Thermoplastic resin composition
A polycarbonate resin composition with specific cyclic acetal diols addresses the challenge of refractive index adjustment and heat resistance, ensuring transparency and high heat resistance in thermoplastic resin applications.
Patent Information
- Application Number
- JP2020099382
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-06-21
- Filing Date
- 2020-06-08
- Publication Date
- 2024-10-02
- Estimated Expiration
- 2040-06-08
AI Technical Summary
Existing thermoplastic resin compositions struggle to adjust the refractive index of polycarbonate resin while maintaining transparency and high heat resistance, often leading to reduced transparency and heat resistance due to the use of modifiers like PET and PBT.
A thermoplastic resin composition comprising a polycarbonate resin blended with a polycondensate containing specific cyclic acetal diols, such as spiro ring-containing cyclic acetal skeletons, to achieve refractive index adjustment with a lower alloy ratio while maintaining transparency and enhancing heat resistance.
The composition allows for the adjustment of refractive index and maintains transparency with high heat resistance, achieving glass transition temperatures above 130°C and refractive indices between 1.45 to 1.60, suitable for injection molded articles and films.
Smart Images

Figure 0007559361000001 
Figure 0007559361000002 
Figure 0007559361000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a thermoplastic resin composition. More specifically, the present invention relates to a polycarbonate resin-based thermoplastic resin composition that can adjust the refractive index of a polycarbonate resin even with a smaller alloy ratio while maintaining the transparency of the polycarbonate resin, and also to a polycarbonate resin-based thermoplastic resin composition having high heat resistance, and an injection molded article, sheet, and film made using the thermoplastic resin composition. [Background technology]
[0002] Polycarbonate resin (hereinafter sometimes referred to as "PC") has been used in fields such as exteriors, electronic and electrical applications, and optical disk substrates due to its characteristics such as heat resistance, impact resistance, and transparency. Furthermore, as its applications in automobiles and medical materials expand, there is an increasing demand for thermoplastic resin compositions that not only maintain the transparency of PC, but also adjust the refractive index of PC with a smaller alloy ratio, and have high heat resistance.
[0003] The refractive index of PC is about 1.58 to 1.59, and it is possible to use polyethylene terephthalate (hereinafter sometimes referred to as "PET") as a modifier for PC to adjust the refractive index, but it is known that the addition of PET significantly impairs the transparency of PC. As a countermeasure, a method of lengthening the residence time during melt mixing and a method of using a Ti-based catalyst as a catalyst during melt mixing have been considered. However, this method does not provide sufficient transparency, and furthermore, there are problems such as yellowing of the composition due to thermal decomposition and generation of gases such as aldehyde due to decomposition. Furthermore, there is a problem that the heat resistance of the resin composition is significantly reduced because the glass transition temperature (Tg) of PET is relatively low.
[0004] When polybutylene terephthalate resin (hereinafter sometimes referred to as "PBT") is used as a modifier for PC, the transparency is relatively high, but it is not sufficient, and there is a problem that the heat resistance is significantly reduced. Also, a thermoplastic resin composition of PC and modified PET in which 40 mol % of the diol constituent units are 1,4-cyclohexanedimethanol units has been proposed (see Patent Document 1), but this resin composition has good transparency but has a problem that the heat resistance is reduced.
[0005] Although a technology has been proposed for a thermoplastic resin composition having excellent transparency, which is composed of a polycarbonate resin and a specific copolymerized polyester resin, and an injection molded body, sheet, and film made of the thermoplastic resin composition (see Patent Document 2), the heat resistance is insufficient, and since the refractive index of the copolymerized polyester resin is large, it is necessary to melt-mix a larger amount of the copolymerized polyester resin in order to adjust the refractive index of the base resin PC, and in this case, the transparency of PC cannot be maintained. Therefore, a polyester resin-added polycarbonate resin-based thermoplastic resin composition that not only can adjust the refractive index of PC even with a smaller alloy ratio while maintaining the transparency of PC, but also has high heat resistance, is not known.
[0006] Also, known thermoplastic resins include polyester resin (hereinafter sometimes referred to as "PE"), polycarbonate resin, and polyester carbonate resin (hereinafter sometimes referred to as "PEC") (Patent Documents 3 to 7). However, no polycarbonate resin-based thermoplastic resin composition is known that uses these thermoplastic resins as a modifier for PC, and that not only can adjust the refractive index of PC even with a smaller alloy ratio while maintaining the transparency of PC, but also has high heat resistance. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] JP 2000-63641 A [Patent Document 2] JP 2003-246925 A [Patent Document 3] Patent No. 4062416 [Patent Document 4] Patent No. 5445652 [Patent Document 5] JP 2014-044394 A [Patent Document 6] Special Publication No. 2016-525610 [Patent Document 7] Special Publication No. 2018-504497 Summary of the Invention [Problem to be solved by the invention]
[0008] In view of the above-mentioned circumstances, the present invention provides a PC-based thermoplastic resin composition that not only can adjust the refractive index of PC even with a smaller alloy ratio while maintaining the transparency of PC, but also has high heat resistance, and an injection-molded article, sheet, and film made using the thermoplastic resin composition. [Means for solving the problem]
[0009] As a result of extensive investigations aimed at solving the above problems, the present inventors have found that a thermoplastic resin composition obtained by blending a polycarbonate resin with a polycondensate containing a certain proportion of a diol having a specific cyclic acetal skeleton as a diol constituent unit not only maintains the transparency of PC while adjusting the refractive index of PC even with a smaller alloy ratio, but also has high heat resistance, thereby completing the present invention.
[0010] That is, the present invention provides the following: <1> ~ <21> The present invention includes the following aspects.
[0011] <1> A thermoplastic resin composition (C) comprising a polycarbonate resin (A) and a polycondensate (B), The thermoplastic resin composition (C) contains 40 to 99% by weight of a polycarbonate resin (A) and 60 to 1% by weight of a polycondensate (B), and The polycondensate (B) is selected from at least one resin selected from the group consisting of a polyester resin (B1), a polycarbonate resin (B2), and a polyester carbonate resin (B3); The polyester resin (B1) contains, in its diol constituent units, (i) 61 to 100 mol % of a diol (a1) having a spiro ring-containing cyclic acetal skeleton, (ii) containing 0 to 39 mol % of a diol (b1) having a non-spiro ring-containing cyclic acetal skeleton and / or an alicyclic diol (b2); The polycarbonate resin (B2) contains, in its diol constituent units, (i) 1 to 100 mol % of a diol (a1) having a spiro ring-containing cyclic acetal skeleton, (ii) containing 0 to 99 mol % of a diol (b1) having a non-spiro ring-containing cyclic acetal skeleton and / or an alicyclic diol (b2); The polyester carbonate resin (B3) contains, in its diol constituent units, (i) containing 1 to 100 mol % of a diol (a1) having a spiro ring-containing cyclic acetal skeleton; Thermoplastic resin composition (C).
[0012] <2> The polycarbonate resin (A) is a polycarbonate resin composed of repeating units represented by general formula (1) and / or (2). <1> The thermoplastic resin composition (C) according to claim 1. [ka] [ka] (In the formula, R 1 and R 2 are each independently selected from a hydrogen atom, a non-cyclic hydrocarbon group having 1 to 10 carbon atoms, and an alicyclic hydrocarbon group having 5 to 10 carbon atoms; R 3 and R 4are each independently selected from a hydrogen atom, a non-cyclic hydrocarbon group having 1 to 10 carbon atoms, a halogen atom, and a substituted or unsubstituted phenyl group; m and n are each independently 1 or 2; k is 4 or 5.)
[0013] <3> The polycarbonate resin (A) is a polycarbonate ester of bisphenol. <1> The thermoplastic resin composition (C) according to claim 1.
[0014] <4> The bisphenol is selected from the group consisting of bisphenol A, bisphenol AP, bisphenol Z, bisphenol CD, bisphenol C, bisphenol IOTD, bisphenol IBTD and bisphenol MIBK. <3> The thermoplastic resin composition (C) according to claim 1.
[0015] <5> The diol component (a1) having a spiro ring-containing cyclic acetal skeleton is represented by general formula (3), <1> Or <4> The thermoplastic resin composition (C) according to any one of the above. [ka] (In the formula, R 5 and R 6 each independently represents a characteristic group selected from a non-cyclic hydrocarbon group having 1 to 10 carbon atoms, an alicyclic hydrocarbon group having 3 to 10 carbon atoms, and an aromatic hydrocarbon group having 6 to 10 carbon atoms.
[0016] <6> The diol component (b1) having a non-spiro ring-containing cyclic acetal skeleton is represented by general formula (4), <1> Or <5> The thermoplastic resin composition (C) according to any one of the above. [ka] (In the formula, R 5 is as above; R 7 represents a characteristic group selected from acyclic hydrocarbon groups having 1 to 10 carbon atoms, alicyclic hydrocarbon groups having 3 to 10 carbon atoms, and aromatic hydrocarbon groups having 6 to 10 carbon atoms.
