Ethylene-based polymerization catalyst component, method for producing ethylene-based polymerization catalyst, and method for producing ethylene-based polymer

The ethylene polymerization catalyst component addresses the imbalance in creep resistance and impact resistance of existing catalysts by producing ethylene polymers with ultra-high molecular weight and controlled molecular weight distribution, enhancing the balance of mechanical properties.

JP7559337B2Active Publication Date: 2024-10-02JAPAN POLYETHYLENE CORP
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
JP2020050579
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-03-28
Filing Date
2020-03-23
Publication Date
2024-10-02
Estimated Expiration
2040-03-23

AI Technical Summary

Technical Problem

Existing ethylene polymerization catalysts, such as Phillips catalysts, struggle to produce ethylene polymers with a balanced combination of creep resistance and impact resistance, as improving one property often deteriorates the other, and they lack precise control over molecular weight distribution and composition.

Method used

An ethylene polymerization catalyst component is developed using an inorganic oxide with specific infrared spectrum and chemical composition, supporting a chromium compound and activating it to produce a catalyst capable of creating ethylene polymers with ultra-high molecular weight components.

Benefits of technology

The catalyst enables the production of ethylene polymers with a superior balance of creep resistance and impact resistance, achieving high molecular weight and controlled molecular weight distribution.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007559337000003
    Figure 0007559337000003
  • Figure 0007559337000004
    Figure 0007559337000004
  • Figure 0007559337000005
    Figure 0007559337000005
Patent Text Reader

Abstract

To provide an ethylenic polymerization catalyst component which is capable of producing an ethylenic polymer containing an ultrahigh molecular weight component.SOLUTION: The ethylenic polymerization catalyst component contains an inorganic oxide having the following characteristic 1 and characteristic 2, as measured after calcination, as a pretreatment for analysis, at 600°C for 24 hours: characteristic 1, in an infrared spectrum, a ratio (Py / Px) of Py, which is an intensity of a maximum peak in a range Y of 3700 cm-1 to 3799 cm-1 to Px, which is an intensity of a maximum peak in a range X of 3600 cm-1 to 3699 cm-1 is less than 10; and characteristic 2, SiO2 is contained in a proportion of 90 wt.% or more.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an ethylene-based polymerization catalyst component, a method for producing an ethylene-based polymerization catalyst, and a method for producing an ethylene-based polymer. More specifically, the present invention relates to an ethylene-based polymerization catalyst component capable of producing an ultrahigh molecular weight ethylene polymer, a method for producing an ethylene-based polymerization catalyst, and a method for producing an ethylene-based polymer. [Background technology]

[0002] Ethylene-based polymers are key materials that represent plastic materials in industrial fields. Ethylene-based polymers are widely used in a wide variety of technical fields, and therefore require a wide range of properties, such as molecular weight distribution and flowability, as well as mechanical and thermal properties, depending on the application and molding method. In order to produce such ethylene polymers, various polymerization catalysts have been developed and improved. Among them, Phillips catalysts are used heavily along with Ziegler catalysts and metallocene catalysts. Phillips catalysts are chromium catalysts in which a chromium compound is supported on an inorganic oxide carrier such as silica, silica-alumina, or silica-titania, and activated in a non-reducing atmosphere to convert at least some of the supported chromium atoms into hexavalent chromium atoms. Phillips catalysts produce ethylene polymers with a wide molecular weight distribution, and generally have good moldability, making them suitable for blow molding and the like.

[0003] In large blow-molded products, creep resistance and impact resistance are important properties. When an ethylene-based polymer having a wide molecular weight distribution obtained by a conventional Phillips catalyst is blow-molded into a large product, the molded product does not necessarily have a sufficient balance between creep resistance and impact resistance. Creep resistance and impact resistance are mutually exclusive physical properties, and generally, when creep resistance is improved, impact resistance is reduced, and conversely, when impact resistance is improved, creep resistance is reduced.

[0004] Therefore, if an ethylene polymer having both excellent physical properties such as creep resistance and moldability can be obtained using the Phillips catalyst, it will be a material having a better balance of physical properties and moldability than the conventional level. However, since it is difficult at the present stage to precisely control the catalyst using the Phillips catalyst to introduce an appropriate amount of long chain branches of an appropriate length in an appropriate molecular weight region, no specific guidelines have yet been obtained for a method of improving both physical properties and moldability. In an attempt to obtain an ethylene polymer having a good balance of physical properties and moldability using a Phillips catalyst, the use of a carrier having a specific structure has been investigated. For example, Patent Document 1 and Patent Document 2 disclose the use of highly porous silica having a specific surface area, average pore volume, and average pore diameter. Patent Document 3 discloses a technique for broadening the molecular weight distribution of a polymer by combining a Phillips catalyst obtained from silica having a specific structure with an organoaluminum compound. Furthermore, Patent Document 4 discloses the use of silica having a unique pore structure and crystallinity. However, it is difficult to control the molecular weight distribution and composition distribution of the polymer using these catalysts, and it has not been possible to design catalysts that will produce the desired material properties.

[0005] Therefore, attempts have been made to polymerize high molecular weight components and low molecular weight components using separate catalysts. For example, if a high molecular weight component with a high molecular weight and a wide molecular weight distribution is produced, and a low molecular weight component with a low molecular weight and a narrow molecular weight distribution is produced at the same time, the high molecular weight component can be increased and the low molecular weight component can be decreased, making it possible to improve both creep resistance and impact resistance. From this perspective, Patent Document 5 discloses that high molecular weight polyethylene can be obtained by a Phillips catalyst using a clay mineral as a carrier. Patent Documents 6 and 7 disclose that the molecular weight distribution of the obtained polymer can be controlled by combining a clay mineral with ordinary silica. As described above, various catalysts have been developed and various ethylene polymers have been synthesized, but the ethylene polymers produced using existing catalysts may not provide the desired effects. Therefore, as one variation of ethylene polymers, an ethylene polymer having an ultra-high molecular weight component is desired. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] Special Publication No. 2002-533536 [Patent Document 2] Patent No. 5821746 [Patent Document 3] Special Publication No. 2006-512454 [Patent Document 4] Special Publication No. 2007-517962 [Patent Document 5] JP 2006-257255 A [Patent Document 6] JP 2008-150566 A [Patent Document 7] International Publication No. 2002 / 088196 Summary of the Invention [Problem to be solved by the invention]

[0007] The present invention has been made in view of the above-mentioned circumstances, and aims to provide an ethylene-based polymerization catalyst component capable of producing an ethylene-based polymer having an ultra-high molecular weight component. Another aim of the present invention is to provide a method for producing an ethylene-based polymerization catalyst capable of producing an ethylene-based polymer having an ultra-high molecular weight component, and a method for producing an ethylene-based polymer having an ultra-high molecular weight component. As a result of intensive research to solve the above-mentioned problems, the present inventors have found that an ethylene-based polymer having an ultra-high molecular weight component can be produced by using an ethylene-based polymerization catalyst component having a specific infrared spectrum and chemical composition, and have completed the present invention based on this finding. The present invention can be realized in the following forms. [Means for solving the problem]

[0008] [1] An ethylene polymerization catalyst component, comprising an inorganic oxide having the following properties 1 and 2, as measured after calcination at 600°C for 24 hours as a pretreatment for analysis: Characteristic 1: In the infrared spectrum, 3600 cm -1 ~3699cm -1 3700cm for the maximum peak intensity Px in the range X -1 ~3799cm -1 The ratio Py / Px of the maximum peak intensity Py in the range Y is less than 10. Property 2: Contains 90% or more by weight of SiO2.

[0009] [2] The ethylene-based polymerization catalyst component according to [1], wherein the inorganic oxide has a peak at 2θ=23° to 29° in powder X-ray diffraction that indicates crystallinity and has a half-width of 0.2° or more and 5° or less.

[0010] [3] A step (I) of supporting a chromium compound on the ethylene-based polymerization catalyst component described in [1] or [2] above; A step (II) of calcining and activating the chromium compound-supported component obtained in the step (I) at 400° C. to 900° C. in a non-reducing atmosphere to convert at least a part of the chromium atoms into hexavalent chromium atoms; 2. A method for producing an ethylene polymerization catalyst comprising the steps of:

[0011] [4] The method for producing an ethylene-based polymerization catalyst according to [3], wherein the chromium compound-supported component containing 0.01% by weight to 2.0% by weight of chromium atoms is obtained in the step (I).

