Block copolymer with excellent vibration damping and heat resistance and method for producing same

A block copolymer with controlled random bonding and vinyl content addresses heat resistance and damping property issues, providing effective vibration damping across a wide temperature range.

JP7559102B2Active Publication Date: 2024-10-01ENEOS KRATON ELASTOMER CO LTD

Patent Information

Application Number
JP2023015873
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2023-02-06
Publication Date
2024-10-01
Estimated Expiration
2043-02-06

AI Technical Summary

Technical Problem

Existing block copolymers with high vinyl bond content face issues with heat resistance and lack of control over tan δ absorption intensity and temperature range, particularly in maintaining vibration damping properties near room temperature and in high-temperature environments.

Method used

A block copolymer composed of aromatic vinyl and conjugated diene monomers with random bonding, controlled vinyl content, and specific molecular weight, ensuring a tan δ peak near room temperature and wide temperature range damping properties, along with improved heat resistance.

Benefits of technology

The copolymer achieves high vibration damping across a wide temperature range with excellent heat resistance, maintaining properties even at elevated temperatures and reducing crosslinking reactions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007559102000001
    Figure 0007559102000001
  • Figure 0007559102000002
    Figure 0007559102000002
Patent Text Reader

Abstract

To provide a block copolymer having excellent vibration-damping properties and heat resistance, and a method for producing the same.SOLUTION: A block copolymer comprises a polymer block composed mainly of at least two aromatic vinyl monomers, and a polymer block in which at least one conjugated diene monomer and an aromatic vinyl monomer are bonded randomly. The block copolymer includes a vinyl group, the content of aromatic vinyl monomers in the block copolymer is 45%-60%, the random bonding rate of the aromatic vinyl monomer in the polymer block in which the conjugated diene monomer and the aromatic vinyl monomer are bonded randomly is 70%-90%, and the vinyl group is non-hydrogenated.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a block copolymer having excellent vibration damping properties and heat resistance. [Background technology]

[0002] Damping is a phenomenon in which vibrations are suppressed by converting the vibration energy of a solid surface into heat and attenuating it. Materials used for the purpose of damping are called damping materials, and are used in automobiles, trains, home appliances, precision instruments, housing, etc. to improve comfort. Typical damping materials include metals, elastomers, plastics, and asphalt, among which elastomers are particularly widely used due to their viscoelasticity and high vibration damping effect.

[0003] The value of tan δ obtained by dynamic viscoelasticity measurement is generally used as an index for judging vibration-damping properties, and the higher the value of tan δ, the greater the vibration-damping effect. As mentioned above, elastomers are often used as vibration-damping materials due to their viscoelastic properties, and among them, styrene-based block copolymers have a high peak value of tan δ and are suitable as vibration-damping materials. In particular, styrene-based block copolymers produced by living anionic polymerization have a high degree of freedom in their molecular design, and it is easy to adjust the tan δ peak value and peak temperature, so various types have been developed to suit the object to which vibration-damping properties are to be imparted. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Japanese Patent Application Publication No. 2-102212 [Patent Document 2] JP 2002-284830 A Summary of the Invention [Problem to be solved by the invention]

[0005] Incidentally, Patent Document 1 discloses a method for producing a block copolymer composed of two or more blocks of aromatic vinyl compounds and one or more blocks of isoprene or isoprene-butadiene. It is shown that by making the vinyl bond content of the block composed of isoprene or isoprene-butadiene 40% or more, the main dispersion peak temperature of tan δ becomes 0°C or higher, and high vibration damping performance can be obtained in a practical temperature range.

[0006] Also, in Patent Document 2, a block copolymer having a block made of an aromatic vinyl compound and a block made of a mixture of isoprene and styrene is studied. It has been found that by adjusting the vinyl bond content of isoprene in this block copolymer to 30-60%, the main dispersion peak temperature of tan δ can be made 30°C or higher, and excellent vibration damping properties are achieved in high-temperature environments.

[0007] However, in Patent Document 1, only the main dispersion peak temperature of tan δ of the block copolymer is described, and there is no description of its absorption intensity or temperature range of absorption intensity. In addition, it is generally known that the heat resistance decreases as the vinyl bond content in a copolymer increases, and since all of the copolymers disclosed in Patent Document 1 have a high vinyl bond content, it is considered that there is a problem with heat resistance.

