Dibutylene glycol copolymerized polybutylene terephthalate and its manufacturing method, compound product and its manufacturing method, and molded product and its manufacturing method

By controlling DBG copolymerization and catalysts in PBT production, the issues of coloration and by-product formation are mitigated, resulting in a stable and high-quality PBT suitable for electrical and electronic parts.

JP7559786B2Active Publication Date: 2024-10-02MITSUBISHI CHEM CORP
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2022029155
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-03-31
Filing Date
2022-02-28
Publication Date
2024-10-02
Estimated Expiration
2042-02-28

AI Technical Summary

Technical Problem

Existing PBT production methods result in dibutylene glycol (DBG) copolymerization, leading to increased coloration and the formation of undesirable by-products like formaldehyde and formic acid, which affect the quality and safety of molded products, especially in electrical and electronic parts.

Method used

Control the DBG copolymerization amount within a predetermined range (0.05 to 1.0 mol%) and manage catalysts and reaction conditions to produce dibutylene glycol copolymerized polybutylene terephthalate (DBG copolymerized PBT) with specific titanium and Group 2A metal contents, ensuring low terminal methoxycarbonyl groups and improved thermal stability.

Benefits of technology

The solution results in PBT with stable color tone and reduced by-product formation, suitable for electrical and electronic parts, with enhanced hydrolysis resistance and moldability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007559786000004
    Figure 0007559786000004
  • Figure 0007559786000005
    Figure 0007559786000005
  • Figure 0007559786000006
    Figure 0007559786000006
Patent Text Reader

Abstract

To provide a dibutylene glycol co-polymerized polybutylene terephthalate with less color tone change in drying under air, and favorably usable in an electric or electronic component, an automobile component, etc.SOLUTION: A dibutylene glycol co-polymerized polybutylene terephthalate includes a unit derived from a dicarboxylic acid component having a terephthalic acid component as a primary component and a unit derived from a diol component containing dibutylene glycol and having 1,4-butanediol as a primary component. A ratio of the unit derived from dibutylene glycol to the unit derived from a dicarboxylic acid component is 0.05 to 1.0 mol%.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to dibutylene glycol copolymerized polybutylene terephthalate, and more particularly to dibutylene glycol copolymerized polybutylene terephthalate which is excellent in color tone, hydrolysis resistance, thermal stability, and moldability, and which can be suitably used for electric / electronic parts, automobile parts, and the like (hereinafter, dibutylene glycol may be abbreviated as DBG and polybutylene terephthalate as PBT). The present invention also relates to a method for producing this DBG copolymer PBT, a compound product using this DBG copolymer PBT and a method for producing the same, and a molded article and a method for producing the same. [Background technology]

[0002] Polyester resins occupy an important position industrially due to their excellent mechanical and chemical properties. Aromatic polyester resins, especially PBT, are resins with excellent heat and chemical resistance, and are widely used in fields such as injection molding for electrical and electronic parts, automotive parts, and precision instrument parts due to their ease of processing and economic efficiency.

[0003] PBT is synthesized by melt polymerization at high temperature and reduced pressure using terephthalic acid and 1,4-butanediol (hereinafter, 1,4-butanediol may be abbreviated as BDO) as raw materials, after esterification or transesterification. In this case, if an ejector driven by the raw material BDO vapor is used as a vacuum generating device for reducing pressure, PBT can be produced efficiently and economically. In this case, more efficient production can be achieved by configuring a polymerization system (including esterification or transesterification) and an ejector circulation system for BDO.

[0004] However, the present inventors have found that BDO recovered from an ejector driven by BDO contains a significant amount of DBG, which is a dimer of BDO. In particular, when terephthalic acid is used as the acid component of the PBT raw material, this tendency is more pronounced than when dimethyl terephthalate is used. It is well known that BDO undergoes dehydration and cyclization when heated, partially converting it into tetrahydrofuran. However, it was not previously known that a certain amount of DBG is produced from the BDO used in the ejector. The inventors have also discovered that since this DBG has a higher boiling point than BDO, it is not distilled out of the system through the circulation system, and that if BDO containing DBG is used as a PBT raw material, the DBG will be copolymerized into the PBT.

[0005] Conventionally, DBG has been described in Patent Documents 1 and 2. Patent Document 1 describes DBG as an example of a diol component used in PBT, but does not disclose anything further, including its physical properties and the effects it has on the physical properties of PBT. Patent Document 2 describes that the free aromatic dicarboxylic acid dibutylene glycol ester in a PBT composition is kept at 100 ppm or less. However, this technology is characterized by reducing the free aromatic dicarboxylic acid dibutylene glycol ester component by adding an antioxidant or the like, and makes no mention of the generation of DBG or the copolymerization of the generated DBG with PBT.

[0006] By the way, when PBT is used in injection molding or other molding processes, it is necessary to dry the PBT before the molding process. This is because if this operation is not performed, the moisture contained in the resin will cause hydrolysis of the ester bonds, resulting in a decrease in molecular weight. A decrease in molecular weight is undesirable because it significantly impairs the quality of the molded product, such as reducing the strength and impact resistance of the molded product. In addition to impairing the quality of the molded product, there is also the problem that moisture evaporates inside the mold, causing various external molding problems such as air bubbles, silver streaks, weld lines, and cloudiness.

[0007] For this reason, PBT is dried before molding before being fed to the molding machine. For drying, various dryers are used, such as vacuum dryers that dry under vacuum, inert oven dryers that heat under nitrogen, shelf dryers that heat under air, hot air dryers, and hopper dryers. Among them, dryers that heat under air are often used because of their ease of use and cost. In this case, the drying temperature is often raised to complete the drying in a short time. Also, when the factory is shut down on a holiday or other day and then restarted to perform molding, the drying time may extend to several tens of hours as the drying process continues from before the shutdown. [Prior art documents] [Patent documents]

[0008] [Patent Document 1] JP 2004-277719 A [Patent Document 2] JP 2008-291237 A Summary of the Invention [Problem to be solved by the invention]

[0009] The present inventors have found that PBT produced using BDO produced by DBG contains copolymerized DBG, and that if PBT containing a certain amount of DBG is heated and dried, for example, under air at normal pressure prior to molding, coloring, particularly yellowing, increases. To prevent coloring by blending an antioxidant into PBT in advance is undesirable because the operation becomes complicated, the economy is poor, and there is also the problem of bleed-out.

[0010] When dimethyl terephthalate is used as the dicarboxylic acid component of the PBT raw material instead of terephthalic acid, the amount of BDO is relatively small compared to the dicarboxylic acid component, and there is no acid catalyst derived from terephthalic acid, so the generation of DBG can be suppressed. However, in this case, it is less economical in terms of raw material costs, and there is a problem that the methoxycarbonyl group derived from the raw material remains at the end of the PBT obtained using dimethyl terephthalate.

[0011] The terminal methoxycarbonyl groups of PBT need to be reduced for the following reasons: That is, in recent years, PBT has come to be widely used in food packaging films, but it generates methanol and its oxides, formaldehyde and formic acid, due to heat during molding, heating in a microwave oven, and enzymes, acids, and bases contained in food, causing harmful problems. Similarly, heat during kneading and molding generates methanol and its oxides, formaldehyde and formic acid. Formic acid can damage metal polymerization equipment, molding equipment, vacuum-related equipment, and so there is a demand for reducing it. Since these problems are caused by the terminal methoxycarbonyl groups of PBT, it is preferable that the terminal methoxycarbonyl groups of PBT are low, and for this reason, it is preferable to use terephthalic acid rather than dimethyl terephthalate. However, in this case, the generation of DBG becomes a problem.

[0012] An object of the present invention is to provide a DBG copolymerized PBT which undergoes little color change when dried in air and can be suitably used in electric / electronic parts, automobile parts, etc. Another object of the present invention is to provide a method for producing this DBG copolymer PBT, a compound product using this DBG copolymer PBT and a method for producing the same, and a molded article and a method for producing the same. [Means for solving the problem]

[0013] As a result of intensive research conducted by the present inventors to solve the above-mentioned problems, they discovered that the problems could be solved by using DBG-copolymerized PBT in which the amount of DBG copolymerized is within a predetermined range, and thus completed the present invention.

[0014] That is, the present invention relates to the following.

[0015] [1] A dibutylene glycol copolymerized polybutylene terephthalate comprising units derived from a dicarboxylic acid component mainly composed of a terephthalic acid component and units derived from a diol component mainly composed of 1,4-butanediol and containing dibutylene glycol, wherein the ratio of the units derived from dibutylene glycol to the units derived from the dicarboxylic acid component is 0.05 to 1.0 mol %.

[0016] [2] The dibutylene glycol copolymerized polybutylene terephthalate according to [1], having a titanium content of 100 ppm by mass or less.

[0017] [3] The dibutylene glycol copolymerized polybutylene terephthalate according to [2], having a titanium content of 50 ppm by mass or less.

[0018] [4] The dibutylene glycol copolymerized polybutylene terephthalate according to any one of [1] to [3], having a terminal methoxycarbonyl group concentration of 0.5 equivalents / ton or less.

[0019] [5] The dibutylene glycol copolymerized polybutylene terephthalate according to any one of [1] to [4], wherein the content of the metal of Group 2A of the Periodic Table is 5 to 50 ppm by weight in terms of metal atoms.

[0020] [6] The dibutylene glycol copolymerized polybutylene terephthalate according to [5], wherein the metal of Group 2A of the Periodic Table is magnesium.

[0021] [7] The dibutylene glycol copolymerized polybutylene terephthalate according to any one of [1] to [6], having a terminal carboxyl group concentration of 5 to 30 equivalents / ton.

[0022] [8] The dibutylene glycol copolymerized polybutylene terephthalate according to any one of [1] to [7], having an intrinsic viscosity of 0.6 to 1.3 dL / g.

