Resin composition and molded article thereof

A resin composition with a thermoplastic α-olefin copolymer and carbon-based filler addresses the need for improved electrical and mechanical properties by optimizing tan δ peak and surface resistivity, enhancing stress absorption and conductivity in molded articles.

JP7560297B2Active Publication Date: 2024-10-02MITSUI CHEMICALS INC
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2020151338
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-03-16
Filing Date
2020-09-09
Publication Date
2024-10-02
Estimated Expiration
2040-09-09

AI Technical Summary

Technical Problem

Existing resin compositions with high tan δ peak values at room temperature lack sufficient electrical and mechanical properties, particularly in applications requiring conductivity and stress absorption.

Method used

A resin composition comprising a thermoplastic resin with specific α-olefin copolymer and carbon-based filler, such as carbon nanotubes, optimized for a tan δ peak between 0°C and 60°C, surface resistivity of 10^14Ω or less, and mechanical properties.

Benefits of technology

The composition achieves high tan δ peak values at room temperature with excellent electrical and mechanical properties, enhancing stress absorption and conductivity in molded articles.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007560297000001
    Figure 0007560297000001
  • Figure 0007560297000002
    Figure 0007560297000002
  • Figure 0007560297000003
    Figure 0007560297000003
Patent Text Reader

Abstract

SOLUTION: There is provided a resin composition (X) that contains 80.0-99.9 pts.mass of a thermoplastic resin (A) and 0.1-20.0 pts.mass of a carbon-based filler (B) (total of thermoplastic resin (A) and carbon-based filler (B) is 100 pts.mass), and satisfies the following requirements (a) to (c): requirement (a); a temperature in which a loss tangent tanδ obtained by dynamic viscoelasticity at a frequency of 10 rad / s (1.6 Hz) in a temperature range of -40 to 150°C becomes a peak value of 0°C or higher and 60°C or lower, requirement (b); a peak value of a loss tangent tanδ obtained by dynamic viscoelasticity at a frequency of 10 rad / s (1.6 Hz) in a temperature range of -40 to 150°C of 0.5 or more and 5.0 or less, and requirement (c); surface resistivity of 10^14 Ω or less.EFFECT: A resin composition has a high tanδ peak value at room temperature, has excellent electric characteristics and mechanical properties, and enables formation of a molding which has a high tanδ peak value at room temperature irrespective of a molding method, has excellent electric characteristics and is excellent in mechanical properties.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a resin composition and a molded article, and more particularly to a resin composition containing a carbon-based filler and a molded article molded using the same.

[0002] More specifically, the present invention relates to a composition containing a copolymer of 4-methyl-1-pentene and an α-olefin and a carbon-based filler, which has excellent stress absorption properties, stress relaxation properties, electrical properties, toughness, and mechanical properties and has a reduced shrinkage rate after molding, and a molded article molded using the composition. [Background technology]

[0003] Olefin polymers have excellent processability, chemical resistance, electrical properties, mechanical properties, and the like, and are therefore processed into extrusion molded products, injection molded products, blow molded products, films, sheets, fibers, and the like, and are used in a wide range of applications, such as daily necessities, kitchen utensils, packaging films, nonwoven fabrics, home appliances, machine parts, electrical parts, and automobile parts.

[0004] Patent Documents 1 and 2 disclose a material having a high tan δ peak at room temperature, which is made of a 4-methyl-1-pentene copolymer, and disclose that this material can be used as a vibration-damping or vibration-proofing material. The vibration-damping properties required for a vibration-damping material can be evaluated, for example, by the loss tangent tan δ, which is the ratio (G” / G’) of the storage modulus (G’) to the loss modulus (G”). Therefore, the higher the tan δ of a material in the temperature environment in which the vibration-damping material is used, the stronger the viscosity of the material is, so that the material is more likely to absorb stress due to vibration and exhibit higher vibration-damping properties. Note that tan δ changes depending on the temperature, so a technology has been developed to adjust the maximum value of tan δ of a vibration-damping material (hereinafter also referred to as the “tan δ peak value”) and the temperature at which the value of tan δ is maximum (hereinafter also simply referred to as the “tan δ peak temperature”) to specific ranges. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2012-82388 A [Patent Document 2] JP 2017-132920 A Summary of the Invention [Problem to be solved by the invention]

[0006] Although the materials described in the above-mentioned Patent Documents 1 and 2 have high tan δ peak values ​​at room temperature, further improvements are required in terms of electrical properties. By imparting electrical conductivity, static electricity can be suppressed when the material is used for the various applications mentioned above, and the material can be applied to stretchable conductive wiring, electrodes, sensors, and the like.

[0007] Therefore, an object of the present invention is to provide a resin composition and a molded article having a high tan δ peak value at room temperature and further excellent electrical properties and mechanical properties. [Means for solving the problem]

[0008] The present inventors have conducted intensive research in view of the above circumstances and have completed the present invention. That is, the present invention relates to the following [1] to

[11] .

[0009] [1] A resin composition (X) comprising 80.0 to 99.9 parts by mass of a thermoplastic resin (A) which is an olefin copolymer containing a structural unit (i) derived from an α-olefin having 6 to 20 carbon atoms and a structural unit (ii) derived from an α-olefin having 2 to 5 carbon atoms, and 0.1 to 20.0 parts by mass of a carbon-based filler (B) (the total of the thermoplastic resin (A) and the carbon-based filler (B) being 100 parts by mass), and which satisfies the following requirements (a) to (c): Requirement (a): The temperature at which the loss tangent tan δ, obtained by performing dynamic viscoelasticity measurement at a frequency of 10 rad / s (1.6 Hz) in the temperature range of -40 to 150°C, reaches its peak value is equal to or higher than 0°C and equal to or lower than 60°C. Requirement (b): The peak value of the loss tangent tan δ obtained by performing dynamic viscoelasticity measurement at a frequency of 10 rad / s (1.6 Hz) in the temperature range of -40 to 150°C is 0.5 or more and 5.0 or less. Requirement (c): Surface resistivity is 10^14 Ω or less. [2] A resin composition (X) comprising 80.0 to 99.9 parts by mass of a thermoplastic resin (A) and 0.1 to 20.0 parts by mass of a carbon-based filler (B) (the total of the thermoplastic resin (A) and the carbon-based filler (B) being 100 parts by mass), and satisfying the following requirements (a) to (c): Requirement (a): The temperature at which the loss tangent tan δ, obtained by performing dynamic viscoelasticity measurement at a frequency of 10 rad / s (1.6 Hz) in the temperature range of -40 to 150°C, reaches its peak value is equal to or higher than 0°C and equal to or lower than 60°C. Requirement (b): The peak value of the loss tangent tan δ obtained by performing dynamic viscoelasticity measurement at a frequency of 10 rad / s (1.6 Hz) in the temperature range of -40 to 150°C is 0.5 or more and 5.0 or less. Requirement (c): Surface resistivity is 10^14 Ω or less. [3] The resin composition (X) according to the above item [1], wherein the thermoplastic resin (A) is a 4-methyl-1-pentene-α-olefin copolymer (A-1), in which the α-olefin having 6 to 20 carbon atoms is 4-methyl-1-pentene. [4] The resin composition (X) according to the above item [3], characterized in that the 4-methyl-1-pentene / α-olefin copolymer (A-1) satisfies the following requirements (d) to (g): Requirement (d): The copolymer (A-1) contains 55 to 90 mol % of the structural unit (i) derived from 4-methyl-1-pentene and the structural unit (ii) derived from an α-olefin having from 2 to 5 carbon atoms, relative to 100 mol % in total of the structural unit (i) and the structural unit (ii) contained in the copolymer (A-1). Requirement (e): The copolymer (A-1) has a melting point (Tm) measured by a differential scanning calorimeter (DSC) of 160° C. or less, or has no melting point measurable by a differential scanning calorimeter (DSC). Requirement (f): The copolymer (A-1) has a peak temperature of loss tangent tanδ, which is obtained by measuring dynamic viscoelasticity at a frequency of 10 rad / s (1.6 Hz) in the temperature range of -40 to 150°C, of ​​15°C or more and 45°C or less. Requirement (g): The copolymer (A-1) has a peak value of loss tangent tan δ of 0.6 or more and 5.0 or less, as determined by dynamic viscoelastic measurement at a frequency of 10 rad / s (1.6 Hz) in a temperature range of -40 to 150°C. [5] The resin composition (X) according to any one of the above [1] to [4], wherein the carbon-based filler (B) is a carbon nanotube. [6] A molded article comprising the resin composition (X) according to any one of the above [1] to [5]. [7] A sheet comprising the resin composition (X) according to any one of the above [1] to [5]. [8] A toy comprising the resin composition (X) according to any one of the above [1] to [5]. [9] Daily necessities comprising the resin composition (X) according to any one of [1] to [5] above.

