Thermoplastic resin and its manufacturing method

A thermoplastic resin derived from natural sources, utilizing methyl-β-D-3,4-dideoxy-galactopyranoside and other dihydroxy compounds, addresses the imbalance in glass transition and mass loss temperatures, providing enhanced heat resistance for practical applications.

JP7558500B2Active Publication Date: 2024-10-01MITSUBISHI GAS CHEM CO INC +1
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2020200923
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-12-03
Publication Date
2024-10-01
Estimated Expiration
2040-12-03

AI Technical Summary

Technical Problem

There is a need for thermoplastic resins, particularly polycarbonate resins, derived from natural products that offer a balanced glass transition temperature and 5% mass loss temperature suitable for practical applications, as existing resins from natural sources often lack this balance.

Method used

A thermoplastic resin containing structural units derived from methyl-β-D-3,4-dideoxy-galactopyranoside, combined with other dihydroxy compounds, is formulated to achieve a balanced glass transition temperature and 5% mass loss temperature, using a specific molar ratio and production method that includes transesterification and polycondensation under controlled conditions.

Benefits of technology

The resulting resin exhibits superior heat resistance with a balanced glass transition temperature and 5% mass loss temperature, making it suitable for various applications including equipment housings and automobile parts.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007558500000001
    Figure 0007558500000001
  • Figure 0007558500000002
    Figure 0007558500000002
  • Figure 0007558500000003
    Figure 0007558500000003
Patent Text Reader

Abstract

To provide a thermoplastic resin which is produced using ingredients derived from natural products, has a glass transformation temperature and a 5% mass loss temperature that are not extremely high or low, and is practically balanced.SOLUTION: The thermoplastic resin comprises a constitutional unit (A) represented by the formula (1) in the figure.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a thermoplastic resin and a method for producing the same, and more particularly to a polycarbonate resin and a method for producing the same. [Background technology]

[0002] Thermoplastic resins, especially polycarbonate resins, are widely used in electrical and electronic equipment, office automation equipment, optical media, automotive parts, building materials, etc. due to their excellent mechanical strength, heat resistance, electrical properties, dimensional stability, flame retardancy, transparency, etc.

[0003] Meanwhile, in recent years, the demand for resins derived from natural products has been increasing due to the movement to reduce the environmental load. As one of the plastic materials derived from natural products, polymers using compounds generated from sugars and carbohydrates as monomers have attracted attention, and research and development is being promoted. For example, Patent Document 1 describes a biodegradable polyester having a structural unit derived from furandicarboxylic acid. Non-Patent Document 1 describes a polycarbonate having a mannitol skeleton. Non-Patent Documents 2 and 3 describe polyesters having a mannitol skeleton, an isosorbide skeleton, and a glucitol skeleton. Non-Patent Document 4 describes a polyester urethane having a glucitol skeleton or an isosorbide skeleton. However, these resins derived from natural products generally do not have a good balance of various physical properties, and there is room for improvement in terms of practical use. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2017-82234 A [Non-patent literature]

[0005] [Non-Patent Document 1] Macromol. Res., 26, 246-253 (2018) [Non-Patent Document 2] Macromolecules, 45,8257-8266 (2012) [Non-Patent Document 3] Designed Monomers and Polymers, 20, 157-166 (2016) [Non-Patent Document 4] Journal of Applied Polymer Science, 114, 3723-3736 (2009) Summary of the Invention [Problem to be solved by the invention]

[0006] There is a demand for thermoplastic resins, particularly polycarbonate resins, which are produced using raw materials derived from natural products and have a well-balanced glass transition temperature and 5% mass loss temperature that are neither too high nor too low for practical use. [Means for solving the problem]

[0007] In view of the above circumstances, the present inventors have conducted extensive research and have found that the above problems can be solved by the present invention.

[0008] <1> The thermoplastic resin contains a structural unit (A) represented by the following formula (1). [ka] <2> The above-mentioned copolymer further contains a structural unit (B) represented by the following general formula (2): <1> The thermoplastic resin is as described in the above. [ka] [In general formula (2), R 1 , R 2 , R 3 , R 4 , R 5 , R 6 , R 7 , and R 8are each independently selected from the group consisting of a hydrogen atom, a fluorine atom, a chlorine atom, a bromine atom, an iodine atom, an alkyl group having 1 to 7 carbon atoms, an aryl group having 6 to 12 carbon atoms, an alkenyl group having 2 to 7 carbon atoms, an alkoxy group having 1 to 7 carbon atoms, and an aralkyl group having 7 to 17 carbon atoms, each of which may have a substituent; X is -O-, -S-, -SO-, -SO 2 represents -, -CO-, a cycloalkylene group having 6 to 12 carbon atoms, or a divalent group represented by the following general formula (3) or the following general formula (4), wherein the cycloalkylene group is optionally substituted by an alkyl group having 1 to 12 carbon atoms and 1 to 3 carbon atoms, Y and Z each independently represent an alkylene group having 1 to 4 carbon atoms; a and b each independently represent an integer of 0 to 10. [ka] (In general formula (3), R 9 and R 10 are each independently selected from the group consisting of a hydrogen atom, a fluorine atom, a chlorine atom, a bromine atom, an iodine atom, an alkyl group having 1 to 20 carbon atoms, an alkoxy group having 1 to 5 carbon atoms, an aryl group having 6 to 12 carbon atoms, an aralkyl group having 7 to 17 carbon atoms, and an alkenyl group having 2 to 15 carbon atoms; R 9 and R 10 wherein the alkyl group, the alkoxy group, the aryl group, the aralkyl group, and the alkenyl group each may have a substituent, R 9 and R 10 may be bonded to each other to form a carbocyclic ring having 3 to 20 carbon atoms or a heterocyclic ring having 1 to 20 carbon atoms, each of which may have a substituent, n represents an integer from 0 to 20. [ka] (In general formula (4), R11 and R 12 are each independently selected from the group consisting of a hydrogen atom, a fluorine atom, a chlorine atom, a bromine atom, an iodine atom, an alkyl group having 1 to 20 carbon atoms, an alkoxy group having 1 to 7 carbon atoms, an aryl group having 6 to 12 carbon atoms, an aralkyl group having 7 to 17 carbon atoms, and an alkenyl group having 2 to 15 carbon atoms, each of which may have a substituent, R 11 and R 12 are bonded together to form the carbon number 7 ~ 24 Carbocyclic ring or carbon number 5 ~ 24 The carbocycle and the heterocycle may each have a substituent. <3> The structural unit (B) is represented by the following formula (5): <2> The thermoplastic resin is as described in the above. [ka] <4> The molar ratio (A / B) of the structural unit (A) to the structural unit (B) is 1 / 99 to 99 / 1. <2> or <3> The thermoplastic resin is as described in the above. <5> The above-mentioned compound (A) is composed only of the structural unit (A) represented by the formula (1). <1> The thermoplastic resin is as described in the above. <6> The thermoplastic resin is a polycarbonate resin or a polyester carbonate resin. <1> ~ <5> The thermoplastic resin according to any one of claims 1 to 5, <7> The polycarbonate resin has a weight average molecular weight (Mw) in terms of polystyrene of 1,000 to 100,000. <6> The thermoplastic resin is as described in the above. <8> The glass transition temperature (Tg) of the polycarbonate resin is 90 to 200° C. <6> or <7> The thermoplastic resin is as described in the above. <9> The polycarbonate resin has a 5% mass loss thermal decomposition temperature of 200 to 500° C. <6> ~ <8> The thermoplastic resin according to any one of claims 1 to 5, <10> The polycarbonate resin has an OH terminal content of 10 to 200,000 ppm. <6> ~ <9> The thermoplastic resin according to any one of claims 1 to 5, <11> The polycarbonate resin has a Ph terminal of 1 to 10 mol %. <6> ~ <10> The thermoplastic resin according to any one of claims 1 to 5, <12> A method for producing a thermoplastic resin containing a structural unit (A) represented by the following formula (1), comprising a step of carrying out a reaction at a molar ratio of a carbonic acid diester to a diol compound (total of a carbonic acid diester / diol compound) of 0.97 to 1.20: [ka] Effect of the Invention

[0009] According to the present invention, it is possible to provide a thermoplastic resin, particularly a polycarbonate resin, which is produced using raw materials derived from natural products and has a glass transition temperature and a 5% mass loss temperature that are neither extremely high nor too low and are well-balanced for practical use. A preferred embodiment of the polycarbonate resin has superior heat resistance (e.g., high glass transition temperature (Tg) and / or thermal decomposition temperature (5% mass loss temperature)) compared to conventional sugar-derived polycarbonate resins, and can be used in a variety of applications such as housings for electronic devices and automobiles, and interior and exterior materials. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] The present invention will be described in detail below with reference to embodiments and examples. However, the present invention is not limited to the embodiments and examples shown below, and can be modified and implemented as desired without departing from the gist of the present invention.

