Polyvinyl chloride resin molded body, method for producing polyvinyl chloride resin molded body, interior material and transport equipment
By integrating a molybdenum compound with zeolite and antioxidants in specific ratios, the vinyl chloride resin composition is stabilized during extrusion, ensuring continuous production of flame-retardant and low-smoke materials for transportation equipment.
Patent Information
- Application Number
- JP2020062020
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-03-31
- Publication Date
- 2024-10-02
- Estimated Expiration
- 2040-03-31
AI Technical Summary
Existing vinyl chloride resin compositions containing molybdenum compounds face issues with thermal decomposition during extrusion molding, leading to instability and inability to be extruded continuously over a long period, which is critical for applications requiring flame retardancy and smoke suppression, especially in transportation equipment.
Incorporating a molybdenum compound with zeolite and antioxidants into the vinyl chloride resin composition, along with specific content ratios and processing conditions, stabilizes the extrusion process by preventing thermal decomposition, ensuring continuous and stable molding.
The solution achieves excellent flame retardancy and suppresses smoke generation, allowing for the stable extrusion of vinyl chloride resin compositions over extended periods, resulting in high-quality molded articles suitable for transportation equipment.
Smart Images

Figure 0007559341000004 
Figure 0007559341000005 
Figure 0007559341000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a polyvinyl chloride resin molded article, a method for producing a polyvinyl chloride resin molded article, an interior material, and a transport device. [Background technology]
[0002] For example, as shown in Patent Document 1, molded articles (vinyl chloride resin molded articles) obtained by molding a rigid polyvinyl chloride resin composition are used for interior materials of vehicles such as automobiles, buses, and trains, transportation equipment such as ships and aircraft, and buildings.
[0003] Such rigid vinyl chloride resin compositions have excellent processability and the vinyl chloride resin molded articles obtained have excellent impact resistance, chemical resistance, flame retardancy, etc., and therefore are preferably used as the interior materials.
[0004] When such interior materials are applied, particularly to transportation equipment such as aircraft, it is required to impart flame retardancy to the interior materials and suppress smoke generation. In order to achieve these functions, it is known to add a molybdenum-based compound as a flame retardant to the rigid polyvinyl chloride resin composition.
[0005] Moreover, the vinyl chloride resin molded article is produced, for example, by preparing a rigid vinyl chloride resin composition by kneading under heating, and then molding the obtained rigid vinyl chloride resin composition by extrusion molding.
[0006] However, as described above, when a rigid polyvinyl chloride resin composition contains a molybdenum compound, the heat applied during extrusion using an extruder induces thermal decomposition of the polyvinyl chloride resin. As a result, when the rigid polyvinyl chloride resin composition is extruded by extrusion molding, the rigid polyvinyl chloride resin composition cannot be stably extruded from the extruder over a long period of time. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] JP 2006-265373 A Summary of the Invention [Problem to be solved by the invention]
[0008] An object of the present invention is to provide a polyvinyl chloride resin molded article which contains a molybdenum compound and thereby has excellent flame retardancy and suppressed smoke generation; a method for producing a polyvinyl chloride resin molded article which, when molding such a polyvinyl chloride resin molded article by extrusion molding using a polyvinyl chloride resin composition, enables the polyvinyl chloride resin composition to be extruded continuously and stably over a long period of time; and an interior material and a transport device which are provided with such a polyvinyl chloride resin molded article and have excellent flame retardancy. [Means for solving the problem]
[0009] Such objectives are as follows: (14) This is achieved by the present invention described in. (1) a polyvinyl chloride resin; A stabilizer including an organotin compound; A molybdenum compound, Zeolite and, Phenol Antioxidant Agent and , Contains death, The content of the stabilizer is 0.1 parts by weight or more and 10.0 parts by weight or less based on 100 parts by weight of the polyvinyl chloride resin, the content of the molybdenum compound is 1.0 parts by weight or more and 15.0 parts by weight or less based on 100 parts by weight of the polyvinyl chloride resin, The content of the zeolite is 0.1 parts by weight or more and 5.0 parts by weight or less with respect to 100 parts by weight of the polyvinyl chloride resin, The content of the phenol-based antioxidant is 0.1 parts by weight or more and 5.0 parts by weight or less based on 100 parts by weight of the polyvinyl chloride resin. A vinyl chloride resin molded article comprising:
[0011] (2) The zeolite is in particulate form, The average particle size of the zeolite is 5.0 μm or more and 50.0 μm or less. ) The vinyl chloride resin molded article according to claim 1 . (3) A polyvinyl chloride resin, A stabilizer including an organotin compound; A molybdenum compound, Phosphite Antioxidants, Contains The content of the stabilizer is 0.1 parts by weight or more and 10.0 parts by weight or less based on 100 parts by weight of the polyvinyl chloride resin, the content of the molybdenum compound is 1.0 parts by weight or more and 15.0 parts by weight or less based on 100 parts by weight of the polyvinyl chloride resin, The content of the phosphite-based antioxidant is 0.1 parts by weight or more and 5.0 parts by weight or less based on 100 parts by weight of the polyvinyl chloride-based resin. A vinyl chloride resin molded article comprising:
[0014] (4) The molybdenum compound is in particulate form, The molybdenum compound has an average particle size of 1.0 μm or more and 50.0 μm or less. (3) 2. The vinyl chloride resin molded article according to claim 1 .
[0015] (5) The above The polyvinyl chloride resin is selected from the group consisting of chlorinated vinyl chloride resin with a chlorine content of 62.0% or more and 69.0% or less, and vinyl chloride-ethylene copolymer. (4) 2. The vinyl chloride resin molded article according to claim 1 .
[0016] (6) The content of the vinyl chloride-ethylene copolymer is 5.0 parts by weight or more and 50.0 parts by weight or less in 100 parts by weight of the polyvinyl chloride resin. (5) 2. The vinyl chloride resin molded article according to claim 1 .
[0017] (7) The vinyl chloride resin molded article may further include a reinforcing agent, a processing aid, , slip The above (1) to (3) contain at least one of an agent and a pigment. (6) 2. The vinyl chloride resin molded article according to claim 1 .
[0018] (8) The vinyl chloride resin molded article is in the form of a sheet, (7) 2. The vinyl chloride resin molded article according to claim 1 .
[0019] (9)The vinyl chloride resin composition used in obtaining the vinyl chloride resin molded product is kneaded using a roller mixer under conditions of a heating temperature of 190° C. and a mixer rotation speed of 60 rpm, and the thermal decomposition time is defined as the time required for the torque to increase by 20% from the steady state, and the thermal decomposition time is longer than 6.0 minutes. (8) 2. The vinyl chloride resin molded article according to claim 1 .
[0020] (10) Above (1 ) or (2) A method for producing the vinyl chloride resin molded article described above, comprising the steps of: A molybdenum compound and a zeolite are added to the powder containing the polyvinyl chloride resin, and then the mixture is kneaded under heating to prepare a polyvinyl chloride resin composition. A method for producing a vinyl chloride resin molded article, comprising molding the vinyl chloride resin composition by extrusion molding to obtain the vinyl chloride resin molded article.
