sulfur, and silicon.

[0062] In tin-silver plating solutions, changes in the silver (Ag) composition can lead to the formation of whisker structures or Ag3Sn phases with high melting points, which can adversely affect the properties of solder bumps, so the silver (Ag) composition must be precisely controlled.

[0063] The silver (Ag) composition is controlled by mixing tin ions and silver ions (Ag + Difficulties arise because the reduction potential difference with the electrolytic solution is very large, and when used for long periods of time, silver precipitates and the plating solution's lifespan is shortened.

[0064] Silver ions (Ag + ) and tin ions (Sn 2+ The reduction potential of ) is as shown in Reaction Scheme 1 below.

[0065] [Reaction Scheme 1] Ag + +e→Ag E0=+0.8V Sn 2+ +2e → Sn E0 = -0.14V

[0066] In one embodiment of the present invention, during plating using a tin-silver plating solution, silver ions (Ag + When exposed to tin ions or under-bump metallurgy (UBM), it spontaneously oxidizes the tin ions or the under-bump metal while simultaneously being reduced to silver (Ag) and precipitated.

[0067] The precipitated silver (Ag) may become finely divided silver (Ag) metal suspended in the plating solution, or it may spontaneously deposit on the substrate, the walls of the plating bath, and the electrodes. It is the silver ions (Ag + ) may make it difficult to control the concentration.

[0068] Therefore, when plating using a tin-silver plating solution, the precipitation of silver (Ag) is prevented, improving stability and reducing the amount of tin ions and silver ions (Ag + It is necessary to minimize the error range of the silver composition of the tin-silver solder by reducing the reduction potential difference between the silver ions (Ag) and the tin ions (Ag). + ) can play a role in minimizing the silver composition error range of tin-silver solder.

[0069] In one embodiment of the present invention, the silver ions (Ag + The silver (Ag) complexing agent to the silver (Ag) source may be provided in a molar ratio of 1:1 to 1:10.

[0070] In one embodiment of the present invention, R1 may be any one of an aldehyde group, a hydroxyl group, a methyl group, a carboxyl group, a mercapto group, an amine group, a thiol group, a nitrile group, and a pyridine, for example, pyridyl, and R2 may be any one of an aldehyde group, a hydroxyl group, a methyl group, a carboxyl group, a mercapto group, an amine group, a thiol group, a nitrile group, and a pyridine, for example, pyridyl, and the compound of Formula 1 may be 3,6-Dithia-1,8-octanediol.

[0071] In one embodiment of the present invention, the tin carrier contained in the organic additive may be a compound represented by the following Chemical Formula 2:

[0072] [ka]

[0073] Here, A2 is a substituted or unsubstituted C6-C 30 an aryl group or a heteroaryl having 6 to 30 ring atoms, at least one of which is a nitrogen, oxygen, or sulfur heteroatom, and R3 is a hydrogen or a substituted or unsubstituted C1 to C 30 Alkyl groups, substituted or unsubstituted, C3-C 30 Cycloalkyl groups, substituted or unsubstituted C2-C 30 Alkenyl groups, substituted or unsubstituted C2-C 30 Alkynyl groups, substituted or unsubstituted C1-C 30 n1 is any one of an alkoxy group, a hydroxy group, a sulfonate group ionically bonded to an alkali metal cation, a phosphonate group ionically bonded to an alkali metal cation, a nitronate group ionically bonded to an alkali metal cation, and a carboxylate group ionically bonded to an alkali metal cation, and n1 to n4 are each an integer of 0 to 26, with the sum of n1 to n4 being 10 to 26.

[0074] In one embodiment of the present invention, the grain refiner contained in the organic additive may be a compound represented by the following Chemical Formula 3:

[0075] [ka]

[0076] Here, R4 is hydrogen, an alkyl having a linear structure having 1 to 20 carbons, an alkyl having a branched structure having 5 to 20 carbons, or an alkyl having a linear structure having 1 to 7 carbons and including a hydroxyl group; R5 is hydrogen, an alkyl having a linear structure having 1 to 20 carbons, an alkyl having a branched structure having 5 to 20 carbons, or an alkyl having a linear structure having 1 to 7 carbons and including a hydroxyl group; R6 is hydrogen, an alkyl having a linear structure having 1 to 20 carbons, or an alkyl having a branched structure having 5 to 20 carbons; R7 is hydrogen, an alkyl having a linear structure having 1 to 20 carbons, or an alkyl having a branched structure having 5 to 20 carbons; and X is any one selected from the group of ions consisting of chlorine (Cl), bromine (Br), iodine (I), nitrate (NO3), sulfate (SO4), carbonate (CO3), and hydroxyl (OH).