[0011] <Thermoplastic resin> A thermoplastic resin according to one embodiment of the present invention contains a structural unit (A) represented by the following formula (1). [ka]

[0012] The thermoplastic resin of the present invention can be produced by using methyl-β-D-3,4-dideoxy-galactopyranoside (MDG) represented by the following structural formula as a diol monomer raw material. The MDG used in the present invention may be a synthesized product or a commercially available product. [ka] In the present invention, by providing a thermoplastic resin having a structure such as the above-mentioned structural unit (A), it is believed that the heat resistance (high glass transition temperature (Tg) and / or thermal decomposition temperature (5% mass loss temperature)) is improved due to the presence of a ring structure in the main chain. Moreover, the above-mentioned structural unit (A) can be obtained from a monomer derived from a natural product, and the thermoplastic resin of the present invention is also preferable in terms of reducing the environmental load.

[0013] The thermoplastic resin of the present invention may consist only of the structural unit (A) represented by the above formula (1), or may contain, in addition to the structural unit (A) represented by the above formula (1), a structural unit derived from an aliphatic dihydroxy compound or a structural unit derived from an aromatic dihydroxy compound that is generally used as a structural unit in polycarbonate resins and polyester carbonate resins. Specifically, various aliphatic dihydroxy compounds may be mentioned, including in particular 1,4-cyclohexanedimethanol, tricyclodecane dimethanol, 1,3-adamantanedimethanol, 2,2-bis(4-hydroxycyclohexyl)-propane, 3,9-bis(2-hydroxy-1,1-dimethylethyl)-2,4,8,10-tetraoxaspiro[5.5]undecane, 2-(5-ethyl-5-hydroxymethyl-1,3-dioxan-2-yl)-2-methylpropan-1-ol, isosorbide, 1,3-propanediol, 1,4-butanediol, and 1,6-hexanediol. Examples of aromatic dihydroxy compounds include various compounds, such as 2,2-bis(4-hydroxyphenyl)propane (bisphenol A), bis(4-hydroxyphenyl)methane, 1,1-bis(4-hydroxyphenyl)ethane, 2,2-bis(4-hydroxy-3,5-dimethylphenyl)propane, 4,4'-dihydroxydiphenyl, bis(4-hydroxyphenyl)cycloalkane, bis(4-hydroxyphenyl)oxide, bis(4-hydroxyphenyl)sulfide, bis(4-hydroxyphenyl)sulfone, bis(4-hydroxyphenyl)sulfoxide, bis(4-hydroxyphenyl)ketone, and bisphenoxyethanolfluorene.

[0014] Among these, it is preferable that the thermoplastic resin of the present invention contains a structural unit (B) represented by the following general formula (2) from the viewpoint of heat resistance (high glass transition temperature (Tg)). [ka] In general formula (2), R 1 , R 2 , R 3 , R 4 , R 5 , R 6 , R 7 , and R 8 are each independently selected from the group consisting of a hydrogen atom, a fluorine atom, a chlorine atom, a bromine atom, an iodine atom, an alkyl group having 1 to 7 carbon atoms (preferably having 1 to 5 carbon atoms, more preferably having 1 to 3 carbon atoms, and even more preferably having 1 carbon atom), an aryl group having 6 to 12 carbon atoms (preferably having 6 to 10 carbon atoms, and more preferably having 6 carbon atoms), an alkenyl group having 2 to 7 carbon atoms (preferably having 2 to 5 carbon atoms, more preferably having 2 to 3 carbon atoms, and even more preferably having 2 carbon atoms), an alkoxy group having 1 to 7 carbon atoms (preferably having 1 to 5 carbon atoms, more preferably having 1 to 3 carbon atoms, and even more preferably having 1 carbon atom), and an aralkyl group having 7 to 17 carbon atoms (preferably having 7 to 10 carbon atoms, and more preferably having 7 carbon atoms), and the alkyl group, the aryl group, the alkenyl group, the alkoxy group, and the aralkyl group each may have a substituent. In this specification, examples of the "substituent" in the case of "optionally having a substituent" include "a fluorine atom, a chlorine atom, a bromine atom, an iodine atom, an alkyl group having 1 to 7 carbon atoms, an aryl group having 6 to 12 carbon atoms, an alkenyl group having 2 to 7 carbon atoms, an alkoxy group having 1 to 7 carbon atoms, and an aralkyl group having 7 to 17 carbon atoms" (the same applies hereinafter).

[0015] In the general formula (2), X is -O-, -S-, -SO-, -SO 2 It represents -, -CO-, a cycloalkylene group having 6 to 12 carbon atoms (preferably having 6 to 10 carbon atoms, more preferably having 6 carbon atoms), or a divalent group represented by the following general formula (3) or the following general formula (4), and the cycloalkylene group may be substituted with 1 to 12 alkyl groups having 1 to 3 carbon atoms.

[0016] In formula (2), Y and Z each independently represent an alkylene group having 1 to 4 carbon atoms, and preferably an alkylene group having 2 carbon atoms. The alkylene group may be a straight chain alkylene group or a branched chain alkylene group, for example, a methylene group (-CH 2 -), ethylene group (-CH 2 CH 2 -), ethylidene group (-CH(CH 3 )-), trimethylene group (-CH 2 CH 2 CH 2 -), propylene group (-CH(CH 3 )CH 2 -), propylidene group (-CHCH 2 (CH 3 )-), isopropylidene group (-C(CH 3 ) 2 -), tetramethylene group (-CH 2 CH 2 CH 2 CH 2 -), 1-methyltrimethylene group (-CH(CH 3 )CH 2 CH 2 -), 2-methyltrimethylene group (-CH 2 CH(CH 3 )CH2 -), and butylene group (-C(CH 3 ) 2 CH 2 -) groups.

[0017] In formula (2), a and b each independently represent an integer of 0 to 10, preferably an integer of 0 to 3, and more preferably 0.