[10] An automotive material comprising the resin composition (X) according to any one of the above [1] to [5].

[11] An electronic part comprising the resin composition (X) according to any one of the above [1] to [5]. Effect of the Invention

[0010] The resin composition of the present invention has a high tan δ peak value at room temperature, and further has excellent electrical properties and mechanical properties, and can form a molded article having a high tan δ peak value at room temperature, excellent electrical properties, and excellent mechanical properties, regardless of the molding method. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] The resin composition and molded article of the present invention will be described below. [Resin composition (X)] The resin composition (X) of the present invention contains a thermoplastic resin (A) and a carbon-based filler (B). The resin composition (X) of the present invention may contain only the thermoplastic resin (A) and the carbon-based filler (B), or, as described below, may further contain, in addition to the thermoplastic resin (A) and the carbon-based filler (B), other components other than the thermoplastic resin (A) and the carbon-based filler (B). The resin composition (X) of the present invention satisfies the following requirements (a) to (c).

[0012] Requirement (a); Resin composition (X) of the present invention has a temperature (hereinafter also referred to as "tan δ peak temperature") at which the loss tangent tan δ, obtained by measuring the dynamic viscoelasticity at a frequency of 10 rad / s in the temperature range of -40 to 150°C, reaches a peak value, of 0°C or more and 60°C or less. From the viewpoint of elasticity, the tan δ peak temperature is preferably 10° C. or more and 50° C. or less, more preferably 20° C. or more and 45° C. or less, and particularly preferably 25° C. or more and 43° C. or less.

[0013] Requirement (b); The resin composition (X) of the present invention has a peak value of loss tangent tanδ (hereinafter also referred to as "peak value tanδ") of 0.5 or more and 5.0 or less, as obtained by dynamic viscoelasticity measurement at a frequency of 10 rad / s (1.6 Hz) in a temperature range of -40 to 150°C. From the viewpoint of flexibility, this tan δ peak value is preferably 0.6 or more and 4.5 or less, and more preferably 0.7 or more and 3.5 or less. Tan δ can be calculated as the ratio of the storage modulus (G') to the loss modulus (G") (G" / G': loss tangent) using the storage modulus (G') and loss modulus (G") obtained during measurement of dynamic viscoelasticity.

[0014] In the present invention, the temperature at which tan δ reaches a peak value (maximum value) in the range of -40 to 150°C is defined as the temperature at which tan δ reaches a peak value, and the value of tan δ at that time is defined as the tan δ peak value. The peak is considered to be due to the glass transition temperature of the thermoplastic resin composition.

[0015] Requirement (c); The resin composition (X) of the present invention has a surface resistivity of 10^14 Ω or less.

[0016] The thermoplastic resin (A) and the carbon-based filler (B) constituting the resin composition (X) of the present invention will be described below. <Thermoplastic resin (A)> The resin composition (X) of the present invention contains a thermoplastic resin (A). The content of the thermoplastic resin (A) in the resin composition (X) is 80.0 to 99.9 parts by mass, preferably 85.0 parts by mass or more, more preferably 90.0 parts by mass or more, and preferably 99.5 parts by mass or less, more preferably 99.2 parts by mass or less, and even more preferably 99.0 parts by mass or less, based on 100 parts by mass of the total of the thermoplastic resin (A) and the carbon-based filler (B).

[0017] Here, the thermoplastic resin (A) used in the present invention is not particularly limited as long as it can solve the problems of the present invention, particularly as long as it can provide a resin composition (X) having the above-mentioned peak temperature and peak value of tan δ. However, in a typical embodiment of the present invention, the thermoplastic resin (A) is preferably an olefin-based copolymer containing a structural unit (i) derived from an α-olefin having 6 to 20 carbon atoms and a structural unit (ii) derived from an α-olefin having 2 to 5 carbon atoms from the viewpoint of impact resistance, and among the above olefin-based copolymers, a 4-methyl-1-pentene-α-olefin copolymer (A-1) in which the α-olefin having 6 to 20 carbon atoms is 4-methyl-1-pentene is particularly preferred. The 4-methyl-1-pentene·α-olefin copolymer (A-1) will be described below.

[0018] ≪4-Methyl-1-pentene / α-olefin copolymer (A-1)≫ The 4-methyl-1-pentene / α-olefin copolymer (A-1) (hereinafter, simply referred to as "copolymer (A-1)") preferably satisfies all of the following requirements (d) to (g). The 4-methyl-1-pentene / α-olefin copolymer (A-1) may be used alone or in combination of two or more. Furthermore, as a more preferred embodiment of the present invention, the following requirements (d) to (k) are described in detail below.

[0019] Requirement (d); The 4-methyl-1-pentene / α-olefin copolymer (A-1) preferably contains 55 mol % to 90 mol % of the structural unit (i) and 10 mol % to 45 mol % of the structural unit (ii), when the total of the structural unit (i) derived from 4-methyl-1-pentene and the structural unit (ii) derived from an α-olefin having from 2 to 5 carbon atoms is taken as 100 mol %. The content (mol%) of each structural unit (4-methyl-1-pentene and α-olefin) in the 4-methyl-1-pentene copolymer (A) is 13 It is measured by C-NMR.

[0020] In the present invention, the term "structural unit derived from an α-olefin" refers to a structural unit corresponding to an α-olefin, i.e., -CH 2 The term "structural unit derived from 4-methyl-1-pentene" is interpreted in the same manner, and the structural unit corresponding to 4-methyl-1-pentene (i.e., -CH 2 -CH(-CH 2 CH(CH 3 ) 2 )-(R is an alkyl group) is a structural unit.

[0021] The lower limit of the proportion of the structural unit (i) constituting the 4-methyl-1-pentene-α-olefin copolymer (A-1) is preferably 55 mol%, more preferably 60 mol%, and particularly preferably 68 mol%. On the other hand, the upper limit of the proportion of the structural unit (i) is preferably 90 mol%, more preferably 86 mol%, and particularly preferably 84 mol%. When the proportion of the structural unit (i) constituting the 4-methyl-1-pentene-α-olefin copolymer (A-1) is equal to or greater than the above lower limit, the temperature at which the tan δ of the 4-methyl-1-pentene-α-olefin copolymer (A-1) reaches its peak value is near room temperature, and therefore the temperature at which the tan δ of the resin composition reaches its peak value is easily adjusted to the above range.