[0023] [9] A method for producing dibutylene glycol-copolymerized polybutylene terephthalate according to any one of [1] to [8], characterized in that a 1,4-butanediol composition used as steam for a vacuum generator is used as a production raw material.

[0024]

[10] The method for producing dibutylene glycol-co-polybutylene terephthalate according to [9], wherein the temperature of the steam generating tank for the vacuum generating device is set to 256°C or lower.

[0025]

[11] A compound product, comprising the dibutylene glycol copolymerized polybutylene terephthalate pellets according to any one of [1] to [8] as at least a part of a raw material.

[0026]

[12] A method for producing a compound product, comprising using the dibutylene glycol copolymerized polybutylene terephthalate pellets according to any one of [1] to [8] as at least a part of a raw material and kneading the pellets using an extruder.

[0027]

[13] The method for producing a compound product according to

[12] , wherein the kneading resin temperature in the extruder is 320°C or lower.

[0028]

[14] A molded product, comprising at least a part of a molding material made from the compound product according to

[11] .

[0029]

[15] A method for producing a molded product, comprising using the compound product according to

[11] as at least a part of a molding material and molding the compound product using an injection molding machine.

[0030]

[16] The method for producing a molded article according to

[15] , wherein the molten resin temperature during the injection molding is 280°C or lower.

[0031]

[17] A method for producing a molded article according to

[15] or

[16] , in which recycled materials are used as at least a part of the molding material. Effect of the Invention

[0032] The DBG copolymer PBT of the present invention shows little color change when dried in air. Such DBG copolymer PBT, compound products containing the same, and molded products can be suitably used for electric / electronic parts, automobile parts, etc. [Brief description of the drawings]

[0033] [Figure 1] FIG. 1 is an explanatory diagram of an example of an esterification reaction step or an ester exchange reaction step used in the present invention. [Diagram 2] FIG. 2 is an explanatory diagram of an example of a polycondensation step employed in the present invention. [Diagram 3] FIG. 2 is an explanatory diagram of another example of the polycondensation step used in the present invention. [Figure 4] FIG. 2 is an explanatory diagram of an example of a vacuum generation process employed in the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0034] The present invention will be described in detail below. However, the explanation of the constituent elements described below is a representative example of the embodiment of the present invention, and the present invention is not limited to these contents.

[0035] [DBG copolymerized PBT] The DBG copolymerized PBT of the present invention is a dibutylene glycol copolymerized polybutylene terephthalate consisting of units derived from a dicarboxylic acid component mainly composed of a terephthalic acid component and units derived from a diol component mainly composed of 1,4-butanediol and containing dibutylene glycol, characterized in that the ratio of the units derived from dibutylene glycol to the units derived from the dicarboxylic acid component (hereinafter, this ratio may be referred to as the "DBG copolymerization amount") is 0.05 to 1.0 mol %.

[0036] In the present invention, the "main component" of the dicarboxylic acid component refers to a component that is contained in the dicarboxylic acid component in an amount of 50 mol % or more. The same applies to the "main component" of the diol component. Further, the term "unit" refers to a structural unit incorporated into the DBG copolymerized PBT from a raw material compound. For example, a unit derived from DBG refers to a structural unit derived from DBG and incorporated into the DBG copolymerized PBT.

[0037] In the present invention, PBT refers to a polymer having a structure in which a terephthalic acid component and a 1,4-butanediol (BDO) component are ester-bonded, in which 50 mol% or more of the dicarboxylic acid component is composed of a terephthalic acid component, and 50 mol% or more of the diol component is composed of BDO. The proportion of the terephthalic acid component in all dicarboxylic acid components is preferably 70 mol% or more, more preferably 80 mol% or more, and particularly preferably 95 mol% or more, and the proportion of BDO in all diol components is preferably 70 mol% or more, more preferably 80 mol% or more, and still more preferably 95 mol% or more, and particularly preferably all except DBG. If the terephthalic acid component or BDO is less than 50 mol%, the crystallization rate of PBT decreases, leading to deterioration of moldability. The DBG copolymerized PBT of the present invention is such a PBT that further incorporates DBG as a copolymerization component, and contains units derived from DBG at a specified ratio.

[0038] In the present invention, the dicarboxylic acid component includes dicarboxylic acid and dicarboxylic acid derivatives. There is no particular limitation on the dicarboxylic acid other than terephthalic acid, and examples thereof include aromatic dicarboxylic acids such as phthalic acid, isophthalic acid, 4,4'-diphenyldicarboxylic acid, 4,4'-diphenyletherdicarboxylic acid, 4,4'-benzophenonedicarboxylic acid, 4,4'-diphenoxyethanedicarboxylic acid, 4,4'-diphenylsulfonedicarboxylic acid, and 2,6-naphthalenedicarboxylic acid, alicyclic dicarboxylic acids such as 1,2-cyclohexanedicarboxylic acid, 1,3-cyclohexanedicarboxylic acid, and 1,4-cyclohexanedicarboxylic acid, and aliphatic dicarboxylic acids such as malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, and sebacic acid. Examples of the dicarboxylic acid derivative include esters of these dicarboxylic acids and ester-forming derivatives such as dicarboxylic acid halides. These dicarboxylic acid components other than the terephthalic acid component may be used alone or in combination of two or more.

[0039] In the present invention, there are no particular limitations on the use of diol components other than BDO and DBG, and examples thereof include aliphatic diols such as ethylene glycol, 1,2-propanediol, 1,3-propanediol, 1,5-pentanediol, neopentyl glycol, 1,6-hexanediol, and 1,8-octanediol; alicyclic diols such as 1,2-cyclohexanediol, 1,4-cyclohexanediol, 1,1-cyclohexanedimethylol, and 1,4-cyclohexanedimethylol; and aromatic diols such as xylylene glycol, 4,4'-dihydroxybiphenyl, 2,2-bis(4-hydroxyphenyl)propane, and bis(4-hydroxyphenyl)sulfone. As for these diol components other than BDO and DBG, one type may be used alone, or two or more types may be used in combination.

[0040] In the present invention, one or more of the following may be used as copolymerization components: hydroxycarboxylic acids such as lactic acid, glycolic acid, m-hydroxybenzoic acid, p-hydroxybenzoic acid, 6-hydroxy-2-naphthalenecarboxylic acid, and p-β-hydroxyethoxybenzoic acid; monofunctional components such as stearyl alcohol, benzyl alcohol, stearic acid, benzoic acid, t-butylbenzoic acid, and benzoylbenzoic acid; and polyfunctional components having three or more functional groups such as tricarballylic acid, trimellitic acid, trimesic acid, pyromellitic acid, gallic acid, trimethylolethane, trimethylolpropane, glycerol, and pentaerythritol.

[0041] The DBG copolymerized PBT of the present invention is used for engineering plastics. Therefore, the flexural modulus is preferably 2,000 MPa or more, more preferably 2,100 MPa, even more preferably 2,200 MPa, and most preferably 2,300 MPa or more. The upper limit is not particularly limited, but is preferably 2,700 MPa. When polyalkylene glycols such as polyethylene glycol, poly 1,3-propylene glycol, poly 1,2-propylene glycol, polytetramethylene ether glycol, polyneopentyl glycol, poly 3-methylpentanediol, and poly 1,5-pentanediol are copolymerized with PBT as a softening component, even a small amount of copolymerization significantly reduces the flexural modulus, making the material unsuitable for use in general engineering plastics. In addition, when these softening components are copolymerized, the color tone increases significantly when dried in air, which is undesirable. For this reason, it is preferable that the DBG copolymerized PBT of the present invention does not contain units derived from these softening components.

[0042] The DBG copolymerized PBT of the present invention is characterized in that the amount of DBG copolymerized is 0.05 to 1.0 mol%. If the amount of DBG copolymerized exceeds 1.0 mol%, the color tone of the DBG copolymerized PBT deteriorates when dried in air, and the object of the present invention cannot be achieved. In order to make the amount of DBG copolymerized less than 0.05 mol%, economically disadvantageous conditions must be adopted, which is not preferable. Even if a DBG copolymerized PBT in this range is produced by a method using, for example, dimethyl terephthalate as a raw material, the terminal methoxycarbonyl group remains in the PBT, and the heat during kneading and molding causes problems such as the generation of methanol, formaldehyde, and formic acid. The DBG copolymerization amount of the DBG copolymerized PBT of the present invention is 0.05 mol% or more, and is preferably 0.95 mol% or less, more preferably 0.75 mol% or less, and even more preferably 0.65 mol% or less, and is more preferably 0.55 mol% or less, 0.50 mol% or less, 0.40 mol% or less, 0.30 mol% or less, 0.20 mol% or less, 0.14 mol% or less, and 0.10 mol% or less, in that order.

[0043] The amount of DBG copolymerized in the DBG-copolymerized PBT can be determined by the method described in the Examples section below.

[0044] When an oligomer obtained by an esterification reaction between a diol component and a dicarboxylic acid component or an ester exchange reaction between a diol component and an ester-forming derivative of a dicarboxylic acid such as a dicarboxylic acid diester is polycondensed, a titanium compound and preferably a compound of a metal of Group 2A of the Periodic Table are usually used as a catalyst. These catalyst components may be used in the esterification reaction or transesterification reaction and then the polycondensation reaction may be carried out as is, or may not be used in the esterification reaction or transesterification reaction, or only the titanium catalyst may be used, and the remaining catalyst components may be added at the polycondensation stage. Furthermore, a part of the catalyst amount finally used in the esterification reaction or transesterification reaction may be used, and the remaining catalyst components may be added as appropriate as the polycondensation reaction proceeds. In any case, in the present invention, the finally obtained DBG copolymerized PBT inevitably contains titanium and preferably a metal of Group 2A of the periodic table, and the amount thereof will be described later. In the following, the titanium compound may be referred to as the titanium catalyst, and the compound of a metal of Group 2A of the periodic table may be referred to as the Group 2A metal catalyst.