[0018] [ka] In general formula (3), R 9 and R 10 are each independently selected from the group consisting of a hydrogen atom, a fluorine atom, a chlorine atom, a bromine atom, an iodine atom, an alkyl group having 1 to 20 carbon atoms (preferably having 1 to 10 carbon atoms, more preferably having 1 to 5 carbon atoms, and even more preferably having 1 to 3 carbon atoms), an alkoxy group having 1 to 5 carbon atoms (preferably having 1 to 3 carbon atoms, and more preferably having 1 carbon atom), an aryl group having 6 to 12 carbon atoms (preferably having 6 to 10 carbon atoms, and more preferably having 6 carbon atoms), an aralkyl group having 7 to 17 carbon atoms (preferably having 7 to 10 carbon atoms, and more preferably having 7 carbon atoms), and an alkenyl group having 2 to 15 carbon atoms (preferably having 2 to 10 carbon atoms, more preferably having 2 to 5 carbon atoms, and even more preferably having 2 to 3 carbon atoms), R 9 and R 10 wherein the alkyl group, the alkoxy group, the aryl group, the aralkyl group, and the alkenyl group each may have a substituent, R 9 and R 10 may be bonded to each other to form a carbocyclic ring having 3 to 20 carbon atoms (preferably having 3 to 10 carbon atoms, more preferably having 3 to 5 carbon atoms) or a heterocyclic ring having 1 to 20 carbon atoms (preferably having 1 to 10 carbon atoms, more preferably having 1 to 5 carbon atoms), each of which may have a substituent, n represents an integer of 0 to 20, preferably an integer of 0 to 10, and more preferably an integer of 0 to 3. [ka] In general formula (4), R 11 and R 12 are each independently selected from the group consisting of a hydrogen atom, a fluorine atom, a chlorine atom, a bromine atom, an iodine atom, an alkyl group having 1 to 20 carbon atoms (preferably having 1 to 10 carbon atoms, more preferably having 1 to 5 carbon atoms, and even more preferably having 1 to 3 carbon atoms), an alkoxy group having 1 to 7 carbon atoms (preferably having 1 to 5 carbon atoms, more preferably having 1 to 3 carbon atoms, and even more preferably having 1 carbon atom), an aryl group having 6 to 12 carbon atoms (preferably having 6 to 10 carbon atoms, and more preferably having 6 carbon atoms), an aralkyl group having 7 to 17 carbon atoms (preferably having 7 to 10 carbon atoms, and more preferably having 7 carbon atoms), and an alkenyl group having 2 to 15 carbon atoms (preferably having 2 to 10 carbon atoms, more preferably having 2 to 5 carbon atoms, and even more preferably having 2 to 3 carbon atoms), and each of the alkyl group, the alkoxy group, the aryl group, the aralkyl group, and the alkenyl group may have a substituent, R 11 and R 12 are bonded together to form the carbon number 7 ~ 24 (Preferably the number of carbon atoms 7 ~ 14 , more preferably the number of carbon atoms 7 ~ 9 ) carbocyclic ring or carbon number 5 ~ 24 (Preferably the number of carbon atoms 5 ~ 14 , more preferably the number of carbon atoms 5 ~ 9 ) may form a heterocycle, and the carbocycle and the heterocycle may each have a substituent.

[0019] Examples of the structural unit (B) represented by the general formula (2) include 4,4-bis(4-hydroxyphenyl)propane (i.e., bisphenol A; BPA), 2,2-bis(4-hydroxy-3-methylphenyl)propane (i.e., bisphenol C; BPC), 4,4'-biphenyldiol, bis(4-hydroxyphenyl)methane, bis(2-hydroxyphenyl)methane, 2,4'-dihydroxydiphenylmethane, bis(4-hydroxyphenyl)ether, bis(4-hydroxyphenyl)sulfone ...bis(4-hydroxyphenyl)sulfone, bis(4 Diphenyl sulfone, bis(2-hydroxyphenyl) sulfone, bis(4-hydroxy-3-methylphenyl) sulfone, bis(4-hydroxyphenyl) sulfoxide, bis(4-hydroxyphenyl) sulfide, bis(4-hydroxyphenyl) ketone, 1,1-bis(4-hydroxyphenyl)ethane, 1,1-bis(4-hydroxyphenyl)-1-phenylethane, bis(4-hydroxyphenyl)diphenylmethane, 2,2-bis(4-hydroxyphenyl)propane, 1,1-bis(4-hydroxy-3-methylphenyl)ethane , bis(4-hydroxy-3-methylphenyl)methane, 2,2-bis(4-hydroxy-3-t-butylphenyl)propane, 2,2-bis(4-hydroxyphenyl)butane, 1,1-bis(4-hydroxyphenyl)cyclohexane, 1,1-bis(4-hydroxy-3-methylphenyl)cyclohexane, 1,1-bis(4-hydroxyphenyl)cycloundecane, 1,1-bis(4-hydroxyphenyl)cyclododecane, 2,2-bis(4-hydroxy-3-allylphenyl)propane, 2,2-bis(4-hydroxyphenyl) Butane, 1,1-bis(4-hydroxyphenyl)-2-ethylhexane, 1,1-bis(4-hydroxyphenyl)-2-methylpropane, 2,2-bis(4-hydroxyphenyl)-4-methylpentane, 1,1-bis(4-hydroxyphenyl)decane, 1,3-bis(4-hydroxyphenyl)-5,7-dimethyladamantane, 2,2-bis(4-(2-hydroxyethoxy)phenyl)propane, 4,4-bis(2-hydroxyethoxy)biphenyl, 2,2'-(1,4-phenylene)bis(ethan-1-ol), 2,2'-(1,4-phenylene)bis(methane-1-ol), 2,2'-(1,4-phenylenebis(oxy))bis(ethan-1-ol), 1,1-bis(4-hydroxyphenyl)cyclododecane, 1,1-bis(4-hydroxy-3-methylphenyl)cyclododecane, 1,1-bis(4-hydroxy-3-phenylphenyl)cyclododecane, 1,1-bis(4-hydroxy-3-t-butylphenyl)cyclododecane, 1,1-bis(4-hydroxy-3-sec-butylphenyl)cyclododecane, 1,1-bis(4-hydroxy-3-allylphenyl)cyclododecane, 1,1-bis(4-hydroxy-3,5-dimethylphenyl)cyclododecane, 1,1-bis(4-hydroxy-3-fluorophenyl)cyclododecane, 1,1-bis(4-hydroxy-3-chlorophenyl)cyclododecane Examples of structural units derived from fluorene, 1-bis(4-hydroxy-3-bromophenyl)cyclododecane, 7-ethyl-1,1-bis(4-hydroxyphenyl)cyclododecane, 3,6-dimethyl-1,1-bis(4-hydroxyphenyl)cyclododecane, 9,9-bis(4-(2-hydroxyethoxy)phenyl)fluorene, 9,9-bis(4-(2-hydroxyethoxy)-3-methylphenyl)fluorene, 9,9-bis(4-(2-hydroxyethoxy)-3-tert-butylphenyl)fluorene, 9,9-bis(4-(2-hydroxyethoxy)-3-isopropylphenyl)fluorene, 9,9-bis(4-(2-hydroxyethoxy)-3-cyclohexylphenyl)fluorene, 9,9-bis(4-(2-hydroxyethoxy)-3-phenylphenyl)fluorene, etc., are given. Among them, structural units derived from 4,4-bis(4-hydroxyphenyl)propane (BPA), 2,2-bis(4-hydroxy-3-methylphenyl)propane (BPC), 1,1-bis(4-hydroxyphenyl)cyclohexane, and 1,1-bis(4-hydroxyphenyl)ethane are preferred, and structural units derived from 4,4-bis(4-hydroxyphenyl)propane (BPA) and 2,2-bis(4-hydroxy-3-methylphenyl)propane (BPC) are more preferred. In particular, the following structural unit derived from 4,4-bis(4-hydroxyphenyl)propane (BPA) is particularly preferred because it is versatile, easy to obtain at a low price as a good monomer that is not contaminated with impurities such as metals, and has excellent heat resistance. [ka]

[0020] In the thermoplastic resin according to one embodiment of the present invention, the structural unit (B) may be used either individually or in combination of two or more. When the thermoplastic resin of the present invention contains the structural unit (B), the molar ratio (A / B) of the structural unit (A) to the structural unit (B) is preferably 1 / 99 to 99 / 1, more preferably 1 / 99 to 50 / 50, and particularly preferably 10 / 90 to 40 / 60. In addition to the structural unit (B), the thermoplastic resin of one embodiment of the present invention can also contain structural units derived from an aliphatic dihydroxy compound or a structural unit derived from an aromatic dihydroxy compound, which are generally used as structural units in polycarbonate resins and polyester carbonate resins, as described above. When the thermoplastic resin of the present invention is a copolymer containing two or more types of constitutional units, the copolymer may have any of a random, block and alternating copolymer structure.