[0022] Naturally, in this case, the upper limit of the proportion of the structural unit (ii) is preferably 45 mol%, more preferably 40 mol%, and particularly preferably 32 mol%, while the lower limit of the proportion of the structural unit (ii) is preferably 10 mol%, more preferably 14 mol%, and particularly preferably 16 mol%.

[0023] Here, in a typical embodiment of the present invention, examples of the α-olefin having 2 to 5 carbon atoms from which the structural unit (ii) is derived include linear α-olefins such as ethylene, propylene, 1-butene, and 1-pentene, and branched α-olefins such as 3-methyl-1-butene. Among these, ethylene, propylene, 1-butene, and 1-pentene are preferred, and ethylene and propylene are particularly preferred. The structural unit (ii) may be derived from one of these compounds, or from two or more compounds.

[0024] However, the 4-methyl-1-pentene-α-olefin copolymer (A-1) may further contain, in addition to the structural units (i) and (ii), a structural unit derived from another monomer other than 4-methyl-1-pentene or the α-olefin from which the structural unit (ii) is derived, as structural unit (iii), so long as the amount is small enough not to impair the object of the present invention (for example, 10 mol % or less, assuming that the total of the structural units (i) and (ii) is 100 mol %). Specific preferred examples of such other monomers include 5-vinyl-2-norbornene and 5-ethylidene-2-norbornene when the copolymer (A-1) is a 4-methyl-1-pentene-propylene copolymer.

[0025] requirement(e); The 4-methyl-1-pentene·α-olefin copolymer (A-1) preferably has a melting point (Tm) measured by a differential scanning calorimeter (DSC) of 160° C. or less, or has no melting point (Tm) measured by a differential scanning calorimeter (DSC). When the copolymer (A-1) satisfies such requirements, it becomes easier to knead with the carbon-based filler in the resin composition of the present invention, and it becomes possible to improve vibration absorption and stress relaxation properties.

[0026] requirement(f); The 4-methyl-1-pentene·α-olefin copolymer (A-1) preferably has a tan δ peak temperature of 15°C or more and 45°C or less, as determined by dynamic viscoelasticity measurement at a frequency of 10 rad / s (1.6 Hz) in a temperature range of −40 to 150°C. The tan δ peak temperature is more preferably from 20° C. to 40° C., particularly preferably from 25° C. to 40° C. By setting the tan δ peak temperature within the above temperature range, the value of tan δ at room temperature can be further increased.

[0027] requirement(g); The 4-methyl-1-pentene·α-olefin copolymer (A-1) preferably has a tan δ peak value of 0.6 or more and 5.0 or less, as obtained by dynamic viscoelasticity measurement at a temperature range of −40 to 150° C. and a frequency of 10 rad / s (1.6 Hz). The tan δ peak value is more preferably 1.0 to 5.0, even more preferably 1.5 to 5.0, and particularly preferably 2.0 to 4.0. By setting the tan δ peak value within the above range, it is possible to change the vibration absorption property, hardness and conformability of the material according to the speed of tension or deformation.

[0028] It is more preferable that the 4-methyl-1-pentene·α-olefin copolymer (A-1) satisfies, in addition to the above requirements (d) to (g), one or more requirements selected from the following requirements (h), (i), (j) and (k):

[0029] requirements(h); The 4-methyl-1-pentene / α-olefin copolymer (A-1) preferably has an intrinsic viscosity [η] measured in decalin at 135° C. of 0.1 dL / g or more and 5.0 dL / g or less. The intrinsic viscosity [η] is more preferably 0.5 dL / g or more and 4.0 dL / g or less, and even more preferably 0.5 dL / g or more and 3.5 dL / g or less. The 4-methyl-1-pentene / α-olefin copolymer (A-1) having the intrinsic viscosity [η] in the above range can be easily molded into a sheet-shaped thermoplastic resin composition.

[0030] The above-mentioned intrinsic viscosity [η] of the 4-methyl-1-pentene·α-olefin copolymer (A-1) can be adjusted to the above-mentioned range by controlling the molecular weight and polymerization activity by adding hydrogen during the production by polymerization. The intrinsic viscosity [η] is the viscosity increase rate η per unit concentration c of each polymer when different amounts of the thermoplastic resin composition are dissolved in decalin at 135°C. sp (i.e. η sp / c) to obtain reduced viscosity η red Let η redcan be obtained by extrapolating the unit concentration of the polymer, c, to zero.

[0031] Requirement(i); The ratio of the weight average molecular weight (Mw) to the number average molecular weight (Mn) (molecular weight distribution: Mw / Mn) of the 4-methyl-1-pentene / α-olefin copolymer (A-1) measured by gel permeation chromatography (GPC) is preferably 1.0 or more and 3.5 or less. The Mw / Mn is more preferably 1.2 or more and 3.0 or less, and even more preferably 1.5 or more and 2.8 or less. The 4-methyl-1-pentene / α-olefin copolymer (A-1) having the above Mw / Mn in the above range is less susceptible to deterioration in moldability due to a low molecular weight, low stereoregularity polymer, and can be easily molded into a sheet-shaped thermoplastic resin composition.

[0032] The 4-methyl-1-pentene / α-olefin copolymer (A-1) has a weight average molecular weight (Mw) measured by gel permeation chromatography (GPC) in terms of polystyrene of preferably 500 or more and 10,000,000 or less, more preferably 1,000 or more and 5,000,000 or less, and even more preferably 1,000 or more and 2,500,000 or less.

[0033] The Mw / Mn and Mw of the 4-methyl-1-pentene·α-olefin copolymer (A-1) can be adjusted to the above range, for example, by using a metallocene catalyst. The above Mw and Mw / Mn can be determined, for example, by using a Waters ALC / GPC 150-C plus type (integrated differential refractometer detector) as a liquid chromatograph, two Tosoh Corporation GMH6-HT columns and two GMH6-HTL columns connected in series, o-dichlorobenzene as the mobile phase medium, and analyzing the chromatogram obtained at a flow rate of 1.0 ml / min and 140°C using a calibration curve using a standard polystyrene sample.

[0034] requirement(j); The density of the 4-methyl-1-pentene / α-olefin copolymer (A-1) (measured according to JIS K7112) is preferably 870 to 830 kg / m 3 The density is more preferably 865 to 830 kg / m 3 , more preferably 855 to 830 kg / m 3 Details of the measurement conditions and the like are as described in the Examples section below. The density can be appropriately changed by adjusting the comonomer composition ratio of the copolymer (A-1), and a copolymer (A-1) having a density within the above range is advantageous in producing a lightweight sheet.

[0035] requirement(k); The melt flow rate (MFR) of the 4-methyl-1-pentene / α-olefin copolymer (A-1) (measured according to ASTM D1238 at 230° C. under a load of 2.16 kg) is preferably 4.0 to 30 g / 10 min. The melt flow rate is more preferably 7.0 to 15 g / 10 min, and further preferably 7.0 to 13 g / 10 min. The copolymer (A-1) having a melt flow rate within the above range is advantageous in producing good pellets, sheets, and molded articles during molding processing.

[0036] A particularly preferred embodiment of the 4-methyl-1-pentene / α-olefin copolymer (A-1) satisfies the above-mentioned requirements (d) to (g) as well as the requirement (h). In a particularly preferred embodiment, in addition to the requirements (d) to (h), it satisfies one or more, preferably two or more, and particularly preferably all, of the requirements (i), (j) and (k).

[0037] <Production method of 4-methyl-1-pentene / α-olefin copolymer (A-1)> The method for producing the copolymer (A-1) is not particularly limited, but for example, the copolymer can be obtained by polymerizing 4-methyl-1-pentene and the above-mentioned "α-olefin from which the structural unit (ii) is derived" in the presence of a suitable polymerization catalyst such as a magnesium-supported titanium catalyst or a metallocene catalyst.

