Copolymer, method for producing said copolymer, and method for producing copolymer having carboxy group or salt thereof

The synthesis of polyethylene glycol-polyglutamic acid block copolymers is improved by using a specific copolymer with a repeating unit and deprotection in the presence of appropriate acids, addressing by-product formation and racemization issues, leading to high-purity copolymers for drug delivery.

JP7560274B2Active Publication Date: 2024-10-02KAWASAKI INST OF IND PROMOTION
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2020099293
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-06-08
Publication Date
2024-10-02
Estimated Expiration
2040-06-08

AI Technical Summary

Technical Problem

Existing methods for synthesizing polyethylene glycol-polyglutamic acid block copolymers face issues such as the formation of polyglutamate Na as a by-product, racemization, and difficulty in controlling the degree of polymerization, necessitating the purification of impurities.

Method used

A method involving the use of a copolymer containing a repeating unit represented by a specific general formula, which is deprotected in the presence of an organic solvent using acids with a pKa of 0 or more to convert ester groups into carboxyl groups or salts, thereby avoiding by-product formation and racemization.

Benefits of technology

The method allows for easy deprotection of ester groups to carboxyl groups or salts, suppressing the formation of impurities like polyglutamate Na and ensuring controlled polymerization, resulting in a high-purity copolymer suitable for drug delivery systems.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007560274000011
    Figure 0007560274000011
  • Figure 0007560274000012
    Figure 0007560274000012
  • Figure 0007560274000013
    Figure 0007560274000013
Patent Text Reader

Abstract

To provide a method for producing a copolymer (Y) having a carboxy group or a salt thereof, in which carboxy group can be easily deprotected, and also to provide a copolymer (X) used in the production method, and a method for producing the copolymer (X).SOLUTION: The copolymer (X) contains a repeating unit (a) represented by the general formula (1) (in the formula, R1 is a tertiary alkyl group having 4 to 7 carbon atoms, and R2 is an alkylene group having 1 to 4 carbon atoms.), and the method for producing the copolymer (Y) includes a step (β) in which R1 constituting -COOR1 in the repeating unit (a) represented by the general formula (1), of the copolymer is deprotected in the presence of an acid having a pKa of 0 or more and converted into a carboxy group or a salt thereof.SELECTED DRAWING: Figure 9
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a copolymer, a method for producing the copolymer, and a method for producing a copolymer having a carboxy group or a salt thereof. [Background technology]

[0002] In the study of drug delivery systems (DDS), it has been proposed to use polymeric micelles formed by polyethylene glycol-polyamino acid block copolymers and drugs as DDS. As the amino acids constituting the polyethylene glycol-polyamino acid block copolymers, anionic amino acids such as aspartic acid and glutamic acid have been particularly considered.

[0003] As a method for synthesizing a polyethylene glycol-polyglutamic acid block copolymer, a method according to the following scheme (I) is known (see, for example, Non-Patent Document 1).

[0004] [ka]

[0005] In the above scheme (I), first, NH 2 Using polyethylene glycol having a group at the end as a macroinitiator, L-glutamic acid 5-benzyl-N-carboxyanhydride is polymerized to synthesize a polyethylene glycol-polyglutamic acid benzyl ester block copolymer in which the carboxyl group of polyglutamic acid is protected with a benzyl group. The benzyl group is then deprotected using sodium hydroxide to obtain a polyethylene glycol-polyglutamic acid Na block copolymer. The polyethylene glycol-polyglutamic acid Na block copolymer can be appropriately neutralized to obtain a polyethylene glycol-polyglutamic acid block copolymer. [Prior art documents] [Non-patent literature]

[0006] [Non-Patent Document 1] K. Suzuki et al., J. Control. Release 301, 2019, 28-41 Summary of the Invention [Problem to be solved by the invention]

[0007] The present inventors have studied the scheme (I) in detail and found that in the scheme (I), sodium polyglutamate (homopolymer) is obtained as a by-product. The present inventors believe that this is because part of the main chain of the polyglutamic acid (and its derivatives) is cleaved during deprotection. It has also been found that racemization occurs in the resulting polyethylene glycol-sodium polyglutamate block copolymer. The present inventors believe that this is because α-protons are abstracted by hydroxide ions during deprotection.

[0008] Furthermore, the present inventors have found that, in the above scheme (I), a part of the main chain is cleaved during deprotection, which causes problems in that it is difficult to control the degree of polymerization of the sodium polyglutamate moiety or the polyglutamic acid moiety in the resulting polyethylene glycol-sodium polyglutamate block copolymer or polyethylene glycol-polyglutamic acid block copolymer, and that it is necessary to purify the by-product sodium polyglutamate.

[0009] The present invention has been made in view of such problems, and an object of the present invention is to provide a method for producing a copolymer having a carboxy group or a salt thereof, which allows for easy deprotection of the carboxy group. Another object of the present invention is to provide a copolymer used in the method for producing a copolymer having a carboxy group or a salt thereof, and a method for producing the copolymer. [Means for solving the problem]

[0010] Means for Solving the Problems The present inventors have conducted intensive research to solve the above-mentioned problems, and as a result have found a method for producing a copolymer having a carboxy group or a salt thereof, which can solve the above-mentioned problems, a copolymer to be used in the production method, and a method for producing the copolymer, thereby completing the present invention.

[0011] That is, the present invention relates to the following [1] to

[16] . [1] A copolymer (X) containing a repeating unit (a) represented by the following general formula (1): [ka] (In the general formula (1), R 1 is a tertiary alkyl group having 4 to 7 carbon atoms, and R 2 is an alkylene group having 1 to 4 carbon atoms.

[0012] [2] R in the general formula (1) 1 The copolymer (X) according to [1], wherein is a tert-butyl group.

[0013] [3] R in the general formula (1) 2 is a methylene group or an ethylene group.

[0014] [4] The copolymer (X) according to any one of [1] to [3], which is a block copolymer, a random copolymer, or a graft copolymer.

[0015] [5] It is a block copolymer, The copolymer (X) according to any one of [1] to [3], which has a polymer block (A) containing a repeating unit (a) represented by the general formula (1).

[0016] [6] Having a polymer block (B), The copolymer (X) according to [5], wherein the polymer block (B) is formed of a polymer selected from polyethylene glycol, polypropylene glycol, polyglycerin, polyvinyl alcohol, polyvinylpyrrolidone, polyacrylamide, poly[N-(2-hydroxypropyl)methacrylamide], divinyl ether-maleic anhydride copolymer, poly(2-methyl-2-oxazoline), poly(2-ethyl-2-oxazoline), polyphosphazene, and poly(2-methacryloyloxyethyl phosphorylcholine).

[0017] [7] The copolymer (X) according to [6], wherein the polymer block (B) is formed of polyethylene glycol.

[0018] [8] The copolymer (X) according to any one of [1] to [3], which is a random copolymer. [9] The copolymer (X) according to [8], which has a repeating unit (excluding the repeating unit (a)) derived from at least one monomer selected from amino acids and amino acid derivatives.

[0019]

[10] The copolymer (X) according to any one of [1] to [9], wherein the repeating unit (a) represented by the general formula (1) has —COOR 1 Configure R 1 in the presence of an acid having an acid dissociation constant (pKa) (25°C) of 0 or more to convert it into a carboxy group or a salt thereof.

[0020]

[11] The method for producing a copolymer (Y) having a carboxy group or a salt thereof according to

[10] , wherein the acid having an acid dissociation constant (pKa) (25°C) of 0 or more is at least one acid selected from phosphoric acid, formic acid, trifluoroacetic acid, and pyruvic acid.

[0021]

[12] The method for producing a copolymer (Y) having a carboxy group or a salt thereof according to

[10] or

[11] , wherein the deprotection is carried out in the presence of an organic solvent, and the organic solvent is at least one organic solvent selected from acetonitrile, hexane, toluene, xylene, acetone, tetrahydrofuran, diethyl ether, dichloromethane and chloroform.

[0022]

[13] A method for producing a copolymer (X) containing a repeating unit (a) represented by the following general formula (1), comprising the step (α) of polymerizing a monomer represented by the following general formula (1'). [ka] [ka] (In general formulas (1') and (1), R 1 is a tertiary alkyl group having 4 to 7 carbon atoms, and R 2 is an alkylene group having 1 to 4 carbon atoms.

[0023]

[14] The copolymer (X) is a block copolymer, The method for producing the copolymer (X) according to

[13] , wherein the step (α) is carried out in the presence of a macroinitiator.

[0024]

[15] The method for producing a copolymer (X) according to

[14] , wherein the macroinitiator is a macroinitiator having a polymer in its molecule selected from polyethylene glycol, polypropylene glycol, polyglycerin, polyvinyl alcohol, polyvinylpyrrolidone, polyacrylamide, poly[N-(2-hydroxypropyl)methacrylamide], divinyl ether-maleic anhydride copolymer, poly(2-methyl-2-oxazoline), poly(2-ethyl-2-oxazoline), polyphosphazene, and poly(2-methacryloyloxyethyl phosphorylcholine).

