Concrete composition and method for producing same

A concrete composition with a stable one-component admixture effectively addresses material separation issues, maintaining high fluidity and workability by using a specific blend of components, including unsaturated monomers and cellulose ether, to enhance production and transportation efficiency.

JP7558473B2Active Publication Date: 2024-10-01OHBAYASHI GUMI LTD +2
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2020070769
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-04-10
Publication Date
2024-10-01
Estimated Expiration
2040-04-10

AI Technical Summary

Technical Problem

Existing high-fluidity concrete compositions suffer from material separation issues, leading to deterioration in pumpability and quality due to aggregate separation, which existing admixtures do not adequately address.

Method used

A concrete composition using a highly stable one-component admixture comprising specific components, including unsaturated monocarboxylic acid monomers, water-soluble cellulose ether, gums, and antifoaming agents, with controlled ionic strength and viscosity, ensuring high fluidity and material separation resistance.

Benefits of technology

The composition maintains high fluidity and prevents material separation, enhancing workability and pumpability while ensuring stable production and transportation efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007558473000001
    Figure 0007558473000001
  • Figure 0007558473000002
    Figure 0007558473000002
  • Figure 0007558473000003
    Figure 0007558473000003
Patent Text Reader

Abstract

To provide a concrete composition which uses one-liquid-type admixture having high stability and exhibits high flowability and good material separation resistance, and a manufacturing method thereof.SOLUTION: A concrete composition includes a binder, water, a fine aggregate, a coarse aggregate, and a predetermined one-liquid-type admixture (X), and has a water-binder ratio of 30-70 mass% and a slump flow of 35-75 cm, with the rate of the one-liquid-type admixture (X) being 0.3-3.0 pts.mass to 100 pts.mass of the binder.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a concrete composition and a method for producing the same, and more particularly to a concrete composition having high fluidity and good resistance to material separation, and a method for producing the same. [Background technology]

[0002] In recent years, in order to improve workability and reduce labor, there has been an increase in the use of highly fluid concrete compositions such as medium-fluidity concrete compositions (slump flow of about 35 to 50 cm) and high-fluidity concrete compositions (slump flow of about 50 to 70 cm).

[0003] One example of its use is tunnel lining construction, where a highly fluid concrete composition is used in pouring concrete in small spaces where work is difficult, improving workability and reducing the labor required for compaction due to its high filling ability.

[0004] However, such a highly fluid concrete composition is prone to separation of aggregates and other materials, which can lead to deterioration in the pumpability and quality of the concrete composition.

[0005] Therefore, in order to improve material separation and workability, it has been proposed to use a one-component admixture that combines cellulose ether, which is one of the few water-soluble polymers that can thicken even in the strong alkaline environment caused by cement, with a water-reducing agent (see, for example, Patent Documents 1 and 2).

[0006] Furthermore, as an improvement over Patent Documents 1 and 2, a concrete composition using a one-liquid admixture combining specific components has been proposed (see, for example, Patent Document 3). [Prior art documents] [Patent documents]

[0007] [Patent Document 1] JP 2008-137889 A [Patent Document 2] JP 2016-56081 A [Patent Document 3] JP 2018-135245 A Summary of the Invention [Problem to be solved by the invention]

[0008] However, the concrete composition of Patent Document 3 may not have sufficient resistance to material separation depending on the concrete mix and material conditions, and there is still room for improvement in terms of resistance to material separation.

[0009] In view of the above circumstances, the present invention provides a concrete composition that uses a highly stable one-component admixture, while having high fluidity and good resistance to material separation, and a method for producing the same. [Means for solving the problem]

[0010] As a result of intensive research aimed at solving the above problems, the present inventors have found that the above problems can be solved by using a specific one-liquid admixture (X). According to the present invention, the following concrete composition and method for producing the same are provided.

[0011] [1] Contains binder, water, fine aggregate, coarse aggregate, and one-component admixture (X); The water-binder ratio is 30 to 70 mass%, and the slump flow is 35 to 75 cm; A concrete composition comprising the one-liquid admixture (X) in an amount of 0.3 to 3.0 parts by mass per 100 parts by mass of the binder. One-component admixture (X): The composition contains the following component A, the following component B, the following component C, the following component D, and water, and the ionic strength derived from the component A is 0.02 to 0.8. the law of nature, The content ratio of the B component is 0.05 to 10 mass% when the total content ratio of the A component, the B component, the C component, the D component, and the water contained in the one-liquid admixture (X) is 100 mass%. One-component admixture. Component A: A polycarboxylic acid-based water-reducing agent comprising at least one selected from the group consisting of unsaturated monocarboxylic acid monomers, unsaturated dicarboxylic acid monomers, and salts thereof, and a copolymer of an unsaturated monomer copolymerizable therewith and having a polyoxyalkylene group composed of 1 to 300 oxyalkylene units having 2 to 4 carbon atoms in the molecule, and a salt thereof. B component: A water-soluble cellulose ether having a mass average molecular weight of 700,000 to 1,200,000. Ingredient C: Gums. Ingredient D: Antifoaming agent.

[0012] [2] When the total content of the A component, the B component, the C component, the D component, and the water contained in the one-component admixture (X) is 100% by mass, The concrete composition according to [1] above, wherein the one-component admixture (X) contains the A component in a proportion of 15 to 40 mass %.

[0013] [3] The concrete composition according to [1] or [2], wherein the B component is at least one selected from the group consisting of alkyl cellulose, hydroxyalkyl cellulose, and hydroxyalkyl alkyl cellulose.

[0014] [4] The concrete composition according to any one of [1] to [3], wherein the component B is a water-soluble cellulose ether having a viscosity of 8,000 to 30,000 mPa s in a 1 mass % aqueous solution at 20°C.

[0015] [5] The concrete composition according to any one of [1] to [4], wherein the component B is a water-soluble cellulose ether having a mass average molecular weight of 800,000 to 1,000,000.

[0016] [6] The concrete composition according to any one of [1] to [5], wherein the component C is at least one selected from diutan gum, welan gum, xanthan gum, and gellan gum.

[0017] [7] The concrete composition according to any one of [1] to [6], wherein the water-binder ratio is 40 to 65 mass % and the slump flow is 50 to 70 cm.

[0018] [8] A method for producing a concrete composition according to any one of [1] to [7], A method for producing a concrete composition comprising preparing a base concrete containing the binder, the water, the fine aggregate, and the coarse aggregate, and then adding the one-component admixture (X) to the base concrete to produce a concrete composition.

