Polyarylene sulfide resin composition
A sea-island structured resin composition with polyarylene sulfide and polycarbonate resins, glass fibers, and a reactive compound addresses burr issues, enhancing mechanical strength and heat resistance for diverse applications.
Patent Information
- Application Number
- JP2020132327
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-08-04
- Publication Date
- 2024-10-02
- Estimated Expiration
- 2040-08-04
AI Technical Summary
Polyarylene sulfide resins generate burrs during molding due to impurities like sodium and chlorine, leading to decomposition of polycarbonate resin and inadequate mechanical and heat resistance in existing resin compositions.
A sea-island structure is formed with polyarylene sulfide resin as the continuous phase and polycarbonate resin as the dispersed phase, incorporating glass fibers and a compound with a reactive functional group to enhance mechanical strength and heat resistance while minimizing burrs.
The resin composition maintains excellent mechanical strength, heat resistance, and low burr properties, suitable for various industrial applications.
Smart Images

Figure 0007560289000006 
Figure 0007560289000007 
Figure 0007560289000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a resin composition which comprises a polyarylene sulfide resin, a polycarbonate resin, a compound having a reactive functional group, and glass fibers, which forms a sea-island structure in which the polyarylene sulfide resin is the continuous phase and the polycarbonate resin is the dispersed phase, and which has a morphology in which the glass fibers are dispersed only in the polyarylene sulfide resin continuous phase, and which has excellent mechanical strength, heat resistance, and low burrs while retaining the excellent properties of the polyarylene sulfide resin. [Background technology]
[0002] Polyarylene sulfide resin is an engineering plastic that is excellent in chemical resistance, heat resistance, mechanical properties, etc. For this reason, polyarylene sulfide resin is widely used as electric and electronic parts, vehicle-related parts, aircraft parts, and housing equipment parts. However, polyarylene sulfide resin has a problem that burrs are generated during molding processing. As a means to solve this problem, Patent Document 1 discloses a resin composition containing polyphenylene sulfide resin and polycarbonate resin. However, conventionally available commercially available polyphenylene sulfide resins contain a certain amount of sodium as an impurity due to the constraints of the polymer polymerization method, so that the polycarbonate resin is significantly decomposed during molding processing, and excellent properties have not been expressed. Patent Documents 2 and 3 propose polyphenylene sulfide resins with reduced chlorine content. However, the decomposition of the polycarbonate resin cannot be suppressed by only using this polyphenylene sulfide resin with reduced chlorine content. In addition, the reaction process becomes complicated in order to reduce the chlorine content, and the cost competitiveness is poor. Patent Document 4 discloses a polyphenylene sulfide resin with reduced alkali metals, but it is not intended to be modified with polycarbonate resin and is inferior in cost competitiveness. Patent Document 5 discloses a resin composition containing a polyphenylene sulfide resin with a dispersity of 2.5 or less and an alkali metal content of 50 ppm or less and a thermoplastic resin. However, it is not intended to modify with polycarbonate resin, particularly to suppress burrs, and the characteristics are not satisfactory. Furthermore, Patent Document 6 discloses a resin composition containing a polyphenylene sulfide resin and a polycarbonate resin in which decomposition of the polycarbonate resin is suppressed, but the mechanical strength and heat resistance of the resin composition are insufficient. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] Japanese Patent Application Publication No. 51-59952 [Patent Document 2] JP 2010-70656 A [Patent Document 3] JP 2013-181044 A [Patent Document 4] JP 2008-231250 A [Patent Document 5] JP 2008-231249 A [Patent Document 6] JP 2015-30779 A Summary of the Invention [Problem to be solved by the invention]
[0004] An object of the present invention is to provide a polyarylene sulfide resin composition which has excellent mechanical strength, heat resistance and low burr while retaining the excellent properties of polyarylene sulfide resins. [Means for solving the problem]
[0005] As a result of intensive research, the present inventors have found that a resin composition which comprises a polyarylene sulfide resin, a polycarbonate resin, a compound having a reactive functional group, and glass fibers, which forms a sea-island structure in which the polyarylene sulfide resin is the continuous phase and the polycarbonate resin is the dispersed phase, and which has a morphology in which the glass fibers are dispersed only in the polyarylene sulfide resin continuous phase, has excellent mechanical strength, heat resistance and low burrs while retaining the excellent properties of the polyarylene sulfide resin, and have arrived at the present invention.
[0006] Specifically, the above-mentioned object is achieved by a resin composition containing 100 parts by weight in total of (A) polyarylene sulfide resin (component A) and (B) polycarbonate resin (component B), 0.001 to 10 parts by weight of (C) a compound having a reactive functional group (component C) and 10 to 350 parts by weight of (D) glass fiber (component D), wherein the resin composition forms a sea-island structure in which the polyarylene sulfide resin is the continuous phase and the polycarbonate resin is the dispersed phase, and has a morphology in which the glass fiber is dispersed only in the polyarylene sulfide resin continuous phase.
[0007] The present invention will be described in detail below.
[0008] (Component A: polyarylene sulfide resin) As the polyarylene sulfide resin used as component A in the present invention, any resin may be used so long as it belongs to the category called polyarylene sulfide resin.
[0009] The polyarylene sulfide resin may be composed of, for example, a p-phenylene sulfide unit, an m-phenylene sulfide unit, an o-phenylene sulfide unit, a phenylene sulfone unit, a phenylene sulfide ketone unit, a phenylene sulfide ether unit, a diphenylene sulfide unit, a phenylene sulfide unit containing a substituent, a phenylene sulfide unit containing a branched structure, or the like, as its constituent units. Among these, those containing 70 mol % or more, particularly 90 mol % or more of p-phenylene sulfide units are preferred, and poly(p-phenylene sulfide) is more preferred.
[0010] The total chlorine content of the polyarylene sulfide resin used as component A of the present invention is preferably 500 ppm or less, more preferably 450 ppm or less, further preferably 300 ppm or less, and particularly preferably 50 ppm or less. If the total chlorine content exceeds 500 ppm, the amount of gas generated increases, mold deposits increase, and releasability may deteriorate.
