Olefin Polymerization Catalysts

A catalyst system using transition metal compounds with cyclopentadienyl ligands and Group 15 or 16 elements, supported by aluminoxane, addresses fouling and agglomeration issues in olefin polymerization, ensuring stable production of ultra-high molecular weight polyethylenes.

JP7558658B2Active Publication Date: 2024-10-01MITSUI CHEMICALS INC
View PDF 16 Cites 0 Cited by

Patent Information

Application Number
JP2020010632
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-01-25
Filing Date
2020-01-27
Publication Date
2024-10-01
Estimated Expiration
2040-01-27

AI Technical Summary

Technical Problem

Transition metal compounds with cyclopentadienyl ligands and Group 15 or 16 elements cause fouling during slurry polymerization, leading to agglomeration issues in ultra-high molecular weight polyethylene production.

Method used

A catalyst system comprising a transition metal compound with cyclopentadienyl ligands and a Group 15 or 16 element, combined with a solid aluminoxane support, prevents fouling by acting as an effective antistatic agent and carrier.

Benefits of technology

The catalyst system produces olefin polymers without fouling, maintaining stable particle size and preventing agglomeration, even for ultra-high molecular weight polyethylenes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007558658000001
    Figure 0007558658000001
  • Figure 0007558658000002
    Figure 0007558658000002
  • Figure 0007558658000003
    Figure 0007558658000003
Patent Text Reader

Abstract

To provide a catalyst for olefin polymerization capable of producing olefin (co)polymers without causing fouling or the like during polymerization.SOLUTION: There is provided a catalyst for olefin polymerization comprising a transition metal compound component represented by the general formula and a solid aluminoxane compound. In the formula, M is a Group 4 transition metal atom; n is 1 to 4; X is H, a halogen atom, a hydrocarbon group, or the like; Cp is an optionally substituted cyclopentadienyl type ligand; L is an atom selected from Group 15 and Group 16 of the periodic table; y is 2 when L is an atom of Group 15 element, and y is 3 when L is an atom of Group 16 element; and R's are each independently a hydrogen atom, a hydrocarbon group having 1 to 40 carbon atoms, and the like.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an olefin polymerization catalyst, and more particularly to an olefin polymerization catalyst capable of producing an olefin (co)polymer without causing fouling or the like during polymerization. [Background technology]

[0002] 2. Description of the Related Art Known catalysts for use in the production of olefin (co)polymers include olefin polymerization catalysts comprising a transition metal compound such as zirconocene and a cocatalyst component such as aluminoxane (organoaluminum oxy compound).

[0003] In particular, when slurry polymerization or gas phase polymerization is carried out, it is generally known to use a solid catalyst component in which a transition metal compound or an aluminoxane is supported on a solid carrier such as silica gel for the purpose of improving the powder properties of the polymer produced and preventing fouling (adhesion to the walls of the polymerization vessel) during polymerization (Non-Patent Document 1).

[0004] The solid support must be appropriately selected depending on the transition metal compound used and the production process, and since higher polymerization activity is required to reduce costs and reduce metal residues in the polymer, many methods for producing solid supports and solid catalyst components have been proposed (Patent Documents 1 to 5). [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2002-179721 A [Patent Document 2] JP 2003-327611 A [Patent Document 3] JP 2004-091498 A [Patent Document 4] JP 2009-001829 A [Patent Document 5] International Publication No. 2014 / 123212 [Patent Document 6] International Publication No. 2009 / 063084 [Patent Document 7] Special table 2016 / 534165 publication [Non-patent literature]

[0006] [Non-Patent Document 1] Chem.Rev.2005,105,pp.4073-4147 Summary of the Invention [Problem to be solved by the invention]

[0007] In particular, it has been disclosed that transition metal compounds having a cyclopentadienyl ligand and a ligand containing a Group 15 element (half metallocene) are suitable for producing ultra-high molecular weight polyethylene (UHMWPE) having an intrinsic viscosity ([η]) of more than 5 dl / g in decalin at 135°C (Patent Documents 6 and 7). However, the present inventors conducted research and discovered that transition metal compounds having a cyclopentadienyl ligand and a ligand containing an atom selected from Group 15 and Group 16 elements are more susceptible to fouling during slurry polymerization than transition metal compounds consisting only of cyclopentadienyl ligands.

[0008] Furthermore, unlike other common polyethylenes, the ultra-high molecular weight polyethylene (UHMWPE) is often used as a polymerized powder, and it is desirable for the powder to have a smaller particle size and be free of agglomerations. However, from the standpoint of fouling and powder agglomeration, the smaller the particle size, the more likely the above phenomena are to occur.

[0009] An object of the present invention is to provide an olefin polymerization catalyst which is capable of producing an olefin (co)polymer without causing fouling or the like during polymerization. [Means for solving the problem]

[0010] As a result of intensive research into solving the above problems, the present inventors have found that a solid catalyst component having a transition metal compound having a cyclopentadienyl ligand and a ligand containing a Group 15 or 16 element, and a solid aluminoxane compound as a solid support, is very effective in preventing fouling, and have thus completed the present invention. That is, the gist of the present invention is as follows. [1] A catalyst for olefin polymerization comprising the following component (A) and the following solid support (S): Component (A): A transition metal compound represented by the following general formula [1] or [2].

[0011] [ka]

[0012] [ka] (In the general formulas [1] and [2], M is a transition metal atom of Group 4 of the periodic table, n is an integer from 1 to 4 satisfying the valence of M; X is a hydrogen atom, a halogen atom, a hydrocarbon group, an anionic ligand, or a neutral ligand capable of coordinating with a lone electron pair, the anionic ligand being a halogen-containing group, a silicon-containing group, an oxygen-containing group, a sulfur-containing group, a nitrogen-containing group, a phosphorus-containing group, a boron-containing group, an aluminum-containing group, or a conjugated diene-based divalent derivative group, and when n is 2 or more, the multiple groups represented by X may be the same or different and may be bonded to each other to form a ring; Cp is a cyclopentadienyl ligand which may have a substituent, and adjacent substituents may be bonded to each other to form a ring which may have a substituent; L is an atom selected from the elements of Groups 15 and 16 of the Periodic Table; P is a phosphorus atom, The solid lines are covalent or coordinate bonds, and the dotted lines are covalent bonds that exist when L is a group 15 element atom. y is 2 when L is an atom of a group 15 element, and y is 3 when L is an atom of a group 16 element. z is 3 when L is an atom of a Group 15 element, and is 4 when L is an atom of a Group 16 element; Each R is independently a hydrogen atom, a hydrocarbon group having 1 to 40 carbon atoms, a halogen-containing group, a silicon-containing group, an oxygen-containing group, a nitrogen-containing group, or a sulfur-containing group, and may be the same or different. Adjacent R may be bonded to each other to form a ring or a bicyclo ring which may have a substituent. Solid support (S): A solid aluminoxane compound. [2] The olefin polymerization catalyst according to [1], wherein L is an atom of an element in Group 15 of the periodic table. [3] The olefin polymerization catalyst according to [1], wherein M is a titanium atom. [4] A method for producing an olefin polymer, comprising polymerizing an olefin in the presence of the olefin polymerization catalyst according to any one of [1] to [3]. Effect of the Invention

[0013] The olefin polymerization catalyst of the present invention can produce an olefin (co)polymer without causing fouling or the like during polymerization. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014] The olefin polymerization catalyst of the present invention comprises the following component (A) and a solid support (S): <Component (A)> Component (A) is a transition metal compound represented by the following general formula [1] or [2] (hereinafter, also referred to as transition metal compound (A)).

[0015] [ka]

[0016] [ka] In the above formulas [1] and [2], M is a transition metal atom of Group 4 of the periodic table, specifically a titanium atom, a zirconium atom or a hafnium atom, and preferably a titanium atom.

[0017] n is an integer of 1 to 4 satisfying the valence of M, and is preferably 1 or 2. X is a hydrogen atom, a halogen atom, a hydrocarbon group, an anionic ligand, or a neutral ligand capable of coordinating with a lone electron pair, and the anionic ligand is a halogen-containing group, a silicon-containing group, an oxygen-containing group, a sulfur-containing group, a nitrogen-containing group, a phosphorus-containing group, a boron-containing group, an aluminum-containing group, or a conjugated diene-based divalent derivative group. When n is 2 or more, the groups represented by X present in a plurality of groups may be the same or different, and may be bonded to each other to form a ring.

[0018] Cp is a cyclopentadienyl ligand which may have a substituent. Among the substituents, adjacent substituents may be bonded to each other to form a ring which may have a substituent.

[0019] L is an atom selected from the elements of Groups 15 and 16 of the periodic table. P is a phosphorus atom. The solid lines are covalent or coordinate bonds, and the dotted lines are covalent bonds that exist when L is a Group 15 element.

[0020] y is 2 when L is an atom of a Group 15 element, and y is 3 when L is an atom of a Group 16 element. z is 3 when L is an atom of a Group 15 element, and is 4 when L is an atom of a Group 16 element.

[0021] R are each independently a hydrogen atom, a hydrocarbon group having 1 to 40 carbon atoms, a halogen-containing group, a silicon-containing group, an oxygen-containing group, a nitrogen-containing group or a sulfur-containing group, and may be the same or different. Adjacent R may be bonded to each other to form a ring or a bicyclo ring which may have a substituent.

[0022] As described above, L is an atom selected from the group 15 and group 16 elements. Preferably, L is an atom of a group 15 element. In this case, y=2 and z=3. Below, we will introduce examples of component (A) in which L is an atom of an element in Group 15. Examples of such component (A) include compounds represented by the following formula [3] or [4].

[0023] [ka]

[0024] [ka] In the above formulas [3] and [4], M is a transition metal atom of Group 4 of the periodic table, specifically a titanium atom, a zirconium atom, or a hafnium atom, and preferably a titanium atom.

[0025] In the formulas [3] and [4], n is an integer of 1 to 4 that satisfies the valence of the transition metal M, and is preferably 1 or 2. In the formulas [3] and [4], X is a hydrogen atom, a halogen atom, a hydrocarbon group, an anionic ligand, or a neutral ligand capable of coordinating with a lone electron pair, and the anionic ligand is a halogen-containing group, a silicon-containing group, an oxygen-containing group, a sulfur-containing group, a nitrogen-containing group, a phosphorus-containing group, a boron-containing group, an aluminum-containing group, or a conjugated diene derivative group.

[0026] X is preferably a hydrogen atom, a halogen atom, a hydrocarbon group having 1 to 20 carbon atoms, a silicon-containing group, an oxygen-containing group, or a conjugated diene derivative group. When n is 2 or more, the multiple Xs may be the same or different and may be bonded to each other to form a ring. When multiple rings are present, the rings may be the same or different.

[0027] The halogen atom includes fluorine, chlorine, bromine, iodine, etc., and is preferably chlorine or bromine. Examples of the hydrocarbon group include: linear or branched alkyl groups such as methyl, ethyl, 1-propyl, 1-butyl, 1-pentyl, 1-hexyl, 1-heptyl, 1-octyl, isopropyl, sec-butyl (butan-2-yl), tert-butyl (2-methylpropan-2-yl), isobutyl (2-methylpropyl), pentan-2-yl, 2-methylbutyl, isopentyl (3-methylbutyl), neopentyl (2,2-dimethylpropyl), cyamyl (1,2-dimethylpropyl), isohexyl (4-methylpentyl), 2,2-dimethylbutyl, 2,3-dimethylbutyl, 3,3-dimethylbutyl, thexyl (2,3-dimethylbut-2-yl), 4,4-dimethylpentyl; Vinyl group, allyl group, propenyl group (prop-1-en-1-yl group), iso-propenyl group (prop-1-en-2-yl group), allenyl group (prop-1,2-dien-1-yl group), but-3-en-1-yl group, crotyl group (but-2-en-1-yl group), but-3-en-2-yl group, methallyl group (2-methylallyl group), buta-1,3-dienyl group, pentaerythritol group, linear or branched alkenyl groups or unsaturated double bond-containing groups, such as ter-4-en-1-yl group, pent-3-en-1-yl group, pent-2-en-1-yl group, iso-pentenyl group (3-methylbut-3-en-1-yl group), 2-methylbut-3-en-1-yl group, pent-4-en-2-yl group, and prenyl group (3-methylbut-2-en-1-yl group); linear or branched alkynyl groups or unsaturated triple bond-containing groups, such as ethynyl, prop-2-yn-1-yl, and propargyl (prop-1-yn-1-yl); aromatic linear or branched alkyl groups and unsaturated double bond-containing groups, such as benzyl, 2-methylbenzyl, 4-methylbenzyl, 2,4,6-trimethylbenzyl, 3,5-dimethylbenzyl, cuminyl (4-isopropylbenzyl), 2,4,6-tri-isopropylbenzyl, 4-tert-butylbenzyl, 3,5-di-tert-butylbenzyl, 1-phenylethyl, and benzhydryl (diphenylmethyl); cyclic saturated hydrocarbon groups such as a cyclopropyl group, a cyclobutyl group, a cyclopentyl group, a cyclohexyl group, a cycloheptyl group, a cycloheptatrienyl group, a norbornyl group, a norbornenyl group, a 1-adamantyl group, and a 2-adamantyl group; Aromatic substituents such as phenyl, tolyl (methylphenyl), xylyl (dimethylphenyl), mesityl (2,4,6-trimethylphenyl), cumenyl (isopropylphenyl), julyl (2,3,5,6-tetramethylphenyl), 2,6-di-isopropylphenyl, 2,4,6-tri-isopropylphenyl, 4-tert-butylphenyl, 3,5-di-tert-butylphenyl, naphthyl, biphenyl, terphenyl, binaphthyl, acenaphthalenyl, phenanthryl, anthracenyl, pyrenyl, and ferrocenyl. Examples include:

[0028] Among the above hydrocarbon groups, a methyl group, an iso-butyl group, a neopentyl group, a cyamyl group, a benzyl group, a phenyl group, a tolyl group, a xylyl group, a mesityl group, and a cumenyl group are preferred.

[0029] Examples of the halogen-containing group include a fluoromethyl group, a trifluoromethyl group, a trichloromethyl group, a pentafluoroethyl group, a 2,2,2-trifluoroethyl group, a fluorophenyl group, a difluorophenyl group, a trifluorophenyl group, a tetrafluorophenyl group, a pentafluorophenyl group, a trifluoromethylphenyl group, a bistrifluoromethylphenyl group, and a hexachloroantimonate anion. Among the above halogen-containing groups, a pentafluorophenyl group is preferred.

[0030] Examples of the silicon-containing group include a trimethylsilyl group, a triethylsilyl group, a tri-iso-propylsilyl group, a diphenylmethylsilyl group, a tert-butyldimethylsilyl group, a tert-butyldiphenylsilyl group, a triphenylsilyl group, a tris(trimethylsilyl)silyl group, and a trimethylsilylmethyl group. Among the above silicon-containing groups, a trimethylsilylmethyl group is preferred.

