Ethylene-vinyl alcohol copolymer composition

The combination of EVOH with unmodified and acid-modified ethylene-butene copolymers addresses the issues of low-temperature elongation and moldability in resin compositions, enhancing their hydrogen barrier properties and processing capabilities.

JP7558485B2Active Publication Date: 2024-10-01MITSUBISHI CHEM CORP

Patent Information

Application Number
JP2020126549
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-07-30
Filing Date
2020-07-27
Publication Date
2024-10-01
Estimated Expiration
2040-07-27

AI Technical Summary

Technical Problem

Existing resin compositions for fuel tanks, particularly those using ethylene-vinyl alcohol copolymers, suffer from insufficient elongation at low temperatures and processing issues such as melt fracture and shear stress during molding, which affect their moldability and hydrogen barrier properties.

Method used

A resin composition comprising ethylene-vinyl alcohol copolymer (EVOH) blended with unmodified and acid-modified ethylene-butene copolymers in specific ratios, optimizing the interaction at the molecular interface to enhance elongation at break and improve moldability while maintaining hydrogen barrier properties.

Benefits of technology

The composition achieves improved elongation at low temperatures and excellent moldability, with enhanced hydrogen barrier properties, suitable for applications requiring flexibility and gas impermeability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007558485000001
    Figure 0007558485000001
  • Figure 0007558485000002
    Figure 0007558485000002
Patent Text Reader

Abstract

To provide an EVOH resin composition that is improved in breaking elongation at low temperature and is easily subjected to molding processing while having hydrogen barrier property.SOLUTION: The resin composition contains (A) an ethylene / vinyl alcohol-based copolymer, (B) an unmodified ethylene / butene copolymer and (C) an acid-modified ethylene / butene copolymer in which the mass ratio [(B) / (C)] of the unmodified ethylene / butene copolymer (B) to the acid-modified ethylene / butene copolymer (C) is 75 / 25 to 1 / 99; and the melt flow rate (at 190°C under 2,160 g load) of the acid-modified ethylene / butene copolymer (C) is 1.0 g or more / 10 min.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an ethylene-vinyl alcohol copolymer (hereinafter sometimes referred to as "EVOH") resin composition. In particular, the present invention relates to an EVOH resin composition having hydrogen barrier properties and low-temperature elongation at break. [Background technology]

[0002] Traditionally, metals have been used as materials for fuel tanks, but recently, resins have been used to reduce weight, etc. Such plastic fuel tanks are generally molded by blow molding, injection molding, tube molding, etc. For applications requiring flexibility, for example, ethylene- A resin composition made by blending a saponified vinyl acetate copolymer with a flexible thermoplastic resin was used. A resin composition has been proposed (Patent Document 1).

[0003] The technology of Patent Document 1 aims to provide a multilayer structure having excellent oxygen barrier properties, high flexibility and flex resistance by blending an unmodified ethylene-α-olefin copolymer, an acid-modified ethylene-α-olefin copolymer, and an ethylene-vinyl alcohol copolymer having a melt flow rate (MFR) within a specific range in specific ratios, and further blending an alkali metal salt. However, there is a problem in that the elongation is insufficient when used at low temperatures.

[0004] Furthermore, a resin composition consisting of EVOH and an ethylene-butene copolymer rubber modified with an anhydride of an unsaturated carboxylic acid has been proposed for use in hydrogen fuel tanks (Patent Document 2).

[0005] The technology of Patent Document 2 aims to provide a resin composition containing EVOH and an acid-modified ethylene-butene copolymer exhibiting a specific storage modulus, which is capable of achieving both fuel (particularly hydrogen) barrier properties and impact resistance at low temperatures, and a molded article (fuel tank) using the resin composition. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] WO15 / 141610 publication [Patent Document 2] JP 2005-68300 A Summary of the Invention [Problem to be solved by the invention]

[0007] However, the technology of Patent Document 2 does not have good elongation at break (%) at low temperatures, and there is room for improvement. This is thought to be because the elastomer component is composed only of an acid-modified elastomer, and the interaction at the interface between EVOH / elastomer is too strong, making it difficult for deformation due to interfacial peeling to occur when the material is deformed, resulting in low elongation. Furthermore, the technology of Patent Document 2 has problems in molding processability when processing the EVOH resin composition into a molded article. For example, in the case of monolayer film formation, melt fracture is likely to occur, and in the case of multilayer film formation, interfacial disturbance is likely to occur due to high shear stress.

[0008] The present invention has been made in consideration of the above-mentioned conventional circumstances, and an object of the present invention is to provide an EVOH resin composition which has hydrogen barrier properties, while also improving breaking elongation at low temperatures and being easily moldable. [Means for solving the problem]

[0009] As a result of intensive research in light of the above-mentioned circumstances, the present inventors have found that the breaking elongation at low temperatures can be improved by combining specific amounts of EVOH and elastomer (unmodified ethylene-butene copolymer and specific acid-modified ethylene-butene copolymer). It is presumed that the elongation increases due to the yield deformation of the material and deformation due to interfacial peeling, because of the moderate interaction at the interface between the EVOH polymers. In addition, it was also found that such an EVOH resin composition has hydrogen barrier properties and is easy to mold, and thus the present invention was completed.