[0011] The total sodium content of the polyarylene sulfide resin used as the A component of the present invention is preferably 39 ppm or less, more preferably 30 ppm or less, even more preferably 10 ppm or less, and particularly preferably 8 ppm or less. If it exceeds 39 ppm, not only the physical properties are reduced due to the promotion of decomposition of the resin, but also the moisture and heat resistance may be reduced due to the increase in the water absorption of the resin caused by the coordinate bond between sodium metal and water molecules under high temperature and high humidity conditions. The total sodium content was measured by ICP atomic emission spectrometry (ICP-AES method).
[0012] The polyarylene sulfide resin used as component A of the present invention preferably has a polydispersity (Mw / Mn) expressed by the weight average molecular weight (Mw) and the number average molecular weight (Mn) of 2.7 or more, more preferably 2.8 or more, and even more preferably 2.9 or more. If the polydispersity is less than 2.7, there may be a large amount of burrs generated during molding. The upper limit of the polydispersity (Mw / Mn) is not particularly specified, but it is preferably 10 or less. Here, the weight average molecular weight (Mw) and the number average molecular weight (Mn) are values calculated in terms of polystyrene by gel permeation chromatography (GPC). 1-chloronaphthalene was used as the solvent, and the column temperature was set to 210°C.
[0013] The method for producing the polyarylene sulfide resin is not particularly limited, and polymerization can be performed by a known method, but particularly suitable polymerization methods include those described in U.S. Patent Nos. 4,746,758 and 4,786,713, JP-A-2013-522385, JP-A-2012-233210, and JP-A-5167276, etc. These production methods involve directly heating a diiodoaryl compound and solid sulfur without a polar solvent to polymerize them.
[0014] The method includes an iodization step and a polymerization step. In the iodization step, an aryl compound is reacted with iodine to obtain a diiodoaryl compound. In the subsequent polymerization step, the diiodoaryl compound is polymerized with solid sulfur using a polymerization terminator to produce a polyarylene sulfide resin. Iodine is generated in gas form in this step, which is recovered and reused in the iodization step. Iodine is essentially a catalyst.
[0015] A representative example of solid sulfur used in the above-mentioned preparation method is cyclooctasulfur (S8) in which eight atoms are linked at room temperature. However, the sulfur compound used in the polymerization reaction is not limited, and any form that is solid or liquid at room temperature can be used.
[0016] Representative diiodoaryl compounds used in the above-mentioned production method include at least one selected from the group consisting of diiodobenzene, diiodonaphthalene, diiodobiphenyl, diiodobisphenol, and diiodobenzophenone. Also, derivatives of iodoaryl compounds to which an alkyl group or a sulfone group is bonded, or to which oxygen or nitrogen is introduced, are used. Iodoaryl compounds are classified into different isomers depending on the bonding position of the iodine atom, and preferred examples of these isomers are compounds in which iodine is symmetrically located at both ends of the molecule of the aryl compound, such as p-diiodobenzene, 2,6-diiodonaphthalene, and p,p'-diiodobiphenyl. The content of the iodoaryl compound is preferably 500 to 10,000 parts by weight based on 100 parts by weight of the solid sulfur. This amount is determined in consideration of the formation of disulfide bonds.
[0017] Representative examples of polymerization terminators used in the above-mentioned production method include monoiodoaryl compounds, benzothiazoles, benzothiazole sulfenamides, thiurams, dithiocarbamates, and aromatic sulfide compounds. Preferred examples of monoiodoaryl compounds include at least one selected from the group consisting of iodobiphenyl, iodophenol, iodoaniline, and iodobenzophenone. Preferred examples of benzothiazoles include at least one selected from the group consisting of 2-mercaptobenzothiazole and 2,2'-dithiobisbenzothiazole. Preferred examples of benzothiazole sulfenamides include at least one selected from the group consisting of N-cyclohexylbenzothiazole 2-sulfenamide, N,N-dicyclohexyl-2-benzothiazole sulfenamide, 2-morpholinothiobenzothiazole, benzothiazole sulfenamide, dibenzothiazole disulfide, and N-dicyclohexylbenzothiazole 2-sulfenamide. A preferred example of the thiurams is at least one selected from the group consisting of tetramethylthiuram monosulfide and tetramethylthiuram disulfide. A preferred example of the dithiocarbamates is at least one selected from the group consisting of zinc dimethyldithiocarbamate and zinc diethyldithiocarbamate. A preferred example of the aromatic sulfide compounds is at least one selected from the group consisting of diphenyl sulfide, diphenyl disulfide, diphenyl ether, biphenyl, and benzophenone. In any of the polymerization terminators, one or more functional groups may be substituted on the conjugated aromatic ring skeleton. Examples of the functional groups include hydroxyl groups, carboxyl groups, mercapto groups, and the like. Examples of the groups include a carboxyl group and an amino group. Examples of the groups that are more preferred are those that have a wavelength of 1600 to 1800 cm in the FT-IR spectrum. -1 or 3300~3500cm -1The content of the polymerization terminator is preferably 1 to 30 parts by weight based on 100 parts by weight of the solid sulfur. This amount is determined taking into consideration the formation of disulfide bonds.
[0018] In addition, as the polyarylene sulfide resin used as the A component of the present invention, a polyarylene sulfide resin having a reactive functional group at the end, such as a carboxyl group, a carboxyl group derivative group, a thiol group, a sulfone group, a hydroxyl group, an amino group, an epoxy group, a mercapto group, a cyano group, or a nitro group, can be used for the purpose of obtaining a higher compatibility. By using a polyarylene sulfide resin having the reactive functional group at the end, it is possible to obtain a resin composition that exhibits excellent compatibility with other polymer materials and carbon fibers, has excellent peelability, and has higher mechanical strength. A more preferred example of the polyarylene sulfide resin having the reactive functional group at the end is a polyarylene sulfide resin having at least one type of end group structure selected from a carboxyl group and an amino group. The polyarylene sulfide resin having at least one type of end group structure selected from a carboxyl group and an amino group is a polyarylene sulfide resin having a carboxyl group-derived peak at about 1600 to 1800 cm in the FT-IR spectrum of FT-IR spectroscopy. -1 Or, amino group-derived 3300-3500 cm -1 and 1400-1600 cm -1 When the height intensity of the aromatic ring stretching peak appearing at about 1600 to 1800 cm is taken as 100%, -1 Or about 3300~3500cm -1 The relative height intensity of the peak is 0.001 to 10%.
[0019] A particularly preferred example of the polyarylene sulfide resin having at least one type of end group structure selected from a carboxyl group and an amino group is a polyarylene sulfide resin having a carboxyl group end group structure, which is represented by a structural unit represented by the following general formula (1).