[0025]

[16] The copolymer (X) is a random copolymer, The method for producing the copolymer (X) according to

[13] , wherein the step (α) is carried out in the presence of at least one monomer selected from amino acids and amino acid derivatives (excluding the monomer represented by general formula (1')). Effect of the Invention

[0026] In the method for producing copolymer (Y) having a carboxy group or a salt thereof of the present invention, the ester group can be easily converted to a carboxy group or a salt thereof (hereinafter, sometimes referred to as "deprotection") by using copolymer (X). The present invention also provides copolymer (X) used in the method for producing copolymer (Y) having a carboxy group or a salt thereof, and a method for producing said copolymer (X). [Brief description of the drawings]

[0027] [Figure 1] FIG. 1 shows the results of 1H-NMR measurement of PEG-b-PGlu(OtBu) obtained in Example 1. [Diagram 2] FIG. 2 shows the results of GPC measurement of PEG-b-PGlu(OtBu) obtained in Example 1. [Diagram 3] FIG. 3 shows the results of 1H-NMR measurement of PEG-b-PGlu(OtBu) obtained in Example 2. [Figure 4] FIG. 4 shows the results of GPC measurement of PEG-b-PGlu(OtBu) obtained in Example 2. [Diagram 5] FIG. 5 shows the results of 1H-NMR measurement of PEG-bP[Glu(OtBu)-ran-Asp(OBzl)] obtained in Example 3. [Figure 6] FIG. 6 shows the results of GPC measurement of PEG-bP[Glu(OtBu)-ran-Asp(OBzl)] obtained in Example 3. [Figure 7]Fig. 7 shows the results of 1H-NMR measurement of the powder obtained in Example 4. It was confirmed that the tert-butyl group of PEG-b-PGlu(OtBu) was deprotected to become -COONa. [Figure 8] FIG. 8 shows the results of GPC measurement of the powder obtained in Example 4. [Figure 9] FIG. 9 shows the results of GPC measurement of the powder obtained in Example 5. [Figure 10] FIG. 10 shows the results of GPC measurement of the powder obtained in Example 6. [Figure 11] FIG. 11 shows the results of GPC measurement of the powder obtained in Example 7. [Figure 12] FIG. 12 shows the results of GPC measurement of the powder obtained in Example 8. [Figure 13] FIG. 13 shows the results of GPC measurement of the powder obtained in Example 9. [Figure 14] FIG. 14 shows the results of GPC measurement of the powder obtained in Example 10. [Figure 15] FIG. 15 shows the results of GPC measurement of the powder obtained in Example 11. [Figure 16] FIG. 16 shows the results of GPC measurement of the powder obtained in Example 12. [Figure 17] FIG. 17 shows the results of GPC measurement of the powder obtained in Example 13. [Figure 18] FIG. 18 shows the results of GPC measurement of the powder obtained in Example 14. [Figure 19] FIG. 19 shows the results of GPC measurement of the powder obtained in Example 15. [Figure 20] FIG. 20 shows the results of GPC measurement of the powder obtained in Example 16. [Figure 21] FIG. 21 shows the results of GPC measurement of the powder obtained in Example 17. [Figure 22] FIG. 22 shows the results of GPC measurement of the powder obtained in Example 18. [Diagram 23] FIG. 23 shows the results of GPC measurement of the powder obtained in Example 19. [Figure 24]24 shows the results of 1H-NMR measurement of the powder obtained in Example 20. It was confirmed that the tert-butyl group of PEG-b-PGlu(OtBu) was deprotected to become -COONa. [Diagram 25] FIG. 25 shows the results of GPC measurement of the powder obtained in Example 20. [Figure 26] FIG. 26 shows the results of GPC measurement of the powder obtained in Example 21. [Figure 27] FIG. 27 shows the results of GPC measurement of the powders obtained in Examples 22, 23, and 24. [Figure 28] FIG. 28 shows the results of GPC measurement of the powders obtained in Examples 25, 26, and 27. [Figure 29] FIG. 29 shows the results of GPC measurement of the powders obtained in Examples 28, 29, 30, and 31. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0028] Next, the present invention will be described in detail. The present invention is roughly divided into three aspects. The first aspect of the present invention is a copolymer (X) containing a repeating unit (a) represented by general formula (1). The second aspect of the present invention is a method for producing the copolymer (X) capable of obtaining the copolymer (X) of the first aspect. The third aspect of the present invention is a method for producing a copolymer (Y) having a carboxy group or a salt thereof using the copolymer (X) of the first aspect. Each aspect of the present invention will be described in order below.

[0029] In the present invention, the copolymer (X) containing the repeating unit (a) represented by the general formula (1) is also simply referred to as the copolymer (X). Also, the copolymer (Y) having a carboxy group or a salt thereof produced by using the copolymer (X) of the first embodiment is also simply referred to as the copolymer (Y).

[0030] (Copolymer(X)) The copolymer (X) according to the first embodiment of the present invention contains a repeating unit (a) represented by the following general formula (1).

[0031] [ka] (In the general formula (1), R 1 is a tertiary alkyl group having 4 to 7 carbon atoms, and R 2 is an alkylene group having 1 to 4 carbon atoms.

[0032] R in the general formula (1) 1 Examples of the alkyl group include a tert-butyl group, a tert-pentyl group, and a triethylcarbyl group, with a tert-butyl group being preferred. R in the general formula (1) 2 R may be a linear alkylene group or a branched alkylene group, and is preferably a linear alkylene group. 2 Examples of the alkyl group include a methylene group, an ethylene group, an n-propylene group, a 1-methylethylene group, a 2-methylethylene group, and an n-butylene group, with a methylene group or an ethylene group being preferred.

[0033] Preferred embodiments of the repeating unit (a) represented by general formula (1) include a repeating unit represented by the following formula (1-1) and a repeating unit represented by the following formula (1-2).

[0034] [ka]

[0035] The copolymer (X) may have only one type of repeating unit (a) represented by general formula (1), or may have two or more types of repeating units. The copolymer (X) is only required to contain the repeating unit (a) represented by the general formula (1), and there are no particular limitations on the other repeating units or the form of copolymerization.

[0036] Examples of the form of the copolymer (X) include block copolymers, random copolymers, and graft copolymers. The form of the copolymer (X) can be appropriately selected depending on the use of the copolymer (X) and the copolymer (Y) described below. The use of the copolymer (X) and the copolymer (Y) varies depending on the type of other monomers to be copolymerized, and is not particularly limited, but can be used for various biological applications such as drug delivery systems (DDS) for therapeutic drugs for treating diseases such as cancer, agricultural, forestry, and fishery materials, civil engineering and construction materials, films and sheets, sanitary products, and various other applications.

[0037] In addition, in order to impart various properties to the copolymer (X) and the copolymer (Y) described later, a functional group, a ligand molecule, a reporter molecule, or the like may be bound to at least one of the ends (e.g., ends of the main chain or ends of the side chain) and / or in the chain (in the main chain or in the side chain), preferably at least to the ends.

[0038] When the copolymer (X) is a block copolymer, it has a polymer block (A) containing the repeating unit (a) represented by the above general formula (1). The polymer block (A) is not particularly limited as long as it has the repeating unit (a), but it is preferable that the repeating unit (a) is present in an amount of 20 to 100 mass%, and more preferably 40 to 100 mass%, of 100 mass% of the polymer block (A). One of the preferable embodiments of the polymer block (A) is an embodiment in which the repeating unit (a) is 100 mass% of the polymer block (A), that is, a homopolymer of the repeating unit (a). The polymer block (A) may have a repeating unit other than the repeating unit (a). Examples of the repeating unit other than the repeating unit (a) include a repeating unit derived from at least one monomer selected from amino acids and amino acid derivatives described below (excluding the repeating unit (a)). The polymer block (A) preferably has a repeating unit derived from at least one monomer selected from amino acids and amino acid derivatives (excluding the repeating unit (a)) in an amount of 0 to 80 mass%, and more preferably 0 to 60 mass%, of 100 mass% of the polymer block (A). When the polymer block (A) has a repeating unit other than the repeating unit (a), the polymer block (A) may be a random copolymer block, an alternating copolymer block, or a gradient copolymer block, and is not particularly limited.

[0039] When the copolymer (X) is a block copolymer, it has a polymer block (B) which is a polymer block other than the polymer block (A). The copolymer (X) preferably has at least one each of the polymer block (A) and the polymer block (B), and may have a plurality of each polymer block. When the copolymer (X) has a plurality of each polymer block, each polymer block may be formed from the same polymer or from a different polymer.