[0021] (11) The above-mentioned method, wherein the heating temperature when the vinyl chloride resin composition is extruded by an extruder during the extrusion molding is 120° C. or higher and 200° C. or lower. (10) 2. A method for producing a vinyl chloride resin molded article according to claim 1 .
[0022] (12) Above (1) or (9) 13. An interior material comprising the vinyl chloride resin molded article according to any one of claims 1 to 12.
[0023] (13) The interior material is for transportation equipment. (12) The interior material according to claim 1. (14) the above (13) A transportation device comprising the interior material according to claim 1. Effect of the Invention
[0024] According to the present invention, the vinyl chloride resin molded body contains a molybdenum-based compound, so that the vinyl chloride resin molded body has excellent flame retardancy and suppresses smoke generation. In addition, since the vinyl chloride resin molded body further contains at least one of a zeolite and an antioxidant in addition to the molybdenum-based compound, when the vinyl chloride resin molded body is molded by extrusion molding using a vinyl chloride resin composition, the vinyl chloride resin composition can be extruded continuously and stably over a long period of time by appropriately suppressing or preventing the induction of thermal decomposition of the vinyl chloride resin. Therefore, it is possible to stably manufacture the vinyl chloride resin molded body by extrusion molding. [Brief description of the drawings]
[0025] [Figure 1] 1 is a longitudinal sectional view showing an embodiment of a vinyl chloride resin molded article of the present invention. [Diagram 2] FIG. 2 is a side view of a manufacturing apparatus for producing the vinyl chloride resin molded article shown in FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0026] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS The polyvinyl chloride resin molded article, the method for producing the polyvinyl chloride resin molded article, the interior material, and the transport equipment will be described in detail below with reference to preferred embodiments shown in the accompanying drawings.
[0027] <Vinyl chloride resin molded body> The vinyl chloride resin molded article 1 of the present invention is characterized by containing a polyvinyl chloride resin, a molybdenum compound, and at least one of a zeolite and an antioxidant.
[0028] According to the present invention, since the vinyl chloride resin molded body 1 contains a molybdenum compound, it is possible to provide the vinyl chloride resin molded body 1 with excellent flame retardancy and suppressed smoke generation. That is, the vinyl chloride resin molded body 1 is realized in which the smoke generation of the vinyl chloride resin molded body 1 is suppressed and the vinyl chloride resin molded body 1 has excellent flame retardancy.
[0029] Furthermore, since the vinyl chloride resin molded product 1 contains at least one of a zeolite and an antioxidant in addition to the molybdenum compound, when the vinyl chloride resin composition is molded by extrusion molding to produce the vinyl chloride resin molded product 1, the vinyl chloride resin composition can be extruded stably and continuously over a long period of time while adequately suppressing or preventing the induction of thermal decomposition of the vinyl chloride resin. Therefore, the vinyl chloride resin molded product 1 can be stably produced by extrusion molding.
[0030] Hereinafter, the vinyl chloride resin molded body 1 of the present invention will be described as being in the form of a sheet, and an example will be described in which the constituent materials in this embodiment contain polyvinyl chloride resin, a reinforcing agent, a processing aid, a stabilizer, a lubricant, a molybdenum compound as a flame retardant, an antioxidant, zeolite, and a pigment.
[0031] FIG. 1 is a vertical cross-sectional view showing an embodiment of a vinyl chloride resin molded article of the present invention. In FIG. 1, the upper side is also referred to as "upper" or "top", and the lower side is also referred to as "lower" or "bottom".
[0032] <<Polyvinyl chloride resin>> The polyvinyl chloride resin is contained in the polyvinyl chloride resin molded body 1 as its main material.
[0033] Polyvinyl chloride resins are polymers having a plurality of groups represented by -CH-CHCl- as repeating units. Specific examples include homopolymers of vinyl chloride and copolymers of vinyl chloride with vinyl monomers (polymerizable monomers) that can copolymerize with vinyl chloride. Furthermore, homopolymers of vinyl chloride also include post-chlorinated vinyl chloride polymers. One or a combination of two or more of these can be used.
[0034] Examples of copolymers of vinyl chloride with a copolymerizable vinyl monomer include vinyl chloride-vinyl acetate copolymer, vinyl chloride-ethylene copolymer, and vinyl chloride-acrylic copolymer.
[0035] The chlorine content of the homopolymer, i.e., the chlorine concentration rate, is preferably set to 56.0% or more and 69.0% or less, more preferably 62.0% or more and 68.0% or less. This makes it possible to more reliably obtain the effect of suppressing smoke generation and heat generation of the vinyl chloride resin molded body. Furthermore, when the vinyl chloride resin molded body 1 is molded by extrusion molding, the extrudability of the vinyl chloride resin composition is improved, and the vinyl chloride resin molded body 1 can be molded to have a uniform thickness. Therefore, the obtained vinyl chloride resin molded body 1 is molded to have excellent appearance.
[0036] Furthermore, so long as the chlorine content of the homopolymer is set within the above range, the chlorine content, i.e., the degree of chlorination, of each homopolymer in the polyvinyl chloride resin contained in the vinyl chloride resin molded product 1 is not particularly limited, but it is preferable that the homopolymer contains at least one of a vinyl chloride resin having a chlorine content of 56.0% to 57.0% and a chlorinated vinyl chloride resin (post-chlorinated vinyl chloride polymer) having a chlorine content of 62.0% to 69.0%. This allows the chlorine concentration rate of the vinyl chloride resin to be adjusted to within the above range relatively easily.
[0037] The homopolymer preferably has a number-average degree of polymerization of 400 to 1200, and more preferably 600 to 1000. If the number-average degree of polymerization exceeds the upper limit, depending on the combination with other constituent materials, the processability may be poor unless a plasticizer is added, and adding a large amount of plasticizer may result in a decrease in the softening temperature. On the other hand, if the average degree of polymerization is lower than the lower limit, depending on the combination with other constituent materials, the heat resistance of the molded vinyl chloride resin molded product 1 may decrease.
[0038] As described above, such polyvinyl chloride resins include homopolymers of vinyl chloride and copolymers of vinyl monomers (polymerizable monomers) copolymerizable with vinyl chloride, and one or more of these can be used in combination, but among them, a combination of a homopolymer and a copolymer is preferable, and a combination of a chlorinated vinyl chloride resin having a chlorine content of 62.0% to 69.0% as a homopolymer and a vinyl chloride-ethylene copolymer as a copolymer is particularly preferable. This makes it possible to more reliably improve the extrudability of the vinyl chloride resin composition when molding the vinyl chloride resin molded body 1 by extrusion molding, and therefore allows the vinyl chloride resin molded body 1 to be molded to have a more uniform thickness.
