Method for producing resin composition and resin composition
Rapid freezing and thawing of latex with resin mixing and water separation methods enhance dispersibility and reduce environmental impact, addressing dispersibility and impurity issues in polymer fine particle dispersion in thermosetting resins.
Patent Information
- Application Number
- JP2021509699
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-03-28
- Filing Date
- 2020-03-30
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2040-03-30
AI Technical Summary
Existing methods for dispersing polymer fine particles in thermosetting resins, such as epoxy resins, face challenges with environmental impact, impurities, and insufficient dispersibility, particularly when using solvents or inorganic salts for recovery, leading to poor surface appearance of cured products.
A method involving rapid freezing and thawing of latex containing polymer fine particles, followed by mixing with a resin and separating the aggregate from water components, without using solvents or coagulants, to achieve uniform dispersion and low impurity content.
The method results in a resin composition with excellent dispersibility and low environmental impact, allowing for high-yield recovery of polymer fine particles with minimal impurities, improving the surface appearance and performance of cured products.
Smart Images

Figure 0007558928000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing a resin composition and a resin composition. [Background technology]
[0002] Thermosetting resins have various excellent properties such as high heat resistance and mechanical strength, and are therefore used in various fields. Among thermosetting resins, epoxy resins are used in a wide range of applications, for example, as electronic circuit sealants, paints, adhesives, and matrix resins for fiber-reinforced materials. Although epoxy resins are excellent in heat resistance, chemical resistance, and insulating properties, they have a problem in that they lack the impact resistance that is characteristic of thermosetting resins. In order to improve the impact resistance of thermosetting resins, a method of adding an elastomer to the thermosetting resin is widely used.
[0003] The elastomer may be polymer fine particles (e.g., crosslinked polymer fine particles). It is easy to simply mix polymer fine particles with a thermosetting resin (e.g., epoxy resin). As a mixing method, for example, a method is given in which several polymer fine particles having a particle diameter smaller than 1 μm are collected to prepare a powder of polymer fine particles having a particle diameter of 1 μm or more, and then the powder is mechanically mixed with a thermosetting resin. The powder of polymer fine particles thus prepared by collecting several polymer fine particles is called a secondary particle, and the polymer fine particles having a particle diameter smaller than 1 μm before becoming a powder are also called a primary particle. It is possible to disperse secondary particles of polymer fine particles in a thermosetting resin by the above-mentioned mixing method. However, it is very difficult at an industrial level to disperse primary particles of polymer fine particles having a particle diameter smaller than 1 μm in a thermosetting resin.
[0004] As described above, when the secondary particles (powder particles) of polymer microparticles and a thermosetting resin are mechanically mixed to obtain a resin composition, the primary particles of the polymer microparticles remain aggregated in the resin composition. Therefore, there is a problem that the surface appearance of the cured product obtained by curing the obtained resin composition is very poor. Therefore, various manufacturing methods have been proposed for dispersing the polymer microparticles in the form of primary particles in the thermosetting resin.
[0005] Patent Document 1 discloses a production method in which rubber-like polymer particles (A) (polymer fine particles) are dispersed in a polymerizable organic compound (H) (thermosetting resin) using a solvent.
[0006] Patent Document 2 discloses a production method for dispersing a cross-linked rubber-like copolymer (polymer fine particles) in a compound containing an epoxy group (thermosetting resin) by utilizing a dehydrated resin without using a solvent. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] International Publication No. WO2005 / 028546 [Patent Document 2] Japanese Patent Publication No. 5-339471 Summary of the Invention [Problem to be solved by the invention]
[0008] However, the above-mentioned conventional techniques are not sufficient from the viewpoint of environmental load or dispersibility of polymer fine particles in a resin composition, and there is room for further improvement. In addition, when recovering polymer fine particles from latex, there are problems such as environmental load and inclusion of impurities when using a solvent or salting out using an inorganic salt or the like.
[0009] One embodiment of the present invention has been made in consideration of the above problems, and its object is to provide a novel resin composition that has a small environmental impact, contains few impurities, and has excellent dispersibility of polymer fine particles. [Means for solving the problem]
[0010] As a result of intensive research to solve the above problems, the present inventors have found a new finding that, in recovering polymer microparticles from latex containing polymer microparticles, the emulsification effect can be weakened by carrying out a step of (i) freezing the latex and / or a step of (ii) shearing the latex, and polymer microparticles can be recovered without using a coagulant such as a solvent or an inorganic salt. Furthermore, the present inventors have independently found that a resin composition containing polymer microparticles obtained by such a method exhibits good dispersibility when mixed into a matrix resin, and have completed the present invention.
[0011] That is, one embodiment of the present invention includes the following configuration.
[0012] A method for producing a resin composition, comprising: a rapid freezing step of rapidly freezing latex containing polymer fine particles (A); a thawing step of thawing the latex frozen in the rapid freezing step; a resin mixing step of mixing a liquid, semi-solid, or solid resin (B) having a viscosity of 100 mPa s to 1,000,000 mPa s at 25°C with the latex after the rapid freezing step; and a separation step of separating a resin composition, which is an aggregate containing the polymer fine particles (A) and the resin (B), and a water component from the latex after the thawing step and the resin mixing step.
[0013] A method for producing a resin composition, comprising: a resin mixing step of mixing a latex containing polymer fine particles (A) with a liquid, semi-solid, or solid resin (B) having a viscosity of 100 mPa s to 1,000,000 mPa s at 25°C; a freezing step of freezing the latex in which the resin (B) is dispersed obtained in the resin mixing step; a thawing step of thawing the latex frozen in the freezing step; and a separation step of separating a resin composition, which is an aggregate containing the polymer fine particles (A) and the resin (B), and a water component from the latex after the thawing step.
[0014] A method for producing a resin composition, comprising: a resin mixing step of mixing a latex containing polymer fine particles (A) with a liquid, semi-solid, or solid resin (B) having a viscosity of 100 mPa s to 1,000,000 mPa s at 25°C; a shearing step of applying a shear stress to the latex obtained in the resin mixing step; and a first separation step of separating a resin composition, which is an aggregate containing the polymer fine particles (A) and the resin (B), and a water component from the latex after the shearing step.
[0015] The present invention comprises polymer fine particles (A) having a graft portion made of a polymer containing, as a structural unit, a structural unit derived from one or more monomers selected from the group consisting of aromatic vinyl monomers, vinyl cyan monomers, and (meth)acrylate monomers, and resin (B) which is a liquid, semi-solid, or solid having a viscosity of 100 mPa·s to 1,000,000 mPa·s at 25°C, wherein, when the total of the polymer fine particles (A) and the resin (B) is taken as 100% by weight, the polymer fine particles (A) account for 1 to 70% by weight and the resin (B) for 30 to 99% by weight, and the content of the polymer fine particles (A) in the resin (B) is taken as 5% by weight, the dispersibility of the polymer fine particles (A) in the resin (B) is measured using a grind gauge according to the JIS A resin composition having a particle size of 0 μm or less, substantially no organic solvent, an elemental S and P content of 150 ppm or less each, and an electrical conductivity of 0.6 mS / cm or less, when evaluated in accordance with K5101. Effect of the Invention
[0016] According to one embodiment of the present invention, it is possible to provide a resin composition which has a small environmental impact, contains few impurities, and has excellent dispersibility of polymer fine particles. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0017] An embodiment of the present invention will be described below, but the present invention is not limited thereto. The present invention is not limited to each configuration described below, and various modifications are possible within the scope of the claims. In addition, embodiments or examples obtained by appropriately combining the technical means disclosed in different embodiments or examples are also included in the technical scope of the present invention. Furthermore, new technical features can be formed by combining the technical means disclosed in each embodiment. All academic documents and patent documents described in this specification are incorporated herein by reference. In addition, unless otherwise specified in this specification, "A to B" representing a numerical range means "A or more (including A and greater than A) and B or less (including B and smaller than B)".
[0018] 1. Method for producing resin composition (embodiment 1 including freezing step) The method for producing a resin composition according to one embodiment of the present invention includes a rapid freezing step of rapidly freezing latex containing polymer fine particles (A), a thawing step of thawing the latex frozen in the rapid freezing step, a resin mixing step of mixing a resin (B) having a viscosity of 1,000,000 mPa·s or less at 25°C with the latex after the rapid freezing step, and a separation step of separating a resin composition, which is an aggregate containing the polymer fine particles (A) and the resin (B), and a water component from the latex after the thawing step and the resin mixing step. Hereinafter, the method for producing a resin composition according to one embodiment of the present invention may be simply referred to as the present production method.
[0019] The present inventors have found that by rapidly freezing a latex containing polymer fine particles (A), the freezing speed of water is faster than the aggregation of the polymer fine particles (A) themselves, and thus a loose aggregate of the polymer fine particles (A) is formed. By adding and mixing the resin (B) to the loose aggregate of the polymer fine particles (A), an aggregate in which the polymer fine particles (A) are uniformly dispersed in the resin (B) is obtained. On the other hand, if the latex containing the polymer fine particles (A) is slowly frozen, the polymer fine particles (A) will be firmly aggregated, and even if it is subsequently mixed with the resin (B), it is difficult to obtain an aggregate in which the polymer fine particles (A) are uniformly dispersed in the resin (B), which is not preferable. That is, in this production method, it can be said that a fast freezing speed is important.
[0020] According to this production method, since no salt such as a coagulant is used, it is possible to obtain aggregates with low contaminants (low impurities). In addition, since no organic solvent is used, the environmental impact is small. In addition, since the freezing step is performed, the aggregates such as polymer microparticles (A) can be efficiently separated from the water component, so that the polymer microparticles (A) can be recovered in a high yield. Furthermore, the emulsifier can be reduced from being entrained in the aggregates, and it is possible to obtain aggregates with a low content of emulsifier-derived substances (impurities).
[0021] Each step of the present production method will be described in detail below, followed by an explanation of the polymer fine particles (A), the resin (B), etc.
[0022] (1-1. Rapid freezing process) The rapid freezing step is a step of rapidly freezing the latex containing the polymer fine particles (A). This step is a step for agglomerating the polymer fine particles (A) in the latex. In this specification, "rapid freezing" means freezing the latex in 1 second to less than 20 minutes. In this step, the latex is preferably frozen for 5 seconds to 15 minutes, more preferably for 15 seconds to 10 minutes, and even more preferably for 20 seconds to 5 minutes.
[0023] The specific method for rapidly freezing the latex containing the polymer fine particles (A) is not particularly limited, and various techniques related to instant freezing and quick freezing can be used. For example, preferred examples include a method of contacting the latex with a metal surface cooled to -80°C to -10°C, a method of spraying the latex into cold air using a spray cooler to instantly cool and solidify it, a method of putting the latex in a solvent such as liquid nitrogen or cooled alcohol, and a method of contacting the latex with dry ice or cold stones.
[0024] In this specification, the term "freezing" refers to a state in which the latex is in a solid state. In this step, it is preferable that a part of the latex is in a solid state, and it is preferable that 50% or more of the latex is in a solid state, more preferably 70% or more of the latex is in a solid state, more preferably 80% or more of the latex is in a solid state, more preferably 90% or more of the latex is in a solid state, even more preferably 98% or more of the latex is in a solid state, and most preferably 100% of the latex is in a solid state.
[0025] Rapid freezing is a method in which the temperature of the latex drops and passes through the maximum ice crystal formation temperature range (between -1°C and -5°C) in a short period of time, and means that the ice crystals are 100 μm or less. In this step, the size is preferably 50 μm or less, more preferably 30 μm or less, more preferably 15 μm or less, and more preferably 5 μm or less. Further preferably, the size is 1 μm or less, 0.8 μm or less, 0.5 μm or less, 0.3 μm or less, 0.2 μm or less, and particularly preferably 0.1 μm or less.
[0026] The period from freezing to carrying out the thawing step described below is not particularly limited, but is preferably within 2 weeks, 1 week, 2 days, or 1 day after freezing, and more preferably, the thawing step is carried out without delay after the freezing step. The shorter the storage period in the frozen state, the more the growth of ice crystals can be suppressed, and the better the dispersibility of the resulting polymer microparticles (A) will be.
[0027] (1-2. Thawing process) The thawing step is a step of thawing the latex frozen by the quick freezing step. The specific thawing method is not particularly limited, and known thawing techniques can be used. For example, preferred examples include a method of returning the frozen latex in a room temperature or heated heating chamber, a method of directly or indirectly spraying steam, a method of pouring hot water, a method of placing in a hot water bath, a method of contacting with a heated metal surface, a method of putting into a heated liquid, and a method of irradiating with microwaves. From the viewpoint of productivity, a method of contacting with a heated metal surface such as an extruder and a method of putting into a heated liquid are preferred. The thawing time is also not particularly limited. For example, it is preferably performed for 1 second to 180 minutes, more preferably 1 second to 60 minutes, further preferably 1 second to 30 minutes, and particularly preferably 1 second to 15 minutes.
[0028] (1-3. Resin mixing process) The resin mixing step is a step of mixing the latex after the quick freezing step with a resin (B) having a viscosity of 1,000,000 mPa·s or less at 25°C. This step is a step of adding and mixing the resin (B) into the latex.
[0029] The resin mixing step may be carried out at any stage before or after the thawing step, or may be carried out simultaneously with the thawing step (at an intermediate stage of the thawing step). For example, when the resin mixing step is carried out before the thawing step, the resin (B) can be added to the frozen latex, the latex can be thawed, and the latex and the resin (B) can be mixed. When the resin mixing step is carried out after the thawing step, the resin (B) can be added to the thawed latex and mixed. When the resin mixing step is carried out during the thawing step, the resin (B) can be added to the latex during thawing and mixed.
[0030] The method of mixing the polymer fine particles (A) and the resin (B) can be various and is not particularly limited. For example, the method of directly adding the resin (B) to the aqueous latex of the polymer fine particles (A) or the method of adding the resin (B) in a dissolved state to the aqueous latex of the polymer fine particles (A) can be mentioned.
[0031] The means for mixing the polymer fine particles (A) and the resin (B) is not particularly limited, and examples thereof include stirring the latex containing the polymer fine particles (A) and the resin (B), kneading with a kneader, kneading with an extruder, and mixing with a planetary centrifugal mixer.
[0032] (1-4. Separation process) The separation step is a step of separating the resin composition, which is an aggregate containing the polymer fine particles (A) and the resin (B), from the latex after the thawing step and the resin mixing step, and the water component. In other words, it is a step of removing the water generated in the latex by the above steps to obtain the resin composition, which is an aggregate containing the polymer fine particles (A) and the resin (B).
[0033] The method for separating the aggregates from the water component is not particularly limited. For example, filtration, squeeze dehydration, etc. are included. The water component is a mixture containing water as the main component, an emulsifier, non-aggregated polymer fine particles (A), a resin (B), etc.
[0034] In this separation step, it is preferable to include a step of adjusting the water content of the aggregate to 5% by weight to 60% by weight based on 100% by weight of the aggregate. By adjusting the water content of the aggregate to this range, when the obtained resin composition is blended with a thermosetting resin, the viscosity does not become too high, and handling becomes easy. In this specification, the water content of the resin composition is a value measured using a water content measuring device. The method for measuring the water content will be described in detail in the following examples.
[0035] (1-5. Cleaning process) The present production method preferably further includes a washing step of washing the resin composition obtained in the separation step. By washing the resin composition in the form of an aggregate, an aggregate having a low content of impurities and the like can be obtained. In the washing step, washing with water is more preferable, and washing with ion-exchanged water or pure water is even more preferable.
[0036] The washing step is not particularly limited as long as it is a step of washing the resin composition. For example, the resin composition and water are mixed and stirred by applying shear with a stirrer, homomixer, high shear emulsifier, etc., the resin composition and water are kneaded using a kneader, and the resin composition and water are mixed using a planetary centrifugal mixer, etc. As the kneader, various types such as a batch kneader, a continuous kneader, and an extruder can be used.
[0037] The cleaning time is not particularly limited and can be, for example, from 1 second to 60 minutes, preferably from 1 second to 45 minutes, and more preferably from 1 second to 30 minutes.
[0038] The number of washing times is not particularly limited and may be, for example, 1 to 10 times, preferably 1 to 6 times, and more preferably 1 to 4 times.
[0039] The amount of washing water is not particularly limited, and may be, for example, 0.5 to 1000 parts by weight relative to 1 part by weight of the resin composition, but is preferably 1.0 to 500 parts by weight, and more preferably 1.5 to 200 parts by weight. Furthermore, washing by kneading using a kneader is more preferable because it allows the amount of washing water to be reduced.
[0040] The temperature of the washing water is not limited, and for example, room temperature water or heated water may be used as appropriate. The temperature of the hot water may be, for example, 10°C to 100°C, preferably 15°C to 90°C, more preferably 20°C to 85°C, and particularly preferably 25°C to 60°C. Since hot water has a higher washing effect, it is preferable to use heated washing water. In addition, when the resin composition deteriorates due to heat, a lower washing temperature is preferable, and a shorter washing time is preferable.
[0041] The method for removing the washing water is not limited, and examples thereof include draining the washing water, filtration under reduced pressure, oil-water separation, and squeeze dehydration.
[0042] (Other processes) In addition to the above-mentioned steps, the method may include a step of heating the obtained resin composition, devolatilizing and drying it. Various methods can be used for such a step, and there is no particular limitation. For example, heating and vacuum devolatilization can be used.
[0043] (1-6. Polymer fine particles (A)) The polymer fine particles (A) are not particularly limited as long as they are fine particles obtained by polymerization. For example, the polymer fine particles (A) preferably have a graft portion made of a polymer containing, as a constituent unit, one or more monomers selected from the group consisting of aromatic vinyl monomers, vinyl cyan monomers, and (meth)acrylate monomers. The polymer fine particles (A) can also be called a graft copolymer.
[0044] (Graft part) In this specification, a polymer grafted to an arbitrary polymer is referred to as a graft portion. The graft portion is a polymer containing, as a constituent unit, a constituent unit derived from one or more monomers selected from the group consisting of an aromatic vinyl monomer, a vinyl cyan monomer, and a (meth)acrylate monomer. Since the graft portion has the above-mentioned structure, it can play various roles. The "various roles" include, for example, (a) improving the compatibility between the polymer fine particles (A) and the thermosetting resin, (b) improving the dispersibility of the polymer fine particles (A) in the thermosetting resin, which is the matrix resin to be mixed, and (c) dispersing the polymer fine particles (A) in the form of primary particles in the resin composition or the cured product thereof.
[0045] Specific examples of aromatic vinyl monomers include styrene, α-methylstyrene, p-methylstyrene, and divinylbenzene.
[0046] Specific examples of vinyl cyanide monomers include acrylonitrile and methacrylonitrile.
[0047] Specific examples of the (meth)acrylate monomer include methyl (meth)acrylate, ethyl (meth)acrylate, butyl (meth)acrylate, hydroxyethyl (meth)acrylate, and hydroxybutyl (meth)acrylate, etc. In this specification, (meth)acrylate means acrylate and / or methacrylate.
[0048] The one or more monomers selected from the group consisting of the aromatic vinyl monomer, the vinyl cyan monomer, and the (meth)acrylate monomer may be used alone or in combination of two or more.
[0049] The graft portion preferably contains a constituent unit derived from a reactive group-containing monomer as a constituent unit. The reactive group-containing monomer is preferably a monomer containing one or more reactive groups selected from the group consisting of an epoxy group, an oxetane group, a hydroxyl group, an amino group, an imide group, a carboxylic acid group, a carboxylic anhydride group, a cyclic ester, a cyclic amide, a benzoxazine group, and a cyanate ester group, and more preferably a monomer containing one or more reactive groups selected from the group consisting of an epoxy group, a hydroxyl group, and a carboxylic acid group. According to the above configuration, the graft portion of the polymer fine particles (A) can be chemically bonded to the thermosetting resin in the resin composition. This allows the polymer fine particles (A) to be maintained in a good dispersed state in the resin composition or in the cured product thereof without agglomerating.