[0031] Examples of the oxygen-containing group include a methoxy group, an ethoxy group, an n-propoxy group, an isopropoxy group, an allyloxy group, an n-butoxy group, a sec-butoxy group, an isobutoxy group, a tert-butoxy group, a benzyloxy group, a methoxymethoxy group, a phenoxy group, a 2,6-dimethylphenoxy group, a 2,6-di-isopropylphenoxy group, a 2,6-di-tert-butylphenoxy group, a 2,4,6-trimethylphenoxy group, a 2,4,6-tri-isopropylphenoxy group, an acetoxy group, a pivaloyloxy group, a benzoyloxy group, a trifluoroacetoxy group, a perchlorate anion, and a periodate anion. Among the oxygen-containing groups, a methoxy group, an ethoxy group, an iso-propoxy group, and a tert-butoxy group are preferred.

[0032] Examples of the sulfur-containing group include a mesyl group (methanesulfonyl group), a phenylsulfonyl group, a tosyl group (p-toluenesulfonyl group), a triflyl group (trifluoromethanesulfonyl group), a nonaflyl group (nonafluorobutanesulfonyl group), a mesylate group (methanesulfonate group), a tosylate group (p-toluenesulfonate group), a triflate group (trifluoromethanesulfonate group), and a nonaflate group (nonafluorobutanesulfonate group). Of the above sulfur-containing groups, triflate (trifluoromethanesulfonate) is preferred.

[0033] Examples of the nitrogen-containing group include an amino group, a cyano group, a methylamino group, a dimethylamino group, an ethylamino group, a diethylamino group, an allylamino group, a diallylamino group, a benzylamino group, a dibenzylamino group, a pyrrolidinyl group, a piperidinyl group, a morpholyl group, a pyrrolyl group, and a bistriflyl imide group. Among the nitrogen-containing groups, a dimethylamino group, a diethylamino group, a pyrrolidinyl group, a pyrrolyl group, and a bistriflylimide group are preferred.

[0034] The phosphorus-containing group may, for example, be a hexafluorophosphate anion. Examples of the boron-containing group include tetrafluoroborate anion, tetrakis(pentafluorophenyl)borate anion, (methyl)(tris(pentafluorophenyl))borate anion, (benzyl)(tris(pentafluorophenyl))borate anion, tetrakis((3,5-bistrifluoromethyl)phenyl)borate anion, and groups represented by BR4 (each R independently represents hydrogen, an alkyl group, an aryl group which may have a substituent, a halogen atom, or the like).

[0035] Examples of the aluminum-containing group include

[0036] [ka] or

[0037] [ka] A four-membered ring represented by (M represents M in the general formula [3] or [4].) Examples of the group include a group represented by AlR4 (R represents hydrogen, an alkyl group, an aryl group which may have a substituent, a halogen atom, or the like) which can form the following formula:

[0038] Examples of the conjugated diene derivative group include a 1,3-butadienyl group, an isoprenyl group (2-methyl-1,3-butadienyl group), a piperylenyl group (1,3-pentadienyl group), a 2,4-hexadienyl group, a 1,4-diphenyl-1,3-pentadienyl group, a cyclopentadienyl group, and a metallocyclopentene group.

[0039] Examples of neutral ligands capable of coordinating with lone electron pairs include ethers such as diethyl ether, tetrahydrofuran, dioxane, and 1,2-dimethoxyethane; amines such as triethylamine and diethylamine; heterocyclic compounds such as pyridine, picoline, lutidine, oxazoline, oxazole, thiazole, imidazole, and thiophene; and organic phosphorus compounds such as triphenylphosphine, tricyclohexylphosphine, and tri-tert-butylphosphine.

[0040] In the formulas [3] and [4], Cp is a cyclopentadienyl ligand which may have a substituent, and the substituent may be bonded to another adjacent substituent to form a ring which may have a substituent. The cyclopentadienyl-type ligand is a substituted ligand having a five-membered carbon ring bonded to a metal by a π-type bond, and includes substituted cyclopentadienyl-type ligands such as substituted cyclopentadienyl ligands, substituted tetrahydroindenyl ligands, substituted octahydrofluorenyl ligands, substituted hydroazulenyl ligands, substituted pentahydroazulenyl ligands, substituted dihydrocyclopentenoannulene ligands, substituted cyclopentenopyrrole ligands, substituted cyclopentenothiophene ligands, and substituted cyclopentenodithiophene ligands, substituted indenyl-type ligands such as substituted indenyl ligands, substituted tetrahydroindenyl ligands, substituted benzoindenyl ligands, substituted dihydroindacenyl ligands, substituted indenopyrrole ligands, substituted indenoindole ligands, and substituted indenothiophenes, and substituted fluorenyl ligands. As the cyclopentadienyl type ligand, a substituted cyclopentadienyl type ligand and a substituted indenyl type ligand are preferred, and a substituted cyclopentadienyl ligand, a substituted dihydrocyclopentenoannulene ligand, a substituted cyclopentenothiophene ligand, a substituted cyclopentenodithiophene ligand, and a substituted indenyl ligand are more preferred.

[0041] In the formulas [3] and [4], N is a nitrogen atom, and in the formula [4], P is a phosphorus atom. R in the above formula [3] 1 and R 2 , R in Equation [4] 1 ~R 3 and the substituents of the cyclopentadienyl ligand are each independently a hydrogen atom, a hydrocarbon group having 1 to 40 carbon atoms, a halogen-containing group, a silicon-containing group, an oxygen-containing group, a nitrogen-containing group, or a sulfur-containing group. 1 ~R 3is preferably a hydrocarbon group having 1 to 20 carbon atoms, an oxygen-containing group having 1 to 20 carbon atoms, or a nitrogen-containing group having 1 to 20 carbon atoms, and more preferably a hydrocarbon group having 1 to 20 carbon atoms, or a nitrogen-containing group having 1 to 20 carbon atoms. 1 ~R 3 may be the same or different.

[0042] The hydrocarbon group having 1 to 40 carbon atoms includes a hydrocarbon group having 1 to 20 carbon atoms, and more specific examples include the specific examples of the hydrocarbon groups given as the examples of X above.

[0043] The hydrocarbon group having 1 to 40 carbon atoms is preferably a hydrocarbon group having 1 to 20 carbon atoms (excluding aromatic hydrocarbon groups) or an aromatic hydrocarbon group having 6 to 40 carbon atoms. The hydrocarbon group having 1 to 20 carbon atoms is preferably an aliphatic or alicyclic hydrocarbon group having 1 to 20 carbon atoms. The hydrocarbon group having 1 to 20 carbon atoms also includes a substituent having an aromatic structure such as an arylalkyl group.

[0044] Examples of the hydrocarbon group having 1 to 40 carbon atoms include Methyl, ethyl, 1-propyl, 1-butyl, 1-pentyl, 1-hexyl, 1-heptyl, 1-octyl, 1-nonyl, 1-decanyl, 1-undecanyl, 1-dodecanyl, 1-eicosanyl, isopropyl, sec-butyl, tert-butyl, isobutyl, pentan-2-yl, 2-methylbutyl, isopentyl, neopentyl, tert-pentyl (1,1-dimethylpropyl), cyamyl, pentan-3-yl, 2-methylpentyl, 3-methylpentyl, isohexyl, 1,1-dimethylbutyl (2-methylpentan-2-yl), 3-methylpentane linear or branched alkyl groups having 1 to 40 carbon atoms, such as 2-methylpentan-2-yl, 4-methylpentan-2-yl, 2,2-dimethylbutyl, 2,3-dimethylbutyl, 3,3-dimethylbutyl, thexyl, 3-methylpentan-3-yl, 3,3-dimethylbut-2-yl, hexane-3-yl, 2-methylpentan-3-yl, heptan-4-yl, 2,4-dimethylpentan-2-yl, 3-ethylpentan-3-yl, 4,4-dimethylpentyl, 4-methylheptan-4-yl, 4-propylheptan-4-yl, 2,3,3-trimethylbutan-2-yl, and 2,4,4-trimethylpentan-2-yl; Vinyl, allyl, propenyl, isopropenyl, allenyl, but-3-en-1-yl, crotyl, but-3-en-2-yl, methallyl, but-1,3-dienyl, pent-4-en-1-yl, pent-3-en-1-yl, pent-2-en-1-yl, isopentenyl, 2-methylbut-3-en-1-yl, pent-4-en-2-yl, prenyl, 2-methyl-but-2-en-1 -yl group, pent-3-en-2-yl group, 2-methyl-but-3-en-2-yl group, pent-1-en-3-yl group, penta-2,4-dien-1-yl group, penta-1,3-dien-1-yl group, penta-1,4-dien-3-yl group, iso-prenyl group (2-methyl-but-1,3-dien-1-yl group), penta-2,4-dien-2-yl group, hex-5-en-1-yl group, hex-4-en-1-yl group, hex-3-en -1-yl group, hex-2-en-1-yl group, 4-methyl-pent-4-en-1-yl group, 3-methyl-pent-4-en-1-yl group, 2-methyl-pent-4-en-1-yl group, hex-5-en-2-yl group, 4-methyl-pent-3-en-1-yl group, 3-methyl-pent-3-en-1-yl group, 2,3-dimethyl-but-2-en-1-yl group, 2-methylpent-4-en-2-yl group, 3-ethyl-pent-1-en- linear or branched alkenyl groups or unsaturated double bond-containing groups having 2 to 40 carbon atoms, such as a 3-yl group, a hexa-3,5-dien-1-yl group, a hexa-2,4-dien-1-yl group, a 4-methylpenta-1,3-dien-1-yl group, a 2,3-dimethyl-buta-1,3-dien-1-yl group, a hexa-1,3,5-trien-1-yl group, a 2-(cyclopentadienyl)propan-2-yl group, or a 2-(cyclopentadienyl)ethyl group; Ethynyl group, prop-2-yn-1-yl group, propargyl group, but-1-yn-1-yl group, but-2-yn-1-yl group, but-3-yn-1-yl group, pent-1-yn-1-yl group, pent-2-yn-1-yl group, pent-3-yn-1-yl group, pent-4-yn-1-yl group, 3-methyl-but-1-yn-1-yl group, pent-3-yn-2-yl group, 2-methyl-but-3-yn-1-yl group, linear or branched alkynyl groups or unsaturated triple bond-containing groups having 2 to 40 carbon atoms, such as but-1-yn-yl, pent-4-yn-2-yl, hex-1-yn-1-yl, 3,3-dimethyl-but-1-yn-1-yl, 2-methyl-pent-3-yn-2-yl, 2,2-dimethyl-but-3-yn-1-yl, hex-4-yn-1-yl, and hex-5-yn-1-yl; Benzyl group, 2-methylbenzyl group, 4-methylbenzyl group, 2,4,6-trimethylbenzyl group, 3,5-dimethylbenzyl group, cuminyl group, 2,4,6-tri-iso-propylbenzyl group, 4-tert-butylbenzyl group, 3,5-di-tert-butylbenzyl group, 1-phenylethyl group, benzhydryl group, cumyl group (2-phenylpropan-2-yl group), 2-(4-methylphenyl)propan-2-yl group, 2-(3,5-dimethylphenyl)propan-2-yl group, 2-(4-tert-butylphenyl)propan-2-yl group, 2-(3,5-di-tert-butylphenyl)propan-2-yl group, 3-phenylpentan-3-yl group, 4-phenylhepta-1, 6-dien-4-yl, 1,2,3-triphenylpropan-2-yl, 1,1-diphenylethyl, 1,1-diphenylpropyl, 1,1-diphenyl-but-3-en-1-yl, 1,1,2-triphenylethyl, trityl (triphenylmethyl), tri-(4-methylphenyl)methyl, 2-phenylethyl, styryl (2-phenylvinyl), 2-(2-methylphenyl)ethyl, 2-(4-methylphenyl)ethyl, 2-(2,4,6-trimethylphenyl)ethyl, 2-(3,5-dimethylphenyl)ethyl, 2-(2,4,6-tri-isopropylphenyl)ethyl, 2-(4-tert-butylphenyl)ethyl, 2-(3,5-di-tert-butylphenyl)ethyl group, 2-methyl-1-phenylpropan-2-yl group, 3-phenylpropyl group, cinnamyl group (3-phenylallyl group), neophyl group (2-methyl-2-phenylpropyl group), 3-methyl-3-phenylbutyl group, 2-methyl-4-phenylbutan-2-yl group, cyclopentadienyldiphenylmethyl group, 2-(1-indenyl)propan-2-yl group, (1-indenyl)diphenylmethyl group, 2-(1-indenyl)ethyl group, 2-(tetrahydro-1-indacenyl)propan-2-yl group, (tetrahydro-1-indacenyl ) Aromatic-containing linear or branched alkyl groups and unsaturated double bond-containing groups having 7 to 40 carbon atoms, such as diphenylmethyl group, 2-(tetrahydro-1-indacenyl)ethyl group, 2-(1-benzoindenyl)propan-2-yl group, (1-benzoindenyl)diphenylmethyl group, 2-(1-benzoindenyl)ethyl group, 2-(9-fluorenyl)propan-2-yl group, (9-fluorenyl)diphenylmethyl group, 2-(9-fluorenyl)ethyl group, 2-(1-azulenyl)propan-2-yl group, (1-azulenyl)diphenylmethyl group, and 2-(1-azulenyl)ethyl group; Cyclopropyl, cyclobutyl, cyclopentyl, cyclopentenyl, cyclopentadienyl, dimethylcyclopentadienyl, n-butylcyclopentadienyl, n-butyl-methylcyclopentadienyl, tetramethylcyclopentadienyl, 1-methylcyclopentyl, 1-allylcyclopentyl, 1-benzylcyclopentyl, cyclohexyl, cyclohexenyl, cyclohexadienyl, 1-methylcyclohexyl group, 1-allylcyclohexyl group, 1-benzylcyclohexyl group, cycloheptyl group, cycloheptenyl group, cycloheptatrienyl group, 1-methylcycloheptyl group, 1-allylcycloheptyl group, 1-benzylcycloheptyl group, cyclooctyl group, cyclooctenyl group, cyclooctadienyl group, cyclooctatrienyl group, 1-methylcyclooctyl group, cyclododecyl group, 1-allylcyclooctyl group, 1-benzylcyclooctyl group, 4-cyclo Hexyl-tert-butyl, norbornyl, norbornenyl, norbornadienyl, 2-methylbicyclo[2.2.1]heptan-2-yl, 7-methylbicyclo[2.2.1]heptan-7-yl, bicyclo[2.2.2]octan-1-yl, bicyclo[2.2.2]octan-2-yl, 1-adamantyl, 2-adamantyl, 1-(2-methyladamantyl), 1-(3-methyladamantyl), 1-(4-methyladamantyl) ), 1-(2-phenyladamantyl), 1-(3-phenyladamantyl), 1-(4-phenyladamantyl), 1-(3,5-dimethyladamantyl), 1-(3,5,7-trimethyladamantyl), 1-(3,5,7-triphenyladamantyl), pentalenyl group, indenyl group, fluorenyl group, indacenyl group, tetrahydroindacenyl group, benzoindenyl group, azulenyl group, and other cyclic saturated and unsaturated hydrocarbon groups having 3 to 40 carbon atoms; Aromatic substituents having 6 to 40 carbon atoms, such as phenyl, tolyl, xylyl, mesityl, cumenyl, duryl, 2,6-di-isopropylphenyl, 2,4,6-tri-isopropylphenyl, 4-tert-butylphenyl, 3,5-di-tert-butylphenyl, allylphenyl, (but-3-en-1-yl)phenyl, (but-2-en-1-yl)phenyl, methallylphenyl, prenylphenyl, 4-adamantylphenyl, 3,5-di-adamantylphenyl, naphthyl, biphenyl, terphenyl, binaphthyl, acenaphthalenyl, phenanthryl, anthracenyl, pyrenyl, and ferrocenyl groups. etc.

