Polyethylene resin composition

The addition of an organic phosphate ester salt compound to a polyethylene resin and liquid crystal polymer blend addresses delamination and gas barrier issues, enhancing tape peeling resistance and mechanical properties for improved container performance.

JP7558771B2Active Publication Date: 2024-10-01UENO PHARMA CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2020194364
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-11-24
Publication Date
2024-10-01
Estimated Expiration
2040-11-24

AI Technical Summary

Technical Problem

Polyethylene resin containers suffer from delamination issues and inferior gas barrier properties, which can lead to contamination when used for long-term storage, especially in food and drink containers.

Method used

A polyethylene resin composition is developed by adding an organic phosphate ester salt compound to a blend of polyethylene resin and liquid crystal polymer, enhancing moldability, mechanical strength, and tape peeling resistance while maintaining heat resistance.

Benefits of technology

The composition improves tape peeling resistance and maintains mechanical strength and heat resistance, making it suitable for applications like injection molded products, films, sheets, fibers, and blow molded articles.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007558771000001
    Figure 0007558771000001
  • Figure 0007558771000002
    Figure 0007558771000002
  • Figure 0007558771000003
    Figure 0007558771000003
Patent Text Reader

Abstract

To provide a polyethylene resin composition which is excellent in moldability, mechanical strength and heat resistance, and improves tape peeling resistance of a molded article.SOLUTION: A polyethylene resin composition contains, with respect to 100 pts.mass of a polyethylene resin, 1-100 pts.mass of a liquid crystal polymer, and 0.001-5 pts.mass of an organic phosphate salt compound.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a polyethylene resin composition having excellent tape peeling resistance, and to a molded article made from the polyethylene resin composition. [Background technology]

[0002] Polyethylene resin has excellent moldability and is therefore useful as a molding material for food packaging containers, automobile parts, daily necessities, electrical and electronic parts, building parts, machine parts, and more. In particular, because of their light weight and excellent impact resistance, they are widely used as packaging containers for food, cosmetics, detergents and various chemicals.

[0003] However, resin containers have inferior gas barrier properties compared to metal or glass containers and are therefore unsuitable for long-term storage.

[0004] In order to improve the gas barrier properties of polyethylene resin, a molded structure with excellent gas barrier properties, heat resistance, mechanical strength, etc., has been proposed by melt molding a blend containing high-density polyethylene and liquid crystal polyester (Patent Document 1). [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Japanese Patent Application Publication No. 5-309692 Summary of the Invention [Problem to be solved by the invention]

[0006] However, the molded structure described in Patent Document 1 may experience layer peeling on the surface of the molded product, and when such a molded product is used as a container for eating and drinking, there is a risk that the peeled resin layer may become mixed into the contents.

[0007] An object of the present invention is to provide a polyethylene resin composition which is excellent in moldability, mechanical strength and heat resistance and which produces a molded article with improved tape peel resistance. [Means for solving the problem]

[0008] Means for Solving the Problems In view of the above, the present inventors have intensively studied the physical properties of polyethylene resin compositions and, as a result, have found that by adding an organic phosphate ester salt compound to a blend composition of a polyethylene resin and a liquid crystal polymer, the tape peel resistance of the obtained molded article is improved while maintaining the moldability, mechanical strength and heat resistance, and have thus completed the present invention.

[0009] That is, the present invention includes the following preferred embodiments. [1] A polyethylene resin composition containing 1 to 100 parts by mass of a liquid crystal polymer and 0.001 to 5 parts by mass of an organic phosphate ester salt compound relative to 100 parts by mass of a polyethylene resin. [2] The polyethylene resin composition according to [1], wherein the organic phosphate ester salt compound is an organic phosphate ester salt compound containing one or more metal atoms selected from lithium, sodium, potassium, magnesium, calcium, barium, and aluminum. [3] The polyethylene resin composition according to [1] or [2], further comprising 0.1 to 30 parts by mass of a functional group-containing polyolefin resin per 100 parts by mass of the liquid crystal polymer. [4] The polyethylene resin composition according to [3], wherein the functional group-containing polyolefin resin is an acid-modified polyolefin resin and / or an epoxy group-containing polyolefin resin. [5] The polyethylene resin composition according to any one of [1] to [4], wherein the liquid crystal polymer has a crystalline melting temperature of lower than 260°C. [6] The liquid crystal polymer is represented by the formula (I) and the formula (II) [ka] The polyethylene resin composition according to any one of [1] to [5], which is a wholly aromatic liquid crystal polyester resin containing a repeating unit represented by the following formula: [7] The liquid crystal polymer is represented by the formulas (I) to (IV) [ka] [In the formula, Ar1 and Ar2 each represent a divalent aromatic group.] The polyethylene resin composition according to any one of [1] to [6], which is a wholly aromatic liquid crystal polyester resin composed of a repeating unit represented by the following formula: [8] The repeating units represented by the formulae (III) to (IV) are each independently represented by the formulae (1) to (4). [ka] The polyethylene resin composition according to [7], wherein each of the repeating units is one or more types selected from aromatic groups represented by the following formula: [9] The organic phosphate ester salt compound is represented by the formula (V) [ka] (In the formula, R 1 is a divalent hydrocarbon group having 1 to 10 carbon atoms, R 2 and R 3 are each independently a hydrogen atom or a hydrocarbon group having 1 to 10 carbon atoms, M is a monovalent to trivalent metal atom, and n is an integer of 1 to 3. and / or formula (VI) [ka] [In the formula, R 1 is a divalent hydrocarbon group having 1 to 10 carbon atoms, R 2 and R 3 are each independently a hydrogen atom or a hydrocarbon group having 1 to 10 carbon atoms, and m is 1 or 2. The polyethylene resin composition according to any one of [1] to [8], wherein the compound is represented by the following formula:

[10] A molded article made from the polyethylene resin composition according to any one of [1] to [9].

[11] The molded article according to

[10] , which is an injection molded article, a film, a sheet, a fiber or a blown molded article. Effect of the Invention

[0010] The polyethylene resin composition of the present invention has excellent moldability, mechanical strength, and heat resistance, and also has the effect of improving tape peel resistance, and is therefore useful for applications such as injection molded articles, films, sheets, fibers, and blow molded articles. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] The polyethylene resin used in the present invention is not particularly limited, but examples thereof include low-density polyethylene, linear low-density polyethylene, high-density polyethylene, etc. These may be used alone or in combination of two or more kinds.

[0012] Among these, high density polyethylene is preferred from the viewpoint of excellent moldability and mechanical strength.

[0013] The polyethylene resin used in the present invention is an ethylene polymer made mainly from ethylene, and may be an ethylene homopolymer or a copolymer of ethylene and an α-olefin having 3 to 20 carbon atoms.

[0014] Examples of the α-olefin having 3 to 20 carbon atoms include propylene, 1-butene, 1-pentene, 4-methyl-1-pentene, 1-hexene, 4-methyl-1-hexene, 1-heptene, 1-octene, 1-nonene, 1-decene, 1-dodecene, 1-tetradecene, 1-octadecene, and 1-eicosene.

