Fast-hardening grout composition and fast-hardening grout

A fast-setting grout composition using calcium aluminates coated with hydrates and alkali metal carbonates addresses temperature dependence issues, ensuring fluidity and strength development for rapid construction in cold conditions.

JP7558625B2Active Publication Date: 2024-10-01TAIHEIYO MATERIALS CORP
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
JP2021042441
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-03-16
Publication Date
2024-10-01
Estimated Expiration
2041-03-16

AI Technical Summary

Technical Problem

Grouting materials with rapid hardening properties exhibit poor strength development at low temperatures and have significant temperature dependence, limiting their effectiveness in cold environments.

Method used

A fast-setting grout composition comprising a binder made of cement, calcium aluminates coated with hydrates, and at least two types of alkali metal carbonates, with specific ratios and adjustments to ensure fluidity and strength development even at low temperatures.

Benefits of technology

The composition provides good fluidity, sufficient pot life, and excellent strength development in low-temperature conditions, making it suitable for rapid construction in cold environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007558625000001
    Figure 0007558625000001
Patent Text Reader

Abstract

To provide a fast curing grout composition and fast curing grout having good fluidity as a grout material even at low temperatures, ensuring sufficient pot life required for workability, and having excellent fast curing and strength development properties.SOLUTION: A fast curing grout composition of the invention contains: a binder consisting of cement, calcium aluminates, and gypsum; and at least two alkali metal carbonates, wherein the calcium aluminates contain hydrate-coated calcium aluminates, the amount of coverage of the hydrate in the hydrate-coated calcium aluminates is 0.1 to 4.8 mass% relative to the mass of the hydrate-coated calcium aluminates, and the total content of the alkali metal carbonates is 0.15 to 1.05 pts.mass relative to 100 pts.mass of the binder.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a fast setting grout composition and to a fast setting grout. [Background technology]

[0002] Conventionally, highly fluid cement-based grout materials have been used in the construction or repair of civil engineering structures and architectural structures, installation of machines, etc. In particular, when the time available for construction is limited, such as in repair work of structures such as roads and railways, it is desirable to use grout materials that quickly develop strength after filling. As such grout materials, fast-hardening grout materials that develop the required strength at an age of 3 hours have been proposed (for example, Patent Documents 1 and 2).

[0003] The performance required for grout materials is not only strength but also pot life, and it is desirable for the pot life to ensure sufficient workability. Therefore, in order to ensure the pot life, an admixture using calcium aluminate with a water-treated surface has been proposed (Patent Document 3). [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Japanese Patent Application Publication No. 11-021160 [Patent Document 2] JP 2005-289656 A [Patent Document 3] JP 2020-050557 A Summary of the Invention [Problem to be solved by the invention]

[0005] However, the fast-hardening grout material has a problem that it is highly temperature-dependent and has poor strength development at low temperatures. Therefore, a grout material that has little temperature dependence even at low temperatures and has sufficient strength development is desired.

[0006] Therefore, an object of the present invention is to provide a fast-hardening grout composition and a fast-hardening grout which have good fluidity as a grout material even at low temperatures, ensure sufficient pot life necessary for workability, and are excellent in fast-hardening properties and strength development. [Means for solving the problem]

[0007] As a result of intensive research by the present inventors into the above-mentioned problems, it has been found that by using calcium aluminates coated with hydrates and adjusting the total content of a plurality of alkali metal carbonates, it is possible to obtain a fast-hardening grout composition that achieves good fluidity, pot life, and strength development even in low temperature environments.

[0008] That is, the present invention is as follows. [1] A fast-setting grout composition comprising a binder comprising cement, calcium aluminates, and gypsum, and at least two types of alkali metal carbonates, wherein the calcium aluminates include calcium aluminates coated with hydrates, the amount of hydrate coating in the hydrate-coated calcium aluminates being 0.1-4.8% by mass relative to the mass of the hydrate-coated calcium aluminates, and the total content of the alkali metal carbonates being 0.15-1.05 parts by mass relative to 100 parts by mass of the binder. [2] The fast-hardening grout composition according to [1], wherein the alkali metal carbonate is at least two selected from the group consisting of lithium carbonate, sodium carbonate, and potassium carbonate. [3] The fast-hardening grout composition according to [1] or [2], further comprising a foaming agent. [4] The fast-hardening grout composition according to any one of [1] to [3], which is for use in low temperature environments. [5] A rapid-hardening grout comprising the rapid-hardening grout composition according to any one of [1] to [4] and water, the water content being 35 to 45 parts by mass per 100 parts by mass of the binder. Effect of the Invention