[0019] [9] A method for producing a concrete composition according to any one of [1] to [7], A method for producing a concrete composition by adding all of the components including the binder, the water, the fine aggregate, the coarse aggregate, and the one-liquid admixture (X) at once to produce a concrete composition. Effect of the Invention

[0020] The concrete composition of the present invention uses a highly stable one-liquid type admixture, and has the effects of having high fluidity and good resistance to material separation.

[0021] According to the method for producing a concrete composition of the present invention, a highly stable one-component admixture is used, and therefore, even when, for example, a method is adopted in which all components including the binder, water, fine aggregate, coarse aggregate, and one-component admixture are added at once, or a method is adopted in which the one-component admixture is added later, workability is good, and further, a concrete composition having high fluidity and good resistance to material separation can be produced. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0022] Hereinafter, the embodiments of the present invention will be described. However, the present invention is not limited to the following embodiments. Therefore, it should be understood that appropriate modifications, improvements, etc. can be made to the following embodiments based on the ordinary knowledge of those skilled in the art without departing from the spirit of the present invention. In the following examples, etc., % means % by mass, and parts means parts by mass, unless otherwise specified.

[0023] (1) Concrete composition: The concrete composition of the present invention contains a binder, water, fine aggregate, coarse aggregate, and a one-liquid type admixture (X), has a water-binder ratio of 30 to 70 mass %, a slump flow of 35 to 75 cm, and contains the one-liquid type admixture (X) in a ratio of 0.3 to 3.0 parts by mass per 100 parts by mass of the binder. <One-liquid admixture (X)> A one-component admixture comprising the following component A, component B, component C, component D, and water, and having an ionic strength derived from component A of 0.02 to 0.8. "Component A": A polycarboxylic acid-based water-reducing agent comprising at least one selected from the group consisting of unsaturated monocarboxylic acid monomers, unsaturated dicarboxylic acid monomers, and salts thereof, and a copolymer of an unsaturated monomer copolymerizable therewith and having a polyoxyalkylene group composed of 1 to 300 oxyalkylene units having 2 to 4 carbon atoms in the molecule, and a salt thereof. "B component": A water-soluble cellulose ether having a mass average molecular weight of 700,000 to 1,200,000. "Ingredient C": Gums. "Component D": Antifoaming agent.

[0024] Such a concrete composition uses a highly stable one-liquid type admixture, has high fluidity, and has resistance to material separation. Furthermore, the concrete composition of the present invention uses a one-liquid type admixture that has a high degree of water-reducing component solids concentration and is highly stable, and exhibits sufficient resistance to material separation even under conditions with a small amount of powder or when material conditions change, and further has high fluidity.

[0025] (1-1) Binding material: Examples of the binder include various types of Portland cement, such as ordinary Portland cement, moderate heat Portland cement, low heat Portland cement, high early strength Portland cement, and sulfate resistant Portland cement, as well as various types of mixed cement, such as blast furnace cement and fly ash cement.

[0026] As the binder, various admixtures such as fly ash, ground granulated blast furnace slag, ground limestone, stone powder, silica fume, and an expanding agent may be used in combination with the various cements mentioned above.

[0027] (1-2) Fine aggregate: Examples of fine aggregate include river sand, mountain sand, land sand, sea sand, silica sand, crushed sand, and various types of slag fine aggregate.

[0028] (1-3) Coarse aggregate: Examples of coarse aggregate include river gravel, mountain gravel, land gravel, crushed stone, various types of slag coarse aggregate, lightweight aggregate, and the like.

[0029] (1-4) One-component admixture (X): The one-liquid type admixture (X) is a one-liquid type admixture prepared by blending a plurality of components in advance. This one-liquid type admixture (X) maintains a uniformly dissolved state without salting out over a long period of time (i.e., is stable), and therefore the one-liquid type admixture (X) of the present invention has excellent stability.

[0030] The one-liquid admixture (X) is contained in a ratio of 0.3 to 3.0 parts by mass relative to 100 parts by mass of the binder, preferably 0.4 to 2.5 parts by mass, and more preferably 0.5 to 2.0 parts by mass. At such a content ratio, the material separation resistance of the concrete composition can be ensured, and the concrete composition is easy to handle from the viewpoint of production efficiency. If the content ratio of the one-liquid admixture (X) is less than the above lower limit, the B component and the C component are insufficient, making it difficult to ensure the material separation resistance of the concrete composition. On the other hand, if the content ratio of the one-liquid admixture (X) is more than the above upper limit, problems such as difficulty in measuring at once with a measuring device at a concrete manufacturing plant or the like arise, leading to a decrease in the production efficiency of the concrete composition and an increase in transportation costs.

[0031] Moreover, the one-component admixture (X) has an ionic strength derived from the A component of 0.02 to 0.8, and this ionic strength is preferably 0.05 to 0.5. With such a content ratio, the precipitation phenomenon of the water-soluble cellulose ether in the one-component admixture (X) is suppressed, and the state in which it is uniformly dissolved is maintained. If the ionic strength derived from the A component is less than the above lower limit, the adsorption points to the binder are insufficient, and sufficient water-reducing performance cannot be obtained. On the other hand, if the ionic strength derived from the A component is more than the above upper limit, the water-soluble cellulose ether is salted out by the ionic substance, and the stability of the one-component admixture (X) is reduced.

[0032] In addition, polycarboxylic acid-based water-reducing agents exhibit water-reducing properties by using the carboxyl groups in the structure as adsorption points for the binder, so ionic substances are essential. On the other hand, water-soluble cellulose ether cannot dissolve when the concentration of ionic substances exceeds a certain level, causing salting out and resulting in precipitation without stabilization. Therefore, in order to improve the stability of the one-component admixture (X), it is very important to eliminate ionic substances that do not contribute to water-reducing properties and adjust the ionic strength of the water-reducing agent to an appropriate range. Examples of ionic substances that do not contribute to water-reducing properties include polymerization initiators and alkali metal salts used for neutralization.

[0033] In the present invention, the ionic strength is represented by the following formula (1), and the molar concentration m of each ion in the one-component admixture (X) for all ion species in the water-reducing agent is i and charge z i It is calculated by adding the product of the square of and then multiplying it by 1 / 2.

[0034]

number

[0035] (1-4-1)A component: Component A is a specific polycarboxylic acid-based water-reducing agent. Specifically, it is a polycarboxylic acid-based water-reducing agent containing at least one selected from a copolymer (hereinafter sometimes referred to as "copolymer (i)") of "at least one selected from unsaturated monocarboxylic acid monomers, unsaturated dicarboxylic acid monomers, and salts thereof" and "an unsaturated monomer copolymerizable with them and having a polyoxyalkylene group composed of 1 to 300 oxyalkylene units having 2 to 4 carbon atoms in the molecule" (hereinafter sometimes referred to as "unsaturated monomer (i)"), and a salt thereof.