[0015] The α-olefins having 3 to 20 carbon atoms may be used alone or in combination of two or more kinds.

[0016] Specific examples of copolymers of ethylene and an α-olefin having 3 to 20 carbon atoms include an ethylene-propylene copolymer, an ethylene-1-butene copolymer, an ethylene-1-hexene copolymer, an ethylene-1-octene copolymer, an ethylene-1-butene-1-hexene copolymer, and an ethylene-1-butene-1-octene copolymer.

[0017] The copolymer of ethylene and an α-olefin may be a random copolymer or a block copolymer.

[0018] The polyethylene resin used in the present invention may be a single ethylene polymer polymerized in a single polymerization tank, or a mixture of two or more ethylene polymers. The mixture can be obtained by a method of melt kneading using a single-screw or multi-screw extruder, or a method of multi-stage polymerization in two or more polymerization tanks under different conditions.

[0019] In the copolymer of ethylene and an α-olefin, the content of structural units provided by the α-olefin in the copolymer is preferably 5 mol % or less, and more preferably 2 mol % or less, in order to provide excellent thermal stability to the polyethylene resin composition of the present invention.

[0020] That is, the content of ethylene structural units in the polyethylene resin is preferably 95 mol % or more, and more preferably 98 mol % or more.

[0021] The melt flow rate (MFR) of the polyethylene resin used in the present invention is preferably from 0.1 to 80 g / 10 min, more preferably from 0.3 to 60 g / 10 min, and even more preferably from 0.5 to 50 g / 10 min.

[0022] Here, the MFR is a value measured at 190° C. under a load of 2.16 kg in accordance with JIS K 6922-1.

[0023] If the MFR of the polyethylene resin is less than 0.1 g / 10 min, the fluidity of the polyethylene resin composition tends to decrease, whereas if it exceeds 80 g / 10 min, mechanical strength such as tensile strength and impact strength tend to decrease.

[0024] The polyethylene resin used in the present invention has a weight average molecular weight (Mw) / number average molecular weight (Mn) ratio, as determined by gel permeation chromatography (GPC), of preferably 1.5 to 20, more preferably 1.7 to 15, and even more preferably 2.0 to 10.

[0025] If the Mw / Mn of the polyethylene resin is less than 1.5, the fluidity of the polyethylene resin composition tends to be insufficient, and if the Mw / Mn of the polyethylene resin exceeds 20, the mechanical strength such as tensile strength tends to be reduced.

[0026] The method for producing the polyethylene resin used in the present invention is not particularly limited, but it can be produced, for example, by the method shown below.

[0027] When the polyethylene resin is a high-density polyethylene, it is produced by (co)polymerizing ethylene or ethylene and an α-olefin using a catalyst such as a transition metal compound such as titanium or zirconium, a Ziegler catalyst made of a magnesium compound, a Phillips catalyst represented by a chromium oxide-based catalyst, or a metallocene catalyst having at least one cyclopentadienyl group or substituted cyclopentadienyl group in a transition metal compound such as zirconium, hafnium, or titanium, in a process such as a gas phase method, a solution method, a high-pressure method, or a slurry method.

[0028] Furthermore, when the polyethylene resin is a linear low-density polyethylene, it is produced by copolymerizing ethylene and an α-olefin using a catalyst such as the Ziegler catalyst, the Phillips catalyst, or the metallocene catalyst through a process such as a gas phase method, a solution method, a high-pressure method, or a slurry method.

[0029] Furthermore, when the polyethylene resin is a low-density polyethylene, it is produced, for example, by polymerizing ethylene or copolymerizing ethylene and an α-olefin using a process such as a high-pressure radical polymerization method using a radical generator such as a peroxide as a polymerization initiator.

[0030] The polymerization may be carried out batchwise or continuously, and may be a one-stage production method or a multi-stage polymerization method in which the polymer is produced in two or more stages under different conditions.

[0031] The polyethylene resin composition of the present invention contains 1 to 100 parts by mass, preferably 2 to 80 parts by mass, more preferably 3 to 65 parts by mass, and further preferably 5 to 45 parts by mass of a liquid crystal polymer per 100 parts by mass of polyethylene resin.

[0032] If the content of the liquid crystal polymer is less than 1 part by mass, the mechanical strength and heat resistance of the resin composition will be insufficient, whereas if the content of the liquid crystal polymer is more than 100 parts by mass, the flexibility and toughness of the polyethylene resin will be impaired and the composition will be unsuitable for blow molding or film processing.

[0033] The liquid crystal polymer (hereinafter also referred to as LCP) used in the polyethylene resin composition of the present invention is a polyester or polyesteramide that forms an anisotropic molten phase, and is not particularly limited as long as it is what is called a thermotropic liquid crystal polyester or a thermotropic liquid crystal polyesteramide in the relevant technical field.

[0034] The nature of the anisotropic molten phase can be confirmed by conventional polarized light examination using crossed polarizers. More specifically, the anisotropic molten phase can be confirmed by observing the sample on a Leitz hot stage under nitrogen atmosphere at 40x magnification using a Leitz polarized microscope. The liquid crystal polymers of the present invention are optically anisotropic, i.e., transmit light when examined between crossed polarizers. If the sample is optically anisotropic, polarized light will be transmitted even when it is stationary.

[0035] The liquid crystal polymer used in the present invention preferably has a crystalline melting temperature measured by a differential scanning calorimeter of less than 260°C, more preferably 160 to 250°C, even more preferably 170 to 240°C, and particularly preferably 180 to 230°C.

[0036] In the present specification and claims, the "crystalline melting temperature" is determined from the crystalline melting temperature peak temperature when measured at a heating rate of 20°C / min using a differential scanning calorimeter (hereinafter abbreviated as DSC). More specifically, after observing the endothermic peak temperature (Tm1) observed when a sample of a liquid crystal polymer is measured under a heating condition of 20°C / min from room temperature, the sample is held at a temperature 20 to 50°C higher than Tm1 for 10 minutes, and then cooled to room temperature under a cooling condition of 20°C / min, and then measured again under a heating condition of 20°C / min. The temperature showing the peak top is taken as the crystalline melting temperature of the liquid crystal polymer. For example, a Seiko Instruments Inc. Exstar6000 or the like can be used as a measuring instrument.

[0037] Examples of the polymerizable monomers constituting the liquid crystal polymer used in the present invention include aromatic hydroxycarboxylic acids, aromatic dicarboxylic acids, aromatic diols, aromatic aminocarboxylic acids, aromatic hydroxyamines, aromatic diamines, aliphatic diols, and aliphatic dicarboxylic acids. The polymerizable monomers constituting the liquid crystal polymer may be one of these compounds or a combination of two or more compounds, but it is preferable to include at least one polymerizable monomer having a hydroxy group and a carboxyl group.

[0038] The polymerizable monomer constituting the structural unit of the liquid crystal polymer may be an oligomer formed by bonding one or more of the above compounds, that is, an oligomer constituted by one or more of the above compounds.