[0020] [ka] (In the formula, Ar is an arylene group, and n is the number of repeating units.)
[0021] Here, the arylene group can be a p-phenylene group, an m-phenylene group, an o-phenylene group, a substituted phenylene group, etc. Specifically, the substituted phenylene group is a phenylene group optionally substituted with one or more of F, Cl, Br, C1-C3 alkyl, trifluoromethyl, C1-C3 alkoxy, trifluoromethoxy, trifluoromethylthio, dimethylamino, cyano, (C1-C3 alkyl)SO2-, (C1-C3 alkyl)NHSO2-, (C1-C3 alkyl)2NSO2-, and NH2SO2-.
[0022] The method of introducing the reactive functional group into the polyarylene sulfide resin is not particularly limited, and the resin is polymerized by a known method, but a method of using a polymerization terminator having one or more groups represented by general formula (2) on a conjugated aromatic ring skeleton is exemplified. Examples of the conjugated aromatic ring skeleton used in the polymerization terminator include diphenyl disulfide, monoiodobenzene, thiophenol, 2,2'-dibenzothiazolyl disulfide, 2-mercaptobenzothiazole, N-cyclohexyl-2-benzothiazolyl sulfenamide, 2-(morpholinothio)benzothiazole, and N,N'-dicyclohexyl-1,3-benzothiazole-2-sulfenamide.
[0023] [ka] (wherein R is a hydrogen atom or an alkali metal atom).
[0024] A suitable polymerization method for producing a polyarylene sulfide resin having a terminal group structure of a carboxyl group includes a step of polymerizing a diiodo aromatic compound and a reactant containing sulfur element, and a production method in which a compound having a carboxyl group is added while the polymerization reaction step is proceeding to substitute the terminal group of the polyarylene sulfide main chain with a carboxyl group. A representative example of the compound having a carboxyl group is at least one selected from the group consisting of 2-iodobenzoic acid, 3-iodobenzoic acid, 4-iodobenzoic acid, and 2,2'-dithiobenzoic acid. The compound having a carboxyl group can be added in an amount of about 0.0001 to 5 parts by weight based on 100 parts by weight of the diiodo aromatic compound.
[0025] In the above-mentioned production method, a polymerization catalyst may be used, and a representative example of the polymerization catalyst is a nitrobenzene-based catalyst. A preferred example of the nitrobenzene-based catalyst is at least one selected from the group consisting of 1,3-diiodo-4-nitrobenzene, 1-iodo-4-nitrobenzene, 2,6-diiodo-4-nitrophenol, iodonitrobenzene, and 2,6-diiodo-4-nitroamine. The content of the polymerization catalyst is preferably 0.01 to 20 parts by weight based on 100 parts by weight of the solid sulfur. This amount is determined in consideration of the formation of disulfide bonds.
[0026] A typical example of the reaction conditions for this production method is to proceed for 1 to 30 hours while increasing the temperature and decreasing the pressure from initial reaction conditions of 180 to 250°C temperature and 50 to 450 Torr (6.7 to 60 kPa) to final reaction conditions of 270 to 350°C temperature and 0.001 to 20 Torr (0.00013 to 2.7 kPa). Preferably, the initial reaction conditions are a temperature of 180°C or higher and a pressure of 450 Torr (60 kPa) or lower, taking into account the reaction rate, and the final reaction conditions are a temperature of 350°C or lower and a pressure of 20 Torr (2.7 kPa) or lower, taking into account the thermal decomposition of the polymer.
[0027] However, the polymerization reaction conditions depend on the structural design and production rate of the reactor, and are known to those skilled in the art, so they are not particularly limited. The reaction conditions can be appropriately set by those skilled in the art in consideration of the process conditions.
[0028] By using this polymerization method, it is not necessary to substantially reduce the sodium content, and a polyphenylene sulfide resin excellent in cost performance can be obtained.
[0029] The polyphenylene sulfide resin of the present invention may also contain polyphenylene sulfide resins obtained by other polymerization methods.
[0030] (B component: polycarbonate resin) The polycarbonate resin used in the present invention is obtained by reacting a dihydric phenol with a carbonate precursor. Examples of reaction methods include interfacial polymerization, melt transesterification, solid-phase transesterification of carbonate prepolymers, and ring-opening polymerization of cyclic carbonate compounds, but the melt transesterification method is preferred. The polycarbonate resin may also be a branched polycarbonate resin obtained by polymerizing trifunctional phenols, or may be a copolymerized polycarbonate obtained by copolymerizing an aliphatic dicarboxylic acid, an aromatic dicarboxylic acid, or a divalent aliphatic or alicyclic alcohol.
[0031] The viscosity average molecular weight of the polycarbonate resin is preferably 1.3×10 4 ~4.0×10 4 , more preferably 1.5×10 4 ~3.8×10 4 The viscosity average molecular weight (M) of aromatic polycarbonate resin is calculated by the specific viscosity (η sp ) into the following formula. Details of such polycarbonate resins are described in JP-A-2002-129003. η sp / c=[η]+0.45×[η]2 c (where [η] is the intrinsic viscosity) [η]=1.23×10 -4 M 0.83 c=0.7
[0032] The polycarbonate resin used in the present invention may be any of various polycarbonate resins having high heat resistance or low water absorption rate polymerized using other dihydric phenols other than the commonly used bisphenol A polycarbonate. Specific examples of various polycarbonate resins having high heat resistance or low water absorption rate polymerized using other dihydric phenols include the following.
[0033] (1) A copolymer polycarbonate in which, based on 100 mol % of dihydric phenol components constituting the polycarbonate, 4,4'-(m-phenylenediisopropylidene)diphenol (hereinafter abbreviated as "BPM") components account for 20 to 80 mol % (more preferably 40 to 75 mol %, and even more preferably 45 to 65 mol %) and 9,9-bis(4-hydroxy-3-methylphenyl)fluorene (hereinafter abbreviated as "BCF") components account for 20 to 80 mol % (more preferably 25 to 60 mol %, and even more preferably 35 to 55 mol %).
[0034] (2) A copolymer polycarbonate in which, relative to 100 mol % of the dihydric phenol components constituting the polycarbonate, the bisphenol A component is 10 to 95 mol % (more preferably 50 to 90 mol %, and even more preferably 60 to 85 mol %) and the BCF component is 5 to 90 mol % (more preferably 10 to 50 mol %, and even more preferably 15 to 40 mol %).