[0040] The polymer block (B) is not particularly limited, but is preferably formed of a polymer selected from polyethylene glycol, polypropylene glycol, polyglycerin, polyvinyl alcohol, polyvinylpyrrolidone, polyacrylamide, poly[N-(2-hydroxypropyl)methacrylamide], divinyl ether-maleic anhydride copolymer, poly(2-methyl-2-oxazoline), poly(2-ethyl-2-oxazoline), polyphosphazene, and poly(2-methacryloyloxyethyl phosphorylcholine). The polymer block (B) is more preferably formed of a polymer selected from polyethylene glycol, polypropylene glycol, poly(2-methyl-2-oxazoline), and poly(2-ethyl-2-oxazoline), and is particularly preferably polyethylene glycol. Polyethylene glycol, polypropylene glycol, poly(2-methyl-2-oxazoline), and poly(2-ethyl-2-oxazoline) are particularly excellent in biocompatibility, and are therefore preferable when the copolymer (X) or copolymer (Y) is used for biological applications.

[0041] When the copolymer (X) is a block copolymer, its molecular weight is not particularly limited, but is usually 2 to 200 kDa, preferably 4 to 100 kDa, more preferably 4 to 40 kDa. The molecular weight of the polymer block (A) is usually 1 to 100 kDa, preferably 2 to 50 kDa, more preferably 2 to 20 kDa, and the molecular weight of the polymer block (B) is usually 1 to 100 kDa, preferably 2 to 50 kDa, more preferably 2 to 20 kDa. When a plurality of each polymer block is present, the molecular weights of the polymer blocks (A) and (B) are the molecular weights of each polymer block.

[0042] A preferred embodiment is when the copolymer (X) is a random copolymer. When the copolymer (X) is a random copolymer, it is preferable that the copolymer (X) has a repeating unit derived from at least one monomer selected from amino acids and amino acid derivatives. However, the repeating unit derived from at least one monomer selected from the amino acids and amino acid derivatives does not include the repeating unit (a). In addition, the at least one monomer selected from the amino acids and amino acid derivatives does not include a monomer represented by the general formula (1') described below.

[0043] When the copolymer (X) is a random copolymer, the content of the repeating unit (a) is not particularly limited, but the content of the repeating unit (a) in 100% by mass of the copolymer (X) is preferably 20% by mass or more and less than 100% by mass, and more preferably 40% by mass or more and less than 100% by mass.

[0044] When the copolymer (X) is a random copolymer, it preferably contains more than 0% by mass and not more than 80% by mass, and more preferably more than 0% by mass and not more than 60% by mass, of repeating units other than the repeating unit (a), preferably repeating units derived from at least one monomer selected from amino acids and amino acid derivatives.

[0045] When the copolymer (X) is a random copolymer, its molecular weight is not particularly limited, but is usually 2 to 200 kDa, preferably 4 to 100 kDa, and more preferably 4 to 40 kDa.

[0046] When the copolymer (X) is a graft copolymer, the repeating unit (a) represented by the general formula (1) may be contained in the trunk component (trunk polymer) or in the branch component (branch polymer). An example of the case where the copolymer (X) is a graft copolymer is a graft copolymer in which the trunk component is a polymer having at least one group selected from an amino group, a hydroxyl group, and a thiol group, a branch component is grafted from at least a part of the group, and the branch component has the repeating unit (a). The repeating units other than the repeating unit (a) constituting the graft copolymer are preferably repeating units derived from at least one monomer selected from amino acids and amino acid derivatives.

[0047] Examples of the polymer having at least one group selected from the amino group, hydroxy group, and thiol group, which is used as the trunk component, include polymers having repeating units derived from lysine, ornithine, serine, threonine, tyrosine, and cysteine. In addition, examples of the trunk component that can be used include polyallylamine, polyethyleneimine, chitosan, polyglycerin, polyvinyl alcohol, poly(N-(2-hydroxypropyl)methacrylamide, poly(2-hydroxyethyl methacrylate), and polymers having repeating units derived from amino acid derivatives. The trunk component may be a polymer having a functional group other than an amino group, a hydroxy group, and a thiol group, so long as the polymer having the repeating unit (a) as the branch component has a graftable functional group. Specific examples of the trunk polymer include polylysine and polyornithine. The trunk polymer may be a homopolymer or a block copolymer. The trunk polymer may be a copolymer such as a copolymer or a random copolymer. When the trunk polymer is a copolymer of a repeating unit that acts as an initiator for a branch polymer (for example, a repeating unit derived from a monomer that provides at least one group selected from an amino group, a hydroxyl group, and a thiol group in the trunk polymer) and a repeating unit that does not act as an initiator for a branch polymer (for example, a repeating unit derived from a monomer that does not provide a reactive group in the trunk polymer), the number of branch polymers in the graft copolymer can be easily adjusted by adjusting the ratio of the two repeating units. The molecular weight of the trunk polymer is usually 1 to 100 kDa, preferably 2 to 50 kDa, and more preferably 2 to 20 kDa.

[0048] When the branch component is a polymer containing the repeating unit (a) represented by the general formula (1), the polymer is not particularly limited as long as it has the repeating unit (a), but it is preferable that the repeating unit (a) is present in an amount of 20 to 100 mass%, and more preferably 40 to 100 mass%, of 100 mass% of the branch component (branch polymer). One of the preferred aspects of the branch component (branch polymer) is an aspect in which the repeating unit (a) is 100 mass% of the branch component (branch polymer), that is, a homopolymer of the repeating unit (a). The branch component (branch polymer) may have a repeating unit other than the repeating unit (a). Examples of the repeating unit other than the repeating unit (a) include a repeating unit derived from at least one monomer selected from the amino acids and amino acid derivatives described below (excluding the repeating unit (a)). The branch component (branch polymer) preferably contains 0 to 80 mass %, more preferably 0 to 60 mass %, of repeating units (excluding repeating unit (a)) derived from at least one monomer selected from amino acids and amino acid derivatives in 100 mass % of the polymer block (A). When the branch component (branch polymer) contains a repeating unit other than the repeating unit (a), the branch component (branch polymer) may be a random copolymer, an alternating copolymer, or a gradient copolymer, without any particular limitation.

[0049] Another example of the copolymer (X) being a graft copolymer is a graft copolymer in which the trunk component is a polymer having a repeating unit (a) and a branch component is grafted from at least a part of the side chain of the trunk component. In the graft copolymer, the trunk component may have a repeating unit other than the repeating unit (a), for example, a repeating unit derived from at least one monomer selected from amino acids and amino acid derivatives. In addition, the branch component is not particularly limited as long as it can be grafted to the trunk component.

[0050] Examples of amino acids include alanine, arginine, asparagine, aspartic acid, cysteine, glutamine, glutamic acid, glycine, histidine, isoleucine, leucine, lysine, methionine, phenylalanine, proline, serine, threonine, tryptophan, tyrosine, valine, selenocysteine, pyrrolysine, ornithine, citrulline, and hydroxylysine.

[0051] Examples of amino acid derivatives include those in which some functional groups are protected for the purpose of controlling polymerization, and N-carboxyanhydrides. Examples of amino acid derivatives include β-benzyl-L-aspartic acid-N-carboxyanhydride (L-aspartic acid 4-benzyl ester-N-carboxyanhydride), γ-benzyl-L-glutamic acid-N-carboxyanhydride, and Nε-trifluoroacetyl-L-lysine-N-carboxylic anhydride (Lys(TFA)-NCA). For example, in β-benzyl-L-aspartic acid-N-carboxyanhydride, one of the carboxy groups of aspartic acid is protected by a benzyl group, and another carboxy group and an amino group form an N-carboxyanhydride. When these amino acid derivatives are used as monomers, the N-carboxyanhydride structure is ring-opened by polymerization. Therefore, for example, β-benzyl-L-aspartic acid units, γ-benzyl-L-glutamic acid units, and Nε-trifluoroacetyl-L-lysine units can be introduced into the polymer.

[0052] (Method for producing copolymer (X)) The method for producing the copolymer (X), which is the second aspect of the present invention, comprises a step (α) of polymerizing a monomer represented by general formula (1′).

[0053] [ka] (In the general formula (1'), R 1 is a tertiary alkyl group having 4 to 7 carbon atoms, and R 2 is an alkylene group having 1 to 4 carbon atoms.

[0054] In the general formula (1'), R 1 and R 2 As the group, R in the general formula (1) 1 and R 2 The same can be mentioned. Preferred embodiments of the monomer represented by general formula (1') include a monomer represented by the following formula (1'-1) (L-glutamic acid 5-tert-butyl ester-N-carboxyanhydride) and a monomer represented by the following formula (1'-2).