[0039] Specific examples of aromatic hydroxycarboxylic acids include 4-hydroxybenzoic acid, 3-hydroxybenzoic acid, 2-hydroxybenzoic acid, 6-hydroxy-2-naphthoic acid, 5-hydroxy-2-naphthoic acid, 7-hydroxy-2-naphthoic acid, 3-hydroxy-2-naphthoic acid, 4'-hydroxyphenyl-4-benzoic acid, 3'-hydroxyphenyl-4-benzoic acid, 4'-hydroxyphenyl-3-benzoic acid, and their alkyl, alkoxy or halogen-substituted derivatives, as well as their acylated derivatives, ester derivatives, acid halides and other ester-forming derivatives. Among these, from the viewpoint of the heat resistance, mechanical strength and ease of adjusting the melting point of the resulting liquid crystal polymer, one or more compounds selected from the group consisting of 4-hydroxybenzoic acid and 6-hydroxy-2-naphthoic acid are preferred.

[0040] Specific examples of aromatic dicarboxylic acids include terephthalic acid, isophthalic acid, 2,6-naphthalenedicarboxylic acid, 1,6-naphthalenedicarboxylic acid, 2,7-naphthalenedicarboxylic acid, 4,4'-dicarboxybiphenyl, 3,4'-dicarboxybiphenyl, and 4,4"-dicarboxyterphenyl, as well as their alkyl, alkoxy, or halogen-substituted derivatives and their ester derivatives, such as acid halides. Among these, from the viewpoint of effectively enhancing the heat resistance of the resulting liquid crystal polymer, one or more compounds selected from the group consisting of terephthalic acid, isophthalic acid, and 2,6-naphthalenedicarboxylic acid are preferred, and terephthalic acid and 2,6-naphthalenedicarboxylic acid are more preferred.

[0041] Specific examples of aromatic diols include hydroquinone, resorcin, 2,6-dihydroxynaphthalene, 2,7-dihydroxynaphthalene, 1,6-dihydroxynaphthalene, 3,3'-dihydroxybiphenyl, 3,4'-dihydroxybiphenyl, 4,4'-dihydroxybiphenyl, 4,4'-dihydroxybiphenyl ether, and 2,2'-dihydroxybinaphthyl, their alkyl, alkoxy or halogen substitution products, and their acylated derivatives. Among these, from the viewpoint of excellent reactivity during polymerization, one or more compounds selected from the group consisting of hydroquinone, resorcin, 4,4'-dihydroxybiphenyl, and 2,6-dihydroxynaphthalene are preferred, and one or more compounds selected from the group consisting of hydroquinone, 4,4'-dihydroxybiphenyl, and 2,6-dihydroxynaphthalene are more preferred.

[0042] Specific examples of aromatic aminocarboxylic acids include 4-aminobenzoic acid, 3-aminobenzoic acid, 6-amino-2-naphthoic acid, alkyl, alkoxy or halogen substituted derivatives thereof, and ester-forming derivatives thereof such as acylation products, ester derivatives and acid halides.

[0043] Specific examples of aromatic hydroxyamines include 4-aminophenol, N-methyl-4-aminophenol, 3-aminophenol, 3-methyl-4-aminophenol, 4-amino-1-naphthol, 4-amino-4'-hydroxybiphenyl, 4-amino-4'-hydroxybiphenyl ether, 4-amino-4'-hydroxybiphenylmethane, 4-amino-4'-hydroxybiphenyl sulfide, and 2,2'-diaminobinaphthyl, their alkyl, alkoxy or halogen-substituted products, and their acylated products and other ester-forming derivatives. Among these, 4-aminophenol is preferred from the viewpoint of easily achieving a balance between the heat resistance and mechanical strength of the resulting liquid crystal polymer.

[0044] Specific examples of aromatic diamines include amide-forming derivatives such as 1,4-phenylenediamine, 1,3-phenylenediamine, 1,5-diaminonaphthalene, 1,8-diaminonaphthalene, alkyl, alkoxy or halogen-substituted derivatives thereof, and acylated derivatives thereof.

[0045] Specific examples of the aliphatic diol include ethylene glycol, 1,4-butanediol, 1,6-hexanediol, and acylated products thereof. In addition, a polymer containing an aliphatic diol, such as polyethylene terephthalate or polybutylene terephthalate, may be reacted with the aromatic oxycarboxylic acid, aromatic dicarboxylic acid, aromatic diol, and their acylated products, ester derivatives, acid halides, etc.

[0046] Specific examples of aliphatic dicarboxylic acids include oxalic acid, malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, dodecanedioic acid, tetradecanedioic acid, fumaric acid, maleic acid, 1,4-cyclohexanedicarboxylic acid, and hexahydroterephthalic acid. Among these, oxalic acid, succinic acid, adipic acid, suberic acid, sebacic acid, dodecanedioic acid, and 1,4-cyclohexanedicarboxylic acid are preferred from the viewpoint of excellent reactivity during polymerization.

[0047] The polymerizable monomer forming the constitutional unit of the liquid crystal polymer in the present invention may contain, as other copolymerization components, dihydroxyterephthalic acid, 4-hydroxyisophthalic acid, 5-hydroxyisophthalic acid, trimellitic acid, 1,3,5-benzenetricarboxylic acid, pyromellitic acid, or their alkyl, alkoxy or halogen-substituted derivatives, as well as their acylated derivatives, ester derivatives, acid halides, and other ester-forming derivatives, or aromatic diols and aromatic dicarboxylic acids, within the scope of the present invention. The amount of these polymerizable monomers used is preferably 10 mol % or less based on the total constitutional units constituting the liquid crystal polymer.

[0048] In the present invention, the liquid crystal polymer may contain a thioester bond, provided that the object of the present invention is not impaired. Polymerizable monomers that provide such bonds include aromatic mercaptocarboxylic acids, aromatic dithiols, and hydroxy aromatic thiols. The content of these polymerizable monomers is preferably 10 mol % or less based on the total constitutional units that constitute the liquid crystal polymer.

[0049] Polymers combining these repeating units include those that form an anisotropic molten phase and those that do not, depending on the monomer composition, composition ratio, and sequence distribution of each repeating unit in the polymer. However, the liquid crystal polymers used in the present invention are limited to those that form an anisotropic molten phase.

[0050] As the liquid crystal polymer used in the present invention, a wholly aromatic liquid crystal polyester resin containing repeating units represented by formula (I) and formula (II) is preferably used because of its excellent fluidity and mechanical properties. [ka]

[0051] As the liquid crystal polymer used in the present invention, a wholly aromatic liquid crystal polyester resin composed of repeating units represented by formulae (I) and (II) is preferably used because of its excellent fluidity and mechanical properties.

[0052] Furthermore, as the liquid crystal polymer used in the present invention, a wholly aromatic liquid crystal polyester resin composed of repeating units represented by formulas (I) to (IV) is preferably used because of its excellent fluidity and mechanical properties. [ka] [In the formula, Ar1 and Ar2 each represent a divalent aromatic group.]