[0077] In one embodiment of the present invention, when tin-silver plating is performed on the lower bump metal, for example, copper, an intermetallic compound (IMC) is generated during the heating process after tin plating, and whiskers may be generated due to stress caused by thermal expansion. Specifically, stress may be generated due to the formation of an intermetallic compound, direct mechanical stress such as tension or compression, thermomechanical stress due to differences in thermal expansion coefficients, surface oxidation, etc., which may cause whiskers to grow.

[0078] In one embodiment of the present invention, the grain refiner contained in the organic additive can suppress the growth of the intermetallic compounds of copper and tin, thereby reducing the internal stress of the tin plating layer and suppressing the growth of whiskers.

[0079] In one embodiment of the present invention, R4 is a linear alkyl having two carbons containing a hydroxyl group, R5 is a linear alkyl having two carbons containing a hydroxyl group, R6 is a linear alkyl having 12 carbons, R7 may contain only hydrogen, X may be a halogen ion, and the grain refiner may be, for example, Bis(2-hydroxyethyl)-methyl-tridecylazanium.

[0080] The tin-silver plating solution of the present invention may further include at least one of a conductive salt, an antioxidant, and a leveling agent.

[0081] In one embodiment of the present invention, the conductive salt serves to maintain the pH of the tin-silver plating solution and to impart electrical conductivity. The conductive salt may be at least one selected from the group consisting of hydroxycarboxylic acids and alkanesulfonic acids, but is not limited thereto. For example, the conductive salt may be at least one selected from the group consisting of methanesulfonic acid, ethanesulfonic acid, and propanesulfonic acid, for example, methanesulfonic acid.

[0082] The conductive salt may be contained in an amount of 5 to 30 wt% relative to 100 wt% of the tin-silver plating solution. If the content of the conductive salt is less than 5 wt%, the plating solution may not have sufficient electrical conductivity, resulting in a decrease in plating speed, whereas if the content of the conductive salt is more than 30 wt%, it may be difficult to control the plating shape.

[0083] In one embodiment of the present invention, the antioxidant is a divalent tin ion (Sn 2+ ) is a tetravalent tin ion (Sn 4+ ) and minimize or prevent oxidation to divalent tin ions (Sn 2+The antioxidant is intended to help maintain the antioxidant activity of the present invention. The antioxidant may be one or more selected from polyhydroxy aromatic compounds, but is not limited thereto. For example, the antioxidant may be at least one selected from the group consisting of catechol, hydroquinone, resorcinol, cresol, phloroglucinol, oxyhydroquinone, and pyrogallol.

[0084] The content of the antioxidant is 0.01 to 20 g / L. If the content of the antioxidant is less than 0.01 g / L, the plating solution may contain tetravalent tin ions (Sn 4+ ) increases, the life of the plating solution becomes shorter, and if it exceeds 20g / L, the uniformity and smoothness of the solder deteriorates.

[0085] In one embodiment of the present invention, the leveling agent serves to improve the wettability of the solution during plating, improve the ability to wet even fine patterns and narrow spaces with the solution, and widen the scope of work. The leveling agent may be at least one selected from the group consisting of nonionic surfactants, cationic surfactants, anionic surfactants, and synthetic polymers, but is not limited thereto, and may be, for example, any one of nonionic surfactants, such as 2-naphthyl ethyl ether, polyoxyalkylene ether, polyoxyethylene glycol, polyoxyethylene alkyl phenyl ether, and polyoxyethylene alkyl amino ether.

[0086] One aspect of the present invention provides a method for forming a tin-silver solder bump.

[0087] FIG. 1 is a flow chart illustrating a method for forming a tin-silver solder bump of the present invention.

