Manufacturing method of coated pipe

By controlling the speed difference between the resin pipe and foam-covered pipe to within 2%, the method addresses foam shrinkage issues in foam-covered pipe manufacturing, enhancing production efficiency and preventing peeling.

JP7559648B2Active Publication Date: 2024-10-02MITSUBISHI CHEMICAL INFRATEC CO LTD
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
JP2021055633
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-03-29
Publication Date
2024-10-02
Estimated Expiration
2041-03-29

AI Technical Summary

Technical Problem

Existing methods for manufacturing foam-covered pipes face issues with shrinkage of the foam material due to high resistance during passage through a cylindrical former, leading to peeling and reduced production efficiency, especially for pipes with small diameters or thick foam sheets.

Method used

The method involves continuously feeding a resin pipe and foam sheet into a former, rolling the foam sheet around the pipe, heating and melting the side edges, and controlling the speed difference between the resin pipe and foam-covered pipe to within 2% to suppress shrinkage by matching their speeds.

Benefits of technology

This approach effectively suppresses the shrinkage rate of the foam material, maintaining production efficiency and preventing peeling, even at high line speeds of 10 m/min or higher.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007559648000002
    Figure 0007559648000002
  • Figure 0007559648000003
    Figure 0007559648000003
  • Figure 0007559648000004
    Figure 0007559648000004
Patent Text Reader

Abstract

To provide a method for manufacturing foam material coated pipe that can suppress the shrinkage rate of the coated foam material after it is taken back.SOLUTION: A method of manufacturing a coated pipe 8 continuously covering a resin pipe by feeding resin pipe 2 and foam material sheet 4 each continuously to former 6, encircling resin pipe 2 by rounding up the foam material sheet 4, heating and melting the side edges of the foam material sheet 4 in the width direction, and then fusion bonding the side edges together in the former 6, so that the measured speed difference of the foam material coated pipe to the resin pipe speed is within 2%.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing a foam-coated pipe in which a resin pipe is coated with a resin foam (thermal insulation material). [Background technology]

[0002] Pipes for supplying cold water and hot water, particularly in cold regions, are made of resin pipes covered with resin foam material.

[0003] The method for manufacturing this coated pipe involves continuously feeding a pipe and a foam sheet (sheet-like foam) through a cylindrical former, covering the resin pipe with the sheet-like foam, joining both ends of the sheet (the mating ends) by thermal fusion, and continuously taking up the foam-coated pipe with a take-up machine.

[0004] In this method, the foam sheet is formed into a cylindrical shape by passing it through a cylindrical former. Therefore, particularly in the case of a foam-coated pipe with a small diameter or a pipe covered with a foam sheet that is thicker than the diameter, the resistance of the foam sheet when passing through the cylindrical former is large. As a result, the coated foam material coming out of the former is stretched by the take-up force of the take-up machine. After passing through the take-up machine, the stretched coated foam material shrinks in the longitudinal direction of the resin pipe. The ratio of the shrinkage length of the coated foam material to the unit length of the resin pipe is hereinafter referred to as the shrinkage rate of the coated foam material.

[0005] Methods for suppressing the shrinkage of such covering foam material include shortening the cylindrical former to reduce the resistance to passage and reducing the take-up speed. However, shortening the cylindrical former causes problems such as peeling of the fused joint surface due to insufficient cooling, and reducing the take-up speed reduces production efficiency.

[0006] In order to solve these problems, methods have been proposed in which the inner diameter side of the former is knurled or threaded to reduce the contact area between the former and the covering material and thereby reduce the passage resistance (Japanese Utility Model Application Publication No. 6-55728), a method in which multiple guide rollers are placed on the inner diameter side of the former to reduce the passage resistance (Japanese Patent Publication No. 2003-127220), and a method in which a liner or tape is placed between the outer surface of the foamed material and the inner diameter side of the former to reduce the passage resistance (Japanese Patent No. 5271131, Japanese Patent Publication No. 07-241905).