[0055] [ka]

[0056] In the method for producing the copolymer (X), as the monomer represented by the general formula (1'), only one type of monomer may be used, or two or more types of monomers may be used. The method for producing copolymer (X) includes a step (α) of polymerizing a monomer represented by general formula (1'), which becomes the repeating unit (a) represented by general formula (1) in copolymer (X).

[0057] The method for producing the copolymer (X) is not particularly limited as long as it includes the step (α). Hereinafter, the method for producing the copolymer (X) will be described as an example for the case where the copolymer (X) is a block copolymer and the case where the copolymer (X) is a random copolymer.

[0058] When the copolymer (X) is a block copolymer, the step (α) is preferably carried out in the presence of a macroinitiator. As the macroinitiator, for example, a polymer having any one of an amine end, a hydroxyl end, and a thiol end and a polymer chain (a polymer corresponding to the above-mentioned polymer block (B)) can be used.

[0059] The macroinitiator preferably has a polymer selected from polyethylene glycol, polypropylene glycol, polyglycerin, polyvinyl alcohol, polyvinylpyrrolidone, polyacrylamide, poly[N-(2-hydroxypropyl)methacrylamide], divinyl ether-maleic anhydride copolymer, poly(2-methyl-2-oxazoline), poly(2-ethyl-2-oxazoline), polyphosphazene, and poly(2-methacryloyloxyethyl phosphorylcholine) in its molecule, more preferably has polyethylene glycol, polypropylene glycol, poly(2-methyl-2-oxazoline), or poly(2-ethyl-2-oxazoline), and particularly preferably has polyethylene glycol.

[0060] The amount of the macroinitiator and the monomer represented by general formula (1') used varies depending on the application of the resulting block copolymer and is not particularly limited, but the amount of the monomer represented by general formula (1') used per mole of the macroinitiator is usually 10 to 200 moles, preferably 20 to 100 moles.

[0061] When the copolymer (X) is a block copolymer, the step (α) is usually carried out by adding a macroinitiator and a monomer represented by general formula (1′), and, if necessary, a monomer other than the monomer represented by general formula (1′) to an aqueous solvent or an organic solvent, and carrying out a polymerization reaction.

[0062] The aqueous solvent may be water or a weakly alkaline aqueous solution. The weakly alkaline aqueous solution may be, for example, an aqueous sodium hydrogen carbonate solution. When an aqueous solvent is used, the pH is preferably in the range of 7 to 11.

[0063] The organic solvent is preferably an aprotic solvent, such as acetonitrile, N,N-dimethylformamide (DMF), N,N-dimethylacetamide (DMA), N-methylpyrrolidone (NMP), dimethylsulfoxide (DMSO), tetrahydrofuran (THF), cyanobenzene, phenylacetonitrile, chlorobenzene, dichloromethane, and nitromethane.

[0064] The amount of the solvent (aqueous solvent or organic solvent) used is usually 1,000 to 10,000 parts by mass per 100 parts by mass of the monomer represented by the general formula (1'). In the step (α), thiourea may be used to ensure that the polymerization reaction proceeds uniformly.

[0065] Step (α) may be carried out under atmospheric conditions (in air) or under an inert gas atmosphere such as argon or nitrogen. When an aqueous solvent is used as the solvent, it is preferably carried out under atmospheric conditions from the viewpoint of cost. When an organic solvent or a mixed solvent is used as the solvent, it is preferably carried out under an inert gas atmosphere from the viewpoint of stably proceeding with the reaction.

[0066] The temperature (polymerization temperature) when carrying out the step (α) varies depending on the type of monomer, but is usually within the range of 0 to 40° C., and the polymerization time is usually 1 to 120 hours. The monomer other than the monomer represented by the general formula (1') may be, for example, at least one monomer selected from amino acids and amino acid derivatives. As the amino acid and amino acid derivative, those mentioned above can be used.

[0067] When the copolymer (X) is a random copolymer, the step (α) is usually carried out by adding a monomer represented by general formula (1') and at least one monomer selected from amino acids and amino acid derivatives (excluding the monomer represented by general formula (1')) to a solvent (aqueous solvent or organic solvent) and carrying out a polymerization reaction. As the amino acid and amino acid derivative, those described above can be used. As the solvent (aqueous solvent or organic solvent), those described above can be used.

[0068] When the copolymer (X) is a random copolymer, the step (α) is preferably carried out in the presence of a polymerization initiator. The polymerization initiator is not particularly limited as long as it can randomly copolymerize the monomer represented by the general formula (1') and at least one monomer selected from amino acids and amino acid derivatives (excluding the monomer represented by the general formula (1')), and can be, for example, an amine, an alcohol, or a thiol.

[0069] The relationship between the amounts of polymerization initiator and monomers used varies depending on the application of the resulting random copolymer and is not particularly limited, but the total amount of all monomers per mole of polymerization initiator is usually 10 to 200 moles, and preferably 20 to 100 moles.

[0070] Step (α) is preferably carried out under an atmosphere of an inert gas such as argon, nitrogen, etc. The temperature (polymerization temperature) when carrying out step (α) varies depending on the type of monomer, but is usually carried out within a range of 0 to 40° C., and the polymerization time is usually 1 to 168 hours.

[0071] When the copolymer (X) is a graft copolymer, the step (α) can be carried out by changing the macroinitiator when the copolymer (X) is a block copolymer to, for example, a polymer having at least one group selected from the amino group, hydroxyl group, and thiol group. The amount of the polymer having at least one group selected from the amino group, hydroxyl group, and thiol group and the monomer represented by general formula (1') used is not particularly limited, and varies depending on the application of the obtained graft copolymer, but the amount of the monomer represented by general formula (1') is usually 10 to 200 moles, preferably 20 to 100 moles, per mole of the nucleophilic functional group (at least one group selected from the amino group, hydroxyl group, and thiol group) of the polymer having at least one group selected from the amino group, hydroxyl group, and thiol group.

[0072] The conditions such as temperature, atmosphere, and solvent may be the same as those in the production method of the block copolymer. In any case where the copolymer (X) is a block copolymer, a random copolymer, or a graft copolymer, the pressure during polymerization may be any of reduced pressure, increased pressure, and normal pressure, but from the viewpoint of production costs, it is preferable to carry out the polymerization at normal pressure.

[0073] In the method for producing the copolymer (X) of the second embodiment, after the step (α), a step of purifying the obtained polymer may be carried out as an optional step. As the purification step, methods such as dialysis, reprecipitation, and recrystallization can be adopted.

[0074] (Method for producing copolymer (Y)) The method for producing the copolymer (Y) according to the third embodiment of the present invention comprises the steps of: 1 Configure R 1The process further comprises a step (β) of deprotecting the above in the presence of an acid having an acid dissociation constant (pKa) (25°C) of 0 or more to convert the above to a carboxy group or a salt thereof. The copolymer (Y) obtained by the production method of the third embodiment is a copolymer having a carboxy group or a salt thereof. In the production method of the copolymer (Y) of the present invention, the production of impurities (polyglutamic acid Na (homopolymer)) by-produced during the reaction in the above scheme (I) is suppressed, and the racemization of the obtained copolymer (Y) is unlikely to occur. In addition, this is preferable because the deprotection easily proceeds.

[0075] The acid having an acid dissociation constant (pKa) (25°C) of 0 or more is preferably an acid having a pKa (25°C) of 4.8 or less, from the viewpoint of rapidly progressing the step (β). Examples of the acid having an acid dissociation constant (pKa) (25°C) of 0 or more include phosphoric acid (2.12), formic acid (3.75), acetic acid (4.74), trifluoroacetic acid (0.23), pyruvic acid (2.50), benzoic acid (4.19), citric acid (3.09), succinic acid (4.19), oxalic acid (1.27), malonic acid (2.85), maleic acid (2.00), fumaric acid (3.02), phthalic acid (2.96), isophthalic acid (3.54), terephthalic acid (3. 51), thiocyanic acid (0.926), sulfurous acid (1.9), and nitrous acid (3.29) (note that the values ​​in parentheses indicate pKa at 25°C. For acids with two or more acid dissociation sites, the lower pKa is indicated), and at least one acid selected from phosphoric acid, formic acid, trifluoroacetic acid, and pyruvic acid is more preferred, with phosphoric acid, formic acid, or trifluoroacetic acid being particularly preferred. When phosphoric acid is used as the acid, it is usually used as an aqueous phosphoric acid solution. The concentration of phosphoric acid in the aqueous phosphoric acid solution is not particularly limited, but is preferably 41 to 90% by mass, more preferably 45 to 88% by mass, and particularly preferably 50 to 87% by mass.

[0076] The amount of the acid having an acid dissociation constant (pKa) (25° C.) of 0 or more used is usually 1 to 10,000 mol, preferably 2,000 to 6,000 mol, per mol of the repeating unit (a) represented by general formula (1) contained in the copolymer (X).