[0008] Patent Document 2 shows that by adjusting the structure of a block composed of a mixture of isoprene and styrene, tan δ is 0.2 or more in the range of 30 to 70 ° C. and the tan δ main dispersion peak temperature is 30 ° C. or more, but there is no mention of a method for making the tan δ main dispersion peak temperature near room temperature and reducing the vinyl content. In addition, there is no particular limitation on the form of chain distribution of isoprene units and styrene units in the block, and there is no mention of the random bond rate. Furthermore, Patent Document 2 shows that the double bonds of the block copolymer are hydrogenated for the purpose of improving heat resistance, but considering industrial production, the additional hydrogenation process will certainly result in a decrease in productivity and an increase in energy costs, which is undesirable from the standpoint of cost and environmental impact. [Means for solving the problem]

[0009] As a result of intensive research into the above problems, the present inventors have found that in a polymer composed of a polymer block made of an aromatic vinyl monomer such as styrene, and a polymer block made of at least one conjugated diene monomer and an aromatic vinyl monomer, when the chain distribution form of the conjugated diene monomer and the aromatic vinyl monomer is random and the random bond rate is within a specific range, even with a low vinyl content, the main dispersion peak of tan δ is near room temperature, and a block polymer which is suitable for a wide range of applications in a working environment at room temperature and has a high vibration damping effect over a wide temperature range can be obtained, thereby completing the present invention.

[0010] That is, in order to solve the above-mentioned problems, the present invention includes the following aspects. (1) A block copolymer comprising at least two polymer blocks mainly composed of aromatic vinyl monomers and at least one polymer block in which a conjugated diene monomer and an aromatic vinyl monomer are randomly bonded, containing a vinyl group, and satisfying the following a) to d), the vinyl group being non-hydrogenated. a) The aromatic vinyl monomer content in the block copolymer is 45 to 60 weight%, and the random bonding rate of the aromatic vinyl monomer in the polymer block in which the conjugated diene monomer and the aromatic vinyl monomer are randomly bonded is 70 to 90%. Mole %. b) The tan δ peak temperature at a measurement frequency of 10 Hz is 0 to 30°C and the peak value is 0.7 or more. c) At a measurement frequency of 10 Hz, the temperature range in which tan δ is 0.3 or more is 45°C or more. (2) A conjugated diene polymer having a vinyl bond content of 40 Mole % or less. (3) The block copolymer according to any one of (1) to (2), wherein the block copolymer has a weight average molecular weight of 100,000 to 300,000. (4) A method for producing a block copolymer, comprising: a first step of producing a polymer block mainly composed of at least two aromatic vinyl monomers; a second step of producing a polymer block obtained by randomly bonding at least one conjugated diene monomer and an aromatic vinyl monomer to the polymer block obtained in the first step; and a third step of producing a polymer block mainly composed of at least two aromatic vinyl monomers from the polymer block obtained in the second step. (5) The method according to (4), wherein in the second step, the aromatic vinyl monomer and the conjugated diene monomer are added simultaneously, or one of them is added immediately followed by the other. (6) The method according to (4), wherein the randomizer is an ether or an amine. (7) The method according to (6), wherein the randomizing agent is at least one selected from the group consisting of tetrahydrofuran, tetrahydropyran, 1,2-dimethoxyethane, 1,2-diethoxyethane, 2,2-di(tetrahydrofuryl)propane, crown ether, triethylamine, N,N-dimethylaniline and N,N,N',N'-tetramethylethylenediamine. (8) The method according to (4), wherein in the first step, the molecular weight of the polymer block obtained is in the range of 7,000 to 25,000. Effect of the Invention

[0011] According to the present invention, it is possible to provide a block copolymer having excellent vibration damping properties and heat resistance. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] The present invention will be described in detail below. The block copolymer of the present invention comprises at least two polymer blocks mainly composed of aromatic vinyl monomers and at least one polymer block mainly composed of a conjugated diene monomer, and the aromatic vinyl monomer content in the block copolymer is 45 to 60%. weight %, and the random bonding rate of the aromatic vinyl monomer in the polymer block in which the conjugated diene monomer and the aromatic vinyl monomer are randomly bonded is 70 to 90%. Mole %, and a representative example is represented by the following general formula: Ar1-D-Ar2 (A)