[0007] However, this method requires a complex former structure and a large number of parts, which means it takes time and costs to manufacture a former for each aperture size.In addition, it is difficult to perform additional processing to adjust the inner diameter of the former, which is related to passage resistance, fusion and crimping, and joining. [Prior art documents] [Patent documents]

[0008] [Patent Document 1] Japanese Utility Model Application Publication No. 6-55728 [Patent Document 2] JP 2003-127220 A [Patent Document 3] Patent No. 5271131 [Patent Document 4] Japanese Patent Application Publication No. 07-241905 Summary of the Invention [Problem to be solved by the invention]

[0009] An object of the present invention is to provide a method for producing a foam-coated pipe, which is capable of suppressing the shrinkage rate of the foam-coated pipe after withdrawal. [Means for solving the problem]

[0010] The method for manufacturing a foam-coated pipe of the present invention involves continuously feeding a resin pipe and a foam material sheet into a former, rolling the foam material sheet to surround the resin pipe, heating and melting the widthwise side ends of the foam material sheet, and then fusion-joining the side ends in the former to continuously coat the resin pipe.The method for manufacturing a foam-coated pipe of the present invention is characterized in that it includes a feeder for feeding the resin pipe at a constant speed before it is passed through the cylindrical former, a first speed counter for measuring the feed speed of the resin pipe between the feeder and the cylindrical former, and a second speed counter for measuring the feed speed of the foam-coated pipe fed from the take-up machine on the outer surface of the coating material, and the difference between the speed of the resin pipe measured by the first speed counter and the speed of the foam-coated pipe measured by the second speed counter is within 2%.

[0011] In one embodiment of the present invention, if the feed speed setting value of the resin pipe feed machine is Va, the feed speed of the resin pipe measured by the first speed gauge is Vb, the set speed of the take-up machine is Vc, and the feed speed of the foam-coated pipe measured by the second gauge is Vd, then Va=Vb=Vd, Vc>Vd are satisfied.

[0012] In one embodiment of the present invention, the line speed (resin pipe feed speed) is set to 10 m / min or more. Effect of the Invention

[0013] According to the method for producing a coated pipe of the present invention, a resin pipe and a foaming material sheet are continuously fed to a former, the foaming material sheet is rolled to surround the resin pipe, the side ends in the width direction of the foaming material sheet are heated and melted, and then the side ends are fused together in the former to continuously coat the resin pipe. In this method for producing a foaming material coated pipe, the foaming material sheet (coated foaming material) coated on the outer surface of the resin pipe is fed faster than the resin pipe between the former and the take-off machine, so that the foaming material sheet (coated foaming material) that was delayed in the cylindrical former is returned to its original position, and the speeds of the resin pipe and the foaming material sheet (coated foaming material) are roughly equalized at the time of leaving the take-off machine. This suppresses the shrinkage rate of the coated foaming material. [Brief description of the drawings]

[0014] [Figure 1] 4A to 4C are side views showing a method for manufacturing a coated pipe according to an embodiment. [Diagram 2] 2A, 2B, 2C, and 2D are cross-sectional views taken along lines IIa-IIa, IIb-IIb, IIc-IIc, and IId-IId in FIG. 1, respectively. [Diagram 3] 1A to 1C are schematic cross-sectional views illustrating a method for producing a coated pipe according to an embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0015] In one embodiment of the method for producing a coated pipe of the present invention, a resin pipe and a foaming material sheet are each continuously fed into a former, the foaming material sheet is rolled into a cylindrical shape at the introduction section of the former to surround the resin pipe with the foaming material sheet, the widthwise side ends (mating end faces) of the foaming material sheet are heated and melted, and then these opposing side ends are fusion-joined to each other in the former, thereby continuously producing a coated pipe.

[0016] In the present invention, the resin pipe is preferably a polyolefin pipe having a diameter of 5 to 50 mm, particularly 10 to 30 mm. The foamed material sheet is preferably a polyolefin pipe having a thickness of 3 to 20 mm, particularly 5 to 10 mm. Examples of polyolefin include cross-linked polyethylene, non-cross-linked polyethylene, and polypropylene.

[0017] Next, a method for producing such a foam-coated pipe will be described with reference to FIGS.

