Elastomer composition and molded article
The use of a specific elastomer composition with 90% single-walled carbon nanotubes and controlled surface resistivity variation enables molded articles to achieve both high friction and low wear, addressing the trade-off issue in conventional compositions.
Patent Information
- Application Number
- JP2021508988
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-03-28
- Filing Date
- 2020-03-10
- Publication Date
- 2024-10-02
- Estimated Expiration
- 2040-03-10
AI Technical Summary
Molded articles formed using conventional elastomer compositions face a trade-off between high friction coefficient and low wear amount, making it difficult to achieve both properties simultaneously.
An elastomer composition containing 90% single-walled carbon nanotubes as a reinforcing filler and a coefficient of variation in surface resistivity of 20% or less is used to form a crosslinked sheet, which results in a molded article with high friction coefficient and low wear.
The composition allows for the production of molded articles with both high friction coefficient and low wear, suitable for applications such as belts, vibration-proof rubber, and outsoles.
Smart Images

Figure 0007559747000001
Abstract
Description
[Technical field]
[0001] The present invention relates to an elastomer composition and a molded article. [Background technology]
[0002] Fillers have been conventionally blended into elastomers for the purpose of providing reinforcement and various functions. In recent years, carbon nanotubes (hereinafter sometimes abbreviated as CNTs) have been attracting attention as a filler to be added to elastomers.
[0003] Specifically, Patent Document 1 proposes a technique for sufficiently improving both the flexibility of molded articles such as sealing members, as well as the tensile breaking energy at high temperatures and the tear strength at high temperatures, by using a composition containing a fibrous carbon nanostructure including single-walled CNTs in a specified ratio relative to a fluorine-containing elastomer. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] International Publication No. 2017 / 175807 Summary of the Invention [Problem to be solved by the invention]
[0005] Here, a molded article formed using the elastomer composition is required to have both high frictional force (i.e., a high coefficient of friction) and low wear (i.e., a low amount of wear).
[0006] However, in the case of molded articles formed using the above-mentioned conventional elastomer compositions, there is a trade-off between the friction coefficient and the wear amount, and there are cases in which a problem occurs in that increasing the friction coefficient results in an increase in the wear amount, and conversely, decreasing the wear amount results in a decrease in the friction coefficient.
[0007] Therefore, an object of the present invention is to provide an elastomer composition capable of forming a molded article having both a high friction coefficient and a low wear amount. Another object of the present invention is to provide a molded article that achieves both a high friction coefficient and a low wear rate. [Means for solving the problem]
[0008] The present inventors have conducted extensive research to solve the above problems, and have found that a molded article having both a high friction coefficient and a low wear amount can be formed by using an elastomer composition that contains an elastomer and a reinforcing filler in which single-walled carbon nanotubes account for a predetermined ratio, and that has a coefficient of variation of surface resistivity of a predetermined value or less when made into a crosslinked sheet, and have thus completed the present invention.
[0009] That is, the present invention aims to advantageously solve the above problems, and the elastomer composition of the present invention is an elastomer composition containing an elastomer and a reinforcing filler, the reinforcing filler containing carbon nanotubes, the proportion of single-walled carbon nanotubes in the reinforcing filler being 90 mass% or more, and the coefficient of variation of the surface resistivity of a crosslinked sheet obtained by crosslinking the elastomer composition is 20% or less. In this way, with an elastomer composition containing an elastomer and a reinforcing filler in which the proportion of single-walled CNTs is the above value or more, and in which the coefficient of variation of the surface resistivity of a crosslinked sheet obtained by crosslinking is the above value or less, a molded product that combines a high friction coefficient and a low wear amount can be formed. In the present invention, the "crosslinked sheet" used in measuring the surface resistivity can be prepared by the method described in the examples of this specification. In the present invention, the "surface resistivity" can be measured by the method described in the examples of this specification. Furthermore, in the present invention, the "coefficient of variation of surface resistivity" means "the value (%) obtained by dividing the standard deviation of the surface resistivity by the average value and multiplying the result by 100", and specifically, it can be determined using the method described in the examples of this specification.
[0010] In the elastomer composition of the present invention, the elastomer is preferably a fluorine-containing elastomer. If the elastomer in the elastomer composition is a fluorine-containing elastomer, heat resistance and chemical resistance can be improved.
[0011] In the elastomer composition of the present invention, the carbon nanotubes have a BET specific surface area of 600 m 2 When the BET specific surface area of the CNT is equal to or greater than the above value, the molded article can have both a high friction coefficient and a low wear amount at an even higher level. In the present invention, the "BET specific surface area" means a nitrogen adsorption specific surface area measured by the BET method, and can be measured, for example, by using a BET specific surface area meter.
[0012] In the elastomer composition of the present invention, the carbon nanotubes preferably have an average length of 10 μm or more. If the average length of the CNTs is equal to or greater than the above value, the molded article can have a high friction coefficient and a low wear amount at the same time at an even higher level. In the present invention, the "average length of carbon nanotubes" in the elastomer composition can be determined, for example, by scanning electron microscope (SEM) observation and image processing.
[0013] Here, the elastomer composition of the present invention preferably contains 0.1 to 4 parts by mass of carbon nanotubes per 100 parts by mass of the elastomer. If the ratio of the CNTs to the elastomer in the elastomer composition is within the above range, the molded article can have a high friction coefficient and a low wear rate at the same time at a higher level.
[0014] The elastomer composition of the present invention may further contain a crosslinking agent.
[0015] The present invention also aims to advantageously solve the above problems, and the molded article of the present invention is characterized in that it is obtained by crosslinking the above-mentioned elastomer composition. In this way, by crosslinking the above-mentioned elastomer composition, a molded article that achieves both a high friction coefficient and a low wear amount can be formed.
[0016] The molded article of the present invention can be advantageously used as any one of a belt, a vibration-proof rubber, a rubber roll, and an outsole, for example. Effect of the Invention
[0017] According to the present invention, it is possible to provide an elastomer composition capable of forming a molded article having both a high friction coefficient and a low wear amount. Moreover, according to the present invention, it is possible to provide a molded article that achieves both a high friction coefficient and a low wear amount. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0018] Hereinafter, an embodiment of the present invention will be described in detail. Here, the elastomer composition of the present invention can be used to form the molded article of the present invention. The molded article of the present invention is a crosslinked article formed using the elastomer composition of the present invention.