[0009] According to the present invention, it is possible to provide a fast-hardening grout composition and a fast-hardening grout which have good fluidity as a grout material even at low temperatures, ensure sufficient pot life necessary for workability, and are excellent in fast-hardening properties and strength development. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] Hereinafter, one embodiment of the present invention will be described in detail.

[0011] The rapid hardening concrete of this embodiment includes a binder made of cement, calcium aluminates, and gypsum, and at least two types of alkali metal carbonates, and the calcium aluminates include calcium aluminates coated with hydrates.

[0012] In this specification, the binder is composed of three components: cement, calcium aluminates, and gypsum.

[0013] Various types of cement can be used, including, for example, various Portland cements such as ordinary, early strength, super early strength, low heat and moderate heat; mixed cements containing blast furnace slag, fly ash or silica fume; ecocement; rapid hardening cement, etc. As the cement, ordinary Portland cement or early strength Portland cement is preferable from the viewpoint of easily achieving both early strength development and improvement in fluidity. One type of cement may be used alone, or two or more types may be used in combination.

[0014] The content of cement is preferably 30 to 80 parts by mass, more preferably 35 to 70 parts by mass, and even more preferably 40 to 55 parts by mass, relative to 100 parts by mass of the binder. When the content of cement is within the above range, good fluidity is easily obtained and initial strength development is excellent.

[0015] Calcium aluminates are calcium aluminates with mineral compositions indicated as C3A, C2A, C12A7, CA, or CA2, where CaO is C, Al2O3 is A, Na2O is N, and Fe2O3 is F. Calcium aluminates include calcium aluminoferrites indicated as C4AF, etc., calcium aluminates with halogens dissolved or substituted in a solid solution, such as C3A3·CaF2 and C 11 A general term for calcium haloaluminates including calcium fluoroaluminates designated as A7·CaF2, calcium sodium aluminates designated as C8NA3 or C3N2A5, calcium lithium aluminate, alumina cement, and calcium sulfoaluminates designated as C3A3·CaSO4. These calcium aluminates can be crystalline, amorphous, or a mixture of amorphous and crystalline. The calcium aluminates may be used alone or in combination of two or more. From the viewpoint of further improving early strength development, the fineness of calcium aluminates is set to 3000 cm2 in terms of Blaine specific surface area. 2 / g or more, and 2 / g or more. The fineness of calcium aluminates is preferably 8000 cm2 in terms of Blaine specific surface area. 2 It is preferable that the molecular weight is not more than 1 / g.

[0016] The calcium aluminates according to the present embodiment include calcium aluminates whose surfaces are coated with a hydrate of calcium aluminates. The amount of the hydrate of the calcium aluminates coated with a hydrate is 0.1 to 4.8% by mass relative to the mass of the calcium aluminates coated with a hydrate. If the amount of the hydrate is outside the above range, the pot life cannot be sufficiently secured, and the storage manageability is also reduced. From the viewpoint of securing a sufficient pot life and further improving the fluidity in a low-temperature environment, the amount of the hydrate of the calcium aluminates coated with a hydrate is preferably 0.2 to 4% by mass, more preferably 0.4 to 2.5% by mass, relative to the mass of the calcium aluminates coated with a hydrate. As the calcium aluminates, calcium aluminates coated with a hydrate may be used alone, or calcium aluminates coated with a hydrate and calcium aluminates not coated with a hydrate may be used in combination. When calcium aluminates coated with hydrates are used in combination with calcium aluminates not coated with hydrates, the content of the calcium aluminates coated with hydrates is preferably 10 to 90 parts by mass, more preferably 15 to 75 parts by mass, and even more preferably 25 to 60 parts by mass, relative to 100 parts by mass of the total calcium aluminates. If the content of the calcium aluminates coated with hydrates is within the above range, it is easy to ensure both rapid hardening and pot life.