[0088] Referring to FIG. 1, the method for forming a tin-silver solder bump of the present invention comprises the steps of: + and an organic additive, the organic additive comprising a silver (Ag) complexing agent represented by the following Chemical Formula 1, a tin carrier represented by the following Chemical Formula 2, and a grain refiner represented by the following Chemical Formula 3:

[0089] [ka]

[0090] Here, A1 is an alkylene having a linear structure and having 1 to 10 carbons, and R1 and R2 are each a functional group containing at least one of carbon, oxygen, nitrogen, sulfur, and silicon.

[0091] [ka]

[0092] Here, A2 is a substituted or unsubstituted C6 to C 30 an aryl group or a heteroaryl having 6 to 30 ring atoms, in which at least one ring carbon contains at least one heteroatom selected from the group consisting of nitrogen, oxygen, and sulfur; The R3 is hydrogen or a substituted or unsubstituted C1-C 30 Alkyl groups, substituted or unsubstituted, C3-C 30 Cycloalkyl groups, substituted or unsubstituted C2-C 30 Alkenyl groups, substituted or unsubstituted C2-C 30 Alkynyl groups, substituted or unsubstituted C1-C 30one of an alkoxy group, a hydroxy group, a sulfonate group ionically bonded to an alkali metal cation, a phosphonate group ionically bonded to an alkali metal cation, a nitronate group ionically bonded to an alkali metal cation, and a carboxylate group ionically bonded to an alkali metal cation; The above n1 to n4 are each an integer of 0 to 26, and the sum of n1 to n4 is 10 to 26.

[0093] [ka]

[0094] Here, R4 is hydrogen, an alkyl having a linear structure having 1 to 20 carbons, an alkyl having a branched structure having 5 to 20 carbons, or an alkyl having a linear structure having 1 to 7 carbons and including a hydroxyl group; R5 is hydrogen, an alkyl having a linear structure having 1 to 20 carbons, an alkyl having a branched structure having 5 to 20 carbons, or an alkyl having a linear structure having 1 to 7 carbons and including a hydroxyl group; R6 is hydrogen, an alkyl having a linear structure having 1 to 20 carbons, or an alkyl having a branched structure having 5 to 20 carbons; R7 is hydrogen, an alkyl having a linear structure having 1 to 20 carbons, or an alkyl having a branched structure having 5 to 20 carbons; and X is any one selected from the group of ions consisting of chlorine (Cl), bromine (Br), iodine (I), nitrate (NO3), sulfate (SO4), carbonate (CO3), and hydroxyl (OH).

[0095] The method of forming a tin-silver solder bump of the present invention includes the step (S10) of exposing an underlying bump metallurgy to a plating bath containing a tin-silver plating solution.

[0096] In one embodiment of the present invention, the tin-silver plating solution may be the tin-silver plating solution of the above aspect, and the tin ion source, silver ions (Ag + The tin ion source and the organic additive are the tin ion source and the silver ion (Ag + ) sources and organic additives.

[0097] The tin ion source, silver ions (Ag + The description of the source and organic additives is substituted for the description of the above embodiment.

[0098] The method of forming a Sn-Ag solder bump of the present invention includes applying an electric current to plate a Sn-Ag alloy onto the underlying bump metallurgy (S20).

[0099] In one embodiment of the present invention, the step of plating the Sn-silver alloy (S20) may be performed using an electroplating method, for example, in an electroplating bath containing the Sn-silver plating solution.

[0100] The method for forming a tin-silver solder bump of the present invention can be any method for forming solder using an electroplating method in the technical field of the present invention without any restrictions, and can be used to manufacture a microelectronic device.

[0101] For example, the method begins by forming a lower bump metal structure on a silicon wafer substrate having a pattern on which a microelectronic device can be manufactured, and then immersing the silicon wafer substrate having the lower bump metal structure formed thereon into an electroplating bath containing the tin-silver plating solution to expose the lower bump metal structure.

[0102] In this case, the lower bump metal structure may be formed by sequentially forming titanium (Ti) and copper (Cu), titanium and nickel (Ni), chromium (Cr) and copper, chromium and nickel, titanium tungsten (TiW) and copper, or titanium tungsten and nickel, etc., to a predetermined thickness on a silicon wafer substrate, but is not limited thereto, and may be, for example, copper formed on the silicon wafer substrate.

[0103] In one embodiment of the present invention, the current applied in the step of plating the tin-silver alloy is 1 to 20 ASD (Amp / dm 2 ), for example, 1 to 10 ASD.