[0019] (Elastomer composition) The elastomeric compositions of the present invention contain an elastomer and a reinforcing filler, and optionally further contain a crosslinker and other ingredients. Here, the elastomer composition of the present invention is characterized in that it contains carbon nanotubes as a reinforcing filler, in which 90 mass% or more of the reinforcing filler is single-walled carbon nanotubes, and in that the coefficient of variation of the surface resistivity of a crosslinked sheet obtained by crosslinking the elastomer composition is 20% or less.
[0020] The elastomer composition of the present invention contains a reinforcing filler having a ratio of single-walled CNTs equal to or greater than the above value, and has a coefficient of variation of surface resistivity equal to or less than the above value when made into a crosslinked sheet, so that the use of the elastomer composition makes it possible to achieve both a high friction coefficient and a low wear amount in a molded article. Although the reason why the above effects are obtained by using the elastomer composition of the present invention is not clear, it is presumed to be as follows. First, in a molded body formed using an elastomer composition, the friction coefficient depends on the volume fraction of the elastomer in the elastomer composition, and the wear amount depends on the fracture energy of the elastomer composition. The friction coefficient of the molded body can be increased by reducing the amount of reinforcing filler added and increasing the volume fraction of the elastomer in the elastomer composition. Conversely, the wear amount of the molded body can be reduced by increasing the amount of reinforcing filler added and increasing the fracture energy of the elastomer composition. Thus, in a molded body obtained using a conventional elastomer composition, the friction coefficient and the wear amount are in a trade-off relationship, and it has generally been difficult to achieve both a high friction coefficient and a low wear amount of a molded body. However, since the reinforcing filler contained in the elastomer composition of the present invention is 90% by mass or more of single-walled CNTs, which have an extremely high reinforcing effect, it is possible to obtain a sufficiently high fracture energy by adding a small amount of reinforcing filler, which is believed to reduce the wear amount of the molded body while maintaining a high friction coefficient of the molded body. Here, in order to obtain the above-mentioned effect of the single-walled CNT, it is necessary that the dispersibility of the single-walled CNT in the molded body is good. If the single-walled CNT is not well dispersed in the molded body, it is not possible to obtain a sufficiently high fracture energy by adding a reinforcing filler containing the single-walled CNT. In contrast, the elastomer composition of the present invention has a coefficient of variation of surface resistivity of 20% or less when made into a crosslinked sheet. Here, the coefficient of variation of surface resistivity can be correlated with the degree of dispersion of the conductive CNT, and by using an elastomer composition having a coefficient of variation of surface resistivity of 20% or less when made into a crosslinked sheet, a molded body in which the single-walled CNT is well dispersed can be obtained. Therefore, it is considered that the above-mentioned effect of achieving both a high friction coefficient and a low wear amount due to the single-walled CNT can be obtained remarkably well. Therefore, by using the elastomer composition of the present invention, it is possible to achieve both a high friction coefficient and a low wear amount of a molded article. <Elastomer>
[0021] The elastomer contained in the elastomer composition is not particularly limited, and known elastomers can be used. Specifically, acrylonitrile-butadiene rubber (NBR), acrylonitrile-isoprene rubber, acrylonitrile-butadiene-isoprene rubber, styrene-butadiene rubber (SBR), butadiene rubber (BR), isoprene rubber (IR), natural rubber (NR), ethylene-propylene-diene rubber (EPDM), butyl rubber (IIR), and hydrogenated products thereof (hydrogenated acrylonitrile-butadiene rubber, hydrogenated acrylonitrile-isoprene rubber, hydrogenated acrylonitrile-butadiene-isoprene rubber, hydrogenated styrene-butadiene rubber, hydrogenated butadiene rubber, hydrogenated isoprene rubber, hydrogenated natural rubber, hydrogenated ethylene-propylene-diene rubber, hydrogenated butyl rubber). The above-mentioned elastomers also include those into which hydrophilic groups such as carboxylic acid groups, sulfonic acid groups, phosphoric acid groups, and hydroxyl groups have been introduced. These elastomers may be used alone or in combination of two or more.
[0022] Here, the elastomer contained in the elastomer composition is preferably a fluorine-containing elastomer from the viewpoint of excellent heat resistance, chemical resistance, etc. Examples of the fluorine-containing elastomer include tetrafluoroethylene-propylene rubber (FEPM), vinylidene fluoride rubber (FKM), tetrafluoroethylene-perfluoromethylvinyl ether rubber (FFKM), and tetrafluoroethylene rubber (TFE).
[0023] Among the above, as the fluorine-containing elastomer, vinylidene fluoride rubber (FKM) and tetrafluoroethylene-propylene rubber (FEPM) are preferable, and vinylidene fluoride rubber (FKM) is more preferable.
[0024] Here, vinylidene fluoride rubber (FKM) is a fluororubber that is mainly composed of vinylidene fluoride and has excellent heat resistance, oil resistance, chemical resistance, solvent resistance, and processability. FKM is not particularly limited, but examples thereof include a binary copolymer of vinylidene fluoride and hexafluoropropylene, a ternary copolymer of vinylidene fluoride, hexafluoropropylene, and tetrafluoroethylene, and a quaternary copolymer of vinylidene fluoride, hexafluoropropylene, tetrafluoroethylene, and a vulcanization site monomer. Examples of commercially available products include "Viton (registered trademark)" from Chemours Inc. and "Dai-el (registered trademark) G" from Daikin Industries, Ltd. Among them, a quaternary copolymer of vinylidene fluoride, hexafluoropyrene, tetrafluoroethylene, and a vulcanization site monomer is preferable. The quaternary copolymer is available, for example, as a commercial product "Viton GBL-600S" (manufactured by Chemours Inc.).