[0035] (3) A copolymer polycarbonate in which the BPM component is 20 to 80 mol % (more preferably 40 to 75 mol %, even more preferably 45 to 65 mol %) and the 1,1-bis(4-hydroxyphenyl)-3,3,5-trimethylcyclohexane component is 20 to 80 mol % (more preferably 25 to 60 mol %, even more preferably 35 to 55 mol %) out of 100 mol % of the dihydric phenol component constituting the polycarbonate. These special polycarbonates may be used alone or in a suitable mixture of two or more kinds. They may also be used in a mixture with a commonly used bisphenol A type polycarbonate. The production methods and properties of these special polycarbonates are described in detail in, for example, JP-A-6-172508, JP-A-8-27370, JP-A-2001-55435, and JP-A-2002-117580. Furthermore, it is also possible to use a polycarbonate-polyorganosiloxane copolymer in which a polyorganosiloxane unit is copolymerized.
[0036] Polycarbonate resin can be produced not only from virgin raw materials, but also from polycarbonate resin recycled from used products, such as containers such as water bottles, optical disks, and automobile headlamps.
[0037] The content of component B is preferably 1 to 50 parts by weight, more preferably 5 to 45 parts by weight, and even more preferably 5 to 40 parts by weight, per 100 parts by weight of the total of components A and B. If the content is less than 1 part by weight, the characteristics of the polycarbonate resin may not be expressed, and the generation of burrs may not be suppressed. Also, a sea-island structure in which the polyarylene sulfide resin is the continuous phase and the polycarbonate resin is the dispersed phase may not be formed. On the other hand, if the content is more than 50 parts by weight, the polyphenylene In some cases, the characteristics of the polyarylene sulfide resin will not be expressed, resulting in a decrease in mechanical strength and deterioration of heat resistance. Also, a sea-island structure in which the polyarylene sulfide resin is the continuous phase and the polycarbonate resin is the dispersed phase may not be formed.
[0038] (Component C: Compound having a reactive functional group) The resin composition of the present invention contains a compound having a reactive functional group as component C. The compound having a reactive functional group used in the present invention is preferably a compound represented by the following general formula (3).
[0039] [ka]
[0040] (In formula (3), R 1 R is a hydrocarbon group or an organosilicon group containing up to 20 carbon atoms, having at least one sulfur atom in the molecule, and having a reactive functional group containing at least one group selected from the group consisting of a thiol group, a carboxyl group, a hydroxyl group, an epoxy group, and an amino group. 2 is a hydrogen atom, or a hydrocarbon group or an organosilicon group containing up to 20 carbon atoms, having at least one sulfur atom in the molecule, containing a thiol group or a disulfide group, and having a reactive functional group containing at least one group selected from the group consisting of a carboxyl group, a hydroxyl group, an epoxy group, and an amino group.
[0041] Examples of compounds having a reactive functional group include 2-mercaptobenzoic acid, 3-mercaptobenzoic acid, 4-mercaptobenzoic acid, thioglycolic acid, thiolactic acid, 2-mercaptoaniline, 3-mercaptoaniline, 4-mercaptoaniline, 2-mercaptopyridine, 4-mercaptopyridine, 2-mercaptobenzothiazole, 3-mercaptopropyltrimethoxysilane, 2,2'-dithiodibenzoic acid, dithioglycolic acid, thiolactic acid, 2-mercaptoaniline, 3-mercaptoaniline, 4-mercaptoaniline, 2-mercaptopyridine, 4-mercaptopyr ...thioglycolic acid, thiolactic acid, thiolactic acid, thioglycolic acid, thiolactic acid, thiolactic acid, thioglycolic acid, thiolactic acid, thiolactic acid, thioglycolic acid, thiolactic acid, thiolactic acid, thioglycolic acid, thiolactic acid, thiolactic acid, thioglycolic acid, thiolactic acid, thiolactic acid, thioglycolic acid, thiolactic acid, thioglycolic acid, thiolactic acid, thioglycolic acid, thiolactic acid, thioglycolic acid, thiolactic acid, thioglycolic acid, thiolactic acid, thioglycolic acid, thiolactic acid, thioglyc Examples of suitable compounds include cholic acid, α,α'-dithiodilactic acid, β,β'-dithiodilactic acid, 2,2'-dithiodianiline, 3,3'-dithiodianiline, 4,4'-dithiodianiline, 3,3'-dithiodipyridine, 2,2'-dithiobis(benzothiazole), 2,2'-dithiobis(benzimidazole), 2,2'-dithiobis(benzoxazole), and 2-(4'-morpholinodithio)benzothiazole. If a compound containing a sulfur atom that does not have a reactive functional group is used, the viscosity of the resin decreases and flashing worsens.
[0042] The content of component C is 0.001 to 10 parts by weight, preferably 0.005 to 5 parts by weight, and more preferably 0.05 to 1 part by weight, relative to 100 parts by weight of the total of components A and B. If the content of component C is less than 0.001 part by weight, the morphology in which glass fibers are dispersed only in the polyarylene sulfide resin continuous phase will not be obtained, and mechanical strength and heat resistance will be poor, whereas if the content exceeds 10 parts by weight, the mechanical strength will decrease, the resin will be plasticized, and burrs will worsen.
[0043] (D component: glass fiber) The glass fiber used in the present invention is not particularly limited to a glass composition such as A glass, C glass, E glass, etc., and may contain components such as TiO2, SO3, P2O5, etc., depending on the case. However, E glass (alkali-free glass) is more preferable when blended with a thermoplastic resin. Furthermore, it is possible to use two or more of these glass fibers in combination. Glass fiber is obtained by quenching molten glass while stretching it by various methods, and forming it into a predetermined fiber shape or milled shape. The quenching and stretching conditions in such cases are not particularly limited. In addition to a perfect circle, the cross-sectional shape may be an ellipse, a cocoon shape, a trefoil shape, or any other shape other than a perfect circle. Furthermore, a combination of a perfect circle glass fiber and a glass fiber with a shape other than a perfect circle may be used. The glass fibers may be a mixture of fibers. Among these, circular glass fibers are more preferable. In addition, it is preferable to pretreat these glass fibers with coupling agents such as isocyanate compounds, organic silane compounds, organic titanate compounds, organic borane compounds, and epoxy compounds, or with organic onium ions in the case of swellable layered silicates, in order to obtain better mechanical strength. The glass fibers used in the present invention preferably have a diameter (D) of 6 to 13 μm, a cut length (L) of 30 μm to 9 mm, and an L / D of 2.3 to 1500.