[0104] The method for forming tin-silver solder bumps of the present invention allows plating to be performed at high current density and high speed, thereby achieving high throughput.

[0105] In addition, the Sn-Ag solder bumps formed using the Sn-Ag solder bump forming method of the present invention have uniform bump height, improved surface roughness and solderability, uniform silver (Ag) content and distribution in the bump, reduced whisker generation, and good reflow characteristics. Furthermore, there is an effect that the excellent processability and reliability of ultra-fine bumps can be maintained.

[0106] The present invention will be described in more detail below with reference to Production Examples, Comparative Examples and Experimental Examples, but the present invention is not limited to the following Production Examples, Comparative Examples and Experimental Examples.

[0107] [Production Example 1] In this manufacturing example 1, a lower bump metal structure was formed, and electrolytic plating was performed to a thickness of 10 μm on a silicon wafer having a pattern using a copper plating solution.

[0108] The copper plating solution was prepared by adding 50 g of copper ions, 150 g of sulfate ions, 50 mg of chloride ions, a polyethylene oxide derivative containing aromatic hydrocarbon as an inhibitor, an organic compound containing a mercapto group as an accelerator, and a saturated heterocyclic compound containing nitrogen as a leveling agent per 1 L of plating solution, and the electrolytic plating was performed by applying a current at a current density of 5 ASD for 10 minutes. [Example 1]

[0109] In this Example 1, a tin-silver plating solution containing a grain refiner was prepared.

[0110] Specifically, tin methanesulfonate and silver methanesulfonate were mixed to obtain a tin ion (Sn 2+ ), 0.5g / L silver ion (Ag +To this was added, as organic additives, 2 g / L of a silvering agent represented by the following chemical formula 1, 20 g / L of a tin carrier represented by the following chemical formula 2, 1 g / L of catechol as an antioxidant, and 10 g / L of a crystal grain refiner represented by the following chemical formula 3, to prepare a tin-silver plating solution.

[0111] [ka]

[0112] Here, A1 is ethylene, and R1 and R2 are each pyridyl.

[0113] [ka]

[0114] Here, A2 is a phenyl group, R3 is a hydroxy group, n1 to n3 are each 0, n4 is 12, and the sum is 12.

[0115] [ka]

[0116] Here, R4 is an alkyl having a linear structure with two carbons and a hydroxyl group at the end, R5 is an alkyl having a linear structure with two carbons and a hydroxyl group at the end, R6 is an alkyl having a linear structure with 12 carbons, R7 is an alkyl having a linear structure with one carbon, and X is chlorine (Cl).

[0117] [Comparative Example 1] In this Comparative Example 1, a tin-silver plating solution containing no grain refiner was prepared.

[0118] As a specific preparation method, a tin-silver plating solution was prepared in the same manner as in Example 1, except that the grain refiner was not added.

[0119] [Experimental Example 1] In the present Experimental Example 1, tin-silver plating was carried out using the tin-silver plating solutions prepared in Example 1 and Comparative Example 1, and an experiment was carried out on the performance of the plating solutions during plating.

[0120] The silicon wafer on which the lower bump metal structure of Manufacturing Example 1 was formed was immersed in the tin-silver plating solutions prepared in Example 1 and Comparative Example 1, respectively, and tin-silver plating was performed by applying a current in the current density range of 1 to 10 ASD.

[0121] FIG. 2 shows scanning electron microscope (SEM) images of the surface of the tin-silver solder bumps formed using the tin-silver plating solutions of Comparative Example 1 and Example 1.

[0122] The tin-silver solder bumps formed using the tin-silver plating solutions of Comparative Example 1 and Example 1 were subjected to a reflow process, and the resulting soldered bumps were photographed by a scanning electron microscope (SEM) as shown in Fig. 3. The surface roughness and silver content are shown in Table 1 below.

[0123] [Table 1]

[0124] 2, 3 and Table 1, it was confirmed that in Example 1, the roughness of the pattern surface and the solderability were improved compared to Comparative Example 1. [Example 2]

[0125] In this Example 2, tin-silver plating solutions were prepared using various silver complexing agents.

[0126] In this Example 2, preparation was performed by changing only the silver complexing agent from Example 1. At that time, the silver complexing agent was different only in A1, R1, and R2 in Chemical Formula 1, as described later.

[0127] The A1, R1, and R2 are as shown in Table 2 below.