[0018] A resin pipe 2 manufactured by extrusion molding and rolls 1 and 3 each wrapped with a strip-shaped foaming sheet 4 that has been previously foamed and has a film on the outside are set on the upstream side of the manufacturing process line. The foaming sheet 4 continuously drawn out from the roll 3 is aligned with the resin pipe 2 that is continuously drawn out from the roll 1 and fed by a resin pipe feeder 10. Then, at the introduction section of the former 6, the foaming sheet 4 is rolled up to surround the resin pipe 2, as shown in Figure 2(b).

[0019] Just before entering the cylindrical former 6, a pair of side ends (mating end faces) of the foam material sheet 4 are heated and melted by a heater 5, and the foam material sheet 4 is passed through an inner hole of the cylindrical former 6 so that the ends are butted together, and while being squeezed, the mating end faces are pressed together and pressure-bonded. As a result, a coated pipe 8 is formed in which the periphery of the resin pipe 2 is coated with the coating foam material made of the foam material sheet 4, and the coated pipe 8 passes through the cylindrical former 6 and comes out. The coated pipe 8 coming out of the cylindrical former 6 is continuously taken up by a take-up machine 7 and wound up by a winding machine 9 downstream in the manufacturing process.

[0020] This coated pipe manufacturing apparatus is provided with a measuring device 11 for measuring the feed speed of the resin pipe 2, a measuring device 12 for measuring the take-up speed of the coated pipe 8, other measuring devices necessary for quality control, and a control device for controlling the feed speed and take-up speed of the feed machine 10 and the take-up machine 7 (specifically, controlling the rotation speed of the drive motor), etc. The taking-up speed measuring device 12 measures the speed of the outer surface of the coating foam material of the coated pipe 8.

[0021] The resin pipe 2 is fed at a constant speed by the resin pipe feeder 10. As described above, the foam material sheet 4 is fed together with the resin pipe 2 and rolled up around the resin pipe 2. Just before entering the cylindrical former 6, both side portions of the foam material sheet 4 along the feeding direction are heated and melted by the heater 5. Inside the cylindrical former 6, the both side portions are pressed together and the foam material sheet 4 passes through the cylindrical former 6.

[0022] As described above, inside the cylindrical former 6, the foaming material sheet 4 moves while being in contact with the inner wall of the former 6, so the foaming material sheet 4 decelerates due to contact resistance with the inner wall of the former 6, and becomes slower than the speed of the resin pipe 2. For this reason, the covering foaming material coming out of the former 6 is stretched by the take-up force of the take-up machine 7. After passing through the take-up machine 7, the stretched covering foaming material shrinks in the longitudinal direction of the resin pipe 2.

[0023] Therefore, in this embodiment, the take-up speed by the take-up machine 7 is made faster than the feed speed of the resin pipe 2, and the surface of the foam material sheet 4 covering the outer surface of the resin pipe 2 is fed between the former 6 and the take-up machine 7 faster than the speed of the resin pipe 2, thereby causing the foam material sheet 4 (coated foam material) that was delayed inside the cylindrical former 6 to return to its original position (make up for the delay), and by making the speeds of the resin pipe 2 and the foam material sheet 4 (coated foam material) approximately match at the time they leave the take-up machine 7 (the difference between the two is within 2% of the feed speed of the resin pipe 2), the shrinkage rate of the coated foam material is suppressed.

[0024] Preferably, when the feed speed setting value of the resin pipe feeder 10 is Va, the feed speed of the resin pipe 2 measured by the speed gauge 11 is Vb, the set speed of the take-up machine 7 is Vc, and the feed speed of the foamed material-coated pipe 8 measured by the gauge 12 is Vd, Va=Vb=Vd, Vc>Vd This allows the take-up machine 7 to return only the outer covering foam sheet 4.

[0025] In the take-up machine 7, it is common practice to firmly chuck the entire covering foam material to prevent it from shifting, but in this embodiment, the chucking force is loosened appropriately so as not to hinder the advancement of the foam material sheet 4.