[0044] The content of component D is 10 to 350 parts by weight, preferably 20 to 300 parts by weight, and more preferably 60 to 200 parts by weight, per 100 parts by weight of the total of components A and B. If the content of component D is less than 10 parts by weight, the mechanical strength and heat resistance are poor and flashing is also increased. If it exceeds 350 parts by weight, the moldability is reduced.
[0045] (Other Ingredients) The resin composition of the present invention may contain a filler component other than component D, provided that the effect of the present invention is not impaired. Suitable filler components are not particularly limited, and may be fibrous, plate-like, powdery, granular, or other reinforcing materials. Specific examples include inorganic fibers such as wollastonite, carbon fiber, potassium titanate whisker, zinc oxide whisker, alumina fiber, silicon carbide fiber, ceramic fiber, asbestos fiber, gypsum fiber, and metal fiber, and organic fibers such as fully aromatic polyamide fiber, with wollastonite, carbon fiber, and fully aromatic polyamide fiber being preferred. Other examples include silicates such as sericite, kaolin, mica, clay, bentonite, asbestos, talc, alumina silicate, swellable layered silicates such as montmorillonite and synthetic mica, metal compounds such as alumina, silicon oxide, magnesium oxide, zirconium oxide, titanium oxide, and iron oxide, carbonates such as magnesium carbonate and dolomite, sulfates such as calcium sulfate and barium sulfate, glass flakes, glass beads, ceramic beads, boron nitride, silicon carbide, calcium phosphate, and silica, and glass flakes, mica, talc, and glass beads are preferably used. These may be hollow, and two or more of these reinforcing materials may be used in combination.
[0046] In addition, it is preferable to pre-treat these reinforcing materials with a coupling agent such as an isocyanate compound, an organic silane compound, an organic titanate compound, an organic borane compound or an epoxy compound, or with an organic onium ion in the case of a swellable layered silicate, in order to obtain better mechanical strength.
[0047] A conductive filler can be used as a reinforcing material to impart electrical conductivity to the resin composition of the present invention. The conductive filler is not particularly limited as long as it is a conductive filler that is usually used to make resins conductive, and specific examples thereof include metal powder, metal flakes, metal ribbons, metal fibers, metal oxides, inorganic fillers coated with conductive substances, carbon powder, graphite, carbon fibers, carbon flakes, and scaly carbon. Specific examples of the metal species of the metal powder, metal flakes, and metal ribbons include silver, nickel, copper, zinc, aluminum, stainless steel, iron, brass, chromium, and tin. Specific examples of the metal species of the metal fibers include iron, copper, stainless steel, aluminum, and brass. Such metal powder, metal flakes, metal ribbons, and metal fibers may be surface-treated with a titanate-based, aluminum-based, silane-based, or other surface treatment agent.
[0048] Specific examples of metal oxides include SnO2 (antimony doped), In2O3 (antimony doped), ZnO (aluminum doped), etc., which may be surface-treated with a surface treatment agent such as a titanate-based, aluminum-based, or silane-based coupling agent.
[0049] Specific examples of the conductive material in the inorganic filler coated with a conductive material include aluminum, nickel, silver, carbon, SnO2 (antimony doped), and In2O3 (antimony doped). Examples of the inorganic filler to be coated include mica, glass beads, glass fibers, carbon fibers, potassium titanate whiskers, barium sulfate, zinc oxide, titanium oxide, aluminum borate whiskers, zinc oxide whiskers, titanate whiskers, and silicon carbide whiskers. Coating methods include vacuum deposition, sputtering, electroless plating, and baking. These may also be surface-treated with a surface treatment agent such as a titanate-based, aluminum-based, or silane-based coupling agent.
[0050] Carbon powders are classified according to their raw materials and manufacturing methods into acetylene black, gas black, oil black, naphthalene black, thermal black, furnace black, lamp black, channel black, roll black, disc black, etc. The carbon powders that can be used in the present invention are not particularly limited in terms of their raw materials and manufacturing methods, but acetylene black and furnace black are particularly preferably used.
[0051] The resin composition of the present invention may contain an elastomer component within a range that does not impair the effects of the present invention. Suitable elastomer components include core-shell graft copolymer resins such as acrylonitrile-butadiene-styrene copolymers (ABS resins), methyl methacrylate-butadiene-styrene copolymers (MBS resins), and silicone-acrylic composite rubber graft copolymers, or thermoplastic elastomers such as silicone thermoplastic elastomers, olefin thermoplastic elastomers, polyamide thermoplastic elastomers, polyester thermoplastic elastomers, and polyurethane thermoplastic elastomers.
[0052] The resin composition of the present invention may contain other thermoplastic resins within the range that does not impair the effects of the present invention. Examples of other thermoplastic resins include general-purpose plastics such as polyethylene resins, polypropylene resins, and polyalkyl methacrylate resins, engineering plastics such as polyphenylene ether resins, polyacetal resins, aromatic polyester resins, liquid crystal polyester resins, polyamide resins, cyclic polyolefin resins, and polyarylate resins (amorphous polyarylate, liquid crystal polyarylate), and so-called super engineering plastics such as polytetrafluoroethylene, polyether ether ketone, polyetherimide, polysulfone, and polyether sulfone.
[0053] The resin composition of the present invention may contain antioxidants and heat stabilizers (hindered phenols, hydroquinones, phosphites, and their substituted derivatives, etc.), weathering agents (resorcinols, salicylates, benzotriazoles, benzophenones, hindered amines, etc.), release agents and lubricants (montanic acid and its metal salts, its esters, its half esters, stearyl alcohol, stearamide, various bisamides, bisureas, polyethylene wax, etc.), pigments (cadmium sulfide, phthalocyanine, carbon black, etc.), dyes (nigrosine, etc.), crystal nucleating agents (talc, silica, kaolin, clay, etc.), plasticizers (p-octyl ether, ethyl ether, butyl ... and the like), antistatic agents (alkyl sulfate-type anionic antistatic agents, quaternary ammonium salt-type cationic antistatic agents, nonionic antistatic agents such as polyoxyethylene sorbitan monostearate, betaine-type amphoteric antistatic agents, etc.), flame retardants (red phosphorus, phosphate esters, melamine cyanurate, hydroxides such as magnesium hydroxide and aluminum hydroxide, ammonium polyphosphate, brominated polystyrene, brominated polyphenylene ether, brominated polycarbonate, brominated epoxy resin, or combinations of these brominated flame retardants with antimony trioxide, etc.) and other polymers can be added.