[0025] Tetrafluoroethylene-propylene rubber (FEPM) is a fluororubber based on an alternating copolymer of tetrafluoroethylene and propylene, and has excellent heat resistance, chemical resistance, polar solvent resistance, steam resistance, and the like. FEPM is not particularly limited, but examples thereof include a binary copolymer of tetrafluoroethylene and propylene, a ternary copolymer of tetrafluoroethylene, propylene, and vinylidene fluoride, and a ternary copolymer of tetrafluoroethylene, propylene, and a crosslinking point monomer. Commercially available products of binary copolymers of tetrafluoroethylene and propylene include "Aflas (registered trademark) 100" and "Aflas 150" from AGC Corporation. Commercially available products of ternary copolymers of tetrafluoroethylene, propylene, and vinylidene fluoride include "Aflas 200" from AGC Corporation. An example of a commercially available terpolymer consisting of tetrafluoroethylene, propylene, and a cross-linking point monomer is "Aflas 300" manufactured by AGC Corporation.
[0026] The content of the elastomer in the elastomer composition is preferably 85% by mass or more, more preferably 88% by mass or more, and is preferably 95% by mass or less, and more preferably 92% by mass or less. When the content of the elastomer in the elastomer composition is within the above-mentioned range, a molded article formed using the elastomer composition can have both a high friction coefficient and a low wear amount at an even higher level.
[0027] <Reinforcing filler> The reinforcing filler is a filler that can improve the strength (particularly the breaking energy) of a molded body obtained by crosslinking the elastomer composition by adding it to the elastomer composition. The reinforcing filler is usually a component that does not substantially participate in the crosslinking reaction of the elastomer when the elastomer composition is subjected to a crosslinking reaction, and contributes to improving the strength of the molded body by maintaining its shape (cylindrical, particulate) even in the molded body after crosslinking. Therefore, in the present invention, the reinforcing filler does not include, for example, substances that correspond to the crosslinking agent and crosslinking assistant described below. In addition, in the present invention, the reinforcing filler does not include the non-reinforcing filler described below that is blended for the purpose of increasing the amount or improving processability.
[0028] Here, the elastomer composition of the present invention needs to use CNTs containing single-walled CNTs as a reinforcing filler. The elastomer composition of the present invention may contain a reinforcing filler other than CNTs. However, from the viewpoint of further increasing the friction coefficient of the molded article, it is preferable that the elastomer composition of the present invention contains only CNTs as a reinforcing filler.
[0029] <<Carbon nanotubes>> The CNTs used as the reinforcing filler are not particularly limited as long as the proportion of single-walled CNTs in the entire reinforcing filler can be 90% by mass or more, and may be CNTs consisting of only single-walled CNTs or a mixture of single-walled CNTs and multi-walled CNTs. When a mixture of single-walled CNTs and multi-walled CNTs is used, the mixture must contain 90% by mass or more of single-walled CNTs.
[0030] The average diameter (Av) of the CNTs is preferably 0.5 nm or more, more preferably 1 nm or more, and preferably 15 nm or less, and more preferably 10 nm or less. If the average diameter (Av) of the CNTs is 0.5 nm or more, the CNTs can be well dispersed and arranged in the molded body. If the average diameter (Av) of the CNTs is 15 nm or less, the physical properties of the molded body can be further improved. Therefore, by having the average diameter (Av) of the CNTs within the above range, the molded body can have a high friction coefficient and a low wear amount at a higher level.
[0031] In addition, it is preferable that the CNTs have a t-plot obtained from the adsorption isotherm that shows a convex shape. In particular, it is more preferable that the CNTs are not subjected to an opening treatment and have a t-plot that shows a convex shape. If a CNT is used that has a t-plot obtained from the adsorption isotherm that shows a convex shape, it is possible to achieve a high friction coefficient and a low wear amount of the molded body at a higher level.
[0032] Generally, adsorption is a phenomenon in which gas molecules are removed from the gas phase to a solid surface, and is classified into physical adsorption and chemical adsorption depending on the cause. Physical adsorption is used in the nitrogen gas adsorption method used to obtain t-plots. Normally, if the adsorption temperature is constant, the number of nitrogen gas molecules adsorbed to CNTs increases with increasing pressure. Also, a plot of relative pressure (the ratio of the pressure P at adsorption equilibrium to the saturated vapor pressure P0) on the horizontal axis and the amount of nitrogen gas adsorption on the vertical axis is called an "isotherm." When the amount of nitrogen gas adsorption is measured while increasing the pressure, it is called an "adsorption isotherm," and when the amount of nitrogen gas adsorption is measured while decreasing the pressure, it is called a "desorption isotherm."
[0033] The t-plot is obtained by converting the relative pressure into the average thickness t (nm) of the nitrogen gas adsorption layer in the adsorption isotherm measured by the nitrogen gas adsorption method. That is, the t-plot of CNTs can be obtained by determining the average thickness t of the nitrogen gas adsorption layer corresponding to the relative pressure from a known standard isotherm in which the average thickness t of the nitrogen gas adsorption layer is plotted against the relative pressure P / P0 and performing the above conversion (the t-plot method by de Boer et al.).
[0034] Here, in a sample having pores on the surface, the growth of the nitrogen gas adsorption layer is classified into the following processes (1) to (3). The slope of the t-plot changes depending on the following processes (1) to (3). (1) The process of forming a monolayer of nitrogen molecules on the entire surface (2) Formation of multilayer adsorption and the associated capillary condensation filling process in the pores (3) The formation of multilayer adsorption on an apparently non-porous surface whose pores are filled with nitrogen
[0035] In the t-plot showing an upward convex shape, the plot is located on a straight line passing through the origin in the region where the average thickness t of the nitrogen gas adsorption layer is small, whereas as t increases, the plot shifts downward from the straight line. CNTs having such a t-plot shape have a large ratio of the internal specific surface area to the total specific surface area of the CNTs, indicating that many openings are formed in the CNTs.
[0036] The bending point of the t-plot of the CNT is preferably in the range of 0.2≦t(nm)≦1.5, more preferably in the range of 0.45≦t(nm)≦1.5, and even more preferably in the range of 0.55≦t(nm)≦1.0. When the bending point of the t-plot is in the above range, the characteristics of the CNT are further improved, so that the molded body can have both a high friction coefficient and a low wear amount at an even higher level. Here, the "position of the bending point" is the intersection point of the approximation line A in the above-mentioned process (1) and the approximation line B in the above-mentioned process (3) in the t-plot.