[0045] Specific examples of titanium compounds include inorganic titanium compounds such as titanium oxide and titanium tetrachloride, titanium alcoholates such as tetramethyl titanate, tetraisopropyl titanate, and tetrabutyl titanate, and titanium phenolates such as tetraphenyl titanate, etc. These may be used alone or in combination of two or more. Of these, tetraalkyl titanates are preferred, and among these, tetrabutyl titanate is preferred.

[0046] The titanium content in the DBG copolymer PBT of the present invention is preferably 5 to 100 ppm as titanium atoms in terms of mass ratio relative to the DBG copolymer PBT. This amount is more preferably 10 ppm or more, even more preferably 20 ppm or more, and most preferably 25 ppm or more. This amount is also preferably 80 ppm or less, more preferably 60 ppm or less, even more preferably 50 ppm or less, and most preferably 40 ppm or less. If the titanium content is too high, the color tone, hydrolysis resistance, etc. deteriorate, whereas if the titanium content is too low, polymerization properties deteriorate.

[0047] Specific examples of the periodic table Group 2A metal compound in the present invention include various compounds of beryllium, magnesium, calcium, strontium, and barium, but from the viewpoints of ease of handling and availability, and catalytic effect, magnesium compounds and / or calcium compounds are preferred, and magnesium compounds with excellent catalytic effect are particularly preferred. Specific examples of magnesium compounds include magnesium acetate, magnesium hydroxide, magnesium carbonate, magnesium oxide, magnesium alkoxide, magnesium hydrogen phosphate, etc. Specific examples of calcium compounds include calcium acetate, calcium hydroxide, calcium carbonate, calcium oxide, calcium alkoxide, calcium hydrogen phosphate, etc. These periodic table Group 2A metal compounds may be used alone or in combination of two or more. Of these, magnesium acetate is preferred.

[0048] The content of the metal of Group 2A of the periodic table in the DBG copolymerized PBT of the present invention is not particularly limited, but is preferably 3 to 150 ppm in terms of the mass ratio of the metal atom of Group 2A of the periodic table to the PBT. This amount is more preferably 5 ppm or more, and even more preferably 10 ppm or more. This amount is more preferably 50 ppm or less, even more preferably 40 ppm or less, particularly preferably 30 ppm or less, and most preferably 15 ppm or less. If the content of the metal of Group 2A of the periodic table is too high, the color tone, hydrolysis resistance, etc. are deteriorated, and if it is too low, the polymerizability is deteriorated.

[0049] The molar ratio of titanium atoms to Group 2A metal atoms in the periodic table (Group 2A metal / titanium) contained in the DBG copolymer PBT of the present invention is usually 0.01 to 100, preferably 0.1 to 10, more preferably 0.3 to 3, and particularly preferably 0.3 to 1.5.

[0050] The content of metals such as titanium atoms in DBG copolymerized PBT can be measured using methods such as atomic emission, atomic absorption, and Inductively Coupled Plasma (ICP) after recovering the metals in the polymer using a method such as wet ashing.

[0051] In producing the DBG copolymer PBT of the present invention, in addition to the above-mentioned titanium compound and the compound of a metal of Group 2A of the periodic table, reaction aids such as antimony compounds such as antimony trioxide, germanium compounds such as germanium dioxide and germanium tetroxide, manganese compounds, zinc compounds, zirconium compounds, cobalt compounds, phosphorus compounds such as orthophosphoric acid, phosphorous acid, hypophosphorous acid, polyphosphoric acid, esters or metal salts thereof, sodium hydroxide, sodium benzoate, etc. may be used.

[0052] In addition to hydroxyl, carboxyl, and vinyl groups, methoxycarbonyl groups derived from the raw materials may remain at the ends of DBG copolymer PBT, and especially when dimethyl terephthalate is used as the raw material, a large amount of methoxycarbonyl groups may remain. These terminal methoxycarbonyl groups generate methanol and its oxides, formaldehyde and formic acid, due to heat during kneading and molding. As mentioned above, for use in electrical and electronic components, formic acid is not preferable because it may cause contact corrosion and damage metallic molding equipment and vacuum-related equipment. Therefore, the concentration of the terminal methoxycarbonyl groups in the DBG copolymer PBT of the present invention is preferably 0.5 equivalents / ton or less. The concentration of the terminal methoxycarbonyl groups is preferably 0.3 equivalents / ton or less, more preferably 0.2 equivalents / ton or less, and even more preferably 0.1 equivalents / ton or less. In order to make the terminal methoxycarbonyl groups below the upper limit, a dicarboxylic acid, preferably terephthalic acid, may be used as the dicarboxylic acid component.

[0053] The terminal carboxyl group concentration of the DBG copolymerized PBT of the present invention is usually 0.1 to 50 equivalents / ton, preferably 1 to 40 equivalents / ton, more preferably 5 to 30 equivalents / ton, and particularly preferably 10 to 25 equivalents / ton. If the terminal carboxyl group concentration is too high, the hydrolysis resistance may deteriorate. In order to make this value less than 0.1 equivalents / ton, for example, an extremely small production scale must be adopted, which is not realistic.

[0054] The terminal vinyl group concentration of the DBG copolymerized PBT of the present invention is usually 0.1 to 10 equivalents / ton, preferably 0.5 to 8 equivalents / ton, more preferably 1 to 5 equivalents / ton. If the terminal vinyl group concentration is too high, it will cause deterioration in color tone. Since the terminal vinyl group concentration tends to increase further due to the thermal history during molding, the deterioration in color tone becomes more noticeable when the molding temperature is high or when a manufacturing method having a recycling process is used.

[0055] The terminal methoxycarbonyl group concentration, terminal carboxyl group concentration, and terminal vinyl group concentration of the DBG copolymerized PBT can be determined by the method described in the Examples section below.

[0056] The intrinsic viscosity of the DBG copolymer PBT of the present invention is preferably 0.6 to 1.3 dL / g. If the intrinsic viscosity is less than 0.6 dL / g, the mechanical strength of the molded product will be insufficient, and if it exceeds 1.3 dL / g, the melt viscosity will be high, the fluidity will be deteriorated, and the moldability will tend to be deteriorated. The intrinsic viscosity of the DBG copolymer PBT of the present invention is more preferably 0.65 to 1.26 dL / g, and even more preferably 0.7 to 1.2 dL / g. The intrinsic viscosity of the DBG copolymerized PBT can be determined by the method described in the Examples section below.

[0057] The crystallization temperature of the DBG copolymer PBT of the present invention is usually 160 to 200°C, preferably 170 to 195°C, and more preferably 175 to 190°C. The crystallization temperature of the present invention is the temperature of an exothermic peak due to crystallization that appears when the resin is cooled from a molten state at a temperature drop rate of 20°C / min using a differential scanning calorimeter. The crystallization temperature of the present invention corresponds to the crystallization rate, and the higher the crystallization temperature of the crystallization, the faster the crystallization rate, so that the cooling time during injection molding can be shortened and the productivity can be increased. When the crystallization temperature of the crystallization is low, it takes a long time for crystallization during injection molding, and the cooling time after injection molding must be extended, which tends to extend the molding cycle and reduce productivity. The temperature-lowering crystallization temperature of the DBG copolymerized PBT of the present invention can be determined by the method described in the Examples section below.

[0058] The solution haze of the DBG copolymerized PBT of the present invention is not particularly limited, but is usually 10% or less, preferably 5% or less, more preferably 3% or less, and even more preferably 1% or less. When the solution haze is high, the amount of foreign matter tends to increase, significantly reducing the commercial value. The solution haze tends to increase when the titanium catalyst is largely deactivated. The solution haze of the DBG-copolymerized PBT can be determined by the method described in the Examples section below.

[0059] [Method of manufacturing DBG copolymer PBT] Next, the method for producing the DBG copolymer PBT of the present invention will be described. From the viewpoint of raw materials, the method for producing the DBG copolymer PBT of the present invention can be roughly divided into the so-called direct polymerization method using dicarboxylic acid as the main raw material and the transesterification method using dialkyl dicarboxylate as the main raw material. The difference is that the former mainly produces water in the initial esterification reaction, and the latter mainly produces alcohol in the initial transesterification reaction.

[0060] In addition, the manufacturing method of DBG copolymerized PBT is roughly classified into a batch method and a continuous method according to the raw material supply or polymer delivery form. There are methods in which the initial esterification reaction or ester exchange reaction is performed by continuous operation, and the subsequent polycondensation is performed by batch operation, and conversely, there are methods in which the initial esterification reaction or ester exchange reaction is performed by batch operation, and the subsequent polycondensation is performed by continuous operation.

[0061] In the present invention, from the viewpoints of stable availability of raw materials, ease of processing of distillate, high raw material unit consumption, and the improvement effect of the present invention, a continuous polymerization method using BDO as vapor for generating vacuum is preferred. Also, in the present invention, from the viewpoints of productivity and stability of product quality, and the improvement effect of the present invention, a so-called continuous method is preferred in which a method is adopted in which raw materials are continuously supplied and an esterification reaction or transesterification reaction is continuously carried out, and the polycondensation reaction following the esterification reaction or transesterification reaction is also continuously carried out.

[0062] In the present invention, a process is preferably employed in which terephthalic acid (or dialkyl terephthalate) and BDO are continuously esterified or transesterified in an esterification reaction tank or transesterification reaction tank, preferably in the presence of a titanium catalyst, while at least a portion of BDO is supplied to the esterification reaction tank or transesterification reaction tank independently of terephthalic acid (or dialkyl terephthalate). Hereinafter, the BDO supplied to the esterification reaction tank or transesterification reaction tank independently of terephthalic acid (or dialkyl terephthalate) may be referred to as "separately supplied BDO".