[0039] Furthermore, when the polyvinyl chloride resin contains a chlorinated vinyl chloride resin having a chlorine content of 62.0% to 69.0% and a vinyl chloride-ethylene copolymer, the content of the vinyl chloride-ethylene copolymer is preferably 5.0 to 50.0 parts by weight, more preferably 15.0 to 30.0 parts by weight, per 100 parts by weight of the polyvinyl chloride resin, which allows the effect obtained by combining a chlorinated vinyl chloride resin having a chlorine content of 62.0% to 69.0% with a vinyl chloride-ethylene copolymer to be more significantly exhibited.
[0040] <<Reinforcing agent>> The reinforcing agent is contained in the vinyl chloride resin molded body 1 mainly for the purpose of improving the impact resistance of the vinyl chloride resin molded body 1, and further for the purpose of improving the moldability of the vinyl chloride resin molded body 1 during molding.
[0041] Examples of the reinforcing agent include chlorinated polyethylene, ethylene-vinyl acetate copolymer, and multicomponent acrylic rubber resin, among which multicomponent acrylic rubber resin is preferably used, which can provide the vinyl chloride resin molded body 1 with superior durability.
[0042] Multicomponent acrylic rubber-based resins (acrylic polymers) are copolymers of acrylic acid esters, such as methyl acrylate, ethyl acrylate, butyl acrylate, and octyl acrylate, as the main component, with these monomers and 2-chloroethyl vinyl ether, methyl vinyl ketone, acrylic acid, styrene, acrylonitrile, butadiene, and the like, and examples thereof include "Kane Ace FM" manufactured by Kaneka Corporation and "Kureha KM-334" manufactured by Kureha Chemical Industry Co., Ltd.
[0043] The weight average molecular weight of the multi-component acrylic rubber resin is 1.0×10 5 Above 1.0×10 7 Preferably, it is less than 1.0×10 6 Above 7.0×10 6 More preferably, it is:
[0044] The content of the multi-component acrylic rubber resin is preferably 5.0 parts by weight or more and 20.0 parts by weight or less, and more preferably 7.0 parts by weight or more and 14.0 parts by weight or less, relative to 100 parts by weight of the polyvinyl chloride resin which is the main material. This can reliably increase the impact resistance of the polyvinyl chloride resin molded product 1.
[0045] The addition of a reinforcing agent to the vinyl chloride resin molded article 1 may be omitted depending on the impact resistance required for the interior material to which the vinyl chloride resin molded article 1 is applied.
[0046] <<Processing aids>> The processing aid is contained in the vinyl chloride resin molded article 1 in order to improve the moldability of the vinyl chloride resin molded article 1 when it is molded.
[0047] As this processing aid, for example, an acrylic processing aid is used. Specific examples include high molecular weight copolymers of acrylic esters, such as 2-ethylhexyl acrylate-butyl acrylate copolymer, and copolymers of methyl methacrylate and acrylic esters.
[0048] The weight average molecular weight of the processing aid is 1.0×10 5 Above 5.0×10 6 Preferably, it is less than 1.0×10 6 Above 2.0×10 6 Preferably, it is:
[0049] The content of the processing aid is preferably 1.0 to 15.0 parts by weight, more preferably 2.0 to 10.0 parts by weight, based on 100 parts by weight of the polyvinyl chloride resin, which is the main material, which ensures improved moldability during molding of the polyvinyl chloride resin molded article 1.
[0050] The addition of the processing aid to the vinyl chloride resin molded article 1 may be omitted depending on the combination of the constituent materials contained in the vinyl chloride resin molded article 1, etc.
[0051] <<Stabilizer>> The stabilizer is contained in the vinyl chloride resin molded article 1 in order to suppress decomposition and coloring of the vinyl chloride resin molded article 1 due to heat or light.
[0052] The stabilizer is not particularly limited, and examples thereof include metal soaps such as dibasic lead stearate, cadmium stearate, barium stearate, and calcium stearate; organotin compounds such as monobutyltin trimethyl maleate, dibutyltin dilaurate, dibutyltin maleate, dibutyltin mercaptide, dimethyltin mercaptide, and metal salts thereof; and lead-based stabilizers such as tribasic lead sulfate and dibasic lead stearate. These may be used alone or in combination of two or more.
[0053] The content of the stabilizer is preferably 0.1 to 10.0 parts by weight, more preferably 0.5 to 8.0 parts by weight, based on 100 parts by weight of the polyvinyl chloride resin, which allows the vinyl chloride resin molded product 1 to maintain its mechanical strength while improving its stability against heat and light.
[0054] The addition of a stabilizer to the vinyl chloride resin molded article 1 may be omitted depending on the application of the vinyl chloride resin molded article 1 as an interior material.
[0055] <<Lubricant>> The lubricant is contained in the vinyl chloride resin molded article 1 in order to improve moldability by providing excellent slipperiness against dies, rollers, and the like during molding of the vinyl chloride resin molded article 1.
[0056] Examples of the lubricant include aliphatic monocarboxylic acids such as stearic acid, palmitic acid, behenic acid, and montanic acid (preferably aliphatic monocarboxylic acids having 16 or more carbon atoms) and their derivatives such as metal salts, metal soaps, natural waxes such as carnauba wax and candelilla wax, petroleum waxes such as paraffin wax, and synthetic waxes such as oxidized polyethylene wax. These may be used alone or in combination of two or more kinds.
[0057] Examples of the metal in the metal salt of an aliphatic monocarboxylic acid include calcium, barium, magnesium, aluminum, and zinc.
[0058] The content of the lubricant varies slightly depending on the type of the lubricant, but is preferably 0.05 parts by weight or more and 5.00 parts by weight or less, and more preferably 0.30 parts by weight or more and 4.00 parts by weight or less, relative to 100 parts by weight of the polyvinyl chloride resin. This ensures that the above-mentioned effects can be achieved.
[0059] The addition of a lubricant to the vinyl chloride resin molded body 1 may be omitted depending on the combination of constituent materials contained in the vinyl chloride resin molded body 1, etc.
[0060] <<Flame retardants>> The flame retardant is contained in the vinyl chloride resin molded article 1 in order to impart flame retardancy to the vinyl chloride resin molded article 1, inhibit combustion of the vinyl chloride resin molded article 1, and improve its safety.
[0061] Examples of the flame retardant include antimony compounds such as antimony trioxide, metal hydroxides such as aluminum hydroxide and magnesium hydroxide, phosphorus compounds such as cresyl diphenyl phosphate, trischloroethyl phosphate, trischloropropyl phosphate and trisdichloropropyl phosphate, nitrogen-containing compounds such as melamine compounds and guanidine compounds, and halogen compounds such as chlorinated paraffins. These can be used alone or in combination of two or more.
[0062] The content of the flame retardant varies slightly depending on the type of the flame retardant, but is preferably 0.1 to 20.0 parts by weight, more preferably 0.5 to 8.0 parts by weight, per 100 parts by weight of the polyvinyl chloride resin. This ensures that the vinyl chloride resin molded article 1 has excellent flame retardancy.
[0063] Furthermore, in the present invention, in addition to the above-mentioned flame retardant, a molybdenum compound is contained in the vinyl chloride resin molded product 1. This imparts flame retardancy to the vinyl chloride resin molded product 1 and also suppresses the smoke generation of the vinyl chloride resin molded product 1, thereby realizing low toxic gas properties of the vinyl chloride resin molded product 1 and further improving its safety.