[0045] Among the linear or branched alkyl groups having 1 to 40 carbon atoms, a methyl group, an ethyl group, a 1-propyl group, a 1-butyl group, a 1-pentyl group, a 1-hexyl group, a 1-heptyl group, a 1-octyl group, an isopropyl group, a sec-butyl group, a tert-butyl group, an isobutyl group, an isopentyl group, a neopentyl group, a tert-pentyl group, a pentan-3-yl group, an isohexyl group, a 1,1-dimethylbutyl group, a 3,3-dimethylbutyl group, a thexyl group, a 3-methylpentan-3-yl group, a heptane-4-yl group, Preferred are methyl, ethyl, 1-propyl, 1-butyl, 1-pentyl, 1-hexyl, isopropyl, tert-butyl, neopentyl, 2,4-dimethylpentan-2-yl, and 2,4,4-trimethylpentan-2-yl groups.

[0046] Among the linear or branched alkenyl groups or unsaturated double bond-containing groups having 2 to 40 carbon atoms, a vinyl group, an allyl group, a but-3-en-1-yl group, a crotyl group, a methallyl group, a pent-4-en-1-yl group, a prenyl group, a penta-1,4-dien-3-yl group, a hex-5-en-1-yl group, a 2-methylpent-4-en-2-yl group, a 2-(cyclopentadienyl)propan-2-yl group, a 2-(cyclopentadienyl)ethyl group, and the like are preferred, and a vinyl group, an allyl group, a but-3-en-1-yl group, a pent-4-en-1-yl group, a prenyl group, and a hex-5-en-1-yl group are more preferred.

[0047] Among the linear or branched alkynyl groups or unsaturated triple bond-containing groups having 2 to 40 carbon atoms, an ethynyl group, a propargyl group, a but-2-yn-1-yl group, a but-3-yn-1-yl group, a penta-3-yn-1-yl group, a penta-4-yn-1-yl group, a 3-methyl-but-1-yn-1-yl group, a 3,3-dimethyl-but-1-yn-1-yl group, a hex-4-yn-1-yl group, a hex-5-yn-1-yl group, and the like are preferred, with a propa-2-yn-1-yl group, a propargyl group, a but-2-yn-1-yl group, and a but-3-yn-1-yl group being more preferred.

[0048] Among the aromatic linear or branched alkyl groups and unsaturated double bond-containing groups having 7 to 40 carbon atoms, benzyl group, 2-methylbenzyl group, 4-methylbenzyl group, 2,4,6-trimethylbenzyl group, 3,5-dimethylbenzyl group, cuminyl group, 2,4,6-tri-iso-propylbenzyl group, 4-tert-butylbenzyl group, 3,5-di-tert-butylbenzyl group, benzhydryl group, cumyl group, 1,1-diphenylethyl group, trityl group, 2-phenylethyl group, 2-(4-methylphenyl)ethyl group, 2-(2,4,6-trimethylphenyl)ethyl group, 2-(3,5-dimethylphenyl)ethyl group, 2-(2,4,6-tri-iso-propylphenyl)ethyl group, 2-(4-tert-butyl ... Preferred are a 2-(3,5-di-tert-butylphenyl)ethyl group, a 2-(3,5-di-tert-butylphenyl)ethyl group, a styryl group, a 2-methyl-1-phenylpropan-2-yl group, a 3-phenylpropyl group, a cinnamyl group, a neophyl group, a cyclopentadienyldiphenylmethyl group, a 2-(1-indenyl)propan-2-yl group, a (1-indenyl)diphenylmethyl group, a 2-(1-indenyl)ethyl group, a 2-(9-fluorenyl)propan-2-yl group, a (9-fluorenyl)diphenylmethyl group, a 2-(9-fluorenyl)ethyl group, and the like, and more preferred are a benzyl group, a benzhydryl group, a cumyl group, a 1,1-diphenylethyl group, a trityl group, a 2-phenylethyl group, a 3-phenylpropyl group, and a cinnamyl group.

[0049] Among the above-mentioned cyclic saturated and unsaturated hydrocarbon groups having 3 to 40 carbon atoms, a cyclopropyl group, a cyclobutyl group, a cyclopentyl group, a cyclopentenyl group, a cyclopentadienyl group, a 1-methylcyclopentyl group, a 1-allylcyclopentyl group, a 1-benzylcyclopentyl group, a cyclohexyl group, a cyclohexenyl group, a 1-methylcyclohexyl group, a 1-allylcyclohexyl group, a 1-benzylcyclohexyl group, a cycloheptyl group, a cycloheptenyl group, a cycloheptatrienyl group, a 1-methylcycloheptyl group, a 1-allylcycloheptyl group, a 1-benzylcycloheptyl group, a cycloo Preferred are octyl, cyclooctenyl, cyclooctadienyl, cyclododecyl, 4-cyclohexyl-tert-butyl, norbornyl, 2-methylbicyclo[2.2.1]heptan-2-yl, bicyclo[2.2.2]octan-1-yl, 1-adamantyl, 2-adamantyl, pentalenyl, indenyl, and fluorenyl groups, and more preferred are cyclopentyl, cyclopentenyl, 1-methylcyclopentyl, cyclohexyl, cyclohexenyl, 1-methylcyclohexyl, cyclooctyl, cyclododecyl, and 1-adamantyl groups.

[0050] Among the aromatic substituents having 6 to 40 carbon atoms, a phenyl group, a tolyl group, a xylyl group, a mesityl group, a cumenyl group, a 2,6-di-isopropylphenyl group, a 2,4,6-tri-isopropylphenyl group, a 4-tert-butylphenyl group, a 3,5-di-tert-butylphenyl group, an allylphenyl group, a prenylphenyl group, a 4-adamantylphenyl group, a naphthyl group, a biphenyl group, a terphenyl group, a binaphthyl group, and a phenanthryl group are preferred. , anthracenyl group, ferrocenyl group, etc. are preferred, and a phenyl group, a tolyl group, a xylyl group, a mesityl group, a cumenyl group, a 2,6-di-isopropylphenyl group, a 2,4,6-tri-isopropylphenyl group, a 4-tert-butylphenyl group, a 3,5-di-tert-butylphenyl group, an allylphenyl group, a 4-adamantylphenyl group, a naphthyl group, a biphenyl group, a binaphthyl group, a phenanthryl group, and an anthracenyl group are more preferred.

[0051] Examples of the halogen-containing group include a fluoromethyl group, a trifluoromethyl group, a trichloromethyl group, a pentafluoroethyl group, a 2,2,2-trifluoroethyl group, a heptafluoropropyl group, a 3,3,3-trifluoropropyl group, a nonafluorobutyl group, a 4,4,4-trifluorobutyl group, a dodecafluorohexyl group, a 6,6,6-trifluorohexyl group, a chlorophenyl group, a fluorophenyl group, a difluorophenyl group, a trifluorophenyl group, a tetrafluorophenyl group, a pentafluorophenyl group, a pentafluorophenylmethyl group, a di-tert-butyl-fluorophenyl group, a trifluoromethylphenyl group, a bistrifluoromethylphenyl group, a trifluoromethoxyphenyl group, a bistrifluoromethoxyphenyl group, a trifluoromethylthiophenyl group, a bistrifluoromethylthiophenyl group, a fluorobiphenyl group, a difluoromethylphenyl group, a fluoromethylthio ... Examples of such a group include a fluorobiphenyl group, a trifluorobiphenyl group, a tetrafluorobiphenyl group, a pentafluorobiphenyl group, a di-tert-butyl-fluorobiphenyl group, a trifluoromethylbiphenyl group, a bistrifluoromethylbiphenyl group, a trifluoromethoxybiphenyl group, a bistrifluoromethoxybiphenyl group, a trifluoromethyldimethylsilyl group, a trifluoromethoxy group, a pentafluoroethoxy group, a fluorophenoxy group, a difluorophenoxy group, a trifluorophenoxy group, a pentafluorophenoxy group, a di-tert-butyl-fluorophenoxy group, a trifluoromethylphenoxy group, a bistrifluoromethylphenoxy group, a trifluoromethoxyphenoxy group, a bistrifluoromethoxyphenoxy group, a difluoromethylenedioxyphenyl group, a bistrifluoromethylphenyliminomethyl group, and a trifluoromethylthio group.

[0052] Among the halogen-containing groups, a fluoromethyl group, a trifluoromethyl group, a pentafluoroethyl group, a 2,2,2-trifluoroethyl group, a 3,3,3-trifluoropropyl group, a 4,4,4-trifluorobutyl group, a fluorophenyl group, a difluorophenyl group, a trifluorophenyl group, a tetrafluorophenyl group, a pentafluorophenyl group, a pentafluorophenylmethyl group, a trifluoromethylphenyl group, a bistrifluoromethylphenyl group, a trifluoromethoxyphenyl group, a pentafluorobiphenyl group, a trifluoromethylbiphenyl group, a bistrifluoromethylbiphenyl group, a trifluoromethoxy group, a pentafluorophenoxy group, a bistrifluoromethylphenoxy group, a bistrifluoromethylphenoxy group, a difluoromethylenedioxyphenyl group, and a trifluoromethylthio group are preferred, and a trifluoromethyl group, a fluorophenyl group, a difluorophenyl group, a pentafluorophenyl group, a pentafluorophenylmethyl group, a trifluoromethylphenyl group, a bistrifluoromethylphenyl group, a pentafluorobiphenyl group, a trifluoromethoxy group, and a pentafluorophenoxy group are more preferred.

[0053] Examples of the silicon-containing group include a trimethylsilyl group, a triethylsilyl group, a tri-isopropylsilyl group, a diphenylmethylsilyl group, a tert-butyldimethylsilyl group, a tert-butyldiphenylsilyl group, a triphenylsilyl group, a tris(trimethylsilyl)silyl group, a cyclopentadienyldimethylsilyl group, a di-n-butyl(cyclopentadienyl)silyl group, a cyclopentadienyldiphenylsilyl group, an indenyldimethylsilyl group, a di-n-butyl(indenyl)silyl group, )silyl group, indenyldiphenylsilyl group, fluorenyldimethylsilyl group, di-n-butyl(fluorenyl)silyl group, fluorenyldiphenylsilyl group, 4-trimethylsilylphenyl group, 4-triethylsilylphenyl group, 4-tri-iso-propylsilylphenyl group, 4-tert-butyldiphenylsilylphenyl group, 4-triphenylsilylphenyl group, 4-tris(trimethylsilyl)silylphenyl group, and 3,5-bis(trimethylsilyl)phenyl group.

[0054] Among the silicon-containing groups, a trimethylsilyl group, a triethylsilyl group, a tri-iso-propylsilyl group, a tert-butyldimethylsilyl group, a triphenylsilyl group, a cyclopentadienyldimethylsilyl group, a cyclopentadienyldiphenylsilyl group, an indenyldimethylsilyl group, an indenyldiphenylsilyl group, a fluorenyldimethylsilyl group, a fluorenyldiphenylsilyl group, a 4-trimethylsilylphenyl group, a 4-triethylsilylphenyl group, a 4-tri-iso-propylsilylphenyl group, a 4-triphenylsilylphenyl group, a 3,5-bis(trimethylsilyl)phenyl group, and the like are preferred, and a trimethylsilyl group, a triethylsilyl group, a tert-butyldimethylsilyl group, a 4-trimethylsilylphenyl group, a 4-triethylsilylphenyl group, a 4-tri-iso-propylsilylphenyl group, and a 3,5-bis(trimethylsilyl)phenyl group are more preferred.

[0055] The oxygen-containing group is preferably an oxygen-containing group having 1 to 20 carbon atoms, and examples thereof include a methoxy group, an ethoxy group, an n-propoxy group, an isopropoxy group, an allyloxy group, an n-butoxy group, a sec-butoxy group, an isobutoxy group, a tert-butoxy group, a methallyloxy group, a prenyloxy group, a benzyloxy group, a methoxymethoxy group, a methoxyethoxy group, a phenoxy group, a naphthoxy group, a toluyloxy group, an isopropylphenoxy group, an allylphenoxy group, a tert-butylphenoxy group, a methoxyphenoxy group, an isopropoxyphenoxy group, an allyloxyphenoxy group, a biphenyloxy group, a binaphthyloxy group, a methoxymethyl group, an allyloxymethyl group, a benzyloxymethyl group, a phenoxymethyl group, a methoxyethyl group, an allyloxyethyl group, a benzyloxyethyl group, a phenoxyethyl group, a methallyloxy group, a methoxymethyl group, a methoxyethyl ... Examples of such groups include an aryloxypropyl group, an allyloxypropyl group, a benzyloxypropyl group, a phenoxypropyl group, a methoxyvinyl group, an allyloxyvinyl group, a benzyloxyvinyl group, a phenoxyvinyl group, a methoxyallyl group, an allyloxyallyl group, a benzyloxyallyl group, a phenoxyallyl group, a dimethoxymethyl group, a di-iso-propoxymethyl group, a dioxolanyl group, a tetramethyldioxolanyl group, a dioxanyl group, a methoxyphenyl group, an iso-propoxyphenyl group, an allyloxyphenyl group, a phenoxyphenyl group, a methylenedioxyphenyl group, a 3,5-dimethyl-4-methoxyphenyl group, a 3,5-di-tert-butyl-4-methoxyphenyl group, a furyl group, a methylfuryl group, a tetrahydrofuryl group, a pyranyl group, a tetrahydropyranyl group, a furofuryl group, a benzofuryl group, and a dibenzofuryl group.

[0056] Among the oxygen-containing groups, a methoxy group, an ethoxy group, an isopropoxy group, an allyloxy group, an n-butoxy group, a tert-butoxy group, a prenyloxy group, a benzyloxy group, a phenoxy group, a naphthoxy group, a toluyloxy group, an isopropylphenoxy group, an allylphenoxy group, a tert-butylphenoxy group, a methoxyphenoxy group, a biphenyloxy group, a binaphthyloxy group, an allyloxymethyl group, a benzyloxymethyl group, a phenoxymethyl group, a methoxyethyl group, a methoxyallyl group, a benzyloxyallyl group, a phenoxyallyl group, a dimethoxymethyl group, a dioxolanyl group, a tetramethyldioxolanyl group, a dioxanyl group, a dimethyldioxanyl group, a methoxyphenyl group, an isopropoxyphenyl group, an allyloxymethyl group, a Preferred are a diphenyl group, a phenoxyphenyl group, a methylenedioxyphenyl group, a 3,5-dimethyl-4-methoxyphenyl group, a 3,5-di-tert-butyl-4-methoxyphenyl group, a furyl group, a methylfuryl group, a tetrahydropyranyl group, a furyl group, a benzofuryl group, a dibenzofuryl group, and the like, and more preferred are a methoxy group, an isopropoxy group, a tert-butoxy group, an allyloxy group, a phenoxy group, a dimethoxymethyl group, a dioxolanyl group, a methoxyphenyl group, an isopropoxyphenyl group, an allyloxyphenyl group, a phenoxyphenyl group, a 3,5-dimethyl-4-methoxyphenyl group, a 3,5-di-tert-butyl-4-methoxyphenyl group, a furyl group, a methylfuryl group, a benzofuryl group, and a dibenzofuryl group.

