Nanocellulose-containing gas barrier molded body and its manufacturing method
The use of anionic functional group-containing cellulose nanocrystals with specific dimensions and a hydrophilic resin, formed at low concentration, addresses gas barrier and handling issues, achieving superior gas barrier performance and structural stability.
Patent Information
- Application Number
- JP2021526013
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-06-12
- Filing Date
- 2020-06-01
- Publication Date
- 2024-10-02
- Estimated Expiration
- 2040-06-01
AI Technical Summary
Existing cellulose nanofibers and nanocrystals do not fully satisfy gas barrier properties and handling properties, particularly when chemically treated with TEMPO catalysts, and further shortening fiber length for improved barrier properties is not economical.
A gas barrier molded article using anionic functional group-containing cellulose nanocrystals with a fiber length less than 500nm, aspect ratio of 5 to 50, and a mixture with a hydrophilic resin, formed at a concentration below the critical interaction concentration to minimize shear force impact, resulting in a self-assembled structure with orientation less than 1.14.
The article achieves excellent gas barrier properties with oxygen permeability of 0.59 cc/m²·day·atm at 23°C and 0%RH, maintaining structural integrity and handling properties without shearing effects.
Smart Images

Figure 0007559755000002 
Figure 0007559755000003 
Figure 0007559755000004
Abstract
Description
[Technical field]
[0001] The present invention relates to a nanocellulose-containing gas barrier molded article and a manufacturing method thereof, and more specifically, to a gas barrier molded article capable of exhibiting high gas barrier performance using anionic functional group-containing cellulose nanocrystals and a manufacturing method thereof. [Background technology]
[0002] Nanocellulose has been proposed for use in a variety of applications as an advanced biomass raw material, functional additive, film composite material, etc. In particular, materials such as membranes made of cellulose nanofibers and laminates containing cellulose nanofibers are known to have excellent gas barrier properties, such as oxygen barrier properties, because they suppress the dissolution and diffusion of gases due to hydrogen bonds and strong cross-linking interactions between cellulose fibers, and barrier materials using cellulose nanofibers have been proposed. In order to reduce the size of cellulose fibers, in addition to mechanical treatment, chemical treatment is carried out to introduce hydrophilic functional groups, such as carboxyl groups or phosphate groups, into the hydroxyl groups of cellulose. This not only reduces the energy required for the reduction process, but also improves the barrier properties and dispersibility in aqueous solvents.
[0003] For example, Patent Document 1 listed below describes a gas barrier material that contains cellulose fibers with an average fiber diameter of 200 nm or less, and in which the carboxyl group content of the cellulose constituting the cellulose fibers is 0.4 to 2 mmol / g. Furthermore, for the purpose of improving gas barrier properties under high humidity conditions, Patent Document 2 listed below describes a gas barrier material consisting of a sheet having a membrane composed of cellulose nanofibers, in which the membrane is formed by forming a coating of an aqueous dispersion in which the cellulose nanofibers are dispersed in an aqueous medium, and by carrying out a specified orientation treatment, the cellulose nanofibers located near at least one surface within the membrane are oriented approximately parallel to the membrane surface. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Patent No. 4965528 [Patent Document 2] Patent No. 5678450 Summary of the Invention [Problem to be solved by the invention]
[0005] However, the cellulose nanofibers described in the above patent documents are not yet fully satisfactory in terms of gas barrier properties because of their long fiber length. Also, the cellulose nanofibers chemically treated with the TEMPO catalyst have high viscosity, and are not yet fully satisfactory in terms of handling, such as poor coatability. Furthermore, even the above cellulose nanofibers can have higher gas barrier properties if their fiber length is shortened, but further processing is required for this, which is less economical. In addition, cellulose nanocrystals, which are made by hydrolyzing cellulose fibers with strong acids, are known as nanocelluloses with shorter fiber length than cellulose nanofibers. However, cellulose nanocrystals generally have inferior gas barrier properties to cellulose nanofibers with carboxyl groups or the like introduced therein.
[0006] Therefore, an object of the present invention is to provide a gas barrier molded article that can exhibit excellent barrier properties even when using anionic functional group-containing cellulose nanocrystals having a short fiber length, and a method for producing the same. [Means for solving the problem]
[0007] According to the present invention, Fiber length is 500 nm or less, and aspect ratio is in the range of 5 to 50. Anionic functional group-containing cellulose nanocrystals and a water-soluble amine and / or amino group-containing polymer. It consists of The anionic functional group contains at least a sulfate group and / or a sulfo group, The present invention provides a gas-barrier molded article having a degree of orientation of less than 1.14 as measured using a fiber orientation measurement program. In the gas barrier molded article of the present invention, 1. The anionic functional group is Furthermore , phosphate group ,mosquito At least one carboxyl group Includes thing, 2. The anionic functional group-containing cellulose nanocrystal contains 0.01 to 4.0 mmol / g of phosphate group or carboxyl group; 3. The anionic functional group-containing cellulose nanocrystal contains 0.01 to 4.0 mmol / g of sulfate group and / or sulfo group; 4. The anionic functional group-containing cellulose nanocrystal has a fiber width of 50 nm or less, a fiber length of 500 nm or less, and a crystallinity of 60% or more; 5. The anionic functional group-containing cellulose nanocrystal is composed of a mixture of a hydrophilic resin; 6. The anionic functional group-containing cellulose nanocrystal is dissolved in 1 ml of solids. 2 When the oxygen content is 1.0 g per unit, the oxygen permeability at 23°C and 0% RH is 0.59 cc / m 2 ·day·atm, is preferred.