[0017] <7> The alicyclic diol (b2) is represented by general formula (5), <1> Or <6> The thermoplastic resin composition (C) according to any one of the above. [ka] (In the formula, R 8 , R 9 , R 10 and R 11 are each independently selected from a hydrogen atom and a non-cyclic hydrocarbon group having 1 to 6 carbon atoms; p, q, r and s are each independently 0, 1 or 2.
[0018] <8> The above polyester carbonate (B3) contains a dicarboxylic acid constituent unit of an alicyclic dicarboxylic acid or a diester thereof (b3). <1> Or <7> The thermoplastic resin composition (C) according to any one of the above.
[0019] <9> The alicyclic dicarboxylic acid or its diester (b3) is represented by general formula (6), <1> Or <8> The thermoplastic resin composition (C) according to any one of the above. [ka] (In the formula, R 8 , R 9 , R 10 , R 11 , R 12 , and R 13 each independently selected from a hydrogen atom and a non-cyclic hydrocarbon group having 1 to 6 carbon atoms; p and q are each independently 0, 1, or 2.
[0020] <10> The diol component (a1) having a spiro ring-containing cyclic acetal skeleton is 3,9-bis(1,1-dimethyl-2-hydroxyethyl)-2,4,8,10-tetraoxaspiro[5.5]undecane. <1> Or <9> The thermoplastic resin composition (C) according to any one of the above.
[0021] <11> The diol component (b1) having a non-spiro ring-containing cyclic acetal skeleton is 5-methylol-5-ethyl-2-(1,1-dimethyl-2-hydroxyethyl)-1,3-dioxane. <1> Or <10> The thermoplastic resin composition (C) according to any one of the above.
[0022] <12> The alicyclic diol (b2) is 1,4-cyclohexanedimethanol. <1> Or <11> The thermoplastic resin composition (C) according to any one of the above.
[0023] <13> The alicyclic dicarboxylic acid or its diester (b3) is 1,4-cyclohexanedicarboxylic acid or dimethyl 1,4-cyclohexanedicarboxylate. <8> The thermoplastic resin composition (C) according to claim 1.
[0024] <14> The polyester resin (B1) contains, in its diol constituent units, A diol (a1) having a spiro ring-containing cyclic acetal skeleton, and Diol having a non-spiro ring-containing cyclic acetal skeleton (b1) Including the above <1> Or <13> The thermoplastic resin composition (C) according to any one of the above.
[0025] <15> The polyester resin (B1) contains, in its diol constituent units, Diol (a1) having a spiro ring-containing cyclic acetal skeleton, A diol (b1) having a non-spiro ring-containing cyclic acetal skeleton, and Alicyclic diol (b2) Including the above <1> Or <13> The thermoplastic resin composition (C) according to any one of the above.
[0026] <16> The dicarboxylic acid constituent unit of the polyester resin (B1) is a dicarboxylic acid unit selected from at least one of a terephthalic acid residue, an isophthalic acid residue, and a 1,4-cyclohexanedicarboxylic acid residue. <1> Or <15> The thermoplastic resin composition (C) according to any one of the above.
[0027] <17> The above, which has the following physical properties (i) to (iii): <1> Or <16> The thermoplastic resin composition (C) according to any one of the above. (i) A glass transition temperature measured by a differential scanning calorimeter of 130°C or higher (ii) A 1 mm thick injection molded article has a total light transmittance of 87% or more and a haze value of 4% or less. (iii) A refractive index measured by the critical angle method is 1.45 to 1.60
[0028] <18> the above <1> Or <17> 2. A sheet obtained by using the thermoplastic resin composition (C) according to any one of 1 to 11, wherein the sheet has a total light transmittance of 87% or more when it is 500 μm thick.
[0029] <19> the above <1> Or <17> 2. A film obtained by using the thermoplastic resin composition (C) according to any one of 1 to 11, wherein the haze of a 50 μm-thick film is 4% or less.
[0030] <20> the above <1> Or <17> 1. A blend composition (E) of the thermoplastic resin composition (C) according to any one of claims 1 to 9 and a thermoplastic resin composition (D), wherein a difference in refractive index between the thermoplastic resin composition (C) and the thermoplastic resin composition (D) measured by a critical angle method is 0.02 or less.
[0031] <21> The thermoplastic resin composition (D) is a thermoplastic resin composition containing at least one thermoplastic resin selected from a polyetherester resin, a polyamide resin, an acrylic resin, a polyvinyl chloride resin, and a polycarbonate resin. <20> The blend composition (E) described above. Effect of the Invention
[0032] According to the present invention, it is possible to adjust the refractive index of a polycarbonate resin even with a smaller alloy ratio while maintaining the transparency of the polycarbonate resin, and also to obtain a polycarbonate resin-thermoplastic resin composition having high heat resistance. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0033] 1.Thermoplastic resin composition (C) The thermoplastic resin composition (C) of the present invention contains a polycarbonate resin (A) and a polycondensate (B).
[0034] In one embodiment of the present invention, the thermoplastic resin composition (C) may contain 40 to 99% by weight of a polycarbonate resin (A) and 60 to 1% by weight of a polycondensate (B). In one embodiment of the present invention, the thermoplastic resin composition (C) may contain 40 to 95% by weight of a polycarbonate resin (A) and 60 to 5% by weight of a polycondensate (B). In one embodiment of the present invention, the thermoplastic resin composition (C) may contain 50 to 99% by weight of a polycarbonate resin (A) and 50 to 1% by weight of a polycondensate (B). In one embodiment of the present invention, the thermoplastic resin composition (C) may contain 50 to 95% by weight of a polycarbonate resin (A) and 50 to 5% by weight of a polycondensate (B). In one embodiment of the present invention, the thermoplastic resin composition (C) may contain 60 to 99% by weight of a polycarbonate resin (A) and 40 to 1% by weight of a polycondensate (B). In one embodiment of the present invention, the thermoplastic resin composition (C) may contain 60 to 95% by weight of the polycarbonate resin (A) and 40 to 5% by weight of the polycondensate (B). In one embodiment of the present invention, the thermoplastic resin composition (C) may contain 70 to 99% by weight of the polycarbonate resin (A) and 30 to 1% by weight of the polycondensate (B). In one embodiment of the present invention, the thermoplastic resin composition (C) may contain 70 to 95% by weight of the polycarbonate resin (A) and 30 to 5% by weight of the polycondensate (B). In one embodiment of the present invention, the thermoplastic resin composition (C) may contain 75 to 99% by weight of the polycarbonate resin (A) and 25 to 1% by weight of the polycondensate (B). In one embodiment of the present invention, the thermoplastic resin composition (C) may contain 75 to 95% by weight of the polycarbonate resin (A) and 25 to 5% by weight of the polycondensate (B). In one embodiment of the present invention, the thermoplastic resin composition (C) may contain 80 to 99% by weight of the polycarbonate resin (A) and 20 to 1% by weight of the polycondensate (B). In one embodiment of the present invention, the thermoplastic resin composition (C) may contain 80 to 95% by weight of the polycarbonate resin (A) and 20 to 5% by weight of the polycondensate (B). In one embodiment of the present invention, the thermoplastic resin composition (C) may contain 90 to 99% by weight of the polycarbonate resin (A) and 10 to 1% by weight of the polycondensate (B).In one embodiment of the present invention, the thermoplastic resin composition (C) may contain 90 to 95% by weight of the polycarbonate resin (A) and 10 to 5% by weight of the polycondensate (B). In one embodiment of the present invention, the thermoplastic resin composition (C) may contain 95 to 99% by weight of the polycarbonate resin (A) and 5 to 1% by weight of the polycondensate (B).
[0035] In the thermoplastic resin composition (C) of the present invention, by adjusting the compounding ratio of the polycarbonate resin (A) and the polycondensate (B) within the above range, it is possible to adjust not only the refractive index of the polycarbonate resin but also to obtain a polycarbonate resin-thermoplastic resin composition having high heat resistance. In addition, since the refractive index can be appropriately adjusted, transparency can be ensured even when a blend composition with other resin compositions is prepared.
[0036] The thermoplastic resin composition (C) of the present invention can be obtained by kneading the polycarbonate resin (A) and the polycondensate (B) by a conventional method.
[0037] 2. Polycarbonate resin (A) In the present invention, the polycarbonate resin (A) may be composed of repeating units represented by general formula (1) and / or (2). [ka] [ka] (In the formula, R 1 and R 2 are each independently selected from a hydrogen atom, a non-cyclic hydrocarbon group having 1 to 10 carbon atoms, and an alicyclic hydrocarbon group having 5 to 10 carbon atoms; R 3 and R 4 are each independently selected from a hydrogen atom, a non-cyclic hydrocarbon group having 1 to 10 carbon atoms, a halogen atom, and a substituted or unsubstituted phenyl group; m and n are each independently 1 or 2; k is 4 or 5.)
[0038] In one embodiment of the present invention, in the above general formula (1), R 1 and R 2 may each independently be selected from a hydrogen atom, a non-cyclic hydrocarbon group having 1 to 4 carbon atoms, and an alicyclic hydrocarbon group having 5 to 7 carbon atoms.