[0057] The nitrogen-containing group is preferably a nitrogen-containing group having 1 to 20 carbon atoms, and examples thereof include an amino group, a dimethylamino group, a diethylamino group, a di-n-propylamino group, a di-iso-propylamino group, a di-n-butylamino group, a di-iso-butylamino group, a dicyclopentylamino group, a dicyclohexylamino group, an allylamino group, a diallylamino group, a didecylamino group, a benzylamino group, a dibenzylamino group, a pyrrolidinyl group, a piperidinyl group, a morpholyl group, an azepinyl group, an adamantylamino group, a dimethylaminomethyl group, a dibenzylaminomethyl group, a pyrrolidinylmethyl group, a dimethylaminoethyl group, a benzylaminomethyl group, a benzylaminoethyl group, a pyrrolidinylethyl group, a dimethylaminovinyl group, a benzylaminovinyl group, a pyrrolidinylvinyl group, a dimethylaminopropyl group, a benzylaminopropyl group, a pyrrolidinylpropyl group, a dimethylaminoallyl group, a benzylaminoallyl group, a pyrrolidinylallyl group, an aminophenyl group, a phenyl ... phenyl group, dimethylaminophenyl group, 3,5-dimethyl-4-dimethylaminophenyl group, 3,5-di-isopropyl-4-dimethylaminophenyl group, julolidinyl group, tetramethyljulolidinyl group, pyrrolidinylphenyl group, piperidinylphenyl group, morpholylphenyl group, pyrrolylphenyl group, pyridylphenyl group, quinolylphenyl group, isoquinolylphenyl group, indolinylphenyl group, indolylphenyl group, carbazolylphenyl group, Examples of such groups include a di-tert-butylcarbazolylphenyl group, a pyrrolyl group, a methylpyrrolyl group, a phenylpyrrolyl group, a pyridyl group, a quinolyl group, a tetrahydroquinolyl group, an iso-quinolyl group, a tetrahydro-iso-quinolyl group, an indolyl group, an indolinyl group, a carbazolyl group, a di-tert-butylcarbazolyl group, an imidazolyl group, a dimethylimidazolidinyl group, a benzimidazolyl group, an oxazolyl group, an oxazolidinyl group, and a benzoxazolyl group.

[0058] Among the nitrogen-containing groups, an amino group, a dimethylamino group, a diethylamino group, a di-n-propylamino group, a di-isopropylamino group, a di-n-butylamino group, a di-isobutylamino group, a dicyclopentylamino group, a dicyclohexylamino group, an allylamino group, a benzylamino group, a dibenzylamino group, a pyrrolidinyl group, a piperidinyl group, a morpholyl group, an adamantylamino group, a dimethylaminomethyl group, a benzylaminomethyl group, a pyrrolidinylmethyl group, a dimethylaminoethyl group, , pyrrolidinylethyl group, dimethylaminopropyl group, pyrrolidinylpropyl group, dimethylaminoallyl group, pyrrolidinylallyl group, aminophenyl group, dimethylaminophenyl group, 3,5-dimethyl-4-dimethylaminophenyl group, 3,5-di-iso-propyl-4-dimethylaminophenyl group, julolidinyl group, tetramethyljulolidinyl group, pyrrolidinylphenyl group, piperidinylphenyl group, morpholylphenyl group, pyrrolylphenyl group, carbazolylphenyl group, di-te Preferred are rt-butylcarbazolylphenyl group, pyrrolyl group, pyridyl group, quinolyl group, tetrahydroquinolyl group, isoquinolyl group, tetrahydro-isoquinolyl group, indolyl group, indolinyl group, carbazolyl group, di-tert-butylcarbazolyl group, imidazolyl group, dimethylimidazolidinyl group, benzimidazolyl group, oxazolyl group, oxazolidinyl group, and benzoxazolyl group, and further preferably an amino group, a dimethylamino group, a diethylamino group, or a di-isopropylamino group. , a dicyclopentylamino group, a dicyclohexylamino group, a pyrrolidinyl group, a piperidinyl group, a morpholyl group, a dimethylaminophenyl group, a 3,5-dimethyl-4-dimethylaminophenyl group, a 3,5-di-iso-propyl-4-dimethylaminophenyl group, a julolidinyl group, a tetramethyljulolidinyl group, a pyrrolidinylphenyl group, a piperidinylphenyl group, a morpholylphenyl group, a pyrrolylphenyl group, a pyrrolyl group, a pyridyl group, a carbazolyl group, or an imidazolyl group is more preferred.

[0059] Examples of the sulfur-containing group include a methylthio group, an ethylthio group, a benzylthio group, a phenylthio group, a naphthylthio group, a methylthiomethyl group, a benzylthiomethyl group, a phenylthiomethyl group, a naphthylthiomethyl group, a methylthioethyl group, a benzylthioethyl group, a phenylthioethyl group, a naphthylthioethyl group, a methylthiovinyl group, a benzylthiovinyl group, a phenylthiovinyl group, a naphthylthiovinyl group, a methylthiopropyl group, a benzylthiopropyl group, a phenylthiopropyl group, a naphthylthiopropyl group, a methylthioallyl group, a benzylthioallyl group, a phenyl Examples of such groups include a thioallyl group, a naphthylthioallyl group, a mercaptophenyl group, a methylthiophenyl group, a thienylphenyl group, a methylthienylphenyl group, a benzothienylphenyl group, a dibenzothienylphenyl group, a benzodithienylphenyl group, a thienyl group, a tetrahydrothienyl group, a methylthienyl group, a thienofuryl group, a thienothienyl group, a benzothienyl group, a dibenzothienyl group, a thienobenzofuryl group, a benzodithienyl group, a dithiolanyl group, a dithianyl group, an oxathiolanyl group, an oxathianyl group, a thiazolyl group, a benzothiazolyl group, and a thiazolidinyl group.

[0060] Among the above sulfur-containing groups, a thienyl group, a methylthienyl group, a thienofuryl group, a thienothienyl group, a benzothienyl group, a dibenzothienyl group, a thienobenzofuryl group, a benzodithienyl group, a thiazolyl group, and a benzothiazolyl group are preferred.

[0061] R in the above formula [3] 1 and R 2They may be bonded to each other to form a monocyclic or bicyclo ring which may have a substituent. In this case, the ring formed is preferably a 4-8 membered saturated or unsaturated hydrocarbon ring or hetero ring which may have a substituent containing an imine carbon atom. Although not particularly limited as long as the effects of the present invention are exhibited, a 5- or 6-membered ring is preferable. In this case, the structure combined with the imine carbon atom may be, for example, a substituted cyclopentane ring, a substituted cyclohexane ring, a substituted cycloheptane ring, a substituted bicyclo[2.2.1]heptane ring, a substituted bicyclo[2.2.2]octane ring, a substituted pyrrolidine ring, a substituted isoindoline ring, a substituted imidazolidine ring, a substituted dihydroimidazole ring, a substituted tetrahydropyrimidine ring, etc., and a substituted cyclopentane ring, a substituted cyclohexane ring, a substituted pyrrolidine ring, a substituted isoindoline ring, a substituted imidazolidine ring, or a substituted dihydroimidazole ring is preferable.

[0062] R in the above formula [4] 1 ~R 3 The adjacent substituents may be bonded to each other to form a monocyclic or bicyclic ring which may have a substituent. In this case, the ring formed is preferably a 4- to 8-membered saturated or unsaturated heterocyclic ring which may have a substituent containing a phosphorus atom. Although not particularly limited as long as the effects of the present invention are exhibited, a 5- or 7-membered ring is preferable. In this case, examples of the structure combined with the phosphorus atom include a substituted phosphorane ring, a substituted phosphorane ring, a substituted dihydrophosphepine ring, a substituted dioxaphosphepine ring, a substituted diazaphosphepine ring, a substituted phospha-adamantane ring, and a substituted trioxaphospha-adamantane ring, and the like. A substituted dihydrophosphepine ring, a substituted dioxaphosphepine ring, a substituted diazaphosphepine ring, and a substituted trioxaphospha-adamantane ring are preferable.

[0063] Specific examples of the component (A), which is a transition metal compound represented by the above general formula [3] or [4], are shown below, but the scope of the present invention is not particularly limited thereto. For convenience, the ligand structure of the transition metal compound component (A) excluding the portion represented by MXn (metal portion) is divided into two structures: a cyclopentadienyl-type ligand portion and an imide-type ligand portion. The abbreviation for the cyclopentadienyl-type ligand portion is α, and the abbreviation for the imide-type ligand portion is R. 1 , R 2 and R 3 The abbreviation for the substituent is β, the abbreviation for the imide-type ligand partial cyclic structure is γ, and the abbreviations for each substituent are shown in [Table 1] to [Table 3].

[0064] [Table 1]

[0065] [Table 2]

[0066] [Table 3] In addition, R in [Table 3] a and R b is a substituent represented by the abbreviation β in [Table 2]. Also, the wavy line in [Table 3] indicates the bonding site with the nitrogen atom.

[0067] Specific examples of the metal moiety MXn include TiF2, TiCl2, TiBr2, TiI2, Ti(Me)2, Ti(Bn)2, Ti(Allyl)2, Ti(CH2-tBu)2, Ti(1,3-butadienyl), Ti(1,3-pentadienyl), Ti(2,4-hexadienyl), Ti(1,4-diphenyl-1,3-pentadienyl), Ti(CH2-S i(Me)3)2, Ti(ОMe)2, Ti(ОiPr)2, Ti(NMe2)2, Ti(ОMs)2, Ti(ОTs)2, Ti(ОTf)2, ZrF2, ZrCl2, ZrBr2, ZrI2, Zr(Me)2, Zr(Bn)2, Zr(Allyl)2, Zr(CH2-tBu)2, Zr(1,3-butadienyl), Zr(1,3-pentadienyl), Zr(2, 4-Hexadienyl), Zr(1,4-diphenyl-1,3-pentadienyl), Zr(CH2-Si(Me)3)2, Zr(ОMe)2, Zr(ОiPr)2, Zr(NMe2)2, Zr(ОMs)2, Zr(ОTs)2, Zr(ОTf)2, HfF2, HfCl2, HfBr2, Hfh2, Hf(Me)2, Hf(Bn)2, Hf(Allyl)2, Hf(C Examples include H2-tBu), Hf(1,3-butadienyl), Hf(1,3-pentadienyl), Hf(2,4-hexadienyl), Hf(1,4-diphenyl-1,3-pentadienyl), Hf(CH2-Si(Me)3), Hf(OMe), Hf(OMiPr), Hf(NMe2), Hf(OMs), Hf(OTs), and Hf(OTf). Me is a methyl group, Bn is a benzyl group, tBu is a tert-butyl group, Si(Me)3 is a trimethylsilyl group, OMe is a methoxy group, OMe is an isopropoxy group, NMe2 is a dimethylamino group, OMs is a methanesulfonate group, OTs is a p-toluenesulfonate group, and OTf is a trifluoromethanesulfonate group.

[0068] When component (A) is a transition metal compound represented by the general formula [3], according to the above notation, the cyclopentadienyl type ligand moiety is α-7 in [Table 1], and the imide type ligand moiety R 1 The substituent is β-51 in [Table 2], the imide-type ligand portion R 2When the substituents are composed of a combination of β-32 in [Table 2] and the metal portion MXn is TiCl2, the compound represented by the following formula [7] is exemplified.

[0069] [ka]

[0070] In addition, the cyclopentadienyl ligand portion is α-7 in [Table 1], the imide ligand portion cyclic structure is γ-9 in [Table 3], and the imide ligand portion cyclic structure R a When the substituents are composed of a combination of β-13 in [Table 2] and the metal portion MXn is TiMe2, the compound represented by the following formula [8] is exemplified.

[0071] [ka]

[0072] In addition, the cyclopentadienyl ligand portion is α-1 in [Table 1], the imide ligand portion cyclic structure is γ-10 in [Table 3], and the imide ligand portion cyclic structure R a and R b When all of the substituents are composed of a combination of β-9 in [Table 2] and the metal portion MXn is TiBn2, the compound represented by the following formula [9] is exemplified.

[0073] [ka]

[0074] In addition, the cyclopentadienyl-type ligand portion is α-41 in [Table 1], and the imide-type ligand portion is R 1 and R 2 When the substituents are all composed of the combination of β-9 in [Table 2] and the metal portion MXn is Ti(1,3-pentadienyl), the compound represented by the following formula

[10] is exemplified.

[0075] [ka]

[0076] Similarly, when component (A) is a transition metal compound represented by the general formula [4], according to the above notation, the cyclopentadienyl-type ligand moiety is α-25 in [Table 1], and the imide-type ligand moiety R 1 , R 2 and R 3 When all of the substituents are composed of a combination of β-9 in [Table 2] and the metal portion MXn is TiCl2, the compound represented by the following formula

[11] is exemplified.

[0077] [ka]

[0078] In addition, the cyclopentadienyl-type ligand portion is α-7 in [Table 1], and the imide-type ligand portion is R 1 , R 2 and R 3 When all of the substituents are composed of a combination of β-9 in [Table 2] and the metal portion MXn is TiMe2, the compound represented by the following formula

[12] is exemplified.

[0079] [ka]

[0080] In addition, the cyclopentadienyl-type ligand portion is α-18 in [Table 1], and the imide-type ligand portion is R 1 , R 2 and R 3 When all of the substituents are composed of the combination of β-11 in [Table 2] and the metal portion MXn is TiBn2, the compound represented by the following formula

[13] is exemplified.

[0081] [ka]

[0082] In addition, the cyclopentadienyl-type ligand portion is α-1 in [Table 1], and the imide-type ligand portion is R 1 and R 2 The substituents are all β-9 in [Table 2], imide-type ligand moiety R 3 When the substituents are composed of a combination of β-60 in [Table 2] and the metal portion MXn is Ti(1,3-pentadienyl), the compound represented by the following formula

[14] is exemplified.

[0083] [ka]

[0084] The compound represented by the formula [1] or [2] can be produced by a conventionally known method, and the production method is not particularly limited. Examples of known production methods include those described in "Organometallics 1999,18,1116.", JP-T-2001-516776, "Organometallics 2001,20,4424.", "Chem. Commun. 2002,608.", "Organometallics 2003,22,1937.", "J. Organomet. Chem. 2004,689,203.", "Organometallics 2004,23,1562.", "Organometallics 2004,23,3309.", WO2005 / 090418, US6239061, and "Organometallics 2005,24,2548.'', Special Publication No. 2007-529584, ``J.Organomet.Chem. 2011,696,2451.'', ``Dalton Trans. 2011,40,7842.", JP 2012-007171 A, JP 2012-046764 A, JP 2013-155371 A, JP 2013-510214 A, JP 2013-515120 A, US9045504 A, JP 2014-509670 A, US9035081 A, JP 2015-520276 A, JP 2016-532730 A, and JP 2017-509595 A.

