Acrylic rubber manufacturing method

By washing the water-containing crumb until the electrical conductivity of the washing water reaches 6.0 mS/cm or less, the method produces acrylic rubber with enhanced water resistance, addressing the issue of coagulant residue and improving the suitability of crosslinked products for automotive applications.

JP7559749B2Active Publication Date: 2024-10-02OSAKA SODA CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2021511421
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-03-29
Filing Date
2020-03-18
Publication Date
2024-10-02
Estimated Expiration
2040-03-18

AI Technical Summary

Technical Problem

Existing methods for producing acrylic rubber do not effectively control the amount of coagulant remaining in the product, affecting the water resistance of crosslinked acrylic rubber, and lack efficient methods for measuring coagulant residue during the manufacturing process.

Method used

The method involves washing the water-containing crumb until the electrical conductivity of the washing water reaches 6.0 mS/cm or less, followed by drying, to produce acrylic rubber with enhanced water resistance.

Benefits of technology

This approach results in acrylic rubber with improved water resistance, suitable for automotive parts such as sealing materials, hoses, and other rubber components.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007559749000001
    Figure 0007559749000001
  • Figure 0007559749000002
    Figure 0007559749000002
  • Figure 0007559749000003
    Figure 0007559749000003
Patent Text Reader

Abstract

Provided is a method for more easily producing an acrylic rubber capable of giving a crosslinked rubber having excellent water resistance. A method for producing acrylic rubber including a step for obtaining an emulsion polymerization solution by emulsion polymerization of monomers, a step for mixing the emulsion polymerization solution and a coagulant to obtain a water-containing crumb, and a step for washing the water-containing crumb with water, wherein the water-containing crumb is washed in the step for washing the water-containing crumb with water until the electrical conductivity of the wash water after washing the water-containing crumb becomes 6.0 mS / cm or lower.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing acrylic rubber, and more particularly to a method for producing acrylic rubber which can give a cross-linked rubber having excellent water resistance. [Background technology]

[0002] Acrylic rubber is a polymer whose main component is an acrylic ester, and is generally known as a rubber having excellent heat resistance, oil resistance, and ozone resistance, and is widely used in the automotive industry.

[0003] Such acrylic rubber is usually obtained by emulsion polymerizing the monomer mixture that constitutes the acrylic rubber, adding a coagulant to the resulting emulsion polymerization liquid, and drying the resulting water-containing crumbs (i.e., water-containing acrylic rubber).

[0004] Meanwhile, in recent years, automobile components, such as sealing materials, hose materials, vibration-proofing materials, tube materials, belt materials, and boot materials, are required to have excellent water resistance in addition to heat resistance and oil resistance. The water resistance of the cross-linked acrylic rubber is affected by the amount of coagulant remaining in the acrylic rubber, so a process is required to remove it as much as possible. Patent documents 1 and 2 also describe a washing process for the water-containing crumb obtained in the coagulation process from the viewpoint of reducing the amount of coagulant remaining in the acrylic rubber, but there is no description of a management method other than the number of times of washing with water. Patent document 2 also describes the measured value of the amount of coagulant remaining in the acrylic rubber, but it is difficult to measure the amount of coagulant remaining in the process analysis during manufacturing from the viewpoint of time and cost for analyzing a small amount of coagulant. Therefore, a method is required to more easily control the amount of coagulant remaining in the acrylic rubber within a range that does not impair the water resistance of the cross-linked acrylic rubber. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2016-213493 A [Patent Document 2] Patent No. 6394834 Summary of the Invention [Problem to be solved by the invention]

[0006] The present invention has been made in view of the above circumstances, and an object of the present invention is to provide a simpler method for producing an acrylic rubber which is capable of giving a cross-linked rubber product having excellent water resistance. [Means for solving the problem]

[0007] As a result of intensive research to achieve the above object, the present inventors have found that the above object can be achieved by washing the hydrous crumbs with water until the electrical conductivity of the washing water is 6.0 mS / cm or less in a water washing step of the hydrous crumbs obtained by adding a coagulant to an emulsion polymerization liquid obtained by emulsion polymerizing a monomer for obtaining an acrylic rubber, and have completed the present invention. Conventionally, hydrous crumbs have not been washed until the electrical conductivity of the washing water (usually, the electrical conductivity of the washing water before washing the hydrous crumbs is 0.1 mS / cm or less) is such a low value, and hydrous crumbs have not been washed until the electrical conductivity is 6.0 mS / cm or less, and the electrical conductivity of the washing water for the hydrous crumbs has not been controlled.

[0008] The aspects of the present invention are as follows. Item 1. A step of obtaining an emulsion polymerization liquid by emulsion polymerization of a monomer; A step of mixing the emulsion polymerization liquid with a coagulant to obtain a water-containing crumb; and washing the hydrous crumbs with water A method for producing an acrylic rubber, comprising: In the step of washing the hydrous crumbs with water, the hydrous crumbs are washed with water until the washing water after washing has an electrical conductivity of 6.0 mS / cm or less. Item 2. The method for producing acrylic rubber according to Item 1, further comprising a drying step after the step of washing the water-containing crumbs with water. Item 3. A method for producing an acrylic rubber-containing composition, further comprising a step of blending a crosslinking agent with the acrylic rubber obtained by the method for producing an acrylic rubber according to item 1 or 2. Item 4. A method for producing a cross-linked acrylic rubber product, further comprising a step of cross-linking the acrylic rubber composition obtained by the method for producing an acrylic rubber-containing composition according to Item 3. Item 5. A water-containing crumb of acrylic rubber, A hydrous crumb of an acrylic rubber, in which, when the hydrous crumb is washed with water, the electrical conductivity of the water is 6.0 mS / cm or less. Effect of the Invention