[0039] In one embodiment of the present invention, in the above general formula (1), R 1 and R 2 may each independently be, but is not limited to, a hydrogen atom, methyl, ethyl, propyl, isopropyl, n-butyl, sec-butyl, tert-butyl, isobutyl, pentyl, hexyl, heptyl, octyl, nonyl, decyl, cyclopentyl, cyclohexyl, cycloheptyl, cyclooctyl, cyclononyl, or cyclodecyl. 1 and R 2 may each independently be a hydrogen atom, methyl, ethyl, propyl, isopropyl, n-butyl, sec-butyl, tert-butyl, isobutyl, cyclopentyl, cyclohexyl, or cycloheptyl.
[0040] In one embodiment of the present invention, in the above general formulas (1) and (2), R 3 and R 4 are each independently selected from a hydrogen atom, a non-cyclic hydrocarbon group having 1 to 4 carbon atoms, a halogen atom, and a substituted or unsubstituted phenyl group.
[0041] In one embodiment of the present invention, in the above general formulas (1) and (2), R 3 and R 4 may each independently be, but is not limited to, a hydrogen atom, methyl, ethyl, propyl, isopropyl, n-butyl, sec-butyl, tert-butyl, isobutyl, pentyl, hexyl, heptyl, octyl, nonyl, decyl, chloro, fluoro, bromo, iodo, or phenyl. 3 and R 4may each independently be a hydrogen atom, methyl, ethyl, propyl, isopropyl, n-butyl, sec-butyl, tert-butyl, or isobutyl.
[0042] In the present invention, the polycarbonate resin (A) may be a polycarbonate ester of bisphenol.
[0043] In one embodiment of the present invention, the bisphenol may be selected from the group consisting of, for example, but not limited to, bisphenol A, bisphenol AP, bisphenol Z, bisphenol CD, bisphenol C, bisphenol IOTD, bisphenol IBTD and bisphenol MIBK.
[0044] In one embodiment of the present invention, the polycarbonate resin (A) may be a polycarbonate ester of bisphenol A.
[0045] The polycarbonate resin (A) used in the present invention can be produced by a conventional method.
[0046] 3. Polycondensate (B) In the present invention, the polycondensate (B) is selected from at least one resin selected from the following polyester resin (B1), polycarbonate resin (B2), and polyester carbonate resin (B3). The polycondensate (B) can be produced by any of the conventional methods.
[0047] (1) Polyester resin (B1) In the present invention, the polyester resin (B1) contains, in its diol constituent units, (i) a diol (a1) having a spiro ring-containing cyclic acetal skeleton; (ii) a diol (b1) having a non-spiro ring-containing cyclic acetal skeleton, and / or an alicyclic diol (b2); The polyester resin (B1) may further contain, in its diol constituent units, a diol other than the above.
[0048] In one embodiment of the present invention, the polyester resin (B1) may contain, in its diol constituent units, (i) a diol (a1) having a spiro ring-containing cyclic acetal skeleton in an amount of more than 60 mol%, for example, 61 mol%, 62 mol%, 63 mol%, 64 mol%, 65 mol%, 66 mol%, 67 mol%, 68 mol%, 69 mol%, 70 mol%, 71 mol%, 72 mol%, 73 mol%, 74 mol%, 75 mol%, 80 mol%, 85 mol%, 90 mol%, 95 mol%, 99 mol%, or 100 mol%.
[0049] In one embodiment of the present invention, the polyester resin (B1) may contain, in its diol constituent units, (ii) a diol (b1) having a non-spiro ring-containing cyclic acetal skeleton and / or an alicyclic diol (b2) in an amount of less than 40 mol%, for example, 39 mol%, 38 mol%, 37 mol%, 36 mol%, 35 mol%, 34 mol%, 33 mol%, 32 mol%, 31 mol%, 30 mol%, 29 mol%, 28 mol%, 27 mol%, 26 mol%, 25 mol%, 20 mol%, 15 mol%, 10 mol%, 5 mol%, 1 mol%, or 0 mol%.
[0050] In one embodiment of the present invention, the polyester resin (B1) has, in its diol constituent units, (i) 61 to 100 mol % of a diol (a1) having a spiro ring-containing cyclic acetal skeleton, (ii) It may contain 0 to 39 mol % of a diol (b1) having a non-spiro ring-containing cyclic acetal skeleton and / or an alicyclic diol (b2).
[0051] In one embodiment of the present invention, the polyester resin (B1) has, in its diol constituent units, (i) 65 to 100 mol % of a diol (a1) having a spiro ring-containing cyclic acetal skeleton, (ii) It may contain 0 to 35 mol % of a diol (b1) having a non-spiro ring-containing cyclic acetal skeleton and / or an alicyclic diol (b2).
[0052] In one embodiment of the present invention, the polyester resin (B1) has, in its diol constituent units, (i) 70 to 100 mol % of a diol (a1) having a spiro ring-containing cyclic acetal skeleton, (ii) It may contain 0 to 30 mol % of a diol (b1) having a non-spiro ring-containing cyclic acetal skeleton and / or an alicyclic diol (b2).
[0053] In one embodiment of the present invention, the polyester resin (B1) has, in its diol constituent units, (i) 75 to 100 mol % of a diol (a1) having a spiro ring-containing cyclic acetal skeleton, (ii) It may contain 0 to 25 mol % of a diol (b1) having a non-spiro ring-containing cyclic acetal skeleton and / or an alicyclic diol (b2).
[0054] In one embodiment of the present invention, the polyester resin (B1) has, in its diol constituent units, A diol (a1) having a spiro ring-containing cyclic acetal skeleton, and Diol having a non-spiro ring-containing cyclic acetal skeleton (b1) Includes.
[0055] In one embodiment of the present invention, the polyester resin (B1) has, in its diol constituent units, Diol (a1) having a spiro ring-containing cyclic acetal skeleton, A diol (b1) having a non-spiro ring-containing cyclic acetal skeleton, and Alicyclic diol (b2) Includes.
[0056] In one embodiment of the present invention, the dicarboxylic acid constituent unit of the polyester resin (B1) may be at least one selected from the group consisting of a terephthalic acid residue, an isophthalic acid residue, and a 1,4-cyclohexanedicarboxylic acid residue. In a preferred embodiment of the present invention, the dicarboxylic acid constituent unit of the polyester resin (B1) may be a terephthalic acid residue or a 1,4-cyclohexanedicarboxylic acid residue.
[0057] (2) Polycarbonate resin (B2) In the present invention, the polycarbonate resin (B2) contains, in its diol constituent units, (i) a diol (a1) having a spiro ring-containing cyclic acetal skeleton; (ii) a diol (b1) having a non-spiro ring-containing cyclic acetal skeleton, and / or an alicyclic diol (b2); The polyester resin (B2) may further contain a diol other than the above in its diol constituent units.
[0058] In one embodiment of the present invention, the polycarbonate resin (B2) may contain, in its diol constituent units, (i) a diol (a1) having a spiro ring-containing cyclic acetal skeleton in an amount greater than 0 mol%, for example, 1 mol%, 2 mol%, 5 mol%, 10 mol%, 15 mol%, 20 mol%, 25 mol%, 30 mol%, 35 mol%, 40 mol%, 45 mol%, 50 mol%, 55 mol%, 60 mol%, 65 mol%, 70 mol%, 75 mol%, 80 mol%, 85 mol%, 90 mol%, 95 mol%, 98 mol%, 99 mol%, or 100 mol%.
[0059] In one embodiment of the present invention, the polycarbonate (B2) may contain, in its diol constituent units, (ii) a diol (b1) having a non-spiro ring-containing cyclic acetal skeleton and / or an alicyclic diol (b2) in an amount of less than 100 mol%, for example, 99 mol%, 98 mol%, 95 mol%, 90 mol%, 85 mol%, 80 mol%, 75 mol%, 70 mol%, 65 mol%, 60 mol%, 55 mol%, 50 mol%, 45 mol%, 40 mol%, 35 mol%, 30 mol%, 25 mol%, 20 mol%, 15 mol%, 10 mol%, 5 mol%, 2 mol%, 1 mol%, or 0 mol%.
[0060] In one embodiment of the present invention, the polycarbonate resin (B2) has, in its diol constitutional unit, (i) 1 to 100 mol % of a diol (a1) having a spiro ring-containing cyclic acetal skeleton, (ii) It may contain 0 to 99 mol % of a diol (b1) having a non-spiro ring-containing cyclic acetal skeleton and / or an alicyclic diol (b2).
[0061] (3) Polyester carbonate resin (B3) In one embodiment of the present invention, the polyester carbonate resin (B3) has, as its diol constituent unit, (i) Diol having a spiro ring-containing cyclic acetal skeleton (a1) may include.
[0062] In one embodiment of the present invention, the polyester carbonate resin (B3) may contain, in its diol constituent units, (i) a diol (a1) having a spiro ring-containing cyclic acetal skeleton in an amount greater than 0 mol%, for example, 1 mol%, 2 mol%, 5 mol%, 10 mol%, 15 mol%, 20 mol%, 25 mol%, 30 mol%, 35 mol%, 40 mol%, 45 mol%, 50 mol%, 55 mol%, 60 mol%, 65 mol%, 70 mol%, 75 mol%, 80 mol%, 85 mol%, 90 mol%, 95 mol%, 98 mol%, 99 mol%, or 100 mol%.