[0050] Specific examples of the monomer having an epoxy group include glycidyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate glycidyl ether, and allyl glycidyl ether.
[0051] Specific examples of monomers having a hydroxyl group include hydroxy linear alkyl (meth)acrylates (particularly, hydroxy linear C1-6 alkyl (meth)acrylates) such as 2-hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate, and 4-hydroxybutyl (meth)acrylate; caprolactone-modified hydroxy (meth)acrylates; hydroxy branched alkyl (meth)acrylates such as α-(hydroxymethyl)methyl acrylate and α-(hydroxymethyl)ethyl acrylate; and hydroxyl group-containing (meth)acrylates such as mono(meth)acrylates of polyester diols (particularly saturated polyester diols) obtained from divalent carboxylic acids (such as phthalic acid) and dihydric alcohols (such as propylene glycol).
[0052] Specific examples of the monomer having a carboxylic acid group include monocarboxylic acids such as acrylic acid, methacrylic acid, and crotonic acid, and dicarboxylic acids such as maleic acid, fumaric acid, and itaconic acid. As the monomer having a carboxylic acid group, the above-mentioned monocarboxylic acids are preferably used.
[0053] The reactive group-containing monomers described above may be used alone or in combination of two or more.
[0054] The graft portion preferably contains 0.5 to 90% by weight, more preferably 1 to 50% by weight, even more preferably 2 to 35% by weight, and particularly preferably 3 to 20% by weight of the structural unit derived from the reactive group-containing monomer in 100% by weight of the graft portion. When the graft portion contains (a) 0.5% by weight or more of the structural unit derived from the reactive group-containing monomer in 100% by weight of the graft portion, the obtained resin composition can provide a cured product having sufficient impact resistance, and when (b) 90% by weight or less of the structural unit is contained, the obtained resin composition can provide a cured product having sufficient impact resistance, and has the advantage that the storage stability of the resin composition is good.
[0055] The structural unit derived from the reactive group-containing monomer is preferably contained in the graft portion, and more preferably contained only in the graft portion.
[0056] The graft portion may contain a structural unit derived from a polyfunctional monomer as a structural unit. When the graft portion contains a structural unit derived from a polyfunctional monomer, it has the following advantages: (a) swelling of the polymer fine particles (A) in the resin composition can be prevented, (b) the viscosity of the resin composition is reduced, so that the handleability of the resin composition tends to be improved, and (c) the dispersibility of the polymer fine particles (A) in the thermosetting resin is improved.
[0057] When the graft portion does not contain a structural unit derived from a polyfunctional monomer, the resulting resin composition can provide a cured product that is more excellent in toughness and impact resistance, compared to when the graft portion contains a structural unit derived from a polyfunctional monomer.
[0058] A polyfunctional monomer can be said to be a monomer having two or more radically polymerizable reactive groups in the same molecule. The radically polymerizable reactive group is preferably a carbon-carbon double bond. Examples of polyfunctional monomers include (meth)acrylates having an ethylenically unsaturated double bond such as allyl (meth)acrylate, excluding butadiene. Examples of monomers having two (meth)acrylic groups include ethylene glycol di(meth)acrylate, butanediol di(meth)acrylate, hexanediol di(meth)acrylate, cyclohexanedimethanol di(meth)acrylate, and polyethylene glycol di(meth)acrylates. Examples of the polyethylene glycol di(meth)acrylates include triethylene glycol di(meth)acrylate, tripropylene glycol di(meth)acrylate, tetraethylene glycol di(meth)acrylate, and polyethylene glycol (600) di(meth)acrylate. Examples of monomers having three (meth)acrylate groups include alkoxylated trimethylolpropane tri(meth)acrylates, glycerol propoxy tri(meth)acrylate, pentaerythritol tri(meth)acrylate, and tris(2-hydroxyethyl)isocyanurate tri(meth)acrylate. Examples of alkoxylated trimethylolpropane tri(meth)acrylates include trimethylolpropane tri(meth)acrylate and trimethylolpropane triethoxy tri(meth)acrylate. Examples of monomers having four (meth)acrylic groups include pentaerythritol tetra(meth)acrylate and ditrimethylolpropane tetra(meth)acrylate. Examples of monomers having five (meth)acrylic groups include dipentaerythritol penta(meth)acrylate. Furthermore, an example of a monomer having six (meth)acrylic groups is ditrimethylolpropane hexa(meth)acrylate.
[0059] Among the above-mentioned polyfunctional monomers, polyfunctional monomers that can be preferably used for polymerization of the graft portion include allyl methacrylate, ethylene glycol di(meth)acrylate, butanediol di(meth)acrylate, hexanediol di(meth)acrylate, cyclohexanedimethanol di(meth)acrylate, and polyethylene glycol di(meth)acrylates. These polyfunctional monomers may be used alone or in combination of two or more.
[0060] The graft portion preferably contains 1 to 20% by weight, and more preferably 5 to 15% by weight, of structural units derived from polyfunctional monomers, based on 100% by weight of the graft portion.
[0061] The graft portion may contain, as a structural unit, a structural unit derived from another monomer in addition to the structural units derived from the above-mentioned monomers.
[0062] The graft portion is preferably a polymer graft-bonded to an elastomer, which will be described later.
[0063] (Glass transition temperature of grafted part) The glass transition temperature of the graft portion is preferably 190°C or less, more preferably 160°C or less, more preferably 140°C or less, more preferably 120°C or less, more preferably 80°C or less, more preferably 70°C or less, more preferably 60°C or less, more preferably 50°C or less, more preferably 40°C or less, more preferably 30°C or less, more preferably 20°C or less, more preferably 10°C or less, more preferably 0°C or less, more preferably -20°C or less, more preferably -40°C or less, more preferably -45°C or less, more preferably -50°C or less. °C or less, more preferably -55°C or less, more preferably -60°C or less, more preferably -65°C or less, more preferably -70°C or less, more preferably -75°C or less, more preferably -80°C or less, more preferably -85°C or less, more preferably -90°C or less, more preferably -95°C or less, more preferably -100°C or less, more preferably -105°C or less, more preferably -110°C or less, more preferably -115°C or less, even more preferably -120°C or less, and particularly preferably -125°C or less.
[0064] The glass transition temperature of the graft portion is preferably 0°C or higher, more preferably 30°C or higher, more preferably 50°C or higher, more preferably 70°C or higher, even more preferably 90°C or higher, and particularly preferably 110°C or lower.
[0065] The Tg of the graft portion can be determined by the composition of the structural units contained in the graft portion, etc. In other words, the Tg of the resulting graft portion can be adjusted by changing the composition of the monomers used when producing (polymerizing) the graft portion.
[0066] The Tg of the graft portion can be obtained by performing viscoelasticity measurement using a flat plate made of polymer microparticles. Specifically, the Tg can be measured as follows: (1) A dynamic viscoelasticity measurement is performed under tensile conditions on a flat plate made of polymer microparticles using a dynamic viscoelasticity measuring device (e.g., DVA-200, manufactured by IT Measurement & Control Co., Ltd.) to obtain a tan δ graph; (2) The peak temperature of tan δ in the obtained tan δ graph is taken as the glass transition temperature. Here, when multiple peaks are obtained in the tan δ graph, the highest peak temperature is taken as the glass transition temperature of the graft portion.
[0067] (Graft ratio of grafted part) In one embodiment of the present invention, the polymer fine particles (A) may have a polymer having the same structure as the graft portion and not grafted to the elastomer described below. In this specification, a polymer having the same structure as the graft portion and not grafted to the elastomer is also called a non-graft polymer. The non-graft polymer also constitutes a part of the polymer fine particles (A) according to one embodiment of the present invention. The non-graft polymer can also be said to be a polymer produced in the polymerization of the graft portion that is not grafted to the elastomer described below.
[0068] In this specification, the ratio of the polymer grafted to the elastomer described below, that is, the ratio of the grafted portion, among the polymers produced in the polymerization of the grafted portion, is referred to as the graft ratio. The graft ratio can also be said to be a value expressed by (weight of the grafted portion) / {(weight of the grafted portion)+(weight of the non-grafted polymer)}×100.
[0069] The graft ratio of the graft portion is preferably 70% or more, more preferably 80% or more, and even more preferably 90% or more. When the graft ratio is 70% or more, there is an advantage that the viscosity of the resin composition does not become too high.
[0070] In this specification, the graft ratio is calculated as follows. First, an aqueous latex containing polymer fine particles (A) is obtained, and then a powder of polymer fine particles (A) is obtained from the aqueous latex. A specific method for obtaining a powder of polymer fine particles (A) from an aqueous latex includes (i) coagulating the polymer fine particles (A) in the aqueous latex, (ii) dehydrating the obtained coagulated material, and (iii) further drying the coagulated material to obtain a powder of polymer fine particles (A). Next, 2 g of the powder of polymer fine particles (A) is dissolved in 50 mL of methyl ethyl ketone (hereinafter also referred to as MEK). Thereafter, the obtained MEK solution is separated into a component soluble in MEK (MEK soluble component) and a component insoluble in MEK (MEK insoluble component). Specifically, the obtained MEK soluble matter is centrifuged at 30,000 rpm for 1 hour using a centrifuge (CP60E, manufactured by Hitachi Koki Co., Ltd.), and the soluble matter is separated into MEK soluble matter and MEK insoluble matter. Here, a total of three sets of centrifugation are performed. The weights of the obtained MEK soluble matter and MEK insoluble matter are measured, and the graft ratio is calculated by the following formula. Graft rate (%) = {(weight of methyl ethyl ketone insoluble matter) - (weight of polymer other than grafted portion)} / (weight of polymer other than grafted portion) x 100 The weight of the polymer other than the graft portion is the amount of monomers that constitute the polymer other than the graft portion. The polymer other than the graft portion is, for example, an elastomer. When the polymer fine particles (A) contain a surface cross-linked polymer described later, the polymer other than the graft portion includes both an elastomer and a surface cross-linked polymer. In addition, in calculating the graft ratio, the method of coagulating the polymer fine particles (A) is not particularly limited, and a method using a solvent, a method using a coagulant, a method spraying an aqueous latex, etc. may be used.
[0071] (Modification of the graft part) In one embodiment of the present invention, the graft portion may be composed of only one type of graft portion having structural units of the same composition. In one embodiment of the present invention, the graft portion may be composed of multiple types of graft portions each having a structural unit of a different composition.
[0072] In one embodiment of the present invention, a case where the graft portion is composed of a plurality of types of graft portions will be described. In this case, each of the plurality of types of graft portions will be referred to as graft portion 1, graft portion 2, ..., graft portion n (n is an integer of 2 or more). The graft portion is composed of graft portion 1, graft portion 2, ..., and graft portion n The graft portion may include a mixture obtained by mixing the graft portion 1, the graft portion 2, ..., and the graft portion n The polymer may contain a polymer obtained by sequentially polymerizing each of the above. Such sequential polymerization of a plurality of polymers (graft portions) is also called multistage polymerization. A polymer obtained by multistage polymerization of a plurality of types of graft portions is also called a multistage polymerization graft portion. The method for producing the multistage polymerization graft portion will be described in detail later.
[0073] When the graft portion is composed of multiple types of graft portions, not all of these multiple types of graft portions need to be graft-bonded to the elastomer. At least a portion of at least one type of graft portion needs to be graft-bonded to the elastomer, and the other types (multiple other types) of graft portions may be graft-bonded to the graft portion grafted to the elastomer. When the graft portion is composed of multiple types of graft portions, it may have multiple types of polymers (multiple types of non-graft polymers) that have the same structure as the multiple types of graft portions and are not graft-bonded to the elastomer.
[0074] Graft portion 1, graft portion 2, ..., and graft portion n In the multi-stage polymerization graft portion, n The graft part n-1 or a graft portion. n-1 In the multi-stage polymerization graft portion, n Part of the graft n-1 Sometimes it penetrates inside the
[0075] In the multi-stage polymerization graft portion, each of the multiple graft portions may have a layer structure. For example, when the multi-stage polymerization graft portion is composed of graft portion 1, graft portion 2, and graft portion 3, an embodiment in which graft portion 1 is the innermost layer in the graft portion, a layer of graft portion 2 is present outside graft portion 1, and a layer of graft portion 3 is present outside the layer of graft portion 2 as the outermost layer is also one aspect of the present invention. In this way, a multi-stage polymerization graft portion in which each of the multiple graft portions has a layer structure can also be called a multi-layer graft portion. That is, in one embodiment of the present invention, the graft portion may include a mixture of multiple types of graft portions, a multi-stage polymerization graft portion, and / or a multi-layer graft portion.
[0076] When the elastomer and the graft portion are polymerized in this order in the production of the polymer microparticles (A), at least a part of the graft portion can cover at least a part of the elastomer in the obtained polymer microparticles (A). In other words, the elastomer and the graft portion are polymerized in this order, and the elastomer and the graft portion are polymerized in multiple stages. The polymer microparticles (A) obtained by multistage polymerization of the elastomer and the graft portion can also be called a multistage polymer.
[0077] When the polymer fine particles (A) are multi-stage polymers, the graft moiety may cover at least a part of the elastomer, or may cover the entire elastomer. When the polymer fine particles (A) are multi-stage polymers, the graft moiety may be partially embedded inside the elastomer.
[0078] When the polymer microparticles (A) are multistage polymers, the elastomer and the graft portion may have a layer structure. For example, one embodiment of the present invention is one in which the elastomer is the innermost layer (also referred to as the core layer) and the layer of the graft portion is present on the outside of the elastomer as the outermost layer (also referred to as the shell layer). A structure in which the elastomer is the core layer and the graft portion is the shell layer can also be called a core-shell structure. Thus, the polymer microparticles (A) in which the elastomer and the graft portion have a layer structure (core-shell structure) can also be called a multilayer polymer or a core-shell polymer. That is, in one embodiment of the present invention, the polymer microparticles (A) may be a multistage polymer and / or a multilayer polymer or a core-shell polymer. However, as long as they have a graft portion, the polymer microparticles (A) are not limited to the above structure.
[0079] At least a portion of the graft portion preferably covers at least a portion of the elastomer, in other words, at least a portion of the graft portion preferably exists on the outermost side of the polymer fine particles (A).
[0080] (Elastic body) The polymer fine particles (A) preferably further have an elastomer. That is, the polymer fine particles (A) are preferably rubber-containing graft copolymers having an elastomer and a graft portion grafted to the elastomer. Hereinafter, one embodiment of the present invention will be described by taking the case where the polymer fine particles (A) are rubber-containing graft copolymers as an example.
[0081] The elastomer preferably contains at least one selected from the group consisting of diene rubber, (meth)acrylate rubber, and polysiloxane rubber elastomer. The elastomer can also be referred to as rubber particles.
[0082] The case where the polymer fine particles (A) contain a diene rubber (Case A) will be described. In Case A, when the elastomer contains a diene rubber, the resulting resin composition can provide a cured product having excellent toughness and impact resistance.
[0083] The diene rubber is an elastomer containing, as a constituent unit, a constituent unit derived from a diene monomer. The diene monomer can also be called a conjugated diene monomer. In case A, the diene rubber may contain, in 100% by weight of the constituent units, 50 to 100% by weight of constituent units derived from diene monomers and 0 to 50% by weight of constituent units derived from vinyl monomers other than diene monomers copolymerizable with the diene monomers. In case A, the diene rubber may contain, as a constituent unit, a constituent unit derived from a (meth)acrylate monomer in an amount less than the constituent units derived from the diene monomers.
[0084] Examples of diene monomers include 1,3-butadiene, isoprene (2-methyl-1,3-butadiene), 2-chloro-1,3-butadiene, etc. These monomers may be used alone or in combination of two or more.
[0085] Examples of vinyl monomers other than diene monomers that can be copolymerized with diene monomers (hereinafter, also referred to as vinyl monomer A) include vinyl arenes such as styrene, α-methylstyrene, monochlorostyrene, and dichlorostyrene; vinyl carboxylic acids such as acrylic acid and methacrylic acid; vinyl cyanides such as acrylonitrile and methacrylonitrile; vinyl halides such as vinyl chloride, vinyl bromide, and chloroprene; vinyl acetate; alkenes such as ethylene, propylene, butylene, and isobutylene; and polyfunctional monomers such as diallyl phthalate, triallyl cyanurate, triallyl isocyanurate, and divinylbenzene. The vinyl monomers other than diene monomers described above may be used alone or in combination of two or more. Among the vinyl monomers other than diene monomers described above, styrene is particularly preferred. In the diene rubber in case A, the constituent units derived from vinyl monomers other than diene monomers are optional components. In case A, the diene rubber may be composed only of structural units derived from diene monomers.
[0086] In case A, the diene rubber is preferably butadiene rubber (also called polybutadiene rubber) consisting of structural units derived from 1,3-butadiene, or butadiene-styrene rubber (also called polystyrene-butadiene) which is a copolymer of 1,3-butadiene and styrene, and more preferably butadiene rubber. According to the above configuration, the desired effect of the polymer microparticles (A) containing the diene rubber can be more effectively exhibited. In addition, butadiene-styrene rubber is more preferable in that the transparency of the obtained cured product can be increased by adjusting the refractive index.
[0087] The case where the elastomer contains a (meth)acrylate rubber (Case B) will be described. In Case B, a wide range of polymer designs for the elastomer are possible by combining a variety of monomers.
[0088] The (meth)acrylate rubber is an elastomer containing, as a structural unit, a structural unit derived from a (meth)acrylate monomer. In case B, the (meth)acrylate rubber may contain, in 100% by weight of structural units, 50 to 100% by weight of structural units derived from a (meth)acrylate monomer, and 0 to 50% by weight of structural units derived from a vinyl monomer other than the (meth)acrylate monomer that is copolymerizable with the (meth)acrylate monomer. In case B, the (meth)acrylate rubber may contain, as a structural unit, a structural unit derived from a diene monomer in an amount less than the structural unit derived from the (meth)acrylate monomer.
[0089] Examples of the (meth)acrylate monomer include alkyl (meth)acrylates such as methyl (meth)acrylate, ethyl (meth)acrylate, butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, octyl (meth)acrylate, dodecyl (meth)acrylate, stearyl (meth)acrylate, and behenyl (meth)acrylate; aromatic ring-containing (meth)acrylates such as phenoxyethyl (meth)acrylate and benzyl (meth)acrylate; 2-hydroxyethyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, and the like. Examples of the monomers include hydroxyalkyl (meth)acrylates such as acrylate; glycidyl (meth)acrylates such as glycidyl (meth)acrylate and glycidyl alkyl (meth)acrylate; alkoxyalkyl (meth)acrylates; allyl alkyl (meth)acrylates such as allyl (meth)acrylate and allyl alkyl (meth)acrylate; and polyfunctional (meth)acrylates such as monoethylene glycol di(meth)acrylate, triethylene glycol di(meth)acrylate, and tetraethylene glycol di(meth)acrylate. These (meth)acrylate monomers may be used alone or in combination of two or more. Among these (meth)acrylate monomers, particularly preferred are ethyl (meth)acrylate, butyl (meth)acrylate, and 2-ethylhexyl (meth)acrylate.
[0090] Examples of vinyl monomers other than (meth)acrylate monomers copolymerizable with (meth)acrylate monomers (hereinafter also referred to as vinyl monomers other than (meth)acrylate monomers) include the monomers listed in the vinyl monomer A. The vinyl monomers other than (meth)acrylate monomers may be used alone or in combination of two or more. Among the vinyl monomers other than (meth)acrylate monomers, styrene is particularly preferred. In the (meth)acrylate rubber in case B, the constituent unit derived from a vinyl monomer other than (meth)acrylate monomer is an optional component. In case B, the (meth)acrylate rubber may be composed only of constituent units derived from (meth)acrylate monomers.
[0091] The case where the elastomer contains a polysiloxane rubber-based elastomer (Case C) will be described below. In Case C, the obtained resin composition has sufficient heat resistance and can provide a cured product having excellent impact resistance at low temperatures.