[0021] <Physical properties of polycarbonate resin> The thermoplastic resin in one embodiment of the present invention is preferably a polycarbonate resin or a polyester carbonate resin, and more preferably a polycarbonate resin. The weight average molecular weight (Mw) of the polycarbonate resin is not particularly limited, but from the viewpoint of moldability, it is preferably from 1,000 to 100,000, more preferably from 5,000 to 50,000, and particularly preferably from 10,000 to 30,000.

[0022] The molecular weight distribution (Mw / Mn) of the polycarbonate resin is preferably 5.0 or less, more preferably 3.5 or less, further preferably 3.0 or less, and particularly preferably 2.5 or less. In this specification, the weight average molecular weight (Mw) and number average molecular weight (Mn) are values ​​measured by gel permeation chromatography (GPC) in terms of standard polystyrene, specifically, values ​​measured by the method described in the Examples. The molecular weight distribution means the ratio of the weight average molecular weight (Mw) to the number average molecular weight (Mn) [Mw / Mn].

[0023] The glass transition temperature (Tg) of the polycarbonate resin is preferably from 80 to 250°C, more preferably from 90 to 200°C, and particularly preferably from 90 to 125°C. In this specification, the glass transition temperature (Tg) is a value measured using a differential scanning calorimeter (DSC), specifically, it means a value measured by the method described in the examples.

[0024] In the polycarbonate resin, the thermal decomposition temperature at which a 5% mass loss occurs (5% mass loss temperature) is preferably 200 to 500° C., more preferably 250 to 370° C., and particularly preferably 300 to 340° C. In this specification, the thermal decomposition temperature at which a 5% mass loss occurs (5% mass loss temperature) is a value measured using a thermogravimetric / differential thermal analyzer (TG / TDA), and specifically means a value measured by the method described in the examples.

[0025] The OH terminal of the polycarbonate resin is preferably 10 to 200,000 ppm, more preferably 100 to 150,000 ppm, further preferably 1,000 to 10,000 ppm, and particularly preferably 2,000 to 6,000 ppm. In this specification, the hydroxyl (OH) terminal is a value measured using a nuclear magnetic resonance (NMR) apparatus, specifically, a value measured by the method described in the examples.

[0026] The Ph terminal content of the polycarbonate resin is preferably 1 to 10 mol%, more preferably 2 to 7 mol%, and particularly preferably 3 to 6 mol%. In this specification, the phenyl (Ph) terminal content is a value measured using a nuclear magnetic resonance (NMR) spectrometer, specifically, a value measured by the method described in the Examples.

[0027] <Production method of polycarbonate resin> Another embodiment of the present invention is a method for producing a thermoplastic resin (preferably a polycarbonate resin or polyester carbonate resin, more preferably a polycarbonate resin) containing a structural unit (A) represented by the following formula (1), which includes a step of carrying out a reaction at a molar ratio of a carbonic acid diester to a diol compound (total of a carbonic acid diester / diol compound) of 0.97 to 1.20. A more preferred polycarbonate resin will be specifically described below as an example. [ka]

[0028] The method for producing the polycarbonate resin is not particularly limited, but is preferably a method having a step of carrying out an ester exchange reaction, in which the above-mentioned polycarbonate resin is obtained by carrying out an ester exchange reaction between a diol component, which is a raw material monomer, and a carbonate diester. As the diol component, which is a raw material monomer, at least methyl-β-D-3,4-dideoxy-galactopyranoside (MDG) represented by the following structural formula is used. [ka]

[0029] Examples of the carbonic acid diester include diphenyl carbonate (DPC), ditolyl carbonate, bis(chlorophenyl) carbonate, m-cresyl carbonate, dimethyl carbonate, diethyl carbonate, dibutyl carbonate, and dicyclohexyl carbonate. Among these, from the viewpoint of reducing by-product alcohol compounds described later, diaryl carbonate compounds (e.g., diphenyl carbonate, ditolyl carbonate, bis(chlorophenyl) carbonate, and m-cresyl carbonate) are preferred, and from the viewpoint of reactivity and purity, diphenyl carbonate is more preferred. When a dialkyl carbonate is used as the carbonic acid diester, the amount of by-product alkyl alcohol compounds remaining tends to be high. These carbonic acid diesters may be used alone or in combination of two or more kinds.

[0030] The molar ratio of the carbonic acid diester to the diol compound in total (carbonic acid diester / total of diol compounds) is from 0.97 to 1.20, preferably from 1.00 to 1.10, and more preferably from 1.00 to 1.05.

[0031] In the transesterification reaction, it is preferable to use a transesterification catalyst. Examples of the transesterification catalyst include organic acid salts, carbonates, oxides, hydroxides, hydrides, and alkoxides of metals selected from alkali metals and alkaline earth metals, as well as zinc acetate, zinc benzoate, zinc 2-ethylhexanoate, tin chloride (II), tin chloride (IV), tin acetate (II), tin acetate (IV), dibutyltin dilaurate, dibutyltin oxide, dibutyltin dimethoxide, zirconium acetylacetonate, zirconium oxyacetate, zirconium tetrabutoxide, lead acetate (II), lead acetate (IV), zirconium acetate, titanium tetrabutoxide, and cesium carbonate. Of these, cesium carbonate is preferably used. These transesterification catalysts may be used alone or in combination of two or more kinds.

[0032] The amount of the transesterification catalyst used is preferably 1×10 -9 ~1×10 -3 mole, more preferably 1×10 -7 ~1×10 -4 It is a mole.

[0033] Specific reaction conditions for the ester exchange reaction are preferably a reaction temperature of 120 to 260° C. (preferably 180 to 260° C.) and a reaction time of 0.1 to 5 hours (preferably 0.5 to 3 hours). Next, while increasing the degree of vacuum of the reaction system, the reaction temperature is increased to react the diol compound with other monomers, and it is preferable to carry out the polycondensation reaction at a temperature of 180 to 280°C for 0.05 to 2 hours under a final reduced pressure (final reduced pressure) of 300 kPa or less (more preferably 100 kPa or less, and even more preferably 10 kPa or less). Furthermore, from the viewpoint of reducing alcohol-based compounds such as phenol-based compounds described later, it is particularly preferable to finally carry out the polycondensation reaction at a temperature of 200 to 280°C under a reduced pressure of 1 kPa or less (final reduced pressure) for 0.05 to 2 hours. In one embodiment, the transesterification reaction is carried out under reduced pressure of 1 kPa or less (final reduced pressure) and at a temperature of 200° C. or more (preferably 180 to 280° C.).

[0034] The transesterification reaction may be carried out in a continuous manner or in a batch manner. The reaction apparatus used in carrying out the above reaction may be a vertical type equipped with an anchor-type impeller, a Max Blend impeller, a helical ribbon-type impeller, or the like, or may be a horizontal type equipped with a paddle impeller, a lattice impeller, a spectacle impeller, or the like, or an extruder type equipped with a screw. In addition, it is preferable to use a reaction apparatus in which these types are appropriately combined in consideration of the viscosity of the polymer.

[0035] In the method for producing a polycarbonate resin according to one embodiment of the present invention, the catalyst may be removed or deactivated after completion of the polymerization reaction, from the viewpoint of maintaining thermal stability and hydrolytic stability. In addition, after the catalyst is deactivated, in order to remove low boiling point compounds in the resin, a step of volatilization and removal may be provided at a pressure of 1.33 to 133 Pa and a temperature of 200 to 350° C. In this step, a horizontal device equipped with stirring blades with excellent surface renewal ability, such as paddle blades, lattice blades, and spectacle blades, or a thin film evaporator is preferably used.