[0063] In one embodiment of the present invention, the polyester carbonate resin (B3) has, in its diol constituent unit, (i) The diol (a1) having a spiro ring-containing cyclic acetal skeleton may be contained in an amount of 1 to 100 mol %.
[0064] In one embodiment of the present invention, the polyester carbonate resin (B3) may contain an alicyclic dicarboxylic acid or a diester thereof (b3) as a dicarboxylic acid constituent unit thereof. The polyester resin (B3) may further contain a diol other than the above in its diol constituent unit.
[0065] (4) Diol having a spiro ring-containing cyclic acetal skeleton (a1) In the present invention, the diol component (a1) having a spiro ring-containing cyclic acetal skeleton can be represented by general formula (3). [ka] (In the formula, R 5 and R 6 each independently represents a characteristic group selected from a non-cyclic hydrocarbon group having 1 to 10 carbon atoms, an alicyclic hydrocarbon group having 3 to 10 carbon atoms, and an aromatic hydrocarbon group having 6 to 10 carbon atoms.
[0066] In one embodiment of the present invention, in the above general formula (3), R 5 and R 6 may each independently be selected from a non-cyclic hydrocarbon group having 1 to 4 carbon atoms, an alicyclic hydrocarbon group having 5 to 7 carbon atoms, and a phenylene group.
[0067] In one embodiment of the present invention, in the above general formula (3), R 5 and R 6 may each independently be a methylene group, an ethylene group, a propylene group, a butylene group, or a structural isomer thereof, such as, but not limited to, a dimethylethylenyl group, an isopropylene group, an isobutylene group, or a phenylene group. 5 and R 6 may each independently be a methylene group, an ethylene group, a propylene group, a butylene group, or a dimethylethylenyl group.
[0068] In one embodiment of the present invention, the diol component (a1) having a spiro ring-containing cyclic acetal skeleton is 3,9-bis(1,1-dimethyl-2-hydroxyethyl)-2,4,8,10-tetraoxaspiro[5.5]undecane.
[0069] (5) Diol having a non-spiro ring-containing cyclic acetal skeleton (b1) In the present invention, the diol component (b1) having a non-spiro ring-containing cyclic acetal skeleton can be represented by general formula (4). [ka] (In the formula, R 5 is as above; R 7represents a characteristic group selected from acyclic hydrocarbon groups having 1 to 10 carbon atoms, alicyclic hydrocarbon groups having 3 to 10 carbon atoms, and aromatic hydrocarbon groups having 6 to 10 carbon atoms.
[0070] In one embodiment of the present invention, in the above general formula (4), R 5 may be selected from acyclic hydrocarbon groups having 1 to 4 carbon atoms, alicyclic hydrocarbon groups having 5 to 7 carbon atoms, and a phenylene group.
[0071] In one embodiment of the present invention, in the above general formula (4), R 5 may be, but is not limited to, a methylene group, an ethylene group, a propylene group, a butylene group, or a structural isomer thereof, such as a dimethylethylenyl group, an isopropylene group, an isobutylene group, or a phenylene group. 5 may be a methylene group, an ethylene group, a propylene group, a butylene group, or a dimethylethylenyl group.
[0072] In one embodiment of the present invention, in the above general formula (4), R 7 may be selected from a hydrogen atom, acyclic hydrocarbon groups having 1 to 4 carbon atoms, alicyclic hydrocarbon groups having 5 to 7 carbon atoms, and substituted or unsubstituted phenyl groups.
[0073] In one embodiment of the present invention, in the above general formula (4), R 7 may be, but is not limited to, a hydrogen atom, methyl, ethyl, propyl, isopropyl, n-butyl, sec-butyl, tert-butyl, isobutyl, pentyl, hexyl, heptyl, octyl, nonyl, decyl, cyclopropyl, cyclobutyl, cyclopentyl, cyclohexyl, cycloheptyl, cyclooctyl, cyclononyl, cyclodecyl, phenyl, o-methylphenyl, m-methylphenyl, p-methylphenyl. 7 may be a hydrogen atom, methyl, ethyl, propyl, isopropyl, n-butyl, sec-butyl, tert-butyl, isobutyl, or phenyl.
[0074] In one embodiment of the present invention, the diol component (b1) having a non-spiro ring-containing cyclic acetal skeleton is 5-methylol-5-ethyl-2-(1,1-dimethyl-2-hydroxyethyl)-1,3-dioxane.
[0075] (6) Alicyclic diol (b2) In the present invention, the alicyclic diol (b2) can be represented by general formula (5). [ka] (In the formula, R 8 , R 9 , R 10 and R 11 are each independently selected from a hydrogen atom and a non-cyclic hydrocarbon group having 1 to 6 carbon atoms; p, q, r and s are each independently 0, 1 or 2.
[0076] In one embodiment of the present invention, in the above general formula (5), R 8 , R 9 , R 10 and R 11 can be selected from a hydrogen atom and acyclic hydrocarbon groups having 1 to 4 carbon atoms.
[0077] In one embodiment of the present invention, in the above general formula (5), R 8 , R 9 , R 10 and R 11 may each independently be, but is not limited to, a hydrogen atom, methyl, ethyl, propyl, isopropyl, n-butyl, sec-butyl, tert-butyl, isobutyl, pentyl, or hexyl. 8 , R 9 , R 10 and R 11 may each independently be a hydrogen atom, methyl, ethyl, propyl, isopropyl, n-butyl, sec-butyl, tert-butyl, or isobutyl.
[0078] In one embodiment of the present invention, the alicyclic diol (b2) may be, but is not limited to, 1,4-cyclohexanedimethanol, 1,3-cyclopentanedimethanol, 1,3-cyclobutanedimethanol, 1,3-cyclobutanediol, 2,2,4,4-tetramethyl-1,3-cyclobutanediol.
[0079] In one embodiment of the present invention, the alicyclic diol (b2) is 1,4-cyclohexanedimethanol.
[0080] (7) Alicyclic dicarboxylic acids or their diesters (b3) In the present invention, the alicyclic dicarboxylic acid or diester thereof (b3) is represented by the general formula (6). [ka] (In the formula, R 8 , R 9 , R 10 , R 11 , R 12 , and R 13 each independently selected from a hydrogen atom and a non-cyclic hydrocarbon group having 1 to 6 carbon atoms; p and q are each independently 0, 1, or 2.
[0081] In one embodiment of the present invention, in the above general formula (6), R 8 , R 9 , R 10 , R 11 , R 12 , and R 13 can be selected from a hydrogen atom and acyclic hydrocarbon groups having 1 to 4 carbon atoms.
[0082] In one embodiment of the present invention, in the above general formula (6), R 8 , R 9 , R 10 , R 11 , R 12 , and R 13may each independently be, but is not limited to, a hydrogen atom, methyl, ethyl, propyl, isopropyl, n-butyl, sec-butyl, tert-butyl, isobutyl, pentyl, or hexyl. 8 , R 9 , R 10 and R 11 may each independently be a hydrogen atom, methyl, ethyl, propyl, isopropyl, n-butyl, sec-butyl, tert-butyl, or isobutyl.
[0083] In one embodiment of the present invention, the alicyclic dicarboxylic acid or its diester (b3) may be, but is not limited to, 1,4-cyclohexanedicarboxylic acid, dimethyl 1,4-cyclohexanedicarboxylate, or diethyl 1,4-cyclohexanedicarboxylate.
[0084] In one embodiment of the present invention, the alicyclic dicarboxylic acid or diester thereof (b3) is 1,4-cyclohexanedicarboxylic acid or dimethyl 1,4-cyclohexanedicarboxylate.
[0085] 4. Physical Properties of Thermoplastic Resin Composition (C) The thermoplastic resin composition (C) of the present invention can adjust the refractive index of the polycarbonate resin even with a smaller alloy ratio while maintaining the transparency of the polycarbonate resin, and can also have high heat resistance. The thermoplastic resin composition (C) of the present invention was evaluated according to the following items.
[0086] (1) Glass transition temperature (Tg) The thermoplastic resin composition (C) of the present invention may have a glass transition temperature of 90° C. or more and 160° C. or less. In one embodiment of the present invention, the thermoplastic resin composition (C) may have a glass transition temperature of, for example, 90° C. or more, 95° C. or more, 100° C. or more, 105° C. or more, 110° C. or more, 115° C. or more, 120° C. or more, 125° C. or more, 130° C. or more, 135° C. or more, 140° C. or more, 145° C. or more, 150° C. or more, but is not limited thereto. In one embodiment of the present invention, the thermoplastic resin composition (C) may have a glass transition temperature of, for example, 110° C. or more and less than 130° C., 130° C. or more and less than 140° C., 140° C. or more and less than 149° C., 149° C. or more and 160° C. or less, but is not limited thereto.
[0087] The glass transition temperature can be measured by a conventional method, for example, by using a differential scanning calorimeter.