[0064] The molybdenum compound is contained in the polyvinyl chloride resin molded body 1 as particles, more specifically, as secondary particles including primary particles of the molybdenum compound and primary particles of a flame retardant other than the molybdenum compound. The average particle size of the particles is not particularly limited, but is preferably set to, for example, about 1.0 μm or more and 50.0 μm or less, more preferably about 3.0 μm or more and 15.0 μm or less. This allows the molybdenum compound to be uniformly dispersed in the polyvinyl chloride resin molded body 1 without aggregation.
[0065] The shape of the particles containing a molybdenum compound is not particularly limited and may be any of spherical, elliptical, flat, acicular, etc., and in this specification, the particle size of the particles refers to the maximum diameter of the particles having each shape, and for example, in the case of a spherical particle, it refers to the diameter.
[0066] In addition, the molybdenum compound is not particularly limited, but examples thereof include inorganic molybdenum compounds such as molybdenum trioxide, zinc molybdate, ammonium molybdate, magnesium molybdate, calcium molybdate, barium molybdate, sodium molybdate, potassium molybdate, molybdenum disulfide, and molybdenum nitride, and organic molybdenum compounds such as molybdenum dialkyldithiophosphate, and the like. These compounds may be used alone or in combination of two or more.
[0067] Furthermore, the particles containing the molybdenum compound may have a coupling agent having a hydrocarbon group bonded to their surfaces.
[0068] As the coupling agent, for example, a silane-based coupling agent, a titanium-based coupling agent, an aluminum-based coupling agent, or the like can be used.
[0069] The content of the molybdenum compound is preferably 1.0 to 15.0 parts by weight, more preferably 2.0 to 8.0 parts by weight, based on 100 parts by weight of the polyvinyl chloride resin, which makes it possible to more reliably suppress the smoke generation of the polyvinyl chloride resin molded article 1.
[0070] In addition, the addition of flame retardants to the polyvinyl chloride resin molding 1, other than molybdenum-based compounds, may be omitted depending on the use of the interior material to which the polyvinyl chloride resin molding 1 is applied, i.e., depending on the flame retardant properties required of the polyvinyl chloride resin molding 1.
[0071] <<Zeolite>> Zeolite is contained in the polyvinyl chloride resin molding 1 in order to effectively suppress or prevent thermal decomposition of the polyvinyl chloride resin caused by heating during extrusion by an extruder, which is caused by the presence of a molybdenum compound in the polyvinyl chloride resin composition when the polyvinyl chloride resin molding 1 is extruded, as described in detail below.
[0072] This allows the vinyl chloride resin composition to be continuously and stably extruded by the extruder over a long period of time, thereby enabling the vinyl chloride resin molded article to be stably produced by extrusion molding.
[0073] In addition, the zeolite is not particularly limited, but examples thereof include natural zeolites such as chabazite, mordenite, erionite, and clinoptilolite, and synthetic zeolites such as A-type zeolite, X-type zeolite, and Y-type zeolite, and one or more of these can be used in combination.
[0074] Zeolite is contained as particles in the vinyl chloride resin molded product 1. The average particle size of the particles is not particularly limited, but is preferably set to, for example, about 1.0 μm or more and 50.0 μm or less, more preferably about 5.0 μm or more and 30.0 μm or less. This allows the zeolite to be uniformly dispersed in the vinyl chloride resin molded product 1 without agglomeration.
[0075] The shape of the particles containing zeolite is not particularly limited, and may be any of spherical, elliptical, flat, and acicular shapes.
[0076] The content of zeolite is preferably 0.1 to 5.0 parts by weight, more preferably 0.5 to 2.0 parts by weight, based on 100 parts by weight of polyvinyl chloride resin, which makes it possible to more accurately suppress or prevent the induction of thermal decomposition of the polyvinyl chloride resin due to heating during extrusion of the vinyl chloride resin composition by an extruder.
[0077] The addition of zeolite to the polyvinyl chloride resin molded article 1 may be omitted if the induction of thermal decomposition of the polyvinyl chloride resin is sufficiently suppressed or prevented by the addition of an antioxidant.
[0078] <<Antioxidants>> The antioxidant is contained in order to prevent oxidation of the constituent materials contained in the vinyl chloride resin molded product 1. Furthermore, like zeolite, the antioxidant is contained in the vinyl chloride resin molded product 1 in order to precisely suppress or prevent thermal decomposition of the polyvinyl chloride resin caused by heating during extrusion by an extruder, which is caused by the presence of a molybdenum compound in the vinyl chloride resin composition during molding of the vinyl chloride resin molded product 1 by extrusion molding, as described in detail below.
[0079] This allows the vinyl chloride resin composition to be continuously and stably extruded by the extruder over a long period of time, thereby enabling the vinyl chloride resin molded article to be stably produced by extrusion molding.
[0080] Examples of the antioxidant include phosphite-based antioxidants (phosphorus-based antioxidants) such as trisnonylphenyl phosphite, tridecyl phosphite, and diphenyldecyl phosphite, hindered phenol-based antioxidants, phenol-based antioxidants such as alkylated monophenols and alkylated hydroquinones, and amine-based antioxidants such as alkylated tert-butylphenylenediamine and hydroxylamine, and one or more of these can be used in combination, but among them, phosphite-based antioxidants and phenol-based antioxidants are preferable, which can more significantly exhibit the above-mentioned effects.
[0081] Examples of the hindered phenol-based antioxidant include 2,2'-methylenebis(4-methyl-6-tert-butylphenol) and pentaerythritol tetrakis[3-(3',5'-di-tert-butyl-4'-hydroxyphenyl)propionate].
[0082] The content of the antioxidant is preferably 0.01 to 5.0 parts by weight, more preferably 0.1 to 2.0 parts by weight, based on 100 parts by weight of the polyvinyl chloride resin, which makes it possible to more accurately suppress or prevent the induction of thermal decomposition of the polyvinyl chloride resin due to heating during extrusion of the vinyl chloride resin composition by an extruder.
[0083] The addition of an antioxidant to the polyvinyl chloride resin molded body 1 may be omitted if the induction of thermal decomposition of the polyvinyl chloride resin is sufficiently suppressed or prevented by the addition of zeolite.
[0084] However, by adding both zeolite and an antioxidant to the polyvinyl chloride resin molding 1, as in this embodiment, the induction of thermal decomposition of the polyvinyl chloride resin can be more accurately suppressed or prevented.
[0085] <<Pigments>> The pigment is contained in the vinyl chloride resin molded article 1 as a coloring material in the vinyl chloride resin molded article 1.
[0086] The pigment is selected according to the required coloring (color tone). Examples of the pigment include organic pigments such as azo pigments, benzimidazolone pigments, diarylide pigments, quinacridone pigments, isoindolinone pigments, vat pigments, phthalocyanine pigments, and dioxane pigments, as well as inorganic pigments such as titanium yellow and yellow lead pigments. These pigments may be used alone or in combination of two or more kinds.