[0092] Examples of polysiloxane rubber-based elastomers include (a) polysiloxane-based polymers composed of alkyl or aryl di-substituted silyloxy units, such as dimethylsilyloxy, diethylsilyloxy, methylphenylsilyloxy, diphenylsilyloxy, and dimethylsilyloxy-diphenylsilyloxy, and (b) polysiloxane-based polymers composed of alkyl or aryl mono-substituted silyloxy units, such as organohydrogensilyloxy in which a portion of the alkyl in the side chain is substituted with a hydrogen atom. These polysiloxane-based polymers may be used alone or in combination of two or more. Among these polysiloxane-based polymers, (a) polymers composed of dimethylsilyloxy units, methylphenylsilyloxy units, and / or dimethylsilyloxy-diphenylsilyloxy units are preferred because the resulting resin composition can provide a cured product with excellent heat resistance, and (b) polymers composed of dimethylsilyloxy units are most preferred because they are easily available and economical.
[0093] In case C, the polymer fine particles (A) preferably contain 80% by weight or more, and more preferably 90% by weight or more, of the polysiloxane rubber-based elastomer in 100% by weight of the elastomer contained in the polymer fine particles (A). According to the above-mentioned constitution, the obtained resin composition can provide a cured product having excellent heat resistance.
[0094] The elastomer may further include an elastomer other than diene rubber, (meth)acrylate rubber, and polysiloxane rubber elastomer. Examples of the elastomer other than diene rubber, (meth)acrylate rubber, and polysiloxane rubber elastomer include natural rubber.
[0095] (Elastomeric bridge structure) From the viewpoint of maintaining the dispersion stability of the polymer fine particles (A) in the thermosetting resin, it is preferable that a crosslinked structure is introduced into the elastomer. A commonly used method can be adopted as a method for introducing a crosslinked structure into the elastomer, and examples thereof include the following methods. That is, in the production of the elastomer, a method is exemplified in which a crosslinkable monomer such as a multifunctional monomer and / or a mercapto group-containing compound is mixed with a monomer capable of constituting the elastomer, and then polymerized. In this specification, the production of a polymer such as an elastomer is also referred to as polymerizing a polymer.
[0096] Methods for introducing a crosslinked structure into a polysiloxane rubber-based elastomer include the following: (a) a method in which a polyfunctional alkoxysilane compound is used in combination with other materials when polymerizing a polysiloxane rubber-based elastomer; (b) a method in which a reactive group such as a vinyl reactive group or a mercapto group is introduced into a polysiloxane rubber-based elastomer, and then a vinyl polymerizable monomer or an organic peroxide is added to cause a radical reaction; or (c) a method in which a crosslinkable monomer such as a polyfunctional monomer and / or a mercapto group-containing compound is mixed with other materials when polymerizing a polysiloxane rubber-based elastomer, and then polymerization is carried out.
[0097] Examples of the polyfunctional monomer include the polyfunctional monomers exemplified in the above section (graft portion).
[0098] Examples of the mercapto group-containing compound include alkyl group-substituted mercaptans, allyl group-substituted mercaptans, aryl group-substituted mercaptans, hydroxy group-substituted mercaptans, alkoxy group-substituted mercaptans, cyano group-substituted mercaptans, amino group-substituted mercaptans, silyl group-substituted mercaptans, acid group-substituted mercaptans, halo group-substituted mercaptans, and acyl group-substituted mercaptans. The alkyl group-substituted mercaptans are preferably alkyl group-substituted mercaptans having 1 to 20 carbon atoms, and more preferably alkyl group-substituted mercaptans having 1 to 10 carbon atoms. The aryl group-substituted mercaptans are preferably phenyl group-substituted mercaptans. The alkoxy group-substituted mercaptans are preferably alkoxy group-substituted mercaptans having 1 to 20 carbon atoms, and more preferably alkoxy group-substituted mercaptans having 1 to 10 carbon atoms. The acid group-substituted mercaptan is preferably an alkyl group-substituted mercaptan having 1 to 10 carbon atoms and a carboxyl group, or an aryl group-substituted mercaptan having 1 to 12 carbon atoms and a carboxyl group.
[0099] (Glass transition temperature of elastic body) The glass transition temperature of the elastic body is preferably 80°C or lower, more preferably 70°C or lower, more preferably 60°C or lower, more preferably 50°C or lower, more preferably 40°C or lower, more preferably 30°C or lower, more preferably 20°C or lower, more preferably 10°C or lower, more preferably 0°C or lower, more preferably -20°C or lower, more preferably -40°C or lower, more preferably -45°C or lower, more preferably -50°C or lower, more preferably -55°C or lower, more preferably -60°C or lower, more preferably -65°C or lower, more preferably -70°C or lower, more preferably -75°C or lower, more preferably -80°C or lower, more preferably -85°C or lower, more preferably -90°C or lower, more preferably -95°C or lower, more preferably -100°C or lower, more preferably -105°C or lower, more preferably -110°C or lower, more preferably -115°C or lower, even more preferably -120°C or lower, and particularly preferably -125°C or lower. In this specification, "glass transition temperature" may be referred to as "Tg". According to this configuration, a powder having a low Tg can be obtained. As a result, a resin composition containing the obtained powder can provide a cured product or molded product having excellent toughness. The Tg of the elastic body can be obtained by performing viscoelasticity measurement using a flat plate made of an elastic body. Specifically, the Tg can be measured as follows: (1) A dynamic viscoelasticity measurement is performed under tensile conditions on a flat plate made of an elastic body using a dynamic viscoelasticity measuring device (for example, DVA-200, manufactured by IT Measurement and Control Co., Ltd.) to obtain a graph of tan δ; (2) The peak temperature of tan δ in the obtained graph of tan δ is taken as the glass transition temperature. Here, when multiple peaks are obtained in the graph of tan δ, the lowest peak temperature is taken as the glass transition temperature of the elastic body.
[0100] On the other hand, since this can suppress a decrease in the elastic modulus (rigidity) of the resulting cured product, i.e., a cured product having sufficient elastic modulus (rigidity) can be obtained, the Tg of the elastomer is preferably greater than 0°C, more preferably 20°C or higher, even more preferably 50°C or higher, particularly preferably 80°C or higher, and most preferably 120°C or higher.
[0101] The Tg of the elastomer can be determined by the composition of the structural units contained in the elastomer, etc. In other words, the Tg of the resulting elastomer can be adjusted by changing the composition of the monomers used when producing (polymerizing) the elastomer.
[0102] Here, when a homopolymer is obtained by polymerizing only one type of monomer, a group of monomers that provides a homopolymer having a Tg greater than 0°C is referred to as monomer group a. When a homopolymer is obtained by polymerizing only one type of monomer, a group of monomers that provides a homopolymer having a Tg less than 0°C is referred to as monomer group b. An elastomer that contains 50 to 100% by weight (more preferably 65 to 99% by weight) of a structural unit derived from at least one monomer selected from monomer group a and 0 to 50% by weight (more preferably 1 to 35% by weight) of a structural unit derived from at least one monomer selected from monomer group b is referred to as elastomer X. The elastomer X has a Tg greater than 0°C. When the elastomer contains elastomer X, the resulting resin composition can provide a cured product having sufficient rigidity.
[0103] It is preferable that a crosslinked structure is introduced into the elastomer even when the Tg of the elastomer is higher than 0° C. Methods for introducing a crosslinked structure include the methods described above.
[0104] Examples of monomers that may be included in the monomer group a include, but are not limited to, unsubstituted vinyl aromatic compounds such as styrene and 2-vinylnaphthalene; vinyl substituted aromatic compounds such as α-methylstyrene; ring-alkylated vinyl aromatic compounds such as 3-methylstyrene, 4-methylstyrene, 2,4-dimethylstyrene, 2,5-dimethylstyrene, 3,5-dimethylstyrene, and 2,4,6-trimethylstyrene; ring-alkoxylated vinyl aromatic compounds such as 4-methoxystyrene and 4-ethoxystyrene; ring-halogenated vinyl aromatic compounds such as 2-chlorostyrene and 3-chlorostyrene; ring-ester substituted vinyl aromatic compounds such as 4-acetoxystyrene; ring-hydroxylated vinyl aromatic compounds such as 4-hydroxystyrene. vinyl esters such as vinyl benzoate and vinyl cyclohexanoate; vinyl halides such as vinyl chloride; aromatic monomers such as acenaphthalene and indene; alkyl methacrylates such as methyl methacrylate, ethyl methacrylate and isopropyl methacrylate; aromatic methacrylates such as phenyl methacrylate; methacrylates such as isobornyl methacrylate and trimethylsilyl methacrylate; methacrylic monomers including methacrylic acid derivatives such as methacrylonitrile; certain acrylic acid esters such as isobornyl acrylate and tert-butyl acrylate; acrylic monomers including acrylic acid derivatives such as acrylonitrile, and the like. Further, examples of monomers that may be included in the monomer group a include acrylamide, isopropylacrylamide, N-vinylpyrrolidone, isobornyl methacrylate, dicyclopentanyl methacrylate, 2-methyl-2-adamantyl methacrylate, 1-adamantyl acrylate, 1-adamantyl methacrylate, etc., which, when made into a homopolymer, can provide a homopolymer having a Tg of 120° C. or higher. These monomers a may be used alone or in combination of two or more kinds.
[0105] Examples of the monomer b include ethyl acrylate, butyl acrylate, 2-ethylhexyl acrylate, octyl (meth)acrylate, dodecyl (meth)acrylate, 2-hydroxyethyl acrylate, and 4-hydroxybutyl acrylate. These monomers b may be used alone or in combination of two or more. Among these monomers b, ethyl acrylate, butyl acrylate, and 2-ethylhexyl acrylate are particularly preferred.
[0106] (Volume average particle size of elastic body) The volume average particle diameter of the elastic body is preferably 0.03 μm to 50.00 μm, more preferably 0.05 μm to 10.00 μm, more preferably 0.08 μm to 2.00 μm, even more preferably 0.10 μm to 1.00 μm, even more preferably 0.10 μm to 0.80 μm, and particularly preferably 0.10 μm to 0.50 μm. When the volume average particle diameter of the elastic body is (a) 0.03 μm or more, an elastic body having a desired volume average particle diameter can be stably obtained, and when it is (b) 50.00 μm or less, the heat resistance and impact resistance of the obtained cured product or molded product become good. The volume average particle diameter of the elastic body can be measured using a dynamic light scattering type particle size distribution measuring device or the like, using an aqueous latex containing the elastic body as a sample. The method for measuring the volume average particle diameter of the elastic body will be described in detail in the following examples.
[0107] (Ratio of elastic body) The proportion of the elastomer in the polymer fine particles (A) is preferably 40 to 97% by weight, more preferably 60 to 95% by weight, and even more preferably 70 to 93% by weight, based on 100% by weight of the entire polymer fine particles (A). When the proportion of the elastomer is (a) 40% by weight or more, the resulting resin composition can provide a cured product excellent in toughness and impact resistance, and when it is (b) 97% by weight or less, the polymer fine particles (A) do not easily aggregate, so that the resin composition does not become highly viscous, and as a result, the resulting resin composition can be easy to handle.
[0108] (gel content of elastomer) The elastomer is preferably one that can swell in a suitable solvent but is not substantially soluble in the solvent, and is preferably unnecessary for the thermosetting resin used.
[0109] The elastomer preferably has a gel content of 60% by weight or more, more preferably 80% by weight or more, even more preferably 90% by weight or more, and particularly preferably 95% by weight or more. When the gel content of the elastomer is within the above range, the resulting resin composition can provide a cured product with excellent toughness.
[0110] In this specification, the method of calculating the gel content is as follows. First, an aqueous latex containing polymer fine particles (A) is obtained, and then a powder of polymer fine particles (A) is obtained from the aqueous latex. The method of obtaining the powder of polymer fine particles (A) from the aqueous latex is not particularly limited, but for example, there is a method of (i) agglomerating the polymer fine particles (A) in the aqueous latex, (ii) dehydrating the obtained agglomerate, and (iii) further drying the agglomerate to obtain a powder of polymer fine particles (A). Next, 2.0 g of the powder of polymer fine particles (A) is dissolved in 50 mL of methyl ethyl ketone (MEK). Then, the obtained MEK solution is separated into a component soluble in MEK (MEK soluble content) and a component insoluble in MEK (MEK insoluble content). Specifically, the obtained MEK soluble matter is centrifuged at 30,000 rpm for 1 hour using a centrifuge (CP60E, manufactured by Hitachi Koki Co., Ltd.), and the soluble matter is separated into MEK soluble matter and MEK insoluble matter. A total of three sets of centrifugation are performed. The weights of the obtained MEK soluble matter and MEK insoluble matter are measured, and the gel content is calculated using the following formula. Gel content (%) = (weight of methyl ethyl ketone insoluble matter) / {(weight of methyl ethyl ketone insoluble matter) + (weight of methyl ethyl ketone soluble matter)} x 100 (Deformation of Elastic Body) In one embodiment of the present invention, the elastomer is one selected from the group consisting of diene rubber, (meth)acrylate rubber, and polysiloxane rubber elastomers, and may be composed of only one type of elastomer having the same composition of structural units. In one embodiment of the present invention, the elastomer may be composed of multiple types of elastomers each having a different composition of structural units.
[0111] In one embodiment of the present invention, a case where the elastic body is made of a plurality of types of elastic bodies will be described. In this case, the plurality of types of elastic bodies will be referred to as elastic body 1, elastic body 2, ..., and elastic body n Here, n is an integer of 2 or more. The elastic bodies are elastic body 1, elastic body 2, ..., and elastic body n The elastic body may include a mixture obtained by mixing the elastic body 1, the elastic body 2, ..., and the elastic body n The polymer obtained by multi-stage polymerization of a plurality of types of elastomers may also be called a multi-stage polymerized elastomer. The method for producing the multi-stage polymerized elastomer will be described in detail later.
[0112] Elastic body 1, Elastic body 2, ..., and Elastic body n In the multi-stage polymerized elastomer, n is an elastic body n-1 or an elastic body. n-1 In the multi-stage polymerized elastomer, n Part of the material is elastic. n-1 Sometimes it penetrates inside the
[0113] In the multi-stage polymerized elastomer, each of the multiple elastomers may have a layer structure. For example, when the multi-stage polymerized elastomer is composed of elastomer 1, elastomer 2, and elastomer 3, an embodiment in which elastomer 1 is the innermost layer, a layer of elastomer 2 is present outside of elastomer 1, and a layer of elastomer 3 is present outside of the layer of elastomer 2 as the outermost layer of the elastomer is also one aspect of the present invention. In this way, a multi-stage polymerized elastomer in which each of the multiple elastomers has a layer structure can also be called a multi-layered elastomer. That is, in one embodiment of the present invention, the elastomer may include a mixture of multiple types of elastomers, a multi-stage polymerized elastomer, and / or a multi-layered elastomer.
[0114] (Surface crosslinked polymer) The polymer microparticles (A) preferably have a surface cross-linked polymer in addition to the elastomer and the graft portion grafted to the elastomer. According to the above-mentioned configuration, (a) the blocking resistance can be improved in the production of the polymer microparticles (A), and (b) the dispersibility of the polymer microparticles (A) in the thermosetting resin is improved. The reason for this is not particularly limited, but can be assumed as follows: By covering at least a part of the elastomer with the surface cross-linked polymer, the exposure of the elastomer part of the polymer microparticles (A) is reduced, and as a result, the elastomers are less likely to stick to each other, thereby improving the dispersibility of the polymer microparticles (A).
[0115] When the polymer microparticles (A) contain a surface-crosslinked polymer, they can also have the following effects: (a) reducing the viscosity of the resin composition, (b) increasing the crosslink density in the elastomer, and (c) increasing the graft efficiency of the grafted portion. The crosslink density in the elastomer means the degree of the number of crosslinked structures in the entire elastomer.
[0116] The surface cross-linked polymer is composed of a polymer containing, as structural units, 30 to 100% by weight of structural units derived from polyfunctional monomers and 0 to 70% by weight of structural units derived from other vinyl monomers, totaling 100% by weight.
[0117] The polyfunctional monomer that can be used for the polymerization of the surface cross-linked polymer includes the same monomer as the above-mentioned polyfunctional monomer. Among these polyfunctional monomers, the polyfunctional monomer that can be preferably used for the polymerization of the surface cross-linked polymer includes allyl methacrylate, ethylene glycol di(meth)acrylate, butanediol di(meth)acrylate, hexanediol di(meth)acrylate, cyclohexanedimethanol di(meth)acrylate, and polyethylene glycol di(meth)acrylates. These polyfunctional monomers may be used alone or in combination of two or more.
[0118] The polymer fine particles (A) may contain a surface cross-linked polymer polymerized independently of the polymerization of the rubber-containing graft copolymer, or may contain a surface cross-linked polymer polymerized together with the rubber-containing graft copolymer. The polymer fine particles (A) may be a multi-stage polymer obtained by multi-stage polymerization of an elastomer, a surface cross-linked polymer, and a graft portion in this order. In either of these embodiments, the surface cross-linked polymer can cover at least a part of the elastomer.
[0119] The surface cross-linked polymer can be regarded as a part of the elastomer. When the polymer microparticle (A) contains a surface cross-linked polymer, the graft part may be (a) grafted to an elastomer other than the surface cross-linked polymer, (b) grafted to a surface cross-linked polymer, or (c) grafted to both an elastomer other than the surface cross-linked polymer and a surface cross-linked polymer. When the polymer microparticle (A) contains a surface cross-linked polymer, the volume average particle diameter of the elastomer mentioned above refers to the volume average particle diameter of the elastomer containing the surface cross-linked polymer.
[0120] The case where the polymer microparticle (A) is a multi-stage polymer obtained by multi-stage polymerization of an elastomer, a surface cross-linked polymer, and a graft portion in this order (case D) will be described. In case D, the surface cross-linked polymer may cover a part of the elastomer, or may cover the whole of the elastomer. In case D, a part of the surface cross-linked polymer may penetrate into the inside of the elastomer. In case D, the graft portion may cover a part of the surface cross-linked polymer, or may cover the whole of the surface cross-linked polymer. In case D, a part of the graft portion may penetrate into the inside of the surface cross-linked polymer. In case D, the elastomer, the surface cross-linked polymer, and the graft portion may have a layer structure. For example, an embodiment in which the elastomer is the innermost layer (core layer), a layer of the surface cross-linked polymer exists outside the elastomer as an intermediate layer, and a layer of the graft portion exists outside the surface cross-linked polymer as an outermost layer (shell layer) is also one embodiment of the present invention.
[0121] (Volume average particle size (Mv) of polymer microparticles (A)) The volume average particle diameter (Mv) of the polymer fine particles (A) is preferably 0.03 μm to 50.00 μm, more preferably 0.05 μm to 10.00 μm, more preferably 0.08 μm to 2.00 μm, even more preferably 0.10 μm to 1.00 μm, even more preferably 0.10 μm to 0.80 μm, and particularly preferably 0.10 μm to 0.50 μm, since a resin composition having a desired viscosity and high stability can be obtained. When the volume average particle diameter (Mv) of the polymer fine particles (A) is within the above range, there is also an advantage that the dispersibility of the polymer fine particles (A) in the matrix resin is improved. In this specification, the "volume average particle diameter (Mv) of the polymer fine particles (A)" means the volume average particle diameter of the primary particles of the polymer fine particles (A), unless otherwise specified. The volume average particle diameter of the polymer fine particles (A) can be measured using a dynamic light scattering particle size distribution measuring device or the like, using an aqueous latex containing the polymer fine particles (A) as a sample. The volume average particle diameter of the polymer fine particles (A) will be described in detail in the following examples. The volume average particle diameter of the polymer fine particles (A) can also be measured using the image data (image) obtained by cutting the cured resin composition and photographing the cut surface using an electron microscope or the like.
[0122] The particle size number distribution of the polymer fine particles (A) in the thermosetting resin preferably has a half width of 0.5 to 1 times the volume average particle size, since this gives a resin composition that is low in viscosity and easy to handle.