[0088] (2) Total light transmittance The thermoplastic resin composition (C) of the present invention may have a total light transmittance of 87% or more for an injection molded article having a thickness of 1 mm. In one embodiment of the present invention, the thermoplastic resin composition (C) may have a total light transmittance of 87%, 88%, 89%, 90%, 91%, 92%, 93%, 94%, 95%, 96%, 97%, 98%, 99%, 100%, etc. for an injection molded article having a thickness of 1 mm.
[0089] The total light transmittance can be measured by a conventional method, for example, in accordance with JIS K7105 using a color / turbidity simultaneous measuring instrument (model: COH-400) manufactured by Nippon Denshoku Industries Co., Ltd.
[0090] (3) Cloud value The thermoplastic resin composition (C) of the present invention may have a haze of 4% or less when injected into a 1 mm-thick article. In one embodiment of the present invention, the thermoplastic resin composition (C) may have a total light transmittance of, for example, 4.0%, 3.5%, 3.0%, 2.5%, 2.0%, 1.5%, 1.0%, 0.5%, 0.3%, 0.1%, 0%, etc. when injected into a 1 mm-thick article.
[0091] The haze value can be measured by a conventional method, for example, according to JIS K7105 using a color / turbidity simultaneous measuring instrument (model: COH-400) manufactured by Nippon Denshoku Industries Co., Ltd.
[0092] (4) Refractive index The thermoplastic resin composition (C) of the present invention may have a refractive index measured by the critical angle method of 1.45 to 1.60. In one embodiment of the present invention, the thermoplastic resin composition (C) may have a refractive index measured by the critical angle method of, for example, 1.45 to 1.60, 1.45 to 1.58, 1.45 to 1.57, 1.45 to 1.56, 1.45 to 1.55, 1.45 to 1.54, 1.45 to 1.50, 1.50 to 1.60, 1.50 to 1.58, 1.50 to 1.57, 1.50 to 1.56, 1.50 to 1.55, 1.50 to 1.54, 1. The refractive index of the thermoplastic resin composition (C) measured by the critical angle method may be, but is not limited to, 1.54 to 1.60, 1.54 to 1.58, 1.54 to 1.57, 1.54 to 1.56, 1.54 to 1.55, 1.55 to 1.60, 1.55 to 1.58, 1.55 to 1.57, 1.55 to 1.56, 1.56 to 1.60, 1.56 to 1.58, 1.56 to 1.57, 1.57 to 1.60, 1.57 to 1.58, 1.58 to 1.60, 1.59 to 1.60, etc. In one embodiment of the present invention, the refractive index of the thermoplastic resin composition (C) measured by the critical angle method may be, but is not limited to, 1.50 or more and less than 1.54, 1.54 or more and less than 1.56, 1.56 or more and less than 1.57, 1.57 or more and less than 1.58, etc.
[0093] In the present invention, the refractive index can be measured by the critical angle method using an injection molded body having a thickness of 1.0 mm in accordance with JIS K7142 using a multi-wavelength Abbe refractometer (model: DR-M2) manufactured by Atago Co., Ltd., but is not limited to this method.
[0094] In one embodiment of the present invention, the thermoplastic resin composition (C) is (i) A glass transition temperature measured by a differential scanning calorimeter of 130°C or higher (ii) A 1 mm thick injection molded article has a total light transmittance of 87% or more and a haze value of 4% or less. (iii) A refractive index measured by the critical angle method is 1.45 to 1.60 It may be.
[0095] In another embodiment of the present invention, the thermoplastic resin composition (C) is (i) A glass transition temperature measured by a differential scanning calorimeter is 149°C or higher and 160°C or lower. (ii) A 1 mm thick injection molded article has a total light transmittance of 87% or more and a haze value of 4% or less. (iii) A refractive index measured by the critical angle method is 1.57 or more and 1.58 or less. It may be.
[0096] In yet another embodiment of the present invention, the thermoplastic resin composition (C) is (i) A glass transition temperature measured by a differential scanning calorimeter is 140°C or higher and less than 149°C. (ii) A 1 mm thick injection molded article has a total light transmittance of 87% or more and a haze value of 4% or less. (iii) A refractive index measured by the critical angle method is 1.56 or more and less than 1.57 It may be.
[0097] In yet another embodiment of the present invention, the thermoplastic resin composition (C) is (i) A glass transition temperature measured by a differential scanning calorimeter is 130°C or higher and less than 140°C. (ii) A 1 mm thick injection molded article has a total light transmittance of 87% or more and a haze value of 4% or less. (iii) A refractive index measured by the critical angle method is 1.54 or more and less than 1.56 It may be.
[0098] 5. Sheet using thermoplastic resin composition (C) A sheet can be produced using the thermoplastic resin composition (C) of the present invention. In one embodiment of the present invention, the sheet obtained using the thermoplastic resin composition (C) of the present invention may have a total light transmittance of 87% or more when the sheet is 500 μm thick. The sheet obtained using the thermoplastic resin composition (C) of the present invention may have a total light transmittance of 87%, 88%, 89%, 90%, 91%, 92%, 93%, 94%, 95%, 96%, 97%, 98%, 99%, 100%, etc. when the sheet is 500 μm thick.
[0099] 6. Film using thermoplastic resin composition (C) A film can be produced using the thermoplastic resin composition (C) of the present invention. In one embodiment of the present invention, the film obtained using the thermoplastic resin composition (C) of the present invention may have a haze value of 4% or less when the film is 50 μm thick. The film obtained using the thermoplastic resin composition (C) of the present invention may have a haze value of 4.0%, 3.5%, 3.0%, 2.5%, 2.0%, 1.5%, 1.0%, 0.5%, 0.3%, 0.1%, 0%, etc. when the film is 50 μm thick.
[0100] 7. Blend composition (E) with other thermoplastic resin composition (D) The thermoplastic resin composition (C) of the present invention can be blended with another thermoplastic resin composition (D) to produce a blend composition (E). The thermoplastic resin composition (C) of the present invention and the other thermoplastic resin composition (D) can be blended by a conventional method.
[0101] In one embodiment of the present invention, the difference in refractive index between the thermoplastic resin composition (C) and the thermoplastic resin composition (D) measured by the critical angle method may be 0.02 or less. If the difference in refractive index between the thermoplastic resin composition (C) and the thermoplastic resin composition (D) is 0.02 or less, the transparency of the blend composition (E) obtained by blending can be ensured. In one embodiment of the present invention, the difference in refractive index between the thermoplastic resin composition (C) and the thermoplastic resin composition (D) measured by the critical angle method may be, for example, 0.02, 0.01, 0.005, 0.002, 0, etc.
[0102] The other thermoplastic resin composition (D) used to produce the blend composition (E) by blending with the thermoplastic resin composition (C) of the present invention is preferably one having a refractive index difference of 0.02 or less from that of the thermoplastic resin composition (C) and not impairing heat resistance, as described above. In one embodiment of the present invention, the thermoplastic resin composition (D) may be a thermoplastic resin composition containing at least one thermoplastic resin selected from polyetherester resins, polyamide resins, acrylic resins, polyvinyl chloride resins, and polycarbonate resins. EXAMPLES
[0103] The present invention will now be described in more detail with reference to examples and comparative examples. The methods for synthesizing samples used in the evaluation of the examples and comparative examples, and the methods for measuring their physical properties are as follows. The meanings of abbreviations are also described. DMT: Dimethyl terephthalate ·TBT: Tetra-n-butyl titanate EG: Ethylene glycol 1,4-CHDM: 1,4-Cyclohexanedimethanol SPG: 3,9-bis(1,1-dimethyl-2-hydroxyethyl)-2,4,8,10-tetraoxaspiro[5.5]undecane TEP: Triethyl phosphate DOG: 5-methylol-5-ethyl-2-(1,1-dimethyl-2-hydroxyethyl)-1,3-dioxane
[0104] 1. Preparation of polycondensate (B) In the present invention, the polycondensate (B) can be selected from at least one resin selected from the polyester resin (B1), the polycarbonate resin (B2), and the polyester carbonate resin (B3), as described above.
[0105] (Production of Polyester Resin (B1-1) (Production Example 1)) DMT (31.7 mol), germanium oxide (0.016 mol), TBT in EG solution (0.0019 mol as TBT), and a mixed solution of 1,4-CHDM and EG (6.5 mol of 1,4-CHDM and 28.1 mol of EG) were charged into a 30 liter (L) polyester production apparatus equipped with a packed column type rectification column, a partial condenser, a total condenser, a cold trap, an agitator, a heating device, and a nitrogen inlet tube. The temperature was raised to 225°C under normal pressure and nitrogen atmosphere to carry out an ester exchange reaction. After the reaction conversion rate of the dicarboxylic acid component was 85 mol% or more, a potassium acetate in EG solution (0.0063 mol as potassium acetate) was added. EG was extracted from the system by reducing the temperature to 185°C and reducing the pressure to 13.3 kPa at the same time. After the pressure was restored, SPG (22.5 mol) was added. The temperature was raised to 225°C and the pressure was gradually reduced to 13.3kPa to allow the ester exchange reaction to proceed, and the pressure was then restored and TEP (0.098 mol) was added. After the pressure was reduced to 13.3kPa again, the polycondensation reaction was finally carried out at 280°C and 0.3kPa or less. The viscosity of the reactant gradually increased, and the reaction was terminated when it reached an appropriate melt viscosity, to obtain the polyester resin (B1-1) of the present invention.