[0009] The present invention relates to a simple method for producing an acrylic rubber having excellent water resistance, and a rubber material (specifically, a cross-linked product obtained by cross-linking) produced using a composition containing the acrylic rubber of the present invention has excellent water resistance and is therefore suitable as a rubber material for various components for automobiles, such as sealing materials, hose materials, vibration-proof materials, tube materials, belt materials, and boots materials. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] The method for producing acrylic rubber of the present invention includes a step of obtaining an emulsion polymerization liquid by emulsion polymerizing a monomer, a step of obtaining water-containing crumbs by mixing the emulsion polymerization liquid with a coagulant, and a step of washing the water-containing crumbs with water, and is characterized in that in the step of washing the water-containing crumbs with water, the water-containing crumbs are washed with water until the electric conductivity of the washing water for the water-containing crumbs becomes 6.0 mS / cm or less. By being provided with the above-mentioned configuration, the method for producing acrylic rubber of the present invention can obtain an acrylic rubber having excellent water resistance. The method for producing acrylic rubber of the present invention, the water-containing crumbs (water-containing acrylic rubber) obtained by the method, and the method for producing a cross-linked acrylic rubber using the method will be described in detail below.

[0011] The acrylic rubber produced by the production method of the present invention is a polymer mainly composed of structural units derived from (meth)acrylic acid esters, and the term "main component" refers to a polymer containing 50 mass % or more of structural units derived from (meth)acrylic acid esters. Note that "(meth)acrylic acid esters" means "acrylic acid esters or methacrylic acid esters," and the same applies to similar expressions in this application.

[0012] Examples of the structural unit derived from the (meth)acrylic acid ester include a structural unit derived from an alkyl (meth)acrylic acid ester and a structural unit derived from an alkoxyalkyl (meth)acrylic acid ester. The structural unit derived from an alkyl acrylate having an alkyl group having 1 to 8 carbon atoms and the structural unit derived from an alkoxyalkyl acrylate having an alkoxyalkyl group having 2 to 8 carbon atoms are preferable. The structural unit derived from an alkyl acrylate having an alkyl group having 2 to 6 carbon atoms and / or the structural unit derived from an alkoxyalkyl acrylate having an alkoxyalkyl group having 2 to 6 carbon atoms are more preferable. The structural unit derived from the (meth)acrylic acid ester may be a single structural unit or two or more structural units derived from a (meth)acrylic acid ester.

[0013] Specific examples of (meth)acrylic acid alkyl esters include (meth)acrylic acid esters such as methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, n-pentyl (meth)acrylate, n-hexyl (meth)acrylate, n-heptyl (meth)acrylate, n-octyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, and cyclohexyl (meth)acrylate, of which ethyl (meth)acrylate and n-butyl (meth)acrylate are preferred. Specific examples of the (meth)acrylic acid alkoxyalkyl ester include (meth)acrylic acid esters such as methoxymethyl (meth)acrylate, methoxyethyl (meth)acrylate, ethoxymethyl (meth)acrylate, 2-ethoxyethyl (meth)acrylate, 2-propoxyethyl (meth)acrylate, 2-butoxyethyl (meth)acrylate, 2-methoxypropyl (meth)acrylate, 2-ethoxypropyl (meth)acrylate, 3-methoxypropyl (meth)acrylate, 3-ethoxypropyl (meth)acrylate, 4-methoxybutyl (meth)acrylate, and 4-ethoxybutyl (meth)acrylate, with methoxyethyl (meth)acrylate being preferred.

[0014] The content of structural units derived from (meth)acrylic acid ester in the acrylic rubber of the present invention is more preferably 50 mass% or more, and particularly preferably 60 mass% or more, of all structural units of the acrylic rubber, and the upper limit is preferably 99.5 mass% or less, more preferably 99 mass% or less, and particularly preferably 97.5 mass% or less.

[0015] The acrylic rubber of the present invention contains a structural unit derived from an unsaturated monomer having a crosslinking group. Examples of the structural unit derived from an unsaturated monomer having a crosslinking group include a structural unit derived from an unsaturated monomer having a halogen group (e.g., a chlorine group), a structural unit derived from an unsaturated monomer having a carboxyl group, and a structural unit derived from an unsaturated monomer having an epoxy group, and the structural unit derived from an unsaturated monomer having a halogen group (especially a chlorine group) or a carboxyl group is particularly preferred.

[0016] Examples of the unsaturated monomer having a halogen group include vinyl monochloroacetate and allyl chloroacetate, with vinyl monochloroacetate being preferred.

[0017] Examples of the unsaturated monomer having a carboxy group include unsaturated monocarboxylic acids such as (meth)acrylic acid, crotonic acid, 2-pentenoic acid, and cinnamic acid, unsaturated dicarboxylic acids such as fumaric acid, maleic acid, and itaconic acid, carboxylic anhydrides such as maleic anhydride and citraconic anhydride, butenedioic acid mono-chain alkyl esters such as monomethyl fumarate, monoethyl fumarate, mono-n-butyl fumarate, monomethyl maleate, monoethyl maleate, mono-2-ethylhexyl maleate, and mono-n-butyl maleate, butenedioic acid mono-cyclic alkyl esters such as monocyclopentyl fumarate, monocyclohexyl fumarate, monocyclopentyl maleate, and monocyclohexyl maleate, and itaconic acid monoesters such as monomethyl itaconate, monoethyl itaconate, mono-n-butyl itaconate, and monocyclohexyl itaconate. Among these, there may be mentioned unsaturated dicarboxylic acid monoesters such as monoethyl fumarate, monopropyl fumarate, monobutyl fumarate, monoethyl itaconate, monopropyl itaconate, and monobutyl itaconate.