[0012] [5] The method for producing an ethylene-based polymerization catalyst according to [3] or [4], characterized in that in the step (II), 50% or more of chromium atoms contained in the chromium compound-supported component are oxidized to hexavalent chromium atoms.

[0013] [6] A method for producing an ethylene-based polymer, comprising polymerizing a monomer containing at least ethylene using an ethylene-based polymerization catalyst obtained by the production method according to any one of the above [3] to [5]. Effect of the Invention

[0014] By using the ethylene-based polymerization catalyst component of the present invention, it is possible to provide an ethylene-based polymerization catalyst capable of producing an ethylene-based polymer having an ultrahigh molecular weight component. According to the process for producing an ethylene polymer catalyst of the present invention, it is possible to produce an ethylene polymerization catalyst capable of producing an ethylene polymer having an ultra-high molecular weight component. According to the process for producing an ethylene polymer of the present invention, an ethylene polymer having an ultra-high molecular weight component can be produced. [Brief description of the drawings]

[0015] [Figure 1] 1 is a graph showing infrared spectra of Example 1 and Comparative Example 1. [Diagram 2] FIG. 2 is a schematic diagram for explaining the plate thickness T and D / T of an inorganic oxide particle B1. [Diagram 3] 1 is a SEM image of chromium catalyst A1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0016] Hereinafter, the present invention will be described specifically and in detail for each item. In this specification, when a numerical range is described using "to", the range includes the lower limit and the upper limit unless otherwise specified. For example, the description "10 to 20" includes both the lower limit "10" and the upper limit "20". In other words, "10 to 20" has the same meaning as "10 or more and 20 or less".

[0017] 1. Ethylene-based polymerization catalyst components The ethylene polymerization catalyst component is characterized in that it contains an inorganic oxide having the following properties 1 and 2, as measured after calcination at 600° C. for 24 hours as a pretreatment for analysis. Characteristic 1: In the infrared spectrum, 3600 cm -1 ~3699cm -1 3700cm for the maximum peak intensity Px in the range X -1 ~3799cm -1 The ratio Py / Px of the maximum peak intensity Py in the range Y is less than 10. Property 2: Contains 90% or more by weight of SiO2.

[0018] 2. Inorganic oxide particles B1 as inorganic oxide A suitable example of an inorganic oxide having the properties 1 and 2 is the following inorganic oxide particle B1.

[0019] (1) Characteristics of inorganic oxide particles B1 Characteristic 1 is the infrared spectrum at 3600 cm -1 ~3699cm -1 3700cm for the maximum peak intensity Px in the range X -1 ~3799cm -1 The characteristic is that the ratio Py / Px of the peak intensity Py that is maximum in the range Y is less than 10. In the infrared spectrum, 3550 cm -1 The peaks appearing around 3650 cm are due to hydrogen-bonded OH groups. -1 The peaks appearing around 3750 cm are due to OH groups at sites that cannot interact with others. -1 The peak appearing around 3650 cm is due to isolated OH groups on the outer surface. Inorganic oxides that satisfy the requirements of the above-mentioned characteristic 1 have a peak around 3650 cm. -1 The peak intensity around 0.05 is relatively strong. This indicates that inorganic oxide particle B1 has a structure containing many OH groups that are not involved in dehydration condensation even when heated to high temperatures. Such a structure is considered to be a thermally stable regular structure, and it is presumed that the regularity of the structure affects the arrangement of the OH groups. In the graph of FIG. 1, the infrared spectrum of one example of the inorganic oxide particles B1 (Example 1 described below) is shown by a solid line.

[0020] (2) Characteristics of inorganic oxide particles B1 2 Characteristic 2 is a characteristic that the inorganic oxide particles B1 contain 90% or more by weight of SiO2. In other words, the inorganic oxide particles B1 are inorganic oxides whose main component is SiO2. The content of SiO2 in the inorganic oxide particles B1 may be 90% by weight or more, preferably 95% by weight or more, and more preferably 98% by weight or more. Of course, the content of SiO2 may be 100% by weight. Since the inorganic oxide particles B1 are particles whose main component is SiO2, it is easy to control the shape of the inorganic oxide and the catalytic performance is excellent. When the content is less than 100% by weight, the remaining components may be any inorganic oxide components, but oxides containing metals of Groups 2, 3, 4, and 13 of the Periodic Table (Periodic Table according to the 1990 Rules for the Nomenclature of Inorganic Compounds) are preferred. Specific examples include magnesia (MgO), alumina (Al2O3), titania (TiO2), zirconia (ZrO2), and composite oxides thereof, i.e., alumina-titania (Al2O3-TiO2), alumina-magnesia (Al2O3-MgO), alumina-zirconia (Al2O3-ZrO2), titania-magnesia (TiO2-MgO), titania-zirconia (TiO2-ZrO2), etc. Among these, magnesia, alumina, and titania are preferred, and alumina and titania are more preferred.

[0021] (3) Powder X-ray diffraction of inorganic oxide particles B1 The inorganic oxide particles B1 preferably have a peak showing crystallinity at a half width of 0.2° to 5° at 2θ=23° to 29° in powder X-ray diffraction. When the inorganic oxide particles B1 are crystalline, the molecular weight of the ethylene-based polymer tends to be increased.

[0022] (4) Surface area of ​​inorganic oxide particles B1 The surface area of ​​the inorganic oxide particles B1 is not particularly limited. From the viewpoint of supporting chromium atoms in a dispersed state, a surface area of ​​10 m 2 / g or more 1000m2 / g or less, and 2 / g or more 500m 2 / g or less is more preferable, and 50m 2 / g or more 400m 2 It is more preferable that the molecular weight is not more than 1 / g.

[0023] (5) Pore volume of inorganic oxide particles B1 The pore volume of the inorganic oxide particles B1 is not particularly limited, but the pore volume is preferably from 0.05 to 5 mL / g, and more preferably from 0.1 to 3 mL / g.

[0024] (6) Shape of inorganic oxide particles B1 The shape of the inorganic oxide particles B1 is not particularly limited. For example, the inorganic oxide particles B1 may have a plate-like particle shape (first embodiment). Alternatively, the inorganic oxide particles B1 may contain aggregates of plate-like inorganic oxide particles B1 (second embodiment). In this second embodiment, the inorganic oxide particles B1 may be composed of aggregates only. In addition, in this second embodiment, aggregates of plate-like inorganic oxide particles B1 and non-aggregated plate-like inorganic oxide particles B1 may be mixed. The plate thickness T (nm) of the plate-like inorganic oxide particles B1 is not particularly limited. From the viewpoint of maintaining the crystalline structure and maintaining dispersibility in the polymer during polymerization, the average plate thickness T (nm) of the inorganic oxide particles B1 is preferably 1 nm or more and 100 nm or less, more preferably 5 nm or more and 50 nm or less, and even more preferably 10 nm or more and 40 nm or less. The average plate thickness T (nm) of the inorganic oxide particles B1 is determined by measuring the plate thickness T (nm) of 10 inorganic oxide particles B1 with a scanning electron microscope (SEM) and averaging the measured values. Figure 2 is a schematic diagram of an SEM image of the inorganic oxide particles B1 observed with a scanning electron microscope, and shows the plate thickness T (nm). The average value of D / T, which is the ratio of the maximum diameter D (nm) to the plate thickness T (nm) of the inorganic oxide particles B1, is not particularly limited. From the viewpoint of being present as a plate-like structure in the particles, the average value of D / T is preferably 10 or more, more preferably 20 or more, and even more preferably 30 or more. The upper limit of the average value of D / T is not particularly limited, but is usually 2000. The average value of D / T is determined by observing 10 inorganic oxide particles B1 with a scanning electron microscope (SEM). That is, the average value of D / T is determined by calculating D / T, which is the ratio of the maximum particle diameter D (nm) to the plate thickness T (nm) for each of 10 inorganic oxide particles B1, and averaging these values. FIG. 2 is a schematic diagram of an SEM image of inorganic oxide particles B1 observed with a scanning electron microscope, showing the maximum diameter D (nm). The D / T of each particle can be determined from this maximum diameter D (nm) and the above-mentioned plate thickness T (nm).