[0008] The present invention also provides A hydrophilic resin-containing solution is applied and dried to form a layer made of a hydrophilic resin, and then a layer made of a hydrophilic resin is applied on the layer made of the hydrophilic resin. A dispersion containing anionic functional group-containing cellulose nanocrystals at a concentration equal to or lower than the critical interaction concentration. The mixture is coated and dried to form a layer containing cellulose nanocrystals having anionic functional groups. The present invention provides a method for producing a gas barrier molded article, comprising the steps of: In the method for producing a gas barrier molded article of the present invention, 1. The critical interaction concentration of the dispersion is less than 5% by weight; 2. The dispersion contains anionic functional group-containing cellulose nanocrystals at a concentration of 1 to 3% by mass. and, is preferred. Effect of the Invention
[0009] The gas barrier molded article of the present invention has an orientation degree of less than 1.14 as measured using a fiber orientation measurement program, and therefore has a densified self-assembled structure in which the fibers are oriented in random directions, making it possible to exhibit excellent gas barrier properties. Furthermore, by using anionic functional group-containing cellulose nanocrystals, nanocellulose with short fiber length and excellent gas barrier properties can be obtained, and in combination with the above-mentioned densified self-assembled structure, even more excellent gas barrier properties can be exhibited. The gas barrier molded article of the present invention contains the anionic functional group-containing cellulose nanocrystals as a solid content of 1 m 2 When the content is 1.0 g per unit, the oxygen permeability at 23°C and 0% RH is 0.59 cc / m 2 It has excellent gas barrier properties of less than 1000m / day atm. Furthermore, according to the method for producing a gas barrier molded article of the present invention, by using a dispersion containing anionic functional group-containing cellulose nanocrystals at a concentration equal to or lower than the critical interaction concentration, a gas barrier molded article having an orientation degree in the above range can be efficiently molded without being affected by the shear force during molding. [Brief description of the drawings]
[0010] [Figure 1] 1 shows an atomic force microscope photograph (A), a binarized photograph (B), and a Fourier transform image (C) of the molded product obtained in Example 1. [Diagram 2] 1 shows an atomic force microscope photograph (A), a binarized photograph (B), and a Fourier transform image (C) of the molded body obtained in Comparative Example 1. [Diagram 3] This figure shows the relationship between the shear viscosity η (Pa·s) and shear rate (1 / s) of nanocellulose-containing aqueous dispersions at 25°C. [Figure 4] FIG. 1 is a diagram showing the relationship between the specific viscosity ηsp and the concentration (mass%) of a nanocellulose-containing aqueous dispersion. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] (Gas barrier molded article) The gas barrier properties provided by nanocellulose are achieved when the self-organized structure formed by the charged repulsion between nanocellulose particles becomes dense and acts as a barrier to the permeation path of the permeating gas. However, in gas barrier molded products containing nanocellulose, a self-organized structure in which the nanocellulose is oriented is formed due to the application of shear forces, etc. during molding into the product, which has been a problem in that sufficient gas barrier properties cannot be obtained. The gas barrier molded article of the present invention is capable of exhibiting excellent gas barrier properties because the self-organized structure of the nanocellulose is densified without being affected by shear. In the present invention, the degree of orientation of nanocellulose in the self-organized structure of a gas barrier molded body was quantified using a fiber orientation measurement program (Emae Toshiharu, "Application of image correlation method to measure in-plane strain distribution of paper", Nondestructive Inspection 56(11) 561-566 (2007)). It was found that in molded bodies with an orientation degree of less than 1.14, particularly in the range of 1.00 to 1.05, the self-organized structure in which nanocellulose is not oriented is densified, resulting in excellent barrier properties.
[0012] That is, in this fiber orientation measurement program, a photograph (A) of a gas barrier molded product made of nanocellulose is taken with an atomic force microscope (AFM) as shown in Figures 1 and 2, this photograph (A) is binarized as shown in (B), and the binarized image (B) is Fourier transformed to obtain an image (C), from which the degree of orientation is determined. The closer the image (C) is to a perfect circle, the more non-oriented it is. As is clear from comparing Fig. 1 for the molded product obtained in Example 1 of the present invention with Fig. 2 for the molded product obtained in Comparative Example 2, the nanocellulose in the molded product of Comparative Example 1 (orientation degree 1.02) is oriented in the coating direction, whereas the nanocellulose in the molded product of Example 1 (orientation degree 1.14) is randomly present and not oriented. In addition, when comparing the evaluation of the gas barrier properties of the molded products of Example 1 and Comparative Example 1, the molded product of Example 1 had an oxygen permeability of 0.59 cc / m 2The gas barrier properties and the degree of orientation are shown in Table 1.
[0013] (Cellulose nanocrystals containing anionic functional groups) It is important that the gas barrier molded article of the present invention is made of anionic functional group-containing cellulose nanocrystals. As described above, by using anionic functional group-containing cellulose nanocrystals, nanocellulose with short fiber length and excellent gas barrier properties can be obtained, and in combination with the above-mentioned self-organized structure of nanocellulose without orientation, particularly excellent gas barrier properties can be expressed. In addition, the gas barrier properties of nanocellulose are expressed by the self-organized structure formed by charge repulsion between nanocellulose particles becoming a barrier to the permeation path of the permeating gas. Therefore, by the presence of anionic functional groups such as sulfate groups and / or sulfo groups, phosphate groups, or carboxyl groups on the surface of anionic functional group-containing cellulose nanocrystals, the charges (anions) of these anionic functional groups efficiently form a self-organized structure, and excellent gas barrier properties can be expressed. As the anionic functional group to be contained in the anionic functional group-containing cellulose nanocrystal, as described later, it is preferable that the phosphate group or carboxyl group is at least one of 0.01 to 4.0 mmol / g, particularly 0.1 to 2.0 mmol / g, and the sulfate group and / or sulfo group are preferably contained in an amount of 0.01 to 4.0 mmol / g, particularly 0.1 to 2.0 mmol / g. By the amount of the anionic functional group being within the above range, a sufficient self-organized structure is formed, the crystal structure of the nanocellulose is maintained, and excellent gas barrier properties can be obtained.