[0010] That is, the present invention is a resin composition containing an ethylene-vinyl alcohol-based copolymer (A), an unmodified ethylene-butene copolymer (B), and an acid-modified ethylene-butene copolymer (C), in which the mass ratio [(B) / (C)] of the unmodified ethylene-butene copolymer (B) to the acid-modified ethylene-butene copolymer (C) is 75 / 25 to 1 / 99, and the melt flow rate (190°C, under a load of 2160 g) of the acid-modified ethylene-butene copolymer (C) is 1.0 g / 10 min or more. The present invention also relates to a molded article having at least one layer made of the EVOH resin composition of the present invention. Effect of the Invention

[0011] The EVOH resin composition of the present invention has hydrogen barrier properties, while also improving elongation at break at low temperatures and exhibiting excellent moldability. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] The configuration of the present invention will be described in detail below, but these are merely examples of preferred embodiments, and the present invention is not limited to these contents. First, the EVOH of the present invention will be described.

[0013] <EVOH(A)> EVOH is a resin obtained by saponifying a copolymer of ethylene and a vinyl ester monomer (ethylene-vinyl ester copolymer), and is a water-insoluble thermoplastic resin. The polymerization can be carried out by any known polymerization method, such as solution polymerization, suspension polymerization, or emulsion polymerization, but generally, solution polymerization using a lower alcohol such as methanol as a solvent is used. The saponification of the obtained ethylene-vinyl ester copolymer can also be carried out by a known method. The EVOH produced in this way has ethylene structural units and vinyl alcohol structural units as main structural units, and contains a small amount of vinyl ester structural units remaining without being saponified.

[0014] As the vinyl ester monomer, vinyl acetate is typically used because of its ease of availability on the market and its high efficiency in treating impurities during production. Other vinyl ester monomers include, for example, aliphatic vinyl esters such as vinyl formate, vinyl propionate, vinyl valerate, vinyl butyrate, vinyl isobutyrate, vinyl pivalate, vinyl caprate, vinyl laurate, vinyl stearate, and vinyl versatate, and aromatic vinyl esters such as vinyl benzoate, and aliphatic vinyl esters having 3 to 20 carbon atoms, preferably 4 to 10 carbon atoms, and particularly preferably 4 to 7 carbon atoms can be used. These are usually used alone, but multiple types may be used simultaneously as necessary.

[0015] The ethylene content in EVOH is preferably 20 to 60 mol%, more preferably 25 to 50 mol%, particularly preferably 25 to 30 mol%, and especially preferably 25 to 28 mol%, as measured based on ISO 14663. If the ethylene content is too low, the oxygen barrier properties and melt moldability under high humidity conditions tend to decrease, whereas if the ethylene content is too high, the melt viscosity on the low shear side tends to decrease.

[0016] The degree of saponification of the vinyl ester component in EVOH is preferably 90 to 100 mol%, more preferably 95 to 100 mol%, and particularly preferably 99 to 100 mol%, as measured according to JIS K6726 (wherein EVOH is a solution uniformly dissolved in a water / methanol solvent). If the degree of saponification is too low, the oxygen barrier property, heat stability, moisture resistance, etc. tend to decrease.

[0017] The melt flow rate (MFR) of EVOH (210°C, load 2,160 g) is preferably 0.5 to 100 g / 10 min, more preferably 1 to 50 g / 10 min, and particularly preferably 3 to 35 g / 10 min. If the MFR is too high, the film formability tends to decrease, and if the MFR is too low, the melt viscosity tends to be too high, making melt extrusion difficult.

[0018] EVOH may further contain structural units derived from the comonomers shown below, in addition to ethylene structural units and vinyl alcohol structural units (including unsaponified vinyl ester structural units). Examples of the comonomers include α-olefins such as propylene, isobutene, α-octene, α-dodecene, and α-octadecene; hydroxyl-containing α-olefins such as 3-buten-1-ol, 4-penten-1-ol, and 3-buten-1,2-diol, and hydroxyl-containing α-olefin derivatives such as esters and acylations thereof; unsaturated carboxylic acids or salts thereof, partial alkyl esters thereof, complete alkyl esters thereof, nitriles thereof, amides thereof, or anhydrides thereof; unsaturated sulfonic acids or salts thereof; vinylsilane compounds; vinyl chloride; and styrene.

[0019] Furthermore, EVOH that has been "post-modified" by urethanization, acetalization, cyanoethylation, oxyalkylenation, or the like can also be used.

[0020] Among the above-mentioned modified products, EVOH in which a primary hydroxyl group has been introduced into the side chain by copolymerization is preferred because it has good secondary formability in stretching treatment and vacuum / pressure molding, and among these, EVOH having a 1,2-diol structure in the side chain is preferred.

[0021] The EVOH may contain additives that can generally be added to EVOH, such as heat stabilizers, antioxidants, antistatic agents, colorants, ultraviolet absorbers, lubricants, plasticizers, light stabilizers, surfactants, antibacterial agents, drying agents, antiblocking agents, flame retardants, crosslinking agents, curing agents, foaming agents, crystal nucleating agents, antifogging agents, biodegradable additives, silane coupling agents, oxygen absorbers, etc., within the scope of the invention.

[0022] The heat stabilizer is used for the purpose of improving various physical properties such as thermal stability during melt molding, and examples thereof include organic acids such as acetic acid, propionic acid, butyric acid, lauric acid, stearic acid, oleic acid, behenic acid, etc., or salts thereof such as alkali metal salts (sodium, potassium, etc.), alkaline earth metal salts (calcium, magnesium, etc.), zinc salts, etc.; or inorganic acids such as sulfuric acid, sulfurous acid, carbonic acid, phosphoric acid, boric acid, etc., or salts thereof such as alkali metal salts (sodium, potassium, etc.), alkaline earth metal salts (calcium, magnesium, etc.), zinc salts, etc.