[0128] [ka]

[0129] [Table 2] [Example 3]

[0130] In this Example 3, tin-silver plating solutions were prepared using various tin carriers.

[0131] In this Example 3, preparation was performed by changing only the tin support from Example 1. At that time, the tin support was different only in A2, R3, and n1 to n4 in Chemical Formula 2, as described later.

[0132] The A2, R3, and n1 to n4 are as shown in Table 3 below.

[0133] [ka]

[0134] [Table 3] [Example 4]

[0135] In this Example 4, tin-silver plating solutions were prepared using various grain refiners.

[0136] In this Example 4, preparation was carried out by changing only the grain refiner from Example 1. At this time, the grain refiner is different only in R4, R5, R6, R7 and X in Chemical Formula 3, as described later, and R4, R5, R6, R7 and X are as shown in Table 4 below.

[0137] [ka]

[0138] [Table 4]

[0139] [Experimental Example 2] In the present Experimental Example 2, various tin-silver plating solutions prepared according to Examples 2 to 4 were used to carry out plating experiments.

[0140] The specific experimental method of the present Experimental Example 2 was the same as that used in Experimental Example 1, except that the tin-silver plating solution used in Examples 2 to 4 was different.

[0141] The silicon wafer on which the lower bump metal structure of Production Example 1 was formed was immersed in the tin-silver plating solutions prepared in Examples 2 to 4, respectively, and tin-silver plating was performed by applying a current in the current density range of 1 to 10 ASD.

[0142] The tin-silver solder bumps formed using the tin-silver plating solutions of Examples 2 to 4 were subjected to a reflow process, and scanning electron microscope (SEM) images of the soldered products formed are shown in Table 5. The surface roughness and silver content are also shown in Table 5 below.

[0143] [Table 5]

[0144] As a result of the above experiments, it was found that by controlling various silvering agents, tin carriers, and crystal grain refining agents, it was possible to obtain excellent pattern surface roughness and solderability.

[0145] [Experimental Example 3] In Experimental Example 3, the weight ratio of tin ions and silver ions in the tin-silver plating solution was varied, and an experiment was carried out to confirm the effect of the weight ratio.

[0146] The silver content and solution state according to the specific weight ratio conditions of tin ions and silver ions are shown in Table 6 below.

[0147] If the weight ratio is higher than 99.9:0.1, there are too few silver ions, so only a small amount is incorporated into the plating film, and the silver content converges to 0. Also, if the weight ratio is lower than 75:25, the excess silver ions react with the tin ions to generate precipitates.

[0148] [Table 6]

[0149] [Experimental Example 4] In the present Experimental Example 4, an experiment was carried out in which the molar ratio of the silver (Ag) complexing agent to the silver ions was varied to confirm the effect of changing the molar ratio.

[0150] The molar ratio of silver ions to silver complexing agent was varied, and the silver content and solution state for each molar ratio are shown in Table 7 below.

[0151] If the weight ratio is less than 1:1, the silver ions cannot form sufficient complexes, resulting in precipitation.

[0152] On the other hand, if the weight ratio is higher than 1:1, the silver ions are sufficiently complexed so that the solution remains stable and maintains a uniform silver content.

[0153] [Table 7]

[0154] The above description of the present invention is for illustrative purposes only, and a person having ordinary skill in the art to which the present invention pertains may easily modify the present invention into other specific forms without changing the technical ideas or essential features of the present invention. Therefore, the above-described embodiments are merely illustrative and not limiting. For example, each component described as a single entity may be implemented in a distributed form, and similarly, each component described as a distributed entity may be implemented in a combined form.

[0155] The scope of the present invention is defined by the claims, and all modifications and variations that fall within the meaning and scope of the claims, as well as the equivalent concepts, are included in the present invention.