[0054] (Production of resin composition) The resin composition of the present invention can be produced by mixing the above-mentioned components simultaneously or in any order using a mixer such as a tumbler, V-type blender, Nauter mixer, Banbury mixer, kneading roll, or extruder. Melt kneading using a twin-screw extruder is preferable, and if necessary, any component is preferably fed into the other melt-mixed components from a second feed port using a side feeder or the like. As the extruder, one having a vent that can degas the moisture in the raw materials and the volatile gas generated from the melt-kneaded resin is preferably used. A vacuum pump is preferably installed from the vent to efficiently discharge the generated moisture and volatile gas to the outside of the extruder. It is also possible to install a screen for removing foreign matter mixed in the extrusion raw materials in a zone before the extruder die section, and to remove foreign matter from the resin composition. Examples of such screens include wire mesh, screen changers, and sintered metal plates (disc filters, etc.).
[0055] The screws used in twin-screw extruders are constructed as a single screw by inserting screw pieces of various shapes between forward flight pieces for transport, combining them in a complex manner, and integrating them together, and examples of such screws include forward flight pieces, forward kneading pieces, reverse kneading pieces, reverse flight pieces, forward flight pieces with notches, and reverse flight pieces, which are arranged in an appropriate order and position in consideration of the characteristics of the raw materials to be processed. Examples of melt kneaders include Banbury mixers, kneading rolls, single-screw extruders, and multi-screw extruders with three or more screws, in addition to twin-screw extruders.
[0056] The resin extruded as described above is directly cut and pelletized, or strands are formed and then the strands are cut by a pelletizer and pelletized. When it is necessary to reduce the influence of external dust during pelletization, it is preferable to purify the atmosphere around the extruder. The shape of the obtained pellets may be a general shape such as a cylinder, a prism, or a sphere, but is more preferably a cylinder. The diameter of such a cylinder is preferably 1 to 5 mm, more preferably 1.5 to 4 mm, and even more preferably 2 to 3.5 mm. On the other hand, the length of the cylinder is preferably 1 to 30 mm, more preferably 2 to 5 mm, and even more preferably 2.5 to 4 mm.
[0057] The total sodium content of the resin composition of the present invention is preferably 39 ppm or less, more preferably 30 ppm or less, even more preferably 10 ppm or less, and particularly preferably 8 ppm or less. If the total sodium content exceeds 39 ppm, the decomposition of the polycarbonate resin cannot be suppressed, and therefore not only is the burr suppression effect of the polycarbonate resin not exhibited, but in more severe cases, pelletization may become difficult.
[0058] The resin composition of the present invention has a morphology in which a sea-island structure is formed in which the polyarylene sulfide resin is the continuous phase and the polycarbonate resin is the dispersed phase, and the glass fiber is dispersed only in the polyarylene sulfide resin continuous phase. If the sea-island structure is not formed in which the polyarylene sulfide resin is the continuous phase and the polycarbonate resin is the dispersed phase, the characteristics of the polyphenylene sulfide resin are not expressed, the mechanical strength is reduced, and the heat resistance is also deteriorated. In addition, if the glass fiber is not dispersed only in the polyarylene sulfide resin continuous phase, the characteristics of the polyphenylene sulfide resin are not expressed, the mechanical strength is reduced, and the heat resistance is also deteriorated.
[0059] (About molded products) Molded articles made of the resin composition of the present invention can be obtained by molding the pellets produced as described above. Preferably, they are obtained by injection molding or extrusion molding. Injection molding includes not only ordinary molding methods, but also injection compression molding, injection press molding, gas-assisted injection molding, foam molding (including a method of injecting a supercritical fluid), insert molding, in-mold coating molding, heat-insulating mold molding, rapid heating and cooling mold molding, two-color molding, multi-color molding, sandwich molding, and ultra-high speed injection molding. Molding can be performed using either a cold runner method or a hot runner method. In addition, extrusion molding can produce various profile extrusion molded products, sheets, films, and the like. Sheets and films can also be molded using an inflation method, a calendar method, a casting method, and the like. Furthermore, it is possible to mold the resin composition of the present invention into a heat-shrinkable tube by applying a specific stretching operation. It is also possible to mold the resin composition of the present invention into a molded article by rotational molding, blow molding, and the like. Effect of the Invention
[0060] The resin composition of the present invention is a resin composition comprising a polyarylene sulfide resin, a polycarbonate resin, a compound having a reactive functional group, and glass fibers, and is a polyarylene sulfide resin composition that has excellent mechanical strength, heat resistance, and low burrs while retaining the excellent properties of the polyarylene sulfide resin. Therefore, the resin composition can be used in a wide range of applications, including: housings for personal computers, tablets, mobile phones, displays, office automation equipment, mobile phones, personal digital assistants, facsimiles, compact discs, portable MDs, portable radio cassettes, PDAs (personal digital assistants such as electronic organizers), video cameras, digital still cameras, optical equipment, audio equipment, air conditioners, lighting equipment, entertainment equipment, toys, and other home appliances, as well as internal members such as trays and chassis of electric and electronic devices, cases thereof, mechanism parts, panels, and other building material applications; motor parts, alternator terminals, alternator connectors, IC regulators, potentiometer