[0085] The compound represented by the general formula [2] is more preferred than the compound represented by the general formula [1] because it can produce a polymer with higher polymerization activity. In the present invention, among the transition metal compounds represented by the general formula [1] or [2], one kind may be used alone, or two or more kinds of transition metal compounds having different chemical structures may be used. In addition, one kind of optical isomer having the same chemical structure may be used alone, or a mixture of optical isomers (e.g., a meso mixture or a racemic mixture) may be used. When L is a Group 16 element, the same compounds as above except that y=3 and z=4 can be exemplified.

[0086] <Solid Carrier (S)> The solid support (S) is a solid aluminoxane compound, and examples of the aluminoxane include at least one selected from aluminoxanes having a structure represented by the following general formula (Sa) and aluminoxanes having a structure represented by the following general formula (Sb), and aluminoxanes having a structure comprising a repeating unit represented by the following general formula (Sc) and a repeating unit represented by the following general formula (Sd).

[0087] [ka]

[0088] In the general formulae (Sa) to (Sd), R e are each independently a hydrocarbon group having 1 to 10 carbon atoms, preferably 1 to 4 carbon atoms, and specific examples thereof include hydrocarbon groups such as methyl, ethyl, propyl, isopropyl, isopropenyl, n-butyl, sec-butyl, tert-butyl, pentyl, hexyl, octyl, decyl, dodecyl, tridecyl, tetradecyl, hexadecyl, octadecyl, eicosyl, cyclohexyl, cyclooctyl, phenyl, tolyl, and ethylphenyl groups, with methyl, ethyl, and isobutyl groups being preferred, and methyl being particularly preferred. eA part of is replaced by halogen atoms such as chlorine and bromine, and the halogen content is R e In (Sc) and (Sd), a line segment having one end that is not connected to an atom represents a bond to another atom not shown.

[0089] In the general formulae (Sa) and (Sb), r represents an integer of 2 to 500, preferably 6 to 300, and particularly preferably 10 to 100. In the general formulae (Sc) and (Sd), s and t each represent an integer of 1 or more. r, s, and t are selected so that the aluminoxane can be maintained in a substantially solid state in the reaction environment used.

[0090] The solid aluminoxane compound differs from conventionally known olefin polymerization catalyst supports in that it does not contain inorganic solid components such as silica or alumina or organic polymer components such as polyethylene or polystyrene, but is a solidified product containing an alkylaluminum compound as a main component.

[0091] The term "solid state" means that the aluminoxane component substantially maintains a solid state in the reaction environment in which it is used. More specifically, it means that the aluminoxane component substantially maintains a solid state when the transition metal compound (A) is contacted with the aluminoxane component to prepare an olefin polymerization catalyst as described below, and when the prepared olefin polymerization catalyst is used to polymerize olefins (e.g., slurry polymerization).

[0092] The easiest method to check whether the aluminoxane component is in a solid state is to check visually, but in many cases, for example, during polymerization, visual confirmation is difficult. In that case, it can be judged, for example, from the properties of the polymer powder obtained after polymerization and the state of adhesion to the reactor. Conversely, if the properties of the polymer powder are good and adhesion to the reactor is small, even if a part of the aluminoxane component is eluted to some extent under the polymerization environment, it does not deviate from the gist of the present invention. Examples of indices for judging the properties of the polymer powder include bulk density, particle shape, surface shape, and the degree of presence of amorphous polymers, but from the viewpoint of quantitativeness, polymer bulk density is preferred. The bulk density is usually within the range of 0.01 to 0.9, preferably 0.05 to 0.6, and more preferably 0.1 to 0.5.

[0093] The solubility of the solid aluminoxane compound in n-hexane maintained at a temperature of 25° C. is usually in the range of 0 to 40 mol %, preferably 0 to 20 mol %, and particularly preferably 0 to 10 mol %.

[0094] The dissolution ratio is determined by adding 2 g of the solid aluminoxane compound carrier to 50 ml of n-hexane kept at 25° C., stirring for 2 hours, separating the solution using a G-4 glass filter, and measuring the aluminum concentration in the filtrate. Therefore, the dissolution ratio is determined as the ratio of aluminum atoms present in the filtrate to the amount of aluminum atoms equivalent to 2 g of the aluminoxane used.

[0095] As the solid aluminoxane compound, known solid aluminoxanes can be used without limit, and for example, the solid polyaluminoxane composition described in International Publication No. 2014 / 123212 can be used. Known production methods include, for example, those described in JP-B-7-42301, JP-A-6-220126, JP-A-6-220128, JP-A-11-140113, JP-A-11-310607, JP-A-2000-38410, JP-A-2000-95810, and International Publication No. 2010 / 55652.

[0096] The average particle size of the solid aluminoxane compound is generally in the range of 0.01 to 50,000 μm, preferably 1 to 1,000 μm, and particularly preferably 1 to 200 μm. The average particle size of the solid aluminoxane compound is obtained by observing the particles with a scanning electron microscope, measuring the particle sizes of 100 or more particles, and averaging the weights. First, the particle size of each particle is measured by sandwiching the particle image between two parallel lines in the horizontal and vertical directions, and is calculated according to the following formula. Particle size = ((horizontal length) 2 +(Vertical length) 2 ) 0.5

[0097] Next, the weight average particle size of the solid aluminoxane compound is calculated from the particle size calculated above according to the following formula. Average particle diameter=Σnd 4 / Σnd 3 (n: number of particles, d: particle size)

[0098] The solid aluminoxane compound has a specific surface area of ​​50 to 1000 m 2 / g, preferably 100 to 800m 2 / g and the pore volume is 0.1-2.5 cm 3 / g is preferable.

[0099] The particle size of the polymer particles obtained by carrying out olefin polymerization using the olefin polymerization catalyst of the present invention is not particularly limited, but is preferably 3 to 50,000 μm. A more preferred lower limit is 5 μm, a further preferred lower limit is 10 μm, and a particularly preferred lower limit is 20 μm. On the other hand, a more preferred upper limit is 30,000 μm, a further preferred upper limit is 20,000 μm, and a particularly preferred upper limit is 10,000 μm. When the olefin polymerization catalyst of the present invention is used, even if an ultra-high molecular weight polymer having an intrinsic viscosity ([η]) exceeding 5 dl / g is produced, fouling or aggregation of the obtained olefin polymer particles tends not to occur, which is advantageous for efficient and stable production of the polymer particles.

[0100] The factors behind the above-mentioned advantages in terms of fouling and particle aggregation are unclear at present, but the present inventors speculate as follows. There are two main causes of fouling and aggregation during polymerization. One is a physical factor that occurs when component (A), which becomes the polymerization active species, is liberated (leached) from the solid support (S) in the polymerization environment, resulting in the production of amorphous polymers. The other is an electrostatic factor that occurs when frictional charging occurs between the solid catalyst component (X), which will be described later, and the produced polymer and polymerization reactor.

[0101] Many of the conventional techniques involve suppressing leaching of component (A) or precisely controlling the shape or amount of fine powder of the solid carrier (S), which can be said to have an effect against the above-mentioned physical factors.

[0102] The present inventors believe that the use of a solid aluminoxane compound as the solid support (S) in the olefin polymerization catalyst of the present invention is extremely effective against electrostatic fouling believed to be caused by the component (A) having a cyclopentadienyl ligand and a ligand containing an atom selected from Group 15 or Group 16 elements. The present inventors believe that such an effect is due to the fact that the solid aluminoxane has a relatively flexible structure and high polarity, and therefore exhibits not only the performance of a support and cocatalyst but also the performance of an antistatic agent.

[0103] Such an effect provided by solid aluminoxane is an effect that cannot be seen in transition metal compounds whose ligands are composed only of cyclopentadienyl ligands, or in transition metal compounds that contain Group 15 and Group 16 elements and have no cyclopentadienyl ligands, such as phenoxyimine ligands, and it is difficult to infer this effect from the prior art.

[0104] <Method for preparing olefin polymerization catalyst> As a preferred embodiment of the olefin polymerization catalyst according to the present invention, a solid catalyst component (X) is prepared by adding the component (A) and the solid support (S) to an inert hydrocarbon or to a polymerization system using an inert hydrocarbon.

[0105] The contact method of each component is not particularly limited as long as the effect of the present invention is exhibited. For example, the component (A) in a solid or liquid form is added all at once or in portions to a suspension consisting of a solid carrier (S) and an organic solvent, the component (A) dissolved or suspended in an organic solvent is added all at once or in portions to a suspension consisting of a solid carrier (S) and an organic solvent, and the component (A) is added in a solid or suspended in an organic solvent to the component (A) for contact. From the viewpoint of making the reaction uniform, it is preferable to add the component (A) to the solid carrier (S). When two or more kinds of components (A) are used in combination, the components (A) may be added one by one, or two or more may be mixed and added.

[0106] In any step of the contact method, by adding component (G), fouling during the polymerization reaction can be suppressed to a higher degree and the particle properties of the resulting polymer can be further improved. As component (G), a compound having a polar functional group can be used, and a nonionic surfactant is preferable, and a polyalkylene oxide block, a higher aliphatic amide, a polyalkylene oxide, a polyalkylene oxide alkyl ether, an alkyldiethanolamine, a polyoxyalkylene alkylamine, a glycerin fatty acid ester, or an N-acyl amino acid is more preferable. These may be used alone or in combination of two or more kinds.

[0107] The solvent used in the preparation of the ethylene polymerization catalyst according to the present invention includes an inert hydrocarbon solvent. Specific examples of the solvent include aliphatic hydrocarbons such as propane, butane, pentane, hexane, heptane, octane, decane, dodecane, and kerosene; alicyclic hydrocarbons such as cyclopentane, cyclohexane, and methylcyclopentane; aromatic hydrocarbons such as benzene, toluene, and xylene; halogenated hydrocarbons such as ethylene chloride, chlorobenzene, and dichloromethane; and mixtures of these.

[0108] For the polymerization of olefins, the above-mentioned solid catalyst component (X) can be used as it is. However, by prepolymerizing an olefin on this solid catalyst component (X) to form a prepolymerized catalyst component (XP) and then using the prepolymerized catalyst component, it is possible to more highly suppress fouling during the polymerization reaction and to further improve the particle properties of the resulting polymer.

[0109] The prepolymerized catalyst component (XP) can be prepared by introducing an olefin into the solid catalyst component (X), usually in an inert hydrocarbon solvent. The reaction can be carried out in any of batch, semi-continuous and continuous modes. The reaction can be carried out under reduced pressure, normal pressure or increased pressure. The solid catalyst component (X) produces 0.2 to 500 g of polymer by this prepolymerization.

[0110] The prepolymerized catalyst component (XP) prepared in an inert hydrocarbon solvent may be separated from the suspension and then suspended again in an inert hydrocarbon, and an olefin may be introduced into the resulting suspension, or the olefin may be introduced into the suspension after drying.

[0111] The prepolymerization temperature is usually −20 to 80° C., and preferably 0 to 60° C. The prepolymerization time is usually 0.5 to 100 hours, and preferably 1 to 50 hours. As the form of the solid catalyst component (X) used in the prepolymerization, those already mentioned can be used without any limitation.

[0112] Further, the following component (B) can be used as necessary. Component (B): at least one compound selected from the group consisting of (b-1) an organometallic compound represented by the following general formula [b-1-1], [b-1-2] or [b-1-3], (b-2) an organoaluminum oxy compound, and (b-3) a compound that reacts with component (A) and component (B) to form an ion pair. RamAl(ORb)n Hp Xq ···[b-1-1] (In general formula [b-1-1], Ra and Rb each represent a hydrocarbon group having 1 to 15 carbon atoms, which may be the same as or different from each other, X represents a halogen atom, m is a number where 0 < m ≦ 3, n is a number where 0 ≦ n < 3, p is a number where 0 ≦ p < 3, q is a number where 0 ≦ q < 3, and m + n + p + q = 3.) Ma AlRa4···[b-1-2] (In general formula [b-1-2], Ma represents Li, Na or K, and Ra represents a hydrocarbon group having 1 to 15 carbon atoms.) RarMbRbs Xt ···[b-1-3] (In general formula [b-1-3], Ra and Rb each represent a hydrocarbon group having 1 to 15 carbon atoms, which may be the same as or different from each other, Mb represents Mg, Zn or Cd, X represents a halogen atom, r is a number where 0 < r ≦ 2, s is a number where 0 ≦ s ≦ 1, t is a number where 0 ≦ t ≦ 1, and r + s + t = 2.)

[0113] In particular, the organoaluminum compound represented by the formula [b-1-1] in the compound (b-1) is preferably used. When the organoaluminum compound of the formula [b-1-1] is used as component (B), the molar ratio of the aluminum atom (Al) in component (B) to the transition metal complex which is component (A) (component (B) / transition metal compound) is usually 0.1 to 10000, preferably or 0.5 to 5000 and is used in such an amount.

[0114] The concentration of the solid catalyst component (X) in the prepolymerization system is usually 1 to 1000 g / L, preferably 10 to 500 g / L, in terms of the ratio of the solid catalyst component (X) / 1 liter of polymerization volume. During the prepolymerization, the component (G) can be allowed to coexist with the catalyst component (X) for the purpose of suppressing fouling or improving particle properties.

[0115] In order to improve the fluidity of the prepolymerized catalyst component (XP) and to suppress the occurrence of heat spots, sheeting, and polymer lumps during polymerization, the prepolymerized catalyst component (XP) may be contacted with the component (G) once produced by prepolymerization.

[0116] The temperature when component (G) is mixed and contacted is usually −50 to 50° C., and preferably −20 to 50° C., and the contact time is 1 to 1000 minutes, and preferably 5 to 600 minutes. When the solid catalyst component (X) and the component (G) are mixed and contacted, the component (G) is usually used in an amount of 0.1 to 20 parts by weight, preferably 0.3 to 10 parts by weight, and more preferably 0.4 to 5 parts by weight, per 100 parts by weight of the solid catalyst component (X).

[0117] The solid catalyst component (X) and the component (G) can be mixed and contacted in an inert hydrocarbon solvent. Examples of the inert hydrocarbon solvent include the same solvents as those used in the preparation of the solid catalyst component (X).

[0118] The olefin polymerization catalyst according to the present invention can be used as a dried prepolymerized catalyst by drying the prepolymerized catalyst component (XP). This embodiment is particularly preferred when a gas phase polymerization method is used. Of course, it can also be used in the case of a liquid phase polymerization method.

[0119] The prepolymerized catalyst component (XP) is usually dried after removing the hydrocarbon, which is the dispersion medium, from the resulting suspension of the prepolymerized catalyst by filtration or the like. The drying of the prepolymerized catalyst component (XP) is carried out by keeping the prepolymerized catalyst component (XP) at a temperature of 70°C or less, preferably in the range of 20 to 50°C, under a flow of an inert gas. The amount of volatile components in the obtained dried prepolymerized catalyst is desirably 2.0% by weight or less, preferably 1.0% by weight or less. The amount of volatile components in the dried prepolymerized catalyst is preferably as small as possible, and there is no particular lower limit, but in practice it is 0.001% by weight. The drying time is usually 3 to 8 hours, depending on the drying temperature. If the amount of volatile components in the dried prepolymerized catalyst exceeds 2.0% by weight, the fluidity of the dried prepolymerized catalyst decreases, and it may not be possible to stably supply the dried prepolymerized catalyst to a polymerization reactor.