Claims

1. A source of tin ions and a source of silver ions (Ag + ) source and an organic additive, The organic additive comprises a silver (Ag) complexing agent represented by the following formula 1, a tin carrier represented by the following formula 2, and a grain refiner represented by the following formula 3: 【Chemistry 1】 (wherein, the A 1 is a linear alkylene having 1 to 10 carbon atoms, 1 and R 2 are each independently a functional group containing at least one of carbon, oxygen, nitrogen, sulfur, and silicon. 【Chemistry 2】 (where: The above A 2 is a substituted or unsubstituted C 6 ~C 30 an aryl group or a heteroaryl having 6 to 30 ring atoms, in which at least one ring carbon contains a heteroatom consisting of at least one of nitrogen, oxygen, and sulfur; The R 3 is hydrogen, substituted or unsubstituted C 1 ~C 30 Alkyl group, substituted or unsubstituted C 3 ~C 30 Cycloalkyl groups, substituted or unsubstituted C 2 ~C 30 Alkenyl group, substituted or unsubstituted C 2 ~C 30 Alkynyl group, substituted or unsubstituted C 1 ~C 30 one of an alkoxy group, a hydroxy group, a sulfonate group ionically bonded to an alkali metal cation, a phosphonate group ionically bonded to an alkali metal cation, a nitronate group ionically bonded to an alkali metal cation, and a carboxylate group ionically bonded to an alkali metal cation; The n 1 ~n 4 are each independently an integer from 0 to 26, 1 ~n 4 The sum of is 10 to 26. 【Chemistry 3】 (where: The R 4 is hydrogen, an alkyl of a linear structure having 1 to 20 carbons, an alkyl of a branched structure having 5 to 20 carbons, or an alkyl of a linear structure having 1 to 7 carbons containing a hydroxy group; The R 5 is hydrogen, an alkyl of a linear structure having 1 to 20 carbons, an alkyl of a branched structure having 5 to 20 carbons, or an alkyl of a linear structure having 1 to 7 carbons containing a hydroxy group; The R 6 is hydrogen, alkyl of a linear structure having 1 to 20 carbons, or alkyl of a branched structure having 5 to 20 carbons; The R 7 is hydrogen, alkyl of a linear structure having 1 to 20 carbons, or alkyl of a branched structure having 5 to 20 carbons; The X is chlorine (Cl), bromine (Br), iodine (I), nitrate (NO 3 ), sulfate (SO 4 ), carbonate (CO 3 ) and a hydroxyl group (OH) The silver (Ag) complexing agent is provided in a molar ratio of 1:1 to 1:10 relative to the silver ion (Ag + ) source. A tin-silver plating solution comprising:

2. The tin ion source comprises at least one water-soluble tin compound selected from the group consisting of tin sulfate, tin chloride, tin sulfamate, tin acetate, tin phosphate, tin methanesulfonate, tin gluconate, and tin carboxylate. The tin-silver plating solution according to claim 1.

3. The silver ions (Ag + ) the source comprises at least one water-soluble silver (Ag) compound selected from the group consisting of silver sulfate, silver chloride, silver sulfamate, silver acetate, silver phosphate, silver methanesulfonate, silver gluconate, and silver carboxylate. The tin-silver plating solution according to claim 1.

4. In the tin-silver plating solution, tin ions and silver ions (Ag + ) are provided in a weight ratio of 75:25 to 99.9:0.