[0037] Furthermore, the ratio of the internal specific surface area S2 to the total specific surface area S1 (S2 / S1) of the CNT obtained from the t-plot is preferably 0.05 or more, more preferably 0.06 or more, even more preferably 0.08 or more, and preferably 0.30 or less. If S2 / S1 is 0.05 or more and 0.30 or less, the characteristics of the CNT can be further improved, so that the molded body can have both a high friction coefficient and a low wear amount at an even higher level.
[0038] Incidentally, the measurement of the adsorption isotherm of CNT, the creation of t-plots, and the calculation of the total specific surface area S1 and the internal specific surface area S2 based on the analysis of the t-plots can be performed using, for example, a commercially available measuring device, "BELSORP (registered trademark)-mini" (manufactured by BEL Japan, Inc.).
[0039] Here, it is preferable to use CNTs having a ratio (3σ / Av) of the standard deviation (σ) of the diameter multiplied by 3 to the average diameter (Av) of more than 0.20 and less than 0.80, more preferably CNTs having a 3σ / Av of more than 0.25, even more preferably CNTs having a 3σ / Av of more than 0.40, and particularly preferably CNTs having a 3σ / Av of more than 0.50. By using CNTs having a 3σ / Av of more than 0.20 and less than 0.80, it is possible to achieve both a high friction coefficient and a low wear amount of the molded body at an even higher level. The "average diameter (Av) of CNTs" and the "standard deviation of CNT diameters (σ: sample standard deviation)" can be determined by measuring the diameter (outer diameter) of 100 randomly selected CNTs using a transmission electron microscope. The average diameter (Av) and standard deviation (σ) of CNTs may be adjusted by changing the manufacturing method or manufacturing conditions of CNTs, or by combining multiple types of CNTs obtained by different manufacturing methods.
[0040] Here, the CNT has a BET specific surface area of 600 m 2 / g or more, and 2 / g or more is more preferable, and 2000m 2 / g or less, and 2 It is more preferable that the BET specific surface area of the single-walled CNT is 600 m 2 When the BET specific surface area of the single-walled CNT is 2000 m / g or more, the physical properties of the molded product can be further improved. 2 When the BET specific surface area is within the above range, the molded body can have a high friction coefficient and a low wear amount at the same time at a higher level.
[0041] In addition, the average length of the CNTs contained in the elastomer composition of the present invention is preferably 10 μm or more, more preferably 15 μm or more, and even more preferably 20 μm or more. If the average length of the CNTs as a reinforcing filler is 10 μm or more, the reinforcing effect of the CNTs (especially single-walled CNTs) is sufficiently large, so that a small amount of CNTs can provide high breaking energy. Therefore, the molded body can have a high friction coefficient and a low wear amount at a higher level. The upper limit of the average length of the CNTs is not particularly limited, but is usually 800 μm or less. Here, the average length of the CNTs contained in the elastomer composition can be determined by, for example, removing the elastomer from the elastomer composition, measuring the lengths of 100 CNTs, and averaging the measured values. The method for removing the elastomer from the elastomer composition is not particularly limited. For example, the elastomer in the elastomer composition is burned, and then a solvent is added to the resulting ash to elute the CNTs, which are then applied to the surface of a substrate for observation, thereby making it possible to make each CNT observable. A scanning electron microscope (SEM) or known image processing can be used to observe the CNTs.
[0042] CNTs having the above-mentioned properties can be efficiently manufactured by, for example, forming a catalyst layer on the substrate surface by a wet process in a method (super-growth method; see International Publication No. 2006 / 011655) in which a trace amount of oxidant (catalytic activation material) is present in the system when supplying raw material compounds and a carrier gas onto a substrate having a catalyst layer for CNT production on its surface and synthesizing CNTs by chemical vapor deposition (CVD) to dramatically improve the catalytic activity of the catalyst layer. Note that, hereinafter, carbon nanotubes obtained by the super-growth method may be referred to as "SGCNTs".
[0043] In the elastomer composition of the present invention, the proportion of the single-walled carbon nanotubes in the reinforcing filler must be 90% by mass or more, and preferably 92% by mass or more, based on the total amount of the reinforcing filler contained in the elastomer composition being 100% by mass. If the proportion of the single-walled carbon nanotubes in the reinforcing filler is less than 90% by mass, it is not possible to achieve both a high friction coefficient and a low wear amount of the molded article.
[0044] Furthermore, the elastomer composition of the present invention preferably contains CNTs in an amount of 0.1 part by mass or more per 100 parts by mass of elastomer, more preferably 0.2 parts by mass or more, even more preferably 0.4 parts by mass or more, and particularly preferably 0.5 parts by mass or more, preferably 4 parts by mass or less, more preferably 3 parts by mass or less, even more preferably 2.5 parts by mass or less, even more preferably 2 parts by mass or less, and particularly preferably 1 part by mass or less. If the CNT content in the elastomer composition is 0.1 parts by mass or more per 100 parts by mass of elastomer, a sufficiently high fracture energy can be obtained, and the wear amount of the molded article can be reduced. On the other hand, if the CNT content in the elastomer composition is 4 parts by mass or less per 100 parts by mass of elastomer, the volume fraction of the elastomer in the elastomer composition can be sufficiently high, and the friction coefficient of the molded article can be increased.
[0045] <<Reinforcing filler other than CNT>> Examples of the reinforcing filler other than CNT include carbon-based fillers other than CNT (for example, carbon black, graphene, graphite), silica, and the like.
[0046] Here, from the viewpoint of achieving a higher level of compatibility between the high friction coefficient and the low wear amount of the molded body, the elastomer composition of the present invention preferably does not contain a carbon-based filler other than carbon nanotubes and silica. For example, it preferably does not contain carbon black, graphene, graphite, and silica. In other words, the "elastomer composition comprising an elastomer and a reinforcing filler" of the present invention is preferably an "elastomer composition comprising an elastomer, carbon nanotubes, and not containing a carbon-based filler other than carbon nanotubes and silica" from the viewpoint of achieving a higher level of compatibility between the high friction coefficient and the low wear amount of the molded body. For example, it is preferably an "elastomer composition comprising an elastomer, carbon nanotubes, and not containing carbon black, graphene, graphite, and silica".