[0077] In the present invention, the acid having an acid dissociation constant (pKa) (25° C.) of 0 or more is used, so that R 1 It is possible to easily remove the The deprotection may be carried out in the absence of a solvent, or in the presence of water, an organic solvent, or water and an organic solvent. It is preferable to carry out the deprotection in the presence of an organic solvent, or in the presence of water and an organic solvent, in which the generation of homopolymers, which are impurities, tends to be more suppressed. When the deprotection is carried out in the presence of water and an organic solvent, it is a two-phase reaction of an aqueous phase / an organic phase. When the deprotection is carried out in the presence of an organic solvent, the reaction system changes depending on the combination of the acid and the organic solvent. When the acid and the organic solvent are not mixed, it is a two-phase reaction of an acid / an organic phase, and when they are mixed, it is a one-phase reaction. When an organic solvent is not used, the copolymer (X) is in a solid state, and the acid and water are liquid, so it is a solid-liquid reaction. It is preferable to carry out the deprotection in a state in which the copolymer (X) is dissolved in an organic solvent from the viewpoint of efficient deprotection.

[0078] The organic solvent is preferably at least one organic solvent selected from acetonitrile, hexane, toluene, xylene, acetone, tetrahydrofuran, diethyl ether, dichloromethane, and chloroform, and more preferably at least one organic solvent selected from acetonitrile, hexane, toluene, and xylene.

[0079] In the deprotection, when formic acid is used as the acid, it is preferable to use at least one organic solvent selected from acetonitrile, hexane, toluene, and xylene as the organic solvent, and it is more preferable to use acetonitrile, toluene, or xylene. When trifluoroacetic acid is used as the acid, it is preferable to use at least one organic solvent selected from acetone, acetonitrile, diethyl ether, hexane, toluene, xylene, and chloroform as the organic solvent, and it is more preferable to use toluene or xylene. When phosphoric acid is used as the acid, it is preferable to use at least one organic solvent selected from acetonitrile, hexane, toluene, xylene, chloroform, and dichloromethane as the organic solvent, and it is more preferable to use acetonitrile. The combination of these acids and organic solvents is particularly preferable because the impurities are reduced. When phosphoric acid is used as the acid, it is preferable to perform the deprotection in the presence of water and an organic solvent.

[0080] The amount of the organic solvent used is not particularly limited, but from the viewpoint of carrying out the reaction efficiently, the volume ratio of the acid to the organic solvent (volume of the acid:volume of the organic solvent) is preferably 10:90 to 90:10, more preferably 15:85 to 85:15, and particularly preferably 20:80 to 80:20. However, when an aqueous phosphoric acid solution is used, the volume of the aqueous phosphoric acid solution:volume of the organic solvent may be within the above range.

[0081] Acid and -COOR 1 When reacted with carboxylate (-COO - ), it is preferable to neutralize the copolymer with a salt of a carboxy group using at least one selected from sodium hydroxide, potassium hydroxide, sodium carbonate, potassium carbonate, sodium hydrogen carbonate, potassium hydrogen carbonate, sodium phosphate, potassium phosphate, disodium hydrogen phosphate, and dipotassium hydrogen phosphate. The neutralization may be performed using a carbonate buffer solution (pH 10) or a phosphate buffer solution (pH 7.4). The use of these buffer solutions allows neutralization under mild conditions.

[0082] As a method for obtaining the copolymer (Y) having a carboxy group, for example, a method for obtaining the copolymer (Y) by the reaction of an acid with -COOR 1 and then performing deprotection, followed by reprecipitation using diethyl ether or the like to obtain a copolymer having a carboxy group; a method in which after deprotection, the acid is removed by dialysis, and then the copolymer having a carboxy group is obtained by freeze-drying; and a combination of these methods.

[0083] Step (β) may be carried out under atmospheric conditions (in air) or in an inert gas atmosphere such as argon, nitrogen, etc. Step (β) is usually carried out at a temperature within the range of 0 to 30° C. for a period of time of usually 0.5 to 24 hours.

[0084] Step (β) may be carried out once or twice or more depending on the progress of deprotection. Step (β) is usually carried out once or twice, preferably once. The step (β) may be carried out under any of reduced pressure, increased pressure, and normal pressure conditions, but from the viewpoint of production costs, it is preferably carried out under normal pressure. EXAMPLES

[0085] The present invention will now be described in more detail with reference to examples, but the present invention is not limited to these.

[0086] [Example 1] (Synthesis of PEG-b-PGlu(OtBu)) 2.06 g of L-glutamic acid 5-tert-butyl ester-N-carboxyanhydride was dissolved in 3.60 g of α-methoxy-ω-aminopolyethylene glycol (CH 3 O-PEG-NH 2 ) (Molecular weight: 12 kDa) (One end is CH 3 O-, the other end is -NH 2Polymerization was carried out in 85 ml of 1 M thiourea in N,N-dimethylformamide (DMF) using 1M polyethylene glycol (PEG) as a macroinitiator. Thiourea was added to inhibit secondary structure formation in the growing polymer chain and to control the polymerization reaction. Polymerization was carried out at 25°C for 2 days under an argon atmosphere. After 2 days, the resulting solution was dialyzed against pure water at room temperature and then lyophilized.

[0087] The resulting polymer was dissolved in dimethylacetamide (DMAc) and reprecipitated by adding diethyl ether three times to increase the purity. The amount of DMAc used in the first, second, and third reprecipitations was 75 ml, and the amount of diethyl ether used was 375 ml, 400 ml, and 450 ml, respectively.

[0088] The resulting final product is 1 The results were analyzed by H-NMR spectroscopy (400 MHz) (JNM-ECS400, JEOL Ltd., Tokyo, Japan) and gel filtration chromatography (GPC) (LC-2000Plus series, equipped with G4000HHR and G3000HHR columns, JASCO Corporation, Tokyo, Japan) using DMF containing 10 mM LiCl as the mobile phase, and it was confirmed that PEG-b-poly(L-glutamic acid 5-tert-butyl ester) (hereinafter also referred to as PEG-b-PGlu(OtBu)) was obtained. Note that an RI detector (differential refractometer) was used as the detector for GPC.

[0089] 1 The results of H-NMR are shown in Figure 1, and the results of GPC are shown in Figure 2. From Figure 1, it was confirmed that the degree of polymerization of the poly(L-glutamic acid 5-tert-butyl ester) chain was 20, and from Figure 2, it was confirmed that the monodispersity of the block copolymer was good.

[0090] [Example 2] (Synthesis of PEG-b-PGlu(OtBu) 2) 0.100 g of α-methoxy-ω-aminopolyethylene glycol (CH3 O-PEG-NH 2 A 0.05 M aqueous hydrogen carbonate solution containing 5-tert-butyl L-glutamate (molecular weight: 12 kDa) was cooled on ice, and 0.0860 g of L-glutamic acid 5-tert-butyl ester-N-carboxyanhydride was added thereto. The mixture was stirred for 3 hours with ice cooling and then for 18 hours at room temperature to carry out polymerization.

[0091] The resulting solution was purified by dialysis against methanol using a dialysis membrane with a molecular weight cutoff of 6000-8000, and the solvent was removed using a rotary evaporator. The product was then dissolved in benzene and freeze-dried to obtain a product.

[0092] The resulting final product was subjected to the same procedure as in Example 1. 1 Analysis using H-NMR spectroscopy and GPC confirmed that PEG-b-PGlu(OtBu) was obtained. 1 The H-NMR measurement results are shown in Figure 3, and the GPC measurement results are shown in Figure 4. From Figure 3, it was confirmed that the degree of polymerization of the poly(L-glutamic acid 5-tert-butyl ester) chain was 41, and from Figure 4, it was confirmed that the monodispersity of the block copolymer was good.

[0093] [Example 3] (Synthesis of PEG-bP[Glu(OtBu)-ran-Asp(OBzl)]) 0.215 g of L-glutamic acid 5-tert-butyl ester-N-carboxyanhydride and 0.233 g of L-aspartic acid 4-benzyl ester-N-carboxyanhydride were dissolved in 0.500 g of α-methoxy-ω-aminopolyethylene glycol (CH 3 O-PEG-NH 2 ) (Molecular weight: 12 kDa) (One end is CH 3 O-, the other end is -NH 2Polyethylene glycol (POG) was used as a macroinitiator and polymerization was carried out in 15.8 ml of a mixed solvent of N,N-dimethylformamide (DMF) and dichloromethane (volume ratio 1:9). The polymerization was carried out at 25°C for 3 days under an argon atmosphere. After 3 days, the resulting solution was reprecipitated in a mixed solvent of hexane and ethyl acetate (volume ratio 6:4), dissolved in benzene, and freeze-dried to obtain the product.