[0018] Examples of the unsaturated monomer having an epoxy group include glycidyl (meth)acrylate and (meth)allyl glycidyl ether.

[0019] The content of the structural units derived from unsaturated monomers having a crosslinking group in the acrylic rubber is preferably 0.1% by mass or more, more preferably 0.3% by mass or more, particularly preferably 0.5% by mass or more, and preferably 10% by mass or less, more preferably 5% by mass or less, particularly preferably 2.5% by mass or less, based on the total structural units of the acrylic rubber. The above range of the structural units derived from unsaturated monomers having a crosslinking group is preferable in terms of physical properties such as strength and compression set, and processability.

[0020] Furthermore, the acrylic rubber of the present invention may contain, in addition to the above-mentioned structural units, structural units derived from other monomers copolymerizable therewith. Examples of the other structural units include structural units derived from ethylenically unsaturated nitriles, structural units derived from (meth)acrylamide monomers, structural units derived from aromatic vinyl monomers, structural units derived from conjugated diene monomers, structural units derived from non-conjugated dienes, structural units derived from other olefins, etc.

[0021] Examples of the ethylenically unsaturated nitrile include compounds such as acrylonitrile, methacrylonitrile, α-methoxyacrylonitrile, and vinylidene cyanide.

[0022] Examples of the (meth)acrylamide monomer include acrylamide, methacrylamide, diacetone acrylamide, diacetone methacrylamide, N-butoxymethyl acrylamide, N-butoxymethyl methacrylamide, N-butoxyethyl acrylamide, N-butoxyethyl methacrylamide, N-methoxymethyl acrylamide, N-methoxymethyl methacrylamide, N-propioxymethyl acrylamide, N-propioxymethyl methacrylamide, N-methyl acrylamide, N-methyl methacrylamide, N,N-dimethyl acrylamide, N,N-dimethyl methacrylamide, N,N-diethyl acrylamide, N,N-diethyl methacrylamide, N-methylolacrylamide, N-methylol methacrylamide, ethacrylamide, crotonamide, cinnamic acid amide, maleindiamide, itacondiamide, methylmaleamide, methyl itaconamide, maleimide, itaconimide, and other compounds.

[0023] Examples of aromatic vinyl monomers include compounds such as styrene, α-methylstyrene, o-methylstyrene, p-methylstyrene, o-ethylstyrene, p-ethylstyrene, α-fluorostyrene, p-trifluoromethylstyrene, p-methoxystyrene, p-aminostyrene, p-dimethylaminostyrene, p-acetoxystyrene, styrenesulfonic acid or a salt thereof, α-vinylnaphthalene, 1-vinylnaphthalene-4-sulfonic acid or a salt thereof, 2-vinylfluorene, 2-vinylpyridine, 4-vinylpyridine, divinylbenzene, diisopropenylbenzene, and vinylbenzyl chloride.

[0024] Examples of conjugated diene monomers include compounds such as 1,3-butadiene, 2-methyl-1,3-butadiene, 2-chloro-1,3-butadiene, 1,2-dichloro-1,3-butadiene, 2,3-dichloro-1,3-butadiene, 2,3-dimethyl-1,3-butadiene, 2-neopentyl-1,3-butadiene, 2-bromo-1,3-butadiene, 2-cyano-1,3-butadiene, 1,3-pentadiene, 1,3-hexadiene, chloroprene, and piperylene.

[0025] Examples of structural units derived from non-conjugated dienes include structural units derived from non-conjugated diene compounds such as 1,4-pentadiene, 1,4-hexadiene, ethylidenenorbornene, norbornadiene, and dicyclopentadiene.

[0026] Other olefin monomers include esters such as dicyclopentadienyl acrylate, dicyclopentadienyl methacrylate, dicyclopentadienyl ethyl acrylate, and dicyclopentadienyl ethyl methacrylate, as well as compounds such as ethylene, propylene, vinyl chloride, vinylidene chloride, 1,2-dichloroethylene, vinyl acetate, vinyl fluoride, vinylidene fluoride, 1,2-difluoroethylene, vinyl bromide, vinylidene bromide, 1,2-dibromoethylene, ethyl vinyl ether, and butyl vinyl ether.

[0027] In the acrylic rubber of the present invention, when structural units derived from these other copolymerizable monomers are contained, the content in all structural units is preferably 0 to 45% by mass, more preferably 0 to 20% by mass.

[0028] The method for producing acrylic rubber of the present invention includes a step of obtaining an emulsion polymerization liquid by emulsion polymerizing a monomer, a step of mixing the emulsion polymerization liquid with a coagulant to obtain water-containing crumbs, and a step of washing the water-containing crumbs with water, and is characterized in that in the step of washing the water-containing crumbs with water, the water-containing crumbs are washed with water until the electric conductivity of the wash water after washing the water-containing crumbs with water is 6.0 mS / cm or less.

[0029] The process for obtaining an emulsion polymerization liquid by emulsion polymerization of monomers will be described below. Hereinafter, this process may also be referred to as an emulsion polymerization process.

[0030] The emulsion polymerization step is a step of obtaining an emulsion polymerization liquid by emulsion polymerizing monomers that will constitute the acrylic rubber.

[0031] In the emulsion polymerization step, a conventional method may be used, and the emulsifier, polymerization initiator, chain transfer agent, polymerization terminator and the like may be any of the conventionally known agents that are generally used.