[0106] (Production of Polyester Resin (B1-2) (Production Example 2)) A polyester resin (B1-2) was obtained by the same operation as in Production Example 1, except that the DMT was 30.7 mol, the germanium oxide was 0.015 mol, the EG solution of TBT (0.0018 mol as TBT), the mixed solution of 1,4-CHDM and EG (6.3 mol of 1,4-CHDM, 25.7 mol of EG), the potassium acetate solution of EG (0.0061 mol as potassium acetate), the SPG was 23.4 mol, and the TEP was 0.095 mol.
[0107] (Production of Polyester Resin (B1-3) (Production Example 3)) DMT (1.1 mol), germanium oxide (0.00055 mol), TBT in EG solution (0.00007 mol as TBT), and a mixed solution of 1,4-CHDM and EG (0.22 mol of 1,4-CHDM, 0.97 mol of EG) were charged into a 1 liter (L) polyester manufacturing apparatus equipped with a packed column type rectification column, a partial condenser, a cold trap, an agitator, a heating device, and a nitrogen inlet tube. The temperature was raised to 225°C under normal pressure and nitrogen atmosphere to carry out an ester exchange reaction. After the reaction conversion rate of the dicarboxylic acid component was increased to 70 mol% or more, a potassium acetate in EG solution (0.0002 mol as potassium acetate) was added. EG was extracted from the system by reducing the temperature to 185°C and reducing the pressure to 13.3 kPa at the same time. After the pressure was restored, SPG (0.72 mol) was added. The temperature was raised to 225°C and the pressure was gradually reduced to 13.3kPa to allow the ester exchange reaction to proceed, and the pressure was then restored and TEP (0.0034 mol) was added. After the pressure was reduced to 13.3kPa again, the polycondensation reaction was finally carried out at 280°C and 0.3kPa or less. The viscosity of the reactant gradually increased, and the reaction was terminated when it reached an appropriate melt viscosity, to obtain the polyester resin (B1-3) of the present invention.
[0108] (Production of Polyester Resin (B1-4) (Production Example 4)) DMT (1.0 mol), DOG (0.21 mol), germanium oxide (0.00051 mol), EG solution of TBT (0.00006 mol as TBT), and EG (0.90 mol) were charged into a 1 liter (L) polyester manufacturing apparatus equipped with a packed column type rectification column, a partial condenser, a cold trap, an agitator, a heating device, and a nitrogen inlet tube. The temperature was raised to 225°C under normal pressure and nitrogen atmosphere to carry out an ester exchange reaction. After the reaction conversion rate of the dicarboxylic acid component was increased to 70 mol% or more, an EG solution of potassium acetate (0.0002 mol as potassium acetate) was added. EG was extracted from the system by reducing the temperature to 185°C and reducing the pressure to 13.3 kPa at the same time. After the pressure was restored, SPG (0.72 mol) was added. The temperature was raised to 225°C and the pressure was gradually reduced to 13.3kPa to allow the ester exchange reaction to proceed, and the pressure was then restored and TEP (0.0031 mol) was added. After the pressure was reduced to 13.3kPa again, the polycondensation reaction was finally carried out at 280°C and 0.3kPa or less. The viscosity of the reactant gradually increased, and the reaction was terminated when it reached an appropriate melt viscosity, to obtain the polyester resin (B1-4) of the present invention.
[0109] (Production of Polyester Resin (B1-5) (Production Example 5)) DMT (1.0 mol), germanium oxide (0.00052 mol), TBT in EG solution (0.00006 mol as TBT), DOG (0.11 mol) and a mixed solution of 1,4-CHDM and EG (0.14 mol of 1,4-CHDM and 0.92 mol of EG) were charged into a 1 liter (L) polyester production apparatus equipped with a packed column type rectification column, a partial condenser, a cold trap, an agitator, a heating device and a nitrogen inlet tube. The temperature was raised to 225°C under normal pressure and nitrogen atmosphere to carry out an ester exchange reaction. After the reaction conversion rate of the dicarboxylic acid component was increased to 70 mol% or more, a potassium acetate in EG solution (0.0002 mol as potassium acetate) was added. EG was extracted from the system by reducing the temperature to 185°C and reducing the pressure to 13.3 kPa at the same time. After the pressure was restored, SPG (0.74 mol) was added. The temperature was raised to 225°C and the pressure was gradually reduced to 13.3kPa to allow the ester exchange reaction to proceed, and the pressure was then restored and TEP (0.0032 mol) was added. After the pressure was reduced to 13.3kPa again, the polycondensation reaction was finally carried out at 280°C and 0.3kPa or less. The viscosity of the reactant gradually increased, and the reaction was terminated when it reached an appropriate melt viscosity, to obtain the polyester resin (B1-5) of the present invention.
[0110] (Production of Polyester Resin (B1-6) (Production Example 6)) DMT (1.5 mol), germanium oxide (0.00073 mol), TBT in EG solution (0.00009 mol as TBT), and a mixed solution of 1,4-CHDM and EG (0.15 mol of 1,4-CHDM and 1.47 mol of EG) were charged into a 1 liter (L) polyester production apparatus equipped with a packed column type rectification column, a partial condenser, a cold trap, an agitator, a heating device, and a nitrogen inlet tube. The temperature was raised to 225°C under normal pressure and nitrogen atmosphere to carry out an ester exchange reaction. After the reaction conversion rate of the dicarboxylic acid component was increased to 70 mol% or more, a potassium acetate in EG solution (0.0003 mol as potassium acetate) was added. EG was extracted from the system by reducing the temperature to 185°C and reducing the pressure to 13.3 kPa at the same time. After the pressure was restored, SPG (0.45 mol) was added. The temperature was raised to 225°C and the pressure was gradually reduced to 13.3kPa to allow the ester exchange reaction to proceed, and the pressure was then restored and TEP (0.0045 mol) was added. After the pressure was reduced to 13.3kPa again, the polycondensation reaction was finally carried out at 280°C and 0.3kPa or less. The viscosity of the reactant gradually increased, and the reaction was terminated when it reached an appropriate melt viscosity, to obtain the polyester resin (B1-6) of the present invention.
[0111] (Production of Polycarbonate Resin (B2-1) (Production Example 7)) 2 kg (6.57 mol) of spiroglycol, 643 g (2.82 mol) of bisphenol A, 2.1 kg (9.72 mol) of diphenyl carbonate, and 0.0047 g (5.6 × 10 -5(mol) was placed in a 10-liter reactor equipped with a stirrer and a distillation device, heated to 215 ° C. for 1 hour under a nitrogen atmosphere of 150 Torr, and stirred. Then, the temperature was increased to 230 ° C. for 10 minutes, and the temperature was increased to 230 ° C. for 1 hour under conditions of 230 ° C. and 150 Torr to allow the transesterification reaction to proceed. Then, the temperature was increased to 240 ° C. for 10 minutes, and the transesterification reaction was allowed to proceed at 240 ° C. for 50 minutes. Then, the pressure was adjusted to 100 Torr for 10 minutes, and the pressure was increased to 240 ° C. for 20 minutes. Then, the pressure was adjusted to 40 Torr for 10 minutes, and the pressure was increased to 240 ° C. for 30 minutes under conditions of 40 Torr. Then, the pressure was reduced to 1 Torr or less for 20 minutes, and the polymerization reaction was allowed to proceed under stirring at 240 ° C. for 1 hour under conditions of 1 Torr or less. After the reaction was completed, nitrogen was blown into the reactor to apply pressure, and the produced resin was discharged while being pelletized, to obtain a polycarbonate resin (B2-1).
[0112] (Production of Polycarbonate Resin (B2-2) (Production Example 8)) 1.5 kg (4.9 mol) of spiroglycol, 1.12 kg (4.9 mol) of bisphenol A, 2.2 kg (10.2 mol) of diphenyl carbonate, and 0.0050 g (5.9 × 10 -5 The same operations as in Production Example 7 were carried out except that the amount of methyl ethyl ketone (B2-1) was changed to 1.0 moles, thereby obtaining a polycarbonate resin (B2-2).
[0113] (Production of Polycarbonate Resin (B2-3) (Production Example 9)) 300 g (0.99 mol) of spiroglycol, 2.02 kg (8.87 mol) of bisphenol A, 2.2 kg (10.2 mol) of diphenyl carbonate, and 0.0050 g (5.9 × 10 -5 The same operations as in Production Example 7 were carried out except that the amount of methyl ketone was changed to 1.0 moles, thereby obtaining a polycarbonate resin (B2-3).
[0114] (Production of Polycarbonate Resin (B2-4) (Production Example 10)) 1200 g (3.9 mol) of spiroglycol, 1.5 kg (6.6 mol) of bisphenol A, 2.9 kg (13.6 mol) of diphenyl carbonate, and 0.0066 g (7.9 × 10 -5 The same operations as in Production Example 7 were carried out except that 380 g (2.6 mol) of 1,4-CHDM was added at the same time, to obtain a polycarbonate resin (B2-4).