[0047] Here, the carbon black that can be used as the reinforcing filler is not particularly limited, and known carbon black that can be used in the elastomer composition can be used. Specifically, furnace black, acetylene black, thermal black, channel black, ketjen black, and the like can be mentioned. These carbon blacks can be used alone or in combination of two or more. Further, the particle diameter and structure of the carbon black are not particularly limited.
[0048] The silica that can be used as a reinforcing filler is not particularly limited, and any known silica that can be used in elastomer compositions can be used. Specific examples include colloidal silica, wet silica, amorphous silica, fumed silica, silica sol, and silica gel. These silicas can be used alone or in combination of two or more. The surface of the silica may be modified with a functional group such as hydrophilic or hydrophobic functional groups.
[0049] <Crosslinking agent> Here, the crosslinking agent that may be optionally contained in the elastomer composition of the present invention is not particularly limited. Specifically, the crosslinking agent may be a known crosslinking agent capable of crosslinking the elastomer contained in the elastomer composition. More specifically, the crosslinking agent may be, for example, sulfur, a peroxide-based crosslinking agent, triallyl isocyanurate, or the like. These crosslinking agents can be used alone or in combination of two or more. The amount of the crosslinking agent in the elastomer composition of the present invention is not particularly limited, but is preferably 1 part by mass or more, more preferably 3 parts by mass or more, and even more preferably 5 parts by mass or more, and is preferably 10 parts by mass or less, and more preferably 7 parts by mass or less, relative to 100 parts by mass of the elastomer.
[0050] <Other ingredients> The elastomer composition of the present invention may contain components (other components) other than the above components. For example, the elastomer composition may contain a known filler (non-reinforcing filler) other than the above-mentioned reinforcing filler. In addition, the elastomer composition may contain known additives such as a crosslinking aid and an antioxidant. Specifically, the filler other than the reinforcing filler is not particularly limited, and examples thereof that can be used include clay, talc, calcium carbonate, and barium sulfate. Furthermore, the crosslinking aid is not particularly limited, and examples thereof include zinc oxide and stearic acid. The antioxidant is not particularly limited, and an amine-based antioxidant, an imidazole-based antioxidant, or the like can be used. The other components may be used alone or in combination of two or more. The amount of the other components may be any amount as long as the desired effect is not inhibited.
[0051] <Variation coefficient of surface resistivity> Here, the elastomer composition of the present invention requires that the coefficient of variation of the surface resistivity of the crosslinked sheet obtained by crosslinking the elastomer composition is 20% or less, preferably 17% or less, and more preferably 14% or less. If the coefficient of variation of the surface resistivity of the crosslinked sheet exceeds 20%, the single-walled CNTs tend to aggregate in the crosslinked sheet (molded product). Therefore, the dispersibility of the single-walled CNTs in the crosslinked sheet (molded product) cannot be improved, and the molded product cannot have both a high friction coefficient and a low wear amount. Here, the lower limit of the coefficient of variation of the surface resistivity of the crosslinked sheet is not particularly limited, but can be, for example, 0.1% or more, 1% or more, or 5.9% or more. The coefficient of variation of the surface resistivity of the crosslinked sheet can be adjusted by changing the preparation method of the elastomer composition. For example, it can be adjusted by changing the number of passes of the bead mill dispersion treatment in the preparation process of the rubber kneaded product (elastomer composition). More specifically, the coefficient of variation of the surface resistivity of the crosslinked sheet can be reduced by increasing the number of passes of the bead mill dispersion treatment.
[0052] <Preparation of Elastomer Composition> Here, the elastomer composition can be prepared, for example, by mixing or kneading the above-mentioned elastomer, a reinforcing filler in which single-walled CNTs account for a specified ratio, and an optional crosslinking agent and other components in a desired compounding ratio.
[0053] The elastomer composition is preferably prepared through a step of obtaining a mixture (master batch) of an elastomer and CNTs (master batch preparation step), and a step of kneading the obtained mixture (master batch) with optional components such as a reinforcing filler other than CNTs, a crosslinking agent, and other components (kneading step). By premixing the elastomer and CNTs in the absence of a reinforcing filler other than CNTs, a crosslinking agent, and other components, the aggregation of the CNTs in the elastomer can be suppressed and the CNTs can be well dispersed, thereby reducing the coefficient of variation of the surface resistivity of a given crosslinked sheet.
[0054] [Masterbatch preparation process] The master batch can be prepared by any mixing method capable of dispersing CNTs in an elastomer. The master batch is preferably prepared, for example, by adding CNTs to an elastomer solution obtained by dissolving an elastomer in an organic solvent, or an elastomer dispersion obtained by dispersing an elastomer in a dispersion medium, dispersing the CNTs using a high-speed emulsifying and dispersing device or a wet jet mill to prepare a slurry, and then removing the organic solvent or the dispersion medium from the resulting dispersion treatment liquid as a slurry.
[0055] Here, as described above, by changing the number of passes of the dispersion treatment (the number of times the dispersion target passes through a dispersing device such as a high-speed emulsifying and dispersing device or a wet jet mill), the variation coefficient of the surface resistivity of the crosslinked sheet obtained by crosslinking the elastomer composition can be adjusted. From the viewpoint of dispersing the CNTs well, the number of passes is preferably 2 or more, and more preferably 3 or more. The upper limit of the number of passes is not particularly limited, but can be, for example, 20 or less from the viewpoint of the preparation efficiency of the master batch.
[0056] The solvent or dispersion medium can be removed by, for example, a coagulation method, a casting method, or a drying method. Alternatively, when preparing the master batch, it is of course possible to directly knead the elastomer and CNTs by a known kneading method as described below, without using a solvent.
