Fiber-reinforced resin material, fiber-reinforced resin molded body, and method for producing same
The fiber-reinforced resin material with a difunctional epoxy and polyfunctional phenol compound forms a three-dimensional network structure, addressing handling and property challenges, achieving high heat resistance and mechanical strength comparable to thermosetting resins.
Patent Information
- Application Number
- JP2020102463
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-06-12
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2040-06-12
AI Technical Summary
Conventional fiber-reinforced resin materials using thermosetting epoxy resin as a matrix face challenges in handling, heat resistance, and mechanical properties, particularly when using thermoplastic resins, which lack crosslinked structures and result in inadequate impregnation and mechanical properties inferior to thermosetting resins.
A fiber-reinforced resin material containing a matrix composed of a difunctional epoxy compound and a polyfunctional phenol compound that generates isocyanate groups by thermal dissociation, optionally with a non-nucleophilic base catalyst, forming a three-dimensional network structure through polyaddition and heating, allowing for improved handling and enhanced mechanical and thermal properties.
The material achieves ease of handling, high heat resistance, and superior mechanical properties, with a storage modulus of 10 GPa or more at 200°C, comparable to thermosetting resins, without the need for special storage conditions and with uniform distribution of isocyanate groups.
Smart Images

Figure 0007558506000001
Abstract
Description
[Technical field]
[0001] The present application relates to a fiber-reinforced resin material, a fiber-reinforced resin molded product, and a method for producing the same. [Background technology]
[0002] Fiber-reinforced resin materials using a thermosetting epoxy resin as a matrix have traditionally been used for parts that require high heat resistance and excellent mechanical properties, such as robot parts used in high-temperature environments, rolls used in ovens, printed circuit boards that require solder heat resistance, and heat-resistant rods for tension members of electric wires and cables.
[0003] Fiber-reinforced resin materials using a thermosetting epoxy resin as a matrix are generally produced by impregnating reinforcing fibers with a liquid monomer to form a prepreg in which the matrix and reinforcing fibers are highly integrated, and then molding the prepreg into a molded product of any shape. However, the prepreg must be stored in a cool, dark place, and is not easy to handle.
[0004] On the other hand, fiber-reinforced resin materials using thermoplastic resin as a matrix are also known. The thermoplastic resin obtained by polymerization in a polymerization kettle or the like is melted by heating and impregnated into the reinforcing fibers to obtain a prepreg. Since the fiber-reinforced resin material using thermoplastic resin as a matrix can be melted at any time by heating, it is not difficult to handle like the fiber-reinforced resin material using thermosetting resin as a matrix, but it cannot be applied to parts that require heat resistance. In addition, since the thermoplastic resin does not have a cross-linked structure in the molecular chain, it often has inferior mechanical properties compared to the thermosetting resin whose molecular chain has a three-dimensional network structure. Furthermore, the viscosity of the molten thermoplastic resin is higher than that of the monomer, so the impregnation into the reinforcing fibers is insufficient, making it difficult to integrate them to a high degree, and it is difficult to obtain a molded body with stable high strength without variation.
[0005] To solve these problems, prepregs have been proposed in which a curing agent or a thermoplastic resin is added to an epoxy prepolymer before crosslinking network formation, and the prepregs are thermally cured to form a thermosetting epoxy resin composition (e.g., Patent Documents 1 and 2). However, in the prepregs disclosed in Patent Documents 1 and 2, a considerable amount of additive components are present in the matrix, which tends to sacrifice the high heat resistance and mechanical properties inherent to thermosetting epoxy resins. In addition, these additive components have poor compatibility with epoxy monomers, making it difficult to disperse them uniformly. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] Japanese Patent Publication No. 61-40317 [Patent Document 2] Japanese Patent Application Publication No. 6-9802 Summary of the Invention [Problem to be solved by the invention]
[0007] As described above, in conventional techniques, it is difficult to achieve both easy handling and good heat resistance and mechanical properties after thermosetting in a fiber-reinforced resin material. [Means for solving the problem]
[0008] As one of the means for solving the above problems, the present application discloses the following fiber reinforced resin materials (1) to (3). (1) A fiber-reinforced resin material comprising a matrix and reinforcing fibers, the matrix containing an oligomer obtained by polyaddition of (A) a difunctional epoxy compound and (B) a polyfunctional phenol compound having a structure that generates an isocyanate group upon thermal dissociation in a molecular chain. (2) In the fiber-reinforced resin material, the structure that generates an isocyanate group upon thermal dissociation may be a urea bond. (3) In the fiber-reinforced resin material, the matrix may further contain (C) a non-nucleophilic base as a catalyst.