[0063] The above-mentioned "separately supplied BDO" can be fresh BDO unrelated to the process. In addition, "separately supplied BDO" can be obtained by collecting BDO distilled from the esterification reactor or transesterification reactor in a condenser or the like, and then supplying it as is or temporarily holding it in a tank or the like and refluxing it to the reactor, or by separating and purifying it to increase the purity. Hereinafter, the "separately supplied BDO" consisting of BDO collected in a condenser or the like may be referred to as "recirculated BDO" or "recycled BDO". From the viewpoints of effective resource utilization and simplicity of equipment, it is preferable to use "recirculated BDO (recycled BDO)" as "separately supplied BDO".

[0064] Furthermore, the BDO distilled from the esterification reaction tank or transesterification reaction tank usually contains, in addition to BDO, components such as water, alcohol, tetrahydrofuran, dihydrofuran, etc. Therefore, it is preferable that the distilled BDO is separated from the components such as water, alcohol, tetrahydrofuran, etc., after or while being collected in a condenser or the like, purified, and returned to the reaction tank.

[0065] In the present invention, in order to prevent the catalyst from being deactivated, it is preferable to directly supply 10% by mass or more of the titanium catalyst used in the esterification reaction or transesterification reaction to the reaction liquid phase section independently of terephthalic acid (or dialkyl terephthalate). Here, the reaction liquid phase section refers to the liquid phase side of the gas-liquid interface in the esterification reaction tank or transesterification reaction tank, and directly supplying to the reaction liquid phase section means that the titanium catalyst is directly supplied to the liquid phase section without passing through the gas phase section of the reactor using piping or the like. The proportion of the titanium catalyst added directly to the reaction liquid phase section is preferably 30% by mass or more, more preferably 50% by mass or more, even more preferably 80% by mass or more, and most preferably 90% by mass or more.

[0066] The titanium catalyst may be dissolved in a solvent or directly supplied to the liquid phase of the reaction liquid of the esterification reaction tank or the transesterification reaction tank. However, in order to stabilize the supply amount and reduce adverse effects such as denaturation due to heat from the heat medium jacket of the reactor, it is preferable to dilute the titanium catalyst with a solvent such as BDO. The titanium catalyst concentration in this case is usually 0.01 to 20 mass%, preferably 0.05 to 10 mass%, more preferably 0.08 to 8 mass% relative to the entire solution. In addition, from the viewpoint of reducing foreign matter, the water concentration in the solution is usually 0.05 to 1.0 mass%. In order to prevent deactivation and aggregation, the temperature during preparation of the catalyst solution is usually 20 to 150°C, preferably 30 to 100°C, more preferably 40 to 80°C. In addition, in order to prevent deterioration, precipitation, and deactivation, the catalyst solution is preferably mixed with separately supplied BDO through a pipe or the like and then supplied to the esterification reaction tank or the transesterification reaction tank.

[0067] The Group 2A metal catalyst may also be supplied to the esterification reaction tank or the transesterification reaction tank. There is no particular restriction on the supply position of the Group 2A metal catalyst, and it may be supplied from the gas phase of the reaction liquid to the top surface of the reaction liquid in these reaction tanks, or it may be supplied directly to the liquid phase of the reaction liquid. In this case, it may be supplied together with terephthalic acid and the titanium compound, or it may be supplied independently, but from the viewpoint of catalyst stability, it is preferable to supply it from the gas phase of the reaction liquid to the top surface of the reaction liquid, independently of terephthalic acid and the titanium compound.

[0068] The Group 2A metal catalyst is usually a solid and can be supplied as is, but it is preferable to dilute it with a solvent such as BDO before supplying it in order to stabilize the supply amount and reduce adverse effects such as thermal denaturation. The concentration of the Group 2A metal catalyst in the entire solution is usually 0.01 to 20 mass%, preferably 0.05 to 10 mass%, and more preferably 0.08 to 8 mass%. A small amount of water may be added to this solution for the purpose of preventing precipitation, improving thermal stability, etc.

[0069] On the other hand, the Group 2A metal catalyst can also be added to the oligomer piping leading to the polycondensation reaction tank following the esterification reaction tank or the transesterification reaction tank, or to the polycondensation reaction tank. In this case, it is preferable to dilute the Group 2A metal catalyst with a solvent such as BDO in order to stabilize the supply amount and reduce adverse effects such as denaturation due to heat. The concentration of the Group 2A metal catalyst in this case is usually 0.01 to 20 mass%, preferably 0.05 to 10 mass%, and more preferably 0.08 to 8 mass% relative to the entire solution. A small amount of water may be added to this solution for the purpose of preventing precipitation, improving thermal stability, etc.

[0070] An example of a continuous esterification process employing a direct polymerization method is as follows. That is, the dicarboxylic acid component mainly composed of terephthalic acid and the diol component mainly composed of BDO are mixed in a raw material mixing tank to form a slurry, and the esterification reaction is carried out in one or more esterification reaction tanks, preferably in the presence of a titanium catalyst and a Group 2A metal catalyst, while controlling the generation of DBG. The reaction temperature is preferably 230°C or less, more preferably 228°C or less, even more preferably 227°C or less, and most preferably 226°C or less. The lower limit of the reaction temperature is not particularly limited, but is preferably 210°C, more preferably 215°C. The pressure is usually 10 to 133 kPa, preferably 13 to 101 kPa, and more preferably 60 to 90 kPa (absolute pressure, the same applies below). The residence time is preferably 3.6 hours or less, more preferably 3.1 hours or less, even more preferably 2.6 hours or less, and most preferably 2.5 hours or less. The lower limit of the residence time is not particularly limited, but is preferably 1 hour.

[0071] In the case of the direct polymerization method, it is preferable that the molar ratio of terephthalic acid to BDO satisfies the following formula (1). BM / TM=1.1-4.0 (mol / mol) …(1) (where BM is the number of moles of BDO supplied from the outside to the esterification reactor per unit time, and TM is the number of moles of terephthalic acid supplied from the outside to the esterification reactor per unit time)

[0072] The above-mentioned "BDO supplied from outside to the esterification reaction tank" refers to the total amount of BDO that enters the reaction tank from outside the reaction tank, such as BDO supplied together with terephthalic acid as a raw material slurry or solution, BDO supplied independently of these (separately supplied BDO), and BDO used as a catalyst solvent.

[0073] In order to adjust the amount of DBG copolymerized in the resulting DBG-copolymerized PBT to fall within the range specified by the present invention, it is effective to adjust the BM / TM ratio. If the BM / TM value is less than 1.1, the conversion rate decreases and the catalyst is deactivated, and if it is more than 4.0, not only the thermal efficiency decreases but also the amount of by-products such as tetrahydrofuran and DBG tends to increase. The BM / TM value is preferably 1.5 to 3.9, more preferably 2.5 to 3.8, and further preferably 3.1 to 3.5.

[0074] In the present invention, it is necessary to control the amount of DBG in the BDO to be fed in order to make the amount of DBG copolymerized in the resulting DBG-copolymerized PBT 1.0 mol % or less. For this purpose, it is preferable to set the temperature of the steam generation tank of the ejector to 256° C. or less, preferably 251° C. or less, more preferably 246° C. or less, and even more preferably 242° C. or less, rather than the commonly used temperature exceeding 256° C. The present inventors were the first to discover that there is a relationship between the temperature of the steam generation tank and the generation of DBG, and that keeping this temperature at 256°C or less is extremely effective in suppressing the generation of DBG. Even when the temperature is 242° C. or lower, if the average residence time of BDO in the steam generation tank is long, the amount of DBG produced may increase beyond the range specified in the present invention (the ratio of units derived from dibutylene glycol to units derived from dicarboxylic acid components is 0.05 to 1.0 mol%). Therefore, in order to control the amount of DBG produced, it is preferable to set the residence time as follows. The average residence time of the BDO in the steam generation vessel is preferably 5 hours or less, more preferably 4 hours or less, even more preferably 3 hours or less, and most preferably 2 hours or less. The BDO used in the steam generation tank is used in the production of DBG copolymerized PBT, and the amount thereof is preferably 50% or more by mass of the total BDO used in the production, more preferably 60% or more, even more preferably 70% or more, particularly preferably 90% or more, and most preferably 100%. In addition, since DBG has a higher boiling point than BDO, it is likely to accumulate in the liquid phase of the steam generation tank. In order to produce DBG copolymer PBT with stable quality, it is preferable to use both the liquid phase composition and the vapor phase composition of the steam generation tank continuously as production raw materials.

[0075] An example of a continuous process employing the transesterification method is as follows. That is, in one or more transesterification reaction tanks, a continuous transesterification reaction is carried out in the presence of a titanium catalyst and a Group 2A metal catalyst at a temperature of usually 110 to 260°C, preferably 140 to 245°C, and more preferably 180 to 220°C and under a pressure of usually 10 to 133 kPa, preferably 13 to 120 kPa, and more preferably 60 to 101 kPa, for usually 0.5 to 5 hours, and preferably 1 to 3 hours. In the case of the transesterification method, it is preferable that the molar ratio of dialkyl terephthalate such as methyl terephthalate to BDO satisfies the following formula (2).

[0076] BM / DM=1.1 to 2.5 (mol / mol) … (2) (where BM is the number of moles of BDO supplied from the outside to the transesterification reactor per unit time, and DM is the number of moles of dialkyl terephthalate supplied from the outside to the transesterification reactor per unit time)

[0077] If the BM / DM value is less than 1.1, the conversion rate and catalytic activity will decrease, and if it is more than 2.5, not only will the thermal efficiency decrease, but the amount of by-products such as tetrahydrofuran will tend to increase. The BM / DM value is preferably 1.1 to 1.8, more preferably 1.2 to 1.5.

[0078] The esterification reaction tank or transesterification reaction tank may be any of the known types, such as a vertical agitated complete mixing tank, a vertical thermal convection mixing tank, or a tower-type continuous reaction tank, and may be a single tank or a plurality of tanks of the same or different types connected in series or parallel. Of these, a reaction tank having an agitator is preferred, and as the agitator, in addition to a normal type consisting of a power unit, bearings, a shaft, and an agitator blade, a high-speed rotating type such as a turbine stator type high-speed rotating agitator, a disk mill type agitator, or a rotor mill type agitator may be used.