[0038] Here, as the polymerization catalyst that can be used in the present invention, a conventionally known catalyst, for example, a magnesium-supported titanium catalyst, or a metallocene catalyst described in WO 01 / 53369, WO 01 / 27124, JP-A-3-193796 or JP-A-2-41303, WO 2011 / 055803, WO 2014 / 050817, or the like, can be suitably used.

[0039] The polymerization can be carried out by a method appropriately selected from liquid phase polymerization methods including solution polymerization and suspension polymerization, and gas phase polymerization methods. In the liquid phase polymerization method, an inert hydrocarbon solvent can be used as the solvent that constitutes the liquid phase.Examples of the inert hydrocarbon include aliphatic hydrocarbons including propane, butane, pentane, hexane, heptane, octane, decane, dodecane, and kerosene, alicyclic hydrocarbons including cyclopentane, cyclohexane, methylcyclopentane, and methylcyclohexane, aromatic hydrocarbons including benzene, toluene, and xylene, and halogenated hydrocarbons including ethylene chloride, chlorobenzene, dichloromethane, trichloromethane, and tetrachloromethane, and mixtures thereof.

[0040] Furthermore, in the liquid phase polymerization method, bulk polymerization can also be carried out using the monomers themselves from which the above structural units (i) to (iii) are derived as a solvent. Furthermore, by carrying out the copolymerization of monomers leading to the above-mentioned structural units (i) to (iii) in a stepwise manner, it is also possible to appropriately control the composition distribution of the structural units (i) to (iii) constituting the 4-methyl-1-pentene / α-olefin copolymer (A-1). The polymerization temperature is preferably from -50°C to 200°C, more preferably from 0°C to 100°C, and even more preferably from 20°C to 100°C.

[0041] The polymerization pressure is preferably from normal pressure to 10 MPa gauge pressure, and more preferably from normal pressure to 5 MPa gauge pressure. During polymerization, hydrogen may be added for the purpose of controlling the molecular weight and polymerization activity of the polymer produced. The amount of hydrogen added is suitably about 0.001 NL or more and 100 NL or less per 1 kg of the total amount of monomers from which the structural units (i) to (iii) are derived.

[0042] <Carbon-based filler (B)> The carbon-based filler (B) is a material having electrical conductivity. Examples thereof include carbon nanotubes (CNTs) and carbon fibers. The carbon-based filler (B) is not particularly limited as long as it is a material having electrical conductivity, but among these, carbon nanotubes are preferred because they have an excellent effect of reducing the surface resistivity of the molded body.

[0043] Carbon nanotubes are cylindrical hollow fibrous substances made of carbon, and may be either multi-walled or single-walled carbon nanotubes. The average diameter of the carbon nanotubes is preferably 1 nm or more, more preferably 5 nm or more, and even more preferably 7 nm or more, and is preferably 100 nm or less, more preferably 50 nm or less, and even more preferably 20 nm or less. The average length of the carbon nanotubes is preferably 0.5 μm or more, more preferably 0.6 μm or more, and preferably 50 μm or less, more preferably 30 μm or less, and even more preferably 15 μm or less. If the average diameter is 1 nm or more, it is possible to make the nanotubes less likely to break during kneading, and if it is 20 nm or less, it is likely to increase the electrical conductivity. If the average length is 0.5 μm or more, it is possible to increase the electrical conductivity, and if it is 50 μm or less, it is likely to suppress the increase in viscosity during kneading, and to facilitate kneading and molding.

[0044] The average diameter and average length of the carbon nanotubes can be determined by observing the carbon nanotubes under an electron microscope (SEM, TEM) and calculating the arithmetic average. Carbon nanotubes can be produced by, for example, an arc discharge method, a chemical vapor deposition method (CVD method), or a laser ablation method. Commercially available carbon nanotubes may also be used. Carbon nanotubes tend to exhibit high conductivity in relatively small amounts compared to, for example, carbon black, but are expensive, so it is advantageous from the standpoint of cost if they can be used in smaller amounts.

[0045] As the carbon fiber, various known carbon fibers can be used, for example, polyacrylonitrile-based, rayon-based, pitch-based, polyvinyl alcohol-based, regenerated cellulose-based, pitch-based produced from mesophase pitch, etc. Carbon fibers have an advantage in that they have excellent specific strength, in applications where light weight and strength are important, such as for aircraft.

[0046] The carbon fibers may be general-purpose fibers or high-strength fibers, and may be long fibers, short fibers, chopped fibers, or recycled fibers. As a sizing agent (sizing agent) for carbon fibers, for example, any of urethane-based emulsion, epoxy-based emulsion, nylon-based emulsion, and olefin-based emulsion can be used.

[0047] The average length of the carbon fibers, i.e., the average fiber length, is preferably 0.1 mm or more, more preferably 0.3 mm or more, even more preferably 0.5 mm or more, and is preferably 15.0 mm or less, more preferably 13.0 mm or less. When the average fiber length is 0.1 mm or more, the reinforcing effect of the mechanical properties due to the carbon fibers tends to be fully expressed. When the average fiber length is 15.0 mm or less, the dispersibility of the carbon fibers in the resin composition (X), and therefore the appearance, tends to be good.

[0048] The average diameter of the carbon fibers is preferably 3 μm or more, more preferably 5 μm or more, and preferably 30 μm or less, more preferably 21 μm or less, and even more preferably 19 μm or less. When the average diameter of the carbon fibers is 3 μm or more, the carbon fibers are less likely to break during molding, and the impact strength of the resulting molded body tends to be high. When the average diameter of the carbon fibers is 30 μm or less, the appearance of the molded body is good, and the aspect ratio of the carbon fibers does not decrease, and sufficient reinforcing effect is likely to be obtained in the mechanical properties such as rigidity and heat resistance of the molded body.

[0049] The carbon-based filler (B) can be used alone or in combination. The content of the carbon-based filler (B) in the resin composition (X) is 0.1 to 20.0 parts by mass, based on 100 parts by mass of the total of the thermoplastic resin (A) and the carbon-based filler (B). The content of the carbon-based filler (B) is preferably 0.5 parts by mass or more, more preferably 0.8 parts by mass or more, and even more preferably 1.0 part by mass or more, and is preferably 15.0 parts by mass or less, and more preferably 10.0 parts by mass or less.

[0050] <Other ingredients> The resin composition may further contain resins other than the thermoplastic resin (A) and the carbon-based filler (B) and various resin additives.

[0051] Other polymers The resin composition (X) of the present invention may further contain other polymers (hereinafter referred to as "other polymers") not falling under the category of the thermoplastic resin (A), such as the 4-methyl-1-pentene / α-olefin copolymer (A-1), within the scope not impairing the effects of the present invention.

[0052] Examples of "other polymers" include conventionally known resins such as low-density, medium-density, and high-density polyethylene, high-pressure low-density polyethylene, isotactic polypropylene, syndiotactic polypropylene, poly-1-butene, poly-4-methyl-1-pentene, poly-3-methyl-1-butene, cyclic olefin copolymers, chlorinated polyolefins, thermoplastic polyurethanes, etc. These resins may be used alone or in combination of two or more.

[0053] The blending amount of these resins is preferably 0 to 25 parts by mass, more preferably 0.1 to 20 parts by mass, and particularly preferably 0.3 to 10 parts by mass, based on 100 parts by mass of the thermoplastic resin (A). Here, when producing the resin composition (X), these resins may be used in the form of a composition containing the additives described below, and in that case, the blending amount of the resin is based on the mass obtained by subtracting the mass of the additives from the mass of this composition.