[0036] Examples of the unsaturated monocarboxylic acid monomer, the unsaturated dicarboxylic acid monomer, and their salts include those selected from (meth)acrylic acid, crotonic acid, (anhydrous) maleic acid, (anhydrous) itaconic acid, fumaric acid, and their salts. From the viewpoint of stabilizing the water-soluble cellulose ether in the one-liquid type admixture (X), it is preferable that they are in the form of an acid rather than a salt.

[0037] The salts of the unsaturated monocarboxylic acid monomer and the unsaturated dicarboxylic acid monomer are not particularly limited, but examples thereof include alkali metal salts such as sodium salts and potassium salts, alkaline earth metal salts such as calcium salts and magnesium salts, ammonium salts, and amine salts such as diethanolamine salts and triethanolamine salts.

[0038] Examples of the unsaturated monomer (i) include α-allyl-ω-methoxy-(poly)oxyethylene, α-allyl-ω-methoxy-(poly)oxyethylene (poly)oxypropylene, α-allyl-ω-hydroxy-(poly)oxyethylene, α-allyl-ω-hydroxy-(poly)oxyethylene (poly)oxypropylene, α-methallyl-ω-hydroxy-(poly)oxyethylene, α-methallyl-ω-methoxy-(poly)oxyethylene, α-methallyl-ω-hydroxy-(poly)oxyethylene (poly)oxypropylene, α-(3-methyl-3-butenyl)-ω-hydroxy-(poly)oxyethylene, α-(3-methyl-3-butenyl)-ω-hydroxy-(poly)oxyethylene (poly)oxypropylene, α-(3-methyl-3-butenyl)-ω-butoxy-(poly)oxyethylene, α-(3-methyl-3-butenyl)-ω-acetyl-(poly)oxyethylene (poly)oxypropylene, α-acryloyl-ω-hydroxy Si-(poly)oxyethylene, α-acryloyl-ω-hydroxy-(poly)oxypropylene, α-acryloyl-ω-methoxy-(poly)oxyethylene, α-acryloyl-ω-methoxy-(poly)oxyethylene(poly)oxypropylene, α-acryloyl-ω-butoxy-(poly)oxyethylene, α-methacryloyl-ω-hydroxy-(poly)oxyethylene, α-methacryloyl-ω-hydroxy-(poly)oxypropylene, α-methacryloyl-ω-hydroxy-(poly )oxyethylene (poly)oxypropylene, α-methacryloyl-ω-methoxy-(poly)oxyethylene, α-methacryloyl-ω-butoxy-(poly)oxyethylene, α-methacryloyl-ω-acetyl-(poly)oxyethylene (poly)oxypropylene, polyamide polyamine (poly)oxyethylene, polyamide polyamine (poly)oxyethylene (poly)oxypropylene, α-vinyl-ω-hydroxy(poly)oxybutylene (poly)oxyethylene, and the like.

[0039] The copolymer (i) and its salt contained in the component A may be copolymerized with other monomers within a range that does not impair the effects of the present invention, and the copolymerization ratio of the other monomers is preferably 20 mass% or less, and more preferably 10 mass% or less.

[0040] Examples of the other monomers include styrene, acrylamide, (meth)allylsulfonic acid or a salt thereof, and methyl (meth)acrylate.

[0041] The copolymer (i) can be synthesized by a conventionally known method, specifically, radical polymerization using water as a solvent, radical polymerization using an organic solvent as a solvent, solvent-free radical polymerization, and the like.

[0042] The radical polymerization initiator used in the radical polymerization is not particularly limited and may be any suitable one that decomposes at the polymerization reaction temperature to generate radicals, such as peroxides such as benzoyl peroxide, hydrogen peroxide, ammonium persulfate, sodium persulfate, and potassium persulfate, and azo compounds such as 2,2'-azobis(isobutyronitrile) and 2,2'-azobis(2-methylbutyronitrile). Among these, from the viewpoint of obtaining a predetermined ionic strength, those that do not generate ionic substances even after decomposition, such as hydrogen peroxide, are preferred.

[0043] In the radical polymerization, reducing agents such as sodium hydrogen sulfite, sodium bisulfite, and ascorbic acid, and amine compounds such as ethylenediamine and glycine can also be used as accelerators. In order to adjust the mass average molecular weight of the resulting polymer and its salt to a desired range, chain transfer agents such as 2-mercaptoethanol, 2-mercaptopropionic acid, 3-mercaptopropionic acid, thioglycolic acid, thioglycerin, and thiomalic acid can also be used.

[0044] The mass average molecular weight of the copolymer (i) and its salt contained in the component A is not particularly limited, but is preferably, for example, in terms of pullulan, 2000 to 500000, and more preferably 10000 to 100000. By setting it in such a range, the desired water reducing performance can be obtained.

[0045] The content of the A component in the one-liquid admixture (X) is not particularly limited, but is preferably 15 to 40% by mass, and more preferably 15 to 30% by mass, when the total content of the A component, the B component, the C component, the D component, and the water contained in the one-liquid admixture (X) is taken as 100% by mass. By making it in such a range, the one-liquid admixture (X) exhibits the desired water-reducing performance, and at the same time, the salting out of the water-soluble cellulose ether can be suppressed and stabilized. If the content of the A component is less than the above lower limit, the water-reducing performance of the one-liquid admixture (X) decreases, and in particular, in the preparation of a concrete composition with high fluidity, the amount of addition increases, which causes problems such as difficulty in measuring at a time with a measuring device at a concrete manufacturing plant, etc., and this may result in a decrease in the production efficiency of the concrete composition or an increase in transportation costs. On the other hand, if it exceeds the above upper limit, the water-soluble cellulose ether, which is the B component, may be easily salted out.

[0046] (1-4-2)B component: Component B is a water-soluble cellulose ether having a mass average molecular weight of 700,000 to 1,200,000. By containing such component B, a one-liquid admixture having high stability can be obtained, and further, the material separation resistance can be further improved, and good material separation resistance can be obtained.