[0079] The form of stirring is not particularly limited, and in addition to a typical stirring method in which the reaction liquid in the reaction tank is directly stirred from the top, bottom, side, etc. of the reaction tank, a method in which a part of the reaction liquid is taken out of the reactor through piping or the like and stirred with a line mixer or the like to circulate the reaction liquid can also be used.

[0080] The type of stirring blade can be selected from known types, and specific examples include propeller blades, screw blades, turbine blades, fan turbine blades, disk turbine blades, Pfaudler blades, full zone blades, and max blend blades.

[0081] The oligomer obtained as a reaction product of such an esterification reaction or transesterification reaction is transferred to a polycondensation reaction tank. The number average molecular weight of the oligomer at this time is usually 300 to 3,000, and preferably 500 to 1,500.

[0082] In the production of DBG copolymerized PBT, usually, multiple stages, preferably 2 to 5 stages, particularly preferably 2 to 3 stages of polycondensation reaction tanks with different reaction conditions are used to sequentially increase the molecular weight. The form of the polycondensation reaction tank may be any type such as a vertical agitation complete mixing tank, a vertical thermal convection type mixing tank, or a tower type continuous reaction tank, or these may be combined. Among them, at least one of the polycondensation reaction tanks is preferably a type having an agitator, and as the agitator, in addition to a normal type consisting of a power unit, bearings, a shaft, and an agitator blade, a high-speed rotating type such as a turbine stator type high-speed rotating agitator, a disk mill type agitator, or a rotor mill type agitator may be used.

[0083] The form of stirring is not particularly limited, and in addition to the usual stirring method of directly stirring the reaction liquid in the reaction tank from the top, bottom, side, etc. of the reaction tank, a method of circulating the reaction liquid by taking a part of the reaction liquid outside the reactor through piping, etc. and stirring it with a line mixer, etc., can be adopted. Among these, it is recommended that at least one of the polycondensation reaction tanks be a horizontal reactor with a horizontal rotation axis that has excellent surface renewal and self-cleaning properties.

[0084] The polycondensation reaction is carried out in the presence of a catalyst at a temperature of usually 210 to 280°C, preferably 220 to 250°C, more preferably 230 to 245°C, and particularly preferably 230 to 240°C in at least one reaction tank, preferably with stirring, for usually 1 to 12 hours, preferably 3 to 10 hours, under reduced pressure of usually 27 kPa or less, preferably 20 kPa or less, and particularly preferably 13 kPa or less. The reaction may be performed by a batch method or a continuous method, but from the viewpoint of the stability of the polymer quality and the reduction of terminal carboxyl groups, the continuous method is preferred. In addition, in order to suppress coloration and deterioration and to suppress the increase of terminal groups such as vinyl groups, it is preferable to carry out the reaction in at least one reaction tank under high vacuum of usually 1.3 kPa or less, preferably 0.5 kPa or less, and more preferably 0.3 kPa or less.

[0085] The polymer obtained by the polycondensation reaction is usually transferred from the bottom of the polycondensation reaction tank to a polymer discharge die and discharged in the form of a strand. The strand is then cut with a cutter while being cooled with water or after being cooled with water, and made into granular materials such as pellets or chips.

[0086] The DBG copolymerized PBT of the present invention can be made into a polymer of even higher quality by installing a filter in the flow path of the polymer precursor or the polymer.

[0087] If the filter is installed too far upstream in the manufacturing process, foreign matter generated downstream cannot be removed, and the pressure loss of the filter increases in areas with high viscosity downstream, and in order to maintain the flow rate, it is necessary to enlarge the filter openings or to oversize the filter filtration area and piping equipment, and since the fluid is subjected to high shear when passing through, deterioration of the DBG copolymerized PBT due to shear heat is inevitable. Therefore, the filter is installed at a position where the intrinsic viscosity of the DBG copolymerized PBT or its precursor is usually 0.1 to 0.9 dL / g.

[0088] The filter material constituting the filter may be any of metal winding, laminated metal mesh, metal nonwoven fabric, porous metal plate, etc., but from the viewpoint of filtration accuracy, laminated metal mesh or metal nonwoven fabric is preferred, and in particular, the mesh size is fixed by sintering. The shape of the filter may be any type such as basket type, disk type, leaf disk type, tube type, flat cylindrical type, pleated cylindrical type, etc. In addition, in order not to affect the operation of the plant, it is preferable to install multiple filters and make them switchable or to install an auto screen changer.

[0089] The absolute filtration accuracy of the filter is not particularly limited, but is usually 0.5 to 200 μm, preferably 1 to 100 μm, more preferably 5 to 50 μm, and particularly preferably 10 to 30 μm. If the absolute filtration accuracy is too high, the effect of reducing foreign matter in the product is lost, and if it is too low, it leads to reduced productivity and increased frequency of filter replacement. Here, the absolute filtration accuracy refers to the minimum particle size that is completely filtered out and removed when a filtration test is performed using standard particle size products such as glass beads with known and uniform particle size.

[0090] A preferred embodiment of the method for producing DBG copolymerized PBT of the present invention will be described below with reference to the accompanying drawings. Fig. 1 is an explanatory diagram of an example of the esterification or transesterification reaction process used in the present invention, Figs. 2 and 3 are explanatory diagrams of an example of the polycondensation process used in the present invention, and Fig. 4 is an explanatory diagram of an example of the vacuum generation equipment process used in the present invention.

[0091] In FIG. 1, the raw material terephthalic acid is usually mixed with BDO in a raw material mixing tank (not shown) and supplied to the reaction tank (A) in the form of a slurry or liquid from the raw material supply line (1). On the other hand, when the raw material is dialkyl terephthalate, it is usually supplied to the reaction tank (A) as a molten liquid independently of BDO. In addition, the titanium catalyst is preferably prepared as a BDO solution in a catalyst preparation tank (not shown) and then supplied from the titanium catalyst supply line (3). FIG. 1 shows an embodiment in which the catalyst supply line (3) is connected to the recycle line (2) for recycled BDO, and the two are mixed and then supplied to the liquid phase part of the reaction tank (A). In addition, the Group 2A metal catalyst is preferably prepared as a BDO solution in a catalyst preparation tank (not shown) and then supplied from the Group 2A metal catalyst supply line (15).

[0092] The gas distilled from the reaction tank (A) passes through the distillation line (5) and is separated into high-boiling components and low-boiling components in the rectification tower (C). Usually, the main component of the high-boiling components is BDO, and the main components of the low-boiling components are water and tetrahydrofuran in the case of the direct polymerization method, and alcohol, tetrahydrofuran, and water in the case of the transesterification method.

[0093] The high boiling components separated in the rectification tower (C) are withdrawn through the withdrawal line (6) and pump (D), some of which are circulated through the recirculation line (2) to the reaction tank (A), and some of which are returned through the circulation line (7) to the rectification tower (C). The surplus is withdrawn through the withdrawal line (8) to the outside. On the other hand, the low boiling components separated in the rectification tower (C) are withdrawn through the gas withdrawal line (9), condensed in the condenser (G), and temporarily stored in the tank (F) through the condensate line (10). A part of the low boiling components collected in the tank (F) is returned to the rectification tower (C) through the withdrawal line (11), pump (E) and circulation line (12), and the remainder is withdrawn through the withdrawal line (13) to the outside. The condenser (G) is connected to an exhaust device (not shown) through a vent line (14). The oligomers produced in the reaction vessel (A) are withdrawn via the withdrawal pump (B) and the withdrawal line (4).

[0094] In the process shown in Fig. 1, the catalyst supply line (3) is connected to the recirculation line (2), but the two may be independent. Also, the raw material supply line (1) may be connected to the liquid phase part of the reaction vessel (A).

[0095] In FIG. 2, the oligomer supplied from the discharge line (4) shown in FIG. 1 is polycondensed under reduced pressure in the first polycondensation reaction tank (a) to form a prepolymer, and then supplied to the second polycondensation reaction tank (d) through the discharge gear pump (c) and the discharge line (L1). In the second polycondensation reaction tank (d), polycondensation usually proceeds further at a pressure lower than that in the first polycondensation reaction tank (a) to form a polymer. The resulting polymer passes through the discharge gear pump (e) and the discharge line (L3) and the filter (f), and is discharged from the die head (g) in the form of a molten strand, and is cooled with water or the like, and then cut by a rotary cutter (h) to form pellets. The symbol (L2) is the vent line of the first polycondensation reaction tank (a), and the symbol (L4) is the vent line of the second polycondensation reaction tank (d).

[0096] The process shown in FIG. 3 is different from the process shown in FIG. 2 in that a third polycondensation reaction tank (k) is provided after the second polycondensation reaction tank (d). The third polycondensation reaction tank (k) is a horizontal reaction tank consisting of a plurality of stirring blade blocks and equipped with a two-shaft self-cleaning type stirring blade. The polymer introduced from the second polycondensation reaction tank (d) to the third polycondensation reaction tank (k) through the discharge line (L3) is further polycondensed here, and then passes through the discharge gear pump (m) and the discharge line (L5) and the filter (f), and is discharged from the die head (g) in the form of a molten strand, and is cooled with water or the like, and then cut by a rotary cutter (h) to become pellets. The symbol (L6) is the vent line of the third polycondensation reaction tank (k).

[0097] The vacuum required for each reaction step was obtained using the BDO vapor ejector shown in Figure 4. Specifically, the BDO inlet line (16) was continuously supplied to the BDO evaporator (I) and operated at a specified temperature, pressure, and residence time. This process produces tetrahydrofuran, water, DBG, etc. from BDO. This BDO vapor was continuously supplied to the ejector facility (J) via a vapor line (19). At the same time, BDO containing DBG (BDO composition) was continuously supplied to the recycled BDO tank (M) via a liquid phase line (18) by pump P1.