[0087] The content of the pigment is set according to the required coloring (tone), but is preferably 0.01 to 8.00 parts by weight, more preferably 0.05 to 6.00 parts by weight, based on 100 parts by weight of the polyvinyl chloride resin, which allows the above-mentioned effects to be reliably achieved.
[0088] In the vinyl chloride resin molded product 1, the primary particles of the molybdenum compound and the secondary particles containing the molybdenum compound have a white color. Therefore, when the vinyl chloride resin molded product 1 contains a colored pigment, the spotted pattern caused by the particles containing the molybdenum compound is more clearly visible, and in such a case, the vinyl chloride resin molded product 1 of the present invention is more preferably applied.
[0089] Furthermore, the addition of a pigment to the vinyl chloride resin molded article 1 can be omitted if there is no need to color the vinyl chloride resin molded article 1.
[0090] In addition, the vinyl chloride resin molded body 1 may contain, in addition to the polyvinyl chloride resin, reinforcing agent, processing aid, stabilizer, lubricant, flame retardant, zeolite, antioxidant, and pigment described above, for example, ultraviolet absorbers, plasticizers, antistatic agents, etc.
[0091] When the vinyl chloride resin molded article 1 described above is in the form of a sheet as in this embodiment, its thickness is preferably set to 0.5 mm to 8.0 mm, more preferably 1.0 mm to 5.0 mm. By setting the thickness of the vinyl chloride resin molded article 1 within this range, the vinyl chloride resin molded article 1 can be made lightweight while having excellent strength.
[0092] Specifically, it is preferable that the vinyl chloride resin molded article 1 as described above exhibits the following flame retardancy.
[0093] That is, when the polyvinyl chloride resin molded body 1 was burned in accordance with the heat release test specified in ASTM E906, the maximum heat release rate measured within 5 minutes after the ignition of the polyvinyl chloride resin molded body 1 was 65 kW / m 2 It is preferable that the maximum power consumption is 55 kW / m or less. 2 It is more preferable that:
[0094] Furthermore, the total heat generated by the polyvinyl chloride resin molded body 1 for two minutes after ignition was 65 kW min / m 2 It is preferable that the speed is less than 55kW·min / m 2 It is more preferable that:
[0095] When the maximum heat release rate and the total heat release amount are equal to or less than the aforementioned values, the vinyl chloride resin molded article 1 can be said to exhibit excellent flame retardancy.
[0096] Furthermore, in the smoke generation test specified in ASTM E662, i.e., the smoke density test during combustion using an NBS smoke chamber, the smoke density (Ds) after 4.0 minutes of combustion is preferably 200 or less, and more preferably 150 or less. When the smoke density (Ds) is equal to or less than this value, it can be said that the polyvinyl chloride resin molded product 1 has suppressed smoke generation.
[0097] The vinyl chloride resin molded article 1 as described above is produced as follows by applying the method for producing a vinyl chloride resin molded article of the present invention.
[0098] <Method of manufacturing polyvinyl chloride resin molded product> First, prior to describing the method for producing a vinyl chloride resin molded article of the present invention, a production apparatus 10 used for producing the vinyl chloride resin molded article 1 will be described.
[0099] FIG. 2 is a side view of a production apparatus for producing the vinyl chloride resin molded article shown in FIG. In addition, in Fig. 2, the upper side is also referred to as "upper" or "top", and the lower side is also referred to as "lower" or "bottom". Also, in Fig. 2, some parts are exaggerated and greatly differ from the actual dimensions.
[0100] The flat-plate-shaped vinyl chloride resin molded article 1 shown in FIG. 1 is produced, in this embodiment, by molding a vinyl chloride resin composition containing a polyvinyl chloride resin, a reinforcing agent, a processing aid, a stabilizer, a lubricant, a molybdenum compound as a flame retardant, an antioxidant, zeolite, and a pigment, using a production apparatus 10.
[0101] As shown in FIG. 2, the manufacturing apparatus 10 includes a supply section 100, an extruder 200, a molding section 300, a cooling section 400, and a cutting section 500.
[0102] The supply section 100 stores the vinyl chloride resin composition and supplies the stored vinyl chloride resin composition to the extruder 200. In the supply section 100, the vinyl chloride resin composition is stored in a mixed (kneaded) state.
[0103] The extruder 200 extrudes the vinyl chloride resin composition supplied from the supply unit 100 into a sheet by an extrusion method. The extruder 200 has a flow path through which the vinyl chloride resin composition passes and a screw provided in the flow path. The vinyl chloride resin composition is extruded into a sheet by rotating the screw.
[0104] Here, when the vinyl chloride resin composition is extruded by the extruder 200, the vinyl chloride resin composition is heated by the temperature setting of the extruder barrel (cylinder) equipped in the extruder 200 and the rotation of the screw. As a result, the vinyl chloride resin composition supplied from the supply section 100 to the extruder 200 is continuously heated, but in the present invention, in addition to the molybdenum compound, at least one of zeolite and an antioxidant is further contained in the vinyl chloride resin composition. Therefore, the vinyl chloride resin composition can be extruded by the extruder 200 continuously and stably for a long period of time by appropriately suppressing or preventing the induction of thermal decomposition of the polyvinyl chloride resin due to this heating. Therefore, the manufacturing apparatus 10 to which extrusion molding is applied can stably manufacture the vinyl chloride resin molded body 1.
[0105] In this embodiment, the forming section 300 has three rollers 301, 302, and 303. The rollers 301 to 303 are arranged in a line in the vertical direction and are configured to rotate independently of each other. The extruded sheet material is wrapped around these rollers 301 to 303, and the sheet material is sandwiched between the rollers 301 to 303 and formed to a uniform thickness.
[0106] The cooling section 400 has a plurality of cooling rollers 401. Each cooling roller 401 comes into contact with one surface of the formed sheet, thereby cooling the sheet.
[0107] The cutting section 500 has a blade portion 501, and cuts the sheet to a predetermined length using the blade portion 501.
[0108] Using such a production apparatus 10, the vinyl chloride resin molded article 1 is produced as follows.
[0109] [1] First, a reinforcing agent, a processing aid, a stabilizer, a lubricant, a flame retardant including a molybdenum compound, an antioxidant, a zeolite, and a pigment are added to a powder containing a polyvinyl chloride resin, and then the mixture is kneaded using a super mixer, a Henschel mixer, a blender, or the like to prepare a polyvinyl chloride resin composition.
[0110] [2] Next, the prepared vinyl chloride resin composition is molded using a production apparatus 10 to obtain a vinyl chloride resin molded article 1.
[0111] In the manufacturing method using the manufacturing apparatus 10 described above, the vinyl chloride resin composition supplied from the supply unit 100 is continuously extruded by the extruder 200 into a sheet material, and the surface is flattened and molded to a predetermined thickness by the molding unit 300. The sheet is then cooled in contact with the cooling unit 400 and cut to a predetermined length by the cutting unit 500 to obtain the vinyl chloride resin molded product 1.