bases for light dimmers, suspension parts, various valves such as exhaust gas valves, fuel-related products, various pipes for exhaust systems or intake systems, air intake nozzle snorkels, intake manifolds, various Arms, various frames, various hinges, various bearings, fuel pumps, gasoline tanks, CNG tanks, engine coolant joints, carburetor main bodies, carburetor spacers, exhaust gas sensors, coolant sensors, oil temperature sensors, brake pad wear sensors, throttle position sensors, crankshaft position sensors, air flow meters, brake butt wear sensors, thermostat bases for air conditioners, heating hot air flow control valves, brush holders for radiator motors, water pump impellers, turbine vanes, wiper motor related parts, distributors, starter switches, starter relays, transmission wire harnesses, windshield washer nozzles, air conditioner panel switch boards, coils for fuel-related electromagnetic valves, fuse connectors, battery trays, AT brackets, headlamp supports, pedal housings, handles, door beams, protectors, chassis, frames, armrests, horn terminals, step motor rotors, lamp sockets, lamp reflectors, lamp housings, brake pistons,It is widely useful in automobile and motorcycle related parts, components and outer panels such as noise shields, radiator supports, spare tire covers, seat shells, solenoid bobbins, engine oil filters, ignition device cases, under covers, scuff plates, pillar trims, propeller shafts, wheels, fenders, fascias, bumpers, bumper beams, bonnets, aero parts, platforms, cowl louvers, roofs, instrument panels, spoilers and various modules, and aircraft related parts, components and outer panels such as landing gear pods, winglets, spoilers, edges, rudders, elevators, failings and ribs, wind turbine blades, etc., and is particularly useful in electronic device housings such as computers, notebooks, ultrabooks, tablets, mobile phone housings, inverter housings for hybrid cars and electric cars, etc., and the industrial effects it produces are exceptional. [Brief description of the drawings]
[0061] [Figure 1] 1 is an SEM image of a cross section of a test piece of Example 6. [Diagram 2] 1 is an SEM image of a cross section of a test piece of Comparative Example 3. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0062] The present inventors currently consider the best embodiment of the present invention to be one that embodies the preferred ranges of each of the above-mentioned requirements, and representative examples thereof are described in the following examples, although the present invention is not limited to these embodiments. EXAMPLES
[0063] [Evaluation of resin composition] (1) Mechanical strength evaluation Tensile strength at break was measured according to ISO527-1 and ISO527-2 (measurement condition: 23°C). Test pieces were prepared by drying the pellets in a hot air circulation dryer at 130°C for 6 hours, and then molding the pellets in an injection molding machine (SG-150U manufactured by Sumitomo Heavy Industries, Ltd.) at a cylinder temperature of 300°C and a mold temperature of 150°C. The higher this value, the better the mechanical strength of the resin composition.
[0064] (2) Heat resistance evaluation The deflection temperature under load was measured using a 4 mm thick test piece prepared in accordance with ISO standards ISO75-1 and 2 at a load of 1.80 MPa.
[0065] (3) Bali evaluation The evaluation of burrs was carried out by measuring the length of the burrs on the part of the test piece that contacted the gas vent conforming to the above ISO 527-1 and ISO 527-2. The thickness of the gas vent was 10 μm and the width was 5 mm.
[0066] (4) Morphological observation For morphology observation, the center of the test piece conforming to the above ISO527-1 and ISO527-2 was cut and polished, gold was deposited, and a backscattered electron image was observed with a scanning electron microscope (SEM) at a measurement magnification of 3000. In the SEM image, the gray part is the polyarylene sulfide resin (PPS resin) phase, the black part is the polycarbonate resin (PC resin) phase, and the white part is the glass fiber (GF).
[0067] [Examples 1 to 17, Comparative Examples 1 to 8] A polyphenylene sulfide resin, a polycarbonate resin, a compound having a reactive functional group, and glass fibers were melt-kneaded using a vented twin-screw extruder at the respective compounding amounts shown in Table 1 and Table 2 to obtain pellets. The vented twin-screw extruder used was TEX-30XSST (fully meshing, co-rotating) manufactured by Japan Steel Works, Ltd. The extrusion conditions were a discharge rate of 12 kg / h, a screw rotation speed of 150 rpm, a vacuum degree of the vent of 3 kPa, and the extrusion temperature was 300 °C from the first feed port to the die part. The glass fibers were supplied from the second feed port using the side feeder of the above extruder, and the polyphenylene sulfide resin, polycarbonate resin, and compound having a reactive functional group were supplied to the extruder from the first feed port. Here, the first feed port refers to the feed port farthest from the die, and the second feed port refers to the feed port located between the die and the first feed port of the extruder. The obtained pellets were dried in a hot air circulation dryer at 130 °C for 6 hours, and then test pieces for evaluation were molded using an injection molding machine (SG-150U manufactured by Sumitomo Heavy Industries, Ltd.) under the conditions of a cylinder temperature of 300 °C and a mold temperature of 150 °C.
[0068] <Component A> A-1: Polyphenylene sulfide resin obtained by Production Method 1 [Production Method 1] 300.00 g of para-diiodobenzene and 27.00 g of sulfur were charged with 0.60 g of diphenyl disulfide (content of 0.65% by weight based on the weight of the finally polymerized PPS) as a polymerization terminator, heated to 180 °C to completely melt and mix them, then the temperature was raised to 220 °C, and the pressure was reduced to 200 Torr. The obtained mixture was subjected to a polymerization reaction for 8 hours while gradually changing the temperature and pressure so that the final temperature and pressure were 320 °C and 1 Torr, respectively, to produce a polyphenylene sulfide resin. The total sodium content was 7 ppm. Also, the dispersity (Mw / Mn) represented by the weight average molecular weight (Mw) and the number average molecular weight (Mn) was 4.7.