[0025] 3. Inorganic oxide particles B2 as inorganic oxide The ethylene-based polymerization catalyst component can contain inorganic oxide particles B2 in addition to inorganic oxide particles B1. The inorganic oxide particles B2 are amorphous. The inorganic oxide particles B2 are preferably composed of at least one type of particles selected from the group consisting of particles whose main component is silica (SiO2), particles whose main component is silica-titania (SiO2-TiO2), and particles whose main component is silica-alumina (SiO2-Al2O3). Here, the main component refers to a substance whose content (wt%) is 90 wt% or more. The content of silica (SiO2) in the particles whose main component is silica (SiO2) may be 90% by weight or more, preferably 95% by weight or more, and more preferably 98% by weight or more. Of course, the content of silica (SiO2) may be 100% by weight. The total content of silica (SiO2) and titania (TiO2) in the particles whose main component is silica-titania (SiO2-TiO2) may be 90% by weight or more, preferably 95% by weight or more, and more preferably 98% by weight or more. Of course, the total content of silica (SiO2) and titania (TiO2) may be 100% by weight. The total content of silica (SiO2) and alumina (Al2O3) in the particles whose main component is silica-alumina (SiO2-Al2O3) may be 90% by weight or more, preferably 95% by weight or more, and more preferably 98% by weight or more. Of course, the total content of silica (SiO2) and alumina (Al2O3) may be 100% by weight. Among these, from the viewpoints of ease of controlling the particle shape of the inorganic oxide and catalyst performance, it is preferable that the inorganic oxide particles B2 are particles whose main component is silica (SiO2). When particles whose main component is silica-titania (SiO2-TiO2) are used, the particles contain titanium atoms in an amount of 0.2 to 40% by weight, preferably 0.5 to 30% by weight, and more preferably 1 to 20% by weight, as the metal component. Furthermore, when particles whose main component is silica-zirconia (SiO2-ZrO2) are used, the particles contain 0.2 wt% to 40 wt%, preferably 0.5 wt% to 30 wt%, and more preferably 1 wt% to 20 wt% of zirconium atoms as the metal component. Furthermore, when particles whose main component is silica-alumina (SiO2-Al2O3) are used, the particles contain 0.2 wt% to 40 wt%, preferably 0.5 wt% to 30 wt%, and more preferably 1 wt% to 20 wt% of aluminum atoms as the metal component.

[0026] The surface area of ​​the inorganic oxide particles B2 is not particularly limited. From the viewpoint of supporting chromium atoms in a dispersed state, a surface area of ​​100 m 2 / g or more 1000m 2 / g or less, and 2 / g or more 950m 2 / g or less is more preferable, and 200m2 / g or more 900m 2 It is more preferable that the molecular weight is not more than 1 / g.

[0027] The pore volume of the inorganic oxide particles B2 is not particularly limited. From the viewpoint that the chromium atoms are supported in a dispersed state and the particles are easily disintegrated during polymerization to allow the polymer to grow, the pore volume is preferably 0.1 mL / g or more and 5.0 mL / g or less, and more preferably 0.2 mL / g or more and 3.0 mL / g or less.

[0028] 4. Method for producing ethylene polymerization catalyst The method for producing an ethylene-based polymerization catalyst includes the steps of: (I) supporting a chromium compound on an ethylene-based polymerization catalyst component; A step (II) of calcining and activating the chromium compound-supported component obtained in the step (I) at 400° C. to 900° C. in a non-reducing atmosphere to convert at least a part of the chromium atoms into hexavalent chromium atoms; Includes.

[0029] 4.1 Method for producing chromium catalyst A1 In the method for producing an ethylene-based polymerization catalyst, when the ethylene-based polymerization catalyst component contains inorganic oxide particles B1, the following production method is used (the ethylene-based polymerization catalyst produced by this production method is referred to as chromium catalyst A1). The method for producing the chromium catalyst A1 includes the steps of: (I) supporting a chromium compound D on inorganic oxide particles B1; and (II) calcining and activating the inorganic oxide particles B1 supporting the chromium compound D obtained in the step (I) at 400°C to 900°C in a non-reducing atmosphere to convert at least a portion of the chromium atoms to hexavalent chromium.

[0030] Here, the chromium catalyst A1 will be described. The chromium catalyst A1 is a catalyst in which a chromium compound C1 is supported on inorganic oxide particles B1. Chromium catalyst A1 is a chromium catalyst in which at least some of the chromium atoms are hexavalent, and is generally classified as a catalyst known as a Phillips catalyst. The outline of this catalyst is described in the literature such as "Polyethylene Technology Reader" edited by Kazuo Matsuura and Naotaka Mikami, p.81, 2001, Kogyo Chosakai, MPMcDaniel; Advances in Catalysis Vol.33 p.47(1985) Academic Press Inc., MPMcDaniel "Handbook of Heterogeneous Catalysis" p.2400(1997) VCH, MBWelch et al. "Handbook of Polyolefins Synthesis and Properties" p.21(1993) Marcel Dekker, etc. The chromium catalyst A1 is generally produced by contacting inorganic oxide particles B1 (inorganic oxide support) with a chromium compound D described later and activating it in a non-reducing atmosphere.

[0031] The chromium compound C1 is not particularly limited as long as it is a chromium compound in which at least some of the chromium atoms are hexavalent. For example, the chromium compound C1 is derived from chromium oxide, chromium halide, oxyhalide, chromate, dichromate, nitrate, carboxylate, sulfate, chromium-1,3-diketo compound, chromate ester, etc. (hereinafter, the trivalent chromium compounds such as chromium oxide to chromate ester listed here are also referred to as "chromium compound D"). The chromium compound D is supported on the inorganic oxide particles B1, and then activated in a non-reducing atmosphere to become the chromium compound C1. The hexavalent chromium compound C1 may be directly supported on the inorganic oxide particles B1. More specifically, examples of the chromium compound D include chromium (III) oxide, chromium trichloride, chromyl chloride, potassium chromate, ammonium chromate, potassium dichromate, chromium nitrate, chromium sulfate, chromium acetate, tris(2-ethylhexanoate)chromium, chromium acetylacetonate, bis(tert-butyl)chromate, etc. In particular, chromium compound D is preferably chromium (III) oxide, chromium acetate, or chromium acetylacetonate. It is known that even when a chromium compound having an organic group, such as chromium acetate or chromium acetylacetonate, is used, the organic group portion is burned by activation in a non-reducing atmosphere, which will be described later, and ultimately reacts with hydroxyl groups on the surface of the inorganic oxide support, as in the case of using chromium (III) oxide, and at least a part of the chromium atoms become hexavalent and are fixed in a chromate ester structure (see VJ Ruddic et al.; J. Phys. Chem. Vol. 100, p. 11062 (1996); SM Augustin et al.; J. Catal. Vol. 161, p. 641 (1996)).

[0032] In step (I), the following methods can be used. Suitable examples include a method in which the inorganic oxide particles B1 are impregnated with a chromium compound D solution and then the solvent is removed, and a method in which the chromium compound D is sublimated without using a solvent. Other known methods can also be used. The supporting method is appropriately selected depending on the type of chromium compound D used. Furthermore, during the production of the inorganic oxide particles B1, a raw material to which the chromium compound D has been added beforehand may be used to directly obtain the inorganic oxide particles B1 carrying the chromium compound D.

[0033] In the step (I), inorganic oxide particles B1 supporting chromium compound D containing 0.01 to 2.0% by weight of chromium atoms may be obtained. The content of chromium atoms in chromium catalyst A1 is not particularly limited, but from the viewpoint of preventing the supported chromium atoms from agglomerating with each other and being efficiently activated, the content is preferably 0.01 to 2.0% by weight, more preferably 0.1 to 2.0% by weight, and even more preferably 0.2 to 1.5% by weight.