[0057] [Mixing process] Furthermore, when adding optional components such as reinforcing fillers other than CNTs, crosslinking agents and other components to the master batch obtained as described above and kneading them, for example, a mixer, a single-screw kneader, a twin-screw kneader, a roll, a Brabender, an extruder, etc. can be used. The kneading conditions can be appropriately adjusted so that the CNTs can be appropriately dispersed. In addition, when the reinforcing filler consists only of CNTs, it is not necessary to add reinforcing fillers other than CNTs, and in the present invention, it is preferable not to add reinforcing fillers other than CNTs. In the kneading step, an elastomer may be additionally added.
[0058] (Molded body) The molded article of the present invention can be obtained by crosslinking the elastomer composition of the present invention described above. Since the molded article of the present invention is obtained by crosslinking the elastomer composition of the present invention described above, it is possible to achieve both a high friction coefficient and a low wear amount. The preferred range of the above-mentioned CNT content per 100 parts by mass of the elastomer in the molded article is the same as the above-mentioned range in the elastomer composition of the present invention. As described above, the molded article of the present invention is formed by crosslinking the elastomer composition of the present invention. Therefore, one embodiment of the molded article of the present invention is a molded article (e.g., a crosslinked sheet) formed by crosslinking an elastomer composition containing an elastomer and a reinforcing filler, the reinforcing filler containing carbon nanotubes, the proportion of single-walled carbon nanotubes in the reinforcing filler being 90 mass% or more, and the coefficient of variation of surface resistivity being 20% or less.
[0059] The conditions for obtaining a molded article by crosslinking the elastomer composition of the present invention can be appropriately determined depending on the shape of the desired molded article, the type and amount of elastomer contained in the elastomer composition, and the types and amounts of crosslinking agent and other components optionally contained in the elastomer composition, etc. For example, the crosslinking temperature can be 140°C to 250°C, the pressure can be 1 MPa to 20 MPa, and the time can be 1 minute to 180 minutes.
[0060] The molded article of the present invention is obtained by crosslinking the elastomer composition of the present invention, and therefore has both a high friction coefficient and a low wear amount, and can therefore be advantageously used as, for example, any of belts, anti-vibration rubber, rubber rolls, and outsoles. The method for producing the molded article of the present invention is not particularly limited as long as it is possible to mold the elastomer composition of the present invention into a desired shape, and any known method can be used. Specifically, for example, the elastomer composition is placed in a mold, crosslinking of the elastomer composition is allowed to proceed in the mold, and then various processing steps are further performed to produce a molded article having a desired shape. EXAMPLES
[0061] The present invention will be specifically described below based on examples, but the present invention is not limited to these examples. In the following description, the "%" and "parts" that represent amounts are based on mass unless otherwise specified. In the examples and comparative examples, the coefficient of variation of the surface resistivity of the crosslinked sheet, the friction coefficient and friction coefficient index of the molded body, and the specific wear rate and specific wear rate index of the molded body were evaluated by the following methods. <Variation coefficient of surface resistivity of crosslinked sheet> The elastomer composition was crosslinked to obtain a crosslinked sheet (length: 150 mm, width: 150 mm, thickness: 2 mm). The surface resistivity (Ω / sq.) of the crosslinked sheet was measured 10 times at different measurement points using a resistivity meter (manufactured by Mitsubishi Chemical Analytech Co., Ltd., product name "Loresta-GX MCP-T700", probe: LSP). The average value and standard deviation were calculated from the 10 measured values, and the standard deviation was divided by the average value, multiplied by 100 to obtain the coefficient of variation (%) of the surface resistivity. Here, the crosslinking conditions (temperature, pressure, heating time, etc.) when obtaining a crosslinked sheet from the elastomer composition are determined based on the minimum torque M measured at any temperature and time using a vulcanization tester in accordance with JIS K6300-2:2001. L Maximum torque M H Torque increase to M E (M E =M H -M L ) with torque M E Any condition can be adopted under which the torque in the vulcanization test of the elastomer composition is 90% or more of M E If the crosslinking conditions are such that the torque is 90% or more of the original torque, then the crosslinking is sufficiently advanced. E Regardless of the conditions selected, the surface resistivity and its standard deviation of the crosslinked sheet obtained will not change substantially. In other words, the torque in the vulcanization test of the elastomer composition is M E By adopting crosslinking conditions in which the coefficient of variation of the surface resistivity of a crosslinked sheet obtained by crosslinking an elastomer composition is 90% or more, it is possible to uniquely specify the "coefficient of variation of the surface resistivity of a crosslinked sheet obtained by crosslinking an elastomer composition." <Friction coefficient and friction coefficient index of molded body> The molded bodies (crosslinked sheets) obtained in the examples and comparative examples were cut into 2 mm wide x 2 mm long x 1 mm thick to obtain rubber test pieces. A pin-disk type friction and wear tester and water-resistant abrasive paper with abrasive material of silicon carbide and a grain size of 1500 were used as the abrasive paper, and the friction surface temperature was heated to 60°C with a heater, and a friction speed of 100 mm / s and contact pressure of 0.2 MPa (load 0.8 N) were used to perform the friction test. The friction coefficient during wear was measured using a load cell, and the wear dimension was obtained as a displacement in the thickness direction by a differential transformer placed above the rubber test piece. The larger the friction coefficient, the higher the frictional force of the molded body. The friction coefficient (μ A ) and the friction coefficient (μ B ) was used to calculate the friction coefficient index using the following formula. A larger friction coefficient index means that the molded body has a higher friction force. Friction coefficient index=(μ A / μ B ) x 100 <Specific wear rate and specific wear rate index of compacts> A friction test was carried out in the same manner as in the measurement of the friction coefficient, and the specific wear rate was calculated from the following formula: The lower the specific wear rate, the lower the wear rate of the molded body. Specific wear rate (mm 3 / (N m)) = (wear dimension × width × length) / (load × friction time × friction speed) The specific wear rate (K A ) and the specific abrasion rate (K B ) and the specific wear rate index was calculated from the following formula. The larger the specific wear rate index, the lower the wear rate of the molded body. Specific wear amount index=(K B / K A ) x 100