[0047] The mass average molecular weight of the B component is 700000 to 1200000, preferably 800000 to 1000000. When the mass average molecular weight of the B component is within the above range, it can impart appropriate viscosity to the concrete composition and can impart material separation resistance that can cope with conditions with a small amount of powder and fluctuations in material conditions. Here, when the mass average molecular weight is below the lower limit, the material separation resistance of the concrete composition is insufficient, and the concrete composition cannot cope with conditions with a small amount of powder and fluctuations in material conditions, and separates. On the other hand, when the mass average molecular weight is above the upper limit, it imparts excessive viscosity to the concrete composition, and the fluidity of the concrete composition decreases due to an increase in the amount of bleeding associated with an increase in the amount of water reducing agent used and a plateauing phenomenon of slump flow. The "mass average molecular weight" is a value measured by the GPC-MALS method.

[0048] The water-soluble cellulose ether, which is the B component, is not particularly limited with respect to its viscosity (viscosity of a 1% by mass aqueous solution at 20°C), but for example, it is preferably 8000 to 30000 mPa·s, and more preferably 10000 to 25000 mPa·s. Here, if the viscosity is below the lower limit, the material separation resistance to concrete is insufficient, and the concrete may separate due to inability to respond to conditions with a small amount of powder or fluctuations in material conditions. On the other hand, if the viscosity is above the upper limit, excessive viscosity is imparted to concrete, and there is a risk of an increase in the amount of bleeding due to an increase in the amount of water reducing agent used, or a decrease in the fluidity of concrete due to a plateauing phenomenon of slump flow.

[0049] The viscosity of the water-soluble cellulose ether which is component B, that is, the viscosity of a 1% by mass aqueous solution of component B at 20° C., is a value measured at 20 rpm using a BH viscometer.

[0050] Examples of the water-soluble cellulose ether which is component B include alkyl celluloses such as methyl cellulose and ethyl cellulose, hydroxyalkyl celluloses such as hydroxypropyl cellulose and hydroxyethyl cellulose, and hydroxyalkyl alkyl celluloses such as hydroxyethyl methyl cellulose, hydroxypropyl methyl cellulose and hydroxyethyl ethyl cellulose. It is preferable that component B is at least one selected from the group consisting of alkyl celluloses, hydroxyalkyl celluloses, and hydroxyalkyl alkyl celluloses.

[0051] Specific examples of alkyl cellulose include methyl cellulose having a degree of substitution (DS) of preferably 1.0 to 2.2, more preferably 1.2 to 2.0, and ethyl cellulose having a degree of substitution (DS) of preferably 1.0 to 2.2, more preferably 1.2 to 2.0.

[0052] Examples of hydroxyalkyl cellulose include hydroxyethyl cellulose having a molar substitution (MS) of preferably 0.1 to 3.0, more preferably 0.5 to 2.8, and hydroxypropyl cellulose having a molar substitution (MS) of preferably 0.05 to 3.3, more preferably 0.1 to 3.0.

[0053] Examples of the hydroxyalkyl alkyl cellulose include hydroxyethyl methyl cellulose having a degree of substitution (DS) of preferably 1.0 to 2.2, more preferably 1.2 to 2.0, and a molar substitution (MS) of preferably 0.05 to 0.6, more preferably 0.1 to 0.5; hydroxypropyl methyl cellulose having a degree of substitution (DS) of preferably 1.0 to 2.2, more preferably 1.2 to 2.0, and a molar substitution (MS) of preferably 0.05 to 0.6, more preferably 0.1 to 0.5; and hydroxyethyl ethyl cellulose having a degree of substitution (DS) of preferably 1.0 to 2.2, more preferably 1.2 to 2.0, and a molar substitution (MS) of preferably 0.05 to 0.6, more preferably 0.1 to 0.5.

[0054] The "degree of substitution (DS)" refers to the average number of alkoxy groups per unit of anhydroglucose, and the "molar substitution (MS)" refers to the average mole number of hydroxyalkoxy groups per mole of anhydroglucose.

[0055] The degree of substitution (DS) and molar substitution (MS) can be determined by converting values ​​measured by the analytical method for degree of substitution of hypromellose (hydroxypropyl methylcellulose) described in the 17th Edition of the Japanese Pharmacopoeia.

[0056] The content of component B in one-component admixture (X) is 、A 0.05 to 10% by mass when the total content of component B, component C, component D, and water contained in the one-component admixture (X) is 100% by mass. and , 0.1 to 5 mass% I like I wish.

[0057] (1-4-3)C component: Component C is a gum that is effective in stabilizing the water-soluble cellulose ether in the one-part admixture (X).

[0058] The gums of component C are not particularly limited in type, and examples thereof include diutan gum, welan gum, xanthan gum, gellan gum, etc., and it is preferable that the gum is at least one selected from diutan gum, welan gum, xanthan gum, and gellan gum.

[0059] Diutan gum is composed of D-glucose, D-glucuronic acid, D-glucose and L-rhamnose, and two L-rhamnoses.

[0060] An example of a commercially available diutan gum product is KELCO-CRETE DG-F (product name manufactured by CP Kelco).

[0061] Welan gum has a main chain consisting of D-glucose, D-glucuronic acid, and L-rhamnose in a 2:2:1 ratio, to which L-rhamnose or L-mannose side chains are attached.

[0062] An example of a commercially available Welan gum product is CP KELCO KIA-96 (product name manufactured by CP Kelco).

[0063] Like cellulose, xanthan gum has a main chain consisting of β-1,4 bonds of D-glucose, and side chains consisting of two mannose units and one glucuronic acid unit.

[0064] An example of a commercially available xanthan gum product is KELZAN (a product name manufactured by Sansho Corporation).

[0065] Gellan gum is a heteropolysaccharide with four repeating sugar units: D-glucose, D-glucuronic acid, and L-rhamnose, linked in a 2:1:1 ratio.

[0066] An example of a commercially available gellan gum product is KELCOGEL AFT (product name manufactured by CP Kelco).

[0067] The content of the C component (gums) in the one-liquid admixture (X) is not particularly limited, but when the total content of the A component, the B component, the C component, the D component, and the water contained in the one-liquid admixture (X) is taken as 100% by mass, for example, in the case of diutan gum, it is preferably 0.005 to 2% by mass, more preferably 0.01 to 1% by mass, and particularly preferably 0.02 to 0.8% by mass. By setting it in such a range, the solution viscosity of the one-liquid admixture (X) can be appropriately increased, and salting out and precipitation of the water-soluble cellulose ether can be suppressed.

[0068] In the case of Welan gum, xanthan gum, or gellan gum, when the total content of the water contained in the A component, the B component, the C component, the D component, and the one-liquid type admixture (X) is taken as 100% by mass, the content is preferably 0.005 to 10% by mass, more preferably 0.01 to 5% by mass, and particularly preferably 0.02 to 3% by mass. By setting the content in such a range, the solution viscosity of the one-liquid type admixture (X) can be appropriately increased, and salting out and precipitation of the water-soluble cellulose ether can be suppressed.