[0017] The method for hydrating the surface of calcium aluminates is not particularly limited. For example, the powder of calcium aluminates may be charged into a mixer and stirred and mixed while spraying water in an amount equivalent to the amount of the hydrate to be prepared.

[0018] The content of calcium aluminates is preferably 10 to 50 parts by mass, more preferably 15 to 45 parts by mass, and even more preferably 25 to 40 parts by mass, relative to 100 parts by mass of the binder. If the content of calcium aluminates is within the above range, it is easy to achieve both rapid curing and pot life, and excellent initial strength development.

[0019] Examples of gypsum include anhydrous gypsum, hemihydrate gypsum, and dihydrate gypsum. As the gypsum, anhydrous gypsum is preferable from the viewpoint of further improving the strength development. One type of gypsum may be used alone, or two or more types may be used in combination.

[0020] The specific surface area of ​​gypsum is 3000 to 10000 cm 2 / g, and 3000 to 9000 cm 2 / g, and more preferably 5000 to 8000 cm 2 When the Blaine specific surface area of ​​the gypsum is within the above range, the initial strength development is further improved.

[0021] The content of the gypsum is preferably 5 to 30 parts by mass, more preferably 10 to 25 parts by mass, and even more preferably 14 to 20 parts by mass, relative to 100 parts by mass of the binder. If the content of the gypsum is within the above range, good fluidity and pot life are easily ensured, and rapid hardening and initial strength development are easily excellent.

[0022] The fast-setting grout composition of the present embodiment contains at least two types of alkali metal carbonates. The alkali metal carbonate is not particularly limited as long as it is a carbonate of an alkali metal (a Group 1 element of the periodic table excluding hydrogen atoms). As the alkali metal carbonate, lithium carbonate, sodium carbonate, and potassium carbonate are preferred. From the viewpoint of further promoting the strength development, the alkali metal carbonate preferably contains sodium carbonate, and lithium carbonate and sodium carbonate are more preferred. Three or more types of alkali metal carbonates may be used in combination.

[0023] The total content of the alkali metal carbonate is 0.15 to 1.05 parts by mass relative to 100 parts by mass of the binder. When the content of the alkali metal carbonate is within the above range, good fluidity and strength development can be obtained. From the viewpoint of further improving the fluidity and strength development, the total content of the alkali metal carbonate is preferably 0.18 to 1.00 parts by mass, and more preferably 0.2 to 0.9 parts by mass.

[0024] When the alkali metal carbonate contains sodium carbonate, the content of sodium carbonate is preferably 20 to 70 parts by mass, more preferably 30 to 65 parts by mass, and even more preferably 35 to 60 parts by mass, relative to 100 parts by mass of the alkali metal carbonate. When the content of sodium carbonate is within the above range, good fluidity is easily ensured, and strength development is further improved.

[0025] The fast-setting grout composition of the present embodiment may contain a water reducing agent. The water reducing agent includes a high-performance water reducing agent, a high-performance AE water reducing agent, an AE water reducing agent, and a superplasticizer. Examples of such water reducing agents include those specified in JIS A 6204:2011 "Chemical admixtures for concrete". Examples of the water reducing agent include polycarboxylic acid-based water reducing agents, naphthalenesulfonic acid-based water reducing agents, ligninsulfonic acid-based water reducing agents, and melamine-based water reducing agents. Among these, ligninsulfonic acid-based water reducing agents and naphthalenesulfonic acid-based water reducing agents are preferred. The water reducing agents may be used alone or in combination of two or more types.

[0026] The content of the water reducing agent is preferably 0.05 to 1.0 parts by mass, more preferably 0.1 to 0.7 parts by mass, and even more preferably 0.1 to 0.5 parts by mass, relative to 100 parts by mass of the binder. If the content of the water reducing agent is within the above range, the composition tends to have excellent fluidity.