[0036] Since it is desirable that the resin thus obtained contains as little foreign matter as possible, the molten raw material and the catalyst liquid may be filtered. The mesh of the filter used for filtration is preferably 5 μm or less, more preferably 1 μm or less.

[0037] The polycarbonate resin obtained in this step may be in the form of pellets or flakes and adjusted to a polycarbonate resin composition. In addition, if necessary, the polycarbonate resin may be isolated based on a known method, and then the polycarbonate resin composition may be made into pellets by, for example, a known strand-type cold cut method (a method in which a polycarbonate resin composition that has been melted once is molded into a strand shape, cooled, and then cut into a predetermined shape to form pellets), an air hot cut method (a method in which a polycarbonate resin composition that has been melted once is cut into pellets in the air without coming into contact with water), or an underwater hot cut method (a method in which a polycarbonate resin composition that has been melted once is cut in water and simultaneously cooled to form pellets). The obtained pellets of the polycarbonate resin composition are preferably dried using a hot air drying oven, a vacuum drying oven, or a dehumidifying drying oven, as necessary.

[0038] The polycarbonate resin thus obtained may contain impurities such as alcohol compounds, such as phenolic compounds, which may be produced as by-products during production, and diol components or carbonate diesters that remain unreacted. Impurities such as alcohol compounds such as phenol compounds and carbonic acid diesters can cause a decrease in strength and odor when molded into a molded article, so it is preferable that the content of these compounds is as small as possible.

[0039] The content of the remaining phenolic compounds is preferably 3000 ppm by mass or less, more preferably 1000 ppm by mass or less, and particularly preferably 300 ppm by mass or less, based on 100% by mass of the polycarbonate resin. The content of the remaining diol component is preferably 1000 ppm by mass or less, more preferably 100 ppm by mass or less, and particularly preferably 10 ppm by mass or less, based on 100% by mass of the polycarbonate resin. The content of the remaining carbonate diester is preferably 1000 ppm by mass or less, more preferably 100 ppm by mass or less, and particularly preferably 10 ppm by mass or less, based on 100% by mass of the polycarbonate resin. In particular, it is preferable that the content of compounds such as phenol and t-butylphenol is small, and it is preferable that the content of these compounds is within the above range.

[0040] The content of the phenolic compound remaining in the polycarbonate resin can be measured by a method in which the phenolic compound extracted from the polycarbonate resin is analyzed by gas chromatography. The content of the alcohol-based compound remaining in the polycarbonate resin can also be measured by a method in which the alcohol-based compound extracted from the polycarbonate resin is analyzed by gas chromatography. The contents of the diol component and the carbonate diester remaining in the polycarbonate resin can also be measured by a method in which these compounds are extracted from the polycarbonate resin and analyzed by gas chromatography.

[0041] The contents of by-produced alcohol compounds such as phenol compounds, diol components and carbonic acid diesters may be reduced to an undetectable level, but from the viewpoint of productivity, they may be contained in small amounts within a range that does not impair the effect. Also, small amounts can improve the plasticity of the resin when it is melted.

[0042] The content of each of the remaining phenolic compounds, diol components, or carbonate diesters may be, for example, 0.01 ppm by mass or more, 0.1 ppm by mass or more, or 1 ppm by mass or more, relative to 100% by mass of the polycarbonate resin. The content of the remaining alcohol-based compound may be, for example, 0.01 ppm by mass or more, 0.1 ppm by mass or more, or 1 ppm by mass or more relative to 100% by mass of the polycarbonate resin.

[0043] The contents of by-produced alcohol compounds such as phenolic compounds, diol components and carbonate diesters in the polycarbonate resin can be adjusted to fall within the above ranges by appropriately adjusting the polycondensation conditions and the settings of the apparatus, and can also be adjusted by the conditions of the extrusion step after polycondensation.

[0044] For example, the remaining amount of by-produced alcohol-based compounds such as phenol-based compounds is related to the type of carbonate diester used in the polymerization of the polycarbonate resin, the polymerization reaction temperature, the polymerization pressure, etc. By adjusting these factors, the remaining amount of by-produced alcohol-based compounds such as phenol-based compounds can be reduced.

[0045] For example, when a polycarbonate resin is produced using a dialkyl carbonate such as diethyl carbonate, the molecular weight is difficult to increase, resulting in a low molecular weight polycarbonate, and the content of by-produced alkyl alcohol compounds tends to be high. Such alkyl alcohols are highly volatile, and if they remain in the polycarbonate resin, the moldability of the resin tends to deteriorate. In addition, if the amount of by-produced alcohol compounds such as phenolic compounds remaining is large, there is a possibility that odor problems will occur during molding of the resin, and that the cleavage reaction of the resin skeleton will proceed during compounding, resulting in a decrease in molecular weight. Therefore, it is preferable that the content of the by-produced alcohol compounds remaining in the obtained polycarbonate resin is 3000 mass ppm or less relative to the polycarbonate resin (100 mass%). The content of the remaining alcohol compounds is preferably 3000 mass ppm or less, more preferably 1000 mass ppm or less, and particularly preferably 300 mass ppm or less relative to 100 mass% of the polycarbonate resin.

[0046] <Polycarbonate resin composition> Another embodiment of the present invention is a polycarbonate resin composition (hereinafter, also simply referred to as a "resin composition") containing the polycarbonate resin of the above-mentioned embodiment. In the resin composition, the content of the polycarbonate resin of the above-mentioned embodiment is usually 30 to 100 mass%, preferably 50 to 100 mass%, more preferably 60 to 100 mass%, even more preferably 70 to 100 mass%, and particularly preferably 80 to 100 mass%, relative to the total amount (100 mass%) of the resin composition.

[0047] The resin composition may contain a resin other than the polycarbonate resin of the above-mentioned embodiment. The other resin may or may not contain the structural unit (A) represented by the above-mentioned formula (1). Examples of such other resins include thermoplastic polyester resins such as polycarbonate resins other than the polycarbonate resins of the above-mentioned embodiments, polyester carbonate resins, polyethylene terephthalate resins (PET resins), polytrimethylene terephthalate resins (PTT resins), and polybutylene terephthalate resins (PBT resins); styrene-based resins such as polystyrene resins (PS resins), high-impact polystyrene resins (HIPS), acrylonitrile-styrene copolymers (AS resins), and methyl methacrylate-styrene copolymers (MS resins); and methyl methacrylate-acrylic rubber-styrene copolymers (MS resins). Examples of elastomers include core / shell elastomers such as polyolefin copolymers (MAS), polyester-based elastomers, and other elastomers; polyolefin resins such as cyclic cycloolefin resins (COP resins) and cyclic cycloolefin (COP) copolymer resins; polyamide resins (PA resins); polyimide resins (PI resins); polyetherimide resins (PEI resins); polyurethane resins (PU resins); polyphenylene ether resins (PPE resins); polyphenylene sulfide resins (PPS resins); polysulfone resins (PSU resins); polymethacrylate resins (PMMA resins); and polycaprolactones. These other resins may be contained alone or in combination of two or more kinds.

[0048] In the resin composition, the content of these other resins is not particularly limited as long as it is within a range that does not impair the effects of the present invention, but for example, it is preferably 0 to 50 parts by mass, more preferably 0 to 20 parts by mass, even more preferably 0 to 10 parts by mass, and particularly preferably 0 to 1 part by mass, relative to 100 parts by mass of the total amount of the polycarbonate resin of the present invention contained in the resin composition.

[0049] The resin composition may contain various additives within the range not impairing the effects of the present invention. Such various additives are appropriately selected depending on the application. For example, it is preferable to contain a heat stabilizer, an antioxidant, a flame retardant, a flame retardant assistant, an ultraviolet absorber, a release agent, a colorant, etc., and further, if necessary, an antistatic agent, a fluorescent brightener, an antifogging agent, a flow improver, a plasticizer, a dispersant, an antibacterial agent, etc. may be contained.