[0009] As one of the means for solving the above problems, the present application discloses the following fiber-reinforced resin moldings (4) and (5). (4) A fiber-reinforced resin molded product in which the fiber-reinforced resin material of the present disclosure forms a three-dimensional network structure. (5) The fiber-reinforced resin molding may have a storage modulus at 200° C. of 10 GPa or more.
[0010] As one of the means for solving the above problems, the present application discloses the following methods for producing a fiber-reinforced resin material (6) and (7). (6) A method for producing a fiber-reinforced resin material, comprising: impregnating reinforcing fibers with a liquid containing (A) a difunctional epoxy compound and (B) a polyfunctional phenol compound having a structure that thermally dissociates to generate an isocyanate group in a molecular chain; and heating the reinforcing fibers after impregnation to polyaddition-polymerize the (A) difunctional epoxy compound and the (B) polyfunctional phenol compound into an oligomer. (7) In the method for producing a fiber-reinforced resin material, the heating temperature during the polyaddition may be 90° C. or higher and 150° C. or lower.
[0011] As one of the means for solving the above problems, the present application discloses the following methods for producing a fiber-reinforced resin molding as set forth in (8) to (10). (8) A method for producing a fiber-reinforced resin molded product, comprising heating the fiber-reinforced resin material of the present disclosure. (9) In the method for producing a fiber-reinforced resin molding, the heating temperature may be 150° C. or higher. (10) In the method for producing a fiber-reinforced resin molding, a pressure of 15 MPa or more may be applied simultaneously with the heating. Effect of the Invention
[0012] The fiber-reinforced resin material of the present disclosure does not need to be stored in a cool, dark place, and is easier to handle than conventional fiber-reinforced thermosetting resin materials. In addition, the fiber-reinforced resin material of the present disclosure can easily produce a system in which isocyanate groups are uniformly present in the matrix by heating to a temperature equal to or higher than the thermal dissociation temperature, and can form a three-dimensional network structure, resulting in excellent heat resistance and mechanical properties. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] Hereinafter, an embodiment of the present invention will be described in detail. However, the present invention is not limited to the following embodiment, and various modifications can be made without departing from the spirit of the present invention.
[0014] <Fiber reinforced resin material> The fiber-reinforced resin material according to the present embodiment includes a matrix and reinforcing fibers. The matrix includes an oligomer obtained by polyaddition of (A) a difunctional epoxy compound and (B) a polyfunctional phenol compound having a structure that generates an isocyanate group in the molecular chain upon thermal dissociation.
[0015] As the (A) bifunctional epoxy compound useful for forming the oligomer in the present embodiment, any compound having two epoxy groups in the molecule may be used without particular limitation. In terms of storage stability, tack-free property, thermoplasticity, and mechanical properties of the fiber-reinforced resin material, at least one of bisphenol-type epoxy compounds and oligomer mixtures (bisphenol-type epoxy resins) in which these are partially condensed or added, and dihydroxynaphthalene diglycidyl ether is preferred, and bisphenol-type epoxy resins are particularly preferred due to their low viscosity.
[0016] Examples of the polyfunctional phenol compound (B) having a structure that generates an isocyanate group by thermal dissociation in the molecular chain, which is useful for forming the oligomer in this embodiment, include compounds that contain an isocyanate group blocked with a blocking agent (which may also be called an isocyanate group protected by a protecting group) in the molecular chain and have a total of two or more phenolic hydroxyl groups. The isocyanate group blocked with a blocking agent (blocked isocyanate group) may have a structure (-NHC(=O)-) obtained by reacting an isocyanate (RN=C=O) with a compound (HX) having active hydrogen, such as an amine, alcohol, or carboxylic acid, as a blocking agent. The polyfunctional phenol compound (B) may have a structure that generates an isocyanate group by thermal dissociation at a temperature of, for example, 150°C or higher, 160°C or higher, or 170°C or higher, and 350°C or lower. The thermal dissociation temperature in the polyfunctional phenol compound (B) may be 20° C. or more, 30° C. or more, or 40° C. or more, and 260° C. or less, higher than the temperature at which a polyaddition reaction occurs between the epoxy group of component (A) and the phenolic hydroxyl group of component (B). Examples of structures that satisfy this thermal dissociation temperature include a urea bond using a compound having a primary amino group as a blocking agent, as described below, a secondary amide bond using a compound having a secondary amino group such as caprolactam as a blocking agent, and a urethane bond using a compound having a carboxyl group as a blocking agent.
[0017] The isocyanate compound which is the base of the structure which dissociates thermally to generate the isocyanate group may be monofunctional or polyfunctional, but polyfunctional is preferable from the viewpoint of increasing the crosslink density of the finally obtained fiber reinforced resin molding and easily increasing the heat resistance and mechanical properties. In addition, since the molecular structure is preferably as linear as possible in order to lower the thermal melting temperature and viscosity of the fiber reinforced resin material before molding, bifunctional is particularly preferable. That is, the (B) polyfunctional phenol compound preferably has two or more structures which dissociate thermally to generate the isocyanate group, and particularly preferably has two. Specific examples of the isocyanate compound include toluene diisocyanate, xylylene diisocyanate, naphthalene diisocyanate, diphenylmethane diisocyanate, hexamethylene diisocyanate, isophorone diisocyanate, bis(isocyanatomethyl)cyclohexane, and at least one of their derivatives.