[0053] Here, each of formula (III) and formula (IV) may contain multiple types of Ar1 and Ar2. That is, the repeating unit represented by formula (III) may be multiple repeating units such as a repeating unit having one type of Ar1 and a repeating unit having another type of Ar1, and similarly, the repeating unit represented by formula (IV) may be multiple repeating units such as a repeating unit having one type of Ar2 and a repeating unit having another type of Ar2. In addition, the "aromatic group" refers to an aromatic group that is a 6-membered monocyclic or fused ring having two rings.

[0054] In terms of excellent gas barrier properties and mechanical properties, it is more preferable that the repeating units represented by formulas (III) to (IV) are such that Ar1 and Ar2 are each independently one or more repeating units selected from the aromatic groups represented by the following formulas (1) to (4). It is particularly preferable that Ar1 is an aromatic group represented by formula (1) and / or formula (4), and Ar2 is an aromatic group represented by formula (1) and / or formula (3). [ka]

[0055] In addition, the liquid crystal polymer used in the present invention may be a mixture of a wholly aromatic liquid crystal polyester resin composed of repeating units represented by formula (I) and formula (II) and a wholly aromatic liquid crystal polyester resin composed of repeating units represented by formulas (I) to (IV).

[0056] Specific examples of the combination of polymerizable monomers forming the structural units of the liquid crystal polymer of the present invention include the following. 1) 4-hydroxybenzoic acid / 6-hydroxy-2-naphthoic acid, 2) 4-hydroxybenzoic acid / terephthalic acid / 4,4'-dihydroxybiphenyl, 3) 4-hydroxybenzoic acid / terephthalic acid / isophthalic acid / 4,4'-dihydroxybiphenyl, 4) 4-hydroxybenzoic acid / terephthalic acid / isophthalic acid / 4,4'-dihydroxybiphenyl / hydroquinone, 5) 4-hydroxybenzoic acid / terephthalic acid / hydroquinone, 6) 6-hydroxy-2-naphthoic acid / terephthalic acid / hydroquinone, 7) 4-hydroxybenzoic acid / 6-hydroxy-2-naphthoic acid / terephthalic acid / 4,4'-dihydroxybiphenyl, 8) 6-hydroxy-2-naphthoic acid / terephthalic acid / 4,4'-dihydroxybiphenyl, 9) 4-hydroxybenzoic acid / 6-hydroxy-2-naphthoic acid / terephthalic acid / hydroquinone, 10) 4-hydroxybenzoic acid / 6-hydroxy-2-naphthoic acid / terephthalic acid / hydroquinone / 4,4'-dihydroxybiphenyl, 11) 4-hydroxybenzoic acid / 2,6-naphthalenedicarboxylic acid / 4,4'-dihydroxybiphenyl, 12) 4-hydroxybenzoic acid / terephthalic acid / 2,6-naphthalenedicarboxylic acid / hydroquinone, 13) 4-hydroxybenzoic acid / 2,6-naphthalenedicarboxylic acid / hydroquinone, 14) 4-hydroxybenzoic acid / 6-hydroxy-2-naphthoic acid / 2,6-naphthalenedicarboxylic acid / hydroquinone, 15) 4-hydroxybenzoic acid / terephthalic acid / 2,6-naphthalenedicarboxylic acid / hydroquinone / 4,4'-dihydroxybiphenyl, 16) 4-Hydroxybenzoic acid / terephthalic acid / 4-aminophenol, 17) 6-Hydroxy-2-naphthoic acid / terephthalic acid / 4-aminophenol, 18) 4-Hydroxybenzoic acid / 6-hydroxy-2-naphthoic acid / terephthalic acid / 4-aminophenol, 19) 4-Hydroxybenzoic acid / terephthalic acid / 4,4'-dihydroxybiphenyl / 4-aminophenol, 20) 4-hydroxybenzoic acid / terephthalic acid / ethylene glycol, 21) 4-hydroxybenzoic acid / terephthalic acid / 4,4'-dihydroxybiphenyl / ethylene glycol, 22) 4-hydroxybenzoic acid / 6-hydroxy-2-naphthoic acid / terephthalic acid / ethylene glycol, 23) 4-hydroxybenzoic acid / 6-hydroxy-2-naphthoic acid / terephthalic acid / 4,4'-dihydroxybiphenyl / ethylene glycol, 24) 4-Hydroxybenzoic acid / terephthalic acid / 2,6-naphthalenedicarboxylic acid / 4,4'-dihydroxybiphenyl. 25) 4-Hydroxybenzoic acid / 6-hydroxy-2-naphthoic acid / isophthalic acid / 2,6-naphthalenedicarboxylic acid / 4,4'-dihydroxybiphenyl.

[0057] Among these, wholly aromatic liquid crystal polyester resins consisting of structural units derived from polymerizable monomers of 1), 9), 10), 14) or 25) are preferred, and wholly aromatic liquid crystal polyester resins consisting of structural units derived from polymerizable monomers of 1), 9) or 25) are more preferred.

[0058] The above liquid crystal polymers may be used alone or in combination of two or more liquid crystal polymers.

[0059] The method for producing the liquid crystal polymer used in the present invention will now be described.

[0060] There is no particular limitation on the method for producing the liquid crystal polymer used in the present invention, and the liquid crystal polymer can be obtained by subjecting a polymerizable monomer to a known polycondensation method for forming an ester bond or an amide bond, such as a molten acidolysis method or a slurry polymerization method.

[0061] The melt acidolysis method is a preferred method for preparing the liquid crystal polymers used in the present invention. This method involves first heating the polymerizable monomers to form a molten solution of the reactants, followed by a polycondensation reaction to obtain a molten polymer. A vacuum may be applied to facilitate removal of volatile by-products (e.g., acetic acid, water, etc.) produced during the final stage of condensation.

[0062] A slurry polymerization process is a process in which polymerizable monomers are reacted in the presence of a heat exchange fluid, resulting in a solid product suspended in the heat exchange medium.

[0063] In either the molten acidolysis method or the slurry polymerization method, the polymerizable monomer used in producing the liquid crystal polymer can also be subjected to the reaction at room temperature in a modified form in which the hydroxyl group and / or amino group is acylated, i.e., a lower acylated product.

[0064] The lower acyl group preferably has 2 to 5 carbon atoms, more preferably 2 or 3. In a preferred embodiment of the present invention, an acetylated product of the polymerizable monomer is subjected to the reaction.

[0065] The lower acylated product of the polymerizable monomer may be a product previously synthesized by separate acylation, or may be produced in the reaction system by adding an acylating agent such as acetic anhydride to the polymerizable monomer during the production of the liquid crystal polymer.

[0066] In either the molten acidolysis method or the slurry polymerization method, the polycondensation reaction is carried out at a temperature of 150 to 400° C., preferably 250 to 370° C., under normal pressure and / or reduced pressure, and a catalyst may be used as necessary.

[0067] Specific examples of catalysts include organotin compounds such as dialkyltin oxides (e.g., dibutyltin oxide) and diaryltin oxides; titanium dioxide; antimony trioxide; organotitanium compounds such as alkoxytitanium silicates and titanium alkoxides; alkali and alkaline earth metal salts of carboxylic acids (e.g., potassium acetate, sodium acetate); and gaseous acid catalysts such as Lewis acids (e.g., boron trifluoride) and hydrogen halides (e.g., hydrogen chloride).