[0014] The anionic functional group-containing cellulose nanocrystals used in the present invention desirably have a crystallinity of 60% or more since the anionic functional groups such as sulfate groups and / or sulfo groups, phosphate groups, or carboxyl groups are within the above ranges. The cellulose nanocrystal preferably has a fiber width of 50 nm or less, particularly from 2 to 50 nm, and a fiber length of 500 nm or less, particularly from 100 to 500 nm.
[0015] The anionic functional group-containing cellulose nanocrystals constituting the molded article of the present invention are sulfate group- and / or sulfo group-containing cellulose nanocrystals obtained by treating a cellulose raw material with sulfuric acid, and can also be produced by further subjecting the raw material to hydrophilization treatment. Furthermore, before or after the hydrophilization treatment, the raw material can be subjected to defibration treatment and dispersion treatment, if necessary.
[0016] [Cellulose nanocrystals containing anionic functional groups] The anionic functional group-containing cellulose nanocrystals constituting the molded article of the present invention are rod-shaped cellulose crystal fibers obtained by acid hydrolysis of cellulose fibers such as pulp with sulfuric acid or the like, but in the present invention, anionic functional group-containing cellulose nanocrystals obtained by sulfuric acid treatment are used, which have sulfate groups and / or sulfo groups that can contribute to the formation of a self-organized structure. In this specification, the term "sulfate group" is used as a concept that includes sulfate ester groups. The anionic functional group-containing cellulose nanocrystal preferably contains sulfate groups and / or sulfo groups in an amount of 0.01 to 0.17 mmol / g. The cellulose nanocrystal preferably has an average fiber diameter of 50 nm or less, particularly 2 to 50 nm, an average fiber length of 100 to 500 nm, an aspect ratio of 5 to 50, and a crystallinity of 60% or more, particularly 70% or more. Furthermore, the anionic functional group-containing cellulose nanocrystals used in the present invention can also be obtained by subjecting anionic functional group-containing cellulose nanocrystals having sulfate groups and / or sulfo groups to the hydrophilization treatment described below. However, cellulose nanofibers produced by conventional oxidation methods and having a fiber width of 50 nm or less and an aspect ratio of 10 or more may also be contained within a range that does not impair the excellent barrier properties and handleability of the nanocellulose of the present invention. Specifically, they can be used in an amount of less than 50% of the anionic functional group-containing cellulose nanocrystals.
[0017] [Hydrophilic treatment] By subjecting the above-mentioned anionic functional group-containing cellulose nanocrystals having sulfate and / or sulfo groups to hydrophilization treatment, the amount of sulfate and / or sulfo groups is adjusted, or anionic functional groups such as phosphate and carboxyl groups are introduced into the hydroxyl groups of cellulose to prepare cellulose nanocrystals having a total amount of anionic functional groups such as sulfate and / or sulfo groups, phosphate and carboxyl groups in the range of 0.01 to 4.0 mmol / g, particularly 0.1 to 3.0 mmol / g. As described above, it is particularly preferable to contain at least one of phosphate groups, sulfate groups, sulfo groups and carboxyl groups in an amount of 0.01 to 4.0 mmol / g. The hydrophilization treatment is carried out by never-dry treatment, or by using either of never-dry treatment and water-soluble carbodiimide, sulfuric acid, sulfur trioxide-pyridine complex, phosphoric acid-urea, TEMPO catalyst, or oxidizing agent. By the treatment using either of carbodiimide, sulfuric acid, or sulfur trioxide-pyridine complex, the amount of sulfate group and / or sulfo group of the anionic functional group-containing cellulose nanocrystal is adjusted, and further, the anionic functional group-containing cellulose nanocrystal is further shortened. Furthermore, by the treatment using either of phosphoric acid-urea, TEMPO catalyst, or oxidizing agent, anionic functional group of phosphoric acid group or carboxyl group is introduced, and the total amount of anionic functional group of the anionic functional group-containing cellulose nanocrystal is adjusted to the above range. As for the hydrophilization treatment, any one of the treatments may be carried out so long as the total amount of anionic functional groups falls within the above-mentioned range, but the same treatment may be carried out multiple times, or may be carried out multiple times in combination with other treatments.
[0018] <Hydrophilic treatment using Never Dry treatment> Anionic functional group-containing cellulose nanocrystals are solidified into powder or the like by drying treatment such as spray drying, heating, and reduced pressure, but during solidification by drying treatment, some of the anionic functional groups contained in the anionic functional group-containing cellulose nanocrystals are eliminated, resulting in a decrease in hydrophilicity. In other words, a never-dry treatment that does not solidify the anionic functional group-containing cellulose nanocrystal into powder or the like is an example of a hydrophilization treatment. The anionic functional groups in the never-dry treatment alone are sulfate groups and / or sulfo groups, but by combining it with a hydrophilization treatment described below, phosphate groups and carboxyl groups are further added.