[0018] The blocking agent is not particularly limited. For example, as described above, it may be a compound (HX) having active hydrogen such as amine, alcohol, or carboxylic acid. In particular, the blocking agent is preferably a compound that generates a primary amino group on the blocking agent side after thermal dissociation and elimination of the isocyanate group. Since the thermal dissociation temperature of the primary amino group is relatively high, it has the advantage that it is difficult to thermally dissociate in the process of heating to a relatively low temperature to polyaddition component (A) and component (B) to form an oligomer, but is easily thermally dissociated in the process of heating to a high temperature to form a molded product. Furthermore, since the primary amino group has two active hydrogens, it also has the advantage that it is easy to increase the crosslink density of the finally obtained fiber-reinforced resin molded product and to increase the heat resistance and mechanical properties. From the above, it is preferable that the structure that generates the isocyanate group by thermal dissociation includes a structure obtained by reacting an isocyanate group with an amino group. That is, the (B) polyfunctional phenol compound may have a structure in the molecular chain that is thermally dissociated to generate an isocyanate group and an amino group, and for example, the above-mentioned "structure that is thermally dissociated to generate an isocyanate group" may be a urea bond. Note that the (B) polyfunctional phenol compound may have a plurality of the same structures as the structure that is thermally dissociated to generate an isocyanate group, or may have a plurality of different structures, for example, may have a plurality of urea bonds, or may have a structure other than a urea bond in addition to the urea bond.
[0019] Furthermore, the (B) polyfunctional phenolic compound has two or more phenolic hydroxyl groups. The phenolic hydroxyl groups and the epoxy groups of the component (A) undergo polyaddition to form an oligomer that constitutes the matrix. When the (B) polyfunctional phenolic compound is composed of an isocyanate compound and a blocking agent, the phenolic hydroxyl groups may be contained in the isocyanate compound or in the blocking agent. Since it is preferable that the molecular structure is as linear as possible in order to lower the thermal melting temperature and thermal melting viscosity of the fiber reinforced resin material before molding, it is preferable that the (B) polyfunctional phenolic compound is a bifunctional phenolic compound as a whole molecule.
[0020] As described above, the epoxy group of component (A) and the phenolic hydroxyl group of component (B) undergo polyaddition to obtain an oligomer that serves as a matrix. The oligomer has high stability, for example, at room temperature, and does not need to be stored in a cool, dark place. The molecular weight of the oligomer is not particularly limited. For example, the mass average molecular weight of the oligomer may be 1000 to 15000 g / mol. In order to improve the hot melt viscosity of the oligomer and the toughness of the finally obtained fiber-reinforced resin molding, a general polyfunctional phenol compound (B)' such as catechol or bisphenol A may be added as a chain-extending component.
[0021] The ratio of the epoxy groups of component (A) to the phenolic hydroxyl groups of component (B) (and component (B)' in total) is preferably in the range of 3:1 to 1:1 in terms of molar ratio, from the viewpoints of controlling the degree of polymerization in the polyaddition system, rendering the fiber-reinforced resin material tack-free before molding, and adjusting the thermal melting temperature and thermal melting viscosity. When components (B) and (B)' are used in combination, the molar ratio of components (B) to (B)' is preferably in the range of 1:1 to 1:5.
[0022] It is also preferable that the polyaddition system contains a non-nucleophilic base (C) as a catalyst. That is, in the fiber-reinforced resin material of the present disclosure, the matrix may further contain a non-nucleophilic base (C) as a catalyst in addition to the above components (A) and (B) (and optionally (B)', etc.). Organophosphorus compounds having three bulky organic groups such as dicyclohexylphenylphosphine and tris(methylphenyl)phosphine, and non-nucleophilic bases having significantly reduced nucleophilicity such as 1,2-alkylenebenzimidazole and 2-aryl-4,5-diphenylimidazole have catalytic activity that prioritizes the addition reaction between epoxy groups and phenolic hydroxyl groups over the anionic polymerization of epoxy groups, thereby suppressing the crosslinking reaction during oligomer formation, growing molecular chains in a linear chain, and contributing to lowering the thermal melting temperature and thermal melting viscosity of the fiber-reinforced resin material before molding. The amount of the non-nucleophilic base (C) added is preferably 0.1 to 1 part by mass relative to 100 parts by mass of component (A).