[0120] The amount of volatile components in the dried prepolymerized catalyst is measured, for example, by a weight loss method or a method using gas chromatography. In the weight loss method, a dry prepolymerized catalyst is heated at 110°C for 1 hour in an inert gas atmosphere, the weight loss is determined, and expressed as a percentage of the dry prepolymerized catalyst before heating.

[0121] In the method using gas chromatography, volatile components such as hydrocarbons are extracted from the dried prepolymerized catalyst, a calibration curve is prepared according to the internal standard method, and the weight percentage is calculated from the GC area.

[0122] As for the method of measuring the amount of volatile components in the dried prepolymerized catalyst, when the amount of volatile components in the dried prepolymerized catalyst is about 1% by weight or more, a weight loss method is adopted, and when the amount of volatile components in the dried prepolymerized catalyst is about 1% by weight or less, a method using gas chromatography is adopted.

[0123] Examples of the inert gas used for drying the prepolymerized catalyst component (XP) include nitrogen gas, argon gas, and neon gas. Such an inert gas has an oxygen concentration of 20 ppm or less, preferably 10 ppm or less, and more preferably 5 ppm or less (volume basis), and a moisture content of 20 ppm or less, preferably 10 ppm or less, and more preferably 5 ppm or less (weight basis). If the oxygen concentration and moisture content in the inert gas exceed the above ranges, the olefin polymerization activity of the dried prepolymerized catalyst may be significantly reduced.

[0124] The dried prepolymerized catalyst has excellent fluidity and can be stably supplied to a polymerization reactor. In addition, the solvent used for suspension does not need to be entrained in the gas phase polymerization system, and therefore the polymerization can be stably carried out.

[0125] <Production method of olefin polymer> According to the present invention, by polymerizing one or more α-olefins having 2 to 30 carbon atoms in the presence of an olefin polymerization catalyst comprising the above-mentioned component (A) and the solid support (S), preferably by homopolymerizing ethylene or copolymerizing ethylene with an α-olefin having 3 to 20 carbon atoms, it is possible to prevent fouling during polymerization and efficiently produce an olefin polymer.

[0126] In the present invention, the polymerization can be carried out by any of liquid phase polymerization methods such as solution polymerization and suspension polymerization, or gas phase polymerization methods. In the suspension polymerization method and gas phase polymerization method, it is preferable to use the above-mentioned solid catalyst component (X).

[0127] Specific examples of the inert hydrocarbon medium used in the liquid phase polymerization method include aliphatic hydrocarbons such as propane, butane, pentane, hexane, heptane, octane, decane, dodecane, kerosene, etc.; alicyclic hydrocarbons such as cyclopentane, cyclohexane, methylcyclopentane, etc.; aromatic hydrocarbons such as benzene, toluene, xylene, etc.; halogenated hydrocarbons such as ethylene chloride, chlorobenzene, dichloromethane, etc., and mixtures thereof. In the liquid phase polymerization method, the olefin itself can also be used as the solvent.

[0128] When polymerization is carried out using the above-mentioned olefin polymerization catalyst, the component (A) is usually used in an amount of 10 -12 ~10 -1 Molar, preferably 10 -8 ~10 -2 Like becoming a mole Used in quantity.

[0129] The polymerization temperature using the above-mentioned solid catalyst component (X) is usually in the range of −50 to 200° C., preferably 0 to 170° C., and particularly preferably 60 to 170° C. The polymerization pressure is usually in the range of normal pressure to 100 kg / cm. 2 , preferably normal pressure to 50 kg / cm 2 The polymerization reaction can be carried out in any of batch, semi-continuous and continuous modes. It is also possible to carry out the polymerization in two or more stages with different reaction conditions.

[0130] The molecular weight of the resulting polymer can be adjusted by adding hydrogen to the polymerization system or by changing the polymerization temperature. Generally, the more low molecular weight components there are, the more they adhere to the walls of the polymerization reactor and the agitator blades, which can lead to a decrease in productivity due to the burden on the cleaning process. Component (G) can be added during polymerization to suppress fouling or improve particle properties.

[0131] In the present invention, the olefin supplied to the polymerization reaction is, for example, one or more monomers selected from olefins having from 2 to 20 carbon atoms. Specific examples of the olefins having from 2 to 20 carbon atoms include α-olefins such as ethylene, propylene, 1-butene, 1-pentene, 1-hexene, 4-methyl-1-pentene, 1-octene, 1-decene, 1-dodecene, 1-tetradecene, 1-hexadecene, 1-octadecene, and 1-eicosene; and cyclic olefins such as cyclopentene, cycloheptene, norbornene, 5-methyl-2-norbornene, tetracyclododecene, and 2-methyl-1,4,5,8-dimethano-1,2,3,4,4a,5,8,8a-octahydronaphthalene.

[0132] Further, examples of monomers supplied to the polymerization reaction include styrene, vinylcyclohexane, dienes, acrylic acid, methacrylic acid, fumaric acid, maleic anhydride, and the like; and polar monomers such as methyl acrylate, ethyl acrylate, methyl methacrylate, ethyl methacrylate, and methacrylic acid.

[0133] <Olefin polymer> One embodiment of the olefin polymer obtained by the polymerization reaction using the olefin catalyst of the present invention is an ethylene-based polymer containing ethylene-derived structural units in the range of preferably 90 to 100 mol%, more preferably 95 to 100 mol%, and even more preferably 98 to 100 mol%. The ethylene-based polymer contains ethylene-derived structural units in the range of preferably 0 to 10 mol%, more preferably 0 to 5 mol%, and even more preferably 0.2 mol% in total. However, the total of the content of ethylene-derived structural units and the content of ethylene-derived structural units are 100 mol%.

[0134] Among these polymers, ethylene homopolymer, ethylene / propylene copolymer, ethylene / 1-butene copolymer, ethylene / propylene / 1-butene copolymer, ethylene / 1-octene polymer, ethylene / 1-hexene polymer, ethylene / 4-methyl-1-pentene polymer, ethylene / propylene / 1-octene polymer, ethylene / propylene / 1-hexene polymer, and ethylene / propylene / 4-methyl-1-pentene polymer are preferred. Also, so-called block copolymers (impact copolymers) obtained by mixing or continuously producing two or more types selected from these polymers may be used.

[0135] Although there is no particular restriction on the molecular weight of the olefin polymer produced by the olefin polymerization catalyst of the present invention, the effect of the present invention often provides favorable results in the production of polymers with high molecular weights. The intrinsic viscosity ([η]) of such an olefin polymer is preferably 5.0 dl / g or more. A more preferred lower limit is 6.0 d / g, further 8.0 d / g, and particularly (10.0) d / g. On the other hand, a preferred upper limit is (40) d / g, more preferably (35 d / g, further (30) d / g, and particularly (25) d / g. The molecular weight of the high molecular weight polymer produced by the olefin polymerization catalyst of the present invention can be determined, for example, by the ASTM-D4020 standard, and is preferably 500,000 or more, more preferably 1,000,000 or more.

[0136] Furthermore, the ethylene homopolymer obtained by homopolymerization of ethylene using the olefin polymerization catalyst of the present invention may exhibit a characteristic of high density commensurate with molecular weight (MFR) in a relatively low molecular weight range. This is because there are few methyl and ethyl branches, and further there are few double bond structures such as vinyl and vinylidene. Specifically, the ethylene homopolymer obtained using the olefin polymerization catalyst of the present invention and having an intrinsic viscosity ([η]) of 3.0 dl / g or less, more preferably 2.0 dl / g or less, has the characteristics represented by the following requirements (I) to (III).

[0137] Requirement (I): The weight average molecular weight (Mw) / number average molecular weight (Mn) measured by GPC is 2.0 to 5.0. In the weight average molecular weight (Mw) / number average molecular weight (Mn), the lower limit is preferably 2.2, and the particularly preferred lower limit is 2.5, while the preferred upper limit is 4.8, and the particularly preferred upper limit is 4.5. Requirement (II): The melt flow rate (MFR) and density satisfy the relationship: (density) ≧ 10.0 × log(MFR) + 958. Requirement (III): 1 The total number of double bonds (vinyl, vinylidene, vinylene) per 1,000 carbons measured by H-NMR is less than 0.02. The total amount of double bonds is preferably less than 0.01 per 1000 carbon atoms. The methods for measuring the physical properties and characteristics of the polymer are described below.

[0138] Intrinsic viscosity [η] In accordance with the ASTM-D4020 standard, approximately 20 mg of the measurement sample was dissolved in 15 ml of decalin and the specific viscosity η sp After diluting the decalin solution by adding 5 ml of decalin solvent, the specific viscosity η sp This dilution procedure is repeated two more times, and the η when the concentration (C) is extrapolated to 0 is measured as shown in the following formula (Eq-1). sp The value of / C is calculated as the intrinsic viscosity [η] (unit: dl / g). [η]=lim(η sp / C) (C→0) -------- (Eq-1)

[0139] Melt Flow Rate (MFR) It is measured in accordance with the ASTM-D1238 standard at 190°C and a load of 2.16 kg (kgf).

[0140] Density (kg / m 3 ) The density is measured by a density gradient tube method after the strand obtained during the MFR measurement is heat-treated at 120° C. for 30 minutes and then allowed to stand at room temperature for 1 hour.

[0141] Weight average molecular weight (Mw), number average molecular weight (Mn) The weight average molecular weight (Mw) and number average molecular weight (Mn) of the olefin polymer are determined by gel permeation chromatography (GPC). They are calculated from a molecular weight distribution curve obtained by a gel permeation chromatograph (high temperature size exclusion chromatograph) "Alliance GPC 2000" manufactured by Waters, and the operating conditions are as follows: [Equipment and conditions used] Measurement equipment: Gel permeation chromatograph Alliance GPC2000 (Waters) Analysis software: Chromatography Data System Empower (trademark, Waters) Column: TSKgel GMH6-HT x 2 + TSKgel GMH6-HT x 2 (Inner diameter 7.5mm x length 30cm, Tosoh Corporation) Mobile phase: o-Dichlorobenzene [ODCB] (Wako Pure Chemical Industries, Ltd., special grade reagent) Detector: Differential refractometer (built into the device) Column temperature: 140℃ Flow rate: 1.0mL / min Injection volume: 500μL Sampling time interval: 1 second Sample concentration: 0.15% (w / v) Molecular weight calibration: Monodisperse polystyrene (Tosoh Corporation) / molecular weight 495 to 20.6 million The molecular weight distribution and various average molecular weights are calculated in terms of polyethylene molecular weight according to the general calibration procedure described in J. Polym. Sci. 1967, B5, 753.

[0142] Amount of double bonds, number of branches (per 1000 carbons) The number of double bonds and the number of branches of an olefin polymer are determined by a nuclear magnetic resonance (NMR) spectrometer. 1 Determined by 1 H-NMR as follows or an equivalent method. [Equipment and conditions used] Measurement equipment: Bruker Biospin AVANCEIIIcryo-500 nuclear magnetic resonance spectrometer (1H: 500MHz) Measurement solvent: orthodichlorobenzene-d4 Sample concentration: ca. 20mg / 0.6mL Measurement temperature: 120℃ Number of times: 64 to 256 Chemical shift reference: Main chain methylene peak (1.2 ppm) The amount of double bonds per 1000 carbon atoms is calculated from the integral intensity ratio of the integral intensities of 4.8 to 4.9 and 5.6 to 5.7 ppm for vinyl groups, 4.6 to 4.7 ppm for vinylidene groups, and 5.1 to 5.2 (tri-substitution) and 5.3 to 5.4 (di-substitution) ppm for vinylene (internal olefin) to the integral sum of hydrogen atoms in the polymer. The amount of branching is 13 It is determined by C-NMR as follows or an equivalent method. [Equipment and conditions used] Measurement equipment: Bruker Biospin AVANCEIIIcryo-500 nuclear magnetic resonance spectrometer (13C: 125MHz) Measurement solvent: orthodichlorobenzene / benzene-d6 (4 / 1 v / v) Sample concentration: ca. 60mg / 0.6mL Measurement temperature: 120℃ Number of times accumulated: 128 or more Chemical shift reference: Main chain methylene peak (29.7 ppm) The number of branches per 1000 carbon atoms is calculated from the integral intensity ratio of the integrated intensity of 19.9 ppm for the number of methyl branches and 10.8 ppm for the number of ethyl branches to the total integral of carbon (5 to 45 ppm) in the polymer.

[0143] The olefin polymer obtained by the polymerization reaction using the olefin polymerization catalyst of the present invention may contain additives such as weather resistance stabilizers, heat resistance stabilizers, antistatic agents, antislip agents, antiblocking agents, antifogging agents, lubricants, pigments, dyes, nucleating agents, plasticizers, antioxidants, hydrochloric acid absorbers and antioxidants, as necessary, within the scope of the object of the present invention.

[0144] The olefin polymer obtained by the polymerization reaction using the olefin polymerization catalyst of the present invention, and the resin composition containing a thermoplastic resin or an additive as necessary, can be molded by any molding method suitable for ultra-high molecular weight olefin polymers without any restrictions. For example, compression molding, gel sheet molding, gel spinning molding, solid-phase stretch molding, etc. can be mentioned. In addition, it can be molded into a container, tray, sheet, rod, film, or various molded body covering by molding methods such as injection molding, profile extrusion molding, pipe molding, tube molding, heterogeneous molded body covering molding, injection blow molding, direct blow molding, T-die sheet or film molding, inflation molding, and press molding.

[0145] Furthermore, ultra-high molecular weight ethylene polymers have an excellent balance of properties such as abrasion resistance, self-lubrication, impact strength, and thin-wall formability, and are therefore used in applications requiring these properties, such as metal coatings (laminations) for steel pipes, electric wires, automobile sliding door rails, etc., pressure-resistant rubber hoses, automobile door gaskets, clean room door gaskets, automobile glass run channels, automobile weather strips, and other various rubber coatings (laminations), linings for hoppers, chutes, etc., and sliding materials such as gears, bearings, rollers, tape reels, various guide rails and elevator rail guides, and various protective liner materials.

[0146] If the olefin polymer has a relatively low molecular weight, it is suitable for processing by general film molding, blow molding, injection molding, and extrusion molding. In film molding, it can be obtained by extrusion lamination molding, T-die film molding, inflation molding (air cooling, water cooling, multi-stage cooling, high-speed processing), etc. Furthermore, it can be stretched. The film obtained by using the ethylene polymer can be used as a single layer, but by making it multilayer, it can be given various functions. In that case, the co-extrusion method in each of the above-mentioned molding methods can be mentioned. On the other hand, by lamination lamination molding methods such as extrusion lamination molding and dry lamination method, it can be mentioned that it is laminated with paper or barrier film (aluminum foil, vapor deposition film, coating film, etc.) that is difficult to co-extrude. It is possible to manufacture high-performance products by multilayering by co-extrusion method in blow molding, injection molding, and extrusion molding, just like film molding.

[0147] Examples of molded articles obtained by processing an olefin polymer obtained by a polymerization reaction using the olefin polymerization catalyst of the present invention and a resin composition containing a thermoplastic resin and / or an additive as required include films, blown infusion bags, blown bottles, gasoline tanks, tubes, pipes, tear-off caps, injection molded articles such as daily necessities, fibers, and large molded articles by rotational molding.