[0069] A-2: Polyphenylene sulfide resin obtained by Production Method 2 [Production Method 2] 5130 g of paradibenzene and 450 g of sulfur were heated to 180°C with 4 g of mercaptobenzothiazole as a reaction initiator to completely melt and mix. Then, the temperature was raised to 220°C and the pressure was reduced to 350 Torr. The resulting mixture was subjected to a polymerization reaction while gradually changing the temperature and pressure so that the final temperature and pressure were 300°C and 1 Torr or less, respectively. When the polymerization reaction had proceeded 80% (the degree of progress of the polymerization reaction was confirmed by the method of relative ratio based on viscosity ((current viscosity / target viscosity)×100%)), 25 g of mercaptobenzothiazole was added as a polymerization terminator to carry out the reaction. After 1 hour, 51 g of 4-iodobenzoic acid was added and the reaction was carried out for 10 minutes under a nitrogen atmosphere. The degree of vacuum was gradually increased to 0.5 Torr or less and the reaction was carried out for another 1 hour, after which the reaction was terminated to produce a polyarylene sulfide resin containing a carboxyl group at the main chain end. In the FT-IR spectrum of the obtained polyarylene sulfide, the presence of a carboxyl group peak at 1600~1800 cm -1 was confirmed. Also, when the height intensity of the aromatic ring stretching peak appearing at 1400~1600 cm -1 was taken as 100%, the relative height intensity of the peak at 1600~1800 cm -1 was 3.4%. The total sodium content was 7 ppm. Also, the dispersity (Mw / Mn) represented by the weight average molecular weight (Mw) and the number average molecular weight (Mn) was 4.11. A-3: Polyphenylene sulfide resin (DIC-PPS MA-510 manufactured by DIC)
[0070] <Component B> B-1: Polycarbonate resin obtained by Production Method 3 (viscosity average molecular weight 12500) [Production Method 3] A reactor equipped with a thermometer, a stirrer and a reflux condenser was charged with 219.4 parts of ion-exchanged water and 40.2 parts of 48% aqueous sodium hydroxide solution, to which 57.5 parts of 2,2-bis(4-hydroxyphenyl)propane and 0.12 parts of hydrosulfite were added and dissolved in 25 minutes, after which 181 parts of methylene chloride was added in 5 minutes, and 27.8 parts of phosgene was blown in over 40 minutes at 15-25° C. under stirring. After the blowing of phosgene was completed, 7.2 parts of an aqueous 48% sodium hydroxide solution and 0.65 parts of a solution in which 0.20 parts of 2,2-bis(4-hydroxyphenyl)propane was dissolved in 3.10 parts of p-tert-butylphenol and 1 part of an aqueous 7.4% sodium hydroxide solution were added, emulsified with a homomixer, and then the stirring was stopped and the mixture was left to stand at 28-33° C. for 2.5 hours to complete the reaction. After the reaction was completed, 200 parts of methylene chloride was added to the product and mixed, then stirring was stopped, and the aqueous phase and organic phase were separated to obtain an organic solvent solution with a polycarbonate resin concentration of 15% by weight. 200 parts of ion-exchanged water was added to this organic solvent solution and mixed with stirring, then stirring was stopped, and the aqueous phase and organic phase were separated. This operation was repeated (4 times) until the conductivity of the aqueous phase was almost the same as that of the ion-exchanged water. The obtained purified polycarbonate resin solution was filtered through a SUS304 filter with a filtration accuracy of 1 μm. Next, the organic solvent solution was charged with 100 L of ion-exchanged water in a 1000 L kneader with an inner wall material made of SUS316L and an isolation chamber with a foreign matter outlet in the bearing part, and methylene chloride was evaporated at a water temperature of 42 ° C to obtain powder and granules, and the mixture of the powder and water was charged into a hot water treatment tank of a hot water treatment process having a hot water treatment tank with an agitator whose water temperature was controlled to 95 ° C, and mixed with an agitator for 30 minutes at a mixing ratio of 25 parts of powder and 75 parts of water. The mixture of powder and water was separated by a centrifuge to obtain a powder containing 0.5% by weight of methylene chloride and 45% by weight of water. Next, the powder was continuously fed at 50 kg / Hr (polycarbonate resin equivalent) to a SUS316L conductive heat receiving groove type two-shaft agitation continuous dryer controlled at 140°C, and dried under the condition of an average drying time of 6 hours to obtain a powder with a viscosity average molecular weight of 11,800. The obtained powder was put into acetone, stirred for 30 minutes, and then the powder slurry solution was taken out, and after solid-liquid separation, it was dried at 140°C for 4 hours under a nitrogen atmosphere to obtain a powder (powder) extracted with acetone with a viscosity average molecular weight of 12,500 and a hydroxyl group amount of 13 eq / ton.
[0071] <Component C> C-1: 1,3,5-Tris(2-(3-sulfanylbutanoyloxy)ethyl)-1,3,5-triazinane-2,4,6-trione (Karenz MT·NR1, manufactured by Showa Denko K.K.) C-2: 1,4-Benzenedithiol (manufactured by Tokyo Chemical Industry Co., Ltd.) C-3: 4-Mercaptobenzoic acid (manufactured by Tokyo Chemical Industry Co., Ltd.) C-4: 2,2'-Dithiobisbenzoic acid (manufactured by Tokyo Chemical Industry Co., Ltd.) C-5: 4,4'-Dithiobenzidine (manufactured by Tokyo Chemical Industry Co., Ltd.) C-6: 4,4'-Dithiobiphenol (manufactured by Tokyo Chemical Industry Co., Ltd.) C-7: 4-Mercaptophenol (manufactured by Tokyo Chemical Industry Co., Ltd.) C-8: 3-Mercaptopropyltrimethoxysilane (KBM-803, manufactured by Shin-Etsu Chemical Co., Ltd.) C-9: Diphenyldisulfide (manufactured by Tokyo Chemical Industry Co., Ltd.) C-10: p-Toluenethiol (manufactured by Tokyo Chemical Industry Co., Ltd.)
[0072] <Component D> D-1: Chopped glass fiber with circular cross-section (T-732H, manufactured by Nippon Electric Glass Co., Ltd., diameter: 10.5 μm, cut length: 3 mm, epoxy-based sizing agent) D-2: Chopped glass fiber with circular cross-section (T-756H, manufactured by Nippon Electric Glass Co., Ltd., diameter: 10.5 μm, cut length: 3 mm, urethane-based sizing agent)
[0073]
Table 1
[0074]
Table 2
Claims
1. The resin composition contains 100 parts by weight in total of (A) a polyarylene sulfide resin (component A) and (B) a polycarbonate resin (component B), 0.001 to 10 parts by weight of (C) a compound (component C) having at least one sulfur atom and having at least one reactive functional group selected from the group consisting of a thiol group, a carboxyl group, an epoxy group, and an amino group, and 10 to 350 parts by weight of (D) glass fiber (component D), wherein the resin composition forms a sea-island structure in which the polyarylene sulfide resin is the continuous phase and the polycarbonate resin is the dispersed phase, and has a morphology in which the glass fiber is dispersed only in the polyarylene sulfide resin continuous phase.
2. 2. The resin composition according to claim 1, wherein the weight ratio of component A to component B (component A / component B) is 99 / 1 to 50 / 50.
Citation Information
Patent Citations
Ultra-high strength glass fiber reinforced thermoplastic resin composite plate and preparation method thereof
CN103571046A
Horiariirensurufuidososeibutsu
JP1976059952A
Compound of modified polyarylene sulfide and polycarbonate
JP1992233971A
Polyphenylene sulfide resin composition and method for producing the same
JP2003113307A
Low-contaminated injection-molded form
JP2005290328A