[0098] The reaction tank (A), the first polycondensation reaction tank (a), the second polycondensation reaction tank (d), and the third polycondensation reaction tank (k) were vacuumed by the ejector equipment (J) and the BDO vapor used in the ejector equipment (J) was condensed by the barocon equipment (K) and continuously recovered in the barocon tank (L) via the barocon line (22), and further continuously transferred to the recycled BDO tank (M) by the pump P2 via the barocon tank line (23). The recycled BDO is extracted by the pump P3 via the recycled BDO line (24) and used for preparing a slurry with terephthalic acid in the raw material slurry tank (N). The raw material slurry prepared in the raw material slurry tank (N) is fed to the reaction tank (O) via the raw material slurry line (25) by the pump P4.

[0099] [Additives / Additional ingredients] To the DBG copolymer PBT of the present invention, antioxidants such as phenol compounds such as 2,6-di-t-butyl-4-octylphenol and pentaerythrityl-tetrakis[3-(3',5'-t-butyl-4'-hydroxyphenyl)propionate], thioether compounds such as dilauryl-3,3'-thiodipropionate and pentaerythrityl-tetrakis(3-laurylthiodipropionate), phosphorus compounds such as triphenyl phosphite, tris(nonylphenyl)phosphite and tris(2,4-di-t-butylphenyl)phosphite, release agents such as paraffin wax, microcrystalline wax, polyethylene wax, long-chain fatty acids and their esters represented by montanic acid and montanic acid esters, and silicone oil may be added.

[0100] The DBG copolymer PBT of the present invention can be blended with a reinforcing filler. The reinforcing filler is not particularly limited, but examples thereof include inorganic fibers such as glass fiber, carbon fiber, silica-alumina fiber, zirconia fiber, boron fiber, boron nitride fiber, potassium silicon nitride titanate fiber, and metal fiber, and organic fibers such as aromatic polyamide fiber and fluororesin fiber. These reinforcing fillers can be used in combination of two or more. Among the above reinforcing fillers, inorganic fillers, especially glass fiber, are preferably used.

[0101] When the reinforcing filler is an inorganic fiber or an organic fiber, the average fiber diameter is not particularly limited, but is usually 1 to 100 μm, preferably 2 to 50 μm, more preferably 3 to 30 μm, and particularly preferably 5 to 20 μm, and the average fiber length is not particularly limited, but is usually 0.1 to 20 mm, and preferably 0.1 to 10 mm.

[0102] In order to improve the interface adhesion with the DBG copolymer PBT, the reinforcing filler is preferably surface-treated with a sizing agent or a surface treatment agent before use. Examples of the sizing agent or surface treatment agent include functional compounds such as epoxy compounds, acrylic compounds, isocyanate compounds, silane compounds, and titanate compounds. The reinforcing filler can be surface-treated in advance with a sizing agent or a surface treatment agent, or can be surface-treated by adding a sizing agent or a surface treatment agent during preparation of the DBG copolymer PBT composition. The amount of the reinforcing filler added is usually 150 parts by mass or less, preferably 5 to 100 parts by mass, based on 100 parts by mass of the DBG copolymer PBT.

[0103] The DBG copolymer PBT of the present invention can be blended with other fillers together with the reinforcing filler. Examples of the other fillers to be blended include plate-like inorganic fillers, ceramic beads, asbestos, wollastonite, talc, clay, mica, zeolite, kaolin, potassium titanate, barium sulfate, titanium oxide, silicon oxide, aluminum oxide, magnesium hydroxide, etc. By blending the plate-like inorganic fillers, the anisotropy and warpage of the resulting molded product can be reduced. Examples of the plate-like inorganic fillers include glass flakes, mica, and metal foils. Among these, glass flakes are preferably used.

[0104] A flame retardant can be blended in the DBG copolymer PBT of the present invention to impart flame retardancy. The flame retardant is not particularly limited, and examples thereof include organic halogen compounds, antimony compounds, phosphorus compounds, other organic flame retardants, and inorganic flame retardants. Examples of organic halogen compounds include brominated polycarbonate, brominated epoxy resin, brominated phenoxy resin, brominated polyphenylene ether resin, brominated polystyrene resin, brominated bisphenol A, and polypentabromobenzyl acrylate. Examples of antimony compounds include antimony trioxide, antimony pentoxide, and sodium antimonate. Examples of phosphorus compounds include phosphate esters, polyphosphoric acid, ammonium polyphosphate, red phosphorus, and metal phosphinate. Examples of other organic flame retardants include nitrogen compounds such as melamine and cyanuric acid. Examples of other inorganic flame retardants include aluminum hydroxide, magnesium hydroxide, silicon compounds, and boron compounds.

[0105] The DBG copolymer PBT of the present invention may contain other conventional additives as necessary. Such additives are not particularly limited, and examples thereof include stabilizers such as antioxidants and heat stabilizers, as well as lubricants, release agents, catalyst deactivators, crystal nucleating agents, and crystallization promoters. These additives may be added during or after polymerization. Furthermore, in order to impart desired performance to the DBG copolymer PBT, stabilizers such as ultraviolet absorbers and weathering stabilizers, colorants such as dyes and pigments, antistatic agents, foaming agents, plasticizers, impact modifiers, and the like may be added.

[0106] The DBG copolymer PBT of the present invention can be blended with thermoplastic resins such as polyethylene, polypropylene, polystyrene, polyacrylonitrile, polymethacrylic acid ester, ABS resin, polycarbonate, polyamide, polyphenylene sulfide, polyethylene terephthalate, liquid crystal polyester, polyacetal, polyphenylene oxide, etc., and thermosetting resins such as phenol resin, melamine resin, silicone resin, epoxy resin, etc. These thermoplastic resins and thermosetting resins can also be used in combination of two or more kinds.

[0107] The method of blending the various additives and additional components such as resins is not particularly limited, but a method of melt-kneading using a single-screw or twin-screw extruder having a vent port for volatilization is preferred. Each component, including the additional components, can be fed to the kneader all at once, or can be fed sequentially. Also, two or more components selected from each component, including the additional components, can be mixed in advance.

[0108] When the DBG copolymerized PBT of the present invention is used as at least a part of the raw material and melt-kneaded by an extruder as described above to produce the compound product of the present invention, it is preferable that the kneading resin temperature in the extruder is 320°C or less. If the kneading resin temperature is 320°C or less, thermal decomposition tends to be suppressed. From this viewpoint, the kneading resin temperature in the extruder is more preferably 310°C or less, and even more preferably 300°C or less. On the other hand, from the viewpoint of ensuring uniform melting, the kneading resin temperature in the extruder is preferably 240°C or more, particularly 250°C or more.

[0109] [Forming method] The molding method of the DBG copolymer PBT of the present invention and the compound product of the present invention containing the DBG copolymer PBT of the present invention is not particularly limited, and molding methods generally used for thermoplastic resins, i.e., injection molding, blow molding, extrusion molding, press molding, etc., can be applied. Among these, when used for automobile parts and electric / electronic parts, it is preferable to use an injection molding machine. The molten resin temperature during injection molding is preferably 280° C. or lower. If the molten resin temperature is 280° C. or lower, it is preferable in that thermal decomposition is suppressed. From this viewpoint, the molten resin temperature during injection molding is more preferably 275° C. or lower, and further preferably 270° C. or lower. On the other hand, from the viewpoint of ensuring uniform melting, the molten resin temperature during injection molding is preferably 240° C. or higher, particularly preferably 250° C. or higher.

[0110] In addition, when molding the DBG copolymer PBT of the present invention or the compound product of the present invention, recycled raw materials may be used as at least a part of the molding material, and the use of recycled raw materials can reduce raw material costs. Even in this case, if the ratio of recycled raw materials used is 30% or less, the decrease in physical properties is within an acceptable range, which is preferable.

[0111] The DBG copolymerized PBT of the present invention has excellent color tone, hydrolysis resistance, thermal stability, and moldability, and is particularly less susceptible to color change when dried under air or by heating. For this reason, it is suitable for injection-molded parts such as electric and electronic parts and automotive parts. EXAMPLES

[0112] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following examples without departing from the gist of the present invention. The methods for measuring physical properties and evaluation items used in the following examples are as follows.

[0113] (1) Esterification rate The acid value was calculated from the acid value and saponification value using the following formula. The acid value was determined by dissolving the oligomer in dimethylformamide and titrating it with a 0.1N KOH / methanol solution. The saponification value was determined by hydrolyzing the oligomer with a 0.5N KOH / ethanol solution and titrating it with 0.5N hydrochloric acid. Esterification rate (%) = ((saponification value - acid value) / saponification value) x 100

[0114] (2) Transesterification rate Approximately 100 mg of oligomer was dissolved in 1 mL of a mixed solvent of deuterated chloroform / hexafluoroisopropanol = 7 / 3 (volume ratio), 36 μL of deuterated pyridine was added, and the mixture was heated at 50 °C. 1 H-NMR was measured to determine the amount of terminal methoxycarbonyl groups (equivalents / ton). The NMR device used was an "α-400" or "AL-400" manufactured by JEOL Ltd. The transesterification rate was calculated using the following formula. Ester exchange rate (%) = 100 - (amount of terminal methoxycarbonyl groups / 9081) x 100

[0115] (2) Terminal carboxyl group concentration The content was determined by dissolving 0.5 g of DBG copolymerized PBT or oligomer in 25 mL of benzyl alcohol and titrating with a 0.01 mol / L benzyl alcohol solution of sodium hydroxide.