[0032] The emulsifier is not particularly limited, and nonionic emulsifiers and anionic emulsifiers that are generally used in emulsion polymerization methods can be used. Examples of nonionic emulsifiers include polyoxyethylene alkyl ethers, polyoxyethylene alcohol ethers, polyoxyethylene alkyl phenyl ethers, polyoxyethylene polycyclic phenyl ethers, polyoxyalkylene alkyl ethers, sorbitan fatty acid esters, polyoxyethylene fatty acid esters, and polyoxyethylene sorbitan fatty acid esters, while examples of anionic emulsifiers include alkylbenzene sulfonates, alkyl sulfates, polyoxyethylene alkyl ether sulfates, polyoxyalkylene alkyl ether phosphates or their salts, polyoxyalkylene alkyl phenyl ether phosphates or their salts, fatty acid salts, and the like, and these may be used alone or in combination.

[0033] The amount of the emulsifier used may be an amount generally used in emulsion polymerization. Specifically, it is in the range of 0.01 to 10% by mass, preferably 0.03 to 7% by mass, and more preferably 0.05 to 5% by mass, based on the amount of the charged monomer. When a reactive surfactant is used as the monomer component, the addition of an emulsifier is not necessarily required.

[0034] The polymerization initiator is not particularly limited, and a polymerization initiator generally used in emulsion polymerization can be used. Specific examples thereof include inorganic polymerization initiators such as persulfates, such as potassium persulfate, sodium persulfate, and ammonium persulfate, 2,2-di(4,4-di(t-butylperoxy)cyclohexyl)propane, 1-di(t-hexylperoxy)cyclohexane, 1,1-di(t-butylperoxy)cyclohexane, 4,4-di(t-butylperoxy)n-butyl valerate, 2,2-di(t-butylperoxy)butane, t-butyl hydroperoxide, and cumene hydroperoxide. Side, diisopropylbenzene hydroperoxide, p-menthane hydroperoxide, 1,1,3,3-tetramethylbutyl hydroperoxide, t-butylcumyl peroxide, di-t-butyl peroxide, di-t-hexyl peroxide, di(2-t-butylperoxyisopropyl)benzene, dicumyl peroxide, diisobutyryl peroxide, di(3,5,5-trimethylhexanoyl) peroxide, dilauroyl peroxide, disuccinic acid peroxide peroxydicarbonate, dibenzoyl peroxide, di(3-methylbenzoyl) peroxide, benzoyl(3-methylbenzoyl) peroxide, diisopropyl peroxydicarbonate, di-n-propyl peroxydicarbonate, di(4-t-butylcyclohexyl) peroxydicarbonate, di(2-ethylhexyl) peroxydicarbonate, di-sec-butyl peroxydicarbonate, cumyl peroxyneodecanate, 1,1,3,3-tetramethylbutyl peroxyneodecanate Canate, t-hexylperoxyneodecanate, t-butylperoxyneodecanate, t-hexylperoxypivalate, t-butylperoxypivalate, 2,5-dimethyl-2,5-di(2-ethylhexanoylperoxy)hexane, 1,1,3,3-tetramethylbutylperoxy-2-ethylhexanate, t-hexylperoxy-2-ethylhexanate, t-butylperoxy-2-ethylhexanate, t-butylperoxylaurate, t-butylperoxy-3,5,Polymerization initiators of organic peroxides such as 5-trimethylhexanate, t-hexylperoxyisopropyl monocarbonate, t-butylperoxyisopropyl monocarbonate, t-butylperoxy2-ethylhexyl monocarbonate, 2,5-dimethyl-2,5-di(benzoylperoxy)hexane, t-butylperoxyacetate, t-hexylperoxybenzoate, t-butylperoxybenzoate, 2,5-dimethyl-2,5-di(t-butylperoxy)hexane, hydroperoxides, azobisisobutyronitrile, 4-4'-azobis(4- Examples of the azo initiator include 2-2'-azobis[2-(2-imidazolin-2-yl)propane, 2-2'-azobis(propane-2-carboxamidine), 2-2'-azobis[N-(2-carboxyethyl)-2-methylpropanamide, 2-2'-azobis[2-[1-(2-hydroxyethyl)-2-imidazolin-2-yl]propane], 2-2'-azobis(1-imino-1-pyrrolidino-2-methylpropane) and 2-2'-azobis[2-methyl-N-[1,1-bis(hydroxymethyl)-2-hydroxyethyl]propanamide]. These polymerization initiators may be used alone or in combination of two or more.

[0035] The amount of the polymerization initiator used may be any amount generally used in emulsion polymerization, specifically, in the range of 0.01 to 5% by mass, preferably 0.01 to 4% by mass, and more preferably 0.02 to 3% by mass, based on the amount of the charged monomer.

[0036] In addition, the organic peroxide and inorganic peroxide as the polymerization initiator can be used as a redox polymerization initiator by combining with a reducing agent. The reducing agent to be used in combination is not particularly limited, but includes compounds containing metal ions in a reduced state such as ferrous sulfate and cuprous naphthenate, methane compounds such as sodium methanesulfonate, amine compounds such as dimethylaniline, ascorbic acid and its salts, and inorganic salts having reducing properties such as alkali metal salts of sulfurous acid and thiosulfuric acid. These reducing agents can be used alone or in combination of two or more. The amount of the reducing agent used is preferably 0.0003 to 10.0 parts by mass relative to 100 parts by mass of the charged monomer.