[0013] In the above general formula (A), Ar1 and Ar2 are polymer blocks mainly composed of aromatic vinyl compounds. The polymer blocks Ar1 and Ar2 may be the same or different from each other. Examples of aromatic vinyl monomers include styrene, t-butylstyrene, α-methylstyrene, p-methylstyrene, o-methoxystyrene, and p-methoxystyrene, among which styrene is particularly preferred.

[0014] In the above general formula (A), D is a polymer block mainly composed of a conjugated diene monomer. Examples of the conjugated diene monomer in the polymer block D include 1,3-butadiene, isoprene, 2,3-dimethyl-1,3-butadiene, 1,3-pentadiene, 2-methyl-1,3-pentadiene, 1,3-hexadiene, 4,5-diethyl-1,3-octadiene, 3-butyl-1,3-octadiene, 7-methyl-3-methylene-1,6-octadiene, and chloroprene. Among these, 1,3-butadiene and isoprene are preferred, and isoprene is more preferred.

[0015] The most important point in the block polymer of the present invention is that the random bonding rate of the aromatic vinyl monomer in the polymer block D in the above general formula (A) is 70 to 90. Mole %. If the random bond ratio is not within this range, the temperature dependency of tan δ becomes high, and tan δ at points outside the absorption peak temperature drops significantly. The random bond ratio is determined by using styrene as a representative example in the following examples, as follows: 1 This value can be estimated by measuring H-NMR and using the intensity (integral value) of the peak due to hydrogen around the aromatic ring in the unit derived from the aromatic vinyl monomer.

[0016] In the block copolymer according to the present embodiment, the aromatic vinyl monomer content in the block copolymer is 45 to 60 weight %, preferably 50-60 weight %. By adjusting the random bonding rate of the aromatic vinyl monomer in the polymer block D and the aromatic vinyl monomer content in the block copolymer, the tan δ peak temperature of the block copolymer can be set to 0 to 30°C, and the tan δ peak value of the block copolymer can be set to 0.7 or more, thereby imparting vibration damping properties over a wide temperature range. The random bonding rate of the aromatic vinyl monomer and the aromatic vinyl monomer content in the block copolymer are values ​​measured by the method described below. In addition, the block copolymer has a temperature range in which tan δ is 0.3 or more of 45°C or more, and can maintain vibration damping properties over a wide temperature range.

[0017] Furthermore, the block copolymer according to this embodiment has excellent heat resistance, and its fluidity is hardly affected even when exposed for 30 minutes at 230° C. This heat resistance can be evaluated by the rate of change in melt flow rate when heated for 30 minutes at 230° C., as measured by the method described below, and is preferably 5% or less, more preferably 3% or less.

[0018] The vinyl bond content (total of 1,2- and 3,4-bonds) of the conjugated diene monomer is 40 Mole % or less, preferably 15% to 40% Mole The vinyl bond content is too high, e.g. 40%. Mole %, crosslinking reaction of vinyl groups is likely to occur during heating, and heat resistance is reduced. The vinyl bond content is calculated by the following formula, as determined by using isoprene as a representative example in the following examples: 1 It is a value that can be estimated by measuring H-NMR and using the intensity (integral value) of the peak due to hydrogen in the unit derived from the carbon chain of isoprene. This vinyl bond content can be adjusted by the type and amount of polymerization initiator used, and, if a randomizer is used, the type and amount of the randomizer used.

[0019] The weight average molecular weight of the block copolymer is 100,000 to 300,000, preferably 120,000 to 300,000, and more preferably 150,000 to 250,000. If this value is too small, for example below 100,000, the block copolymer becomes extremely sticky, and adhesion during the drying process makes industrial production difficult to achieve. On the other hand, if this value is too large, for example above 300,000, the polymer hardness becomes too high, impairing processability and making it difficult to use as a material. The weight average molecular weight is a value measured by the method described below.