[0023] The matrix may contain the above oligomer, as well as the above non-nucleophilic base (C) and additives described below. The matrix is preferably mainly composed of the above oligomer, and may contain, for example, 90% by mass or more, 95% by mass or more, or 98% by mass or more of the above oligomer.
[0024] The reinforcing fiber in the present embodiment is not particularly limited, but inorganic fibers, organic fibers, metal fibers, or a combination of these can be used.Specific examples include carbon fibers, graphite fibers, silicon carbide fibers, alumina fibers, tungsten carbide fibers, boron fibers, glass fibers, basalt fibers, aramid fibers, polyparaphenylene benzobisoxazole fibers, polyarylate fibers, polyphenylene sulfide fibers, polyimide fibers, fluorine fibers, stainless steel fibers, and iron fibers.From the viewpoint of light weight and high strength, carbon fibers and basalt fibers are preferred, and carbon fibers are particularly preferred.
[0025] The carbon fibers may be either PAN-based or pitch-based carbon fibers, but from the viewpoint of the balance between strength and elastic modulus, PAN-based carbon fibers are preferred.
[0026] The reinforcing fibers in this embodiment can take various forms such as fine fibers and continuous fibers. When fine fibers are used, the fiber-reinforced resin material obtained is in a state in which the fibers are dispersed in the matrix, and when continuous fibers are used, the fiber-reinforced resin material obtained is in a state in which the matrix is impregnated in the fibers. From the viewpoint of the strength of the finally obtained fiber-reinforced resin molded body, it is preferable to use continuous fibers. In addition, a fiber-reinforced resin material obtained by using continuous fibers as reinforcing fibers and then cutting or crushing it can also be suitably used.
[0027] The continuous fibers may be in the form of a unidirectional material in which the fibers are aligned, or a sheet-like material such as a woven fabric, knitted fabric, braided fabric, non-crimp fabric, or nonwoven fabric made of the fibers or unidirectional material.
[0028] The volume fraction (Vf value) of the reinforcing fibers in the fiber reinforced resin material is preferably 20% to 80%. This range provides an excellent balance between the ease of molding the fiber reinforced resin material and the strength of the final fiber reinforced resin molded product.
[0029] Various additives may be added to the fiber-reinforced resin material as necessary, such as other monomers or polymers such as bismaleimide, fillers such as ceramics or metal powders, colorants such as pigments or dyes, compatibilizers, dispersants, weather resistance agents, UV absorbers, conductive materials, and antistatic agents.
[0030] As described above, the fiber-reinforced resin material according to the present embodiment (1) does not need to be stored in a cool, dark place, for example, and is easier to handle than conventional fiber-reinforced thermosetting resin materials; (2) is less likely to have compatibility problems, such as those that occur when an additive component is added to a thermosetting resin or a thermoplastic resin; (3) can be easily molded by repeatedly exhibiting thermoplasticity within a specified temperature range, as described below; and (4) can easily produce a system in which isocyanate groups are uniformly present in the matrix, as described below, and can form a three-dimensional mesh structure to exhibit high heat resistance and mechanical properties.
[0031] <Method of manufacturing fiber reinforced resin material> Next, a method for producing the fiber-reinforced resin material of the present embodiment will be described. Note that the present invention is not limited to the manufacturing method described below. Note that some of the descriptions overlapping with those previously described will be omitted or simplified.
[0032] The method for producing a fiber-reinforced resin material according to the present embodiment includes impregnating a reinforcing fiber with a liquid containing (A) a difunctional epoxy compound and (B) a polyfunctional phenol compound having a structure that generates an isocyanate group in the molecular chain by thermal dissociation, and heating the reinforcing fiber after impregnation to polyaddition the difunctional epoxy compound (A) and the polyfunctional phenol compound (B) to form an oligomer. In the present embodiment, the liquid for impregnating the reinforcing fiber may contain component (A) and component (B). Component (A) and component (B) may be liquid themselves, or may be dissolved or dispersed in an appropriate solvent or dispersion medium. In addition, component (B)', component (C), the additives, and the like may be added to the liquid as necessary. The liquid containing component (A) and component (B) has a low viscosity, which makes it easy to uniformly disperse the matrix containing the oligomer obtained by polyaddition and the fine fibers, or to impregnate the matrix into the interior of the continuous fibers. When the matrix and the reinforcing fibers are highly integrated in this way, the final fiber-reinforced resin molding can be given a stable and higher strength without variation. From the above viewpoints, when impregnating the reinforcing fibers, the viscosity of the liquid containing component (A) and component (B) is preferably 5 to 400 mPa s.