[0068] When a catalyst is used, the amount of the catalyst is preferably 1 to 1000 ppm, more preferably 2 to 100 ppm, based on the total amount of polymerizable monomers.

[0069] The liquid crystal polymer thus obtained by the polycondensation reaction is usually withdrawn in a molten state from a polymerization reaction vessel and then processed into pellets, flakes, or powder.

[0070] The polyethylene resin composition of the present invention contains 0.001 to 5 parts by mass, preferably 0.01 to 3 parts by mass, more preferably 0.05 to 2 parts by mass, and even more preferably 0.1 to 1 part by mass of an organic phosphate salt compound per 100 parts by mass of polyethylene resin.

[0071] When the content of the organic phosphate ester salt compound is less than 0.001 parts by mass, the tape peelability is not improved. This is presumably due in part to the fact that the dispersibility of the liquid crystal polymer in the polyethylene resin is not improved, and aggregates having a particle size or diameter of 300 μm or more are generated in the molded product. When the content of the organic phosphate ester salt compound is more than 5 parts by mass, the mechanical properties of the resulting polyethylene resin composition are deteriorated.

[0072] The organic phosphate ester salt compound used in the polyethylene resin composition of the present invention is preferably an organic phosphate ester salt compound containing one or more metal atoms selected from lithium, sodium, potassium, magnesium, calcium, barium and aluminum. The organic phosphate ester salt compound used in the polyethylene resin composition of the present invention is preferably an organic phosphate ester salt compound represented by the following formula (V): [ka] [In the formula, R 1 is a divalent hydrocarbon group having 1 to 10 carbon atoms, R 2 and R 3 are each independently a hydrogen atom or a hydrocarbon group having 1 to 10 carbon atoms, M is a monovalent to trivalent metal atom, and n is an integer of 1 to 3. and / or formula (VI) [ka] [In the formula, R1 is a divalent hydrocarbon group having 1 to 10 carbon atoms, R 2 and R 3 are each independently a hydrogen atom or a hydrocarbon group having 1 to 10 carbon atoms, and m is 1 or 2. It is more preferable that the organic phosphate ester salt compound is represented by the following formula:

[0073] Specific examples of the organic phosphate ester salt compound represented by formula (V) include sodium-2,2'-methylene-bis(4,6-di-t-butylphenyl) phosphate, sodium-2,2'-ethylidene-bis(4,6-di-t-butylphenyl) phosphate, lithium-2,2'-methylene-bis(4,6-di-t-butylphenyl) phosphate, lithium-2,2'-ethylidene-bis(4,6-di-t-butylphenyl) phosphate, sodium-2,2'-ethylidene-bis(4-i-propyl-6-t-butylphenyl) phosphate, lithium-2,2'-methylene-bis(4-methyl-6-t-butylphenyl) phosphate, lithium Sodium 2,2'-methylene-bis(4-ethyl-6-t-butylphenyl) phosphate, sodium 2,2'-butylidene-bis(4,6-dimethylphenyl) phosphate, sodium 2,2'-butylidene-bis(4,6-di-t-butylphenyl) phosphate, sodium 2,2'-t-octylmethylene-bis(4,6-dimethylphenyl) phosphate, sodium 2,2'-t-octylmethylene-bis(4,6-di-t-butylphenyl) phosphate, calcium bis(2,2'-methylene-bis(4,6-di-t-butylphenyl) phosphate), magnesium bis[2,2'-methylene-bis(4,6 -di-t-butylphenyl)phosphate], barium bis[2,2'-methylene-bis(4,6-di-t-butylphenyl)phosphate], sodium-2,2'-methylene-bis(4-methyl-6-t-butylphenyl)phosphate, sodium-2,2'-methylene-bis(4-ethyl-6-t-butylphenyl)phosphate, sodium-2,2'-ethylidene-bis(4-m-butyl-6-t-butylphenyl)phosphate nyl) phosphate, sodium 2,2'-methylene-bis(4,6-dimethylphenyl) phosphate, sodium 2,2'-methylene-bis(4,6-diethylphenyl) phosphate, potassium 2,2'-ethylidene-bis(4,6-di-t-butylphenyl) phosphate, calcium bis[2,2'-ethylidene-bis(4,6-di-t-butylphenyl) phosphate], magnesium bis[2,2'-ethylidene-bis(4,6-di-t-butylphenyl)phosphate], barium-bis[2,2'-ethylidene-bis(4,6-di-t-butylphenyl)phosphate], aluminum-tris[2,2'-methylene-bis(4,6-di-t-butylphenyl)phosphate], aluminum-tris[2,2'-ethylidene-bis(4,6-di-t-butylphenyl)phosphate].

[0074] Of these, sodium-2,2'-methylene-bis(4,6-di-t-butylphenyl)phosphate and lithium-2,2'-methylene-bis(4,6-di-t-butylphenyl)phosphate are preferred, and sodium-2,2'-methylene-bis(4,6-di-t-butylphenyl)phosphate (also known as 2,4,8,10-tetra(t-butyl)-6-hydroxy-12H-dibenzo[d,g][1,3,2]dioxaphosphocin-6-oxide) sodium salt is more preferred.

[0075] The organic phosphate ester salt compound represented by formula (VI) is 2 and R 3 are both tert-butyl groups, [ka] [In the formula, R 1 is a divalent hydrocarbon group having 1 to 10 carbon atoms, and m is 1 or 2. More preferred is a compound represented by the formula (VIII) [ka] [In the formula, R 1 is a methylene group or an ethylidene group. Particularly preferred is a compound represented by the formula:

[0076] Specific examples of the compound represented by formula (VIII) include hydroxyaluminum bis[2,2-methylene-bis(4,6-di-t-butylphenyl)phosphate] (also known as bis(2,4,8,10-tetra-t-butyl-6-hydroxy-12H-dibenzo[d,g][1,3,2]dioxaphosphocin-6-oxide) aluminum hydroxide salt), and hydroxyaluminum bis[2,2-ethylidene-bis(4,6-di-t-butylphenyl)phosphate].

[0077] The above organic phosphate ester salt compounds may be used alone or in combination of two or more kinds.

[0078] The polyethylene resin composition of the present invention may further contain 0.1 to 30 parts by mass of a functional group-containing polyolefin resin relative to 100 parts by mass of the polyethylene resin. By further containing a functional group-containing polyolefin resin, the mechanical strength and tape peel resistance of the resulting polyethylene resin composition can be further improved. The content of the functional group-containing polyolefin resin relative to 100 parts by mass of the polyethylene resin is preferably 0.2 to 20 parts by mass, more preferably 0.3 to 15 parts by mass, and even more preferably 0.5 to 10 parts by mass.

[0079] If the content of the functional group-containing polyolefin resin is less than 0.1 parts by mass, the mechanical strength of the resulting polyethylene resin composition may be insufficient and the effect of improving tape peel resistance may not be sufficiently obtained.If the content of the functional group-containing polyolefin resin is more than 30 parts by mass, the heat resistance of the resulting polyethylene resin composition tends to decrease.