[0062] Example 1 <Preparation of Carbon Nanotubes> As a CNT containing 90% or more of single-walled CNT, single-walled CNT (ZEON Nano Technology Co., Ltd., "ZEONANO SG101", SGCNT) was used. In the measurement with a Raman spectrophotometer, the 100-300 cm -1 A radial breathing mode (RBM) spectrum was observed in the low wavenumber region. In addition, the BET specific surface area of the SGCNT measured using a BET specific surface area meter (BELSORP (registered trademark)-max, manufactured by BEL Japan Co., Ltd.) was 1325 m 2 / g (unopened). Furthermore, the diameter and length of 100 randomly selected SGCNTs were measured using a transmission electron microscope, and the average diameter (Av), standard deviation of the diameter (σ), and average length of the SGCNTs were obtained. The average diameter (Av) was 3.5 nm, the value (3σ) obtained by multiplying the standard deviation (σ) by 3 was 2.1 nm, the ratio (3σ / Av) was 0.6, and the average length was 450 μm. Furthermore, when the t-plot of the SGCNTs was measured using "BELSORP (registered trademark)-mini" manufactured by BEL Japan Co., Ltd., the t-plot was bent in an upward convex shape. S2 / S1 was 0.09, and the position t of the bending point was 0.6 nm. <Preparation of Elastomer Composition> [Preparation of mixture (master batch)] To 1900 g of methyl ethyl ketone as an organic solvent, 100 g of vinylidene fluoride rubber (FKM, manufactured by Chemours, Viton GBL-600S) as an elastomer was added, and the mixture was stirred for 24 hours to dissolve the fluorine-containing elastomer. Next, 4 g of the SGCNTs were added to the obtained fluorine-containing elastomer solution, and the mixture was stirred for 15 minutes using a stirrer (manufactured by PRIMIX, Labo-lution (registered trademark)). Furthermore, the fluorine-containing elastomer solution to which SGCNTs were added was subjected to 4-pass dispersion treatment at a temperature of 45°C using a bead mill (manufactured by Asada Iron Works, Nano Mill NM-G1.4L) and zirconia beads (Vickers hardness: 1250, packing rate of dispersion media: 52%, average diameter of dispersion media: 0.5 mm) as dispersion media under conditions of a peripheral speed of 15 m / s and a discharge rate of 65 g / min. Thereafter, the obtained dispersion treatment liquid (slurry) was dropped into 4000 g of isopropyl alcohol and solidified to obtain a black solid. The obtained black solid was then dried under reduced pressure at 60°C for 12 hours to obtain a mixture (master batch) of the fluorine-containing elastomer and SGCNTs. [Mixing] Thereafter, using an open roll at 20°C, 13 g of the mixture (master batch) obtained above (fluorine-containing elastomer: 12.5 g, SGCNT: 0.5 g), 87.5 g of fluorine-containing elastomer (Viton GBL-600S, manufactured by Chemours), 3 g of zinc oxide (two types of zinc oxide) as a crosslinking aid, 3 g of triallyl isocyanurate (TAIC (registered trademark), manufactured by Mitsubishi Chemical Corporation) as a first crosslinking agent, and 2 g of 2,5-dimethyl-2,5-di(t-butylperoxy)hexane (product name "Perhexa 25B40", manufactured by NOF Corporation) as a second crosslinking agent were kneaded, and the roll gap was adjusted to 2 mm. The rubber kneaded product was then wound around the roll, and the left and right cuts were performed three times each, and then a sheet was discharged, thereby obtaining a rubber kneaded product as the elastomer composition of the present invention. <Preparation of Molded Product (Crosslinked Sheet)> The obtained fluorine-containing elastomer composition was placed in a mold and crosslinked at a temperature of 160°C and a pressure of 10 MPa for 20 minutes (primary crosslinking). Then, the composition was heated in a gear oven at 232°C for 2 hours to carry out secondary vulcanization (secondary crosslinking), thereby obtaining a crosslinked sheet (length: 150 mm, width: 150 mm, thickness: 2 mm) which is the molded article of the present invention. The surface resistivity of the crosslinked sheet thus obtained was measured, and the average value and the coefficient of variation of the surface resistivity were calculated. The results are shown in Table 1. The friction coefficient and specific wear rate of the crosslinked sheet as a molded body were measured. Furthermore, the friction coefficient index and specific wear rate index of the molded body were calculated using the above-mentioned relational expressions. The results are shown in Table 1.
[0063] Example 2 Except for using the elastomer composition prepared as follows, a molded article (crosslinked sheet) was prepared in the same manner as in Example 1, and evaluation was carried out in the same manner as in Example 1. The results are shown in Table 1. <Preparation of Elastomer Composition> [Preparation of mixture (master batch)] In the same manner as in Example 1, a mixture (master batch) was prepared. [Mixing] A rubber kneaded material (elastomer composition) was prepared in the same manner as in Example 1, except that the amount of the mixture (master batch) of the fluorine-containing elastomer and SGCNTs was changed from 13 g to 26 g (fluorine-containing elastomer: 25 g, SGCNT: 1 g) and the amount of the fluorine-containing elastomer (Viton GBL-600S, manufactured by Chemours) was changed from 87.5 g to 75 g.
[0064] Example 3 Except for using the elastomer composition prepared as follows, a molded article (crosslinked sheet) was prepared in the same manner as in Example 1, and evaluation was carried out in the same manner as in Example 1. The results are shown in Table 1. <Preparation of Elastomer Composition> [Preparation of mixture (master batch)] In the same manner as in Example 1, a mixture (master batch) was prepared. [Mixing] A rubber kneaded material (elastomer composition) was prepared in the same manner as in Example 1, except that the amount of the mixture (master batch) of the fluorine-containing elastomer and SGCNTs was changed from 13 g to 52 g (fluorine-containing elastomer: 50 g, SGCNT: 2 g) and the amount of the fluorine-containing elastomer (Viton GBL-600S, manufactured by Chemours) was changed from 87.5 g to 50 g.