[0034] In step (II), the inorganic oxide particles B1 carrying the chromium compound D obtained in step (I) are fired in an activation furnace to activate the inorganic oxide particles B1. The activation is carried out in a non-reducing atmosphere that is substantially free of moisture. For example, the activation is carried out in oxygen or air, but an inert gas may also be present. Preferably, the activation is carried out under a fluidized state using air that has been sufficiently dried by passing molecular sieves or the like through the air. The activation temperature is 400°C to 900°C, preferably 430°C to 900°C, and more preferably 450°C to 850°C. The activation time is not particularly limited. The activation time is preferably 30 minutes to 48 hours, more preferably 1 hour to 35 hours, and even more preferably 2 hours to 30 hours. By the activation, at least a part of the chromium atoms of the chromium compound D supported on the inorganic oxide particles B1 is oxidized to hexavalent chromium, and as described above, the chromium compound C1 is chemically fixed on the inorganic oxide particles B1. If the activation is performed at a temperature lower than 400°C, the polymerization activity decreases, and if the activation is performed at a temperature higher than 900°C, sintering occurs and the activity decreases.

[0035] During the supporting or activation of the chromium compound D, a known method for adjusting the ethylene polymerization activity or the molecular weight and molecular weight distribution of the obtained ethylene polymer by adding a fluorine compound such as ammonium silicofluoride or ammonium hydrogen difluoride, a titanium alkoxide such as titanium tetraisopropoxide, a zirconium alkoxide such as zirconium tetrabutoxide, an aluminum alkoxide such as aluminum tributoxide, an organoaluminum such as trialkylaluminum, an organomagnesium such as dialkylmagnesium, or a metal alkoxide, or an organometallic compound, may be used in combination. In these metal alkoxides or organometallic compounds, the organic group portion is burned by activation in a non-reducing atmosphere, and is oxidized to a metal oxide such as titania, zirconia, alumina or magnesia, which is contained in the catalyst. In addition, the fluorine compound is thermally decomposed during activation to fluorinate the inorganic oxide support. These methods are described in outline or detail in documents such as CE Marsden; Plastics, Rubber and Composites Processing and Applications Vol. 21 p. 193 (1994), T. Pullukat et al.; J. Polym. Sci., Polym. Chem. Ed. Vol. 82 p. 118 (1980), and MP McDaniel et al.; J. Catal. Vol. 82 p. 118 (1983).

[0036] In step (II), it is preferable that 50% or more of the chromium atoms contained in the inorganic oxide particles B1 supporting the chromium compound D are oxidized to a hexavalent state. More preferably, 60% or more of the chromium atoms contained in the inorganic oxide particles B1 supporting the chromium compound D are oxidized to a hexavalent state. The upper limit of the chromium atoms oxidized to a hexavalent state is 100%. The proportion of chromium atoms oxidized to a hexavalent state is adjusted by the activation temperature and time. The total amount of chromium atoms can be measured by a general metal analysis method, such as plasma emission spectrometry or X-ray fluorescence spectrometry. The valence of chromium can be roughly known by visually observing the color change of the solid product (generally, hexavalent chromium is yellow to orange, trivalent chromium is green, and divalent chromium is blue), but for quantitative analysis, chelate titration and absorptiometry are known as simple methods. Specifically, it is described in "Experimental Chemistry Lecture 15 Analysis" edited by the Chemical Society of Japan, Maruzen (1991), pp. 246-248. For example, trivalent chromium can be quantitatively determined by adding an excess of EDTA (ethylenediaminetetraacetic acid) of a known concentration to trivalent chromium in an acidic solution, boiling for 5-10 minutes, and titrating with a standard solution of trivalent iron. Also, in the case of hexavalent chromium, CrO4 2- Quantitation is possible by measuring the absorbance at a wavelength of 366 nm, taking advantage of the fact that it exists as such.

[0037] 4.2 Method for producing chromium catalyst A2 In the method for producing an ethylene-based polymerization catalyst, when the ethylene-based polymerization catalyst component contains inorganic oxide particles B2, the following production method is used (the ethylene-based polymerization catalyst produced by this production method is referred to as chromium catalyst A2). The method for producing the chromium catalyst A2 includes a step (III) of supporting a chromium compound E on inorganic oxide particles B2, and a step (IV) of calcining and activating the inorganic oxide particles B2 supporting the chromium compound E obtained in the step (III) at 400°C to 900°C in a non-reducing atmosphere to convert at least a portion of the chromium atoms to hexavalent chromium.

[0038] Here, the chromium catalyst A2 will be described. The chromium catalyst A2 is formed by supporting a chromium compound C2 on amorphous inorganic oxide particles B2. Chromium catalyst A2 is a chromium catalyst in which at least some of the chromium atoms are hexavalent, and is generally classified as a catalyst known as a Phillips catalyst. The outline of this catalyst is described in the literature such as "Polyethylene Technology Reader" edited by Kazuo Matsuura and Naotaka Mikami, p. 81, 2001, Kogyo Chosakai, MPMcDaniel; Advances in Catalysis Vol. 33 p. 47 (1985) Academic Press Inc., MPMcDaniel "Handbook of Heterogeneous Catalysis" p. 2400 (1997) VCH, MBWelch et al. "Handbook of Polyolefins Synthesis and Properties" p. 21 (1993) Marcel Dekker, etc. The chromium catalyst A2 is generally produced by contacting amorphous inorganic oxide particles B2 (inorganic oxide support) with a chromium compound E (described later) and activating it in a non-reducing atmosphere.

[0039] The average particle size of the particles of the chromium catalyst A2 is not particularly limited. From the viewpoint of handling, the average particle size is preferably 0.001 μm or more and 200 μm or less, more preferably 0.005 μm or more and 150 μm or less, and even more preferably 0.01 μm or more and 100 μm or less. The average particle size of the particles of chromium catalyst A2 can be determined by measuring the particle size of 20 particles of chromium catalyst A2 using a scanning electron microscope (SEM) and averaging the measured values. In this study, the average particle size of particles with an average particle size of 0.1 μm or more was determined using a particle size distribution measuring device using the laser diffraction method, and the average particle size of particles with an average particle size of less than 0.1 μm was determined by SEM observation.

[0040] The chromium compound C2 is not particularly limited as long as it is a chromium compound in which at least some of the chromium atoms are hexavalent. For example, the chromium compound C2 is derived from chromium oxide, chromium halide, oxyhalide, chromate, dichromate, nitrate, carboxylate, sulfate, chromium-1,3-diketo compound, chromate ester, etc. (hereinafter, the trivalent chromium compounds such as chromium oxide to chromate ester listed here are also referred to as "chromium compound E"). The chromium compound E is supported on the inorganic oxide particles B2, and then activated in a non-reducing atmosphere to become the chromium compound C2. The hexavalent chromium compound C2 may be directly supported on the inorganic oxide particles B2. More specifically, examples of the chromium compound E include chromium (III) oxide, chromium trichloride, chromyl chloride, potassium chromate, ammonium chromate, potassium dichromate, chromium nitrate, chromium sulfate, chromium acetate, tris(2-ethylhexanoate)chromium, chromium acetylacetonate, bis(t-butyl)chromate, etc. In particular, chromium compound E is preferably chromium (III) oxide, chromium acetate, or chromium acetylacetonate. It is known that even when a chromium compound having an organic group, such as chromium acetate or chromium acetylacetonate, is used, the organic group portion is burned by activation in a non-reducing atmosphere, which will be described later, and ultimately reacts with hydroxyl groups on the surface of the inorganic oxide support, as in the case of using chromium (III) oxide, and at least a part of the chromium atoms become hexavalent and are fixed in a chromate ester structure (see VJ Ruddic et al.; J. Phys. Chem. Vol. 100, p. 11062 (1996); SM Augustin et al.; J. Catal. Vol. 161, p. 641 (1996)). The chromium compound C1 and the chromium compound C2 may be the same or different. Moreover, chromium compound D and chromium compound E may be the same or different.

[0041] In step (III), the following methods can be used. Suitable examples include a method of impregnating the inorganic oxide particles B2 with a chromium compound E solution and then distilling off the solvent, and a method of sublimating the chromium compound E without using a solvent. Other known methods can also be used. The supporting method is appropriately selected depending on the type of chromium compound E used. Furthermore, during the production of the inorganic oxide particles B2, a raw material to which the chromium compound E has been added beforehand may be used, thereby directly obtaining the inorganic oxide particles B2 carrying the chromium compound E.

[0042] In the step (III), inorganic oxide particles B2 supporting a chromium compound E containing 0.01 to 2.0% by weight of chromium atoms may be obtained. The content of chromium atoms in the chromium catalyst A2 is not particularly limited, but from the viewpoint of preventing the supported chromium atoms from agglomerating with each other and being efficiently activated, the content is preferably 0.01 to 2.0% by weight, more preferably 0.1 to 2.0% by weight, and even more preferably 0.2 to 1.5% by weight.