[0054] In addition, the "other polymer" is not limited to an unmodified polymer, but may be a modified polymer. For this reason, the resin composition (X) of the present invention may contain a modified polyolefin wax (C) in order to facilitate kneading a high content of carbon-based filler (B) into the thermoplastic resin (A). By using this modified polyolefin wax (C), it is considered that the aggregation of the carbon-based filler (B) in the thermoplastic resin (A) is suppressed, making kneading easier. It is also considered that it is easier to knead a high content of carbon-based filler (B) into the thermoplastic resin (A).

[0055] The type of modified polyolefin wax (C) is not particularly limited, but modified polyethylene wax and modified polypropylene wax are preferred, and modified polyethylene wax is more preferred. The modified polyolefin wax (C) can be produced by a known method. For example, a method of adding an unsaturated carboxylic acid or its derivative to a low molecular weight ethylene polymer by radical reaction in a solvent or without a solvent, a method of adding in the presence of a Lewis acid, or a method of adding at high temperature can be mentioned. The reaction temperature is 20°C to 300°C, and particularly 120°C to 250°C is preferable. Since the melting point of the low molecular weight ethylene polymer is about 120°C, it is preferable to set the reaction temperature to 120°C or higher in order to make the reaction system uniform.

[0056] The unsaturated carboxylic acid is not particularly limited as long as it is a compound having a reactive double bond and a carboxylic acid group, and examples of compounds that can be used include known unsaturated carboxylic acids. Also, the derivatives of unsaturated carboxylic acids are not particularly limited as long as they are a compound having a reactive double bond and a group that can be derived from a carboxylic acid group, and examples of such derivatives include anhydrides, esters, acid halides, amides, and imides of unsaturated carboxylic acids.

[0057] Examples of unsaturated carboxylic acids include unsaturated monocarboxylic acids such as acrylic acid, methacrylic acid, crotonic acid, and isocrotonic acid, and unsaturated dicarboxylic acids such as maleic acid, fumaric acid, tetrahydrophthalic acid, itaconic acid, citraconic acid, norbornene dicarboxylic acid, nadic acid endo cis-bicyclo[2.2.1]hept-5-ene-2,3-dicarboxylic acid, etc. By using unsaturated carboxylic acids, modified hydrocarbon resins having carboxylic acid groups can be obtained.

[0058] As the anhydride of the unsaturated carboxylic acid, the anhydride of the above-mentioned unsaturated dicarboxylic acid can be used. Specific examples thereof include maleic anhydride, itaconic anhydride, citraconic anhydride, tetrahydrophthalic anhydride, nadic anhydride, cis-bicyclo[2.2.1]hept-5-ene-2,3-dicarboxylic anhydride, etc. By using the anhydride of the unsaturated carboxylic acid, a modified hydrocarbon resin having a carboxylic anhydride group can be obtained. Maleic anhydride is particularly preferred.

[0059] As the ester of the unsaturated carboxylic acid, an alkyl ester, a hydroxyalkyl ester, or a glycidyl ester of the above-mentioned unsaturated carboxylic acid can be used. Specific examples include monomethyl maleate, dimethyl maleate, glycidyl maleate, hydroxyl (meth)acrylate, hydroxypropyl (meth)acrylate, and glycidyl (meth)acrylate. By using the ester of the unsaturated carboxylic acid, a modified hydrocarbon resin having a carboxylate group can be obtained.

[0060] Specific examples of halides of unsaturated carboxylic acids include malenyl chloride and dichloromaleic anhydride (C 4 Cl 2 O 3 By using a halide of an unsaturated carboxylic acid, a modified hydrocarbon resin having a halogen atom-containing carboxylic acid group can be obtained.

[0061] Specific examples of the amide of an unsaturated carboxylic acid include sulfamide, phthalamide, maleamide, etc. By using an amide of an unsaturated carboxylic acid, a modified hydrocarbon resin having an amide group can be obtained.

[0062] Specific examples of the imide of an unsaturated carboxylic acid include maleimide, phthalimide, sulfimide, etc. By using an imide of an unsaturated carboxylic acid, a modified hydrocarbon resin having an imide group can be obtained.

[0063] The acid value of the modified polyolefin wax (C) is preferably 1 to 100 mg-KOH / g, more preferably 10 to 90 mg-KOH / g. The number average molecular weight (Mn) of the modified polyolefin wax (C) in terms of polystyrene measured by gel permeation chromatography (GPC) is preferably 400 to 20,000. The amount of the modified polyolefin wax (C) added is preferably 0 to 20 parts by mass, more preferably 0.1 to 15 parts by mass, and particularly preferably 0.3 to 10 parts by mass, per 100 parts by mass of the thermoplastic resin (A).

[0064] Additives The resin composition (X) may further contain known additives, if necessary. Examples of additives include, but are not limited to, weather resistance stabilizers, heat resistance stabilizers, ultraviolet absorbers, infrared absorbers, antistatic agents, antislip agents, antiblocking agents, antifogging agents, lubricants, pigments, dyes, plasticizers, antioxidants, hydrochloric acid absorbers, antioxidants, crystal nucleating agents, antifungal agents, antibacterial agents, flame retardants, organic fillers, and softeners. These additives may be used alone or in combination.

[0065] Examples of the softener include known softeners including process oil, lubricating oil, paraffin, liquid paraffin, polyethylene wax, polypropylene wax, petroleum-based substances including petroleum asphalt and Vaseline, coal tars including coal tar and coal tar pitch, fatty oils including castor oil, linseed oil, rapeseed oil, soybean oil and coconut oil, tall oil, beeswax, carnauba wax and lanolin, fatty acids or metal salts thereof including ricinoleic acid, palmitic acid, stearic acid, 12-hydroxystearic acid, montanic acid, oleic acid and erucic acid, synthetic polymers including petroleum resin, coumarone-indene resin and atactic polypropylene, ester-based plasticizers including dioctyl phthalate, dioctyl adipate and dioctyl sebacate, microcrystalline wax, liquid polybutadiene or modified or hydrogenated products thereof, and liquid thiokol.

[0066] Examples of the softening agent include aromatic carboxylates (dibutyl phthalate, etc.), aliphatic carboxylates (methyl acetylricinoleate, etc.), aliphatic dialkoxylates (adipic acid-propylene glycol polyesters, etc.), aliphatic tricarboxylates (triethyl citrate, etc.), phosphate triesters (triphenyl phosphate, etc.), epoxy fatty acid esters (epoxybutyl stearate, etc.), and petroleum resins.

[0067] Examples of the release agent include lower (C1-4) alcohol esters of higher fatty acids (butyl stearate, etc.), polyhydric alcohol esters of fatty acids (C4-30) (hardened castor oil, etc.), glycol esters of fatty acids, and liquid paraffin.

[0068] Examples of the antioxidant include phenol-based (2,6-di-t-butyl-4-methylphenol, etc.), polycyclic phenol-based (2,2'-methylenebis(4-methyl-6-t-butylphenol), etc.), phosphorus-based (tetrakis(2,4-di-t-butylphenyl)-4,4-biphenylenediphosphonate, etc.), and amine-based (N,N-diisopropyl-p-phenylenediamine, etc.) antioxidants.

[0069] Examples of the flame retardant include phosphate esters and other phosphorus compounds such as ammonium polyphosphate, ethylene bis tris(2-cyanoethyl)phosphonium chloride, tris(tribromophenyl)phosphate, tris(tribromophenyl)phosphate, tris(3-hydroxypropyl)phosphine oxide, etc., chlorine-based flame retardants such as chlorinated paraffins, chlorinated polyolefins, perchlorocyclopentadecane, etc., bromine-based flame retardants such as hexabromobenzene, ethylene bis dibromonorbornane dicarboximide, ethylene bis tetrabromophthalimide, tetrabromobisphenol A derivatives, tetrabromobisphenol S, and tetrabromodipentaerythritol, etc., and mixtures thereof.