[0123] (1-7. Manufacturing method of polymer fine particles (A) (latex manufacturing process)) In one embodiment of the present invention, a step of producing polymer fine particles (A), particularly a latex production step of producing a latex containing the polymer fine particles (A), may be included as a preliminary step to the resin mixing step. The latex refers to an aqueous latex.
[0124] For example, the polymer microparticles (A) can be produced by polymerizing an arbitrary polymer, and then graft polymerizing a polymer constituting a graft moiety to the polymer in the presence of the polymer. Hereinafter, an example of the method for producing the polymer microparticles (A) will be described, taking as an example the case where an elastomer is polymerized, and then a polymer constituting a graft moiety to the elastomer in the presence of the elastomer.
[0125] The polymer fine particles (A) can be produced by known methods such as emulsion polymerization, suspension polymerization, microsuspension polymerization, etc. Specifically, the polymerization of the elastomer in the polymer fine particles (A), the polymerization of the graft portion (graft polymerization), and the polymerization of the surface cross-linked polymer can be produced by known methods such as emulsion polymerization, suspension polymerization, microsuspension polymerization, etc. Among these, emulsion polymerization is preferred as a method for producing the polymer fine particles (A) because the composition design of the polymer fine particles (A) is easy, industrial production is easy, and an aqueous latex of the polymer fine particles (A) that can be suitably used in the production of the present resin composition can be easily obtained. Hereinafter, the method for producing the elastomer, graft portion, and surface cross-linked polymer of any configuration that can be contained in the polymer fine particles (A) will be described.
[0126] (Method of manufacturing elastic body) Consider the case where the elastomer contains at least one selected from the group consisting of diene rubber and (meth)acrylate rubber. In this case, the elastomer can be produced by a method such as emulsion polymerization, suspension polymerization, or microsuspension polymerization, and the production method thereof can be, for example, the method described in WO2005 / 028546.
[0127] Consider the case where the elastomer contains a polysiloxane rubber-based elastomer. In this case, the elastomer can be produced by a method such as emulsion polymerization, suspension polymerization, or microsuspension polymerization, and the production method can be, for example, the method described in WO2006 / 070664.
[0128] The elastic body is made up of multiple types of elastic bodies (e.g., elastic body 1, elastic body 2, ..., elastic body n In this case, the method for manufacturing the elastic body will be described. n may be polymerized separately by the above-mentioned method and then mixed to produce an elastomer having a plurality of types of elastomers. n may be sequentially polymerized in multiple stages to produce an elastomer having a plurality of types of elastomers.
[0129] The multi-stage polymerization of elastomers will now be described in detail. For example, (1) elastomer 1 is polymerized to obtain elastomer 1; (2) elastomer 2 is then polymerized in the presence of elastomer 1 to obtain a two-stage elastomer. 1+2 (3) Then, the elastic body is obtained. 1+2 In the presence of 1+2+3 (4) After the same procedure, the elastic body is 1+2+···+(n-1) In the presence of elastic n Multi-stage polymerized elastomer 1+2+···+n get.
[0130] (Method of manufacturing the graft part) The graft portion can be formed, for example, by polymerizing the monomer used for forming the graft portion by known radical polymerization. When (a) the elastomer or (b) the polymer microparticle precursor containing the elastomer and the surface cross-linked polymer is obtained as an aqueous latex, it is preferable to carry out the polymerization of the graft portion by emulsion polymerization. The graft portion can be produced, for example, according to the method described in WO2005 / 028546.
[0131] The graft portion is a portion having a plurality of types of graft portions (e.g., graft portion 1, graft portion 2, ..., graft portion n A method for producing a graft portion in the case where the graft portion is composed of graft portion 1, graft portion 2, ..., graft portion n may be polymerized separately by the above-mentioned method and then mixed to produce a graft portion having a plurality of types of graft portions. Alternatively, graft portion 1, graft portion 2, ..., graft portion n may be sequentially polymerized in multiple stages to produce a graft moiety having a plurality of types of graft moieties.
[0132] The multi-stage polymerization of the graft portion will be specifically described. For example, (1) graft portion 1 is polymerized to obtain graft portion 1; (2) graft portion 2 is then polymerized in the presence of graft portion 1 to obtain a two-stage graft portion. 1+2 (3) Then, the graft part is obtained. 1+2 The graft portion 3 is polymerized in the presence of 1+2+3 (4) After the same procedure, the graft part is obtained. 1+2+···+(n-1) In the presence of n The multi-stage polymerization graft part is obtained by polymerizing 1+2+···+n get.
[0133] When the graft moiety is composed of a plurality of kinds of graft moieties, the graft moiety having the plurality of kinds of graft moieties may be polymerized and then graft polymerized onto the elastomer to produce the polymer fine particles (A). The polymer fine particles (A) may be produced by sequentially graft polymerizing the plurality of kinds of polymers constituting the plurality of kinds of graft moieties onto the elastomer in the presence of the elastomer in multiple stages.
[0134] (Method of producing surface cross-linked polymer) The surface cross-linked polymer can be formed by polymerizing the monomer used for forming the surface cross-linked polymer by known radical polymerization. When the elastomer is obtained as an aqueous latex, the polymerization of the surface cross-linked polymer is preferably carried out by emulsion polymerization.
[0135] When emulsion polymerization is employed as the method for producing the polymer fine particles (A), a known emulsifier (dispersant) can be used in the production of the polymer fine particles (A).
[0136] When the emulsion polymerization method is used as the method for producing the polymer microparticles (A), a thermally decomposable initiator can be used for producing the polymer microparticles (A). Examples of the thermally decomposable initiator include known initiators such as 2,2'-azobisisobutyronitrile, hydrogen peroxide, potassium persulfate, and ammonium persulfate.
[0137] A redox type initiator can also be used to produce the polymer microparticles (A). The redox type initiator is an initiator in which (a) a peroxide such as an organic peroxide or an inorganic peroxide is used in combination with (b) a reducing agent such as sodium formaldehyde sulfoxylate or glucose, if necessary, a transition metal salt such as iron (II) sulfate, if necessary, a chelating agent such as disodium ethylenediaminetetraacetate, if necessary, and a phosphorus-containing compound such as sodium pyrophosphate, if necessary. Examples of the organic peroxide include t-butyl peroxyisopropyl carbonate, paramenthane hydroperoxide, cumene hydroperoxide, dicumyl peroxide, t-butyl hydroperoxide, di-t-butyl peroxide, and t-hexyl peroxide. Examples of the inorganic peroxide include hydrogen peroxide, potassium persulfate, and ammonium persulfate.
[0138] When a redox type initiator is used, polymerization can be performed even at a low temperature where the peroxide does not substantially decompose thermally, and the polymerization temperature can be set in a wide range. Therefore, it is preferable to use a redox type initiator. Among the redox type initiators, it is preferable to use an organic peroxide such as cumene hydroperoxide, dicumyl peroxide, paramenthane hydroperoxide, and t-butyl hydroperoxide as the redox type initiator. The amount of the initiator used, and the amount of the reducing agent, transition metal salt, and chelating agent used when a redox type initiator is used, can be within a known range.
[0139] When a polyfunctional monomer is used in the polymerization of the elastomer, the graft portion or the surface cross-linked polymer for the purpose of introducing a cross-linked structure into the elastomer, the graft portion or the surface cross-linked polymer, a known chain transfer agent can be used within a known range of use amount. By using the chain transfer agent, the molecular weight and / or the degree of cross-linking of the obtained elastomer, the graft portion or the surface cross-linked polymer can be easily adjusted.
[0140] In the production of the polymer microparticles (A), in addition to the above-mentioned components, a surfactant may be used. The type and amount of the surfactant used are within the known ranges.
[0141] In the production of the polymer fine particles (A), known conditions such as polymerization temperature, pressure, and deoxidation can be used.
[0142] (1-8.Resin (B)) Resin (B) is not particularly limited in other properties so long as it is a liquid, semi-solid, or solid having a viscosity of 100 mPa·s to 1,000,000 mPa·s at 25°C. Note that "resin (B) has a viscosity of 100 mPa·s to 1,000,000 mPa·s at 25°C" means "resin (B) at 25°C has a viscosity of 100 mPa·s to 1,000,000 mPa·s."
[0143] When the resin (B) is a liquid, the viscosity of the resin (B) at 25° C. is preferably 750,000 mPa·s or less, more preferably 700,000 mPa·s or less, more preferably 500,000 mPa·s or less, more preferably 350,000 mPa·s or less, more preferably 300,000 mPa·s or less, more preferably 250,000 mPa·s or less, more preferably 100,000 mPa·s or less, more preferably 75,000 mPa·s or less, more preferably 50,000 mPa·s or less, more preferably 30,000 mPa·s or less, more preferably 25,000 mPa·s or less, even more preferably 20,000 mPa·s or less, and particularly preferably 15,000 mPa·s or less. According to the above configuration, the resin (B) has the advantage of excellent fluidity.
[0144] Furthermore, the viscosity of the resin (B) at 25°C is more preferably 200 mPa·s or more, more preferably 300 mPa·s or more, more preferably 400 mPa·s or more, more preferably 500 mPa·s or more, even more preferably 750 mPa·s or more, even more preferably 1000 mPa·s or more, and particularly preferably 1500 mPa·s or more. According to this configuration, the resin (B) does not impregnate the polymer fine particles (A). Therefore, the resin (B) can prevent the polymer fine particles (A) from fusing together.
[0145] The viscosity of resin (B) at 25°C is more preferably 100 mPa·s to 750,000 mPa·s, more preferably 100 mPa·s to 700,000 mPa·s, more preferably 100 mPa·s to 350,000 mPa·s, more preferably 100 mPa·s to 300,000 mPa·s, more preferably 100 mPa·s to 50,000 mPa·s, even more preferably 100 mPa·s to 30,000 mPa·s, and particularly preferably 100 mPa·s to 15,000 mPa·s.
[0146] When resin (B) is semi-solid, it can also be said that resin (B) is semi-liquid, and that resin (B) has a viscosity of more than 1,000,000 mPa s. When resin (B) is semi-solid or solid, the resulting resin composition containing powder or granules has the advantage of being less sticky and easier to handle.
[0147] The viscosity of the resin (B) can be measured by a viscometer. The method for measuring the viscosity of the resin (B) will be described in detail in the following examples.
[0148] Furthermore, the viscosity of the resin (B) at 25°C is more preferably 100 mPa·s or more, even more preferably 500 mPa·s or more, even more preferably 1000 mPa·s or more, and particularly preferably 1500 mPa·s or more, because the infiltration of the resin (B) into the polymer microparticles (A) can prevent the polymer microparticles (A) from fusing together.
[0149] Furthermore, when the matrix resin is a thermosetting resin, the viscosity of resin (B) at 25° C. is preferably equal to or less than the viscosity of the thermosetting matrix resin at 25° C. plus 50,000 mPa·s. In order to facilitate uniform mixing of resin (B) and the thermosetting matrix resin, when the viscosity of resin (B) at 25° C. is equal to or more than the viscosity of the thermosetting matrix resin at 25° C., the viscosity of resin (B) at 25° C. is more preferably equal to or less than the viscosity of the thermosetting matrix resin at 25° C. plus 20,000 mPa·s, more preferably equal to or less than the viscosity of the thermosetting matrix resin at 25° C. plus 10,000 mPa·s, even more preferably equal to or less than the viscosity of the thermosetting matrix resin at 25° C. plus 5,000 mPa·s, and most preferably equal to or less than the viscosity of the thermosetting matrix resin plus 0 mPa·s.
[0150] Resin (B) is preferably a resin having an endothermic peak of 25° C. or less in a differential scanning calorimetry (DSC) thermogram, and more preferably a resin having an endothermic peak of 0° C. or less.
[0151] In addition, the resin (B) may be the same resin as the thermosetting resin, which is the matrix resin to be mixed, as described later, or may be a resin different from the thermosetting resin. As an example, consider a case where the resin (B) is used in the manufacturing method of the resin composition, and the resin (B) is the same type of resin as the thermosetting resin. In this case, the matrix resin and the resin (B) cannot be distinguished in the obtained resin composition, so that the obtained resin composition appears to have only the matrix resin in addition to the polymer fine particles (A). Next, consider a case where the resin (B) is used in the manufacturing method of the resin composition, and the resin (B) is a different type of resin from the matrix resin. In this case, the matrix resin and the resin (B) can be distinguished in the obtained resin composition. In this case, the finally obtained resin composition may contain the resin (B) as a resin other than the matrix resin, in addition to the polymer fine particles (A).
[0152] The resin (B) may be, for example, a thermosetting resin, a thermoplastic resin, or any combination of a thermosetting resin and a thermoplastic resin. When the resin composition contains the resin (B), the resin (B) can have an effect of increasing the dispersibility of the polymer fine particles (A) in the thermosetting resin.
[0153] Examples of the thermosetting resin in resin (B) include various thermosetting resins described in the matrix resin section below. In resin (B), only one type of thermosetting resin may be used, or two or more types may be used in combination.
[0154] The thermoplastic resin in the resin (B) may be, for example, a polymer containing, as a structural unit, a structural unit derived from one or more monomers selected from the group consisting of an aromatic vinyl monomer, a vinyl cyan monomer, and a (meth)acrylate monomer. In the resin (B), only one type of thermoplastic resin may be used, or two or more types may be used in combination.
[0155] When the matrix resin to be mixed is a thermosetting resin, it is preferable that resin (B) is the same type as the thermosetting resin of the matrix resin, since there is no risk of affecting various physical properties. In other words, when the thermosetting resin of the matrix resin is an epoxy resin, resin (B) is also preferably an epoxy resin. When resin (B) is different from the thermosetting resin of the matrix resin, resin (B) is preferably compatible with the thermosetting resin of the matrix resin.
[0156] When the total of the polymer fine particles (A) and the resin (B) is taken as 100% by weight, it is preferable that the polymer fine particles (A) are 1 to 70% by weight and the resin (B) is 30 to 99% by weight. Within the above ranges, it is possible to improve fracture toughness, adhesive strength, surface impact resistance, etc. while maintaining the characteristics of a liquid thermosetting resin (heat resistance, rigidity, etc.). Note that the above ranges are intended to be the ratio of the polymer fine particles (A) and the resin (B) in the aggregate (resin composition) obtained by the production method of the resin composition.
[0157] From the viewpoint of viscosity, the polymer fine particles (A) are more preferably 10 to 60% by weight and the resin (B) is 90 to 40% by weight, the polymer fine particles (A) are even more preferably 20 to 50% by weight and the resin (B) is 80 to 50% by weight, and the polymer fine particles (A) are particularly preferably 25 to 45% by weight and the resin (B) is 75 to 55% by weight.
[0158] (others) In this specification, fats and oils and fatty acid esters are also included in resin (B). Fat and oil that can be suitably used as resin (B) include epoxidized fats and oils such as epoxidized soybean oil and epoxidized linseed oil. As the epoxidized soybean oil, a commercially available product can be used, for example, Adekaiser O-130P manufactured by ADEKA. Fatty acid ester that can be suitably used as resin (B) includes epoxidized fatty acid esters such as epoxidized fatty acid butyl, epoxidized fatty acid 2-ethylhexyl, epoxidized fatty acid octyl ester, and epoxidized fatty acid alkyl ester.
[0159] Epoxidized fats and oils and epoxidized fatty acid esters are sometimes referred to as epoxy plasticizers. That is, in this specification, epoxy plasticizers are also included in resin (B). Examples of epoxy plasticizers other than epoxidized fats and oils and epoxidized fatty acid esters include diepoxystearyl epoxyhexahydrophthalate and di-2-ethylhexyl epoxyhexahydrophthalate.
[0160] The above-mentioned thermosetting resin, thermoplastic resin, mixture of thermosetting resin and thermoplastic resin, oil and fat, and fatty acid ester can be used in combination with an antioxidant. In this specification, the antioxidant is considered to be a part of resin (B) only when it is used in combination with each of the above-mentioned substances. When the antioxidant is used alone, the antioxidant is not considered to be resin (B).
[0161] The antioxidant is not particularly limited, and examples of the antioxidant include (a) primary antioxidants such as phenol-based antioxidants, amine-based antioxidants, lactone-based antioxidants, and hydroxylamine-based antioxidants, and (b) secondary antioxidants such as sulfur-based antioxidants and phosphorus-based antioxidants.
[0162] The phenol-based antioxidant can be a hindered phenol-based antioxidant. The hindered phenol-based antioxidant can be a compound having a hindered phenol structure or a one-sided hindered phenol structure in the molecule. The phenol-based antioxidant can be a commercially available product, such as Irganox 245 manufactured by BASF Japan Ltd.
[0163] The amine-based antioxidant is not particularly limited, and a wide variety of known amine-based antioxidants can be used. Specific examples of the amine-based antioxidant include amine-ketone compounds such as 2,2,4-trimethyl-1,2-dihydroquinoline polymers, 6-ethoxy-1,2-dihydro-2,2,4-trimethylquinoline, and the reaction product of diphenylamine and acetone.
[0164] The amine-based antioxidant also includes aromatic amine compounds, such as naphthylamine-based antioxidants, diphenylamine-based antioxidants, and p-phenylenediamine-based antioxidants.
[0165] The lactone-based antioxidant, the hydroxylamine-based antioxidant, and the sulfur-based antioxidant are not particularly limited, and a wide variety of conventionally known antioxidants can be used.
[0166] The phosphorus-based antioxidant is not particularly limited, and conventionally known ones can be widely used. Phosphoric acid and phosphoric acid esters containing active hydrogen can adversely affect the storage stability of the resin composition containing the obtained powder and the heat resistance of the cured product or molded product provided by the resin composition. Therefore, as the phosphorus-based antioxidant, alkyl phosphite, aryl phosphite, alkylaryl phosphite compounds, etc., which do not contain phosphoric acid or phosphoric acid ester in the molecule, are preferred.
[0167] As the antioxidant, other conventionally known substances may be used. For example, various substances described in "Antioxidant Handbook" published by Taiseisha (first edition published on October 25, 1976) and "Polymer Additives Handbook" published by CMC Publishing (edited by Toru Haruna, first edition published on November 7, 2010) may be used.
[0168] The resin (B) is preferably one or more selected from the group consisting of a thermosetting resin, a mixture of a thermosetting resin and an antioxidant, a thermoplastic resin, a mixture of a thermoplastic resin and an antioxidant, fats and oils, a mixture of fats and oils and an antioxidant, a fatty acid ester, a mixture of a fatty acid ester and an antioxidant, an epoxy curing agent, and a mixture of an epoxy curing agent and an antioxidant, more preferably one or more selected from the group consisting of an epoxy resin, an acrylic polymer, a mixture of an epoxy resin and an antioxidant, a mixture of an acrylic polymer and an antioxidant, and a mixture of an epoxy plasticizer and an antioxidant, further preferably one or more selected from the group consisting of a mixture of an epoxy resin and an antioxidant, a mixture of an acrylic polymer and an antioxidant, and a mixture of an epoxy plasticizer and an antioxidant, and particularly preferably a mixture of an epoxy plasticizer and an antioxidant. According to this configuration, (a) the resin composition containing the obtained powdery material has the advantages of being able to provide a cured product or a molded product having excellent heat resistance, and (b) improving the dispersibility of the polymer fine particles (A) in the matrix resin.
[0169] 2. Method for producing resin composition (embodiment 2 including freezing step) Further, a method for producing a resin composition according to another embodiment of the present invention includes a resin mixing step of mixing a resin (B) having a viscosity of 1,000,000 mPa·s or less at 25° C. with a latex containing polymer fine particles (A); a freezing step of freezing the latex in which the resin (B) is dispersed obtained by the resin mixing step; a thawing step of thawing the latex frozen by the freezing step; and a separation step of separating a resin composition, which is an aggregate containing the polymer fine particles (A) and the resin (B), and a water component from the latex after the thawing step.