[0050] <Molded body> Yet another embodiment of the present invention relates to a molded article obtained by molding the polycarbonate resin composition. The molding method is not particularly limited, and may be any method such as injection molding, high-speed injection molding, injection compression molding, two-color molding, gas-assisted or other hollow molding, molding using a heat-insulating mold, molding using a rapidly heated mold, foam molding (including supercritical fluid), insert molding, IMC (in-mold coating molding) molding, extrusion molding, sheet molding, thermoforming, rotational molding, lamination molding, press molding, compression molding, extrusion molding, solution casting, etc. A molding method using a hot runner system may also be used.

[0051] The shape, pattern, color, size, etc. of the molded product can be appropriately selected depending on the application of the molded product. If necessary, the resin or molded product may be subjected to surface treatment such as hard coating or anti-reflection.

[0052] The molded articles can be, for example, electrical and electronic equipment, OA (Office Automation) equipment, information terminal equipment, machine parts, home appliances, vehicle parts, building materials, various containers, leisure goods and miscellaneous goods, parts for lighting equipment, parts for various household electrical appliances, housings, containers, covers, storage parts, cases for electrical appliances, covers and cases for lighting appliances, etc. Examples of electrical and electronic equipment include personal computers, game consoles, television receivers, display devices such as liquid crystal displays and plasma display devices, printers, copy machines, scanners, fax machines, electronic organizers and personal digital assistants (PDAs), electronic desk calculators, electronic dictionaries, cameras, video cameras, mobile phones, battery packs, drives and readers for recording media, mice, numeric keypads, various music players, portable radios and audio players, etc. Further examples of the molded article include electric signboards, liquid crystal backlights, lighting displays, traffic signs, signboards, screens, reflectors, meter parts and other automobile parts, toys, ornaments, and the like. Among others, the molded article has excellent heat resistance and can be preferably used as housings and interior and exterior materials for electronic devices, automobiles, and the like. EXAMPLES

[0053] The present invention will be described in more detail below with reference to examples. However, the present invention is not limited to the following examples, and can be practiced with any modifications within the scope of the present invention. In this specification, "room temperature" generally refers to about 10°C to about 35°C. The physical properties of the resins obtained in the Examples, Comparative Examples and Reference Examples were measured according to the procedures described below.

[0054] <Evaluation> 1. Weight average molecular weight (Mw), number average molecular weight (Mn), molecular weight distribution (Mw / Mn) A calibration curve was created using gel permeation chromatography (GPC) with chloroform as the developing solvent and standard polystyrene (PStQuick MP-M, Tosoh Corporation) with a known molecular weight (molecular weight distribution = 1). The elution time and molecular weight value of each peak from the measured standard polystyrene were plotted, and a cubic approximation was performed to create a calibration curve. [Measurement conditions] Equipment: Tosoh Corporation, HLC-8320GPC Column: Guard column: TSKguardcolumn SuperMPHZ-M x 1 Analytical column: TSKgel SuperMultiporeHZ-M x 3 Solvent: HPLC grade chloroform ·Injection volume; 10μL Sample concentration: 0.2w / v% HPLC grade chloroform solution Solvent flow rate: 0.35ml / min ·Measurement temperature: 40℃ Detector: RI Based on the obtained calibration curve, the weight average molecular weight (Mw) and number average molecular weight (Mn) were calculated as polystyrene equivalent values ​​according to the following formula: The molecular weight distribution (Mw / Mn) was calculated from the polystyrene equivalent weight average molecular weight (Mw) and polystyrene equivalent number average molecular weight (Mn) according to the following formula: [Calculation formula] Mw = Σ(Wi × Mi) ÷ Σ(Wi) Mn = Σ(Ni × Mi) ÷ Σ(Ni) Molecular weight distribution=Mw / Mn (In the above formula, i represents the i-th division point when dividing the molecular weight M, Wi represents the i-th weight, Ni represents the i-th number of molecules, and Mi represents the i-th molecular weight. The molecular weight M represents the polystyrene molecular weight value at the same elution time on the calibration curve.)

[0055] 2. Glass transition temperature (Tg) The glass transition temperature (Tg) was measured by a differential scanning calorimeter (DSC) (DSC-7000, manufactured by Hitachi High-Tech Science). The measurement sample was prepared by weighing a 7-12 mg test piece into an RDC aluminum pan (sample container for AI autosampler, φ6.8 H2.5 mm) and sealing it with the cover for the AI ​​autosampler. The measurements were performed under a nitrogen atmosphere (nitrogen flow rate: 50 ml / min). 10.0 mg of sapphire was used as a standard substance in the reference cell. The sample temperature was adjusted to 30°C, and the temperature was increased to 220°C at 10°C / min. After that, the temperature was decreased to 30°C by cooling at 10°C / min. After that, the temperature was increased to 270°C at 10°C / min and the measurement was performed.

[0056] 3.Pyrolysis temperature (5% mass loss temperature) The thermal decomposition temperature (5% mass loss temperature) was measured using a thermogravimetric and differential thermal analyzer (TG / DTA) (Hitachi High-Tech Science, TGDTA7300). The measurement sample was prepared by weighing a 2 mg test piece into a platinum pan (Pt open-type sample container, φ5.2, H2.5 mm). The measurements were performed under a nitrogen atmosphere (nitrogen flow rate: 250 ml / min). 0.00519 g of α-alumina was used as a reference material in the reference cell. The sample temperature was adjusted to 30°C, and the temperature was increased to 550°C at 10°C / min for measurement.

[0057] 4. Hydroxyl group (OH) terminal [ppm] The hydroxyl (OH) terminals of the resulting resin were measured by nuclear magnetic resonance (NMR) spectroscopy. 0.05 g of the resin sample was dissolved in 1 ml of deuterated chloroform (containing 0.05 w / v% TMS) and incubated at 23°C. 1 It was determined by measuring H-NMR. Specifically, it was calculated from the integral ratio of the peak derived from the hydroxyl group to the peak derived from other resin skeletons. Equipment: BRUKER 500MHz nuclear magnetic resonance AVANCE III HD

[0058] 5. Phenyl (Ph) end [mol%] The phenyl (Ph) terminals of the obtained resin were measured by a nuclear magnetic resonance (NMR) spectrometer. 0.05 g of the resin sample was dissolved in 1 ml of deuterated chloroform (containing 0.05 w / v% TMS) and incubated at 23°C. 1 It was determined by measuring H-NMR. Specifically, it was calculated from the integral ratio of the peak derived from the phenyl group to the peak derived from other resin skeletons. Equipment: BRUKER 500MHz nuclear magnetic resonance AVANCE III HD