[0116] (3) Intrinsic viscosity (IV) The viscosity was calculated using an Ubbelohde viscometer as follows: A mixed solvent of phenol / tetrachloroethane (mass ratio 1 / 1) was used, and the number of seconds it took for a polymer solution with a concentration of 1.0 g / dL and the solvent alone to fall at 30° C. was measured, and the viscosity was calculated using the following formula. IV=((1+4K H η sp ) 0.5 -1) / (2K H C) (However, η sp = η0-1, where η is the number of seconds the polymer solution falls, η0 is the number of seconds the solvent falls, C is the polymer solution concentration (g / dL), and K H is Huggins' constant, which we used as 0.33.)

[0117] (4) Concentration of titanium and Group 2A metals in DBG copolymerized PBT DBG copolymerized PBT was wet decomposed with high-purity sulfuric acid and nitric acid for the electronics industry, and the content of each component was measured using a high-resolution ICP (Inductively Coupled Plasma)-MS (Mass Spectrometer) (manufactured by Thermoquest).

[0118] (5) Amount of DBG copolymerized, terminal methoxycarbonyl group concentration, terminal vinyl group concentration Approximately 100 mg of DBG copolymerized PBT was dissolved in 1 mL of a mixed solvent of deuterated chloroform / hexafluoroisopropanol = 7 / 3 (volume ratio), 36 μL of deuterated pyridine was added, and the mixture was heated at 50 °C. 1 The results were obtained by measuring H-NMR. The NMR device used was an "α-400" or "AL-400" manufactured by JEOL Ltd. The amount of DBG copolymerization was calculated as mol % / total carboxylic acid (shown as "mol %" in the table), and the terminal methoxycarbonyl group concentration and terminal vinyl group concentration were calculated as equivalents / ton.

[0119] (6) Melting point (Tm)・Crystallization temperature after cooling down Using a PerkinElmer differential scanning calorimeter "Model DSC7", the temperature was raised from room temperature to 300°C at a heating rate of 20°C / min, then cooled to 80°C at a cooling rate of 20°C / min, and the endothermic peak temperature was taken as the melting point, and the exothermic peak temperature was taken as the cooling crystallization temperature. The higher the cooling crystallization temperature, the faster the crystallization speed and the shorter the molding cycle.

[0120] (7) Solution Haze 2.70 g of DBG copolymerized PBT was dissolved in 20 mL of a mixed solvent of phenol / tetrachloroethane = 3 / 2 (mass ratio) at 110 ° C for 30 minutes, then cooled in a thermostatic water bath at 30 ° C for 15 minutes, and measured with a turbidity meter "NDH-300A" manufactured by Nippon Denshoku Co., Ltd. with a cell length of 10 mm. The lower the value, the better the transparency.

[0121] (10) Pellet color 30 g of DBG copolymerized PBT pellets were placed in a 50 mm diameter aluminum dish and heated in an Espec Corporation thermostatic gear oven with a rotating frame at 140°C for 8 hours under normal air pressure. The color tone b value was measured before and after heating. A Nippon Denshoku Corporation color difference meter "Z-300A" was used for the measurement, and evaluation was performed using the b value in the L, a, b color system. The lower the value, the less yellowing and the better the color tone.

[0122] (11) Formaldehyde emissions 1 g of DBG copolymerized PBT and 5 mL of hydrochloric acid solution adjusted to pH = 2.29 were placed in a 10 mL headspace bottle and stirred and extracted at 120 ° C for 1 hour. After cooling the liquid, it was filtered with a chromatographic disk. Furthermore, about 3 g of this liquid was precisely weighed, and 0.2 mL of 0.25% 2,4-dinitrophenylhydrazine-6N hydrochloric acid solution and 1 mL of hexane were added, and reacted at 50 ° C for 20 minutes, and the hexane phase was analyzed by gas chromatography (Shimadzu Corporation "GC2010", column: "HP-5MS").

[0123] (12) Flexural modulus The DBG copolymerized PBT pellets were dried for 8 hours in a tray dryer at 140°C, and then molded into ISO test pieces at a cylinder temperature of 250°C and a mold temperature of 80°C using an injection molding machine (model S-75MIII) manufactured by Sumitomo Heavy Industries, Ltd., and the flexural modulus was measured according to ISO 178. The measurement was performed five times, and the average value of the five measurements was used.

[0124] [Example 1] DBG copolymerized PBT was produced through the esterification process shown in FIG. 1 and the polycondensation process shown in FIG. 2 as follows. First, a 60°C slurry containing 1.80 moles of BDO mixed with 1.00 moles of terephthalic acid was continuously fed from a slurry preparation tank through a raw material feed line (1) to a reaction tank (A) for esterification having a screw-type agitator filled with a PBT oligomer having an esterification rate of 99% in advance, at a rate of 41.0 parts by mass / h. At the same time, a bottom component (98% by mass or more of BDO) from a 185°C rectification tower (C) was fed from a recirculation line (2) at a rate of 15.8 parts by mass / h, and a 3.0% by mass BDO solution of tetrabutyl titanate at 65°C was fed as a catalyst from a titanium catalyst feed line (3) at a rate of 0.26 parts by mass / h (tetrabutyl titanate was 40 ppm by weight as titanium element relative to the theoretical polymer yield). The water content in this catalyst solution was 0.2% by mass.

[0125] The internal temperature of the reaction tank (A) was 226° C., and the pressure was 60 kPa. The produced water, tetrahydrofuran, and excess BDO were distilled through the distillation line (5) and separated into high-boiling components and low-boiling components in the fractionator (C). After the system had stabilized, 98% by mass or more of the high boiling components in the bottom of the column were BDO. A portion of the high boiling components was withdrawn to the outside through withdrawal line (8) so that the liquid level in the distillation column (C) was kept constant. On the other hand, the low boiling components were withdrawn in the form of gas from the top of the column, condensed in a condenser (G), and withdrawn to the outside through a withdrawal line (13) so that the liquid level in the tank (F) was kept constant.

[0126] A certain amount of oligomers produced in the reactor (A) was withdrawn from the withdrawal line (4) using the pump (B), and the liquid level was controlled so that the average residence time of the liquid in the reactor (A) was 3.0 hours. After the system was stabilized, the esterification rate of the oligomers collected at the outlet of the reactor (A) was 96.5%. A 6.0 mass% solution of magnesium acetate tetrahydrate in BDO at 65°C was supplied as a catalyst from the Group 2A metal catalyst supply line (15) at a rate of 0.04 mass parts / h to the oligomer withdrawn from the withdrawal line 4 (magnesium acetate was 10 mass ppm as magnesium element relative to the theoretical polymer yield). The water content in this catalyst solution was 10.0 mass%.

[0127] The oligomer withdrawn from the withdrawal line (4) was continuously supplied to the first polycondensation reaction tank (a). The internal temperature of the first polycondensation reaction tank (a) was set to 230°C, the pressure to 3.9 kPa, and the liquid level was controlled so that the residence time was 120 minutes. An initial polycondensation reaction was carried out while withdrawing water, tetrahydrofuran, and BDO from a vent line (L2) connected to a pressure reducer (not shown). The withdrawn reaction liquid was continuously supplied to the second polycondensation reaction tank (d). The internal temperature of the second polycondensation reaction tank (d) was set to 240°C, the pressure to 130 Pa, and the liquid level was controlled so that the residence time was 80 minutes. The polycondensation reaction was further carried out while extracting water, tetrahydrofuran, and BDO from a vent line (L4) connected to a pressure reducer (not shown). The obtained polymer was passed through a discharge line (L3) by a discharge gear pump (e) and a filter (f), and was continuously discharged in the form of strands from a die head (g) and cut by a rotary cutter (h).

[0128] The vacuum required for each reaction step was obtained using a BDO vapor ejector as described below. BDO was continuously supplied to the BDO evaporator (I) from the BDO inlet line (16) at 14.9 parts by mass / hr, and the evaporator was operated at an internal temperature of 241° C., a pressure of 50 KPa, and a residence time of 1.47 hours. This treatment produces tetrahydrofuran, water, DBG, etc. from BDO. This BDO vapor containing DBG was continuously supplied to the ejector facility (J) at a rate of 14.5 parts by mass / hr using a vapor line (19). At the same time, BDO containing DBG was continuously supplied to the recycle BDO tank (M) at a rate of 0.4 parts by mass / hr using a liquid phase line (18). A vacuum was obtained in the ester reaction tank (A), the first polycondensation reaction tank (a), and the second polycondensation reaction tank (d) using the ejector equipment (J). The vapor from each of the reaction tanks and the BDO vapor used in the ejector equipment (J) were condensed in the barocon equipment (K) and continuously recovered in the barocon tank (4) via the barocon line (22), and continuously transferred to the recycled BDO tank (M) via the barocon tank line (23). Recycled BDO was used for slurry preparation with terephthalic acid.

[0129] The amount of DBG copolymerized in DBG-copolymerized PBT can be controlled by adjusting the temperature and residence time of the vacuum steam generation tank, where BDO exists at high concentrations, and the temperature and residence time of the esterification reaction.

[0130] The intrinsic viscosity (IV) of the resulting polymer was 0.85 dL / g, the concentration of terminal carboxyl groups was 13 equivalents / ton, and the concentration of terminal methoxycarbonyl groups was less than 0.1 equivalents / ton. The obtained polymer was used for the above-mentioned evaluation. The color tone b value of the obtained polymer pellets (major axis about 3 mm, minor axis about 2 mm, length about 4 mm) was measured before and after heating. The evaluation results are shown in Table 1.

[0131] [Examples 2 to 10] DBG copolymerized PBT was obtained in the same manner as in Example 1, except that the esterification conditions, steam generation tank conditions, and titanium and magnesium addition amounts were changed to those shown in Table 1. The physical properties and evaluation results of the obtained DBG copolymerized PBT are shown in Table 1.

[0132] As shown in Table 1, the DBG copolymerized PBTs of Examples 1 to 10, which satisfy the requirements of the present invention, showed little increase in b value (yellowing) even when dried in air at 140°C for 8 hours, and were DBG copolymerized PBTs suitable for molding applications such as injection molding. The DBG-copolymerized PBT of Example 10 also showed a small increase in the b value, but had a high solution haze and poor transparency due to its high titanium content.