[0070] Examples of the ultraviolet absorbing agent include benzotriazole-based, benzophenone-based, salicylic acid-based, and acrylate-based agents.

[0071] Examples of antibacterial agents include quaternary ammonium salts, pyridine compounds, organic acids, organic acid esters, halogenated phenols, and organic iodines.

[0072] The surfactant may be a nonionic, anionic, cationic or amphoteric surfactant. Examples of the nonionic surfactant include polyethylene glycol type nonionic surfactants such as higher alcohol ethylene oxide adducts, fatty acid ethylene oxide adducts, higher alkylamine ethylene oxide adducts, and polypropylene glycol ethylene oxide adducts, polyethylene oxide, fatty acid esters of glycerin, fatty acid esters of pentaerythritol, fatty acid esters of sorbitol or sorbitan, alkyl ethers of polyhydric alcohols, and polyhydric alcohol type nonionic surfactants such as aliphatic amides of alkanolamines. Examples of the anionic surfactant include sulfate ester salts such as alkali metal salts of higher fatty acids, sulfonates such as alkylbenzene sulfonates, alkyl sulfonates, and paraffin sulfonates, and phosphate ester salts such as higher alcohol phosphate ester salts. Examples of the cationic surfactant include quaternary ammonium salts such as alkyltrimethylammonium salts. Examples of the amphoteric surfactant include amino acid type amphoteric surfactants such as higher alkylaminopropionates, and betaine type amphoteric surfactants such as higher alkyldimethyl betaines and higher alkyldihydroxyethyl betaines.

[0073] Examples of the antistatic agent include the above-mentioned surfactants, fatty acid esters, and polymeric antistatic agents. Examples of the fatty acid esters include esters of stearic acid and oleic acid, and examples of the polymeric antistatic agents include polyether ester amides.

[0074] Examples of pigments include inorganic pigments (titanium oxide, iron oxide, chromium oxide, cadmium sulfide, etc.) and organic pigments (azo lake type, thioindigo type, phthalocyanine type, anthraquinone type). Examples of dyes include azo type, anthraquinone type, triphenylmethane type, etc. The amount of these pigments and dyes to be added is not particularly limited, but is usually 5 parts by mass or less, preferably 0.1 to 3 parts by mass, in total, based on 100 parts by mass of the copolymer (A).

[0075] Examples of anti-slip agents include waxes (such as carnauba wax), higher fatty acids (such as stearic acid), higher fatty acid salts (such as calcium stearate), higher alcohols (such as stearyl alcohol), higher fatty acid amides (such as stearamide, erucic acid amide), and the like.

[0076] The amount of each of the above-mentioned various additives to be added is not particularly limited depending on the application as long as the object of the present invention is not impaired. However, it is preferable that each of the additives is added in an amount of 0.01 to 30 parts by mass relative to 100 parts by mass of the thermoplastic resin (A).

[0077] <Production of Resin Composition (X)> The resin composition (X) can be obtained, for example, by dry blending the thermoplastic resin (A), the carbon-based filler (B), and any other components that may be added, followed by melt-kneading in a single-screw or twin-screw extruder, a Banbury mixer, or a pressure kneader, extruding the mixture into strands, and granulating the extruded mixture into pellets. Note that the components such as the carbon-based filler (B) and the inorganic filler may be mixed in advance with the resin components such as the thermoplastic resin (A) to be used in the form of a master batch.

[0078] [Molded body] The molded article of the present embodiment includes the resin composition (X). Specific examples of the molding method include conventionally known polyolefin molding methods, such as extrusion molding, injection molding, film molding, inflation molding, blow molding, extrusion blow molding, injection blow molding, press molding, vacuum molding, powder slush molding, calendar molding, and foam molding. The molded article of the present embodiment including the resin composition (X) can be obtained by processing the resin composition (X) preferably by injection molding. As the molded article, a molded article including a resin composition (X) containing carbon nanotubes as the carbon-based filler (B) is preferred.

[0079] The molded article may be a molded article formed from the resin composition (X) or may be a molded article having a portion, such as a surface layer, formed from the resin composition.

[0080] Furthermore, the molded article of this embodiment is also excellent in mechanical properties. Molded articles are used in a wide range of applications, from household goods such as daily necessities and recreational uses to general industrial and industrial products, including home appliance material parts, communication device parts, electric parts, electronic parts, automotive materials, other vehicle parts, ships, aircraft materials, machine mechanism parts, building materials, civil engineering materials, agricultural materials, power tool parts, food containers, films, sheets, fibers, toys, etc.

[0081] Examples of automotive materials include front doors, back doors, sliding doors, front end modules, door modules, fenders, wheel caps, gasoline tanks, seats (padding, outer material, etc.), belts, ceiling coverings, convertible tops, armrests, door trims, rear package trays, carpets, mats, sun visors, wheel covers, tires, mattress covers, airbags, connectors, insulation materials, hanging handles, hanging handle straps, wire covering materials, electrical insulation materials, paints, coating materials, covering materials, flooring materials, corner walls, deck panels, covers, plywood, ceiling panels, partition panels, side walls, carpets, wallpaper, wall covering materials, exterior materials, interior materials, roofing materials, soundproofing boards, heat insulating boards, and window materials.

[0082] Examples of home appliance material parts, communication equipment parts, electrical parts, and electronic parts include office and OA equipment such as printers, personal computers, word processors, keyboards, PDAs (Personal Digital Assistants), headphone stereos, mobile phones, telephones, facsimiles, copiers, ECRs (Electronic Cash Registers), calculators, electronic organizers, electronic dictionaries, cards, holders, and stationery; home appliances such as washing machines, refrigerators, vacuum cleaners, microwave ovens, lighting fixtures, game consoles, irons, and kotatsu; AV equipment such as TVs, VTRs, video cameras, radio cassette players, tape recorders, minidiscs, CD players, speakers, and liquid crystal displays; connectors, relays, capacitors, switches, printed circuit boards, coil bobbins, semiconductor encapsulation materials, electric wires, cables, transformers, sensors, deflection yokes, distribution boards, clocks, and robot materials.

[0083] Examples of everyday items include clothing, curtains, sheets, plywood, synthetic boards, carpets, entrance mats, seats, buckets, hoses, containers, glasses, bags, cases, goggles, skis, rackets, tents, bicycles, musical instruments, and other lifestyle and sporting goods. EXAMPLES

[0084] The present invention will now be described in detail with reference to examples, but the present invention is not limited to these examples. Various physical properties in the examples and comparative examples were measured by the following methods.