[0027] The fast-setting grout composition of the present embodiment may further contain a foaming agent. The foaming agent is not particularly limited, and may be, for example, a substance that generates gas after being kneaded with water. Examples of the foaming agent include powder of amphoteric metals such as aluminum and zinc, and peroxide substances such as sodium percarbonate. As the foaming agent, peroxide substances are preferred from the viewpoint of being able to foam effectively and to further exert the expansion action, and among them, sodium percarbonate is preferred. The foaming agent may be used alone or in combination of two or more types.

[0028] The content of the foaming agent is preferably 0.01 to 0.2 parts by mass, more preferably 0.03 to 0.18 parts by mass, and even more preferably 0.05 to 0.15 parts by mass, relative to 100 parts by mass of the binder. If the content of the foaming agent is within the above range, it is easy to prevent settlement and reduction in strength after filling with the fast-hardening grout material, and excessive expansion is unlikely to cause a decrease in strength.

[0029] The fast-setting grout composition of the present embodiment may contain a defoaming agent. The defoaming agent is not particularly limited as long as it is a general cement defoaming agent, a cement mortar defoaming agent, or a defoaming agent used in concrete, and examples thereof include mineral oil defoaming agents, ester defoaming agents, amine defoaming agents, amide defoaming agents, polyether defoaming agents, and silicone defoaming agents. The defoaming agent may be used alone or in combination of two or more. The defoaming agent may be liquid or powder, and it is preferable to use a powder defoaming agent from the viewpoint that the material is easily homogenized when the premix, i.e., the cement and the admixture are dry-mixed, as in the case of premix mortar.

[0030] The content of the antifoaming agent is preferably 0.003 to 0.2 parts by mass, more preferably 0.005 to 0.15 parts by mass, and further preferably 0.008 to 0.1 parts by mass, relative to 100 parts by mass of the binder.

[0031] The fast-setting grout composition of the present embodiment may further contain fine aggregate. Examples of fine aggregate include river sand, silica sand, crushed sand, kansui stone, limestone sand, slag aggregate, and the like. Of these, it is preferable to use silica sand, limestone sand, and the like adjusted to a grain size that does not contain fine powder or coarse aggregate as the fine aggregate. One type of fine aggregate may be used alone, or two or more types may be used in combination. It is preferable to use fine aggregate having a grain size of 5 mm or less (passing through a 5 mm sieve), which is commonly used.

[0032] The particle size of the fine aggregate is not particularly limited, and can be adjusted within the required particle size range of the fine aggregate. The particle size of the fine aggregate can be considered from the coarse aggregate ratio defined by JIS A 1102:2014 "Sieving test method for aggregates". From the viewpoint of obtaining better fluidity when made into grout and suppressing bleeding, the coarse aggregate ratio is preferably 1 to 4, more preferably 1.5 to 3.8, and most preferably 2 to 3.5.

[0033] The content of the fine aggregate is preferably 50 to 250 parts by mass, more preferably 60 to 180 parts by mass, and even more preferably 80 to 150 parts by mass, relative to 100 parts by mass of the binder. If the content of the fine aggregate is within the above range, better flowability is ensured, and strength development in a short period of time is further improved.

[0034] The fast-hardening grout composition of the present embodiment may contain a set retarder. Examples of the set retarder include organic acids or salts thereof such as citric acid, gluconic acid, malic acid, and tartaric acid; boric acid, borates such as sodium borate, phosphates, and inorganic salts such as alkali metal bicarbonates; and sugars. Among these, citric acid, citrates, tartaric acid, and tartrates are preferred. The set retarder may be in the form of a powder or a liquid (for example, an aqueous solution, an emulsion, or a suspension). The set retarder may be used alone or in combination of two or more.

[0035] The content of the setting retarder is preferably 0.01 to 1 part by mass, more preferably 0.1 to 0.8 parts by mass, and even more preferably 0.12 to 0.5 parts by mass, relative to 100 parts by mass of the binder. If the content of the setting retarder is within the above range, the pot life is more easily ensured and the initial strength development is less likely to decrease.

[0036] The fast-setting grout composition of the present embodiment may contain various admixtures (materials) within the range that does not impair the effects of the present invention. Examples of the admixtures (materials) include expansive materials, cement polymers, waterproofing agents, rust inhibitors, shrinkage reducing agents, water retention agents, pigments, water repellents, efflorescence inhibitors, fibers, blast furnace slag powder, stone powder, earth mineral powder, slag powder, fly ash, silica fume, inorganic fillers, volcanic ash, etc.