[0133] [Comparative Example 1 and Comparative Example 2] DBG copolymerized PBT was obtained in the same manner as in Example 1, except that the esterification conditions and steam generation tank conditions in Example 1 were changed to those shown in Table 1. The physical properties and evaluation results of the obtained DBG copolymerized PBT are shown in Table 2. As shown in Table 2, the DBG copolymerized PBT of Comparative Examples 1 and 2, which did not satisfy the requirements of the present invention, showed a large increase in b value (yellowing) when dried in air at 140°C for 8 hours, and was not suitable for molding applications such as injection molding.

[0134] [Comparative Example 3] 397.2 parts by mass of dimethyl terephthalate, 213.8 parts by mass of BDO, and 1.75 parts by mass of 6% tetrabutyl titanate BDO solution (tetrabutyl titanate is 33 mass ppm of titanium element relative to theoretical polymer yield) were added to a 200L stainless steel reaction vessel equipped with a turbine type stirring blade, and an ester exchange reaction was carried out at 150 to 215°C for 2 hours. Then, 1.9 parts by mass of 10% magnesium acetate tetrahydrate BDO solution (magnesium acetate is 48 mass ppm of magnesium element relative to theoretical polymer yield) was dissolved in BDO and added, and further, 3.25 parts by mass of 6% tetrabutyl titanate BDO solution (tetrabutyl titanate is 61 mass ppm of titanium element relative to theoretical polymer yield) was added. Next, the oligomer obtained above was transferred to a 200L stainless steel reaction vessel equipped with a vent pipe and a double helical stirring blade, and a polycondensation reaction was carried out. The polycondensation reaction was gradually reduced in pressure from normal pressure to 0.133kPa over 85 minutes, and at the same time the temperature was raised to the designated polymerization temperature of 240°C. Thereafter, the reaction was continued at the designated polymerization temperature and 0.133kPa. When the designated stirring torque was reached, the reaction was terminated and the polymer was extracted. A steam ejector was used as the vacuum generating device. The physical properties and evaluation results of the obtained PBT are shown in Table 2. The DBG copolymer PBT of Comparative Example 3 showed little increase in b value even after drying in air at 140°C for 8 hours, but the terminal methoxycarbonyl group concentration was high and formaldehyde was generated. Since it becomes formic acid when further oxidized, this DBG copolymer PBT is not suitable for use in electrical and electronic parts or automotive parts. In addition, this DBG copolymer PBT uses dimethyl terephthalate as a raw material component and uses a steam ejector, which is a drawback in that the cost is high.

[0135] [Comparative Example 4] In Comparative Example 3, 360.0 parts by mass of dimethyl terephthalate, 189.0 parts by mass of BDO, and 45.8 parts by mass of polytetramethylene ether glycol with an average molecular weight of 1000 were added with 1.33 parts by mass of 6% by mass of tetrabutyl titanate in BDO (tetrabutyl titanate is 25 mass ppm by mass as titanium element with respect to the theoretical polymer yield), and the transesterification reaction was carried out at 150 to 215°C for 2 hours, and then 1.9 parts by mass of 10% by mass of magnesium acetate tetrahydrate BDO solution (magnesium acetate is 48 mass ppm by mass as magnesium element with respect to the theoretical polymer yield) was dissolved in BDO and added, and further 1.75 parts by mass of 6% by mass of tetrabutyl titanate in BDO solution (tetrabutyl titanate is 33 mass ppm by mass as titanium element with respect to the theoretical polymer yield) was added. Next, the oligomer obtained above was transferred to a stainless steel reaction tank with an internal volume of 200 L equipped with a vent pipe and a double helical type stirring blade, and then a polycondensation reaction was carried out. The polycondensation reaction was gradually reduced in pressure from normal pressure to 0.133 kPa over 85 minutes, and at the same time the temperature was raised to the designated polymerization temperature of 240°C. Thereafter, the reaction was continued at the designated polymerization temperature of 0.133 kPa. When the designated stirring torque was reached, the reaction was terminated and the polymer was extracted. A steam ejector was used as the vacuum generating device. The physical properties and evaluation results of the obtained PBT are shown in Table 2. This polymer is copolymerized with 10% by mass of polytetramethylene ether glycol, a softening component, relative to the polymer. The PBT of Comparative Example 4, in which 10% by mass of polytetramethylene ether glycol was copolymerized with respect to the polymer, had a low DBG copolymerization amount, but the increase in b value was large when dried in air at 140°C for 8 hours. In addition, the terminal methoxycarbonyl group concentration was high, and formaldehyde was generated. Since it was further oxidized to formic acid, this PBT was not suitable for use in electrical and electronic parts or automotive parts. In addition, the flexural modulus was low, and it was not suitable as an engineering plastic. In addition, this PBT uses dimethyl terephthalate as a raw material component, and a steam ejector is used, which is a drawback in that the cost is high.

[0136] [Comparative Examples 5 and 6] DBG copolymerized PBT pellets were obtained in the same manner as in Example 1, except that the conditions in Example 1 were changed to those shown in Table 3. The physical properties and evaluation results of the obtained DBG copolymerized PBT pellets are shown in Table 3. As shown in Table 3, the DBG copolymerized PBT pellets of Comparative Examples 5 and 6, which do not satisfy the requirements of the present invention, showed a large increase in b value (yellowing) when dried in air at 140°C for 8 hours, and were not suitable for molding applications such as injection molding.

[0137] [Table 1]

[0138] [Table 2]

[0139] [Table 3] [Explanation of symbols]

[0140] 1. Raw material supply line 2 Recirculation Line 3 Catalyst supply line 4. Extraction Line 5 Distillation Line 6 Extraction Line 7 Circulation Line 8 Extraction Line 9 Gas extraction line 10 Condensate Line 11 Extraction Line 12 Circulation Line 13 Extraction Line 14 Vent Line 15 Catalyst supply line 16 BDO inflow line 17 Recycled BDO inflow line 18 Liquid Phase Line 19 Steam Line 20 Ejector Line 21 Vapor lines for esterification tank, prepolymer tank, first polymerization tank, and second polymerization tank 22 Balcon Line 23 Balcon Tank Line 24 Recycling BDO Line 25 Raw material slurry line A Reactor B Extraction pump C rectification tower D, E, P1, P2, P3, P4 pumps F Tank G Capacitor H Reboiler L1 Extraction line L3, L5 Extraction lines L2, L4, L6 vent lines a First polycondensation reaction tank d Second polycondensation reaction tank k Third polycondensation reaction tank c, e, m Extraction gear pump f Filter g Die head h Rotary cutter I BDO evaporator J Ejector Equipment K Balcony Equipment L Balcon Tank M Recycled BDO Tank N Raw material slurry tank O Reactor

Claims

1. A dibutylene glycol copolymerized polybutylene terephthalate comprising units derived from a dicarboxylic acid component mainly composed of terephthalic acid and units derived from a diol component mainly composed of 1,4-butanediol and containing dibutylene glycol, wherein the ratio of the units derived from dibutylene glycol to the units derived from the dicarboxylic acid component is 0.13 to 1.0 mol %.

2. 2. The dibutylene glycol copolymerized polybutylene terephthalate according to claim 1, having a titanium content of 100 ppm by mass or less.

3. 3. The dibutylene glycol copolymerized polybutylene terephthalate according to claim 2, having a titanium content of 50 ppm by mass or less.

4. The dibutylene glycol copolymerized polybutylene terephthalate according to any one of claims 1 to 3, having a terminal methoxycarbonyl group concentration of 0.5 equivalents / ton or less.

5. The dibutylene glycol copolymerized polybutylene terephthalate according to any one of claims 1 to 4, wherein the content of the metal of Group 2A of the Periodic Table is 5 to 50 ppm in terms of metal atoms.

6. 6. The dibutylene glycol-co-polybutylene terephthalate according to claim 5, wherein the metal of Group 2A of the Periodic Table is magnesium.

7. The dibutylene glycol-copolymerized polybutylene terephthalate according to any one of claims 1 to 6, having a terminal carboxyl group concentration of 5 to 30 equivalents / ton.

8. The dibutylene glycol copolymerized polybutylene terephthalate according to any one of claims 1 to 7, having an intrinsic viscosity of 0.6 to 1.3 dL / g.

9. The method for producing dibutylene glycol-copolymerized polybutylene terephthalate according to any one of claims 1 to 8, characterized in that the 1,4-butanediol composition used as steam for a vacuum generating device is used as a production raw material.

10. The method for producing dibutylene glycol-co-polybutylene terephthalate according to claim 9, wherein the temperature of the steam generating tank for the vacuum generating device is set to 256° C. or lower.

11. A compound product, characterized in that the dibutylene glycol copolymerized polybutylene terephthalate pellets according to any one of claims 1 to 8 are used as at least a part of a raw material.

12. A method for producing a compound product, comprising using the dibutylene glycol copolymerized polybutylene terephthalate pellets according to any one of claims 1 to 8 as at least a part of a raw material, and kneading the pellets using an extruder.

13. The method for producing a compound product according to claim 12, wherein the kneading temperature of the resin in the extruder is 320°C or lower.

14. A molded article, comprising at least a part of a molding material made of the compound product according to claim 11.

15. A method for producing a molded product, comprising using the compound product according to claim 11 as at least a part of a molding material and injection molding the compound product using an injection molding machine.

16. The method for producing a molded article according to claim 15, wherein the molten resin temperature during the injection molding is 280° C. or lower.

17. The method for producing a molded product according to claim 15 or 16, wherein recycled raw materials are used as at least a part of the molding material.

Citation Information

Patent Citations

  • Polybutylene terephthalate and polybutylene terephthalate composition

    JP2004277719A

  • Polyester elastomer composition, use thereof, and process for producing polyester elastomer composition

    JP2008291237A