[0112] When the vinyl chloride resin composition is continuously extruded into a sheet material by extruder 200, the vinyl chloride resin composition is heated, and since the vinyl chloride resin composition further contains at least one of a zeolite and an antioxidant in addition to a molybdenum compound, it is possible to appropriately suppress or prevent the induction of thermal decomposition of the polyvinyl chloride resin due to this heating. Therefore, the vinyl chloride resin composition can be extruded by extruder 200 continuously and stably over a long period of time.
[0113] When the vinyl chloride resin composition is extruded by extruder 200, the vinyl chloride resin composition is usually heated to a temperature of about 120° C. or more and 200° C. or less, and when it is heated to a higher temperature, to a heating temperature of about 170° C. or more and 200° C. or less. Even if the vinyl chloride resin composition is exposed to such high temperatures, the vinyl chloride resin composition contains at least one of a zeolite and an antioxidant in addition to a molybdenum compound, and thus it is possible to appropriately suppress or prevent the induction of thermal decomposition of the polyvinyl chloride resin due to the heating.
[0114] In addition, this vinyl chloride resin composition is kneaded using a roller mixer for a kneading / extrusion molding evaluation test device, Lab Plastomill (manufactured by Toyo Seiki, "R60") under the conditions of a heating temperature of 190°C and a mixer rotation speed of 60 rpm, and the time when the torque increases by 20% from the steady state is taken as the thermal decomposition time. The measured thermal decomposition time is preferably more than 6.0 minutes, more preferably 16.0 minutes or more, and even more preferably 20.0 minutes or more. When the thermal decomposition time is equal to or greater than the lower limit, it can be said that the induction of thermal decomposition of the polyvinyl chloride resin contained in the vinyl chloride resin composition is suppressed. In addition, by making the vinyl chloride resin composition contain at least one of a zeolite and an antioxidant in addition to the molybdenum compound, the thermal decomposition time can be set to equal to or greater than the lower limit. Therefore, by making the vinyl chloride resin composition contain at least one of a zeolite and an antioxidant, and setting the thermal decomposition time of the vinyl chloride resin composition to equal to or greater than the lower limit, the induction of thermal decomposition of the polyvinyl chloride resin contained in the vinyl chloride resin composition can be appropriately suppressed or prevented.
[0115] In this embodiment, the cut sheet has been described as the vinyl chloride resin molded body 1, but the cutting of the sheet may be omitted and the vinyl chloride resin molded body 1 may be a sheet wound into a roll.
[0116] In addition, in the manufacturing apparatus 10, a cooling function may be imparted to the rollers 301, 302, and 303, and the molding section 300 may function as a cooling section.
[0117] By molding a vinyl chloride resin composition using the production apparatus 10 as described above, the vinyl chloride resin molded article 1 can be stably obtained.
[0118] Furthermore, this polyvinyl chloride resin molded body 1 can be applied to interior materials for vehicles such as automobiles, buses, and trains, as well as transportation equipment such as ships, aircraft, and spacecraft, and for buildings, and is particularly suitable for use as an interior material for transportation equipment where higher safety is required, since smoke generation is suppressed.
[0119] The vinyl chloride resin molded article, the method for producing the vinyl chloride resin molded article, the interior material, and the transportation equipment of the present invention have been described above, but the present invention is not limited thereto, and any component may be added to the vinyl chloride resin composition.
[0120] Furthermore, the shape of the vinyl chloride resin molded article of the present invention is not limited to the above-mentioned sheet-like shape, but may be any shape, such as a rod shape, a cylinder shape, or an annular shape. EXAMPLES
[0121] The present invention will now be described more specifically with reference to examples. 1. Selection of polyvinyl chloride resin 1-1. Preparation of raw materials As raw materials for preparing the vinyl chloride resin composition, the following were prepared.
[0122] (Chlorinated polyvinyl chloride (CPVC)) Chlorinated polyvinyl chloride resin (Kaneka Corporation, "H-516A"; chlorine concentration 65%, polymerization degree 600)
[0123] (Polyvinyl chloride (PVC)) Vinyl chloride resin (Shin-Etsu Chemical Co., Ltd., "TK-800Q": chlorine concentration 56%, polymerization degree 800)
[0124] (Vinyl chloride-ethylene copolymer (E-PVC)) Vinyl chloride-ethylene copolymer (manufactured by Taiyo Vinyl, "TE-650")
[0125] (Stabilizer) Dimethyltin compounds (manufactured by Nitto Chemical Industries, Ltd., "AT-1500", dimethyltin mercapto)
[0126] (Reinforcing agent) Acrylic (MMA / BA) polymer (Kaneka Corporation, "FM-50")
[0127] (Processing aids) Acrylic (MMA / BMA / EA / BA) polymer (Kaneka Corporation, "PA-40")
[0128] (lubricant) Stearic acid (Kao Corporation, "Lunac S-70V") Oxidized polyethylene wax (Honeywell, AC-629A)
[0129] (Flame retardant) Molybdenum compounds (Climax Corporation, "AMO-W", ammonium octamolybdate)
[0130] 1-2. Manufacturing of polyvinyl chloride resin molded products [Reference Example 1A] [1A] First, of the raw materials shown above, those shown in Table 1 were mixed and stirred in a Super Mixer in the amounts shown in Table 1 in the parts by weight shown in Table 1 while heating the mixture to 100°C, and then cooled to 30°C to prepare vinyl chloride resin compositions.
[0131] [2A] Next, the prepared vinyl chloride resin composition was placed in extruder 200 provided in production apparatus 10 shown in Fig. 2 and extruded to obtain a molten sheet. The molten sheet was then wrapped around rollers 301-303 and clamped to be flattened, and then cooled in cooling section 400. The sheet was then cut to a predetermined length in cutting section 500 to obtain a sheet-like vinyl chloride resin molded product 1 having a thickness of 3.0 mm.
[0132] [Reference examples 2A~4A] The vinyl chloride resin molded articles 1 of Reference Examples 2A to 4A were obtained in the same manner as in Reference Example 1A, except that the raw materials used in preparing the vinyl chloride resin composition in step [1A], and the weight parts of each raw material contained in the vinyl chloride resin composition, were as shown in Table 1.
[0133] 1-3. Evaluation of sheet appearance and thickness of polyvinyl chloride resin molded products The vinyl chloride resin molded articles of each Reference Example were observed for their appearance and thickness, and were evaluated based on the observation results using the following criteria.
[0134] <Judgment criteria> ⊚: There is no variation in resin discharge, the sheet surface is smooth, and the thickness distribution is uniform. ◯: There is no change in the resin discharge, but the sheet surface is slightly uneven. Δ: There is a variation in the resin discharge, or there are irregularities on part of the sheet surface, and the thickness distribution is non-uniform. ×: The resin discharge fluctuates greatly, or the entire surface of the sheet is uneven, and the thickness distribution is non-uniform.
[0135] The evaluation results of the vinyl chloride resin molded articles of each of the Reference Examples obtained as described above are shown in Table 1 below.