[0020] The melt flow rate (190°C, 2.16 kg load) of the block copolymer is preferably 0.1 to 20, more preferably 1 to 16. The melt flow rate (190°C, 2.16 kg load) is a value measured by the method described below. The molecular weight and melt flow rate of the block copolymer are adjusted by the amount of a polymerization initiator, for example, sec-butyl lithium, added.

[0021] The method for polymerizing a block copolymer according to this embodiment includes a first step of producing a polymer block (Ar1) mainly composed of at least two aromatic vinyl monomers, a second step of producing a polymer block (D) obtained by randomly bonding at least one conjugated diene monomer and an aromatic vinyl monomer to the polymer block obtained in the first step, and a third step of producing a polymer block (Ar2) mainly composed of at least two aromatic vinyl monomers from the polymer block obtained in the second step.

[0022] The polymerization method is not particularly limited, and may be a continuous method, a coupling method, or the like. However, the polymerization by the coupling method may contain a certain amount of diblock copolymer, unreacted coupling agent, and impurities associated with the coupling reaction. These components cause a decrease in strength and deterioration of the block copolymer, so the polymerization method is preferably a continuous method. In addition, the random bonding property of the conjugated diene monomer and the aromatic vinyl monomer in the polymer block D can be adjusted by the timing of the addition of each monomer, but from the viewpoint of improving the efficiency of the reaction and shortening the reaction time, it is preferable to add a randomizer to the polymerization system. Generally, the reaction rate of the conjugated diene monomer is higher than that of the aromatic vinyl monomer, so that the randomizer can be one that acts to increase the reaction rate of the aromatic vinyl monomer, such as ethers such as tetrahydrofuran, tetrahydropyran, 1,2-dimethoxyethane, 1,2-diethoxyethane, 2,2-di(tetrahydrofuryl)propane, crown ether, and amines such as triethylamine, N,N-dimethylaniline, and N,N,N',N'-tetramethylethylenediamine. These may be used alone or in combination of two or more. By using a randomizer, it is possible to suppress the preferential reaction between the conjugated diene monomers, and as a result, the random reaction between the conjugated diene monomers and the aromatic vinyl monomers is promoted.

[0023] The first step may be completed so that the weight average molecular weight of the resulting polymer block (Ar1) is preferably 7000 to 25000, more preferably 9000 to 21000. By making the polymer block (Ar1) obtained in the first step have such a molecular weight, the molecular weight and melt flow rate of the block copolymer can be adjusted to be within preferred ranges.

[0024] In the second step, it is preferable to add the aromatic vinyl monomer and the conjugated diene monomer simultaneously, or to add one of them and then the other immediately, which makes it possible to increase the randomness of the polymer block (D).

[0025] Examples of the polymerization solvent include aliphatic hydrocarbons such as n-pentane, isopentane, n-hexane, isohexane, heptane, octane, methylcyclopentane, cyclohexane, and methylcyclohexane, aromatic hydrocarbons such as benzene, toluene, and xylene, ethers such as diethyl ether, 1,4-dioxane, tetrahydrofuran, tetrahydropyran, and 2-methyltetrahydrofuran, and tertiary amines such as triethylamine and tri(n-propyl)amine, but from the viewpoint of suppressing and adjusting the vinyl content of the conjugated diene monomer, it is preferable to select aliphatic and aromatic hydrocarbons as the polymerization solvent. These solvents may be used alone or in combination of two or more.

[0026] The organic alkali metal compound as the polymerization initiator includes an organic lithium compound, an organic sodium compound, etc., and is particularly preferably an organic lithium compound. Specific examples of the organic lithium compound include methyl lithium, ethyl lithium, n-propyl lithium, isopropyl lithium, n-butyl lithium, sec-butyl lithium, and tert-butyl lithium.

[0027] The polymerization reaction is usually carried out at 30 to 100° C., preferably 40 to 90° C. The polymerization may be carried out at a controlled constant temperature, or at an elevated temperature without heat removal.

[0028] A polymerization terminator may be used to complete the polymerization reaction. Examples of such a polymerization terminator include alcohols and water, such as methanol, ethanol, 1-propanol, 2-propanol, 1-butanol, and 2-butanol.