[0059] (Synthesis Example 1) The methyl-β-D-3,4-dideoxy-galactopyranoside used in the examples was synthesized as follows: x -Pd / CeO 2 It was synthesized by deoxygenation, dehydration and hydrogenation of methyl-β-D-galactopyranoside over the catalyst. <ReO x -Pd / CeO 2 Catalyst preparation (continuous impregnation method) 1. First, the CEO 2(Solvay SpecialChem Japan Co., Ltd., BET surface area 155.3 m 2 g -1 , calcined at 600 °C for 3 h) with NH 4 ReO 4 (Mitsuwa Chemical Co., Ltd.) aqueous solution, and x / CeO 2 A catalyst was prepared. The amount of Re added was 2 wt%. 2. ReO after drying at 110℃ for 12 hours x / CeO 2 Pd(NO 3 ) 2 (NE Chemcat Corp.) aqueous solution, and x -Pd / CeO 2 The catalyst was prepared with a Pd / Re molar ratio of 0.25. 3. After evaporating the solvent and drying at 110°C for 12 hours, the catalyst was calcined in air at 500°C for 3 hours. <Reaction procedure> 1. Methyl-β-D-galactopyranoside, ReO x -Pd / CeO 2 The catalyst, solvent and stir bar were placed in a glass cylinder. 2. The glass cylinder was placed in a stainless steel autoclave, which was then sealed thoroughly. 3. 1MPa H 2 The autoclave was flushed with 0.45 mL of ethyl alcohol three or more times to purge the air from within the autoclave, and the hydrogen pressure was then increased to 0.9 MPa. 4. The autoclave was heated to 160°C and monitored using a thermocouple inserted in the autoclave. When the temperature reached 160°C (which took about 30 minutes), the time was defined as 0 hours and the hydrogen pressure was maintained at 0.9 MPa and the stirring speed at 500 rpm. 5. After 72 hours, the autoclave reactor was removed from the heater and cooled to room temperature in a water bath. 6. The autoclave contents were transferred to vials under nitrogen atmosphere in a glove box. The washing (collection) solvent was methanol and the catalyst was isolated by filtration. 7. Both gaseous and liquid products were analyzed by FID-GC (Shimadzu GC-2014) equipped with a TC-WAX capillary column (0.25 mm diameter, 30 m), and the liquid products were also analyzed by HPLC (Shimadzu LC-10A, refractive index detector) with an Aminex HPX-87C column (7.8 mm diameter, 300 mm) using water as the eluent. 8. The amounts of substrate and product were calculated using a calibration curve obtained using the substrate and isolated product. 9. The solvent was removed from the obtained liquid product by rotary evaporator at 50°C, and then the product was transferred from the flask to a 5 ml glass vial. The yield of MDG obtained was calculated from the vial increment and analyzed by GC and 1 H NMR, 13 The product was analyzed by C NMR, HH COSY NMR, HMQC NMR, and HMBC NMR. The purity was 95.3% based on the GC results. Subsequently, 20 g of the crude MDG obtained was dissolved in 20 g of ultrapure water, and 200 g of ethyl acetate was added and mixed. The organic layer was separated from the aqueous layer, and the organic layer was evaporated at 50°C and 8 mmHg, and then further dried at room temperature and 8 mmHg to obtain purified MDG. The purity was 98.8% based on the GC results.

[0060] [ka]

[0061] Example 1 The raw diol monomers were methyl-β-D-3,4-dideoxy-galactopyranoside (MDG) (5.837 g, 35.99 mmol) and bisphenol A (BPA) (19.172 g, 83.982 mmol) prepared in Synthesis Example 1, diphenyl carbonate (DPC) (27.244 g, 127.18 mmol), and cesium carbonate (Cs 2 CO 3 , 3 × 10 for 1 mole of MDG and BPA combined -6The mixture was precisely weighed into a 100 mL four-neck flask and dried under reduced pressure at room temperature for 1 hour under vacuum. After that, the atmosphere was replaced with nitrogen, and the reaction system was placed under a nitrogen atmosphere. The four-neck flask was equipped with a stirrer and a distillation device, and heated to 180° C. under a nitrogen atmosphere (pressure: 101.3 kPa). After confirming complete dissolution of the raw material monomer after heating, the temperature was raised to 210° C. at a rate of 180° C. / h, and stirring was performed for 10 minutes. Thereafter, the pressure in the reactor was reduced to 33 kPa, and stirring was performed for 40 minutes. Thereafter, the temperature was raised to 220° C. at a rate of 60° C. / h, the pressure was reduced to 27 kPa, and stirring was performed for 20 minutes. Thereafter, the temperature was raised to 230° C. at a rate of 60° C. / h, the degree of vacuum was adjusted to 24 kPa, and stirring was performed for 10 minutes. Thereafter, the pressure was reduced to 20 kPa, and stirring was performed for 20 minutes. Thereafter, the temperature was raised to 240° C. at 60° C. / h, and stirring was performed for 10 minutes. Thereafter, the degree of vacuum was adjusted to 13 kPa, and stirring was performed for 20 minutes. Subsequently, the degree of vacuum was adjusted to 7 Pa at 240°C, and stirring was continued for 20 minutes. After the degree of vacuum was adjusted to 1 kPa or less, stirring was continued for another 60 minutes, and the reaction was terminated (final reaction temperature = 240°C). After the reaction was terminated, nitrogen was introduced into the reactor to return to normal pressure, and a polycarbonate resin was obtained. The production conditions are summarized in Table 1 below. In addition, the weight average molecular weight (Mw), number average molecular weight (Mn), molecular weight distribution (Mw / Mn), glass transition temperature (Tg), thermal decomposition temperature (5% mass reduction temperature), OH terminal and Ph terminal of the resin were measured for the obtained resin, and their physical properties are shown in Table 2 below.

[0062] Example 2 A polycarbonate resin was obtained in the same manner as in Example 1, except that the final reaction temperature was 230° C. The production conditions are summarized in Table 1 below. The physical properties of the obtained resin are shown in Table 2 below.

[0063] Example 3 As a catalyst, cesium carbonate (Cs 2 CO 3 , 6 × 10 for 1 mole of MDG and BPA combined -6A polycarbonate resin was obtained in the same manner as in Example 1, except that a 100% alcohol (mol) was used and the final reaction temperature was 220° C. The production conditions are summarized in Table 1 below. The physical properties of the obtained resin are shown in Table 2 below.

[0064] Example 4 The raw diol monomers were MDG (16.787 g, 103.51 mmol) and DPC (23.504 g, 109.72 mmol), and the catalyst was cesium carbonate (Cs 2 CO 3 , 50 × 10 for 1 mole of MDG -6 A polycarbonate resin was obtained in the same manner as in Example 1, except that a polycarbonate copolymer (100%) was used and the final reaction temperature was 230° C. The production conditions are summarized in Table 1 below. The physical properties of the obtained resin are shown in Table 2 below.

[0065] Comparative Example 1 Cyclohexanedimethanol (CHDM) (25.00 g, 173.4 mmol, a mixture of cis and trans isomers) as raw diol monomers, DPC (36.17 g, 168.9 mmol), and sodium bicarbonate (NaHCO 3 , 6×10 for 1 mol of CHDM -6 The mixture was precisely weighed into a 100 mL four-neck flask and dried under reduced pressure at room temperature for 1 hour under vacuum. After that, the atmosphere was replaced with nitrogen three times to place the reaction system under a nitrogen atmosphere. The four-neck flask was equipped with a stirrer and a distillation device, and heated to 180° C. under a nitrogen atmosphere at a pressure of 101.3 kPa. After confirming complete dissolution of the raw material monomer after heating, the pressure in the reactor was reduced to 20 kPa, and stirring was performed for 20 minutes. Then, the temperature was raised to 200° C. at a rate of 60° C. / h, and stirring was performed at 200° C. for 30 minutes. Then, the temperature was raised to 225° C. at 60° C. / h. Then, the degree of vacuum was adjusted to 16 kPa, and stirring was performed for 10 minutes. Then, the temperature was raised to 240° C. at 60° C. / h, and at the same time, the degree of vacuum was adjusted to 12 kPa, and stirring was performed for 10 minutes. Then, the degree of vacuum was adjusted to 8 kPa, and stirring was performed for 10 minutes. Then, the degree of vacuum was adjusted to 5.3 kPa, and stirring was performed for 10 minutes. Then, the degree of vacuum was adjusted to 2.7 kPa, and stirring was performed for 10 minutes. Thereafter, the degree of vacuum was adjusted to 1.3 kPa, and stirring was performed for 10 minutes. Thereafter, the degree of vacuum was adjusted to 1 kPa or less, and stirring was performed for another 60 minutes to terminate the reaction. After the reaction was completed, nitrogen was introduced into the reactor to return to normal pressure, and the polycarbonate resin produced was taken out. The polycarbonate resin obtained was transparent. The production conditions are summarized in Table 1 below. The physical properties of the resin obtained are also shown in Table 2 below.