[0148] Furthermore, a film obtained by processing an olefin polymer obtained by a polymerization reaction using the olefin polymerization catalyst of the present invention and a resin composition containing a thermoplastic resin or additives as necessary is suitable for various packaging films such as liquid packaging bags, liquid soup bags, liquid paper containers, laminated raw material, special-shaped liquid packaging bags (standing pouches, etc.), standard bags, heavy-duty bags, wrap films, sugar bags, oil packaging bags, food packaging films, protective films, infusion bags, agricultural materials, etc. Also, it can be used as a multilayer film by bonding with a substrate such as nylon or polyester. EXAMPLES

[0149] The present invention will be described in more detail below based on examples, but the present invention is not limited to these examples. The transition metal compound (A) has a frequency of 270 MHz, 1 The solid support (S) was analyzed for Al concentration and the solid catalyst component (X) was analyzed for metal (Ti, Zr) concentration in the supernatant liquid by inductively coupled plasma atomic emission spectrometry (ICP-AES) (Shimadzu ICPS-8100).

[0150] <Synthesis of transition metal compound (A)> [Synthesis Example 1] Synthesis of transition metal compound (A-1) (Pentamethylcyclopentadienyl)Ti(N=P(t-Bu)3)Cl2 represented by the following formula (hereinafter also referred to as "transition metal compound (A-1)") was synthesized by the method described in Organometallics 2003, 22, 1937.

[0151] [ka]

[0152] [Synthesis Example 2] Synthesis of transition metal compound (A-2) (Cyclopentadienyl)Ti(N=P(t-Bu)3)Cl2 represented by the following formula (hereinafter also referred to as "transition metal compound (A-2)") was synthesized by the method described in Organometallics 1999, 18, 1116.

[0153] [ka]

[0154] [Synthesis Example 3] Synthesis of transition metal compound (A-3) (Indenyl)Ti(N=P(t-Bu)3)Cl2 represented by the following formula (hereinafter also referred to as "transition metal compound (A-3)") was synthesized by the method described in J. Organomet. Chem. 2004, 689, 203.

[0155] [ka]

[0156] [Synthesis Example 4] Synthesis of transition metal compound (A-4) The (1-(pentafluorophenylmethyl)indenyl)Ti(N=P(t-Bu)3)Cl2 represented by the following formula (hereinafter also referred to as "transition metal compound (A-4)") was synthesized by the method described in JP2015-520276A.

[0157] [ka]

[0158] [Synthesis Example 5] Synthesis of transition metal compound (A-5) (Cyclopentadienyl)Ti(N=C(t-Bu)2)Cl2 represented by the following formula (hereinafter also referred to as "transition metal compound (A-5)") was synthesized by the method described in J. Am. Chem. Soc. 2000, 122, 5499.

[0159] [ka]

[0160] [Synthesis Example 6] Synthesis of transition metal compound (A-6) (Pentamethylcyclopentadienyl)Ti(N=C(N(iPr)2)(2,6-F2-C6H3))Cl2 (hereinafter also referred to as "transition metal compound (A-6)") represented by the following formula was synthesized by the method described in Chem. Commun. 2010, 46, 3339.

[0161] [ka]

[0162] [Synthesis Example 7] Synthesis of transition metal compound (A-7) Bis(1-butyl-3-methylcyclopentadienyl)ZrCl2 (hereinafter also referred to as "transition metal compound (A-7)") represented by the following formula was synthesized by the method described in JP2015-113282A.

[0163] [ka]

[0164] [Synthesis Example 8] Synthesis of transition metal compound (A-8) Bis[6-cumyl-3-methyl-2-[{(2-methylcyclohexyl)imino}methyl]phenolate]ZrCl2 (hereinafter also referred to as "transition metal compound (A-8)") represented by the following formula was synthesized by the method described in JP-A-2006-206768.

[0165] [ka]

[0166] [Synthesis Example 9] Synthesis of transition metal compound (A-9) Bis(n-butylcyclopentadienyl)ZrCl2 (hereinafter also referred to as "transition metal compound (A-9)") represented by the following formula was purchased from FUJIFILM Wako Pure Chemical Industries, Ltd. and used as is.

[0167] [ka]

[0168] [Synthesis Example 10] Synthesis of transition metal compound (A-10) Di(p-tolyl)methylene(cyclopentadienyl)(octamethyloctahydrodibenzofluorenyl)ZrCl2 (hereinafter also referred to as "transition metal compound (A-10)") represented by the following formula was synthesized by the method described in JP-A-2004-182715.

[0169] [ka]

[0170] [Synthesis Example 11] Synthesis of transition metal compound (A-11) (Dimethylcyclopentadienyl)Ti(N=P(t-Bu)3)Cl2 (hereinafter also referred to as "transition metal compound (A-11)") represented by the following formula was synthesized by the following method.

[0171] [ka]

[0172] In a nitrogen atmosphere, 2957 mg (31.40 mmol) of 1,3-dimethylcyclopentadiene and 40 mL of hexane were added to a Schlenk flask. While cooling in an ice bath, 20.0 mL of a hexane solution (1.57 M) of nBuLi (31.40 mmol) was gradually added, and the mixture was stirred for 2 hours while returning to room temperature. The reaction solution was filtered using a glass filter. The resulting white solid was washed with hexane and dried under reduced pressure to obtain 2.6334 g of a white solid.

[0173] Under nitrogen atmosphere, 205 mg of the white solid obtained in the previous reaction and 15 mL of THF were added to a Schlenk flask. Under nitrogen atmosphere, 741 mg of Ti(N=P(t-Bu)3)Cl3 and 50 mL of toluene were added to another Schlenk flask. This solution was cooled in an ice bath, and the reaction solution obtained earlier was added while washing with 5 mL of THF. The reaction solution was stirred for 19 hours while returning to room temperature. The reaction solvent was distilled off under reduced pressure, and extracted with dichloromethane using Celite. The filtrate was concentrated, then dissolved in dichloromethane and dropped into hexane. The obtained yellow solid was collected by filtration, washed with hexane, and dried under reduced pressure. 699.4 mg of the target product was obtained. The yield was 82%. 1 The target transition metal compound (A-7) was identified by the results of H-NMR (CDCl3) and FD-MS. 1 H-NMR(270MHz,CDCl3)δ 6.10-6.02(3H,m),2.27(6H,s),1.55(27H,d, J=13.5Hz)ppm FD-MS: m / z=427.1 (M + )

[0174] [Synthesis Example 12] Synthesis of transition metal compound (A-12) (n-Butylcyclopentadienyl)Ti(N=P(t-Bu)3)Cl2 represented by the following formula (hereinafter also referred to as "transition metal compound (A-12)") was synthesized by the method described in Organometallics 2003, 22, 1937.

[0175] [ka]

[0176] [Synthesis Example 13] Synthesis of transition metal compound (A-13) (Pentafluorophenylmethylcyclopentadienyl)Ti(N=P(t-Bu)3)Cl2 (hereinafter also referred to as "transition metal compound (A-13)") represented by the following formula was synthesized by the method described in JP-A-2006-169521.

[0177] [ka]

[0178] <Preparation of solid support (S)> [Preparation Example 1] Preparation of solid support (S-1) A 270 L reactor equipped with a stirrer was used, and silica gel (manufactured by Fuji Silysia Chemical Ltd., average particle size 70 μm, specific surface area 340 m) was added under a nitrogen atmosphere. 2 / g, pore volume 1.3cm 3 / g 10 kg of the solid carrier (S-1) was suspended in 77 L of toluene and then cooled to 0-5°C. While maintaining the temperature in the system at 0-5°C, 19.4 L of a toluene solution of methylaluminoxane (3.5 mol / L in terms of Al atoms) was dropped into this suspension over 30 minutes. After contacting each added component for 30 minutes, the temperature in the system was raised to 95°C over 1.5 hours, and then contacted at 93-97°C for 4 hours. After that, the temperature was lowered to room temperature, the supernatant was removed by decantation, and the mixture was washed twice with toluene to obtain a toluene slurry of the solid carrier (S-1) with a total volume of 115 L. A part of this slurry was collected and analyzed, and the solid concentration was 123 g / L and the Al concentration was 0.62 mol / L.

[0179] [Preparation Example 2] Preparation of solid support (S-2) A solid aluminoxane compound was synthesized according to the method described in International Publication WO 2010 / 055652 (preliminary experiment 1 and Example 5), and used as the solid support (S) (hereinafter referred to as solid support (S-2)). However, in consideration of the safety of trimethylaluminum, such as ignition, the experiment was carried out at a concentration about 1 / 6 of the conditions disclosed in the document.

[0180] Specifically, 100 mL of a toluene solution of trimethylaluminum adjusted to 0.5 mol / L was charged into a glass reactor equipped with a stirrer. The solution was cooled to 15°C, and 2.18 g of benzoic acid was slowly added to it at a rate that kept the temperature of the solution below 25°C. Then, heat aging was performed at 50°C for 1 hour. At this time, the molar ratio of oxygen atoms of trimethylaluminum and benzoic acid was 1.40. The reaction solution was heated at 70°C for 4 hours, then heated at 60°C for 6 hours, and then cooled to room temperature once. Then, it was heated at 100°C for 8 hours to precipitate solid components. After cooling the solution to 30°C or less, 100 mL of hexane was added under stirring for washing. After standing for 30 minutes, 150 mL of the supernatant was removed, and another 150 mL of hexane was added under stirring. After standing for 15 minutes, 150 mL of the supernatant was removed, and another 150 mL of hexane was added under stirring. Finally, after leaving it to stand for 15 minutes, 180 mL of the supernatant was removed, and hexane was added to a total volume of 14.6 mL to obtain a hexane slurry of solid carrier (S-2). A part of the obtained slurry was sampled and analyzed, and the solid concentration was 41 g / L and the Al concentration was 0.58 mol / L. In addition, when the particles of the obtained solid carrier (S-2) were observed with a scanning electron microscope, the average particle diameter was 6.8 μm.

[0181] [Preparation Example 3] Preparation of solid support (S-3) A slurry of a solid aluminoxane compound was synthesized according to the method (Test Example A8) described in WO 2014 / 123212 pamphlet, and this was used as a solid support (S) (hereinafter referred to as solid support (S-3)). A part of the obtained slurry was sampled and analyzed, and the solid concentration was 68 g / L and the Al concentration was 0.98 mol / L. In addition, when the particles of the obtained solid support (S-3) were observed with a scanning electron microscope, the average particle size was 32 μm.

[0182] <Preparation of solid catalyst component (X)> [Preparation Example 4] Preparation of solid catalyst component (X-1) In a reactor equipped with a stirrer and having an internal volume of 200 mL, which had been thoroughly purged with nitrogen, 5.12 mL of toluene and 4.88 mL of the slurry of the solid support (S-2) obtained in Preparation Example 2 (solid weight 0.20 g) were charged under a nitrogen atmosphere. Next, 5.00 mL of a toluene solution of the transition metal compound (A-1) obtained in Synthesis Example 1 (10.0 μmol as Ti) was added, and the mixture was contacted at a system temperature of 20 to 25°C for 1 hour, after which the supernatant was removed by decantation. 10 mL of the supernatant was analyzed by ICP atomic emission spectroscopy (ICP-AES), and the Ti concentration in the supernatant was found to be below the lower limit of quantification (less than 0.021 mmol / L). The mixture was further washed twice with hexane. As a result, a slurry of the solid catalyst component (X-1) with a total volume of 20 mL was prepared.

[0183] [Preparation Examples 5 to 9] Preparation of solid catalyst components (X-2) to (X-6) Slurries of solid catalyst components (X-2) to (X-6) were prepared in the same manner as in Preparation Example 4, except that the transition metal compounds (A-2) to (A-6) obtained in Synthesis Examples 2 to 6 were used instead of the transition metal compound (A-1). The Ti concentrations in the supernatants were all below the lower limit of quantification (less than 0.021 mmol / L).

[0184] [Preparation Example 10] Preparation of solid catalyst component (X-7) In a reactor equipped with a stirrer and having an internal volume of 200 mL, which had been thoroughly purged with nitrogen, 7.06 mL of toluene and 2.94 mL of the slurry of the solid support (S-3) obtained in Preparation Example 3 (solid weight 0.20 g) were charged under a nitrogen atmosphere. Next, 5.00 mL of the toluene solution of the transition metal compound (A-1) obtained in Synthesis Example 1 (10.0 μmol as Ti) was added, and the mixture was contacted at a system temperature of 20 to 25°C for 1 hour, after which the supernatant was removed by decantation. 10 mL of the supernatant was analyzed by ICP-AES, and the Ti concentration in the supernatant was found to be below the lower limit of quantification (less than 0.021 mmol / L). The mixture was further washed twice with hexane. As a result, a slurry of the solid catalyst component (X-7) with a total volume of 20 mL was prepared.

[0185] [Preparation Example 11] Preparation of solid catalyst component (X-8) In a reactor equipped with a stirrer and having an internal volume of 200 mL, which had been thoroughly purged with nitrogen, 10.87 mL of toluene and 1.63 mL of the slurry of the solid support (S-1) obtained in Preparation Example 1 (solid weight 0.20 g) were charged under a nitrogen atmosphere. Next, 2.50 mL of the toluene solution of the transition metal compound (A-1) obtained in Synthesis Example 1 (5.0 μmol as Ti) was added, and the mixture was contacted at a system temperature of 20 to 25°C for 1 hour, after which the supernatant was removed by decantation. 10 mL of the supernatant was analyzed by ICP-AES, and the Ti concentration in the supernatant was found to be below the lower limit of quantification (less than 0.021 mmol / L). The mixture was further washed twice with hexane. As a result, a slurry of the solid catalyst component (X-8) with a total volume of 20 mL was prepared.

[0186] [Preparation Example 12] Preparation of solid catalyst component (X-9) A slurry of a solid catalyst component (X-9) was prepared in the same manner as in Preparation Example 11, except that the transition metal compound (A-4) obtained in Synthesis Example 4 was used instead of the transition metal compound (A-1). The Ti concentration in the supernatant was below the lower limit of quantification (less than 0.021 mmol / L).

[0187] [Preparation Example 13] Preparation of solid catalyst component (X-10) A slurry of a solid catalyst component (X-10) was prepared in the same manner as in Preparation Example 11, except that the transition metal compound (A-6) obtained in Synthesis Example 6 was used instead of the transition metal compound (A-1). The Ti concentration in the supernatant was below the lower limit of quantification (less than 0.021 mmol / L).

[0188] [Preparation Examples 14-15] Preparation of solid catalyst components (X-11)-(X-12) Slurries of solid catalyst components (X-11) to (X-12) were prepared in the same manner as in Preparation Example 11, except that the transition metal compounds (A-7) to (A-8) obtained in Synthesis Examples 7 to 8 were used instead of the transition metal compound (A-1). The Zr concentrations in the supernatants were all below the lower limit of quantification (less than 0.011 mmol / L).

[0189] [Preparation Examples 16-17] Preparation of solid catalyst components (X-13)-(X-14) Slurries of solid catalyst components (X-13) to (X-14) were prepared in the same manner as in Preparation Example 4, except that the transition metal compounds (A-9) to (A-10) obtained in Synthesis Examples 9 to 10 were used instead of the transition metal compound (A-1). The Zr concentrations in the supernatants were all below the lower limit of quantification (less than 0.011 mmol / L).