[0069] (1-4-4) D component: Component D is a defoamer. This defoamer is used to stabilize the water-soluble cellulose ether in the one-liquid admixture (X).

[0070] Examples of the defoaming agent which is component D include oxyalkylene-based defoaming agents, silicone-based defoaming agents, alcohol-based defoaming agents, mineral oil-based defoaming agents, fatty acid-based defoaming agents, fatty acid ester-based defoaming agents, etc. Among these, in order to improve the dispersion stability of the one-liquid type water reducing agent, oxyalkylene-based defoaming agents, mineral oil-based defoaming agents, and fatty acid ester-based defoaming agents are preferred.

[0071] Examples of oxyalkylene-based defoaming agents include polyoxyalkylenes such as (poly)oxyethylene (poly)oxypropylene adducts, (poly)oxyalkylene alkyl ethers such as diethylene glycol heptyl ether, polyoxyethylene oleyl ether, polyoxypropylene butyl ether, polyoxyethylene polyoxypropylene 2-ethylhexyl ether, and oxyethylene oxypropylene adducts to higher alcohols having 8 or more carbon atoms or secondary alcohols having 12 to 14 carbon atoms, (poly)oxyalkylene (alkyl)aryl ethers such as polyoxypropylene phenyl ether and polyoxyethylene nonyl phenyl ether, and alkylene aryl ethers to acetylene alcohols such as 2,4,7,9-tetramethyl-5-decyne-4,7-diol, 2,5-dimethyl-3-hexyne-2,5-diol, and 3-methyl-1-butyne-3-ol. acetylene ethers obtained by addition polymerization of ethylene oxides; (poly)oxyalkylene fatty acid esters such as diethylene glycol oleate, diethylene glycol laurate, and ethylene glycol distearate; (poly)oxyalkylene sorbitan fatty acid esters such as polyoxyethylene sorbitan monolaurate and polyoxyethylene sorbitan trioleate; (poly)oxyalkylene alkyl (aryl) ether sulfate salts such as polyoxypropylene methyl ether sodium sulfate and polyoxyethylene dodecylphenol ether sodium sulfate; (poly)oxyalkylene alkyl phosphates such as (poly)oxyethylene stearyl phosphate; (poly)oxyalkylene alkyl amines such as polyoxyethylene laurylamine; and polyoxyalkylene amides.

[0072] Examples of silicone-based defoaming agents include dimethyl silicone oil, silicone paste, silicone emulsion, organic modified polysiloxane, and fluorosilicone oil.

[0073] Examples of alcohol-based defoamers include octyl alcohol, 2-ethylhexyl alcohol, hexadecyl alcohol, acetylene alcohol, and glycols.

[0074] Examples of mineral oil-based defoaming agents include kerosene and liquid paraffin.

[0075] Examples of fatty acid-based antifoaming agents include alkylene oxide adducts of oleic acid, stearic acid, and the like.

[0076] Examples of fatty acid ester-based defoaming agents include glycerin monoricinoleate, alkenyl succinic acid derivatives, sorbitol monolaurate, sorbitol trioleate, and natural waxes.

[0077] The content of component D (antifoaming agent) in the one-component admixture (X) is not particularly limited, but is preferably 0.001 to 10 mass%, and more preferably 0.005 to 5 mass%, when the total content of components A, B, C, D, and water contained in the one-component admixture (X) is taken as 100 mass%. By setting the content in such a range, the stability of the one-component admixture (X) can be improved and the amount of air in the concrete composition can be easily adjusted.

[0078] (1-4-5)Wed: The one-liquid admixture (X) contains water in addition to the above-mentioned components A, B, C, and D. This water can be used as a solvent for components A, B, C, and D, and there is no particular restriction on the content ratio of water in the one-liquid admixture (X).

[0079] (1-5) Other components: The concrete composition of the present invention may contain existing additives as necessary.

[0080] Examples of the additives include air-entraining agents, antifoaming agents, air-entraining water-reducing agents, high-performance water-reducing agents, high-performance air-entraining water-reducing agents, setting retarders, hardening accelerators, shrinkage reducing agents, preservatives, waterproofing agents, and rust inhibitors.

[0081] Examples of the AE agent include an anionic surfactant. Examples of the defoamer include a polyoxyalkylene compound. There are no particular limitations on the AE water reducer, high performance water reducer, and high performance AE water reducer, but commercially available ones can be used. Examples of the setting retarder include oxycarboxylates. Examples of the hardening accelerator include amines. Examples of the shrinkage reducer include polyoxyalkylene compounds. Examples of the preservative include isothiazolinone compounds. Examples of the waterproofing agent include higher fatty acid derivatives. Examples of the rust inhibitor include nitrites.

[0082] (1-6) Physical properties of concrete composition: The concrete composition of the present invention has a water / binder ratio of 30-70% by mass, preferably 40-65% by mass. Within this range, a concrete composition having good workability and sufficient material separation resistance can be obtained. If the water / binder ratio is less than 30% by mass, the viscosity of the concrete composition becomes too high, resulting in poor workability. On the other hand, if the water / binder ratio is more than 70% by mass, sufficient material separation resistance cannot be imparted.

[0083] The concrete composition of the present invention has a slump flow immediately after mixing of 35 to 75 cm, preferably 50 to 70 cm. Within this range, a concrete composition having good workability and sufficient material separation resistance can be obtained. Here, if the slump flow is less than 35 cm, the viscosity of the concrete composition becomes too high, leading to deterioration of workability. On the other hand, if the slump flow is more than 75 cm, sufficient material separation resistance cannot be imparted. Incidentally, a slump flow of about 50 to 70 cm is generally called high-fluidity concrete.

[0084] The concrete composition of the present invention preferably has a water-binder ratio of 40 to 65 mass % and a slump flow of 50 to 70 cm. By satisfying these conditions, excellent resistance to material separation is exhibited.

[0085] The concrete composition of the present invention is used in civil engineering, construction, secondary products, and the like.

[0086] (2) Method for producing concrete composition: The method for producing the concrete composition of the present invention is not particularly limited, and it is sufficient that the concrete composition is produced so that the one-liquid admixture (X) is contained in the concrete composition that is finally used at the construction site.

[0087] Specifically, examples of the method for producing the concrete composition of the present invention include the following methods (a) and (b) depending on the timing of addition.