[0094] The resulting final product was subjected to the same procedure as in Example 1. 1 Analysis using H-NMR spectroscopy and GPC confirmed that PEG-b-poly(L-glutamic acid 5-tert-butyl ester-ran-L-aspartic acid 4-benzyl ester) (hereinafter also referred to as PEG-bP[Glu(OtBu)-ran-Asp(OBzl)]) was obtained.

[0095] 1 The H-NMR measurement results are shown in Figure 5, and the GPC measurement results are shown in Figure 6. From Figure 5, it was confirmed that the degree of polymerization of poly(L-glutamic acid 5-tert-butyl ester) was 18, and that the degree of polymerization of poly(L-aspartic acid 4-benzyl ester) was 19, and from Figure 6, it was confirmed that the monodispersity of the block copolymer was good.

[0096] [Example 4] (Deprotection of tert-butyl group) 5 mg of PEG-b-PGlu(OtBu) obtained in Example 1 was dissolved in 0.5 ml of acetonitrile to obtain a polymer solution. 0.5 ml of 85% aqueous phosphoric acid was added to the obtained polymer solution to obtain a reaction solution, which was stirred in air at room temperature for 24 hours. The reaction solution was cooled in an ice bath, and 5M NaOH (0.98 molar equivalent to the phosphoric acid added) was added little by little to neutralize the acid, and then 1 ml of 1M H 3 PO 4 The neutralized solution was dialyzed against Milli-Q water and then lyophilized.

[0097] The obtained powder is 1The samples were analyzed by H-NMR spectroscopy (400 MHz) (JEOL ECS 400, JEOL Ltd., Tokyo, Japan) and gel filtration chromatography (GPC) (LC-2000Plus series, equipped with a Superdex 200 Increase 10 / 300 GL column, JASCO Corporation, Tokyo, Japan) using 10 mM phosphate buffer (pH 7.4 aqueous solution containing 500 mM NaCl) as the mobile phase. The GPC was performed using both an RI detector (differential refractometer) and a UV detector (ultraviolet detector). The same experiment was performed five times in total.

[0098] 1 The measurement results of H-NMR are shown in Figure 7 (one example), and the measurement results of GPC (RI detector, UV detector) are shown in Figure 8. Since no signal of tert-butyl group (chemical shift = 1.4 ppm) is observed in Figure 7, and no peak is observed at the exclusion limit (elution time 16.5 minutes) in Figure 8, it was confirmed that the tert-butyl group of PEG-b-PGlu(OtBu) was deprotected to become -COONa. Furthermore, since the generation of peaks is suppressed after elution time 28 minutes in Figure 8, it was confirmed that the by-production of sodium polyglutamate (homopolymer) is suppressed.

[0099] [Example 5] (Deprotection of tert-butyl group) 5 mg of PEG-b-PGlu(OtBu) obtained in Example 1 was dissolved in 0.5 ml of acetonitrile to obtain a polymer solution. 0.5 ml of formic acid was added to the obtained polymer solution to obtain a reaction solution, which was stirred in air at room temperature for 24 hours. The reaction solution was cooled in an ice bath, and 5M NaOH (0.98 molar equivalent to the added formic acid) was added little by little to neutralize the acid, and then 1 ml of 1M H 3 PO 4 The neutralized solution was dialyzed against Milli-Q water and then lyophilized.

[0100] The obtained powder was analyzed by GPC in the same manner as in Example 4. The same experiment was carried out twice in total. The results of GPC (RI detector, UV detector) are shown in Figure 9. Since no peak was observed at the exclusion limit (elution time 16.5 minutes) in Figure 9, it was confirmed that the tert-butyl group of PEG-b-PGlu(OtBu) was deprotected, and since the generation of a peak was suppressed after the elution time of 28 minutes, it was confirmed that the by-production of sodium polyglutamate (homopolymer) was suppressed.

[0101] [Example 6] (Deprotection of tert-butyl group) 5 mg of PEG-b-PGlu(OtBu) obtained in Example 1 was suspended in 0.5 ml of hexane to obtain a polymer suspension. 0.5 ml of formic acid was added to the obtained polymer suspension to obtain a reaction solution, which was vigorously stirred at room temperature in air for 24 hours. The reaction solution was cooled in an ice bath, and 5M NaOH (0.98 molar equivalent to the added formic acid) was gradually added to neutralize the acid, followed by 1 ml of 1M H 3 PO 4 The neutralized solution was dialyzed against Milli-Q water and then lyophilized.

[0102] The obtained powder was analyzed by GPC in the same manner as in Example 4. The same experiment was carried out twice in total. The results of GPC measurement (RI detector, UV detector) are shown in Figure 10. Since no peak was observed at the exclusion limit (elution time 16.5 minutes) in Figure 10, it was confirmed that the tert-butyl group of PEG-b-PGlu(OtBu) was deprotected, and since the generation of a peak was suppressed after the elution time of 28 minutes, it was confirmed that the by-production of sodium polyglutamate (homopolymer) was suppressed.

[0103] [Examples 7 and 8] (Deprotection of tert-butyl group) 5 mg of PEG-b-PGlu(OtBu) obtained in Example 1 was dissolved in 0.5 ml of toluene to obtain a polymer solution. 0.5 ml of trifluoroacetic acid (Example 7) or formic acid (Example 8) was added to the obtained polymer solution to obtain a reaction solution, which was vigorously stirred at room temperature in air for 24 hours. The reaction solution was cooled in an ice bath, and 5M NaOH (0.98 molar equivalent to the added trifluoroacetic acid (Example 7) or formic acid (Example 8)) was gradually added to neutralize the acid, followed by adding 1 ml of 1M H 3 PO 4 The neutralized solution was dialyzed against Milli-Q water and then lyophilized.

[0104] The obtained powder was analyzed by GPC in the same manner as in Example 4. The same experiment was carried out a total of two times (Example 7) or three times (Example 8). The results of GPC measurement (RI detector, UV detector) are shown in Figures 11 (Example 7) and 12 (Example 8). Since no peak was observed at the exclusion limit (elution time 16.5 minutes) in Figures 11 and 12, it was confirmed that the tert-butyl group of PEG-b-PGlu(OtBu) was deprotected, and since the generation of a peak was suppressed after the elution time of 28 minutes, it was confirmed that the by-production of sodium polyglutamate (homopolymer) was suppressed.

[0105] [Examples 9 and 10] (Deprotection of tert-butyl group) 5 mg of PEG-b-PGlu(OtBu) obtained in Example 1 was dissolved in 0.5 ml of xylene to obtain a polymer solution. 0.5 ml of trifluoroacetic acid (Example 9) or formic acid (Example 10) was added to the obtained polymer solution to obtain a reaction solution, which was vigorously stirred at room temperature in air for 24 hours. The reaction solution was cooled in an ice bath, and 5M NaOH (0.98 molar equivalent to the added trifluoroacetic acid (Example 9) or formic acid (Example 10)) was gradually added to neutralize the acid, followed by the addition of 1 ml of 1M H 3 PO 4The neutralized solution was dialyzed against Milli-Q water and then lyophilized.

[0106] The resulting powder was analyzed by GPC in the same manner as in Example 4. The results of GPC measurement (RI detector, UV detector) are shown in Figures 13 (Example 9) and 14 (Example 10). Since no peak was observed at the exclusion limit (elution time 16.5 minutes) in Figures 13 and 14, it was confirmed that the tert-butyl group of PEG-b-PGlu(OtBu) was deprotected, and since the generation of a peak was suppressed after the elution time of 28 minutes, it was confirmed that the by-production of sodium polyglutamate (homopolymer) was suppressed.

[0107] [Examples 11, 12, and 13] (Deprotection of tert-butyl group) 5 mg of PEG-b-PGlu(OtBu) obtained in Example 1 was added to 1.0 ml of trifluoroacetic acid (Example 11), formic acid (Example 12), or 85% aqueous phosphoric acid (Example 13) to form a reaction solution, which was vigorously stirred at room temperature in air for 24 hours. The reaction solution was cooled in an ice bath, and 5 M NaOH (0.98 molar equivalent to the amount of trifluoroacetic acid (Example 11), formic acid (Example 12), or phosphoric acid (Example 13) added) was gradually added to neutralize the acid, followed by the addition of 1 ml of 1 M H 3 PO 4 The neutralized solution was dialyzed against Milli-Q water and then lyophilized.

[0108] The obtained powder was analyzed by GPC in the same manner as in Example 4. The same experiment was carried out twice in total. The results of GPC measurement (RI detector, UV detector) are shown in Figure 15 (Example 11), 16 (Example 12), and Figure 17 (Example 13). Since no peak was observed at the exclusion limit (elution time 16.5 minutes) in Figures 15, 16, and 17, it was confirmed that the tert-butyl group of PEG-b-PGlu(OtBu) was deprotected, and since the generation of a peak was suppressed after the elution time of 28 minutes, it was confirmed that the by-production of sodium polyglutamate (homopolymer) was suppressed.