[0080] Specific examples of functional group-containing polyolefin-based resins include maleic anhydride grafted polyolefin-based copolymers, maleic anhydride grafted polystyrene-based copolymers, vinyl monomer / maleic anhydride copolymers, epoxy group-containing polyolefin-based copolymers, epoxy group-containing vinyl-based random, graft or block copolymers, carboxyl group-containing olefin-based random or graft copolymers, etc. Among these, copolymers having at least one functional group selected from the group consisting of acid anhydride groups, carboxyl groups, and epoxy groups are preferred, and maleic anhydride grafted polyolefin-based copolymers and epoxy group-containing polyolefin-based copolymers are more preferred.

[0081] Specific examples of maleic anhydride grafted polyolefin copolymers include maleic anhydride grafted polypropylene (PP-g-MAH), maleic anhydride grafted ethylene / propylene rubber (EPR-g-MAH), and maleic anhydride grafted ethylene / propylene / diene rubber (EPDM-g-MAH).

[0082] Specific examples of maleic anhydride grafted polystyrene copolymers include maleic anhydride grafted polystyrene (PS-g-MAH), maleic anhydride grafted styrene / butadiene / styrene copolymer (SBS-g-MAH), maleic anhydride grafted styrene / ethylene / butene / styrene copolymer (SEBS-g-MAH), and the like.

[0083] Specific examples of vinyl monomer / maleic anhydride copolymers include styrene / maleic anhydride copolymers, styrene / (meth)acrylic acid / maleic anhydride copolymers, and (meth)acrylic acid ester / maleic anhydride copolymers.

[0084] Specific examples of epoxy group-containing polyolefin copolymers include ethylene / glycidyl (meth)acrylate copolymers, ethylene / glycidyl (meth)acrylate / vinyl acetate copolymers, ethylene / glycidyl (meth)acrylate / methyl (meth)acrylate copolymers, ethylene / glycidyl (meth)acrylate / ethyl (meth)acrylate copolymers, polystyrene graft copolymers onto ethylene / glycidyl (meth)acrylate copolymers (EGMA or EGA-g-PS), polymethyl (meth)acrylate graft copolymers onto ethylene / glycidyl methacrylate copolymers (EGMA or EGA-g-PMMA), and styrene / acrylonitrile graft copolymers onto ethylene / glycidyl (meth)acrylate copolymers (EGMA or EGA-g-AS).

[0085] Specific examples of epoxy group-containing vinyl random, graft or block copolymers include glycidyl (meth)acrylate grafted polystyrene (PS-g-GMA or GA), glycidyl (meth)acrylate grafted polymethyl (meth)acrylate (PMMA or PMA-g-GMA or GA), and glycidyl (meth)acrylate grafted polyacrylonitrile (PAN-g-GMA or GA).

[0086] Specific examples of carboxyl group-containing olefin random or graft copolymers include carboxylated polyethylene, carboxylated polypropylene, ethylene / (meth)acrylic acid copolymers (ionomers), and styrene / (meth)acrylic acid copolymers.

[0087] As the functional group-containing polyolefin resin contained in the polyethylene resin composition of the present invention, a maleic anhydride grafted polypropylene copolymer and / or an ethylene / glycidyl (meth)acrylate copolymer are preferred.

[0088] The above-mentioned functional group-containing polyolefin resins may be used alone or in combination of two or more kinds.

[0089] In the polyethylene resin of the present invention, when mixing the polyethylene resin, the liquid crystal polymer, the organic phosphoric acid ester salt compound, and optionally the functional group-containing polyolefin resin, a compatibilizer is not particularly necessary, but a compatibilizer may be added for the purpose of further improving compatibility or modifying physical properties. Here, the compatibilizer refers to a substance that is localized at the interface between the phases of the polymers constituting the mixed polymer and has the function of reducing the interfacial tension between the phases. The amount of the compatibilizer added is preferably 10% by mass or less, more preferably 5% by mass or less, even more preferably 1% by mass or less, and particularly preferably 0.05% by mass or less, based on the total mass of the polyethylene resin and the liquid crystal polymer. In the present invention, it is most preferable that the polyethylene resin composition does not contain a compatibilizer.

[0090] The polyethylene resin composition of the present invention may contain an inorganic filler and / or an organic filler, if necessary.

[0091] Examples of the inorganic and / or organic filler to be blended include one or more selected from the group consisting of glass fiber, silica alumina fiber, alumina fiber, carbon fiber, potassium titanate fiber, aluminum borate fiber, aramid fiber, talc, mica, graphite, wollastonite, dolomite, clay, glass flakes, glass beads, glass balloons, calcium carbonate, barium sulfate, and titanium oxide. Among these, glass fiber is preferred because of its excellent balance between physical properties and cost.

[0092] When an inorganic filler and / or an organic filler is used, the amount of the filler is preferably 0.1 to 200 parts by mass, more preferably 1 to 100 parts by mass, and even more preferably 5 to 50 parts by mass, per 100 parts by mass of the total amount of the polyethylene resin and the liquid crystal polymer.

[0093] The polyethylene resin composition of the present invention may further contain other resin components and additives in addition to the polyethylene resin, the liquid crystal polymer, the organic phosphate salt compound and, if necessary, the functional group-containing polyolefin resin, within the scope of not impairing the object of the present invention.

[0094] Examples of other resin components include thermoplastic resins such as polyamide, polyester, polyacetal, polyphenylene ether, and modified products thereof, as well as polysulfone, polyethersulfone, polyetherimide, and polyamideimide, and thermosetting resins such as phenol resin, epoxy resin, and polyimide resin.

[0095] Examples of the additives include flow improvers such as antioxidants, hydrochloric acid absorbers, heat stabilizers, light stabilizers, ultraviolet absorbers, lubricants, antistatic agents, flame retardants, nucleating agents, pigments, dyes, dispersants, copper damage inhibitors, neutralizing agents, foaming agents, plasticizers, bubble inhibitors, crosslinking agents, and peroxides.

[0096] The other resin components and additives may be blended alone or in combination of two or more kinds.

[0097] When other resin components are blended, the blending amount of the resin components is preferably 0.1 to 100 parts by mass, more preferably 0.1 to 80 parts by mass, per 100 parts by mass of the total amount of the polyethylene resin and the liquid crystal polymer.

[0098] When an additive is added, the amount of the additive is preferably 0.001 to 5 parts by mass, and more preferably 0.01 to 3 parts by mass, per 100 parts by mass of the total amount of the polyethylene resin and the liquid crystal polymer.

[0099] The polyethylene resin composition of the present invention is prepared by melt-kneading the above-mentioned polyethylene resin, liquid crystal polymer and organic phosphate salt compound together with, if necessary, a functional group-containing polyolefin resin, the above-mentioned compatibilizer, inorganic filler and / or organic filler, other resin components and additives in a kneader, and then processing the mixture into pellets, flakes or powder form and subjecting it to molding or melt-kneading. The compatibilizer, inorganic filler and / or organic filler, other resin components and additives may be blended in advance with either the polyethylene resin or the liquid crystal polymer, or may be blended with the molding material when the polyethylene resin composition is molded.