[0065] Comparative Example 1 Except for using the elastomer composition prepared as follows, a molded article (crosslinked sheet) was prepared in the same manner as in Example 1, and evaluation was carried out in the same manner as in Example 1. The results are shown in Table 1. <Preparation of Elastomer Composition> A mixture (master batch) was not prepared, and 15 g of carbon black (Thermax N-990, manufactured by Cancarb) was used instead of 13 g of the mixture (master batch) of fluorine-containing elastomer and SGCNT, and the amount of fluorine-containing elastomer (Viton GBL-600S, manufactured by Chemours) was changed from 87.5 g to 100 g, and kneading was performed. Otherwise, a rubber kneaded product (elastomer composition) was prepared in the same manner as in Example 1.
[0066] Comparative Example 2 Except for using the elastomer composition prepared as follows, a molded article (crosslinked sheet) was prepared in the same manner as in Example 1, and evaluation was carried out in the same manner as in Example 1. The results are shown in Table 1. <Preparation of Elastomer Composition> A rubber kneaded material (elastomer composition) was prepared in the same manner as in Comparative Example 1, except that the amount of carbon black (Cancarb Corporation, Thermax N-990) was changed from 15 g to 30 g.
[0067] Comparative Example 3 Except for using the elastomer composition prepared as follows, a molded article (crosslinked sheet) was prepared in the same manner as in Example 1, and evaluation was carried out in the same manner as in Example 1. The results are shown in Table 1. <Preparation of Elastomer Composition> [Preparation of mixture (master batch)] In the same manner as in Example 1, a mixture (master batch) was prepared. [Mixing] A rubber kneaded material (elastomer composition) was prepared in the same manner as in Example 1, except that 30 g of carbon black (Cancarb Corporation, Thermax N-990) was further added.
[0068] Comparative Example 4 Except for using the elastomer composition prepared as follows, a molded article (crosslinked sheet) was prepared in the same manner as in Example 1, and evaluation was carried out in the same manner as in Example 1. The results are shown in Table 1. <Preparation of Elastomer Composition> [Preparation of mixture (master batch)] In the same manner as in Example 1, a mixture (master batch) was prepared. [Mixing] A rubber mixture (elastomer composition) was prepared in the same manner as in Example 3, except that 30 g of carbon black (Cancarb Corporation, Thermax N-990) was further added.
[0069] Comparative Example 5 Except for using the elastomer composition prepared as follows, a molded article (crosslinked sheet) was prepared in the same manner as in Example 1, and evaluation was carried out in the same manner as in Example 1. The results are shown in Table 1. <Preparation of Elastomer Composition> [Preparation of mixture (master batch)] A mixture (master batch) was prepared in the same manner as in Example 2, except that the number of passes in the bead mill dispersion treatment was changed from 4 passes to 1 pass. [Mixing] A rubber mixture (elastomer composition) was prepared by kneading in the same manner as in Example 2, except that the mixture (master batch) obtained as described above was used.
[0070] In addition, in Table 1 shown below, "FKM" stands for vinylidene fluoride rubber. "CB" stands for carbon black, "ZnO" refers to zinc oxide (zinc oxide type 2), "TAIC" stands for triallyl isocyanurate; "PH" refers to 2,5-dimethyl-2,5-di(t-butylperoxy)hexane.
[0071] [Table 1]
[0072] As can be seen from Table 1, in Examples 1 to 3, which used elastomer compositions containing a reinforcing filler in which the proportion of single-walled CNTs is a predetermined value or more, and in which the coefficient of variation of the surface resistivity of a crosslinked sheet obtained by crosslinking the elastomer composition is a predetermined value or less, molded articles that achieve both a high friction coefficient and a low wear amount were produced. On the other hand, in Comparative Example 1, which contains a reinforcing filler in which the proportion of single-walled CNTs is less than a specified value and uses an elastomer composition in which the coefficient of variation of the surface resistivity of the crosslinked sheet is greater than a specified value, it is clear that the molded body does not achieve both a high friction coefficient and a low wear amount. Moreover, in Comparative Examples 2 to 4, which used elastomer compositions containing a reinforcing filler in which the proportion of single-walled CNTs was less than a predetermined value, it was found that the molded body could not simultaneously achieve a high friction coefficient and a low wear amount. In Comparative Example 5, in which an elastomer composition in which the coefficient of variation of the surface resistivity of the crosslinked sheet was greater than a predetermined value was used, it was found that both a high friction coefficient and a low wear amount of the molded body could not be achieved at the same time. [Industrial Applicability]
[0073] According to the present invention, it is possible to provide an elastomer composition capable of forming a molded article having both a high friction coefficient and a low wear amount. Moreover, according to the present invention, it is possible to provide a molded article that achieves both a high friction coefficient and a low wear amount.
Claims
1. An elastomer composition comprising an elastomer and a reinforcing filler, the reinforcing filler comprises carbon nanotubes, The ratio of single-walled carbon nanotubes in the reinforcing filler is 90% by mass or more, The elastomer composition, wherein a crosslinked sheet obtained by crosslinking the elastomer composition has a coefficient of variation of surface resistivity of 20% or less.
2. The elastomer composition according to claim 1 , wherein the elastomer is a fluorine-containing elastomer.
3. The BET specific surface area of the carbon nanotube is 600 m 2 The elastomer composition according to claim 1 or 2, wherein the elastomer composition has a viscosity of 1 / g or more.
4. 4. The elastomer composition according to claim 1, wherein the carbon nanotubes have an average length of 10 μm or more.
5. 5. The elastomer composition according to claim 1, wherein the content of the carbon nanotubes is 0.1 parts by mass or more and 4 parts by mass or less per 100 parts by mass of the elastomer.
6. The elastomer composition according to any one of claims 1 to 5, further comprising a crosslinking agent.
7. A molded article obtained by crosslinking the elastomer composition according to any one of claims 1 to 6.
8. The molded article according to claim 7, which is any one of a belt, a vibration-proof rubber, a rubber roll, and an outsole.
Citation Information
Patent Citations
Rubber composition for tread of high-performance wet tire, and high-performance wet tire
JP2014080550A
Method for producing slurry and method for producing composite resin material
JP2017031323A
Manufacturing method of composite material
JP2018203914A
Fluorine rubber composition, crosslinked article and hose thereof
JP2019189702A
Conductive composition
WO2013172334A1