[0023] In addition, EVOH may be a mixture with other different EVOHs. Examples of such other EVOHs include those having a different ethylene content, a different degree of saponification, a different melt flow rate (MFR) (210°C, load 2,160 g), a different copolymerization component, and a different degree of modification (for example, those having a different content of 1,2-diol structural units).

[0024] In addition to EVOH, EVOH may contain other resins as necessary, so long as the effects of the present invention are not impaired. For example, EVOH may contain polyamide resins such as nylon 11, nylon 12, nylon 6, nylon 66, and nylon 6-66; unmodified vinyl alcohol resins not having the structural unit of the above general formula (1); and other thermoplastic resins. The content of resins that can be blended in addition to EVOH is usually 50% by weight or less, preferably 40% by weight or less, based on the EVOH, and it is particularly preferred that no other resins are contained.

[0025] The EVOH resin composition of the present invention is characterized in that it uses an unmodified ethylene-butene copolymer (B) and a specific acid-modified ethylene-butene copolymer (C) in combination.

[0026] <Unmodified ethylene-butene copolymer (B)> The unmodified ethylene-butene copolymer of the present invention is not particularly limited, and any known ethylene-butene copolymer can be used.

[0027] The density of the unmodified ethylene-butene copolymer (B) is usually 0.9 g / cm 3 is as follows: Preferably 0.89 g / cm 3 or less, and particularly preferably 0.88 g / cm 3 By using such a low-density unmodified ethylene-butene copolymer (B), a molded article having excellent elongation at break at low temperature can be obtained. The density of the unmodified ethylene-butene copolymer (B) is usually 0.85 g / cm 3 That's all.

[0028] The unmodified ethylene-butene copolymer (B) has an MFR of usually 1.0 g / 10 min to 100 g / 10 min, preferably 2.0 g / 10 min to 60 g / 10 min, at 190° C. and under a load of 2160 g. By using such an unmodified ethylene-butene copolymer (B), the stability of the resulting resin composition during extrusion processing and the elongation at break at low temperatures of the resulting molded article can be further improved.

[0029] Moreover, the unmodified ethylene-butene copolymer (B) is preferably an ethylene-1-butene copolymer from the viewpoint of productivity.

[0030] The term "unmodified ethylene-butene copolymer" used herein refers to an unmodified ethylene-butene copolymer that has not been acid-modified, and is not, for example, the acid-modified ethylene-butene copolymer (C) described below. The acid value of the unmodified ethylene-butene copolymer (B) used in the present invention is preferably less than 0.5 mgKOH / g.

[0031] [Acid-modified ethylene-butene copolymer (C)] The acid-modified ethylene-butene copolymer (C) used in the present invention can be obtained by copolymerizing a part of the monomers constituting the ethylene-butene copolymer by replacing them with an α,β-unsaturated carboxylic acid or anhydride monomer, or by introducing an α,β-unsaturated carboxylic acid or anhydride thereof into a part of the side chain by a graft reaction such as radical addition.

[0032] Examples of the α,β-unsaturated carboxylic acid or anhydride thereof used for the acid modification include maleic acid, acrylic acid, itaconic acid, crotonic acid, maleic anhydride, itaconic anhydride, etc. Among these, maleic anhydride is preferably used.

[0033] The acid value of the acid-modified ethylene-butene copolymer (C) is usually 50 mgKOH / g or less, preferably 30 mgKOH / g or less, and particularly preferably 20 mgKOH / g or less. If the acid value is too high, the number of reaction sites with the hydroxyl groups in the EVOH (A) increases, and high polymerization products are generated during the melt-kneading process, which reduces stability during extrusion processing and tends to make it difficult to obtain a good molded product. On the other hand, if the acid value is too low, the compatibility with the EVOH (A) decreases, and the amount of resin adhering to the die during extrusion processing (pitting) tends to increase and the elongation at break at low temperatures tends to decrease. The lower limit of the acid value is usually 1 mgKOH / g or more, and preferably 2 mgKOH / g or more.

[0034] The density of the acid-modified ethylene-butene copolymer (C) is usually 0.9 g / cm 3 or less, preferably 0.89 g / cm 3 or less, and particularly preferably 0.88 g / cm3 By using such a low-density acid-modified ethylene-butene copolymer (C), it is possible to obtain a molded article and a multilayer structure having excellent elongation at break, particularly at low temperatures. The density of the acid-modified ethylene-butene copolymer (C) is usually 0.85 g / cm 3 That's all.

[0035] The MFR of the acid-modified ethylene-butene copolymer (C) at 190°C and under a load of 2160g is 1.0g or more / 10min, preferably 1.5g or more / 10min, and particularly preferably 2.0g or more / 10min. By using such an acid-modified ethylene-butene copolymer (C), the elongation at break at low temperatures can be further improved. The upper limit of the MFR is usually 60g / 10min or less.

[0036] From the viewpoint of productivity, the acid-modified ethylene-butene copolymer (C) is preferably an acid-modified ethylene-1-butene copolymer.