[0170] The present inventors have found that by mixing a latex containing polymer fine particles (A) with a resin (B) and then freezing, the water in the latex freezes, the polymer fine particles (A) and the resin (B) are concentrated, and the aggregates of the polymer fine particles (A) and the resin (B) are separated from the water. By dispersing the resin (B) in the latex containing the polymer fine particles (A), the resin (B) enters between the polymer fine particles (A). When the latex is then frozen, the aggregation of the polymer fine particles (A) can be prevented even if the freezing speed is slow, and an aggregate in which the polymer fine particles (A) are uniformly dispersed in the resin (B) can be obtained. In addition, in the present production method in which the polymer fine particles (A) and the resin (B) are mixed and then frozen, the freezing speed may be slow or fast.
[0171] According to this production method, as in the above-mentioned production method, since no salt such as a coagulant or organic solvent is used, the environmental load is small and it is possible to obtain aggregates with low impurities. In addition, since a freezing step is performed, the recovery efficiency of the polymer fine particles (A) is good, and further, the emulsifier is less entrained in the aggregates, so that it is possible to obtain aggregates with a low content of emulsifier-derived substances (impurities).
[0172] Each step of this embodiment will be described below, but the description of embodiment 1 will be used as appropriate for matters other than those described in detail below.
[0173] (2-1. Resin mixing process) The resin mixing step is a step of mixing a resin (B) having a viscosity of 1,000,000 mPa·s or less at 25°C with a latex containing polymer fine particles (A). This step can also be said to be a step of adding a resin (B) to a latex containing polymer fine particles (A) and mixing the latex to disperse the resin (B) in the latex. This step is the same as in embodiment 1, except that it is carried out before the freezing step and disperses the resin (B) in the latex.
[0174] In addition, in this resin mixing step, it is preferable that the resin (B) is dispersed in water in advance as an emulsion (also called an emulsion or aqueous emulsion) and then mixed with the latex. This allows the resin (B) to be uniformly dispersed in the latex containing the polymer fine particles (A), and by carrying out the freezing step described later and subsequent steps, an aggregate in which the polymer fine particles (A) and the resin (B) are more uniformly dispersed can be obtained.
[0175] (2-2. Freezing process) The freezing step is a step of freezing the latex in which the resin (B) obtained in the resin mixing step is dispersed, and is a step of freezing the latex to aggregate the polymer fine particles (A) and the resin (B).
[0176] The term "freezing" as used herein includes a process of rapid freezing and a process of slow freezing. The method of rapid freezing is the same as that in the first embodiment. Moreover, "slow freezing" means freezing the latex for 20 minutes to 24 hours, more preferably for 30 minutes to 12 hours, and further preferably for 1 hour to 10 hours. For example, examples of a method with a slow freezing speed include a method of freezing the latex in a freezer at -10°C to -80°C, a method of freezing the latex in a tunnel type or spiral type freezer, etc.
[0177] (2-3. Thawing process) The thawing step is a step of thawing the latex frozen in the freezing step. The specific thawing method is the same as that in the first embodiment.
[0178] (2-4. Separation process) The separation step is a step of separating the resin composition, which is an aggregate containing the polymer fine particles (A) and the resin (B), from the latex after the thawing step. In other words, it is a step of removing the water generated in the latex by the thawing step to obtain the resin composition, which is an aggregate containing the polymer fine particles (A) and the resin (B). The specific method of the separation step is the same as that of the first embodiment.
[0179] The present manufacturing method preferably further includes a washing step of washing the resin composition. By washing the resin composition, which is the aggregate obtained, with water, an aggregate having a low content of water-soluble compounds (impurities) is obtained. The details of the washing step are the same as those of the first embodiment.
[0180] (2-5. Removal process) The present production method preferably further includes a removal step of removing aggregates generated in the resin mixing step before the freezing step. In the resin mixing step, aggregates may be generated in the latex. In that case, it is preferable to remove the aggregated resin composition once before carrying out the freezing step. This is because the aggregates generated in the resin mixing step do not cause the polymer fine particles (A) to aggregate even if the latex is frozen thereafter. This allows the polymer fine particles (A) and the resin (B) to be efficiently aggregated and recovered in the freezing step.
[0181] 3. Method for Producing Resin Composition (Embodiment 3 Including Shearing Step) Further, a method for producing a resin composition according to another embodiment of the present invention includes a resin mixing step of mixing a resin (B) having a viscosity of 1,000,000 mPa s or less at 25° C. with a latex containing polymer fine particles (A), a shearing step of applying a shear stress to the latex obtained by the resin mixing step, and a first separation step of separating a resin composition, which is an aggregate containing the polymer fine particles (A) and the resin (B), and a water component from the latex after the shearing step.
[0182] The present inventors have found that by mixing a latex containing polymer fine particles (A) with a resin (B) and then applying shear to the mixed latex, the emulsifying effect of the latex is weakened, and aggregates are obtained in which the polymer fine particles (A) in the latex are aggregated in a dispersed state in the resin (B), and the water in the latex is separated.
[0183] According to this production method, since no organic solvent or salt such as a coagulant is used, the environmental impact is small and it is possible to obtain an aggregate with a low level of impurities. In addition, since the aggregate and water can be separated by applying shear, it is possible to obtain an aggregate with a low level of emulsifier.
[0184] Each step of this embodiment will be described below, but the descriptions of embodiments 1 and 2 will be cited as appropriate for matters other than those described in detail below.
[0185] (3-1. Resin mixing process) The resin mixing step is a step of mixing a resin (B) having a viscosity of 1,000,000 mPa·s or less at 25° C. with a latex containing polymer fine particles (A). This step is the same as in the first and second embodiments.
[0186] In the production method according to the present embodiment, from the viewpoint of easily forming aggregates by the shearing step described later, the solid content concentration in the latex (total concentration of the polymer fine particles (A) and the resin (B)) is preferably 1% or more, more preferably 3% or more, and even more preferably 5% or more.
[0187] (3-2. Shearing process) The shearing step is a step of applying a shear stress to the latex obtained in the resin mixing step, which is a mixture of the polymer fine particles (A) and the resin (B) obtained in the resin mixing step, to aggregate the polymer fine particles (A) and the resin (B).
[0188] The method of applying shear stress to the latex is not particularly limited, and various techniques can be used. For example, a process of stirring the latex at 3000 rpm to 25000 rpm using a homomixer, a process of stirring the latex at 500 rpm to 12000 rpm using a high-shear emulsifier, and a high-pressure homogenizer can be mentioned. From the viewpoint of aggregation speed, when using a homomixer, stirring is preferably performed at 5000 rpm to 25000 rpm, preferably at 7000 rpm to 20000 rpm, and more preferably at 8000 rpm to 20000 rpm. When stirring the latex using a high-shear emulsifier, stirring is preferably performed at 1000 rpm to 12000 rpm, preferably at 2000 rpm to 20000 rpm, and more preferably at 2500 rpm to 20000 rpm.
[0189] This step also includes a mode in which shear stress is applied in advance to the latex containing the polymer fine particles (A) before mixing with the resin (B) as a preliminary step of the resin mixing step. In addition, it also includes a mode in which shear stress is applied in advance to the resin (B). Furthermore, it may be a mode in which shear stress is applied in advance to both the latex containing the polymer fine particles (A) and the resin (B) before the resin mixing step. These methods are preferred in that they weaken the emulsifying power of the latex and allow for efficient production of aggregates.
[0190] When the viscosity of the resin (B) is high, it is preferable to adjust it to an optimal viscosity. For example, the optimal viscosity is more preferably 100 mPa·s to 750,000 mPa·s, more preferably 150 mPa·s to 700,000 mPa·s, more preferably 200 mPa·s to 350,000 mPa·s, more preferably 250 mPa·s to 300,000 mPa·s, more preferably 300 mPa·s to 50,000 mPa·s, even more preferably 350 mPa·s to 30,000 mPa·s, and particularly preferably 400 mPa·s to 15,000 mPa·s. There is no particular limitation on the means for adjusting the viscosity, but for example, a method of adjusting the temperature can be mentioned. By optimizing the viscosity of the resin (B), it is possible to prevent the pressure during transfer from becoming too high, and the shearing process can be efficiently carried out, and the aggregate can be efficiently obtained.
[0191] In addition, the shearing step is preferably carried out in the presence of a gas-liquid interface. According to this configuration, the polymer fine particles (A) and the resin (B) can be efficiently aggregated. In order to carry out the shearing step in the presence of a gas-liquid interface, it is sufficient that air bubbles (also called air or bubbles) exist in the latex obtained in the resin mixing step. In other words, the shearing step is preferably carried out while mixing the latex obtained in the resin mixing step with a gas (e.g., air, carbon dioxide, and nitrogen).
[0192] The temperature of the latex in this step is not particularly limited, and is preferably 10°C to 90°C, more preferably 15°C to 80°C, and even more preferably 20°C to 70°C, from the viewpoint of preventing deterioration of the polymer fine particles (A).
[0193] This shearing step can be carried out in various embodiments, and is not particularly limited. For example, there can be mentioned (i) an embodiment in which a shearing means (emulsifier, etc.) is provided in a container containing the latex obtained by the resin mixing step, and the step is carried out in a batch manner, (ii) an embodiment in which the step of passing the latex through the shearing means (emulsifier, etc.) is carried out multiple times by circulating, (iii) an embodiment in which the resin mixing step and the shearing step are carried out continuously (a step in which a shearing means (emulsifier, etc.) is provided after the flow path through which the latex passes and the flow path through which the resin (B) passes are joined, and shear is applied to the latex obtained by the resin mixing step), (iv) an embodiment in which the latex passes through the shearing means (emulsifier, etc.) multiple times in the embodiment (iii), and (v) an embodiment in which the latex passed through the shearing means (emulsifier, etc.) in the above (iii) or (iv) is separated into aggregates and water, and the operation of the above (iii) or (iv) is carried out multiple times with shear applied.
[0194] (3-3. First separation step) The first separation step is a step of separating the resin composition, which is an aggregate containing the polymer fine particles (A) and the resin (B), from the latex after the shearing step. This step is a step of removing the water in the latex generated by the shearing aggregation to obtain the first aggregate containing the polymer fine particles (A) and the resin (B). The details of the separation step are the same as those of the first embodiment.
[0195] (3-4. Flocculation step and second separation step) The present production method preferably further comprises an aggregation step of aggregating a resin composition, which is an aggregate containing polymer fine particles (A) and resin (B), from the water component from which the aggregates were separated in the first separation step, and a second separation step of separating the resin composition, which is an aggregate containing polymer fine particles (A) and resin (B), from the water component after the aggregation step. This step is a step of re-aggregating and recovering the aggregates containing polymer fine particles (A) and resin (B) that were not completely recovered in the above-mentioned step.
[0196] These steps allow recovery of unagglomerated polymer fine particles (A), improving productivity, and also lowering the COD (chemical oxygen demand) and reducing the wastewater load.
[0197] Furthermore, the aggregate obtained in the second separation step may be mixed with the aggregate obtained in the first separation step to form a resin composition.
[0198] In the aggregating step, the specific method for aggregating the polymer fine particles (A) and the resin (B) is not particularly limited, and examples thereof include a method using a coagulant and a method of freezing the latex.
[0199] For example, usable coagulants may be aqueous solutions of inorganic acids (salts) and / or organic acids (salts) having the property of coagulating and coagulating emulsion polymerized latex, or polymer flocculants, and examples thereof include sodium chloride, potassium chloride, lithium chloride, sodium bromide, potassium bromide, lithium bromide, potassium iodide, sodium iodide, potassium sulfate, sodium sulfate, ammonium sulfate, ammonium chloride, sodium nitrate, potassium nitrate, calcium chloride, ferrous sulfate, magnesium sulfate, zinc sulfate, copper sulfate, barium chloride, ferrous chloride, ferric chloride, magnesium chloride, and dilute sulfate. Aqueous solutions of inorganic salts such as iron, aluminum sulfate, potassium alum, and iron alum; aqueous solutions of inorganic acids such as hydrochloric acid, sulfuric acid, nitric acid, and phosphoric acid; organic acids such as acetic acid and formic acid and their aqueous solutions; aqueous solutions of organic acid salts such as sodium acetate, calcium acetate, sodium formate, and calcium formate; polymer flocculants are not particularly limited as long as they are polymer compounds having hydrophilic and hydrophobic groups, and may be any of anionic, cationic, and nonionic polymer flocculants, but cationic polymer flocculants are preferred because they can further enhance the effects of one embodiment of the present invention. As cationic polymer flocculants, polymer flocculants having cationic groups in the molecule, that is, polymer flocculants that exhibit cationicity when dissolved in water, such as polyamines, polydicyandiamides, cationized starch, cationic poly(meth)acrylamide, water-soluble aniline resins, polythiourea, polyethyleneimine, quaternary ammonium salts, polyvinylpyridines, chitosan, etc., may be used alone or in combination of two or more. Among these, aqueous solutions of monovalent or divalent inorganic salts or inorganic acids such as sodium chloride, potassium chloride, sodium sulfate, ammonium chloride, calcium chloride, magnesium chloride, magnesium sulfate, barium chloride, hydrochloric acid, sulfuric acid, etc. are preferably used. There is no particular limitation on the method of adding the coagulant, and it can be added all at once, in portions, or continuously.
[0200] The amount of the coagulant to be added is, for example, 1 to 50 parts by weight, preferably 2 to 30 parts by weight, and more preferably 3 to 20 parts by weight, relative to 100 parts by weight of the resin composition. The amount of the coagulant to be added can be appropriately changed depending on the type of latex.
[0201] Among them, the flocculation step preferably includes a freezing step of freezing the water component separated from the aggregate in the first separation step. According to this freezing step, the water component (latex) and the resin (B) separated from the aggregate in the first separation step are frozen, so that the water in the latex freezes, the polymer fine particles (A) and the resin (B) are concentrated to form an aggregate of the polymer fine particles (A) and the resin (B), and the water is separated. By obtaining the aggregate by the freezing step, it is not necessary to use a coagulant or the like, so that an aggregate with few impurities can be obtained. Details of the freezing step are the same as those of the first and second embodiments. Details of the second separation step are the same as those of the first embodiment.
[0202] The present manufacturing method preferably further includes a washing step of washing the resin composition. By washing the resin composition, which is the aggregate obtained, with water, an aggregate having a low content of water-soluble compounds (impurities) is obtained. The details of the washing step are the same as those of the first embodiment.
[0203] [4. Resin composition] A resin composition according to one embodiment of the present invention comprises polymer fine particles (A) having a graft portion made of a polymer containing, as a structural unit, a structural unit derived from one or more monomers selected from the group consisting of aromatic vinyl monomers, vinyl cyan monomers, and (meth)acrylate monomers, and a resin (B) having a viscosity of 1,000,000 mPa·s or less at 25°C, in which, when the total of the polymer fine particles (A) and the resin (B) is taken as 100% by weight, the polymer fine particles (A) account for 1 to 70% by weight and the resin (B) for 30 to 99% by weight, and when the content of the polymer fine particles (A) in the resin (B) is taken as 5% by weight, the dispersibility of the polymer fine particles (A) in the resin (B) is 0 μm or less when evaluated according to JIS K5101 using a grind gauge, the resin composition is substantially free of organic solvents, the contents of the elements S and P are both 150 ppm or less, and the electrical conductivity is 0.6 mS / cm or less. Hereinafter, this may be simply referred to as the present resin composition.
[0204] In addition, the resin composition preferably contains each of the elements Ca, Mg, Fe, Zn, Ba and Al in an amount of 100 ppm or less.
[0205] The resin composition has a low organic solvent content, so it has a low environmental impact and little adverse effect on the human body. In addition, an electrical conductivity of 0.6 mS / cm or less means that the amount of ions in the resin composition is small. A low amount of ions in the resin composition means that the resin composition contains few impurities and contaminants (water-soluble compounds) derived from emulsifiers, coagulants (inorganic salts), and metal soaps. For this reason, the resin composition is suitable for use in electronic materials and the like. This is because the amount of ions can cause corrosion of board wiring and element leads, and cause insulation failure and migration. The resin composition can be obtained, for example, by the above-mentioned method for producing a resin composition.
[0206] (4-1.Dispersibility) In the present resin composition, when the content of the polymer fine particles (A) in the resin (B) is 5% by weight, the dispersibility of the polymer fine particles (A) in the resin (B) is preferably 0 μm or less when evaluated according to JIS K5101 using a grind gauge. Since the polymer fine particles (A) are uniformly dispersed in the resin (B) in the present resin composition, when the present resin composition is mixed with a matrix resin, the polymer fine particles (A) can be well dispersed in the matrix resin. The specific method for evaluating the dispersibility will be described in detail in the following examples.
[0207] (4-2. Organic solvents) The resin composition is substantially free of organic solvents. By "substantially free of organic solvents" it is meant that the amount of organic solvent in the resin composition is 100 ppm or less.
[0208] The amount of organic solvent contained in the resin composition (also referred to as the amount of solvent) is preferably 100 ppm or less, more preferably 50 ppm or less, even more preferably 25 ppm or less, and particularly preferably 10 ppm or less. The amount of organic solvent contained in the resin composition can also be said to be the amount of volatile components (excluding water) contained in the resin composition. The amount of organic solvent (volatile components) contained in the resin composition can be determined as the weight loss by, for example, heating a predetermined amount of the resin composition with a hot air dryer or the like and measuring the weight of the resin composition before and after heating. The amount of organic solvent (volatile components) contained in the resin composition can also be determined by gas chromatography. In addition, when no organic solvent is used in the production of the resin composition and the powder and granules contained in the resin composition, the amount of organic solvent contained in the resulting resin composition can be considered to be 0 ppm.
[0209] Examples of organic solvents that are substantially not contained in the resin composition include (a) esters such as methyl acetate, ethyl acetate, propyl acetate, and butyl acetate; (b) ketones such as acetone, methyl ethyl ketone, diethyl ketone, and methyl isobutyl ketone; (c) alcohols such as ethanol, (iso)propanol, and butanol; (d) ethers such as tetrahydrofuran, tetrahydropyran, dioxane, and diethyl ether; (e) aromatic hydrocarbons such as benzene, toluene, and xylene; and (f) halogenated hydrocarbons such as methylene chloride and chloroform.
[0210] (4-3. Content of element S, etc.) In the resin composition, the contents of elements S and P are each 150 ppm or less. Furthermore, the contents of elements Ca, Mg, Fe, Zn, Ba, and Al are each preferably 100 ppm or less. Moreover, the contents of each of the above elements are preferably 100 ppm or less, more preferably 60 ppm or less, even more preferably 25 ppm or less, and particularly preferably 10 ppm or less.
[0211] (4-4. Electrical Conductivity) The electrical conductivity of the resin composition is 0.6 mS / cm or less. The electrical conductivity is more preferably 0.5 mS / cm or less, further preferably 0.3 mS / cm or less, and particularly preferably 0.15 mS / cm or less. The content of element Na as an impurity is Na + Since the metal soap derived from this is easily soluble in water, this can be understood by the electrical conductivity. For example, if the content of element Na is high, Na + Therefore, when the electrical conductivity is lower than the above-mentioned predetermined value, the content of element Na is also considered to be low.
[0212] In this specification, the term "electrical conductivity" refers to the electrical conductivity of water separated by mixing the resin composition with an equal amount of ion-exchanged water at 90° C. for 30 minutes. A specific measurement method will be described in detail in the examples described later.
[0213] (4-5. Polymer microparticles (A) and resin (B)) The polymer fine particles (A) and the resin (B) are the same as those in the above-mentioned embodiment 1 (method of producing a resin composition), and the descriptions in embodiment 1 can be used. In particular, the polymer fine particles (A) are preferably rubber-containing graft copolymers having an elastomer and a graft portion grafted to the elastomer. In addition, the elastomer preferably contains one or more selected from the group consisting of diene rubber, (meth)acrylate rubber, and polysiloxane rubber elastomer.
[0214] Resin (B) is preferably a thermosetting resin, and more preferably at least one selected from the group consisting of ethylenically unsaturated monomers, epoxy resins, phenolic resins, polyol resins, and amino-formaldehyde resins (melamine resins).
[0215] The above-described structure can improve fracture toughness, adhesive strength, surface impact resistance, and the like while maintaining the characteristics of the liquid curable resin (heat resistance, rigidity, and the like).