[0088] (a) A method in which all components including the binder, water, fine aggregate, coarse aggregate, and one-component admixture (X) are added at once in a ready-mix concrete plant to produce a concrete composition (simultaneous addition), (b) A method in which a base concrete containing the binder, water, fine aggregate, and coarse aggregate is prepared, and then the one-component admixture (X) is added to the prepared base concrete to produce a concrete composition (post-addition), etc.

[0089] As the above-mentioned method (b), specifically, there can be mentioned a method in which unhardened concrete (base concrete) is prepared in advance at a ready-mix concrete factory or the like, and then a one-component admixture (X) or the like is added later at a construction site or the like.

[0090] Here, the one-liquid type admixture (X) used in the present invention has excellent stability and can be stored for a long period of time, and can be suitably adopted in the above method (b) in which the one-liquid type admixture (X) is added later. In the case of the above method (b), it is possible to respond to changes in concrete properties due to variations in transportation time to the construction site due to traffic conditions, etc., and it is possible to obtain concrete properties more suitable for construction. EXAMPLES

[0091] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these examples.

[0092] <Test Category 1> (Synthesis Example 1) Synthesis of component A (a-1): 1400g of water, 1100g of α-methacryloyl-ω-methoxypoly(45 mol)oxyethylene, 104g of methacrylic acid, 24g of thioglycerol as a chain transfer agent, and 50g of 30% aqueous sodium hydroxide solution were charged into a reaction vessel, and the atmosphere in the reaction vessel was replaced with nitrogen, and then the mixture was gradually heated while stirring. The temperature of the reaction system was kept at 60°C using a hot water bath, and 240g of a 0.025% aqueous solution of hydrogen peroxide was added to start the radical polymerization reaction. After 2 hours, 60g of a 0.025% aqueous solution of hydrogen peroxide was further added, and the radical polymerization reaction was continued for 6 hours. 41g of water and 121g of a 30% aqueous sodium hydroxide solution were added to the obtained copolymer to obtain a 40% aqueous solution of A component (a-1). The mass average molecular weight of this A component (a-1) was 41400.

[0093] (Synthesis Examples 2, 4, 5, 7) Synthesis of components (a-2), (a-4), (a-5), and (a-7) A: Except for using the "monomer type" shown in Table 1, 40% aqueous solutions of A components (a-2), (a-4), (a-5), and (a-7) were obtained in the same manner as A component (a-1).

[0094] (Synthesis Example 3) Synthesis of component A (a-3): α-Allyl-ω-methoxy-poly(100 mol)oxyethylene poly(3 mol)oxypropylene and maleic anhydride were charged into a reaction vessel, and the atmosphere in the reaction vessel was replaced with nitrogen, and then the mixture was gradually heated with stirring to dissolve uniformly. The temperature of the reaction system was kept at 80°C in a hot water bath, and 2,2'-azobis(isobutyronitrile) was added to start the radical polymerization reaction. After 2 hours, 2,2'-azobis(isobutyronitrile) was further added, and the radical polymerization reaction was continued for 2 hours. Water and a 30% aqueous solution of sodium hydroxide were added to the obtained copolymer to obtain a 40% aqueous solution of component A (a-3). When this component A (a-3) was analyzed, it was found to have a mass average molecular weight of 69,200.

[0095] (Synthesis Example 6) Synthesis of component A (a-6): Water and α-(3-methyl-3-butenyl)-ω-hydroxy-poly(80 mol)oxyethylene were charged into a reaction vessel, and the atmosphere in the reaction vessel was replaced with nitrogen, and then the mixture was gradually heated while stirring. The temperature of the reaction system was kept at 70°C in a hot water bath to stabilize the temperature. Then, acrylic acid was added dropwise over 3 hours. At the same time, an aqueous solution of thioglycolic acid and L-ascorbic acid dissolved in water and 5% hydrogen peroxide solution were each added dropwise over 3 hours to initiate a radical polymerization reaction. One hour after the end of the dropwise addition, water and a 30% aqueous sodium hydroxide solution were added to the obtained copolymer to obtain a 40% aqueous solution of component A (a-6). When this component A (a-6) was analyzed, it was found to have a mass average molecular weight of 71,300.

[0096] [Conditions for measuring mass average molecular weight] The conditions for measuring the mass average molecular weight of each A component are shown below. [GPC method] Equipment: Showa Denko Shodex GPC-101 Detector: Differential refractometer (RI) Column: Showa Denko OHpak SB-G + SB-806M HQ + SB-806M HQ Eluent: 50mM sodium nitrate aqueous solution Flow rate: 0.7mL / min Column temperature: 40℃ Standard material: "Pullulan" manufactured by Showa Denko Co., Ltd.

[0097] The details of each of the components A (a-1) to (a-7) synthesized above are summarized in Table 1.

[0098] [Table 1]

[0099] <Test Category 2> Components B to D are shown below.

[0100] (B component) The B component is shown in Table 2.

[0101] [Table 2]

[0102] [DS, MS] The degree of substitution was calculated by converting the value measured by the analytical method for the degree of substitution of hypromellose (hydroxypropyl methylcellulose) described in the 17th Edition of the Japanese Pharmacopoeia.

[0103] [Conditions for measuring mass average molecular weight] The mass average molecular weight of the component B was measured by a GPC-MALS method under the following measurement conditions. Liquid delivery pump: Showa Denko Shodex DS-4 Detector: Differential Refractometer (RI), Multi-Atomic Light Scattering Detector (MALS) Column: Showa Denko OHpak SB-806M HQ Eluent: 0.1M sodium nitrate aqueous solution Flow rate: 1.0mL / min Column temperature: 40℃

[0104] [Method for measuring aqueous solution viscosity] The "aqueous solution viscosity (mPa·s)" in Table 2 is the viscosity of a 1% or 2% by mass aqueous solution of the water-soluble cellulose ether of component B at 20°C, which was measured at 20 rpm using a BH viscometer.

[0105] (C component) The C component is shown in Table 3.

[0106] [Table 3]

[0107] c-1 to c-4 in Table 3 are as follows. c-1: KELZAN (product name manufactured by Sansho Co., Ltd.) c-2: CP Kelco K1A-96 (product name manufactured by CP Kelco) c-3: KELCO-CRETE DG-F (CP Kelco product name) c-4: KELCOGEL AFT (CP Kelco product name)

[0108] (D component) As the defoaming agent, which is component D, SN DEFOAMER 14-HP (an oxyalkylene-based defoaming agent, a trade name of San Nopco Ltd., abbreviation: d-1) was used.

[0109] <Test Category 3> The ionic strength of a 40% aqueous solution of component A (a-1) was calculated using the above formula (1). The ionic strength was 0.412. The calculation process is shown in Table 4.