[0136] [Table 1]
[0137] As shown in Table 1, it was revealed that in the vinyl chloride resin molded articles of each Reference Example, by using a combination of chlorinated vinyl chloride resin and vinyl chloride resin as the polyvinyl chloride resin, and further by using a combination of chlorinated vinyl chloride resin and vinyl chloride-ethylene copolymer, it is possible to mold vinyl chloride resin molded articles having a more uniform thickness.
[0138] 2. Check flame retardant performance 2-1. Preparation of raw materials As raw materials for preparing the vinyl chloride resin composition, the following were prepared.
[0139] (Chlorinated polyvinyl chloride (CPVC)) Chlorinated polyvinyl chloride resin (Kaneka Corporation, "H-516A"; chlorine concentration 65%, polymerization degree 600)
[0140] (Vinyl chloride-ethylene copolymer (E-PVC)) Vinyl chloride-ethylene copolymer (manufactured by Taiyo Vinyl, "TE-650")
[0141] (Stabilizer) Dimethyltin compounds (manufactured by Nitto Chemical Industries, Ltd., "AT-1500", dimethyltin mercapto)
[0142] (Reinforcing agent) Acrylic (MMA / BA) polymer (Kaneka Corporation, "FM-50")
[0143] (Processing aids) Acrylic (MMA / BMA / EA / BA) polymer (Kaneka Corporation, "PA-40")
[0144] (lubricant) Stearic acid (Kao Corporation, "Lunac S-70V") Oxidized polyethylene wax (Honeywell, AC-629A)
[0145] (Flame retardant) Molybdenum compounds (Climax Corporation, "AMO-W", ammonium octamolybdate) Magnesium hydroxide (Kyowa Chemical Industry Co., Ltd., "KISUMA 5J")
[0146] 2-2. Manufacturing of polyvinyl chloride resin molded products [Reference example 1B] [1B] First, the raw materials shown above, those shown in Table 2, were mixed and stirred in a Super Mixer in the amounts shown in Table 2 in the parts by weight shown in Table 2 while heating the mixture to 100°C, and then cooled to 30°C to prepare vinyl chloride resin compositions.
[0147] [2B]Next, the prepared vinyl chloride resin composition was stored in the extruder 200 provided in the manufacturing apparatus 10 shown in Fig. 2 and extruded to obtain a sheet in a molten state. Then, the sheet in the molten state was looped around and held by rollers 301 to 303 to be flattened, and then cooled in the cooling unit 400. Then, by cutting at a predetermined length with the cutting unit 500, a vinyl chloride resin molded body 1 in the shape of a sheet with a thickness of 2.0 mm was obtained.
[0148] [Reference Examples 2B to 4B] In the above step [1B], except that the raw materials used when preparing the vinyl chloride resin composition and further the parts by weight of each raw material contained in the vinyl chloride resin composition were as shown in Table 2, the vinyl chloride resin molded bodies 1 of Reference Examples 2B to 4B were obtained in the same manner as in Reference Example 1B.
[0149] 2-3. Evaluation of Flame Retardancy of Vinyl Chloride Resin Molded Body Regarding the vinyl chloride resin molded bodies of each reference example, their flame retardancy was evaluated by the following method.
[0150] <OSU Heat Release Test (specified in AITM 2.0006)> First, in accordance with the OSU heat release test specified in AITM 2.0006, when the vinyl chloride resin molded body was burned, the maximum heat release rate (HRR) measured within 5 minutes from the ignition of the vinyl chloride resin molded body and the total heat release amount (THR) within 2 minutes from the ignition were measured. The total heat release amount within 2 minutes from the ignition was 65 kW·min / m 2 The following cases were regarded as passing (〇), and cases exceeding 65 kW·min / m 2 were regarded as failing (×). Also, when the maximum heat release rate measured within 5 minutes from the ignition was 65 kW / m 2 or less, it was regarded as passing (〇), and cases exceeding 65 kW / m 2 were regarded as failing (×).
[0151] <Smoke Emission Test> The maximum smoke density after 4 minutes was measured using the NBS smoke generation test in accordance with ASTM E662-82. If the maximum smoke density after 4 minutes was 200 ppm or less, it was considered a pass (◯), and if it exceeded that value, it was considered a fail (×).
[0152] The evaluation results of the vinyl chloride resin molded articles of each of the Reference Examples obtained as described above are shown in Table 2 below.
[0153] [Table 2]
[0154] As shown in Table 2, it was found that by using a flame retardant containing a molybdenum compound in the polyvinyl chloride resin molded body in each reference example, the polyvinyl chloride resin molded body can have excellent flame retardancy and reduced smoke generation.
[0155] 3. Confirmation of thermal stability of polyvinyl chloride resin 3-1. Preparation of raw materials As raw materials for preparing the vinyl chloride resin composition, the following were prepared.
[0156] (Chlorinated polyvinyl chloride (CPVC)) Chlorinated polyvinyl chloride resin (Kaneka Corporation, "H-516A"; chlorine concentration 65%, polymerization degree 600)
[0157] (Vinyl chloride-ethylene copolymer (E-PVC)) Vinyl chloride-ethylene copolymer (manufactured by Taiyo Vinyl, "TE-650")
[0158] (Stabilizer) Dimethyltin compounds (manufactured by Nitto Chemical Industry Co., Ltd., "AT-1500", dimethyltin mercapto)
[0159] (Reinforcing agent) Acrylic (MMA / BA) polymer (Kaneka Corporation, "FM-50")
[0160] (Processing aids) Acrylic (MMA / BMA / EA / BA) polymer (Kaneka Corporation, "PA-40")
[0161] (lubricant) Stearic acid (Kao Corporation, "Lunac S-70V") Oxidized polyethylene wax (Honeywell, AC-629A) Ester lubricant mix (manufactured by Daikyo Kasei Kogyo Co., Ltd., "RX-303", zeolite content 0.0 parts by weight) (Antioxidants) Phenolic antioxidant (BASF Japan, hindered phenolic antioxidant, "Irganox1010") Phenolic antioxidant (BASF Japan, hindered phenolic antioxidant, "Irganox245") Phosphite antioxidant (ADEKA, "HP-10")
[0162] (Zeolite) Zeolite (Tosoh Corporation, "GLS-1000") (Flame retardant) Molybdenum compounds (Climax Corporation, "AMO-W", ammonium octamolybdate)
[0163] 3-2. Manufacturing of polyvinyl chloride resin molded products [Example 1C] [1C] First, of the raw materials shown above, those shown in Table 3 were mixed and stirred in a Super Mixer in the amounts shown in Table 3 in the parts by weight shown in Table 3 while heating the mixture to 100°C, and then cooled to 30°C to prepare vinyl chloride resin compositions.
[0164] [2C]Next, the prepared vinyl chloride resin composition was stored in the extruder 200 provided in the manufacturing apparatus 10 shown in FIG. 2 and extruded to obtain a sheet in a molten state. Then, the sheet in the molten state was looped around and held by rollers 301 to 303 to be flattened, and then cooled in the cooling unit 400. Then, by cutting at a predetermined length with the cutting unit 500, a vinyl chloride resin molded body 1 in the form of a sheet with a thickness of 2.0 mm was obtained.