[0037] <Mass ratio of (A), (B), and (C)> In the resin composition of the present invention, the mass ratio [(A) / ((B)+(C))] of the amount of EVOH (A) to the total amount of unmodified ethylene-butene copolymer (B) and acid-modified ethylene-butene copolymer (C) is usually 60 / 40 to 99 / 1, preferably 60 / 40 to 79 / 21, particularly preferably 60 / 40 to 75 / 25, and particularly preferably 60 / 40 to 69 / 31, from the viewpoint of elongation at break at low temperature. If the mass ratio [(A) / ((B)+(C))] exceeds 99 / 1, or if unmodified ethylene-butene copolymer (B) and acid-modified ethylene-butene copolymer (C) are not included, the elongation at break at low temperature of the obtained molded article becomes insufficient. On the other hand, if the mass ratio [(A) / ((B)+(C))] is less than 60 / 40, EVOH (A) does not become a matrix phase, and the hydrogen barrier property of the molded article becomes insufficient.

[0038] [Mass ratio of (B) and (C)] The mass ratio [(B) / (C)] of the unmodified ethylene-butene copolymer (B) and the acid-modified ethylene-butene copolymer (C) is 75 / 25 to 1 / 99, preferably 70 / 30 to 10 / 90, more preferably 65 / 35 to 15 / 85, and particularly preferably 60 / 40 to 35 / 65, from the viewpoint of elongation at break at low temperature. If the mass ratio [(B) / (C)] exceeds 75 / 25, the elongation at break at low temperature of the obtained molded product becomes insufficient. On the other hand, if the mass ratio [(B) / (C)] is less than 1 / 99, eye discharge increases and moldability becomes insufficient.

[0039] [Other additives] The EVOH resin composition used in the present invention may contain, in addition to the above-mentioned EVOH (A), unmodified ethylene-butene copolymer (B) and acid-modified ethylene-butene copolymer (C), polyamide resins such as nylon 11, nylon 12, nylon 6, nylon 66 and nylon 6-66, as necessary, so long as the effects of the present invention are not impaired (for example, less than 5% by weight of the entire resin composition); unmodified vinyl alcohol-based resins not having the structural unit of the above general formula (1); other thermoplastic resins; plasticizers such as aliphatic polyhydric alcohols such as ethylene glycol, glycerin and hexanediol; saturated aliphatic amides (for example, stearic acid amide, etc.), unsaturated fatty acid amides (for example, oleic acid amide, etc.), bisfatty acid amides (for example, ethylene bisstearic acid amide, etc.), etc. and the like), low molecular weight polyolefin (for example, low molecular weight polyethylene having a molecular weight of about 500 to 10,000, or low molecular weight polypropylene); antiblocking agent; antioxidant; colorant; antistatic agent; ultraviolet absorber; antibacterial agent; insoluble inorganic salt (for example, hydrotalcite); filler (for example, inorganic filler); oxygen absorber (for example, ring-opening polymer of cycloalkenes such as polyoctenylene, or cyclized product of conjugated diene polymer such as butadiene); surfactant, wax; dispersant (stearic acid monoglyceride, etc.), heat stabilizer, light stabilizer, drying agent, flame retardant, crosslinking agent, curing agent, foaming agent, crystal nucleating agent, antifogging agent, biodegradable additive, silane coupling agent, conjugated polyene compound, and other known additives can be appropriately blended.

[0040] [EVOH Resin Composition and Its Preparation] The EVOH resin composition can be prepared by blending the above-mentioned EVOH (A), the unmodified ethylene-butene copolymer (B), and the acid-modified ethylene-butene copolymer (C), and further additives added as necessary, in a predetermined ratio, and melt-kneading the mixture.

[0041] For the melt kneading, a known kneading machine such as an extruder, a Banbury mixer, a kneader-ruder, a mixing roll, a blast mill, etc., can be used. For example, in the case of an extruder, a single-screw or twin-screw extruder can be used. After melt kneading, a method can be adopted in which the resin composition is extruded into a strand shape, cut, and pelletized. Such melt-kneading may be carried out by charging the EVOH (A), the unmodified ethylene-butene copolymer (B) and the acid-modified ethylene-butene copolymer (C) all at once, or by side-feeding the unmodified ethylene-butene copolymer (B) and the acid-modified ethylene-butene copolymer (C) in a molten or solid state while melt-kneading the EVOH (A) in a twin-screw extruder.

[0042] The melt-kneading temperature is appropriately selected depending on the types of EVOH (A), unmodified ethylene-butene copolymer (B), and acid-modified ethylene-butene copolymer (C), but is usually 215 to 270°C, preferably 215 to 265°C, more preferably 220 to 260°C, and particularly preferably 220 to 250°C.

[0043] Such a resin composition has excellent hydrogen gas barrier properties based on the constituent EVOH (A), and the unmodified ethylene-butene copolymer (B) and the acid-modified ethylene-butene copolymer (C) improve the breaking elongation at low temperatures, which was a weakness of EVOH. This is because there is a moderate interaction at the interface between EVOH and the elastomer, and the yield deformation of the material is improved. This is presumably because the elongation increases due to deformation caused by interfacial peeling.

[0044] The resin composition as described above not only has excellent gas barrier properties against hydrogen gas, but also has excellent gas barrier properties against other gases such as helium, oxygen, nitrogen, and air, and is particularly excellent in barrier properties against gases having a molecular weight of less than 10, such as hydrogen.

[0045] The hydrogen permeability of the resin composition of the present invention is usually 200cc·20μm / m 2 ·day·atm Less than 180cc 20μm / m 2 ·day·atm or less, especially Preferably 160cc 20μm / m 2 The hydrogen permeability is less than 1000 mbar / day atm. If the thickness is too high, for example in the case of a hydrogen gas container, hydrogen gas permeation from the inside of the container increases, and the amount of gas inside the container tends to decrease excessively over time. 2 If the temperature is below 100°C (days atm), it has hydrogen gas barrier properties.