[0019] <Hydrophilic treatment using carbodiimide> In the treatment using carbodiimide, cellulose nanocrystals and carbodiimide are stirred in a solvent such as dimethylformamide, sulfuric acid is added thereto, and the mixture is reacted for 5 to 300 minutes at a temperature of 0 to 80° C. to form a sulfate ester. The carbodiimide and sulfuric acid are preferably used in amounts of 5 to 30 mmol and 5 to 30 mmol per gram (solid content) of anionic functional group-containing cellulose nanocrystals. Next, it is preferable to add an alkaline compound such as sodium hydroxide to convert the sulfate and / or sulfo groups introduced into the anionic functional group-containing cellulose nanocrystal from H type to Na type in order to improve the yield. Then, impurities are removed by filtration using a dialysis membrane or the like to prepare sulfate and / or sulfo group-modified anionic functional group-containing cellulose nanocrystal. Examples of carbodiimides include 1-ethyl-3-(3-dimethylaminopropyl)carbodiimide, which is a water-soluble compound having a carbodiimide group (-N=C=N-) in the molecule. Dicyclohexylcarbodiimide, which is soluble in organic solvents, can also be used.
[0020] <Hydrophilic treatment using sulfuric acid> The anionic functional group-containing cellulose nanocrystal used in the present invention is obtained by hydrolyzing cellulose fibers with sulfuric acid, but this anionic functional group-containing cellulose nanocrystal can also be further hydrophilized with sulfuric acid. Sulfuric acid is preferably used at 40 to 60 mass% per 1 g (solid content) of the anionic functional group-containing cellulose nanocrystal. The reaction is carried out at a temperature of 40 to 60°C for 5 to 300 minutes, and then the mixture is subjected to a filtration treatment using a dialysis membrane or the like to remove impurities, thereby preparing a sulfate group and / or sulfo group-modified anionic functional group-containing cellulose nanocrystal.
[0021] <Hydrophilic treatment using sulfur trioxide-pyridine complex> In the treatment using a sulfur trioxide-pyridine complex, anionic functional group-containing cellulose nanocrystals are reacted with the sulfur trioxide-pyridine complex in dimethyl sulfoxide at a temperature of 0 to 60°C for 5 to 240 minutes to introduce sulfate and / or sulfo groups into the hydroxyl groups at the 6-position of the cellulose glycol units. The sulfur trioxide-pyridine complex is preferably mixed in an amount of 0.5 to 4 g by mass per 1 g (solid content) of the anionic functional group-containing cellulose nanocrystal. After the reaction, it is preferable to add an alkaline compound such as sodium hydroxide to convert the sulfate and / or sulfo groups introduced into the anionic functional group-containing cellulose nanocrystal from H type to Na type in order to improve the yield. Then, dimethylformamide or isopropyl alcohol is added, the mixture is washed by centrifugation or the like, impurities are removed by filtration using a dialysis membrane or the like, and the resulting concentrate is dispersed in water to prepare sulfate and / or sulfo group-modified anionic functional group-containing cellulose nanocrystal.
[0022] <Hydrophilic treatment using phosphoric acid-urea> The hydrophilic treatment using phosphoric acid-urea can be carried out in the same manner as the conventionally known treatment for introducing a phosphate group using phosphoric acid-urea. Specifically, in the presence of a urea-containing compound, an anionic functional group-containing cellulose nanocrystal having a sulfate group and / or a sulfo group and a phosphate group-containing compound are reacted at a temperature of 135 to 180 ° C for 5 to 120 minutes, thereby introducing a phosphate group into the hydroxyl group of the cellulosic glucose unit. Examples of the phosphate group-containing compound include phosphoric acid, lithium salt of phosphoric acid, sodium salt of phosphoric acid, potassium salt of phosphoric acid, ammonium salt of phosphoric acid, etc. Among them, sodium dihydrogen phosphate, ammonium dihydrogen phosphate, phosphoric acid, etc. can be preferably used alone or in combination. The phosphate group-containing compound is preferably added in an amount of 10 to 100 mmol based on 10 g (solid content) of the anionic functional group-containing cellulose nanocrystal. Examples of the urea-containing compound include urea, thiourea, biuret, phenylurea, benzylurea, dimethylurea, etc. Among them, urea can be preferably used. The urea-containing compound is preferably used in an amount of 150 to 200 mmol based on 10 g (solid content) of the anionic functional group-containing cellulose nanocrystal.
[0023] <Hydrophilic treatment using TEMPO catalyst> The hydrophilic treatment using a TEMPO catalyst (2,2,6,6-tetramethylpiperidine-1-oxyl) can be carried out in the same manner as the conventionally known oxidation method using a TEMPO catalyst. Specifically, an anionic functional group-containing cellulose nanocrystal is caused to undergo a hydrophilic reaction of oxidizing the hydroxyl group at the 6-position of the cellulose glucose unit to a carboxyl group under the conditions of an aqueous system, normal temperature, and normal pressure via a TEMPO catalyst (2,2,6,6-tetramethylpiperidine 1-oxyl). As the TEMPO catalyst, in addition to the above-mentioned 2,2,6,6-tetramethylpiperidine 1-oxyl, derivatives of TEMPO such as 4-acetamido-TEMPO, 4-carboxy-TEMPO, and 4-phosphonoxy-TEMPO can also be used. The amount of the TEMPO catalyst used is 0.01 to 100 mmol, preferably 0.01 to 5 mmol, per 1 g of the anionic functional group-containing cellulose nanocrystal (solid content).