[0043] In step (IV), the inorganic oxide particles B2 carrying the chromium compound E obtained in step (III) are fired in an activation furnace to activate the inorganic oxide particles B2. The activation is carried out in a non-reducing atmosphere that is substantially free of moisture. For example, the activation is carried out in oxygen or air, but an inert gas may also be present. Preferably, the activation is carried out under a fluidized state using air that has been sufficiently dried by passing molecular sieves or the like through the air. The activation temperature is not particularly limited. The activation temperature is 400°C to 900°C, preferably 430°C to 900°C, and more preferably 450°C to 850°C. The activation time is not particularly limited. The activation time is preferably 30 minutes to 48 hours, more preferably 1 hour to 35 hours, and even more preferably 2 hours to 30 hours. If the activation is performed at a temperature lower than 400°C, the polymerization activity decreases, and the molecular weight distribution of the obtained polymer becomes broad, so that the durability improves but the impact resistance decreases. If the activation is performed at a temperature higher than 800°C, the molecular weight distribution of the obtained polymer becomes narrow, so that the impact resistance improves but the durability decreases. Furthermore, if the activation is performed at a temperature higher than 900°C, sintering occurs and the activity decreases. By the activation, at least a part of the chromium atoms of the chromium compound E supported on the inorganic oxide particles B2 is oxidized to hexavalent, and as described above, the chromium compound C2 is chemically fixed on the inorganic oxide particles B2.

[0044] During the supporting or activation of the chromium compound E, a known method for adjusting the ethylene polymerization activity or the molecular weight and molecular weight distribution of the obtained ethylene polymer by adding a fluorine compound such as ammonium silicofluoride or ammonium hydrogen difluoride, a titanium alkoxide such as titanium tetraisopropoxide, a zirconium alkoxide such as zirconium tetrabutoxide, an aluminum alkoxide such as aluminum tributoxide, an organoaluminum such as trialkylaluminum, an organomagnesium such as dialkylmagnesium, or a metal alkoxide, or an organometallic compound, may be used in combination. In these metal alkoxides or organometallic compounds, the organic group portion is burned by activation in a non-reducing atmosphere, and is oxidized to a metal oxide such as titania, zirconia, alumina or magnesia, which is contained in the catalyst. In addition, the fluorine compound is thermally decomposed during activation to fluorinate the inorganic oxide support. These methods are described in outline or detail in documents such as CE Marsden; Plastics, Rubber and Composites Processing and Applications Vol. 21 p. 193 (1994), T. Pullukat et al.; J. Polym. Sci., Polym. Chem. Ed. Vol. 82 p. 118 (1980), and MP McDaniel et al.; J. Catal. Vol. 82 p. 118 (1983).

[0045] In step (IV), it is preferable that 50% or more of the chromium atoms contained in the inorganic oxide particles B2 supporting the chromium compound E are oxidized to a hexavalent state. More preferably, 60% or more of the chromium atoms contained in the inorganic oxide particles B2 supporting the chromium compound E are oxidized to a hexavalent state. The upper limit of the chromium atoms oxidized to a hexavalent state is 100%. The ratio of the chromium atoms oxidized to a hexavalent state is adjusted by the activation temperature and time. The total amount of chromium atoms can be measured by a general metal analysis method, such as plasma emission spectrometry or X-ray fluorescence spectrometry. The valence of chromium can be roughly known by visually observing the color change of the solid product (generally, hexavalent chromium is yellow to orange, trivalent chromium is green, and divalent chromium is blue), but for quantitative analysis, chelate titration and absorptiometry are known as simple methods. Specifically, it is described in "Experimental Chemistry Lecture 15 Analysis" edited by the Chemical Society of Japan, Maruzen (1991), pp. 246-248. For example, trivalent chromium can be quantitatively determined by adding an excess of EDTA (ethylenediaminetetraacetic acid) of a known concentration to trivalent chromium in an acidic solution, boiling for 5-10 minutes, and titrating with a standard solution of trivalent iron. Also, in the case of hexavalent chromium, CrO4 2- Quantitation is possible by measuring the absorbance at a wavelength of 366 nm, taking advantage of the fact that it exists as such.

[0046] 4.3 Method for producing chromium catalyst A3 In the method for producing an ethylene-based polymerization catalyst, when the ethylene-based polymerization catalyst component contains inorganic oxide particles B1 and inorganic oxide particles B2 (mixed carrier), the following production method is used (the ethylene-based polymerization catalyst produced by this production method is a mixture of chromium catalyst A1 and chromium catalyst A2, which is referred to as chromium catalyst A3). The method for producing the chromium catalyst A3 includes a step (V) of supporting a chromium compound D on inorganic oxide particles B1, B2, and a step (VI) of calcining and activating the inorganic oxide particles B1, B2 supporting the chromium compound D obtained in the step (V) at 400°C to 900°C in a non-reducing atmosphere to convert at least a portion of the chromium atoms to hexavalent chromium. Step (V) is the same as step (I) already described, and step (VI) is the same as step (II) already described, so duplicate descriptions will be omitted.

[0047] The chromium catalyst A3 may be produced by mixing inorganic oxide particles B1 and B2 in advance, granulating the inorganic oxide particles B3, supporting the chromium compound D on the inorganic oxide particles B3, and activating the inorganic oxide particles B3 by calcination at 400° C. to 900° C. in a non-reducing atmosphere to convert at least some of the chromium atoms to hexavalent chromium. In this case, the chromium catalyst A3 produced has the chromium compound C1 supported on the inorganic oxide particles B1 and the chromium compound C1 supported on the inorganic oxide particles B2, and the chromium catalyst A3 is ultimately composed of combined particles in which the contact portions of the particles of the chromium catalyst A1 and the particles of the chromium catalyst A2 are combined. The chromium catalyst A3 may be in a form in which the chromium compound C1 is supported on inorganic oxide particles B3 obtained by granulating inorganic oxide particles B1 and inorganic oxide particles B2. In this case, in the produced chromium catalyst A3, the chromium compound C1 is supported on the inorganic oxide particles B1 and the chromium compound C1 is supported on the inorganic oxide particles B2, and ultimately, this chromium catalyst A3 is composed of combined particles in which particles of the chromium catalyst A1 and particles of the chromium catalyst A2 are combined. This ethylene-based polymerization catalyst (chromium catalyst A3) can be produced by a production method in which inorganic oxide particles B1, including plate-like and aggregates thereof, and amorphous inorganic oxide particles B2 are granulated to form inorganic oxide particles B3, and a chromium compound C1 is supported on the inorganic oxide particles B3. The method of granulating to obtain the inorganic oxide particles B3 can be a known granulation method, for example, stirring granulation method, spray granulation method, rolling granulation method, and fluidized bed granulation method. Among these, spray granulation method is preferred from the viewpoint of easily maintaining the properties of the particles before mixing. When spray granulation is performed, the dispersion medium for the raw material slurry can be an organic solvent such as water, methanol, ethanol, chloroform, methylene chloride, pentane, hexane, heptane, toluene, or xylene, preferably water. During granulation, known binders such as organic substances, inorganic solvents, and inorganic salts may be used. In the case of spray granulation, the concentration of inorganic oxide particles (total of B1 and B2) in the raw material slurry is 0.1 to 70% by weight, preferably 1 to 50% by weight. The inlet temperature of the hot air for spray granulation varies depending on the dispersion medium, but for example, water is 80 to 260°C, preferably 100 to 220°C. The mixing ratio of the plate-like inorganic oxide particles B1 and the amorphous inorganic oxide particles B2 is preferably 1:99 to 99:1, more preferably 5:95 to 95:5, and even more preferably 10:90 to 90:10, by weight. The surface area of ​​the chromium catalyst A3 is not particularly limited, but is usually 10 m 2 / g or more 1000m 2 / g or less, and 2 / g or more 950m 2 / g or less, and 2 / g or more 900m 2 It is more preferable that the molecular weight is not more than 1 / g. The pore volume of the chromium catalyst A3 is not particularly limited, but is usually from 0.05 to 5.0 mL / g, preferably from 0.1 to 3.0 mL / g, and more preferably from 0.1 to 2.5 mL / g. The average particle size of the particles of chromium catalyst A3 is not particularly limited, but from the viewpoint of handling, the average particle size is preferably 0.1 μm or more and 200 μm or less, more preferably 0.2 μm or more and 150 μm or less, and even more preferably 0.5 μm or more and 100 μm or less.