[0046] In addition, the method for obtaining a molded article using the resin composition of the present invention is not particularly limited, but a molding method applicable to known thermoplastic resins such as polyolefins and polyamides can be applied. For example, melt molding methods such as extrusion molding, coextrusion molding, injection molding, blow molding, tube molding, and rotational molding can be mentioned. For example, for hollow molded articles such as fuel tanks, extrusion blow molding is generally used, for tube (pipe) shaped containers, tube molding is generally used, and for molded articles with complex shapes or requiring dimensional accuracy, injection molding is generally used.

[0047] The resin composition of the present invention was subjected to a shear rate test at 210°C and a shear rate of 18 sec. -1The melt viscosity at is usually 10000 (mPa·s) or less, preferably 9000 (mPa·s) or less, particularly preferably 8000 (mPa·s) or less. It is usually 1000 (mPa·s) or more, preferably 3000 (mPa·s) or more, particularly preferably 5500 (mPa·s) or more. If the melt viscosity is too high, the molding processability tends to decrease. If it is too low, the molding processability also tends to decrease. For example, if the melt viscosity is too high, melt fracture tends to occur easily in the case of single-layer film formation, and interface disturbance due to high shear stress tends to occur easily in the case of multi-layer film formation. If the melt viscosity is too low, molding tends to be difficult due to the occurrence of drawdown in the molding of films, etc.

[0048] The molded article using the resin composition of the present invention includes at least one layer made of the resin composition (hereinafter, may be referred to as a "gas barrier layer".) For the purpose of adding various physical properties, the molded article may have a multi-layer structure with various other thermoplastic resins. Among the molded articles having a multi-layer structure, the one containing a gas barrier layer as an inner layer (i.e., a layer in contact with high-pressure gas or fuel) or an intermediate layer, more preferably as an intermediate layer. Furthermore, it is preferable that the inner layer and / or the outer layer (i.e., a layer in contact with the outside air) contains a water-resistant, moisture-impermeable thermoplastic resin layer. The intermediate layer refers to a layer between the outer layer and the inner layer. In addition, a reinforcing layer may be provided on the outer layer. When a reinforcing layer is provided, the reinforcing layer becomes the layer in contact with the outside air (the outermost layer). Furthermore, an adhesive layer made of an adhesive resin may be provided between these layers.

[0049] Therefore, examples of the multilayer structure constituting the molded product include, in order from the inside, gas barrier layer / moisture-impermeable thermoplastic resin layer, moisture-impermeable thermoplastic resin layer / gas barrier layer, moisture-impermeable thermoplastic resin layer / gas barrier layer / moisture-impermeable thermoplastic resin layer, gas barrier layer / moisture-impermeable thermoplastic resin layer / reinforcing layer, moisture-impermeable thermoplastic resin layer / gas barrier layer / reinforcing layer, moisture-impermeable thermoplastic resin layer / gas barrier layer / moisture-impermeable thermoplastic resin layer / reinforcing layer, etc. Preferred are moisture-impermeable thermoplastic resin layer / gas barrier layer / moisture-impermeable thermoplastic resin layer, moisture-impermeable thermoplastic resin layer / gas barrier layer / moisture-impermeable thermoplastic resin layer / reinforcing layer. An adhesive layer may be provided between the layers of the multilayer structure constituting these molded products. The number of layers of the multilayer structure, including the reinforcing layer, is usually 3 to 15 layers, preferably 4 to 10 layers.

[0050] As the thermoplastic resin used in the moisture-impermeable thermoplastic resin layer, for example, hydrophobic thermoplastic resin is preferably used.Specific examples of the thermoplastic resin include polyethylene-based resins such as linear low-density polyethylene (LLDPE), low-density polyethylene (LDPE), medium-density polyethylene (MDPE), and high-density polyethylene (HDPE); polypropylene-based resins such as ethylene-vinyl acetate copolymer, ionomer, ethylene-propylene copolymer, ethylene-α-olefin (α-olefin having 4 to 20 carbon atoms) copolymer, ethylene-acrylic acid ester copolymer, polypropylene, and propylene-α-olefin (α-olefin having 4 to 20 carbon atoms) copolymer; olefin homo- or copolymers such as polybutene and polypentene, cyclic polyolefins, or homo- or copolymers of these olefins graft-modified with unsaturated carboxylic acid or its ester (carboxylic acid-modified polyolefin resins). polyolefin resins in the broad sense, such as polyolefin resins (polyolefin resins modified with ethylene glycol, ester-modified polyolefin resins, etc.); polystyrene resins; polyamide resins, such as polyamides such as nylon 11, nylon 12, nylon 6, nylon 66, etc., and copolymer polyamides such as nylon 6·12, nylon 6·66, etc.; vinyl ester resins, such as polyvinyl chloride, polyvinylidene chloride, acrylic resins, and polyvinyl acetate; polyurethane resins; fluorine-based polymers, such as tetrafluoroethylene, tetrafluoroethylene / perfluoro(alkyl vinyl ether) copolymer, ethylene / tetrafluoroethylene copolymer, and tetrafluoroethylene / hexafluoropropylene copolymer; chlorinated polyethylene; chlorinated polypropylene; fluorine-based resins having polar groups, and thermoplastic resins, such as thermoplastic polyurethane.

[0051] For the adhesive layer, known adhesive resins can be used, and usually, carboxylic acid-modified polyolefin resins obtained by modifying polyolefin resins with unsaturated carboxylic acids (or unsaturated carboxylic acid anhydrides) such as maleic acid, or fluororesins having polar groups are preferably used. For the polyolefin resin, the polyolefin resins listed as thermoplastic resins used for the moisture-impermeable thermoplastic resin layer can be used.