[0024] During the hydrophilization treatment, it is preferable to use a co-oxidant such as an oxidant, bromide or iodide alone or in combination with the TEMPO catalyst. Examples of the oxidizing agent include known oxidizing agents such as halogen, hypohalous acid, halous acid, perhalogen acid or their salts, halogen oxides, and peroxides, and sodium hypochlorite and sodium hypobromite are particularly suitable. The amount of the oxidizing agent is 0.5 to 500 mmol, preferably 5 to 50 mmol, per gram of anionic functional group-containing cellulose nanocrystal (solid content). After a certain period of time has elapsed since the addition of the oxidizing agent, the oxidizing agent can be further added to carry out additional oxidation treatment. As the co-oxidizing agent, an alkali metal bromide such as sodium bromide, or an alkali metal iodide such as sodium iodide can be suitably used. The amount of the co-oxidizing agent is 0.1 to 100 mmol, preferably 0.5 to 5 mmol, per 1 g of the anionic functional group-containing cellulose nanocrystal (solid content). The reaction medium for the reaction solution is preferably water or an alcohol solvent.
[0025] The reaction temperature for the hydrophilization treatment is in the range of 1 to 50° C., particularly 10 to 50° C., and may be room temperature. The reaction time is preferably 1 to 360 minutes, particularly 60 to 240 minutes. As the reaction proceeds, carboxyl groups are produced in the cellulose, causing a decrease in the pH of the slurry. However, in order to ensure efficient oxidation reaction, it is desirable to maintain the pH in the range of 9 to 12 using a pH adjuster such as sodium hydroxide. After the oxidation treatment, the catalyst and other substances used are removed by washing with water or the like.
[0026] [Fiber defibration processing] The anionic functional group-containing cellulose nanocrystal used in the present invention uses cellulose nanocrystals having short fiber length as a raw material, so that it is possible to carry out a defibration treatment after the hydrophilization treatment, although this is not necessarily required. The defibration treatment can be carried out by a conventionally known method. Specifically, the fiber can be pulverized using an ultra-high pressure homogenizer, an ultrasonic homogenizer, a grinder, a high-speed blender, a bead mill, a ball mill, a jet mill, a disintegrator, a beater, a twin-screw extruder, or the like. The defibration treatment can be performed in either a dry or wet manner, depending on the state of the nanocellulose after the hydrophilization treatment and the application of the nanocellulose. Since nanocellulose is preferably used in the form of a dispersion, it is preferable to defibrate it using water or the like as a dispersion medium with an ultra-high pressure homogenizer or the like.
[0027] [Mixture of cellulose nanocrystals containing anionic functional groups and hydrophilic resin] The gas barrier molded article of the present invention is a molded article made from anionic functional group-containing cellulose nanocrystals, and is preferably made from a mixture with a hydrophilic resin. As such a hydrophilic resin, known water-soluble polymers such as polyvinyl alcohol, polyvinylpyrrolidone, and polyacrylic acid can be used, but in the present invention, it is particularly desirable to use a polyvalent cationic resin, which will be described later. As will be described later, by forming a layer containing anionic functional group-containing cellulose nanocrystals on a layer made of a polyvalent cationic resin, the self-organized structure of the anionic functional group-containing cellulose nanocrystals is maintained while being mixed with the polyvalent cationic resin, and a molded product of the mixture having a mixed state capable of expressing gas barrier properties and adhesion to the substrate can be formed. In addition, in the molded product made of this mixture, both nanocellulose and polyvalent cationic resin are present from near the surface to the inside.
[0028] The polyvalent cationic resin used in the molded article of the present invention is a resin containing a water-soluble or water-dispersible polyvalent cationic functional group. Examples of such polyvalent cationic resins include water-soluble amine polymers such as polyethyleneimine, polyallylamine, polyamine polyamide epichlorohydrin, polyamine epichlorohydrin, polyacrylamide, poly(diallyldimethylammonium salt), dicyandiamide formalin, poly(meth)acrylate, cationized starch, cationized gum, gelatin, chitin, chitosan, etc., among which water-soluble amine and / or amino group-containing polymers, particularly polyethyleneimine, can be used preferably.
[0029] The molded article of the present invention can be a film, sheet, etc. consisting of only a dispersion containing anionic functional group-containing cellulose nanocrystals described below, or a mixture of anionic functional group-containing cellulose nanocrystals and a hydrophilic resin, but is preferably one consisting of a barrier layer consisting of a mixture of anionic functional group-containing cellulose nanocrystals and a hydrophilic resin formed on a substrate consisting of a hydroxyl group- and / or carboxyl group-containing resin. The presence of the polyvalent cationic resin improves the interfacial peel strength with the thermoplastic resin, and effectively prevents interlayer delamination between the barrier layer and the substrate. Examples of the substrate include films, sheets, and molded articles in the form of bottles, cups, trays, pouches, etc., produced by means of lamination molding, extrusion molding, injection molding, blow molding, stretch blow molding, press molding, or the like using hydroxyl group- and / or carboxyl group-containing resins. The thickness of the substrate cannot be generally defined depending on the shape and application of the laminate, but in the case of a film, it is preferably in the range of 5 to 50 μm.