[0029] The resulting polymerization solution can be subjected to removal of the solvent by a known method such as steam stripping to obtain a block copolymer. If necessary, additives such as an antioxidant may be added to the block copolymer. EXAMPLES

[0030] The present embodiment will be described in more detail with reference to the following examples and comparative examples.

[0031] The block copolymers obtained in the following Examples and Comparative Examples were analyzed by the following methods. Various physical properties of the resulting block copolymer were measured as follows. (1) Weight average molecular weight (Mw) The weight average molecular weight was measured using a gel permeation chromatography (HLC-8320) manufactured by Tosoh Corporation, and an Ultrabondagel E750A column manufactured by Waters Corporation. Tetrahydrofuran was used as the solvent, and the measurement conditions were a temperature of 45°C, a flow rate of 1.0 mL / min, a sample concentration of 0.1%, and an injection volume of 20 μL. The values ​​were converted into standard polystyrene. (2) Block copolymer microstructure (wt% or mol%) 1,1,2,2-Tetrachloroethane-d2 as a solvent 1 H-NMR (Bruker, AVANCE III HD500) was measured, and the integral value obtained was converted to the value per hydrogen atom of each structure, and then the styrene content ( weight %), vinyl bond content (vinyl content ( Mole %)) and the random bonding rate of bound styrene ( Mole %) was calculated. The chemical shift of interest (TMS standard: δ=0), the hydrogen assignment corresponding to each chemical shift, and the relationship with the structure related to the hydrogen are shown below. In addition, in the calculation formula for each value, all hydrogens are treated as having the same intensity (integral value), and A to E respectively indicate the intensity (integral value) at each chemical shift. In addition, the molecular weight of styrene is 104, and the molecular weight of isoprene is 68.

[0032] [Table 1]

[0033] Value per hydrogen atom in each structure 1,4-Polyisoprene: B-2C 3,4-Isoprene: A / 2 1,2-Isoprene: C Block styrene (BS): D / 2 Random styrene (RS): The strength of all hydrogen atoms around the aromatic ring of random styrene divided by 5 = [(Intensity of all hydrogens around the aromatic ring of styrene other than the ortho position of block styrene) - (Intensity of hydrogens around the aromatic ring of block styrene other than the ortho position)] ÷ 5 =[E-3×BS]÷5 =[E-3×D / 2] / 5

[0034] 1,4-Polyisoprene content ( Mole %): [1,4-isoprene / total isoprene] x 100 =[(B-2C) / [(B-2C)+A / 2+C]]×100 Vinyl bond amount = vinyl isoprene content ( Mole %): [(1,2-isoprene and 3,4-isoprene combined) / total isoprene] x 100 =[(A / 2+C) / {(B-2C)+A / 2+C}]×100 Styrene content ( weight %): {(BS+RS)×104} / {(BS+RS)×104+total isoprene×68}]×100 Random binding rate ( Mole %):[RS / (BS+RS)]×100 (3) Dynamic viscoelasticity measurement of block copolymers The measurements were performed using a viscoelasticity measuring device (Rheogel E-4000) manufactured by UBM under conditions of a frequency of 10 Hz and a heating rate of 5° C. / min. (4) Melt flow rate [MFR] (g / 10 min) The measurement was performed using an automelt indexer (TP-404 type) manufactured by Tester Sangyo Co., Ltd., in accordance with JIS K7210 (190° C., 21.2 N). (5) Heat resistance measurement of block copolymer The MFR of each block copolymer at 230°C was measured using the above-mentioned automelt indexer. This value was used as a standard, and compared with the measured value after each block copolymer was held in a heating furnace at 230°C for 30 minutes, and the heat resistance was evaluated based on the ratio (%) of change before and after the holding. The load was set to 21.2N or 49.0N according to the fluidity of the block copolymer.