[0100] As the kneading machine, a Banbury mixer, a kneader, a single-screw or twin-screw extruder, etc. are used. For example, when a twin-screw extruder is used, it is preferable to perform kneading while making the vent port vacuum, but this is not limiting and kneading may be performed in an inert gas atmosphere.

[0101] The polyethylene resin composition of the present invention can be obtained by the preparation as described above.

[0102] When the polyethylene resin composition of the present invention is processed into pellets, the shape of the pellets is not particularly limited and may be, for example, prismatic, spherical, cylindrical, etc. Regarding the size of the pellets, in the case of a prismatic shape, the length of the maximum side is preferably 1 to 20 mm, in the case of a spherical shape, the particle diameter is preferably 1 to 20 mm, and in the case of a cylindrical shape, the diameter is preferably 0.5 to 5 mm and the height is preferably 1.5 to 10 mm. When the pellet size is within the above ranges, the handling property is improved and the packaging work of the molding material is facilitated.

[0103] The method for producing the pellets is not particularly limited, but for example, a method can be used in which the polyethylene resin composition is pulverized or extruded into a strand shape, and the resulting strand is cut into an appropriate size by a cutter or the like to process into pellets.

[0104] The polyethylene resin composition of the present invention can be processed into molded articles such as injection molded articles, films, sheets, fibers, and blow molded articles by known molding methods such as injection molding, extrusion molding, and blow molding.

[0105] Injection molded products are formed using an injection molding machine and are used for applications such as food packaging containers, automobile parts, daily necessities, electrical and electronic parts, building parts, and machine parts.

[0106] The film or sheet is formed by known extrusion molding, such as a T-die method, an inflation method, or a calendar method, and may be stretched or unstretched. The thickness of the film or sheet is preferably 0.005 to 10 mm, more preferably 0.02 to 5 mm, and further preferably 0.05 to 2 mm.

[0107] The film or sheet can be used as a base material for vacuum forming, pressure forming, vacuum and pressure forming, etc., for both large and small molded products. Examples of large molded products include door trims, instrument panels, roof carriers, building interior panels, washstand panels, large carrier trays, etc. Examples of small molded products include trays, plates and cups that are food containers, etc.

[0108] Packaging materials can also be made by folding a film or sheet, or by overlapping and heat sealing a plurality of films or sheets. For example, they can be used for packaging materials with side seals (two-sided seals, three-sided seals, four-sided seals, envelope seals, etc.), packaging materials with cylindrical seals, and packaging materials with hand-joint seals (hand-joint seals, hand-joint four-sided seals, back seals, one-sided back seals, etc.) in pillow seal, pleated seal, flat-bottom seal, square-bottom seal, gusset, and other types. Such packaging materials can be suitably used as packaging products for food, medical, and electrical and electronic components.

[0109] The fibers can be obtained by a known spinning method, for example, a melt spinning method. In the melt spinning method, the molten kneaded material is extruded from a spinneret, spun, and if necessary, stretched and wound up to produce the fibers. The melt spinning step and the stretching step may be carried out continuously or separately. The stretching step may be carried out multiple times.

[0110] The obtained fibers can be processed into textile products such as yarn, cotton, nonwoven fabric, woven fabric, paper, etc. Such textile products can be used for applications such as automobile parts, daily necessities, building parts, machine parts, etc.

[0111] The hollow molded article can be molded by known blow molding methods such as direct blow molding, sheet blow molding, multi-layer sheet blow molding, the hot parison method, and injection stretch blow molding.

[0112] Examples of the shape of the hollow molded article include containers, bottles, tanks, ducts, bags, tubes, hoses, pipes, liners (resin lining layers), and the like, and are used for, for example, food storage and medical purposes.

[0113] The present invention will be described in detail below with reference to examples, but the present invention is not limited thereto. EXAMPLES

[0114] [Synthesis example 1 (LCP-1)] A reaction vessel equipped with a stirrer with a torque meter and a distillation tube was charged with 349.3 g (40 mol%) of 4-hydroxybenzoic acid, 476.0 g (40 mol%) of 6-hydroxy-2-naphthoic acid, 69.7 g (10 mol%) of hydroquinone, and 105.0 g (10 mol%) of terephthalic acid, and further charged with 1.03 times the moles of acetic anhydride relative to the amount (mol) of hydroxyl groups in the total monomers, and deacetic acid polymerization was carried out under the following conditions.

[0115] The temperature was raised from room temperature to 145°C in 1 hour under a nitrogen gas atmosphere, and the temperature was maintained for 30 minutes. Next, the temperature was raised to 350°C over 7 hours while distilling off the by-product acetic acid, and then the pressure was reduced to 10 mmHg over 80 minutes. The polymerization reaction was terminated when a predetermined torque was reached, and the contents were removed from the reaction vessel and pellets of the liquid crystal polymer were obtained using a grinder. The amount of acetic acid distilled during polymerization was almost the theoretical value.

[0116] The crystalline melting temperature of the obtained liquid crystal polymer (LCP-1) was 218°C as measured by DSC.

[0117] [Synthesis example 2 (LCP-2)] A reaction vessel equipped with a stirrer with a torque meter and a distillation tube was charged with 386.0 g (43 mol%) of 4-hydroxybenzoic acid, 403.6 g (33 mol%) of 6-hydroxy-2-naphthoic acid, 145.2 g (12 mol%) of 4,4'-dihydroxybiphenyl, 126.0 g (9 mol%) of 2,6-naphthalenedicarboxylic acid, and 32.4 g (3 mol%) of isophthalic acid, and further charged with 1.03 times the moles of acetic anhydride relative to the amount (mol) of hydroxyl groups in the total monomers, and deacetic acid polymerization was carried out under the following conditions.

[0118] The temperature was raised from room temperature to 150°C in 1 hour under a nitrogen gas atmosphere, and the temperature was maintained for 30 minutes. Next, the temperature was raised to 340°C over 4 hours while distilling off the by-product acetic acid, and then the pressure was reduced to 10 mmHg over 80 minutes. The polymerization reaction was terminated when a predetermined torque was reached, and the contents were removed from the reaction vessel and pellets of the liquid crystal polymer were obtained using a grinder. The amount of acetic acid distilled during polymerization was almost the theoretical value.

[0119] The crystalline melting temperature of the obtained liquid crystal polymer (LCP-2) was 183° C. as measured by DSC.