[0085] 〔composition〕 The content (mol%) of each structural unit (4-methyl-1-pentene and α-olefin) in the 4-methyl-1-pentene copolymer (A-1) is 13 Measurements were performed by C-NMR. Measurement equipment: Nuclear magnetic resonance equipment (ECP500, manufactured by JEOL Ltd.) Observation core: 13 C(125MHz) Sequence: Single pulse proton decoupling Pulse width: 4.7μsec (45° pulse) Repeat time: 5.5 seconds -Number of times: 10,000 or more Solvent: orthodichlorobenzene / deuterated benzene (volume ratio: 80 / 20) mixed solvent Sample concentration: 55mg / 0.6mL ·Measurement temperature: 120℃ Chemical shift reference value: 27.50 ppm

[0086] [Intrinsic viscosity [η]] The intrinsic viscosity [η] of the copolymer was measured at 135° C. in decalin solvent using an Ubbelohde viscometer as the measuring device. About 20 mg of a specific 4-methyl-1-pentene (4MP1) copolymer was dissolved in 25 ml of decalin, and the specific viscosity ηsp was measured in an oil bath at 135°C using an Ubbelohde viscometer. After diluting the decalin solution by adding 5 ml of decalin, the specific viscosity ηsp was measured in the same manner as above. This dilution procedure was repeated two more times, and the value of ηsp / C when the concentration (C) was extrapolated to 0 was calculated as the limiting viscosity [η] (unit: dl / g) (see formula 1 below). [η]=lim(ηsp / C) (C→0)...Equation 1

[0087] [Weight average molecular weight (Mw) and molecular weight distribution (Mw / Mn)] The weight average molecular weight (Mw) of the copolymer and the molecular weight distribution (Mw / Mn), which is expressed as the ratio of the weight average molecular weight (Mw) to the number average molecular weight (Mn), were calculated by a standard polystyrene conversion method using gel permeation chromatography (GPC).

[0088] -conditions- Measurement equipment: GPC (ALC / GPC 150-C plus type, differential refractometer detector integrated type, Waters) Column: Two GMH6-HT (Tosoh Corporation) and two GMH6-HTL (Tosoh Corporation) connected in series Eluent: o-dichlorobenzene Column temperature: 140℃ Flow rate: 1.0mL / min

[0089] [Melt flow rate (MFR)] The melt flow rate (MFR) of the copolymer was measured in accordance with ASTM D1238 at 230° C. under a load of 2.16 kg, with the unit being g / 10 min.

[0090] 〔density〕 The density of the copolymer was measured in accordance with JIS K7112 (density gradient tube method). 3 ) was used as an indicator of lightness.

[0091] [Melting point (Tm)] The melting point (Tm) of the copolymer was measured using a differential scanning calorimeter (DSC220C, manufactured by Seiko Instruments Inc.) as a measuring device. Approximately 5 mg of the polymer was sealed in an aluminum pan for measurement and heated from room temperature to 200°C at 10°C / min. In order to completely melt the polymer, it was held at 200°C for 5 minutes and then cooled to -50°C at 10°C / min. After leaving it at -50°C for 5 minutes, it was heated a second time to 200°C at 10°C / min, and the peak temperature (°C) in this second heating was taken as the melting point (Tm) of the polymer. When multiple peaks were detected, the peak detected on the highest temperature side was adopted.

[0092] [Dynamic Viscoelasticity] In the measurement of dynamic viscoelasticity, a 2 mm thick press sheet made of the copolymer or molded product to be measured was used as the measurement sample, and a 45 mm x 10 mm x 2 mm strip was cut out as required for the dynamic viscoelasticity measurement. Using an ANTON Paar MCR301, the temperature dependence of dynamic viscoelasticity was measured from -40 to 150°C at a frequency of 10 rad / s, and the temperature (tan δ peak temperature) at which the loss tangent (tan δ) due to the glass transition temperature reached its peak value (maximum value) in the range of 0 to 40°C, and the value of that peak value (tan δ peak value) were measured.

[0093] [Synthesis Example 1] <Synthesis of 4-methyl-1-pentene-α-olefin copolymer (A-1)> Into a 1.5 L stainless steel autoclave equipped with an agitator and thoroughly purged with nitrogen, 300 ml of n-hexane (dried over activated alumina under a dry nitrogen atmosphere) and 450 ml of 4-methyl-1-pentene were placed at 23° C. Into this autoclave, 0.75 ml of a 1.0 mmol / ml toluene solution of triisobutylaluminum (TIBAL) was placed, and the agitator was turned on. Next, the autoclave was heated until the internal temperature reached 60° C., and pressurized with propylene to a total pressure (gauge pressure) of 0.40 MPa.

[0094] Next, 0.34 ml of a toluene solution containing 1 mmol of methylaluminoxane (calculated as Al) and 0.01 mmol of diphenylmethylene(1-ethyl-3-t-butyl-cyclopentadienyl)(2,7-di-t-butyl-fluorenyl)zirconium dichloride, which had been prepared in advance, was pressed into the autoclave with nitrogen to initiate the polymerization reaction. During the polymerization reaction, the temperature inside the autoclave was adjusted to 60°C. 60 minutes after the start of polymerization, 5 ml of methanol was injected into the autoclave with nitrogen to terminate the polymerization reaction, and the pressure inside the autoclave was then reduced to atmospheric pressure. After the pressure was reduced, acetone was added to the reaction solution while stirring the reaction solution, to obtain a polymerization reaction product containing the solvent.

[0095] The resulting polymerization reaction product containing the solvent was then dried under reduced pressure at 100°C for 12 hours to obtain 36.9 g of powdered 4-methyl-1-pentene-α-olefin copolymer (A-1) (hereinafter referred to as "copolymer A-1"). The measurement results of various physical properties of the resulting copolymer A-1 are shown in Table 1. In Table 1, "4MP1" and "AO" refer to 4-methyl-1-pentene and α-olefin, respectively.

[0096] The content of 4-methyl-1-pentene in copolymer A-1 was 72.5 mol %, and the content of propylene was 27.5 mol %. The density of copolymer A-1 was 839 kg / m 3 The copolymer A-1 had an intrinsic viscosity [η] of 1.5 dl / g, a weight average molecular weight (Mw) of 337,000, a molecular weight distribution (Mw / Mn) of 2.1, and a melt flow rate (MFR) of 11 g / 10 min. The melting point (Tm) of the copolymer A-1 was not observed.

[0097] Method for producing a molded body The resin and carbon-based filler described in the Examples or Comparative Examples were put into the hopper of a KZW15 manufactured by Technovel Co., Ltd., and melt-kneaded at 200°C to produce resin composition pellets. The resin composition pellets were then put into the hopper of a Toshiba 75-ton injection molding machine manufactured by Toshiba Machine Co., Ltd., melted at 200°C, and injection-molded into a 40°C mold at an injection pressure of 50 MPa and a holding pressure of 30 to 40 MPa to produce a 130 mm x 130 mm x 2 mm thick flat molded body (press sheet) and a dumbbell-shaped molded body test piece conforming to ASTM D638 Type4.

[0098] Surface resistivity measurement The surface resistivity of the molded body was determined as follows. The surface resistivity of the 2.0 mm thick press sheet of the resin composition was measured using a digital ultra-high resistance / microammeter Model 8340A manufactured by ADC Corporation by the double ring method under conditions of room temperature, humidity of 50%, applied voltage of 10 V, and application time of 60 seconds.

[0099] Shrinkage rate The shrinkage rate was calculated by using the 2 mm thick press sheet as a measurement sample, measuring the difference in length between the four sides and the injection mold, and using the dimensional change relative to the mold length.

[0100] Tensile strength, tensile elongation The tensile strength and tensile modulus of the molded body were measured by a tensile test using the dumbbell-shaped molded body test piece. The tensile test was performed at 23° C. and a test speed of 50 mm / min using a five-strand tensile tester 2005X-5 manufactured by Intesco Co., Ltd. in accordance with ASTM D638.

[0101] [Examples 1 to 3] A carbon nanotube master batch (a master batch containing 15 wt% of carbon nanotube NC7000 manufactured by Nanosil Co., Ltd. as a carbon-based filler (B) and 85 wt% of 4-methyl-1-pentene-α-olefin copolymer (A-1) as a thermoplastic resin (A): a carbon-based filler master batch) was dry-blended with 4-methyl-1-pentene-α-olefin copolymer (A-1) as a thermoplastic resin (A) at the "mixing ratio" (parts by mass) shown in Table 2. From each mixing ratio, the "composition" ratio (mass%) of each component of the resin composition was calculated as shown in Table 2. Next, resin composition pellets and test pieces for measuring physical properties were prepared by the above-mentioned method. Using these test pieces, tensile tests, surface resistivity measurements, shrinkage measurements, and viscoelasticity measurements were performed.