[0030] Examples of the resin used as the base material include olefin copolymers such as low-, medium- or high-density polyethylene, linear low-density polyethylene, polypropylene, ethylene-propylene copolymer, ethylene-butene copolymer, ionomer, ethylene-vinyl acetate copolymer, and ethylene-vinyl alcohol copolymer; aromatic polyesters such as polyethylene terephthalate, polybutylene terephthalate, polyethylene terephthalate / isophthalate, and polyethylene naphthalate; aliphatic polyesters such as polylactic acid, polycaprolactone, polybutylene succinate, and polyhydroxyalkanoic acid; polyamides such as nylon 6, nylon 6,6, nylon 6,10, and metaxylylene adipamide; polystyrene, styrene-butadiene block copolymer, and styrene-butadiene block copolymer. Examples of suitable resins include styrene-based copolymers such as styrene-acrylonitrile copolymer and styrene-butadiene-acrylonitrile copolymer (ABS resin); vinyl chloride-based copolymers such as polyvinyl chloride and vinyl chloride-vinyl acetate copolymer; acrylic copolymers such as polymethyl methacrylate and methyl methacrylate-ethyl acrylate copolymer; thermoplastic resins such as polycarbonate, cellulose-based resins such as acetyl cellulose, cellulose acetyl propionate, and cellulose acetate butyrate, regenerated cellulose such as cellophane, polyvinyl alcohol, and polyacrylic acid. Of these, resins containing hydroxyl groups and / or carboxyl groups are preferred, and polyester resins, regenerated cellulose, polyvinyl alcohol, and polyacrylic acid are particularly preferred. The resin serving as the base material may contain one or more additives such as pigments, fine particles, antioxidants, antistatic agents, ultraviolet absorbers, lubricants, etc., as desired.
[0031] In the molded article of the present invention, other layers may be formed, if necessary, in addition to the layer consisting of the substrate and molded article. Since the gas barrier properties of the nanocellulose-containing layer decrease under high humidity conditions, it is preferable to further form a layer made of a conventional moisture-resistant resin such as an olefin resin, a polyester resin, or a cured reaction product of an epoxy resin and a polyamine resin.
[0032] (Method of manufacturing gas barrier molded article) As mentioned above, an important feature of the gas barrier molded article of the present invention is that the orientation degree measured using a fiber orientation measurement program is less than 1.14. In order for the molded article to have such an orientation degree, it is important to use a dispersion liquid containing anionic functional group-containing cellulose nanocrystals at a concentration equal to or lower than the critical interaction concentration. That is, as mentioned above, the barrier properties of nanocellulose are exerted by the densification of the self-organized structure, but when a nanocellulose-containing dispersion is applied, a shear force is applied in the coating direction. This shear force causes interactions in the nanocellulose, which causes it to self-organize in an oriented state in the coating direction, and as a result, the barrier properties tend to decrease, as mentioned above in Figure 2. In the present invention, it has been discovered that by using a dispersion liquid with a dilute concentration below the critical concentration at which interactions between anionic functional group-containing cellulose nanocrystals begin to occur, a self-assembled structure in which anionic functional group-containing cellulose nanocrystals are oriented in random directions can be formed without being affected by the shear force caused by coating.
[0033] The critical interaction concentration of a cellulose nanocrystal-containing dispersion can be calculated as follows. That is, the shear viscosity η (Pa·s, 25°C) of an aqueous dispersion containing anionic functional group-containing cellulose nanocrystals is measured using a rheometer. Using the obtained shear viscosity η and the viscosity η0 of water, which is the solvent, the following formula (1) is used: η sp =(η-η0) / η0 (1) From the specific viscosity η sp Calculate. This specific viscosity η sp The relationship between the concentration (mass%) of the cellulose nanocrystal-containing aqueous dispersion is shown in Figure 4. As is clear from Figure 4, there is a concentration at which the slope of the linear approximation line clearly changes, and the critical interaction concentration can be calculated from the intersection of this linear approximation line. The critical interaction concentration varies depending on the type and amount of functional groups in the anionic functional group-containing cellulose nanocrystals used, and in the present invention, it is preferable to use anionic functional group-containing cellulose nanocrystals whose critical interaction concentration (based on solids content) is less than 5 mass%. Furthermore, it is preferable that the dispersion containing such anionic functional group-containing cellulose nanocrystals is adjusted to a concentration less than the critical interaction concentration, particularly a concentration of 1 to 3 mass %, which allows the formation of a dense self-assembled structure without being affected by shear.
[0034] As mentioned above, the molded article of the present invention can be a molded article consisting of only the anionic functional group-containing cellulose nanocrystal dispersion, but it is preferably a molded article consisting of a mixture with a hydrophilic resin from the viewpoints of barrier properties and adhesion to the substrate. A specific method for producing a molded article made of a mixture of anionic functional group-containing cellulose nanocrystals and a polyvalent cationic resin used as a hydrophilic resin will be described below.
[0035] [Coating and drying of polycation resin-containing solution] To produce a molded article consisting of a mixture of anionic functional group-containing cellulose nanocrystals and polycationic resin, a solution containing the polycationic resin is first coated on a substrate and dried. The polycation resin-containing solution preferably contains the polycation resin in an amount of 0.01 to 30 mass %, particularly 0.1 to 10 mass %, based on the solid content. If the amount of the polycation resin is less than the above range, the gas barrier property and the interfacial peel strength cannot be improved as compared with the case where the amount is within the above range, while if the amount of the polycation resin is more than the above range, the gas barrier property and the interfacial peel strength cannot be further improved, resulting in poor economic efficiency and possibly poor coatability and film-forming property. The solvent used for the polyvalent cation resin-containing solution may be water, alcohols such as methanol, ethanol, and isopropanol, ketones such as 2-butanone and acetone, aromatic solvents such as toluene, and mixed solvents of these with water.