[0035] Example 1 Polymerization of block copolymer 1 A 5 L stainless steel polymerization vessel equipped with a jacket and a stirrer was thoroughly purged with nitrogen, after which 3.3 L of cyclohexane was charged and the reaction system was heated to 55°C by running hot water through the jacket. Next, 3.3 mL of 10% sec-butyllithium cyclohexane solution and 0.30 mL of 2,2-di-(2-tetrahydrofuryl)propane were added and stirred for 1 minute, after which 50 g of styrene was added to initiate polymerization. After 30 minutes of reaction, the weight average molecular weight of the styrene-based polymer block reached 12,200, and 250 g of isoprene and 150 g of styrene were added in two portions and reacted for a total of 60 minutes. After that, 50 g of styrene was added and reacted for 30 minutes. After completion of the reaction, methanol was added to stop the reaction, and block copolymer 1 was obtained.

[0036] Example 2 Polymerization of block copolymer 2 Block copolymer 2 was obtained by the same procedure as in Example 1, except that the amount of sec-butyllithium·cyclohexane solution and the amount of 2,2-di-(2-tetrahydrofuryl)propane added were changed to 2.7 mL and 0.24 mL, the weight average molecular weight of the styrene-based polymer block obtained in the first step was changed to 15,400, and the amounts of isoprene and styrene added were changed to 240 g and 160 g, respectively.

[0037] Example 3 Polymerization of block copolymer 3 Block copolymer 3 was obtained by the same procedure as in Example 1, except that the amount of sec-butyllithium·cyclohexane solution and the amount of 2,2-di-(2-tetrahydrofuryl)propane added were changed to 2.5 mL and 0.23 mL, the weight average molecular weight of the styrene-based polymer block obtained in the first step was changed to 16,200, and the amounts of isoprene and styrene added were changed to 225 g and 175 g, respectively.

[0038] Example 4 Polymerization of block copolymer 4 Block copolymer 4 was obtained by the same procedure as in Example 1, except that the amount of sec-butyllithium·cyclohexane solution and the amount of 2,2-di-(2-tetrahydrofuryl)propane added were changed to 2.4 mL and 0.28 mL, the weight average molecular weight of the styrene-based polymer block obtained in the first step was changed to 16,800, and the amounts of isoprene and styrene added were changed to 225 g and 175 g, respectively.

[0039] Example 5 Polymerization of Block Copolymer 5 Block copolymer 5 was obtained by the same procedure as in Example 1, except that the amount of sec-butyllithium·cyclohexane solution and the amount of 2,2-di-(2-tetrahydrofuryl)propane added were changed to 2.3 mL and 0.31 mL, the weight average molecular weight of the styrene-based polymer block obtained in the first step was changed to 17,600, and the amounts of isoprene and styrene added were changed to 225 g and 175 g, respectively.

[0040] Example 6 Polymerization of block copolymer 6 Block copolymer 6 was obtained by the same procedure as in Example 1, except that the amount of sec-butyllithium-cyclohexane solution added was changed to 2.7 mL and the weight average molecular weight of the styrene-based polymer block obtained in the first step was changed to 15,500.

[0041] Comparative Example 1 Polymerization of block copolymer 7 A 5 L stainless steel polymerization vessel equipped with a jacket and a stirrer was thoroughly purged with nitrogen, after which 3.3 L of cyclohexane was charged and the reaction system was heated to 55°C by running hot water through the jacket. Next, 2.7 mL of sec-butyllithium cyclohexane solution and 0.20 mL of N,N,N',N'-tetramethylethylenediamine were added and stirred for 1 minute, after which 50 g of styrene was added to initiate polymerization. After 30 minutes of reaction, the weight average molecular weight of the styrene-based polymer block reached 15,000, and 250 g of isoprene and 150 g of styrene were added in two portions and reacted for a total of 60 minutes. After that, 50 g of styrene was added and reacted for 30 minutes. After completion of the reaction, methanol was added to stop the reaction, and block copolymer 7 was obtained.

[0042] Comparative Example 2 Polymerization of block copolymer 8 Block copolymer 8 was obtained by the same procedure as in Example 1, except that the amount of sec-butyllithium·cyclohexane solution and the amount of 2,2-di-(2-tetrahydrofuryl)propane added were changed to 2.1 mL and 0.29 mL, respectively, and the weight average molecular weight of the styrene-based polymer block obtained in the first step was changed to 19,400.