[0037] Chain transfer agents can be used as necessary. Specific examples of chain transfer agents include alkyl mercaptans such as n-hexyl mercaptan, n-octyl mercaptan, t-octyl mercaptan, n-dodecyl mercaptan, t-dodecyl mercaptan, and n-stearyl mercaptan, xanthogen compounds such as 2,4-diphenyl-4-methyl-1-pentene, 2,4-diphenyl-4-methyl-2-pentene, dimethyl xanthogen disulfide, and diisopropyl xanthogen disulfide, terpinolene, tetramethylthiuram disulfide, tetraethylthiuram disulfide, and tetramethylthiuram monosulfide. Thiuram compounds, phenolic compounds such as 2,6-di-t-butyl-4-methylphenol and styrenated phenol, allyl compounds such as allyl alcohol, halogenated hydrocarbon compounds such as dichloromethane, dibromomethane and carbon tetrabromide, vinyl ethers such as α-benzyloxystyrene, α-benzyloxyacrylonitrile and α-benzyloxyacrylamide, triphenylethane, pentaphenylethane, acrolein, methacrolein, thioglycolic acid, thiomalic acid, 2-ethylhexyl thioglycolate, etc., may be used alone or in combination. The amount of these chain transfer agents is not particularly limited, but is usually 0 to 5 parts by mass per 100 parts by mass of the charged monomer.

[0038] Examples of the polymerization terminator include hydroxylamine, hydroxylamine sulfate, diethylhydroxyamine, hydroxylamine sulfonic acid and its alkali metal salts, sodium dimethyldithiocarbamate, and quinone compounds such as hydroquinone. The amount of the polymerization terminator used is not particularly limited, but is usually 0 to 2 parts by mass relative to 100 parts by mass of the total monomers.

[0039] In addition, polymerization secondary materials such as particle size regulators, chelating agents, and oxygen scavengers can be used as necessary.

[0040] The emulsion polymerization may be any of batch, semi-batch, and continuous. The polymerization time and temperature are not particularly limited. They can be appropriately selected depending on the type of polymerization initiator used, but generally, the polymerization temperature is 10 to 100°C, and the polymerization time is 0.5 to 100 hours.

[0041] The process of mixing the emulsion polymerization liquid with a coagulant to obtain water-containing crumbs will be described below. Hereinafter, this process may also be referred to as the coagulation process.

[0042] The coagulant used in the coagulation step is not particularly limited, but is preferably an inorganic metal salt, specific examples of which include sodium sulfate, magnesium sulfate, aluminum sulfate, sodium chloride, and calcium chloride.

[0043] The method of coagulation by a coagulant is not particularly limited, and a commonly used method can be adopted. One example of the method is to continuously or batchwise supply the emulsion polymerization liquid to an aqueous solution containing a coagulant, and this operation produces a water-containing crumb (water-containing acrylic rubber). At that time, the temperature of the aqueous solution containing the coagulant is affected by the type and amount of monomer used, shear force due to stirring, etc., so it cannot be uniformly specified, but it is generally 50°C or higher, preferably in the range of 60°C to 100°C.

[0044] The step of washing the wet crumbs with water will be described. Hereinafter, this step may be referred to as the "washing step." In the washing step, the wet crumbs are washed with water until the electrical conductivity of the washing water after washing the wet crumbs with water is 6.0 mS / cm or less.

[0045] The purpose of the water washing step is to remove the coagulant contained in the water-containing crumbs.

[0046] The electrical conductivity of the water (washing water) after washing the hydrous crumbs is 6.0 mS / cm or less, preferably 4.5 mS / cm or less, and particularly preferably 3.0 mS / cm or less. The electrical conductivity of the water after washing the hydrous crumbs is not particularly limited, but may be 0.1 mS / cm or more, and may be 0.3 mS / cm or more. As described above, the electrical conductivity of the washing water before washing, which is used for washing the hydrous crumbs, is usually 0.1 mS / cm or less, and in the present invention, it is preferable to use water having an electrical conductivity of 0.1 mS / cm or less as the washing water for the hydrous crumbs.

[0047] The electrical conductivity of the water after washing the hydrous crumbs is measured as follows. A slurry of 3500 parts by mass of ion-exchanged water added to 100 parts by mass of solids contained in the hydrous crumbs is stirred for a predetermined time. At this time, if the washing of the hydrous crumbs is not sufficient in the first place, the ion-exchanged water is replaced. After removing the washed hydrous crumbs, they are put into 3500 parts by mass of new ion-exchanged water and stirred for 5 minutes, and then the stirring is stopped to confirm that the crumbs have settled, and 100 mL of the supernatant is collected. The electrical conductivity of the collected supernatant at 23°C is measured using an AC two-electrode method. The electrical conductivity can be measured using a portable electrical conductivity meter ES-51 manufactured by Horiba, Ltd. and a waterproof general-purpose electrical conductivity cell 9382-10D manufactured by Horiba, Ltd.

[0048] The step of drying the water-containing crumbs after washing will be described below. Hereinafter, this may also be referred to as the drying step.

[0049] The acrylic rubber can be obtained by removing the water from the hydrous crumb and drying it. The drying method is not particularly limited, but it is generally dried using a flash dryer or a fluidized bed dryer.

[0050] The drying temperature is not particularly limited, but is preferably from 50° C. to 250° C., and more preferably from 80 to 200° C. The drying time varies depending on the drying temperature.

[0051] Before the drying step, a dehydration step using a centrifuge or the like may be performed.

[0052] The production method of the present invention may include a step of adding a pH adjuster.

[0053] A base can be used as the pH adjuster, and specific examples of the base include sodium hydroxide, potassium hydroxide, calcium hydroxide, ammonia, inorganic ammonium compounds, and organic amine compounds.

[0054] The molecular weight range of the acrylic rubber used in the present invention thus produced is set to be within the Mooney viscosity (ML) at 100°C in the Mooney scorch test specified in JIS K 6300 from the viewpoint of processability. 1+4 ) is preferably 10 to 100, more preferably 15 to 90, and even more preferably 20 to 80.