[0048] 5.Characteristics of Ethylene Polymerization Catalysts (1) Ethylene-based polymerization catalyst In the present invention, in producing an ethylene-based polymer, the chromium catalyst A1 may be used alone as an ethylene-based polymerization catalyst, or the chromium catalyst A3 (chromium catalysts A1 and A2) may be used. When the chromium catalyst A1 and the chromium catalyst A2 are used in combination, any of the following methods (a) to (d) may be used. (a) A method in which two types of catalysts are mixed and then activated in an activation furnace, and the extracted mixed catalyst is introduced into a polymerization reactor in the presence or absence of a solvent or in the presence or absence of an organometallic compound. (b) A method in which two types of catalysts are activated separately in an activation furnace, and the extracted catalysts are mixed in advance in the presence or absence of a solvent or in the presence or absence of an organometallic compound, and then introduced into a polymerization reactor. (c) A method in which two types of catalysts are activated separately in an activation furnace, and each of the extracted catalysts is introduced separately into a polymerization reactor in the presence or absence of a solvent or in the presence or absence of an organometallic compound, and then the catalysts are mixed in one polymerization reactor. (d) A method in which inorganic oxide particles B1 and inorganic oxide particles B2 are mixed in advance, then granulated to form inorganic oxide particles B3 (mixed support), which are supported with a chromium compound (chromium compound D or chromium compound E) and activated in an activation furnace, and the extracted mixed catalyst is introduced into a polymerization reactor in the presence or absence of a solvent or in the presence or absence of an organometallic compound.

[0049] (2) Mixing ratio of chromium catalysts A1 and A2 in ethylene polymerization catalysts containing chromium catalyst A3 (chromium catalysts A1 and A2) When the ethylene-based polymerization catalyst contains the chromium catalyst A3, i.e., contains the chromium catalyst A1 and the chromium catalyst A2, the mixing ratio of the chromium catalyst A1 to the chromium catalyst A2 is not particularly limited. The mixing ratio of the chromium catalyst A1 to the chromium catalyst A2 is preferably 1:99 to 99:1, more preferably 5:95 to 95:5, and further preferably 10:90 to 90:10 by weight.

[0050] (3) Chromium atom content in ethylene polymerization catalysts The content of chromium atoms in the ethylene polymerization catalyst is not particularly limited. From the viewpoint of preventing aggregation of the supported chromium atoms with each other and efficient activation, the content of chromium atoms is preferably 0.01% by weight to 2.0% by weight, more preferably 0.1% by weight to 2.0% by weight, and further preferably 0.2% by weight to 1.5% by weight.

[0051] (4) Components other than chromium catalysts A1 and A2 in ethylene polymerization catalysts The ethylene polymerization catalyst may contain components other than the chromium catalysts A1 and A2, so long as they do not impair the effects of the present invention. The other components are not particularly limited, and the content (wt%) of the other components is preferably 5 wt% or less.

[0052] 6. Method for producing ethylene polymer In the process for producing an ethylene-based polymer of the present invention, a monomer containing at least ethylene is polymerized using the above-mentioned ethylene-based polymerization catalyst.

[0053] (1) Polymerization method The process for producing the ethylene polymer of the present invention can be carried out by a liquid phase polymerization method such as slurry polymerization or solution polymerization, or a gas phase polymerization method. The liquid phase polymerization method is usually carried out in a hydrocarbon solvent, such as propane, n-butane, isobutane, n-pentane, isopentane, hexane, heptane, octane, decane, cyclohexane, benzene, toluene, xylene, or a mixture of such inert hydrocarbons. In the gas phase polymerization method, a commonly known polymerization method such as a fluidized bed or a stirred bed can be used in the presence of an inert gas. In the gas phase polymerization method, a so-called condensing mode can be used in which a medium for removing polymerization heat is optionally used. As a polymerization method, not only single-stage polymerization in which an ethylene polymer is produced using one reactor, but also multi-stage polymerization can be carried out by connecting at least two reactors. In the case of multi-stage polymerization, two reactors are connected, and a reaction mixture obtained by polymerization in the first reactor is then continuously fed to the second reactor, in a two-stage polymerization method. The transfer from the first reactor to the second reactor is carried out through a connecting pipe. This transfer is preferably carried out by utilizing the pressure difference caused by the continuous discharge of the polymerization reaction mixture from the second reactor.

[0054] (2) Polymerization conditions The polymerization temperature in the liquid phase or gas phase polymerization method is generally 0°C to 300°C, practically 20°C to 200°C, preferably 50°C to 180°C, and more preferably 70°C to 150°C. The catalyst concentration and ethylene concentration in the reactor may be any concentration sufficient to proceed with the polymerization. For example, the catalyst concentration may be in the range of about 0.0001% by weight to about 5% by weight based on the weight of the reactor contents in the case of liquid phase polymerization. Similarly, the ethylene concentration may be in the range of 0.1 MPa to 10 MPa in terms of total pressure in the case of gas phase polymerization. If necessary, hydrogen can be introduced into the polymerization reactor to adjust the molecular weight.

[0055] (3) Copolymerization In the method for producing an ethylene-based polymer of the present invention, in addition to ethylene homopolymerization, if necessary, α-olefins such as propylene, 1-butene, 1-pentene, 1-hexene, 4-methyl-1-pentene, 1-octene, etc. can be introduced alone or in combination with one or more kinds thereof into a polymerization reactor to be copolymerized. The α-olefin content in the resulting ethylene copolymer is desirably 15 mol % or less, preferably 10 mol % or less.

[0056] (4) Organometallic compounds During the polymerization, an organometallic compound may be introduced as a co-catalyst and brought into contact with the ethylene-based polymerization catalyst for the purpose of finely adjusting the molecular weight or molecular weight distribution of the ethylene-based polymer or for the purpose of removing impurities in the polymerization system as a scavenger. In particular, organometallic compounds have the effect of improving the catalytic activity of ethylene-based polymerization catalysts and the effect of making hydrogen more effective as a molecular weight regulator. As the organometallic compound, organometallic compounds of Groups 1, 2, and 13 of the periodic table, specifically organolithium compounds, organomagnesium compounds, organoaluminum compounds, and organoboron compounds are preferably used, with organoaluminum compounds and organoboron compounds being more preferred.

[0057] The organolithium compound includes alkyllithium, specifically, methyllithium, n-butyllithium, and the like. The organic magnesium compound includes dialkyl magnesium, specifically, butylethyl magnesium, and dibutyl magnesium. The organoaluminum compound includes trialkylaluminum and dialkylaluminum alkoxides, specifically, trimethylaluminum, triethylaluminum, triisobutylaluminum, and diethylaluminum ethoxide. The organoboron compound includes trialkylboranes, specifically triethylborane. The amount of the organometallic compound to be contacted is such that the molar ratio of metal atoms to chromium atoms is 0.2-1000, preferably 0.5-100.

[0058] The resulting ethylene-based polymer is then preferably kneaded. Kneading can be performed using a single-screw or twin-screw extruder or a continuous kneader. The resulting ethylene-based polymer can then be molded, such as by blow molding, by a conventional method.

[0059] 7. Effects of the Present Embodiment According to the ethylene-based polymerization catalyst component, the method for producing an ethylene-based polymer catalyst, and the method for producing an ethylene-based polymer of the present embodiment, it becomes possible to design an HDPE material (high density polyethylene material) having an excellent balance between durability and fluidity. EXAMPLES

[0060] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited to these examples as long as they do not deviate from the gist of the invention.