[0110] [Table 4]

[0111]

number

[0112] The ionic strength of the 40% aqueous solutions of A-components (a-2) to (a-7) was calculated in the same manner as the ionic strength of the 40% aqueous solution of A-component (a-1). The calculation results of the ionic strength derived from A-component (ionic strength derived from A-component in one-liquid admixture (X)) are shown in Table 5.

[0113] <Test Category 4> (Preparation of one-component admixture) Components A to D and water were blended as shown in Table 5, and mixed at 5000 rpm for 1 minute using a homomixer (HM-310, manufactured by AS ONE Co., Ltd.) to prepare a one-liquid admixture.

[0114] [Table 5]

[0115] *1 and *2 in Table 5 are as follows. *1: Highly condensed alkylarylsulfonate (the active ingredient in Takemoto Oil Co., Ltd.'s high-performance water-reducing agent for concrete, product name Polfine 510-AN) *2: Nitrogen-containing sulfonate (the active ingredient in Takemoto Oil Co., Ltd.'s high-performance water-reducing agent for concrete, product name Polfine MF)

[0116] <Test Category 5> (Stability test of one-liquid admixture) 100 ml of the prepared one-component admixture was placed in a measuring cylinder equipped with a stopcock and left to stand at 20°C and 40°C. The sedimentation volume (%) of the water-soluble cellulose ether was measured, and this was used as a stability test for the one-component admixture.

[0117] The sedimentation volume (%) was evaluated by taking a state in which there was no salting out and the mixture was uniformly dispersed as 100%, and reading the graduations on the graduated cylinder at the boundary between the transparent and dispersed parts as transparent parts gradually began to appear at the top of the graduated cylinder over time. For example, if the graduation on the graduated cylinder at the boundary between the transparent and dispersed parts after 7 days is 90 ml, the sedimentation volume is 90%. The results are shown in Table 6.

[0118] [Table 6]

[0119] Based on the results of the sedimentation volume (%) measurement, each one-component admixture was evaluated according to the following criteria. The results are shown in Table 7. The evaluation criteria are as follows. A: Sedimentation volume (%) after standing for 28 days is 95-100% B: Sedimentation volume (%) after standing for 28 days is 80% or more and less than 95% C: Sedimentation volume (%) after standing for 28 days is less than 80%

[0120] [Table 7]

[0121] <Test Category 6> (Preparation of concrete composition) (Examples 1 to 25, Comparative Examples 1 to 11) Using a forced twin-shaft mixer with a nominal capacity of 55 L, mixing was carried out for 90 seconds according to the contents shown in Tables 8, 9 and 10 to prepare the concrete compositions of each example.

[0122] In each concrete composition, the air content was adjusted using an air-entraining agent (product name: AE-300, manufactured by Takemoto Yushi Co., Ltd.) and an antifoaming agent (product name: AFK-2, manufactured by Takemoto Yushi Co., Ltd.). The target slump flow was 60±5 cm, and the target air content was 4.5±1.5%.

[0123] (Examples 26 to 50, Comparative Examples 12 to 22) Using a forced twin-shaft mixer with a nominal capacity of 55 L, mixing was carried out for 60 seconds according to the contents shown in Tables 8, 9 and 12 to prepare the base concrete for each example.

[0124] The slump and air content of the base concrete were adjusted using an air-entraining water-reducing agent (Takemoto Yushi Co., Ltd., product name Chupol EX60), an air-entraining agent (Takemoto Yushi Co., Ltd., product name AE-300), and an antifoaming agent (Takemoto Yushi Co., Ltd., product name AFK-2). The target slump of the base concrete was 15±2.5cm, and the target air content was 4.5±1.5%.

[0125] Next, the prepared base concrete was poured into a tilting mixer with a nominal capacity of 60 L, and the admixtures shown in Table 12 were added. The point where the inlet was facing upward and parallel to the floor surface was defined as 0°, and the concrete was mixed for 60 seconds at a 20° inclination to prepare the concrete composition for each example.

[0126] The air content after fluidization was adjusted as necessary using an air entrainer (AE-300, product name, manufactured by Takemoto Yushi Co., Ltd.) and an antifoaming agent (AFK-2, product name, manufactured by Takemoto Yushi Co., Ltd.) The target slump flow after fluidization was 60±5 cm, and the target air content was 4.5±1.5%.

[0127] In Examples 1 to 25 and Comparative Examples 1 to 11, a method was adopted in which all components including the admixture were added at once to prepare the concrete composition (simultaneous addition). In Examples 26 to 50 and Comparative Examples 12 to 22, a method was adopted in which a prepared but unhardened concrete (base concrete) was prepared in advance, and then a one-liquid admixture was added later to prepare the concrete composition (post-addition).

[0128] [Table 8]

[0129] In Table 8, the binder, fine aggregate, and coarse aggregate are as shown below. Binder: Blast-furnace cement type B, density 3.04g / cm 3 Fine aggregate: Mountain sand surface dry density 2.58g / cm 3 Coarse aggregate: limestone (2005) surface dry density 2.68g / cm 3

[0130] [Table 9]

[0131] In Table 9, the binder, fine aggregate 1, fine aggregate 2, and coarse aggregate are as follows. Binder: Ordinary Portland cement, density 3.16g / cm 3 Fine aggregate 1: River sand Surface dry density 2.62g / cm 3 Fine aggregate 2: Crushed sand Surface dry density 2.65g / cm 3 Coarse aggregate: crushed stone (4005) Surface dry density 2.66g / cm 3

[0132] <Test Category 7> (Property test of prepared concrete composition) For the concrete compositions (simultaneous addition) prepared in Examples 1 to 25 and Comparative Examples 1 to 11, the slump flow (cm), air content (volume %), and bleeding rate (%) immediately after mixing were measured as follows. The results are shown in Table 10.

[0133] [Slump flow (cm)] The concrete composition immediately after mixing was measured in accordance with JIS A 1150. [Air volume (%)] The concrete composition immediately after mixing was measured in accordance with JIS A 1128. [Bleeding rate (%)] The concrete composition immediately after mixing was measured in accordance with JIS A 1123.

[0134] [Table 10]

[0135] Furthermore, the dispersibility of the one-component admixture was evaluated based on the measurement results in Table 10. The dispersibility of the one-component admixture was evaluated based on the addition ratio of the one-component admixture required to obtain the target slump flow for the concrete composition immediately after mixing. In addition, the material separation resistance of each concrete composition was evaluated using the "bleeding rate" and "integrity of materials" as indicators. The evaluation criteria are shown below. The evaluation results are shown in Table 11.