[0115] (Production of Polycarbonate Resin (B2-5) (Production Example 11)) 1200 g (3.9 mol) of spiroglycol, 1.5 kg (6.6 mol) of bisphenol A, 2.9 kg (13.6 mol) of diphenyl carbonate, and 0.0066 g (7.9 × 10 -5 The same operations as in Production Example 7 were carried out except that 570 g (2.6 mol) of DOG was added at the same time, thereby obtaining a polycarbonate resin (B2-5).
[0116] (Production of Polycarbonate Resin (B2-6) (Production Example 12)) 1200 g (3.9 mol) of spiroglycol, 1.5 kg (6.6 mol) of bisphenol A, 2.9 kg (13.6 mol) of diphenyl carbonate, and 0.0066 g (7.9 × 10 -5 The same operations as in Production Example 7 were carried out except that 190 g (1.3 mol) of 1,4-CHDM and 290 g (1.3 mol) of DOG were added at the same time, to obtain a polycarbonate resin (B2-6).
[0117] (Production of Polycarbonate Resin (B2-7) (Production Example 13)) Instead of spiroglycol, 948 g (6.6 mol) of 1,4-CHDM, 1.5 kg (6.6 mol) of bisphenol A, 2.9 kg (13.6 mol) of diphenyl carbonate, and 0.0066 g (7.9 × 10 -5 The same operations as in Production Example 7 were carried out except that the amount of methyl ethyl ketone (B2-1) was changed to 1.0 moles, thereby obtaining a polycarbonate resin (B2-7).
[0118] (Production of polyester carbonate resin (B3-1) (Production Example 14)) A 1-liter reactor equipped with a stirrer, a distillation condenser, a thermometer, and a gas inlet tube was charged with 300 g (0.99 mol) of SPG, 96 g (0.29 mol) of DMT, 41 g (0.20 mol) of dimethyl 1,4-cyclohexanedicarboxylate, and 0.08 g of dibutyltin oxide, and reacted for 6 hours at a temperature of 180 to 230 ° C. under a nitrogen atmosphere to distill off methanol. The terminal hydroxyl value of the obtained prepolymer was 3.0. Next, 57 g (0.26 mol) of diphenyl carbonate was added to 300 g of the prepolymer, and the reaction was continued for 5 hours at a temperature of 230 to 240 ° C., finally at a reduced pressure of 1 mmHg. After the reaction was completed, nitrogen was blown into the reactor to apply pressure, and the produced resin was pelletized and extracted to obtain polyester carbonate resin (B3-1).
[0119] (Production of polyester carbonate resin (B3-2) (Production Example 15)) A 1-liter reactor equipped with a stirrer, a fractionating condenser, a thermometer, and a gas inlet tube was charged with 300 g (0.99 mol) of SPG, 47 g (0.33 mol) of CHDM, 128 g (0.66 mol) of DMT, and 0.09 g of dibutyltin oxide, and reacted for 6 hours at a temperature of 180 to 230 ° C. under a nitrogen atmosphere to distill off methanol. The terminal hydroxyl value of the obtained prepolymer was 2.8. Next, 53 g (0.25 mol) of diphenyl carbonate was added to 300 g of the prepolymer, and the reaction was carried out for 5 hours at a temperature of 230 to 240 ° C., finally at a reduced pressure of 1 mmHg. After the reaction was completed, nitrogen was blown into the reactor to apply pressure, and the produced resin was pelletized and extracted to obtain polyester carbonate resin (B3-2).
[0120] (Production of polyester carbonate resin (B3-3) (Production Example 16)) A 1-liter reactor equipped with a stirrer, a fractionating condenser, a thermometer, and a gas inlet tube was charged with 300 g (0.99 mol) of SPG, 95 g (0.66 mol) of CHDM, 160 g (0.82 mol) of DMT, and 0.11 g of dibutyltin oxide, and reacted for 6 hours at a temperature of 180 to 230 ° C. under a nitrogen atmosphere to distill off methanol. The terminal hydroxyl value of the obtained prepolymer was 3.0. Next, 57 g (0.26 mol) of diphenyl carbonate was added to 300 g of the prepolymer, and the reaction was carried out for 5 hours at a temperature of 230 to 240 ° C., finally at a reduced pressure of 1 mmHg. After the reaction was completed, nitrogen was blown into the reactor to apply pressure, and the produced resin was pelletized and extracted to obtain polyester carbonate resin (B3-3).
[0121] (Production of polyester carbonate resin (B3-4) (Production Example 17)) In a 1-liter reactor equipped with a stirrer, a fractionating condenser, a thermometer, and a gas inlet tube, 100 g (0.69 mol) of CHDM, 129 g (2.1 mol) of EG, 270 g (1.4 mol) of DMT, and 0.09 g of dibutyltin oxide were charged, and the mixture was reacted for 6 hours at a temperature of 180 to 230 ° C. under a nitrogen atmosphere to distill off methanol. The terminal hydroxyl value of the obtained prepolymer was 3.1. Next, 59 g (0.27 mol) of diphenyl carbonate was added to 300 g of the prepolymer, and the mixture was reacted for 5 hours at a temperature of 230 to 240 ° C., finally at a reduced pressure of 1 mmHg. After the reaction was completed, nitrogen was blown into the reactor to apply pressure, and the produced resin was pelletized and extracted to obtain polyester carbonate resin (B3-4).
[0122] (Evaluation of polycondensate (B)) The polycondensate (B) was evaluated by the following methods. The evaluation results are shown in Tables 1, 2 and 3.
[0123] (1) Diol units having a cyclic acetal skeleton and alicyclic diol units in the diol constituent units of the polycondensation product The diol units having a cyclic acetal skeleton and the alicyclic diol units in the diol constituent units of the polycondensate were calculated by 1H-NMR measurement. The measurement was performed using a BRUKER AVANCEIII500 at 500MHz. Deuterated chloroform was used as the solvent.
[0124] (2) Glass transition temperature The glass transition temperature (Tg) of the polycondensate was measured by placing about 10 mg of a sample in an aluminum non-sealed container in a nitrogen gas (50 ml / min) flow at a temperature rise rate of 20°C / min using a DSC / TA-50WS manufactured by Shimadzu Corporation. The temperature at which the temperature changed by half the difference in the baseline before and after the transition of the DSC curve was taken as the glass transition temperature.
[0125] In Tables 1, 2, and 3, 1,4-cyclohexanedimethanol is abbreviated as "CHDM," 3,9-bis(1,1-dimethyl-2-hydroxyethyl)-2,4,8,10-tetraoxaspiro[5.5]undecane is abbreviated as "SPG," 5-methylol-5-ethyl-2-(1,1-dimethyl-2-hydroxyethyl)-1,3-dioxane is abbreviated as "DOG," and bisphenol A is abbreviated as "BPA."
[0126] [Table 1]
[0127] [Table 2]
[0128] [Table 3]
[0129] As product 1, a polyester resin (product name: ALTESTER (registered trademark) "S3000", copolymerization ratio of diol components: SPG 30 mol %, EG 70 mol %, Tg: 103° C.) manufactured by Mitsubishi Gas Chemical Company, Inc. was used.
[0130] As product 2, a polyester resin manufactured by Eastman Chemical Company (product name: EASTAR (registered trademark) "GN001", copolymerization rate of diol component: CHDM 43 mol%, EG 57 mol%, Tg: 83°C) was used.
[0131] [Table 4]
[0132] [Examples 1 to 84, Comparative Examples 1 to 12] The polycarbonate resins used were: (A-1): polycarbonate resin (product name: Iupilon (registered trademark) S-3000) manufactured by Mitsubishi Engineering Plastics Corporation; (A-2): polycarbonate resin (product name: Iupilon (registered trademark) H-4000) manufactured by Mitsubishi Engineering Plastics Corporation; and (A-3): polycarbonate resin (product name: Iupilon (registered trademark) E-2000) manufactured by Mitsubishi Engineering Plastics Corporation.
[0133] 2. Preparation of Thermoplastic Resin Composition (C) The polycarbonate resin (A) and polycondensate (B) were mixed in the amounts shown in Tables 5 to 24 in a tumbler. This resin mixture was melt-mixed in a twin-screw extruder (screw diameter: 20 mm, L / D: 25) under conditions of a cylinder temperature of 265 to 285°C, a die temperature of 265 to 285°C, and a screw rotation speed of 50 rpm.
[0134] 3. Preparation of injection molded bodies The thermoplastic resin composition (C) was molded into various test pieces having a thickness of 1.0 mm using a screw-type injection molding machine (screw diameter: 28 mm, mold clamping force: 490 kN) under conditions of a cylinder temperature of 260 to 280°C and a mold temperature of 30 to 70°C.
[0135] 4. Sheet Preparation The thermoplastic resin composition (C) was produced into a 500 μm thick sheet by the T-die method using a twin-screw extruder (screw diameter: 29.75 mm, L / D: 30) under conditions of a cylinder temperature of 265 to 285°C, a T-die temperature of 265 to 285°C, and a screw rotation speed of 50 rpm.
[0136] 5. Film Preparation The 500 μm thick sheet produced under the conditions described above was simultaneously biaxially stretched 3.0 × 3.0 times at a temperature 10 to 20°C higher than the glass transition temperature of the thermoplastic resin composition (C) to produce a 50 μm thick film.