[0052] Examples of the reinforcing layer include a reinforcing fiber layer using fiber and a reinforcing rubber layer using rubber. Examples of the reinforcing fiber layer that can be used include high-strength fibers such as polyparaphenylene benzbisoxazole (PBO) fibers, aramid fibers, and carbon fibers, nonwoven fabrics, and cloths. A reinforcing fiber layer is preferable, a reinforcing fiber layer using high-strength fibers is particularly preferable, and a sheet layer in which high-strength fibers are woven or a reinforcing fiber layer in which the sheet is spirally wound is even more preferable.

[0053] As described above, the resin composition of the present invention is useful as a molded article having excellent hydrogen gas barrier properties and low-temperature breaking elongation. The molded article using the resin composition of the present invention can be used as a fuel tank for high-pressure hydrogen gas (pressure 1 to 100 MPa) or the like, and a fuel tank part thereof.

[0054] Furthermore, a molded article using the resin composition of the present invention can be processed into, for example, a tubular or bag-like shape and used for a wide range of applications, such as packaging materials for foods, such as mirin, soy sauce, sauce, noodle soup, and edible oil; beverages, such as wine, juice, milk, mineral water, sake, shochu, coffee, and black tea; pharmaceuticals, cosmetics, industrial chemicals, such as sodium hypochlorite, developing solution, and battery fluid; agricultural chemicals, such as liquid fertilizer; and detergents.

[0055] <Multilayer structure> The molded article using the resin composition of the present invention for the above-mentioned applications may be a multilayer structure having at least one layer made of the resin composition of the present invention (hereinafter simply referred to as "resin composition layer"). The resin constituting the layer other than the resin composition layer constituting the multilayer structure of the present invention is not particularly limited, but may be a thermoplastic resin other than EVOH resin.Specific examples of the resin constituting the layer other than the resin composition layer constituting the multilayer structure of the present invention include layers composed of thermoplastic resins such as linear low density polyethylene, low density polyethylene, medium density polyethylene, high density polyethylene, ethylene-vinyl acetate copolymer, ionomer, ethylene-propylene copolymer, ethylene-acrylic acid ester copolymer, polypropylene, propylene-α-olefin (α-olefin having 4 to 20 carbon atoms) copolymer, polybutene, polypentene, and other olefin homo- or copolymers, cyclic polyolefins, or graft-modified homo- or copolymers of these olefins with unsaturated carboxylic acid or its ester, polystyrene resins, polyesters, polyamides, copolymerized polyamides, polyvinyl chloride, polyvinylidene chloride, acrylic resins, vinyl ester resins, polyester elastomers, polyurethane elastomers, chlorinated polyethylene, and chlorinated polypropylene. In addition to these resins, it may be a multilayer structure in which it is combined with paper, metal foil, uniaxially or biaxially oriented plastic film or sheet, woven fabric, nonwoven fabric, metal cotton strip, wood surface, aluminum or silica vapor deposition, etc. Among these, polyolefin resins are preferred in terms of mechanical strength and melt molding processability, and polyethylene and polypropylene are particularly preferred.

[0056] Among these, a multilayer structure having a thermoplastic resin layer having excellent water barrier properties as an outer surface layer and a resin composition layer as an intermediate layer is preferably used for packaging films and packaging containers having gas barrier properties. As such a thermoplastic resin having excellent water barrier properties, polyolefin resins are preferred, and polyethylene and polypropylene are particularly preferred.

[0057] Methods for producing the multilayer structure are roughly classified into a method in which a resin composition is molded in a molten state (melt molding method) and a method in which a resin composition is dissolved in a solvent and molded (e.g., solution coating method), etc. Among them, the melt molding method is preferred from the viewpoint of productivity. Specifically, for example, there may be mentioned a method of melt-extruding a thermoplastic resin onto a molded article (e.g., a film or sheet) of the resin composition of the present invention, a method of melt-extruding a resin composition layer onto a substrate such as a thermoplastic resin, and a method of co-extruding a resin composition layer and a thermoplastic resin layer. In detail, T-die extrusion, tubular extrusion, blow molding, irregular shape extrusion, etc. may be employed. Further, a method of dry laminating the resin composition film of the present invention and a substrate such as a thermoplastic resin film using a known adhesive such as an organic titanium compound, an isocyanate compound, a polyethyleneimine compound, a polyester compound, or a polyurethane compound, or a method of laminating them through an adhesive resin layer may be employed. In some cases, a coinjection method may also be used.

[0058] The adhesive resin constituting the adhesive resin layer is not particularly limited, and various types can be used, but generally, it can be a modified olefin polymer containing a carboxyl group obtained by chemically bonding an unsaturated carboxylic acid or its anhydride to an olefin polymer (the polyolefin resin in the broad sense described above) by addition reaction, graft reaction, or the like. Specifically, suitable examples include one or a mixture of two or more types selected from maleic anhydride grafted modified polyethylene, maleic anhydride grafted modified polypropylene, maleic anhydride grafted modified ethylene-ethyl acrylate copolymer, maleic anhydride grafted modified ethylene-vinyl acetate copolymer, etc.

[0059] As described above, the multilayer structure of the present invention for use as a packaging film or packaging container may include at least one layer of the resin composition of the present invention, and the configuration is not particularly limited. However, for the purpose of preventing a decrease in the gas barrier performance of the resin composition due to moisture, it is preferable that the resin composition layer be an intermediate layer.