[0037] The method for producing the fast-hardening grout composition of the present embodiment is not particularly limited, and the composition can be produced by mixing using a gravity mixer such as a V-type mixer or a tilting concrete mixer, a Henschel mixer, a jet mixer, a ribbon mixer, a paddle mixer, or the like.

[0038] The fast-setting grout composition of the present embodiment can also be used as a fast-setting grout composition for low-temperature environments. In this specification, the term "for low-temperature environments" refers to a fast-setting grout composition that is capable of withstanding an environment of less than 15°C in accordance with the Japan Society of Civil Engineers (JSCE) standard JSCE-F 541-2013 "Test method for fluidity of filling mortar". 14 The funnel flow time is 6 to 10 seconds, and the compressive strength of the hardened mortar at an age of 3 hours is 10 N / mm according to the Japan Society of Civil Engineers standard JSCE-G 505-2018 "Compressive strength test method for mortar or cement paste using cylindrical specimens (draft)". 2 This indicates that the pot life is 10 minutes or more according to the pot life test described below.

[0039] The fast-setting grout composition of the present embodiment can be prepared as a fast-setting grout by mixing with water, and the water content may be appropriately adjusted depending on the application. The water content is preferably 35 to 45 parts by mass, more preferably 37 to 43 parts by mass, and even more preferably 38 to 42 parts by mass, relative to 100 parts by mass of the binder. If the water content is within the above range, it is easier to ensure fluidity, and it is easier to suppress the occurrence of material separation and the decrease in early strength development.

[0040] The preparation of the fast-setting grout of the present embodiment can be carried out using a kneading tool similar to that used for preparing a typical fast-setting grout composition, and is not particularly limited. Examples of the kneading tool include a mortar mixer, a grout mixer, a hand mixer, a tilting mixer, and a twin-shaft mixer.

[0041] According to the fast-setting grout composition and the fast-setting grout of the present embodiment, the pot life can be sufficiently secured, and the fast-setting grout composition and the fast-setting grout have good fluidity and strength development even in a low-temperature environment. Therefore, the fast-setting grout composition and the fast-setting grout of the present embodiment can be suitably used for repair work in a low-temperature environment such as winter, and can also be suitably used for repair work of structures such as roads and railways where rapid construction is required. EXAMPLES

[0042] The present invention will be described in detail below with reference to examples, but the present invention is not limited thereto.

[0043] [material] Cement: Ordinary Portland cement Cement: High early strength Portland cement Calcium aluminate 1 (AC1): Alumina cement (hydration coverage 0 mass%, Blaine specific surface area 5200 cm 2 / g) Calcium aluminate 1 (AC2): Alumina cement (hydration coverage 0.5 mass%, Blaine specific surface area 5200 cm 2 / g) Calcium aluminate 1 (AC3): Alumina cement (hydration coverage 1.0 mass%, Blaine specific surface area 5200 cm 2 / g) Calcium aluminate 1 (AC4): Alumina cement (hydration coverage 2.0 mass%, Blaine specific surface area 5200 cm 2 / g) Calcium aluminate 1 (AC5): Alumina cement (hydration coverage 5.0 mass%, Blaine specific surface area 5200 cm 2 / g) Gypsum: Anhydrous gypsum (Brain specific surface area 7000cm 2 / g) Alkali metal carbonate: Sodium carbonate Alkali metal carbonate: Lithium carbonate Defoamer: Polyether-based defoamer Foaming agent: Sodium percarbonate Set retarder: Citric acid Water reducing agent: Naphthalene sulfone water reducing agent Fine aggregate: Silica sand (coarse grain ratio 2.37)

[0044] [Preparation of calcium aluminate] The alumina cement was placed in a Lödige mixer, and while rotating the mixer, water was added by sprayer in an amount equivalent to the amount of hydrate to be prepared (0.5-5 mass%) over a period of about 2 minutes, and the mixture was further mixed by rotation for 10 minutes. The mixture was left in the air at about 20°C for 3 hours to hydrate the calcium aluminate particle surfaces, thereby preparing calcium aluminate coated with hydrate.