[0026] If the take-up machine 7 is used in a general normal manner in which the resin pipe 2 and the covering foam material are firmly chucked together to prevent them from slipping, not only the covering foam material but also the resin pipe 2 will be firmly chucked, resulting in [take-up machine set speed (Vc)] = [resin pipe feed speed (Vb) measured by the speed meter]. Therefore, if the take-up machine 7 is used to return only the covering foam material 4, and the set speed (Vc) of the take-up machine is set to be greater than the set feed speed (Va) of the resin pipe feeder, then Vc = Vb > Va, and the resin pipe feed speed measured by the speed meter will be greater than the set feed speed (Vb) of the resin pipe, which is greater than the set feed speed (Va) of the resin pipe feeder, and this will not hold unless slippage occurs between the resin pipe feeder and the resin pipe. If slippage occurs between the resin pipe feeder and the resin pipe, the length of the resin pipe, which is the standard length of the covering foam material, will fluctuate, and the shrinkage rate of the covering foam material will become unstable.

[0027] The present invention exerts a more excellent effect of suppressing the shrinkage rate under high-speed conditions of a line speed of 10 m / min or more. This is because the resistance during passage through the cylindrical former 6 increases as the line speed increases. EXAMPLES

[0028] [Examples 1 and 2, Comparative Examples 1 to 3] 1 to 3, coated pipes were manufactured at various feed rates, and the shrinkage rates of the coating materials in the manufactured foam-coated pipes were measured. The results are shown in Table 1.

[0029] In this example and the comparative example, a cross-linked polyethylene resin pipe having a pipe size of 10A (outer diameter 13 mm) and a polyethylene foam sheet having a thickness of 10 mm were used.

[0030] Comparative Examples 1 and 2 relate to a conventional method for manufacturing a foam-covered pipe.

[0031] Examples 1 and 2 relate to the method of the present invention, and show the case where the difference between the measured velocity of the resin pipe (Vb) and the measured velocity of the foam-coated pipe (Vd) is set to 0%.

[0032] Comparative Example 3 shows a case where the difference between the measured velocity of the resin pipe (Vb) and the measured velocity of the foam-coated pipe (Vd) was 6.2%.

[0033] [Table 1]

[0034] As shown in Table 1, in Examples 1 and 2, the shrinkage rate of the covering foam material is suppressed more than in Comparative Example 3. [Explanation of symbols]

[0035] 2 Plastic pipe 4 Foam Sheets 5 Heater 6. Former 7. Coated pipe take-up machine 8. Coated Pipe 10 Resin pipe feeder 11 Plastic pipe feed speed measuring device 12. Insulated pipe withdrawal speed measuring device

Claims

1. The resin pipe and the foaming material sheet are fed into the former in succession. The foam sheet is rolled to surround the resin pipe; In the method for producing a foam-coated pipe, the foam sheet is heated and melted at its widthwise side edges, and then the side edges are fused and joined together in the former to continuously cover a resin pipe, A feeder is provided for feeding the resin pipe at a constant speed before passing it through the cylindrical former, a first speed meter is provided for measuring the feeding speed of the resin pipe between the feeder and the cylindrical former, and a second speed meter is provided for measuring the feeding speed of the foamed material-coated pipe fed from the take-up machine on the outer surface of the coating material, A method for manufacturing a foam-coated pipe, characterized in that the difference between the speed of the resin pipe measured by the first speed gauge and the speed of the foam-coated pipe measured by the second speed gauge is within 2%.

2. When the feed speed setting value of the feeder is Va, the feed speed of the resin pipe measured by the first speed gauge is Vb, the set speed of the take-off machine is Vc, and the feed speed of the foam-coated pipe measured by the second gauge is Vd, Va=Vb=Vd, Vc>Vd 2. The method for manufacturing a foam-covered pipe according to claim 1, wherein the above-mentioned condition is satisfied.

3. 3. The method for producing a foam-coated pipe according to claim 1, wherein the line speed is 10 m / min or more.

Citation Information

Patent Citations

  • Circuit for radiation display use

    JP1977071131A

  • Extrusion coating method

    JP1984118439A

  • Drawing dies for thermoplastic resin foam pipes

    JP1994055728U

  • Manufacture of foamed insulated wire and device therefor

    JP1994150747A

  • Manufacture of foamed pipe

    JP1995241905A