[0036] The amount of the polycation resin-containing solution to be applied is determined based on the amount of anionic functional group-containing cellulose nanocrystals (solid content) in the layer formed from the anionic functional group-containing cellulose nanocrystal-containing dispersion liquid, and is determined by the concentration of the polycation resin-containing solution. 2 When the polyvalent cation resin is contained in an amount of 1.0 g per m 2 It is preferable to coat the polycation resin in an amount of 0.01 to 2.0 g per coating. If the amount of the polycation resin is less than the above range, the interfacial peel strength with respect to a hydrophobic substrate such as a polyester resin cannot be improved as compared with the case where the amount is within the above range, while if the amount of the polycation resin is more than the above range, the gas barrier property of the molded article may not be improved as compared with the case where the amount is within the above range. The coating method is not limited to the above, but can be, for example, spray coating, immersion, or coating with a bar coater, roll coater, gravure coater, etc. The coating is preferably dried at a temperature of 5 to 200° C. for 0.1 seconds to 24 hours. The drying process can be performed by oven drying, infrared heating, high-frequency heating, etc., but natural drying is also possible.
[0037] [Coating and drying of dispersion containing cellulose nanocrystals with anionic functional groups] As described above, it is important to use a dispersion containing cellulose nanocrystals having an anionic functional group at a concentration equal to or lower than the critical interaction concentration. As described above, the critical interaction concentration (based on the solid content) of the dispersion containing the anionic functional group-containing cellulose nanocrystals is preferably 5% by mass or less, particularly in the range of 1 to 3% by mass, which makes it possible to form a film without being affected by the orientation force (shear force) during coating. The dispersion liquid may be water alone, or may be a mixed solvent of water and an alcohol such as methanol, ethanol, isopropanol, etc., a ketone such as 2-butanone, acetone, etc., or an aromatic solvent such as toluene, etc. In addition, the above-mentioned polyvalent cationic resin-containing solution or anionic functional group-containing cellulose nanocrystal-containing dispersion liquid may contain known additives such as fillers, colorants, UV absorbers, antistatic agents, water-resistant agents, clay minerals, crosslinking agents, metal salts, colloidal silica, fine particles, alumina sol, titanium oxide, etc., as necessary.
[0038] The anionic functional group-containing cellulose nanocrystal-containing dispersion liquid is a dispersion liquid containing 1m of anionic functional group-containing cellulose nanocrystals (solid content). 2 It is preferable that the coating amount is 0.1 to 3.0 g per coating, and the coating thickness is preferably in the range of 0.1 to 3.0 μm. The anionic functional group-containing cellulose nanocrystal dispersion liquid used in the present invention uses a dispersibility at a concentration less than the critical interaction concentration, which is less susceptible to the effects of shear forces, and therefore the coating and drying methods can be similar to those for the polyvalent cation-containing solution. However, since it is more desirable to minimize the application of shear forces during film formation, coating with a bar coater, spray, gravure coater, or die coater is particularly preferred, and natural drying (drying at room temperature for 24 hours or more) is particularly preferred. EXAMPLES
[0039] Examples of the present invention will be described below. Note that the following examples are merely examples of the present invention, and the present invention is not limited to these examples. The preparation and analysis methods for each item are as follows.
[0040] <Specific Viscosity and Critical Interaction Concentration> A 0.01% to 5% dispersion of cellulose nanocrystals containing an anionic functional group was prepared, and the shear rate was varied from 1 to 1,000 s using a rheometer (Anton Paar, MCR-300). -1The shear viscosity was measured in the range of η (Pa s, 25°C) and the viscosity of water η0 (Figure 3). The specific viscosity of the dispersion η sp was calculated and the relationship with the concentration was plotted as shown in Figure 4. Linear approximation lines were calculated before and after each clear inflection point, and the critical interaction concentration of the anionic functional group-containing cellulose nanocrystal dispersion used was determined from the intersection with the two linear approximation curves.
[0041] <Atomic Force Microscope (AFM)> A molded body consisting of a mixture of anionic functional group-containing cellulose nanocrystals and polycationic resin was fixed to a holder so that the coating direction could be determined, and a shape image of the molded body was obtained using an atomic force microscope (Hitachi High-Technologies Corporation, AFM5300E, probe SI-DF20Plus) at room temperature and atmospheric pressure. The obtained shape image was corrected for sample tilt and probe shape, and a clear fiber orientation state of the anionic functional group-containing cellulose nanocrystals was confirmed.
[0042] <Orientation degree> The fiber orientation measurement program (Emae Toshiharu, "Application of Image Correlation Method to Measure the In-Plane Strain Distribution of Paper", Nondestructive Inspection 56(11)561-566(2007)) was used to convert the clear fiber shape image obtained from the atomic force microscope into a binary image and perform a Fourier transform to calculate the orientation direction and degree of the molded body.
[0043] <Oxygen permeability> The molded product consisting of a mixture of anionic functional group-containing cellulose nanocrystals and polyvalent cationic resin was measured for oxygen permeability (cc / m) at 23°C and 0% RH using an oxygen permeability measuring device (OX-TRAN2 / 22, manufactured by Mocon). 2 ·day·atm) was measured.
[0044] Example 1 <Preparation of anionic functional group-containing cellulose nanocrystal dispersion> Anionic functional group-containing cellulose nanocrystals with a total amount of anionic functional groups of 0.17 mmol / g were added with ion exchange water so that the solid content was 1% by mass, and the mixture was stirred with a stirrer for 2 hours. After that, dispersion treatment was performed using ultrasonic treatment for 30 minutes to obtain a 1% by mass dispersion liquid of anionic functional group-containing cellulose nanocrystals.