[0033] Examples of the solvent or dispersion medium include ketones such as methyl ethyl ketone and methyl isobutyl ketone, esters such as ethyl acetate and butyl acetate, other aprotic polar solvents such as N,N-dimethylformamide and tetrahydrofuran, aromatics such as toluene and xylene, reactive diluents such as monoglycidyl ether, etc. In particular, from the viewpoint of making it possible to easily remove the solvent simultaneously with heating during the polyaddition reaction, it is preferable to use a solvent or dispersion medium having a boiling point lower than the heating temperature in the polyaddition reaction, and it is preferable to use a solvent or dispersion medium having a boiling point of 150° C. or less.
[0034] In this embodiment, the reinforcing fibers are impregnated with the liquid. For example, when fine fibers are used as the reinforcing fibers, the fine fibers may be dispersed in the liquid by stirring using a mixer, kneading using a kneader, or the like. When continuous fibers are used as the reinforcing fibers, the liquid may be applied to the continuous fibers by immersion in the liquid, coating, transferring, spraying, or the like, and if necessary, the liquid may be squeezed with a mangle or the excess may be removed with a roll.
[0035] Subsequently, the polyaddition reaction between component (A) and component (B) is carried out by heating. At this stage, the solvent or dispersion medium may be removed. The heating temperature during the polyaddition reaction can be set to a temperature at which the polyaddition reaction between component (A) and component (B) occurs or higher and lower than the temperature at which the structure of component (B) is thermally dissociated to generate an isocyanate group, and is preferably 90°C or higher and 150°C or lower. Within this range, the processing time can be shortened by promoting oligomerization, and the loss of thermoplasticity of the fiber-reinforced resin material due to thermal dissociation and crosslinking reaction of isocyanate can be easily suppressed. A more preferable heating temperature is 100°C or higher and 140°C or lower.
[0036] The polyaddition reaction between component (A) and component (B) is controlled to such an extent that the resulting fiber-reinforced resin material is free of tack and does not lose thermoplasticity. Specifically, it is preferable to control the polyaddition reaction so that the mass average molecular weight of the oligomer obtained has a low degree of polymerization of about 1000 to 15000 g / mol. The degree of polymerization of the oligomer may be adjusted by the mixing ratio of component (A) and component (B), the heating temperature, the heating time, etc.
[0037] <Fiber-reinforced resin molding> Next, the fiber-reinforced resin molding of the present embodiment will be described. Note that some of the descriptions overlapping with those previously described will be omitted or simplified.
[0038] The fiber-reinforced resin molding according to the present embodiment is formed by forming a three-dimensional network structure with the fiber-reinforced resin material. The three-dimensional network structure is, for example, a structure in which the functional groups of the thermally dissociated isocyanate and the blocking agent regenerated by thermal dissociation of the isocyanate react with the epoxy groups remaining in the oligomer molecules forming the matrix and the alcoholic hydroxyl groups in the oligomer chain derived from the epoxy groups ring-opened during oligomer formation to form a crosslink. The fiber-reinforced resin material according to the present embodiment can exhibit thermoplasticity in a low temperature range before the above-mentioned thermal dissociation temperature is reached when heated, so that it can be molded before the thermal dissociation temperature is reached by utilizing this. Alternatively, the fiber-reinforced resin material may be heated to a temperature equal to or higher than the thermal dissociation temperature to form the above-mentioned three-dimensional network structure and molded at the same time. Pressure may be applied during molding together with heating. The fiber-reinforced resin molding according to the present embodiment may be formed by forming the three-dimensional network structure after laminating a plurality of the fiber-reinforced resin materials.
[0039] The fiber-reinforced resin molded body in this embodiment can be molded into any shape by utilizing the thermoplasticity of the fiber-reinforced resin material that serves as the molding material. In addition, the isocyanate thermally dissociated by heating and the functional group of the blocking agent regenerated by thermal dissociation of the isocyanate react with the epoxy group remaining in the oligomer molecule that forms the matrix and the alcoholic hydroxyl group in the oligomer chain derived from the epoxy group that was opened during oligomer generation to form a three-dimensional network structure like a thermosetting resin, so that the heat resistance and mechanical properties of the fiber-reinforced resin molded body can be at the same level as a fiber-reinforced resin molded body made of a fiber-reinforced resin material using a thermosetting resin as a matrix. Furthermore, compared with the conventional method of adding a crosslinking agent to a thermoplastic resin or the method of adding a curing agent or a thermoplastic resin to an epoxy prepolymer, compatibility problems are less likely to occur, and a system in which the isocyanate group is uniformly present in the matrix can be easily created, so that the process of dispersing the crosslinking agent in the resin can be reduced, and at the same time, a fiber-reinforced resin molded body having a high strength without variation and a uniform crosslinking point present in the matrix can be obtained.
[0040] The fiber-reinforced resin molded article in this embodiment may have a storage modulus of 10 GPa or more at 200° C., for example. If the storage modulus is 10 GPa or more at 200° C., it is preferable because it has an excellent ability to maintain its shape even under high temperature and high load conditions. It is more preferable that the storage modulus is 20 GPa or more, and particularly preferably 30 GPa or more.