[0043] Comparative Example 3 Polymerization of block copolymer 9 A 5 L stainless steel polymerization vessel equipped with a jacket and a stirrer was thoroughly purged with nitrogen, after which 3.3 L of cyclohexane was charged and the reaction system was heated to 55°C by running hot water through the jacket. Next, 3.3 mL of sec-butyllithium cyclohexane solution and 1.09 mL of 2,2-di-(2-tetrahydrofuryl)propane were added and stirred for 1 minute, after which 50 g of styrene was added to initiate polymerization. After 30 minutes of reaction, the weight average molecular weight of the styrene-based polymer block reached 12,400, and the reaction system was cooled to 40°C, and 400 g of isoprene was added in two portions, and the reaction was continued for a total of 180 minutes. The reaction system was then heated again to 55°C, and 50 g of styrene was added and reacted for 30 minutes. After completion of the reaction, methanol was added to stop the reaction, and block copolymer 8 was obtained.

[0044] Table 2 shows the physical properties of the block copolymers obtained by the methods of the Examples and Comparative Examples.

[0045] [Table 2]

[0046] From Table 1, in Examples 1 to 6, the vinyl content is 40 Mole %, but in all cases tan δ is in the range of 0 to 30°C and is 0.7 or more, indicating high vibration damping properties at room temperature. In addition, the temperature range in which tan δ is 0.3 or more is wide, and it can be seen that vibration damping properties are maintained even when the temperature is shifted from the peak temperature. In addition, thermal stability is also high.

[0047] In Comparative Example 1, the aromatic vinyl monomer introduced into the conjugated diene block has low random bonding property compared with Examples 1 to 6. Due to the lack of random bonding property, the tan δ peak temperature was outside the target range. In addition, the temperature range where tan δ is 0.3 or more is narrow.

[0048] Comparative Examples 2 and 3 had a higher vinyl bond content than Examples 1 to 6, and were inferior in heat resistance. It is presumed that the increase in vinyl bond content made crosslinking reaction more likely to occur during heating. In addition, the tan δ peak temperature of Comparative Example 3 exceeded 30°C.

Claims

1. A block copolymer comprising at least two styrene blocks and at least one polymer block in which isoprene and styrene are randomly bonded, containing a vinyl group, and satisfying the following a) to d), the vinyl group being non-hydrogenated: a) The styrene content in the block copolymer is 45 to 60% by weight, and the random bonding rate of styrene in the polymer block in which isoprene and styrene are bonded randomly is 70 to 90 mol %. b) The tan δ peak temperature at a measurement frequency of 10 Hz is 0 to 30° C. and the peak value is 0.7 or more. c) At a measurement frequency of 10 Hz, the temperature range in which tan δ is 0.3 or more is 45° C. or more. d) The vinyl bond content of the conjugated diene polymer is 40 mol % or less.

2. The block copolymer according to claim 1, wherein the weight average molecular weight of the block copolymer is 100,000 to 300,000.

3. A method for producing a block copolymer, comprising: a first step of producing at least two polymer blocks mainly composed of styrene; a second step of producing a polymer block obtained by randomly bonding at least one of isoprene and styrene to the polymer block obtained in the first step; and a third step of producing at least two polymer blocks mainly composed of styrene to the polymer block obtained in the second step, The polymerization reaction in each step is carried out in the presence of 2,2-di(tetrahydrofuryl)propane, and the amount of the 2,2-di(tetrahydrofuryl)propane added is 0.4 to 0.6 equivalents relative to the organolithium compound.

4. The method according to claim 3, wherein the polymerization temperature range is 40 to 90°C.

Citation Information

Patent Citations

  • Block copolymer excellent in vibration-damping performance and composition containing the same

    JP1990102212A

  • Light guide plate

    JP2002071964A

  • Block copolymer, composition containing the same, and vibration damper

    JP2002284830A

  • Optical film and polarizing plate

    WO2017086265A1

Cited By

  • Block copolymer with excellent vibration damping properties over a wide temperature range and method for producing the same

    JP2026177582A

  • Block copolymer with excellent vibration damping properties over a wide temperature range and method for producing the same

    JP7933943B1