[0190] [Preparation Examples 18 to 20] Preparation of solid catalyst components (X-15) to (X-17) Slurries of solid catalyst components (X-15) to (X-17) were prepared in the same manner as in Preparation Example 4, except that the transition metal compounds (A-11) to (A-13) obtained in Synthesis Examples 11 to 13 were used instead of the transition metal compound (A-1). The Ti concentrations in the supernatants were all below the lower limit of quantification (less than 0.021 mmol / L).

[0191] <Evaluation of fouling in ethylene polymerization reaction> The polymerization reaction evaluations in the following Examples, Comparative Examples and Reference Examples were carried out using a 1-liter SUS autoclave equipped with a stirring blade. All the solvents used in this example were dehydrated solvents.

[0192] After the polymerization reaction was completed, the inside of the autoclave was cooled and depressurized, and the presence or absence of powder adhesion (fouling) to the autoclave walls and agitator blades, as well as the presence or absence of powder agglomeration, were determined. Powder adhesion refers to a state in which powder does not come off even when a hydrocarbon solvent such as heptane or hexane is poured into it, while powder agglomeration refers to a state in which many powder particles are physically or chemically bonded together, and some particles will come apart when a strong force is applied after the polymerization reaction, but some will not.

[0193] In particular, in the case of a polymerization reaction in which severe fouling or aggregation occurs, the number of rotations of the stirring blades, as measured by a rotation meter, decreases with the passage of polymerization time. The physical properties of the resulting polyethylene powder were measured by the methods described above.

[0194] [Reference example 1] In a SUS autoclave with an internal volume of 1 L that had been thoroughly purged with nitrogen, 500 mL of heptane was added under a nitrogen atmosphere, and then ethylene was passed through to saturate the reactor with ethylene. Next, 0.375 mmol of triisobutylaluminum and 30 mg of the solid content of the slurry of the solid catalyst component (X-11) obtained in Preparation Example 14 were added, and the temperature and pressure were raised to 80°C and 0.8 MPaG with ethylene, and a polymerization reaction was started at a rotation speed of 350 rpm.

[0195] Even after 90 minutes had passed since the start of polymerization, no decrease in the rotation speed was observed, and the reaction was stopped by cooling and depressurizing. When the inside of the autoclave was checked, no fouling or aggregation of polyethylene powder was observed on the autoclave wall or stirring blades.

[0196] [Reference example 2] A polymerization reaction was initiated in the same manner as in Reference Example 1, except that 20 mg of the slurry of the solid catalyst component (X-12) obtained in Preparation Example 15 was added in place of the solid catalyst component (X-11) as a solid content.

[0197] 90 minutes after the start of polymerization, no decrease in rotation speed was observed, and the reaction was stopped by cooling and depressurizing. When the inside of the autoclave was checked, no fouling or aggregation of polyethylene powder was observed on the autoclave wall or stirring blade.

[0198] [Comparative Example 1] A polymerization reaction was initiated in the same manner as in Reference Example 1, except that 20 mg of the slurry of the solid catalyst component (X-8) obtained in Preparation Example 11 was added in place of the solid catalyst component (X-11) as a solid content.

[0199] Since a decrease in the rotation speed was confirmed 15 minutes after the start of polymerization, it was determined that a normal stirring state was not being maintained, and the reaction was stopped by cooling and depressurizing. When the inside of the autoclave was checked, fouling on the autoclave wall and stirring blades and aggregation of polyethylene powder were found.

[0200] [Comparative Example 2] A polymerization reaction was initiated in the same manner as in Reference Example 1, except that 10 mg of the slurry of the solid catalyst component (X-9) obtained in Preparation Example 12 was added in place of the solid catalyst component (X-11) in terms of solid content.

[0201] Since a decrease in the rotation speed was confirmed 10 minutes after the start of polymerization, it was determined that a normal stirring state was not being maintained, and the reaction was stopped by cooling and depressurizing. When the inside of the autoclave was checked, fouling on the autoclave wall and stirring blades and aggregation of polyethylene powder were found.

[0202] [Comparative Example 3] A polymerization reaction was initiated in the same manner as in Reference Example 1, except that 50 mg of the slurry of the solid catalyst component (X-10) obtained in Preparation Example 13 was added as a solid content instead of the solid catalyst component (X-11).

[0203] As the rotation speed began to decrease 30 minutes after the start of polymerization, it was determined that normal stirring conditions were not being maintained, and the reaction was stopped by cooling and depressurizing. When the inside of the autoclave was checked, fouling on the autoclave walls and stirring blades and aggregation of polyethylene powder were found.

[0204] The results of Reference Examples 1 and 2 and Comparative Examples 1 to 3 show that the transition metal compound (A) having a cyclopentadienyl ligand and a ligand containing a Group 15 element (nitrogen) is more likely to cause fouling during polymerization than a transition metal compound containing only a cyclopentadienyl ligand.

[0205] [Examples 1 to 7] The polymerization reaction was started in the same manner as in Reference Example 1, except that the slurries of the solid catalyst components (X-1) to (X-7) obtained in Preparation Examples 4 to 10, respectively, were added as solid contents in the amounts shown in Table 4, instead of the solid catalyst component (X-11).

[0206] In all cases, no decrease in rotation speed was observed 90 minutes after the start of polymerization, and the reaction was stopped by cooling and depressurization. When the inside of the autoclave was checked, no fouling or aggregation of polyethylene powder was observed on the autoclave wall or stirring blades.

[0207] The presence or absence of fouling in Examples 1 to 7, Comparative Examples 1 to 3, and Reference Examples 1 and 2, and the intrinsic viscosities [η] of the ethylene polymers obtained in Examples 1 to 7 and Comparative Examples 1 to 3 are shown in Table 4. All of the ethylene polymers obtained in Examples 1 to 7 were ultra-high molecular weight polyethylenes having an [η] of 10 or more.

[0208] [Table 4]

[0209] The results of Examples 1 to 7 and Comparative Examples 1 to 3 show that when the solid catalyst components (X-1) to (X-7) which are olefin polymerization catalysts of the present invention using solid aluminoxane as the solid support (S) are used, fouling and powder aggregation during polymerization are less likely to occur compared to the cases where the solid supports (X-8) to (X-10) prepared by contacting aluminoxane with silica gel are used, even under conditions generally considered unfavorable for fouling, such as a small support particle size and a large amount of contact with the transition metal compound (A).

[0210] <Polymer obtained by ethylene polymerization reaction> [Example 8] In a SUS autoclave with a capacity of 1 liter, 500 milliliters of heptane was added under a nitrogen atmosphere, and ethylene was passed through to saturate the reactor with ethylene. Next, 0.375 mmol of triisobutylaluminum and 5.0 mg of the solid slurry of the solid catalyst component (X-1) obtained in Preparation Example 4 were added, and the temperature and pressure were raised to 75°C and 0.65 MPaG using an ethylene-hydrogen mixed gas with a hydrogen concentration of 0.10 vol%, and a polymerization reaction was carried out for 90 minutes. The obtained polymer was filtered and then vacuum-dried at 80°C for 10 hours to obtain 50.1 g of an ethylene-based polymer. The analytical results of the obtained ethylene-based polymer are shown in Table 5.

[0211] [Example 9] In a SUS autoclave with a capacity of 1 liter, 500 milliliters of heptane was added under a nitrogen atmosphere, and ethylene was passed through to saturate the reactor with ethylene. Next, 0.375 mmol of triisobutylaluminum and 10 mg of the solid slurry of the solid catalyst component (X-2) obtained in Preparation Example 5 were added, and the temperature and pressure were raised to 75°C and 0.65 MPaG using an ethylene-hydrogen mixed gas with a hydrogen concentration of 0.10 vol%, and a polymerization reaction was carried out for 90 minutes. The obtained polymer was filtered and then vacuum-dried at 80°C for 10 hours to obtain 34.9 g of an ethylene-based polymer. The analytical results of the obtained ethylene-based polymer are shown in Table 5.

[0212] [Example 10] In a SUS autoclave with a capacity of 1 liter, 500 milliliters of heptane was added under a nitrogen atmosphere, and ethylene was passed through to saturate the reactor with ethylene. Next, 0.375 mmol of triisobutylaluminum and 6.0 mg of the solid slurry of the solid catalyst component (X-3) obtained in Preparation Example 6 were added, and the temperature and pressure were raised to 75°C and 0.65 MPaG using an ethylene-hydrogen mixed gas with a hydrogen concentration of 0.10 vol%, and a polymerization reaction was carried out for 90 minutes. The obtained polymer was filtered and then vacuum-dried at 80°C for 10 hours to obtain 37.8 g of an ethylene-based polymer. The analytical results of the obtained ethylene-based polymer are shown in Table 5.

[0213] [Comparative Example 4] In a SUS autoclave with a capacity of 1 liter, 500 milliliters of heptane was added under a nitrogen atmosphere, and ethylene was passed through to saturate the reactor with ethylene. Next, 0.375 mmol of triisobutylaluminum and 6.0 mg of the solid slurry of the solid catalyst component (X-13) obtained in Preparation Example 16 were added, and the temperature and pressure were raised to 75°C and 0.65 MPaG using an ethylene-hydrogen mixed gas with a hydrogen concentration of 0.10 vol%, and a polymerization reaction was carried out for 90 minutes. The obtained polymer was filtered and then vacuum-dried at 80°C for 10 hours to obtain 122.5 g of an ethylene-based polymer. The analytical results of the obtained ethylene-based polymer are shown in Table 5.

[0214] [Comparative Example 5] In a SUS autoclave with a capacity of 1 liter, 500 milliliters of heptane was added under a nitrogen atmosphere, and ethylene was passed through to saturate the reactor with ethylene. Next, 0.375 mmol of triisobutylaluminum and 15 mg of the solid slurry of the solid catalyst component (X-14) obtained in Preparation Example 17 were added, and the temperature and pressure were raised to 75°C and 0.65 MPaG using an ethylene-hydrogen mixed gas with a hydrogen concentration of 0.75 vol%, and a polymerization reaction was carried out for 90 minutes. The obtained polymer was filtered and then vacuum-dried at 80°C for 10 hours to obtain 62.5 g of an ethylene-based polymer. The analytical results of the obtained ethylene-based polymer are shown in Table 5.

[0215] [Table 5]

[0216] From the results of Examples 8 to 10 and Comparative Examples 4 to 5, the ethylene homopolymer obtained by homopolymerization of ethylene using the olefin polymerization catalyst of the present invention is characterized by a higher molecular weight (MFR, [η]) and a higher molecular weight density than the case where a transition metal compound (A) having no ligand containing an element of Group 15 or 16 of the periodic table is used. This is because there are fewer methyl and ethyl branches. In addition, there is a characteristic that the amount of double bonds such as vinyl and vinylidene is also smaller.

[0217] [Examples 11 to 13] The polymerization reaction was started in the same manner as in Reference Example 1, except that the slurries of the solid catalyst components (X-15) to (X-17) obtained in Preparation Examples 18 to 20, respectively, were added as solid contents in the amounts shown in Table 6, instead of the solid catalyst component (X-11).

[0218] In all cases, no decrease in rotation speed was observed 90 minutes after the start of polymerization, and the reaction was stopped by cooling and depressurization. When the inside of the autoclave was checked, no fouling or aggregation of polyethylene powder was observed on the autoclave wall or stirring blades.

[0219] The presence or absence of fouling and the intrinsic viscosity [η] of the obtained ethylene polymers in Examples 11 to 13 are shown in Table 6, together with the results of Example 1 and Comparative Examples 1 to 3. The ethylene polymers obtained in Examples 11 to 13 were all ultra-high molecular weight polyethylenes having an [η] of 10 or more.

[0220] [Table 6]

[0221] The results of Examples 11 to 13 and Comparative Examples 1 to 3 show that when the solid catalyst components (X-15) to (X-17), which are olefin polymerization catalysts of the present invention using solid aluminoxane as the solid support (S), are used, fouling and powder aggregation during polymerization are less likely to occur compared to the cases where the solid supports (X-8) to (X-10) prepared by contacting aluminoxane with silica gel are used, even under conditions generally considered unfavorable for fouling, such as a small support particle size and a large amount of contact with the transition metal compound (A).

Claims

1. An olefin polymerization catalyst comprising the following component (A) and the following solid support (S): Component (A): A transition metal compound represented by the following general formula [1] or [2]. [Case 1] [Case 2] (In the general formulas [1] and [2], M is a transition metal atom of Group 4 of the periodic table, n is an integer from 1 to 4 satisfying the valence of M; X is a hydrogen atom, a halogen atom, a hydrocarbon group, an anionic ligand or a neutral ligand capable of coordinating with a lone electron pair, the anionic ligand being a halogen-containing group, a silicon-containing group, an oxygen-containing group, a sulfur-containing group, a nitrogen-containing group, a phosphorus-containing group, a boron-containing group, an aluminum-containing group or a conjugated diene-based divalent derivative group, when n is 2 or more, a plurality of groups represented by X may be the same or different and may be bonded to each other to form a ring, Cp is a cyclopentadienyl ligand which may have a substituent, and adjacent substituents may be bonded to each other to form a ring which may have a substituent; L is an atom selected from the elements of Groups 15 and 16 of the Periodic Table; P is a phosphorus atom; The solid lines are covalent or coordinate bonds, and the dotted lines are covalent bonds that exist when L is an atom of a Group 15 element. y is 2 when L is an atom of a Group 15 element, and is 3 when L is an atom of a Group 16 element; z is 3 when L is an atom of a Group 15 element, and is 4 when L is an atom of a Group 16 element; Each R is independently a hydrogen atom, a hydrocarbon group having 1 to 40 carbon atoms, a halogen-containing group, a silicon-containing group, an oxygen-containing group, a nitrogen-containing group, or a sulfur-containing group, and may be the same or different. Adjacent R may be bonded to each other to form a ring or a bicyclo ring which may have a substituent. Solid support (S): a solid aluminoxane compound.

2. The olefin polymerization catalyst according to claim 1, characterized in that the solid aluminoxane compound has an average particle size of 0.01 to 50,000 μm.

3. The olefin polymerization catalyst according to claim 1, characterized in that the solid aluminoxane compound has an average particle size of 1 to 1000 μm.

4. The olefin polymerization catalyst according to claim 1, wherein the solid aluminoxane compound has an average particle size of 1 to 200 μm.

5. 2. The olefin polymerization catalyst according to claim 1, wherein L is an atom of an element in Group 15 of the periodic table.

6. 2. The olefin polymerization catalyst according to claim 1, wherein M is a titanium atom.

7. A method for producing an olefin polymer, which comprises polymerizing an olefin in the presence of the olefin polymerization catalyst according to any one of claims 1 to 6.

Citation Information

Patent Citations

  • Olefin polymerization catalyst component

    JP1999071420A

  • Catalysts with ketimide ligands

    JP2001516776A

  • Carrier-type metallocene catalyst and method for preparing the same

    JP2002179721A

  • Cyclopentadienyl / phosphinimine catalysts with only one activatable ligand

    JP2002521500A

  • Method for manufacturing carrier material for ethylene (Co)Polymerization catalyst

    JP2003327611A