[0041] <Method of manufacturing fiber-reinforced resin molded body> Next, a fiber-reinforced resin molding according to the present embodiment will be described. Note that the present invention is not limited to the manufacturing method described below. Also, some of the descriptions overlapping with those previously described will be omitted or simplified.
[0042] The manufacturing method of the fiber reinforced resin molded body of this embodiment includes heating the fiber reinforced resin material. As described above, the fiber reinforced resin material of this embodiment can exhibit thermoplasticity in a low temperature range before reaching the thermal dissociation temperature when heated, so that it can be molded before reaching the thermal dissociation temperature and heated to the thermal dissociation temperature or higher after molding to form the above-mentioned three-dimensional network structure, or the fiber reinforced resin material can be heated to the thermal dissociation temperature or higher to form the above-mentioned three-dimensional network structure and molded at the same time. From the viewpoint of simplifying the processing step, it is preferable to heat the fiber reinforced resin material to the thermal dissociation temperature or higher to form the above-mentioned three-dimensional network structure and mold it at the same time. In addition, when molding is performed in multiple steps, such as deep drawing, it is preferable to heat the heating temperature at the time of final molding to the thermal dissociation temperature or higher to form the above-mentioned three-dimensional network structure and mold it at the same time. In addition, from the viewpoint of further improving moldability and further increasing strength as described later, it is preferable to apply pressure together with heating during molding. Furthermore, in the method for producing a fiber-reinforced resin molded product according to the present embodiment, the fiber-reinforced resin material may be laminated in a plurality of layers and then heated, which can further improve the mechanical properties of the fiber-reinforced resin molded product.
[0043] The fiber-reinforced resin material is used in an appropriate shape, such as a block, sheet, tape, or chip, which is placed in a mold.
[0044] Examples of the method for applying heat and pressure include a die pressing method, an autoclave method, and a hot / cold pressing method.
[0045] The heating temperature during molding is higher than the heating temperature during polyaddition of component (A) and component (B) and can be set to a temperature or higher at which the structure of component (B) thermally dissociates to generate isocyanate groups, and is particularly preferably set to 150°C or higher. If the temperature is heated to 150°C or higher, it becomes easier to soften and shape the fiber-reinforced resin material, and at the same time, to thermally dissociate the isocyanate groups and cause a crosslinking reaction to harden the material. A more preferred heating temperature is 160°C or higher, and even more preferred is 170°C or higher. The upper limit of the heating temperature is preferably 350°C or lower from the viewpoint of suppressing scorching of the fiber-reinforced resin molded body and a decrease in strength due to thermal decomposition of the resin.
[0046] When applying pressure, the pressure can be, for example, 1 to 50 MPa, but it is preferable to apply pressure of 15 MPa or more at the same time as heating in order to expel carbon dioxide gas generated when isocyanate generated by thermal dissociation reacts with a trace amount of moisture in the air, and to expel air present between sheets or chips from the matrix when multiple fiber-reinforced resin materials in sheet or chip form are stacked and filled in a mold, thereby reducing the number of voids generated and achieving stable high strength without variation. It may also be combined with reducing the pressure inside the mold.
[0047] The heating time (when pressure is applied, the heating and pressure application time) can be, for example, 1 minute to 24 hours. After heating and pressure application, the fiber-reinforced resin molding can be cooled to obtain a fiber-reinforced resin molding of any shape. EXAMPLES
[0048] The present invention will be further described below with reference to examples, but the present invention is not limited to these examples. In the following examples, "parts" refers to parts by mass.
[0049] <Viscosity of Liquid Monomer (Liquid Containing Component (A) and Component (B))> The viscosity of the liquid monomer was measured using a Brookfield viscometer (TVB-15 viscometer, manufactured by Toki Sangyo Co., Ltd.) with a rotor No. 20 at 12 rpm at room temperature (22° C.).
[0050] <Mass average molecular weight of the matrix of fiber-reinforced resin material> The mass average molecular weight of the matrix of the fiber-reinforced resin material was measured by size exclusion chromatography. Specifically, a solution of the matrix was prepared in tetrahydrofuran at 1 mg / 1 mL, and the solution was injected into a C18 column (Inertsil ODS analysis column, GL Sciences, Inc.) that was connected to two 150 mm columns and set at 40° C., and the solution was pumped at 0.5 mL / min. A chromatogram was obtained using a differential refractometer (RID-20A, Shimadzu Corporation). The mass average molecular weight was calculated using the obtained chromatogram based on a calibration curve prepared using a polystyrene standard sample.