[0045] [Mix design of fast-hardening grout composition] The mix was designed so that 100 parts by mass of binder consisting of cement, calcium aluminates, and gypsum were used with the amounts of various materials shown in Table 1, with 0.12 parts by mass of foaming agent, 0.04 parts by mass of antifoaming agent, 0.16 parts by mass of setting retarder, 0.20 parts by mass of water reducing agent, and 100 parts by mass of fine aggregate.

[0046] [Preparation of fast-hardening grout] In a 5°C environment, 6000 g of the formulated rapid hardening grout composition and water were added to a 10 L cylindrical container, and the mixture was mixed for 90 seconds with a hand mixer to prepare a rapid hardening grout. 41 parts by mass of water was added per 100 parts by mass of the binder.

[0047] [Evaluation method] Various types of fast-hardening grouts were evaluated using the following evaluation methods. All tests were carried out at 5°C. Measurement of J-funnel flow rate In accordance with the Japan Society of Civil Engineers standard JSCE-F 541-2013 "Test method for fluidity of filling mortar" 14 The funnel flow time was measured. ·Pot life The mixed fast-hardening grout was placed in a 500mL container, and transferred to another 500mL container at regular intervals starting immediately after mixing. The pot life was determined as the time until the fast-hardening grout lost its fluidity (until the fast-hardening grout material stopped falling into the other 500mL container). Compressive strength The compressive strength of the grout hardened body was measured at 3 hours of age in accordance with the Japan Society of Civil Engineers standard JSCE-G 505-2018 "Method of compressive strength test for mortar or cement paste using cylindrical specimen (draft)". The dimensions of the specimen were 50 mm in diameter and 100 mm in height. The curing was done by moist curing at 5°C while still in the formwork.

[0048] [Table 1]

[0049] The fast-setting grouts of the examples had sufficient working life and showed good fluidity and strength development even in a low-temperature environment. On the other hand, the fast-setting grouts of the comparative examples did not have good working life or fluidity. In addition, the calcium aluminate with a hydrate coating amount of 5.0 mass% partially softened due to the progress of the hydration reaction, and could not be used as a grout material.

Claims

1. The composition includes a binder including cement, calcium aluminates, and gypsums, at least two types of alkali metal carbonates, a foaming agent, and a defoaming agent, the calcium aluminates include hydrate-coated calcium aluminates; the blowing agent is a peroxide material; the amount of the hydrate coated in the hydrate-coated calcium aluminates is 0.1 to 4.8% by mass based on the mass of the hydrate-coated calcium aluminates; The content of the foaming agent is 0.01 to 0.2 parts by mass relative to 100 parts by mass of the binder, The content of the defoaming agent is 0.003 to 0.2 parts by mass relative to 100 parts by mass of the binder, The total content of the alkali metal carbonate is 0.15 to 1.05 parts by mass per 100 parts by mass of the binder,

2. 2. The fast-setting grout composition according to claim 1, wherein the alkali metal carbonate is at least two selected from the group consisting of lithium carbonate, sodium carbonate, and potassium carbonate.

3. A fast-hardening grout composition as described in claim 1 or 2, wherein the cement is ordinary Portland cement and high-early-strength Portland cement.

4. The fast-hardening grout composition according to any one of claims 1 to 3, which is for use in low temperature environments.

5. The fast-hardening grout composition according to any one of claims 1 to 4 and water are included, The content of the water is 35 to 45 parts by mass per 100 parts by mass of the binder. Out.

Citation Information

Patent Citations

  • Ultra high speed hardening nonshrinkable grout material

    JP1999021160A

  • Quick-hardening material and quick-hardening cement composition

    JP2005060154A

  • Ultra rapid hardening cement admixture, ultra rapid hardening cement composition, ultra rapid hardening grout mortar and mortar hardened body obtained by using the same

    JP2005289656A

  • Hardening accelerator and quick-hardening cement composition

    JP2006182568A

  • Ultra-quick hardening / highly flowable cement composition, and mortar or concrete using same

    JP2007197268A