[0165] [Examples 2C to 10C, Comparative Example 1C] In the step [1C], except that the raw materials used when preparing the vinyl chloride resin composition and further the parts by weight of each raw material contained in the vinyl chloride resin composition were as shown in Table 3, in the same manner as in Example 1C, vinyl chloride resin molded bodies 1 of Examples 2C to 10C and Comparative Example 1C were obtained.
[0166] 3-3. Evaluation of Thermal Stability of Polyvinyl Chloride Resin Regarding the vinyl chloride resin molded bodies of each example and comparative example, their thermal stability was evaluated by the following method.
[0167] <PVC Thermal Decomposition Time> First, the vinyl chloride resin compositions prepared when obtaining the vinyl chloride resin molded bodies of each example and comparative example were kneaded using a roller mixer (manufactured by Toyo Seiki Co., Ltd., "R60") for a laboratory plastomill for kneading and extrusion molding evaluation test apparatus under the conditions of a heating temperature of 190°C and a mixer rotation speed of 60 rpm. The time when the torque increased by 20% from the steady-state torque was defined as the PVC thermal decomposition time, and the PVC thermal decomposition time (laboratory plastomill 190°C, 60 rpm) was measured. And when this PVC thermal decomposition time exceeded 6.0 minutes, it was judged as qualified (〇), and when it was 6.0 minutes or less, it was judged as unqualified (×).
[0168] The evaluation results of the vinyl chloride resin molded bodies of each example obtained as described above are shown in Table 3 below respectively.
[0169]
Table 3
[0170] As shown in Table 3, the PVC thermal decomposition time of the vinyl chloride resin composition used in molding the vinyl chloride resin molded article of each Example could be set long, such as more than 6.0 minutes. As a result, when the vinyl chloride resin composition was used to mold the vinyl chloride resin molded article by the manufacturing apparatus 10 to which extrusion molding was applied, the vinyl chloride resin composition could be extruded continuously and stably over a long period of time.
[0171] On the other hand, the PVC thermal decomposition time of the vinyl chloride resin composition used in molding the vinyl chloride resin molding in the comparative example was 6.0 minutes or less, and when molding the vinyl chloride resin molding using the production apparatus 10, thermal decomposition of the polyvinyl chloride resin was induced by heating during extrusion by the extruder 200, and the vinyl chloride resin composition could not be stably extruded over a long period of time. [Explanation of symbols]
[0172] 1. Polyvinyl chloride resin molding 10 Manufacturing equipment 100 Supply section 200 Extruder 300 Molding section 301 Roller 302 Roller 303 Roller 400 Cooling section 401 Roller 500 cutting section 501 Blade part
Claims
1. A polyvinyl chloride resin, A stabilizer including an organotin compound; A molybdenum compound, Zeolite and A phenolic antioxidant, Contains The content of the stabilizer is 0.1 parts by weight or more and 10.0 parts by weight or less based on 100 parts by weight of the polyvinyl chloride resin, the content of the molybdenum compound is 1.0 part by weight or more and 15.0 parts by weight or less based on 100 parts by weight of the polyvinyl chloride resin, The content of the zeolite is 0.1 parts by weight or more and 5.0 parts by weight or less with respect to 100 parts by weight of the polyvinyl chloride resin, A polyvinyl chloride resin molded article, characterized in that the content of the phenol-based antioxidant is 0.1 parts by weight or more and 5.0 parts by weight or less based on 100 parts by weight of the polyvinyl chloride resin.
2. The zeolite is in particulate form, 2. The polyvinyl chloride resin molded article according to claim 1, wherein the average particle size of the zeolite is from 5.0 μm to 50.0 μm.
3. A polyvinyl chloride resin, A stabilizer including an organotin compound; A molybdenum compound, A phosphite antioxidant; Contains The content of the stabilizer is 0.1 parts by weight or more and 10.0 parts by weight or less based on 100 parts by weight of the polyvinyl chloride resin, the content of the molybdenum compound is 1.0 part by weight or more and 15.0 parts by weight or less based on 100 parts by weight of the polyvinyl chloride resin, A polyvinyl chloride resin molded article, characterized in that the content of the phosphite-based antioxidant is 0.1 parts by weight or more and 5.0 parts by weight or less based on 100 parts by weight of the polyvinyl chloride resin.
4. The molybdenum compound is in particulate form, 4. The polyvinyl chloride resin molded article according to claim 1, wherein the average particle size of the molybdenum compound is 1.0 μm or more and 50.0 μm or less.
5. 5. The polyvinyl chloride resin molded article according to claim 1, wherein the polyvinyl chloride resin contains a chlorinated vinyl chloride resin having a chlorine content of 62.0% or more and 69.0% or less, and a vinyl chloride-ethylene copolymer.
6. 6. The polyvinyl chloride resin molded article according to claim 5, wherein the content of the vinyl chloride-ethylene copolymer is 5.0 parts by weight or more and 50.0 parts by weight or less based on 100 parts by weight of the polyvinyl chloride resin.
7. 7. The vinyl chloride resin molded article according to claim 1, further comprising at least one of a reinforcing agent, a processing aid, a lubricant, and a pigment.
8. 8. The vinyl chloride resin molded article according to claim 1, which is in the form of a sheet.
9. 9. The vinyl chloride resin molded product according to any one of claims 1 to 8, wherein when a vinyl chloride resin composition used in obtaining the vinyl chloride resin molded product is kneaded using a roller mixer under conditions of a heating temperature of 190°C and a mixer rotation speed of 60 rpm, and the thermal decomposition time is defined as the time required for a torque to increase by 20% from a steady state, the thermal decomposition time is longer than 6.0 minutes.
10. A method for producing the vinyl chloride resin molded article according to claim 1 or 2, comprising the steps of: A molybdenum compound and a zeolite are added to the powder containing the polyvinyl chloride resin, and then the mixture is kneaded under heating to prepare a polyvinyl chloride resin composition. A method for producing a vinyl chloride resin molded article, comprising molding the vinyl chloride resin composition by extrusion molding to obtain the vinyl chloride resin molded article.
11. 11. The method for producing a vinyl chloride resin molded article according to claim 10, wherein the heating temperature when the vinyl chloride resin composition is extruded by an extruder during the extrusion molding is 120°C or higher and 200°C or lower.
12. An interior material comprising the vinyl chloride resin molded article according to any one of claims 1 to 9.
13. The interior material according to claim 12, which is for a transport machine.
14. A transport device comprising the interior material according to claim 13.
Citation Information
Patent Citations
Vinyl chloride-based resin composition and plugging part using the same
JP1992332748A
Molding composition
JP1994240083A
Vinyl chloride resin composition, sheet and decorative wall material
JP1995188487A
Chlorinated vinyl chloride-based resin composition
JP2001247737A
Flame retardant polyvinyl chloride resin molded article
JP2002226659A