[0051] <Storage modulus of fiber-reinforced resin molding at 200°C> A sample measuring 10 mm in width, 50 mm in length, and 2 mm in thickness was taken from the fiber-reinforced resin molding, and using a viscoelasticity measuring device (DMS6100, Hitachi High-Tech Science Corporation) the sample was heated from room temperature to 210°C at a heating rate of 2°C / min using a three-point bending mode, a support distance of 40 mm, and a frequency of 1 Hz, and the storage modulus at 200°C was read.
[0052] Example 1 First, a PAN-based carbon fiber twill fabric (PYROFIL TRK510 M, manufactured by Mitsubishi Chemical Corporation) was prepared as a reinforcing fiber.
[0053] Next, the liquid monomer was added as follows: The viscosity of the resulting liquid monomer was 200 mPa·s.
[0054] Component (A): Bisphenol A diglycidyl ether (molecular weight: 340 g / mol) 68 parts Component (B): m-xylylene diisocyanate in which the two isocyanate groups are each blocked with 4-hydroxybenzylamine via a urea bond (molecular weight: 434 g / mol, formula 1 below) 43 parts Solvent: 10 parts methyl ethyl ketone
[0055] [ka]
[0056] Next, the carbon fiber fabric was immersed in a bath containing the liquid monomer and heated at 120° C. for 10 minutes to obtain a tack-free sheet-like fiber reinforced resin material.
[0057] The Vf value of the obtained fiber reinforced resin material was 65%. The mass average molecular weight of the matrix of the obtained fiber reinforced resin material was 2030 g / mol.
[0058] The obtained sheet-like fiber-reinforced resin material was stored in the laboratory for 14 days, after which four sheets of the fiber-reinforced resin material were stacked, placed on a flat-bottomed bowl-shaped mold, and heated and pressurized at 200°C and 30 MPa for 10 minutes using a vacuum press. A bowl-shaped fiber-reinforced resin molding was obtained without any defects such as cracks.
[0059] The storage modulus of the obtained fiber-reinforced resin molding at 200° C. was 57 GPa, and the appearance of the sample after the test was unchanged from before the test.
[0060] Example 2 A tack-free sheet-like fiber-reinforced resin material was obtained in the same manner as in Example 1, except that the liquid monomer of the following composition was used. The viscosity of the liquid monomer was 250 mPa·s.
[0061] Component (A): Bisphenol A diglycidyl ether (molecular weight: 340 g / mol) 68 parts Component (B): m-xylylene diisocyanate in which the two isocyanate groups are each blocked with 4-hydroxybenzylamine via a urea bond (molecular weight: 434 g / mol, formula 1 above) 12 parts Component (B)': Bisphenol A (molecular weight 228 g / mol) 16 parts Component (C): Tris(4-methylphenyl)phosphine 0.4 parts Solvent: 10 parts methyl ethyl ketone
[0062] The Vf value of the obtained fiber reinforced resin material was 63%. The mass average molecular weight of the matrix of the obtained fiber reinforced resin material was 12600 g / mol.
[0063] The obtained sheet-like fiber-reinforced resin material was stored in the laboratory for 14 days, after which four sheets of the fiber-reinforced resin material were stacked, placed on a flat-bottomed bowl-shaped mold, and heated and pressurized at 180°C and 20 MPa for five minutes using a vacuum press. A bowl-shaped fiber-reinforced resin molding was obtained without any defects such as cracks.
[0064] The storage modulus of the obtained fiber-reinforced resin molding at 200° C. was 33 GPa, and the appearance of the sample after the test was unchanged from before the test.
[0065] Comparative Example 1 A tack-free sheet-like fiber-reinforced resin material was obtained in the same manner as in Example 1, except that the liquid monomer of the following composition was used. The viscosity of the liquid monomer was 220 mPa·s.
[0066] Component (A): Bisphenol A diglycidyl ether (molecular weight: 340 g / mol) 68 parts Component (B)': Bisphenol A (molecular weight 228 g / mol) 23 parts Hardener: 0.4 parts 2-methylimidazole Solvent: 10 parts methyl ethyl ketone
[0067] The Vf value of the obtained fiber-reinforced resin material was 61%. In addition, the matrix of the obtained fiber-reinforced resin material was insoluble in tetrahydrofuran because the polyaddition reaction was not controlled and the resin formed a three-dimensional network structure.
[0068] Following the production of the fiber reinforced resin material, four sheets of the obtained fiber reinforced resin material were stacked and placed on a flat-bottomed bowl-shaped mold, and heated and pressurized at 200°C and 30 MPa for 10 minutes using a vacuum press, but the fiber reinforced resin material did not soften and multiple cracks occurred, making it impossible to mold. Note that for Comparative Example 1, the storage modulus of the fiber reinforced resin material at 200°C before molding was 37 GPa.