1. The tin-silver plating solution according to claim 1.

5. A source of tin ions and a source of silver ions (Ag + ) source and an organic additive, The organic additive comprises a silver (Ag) complexing agent represented by the following formula 1, a tin carrier represented by the following formula 2, and a grain refiner represented by the following formula 3: 【Chemistry 1】 (wherein, the A 1 is a linear alkylene having 1 to 10 carbon atoms, 1 and R 2 are each independently a functional group containing at least one of carbon, oxygen, nitrogen, sulfur, and silicon. 【Chemistry 2】 (where: The above A 2 is a substituted or unsubstituted C 6 ~C 30 an aryl group or a heteroaryl having 6 to 30 ring atoms, in which at least one ring carbon contains a heteroatom consisting of at least one of nitrogen, oxygen, and sulfur; The R 3 is hydrogen, substituted or unsubstituted C 1 ~C 30 Alkyl group, substituted or unsubstituted C 3 ~C 30 Cycloalkyl groups, substituted or unsubstituted C 2 ~C 30 Alkenyl group, substituted or unsubstituted C 2 ~C 30 Alkynyl group, substituted or unsubstituted C 1 ~C 30 one of an alkoxy group, a hydroxy group, a sulfonate group ionically bonded to an alkali metal cation, a phosphonate group ionically bonded to an alkali metal cation, a nitronate group ionically bonded to an alkali metal cation, and a carboxylate group ionically bonded to an alkali metal cation; The n 1 ~n 4 are each independently an integer from 0 to 26, 1 ~n 4 The sum of is 10 to 26. 【Chemistry 3】 (where: The R 4 is hydrogen, an alkyl of a linear structure having 1 to 20 carbons, an alkyl of a branched structure having 5 to 20 carbons, or an alkyl of a linear structure having 1 to 7 carbons containing a hydroxy group; The R 5 is hydrogen, an alkyl of a linear structure having 1 to 20 carbons, an alkyl of a branched structure having 5 to 20 carbons, or an alkyl of a linear structure having 1 to 7 carbons containing a hydroxy group; The R 6 is hydrogen, alkyl of a linear structure having 1 to 20 carbons, or alkyl of a branched structure having 5 to 20 carbons; The R 7 is hydrogen, alkyl of a linear structure having 1 to 20 carbons, or alkyl of a branched structure having 5 to 20 carbons; The X is chlorine (Cl), bromine (Br), iodine (I), nitrate (NO 3 ), sulfate (SO 4 ), carbonate (CO 3 ) and a hydroxyl group (OH) Further comprising a conductive salt and an antioxidant; the conductive salt is one of a hydroxycarboxylic acid and an alkane sulfonic acid; The antioxidant is at least one selected from the group consisting of catechol, hydroquinone, resorcinol, cresol, phloroglucinol, oxyhydroquinone, and pyrogallol. A tin-silver plating solution comprising:

6. Further includes a smoothing agent The tin-silver plating solution according to claim 5.

7. The smoothing agent is at least one selected from the group consisting of a nonionic surfactant, a cationic surfactant, an anionic surfactant, and a synthetic polymer. The tin-silver plating solution according to claim 6.

8. A source of tin ions and a source of silver ions (Ag + ) supply source and an organic additive, the organic additive comprising a silver (Ag) complexing agent represented by the following Chemical Formula 1, a tin support represented by the following Chemical Formula 2, and a grain refiner represented by the following Chemical Formula 3: 【Chemistry 4】 (wherein, the A 1 is a linear alkylene having 1 to 10 carbon atoms, 1 and R 2 are functional groups each containing at least one of carbon, oxygen, nitrogen, sulfur, and silicon. 【Chemistry 5】 (where: The above A 2 is a substituted or unsubstituted C 6 ~C 30 an aryl group or a heteroaryl having 6 to 30 ring atoms, in which at least one ring carbon contains a heteroatom consisting of at least one of nitrogen, oxygen, and sulfur; The R 3 is hydrogen, substituted or unsubstituted C 1 ~C 30 Alkyl group, substituted or unsubstituted C 3 ~C 30 Cycloalkyl groups, substituted or unsubstituted C 2 ~C 30 Alkenyl group, substituted or unsubstituted C 2 ~C 30 Alkynyl group, substituted or unsubstituted C 1 ~C 30 one of an alkoxy group, a hydroxy group, a sulfonate group ionically bonded to an alkali metal cation, a phosphonate group ionically bonded to an alkali metal cation, a nitronate group ionically bonded to an alkali metal cation, and a carboxylate group ionically bonded to an alkali metal cation; The n 1 ~n 4 are each independently an integer from 0 to 26, 1 ~n 4 The sum of is 10 to 26. 【Chemistry 6】 (where: The R 4 is hydrogen, an alkyl of a linear structure having 1 to 20 carbons, an alkyl of a branched structure having 5 to 20 carbons, or an alkyl of a linear structure having 1 to 7 carbons containing a hydroxy group; The R 5 is hydrogen, an alkyl of a linear structure having 1 to 20 carbons, an alkyl of a branched structure having 5 to 20 carbons, or an alkyl of a linear structure having 1 to 7 carbons containing a hydroxy group; The R 6 is hydrogen, alkyl of a linear structure having 1 to 20 carbons, or alkyl of a branched structure having 5 to 20 carbons; The R 7 is hydrogen, alkyl of a linear structure having 1 to 20 carbons, or alkyl of a branched structure having 5 to 20 carbons; The X is chlorine (Cl), bromine (Br), iodine (I), nitrate (NO 3 ), sulfate (SO 4 ), carbonate (CO 3 ) and a hydroxyl group (OH) The silver (Ag) complexing agent is provided in a molar ratio of 1:1 to 1:10 relative to the silver ion (Ag + ) source. A plating bath containing a tin-silver plating solution characterized in that exposing a lower bump metal structure; applying a current to plate a tin-silver alloy onto the lower bump metallurgy; Includes 2. A method for forming a tin-silver solder bump comprising the steps of:

9. A source of tin ions and a source of silver ions (Ag + ) supply source and an organic additive, the organic additive comprising a silver (Ag) complexing agent represented by the following Chemical Formula 1, a tin support represented by the following Chemical Formula 2, and a grain refiner represented by the following Chemical Formula 3: 【Chemistry 4】 (wherein, the A 1 is a linear alkylene having 1 to 10 carbon atoms, 1 and R 2 are functional groups each containing at least one of carbon, oxygen, nitrogen, sulfur, and silicon. 【Chemistry 5】 (where: The above A 2 is a substituted or unsubstituted C 6 ~C 30 an aryl group or a heteroaryl having 6 to 30 ring atoms, in which at least one ring carbon contains a heteroatom consisting of at least one of nitrogen, oxygen, and sulfur; The R 3 is hydrogen, substituted or unsubstituted C 1 ~C 30 Alkyl group, substituted or unsubstituted C 3 ~C 30 Cycloalkyl groups, substituted or unsubstituted C 2 ~C 30 Alkenyl group, substituted or unsubstituted C 2 ~C 30 Alkynyl group, substituted or unsubstituted C 1 ~C 30 one of an alkoxy group, a hydroxy group, a sulfonate group ionically bonded to an alkali metal cation, a phosphonate group ionically bonded to an alkali metal cation, a nitronate group ionically bonded to an alkali metal cation, and a carboxylate group ionically bonded to an alkali metal cation; The n 1 ~n 4 are each independently an integer from 0 to 26, 1 ~n 4 The sum of is 10 to 26. 【Chemistry 6】 (where: The R 4 is hydrogen, an alkyl of a linear structure having 1 to 20 carbons, an alkyl of a branched structure having 5 to 20 carbons, or an alkyl of a linear structure having 1 to 7 carbons containing a hydroxy group; The R 5 is hydrogen, an alkyl of a linear structure having 1 to 20 carbons, an alkyl of a branched structure having 5 to 20 carbons, or an alkyl of a linear structure having 1 to 7 carbons containing a hydroxy group; The R 6 is hydrogen, alkyl of a linear structure having 1 to 20 carbons, or alkyl of a branched structure having 5 to 20 carbons; The R 7 is hydrogen, alkyl of a linear structure having 1 to 20 carbons, or alkyl of a branched structure having 5 to 20 carbons; The X is chlorine (Cl), bromine (Br), iodine (I), nitrate (NO 3 ), sulfate (SO 4 ), carbonate (CO 3 ) and a hydroxyl group (OH) Further comprising a conductive salt and an antioxidant; the conductive salt is one of a hydroxycarboxylic acid and an alkane sulfonic acid; The antioxidant is at least one selected from the group consisting of catechol, hydroquinone, resorcinol, cresol, phloroglucinol, oxyhydroquinone, and pyrogallol. A plating bath containing a tin-silver plating solution characterized in that exposing a lower bump metal structure; applying a current to plate a tin-silver alloy onto the lower bump metallurgy; Includes 2. A method for forming a tin-silver solder bump comprising the steps of:

10. The tin-silver plating solution further contains a leveling agent. The method for forming a solder bump using a tin-silver plating solution according to claim 9.

11. The smoothing agent is at least one selected from the group consisting of a nonionic surfactant, a cationic surfactant, an anionic surfactant, and a synthetic polymer. The method for forming a tin-silver solder bump according to claim 10.

12. In the step of plating the tin-silver alloy, the applied current has a current density of 1 to 10 ASD.

12. The method for forming a tin-silver solder bump according to claim 8.

Citation Information

Patent Citations

  • Tin and tin alloy electroplating bath, method for forming electrodeposition using plating bath, and electronic component produced by the method

    JP2017031447A

  • Plating solution

    JP2017179515A

  • Electric tin and tin alloy plating bath, electronic component forming electrodeposition using the plating bath

    JP2017222894A

  • SnAg ALLOY PLATING LIQUID

    JP2019137896A

  • Method for plating sn-ag of lead free solder

    KR101175062B1