[0216] 5. Resin composition (mixture of the present resin composition and matrix resin) An embodiment of the present invention may include a resin composition obtained by mixing the above-mentioned resin composition with a matrix resin. That is, the resin composition contains the above-mentioned resin composition and a matrix resin.
[0217] (5-1. Matrix resin) As the matrix resin, a thermosetting resin can be suitably used. The thermosetting resin preferably contains at least one thermosetting resin selected from the group consisting of a resin containing a polymer obtained by polymerizing an ethylenically unsaturated monomer, an epoxy resin, a phenol resin, a polyol resin, and an amino-formaldehyde resin (melamine resin). In addition, the thermosetting resin may also include a resin containing a polymer obtained by polymerizing an aromatic polyester raw material. Examples of the aromatic polyester raw material include radical polymerizable monomers such as aromatic vinyl compounds, (meth)acrylic acid derivatives, vinyl cyanide compounds, and maleimide compounds, dimethyl terephthalate, and alkylene glycol. Only one type of these thermosetting resins may be used, or two or more types may be used in combination.
[0218] (ethylenically unsaturated monomer) The ethylenically unsaturated monomer is not particularly limited as long as it has at least one ethylenically unsaturated bond in the molecule.
[0219] Examples of the ethylenically unsaturated monomer include acrylic acid, α-alkylacrylic acid, α-alkylacrylic acid ester, β-alkylacrylic acid, β-alkylacrylic acid ester, methacrylic acid, acrylic acid ester, methacrylic acid ester, vinyl acetate, vinyl ester, unsaturated ester, polyunsaturated carboxylic acid, polyunsaturated ester, maleic acid, maleic acid ester, maleic anhydride, and acetoxystyrene. These may be used alone or in combination of two or more.
[0220] (Epoxy resin) The epoxy resin is not particularly limited as long as it has at least one epoxy bond in the molecule.
[0221] Specific examples of epoxy resins include bisphenol A type epoxy resins, bisphenol F type epoxy resins, bisphenol AD type epoxy resins, bisphenol S type epoxy resins, glycidyl ester type epoxy resins, glycidyl amine type epoxy resins, novolac type epoxy resins, glycidyl ether type epoxy resins of bisphenol A propylene oxide adducts, hydrogenated bisphenol A (or F) type epoxy resins, fluorinated epoxy resins, rubber-modified epoxy resins containing polybutadiene or NBR, flame-retardant epoxy resins such as glycidyl ether of tetrabromobisphenol A, p-oxybenzoic acid glycidyl ether ester type epoxy resins, m-aminophenol type epoxy resins, diaminodiphenylmethane type epoxy resins, urethane-modified epoxy resins having a urethane bond, various alicyclic epoxy resins, glycidyl ethers of polyhydric alcohols, hydantoin type epoxy resins, epoxidized products of unsaturated polymers such as petroleum resins, and amino-containing glycidyl ether resins. Examples of the polyhydric alcohol include N,N-diglycidylaniline, N,N-diglycidyl-o-toluidine, triglycidyl isocyanurate, polyalkylene glycol diglycidyl ether, and glycerin. Examples of the epoxy resin include epoxy compounds obtained by subjecting the above-mentioned epoxy resin to an addition reaction with bisphenol A (or F) or polybasic acids. The epoxy resin is not limited to these, and any commonly used epoxy resin may be used. These epoxy resins may be used alone or in combination of two or more.
[0222] Among the above-mentioned epoxy resins, those having at least two epoxy groups in one molecule are preferred because they have high reactivity in curing the resin composition and the obtained cured product is likely to form a three-dimensional network, etc. Furthermore, as the epoxy resin, those mainly composed of bisphenol-type epoxy resins are preferred among the epoxy resins having at least two epoxy groups in one molecule because of their excellent economical efficiency and ease of availability.
[0223] (Phenol Resin) The phenolic resin is not particularly limited as long as it is a compound obtained by reacting a phenol with an aldehyde. The phenol is not particularly limited, but examples thereof include phenols such as phenol, orthocresol, meta-cresol, para-cresol, xylenol, para-tertiary butylphenol, para-octylphenol, para-phenylphenol, bisphenol A, bisphenol F, and resorcin. Particularly preferred phenols include phenol and cresol.
[0224] The aldehydes are not particularly limited, and examples thereof include formaldehyde, acetaldehyde, butylaldehyde, acrolein, and mixtures thereof. As the aldehydes, the above-mentioned substances that are sources of aldehydes or solutions of these aldehydes can also be used. As the aldehydes, formaldehyde is preferred because the operation of reacting phenols with aldehydes is easy.
[0225] When reacting phenols with aldehydes, the molar ratio (F / P) of phenols (P) to aldehydes (F) (hereinafter also referred to as reaction molar ratio) is not particularly limited. When an acid catalyst is used in the reaction, the reaction molar ratio (F / P) is preferably 0.4 to 1.0, more preferably 0.5 to 0.8. When an alkali catalyst is used in the reaction, the reaction molar ratio (F / P) is preferably 0.4 to 4.0, more preferably 0.8 to 2.5. When the reaction molar ratio is equal to or more than the lower limit, the yield is not too low, and there is no risk of the molecular weight of the obtained phenolic resin being small. On the other hand, when the reaction molar ratio is equal to or less than the upper limit, the molecular weight of the phenolic resin is not too high and the softening point is not too high, so that sufficient fluidity can be obtained during heating. Furthermore, when the reaction molar ratio is equal to or less than the upper limit, the molecular weight is easily controlled, and there is no risk of gelation or partial gelation due to the reaction conditions.
[0226] (Polyol resin) The polyol resin is a compound having two or more active hydrogens at the terminals, and is a polyol having two or more functionalities and a molecular weight of about 50 to 20,000. Examples of the polyol resin include aliphatic alcohols, aromatic alcohols, polyether polyols, polyester polyols, polyolefin polyols, and acrylic polyols.
[0227] The aliphatic alcohol may be either a dihydric alcohol or an alcohol having three or more hydricities (such as a trihydric alcohol or a tetrahydric alcohol). Examples of the dihydric alcohol include alkylene glycols such as ethylene glycol, propylene glycol, 1,3-propanediol, 1,3-butanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 3-methyl-1,5-pentanediol, and neopentyl glycol (particularly alkylene glycols having about 1 to 6 carbon atoms), and dehydration condensates of two or more molecules of the alkylene glycols (for example, about 2 to 6 molecules) (diethylene glycol, dipropylene glycol, tripropylene glycol, etc.). Examples of the trihydric alcohol include glycerin, trimethylolpropane, trimethylolethane, and 1,2,6-hexanetriol (particularly trihydric alcohols having about 3 to 10 carbon atoms). Examples of the tetrahydric alcohol include pentaerythritol and diglycerin. Further examples include sugars such as monosaccharides, oligosaccharides, and polysaccharides.
[0228] Examples of aromatic alcohols include bisphenols such as bisphenol A and bisphenol F; biphenyls such as dihydroxybiphenyl; polyhydric phenols such as hydroquinone and phenol formaldehyde condensates; and naphthalenediol.
[0229] Examples of polyether-type polyols include random copolymers or block copolymers obtained by ring-opening polymerization of ethylene oxide, propylene oxide, butylene oxide, styrene oxide, etc. in the presence of one or more types of initiators containing active hydrogen, and mixtures of these copolymers. Examples of initiators containing active hydrogen used in ring-opening polymerization of polyether-type polyols include diols such as ethylene glycol, diethylene glycol, propylene glycol, dipropylene glycol, 1,3-butanediol, 1,4-butanediol, 1,6-hexanediol, neopentyl glycol, and bisphenol A; triols such as trimethylolethane, trimethylolpropane, and glycerin; saccharides such as monosaccharides, oligosaccharides, and polysaccharides; sorbitol; amines such as ammonia, ethylenediamine, urea, monomethyldiethanolamine, and monoethyldiethanolamine; and the like.
[0230] Examples of polyester-type polyols include polymers obtained by polycondensing (a) polybasic acids and / or acid anhydrides thereof, such as maleic acid, fumaric acid, adipic acid, sebacic acid, phthalic acid, dodecanedioic acid, isophthalic acid, and azelaic acid, and (b) polyhydric alcohols, such as ethylene glycol, propylene glycol, 1,4-butanediol, 1,6-hexanediol, diethylene glycol, dipropylene glycol, neopentyl glycol, and 3-methyl-1,5-pentanediol, in the presence of an esterification catalyst at a temperature range of 150 to 270° C. Further, examples of (a) polyester-type polyols include ring-opening polymers such as ε-caprolactone and valerolactone, and (b) active hydrogen compounds having two or more active hydrogens, such as polycarbonate diol and castor oil.
[0231] Examples of polyolefin polyols include polybutadiene polyols, polyisoprene polyols, and hydrogenated products thereof.
[0232] Examples of acrylic polyols include (a) copolymers of hydroxyl group-containing monomers such as hydroxyethyl (meth)acrylate, hydroxybutyl (meth)acrylate, and vinylphenol with general-purpose monomers such as n-butyl (meth)acrylate and 2-ethylhexyl (meth)acrylate, and mixtures of such copolymers.
[0233] Among these polyol resins, polyether-type polyols are preferred because the resulting resin composition has low viscosity and excellent workability, and the resin composition can provide a cured product with an excellent balance between hardness and toughness.Furthermore, among these polyol resins, polyester-type polyols are preferred because the resulting resin composition can provide a cured product with excellent adhesion.
[0234] (Amino-formaldehyde resin) The amino-formaldehyde resin is not particularly limited as long as it is a compound obtained by reacting an amino compound with an aldehyde under an alkaline catalyst. Examples of the amino compound include melamine; 6-substituted guanamines such as guanamine, acetoguanamine, and benzoguanamine; amine-substituted triazine compounds such as CTU guanamine (3,9-bis[2-(3,5-diamino-2,4,6-triazaphenyl)ethyl]-2,4,8,10-tetraoxaspiro[5,5]undecane) and CMTU guanamine (3,9-bis[(3,5-diamino-2,4,6-triazaphenyl)methyl]-2,4,8,10-tetraoxaspiro[5,5]undecane); and ureas such as urea, thiourea, and ethylene urea. As the amino compound, a substituted melamine compound in which hydrogen of an amino group of melamine is substituted with an alkyl group, an alkenyl group, and / or a phenyl group (described in U.S. Pat. No. 5,998,573 (corresponding Japanese Unexamined Patent Publication: JP-A-9-143238)) and a substituted melamine compound in which hydrogen of an amino group of melamine is substituted with a hydroxyalkyl group, a hydroxyalkyloxyalkyl group, and / or an aminoalkyl group (described in U.S. Pat. No. 5,322,915 (corresponding Japanese Unexamined Patent Publication: JP-A-5-202157)) can also be used. As the amino compound, among the above-mentioned compounds, polyfunctional amino compounds such as melamine, guanamine, acetoguanamine, and benzoguanamine are preferred, and melamine is particularly preferred, because they are industrially produced and inexpensive. The above-mentioned amino compounds may be used alone or in combination of two or more kinds. In addition to these amino compounds, (a) phenols such as phenol, cresol, alkylphenols, resorcin, hydroquinone, and pyrogallol, and (b) aniline, etc. may also be used.
[0235] Examples of the aldehydes include formaldehyde, paraformaldehyde, acetaldehyde, benzaldehyde, and furfural. As the aldehydes, formaldehyde and paraformaldehyde are preferred because they are inexpensive and have good reactivity with the amino compounds listed above. In the production of the amino-formaldehyde resin, the aldehydes are preferably used in an amount of 1.1 to 6.0 moles per effective aldehyde group relative to 1 mole of the amino compound, and more preferably 1.2 to 4.0 moles.
[0236] (Physical properties of thermosetting resins) The properties of the thermosetting resin are not particularly limited. The thermosetting resin preferably has a viscosity of 100 mPa·s to 1,000,000 mPa·s at 25°C. The viscosity of the thermosetting resin is more preferably 50,000 mPa·s or less, even more preferably 30,000 mPa·s or less, and particularly preferably 15,000 mPa·s or less at 25°C. According to the above configuration, the thermosetting resin has the advantage of excellent fluidity. A thermosetting resin having a viscosity of 100 mPa·s to 1,000,000 mPa·s at 25°C can also be said to be a liquid.
[0237] The greater the fluidity of the thermosetting resin, in other words, the smaller the viscosity, the more difficult it is to disperse the polymer fine particles (A) in the form of primary particles in the thermosetting resin. Conventionally, it has been very difficult to disperse the polymer fine particles (A) in the form of primary particles in a thermosetting resin having a viscosity of 1,000,000 mPa·s or less at 25°C. However, the resin composition according to one embodiment of the present invention has the advantage that the polymer fine particles (A) having the above-mentioned configuration are well dispersed in a thermosetting resin having a viscosity of 1,000,000 mPa·s or less at 25°C.
[0238] In addition, the viscosity of the thermosetting resin at 25°C is more preferably 100 mPa·s or more, even more preferably 500 mPa·s or more, even more preferably 1000 mPa·s or more, and particularly preferably 1500 mPa·s or more, because the thermosetting resin can penetrate into the polymer microparticles (A) and prevent the polymer microparticles (A) from fusing together.
[0239] The thermosetting resin may have a viscosity of more than 1,000,000 mPa·s. The thermosetting resin may be semi-solid (semi-liquid) or solid. When the thermosetting resin has a viscosity of more than 1,000,000 mPa·s, the resulting resin composition has the advantage of being less sticky and easier to handle.
[0240] The thermosetting resin preferably has an endothermic peak at 25° C. or less in a thermogram obtained by differential scanning calorimetry (DSC), and more preferably has an endothermic peak at 0° C. or less. According to the above-mentioned configuration, the thermosetting resin has an advantage of excellent fluidity.
[0241] (5-2. Blending ratio of the resin composition to the matrix resin, etc.) The blending ratio of the present resin composition to the matrix resin, assuming the total of the present resin composition and the matrix resin to be 100% by weight, is usually preferably 0.5 to 50% by weight of the present resin composition and 50 to 99.5% by weight of the matrix resin, more preferably 1 to 35% by weight of the present resin composition and 65 to 99% by weight of the matrix resin, particularly preferably 1.5 to 25% by weight of the present resin composition and 75 to 98.5% by weight of the matrix resin, and most preferably 2.5 to 20% by weight of the present resin composition and 80 to 97.5% by weight of the matrix resin.
[0242] When the matrix resin is a thermosetting resin, its state is not particularly limited as long as it flows when mixed with the present resin composition, and it may be solid at room temperature, but is preferably liquid from the viewpoint of workability.
[0243] The temperature at which the resin composition is mixed with the thermosetting matrix resin is generally a temperature at which the thermosetting matrix resin can flow. If the resin (B) can flow at a temperature at which the thermosetting matrix resin can flow, it becomes easy to uniformly mix the resin (B) and the thermosetting matrix resin. Conversely, if the thermosetting matrix resin is liquid and the epoxy resin in the resin composition to be added to it is solid, it becomes difficult to uniformly mix the two. In this specification, when the thermosetting matrix resin is liquid at 25°C, it is interpreted that "the viscosity of the thermosetting matrix resin at 25°C is equal to or higher than the viscosity of the resin (B) at 25°C."
[0244] (5-3. Other optional ingredients) The mixture of the resin composition and the matrix resin preferably further contains an antiblocking agent from the viewpoint of improving blocking resistance and dispersibility in the thermosetting matrix resin. The antiblocking agent is not particularly limited as long as it has the above-mentioned effect. Examples of the antiblocking agent include antiblocking agents made of inorganic fine particles such as silicon dioxide, titanium oxide, aluminum oxide, zirconium oxide, aluminum silicate, diatomaceous earth, zeolite, kaolin, talc, calcium carbonate, calcium phosphate, barium sulfate, and magnesium hydrosilicate; antiblocking agents made of organic fine particles; and oil-based antiblocking agents such as polyethylene wax, higher fatty acid amide, metal soap, and silicone oil. Among these, antiblocking agents made of fine particles are preferred, antiblocking agents made of organic fine particles are more preferred, and antiblocking agents made of organic fine particles of a polymer containing one or more monomer units selected from aromatic vinyl monomers, vinyl cyan monomers, and (meth)acrylate monomers are particularly preferred.
[0245] The antiblocking agent consisting of fine particles is generally a dispersion of fine particles in a liquid or a colloidal one. The fine particles in the antiblocking agent usually have a volume average particle diameter (Mv) of 10 μm or less, preferably 0.05 to 10 μm. The content of the antiblocking agent is preferably 0.01 to 5.0% by weight, more preferably 0.5 to 3.0% by weight, based on the total weight of the resin composition and the matrix resin.
[0246] The mixture of the resin composition and the matrix resin may contain optional components other than those described above, as necessary. Examples of the optional components include curing agents, colorants such as pigments and dyes, extender pigments, UV absorbers, antioxidants, heat stabilizers (gelling inhibitors), plasticizers, leveling agents, defoamers, silane coupling agents, antistatic agents, flame retardants, lubricants, viscosity reducers, shrinkage reducing agents, inorganic fillers, organic fillers, thermoplastic resins, desiccants, and dispersants.
[0247] The antiblocking agent and additives (the other optional components) can be added appropriately in any step in the production method of the present resin composition. For example, the antiblocking agent and additives can be added to the aqueous suspension of the polymer fine particles (A) before or after they are solidified, or to the present resin composition or a mixture of the present resin composition and a matrix resin.
[0248] The mixture of the present resin composition and a matrix resin may further contain a known thermosetting resin or a known thermoplastic resin other than the matrix resin.
[0249] [6. Cured product] The cured product according to one embodiment of the present invention is obtained by curing the resin composition described in Section 5. Resin composition (mixture of the present resin composition and matrix resin). Hereinafter, it will also be referred to simply as the present cured product.
[0250] Because the cured product has the above-mentioned constitution, it is resistant to rust even when it is applied to a metal plate or the like and then cured. In addition, the cured product (a) has a beautiful surface, (b) has high rigidity and high elastic modulus, and (c) has excellent toughness and adhesiveness.
[0251] [7. Other uses] The above-mentioned resin composition and the mixture of the resin composition and the matrix resin (hereinafter simply referred to as the resin composition, etc.) can be used for various applications, and the applications are not particularly limited. The resin composition, etc. are preferably used for applications such as adhesives, coating materials, binders for reinforcing fibers, composite materials, 3D printer molding materials, sealants, electronic substrates, ink binders, wood chip binders, rubber chip binders, foam chip binders, binders for castings, rock consolidation materials for flooring and ceramics, and urethane foams. Examples of urethane foams include automobile seats, automobile interior parts, sound absorbing materials, vibration damping materials, shock absorbers (shock absorbing materials), heat insulating materials, and construction flooring cushions.
[0252] Among the above-mentioned applications, the present resin composition etc. is more preferably used as an adhesive, a coating material, a binder for reinforcing fibers, a composite material, a molding material for 3D printers, a sealant, and an electronic substrate.
[0253] (7-1. Adhesive) An adhesive according to one embodiment of the present invention contains the above-mentioned resin composition, etc. Since the adhesive according to one embodiment of the present invention has the above-mentioned configuration, it has excellent adhesiveness.
[0254] The adhesive according to one embodiment of the present invention is also simply referred to as the present adhesive.
[0255] The adhesive can be suitably used for a variety of applications, such as for automotive interior materials, general woodworking, furniture, interior decoration, wall materials, and food packaging.
[0256] The adhesive exhibits good adhesion to a variety of substrates, including cold-rolled steel, aluminum, fiberglass-reinforced polyester (FRP), panels of cured thermosetting resins such as epoxy resins reinforced with carbon fiber, panels of thermoplastic resin sheets reinforced with carbon fiber, sheet molding compound (SMC), acrylonitrile-butadiene-styrene copolymer (ABS), polyvinyl chloride (PVC), polycarbonate, polypropylene, TPO, wood and glass.
[0257] This adhesive has excellent adhesive properties and flexibility not only at low temperatures (about -20°C) to room temperature, but also at high temperatures (about 80°C). Therefore, this adhesive can be used more suitably as a structural adhesive.