[0069] Comparative Example 2 The carbon fiber fabric was immersed in a bath containing liquid monomers having the same composition as in Comparative Example 1 and heated at 90° C. for 10 minutes to obtain a tack-free sheet-like fiber reinforced resin material.
[0070] The Vf value of the obtained fiber reinforced resin material was 61%. The mass average molecular weight of the matrix of the obtained fiber reinforced resin material was 8400 g / mol.
[0071] The obtained sheet-like fiber-reinforced resin material was stored in a laboratory for 14 days. After 14 days, the surface of the fiber-reinforced resin material had turned white and had small bubbles due to the inactivation of the epoxy groups at room temperature. Four sheets of the fiber-reinforced resin material were stacked and placed on a flat-bottomed, bowl-shaped mold, and heated and pressurized at 200°C and 30 MPa for 10 minutes using a vacuum press, but the fiber-reinforced resin material did not harden, and a fiber-reinforced resin molded product was formed that was hard enough to be deformed by hand even at room temperature.
[0072] Comparative Example 3 A tack-free sheet-like fiber-reinforced resin material was obtained in the same manner as in Example 1, except that the liquid monomer of the following composition was used. The viscosity of the liquid monomer was 230 mPa·s.
[0073] Component (A): Bisphenol A diglycidyl ether (molecular weight: 340 g / mol) 68 parts Component (B)': Bisphenol A (molecular weight 228 g / mol) 23 parts Component (C): Tris(4-methylphenyl)phosphine 0.4 parts Solvent: 10 parts methyl ethyl ketone
[0074] The Vf value of the obtained fiber reinforced resin material was 63%. The mass average molecular weight of the matrix of the obtained fiber reinforced resin material was 49,300 g / mol.
[0075] The obtained sheet-like fiber-reinforced resin material was stored in the laboratory for 14 days, after which four sheets of the fiber-reinforced resin material were stacked, placed on a flat-bottomed bowl-shaped mold, and heated and pressurized at 180°C and 20 MPa for five minutes using a vacuum press. A bowl-shaped fiber-reinforced resin molding was obtained without any defects such as cracks.
[0076] The storage modulus of the obtained fiber-reinforced resin molding at 200° C. was 3 GPa, and it was confirmed that the surface of the sample after the test was rough. [Industrial Applicability]
[0077] The fiber reinforced resin material according to the present invention can be handled in the same manner as a fiber reinforced resin material using a thermoplastic resin as a matrix, and can produce a molded body having the same level of heat resistance and mechanical properties as a fiber reinforced resin molded body using a fiber reinforced resin material using a thermosetting resin as a matrix. Therefore, it can be suitably used as a part that requires high heat resistance and excellent mechanical properties, such as a robot member used in a high temperature environment, a roll used in an oven, a printed circuit board that requires solder heat resistance, and a heat-resistant rod for a tension member of an electric cable.
Claims
1. A matrix and reinforcing fibers are included, the matrix contains an oligomer obtained by polyaddition of (A) a difunctional epoxy compound and (B) a polyfunctional phenol compound having a urea bond in a molecular chain, the urea bond being a structure that is thermally dissociated to generate an isocyanate group; Fiber reinforced resin material.
2. The matrix further comprises (C) a non-nucleophilic base as a catalyst; The fiber reinforced resin material according to claim 1.
3. The fiber-reinforced resin material according to claim 1 or 2 forms a three-dimensional network structure. Fiber reinforced resin molding.
4. The storage modulus at 200 ° C. is 10 GPa or more. The fiber-reinforced resin molding according to claim 3.
5. Impregnating reinforcing fibers with a liquid containing (A) a bifunctional epoxy compound and (B) a polyfunctional phenol compound having a urea bond in a molecular chain, the urea bond being a structure that is thermally dissociated to generate an isocyanate group; and Heating the impregnated reinforcing fiber to polyaddition-do the difunctional epoxy compound (A) and the polyfunctional phenol compound (B) to form an oligomer; A method for producing a fiber-reinforced resin material, comprising:
6. The heating temperature during the polyaddition is 90° C. or higher and 150° C. or lower. A method for producing the fiber reinforced resin material according to claim 5.
7. Heating the fiber reinforced resin material according to claim 1 or 2; A method for producing a fiber-reinforced resin molded product comprising the steps of:
8. The heating temperature is 150° C. or higher. The method for producing the fiber-reinforced resin molding according to claim 7.
9. The heating and the pressure application may include applying a pressure of 15 MPa or more at the same time. The method for producing the fiber-reinforced resin molding according to claim 7 or 8.
Citation Information
Patent Citations
Production of prepreg
JP1986040317A
prepreg
JP1994009802A
Prepreg, laminate and multilayer printed wiring board
JP1998251421A
Polyester fiber material having improved adhesion to rubber and its production
JP2000212875A
Curable resin composition
JP2010195919A