[0060] The layer structure of the multilayer structure for use as a packaging film or packaging container, where the resin composition layers are a (a1, a2, ...) and the thermoplastic resin layers other than the EVOH resin are b (b1, b2, ...), is usually 3 to 20 layers, preferably 3 to 15 layers, and particularly preferably 3 to 10 layers. For example, specific combinations such as b / a / b, a / b / a, a1 / a2 / b, a / b1 / b2, b2 / b1 / a / b1 / b2, and b2 / b1 / a / b1 / a / b1 / b2 are possible. Furthermore, when R denotes a recycled layer containing a mixture of a resin composition and a thermoplastic resin other than EVOH, obtained by remelting and molding edges and defective products generated during the manufacturing process of the multilayer structure, it is also possible to designate it as b / a / R, R / b / a, b / R / a / b, b / R / a / R / b, b / a / R / a / b, b / R / a / R / a / R / b, etc. Furthermore, a known adhesive resin may be used between the layers of the multi-layer structure.

[0061] Among them, in order to prevent the gas barrier performance of the resin composition layer from being deteriorated, a multilayer structure in which the resin composition layer serves as an intermediate layer is most preferred so as to prevent moisture from penetrating into the resin composition layer.Specifically, for example, a multilayer structure having a thermoplastic resin layer / adhesive resin layer / resin composition layer / adhesive resin layer / thermoplastic resin layer as constituent units is most preferred.

[0062] The thickness of the multilayer structure of the present invention for use as a packaging film or packaging container is usually 1 to 1500 μm, preferably 1 to 1000 μm, more preferably 10 to 700 μm. The thickness of the thermoplastic resin layer in the multilayer structure is not particularly limited, but is usually 0.1 to 1000 μm, preferably 1 to 500 μm. The thickness of the resin composition layer is not particularly limited, but is usually 0.1 to 500 μm, preferably 1 to 100 μm. The thickness of the adhesive resin layer is not particularly limited, but is usually 0.1 to 250 μm, preferably 0.1 to 100 μm.

[0063] In addition, when there are multiple layers of each type, the thickness ratio of the thermoplastic resin layer / resin composition layer, as the ratio between the thickest layers, is usually greater than 1 and 30, and preferably 2 to 30, and the thickness ratio of the adhesive resin layer / resin composition layer is usually 0.1 to 2, and preferably 0.1 to 1.

[0064] The multilayer structure of the present invention for use as a packaging film or packaging container is, as described above, a multilayer structure simply laminated with other thermoplastic resins or substrates, but may be subjected to a stretching treatment.

[0065] For the stretching, a known stretching method can be used. Examples include uniaxial stretching and biaxial stretching. In the case of biaxial stretching, either a simultaneous biaxial stretching method or a sequential biaxial stretching method can be adopted. The stretching temperature is selected from the range of usually 40 to 170°C, preferably about 60 to 160°C, as the temperature of the multilayer structure (temperature in the vicinity of the multilayer structure). The stretching ratio is usually 2 to 50 times, preferably 2 to 20 times, in terms of area ratio. In addition, for the purpose of imparting dimensional stability to the obtained stretched film, heat setting may be performed after the end of stretching. Heat setting can be performed by a known means, and the stretched film is heat-treated at 80 to 180°C, preferably 100 to 165°C, for about 2 to 600 seconds while maintaining the tension of the stretched film. EXAMPLES

[0066] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following examples as long as it does not depart from the gist of the invention. In the examples, "%" and "parts" are based on weight.

[0067] [Materials used] The following materials were used as the resin composition materials.

[0068] (EVOH) A-1: EVOH (ethylene content: 25 mol%, saponification degree: 99.7 mol%, MFR: 4.0 g / 10 min (210°C, 2,160 g load)) A-2: EVOH (ethylene content: 29 mol%, saponification degree: 99.7 mol%, MFR: 8.0 g / 10 min (210°C, 2,160 g load))

[0069] (Unmodified polyolefin) B-1: "A4085S" ethylene-butene copolymer manufactured by Mitsui Chemicals, Inc. (MFR: 3.6g / 10min (190℃, 2,160g load), density: 0.885g / cm 3 ) B-2: "P0180" ethylene-propylene copolymer manufactured by Mitsui Chemicals Inc. (MFR: 4.4g / 10min (190℃, 2,160g load), density: 0.869g / cm 3 )

[0070] (Acid-modified polyolefin) C-1: Mitsui Chemicals "MA8510" acid-modified ethylene-butene copolymer (MFR: 2.4g / 10min (190℃, 2,160g load), density: 0.885g / cm 3 ) C-2: Mitsui Chemicals "MH7010" acid-modified ethylene-butene copolymer (MFR: 0.9g / 10min (190℃, 2,160g load), density: 0.870g / cm 3 ) C-3: Mitsui Chemicals "MP0610" acid-modified ethylene-propylene copolymer (MFR: 0.4g / 10min (190℃, 2,160g load), density: 0.870g / cm 3 )

[0071] <Example 1> [Preparation of resin composition pellets] The components were dry blended in the ratios shown in Table 1, then melt-kneaded in a twin-screw extruder under the conditions shown below, extruded into strands and cut with a pelletizer to obtain cylindrical pellets of the resin composition. (Melting and kneading conditions) Diameter (D) 30mm L / D=56 Screw rotation speed: 400 rpm Setting temperature: C2 / C3 / C4 / C5 / C6 / C7 / C8 / C9 / C10 / C11 / C12 / C13 / C14 / C15 / C16 / D=80 / 120 / 190 / 210 / 210 / 210 / 210 / 220 / 220 / 220 / 230 / 230 / 230 / 230 / 230 / 230℃ Discharge amount: 25kg / hr

[0072] Next, the following measurements and evaluations were carried out using the prepared resin composition pellets.