[0045] <Preparation of Molded Product Made of Mixture Containing Polyvalent Cationic Resin and Cellulose Nanocrystals> A molded article was prepared from a mixture containing a polycationic resin and anionic functional group-containing cellulose nanocrystals by the following procedure. Polyethylenimine (PEI) (Epomin, P-1000, Nippon Shokubai Co., Ltd.) was applied to a corona-treated biaxially stretched PET film (Lumirror P60, 12 μm, Toray Industries, Inc.) substrate using a bar coater at a solid weight of 0.1 g / m2. 2 The substrate was dried at 50°C for 10 minutes in a hot air dryer (MSO-TP, manufactured by ADVANTEC) to volatilize the solvent, and then coated with 1% by mass of the anionic functional group-containing cellulose nanocrystal dispersion liquid produced by the above method using a bar coater and air-dried at room temperature overnight. The coating amount was 1.0 g / m2 in terms of solid content. 2 It was.
[0046] Example 2 The solids concentration in the anionic functional group-containing cellulose nanocrystal dispersion was adjusted to 2% by mass, and the solids content of the anionic functional group-containing cellulose nanocrystals was adjusted to 1.0 g / m 2 The same procedure as in Example 1 was carried out except that the content was adjusted so that the content was 1.0 to 1.0, and a molded product made of a mixture containing a polyvalent cationic resin and cellulose nanocrystals was obtained.
[0047] Example 3 The solids concentration in the anionic functional group-containing cellulose nanocrystal dispersion was adjusted to 3% by mass, and the solids content of the anionic functional group-containing cellulose nanocrystals was adjusted to 1.0 g / m 2The same procedure as in Example 1 was carried out except that the content was adjusted so that the content was 1.0 to 1.0, and a molded product made of a mixture containing a polyvalent cationic resin and cellulose nanocrystals was obtained.
[0048] Comparative Example 1 The solids concentration in the anionic functional group-containing cellulose nanocrystal dispersion was adjusted to 5% by mass, and the solids content of the anionic functional group-containing cellulose nanocrystals was adjusted to 1.0 g / m 2 The procedure of Example 1 was repeated except that the content was adjusted so that the content was within the range of 1:1 to 1:1, thereby obtaining a molded product made of a mixture containing a polyvalent cationic resin and an anionic functional group-containing cellulose nanocrystal.
[0049] [Table 1] [Industrial Applicability]
[0050] The gas barrier molded article of the present invention has excellent gas barrier properties, and when mixed with a hydrophilic resin, it can exhibit gas barrier properties that are superior to those exhibited by anionic functional group-containing cellulose nanocrystals alone. Since the interfacial peel strength with a hydrophobic substrate made of a thermoplastic resin or the like is also improved, it can be suitably used as a gas barrier film or a gas barrier laminate.
Claims
1. A gas barrier molded body comprising a mixture of anionic functional group-containing cellulose nanocrystals having a fiber length of 500 nm or less and an aspect ratio in the range of 5 to 50, and a water-soluble amine and / or amino group-containing polymer, wherein the anionic functional groups contain at least sulfate groups and / or sulfo groups, and the degree of orientation measured using a fiber orientation measurement program is less than 1.
14.
2. 2. The gas barrier molded article according to claim 1, wherein the anionic functional group further comprises at least one of a phosphate group and a carboxyl group.
3. 3. The gas-barrier molded article according to claim 1, wherein the anionic functional group-containing cellulose nanocrystal contains 0.01 to 4.0 mmol / g of phosphate groups or carboxyl groups.
4. 4. The gas-barrier molded article according to claim 1, wherein the anionic functional group-containing cellulose nanocrystal contains 0.01 to 4.0 mmol / g of sulfate group and / or sulfo group.
5. 5. The gas barrier molded article according to claim 1, wherein the anionic functional group-containing cellulose nanocrystal has a fiber width of 50 nm or less, a fiber length of 500 nm or less, and a crystallinity of 60% or more.
6. 6. The gas barrier molded article according to claim 1, which comprises a mixture of the anionic functional group-containing cellulose nanocrystal and a hydrophilic resin.
7. The anionic functional group-containing cellulose nanocrystals were mixed in an amount of 1 ml as a solid content. 2 When the oxygen content is 1.0 g per unit, the oxygen permeability at 23°C and 0% RH is 0.59 cc / m 2 7. The gas barrier molded article according to claim 6, wherein the gas barrier density is less than 1 / day / atm.
8. A method for producing a gas barrier molded product, comprising coating and drying a solution containing a hydrophilic resin to form a layer consisting of a hydrophilic resin, and coating and drying a dispersion liquid containing cellulose nanocrystals containing anionic functional groups at a concentration not exceeding the critical interaction concentration on the layer consisting of a hydrophilic resin to form a layer containing cellulose nanocrystals containing anionic functional groups.
9. The method for producing a gas barrier molded article according to claim 8, wherein the critical interaction concentration of the dispersion is less than 5% by mass.
10. The method for producing a gas-barrier molded article according to claim 8 or 9, wherein the dispersion contains the anionic functional group-containing cellulose nanocrystals in a concentration of 1 to 3 mass %.
Citation Information
Patent Citations
JP1974065528A
Selffcleaning coating layer
JP1981078450A
Method for producing gas barrier material
JP2012122077A
Gas barrier material, method for producing the same, and gas barrier film
JP2016011392A
Flexible nanocrystalline cellulose (NCC) film with adjustable optical and mechanical properties