[0055] <Acrylic rubber-containing composition> The acrylic rubber-containing composition of the present invention contains at least the above-mentioned acrylic rubber and a crosslinking agent.

[0056] As the crosslinking agent, a conventionally known crosslinking agent such as a polyamine compound, a polyepoxy compound, a polyisocyanate compound, an aziridine compound, a sulfur compound, a higher fatty acid metal salt (fatty acid metal soap), or a thiol compound can be used.

[0057] Examples of higher fatty acid metal salts include alkali metal salts or alkaline earth metal salts of fatty acids having an alkyl or alkenyl group with 8 to 18 carbon atoms, such as sodium stearate, potassium stearate, potassium myristate, sodium palmitate, calcium stearate, magnesium stearate, sodium oleate, potassium oleate, and barium oleate, and these may be used alone or in combination. Examples of the polyamine compound include aliphatic polyamine compounds such as hexamethylenediamine, hexamethylenediamine carbamate, and N,N'-dicinnamylidene-1,6-hexanediamine, and aromatic polyamine compounds such as 4,4'-methylenedianiline, m-phenylenediamine, 4,4'-diaminodiphenyl ether, 3,4'-diaminodiphenyl ether, 4,4'-(m-phenylenediisopropylidene)dianiline, 4,4'-(p-phenylenediisopropylidene)dianiline, 2,2'-bis[4-(4-aminophenoxy)phenyl]propane, 4,4'-diaminobenzanilide, 4,4'-bis(4-aminophenoxy)biphenyl, m-xylylenediamine, p-xylylenediamine, 1,3,5-benzenetriamine, 1,3,5-benzenetriaminomethyl, and isophthalic acid dihydrazide.

[0058] Examples of polyfunctional epoxy compounds include glycidyl ether type epoxy compounds such as phenol novolac type epoxy compounds, cresol novolac type epoxy compounds, cresol type epoxy compounds, bisphenol A type epoxy compounds, bisphenol F type epoxy compounds, brominated bisphenol A type epoxy compounds, brominated bisphenol F type epoxy compounds, and hydrogenated bisphenol A type epoxy compounds; and other polyfunctional epoxy compounds such as alicyclic epoxy compounds, glycidyl ester type epoxy compounds, glycidyl amine type epoxy compounds, and isocyanurate type epoxy compounds.

[0059] Examples of polyisocyanate compounds include 2,4-tolylene diisocyanate, 2,6-tolylene diisocyanate, 4,4'-diphenylmethane diisocyanate, hexamethylene diisocyanate, p-phenylene diisocyanate, m-phenylene diisocyanate, 1,5-naphthylene diisocyanate, 1,3,6-hexamethylene triisocyanate, 1,6,11-undecane triisocyanate, and bicycloheptane triisocyanate.

[0060] Examples of the aziridine compound include tris-2,4,6-(1-aziridinyl)-1,3,5-triazine, tris[1-(2-methyl)aziridinyl]phosphinoxide, and hexa[1-(2-methyl)aziridinyl]triphosphatriazine.

[0061] Examples of the sulfur compound include sulfur, 4,4'-dithiomorpholine, tetramethylthiuram disulfide, and tetraethylthiuram disulfide.

[0062] Examples of the thiol compound include 1,3,5-triazinedithiol or a derivative thereof, and 1,3,5-triazinetrithiols such as 1,3,5-triazine-2,4,6-trithiol. Examples of basic metal oxides include zinc oxide, lead oxide, calcium oxide, and magnesium oxide.

[0063] The organometallic halides are exemplified by dicyclopentadienyl metal dihalides, and the metals include titanium, zirconium, and the like.

[0064] These crosslinking agents may be used alone or in combination of two or more. The amount of each crosslinking agent is 0.05 to 20 parts by mass, preferably 0.1 to 10 parts by mass, per 100 parts by mass of the acrylic rubber of the present invention.

[0065] The acrylic rubber-containing composition of the present invention may also contain any of other additives commonly used in the art, such as a lubricant, an antioxidant, a light stabilizer, a filler, a reinforcing agent, a plasticizer, a processing aid, a pigment, a colorant, a crosslinking accelerator, a crosslinking auxiliary, a crosslinking retarder, an antistatic agent, and a foaming agent.

[0066] Furthermore, it is possible to blend with rubber, resin, etc., as is commonly done in the technical field, without departing from the spirit of the present invention. Examples of rubbers used in the present invention include butadiene rubber, styrene-butadiene rubber, isoprene rubber, natural rubber, acrylonitrile-butadiene rubber, acrylonitrile-butadiene-isoprene rubber, ethylene-propylene-diene rubber, epichlorohydrin rubber, etc., and examples of resins include PMMA (polymethyl methacrylate) resin, PS (polystyrene) resin, PUR (polyurethane) resin, PVC (polyvinyl chloride) resin, EVA (ethylene / vinyl acetate) resin, AS (styrene / acrylonitrile) resin, PE (polyethylene) resin, etc.

[0067] The total amount of the rubber and resin is 50 parts by mass or less, preferably 10 parts by mass or less, and more preferably 1 part by mass or less, per 100 parts by mass of the acrylic rubber of the present invention.

[0068] The method for producing an acrylic rubber-containing composition of the present invention includes a step of blending a crosslinking agent with the acrylic rubber obtained by the above-mentioned method for producing an acrylic rubber.

[0069] The acrylic rubber-containing composition of the present invention can be compounded using any method conventionally used in the field of polymer processing, such as an open roll, a Banbury mixer, or various kneaders.