[0258] Structural adhesives using this adhesive can be used, for example, as adhesives for structural members in the fields of automobiles and vehicles (such as bullet trains and trains), civil engineering, architecture, building materials, woodworking, electricity, electronics, aircraft, and the space industry. In particular, automotive-related applications include adhesion of interior materials such as ceilings, doors, and seats, and adhesion of exterior materials such as automotive lighting fixtures such as lamps and side moldings.
[0259] The present adhesive can be produced using the present resin composition, etc. The method for producing the present adhesive is not particularly limited, and any known method can be used.
[0260] (7-2. Coating materials) The coating material according to one embodiment of the present invention contains the above-mentioned resin composition, etc. Since the coating material according to one embodiment of the present invention has the above-mentioned configuration, it can provide a coating film having excellent load resistance and abrasion resistance.
[0261] The coating material according to one embodiment of the present invention is also simply referred to as the present coating material.
[0262] When applying this coating material to, for example, a floor or a corridor, a commonly used application method can be applied. For example, after applying a primer to the prepared base, the coating material is applied evenly using a trowel, roller, rake, spray gun, etc. depending on the application conditions. After applying this coating material, it hardens and a high-performance pavement film is obtained. The coating film obtained by hardening this coating material can be a coating film with excellent load-bearing and abrasion resistance.
[0263] The viscosity of the resin composition used in the coating material may be adjusted depending on the application method of the coating material. For example, when a trowel or rake is used to apply the coating material, the viscosity of the resin composition used in the coating material can be generally adjusted to about 500 to 9,000 cps / 25°C. When a roller or spray is used to apply the coating material, the viscosity of the resin composition used in the coating material can be generally adjusted to about 100 to 3,000 cps / 25°C.
[0264] There is no particular limitation on the substrate (i.e., the material of the floor or corridor) to which the coating material is applied. Specific examples of the substrate include (a) inorganic substrates such as concrete walls, concrete plates, concrete blocks, CMU (Concrete Masonry Unit), mortar boards, ALC (Autoclaved Light-weight Concrete) boards, gypsum boards (Dens Glass Gold: Georgia Pacific, etc.), and slate boards, (b) organic substrates such as wood substrates (wood, plywood, OSB (Oriented Strand Board), etc.), asphalt, modified bitumen waterproof sheets, ethylene-propylene-diene rubber (EPDM) waterproof sheets, TPO waterproof sheets, plastics, FRP, and polyurethane foam insulation, and (c) metal substrates such as metal panels.
[0265] The present coating material is applied to a metal substrate or a porous substrate. The laminate obtained by curing the coating material after the application is excellent in corrosion resistance to the substrate. In addition, the coating film obtained by curing the coating material after the application can impart excellent crack resistance and load resistance to the substrate. Therefore, the embodiment in which the present coating material is applied to a metal substrate or a porous substrate is particularly preferable.
[0266] The method for applying the coating material is not particularly limited, but can be any known application method such as with a trowel, rake, brush, roller, air spray, or airless spray.
[0267] The uses of the present coating material are not particularly limited, but include automobiles, electrical equipment, office machines, building materials, wood, painted floors, pavement, heavy-duty corrosion protection, concrete corrosion protection, rooftop and roof waterproofing, rooftop and roof corrosion resistance, underground waterproofing coating waterproofing material, automobile repair, can painting, top coat, intermediate coat, undercoat, primer, electrodeposition paint, highly weather-resistant paint, non-yellowing paint, etc. When used as a coating material for painted floors and pavement coating materials, it can be used in factories, laboratories, warehouses, clean rooms, etc.
[0268] The present coating material can be produced using the present resin composition, etc. The method for producing the present coating material is not particularly limited, and any known method can be used.
[0269] (7-3. Composite materials) A composite material according to one embodiment of the present invention contains the above-mentioned resin composition as a binder for reinforcing fibers. Since the composite material according to one embodiment of the present invention has the above-mentioned configuration, it has the advantage of being excellent in toughness and impact resistance.
[0270] The composite material according to one embodiment of the present invention is also simply referred to as the present composite material.
[0271] The composite material may contain reinforcing fibers. Examples of the reinforcing fibers include, but are not limited to, glass fibers, long glass fibers, carbon fibers, natural fibers, metal fibers, thermoplastic resin fibers, boron fibers, aramid fibers, polyethylene fibers, and Zylon reinforcing fibers. Among these reinforcing fibers, glass fibers and carbon fibers are particularly preferred.
[0272] The manufacturing method (molding method) of this composite material is not particularly limited, but examples include autoclave molding using prepreg, filament wind molding, hand lay-up molding, vacuum bag molding, resin transfer molding (RTM) method, vacuum assisted resin transfer molding (VARTM) method, pultrusion molding, injection molding, sheet winding molding, spray-up method, BMC (Bulk Molding Compound) method, SMC (Sheet Molding Compound) method, and the like.
[0273] In particular, when carbon fiber is used as the reinforcing fiber, the preferred manufacturing method for this composite material is an autoclave molding method using a prepreg, a filament wind molding method, a hand lay-up molding method, a vacuum bag molding method, a resin transfer molding (RTM) method, a vacuum assisted resin transfer molding (VARTM) method, or the like.
[0274] Applications of the composite material include, but are not limited to, aircraft, spacecraft, automobiles, bicycles, ships, weapons, windmills, sporting goods, containers, building materials, waterproofing materials, printed circuit boards, and electrical insulating materials.
[0275] The present composite material can be produced using the present resin composition, etc. For more detailed information on the present composite material, such as reinforcing fibers, production method (molding method), production conditions (molding conditions), compounding agents, and applications, see U.S. Patent Publication No. 2006 / 0173128, U.S. Patent Publication No. 2012 / 0245286, JP-A-2002-530445 (International Publication No. WO2000 / 029459), and JP-A-55-157620. Examples of such a compound include those described in U.S. Pat. No. 4,251,428, JP 2013-504007 A (International Publication WO2011 / 028271 A), JP 2007-125889 A (U.S. Patent Publication No. 2007 / 0098997 A), and JP 2003-220661 A (U.S. Patent Publication No. 2003 / 0134085 A).
[0276] (7-4.3D printer modeling materials) The modeling material for a 3D printer according to one embodiment of the present invention contains the above-mentioned resin composition, etc. Since the modeling material for a 3D printer according to one embodiment of the present invention has the above-mentioned configuration, it has the advantage of being excellent in toughness and impact resistance.
[0277] The modeling material of the 3D printer according to one embodiment of the present invention is also referred to simply as the modeling material.
[0278] Applications of the present molding material include, but are not limited to, prototypes for the purpose of verifying designs and functions before actually making a product, aircraft parts, building materials, and medical equipment parts.
[0279] The present modeling material can be produced using the present resin composition, etc. The method for producing the present modeling material is not particularly limited, and any known method can be used.
[0280] (7-5. Sealant) The sealant according to one embodiment of the present invention is formed using the above-mentioned resin composition, etc. Since the sealant according to one embodiment of the present invention has the above-mentioned configuration, it has the advantage of being excellent in toughness and impact resistance.
[0281] The sealant according to one embodiment of the present invention is also simply referred to as the present sealant.
[0282] Applications of the present sealant include, but are not limited to, sealing of various electric devices such as semiconductors and power devices.
[0283] The present sealant can be produced using the present resin composition, etc. The method for producing the present sealant is not particularly limited, and any known method can be used.
[0284] (7-6. Electronic board) The electronic substrate according to one embodiment of the present invention is formed using the above-mentioned resin composition, etc. Since the electronic substrate according to one embodiment of the present invention has the above-mentioned configuration, it has the advantage of being excellent in toughness and impact resistance.
[0285] The electronic board according to one embodiment of the present invention is also simply referred to as the present electronic board.
[0286] Applications of the electronic substrate include, but are not limited to, printed circuits, printed wiring, printed circuit boards, printed circuit mounted products, printed wiring boards, and printed boards.
[0287] The present electronic substrate can be manufactured from the present resin composition, etc. The method for manufacturing the present electronic substrate is not particularly limited, and a known method can be used.
[0288] 〔summary〕 An embodiment of the present invention includes the following inventions.
[0289] (1) A method for producing a resin composition, comprising: a quick freezing step of quickly freezing latex containing polymer fine particles (A); a thawing step of thawing the latex frozen in the quick freezing step; a resin mixing step of mixing a liquid, semi-solid, or solid resin (B) having a viscosity of 100 mPa s to 1,000,000 mPa s at 25°C with the latex after the quick freezing step; and a separation step of separating a resin composition which is an aggregate containing the polymer fine particles (A) and the resin (B) and a water component from the latex after the thawing step and the resin mixing step.
[0290] (2) A method for producing a resin composition, comprising: a resin mixing step of mixing a latex containing polymer fine particles (A) with a liquid, semi-solid or solid resin (B) having a viscosity of 100 mPa s to 1,000,000 mPa s at 25°C; a freezing step of freezing the latex in which the resin (B) is dispersed obtained in the resin mixing step; a thawing step of thawing the latex frozen in the freezing step; and a separation step of separating a resin composition which is an aggregate containing the polymer fine particles (A) and the resin (B) and a water component from the latex after the thawing step.
[0291] (3) The method for producing a resin composition according to (2), further comprising a removing step of removing aggregates generated in the resin mixing step before the freezing step.
[0292] (4) A method for producing a resin composition, comprising: a resin mixing step of mixing a latex containing polymer fine particles (A) with a liquid, semi-solid, or solid resin (B) having a viscosity of 100 mPa s to 1,000,000 mPa s at 25°C; a shearing step of applying a shear stress to the latex obtained by the resin mixing step; and a first separation step of separating a resin composition, which is an aggregate containing the polymer fine particles (A) and the resin (B), and a water component from the latex after the shearing step.
[0293] (5) The method for producing the resin composition according to (4), further comprising: an aggregation step of aggregating a resin composition which is an aggregate containing polymer fine particles (A) and a resin (B) from the water component from which the aggregates have been separated in the first separation step; and a second separation step of separating the resin composition which is an aggregate containing polymer fine particles (A) and a resin (B) from the water component after the aggregation step.
[0294] (6) The method for producing a resin composition according to (5), wherein the agglomeration step includes a step of freezing the water component separated from the agglomerates in the first separation step.
[0295] (7) The method for producing a resin composition according to any one of (1), (2), (4), and (5), further comprising a step of adjusting the water content of the aggregates to 5% by weight to 60% by weight in 100% by weight of the aggregates in the separation step, the first separation step, or the second separation step.
[0296] (8) The method for producing a resin composition according to any one of (1) to (7), further comprising a washing step of washing the resin composition.
[0297] (9) The method for producing a resin composition according to any one of (1) to (8), wherein the polymer fine particles (A) account for 1 to 70% by weight and the resin (B) accounts for 30 to 99% by weight, assuming that the total of the polymer fine particles (A) and the resin (B) is 100% by weight.
[0298] (10) A polymer fine particle (A) having a graft portion made of a polymer containing, as a structural unit, a structural unit derived from one or more monomers selected from the group consisting of an aromatic vinyl monomer, a vinyl cyan monomer, and a (meth)acrylate monomer, and a resin (B) which is liquid, semi-solid, or solid and has a viscosity of 100 mPa·s to 1,000,000 mPa·s at 25°C, wherein, when the total of the polymer fine particle (A) and the resin (B) is taken as 100% by weight, the polymer fine particle (A) is 1 to 70% by weight and the resin (B) is 30 to 99% by weight, and when the content of the polymer fine particle (A) in the resin (B) is 5% by weight, the dispersibility of the polymer fine particle (A) in the resin (B) is 0 μm or less when evaluated according to JIS K5101 using a grind gauge, the resin is substantially free of organic solvents, and the contents of the elements S and P are both 150 ppm or less, A resin composition having an electrical conductivity of 0.6 mS / cm or less.
[0299] (11) The resin composition according to (10), further comprising elements Ca, Mg, Fe, Zn, Ba and Al each having a content of 100 ppm or less.
[0300] (12) The resin composition according to (10) or (11), wherein the polymer fine particles (A) are a rubber-containing graft copolymer having an elastomer and the graft portion graft-bonded to the elastomer.
[0301] (13) The resin composition according to (12), wherein the elastomer comprises at least one selected from the group consisting of diene-based rubbers, (meth)acrylate-based rubbers, and polysiloxane rubber-based elastomers.
[0302] (14) The resin composition according to any one of (10) to (13), wherein the resin (B) contains a thermosetting resin. EXAMPLES
[0303] Hereinafter, one embodiment of the present invention will be described in more detail with reference to examples and comparative examples, but the present invention is not limited thereto. One embodiment of the present invention can be practiced with appropriate modifications within the scope of the above or below-mentioned purpose, and all of these modifications are included in the technical scope of the present invention. In the following examples and comparative examples, "parts" and "%" mean parts by weight or % by weight.
[0304] [Evaluation method] First, the evaluation methods for the resin compositions produced in the examples and comparative examples will be described below.
[0305] <Measurement of volume average particle size> The volume average particle size (Mv) of the elastomer or polymer microparticles (A) dispersed in the aqueous latex was measured using Nanotrac WaveII-EX150 (manufactured by Microtrackbell Co., Ltd.). The aqueous latex was diluted with deionized water and used as the measurement sample. The measurement was performed by inputting the refractive index of water and the elastomer or polymer microparticles (A) obtained in each production example, and adjusting the sample concentration so that the measurement time was 120 seconds and the loading index was within the range of 1 to 20.
[0306] <Differential Scanning Calorimetry (DSC) of Resin (B)> The differential scanning calorimetry of the liquid epoxy resin (JER828, manufactured by Mitsubishi Chemical Corporation) used as resin (B) in the following examples and comparative examples was measured using a DSC7020 (manufactured by Hitachi High-Tech Science Corporation). The heating rate was 10°C / min. As a result, it was found that the liquid epoxy resin had an endothermic peak at -15°C.
[0307] <Viscosity measurement> The viscosity of the liquid epoxy resin (JER828, manufactured by Mitsubishi Chemical Corporation), which is the resin (B) used in the following Examples and Comparative Examples, or the obtained resin composition was measured. The device used was a Brookfield digital viscometer, model DV-II+Pro. The viscosity was measured using a spindle CPE-52 depending on the viscosity range, at a measurement temperature of 25°C, while changing the shear rate as necessary. As a result, the liquid epoxy resin had a viscosity of 12,000 mPa s.
[0308] <Evaluation of dispersibility> Resin (B) was further added to the obtained resin composition to obtain a composition in which the content of polymer fine particles (A) in resin (B) was 5% by weight. The dispersibility of polymer fine particles (A) in resin (B) in the obtained composition was evaluated according to JIS K5101 using a grind gauge. The specific method is as follows. The composition was placed on the grind gauge, the composition on the gauge was scraped off with a metal scraper, and the dispersion state was visually confirmed. The scale was read at the position where 5 to 10 dots of granular marks occurred in a 3 mm wide band due to the movement of the scraper. The smaller the obtained value, the better the dispersibility.
[0309] <Measurement of Solvent Amount in Resin Composition> The amount of solvent contained in the obtained resin composition was measured by gas chromatography (GC-2014, manufactured by Shimadzu Corporation).
[0310] <Measurement of elements S, P, Ca, Mg, Fe, Zn, Ba and Al in resin composition> The contents of the elements S, P, Ca, Mg, Fe, Zn, Ba and Al in the resin composition were measured using a fluorescent X-ray analyzer SPECTROXEPOS (manufactured by SPECTRO Corporation).
[0311] <Measurement of electrical conductivity> 100 g of the resin composition and 100 g of ion-exchanged water were stirred in a stirring tank at 90° C. and 900 rpm for 30 minutes. After that, the oil and water were separated, and the washing water was taken out and measured for electrical conductivity using a portable electrical conductivity meter (manufactured by HORIBA Corporation).
[0312] 1. Polymerization of elastic bodies Production Example 1-1: Preparation of polybutadiene rubber latex (R-1) Into the pressure-resistant polymerization vessel, 200 parts of deionized water, 0.03 parts of tripotassium phosphate, 0.002 parts of disodium ethylenediaminetetraacetate (EDTA), 0.001 parts of ferrous sulfate heptahydrate, and 1.55 parts of sodium dodecylbenzenesulfonate (SDBS) as an emulsifier were charged. Next, while stirring the charged raw materials, the gas inside the pressure-resistant polymerization vessel was replaced with nitrogen to thoroughly remove oxygen from inside the pressure-resistant polymerization vessel. Then, 100 parts of butadiene (Bd) were charged into the pressure-resistant polymerization vessel, and the temperature inside the pressure-resistant polymerization vessel was raised to 45°C. Then, 0.03 parts of paramenthane hydroperoxide (PHP) were charged into the pressure-resistant polymerization vessel, followed by 0.10 parts of sodium formaldehyde sulfoxylate (SFS) into the pressure-resistant polymerization vessel to start polymerization. 15 hours after the start of polymerization, the polymerization was terminated by removing the volatiles under reduced pressure to remove the monomers that were not used in the polymerization. During the polymerization, PHP, EDTA, and ferrous sulfate heptahydrate were added to the pressure polymerization vessel in arbitrary amounts and at arbitrary times. The polymerization yielded an aqueous latex (R-1) containing an elastomer whose main component was polybutadiene rubber. The volume average particle diameter of the elastomer contained in the obtained aqueous latex was was 90 nm.
[0313] Production Example 1-2: Preparation of polybutadiene rubber latex (R-2) Into a pressure-resistant polymerization vessel, 7 parts of the polybutadiene rubber latex (R-1) obtained above in terms of solid content, 200 parts of deionized water, 0.03 parts of tripotassium phosphate, 0.002 parts of EDTA, and 0.001 parts of ferrous sulfate heptahydrate were charged. Next, while stirring the charged raw materials, the gas inside the pressure-resistant polymerization vessel was replaced with nitrogen, thereby thoroughly removing oxygen from inside the pressure-resistant polymerization vessel. Then, 93 parts of Bd were charged into the pressure-resistant polymerization vessel, and the temperature inside the pressure-resistant polymerization vessel was raised to 45°C. Then, 0.02 parts of PHP were charged into the pressure-resistant polymerization vessel, followed by 0.10 parts of SFS, to start polymerization. 30 hours after the start of polymerization, the polymerization was terminated by removing the volatile components under reduced pressure to remove the monomers remaining unused in the polymerization. During the polymerization, PHP, EDTA, ferrous sulfate heptahydrate, and SDBS were added to the pressure polymerization vessel in arbitrary amounts and at arbitrary times. The polymerization produced an aqueous latex (R-2) containing an elastomer whose main component was polybutadiene rubber. The volume average particle size of the elastomer contained in the obtained aqueous latex was 195 nm.
[0314] Production Example 1-3: Preparation of polystyrene-butadiene rubber latex (R-3) Into the pressure-resistant polymerization vessel, 160 parts of deionized water, 0.002 parts of EDTA, 0.001 parts of ferrous sulfate heptahydrate, 0.029 parts of polyoxyethylene lauryl ether phosphate, and 0.003 parts of sodium hydroxide were charged. Here, in the presence of sodium hydroxide, polyoxyethylene lauryl ether phosphate became sodium polyoxyethylene lauryl ether phosphate, which functioned as an emulsifier. Next, while stirring the charged raw materials, the gas inside the pressure-resistant polymerization vessel was replaced with nitrogen, thereby sufficiently removing oxygen from inside the pressure-resistant polymerization vessel. Then, 76.5 parts of Bd and 23.5 parts of styrene (St) were charged into the pressure-resistant polymerization vessel, and the temperature inside the pressure-resistant polymerization vessel was raised to 45°C. Then, 0.03 parts of PHP were charged into the pressure-resistant polymerization vessel, followed by 0.05 parts of SFS, to start polymerization. Twenty hours after the start of polymerization, the polymerization was terminated by removing the remaining monomers that were not used in the polymerization by volatilization under reduced pressure. During the polymerization, PHP, polyoxyethylene lauryl ether phosphate, and sodium hydroxide were each added to the pressure-resistant polymerization vessel in an arbitrary amount and at an arbitrary time. By this polymerization, an aqueous latex (R-3) containing an elastomer mainly composed of polystyrene-butadiene rubber was obtained. The volume average particle diameter of the elastomer contained in the obtained aqueous latex was 192 nm.