[0109] [Example 14] (Deprotection of tert-butyl group) 5 mg of PEG-b-PGlu(OtBu) obtained in Example 1 was suspended in 0.5 ml of water to obtain a polymer suspension. 0.5 ml of trifluoroacetic acid was added to the obtained polymer suspension to obtain a reaction solution, which was vigorously stirred at room temperature in air for 24 hours. The reaction solution was cooled in an ice bath, and 5M NaOH (0.98 molar equivalent to the added trifluoroacetic acid) was gradually added to neutralize the acid, followed by 1 ml of 1M H 3 PO 4 The neutralized solution was dialyzed against Milli-Q water and then lyophilized.

[0110] The resulting powder was analyzed by GPC in the same manner as in Example 4. The results of GPC (RI detector, UV detector) are shown in Figure 18. Since no peak was observed at the exclusion limit (elution time 16.5 minutes) in Figure 18, it was confirmed that the tert-butyl group of PEG-b-PGlu(OtBu) was deprotected, and since the generation of a peak was suppressed after the elution time of 28 minutes, it was confirmed that the by-production of sodium polyglutamate (homopolymer) was suppressed.

[0111] [Examples 15 and 16] (Deprotection of tert-butyl group) 5 mg of PEG-b-PGlu(OtBu) obtained in Example 1 was dissolved in 0.5 ml of acetone (Example 15) or acetonitrile (Example 16) to obtain a polymer solution. 0.5 ml of trifluoroacetic acid was added to the obtained polymer solution to obtain a reaction solution, which was vigorously stirred at room temperature in air for 24 hours. The reaction solution was cooled in an ice bath, and 5M NaOH (0.98 molar equivalent to the added trifluoroacetic acid) was gradually added to neutralize the acid, followed by adding 1 ml of 1M H 3 PO 4 The neutralized solution was dialyzed against Milli-Q water and then lyophilized.

[0112] The obtained powder was analyzed by GPC in the same manner as in Example 4. The same experiment was carried out a total of two times (Example 15) or three times (Example 16). The results of GPC (RI detector, UV detector) are shown in Figures 19 (Example 15) and 20 (Example 16). In Figure 19, no peak was observed at the exclusion limit (elution time 16.5 minutes), confirming that the tert-butyl group of PEG-b-PGlu(OtBu) was deprotected, and the generation of a peak was suppressed after elution time 28 minutes, confirming that the by-production of sodium polyglutamate (homopolymer) was suppressed. In Figure 20, no peak was observed at the exclusion limit (elution time 16.5 minutes), confirming that the tert-butyl group of PEG-b-PGlu(OtBu) was deprotected. In Figure 20, in run 2 and run 3 using the UV detector, a slight peak was observed after elution time 28 minutes, suggesting that a slight by-production of sodium polyglutamate (homopolymer) occurred.

[0113] [Examples 17 and 18] (Deprotection of tert-butyl group) 5 mg of PEG-b-PGlu(OtBu) obtained in Example 1 was suspended in 0.5 ml of diethyl ether (Example 17) or hexane (Example 18) to obtain a polymer suspension. 0.5 ml of trifluoroacetic acid was added to the obtained polymer suspension to obtain a reaction solution, which was vigorously stirred at room temperature in air for 24 hours. The reaction solution was cooled in an ice bath, and 5M NaOH (0.98 molar equivalent to the added trifluoroacetic acid) was added little by little to neutralize the acid, followed by 1 ml of 1M H 3 PO 4 The neutralized solution was dialyzed against Milli-Q water and then lyophilized.

[0114] The obtained powder was analyzed by GPC in the same manner as in Example 4. In Example 18, the same experiment was carried out twice in total. The results of GPC measurement (RI detector, UV detector) are shown in Figures 21 (Example 17) and 22 (Example 18). Since no peak was observed at the exclusion limit (elution time 16.5 minutes) in Figures 21 and 22, it was confirmed that the tert-butyl group of PEG-b-PGlu(OtBu) was deprotected, and since the generation of a peak was suppressed after the elution time of 28 minutes, it was confirmed that the by-production of sodium polyglutamate (homopolymer) was suppressed.

[0115] [Example 19] (Deprotection of tert-butyl group) 5 mg of PEG-b-PGlu(OtBu) obtained in Example 1 was dissolved in 0.5 ml of chloroform to obtain a polymer solution. 0.5 ml of trifluoroacetic acid was added to the obtained polymer solution to obtain a reaction solution, which was vigorously stirred at room temperature in air for 24 hours. The reaction solution was cooled in an ice bath, and 5M NaOH (0.98 molar equivalent to the added trifluoroacetic acid) was added little by little to neutralize the acid, and then 1 ml of 1M H 3 PO 4 The neutralized solution was dialyzed against Milli-Q water and then lyophilized.

[0116] The resulting powder was analyzed by GPC in the same manner as in Example 4. The results of GPC measurement (RI detector, UV detector) are shown in Figure 23. Since no peak was observed at the exclusion limit (elution time 16.5 minutes) in Figure 23, it was confirmed that the tert-butyl group of PEG-b-PGlu(OtBu) was deprotected, and since the generation of a peak was suppressed after the elution time of 28 minutes, it was confirmed that the by-production of sodium polyglutamate (homopolymer) was suppressed.

[0117] [Example 20] (Deprotection of tert-butyl group) 5 mg of PEG-b-PGlu(OtBu) obtained in Example 1 was suspended in 0.5 ml of hexane to obtain a polymer suspension. 0.5 ml of 85% aqueous phosphoric acid was added to the polymer suspension to obtain a reaction solution, which was vigorously stirred at room temperature in air for 24 hours. The reaction solution was cooled in an ice bath, and 5M NaOH (0.98 molar equivalent to the phosphoric acid added) was added little by little to neutralize the acid, and then 1 ml of 1M H 3 PO 4 The neutralized solution was dialyzed against Milli-Q water and then lyophilized.

[0118] The obtained powder was subjected to the same procedure as in Example 4. 1 H-NMR spectroscopy and GPC were used for analysis. 1 The results of H-NMR are shown in Figure 24, and the results of GPC (RI detector, UV detector) are shown in Figure 25. Since no signal of tert-butyl group (chemical shift = 1.4 ppm) is observed in Figure 24, and no peak is observed at the exclusion limit (elution time 16.5 minutes) in Figure 25, it was confirmed that the tert-butyl group of PEG-b-PGlu(OtBu) was deprotected to become -COONa. Furthermore, since the generation of a peak is suppressed after elution time 28 minutes in Figure 25, it was confirmed that the by-production of sodium polyglutamate (homopolymer) is suppressed.

[0119] [Example 21] (Deprotection of tert-butyl group) 5 mg of PEG-b-PGlu(OtBu) obtained in Example 1 was dissolved in 0.5 ml of toluene to obtain a polymer solution. 0.5 ml of 85% aqueous phosphoric acid was added to the obtained polymer solution to obtain a reaction solution, which was vigorously stirred at room temperature in air for 24 hours. The reaction solution was cooled in an ice bath, and 5M NaOH (0.98 molar equivalent to the phosphoric acid added) was added little by little to neutralize the acid, and then 1 ml of 1M H 3 PO 4 The neutralized solution was dialyzed against Milli-Q water and then lyophilized.

[0120] The obtained powder was subjected to the same procedure as in Example 4. 1 The results were analyzed using H-NMR spectroscopy and GPC. Similar experiments were carried out three times in total. The results of GPC (RI detector, UV detector) are shown in Figure 26. Since no peak was observed at the exclusion limit (elution time 16.5 min) in Figure 26, it was confirmed that the tert-butyl group of PEG-b-PGlu(OtBu) was deprotected. In Figure 26, a slight peak was observed after elution time 28 min in run 2 using the UV detector, suggesting that a small amount of sodium polyglutamate (homopolymer) was produced as a by-product.

[0121] [Examples 22, 23, and 24] (Deprotection of tert-butyl group) The following experiment was carried out to examine the effect of changing the ratio of acetonitrile (organic solvent) to acid (phosphoric acid). 5 mg of PEG-b-PGlu(OtBu) obtained in Example 1 was dissolved in 0.75 ml (Example 22), 0.5 ml (Example 23), or 0.25 ml (Example 24) of acetonitrile to obtain a polymer solution. 0.25 ml (Example 22), 0.5 ml (Example 23), or 0.75 ml (Example 24) of an 85% aqueous phosphoric acid solution was added to the obtained polymer solution to obtain a reaction solution, which was stirred in air at room temperature for 24 hours. The reaction solution was cooled in an ice bath, and 5 M NaOH (0.98 molar equivalent to the phosphoric acid added) was added little by little to neutralize the acid, followed by 1 ml of 1 M H 3 PO 4 The neutralized solution was dialyzed against Milli-Q water and then lyophilized.