[0102] [Comparative Example 1] Resin composition pellets and test pieces for measuring physical properties were prepared in the same manner as in Example 1, except that the carbon nanotube master batch was not used and only the 4-methyl-1-pentene / α-olefin copolymer (A-1), which is the thermoplastic resin (A), was used. Tensile tests, surface resistivity measurements, shrinkage rate measurements, and viscoelasticity measurements were then performed.

[0103] [Comparative Examples 2 and 3] A carbon-based filler master batch containing 25 wt % carbon black and 75 wt % polypropylene (DIC Corporation P-5050) was used instead of the carbon nanotube carbon filler master batch of Example 1, and the ratios of each raw material were as shown in Table 2. Except for this, resin composition pellets and test pieces for measuring physical properties were prepared in the same manner as in Example 1, and tensile tests, surface resistivity measurements, shrinkage rate measurements, and viscoelasticity measurements were performed.

[0104] The surface resistivity, shrinkage rate, tan δ peak value, tan δ peak temperature, tensile strength and tensile modulus of the molded bodies obtained in Examples 1 to 3 and Comparative Examples 1 to 3 are shown in Table 2. In Table 2, "CNT" means carbon nanotube, and "CB" means carbon black.

[0105] [Table 1]

[0106] [Table 2]

[0107] In the following Examples and Comparative Examples, the thermal conductivity and thermal resistance were determined by the following methods. (Thermal Conductivity) The thermal conductivity of the thermally conductive composition was measured by a steady-state heat flow meter method using a measuring instrument GH-1 manufactured by ULVAC-RIKO, in accordance with ASTM E1530, at a temperature of 30°C, a sample holding air pressure of 0.3 MPa, and a test piece of 50 mmφ. (thermal resistance) The thermal resistance was calculated using the following formula. Thermal resistance = test piece thickness / thermal conductivity

[0108] [Example 4] The test piece was prepared by the above-mentioned method using the resin composition described in Example 1 (a resin composition obtained by dry blending 100 parts by mass of 4-methyl-1-pentene-α-olefin copolymer (A-1) and 25 parts by mass of the carbon nanotube master batch). The results of the thermal conductivity measurement and thermal resistance obtained by the above-mentioned method are shown in Table 3.

[0109] [Example 5] The test piece was prepared by the above-mentioned method using the resin composition described in Example 2 (a resin composition obtained by dry blending 100 parts by mass of 4-methyl-1-pentene-α-olefin copolymer (A-1) and 66 parts by mass of the carbon nanotube master batch) and the results of the thermal conductivity measurement and thermal resistance obtained by the above-mentioned method are shown in Table 3.

[0110] [Example 6] The test piece was prepared by the above-mentioned method using the resin composition described in Example 3 (a resin composition obtained by dry blending 100 parts by mass of 4-methyl-1-pentene-α-olefin copolymer (A-1) and 115 parts by mass of the carbon nanotube master batch) and the results of the thermal conductivity measurement and thermal resistance obtained by the above-mentioned method are shown in Table 3.

[0111] [Comparative Example 4] The test piece was prepared by the above-mentioned method using the resin composition described in Comparative Example 1, and the results of the thermal conductivity measurement and thermal resistance obtained by the above-mentioned method are shown in Table 3.

[0112] [Comparative Example 5] The test piece was prepared by the above-mentioned method using the resin composition described in Comparative Example 2 (a resin composition obtained by dry blending 100 parts by mass of 4-methyl-1-pentene-α-olefin copolymer (A-1) and 11 parts by mass of a carbon black master batch). The results of the thermal conductivity measurement and thermal resistance obtained by the above-mentioned method are shown in Table 3.

[0113] [Comparative Example 6] The test piece was prepared by the above-mentioned method using the resin composition described in Comparative Example 3 (a resin composition obtained by dry blending 100 parts by mass of 4-methyl-1-pentene-α-olefin copolymer (A-1) and 43 parts by mass of carbon black master batch). The results of the thermal conductivity measurement and thermal resistance obtained by the above-mentioned method are shown in Table 3.

[0114] In Table 3, "CNT" means carbon nanotube and "CB" means carbon black.

[0115] [Table 3]

Claims

1. 80.0 to 99.9 parts by mass of a 4-methyl-1-pentene / α-olefin copolymer (A-1) that contains a structural unit (i) derived from 4-methyl-1-pentene and a structural unit (ii) derived from an α-olefin having from 2 to 5 carbon atoms and satisfies the following requirements (d) to (g); A resin composition (X) comprising 0.1 to 20.0 parts by mass of a carbon-based filler (B) which is a carbon nanotube (the total of the copolymer (A-1) and the carbon-based filler (B) being 100 parts by mass), and satisfying the following requirements (a) to (c): Requirement (a): The temperature at which the loss tangent tan δ, which is obtained by performing dynamic viscoelasticity measurement at a frequency of 10 rad / s (1.6 Hz) in the temperature range of −40 to 150° C., reaches a peak value, is 0° C. or higher and 60° C. or lower. Requirement (b): The peak value of loss tangent tan δ obtained by performing dynamic viscoelasticity measurement at a frequency of 10 rad / s (1.6 Hz) in a temperature range of −40 to 150° C. is 0.5 or more and 5.0 or less. Requirement (c): The surface resistivity is 10^14 Ω or less. Requirement (d): The copolymer (A-1) contains 55 to 90 mol % of the structural unit (i) and 10 to 45 mol % of the structural unit (ii), with the total of the structural unit (i) and the structural unit (ii) being 100 mol %. Requirement (e): The copolymer (A-1) has a melting point (Tm) measured by a differential scanning calorimeter (DSC) of 160° C. or less, or the melting point cannot be measured by a differential scanning calorimeter. Requirement (f): The copolymer (A-1) has a peak temperature of loss tangent tan δ, which is obtained by measuring dynamic viscoelasticity at a frequency of 10 rad / s (1.6 Hz) in a temperature range of −40 to 150° C., of 15° C. or more and 45° C. or less. Requirement (g): The copolymer (A-1) has a peak value of loss tangent tan δ of 0.6 or more and 5.0 or less, as determined by dynamic viscoelastic measurement at a frequency of 10 rad / s (1.6 Hz) in a temperature range of −40 to 150° C.

2. The resin composition (X) according to claim 1, wherein the α-olefin having 2 to 5 carbon atoms from which the structural unit (ii) contained in the copolymer (A-1) is derived is propylene.

3. A molded article comprising the resin composition (X) according to claim 1 or 2.

4. A sheet comprising the resin composition (X) according to claim 1 or 2.

5. A toy comprising the resin composition (X) according to claim 1 or 2.

6. 3. Daily necessities comprising the resin composition (X) according to claim 1 or 2.

7. An automotive material comprising the resin composition (X) according to claim 1 or 2.

8. An electronic part comprising the resin composition (X) according to claim 1 or 2.

Citation Information

Patent Citations

  • Electroconductive resin composition, fuel cell separator and its manufacturing method

    JP2004217689A

  • Method for improving conductivity of resin molded body comprising carbon nanotube by heat treatment

    JP2009074072A

  • Resin composition

    JP2010196012A

  • Vibrationproof material, and vibrationproof member

    JP2012082388A

  • Thermoplastic polymer composition and application thereof

    JP2014210869A