[0315] Production Example 1-4: Preparation of polybutadiene rubber latex (R-4) Into the pressure-resistant polymerization vessel, 200 parts by weight of deionized water, 0.03 parts by weight of tripotassium phosphate, 0.002 parts by weight of disodium ethylenediaminetetraacetate (EDTA), 0.001 parts by weight of ferrous sulfate heptahydrate, and 1.55 parts by weight of sodium dodecylbenzenesulfonate (SDBS) as an emulsifier were charged. Next, while stirring the charged raw materials, the gas inside the pressure-resistant polymerization vessel was replaced with nitrogen to sufficiently remove oxygen from inside the pressure-resistant polymerization vessel. Then, 100 parts by weight of butadiene (Bd) was charged into the pressure-resistant polymerization vessel, and the temperature inside the pressure-resistant polymerization vessel was raised to 45°C. Then, 0.03 parts by weight of paramenthane hydroperoxide (PHP) was charged into the pressure-resistant polymerization vessel, followed by 0.10 parts by weight of sodium formaldehyde sulfoxylate (SFS) into the pressure-resistant polymerization vessel to start polymerization. Fifteen hours after the start of polymerization, the polymerization was terminated by removing the remaining monomers that were not used in the polymerization by volatilization under reduced pressure. During the polymerization, PHP, EDTA, and ferrous sulfate heptahydrate were each added to the pressure polymerization vessel in arbitrary amounts and at arbitrary times. This polymerization produced an aqueous latex (R-4) containing an elastomer whose main component was polybutadiene rubber. The volume average particle size of the elastomer contained in the obtained aqueous latex was 70 nm.
[0316] 2. Preparation of polymer microparticles (A) (polymerization of grafted portion) Production Example 2-1: Preparation of polymer particle latex (L-1) Into a glass reactor, 250 parts of the polybutadiene rubber latex (R-2) (including 87 parts of elastomer mainly composed of polybutadiene rubber) and 50 parts of deionized water were charged. Here, the glass reactor had a thermometer, a stirrer, a reflux condenser, a nitrogen inlet, and a monomer addition device. The gas in the glass reactor was replaced with nitrogen, and the raw materials charged at 60°C were stirred. Next, 0.004 parts of EDTA, 0.001 parts of ferrous sulfate heptahydrate, and 0.2 parts of SFS were added to the glass reactor and stirred for 10 minutes. After that, a mixture of 12.5 parts of methyl methacrylate (MMA), 0.5 parts of St, and 0.035 parts of t-butyl hydroperoxide (BHP) was continuously added to the glass reactor over 80 minutes. Then, 0.013 parts of BHP was added to the glass reactor, and the mixture in the glass reactor was stirred for another hour to complete the polymerization. By the above operations, an aqueous latex (L-1) containing polymer fine particles (A) and an emulsifier was obtained. The polymerization conversion rate of the monomer components was 99% or more. The volume average particle diameter of the polymer fine particles (A) contained in the obtained aqueous latex was 200 nm. The solid content concentration (concentration of polymer fine particles (A)) in the obtained aqueous latex (L-1) was 30%.
[0317] Production Example 2-2: Preparation of polymer particle latex (L-2) Into a glass reactor, 250 parts of the polystyrene-butadiene rubber latex (R-3) (including 87 parts of elastomer mainly composed of polystyrene-butadiene rubber) and 50 parts of deionized water were charged. Here, the glass reactor had a thermometer, a stirrer, a reflux condenser, a nitrogen inlet, and a monomer addition device. The gas in the glass reactor was replaced with nitrogen, and the raw materials charged at 60°C were stirred. Next, 0.004 parts of EDTA, 0.001 parts of ferrous sulfate heptahydrate, and 0.2 parts of SFS were added to the glass reactor and stirred for 10 minutes. Then, a mixture of 12.5 parts of MMA, 0.5 parts of St, and 0.035 parts of BHP was continuously added to the glass reactor over 80 minutes. Then, 0.013 parts of BHP was added to the glass reactor, and the mixture in the glass reactor was further stirred for 1 hour to complete the polymerization. By the above operations, an aqueous latex (L-2) containing polymer fine particles (A) and an emulsifier was obtained. The polymerization conversion rate of the monomer components was 99% or more. The volume average particle diameter of the polymer fine particles (A) contained in the obtained aqueous latex was 200 nm. The solid content concentration (concentration of polymer fine particles (A)) in the obtained aqueous latex (L-2) was 30%.
[0318] Production Example 2-3: Preparation of polymer particle latex (L-3) 250 parts by weight of the polybutadiene rubber latex (R-4) (containing 83 parts by weight of an elastomer mainly composed of polybutadiene rubber) was charged into a glass reactor. The glass reactor had a thermometer, a stirrer, a reflux condenser, a nitrogen inlet, and a monomer addition device. The gas in the glass reactor was replaced with nitrogen, and the raw materials charged at 60°C were stirred. Next, 0.004 parts by weight of EDTA, 0.001 parts by weight of ferrous sulfate heptahydrate, and 0.20 parts by weight of SFS were added to the glass reactor and stirred for 10 minutes. Then, a mixture of 0.8 parts by weight of methyl methacrylate (MMA), 5.4 parts by weight of styrene (St), 3.9 parts by weight of acrylonitrile (AN), 6.9 parts by weight of glycidyl methacrylate (GMA) and 0.043 parts by weight of t-butyl hydroperoxide (BHP) was continuously added to the glass reactor over 120 minutes. Then, 0.013 parts by weight of BHP was added to the glass reactor, and the mixture in the glass reactor was stirred for another hour to complete the polymerization. By the above operations, an aqueous latex (L-3) containing polymer fine particles (A) was obtained. The polymerization conversion rate of the monomer components was 99% or more. The volume average particle diameter of the polymer fine particles (A) contained in the obtained aqueous latex was 80 nm. The solid content concentration (concentration of polymer fine particles (A)) in the obtained aqueous latex (L-3) was 30%.
[0319] Example 1 333 g of the aqueous latex (L-1) was fed to a metal surface at -30°C and scraped off after 1 minute to obtain a frozen latex (L-1). The frozen latex (L-1) was thawed at room temperature. The thawed latex (L-1) and 66.7 g of a liquid epoxy resin (JER828, manufactured by Mitsubishi Chemical Corporation; the same applies below) as resin (B) were kneaded using a continuous kneader. Next, a resin composition, which is an aggregate containing polymer fine particles (A) and resin (B), and a water component were separated from the latex. The operation of feeding the obtained aggregate (resin composition) and 100 g of ion-exchanged water to a continuous kneader and the operation of subjecting the obtained mixture to centrifugal dehydration were repeated three times in total to obtain a washed aggregate. The obtained aggregate was subjected to vacuum devolatilization at 115°C to remove water, and then each analysis was performed.
[0320] Comparative Example 1 Instead of supplying 333 g of the water-based latex (L-1) to a metal surface at -30°C and scraping it off after 1 minute, 333 g of the water-based latex (L-1) was left in a freezer at -20°C for 12 hours to obtain frozen latex (L-1). The rest of the procedure was the same as in Example 1.
[0321] Example 2 333 g of the aqueous latex (L-1) was stirred at 12000 rpm using a homomixer, and 150 g of liquid epoxy resin (resin (B)) was added to the homomixer and stirred for another 30 minutes. The resulting mixture was left in a freezer at -20°C for 12 hours to obtain frozen latex (L-1). The frozen latex (L-1) was thawed in hot water at 50°C. From the thawed latex (L-1), a resin composition, which is an aggregate containing polymer fine particles (A) and resin (B), and a water component were separated. 200 g of the resulting aggregate and 300 g of ion-exchanged water were mixed, and the mixture was stirred at 90°C for 30 minutes. The resulting mixture was subjected to oil-water separation to extract the aggregate. The resulting aggregate was subjected to vacuum devolatilization at 115°C to remove water, and then each analysis was performed.
[0322] Example 3 The same procedure as in Example 2 was carried out, except that 333 g of the aqueous latex (L-2) was used instead of the aqueous latex (L-1).
[0323] Example 4 333 g of the aqueous latex (L-1) was stirred at 12000 rpm using a homomixer, and 150 g of liquid epoxy resin, which is resin (B), was added to the homomixer and stirred for another 30 minutes. The resultant stirred material was filtered through a 16-mesh wire net, and the aggregates remaining on the wire net and the liquid (filtrate) that passed through the wire net were collected. The obtained filtrate was left in a freezer at -20°C for 12 hours to obtain frozen latex (L-1). The frozen latex (L-1) was thawed in a hot water bath at 50°C. Next, the aggregates remaining on the wire net and the thawed latex (L-1) were kneaded using a continuous kneader. From the mixture (latex) after kneading, the resin composition, which is an aggregate containing polymer fine particles (A) and resin (B), and the water component were separated. 200 g of the obtained aggregate and 300 g of ion-exchanged water were mixed, and the mixture was stirred at 90° C. for 30 minutes. The aggregate was taken out from the obtained mixture by oil-water separation. The obtained aggregate was subjected to vacuum devolatilization at 115° C. to remove water, and then each analysis was performed.
[0324] Example 5 333 g of the aqueous latex (L-1) was stirred at 6000 rpm using a high shear emulsifier, and 66.7 g of liquid epoxy resin (resin (B)) was added to the high shear emulsifier and stirred for another 90 minutes. From the resulting stirred product (latex), a resin composition, which is an aggregate containing polymer fine particles (A) and resin (B), and a water component were separated. The operation of feeding the resulting aggregate and 100 g of ion-exchanged water to a continuous kneader and the operation of centrifugal dehydration of the resulting mixture were repeated three times in total to obtain a washed aggregate. The resulting aggregate was subjected to vacuum devolatilization at 115°C to remove water, and then each analysis was performed.
[0325] Example 6 333 g of the aqueous latex (L-1) was stirred at 6000 rpm using a high shear emulsifier, and 66.7 g of liquid epoxy resin (resin (B)) was added to the high shear emulsifier and stirred for another 90 minutes. From the resulting stirred product (latex), a resin composition containing polymer fine particles (A) and resin (B) as an aggregate and a water component were separated. Next, the resulting water component was left in a freezer at -20°C for 12 hours to obtain a frozen water component. The frozen water component was thawed. Next, the thawed water component was mixed with the above aggregate. From the resulting mixture (latex), a resin composition containing polymer fine particles (A) and resin (B) as an aggregate and a water component were separated. Thereafter, the same operation as in Example 4 was performed.
[0326] Example 7 The same procedure as in Example 2 was carried out, except that 333 g of the aqueous latex (L-3) was used instead of the aqueous latex (L-1).
[0327] Comparative Example 2 20 g of 24% sodium sulfate was added to 333 g of the aqueous latex (L-1) and mixed with a spatula to obtain an aggregate containing polymer fine particles (A). The aggregate and water were then separated from the latex. The aggregate obtained and 500 g of ion-exchanged water were mixed, and the mixture was stirred at 50°C for 30 minutes. The stirred product was subjected to vacuum filtration to remove the washing water from the stirred product. This operation was repeated two more times (three times in total) to obtain an aggregate. The aggregate obtained and 150 g of liquid epoxy resin were kneaded using a continuous kneader to obtain an aggregate. The aggregate obtained was subjected to vacuum devolatilization at 115°C to remove water, and then each analysis was performed.
[0328] Comparative Example 3 After the temperature in the 1L mixing tank was adjusted to 30°C, 126 parts of methyl ethyl ketone (MEK) was added to the mixing tank. Then, while stirring the MEK in the mixing tank, 126 parts of the aqueous latex (L-1) of the polymer microparticles (A) was added to the mixing tank. Next, the added raw materials were mixed uniformly, and then, while stirring, 200 parts of water (452 parts in total) was added to the mixing tank at a feed rate of 80 parts / min. After the water supply was completed, the stirring was stopped immediately, and a slurry liquid containing floating aggregates was obtained.
[0329] Next, the aggregates were left in the mixing tank, and 350 parts by mass of the liquid phase was discharged from the outlet at the bottom of the mixing tank. 150 parts of MEK was added to the obtained aggregates (polymer fine particle (A) dope) and mixed to obtain an organic solvent solution in which the polymer fine particles (A) were dispersed. 100 parts of liquid epoxy resin was added to 277 parts of this organic solvent solution (containing 42.9 parts of polymer fine particles (A)), and the obtained blend was mixed, and then MEK was distilled off from the mixture under reduced pressure to obtain a resin composition. The obtained resin composition was subjected to various analyses.
[0330] Comparative Example 4 150 g of liquid epoxy resin was added to 333 g of the water-based latex (L-1). The mixture was subjected to vacuum devolatilization at 115° C. to remove water. The composition was subjected to various analyses.
[0331] Comparative Example 5 20 g of 24% sodium sulfate was added to 150 g of liquid epoxy resin and mixed with a spatula. 333 g of water-based latex (L-1) was added to the resulting mixture and mixed with a spatula to obtain an aggregate containing polymer fine particles (A) and resin (B). Then, the aggregate and water component were separated from the latex. 200 g of the resulting aggregate and 300 g of ion-exchanged water were mixed, and the mixture was stirred at 90°C for 30 minutes. Next, oil-water separation was performed to remove the aggregate from the resulting mixture. The resulting aggregate was subjected to vacuum devolatilization at 115°C to remove water, and then each analysis was performed.
[0332] Comparative Example 6 The same procedure as in Comparative Example 5 was carried out except that 20 g of 24% sodium chloride was used instead of 24% sodium sulfate.
[0333] Comparative Example 7 The same procedure as in Comparative Example 5 was carried out, except that 333 g of the aqueous latex (L-2) was used instead of the aqueous latex (L-1).
[0334] Comparative Example 8 The same procedure as in Comparative Example 5 was carried out, except that 333 g of the aqueous latex (L-3) was used instead of the aqueous latex (L-1).
[0335] The analytical results are shown in Table 1. [Table 1] [Industrial Applicability]
[0336] According to one embodiment of the present invention, the composition can be blended with a thermosetting resin and used suitably for various applications such as adhesives and coating materials.
Claims
1. a resin mixing step of mixing a latex containing polymer fine particles (A) having a graft portion made of a polymer containing, as a structural unit, a structural unit derived from one or more monomers selected from the group consisting of an aromatic vinyl monomer, a vinyl cyan monomer, and a (meth)acrylate monomer with a liquid, semi-solid, or solid resin (B) having a viscosity of 100 mPa·s to 1,000,000 mPa·s at 25° C.; a shearing step of applying a shear stress to the latex obtained by the resin mixing step; a first separation step of separating, after the shearing step, a resin composition which is an aggregate containing the polymer fine particles (A) and the resin (B) from the latex and a water component, The method for producing a resin composition, wherein the polymer fine particles (A) are 1 to 70% by weight and the resin (B) is 30 to 99% by weight, when the total of the polymer fine particles (A) and the resin (B) is 100% by weight.
2. and an aggregation step of aggregating a resin composition, which is an aggregate containing polymer fine particles (A) and a resin (B), from the water component from which the aggregates have been separated in the first separation step.
2. The method for producing a resin composition according to claim 1, further comprising: a second separation step of separating, after the aggregation step, the resin composition which is an aggregate containing the polymer fine particles (A) and the resin (B) from a water component.
3. The method for producing a resin composition according to claim 2 , wherein the aggregating step includes a step of freezing the water component separated from the aggregates in the first separation step.
4. a rapid freezing step of freezing a latex containing polymer fine particles (A) having a graft portion made of a polymer containing, as a structural unit, a structural unit derived from one or more monomers selected from the group consisting of an aromatic vinyl monomer, a vinyl cyan monomer, and a (meth)acrylate monomer, for a time period of 1 second to less than 20 minutes; a thawing step of thawing the latex frozen in the quick freezing step; a resin mixing step of mixing a liquid, semi-solid, or solid resin (B) having a viscosity of 100 mPa·s to 1,000,000 mPa·s at 25°C with the latex after the quick freezing step; a separation step of separating a resin composition, which is an aggregate containing the polymer fine particles (A) and the resin (B), from the latex after the thawing step and the resin mixing step, and a water component; Including, The method for producing a resin composition, wherein the polymer fine particles (A) are 1 to 70% by weight and the resin (B) is 30 to 99% by weight, when the total of the polymer fine particles (A) and the resin (B) is 100% by weight.
5. a resin mixing step of mixing a latex containing polymer fine particles (A) having a graft portion made of a polymer containing, as a structural unit, a structural unit derived from one or more monomers selected from the group consisting of an aromatic vinyl monomer, a vinyl cyan monomer, and a (meth)acrylate monomer with a liquid, semi-solid, or solid resin (B) having a viscosity of 100 mPa·s to 1,000,000 mPa·s at 25° C.; a freezing step of freezing the latex having the resin (B) dispersed therein obtained by the resin mixing step; a thawing step of thawing the latex frozen in the freezing step; a separation step of separating a resin composition, which is an aggregate containing the polymer fine particles (A) and the resin (B), from the latex after the thawing step, and a water component; Including, The method for producing a resin composition, wherein the polymer fine particles (A) are 1 to 70% by weight and the resin (B) is 30 to 99% by weight, when the total of the polymer fine particles (A) and the resin (B) is 100% by weight.
6. The method for producing a resin composition according to claim 5 , further comprising a removing step of removing aggregates generated in the resin mixing step before the freezing step.
7. The method for producing a resin composition according to any one of claims 1 to 5, further comprising a step of adjusting the water content of the aggregates to 5% by weight to 60% by weight in 100% by weight of the aggregates in the separation step, the first separation step or the second separation step.
8. The method for producing a resin composition according to any one of claims 1 to 7, further comprising a washing step of washing the resin composition.
9. Polymer fine particles (A) having a graft portion made of a polymer containing, as a structural unit, a structural unit derived from one or more monomers selected from the group consisting of an aromatic vinyl monomer, a vinyl cyan monomer, and a (meth)acrylate monomer; A resin (B) which is a liquid, semi-solid, or solid having a viscosity of 100 mPa·s to 1,000,000 mPa·s at 25°C; When the total amount of the polymer fine particles (A) and the resin (B) is taken as 100% by weight, the polymer fine particles (A) account for 1 to 70% by weight and the resin (B) accounts for 30 to 99% by weight, When the content of the polymer fine particles (A) in the resin (B) is 5% by weight, the dispersibility of the polymer fine particles (A) in the resin (B) is 0 μm or less when evaluated in accordance with JIS K5101 using a grind gauge; It does not substantially contain organic solvents. The contents of the elements S and P are each 150 ppm or less, The electrical conductivity is 0.6 mS / cm or less, The resin (B) is at least one selected from the group consisting of epoxy resins, phenolic resins, polyol resins, and amino-formaldehyde resins (melamine resins).
10. The resin composition according to claim 9, further comprising elements Ca, Mg, Fe, Zn, Ba and Al each having a content of 100 ppm or less.
11. 11. The resin composition according to claim 9, wherein the polymer fine particles (A) are a rubber-containing graft copolymer having an elastomer and the graft portion graft-bonded to the elastomer.
12. The resin composition according to claim 11, wherein the elastomer comprises at least one selected from the group consisting of diene-based rubbers, (meth)acrylate-based rubbers, and polysiloxane rubber-based elastomers.
13. The resin composition according to any one of claims 9 to 12, wherein the resin (B) comprises a thermosetting resin.
Citation Information
Patent Citations
Composition for casting material
JP1993339471A
Method for producing fluorine-containing polymer latex
JP2002308914A
Ultra-clean fluoropolymer
JP2003522232A
Process for producing rubbery polymer particle and process for producing resin composition containing the same
WO2005028546A1
Curable composition, cured object obtained therefrom, and process for producing same
WO2010082482A1