[0073] (1) Breaking elongation (%) The pellets obtained were used to make ISO1A dumbbells using an injection molding machine, and tensile tests were performed at -40°C using a tensile testing machine. The test pieces were prepared and evaluated in accordance with ISO14663, and measurements were performed at a tensile speed of 50mm / min. The results are shown in Table 1.

[0074] (2) Melt viscosity (mPas) The pellets obtained were mixed at 210°C and a shear rate of 18 sec using a Toyo Seiki Co., Ltd. Capillograph 1D in the following manner. -1 The melt viscosity was measured at 100° C. The results are shown in Table 1. Capillary diameter: 1 mm Capillary length: 10mm

[0075] <Examples 2 to 15> Resin composition pellets were prepared in the same manner as in Example 1, except that the ratios of each component were changed as shown in Table 1, and were evaluated in the same manner.

[0076] <Comparative Examples 1 to 6> Resin composition pellets were prepared in the same manner as in Example 1, except that the ratios of each component were changed as shown in Table 1, and were evaluated in the same manner.

[0077] [Table 1]

[0078] The results in Table 1 show that the resin compositions of Examples 1 to 15 are excellent in elongation at break at low temperatures, and also excellent in moldability.

[0079] Furthermore, for the resin compositions having the formulations shown in Table 2, resin composition films were prepared by the following method, and the following measurements and evaluations were carried out.

[0080] [Preparation of resin composition film] The pellets obtained above were extruded into a single-layer film having a thickness of 100 μm under the following conditions using a single-screw extruder. (Film forming conditions) Diameter (D) 40mm L / D=28 Screw shape: Full flight Screw rotation speed: 20 rpm Setting temperature: C1 / C2 / C3 / C4 / H / D =200 / 220 / 220 / 220 / 22 0 / 220℃ Die: Coat hanger type Roll temperature: 80℃

[0081] (3) Hydrogen permeability (cc 20μm / m 2 ·day·atm) A film test piece with a thickness of 100 μm was measured using the "GTR-30XAD2 G2700T-F" manufactured by GTR Tech Co., Ltd. and Yanako Technical Science Co., Ltd. in the following manner. The hydrogen gas permeability was measured, and the results are shown in Table 2. Test method: Differential pressure method / JIS K 7126-1 Detector: GC [thermal conductivity detector] Test gas: Hydrogen Measurement temperature: 23℃ Transmission area: φ4.4×10 -2 m (15.2×10 -4 m 2 )

[0082] [Table 2]

[0083] The results in Table 2 show that the resin compositions of Examples 1, 6 and 13 have excellent hydrogen gas barrier properties. [Industrial Applicability]

[0084] The EVOH resin composition of the present invention has hydrogen barrier properties, while improving breaking elongation at low temperatures and exhibiting excellent moldability. Therefore, a molded article containing a layer made of the EVOH resin composition is useful as a raw material for fuel tanks for high-pressure hydrogen gas and the like, and parts for such fuel tanks.

Claims

1. A resin composition comprising an ethylene-vinyl alcohol copolymer (A), an unmodified ethylene-butene copolymer (B), and an acid-modified ethylene-butene copolymer (C), the content of the ethylene-vinyl alcohol-based copolymer (A), the unmodified ethylene-butene copolymer (B), and the acid-modified ethylene-butene copolymer (C) in the resin composition is 95 to 100% by weight, a mass ratio of the ethylene-vinyl alcohol-based copolymer (A) to the total amount of the unmodified ethylene-butene copolymer (B) and the acid-modified ethylene-butene copolymer (C) [(A) / ((B)+(C)]] is 60 / 40 to 75 / 25 (excluding 75 / 25); a mass ratio [(B) / (C)] of the unmodified ethylene-butene copolymer (B) to the acid-modified ethylene-butene copolymer (C) is 75 / 25 to 15 / 85; A resin composition characterized in that the ethylene-vinyl alcohol copolymer (A) has an ethylene content of 20 to 60 mol % and a degree of saponification of 90 to 100 mol %, and the acid-modified ethylene-butene copolymer (C) has a melt flow rate (190°C, under a load of 2160 g) of 1.0 g or more / 10 min.

2. The resin composition according to claim 1, wherein a mass ratio of the ethylene-vinyl alcohol-based copolymer (A) to the total amount of the unmodified ethylene-butene copolymer (B) and the acid-modified ethylene-butene copolymer (C) [(A) / ((B)+(C)]] is 60 / 40 to 70 / 30.

3. 210°C, shear rate 18sec -1 3. The resin composition according to claim 1, wherein the melt viscosity at 2000° C. is 10,000 mPas or less.

4. Hydrogen permeability is 200cc / 20μm / m 2 4. The resin composition according to claim 1, wherein the viscosity is 1000 sq.m.

Citation Information

Patent Citations

  • Resin composition and fuel-based resin molded article

    JP2005068300A

  • Blow-molded container with pinch-off part

    WO2013172226A1

  • Resin composition, multi-layer structure, and bag-in-box inner container

    WO2015141610A1

Cited By

  • Ethylene-vinyl alcohol copolymer composition

    JPWO2022158589A1