[0061] 1. Measurement methods for physical properties The methods for measuring physical properties used in the examples and comparative examples are as follows. (1) Measurement of peak intensity in the infrared spectrum of inorganic oxide particles B1 (infrared spectroscopy) In a glove box filled with high-purity argon, the inorganic oxide was loaded into a sample holder for diffuse reflectance IR, and the sample surface was smoothed.Then, the sample was sealed with a lid with a window and placed in an IR measurement device for measurement. The measurement conditions are as follows. Equipment: JASCO FT / IR-6600 Detector: TGS Photometry method: Diffuse reflection method Wavelength range: 1000~4000cm -1 Resolution: 4cm -1 Number of measurements: 512 Atmosphere: Argon (2) Powder X-ray diffraction (XRD): Powder X-ray diffraction was measured using the following apparatus and conditions. Equipment: Rigaku X-ray Diffractometer Smartlab X-ray source: Cu-Kα ray (using Kβ absorber plate), tube voltage 40 kV, tube current 30 mA Optical system: Concentration method Divergence slit 2 / 3 degrees, scattering slit 2 / 3 degrees, receiving slit 0.300mm Scan mode: 2θ / θ scan 2θ scan range: 3.0000~55.0000 degrees Angle step size: 0.0200 degrees Scan speed: 4.0000 degrees / min Detector: Scintillation counter (3) Surface area and pore volume Each silica sample was heated and thoroughly dried under reduced pressure, and then the nitrogen adsorption isotherm was measured at liquid temperature using a Quantorchrome Autosorb 3B. The pore volume was calculated from the amount of adsorption at a relative pressure of 0.95 on the resulting adsorption isotherm, and the specific surface area was calculated by multipoint BET analysis. Furthermore, by assuming the pore structure to be cylindrical, the average pore diameter was calculated according to formula (1). From this formula, D ave is the average pore diameter, V total is the pore volume, S BET indicates the specific surface area measured by the BET multipoint method. D ave =4V total / S BET Formula (1) Furthermore, the mesopore distribution was obtained by BJH analysis, and the pore volume within the specified range was calculated. (4) SEM Observation: SEM observation was carried out using the following equipment and conditions. Equipment: Hitachi FE-SEM Voltage applied: 1kV Device magnification: 20k WD: 4mm (5) HLMI: Measured in accordance with ASTM-D-1238-57T at 190°C and a load of 21.6 kg. (6) Hexavalent chromium content: An aqueous NaOH solution (0.1 M) was added to the catalyst component to dissolve the hexavalent chromium, and a portion of the solution was taken and the absorbance at a wavelength of 366 nm was measured to determine the amount of hexavalent chromium. (7) Average particle size: Measurements were performed using a laser diffraction / scattering particle size distribution analyzer LA-920 manufactured by Horiba, Ltd., under the conditions of ethanol as the dispersion solvent, a refractive index of 1.0, and a shape factor of 1.0, and the median diameter was taken as the average particle size.

[0062] 2. Examples and Comparative Examples (1) Example 1 (1.1) Infrared spectrum of inorganic oxide particle B1 The infrared spectrum of “Sun Lovely” (manufactured by AGC Si-Tech Co., Ltd.), which is inorganic oxide particle B1, is shown by a solid line in FIG. 1. As shown in Table 1, in this infrared spectrum, the maximum peak in the range X is 3661 cm -1 The peak intensity Px was 1.32. The maximum peak in range Y was 3746 cm -1 The peak intensity Py was 0.88. The peak intensity ratio Py / Px was 0.67. (1.2) Structural analysis data of inorganic oxide particle B1 The structural analysis data of the inorganic oxide particles B1 is as follows. <Structural analysis data of inorganic oxide particle B1> XRD: Peak at 2θ=25.8°, half-width 1.5° BET method: Surface area 84m 2 / g Pore ​​volume: 0.2mL / g SiO2 purity: 99.5% (weight basis) (1.3) Preparation of chromium catalyst A1 After impregnating inorganic oxide particles B1 with an aqueous solution of chromium acetate, water was distilled off to obtain chromium-containing silica with a chromium content of 0.5% by weight. The chromium-containing silica was then activated under dry air atmosphere at 600°C for 20 hours to obtain chromium catalyst A1 (Phillips type catalyst). Upon activation, the chromium-containing silica changed color from light blue to light orange. This indicates that the chromium atoms were converted to hexavalent chromium. Substantially 99% by weight of trivalent chromium was converted to hexavalent chromium.

[0063] (1.4) Physical properties of chromium catalyst A1 The XRD peak position of chromium catalyst A1 hardly changed between inorganic oxide particles B1 (raw material) dried at 200°C and chromium catalyst A1 supported with chromium acetate and activated at 600°C. This means that inorganic oxide particles B1 have good thermal stability. The SEM image of chromium catalyst A1 is shown in Figure 3.

[0064] (1.5) Ethylene Polymerization Into a 1.5 L polymerization vessel that had been thoroughly purged with nitrogen, 185 mg of chromium catalyst A1 and 700 mL of isobutane were placed, and the internal temperature was raised to 100°C. Then, ethylene was injected, and polymerization was carried out at a polymerization temperature of 100°C for 120 minutes while maintaining the ethylene partial pressure at 1.4MPa. The polymerization was then terminated by releasing the content gas to the outside of the system. As a result, 21 g of an ethylene-based polymer was obtained. The HLMI of the obtained ethylene-based polymer was that the polymer did not flow. Therefore, it was judged to be less than 0.01 g / 10 min. The density was 0.9520 g / cm 3 It was.

[0065] (2) Example 2 (2.1.1) Preparation of chromium catalyst A1 Prepared as in Example 1. (2.1.2) Preparation of chromium catalyst A2 Inorganic oxide particles B2 (amorphous silica aggregates) were impregnated with an aqueous solution of chromium acetate, and then the water was removed to obtain chromium-containing silica with a chromium content of 1.0% by weight. The chromium-containing silica was then activated under dry air at 820°C for 18 hours to obtain chromium catalyst A2 (Phillips type catalyst). Upon activation, the chromium-containing silica changed color from light blue to light orange. This indicates that the chromium atoms were converted to hexavalent chromium. Substantially 99% by weight of trivalent chromium was converted to hexavalent chromium. The infrared spectrum of inorganic oxide particle B2 is as described later in the section "(3.1) Infrared spectrum of inorganic oxide particle B2". The structural analysis data of inorganic oxide particle B2 is as described later in the section "(3.2) Structural analysis data of inorganic oxide particle B2".

[0066] (2.2) Ethylene Polymerization Into a 1.5 L polymerization vessel that had been thoroughly purged with nitrogen, 152 mg of chromium catalyst A1, 39 mg of chromium catalyst A2, and 700 mL of isobutane were placed, and the internal temperature was raised to 100°C. Then, ethylene was injected, and polymerization was carried out for 120 minutes at a polymerization temperature of 100° C. while maintaining the ethylene partial pressure at 1.4 MPa. The polymerization was then terminated by discharging the content gas to the outside of the system. As a result, 200 g of an ethylene-based polymer was obtained. The HLMI of the obtained ethylene-based polymer was 5.1 g / 10 min, and the density was 0.9577 g / cm 3 It was.

[0067] (3) Comparative Example 1 (3.1) Infrared spectrum of inorganic oxide particle B2 The infrared spectrum of inorganic oxide particle B2 is shown by the dashed line in FIG. 1. As shown in Table 1, in this infrared spectrum, the maximum peak in range X is 3697 cm -1 The peak intensity Px was 0.42. The maximum peak in range Y was 3747 cm -1 The peak intensity Py was 5.82. The peak intensity ratio Py / Px was 13.86. (3.2) Structural analysis data of inorganic oxide particle B2 The structural analysis data of the inorganic oxide particles B2 is as follows. <Structural analysis data of inorganic oxide particle 2> XRD: A broad peak characteristic of amorphous material at around 2θ=22° BET method: Surface area 310m 2 / g Pore ​​volume: 1.7mL / g SiO2 purity: 99.8% (weight basis) (3.3) Preparation of chromium catalyst A2 Prepared as in Example 2.

[0068] (3.4) Ethylene Polymerization Into a 1.5 L polymerization vessel that had been thoroughly purged with nitrogen, 29 mg of chromium catalyst A2 and 700 mL of isobutane were placed, and the internal temperature was raised to 100°C. Then, ethylene was injected, and polymerization was carried out for 120 minutes at a polymerization temperature of 100° C. while maintaining the ethylene partial pressure at 1.4 MPa. Then, the polymerization was terminated by discharging the content gas to the outside of the system. As a result, 149 g of an ethylene-based polymer was obtained. The HLMI of the obtained ethylene-based polymer was 9.8 g / 10 min, and the density was 0.9582 g / cm 3 It was.