[0070] The compounding procedure can be the usual procedure used in the field of polymer processing. For example, the polymer alone is first kneaded, then compounding ingredients other than the crosslinking agent and crosslinking accelerator are added to prepare compound A, and then compound B is kneaded by adding the crosslinking agent and crosslinking accelerator.

[0071] The acrylic rubber cross-linked product can be obtained by cross-linking the acrylic rubber-containing composition, and includes a step of cross-linking the acrylic rubber-containing composition obtained by the above-mentioned method for producing an acrylic rubber-containing composition.

[0072] In the process of crosslinking the acrylic rubber-containing composition, the acrylic rubber-containing composition can be usually heated to 100 to 250°C to form a crosslinked product. The crosslinking time varies depending on the temperature, but is usually performed between 0.5 and 300 minutes. The crosslinking molding may be performed in a single step of crosslinking and molding, or the previously molded acrylic rubber-containing composition may be heated again to form a crosslinked product, or the crosslinked product may be heated first and then processed for molding. As a specific method for crosslinking molding, any method such as compression molding using a mold, injection molding, heating using a steam can, air bath, infrared rays, or microwaves may be used.

[0073] Therefore, taking advantage of the above-mentioned properties, the crosslinked product of the present invention can be suitably used as various gaskets, such as O-rings, packings, diaphragms, oil seals, shaft seals, bearing seals, mechanical seals, wellhead seals, seals for electric and electronic devices, seals for pneumatic devices, cylinder head gaskets attached to the joint between a cylinder block and a cylinder head, rocker cover gaskets attached to the joint between a rocker cover and a cylinder head, oil pan gaskets attached to the joint between an oil pan and a cylinder block or a transmission case, gaskets for fuel cell separators attached between a pair of housings sandwiching a unit cell having a positive electrode, an electrolyte plate, and a negative electrode, and gaskets for the top covers of hard disk drives.

[0074] The crosslinked product of the present invention can be used as a rubber material, and is suitably used as an extrusion molded product and a mold crosslinked product for automobile applications, such as various hoses, including fuel oil hoses around fuel tanks, such as fuel hoses, filler neck hoses, vent hoses, vapor hoses, and oil hoses, air hoses, such as turbo air hoses and emission control hoses, radiator hoses, heater hoses, brake hoses, and air conditioner hoses. EXAMPLES

[0075] The present invention will be specifically described with reference to examples and comparative examples, although the present invention is not limited thereto. In the examples and comparative examples, the production of acrylic rubber, and the physical properties of an acrylic-rubber-containing composition containing the obtained acrylic rubber and a crosslinking agent, and a rubber material (specifically, a crosslinked product obtained by crosslinking) prepared using the acrylic-rubber-containing composition were evaluated.

[0076] <How to wash wet crumbs> In the examples and comparative examples, the emulsion polymerization liquid is coagulated, and the obtained hydrous crumbs are washed with water. The washing method involves adding 3,500 parts by mass of ion-exchanged water to 100 parts by mass of solids contained in the hydrous crumbs after the coagulation, and stirring the resulting slurry for a predetermined period of time to wash the hydrous crumbs.

[0077] <Measurement of electrical conductivity of washing water> In the Examples and Comparative Examples, the electrical conductivity of the washed water was measured by taking out the washed hydrous crumbs, pouring them into 3500 parts by mass of fresh ion-exchanged water (electrical conductivity 0.1 mS / cm or less), stirring for 5 minutes, stopping the stirring, confirming that the crumbs had settled, and collecting 100 mL of the supernatant. The collected supernatant was placed in a 110 mL sample can. The electrical conductivity of the supernatant collected in the 110 mL sample can at 23°C was measured using an AC two-electrode method. A portable electrical conductivity meter ES-51 manufactured by Horiba, Ltd. and a waterproof general-purpose electrical conductivity cell 9382-10D manufactured by Horiba, Ltd. were used to measure the electrical conductivity.

[0078] [Example 1] (Manufacture of acrylic rubber A) In a polymerization reactor equipped with a thermometer, a stirrer, a nitrogen inlet tube and a pressure reducing device, 200 parts by mass of water, 1.7 parts by mass of polyoxyalkylene alkyl ether phosphate ester, 49.0 parts by mass of ethyl acrylate as a monomer, 25.0 parts by mass of n-butyl acrylate, 24.8 parts by mass of 2-methoxyethyl acrylate and 1.2 parts by mass of vinyl 2-chloroacetate were charged, and oxygen was sufficiently removed by repeatedly degassing under reduced pressure and replacing with nitrogen, and then 0.1 parts by mass of sodium ascorbate and 0.1 parts by mass of potassium persulfate were added to start an emulsion polymerization reaction under normal pressure and normal temperature, and the reaction was continued until the polymerization conversion rate reached 95%, and 0.0075 parts by mass of hydroquinone was added to stop the polymerization. The obtained emulsion polymerization liquid was coagulated with an aqueous aluminum sulfate solution, and the water-containing crumbs were washed with water until the electrical conductivity of the washing water after washing with water reached 1.7 mS / cm. The water-containing crumbs after washing were dried to obtain acrylic rubber A.

[0079] [Example 2] (Manufacture of acrylic rubber B) An acrylic rubber B was obtained in the same manner as in Example 1, except that the water-containing crumbs were washed with water until the electrical conductivity of the washing water reached 1.9 mS / cm.

[0080] [Example 3] (Manufacture of acrylic rubber C) Acrylic rubber C was obtained in the same manner as in Example 1, except that the water-containing crumbs were washed with water until the electrical conductivity of the washing water reached 4.3 mS / cm.

[0081] [Example 4] (Manufacture of acrylic rubber D) Acrylic rubber D was obtained in the same manner as in Example 1, except that the water-containing crumbs were washed with water until the electrical conductivity of the washing water reached 0.4 mS / cm.