[0136] [Dispersion performance of one-liquid admixtures] A: The ratio of one-liquid admixture added per 100 parts by mass of binder is 2.00 parts by mass or less. B: The ratio of one-component admixture added to 100 parts by mass of binder is more than 2.00 parts by mass and less than 3.00 parts by mass. C: The ratio of one-liquid admixture to 100 parts by mass of binder is more than 3.00 parts by mass.

[0137] [Breeding rate] A: Bleeding rate is 4.0% or less B: Bleeding rate is over 4.0% and 6.0% or less C: Bleeding rate is over 6.0%

[0138] [Material unity (concrete properties)] A: Very good (no separation of coarse aggregate and mortar paste) B: Good (slight separation of coarse aggregate and mortar paste) C: Poor (clear separation of coarse aggregate and mortar paste)

[0139] [Table 11]

[0140] Next, the slump (cm), slump flow (cm), air content (volume%), and bleeding rate (%) of the concrete compositions (post-added) prepared in Examples 26 to 50 and Comparative Examples 12 to 22 were measured as follows. The results are shown in Table 12.

[0141] [Slump (cm)] The base concrete was measured in accordance with JIS A 1101. [Slump flow (cm)] The concrete composition after fluidization was measured in accordance with JIS A 1150. [Air volume (%)] The base concrete and the concrete composition after fluidization were measured in accordance with JIS A 1128. [Bleeding rate (%)] The concrete composition after fluidization was measured in accordance with JIS A 1123.

[0142] [Table 12]

[0143] Furthermore, the dispersibility of the one-liquid admixture was evaluated based on the measurement results in Table 12. The dispersibility of the one-liquid admixture was evaluated based on the addition ratio of the one-liquid admixture required to obtain the target slump flow for the concrete composition after fluidization. In addition, the material separation resistance of each concrete composition was evaluated using the "bleeding rate" and "integrity of materials" as indicators. The evaluation criteria are shown below. The evaluation results are shown in Table 13.

[0144] [Dispersion performance of one-liquid admixtures] A: The ratio of one-liquid admixture to 100 parts by mass of binder is 1.50 parts by mass or less. B: The ratio of one-component admixture added to 100 parts by mass of binder is more than 1.50 parts by mass and less than 2.00 parts by mass. C: The ratio of one-component admixture to 100 parts by mass of binder is more than 2.00 parts by mass.

[0145] [Breeding rate] A: Bleeding rate is 4.0% or less B: Bleeding rate is over 4.0% and 6.0% or less C: Bleeding rate is over 6.0%

[0146] [Material unity (concrete properties)] A: Very good (no separation of coarse aggregate and mortar paste) B: Good (slight separation of coarse aggregate and mortar paste) C: Poor (clear separation of coarse aggregate and mortar paste)

[0147] [Table 13]

[0148] (result) As is clear from the results shown in Tables 7, 11, and 13, it was confirmed that the present invention uses a one-component admixture (X) having excellent stability, and can provide a concrete composition having high fluidity and little separation of materials such as aggregate. Note that in Comparative Examples 4, 5, 15, and 16, the dispersibility of the one-component admixture and the material separation resistance of the concrete composition are good, but as shown in Table 7, the stability of the one-component admixture is poor. [Industrial Applicability]

[0149] The concrete composition of the present invention has excellent workability and can be used as a concrete composition for preparing a hardened concrete body having high durability.

Claims

1. Contains a binder, water, fine aggregate, coarse aggregate, and a one-component admixture (X); The water-binder ratio is 30 to 70% by mass, and the slump flow is 35 to 75 cm. The one-liquid admixture (X) is contained in a ratio of 0.3 to 3.0 parts by mass per 100 parts by mass of the binder. One-component admixture (X): The composition contains the following component A, the following component B, the following component C, the following component D, and water, and has an ionic strength derived from the component A of 0.02 to 0.8, The content ratio of the B component is 0.05 to 10 mass% when the total content ratio of the A component, the B component, the C component, the D component, and the water contained in the one-liquid admixture (X) is 100 mass%. A one-liquid admixture. Component A: The polycarboxylic acid-based water-reducing agent contains at least one selected from the group consisting of an unsaturated monocarboxylic acid monomer, an unsaturated dicarboxylic acid monomer, and a salt thereof, and a copolymer of an unsaturated monomer copolymerizable therewith and having a polyoxyalkylene group composed of 1 to 300 oxyalkylene units having 2 to 4 carbon atoms in the molecule, and a salt thereof. B component: A water-soluble cellulose ether having a mass average molecular weight of 700,000 to 1,200,000. Ingredient C: Gums. Component D: Antifoaming agent.

2. When the total content of the water contained in the A component, the B component, the C component, the D component, and the one-component admixture (X) is 100% by mass, The concrete composition according to claim 1, wherein the one-liquid admixture (X) contains the A component in a ratio of 15 to 40 mass%.

3. 3. The concrete composition according to claim 1, wherein the component B is at least one selected from the group consisting of alkyl cellulose, hydroxyalkyl cellulose, and hydroxyalkyl alkyl cellulose.

4. The concrete composition according to any one of claims 1 to 3, wherein the B component is a water-soluble cellulose ether having a viscosity of 8000 to 30000 mPa·s in a 1 mass% aqueous solution at 20°C.

5. The concrete composition according to any one of claims 1 to 4, wherein the B component is a water-soluble cellulose ether having a mass average molecular weight of 800,000 to 1,000,000.

6. The concrete composition according to any one of claims 1 to 5, wherein the C component is at least one selected from diutan gum, welan gum, xanthan gum and gellan gum.

7. The concrete composition according to any one of claims 1 to 6, wherein the water-binder ratio is 40 to 65% by mass and the slump flow is 50 to 70 cm.

8. A method for producing a concrete composition according to any one of claims 1 to 7, The method for producing a concrete composition includes preparing a base concrete containing the binder, the water, the fine aggregate, and the coarse aggregate, and then adding the one-component admixture (X) to the base concrete to produce a concrete composition.

9. A method for producing a concrete composition according to any one of claims 1 to 7, A method for producing a concrete composition by adding all of the components including the binder, the water, the fine aggregate, the coarse aggregate, and the one-liquid admixture (X) at once to produce a concrete composition.

Citation Information

Patent Citations

  • Cement composition

    JP2008137889A

  • Additive for a hydraulic composition

    JP2014125397A

  • Thickener for hydraulic composition, one-component type water-reducing agent, and hydraulic composition including thereof

    JP2016056081A

  • Additive for hydraulic composition

    JP2018030769A

  • Concrete composition and preparation method thereof

    JP2018135245A