[0137] [Evaluation method] The resin compositions of Examples 1 to 84 and Comparative Examples 1 to 12 were evaluated as follows. The evaluation results are summarized in Tables 5 to 24.
[0138] (1) Haze value, total light transmittance: The measurements were carried out using a 1.0 mm thick injection molded product, a 500 μm thick sheet, and a 50 μm thick film in accordance with JIS K7105. The measuring device used was a color / turbidity simultaneous measuring instrument (model: COH-400) manufactured by Nippon Denshoku Industries Co., Ltd.
[0139] (2) Refractive index: The measurement was carried out using an injection molded article having a thickness of 1.0 mm in accordance with JIS K7142. The measuring device used was a multi-wavelength Abbe refractometer (model: DR-M2) manufactured by Atago Co., Ltd.
[0140] [Table 5]
[0141] [Table 6]
[0142] [Table 7]
[0143] [Table 8]
[0144] [Table 9]
[0145]
Table 10
[0146]
Table 11
[0147]
Table 12
[0148]
Table 13
[0149]
Table 14
[0150]
Table 15
[0151]
Table 16
[0152]
Table 17
[0153]
Table 18
[0154]
Table 19
[0155]
Table 20
[0156] [Table 21]
[0157] [Table 22]
[0158] [Table 23]
[0159] [Table 24]
[0160] Example 85 (1) Measurement of refractive index of thermoplastic resin composition (D) As the thermoplastic resin composition (D), (D-1): polyether ester resin (trade name: ELECUT (registered trademark) R02) manufactured by Takemoto Oil Co., Ltd. was used. This was molded into a test piece having a thickness of 1.0 mm using a screw-type injection molding machine (screw diameter: 28 mm, mold clamping force: 490 kN) under conditions of a cylinder temperature of 260°C and a mold temperature of 50°C. The refractive index of the molded product thus produced was measured in accordance with JIS K7142 using a multi-wavelength Abbe refractometer (model: DR-M2) manufactured by Atago Co., Ltd. The refractive index value obtained was 1.560.
[0161] (2) Preparation of Thermoplastic Resin Composition (C) As polycarbonate resin (A), (A-1): 60 wt% polycarbonate resin (trade name: Iupilon (registered trademark) S-3000) manufactured by Mitsubishi Engineering Plastics Co., Ltd., and 40 wt% B1-1 (Table 1, Production Example 1) as polycondensate (B) were mixed by a tumbler. This resin mixture was melt-mixed using a twin-screw extruder (screw diameter: 20 mm, L / D: 25) under conditions of cylinder temperature 265 ° C, die temperature 265 ° C, and screw rotation speed 50 rpm to obtain a thermoplastic resin composition (C-6) (Table 5). Then, using a screw-type injection molding machine (screw diameter: 28 mm, mold clamping force: 490 kN), the mixture was molded into a test piece having a thickness of 1.0 mm under conditions of cylinder temperature 265 ° C and mold temperature 50 ° C. The refractive index of the molded product was measured in accordance with JIS K7142 using a multi-wavelength Abbe refractometer (model: DR-M2) manufactured by Atago Co., Ltd. The refractive index value obtained was 1.560.
[0162] (3) Preparation of injection molded article of blend composition (E) 20 wt% of the thermoplastic resin composition (D-1) and 80 wt% of the thermoplastic resin composition (C-6) were mixed in a tumbler. This resin mixture was molded into various test pieces having a thickness of 1.0 mm using a screw-type injection molding machine (screw diameter: 28 mm, mold clamping force: 490 kN) under conditions of a cylinder temperature of 265°C and a mold temperature of 50°C.
[0163] [Evaluation method] The blend composition of Example 85 was evaluated as follows. The evaluation results are shown in Table 25.
[0164] (1) Haze value, total light transmittance: The measurement was carried out using a 1.0 mm thick injection molded article in accordance with JIS K7105. The measuring device used was a color / turbidity simultaneous measuring device (model: COH-400) manufactured by Nippon Denshoku Industries Co., Ltd.
[0165] (2) Refractive index: The measurement was carried out using an injection molded article having a thickness of 1.0 mm in accordance with JIS K7142. The measuring device used was a multi-wavelength Abbe refractometer (model: DR-M2) manufactured by Atago Co., Ltd.
[0166] [Table 25]
[0167] As described above, the thermoplastic resin composition (C) of the present invention and the blend composition (E) with another thermoplastic resin composition (D) can not only adjust the refractive index of the polycarbonate resin even with a smaller alloy ratio while maintaining the transparency of the polycarbonate resin, but also have high heat resistance.
Claims
1. A thermoplastic resin composition (C) comprising a polycarbonate resin (A) and a polycondensate (B), The thermoplastic resin composition (C) contains 40 to 99% by weight of the polycarbonate resin (A) and 60 to 1% by weight of the polycondensate (B); and The polycondensate (B) is selected from a polyester resin (B1), a polycarbonate resin (B2), or a polyester carbonate resin (B3), The polyester resin (B1) contains, in its diol constituent units, (i) 65 to 75 mol % of a diol (a1) having a spiro ring-containing cyclic acetal skeleton, (ii) containing 0 to 20 mol % of a diol (b1) having a non-spiro ring-containing cyclic acetal skeleton and / or an alicyclic diol (b2); The polycarbonate resin (B2) contains, in its diol constituent units, (i) 10 to 30 mol % of a diol (a1) having a spiro ring-containing cyclic acetal skeleton, (ii) 0 to 20 mol % of a diol (b1) having a non-spiro ring-containing cyclic acetal skeleton and / or an alicyclic diol (b2); (iii) containing 50 to 90 mol % bisphenol A; The polyester carbonate resin (B3) contains, in its diol constituent units, (i) containing 60 to 100 mol % of a diol (a1) having a spiro ring-containing cyclic acetal skeleton, The polycarbonate resin (A) is a polycarbonate ester of bisphenol, the diol component (a1) having a spiro ring-containing cyclic acetal skeleton is 3,9-bis(1,1-dimethyl-2-hydroxyethyl)-2,4,8,10-tetraoxaspiro[5.5]undecane, the diol component (b1) having a non-spiro ring-containing cyclic acetal skeleton is 5-methylol-5-ethyl-2-(1,1-dimethyl-2-hydroxyethyl)-1,3-dioxane, the alicyclic diol (b2) is 1,4-cyclohexanedimethanol, the dicarboxylic acid constituent unit of the polyester resin (B1) is a dicarboxylic acid unit selected from at least one of a terephthalic acid residue, an isophthalic acid residue, and a 1,4-cyclohexanedicarboxylic acid residue, The dicarboxylic acid constituent unit of the polyester carbonate (B3) contains an alicyclic dicarboxylic acid or a diester thereof (b3), The thermoplastic resin composition (C), wherein the alicyclic dicarboxylic acid or its diester (b3) is 1,4-cyclohexanedicarboxylic acid or dimethyl 1,4-cyclohexanedicarboxylate.
2. The thermoplastic resin composition (C) according to claim 1, wherein the bisphenol is selected from the group consisting of bisphenol A, bisphenol AP, bisphenol Z, bisphenol CD, bisphenol C, bisphenol IOTD, bisphenol IBTD and bisphenol MIBK.
3. The polyester resin (B1) has, in its diol constituent units, The diol (a1) having a spiro ring-containing cyclic acetal skeleton, The diol (b1) having a non-spiro ring-containing cyclic acetal skeleton, and The alicyclic diol (b2) The thermoplastic resin composition (C) according to claim 1 or 2, comprising:
4. The thermoplastic resin composition (C) according to any one of claims 1 to 3, having the following physical properties (i) to (iii): (i) A glass transition temperature measured by a differential scanning calorimeter of 130°C or higher (ii) A 1 mm thick injection molded article has a total light transmittance of 87% or more and a haze value of 4% or less. (iii) A refractive index measured by the critical angle method is 1.45 to 1.
60.
5. A sheet obtained by using the thermoplastic resin composition (C) according to any one of claims 1 to 4, the sheet having a total light transmittance of 87% or more when it is 500 µm thick.
6. A film obtained by using the thermoplastic resin composition (C) according to any one of claims 1 to 4, the haze of which when measured at a thickness of 50 µm is 4% or less.
7. A blend composition (E) of the thermoplastic resin composition (C) according to any one of claims 1 to 4 and a thermoplastic resin composition (D), wherein the difference in refractive index between the thermoplastic resin composition (C) and the thermoplastic resin composition (D) measured by a critical angle method is 0.02 or less.
8. The blend composition (E) according to claim 7, wherein the thermoplastic resin composition (D) is a thermoplastic resin composition containing at least one thermoplastic resin selected from the group consisting of polyetherester resins, polyamide resins, acrylic resins, polyvinyl chloride resins, and polycarbonate resins.
Citation Information
Patent Citations
Surface hardening of metal base
JP1979045652A
Polycarbonate resin composition
JP1998251500A
Transparent face plate for outdoor use
JP2000063641A
Thermoplastic resin composition
JP2003246925A
Polyester resin
JP2005002237A