[0069] (4) Example 3 (4.1) Preparation of chromium catalyst A3 Inorganic oxide particles B2-2 (amorphous silica aggregates, 40 g, average particle size 12 μm) and inorganic oxide particles B1 (120 g, average particle size 4.3 μm) used in Example 1 were slurried in 340 mL of distilled water. This slurry was spray-dried and granulated using a spray-drying granulation device (Okawahara Kakoki Co., Ltd. "L-8") under the following conditions. Atomizer type: M type rotary disc Atomizer rotation speed: 10,000 rpm Slurry supply rate: 1.0L / h Inlet temperature: 150℃ As a result of the granulation, inorganic oxide particles B3 having an average particle size of 37.5 μm were collected from the bottom of the main body. The inorganic oxide particles B3 obtained were impregnated with an aqueous solution of chromium acetate, and the water was then distilled off to obtain chromium-containing silica with a chromium content of 0.5% by weight. The chromium-containing silica was then activated under dry air at 730°C for 12 hours to obtain chromium catalyst A3 (Phillips type catalyst). Upon activation, the chromium-containing silica changed color from light blue to light orange. This indicates that the chromium atoms were converted to hexavalent chromium. Substantially 99% by weight of the trivalent chromium was converted to hexavalent chromium. <Structural analysis data of inorganic oxide particle B2-2> XRD: A broad peak characteristic of amorphous material at around 2θ=22° BET method: Surface area 320m 2 / g Pore ​​volume: 1.6mL / g SiO2 purity: 99.8% (weight basis) Average particle size: 12μm (4.2) Ethylene Polymerization Into a 2.0 L polymerization vessel thoroughly purged with nitrogen, 130 mg of chromium catalyst A3 obtained in Example 3 (4.1) and 800 mL of isobutane were placed, and the internal temperature was raised to 100°C. Then, ethylene was injected, and polymerization was carried out for 200 minutes at a polymerization temperature of 100° C. while maintaining the ethylene partial pressure at 1.4 MPa. Then, the polymerization was terminated by discharging the content gas to the outside of the system. As a result, 340 g of an ethylene-based polymer was obtained. The HLMI of the obtained ethylene-based polymer was 1.0 g / 10 min, and the density was 0.9522 g / cm 3 It was. (5) Comparative Example 2 (5.1) Preparation of chromium catalyst A4 The inorganic oxide particles B2-2 (amorphous silica aggregates, 100 g, average particle size 12 μm) of Example 3 were slurried in 400 mL of distilled water. This slurry was spray-dried and granulated in the same manner as in Example 3 (4.1) using a spray-drying granulator (Okawahara Kakoki Co., Ltd. "L-8") to obtain granules of inorganic oxide particles B2-2 with an average particle size of 98.2 μm. The obtained inorganic oxide particle B2-2 granules were impregnated with an aqueous solution of chromium acetate, and then the water was distilled off to obtain chromium-containing silica with a chromium content of 0.5% by weight. The chromium-containing silica was then activated under dry air atmosphere at 730°C for 12 hours to obtain chromium catalyst A4 (Phillips type catalyst). Upon activation, the chromium-containing silica changed color from light blue to light orange. This indicates that the chromium atoms were converted to hexavalent chromium. Substantially 99% by weight of trivalent chromium was converted to hexavalent chromium. (5.2) Ethylene Polymerization Into a 2.0 L polymerization vessel thoroughly purged with nitrogen, 60 mg of chromium catalyst A4 obtained in Comparative Example 2 (5.1) and 800 mL of isobutane were placed, and the internal temperature was raised to 100°C. Ethylene was then injected, and polymerization was carried out for 60 minutes at a polymerization temperature of 100°C while maintaining the ethylene partial pressure at 1.4MPa. The polymerization was then terminated by discharging the content gas outside the system. As a result, 170g of an ethylene-based polymer was obtained. The HLMI of the obtained ethylene-based polymer was 2.5g / 10min, and the density was 0.9562g / cm 3 It was.

[0070] 3. Discussion of the Results of Examples and Comparative Examples The results of the Examples and Comparative Examples are shown in Tables 1 and 2. Note that the polymer densities in Table 2 are values ​​rounded off to the fourth decimal place.

[0071] As shown in Table 2, a comparison between Example 1 and Comparative Example 1 shows that an ethylene-based polymer having a high molecular weight can be obtained by using chromium catalyst A1, which is a carrier made of an inorganic oxide having a Px / Py of less than 10. A comparison between Example 2 and Comparative Example 1 shows that a mixture of chromium catalyst A1 and chromium catalyst A2 can be used to obtain an ethylene-based polymer having a higher molecular weight than an ethylene-based polymer obtained from chromium catalyst A2 alone. In addition, Example 2 has a lower HLMI (higher PE molecular weight) than Comparative Example 1, but the density is the same. This is a preferable balance of physical properties for blowing materials. A comparison between Example 3 and Comparative Example 2 shows that a ethylene-based polymer having a higher molecular weight can be obtained from chromium catalyst A3, which uses a carrier made by mixing and granulating inorganic oxide particles B1, which are plate-like silica aggregates, and inorganic oxide particles B2-2, which are amorphous silica aggregates, compared to a carrier made by granulating inorganic oxide particles B2-2, which are amorphous silica aggregates, alone. From the above results, it was confirmed that an ethylene-based polymer having an ultrahigh molecular weight component can be produced by using an ethylene-based polymerization catalyst containing plate-like silica aggregates (planar silica aggregates) having a peak intensity ratio Py / Px of less than 10 and containing 90% by weight or more of SiO2.

[0072] [Table 1]

[0073] [Table 2]

[0074] The present invention is not limited to the above-described embodiments, and various modifications and variations are possible within the scope of the claims of the present invention. [Industrial Applicability]

[0075] According to the present invention, an ethylene polymer having an ultra-high molecular weight component can be produced. This ethylene polymer can be used in a wide range of applications, and is therefore of great industrial utility.

Claims

1. The sample was calcined at 600° C. for 24 hours as a pretreatment for the analysis, and then the measurement was performed. The sample contained a plate-like inorganic oxide having the following properties 1 and 2: The ethylene polymerization catalyst component, wherein the inorganic oxide is Sunlovely (a trade name of AGC Si-Tech Co., Ltd.). Characteristic 1: In the infrared spectrum, 3600 cm -1 ~3699cm -1 3700 cm for the peak intensity Px that is maximum in the range X -1 ~3799cm -1 The ratio Py / Px of the maximum peak intensity Py in the range Y is less than 10. Characteristic 2: SiO 2 Contains 90% by weight or more.

2. The ethylene-based polymerization catalyst component according to claim 1, characterized in that the inorganic oxide has a peak showing crystallinity with a half-width of 0.2° or more and 5° or less at 2θ=23° to 29° in powder X-ray diffraction.

3. A step (I) of supporting a chromium compound on the ethylene-based polymerization catalyst component according to claim 1 or 2; A step (II) of calcining and activating the chromium compound-supported component obtained in the step (I) at 400° C. to 900° C. in a non-reducing atmosphere to convert at least a part of the chromium atoms into hexavalent chromium atoms; 2. A method for producing an ethylene polymerization catalyst comprising the steps of:

4. 4. The method for producing an ethylene polymerization catalyst according to claim 3, wherein the chromium compound-supported component obtained in the step (I) contains 0.01% by weight to 2.0% by weight of chromium atoms.

5. 5. The method for producing an ethylene-based polymerization catalyst according to claim 3, wherein in the step (II), 50% or more of chromium atoms contained in the chromium compound-supported component are oxidized to hexavalent chromium atoms.

6. A method for producing an ethylene-based polymer, comprising polymerizing a monomer containing at least ethylene by using an ethylene-based polymerization catalyst obtained by the method for producing an ethylene-based polymer according to any one of claims 3 to 5.

Citation Information

Patent Citations

  • Electrophotographic receptor

    JP1983021746A

  • Catalytic composition for accelerating 1-olefin polymerization

    JP1983063704A

  • Ethylenic polymer and method for producing the same

    JP2002080521A

  • Improved chromate ester catalyst and method for producing high performance polyethylene products using same

    JP2002533536A

  • Olefin polymerization catalyst and method for producing olefin polymer by using the catalyst