[0120] [Polyethylene resin (PE)] The following polyethylene resins were used: PE-1: High density polyethylene (Hi-Zex (registered trademark) 2200J manufactured by Prime Polymer Co., Ltd., density: 964 kg / m3 ) PE-2: High density polyethylene (Hi-Zex (registered trademark) 1300J manufactured by Prime Polymer Co., Ltd., density: 960 kg / m 3 ) PE-3: High density polyethylene (Hi-Zex (registered trademark) 1608J manufactured by Prime Polymer Co., Ltd., density: 955 kg / m 3 ) PE-4: Linear low-density polyethylene (UltZex (registered trademark) 1030L manufactured by Prime Polymer Co., Ltd., density: 909 kg / m 3 )

[0121] [Organophosphate ester salt compounds (PA)] The following organic phosphate ester salt compounds were used: PA-1: ADEKA STAB NA-21 (hydroxyaluminum bis[2,2-methylene-bis(4,6-di-t-butylphenyl)phosphate) manufactured by ADEKA PA-2: ADEKA STAB NA-11 (sodium 2,2'-methylene-bis(4,6-di-t-butylphenyl) phosphate)

[0122] [Sorbitol compounds (SO)] The following sorbitol-based compounds were used: SO-1: Milliken NX-8000

[0123] [Functional group-containing polyolefin resin (PO)] The following functional group-containing polyolefin resins were used: PO-1: Riken Vitamin Co., Ltd. RIKEAID MG-250P (acid-modified polypropylene resin) PO-2: Bondfast (registered trademark) BF-E (epoxy-containing polyethylene resin) manufactured by Sumitomo Chemical Co., Ltd.

[0124] In the examples, the melt flow rate, bending strength, bending modulus, deflection temperature under load and tape peel resistance were measured by the methods described below.

[0125] <Melt flow rate (MFR)> The measurements were performed in accordance with ASTM D-1238 at a temperature of 230°C and a load of 2.16 kg.

[0126] <Flexural strength and flexural modulus> Using an injection molding machine (UH1000-110, manufactured by Nissei Plastic Industrial Co., Ltd.), the material was molded into rectangular test pieces measuring 80.0 mm in length, 10.0 mm in width, and 4.0 mm in thickness at a cylinder temperature of 250°C and a mold temperature of 40°C. These test pieces were used for measurements in accordance with ISO-178.

[0127] <Deflection temperature under load (DTUL)> The same rectangular test pieces as those used for measuring the bending strength and bending modulus were used, and measurements were performed in accordance with ISO-75, under a load of 0.45 MPa and at a heating rate of 2° C. / min.

[0128] <Tape peeling resistance (peeling area ratio)> Using an injection molding machine (PS-40 manufactured by Nissei Plastic Industrial Co., Ltd.), injection molding was performed at a cylinder temperature of 250°C and a mold temperature of 40°C to mold a flat plate-shaped test piece with a length of 90 mm, a width of 55 mm, and a thickness of 0.8 mm. Cellophane tape (Cellotape (registered trademark) CT-24 manufactured by Nichiban Co., Ltd.) was applied to this test piece so that the area was 500 mm. 2 (50mm x 10mm) by pressing with fingers to ensure close contact, and then peeling in a 180° direction in the longitudinal direction at a speed of 100mm / sec. The peeled portion of the surface of the test piece was scanned with a scanner and analyzed using Keyence VHX-900F communication software to calculate the peeled area. The peeled area was divided by the applied area to obtain the peeled area ratio (%). The smaller the peeled area ratio (%), the better the tape peel resistance.

[0129] [Examples 1 to 5, Comparative Examples 1 to 5, and Reference Examples 1 to 4] Polyethylene resins (PE-1, PE-2, PE-3, PE-4), liquid crystal polymers (LCP-1, LCP-2), organic phosphate ester salt compounds (PA-1, PA-2), sorbitol-based compound (SO-1) and functional group-containing polyolefin-based resins (PO-1, PO-2) were mixed in the amounts shown in Table 1, and melt-kneaded at a cylinder temperature of 250°C using a twin-screw extruder (TEX-30, manufactured by The Japan Steel Works, Ltd.) to obtain pellets of a polyethylene resin composition.

[0130] The pellets thus obtained were used to measure MFR, flexural strength, flexural modulus, deflection temperature under load, and tape peel resistance (peeled area ratio) by the methods described above. The results are shown in Table 1.

[0131] As is clear from Table 1, the polyethylene resin compositions of the present invention described in Examples 1 to 5 containing an organic phosphate salt compound were excellent in tape peel resistance, mechanical properties and heat resistance.

[0132] On the other hand, the polyethylene resin compositions not containing an organic phosphate salt compound (Comparative Example 1 and Comparative Examples 3 to 5) and the polyethylene resin composition containing a sorbitol-based compound (Comparative Example 2) were poor in tape peel resistance.

[0133] [Table 1]

Claims

1. For 100 parts by mass of polyethylene resin, 1 to 100 parts by weight of a liquid crystal polymer, and A polyethylene resin composition containing 0.001 to 5 parts by mass of an organic phosphate ester salt compound, The liquid crystal polymer is represented by the formula (I) and the formula (II): [Case 1] A wholly aromatic liquid crystal polyester resin containing a repeating unit represented by The organic phosphate ester salt compound is represented by the formula (V): [Case 2] [In the formula, R 1 is a divalent hydrocarbon group having 1 to 10 carbon atoms, R 2 and R 3 are each independently a hydrogen atom or a hydrocarbon group having 1 to 10 carbon atoms, M is a monovalent to trivalent metal atom, and n is an integer of 1 to 3.] and / or formula (VI) [C3] [In the formula, R 1 is a divalent hydrocarbon group having 1 to 10 carbon atoms, R 2 and R 3 are each independently a hydrogen atom or a hydrocarbon group having 1 to 10 carbon atoms, and m is 1 or 2.] A polyethylene resin composition, which is a compound represented by the formula:

2. 2. The polyethylene resin composition according to claim 1, wherein the organic phosphate ester salt compound is an organic phosphate ester salt compound containing one or more metal atoms selected from lithium, sodium, potassium, magnesium, calcium, barium and aluminum.

3. 3. The polyethylene resin composition according to claim 1, further comprising 0.1 to 30 parts by mass of a functional group-containing polyolefin resin per 100 parts by mass of the liquid crystal polymer.

4. The polyethylene resin composition according to claim 3, wherein the functional group-containing polyolefin resin is an acid-modified polyolefin resin and / or an epoxy group-containing polyolefin resin.

5. The polyethylene resin composition according to any one of claims 1 to 4, wherein the liquid crystal polymer has a crystalline melting temperature of less than 260°C.

6. The liquid crystal polymer is represented by the formulas (I) to (IV): [C4] [In the formula, Ar 1 and Ar 2 each represents a divalent aromatic group. The polyethylene resin composition according to any one of claims 1 to 5, which is a wholly aromatic liquid crystal polyester resin composed of a repeating unit represented by the following formula:

7. The repeating units represented by formulae (III) to (IV) are Ar 1 and Ar 2 are each independently represented by the formulas (1) to (4). [C5] The polyethylene resin composition according to claim 6, wherein each of the repeating units is one or more types selected from aromatic groups represented by the following formula:

8. A molded article made from the polyethylene resin composition according to any one of claims 1 to 7.

9. The molded article according to claim 8, which is an injection molded article, a film, a sheet, a fiber or a blown molded article.

Citation Information

Patent Citations

  • Composite resin molded structure and production thereof

    JP1993309692A

  • High-density polyethylene resin composition and its molded article

    JP2001192513A

  • Foam

    JP2002167456A

  • Polyethylene composition for blow molded container and container obtained from the same

    JP2010047677A

  • Polyethylene resin composition

    JP2018135486A