[0066] Comparative Example 2 The raw material diol monomer was spiroglycol (SPG) (30.61 g, 0.101 mol), DPC (21.97 g, 0.103 mol), and sodium bicarbonate (NaHCO 3 , 6 × 10 for 1 mol of SPG -6 A polycarbonate resin was obtained by the same procedure as in Comparative Example 1 except for the amounts charged, but crystallization occurred simultaneously with the polymerization, and a transparent polymer was not obtained. The production conditions are summarized in Table 1 below.

[0067] (Reference example 1) The raw diol monomers were 2:4-3:5-di-O-methylene-D-mannitol (DMAN-DOM) (7.48 g, 36.28 mmol) and bisphenol A (BPA) (17.52 g, 76.74 mmol), DPC (25.42 g, 118.66 mmol), and cesium carbonate (Cs 2 CO 3 , 2 × 10 for 1 mol of DMAN-DOM and BPA -6 The mixture was precisely weighed into a 100 mL four-neck flask and dried under reduced pressure at room temperature for 1 hour under vacuum. After that, the atmosphere was replaced with nitrogen three times to place the reaction system under a nitrogen atmosphere. The four-neck flask was equipped with a stirrer and a distillation device, and heated to 180° C. under a nitrogen atmosphere (pressure: 101.3 kPa). After confirming complete dissolution of the raw material monomer after heating, the temperature was raised to 200° C. at a rate of 120° C. / h, and the pressure in the reactor was simultaneously reduced to 27 kPa, and stirring was performed for 40 minutes. The temperature was then raised to 210° C. at a rate of 60° C. / h. The degree of reduced pressure was then adjusted to 24 kPa, and stirring was performed for 10 minutes. The temperature was then raised to 220° C. at 60° C. / h. The temperature was then raised to 230° C. at 60° C. / h. The degree of reduced pressure was then adjusted to 20 kPa, and stirring was performed for 10 minutes. The temperature was then raised to 240° C. at 60° C. / h, and the degree of reduced pressure was then adjusted to 14 Pa, and stirring was performed for 10 minutes. Then, the temperature was raised to 250°C at 60°C / h, and the degree of vacuum was adjusted to 7 Pa, and stirring was performed for 10 minutes. Then, the temperature was raised to 260°C at 60°C / h. Then, the temperature was raised to 270°C at 60°C / h. Then, the degree of vacuum was adjusted to 1 kPa or less, and stirring was performed for another 120 minutes to terminate the reaction. After the reaction was completed, nitrogen was introduced into the reactor to return to normal pressure, and a polycarbonate resin was obtained. The production conditions are summarized in Table 1 below. The physical properties of the obtained resin are also shown in Table 2 below.

[0068] [Table 1]

[0069] [Table 2]

[0070] The results in Table 2 show that the glass transition temperature of Comparative Example 1 is too low, and the 5% mass loss temperature of Reference Example 1 is higher than those of Examples 1-4. The structures of the monomer compounds used in the above Examples, Comparative Examples and Reference Examples are as follows: [ka] [Industrial Applicability]

[0071] The thermoplastic resin, particularly the polycarbonate resin, of the present invention is useful as a resin that has heat resistance and can be produced using raw materials derived from natural products.

Claims

1. A thermoplastic resin comprising a structural unit (A) represented by the following formula (1): 【Chemistry 1】

2. The thermoplastic resin according to claim 1, further comprising a structural unit (B) represented by the following general formula (2): 【Chemistry 2】 [In general formula (2), R 1 , R 2 , R 3 , R 4 , R 5 , R 6 , R 7 , and R 8 are each independently selected from the group consisting of a hydrogen atom, a fluorine atom, a chlorine atom, a bromine atom, an iodine atom, an alkyl group having 1 to 7 carbon atoms, an aryl group having 6 to 12 carbon atoms, an alkenyl group having 2 to 7 carbon atoms, an alkoxy group having 1 to 7 carbon atoms, and an aralkyl group having 7 to 17 carbon atoms, each of which optionally has a substituent; X is -O-, -S-, -SO-, -SO 2 represents -, -CO-, a cycloalkylene group having 6 to 12 carbon atoms, or a divalent group represented by the following general formula (3) or the following general formula (4), wherein the cycloalkylene group is optionally substituted with an alkyl group having 1 to 12 carbon atoms and 1 to 3 carbon atoms, Y and Z each independently represent an alkylene group having 1 to 4 carbon atoms; a and b each independently represent an integer of 0 to 10. 【Chemistry 3】 (In general formula (3), R 9 and R 10 are each independently selected from the group consisting of a hydrogen atom, a fluorine atom, a chlorine atom, a bromine atom, an iodine atom, an alkyl group having 1 to 20 carbon atoms, an alkoxy group having 1 to 5 carbon atoms, an aryl group having 6 to 12 carbon atoms, an aralkyl group having 7 to 17 carbon atoms, and an alkenyl group having 2 to 15 carbon atoms; R 9 and R 10 wherein the alkyl group, the alkoxy group, the aryl group, the aralkyl group, and the alkenyl group each may have a substituent, R 9 and R 10 may be bonded to each other to form a carbocyclic ring having 3 to 20 carbon atoms or a heterocyclic ring having 1 to 20 carbon atoms, each of which may have a substituent; n represents an integer of 0 to 20. 【Chemistry 4】 (In general formula (4), R 11 and R 12 are each independently selected from the group consisting of a hydrogen atom, a fluorine atom, a chlorine atom, a bromine atom, an iodine atom, an alkyl group having 1 to 20 carbon atoms, an alkoxy group having 1 to 7 carbon atoms, an aryl group having 6 to 12 carbon atoms, an aralkyl group having 7 to 17 carbon atoms, and an alkenyl group having 2 to 15 carbon atoms, each of which may have a substituent, R 11 and R 12 may be bonded to each other to form a carbocyclic ring having 7 to 24 carbon atoms or a heterocyclic ring having 5 to 24 carbon atoms, and the carbocyclic ring and the heterocyclic ring each may have a substituent.)]

3. The thermoplastic resin according to claim 2, wherein the structural unit (B) is represented by the following formula (5): 【Chemistry 5】

4. The thermoplastic resin according to claim 2 or 3, wherein the molar ratio (A / B) of the structural unit (A) to the structural unit (B) is 1 / 99 to 99 / 1.

5. The thermoplastic resin according to claim 1, which consists solely of the structural unit (A) represented by the formula (1).

6. The thermoplastic resin according to any one of claims 1 to 5, wherein the thermoplastic resin is a polycarbonate resin or a polyester carbonate resin.

7. The thermoplastic resin according to claim 6, wherein the polycarbonate resin has a weight average molecular weight (Mw) in terms of polystyrene of 1,000 to 100,000.

8. The thermoplastic resin according to claim 6 or 7, wherein the glass transition temperature (Tg) of the polycarbonate resin is 90 to 200°C.

9. The thermoplastic resin according to any one of claims 6 to 8, wherein the polycarbonate resin has a 5% mass loss thermal decomposition temperature of 200 to 500 ° C.

10. The thermoplastic resin according to any one of claims 6 to 9, wherein the polycarbonate resin has an OH terminal content of 10 to 200,000 ppm.

11. The thermoplastic resin according to any one of claims 6 to 10, wherein the polycarbonate resin has a Ph terminal of 1 to 10 mol%.

12. A method for producing a thermoplastic resin containing a structural unit (A) represented by the following formula (1), comprising a step of carrying out a reaction at a molar ratio of a carbonic acid diester to a diol compound (total of the carbonic acid diester / the diol compound) of 0.97 to 1.20: 【Chemistry 6】

Citation Information

Patent Citations

  • Polycarbonate and method of manufacturing the same

    JP2010037551A

  • Material for sustained release of physiologically active substance

    JP2011122007A

  • Biodegradable aliphatic-aromatic polyester

    JP2017082234A