[0122] The resulting powder was analyzed by GPC in the same manner as in Example 4. The results of GPC (RI detector, UV detector) are shown in Figure 27. Since no peak was observed at the exclusion limit (elution time 16.5 minutes) in Figure 27, it was confirmed that the tert-butyl group of PEG-b-PGlu(OtBu) was deprotected, and since the generation of a peak was suppressed after the elution time of 28 minutes, the by-production of sodium polyglutamate (homopolymer) was suppressed. Furthermore, in Examples 22, 23, and 24, no significant difference was observed in the results of GPC analysis even when the ratio of the amount of organic solvent to the amount of acid was changed.

[0123] [Examples 25, 26, and 27] (Deprotection of tert-butyl group) In order to examine the effect of changing the phosphoric acid concentration in the phosphoric acid aqueous solution, the following experiment was carried out. An 85% phosphoric acid solution was diluted with Milli-Q water to prepare a 60% phosphoric acid solution and a 75% phosphoric acid solution. 5 mg of PEG-b-PGlu(OtBu) obtained in Example 1 was dissolved in 0.5 ml of acetonitrile to obtain a polymer solution. 0.5 ml of 60% phosphoric acid aqueous solution (Example 25), 75% phosphoric acid aqueous solution (Example 26), and 85% phosphoric acid aqueous solution (Example 27) were added to the obtained polymer solution to obtain a reaction solution, which was stirred in air at room temperature for 24 hours. The reaction solution was cooled in an ice bath, and 5M NaOH (0.98 molar equivalent to the phosphoric acid added) was added little by little to neutralize the acid, and then 1 ml of 1M H 3 PO 4 The neutralized solution was dialyzed against Milli-Q water and then lyophilized.

[0124] The resulting powder was analyzed by GPC in the same manner as in Example 4. The results of GPC (RI detector, UV detector) are shown in Figure 28. Since no peak was observed at the exclusion limit (elution time 16.5 minutes) in Figure 28, it was confirmed that the tert-butyl group of PEG-b-PGlu(OtBu) was deprotected, and since the generation of a peak was suppressed after the elution time of 28 minutes, the by-production of sodium polyglutamate (homopolymer) was suppressed. In Examples 25, 26, and 27, no significant difference was observed in the results of GPC analysis even when the concentration of phosphoric acid was changed in the range of 60% to 85%.

[0125] [Examples 28, 29, 30, and 31] (Deprotection of tert-butyl group) To examine the effect of temperature, the following experiment was carried out. 5 mg of PEG-b-PGlu(OtBu) obtained in Example 1 was dissolved in 0.5 ml of acetonitrile to obtain a polymer solution. 0.5 ml of 85% aqueous phosphoric acid was added to the obtained polymer solution to obtain a reaction solution, which was stirred in air at 4°C (Example 28), 25°C (Example 29), 40°C (Example 30), or 60°C (Example 31) for 24 hours. The reaction solution was cooled in an ice bath, and 5M NaOH (0.98 molar equivalent to the phosphoric acid added) was added little by little to neutralize the acid, followed by adding 1 ml of 1M H3 PO 4 The neutralized solution was dialyzed against Milli-Q water and then lyophilized.

[0126] The resulting powder was analyzed by GPC in the same manner as in Example 4. The results of GPC (RI detector, UV detector) are shown in Figure 29. Since no peak was observed at the exclusion limit (elution time 16.5 minutes) in Figure 29, it was confirmed that the tert-butyl group of PEG-b-PGlu(OtBu) was deprotected, and since the generation of a peak was suppressed after the elution time of 28 minutes, the by-production of sodium polyglutamate (homopolymer) was suppressed. Furthermore, in Examples 28, 29, 30, and 31, no significant difference was observed in the results of GPC analysis even when the temperature was changed within the range of 4 to 60°C.

Claims

1. The copolymer (X) containing the repeating unit (a) represented by the following general formula (1) has -COOR in the repeating unit (a) represented by the general formula (1): 1 R that constitutes 1 in the presence of an acid having an acid dissociation constant (pKa) (25° C.) of 0 or more to convert it into a carboxy group or a salt thereof, The acid having an acid dissociation constant (pKa) (25° C.) of 0 or more is phosphoric acid, the deprotection is carried out in the presence of water or in the presence of water and an organic solvent; The method for producing a copolymer (Y) having a carboxy group or a salt thereof, wherein the organic solvent is at least one organic solvent selected from the group consisting of acetonitrile, hexane, toluene, xylene, acetone, tetrahydrofuran, diethyl ether, and chloroform. 【Chemistry 1】 (In the general formula (1), R 1 is a tertiary alkyl group having 4 to 7 carbon atoms; R 2 is an alkylene group having 1 to 4 carbon atoms.

2. The deprotection is carried out in the presence of water and an organic solvent; The method for producing a copolymer (Y) having a carboxy group or a salt thereof according to claim 1 , wherein the organic solvent is acetonitrile.

3. R in the general formula (1) 1 The method for producing a copolymer (Y) having a carboxy group or a salt thereof according to claim 1 or 2, wherein is a tert-butyl group.

4. R in the general formula (1) 2 The method for producing a copolymer (Y) having a carboxy group or a salt thereof according to any one of claims 1 to 3, wherein is a methylene group or an ethylene group.

5. A method for producing a copolymer (Y) having a carboxy group or a salt thereof according to any one of claims 1 to 4, wherein the copolymer (X) is a block copolymer, a random copolymer, or a graft copolymer.

6. A method for producing a copolymer (Y) having a carboxy group or a salt thereof according to any one of claims 1 to 5, wherein the copolymer (X) is a block copolymer and has a polymer block (A) containing a repeating unit (a) represented by the general formula (1).

7. The copolymer (X) has a polymer block (B), 7. The method for producing a copolymer (Y) having a carboxy group or a salt thereof according to claim 6, wherein the polymer block (B) is formed of a polymer selected from polyethylene glycol, polypropylene glycol, polyglycerin, polyvinyl alcohol, polyvinylpyrrolidone, polyacrylamide, poly[N-(2-hydroxypropyl)methacrylamide], divinyl ether-maleic anhydride copolymer, poly(2-methyl-2-oxazoline), poly(2-ethyl-2-oxazoline), polyphosphazene, and poly(2-methacryloyloxyethylphosphorylcholine).

8. The method for producing a copolymer (Y) having a carboxy group or a salt thereof according to claim 7, wherein the polymer block (B) is formed of polyethylene glycol.

9. The method for producing a copolymer (Y) having a carboxy group or a salt thereof according to claim 1, wherein the copolymer (X) is a random copolymer.

10. The method for producing the copolymer (Y) having a carboxy group or a salt thereof according to claim 9, which has a repeating unit (excluding the repeating unit (a)) derived from at least one monomer selected from amino acids and amino acid derivatives.

11. A method for producing a copolymer (X) containing a repeating unit (a) represented by the general formula (1), comprising a step (α) of polymerizing a monomer represented by the following general formula (1'): 【Chemistry 2】 (In general formulas (1') and (1), R 1 is a tertiary alkyl group having 4 to 7 carbon atoms; R 2 is an alkylene group having 1 to 4 carbon atoms.

12. The copolymer (X) is a block copolymer, The method for producing a copolymer (Y) having a carboxy group or a salt thereof according to claim 11, wherein the step (α) is carried out in the presence of a macroinitiator.

13. The method for producing a copolymer (Y) having a carboxy group or a salt thereof according to claim 12, wherein the macroinitiator is a macroinitiator having a polymer in its molecule selected from polyethylene glycol, polypropylene glycol, polyglycerin, polyvinyl alcohol, polyvinylpyrrolidone, polyacrylamide, poly[N-(2-hydroxypropyl)methacrylamide], divinyl ether-maleic anhydride copolymer, poly(2-methyl-2-oxazoline), poly(2-ethyl-2-oxazoline), polyphosphazene, and poly(2-methacryloyloxyethyl phosphorylcholine).

14. The copolymer (X) is a random copolymer, The method for producing the copolymer (Y) having a carboxy group or a salt thereof according to claim 11, wherein the step (α) is carried out in the presence of at least one monomer selected from amino acids and amino acid derivatives (excluding the monomer represented by general formula (1')).

Citation Information

Patent Citations

  • Intermediate for thymosin alpha 1 and desacetylthymosin alph1

    JP1984205348A

  • Production of block copolymer, block copolymer and water-soluble polymeric carcinostatic agent

    JP1993117385A

  • Polymeric carrier

    JP1994206832A

  • Production method of copolymer-1

    JP2009504885A

  • Method for producing poly-α-glutamic acid and its derivatives

    JP2009540071A