[0082] [Comparative Example 1] (Manufacture of Acrylic Rubber E) An acrylic rubber E was obtained in the same manner as in Example 1, except that the water-containing crumbs were washed with water until the electric conductivity of the washing water reached 7.1 mS / cm.

[0083] [Comparative Example 2] (Manufacture of Acrylic Rubber F) Acrylic rubber F was obtained in the same manner as in Example 1, except that the water-containing crumbs were washed with water until the electrical conductivity of the washing water reached 26.9 mS / cm.

[0084] [Comparative Example 3] (Manufacture of acrylic rubber G) Acrylic rubber G was obtained in the same manner as in Example 1, except that the water-containing crumbs were washed with water until the electrical conductivity of the washing water reached 63.8 mS / cm.

[0085] <Mooney Viscosity (ML 1+4 , 100℃) For acrylic rubbers A to F, the Mooney viscosity (ML) was measured at a measurement temperature of 100°C using a Mooney Viscometer AM-3 manufactured by Toyo Seiki Co., Ltd. in accordance with the Mooney viscosity test in the JIS K6300 physical test method for uncrosslinked rubber. 1+4 The results are shown in Table 1.

[0086] (Production of acrylic rubber-containing composition) First, the ingredients shown in Tables 2 and 3 were kneaded in a kneader at 120°C to prepare compound A. Compound A was dispersed with a crosslinking agent and a crosslinking accelerator at room temperature using an open roll to obtain compound B. Compound B was extruded using an open roll to obtain an uncrosslinked sheet with a thickness of 2 to 2.5 mm. The units for the ingredients in Tables 2 and 3 are parts by mass.

[0087] The uncrosslinked sheet obtained above was placed in a mold 15 cm long, 15 cm wide, and 0.2 cm deep, and pressed at 180°C for 10 minutes to perform primary crosslinking. The primary crosslinked product obtained was then heated in a gear oven at 180°C for 3 hours to perform secondary crosslinking, resulting in a sheet-like crosslinked product. The crosslinked product obtained was punched out with a No. 3 dumbbell to prepare a test piece. The tensile strength and elongation of this test piece were then measured using Shimadzu Corporation's AGS-5KNY in accordance with JIS K6251. The results are shown in Tables 4 and 5.

[0088] [water resistance] The uncrosslinked sheet was placed in a mold 15 cm long, 15 cm wide, and 0.2 cm deep, and pressed at 180°C for 10 minutes to perform primary crosslinking. The obtained primary crosslinked product was then heated in a gear oven at 180°C for 3 hours to perform secondary crosslinking, thereby obtaining a sheet-like crosslinked product. Then, a test piece measuring 3 cm x 2 cm x 0.2 cm was cut from the obtained crosslinked product sheet, and an immersion test was performed in which the obtained test piece was immersed in distilled water (100 ml) adjusted to a temperature of 100°C for 70 hours in accordance with JIS K6258, and the volume change rate of the test piece before and after immersion was measured according to the following formula. The results are shown in Tables 4 and 5. The smaller the volume change rate before and after immersion, the more suppressed the swelling caused by water is, and the better the water resistance is. It can be determined that: Volume change rate before and after immersion (%) = (volume of test piece after immersion - volume of test piece before immersion) ÷ Volume of test piece before immersion x 100

[0089] [Table 1]

[0090] [Table 2]

[0091] [Table 3]

[0092] [Table 4]

[0093] [Table 5]

[0094] As shown in Tables 4 and 5, Examples 4 to 9, which are crosslinked products obtained by crosslinking compositions using acrylic rubber obtained by the manufacturing method of the present invention, showed smaller volume change rates after the water resistance test compared to Comparative Examples. From these results, it can be seen that the present invention can produce acrylic rubber that forms a crosslinked product with excellent water resistance by the simple method of controlling the electrical conductivity of water after washing with water. [Industrial Applicability]

[0095] The present invention can provide a simple method for producing an acrylic rubber having excellent water resistance. A rubber material (specifically, a crosslinked product obtained by crosslinking) produced using a composition containing the acrylic rubber obtained by this method has excellent water resistance and is therefore suitable as a rubber material for various components for automobiles, such as sealing materials, hose materials, vibration-proof materials, tube materials, belt materials, and boots materials.

Claims

1. A step of obtaining an emulsion polymerization liquid by emulsion polymerizing the monomers; A step of mixing the emulsion polymerization liquid with a coagulant to obtain a water-containing crumb; washing the hydrous crumbs with water; and Measuring the electrical conductivity of the water after washing the hydrous crumbs with water; A method for producing an acrylic rubber, comprising: In the step of washing the hydrous crumbs with water, the hydrous crumbs are washed with water until the washing water after washing the hydrous crumbs with water has an electrical conductivity of 6.0 mS / cm or less.

2. The method for producing an acrylic rubber according to claim 1, further comprising a drying step after the step of washing the water-containing crumbs with water.

3. A method for producing an acrylic rubber-containing composition, further comprising a step of blending a crosslinking agent with the acrylic rubber obtained by the method for producing an acrylic rubber according to claim 1 or 2.

4. A method for producing a cross-linked acrylic rubber product, further comprising a step of cross-linking the acrylic rubber composition obtained by the method for producing an acrylic rubber-containing composition according to claim 3.

Citation Information

Patent Citations

  • Composite material into which granule is sealed

    JP1988094834A

  • Semiconductor device

    JP2016213493A

  • Acrylic rubber and crosslinked rubber

    WO2018079783A1

  • Acrylic rubber and method for producing same

    WO2018079784A1

  • Method for producing acrylic rubber

    WO2018079785A1