Expandable composite resin particles, expanded particles
By optimizing the ethylene-styrene ratio and incorporating a brominated bisphenol flame retardant with specific viscosity, the composite resin particles achieve improved flame retardancy and foaming properties, addressing the limitations of existing technologies.
Patent Information
- Application Number
- JP2020170967
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-10-09
- Publication Date
- 2024-10-02
- Estimated Expiration
- 2040-10-09
AI Technical Summary
Existing expandable composite resin particles lack balanced improvement in flame retardancy, foaming agent retention, and foamability, leading to inadequate performance in molded articles.
The development of composite resin particles comprising a 50:50 to 5:95 mass ratio of ethylene and styrene components, with a brominated bisphenol flame retardant and specific complex shear viscosity, ensuring excellent flame retardancy and foaming properties.
The solution results in molded articles with stable and enhanced flame retardancy, foaming agent retention, and foamability, meeting FMVSS302 standards for automobile interiors.
Smart Images

Figure 0007560311000001 
Figure 0007560311000002 
Figure 0007560311000003
Abstract
Description
[Technical field]
[0001] The present invention relates to expandable composite resin particles and expanded composite resin particles containing a flame retardant. [Background technology]
[0002] Background Art Expanded bead molded articles (hereinafter also referred to as expanded bead molded articles or molded articles) using a composite resin containing an ethylene-based resin component and a styrene-based resin component as a base resin have excellent rigidity, resilience, cushioning properties, etc., and are therefore used as packaging materials for precision parts and heavy products, as well as automotive components such as bumpers and floor spacers.
[0003] Such a molded article is produced, for example, by using expandable composite resin particles as follows. First, an organic physical blowing agent such as butane or pentane is impregnated into the composite resin particles to produce expandable composite resin particles. Next, the expandable composite resin particles are heated with steam or the like to expand the expandable composite resin particles to obtain expanded particles. Next, the expanded particles are expanded in a mold by in-mold molding, and the expanded particles are fused to each other. In this manner, a molded article can be obtained.
[0004] On the other hand, since the molded article obtained as described above is flammable, techniques for imparting flame retardancy to the molded article have been developed. For example, Patent Document 1 proposes expandable composite resin particles containing a brominated styrene-butadiene copolymer as a flame retardant. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2016-180038 A Summary of the Invention [Problem to be solved by the invention]
[0006] In recent years, there has been a demand for further improvement in flame retardancy of the expanded bead molding obtained by using the expandable composite resin particles. In addition, there has been a demand for the expandable composite resin particles to be excellent in retention of the blowing agent and foaming property while enabling the production of a molding having excellent flame retardancy as described above. In terms of improving such flame retardancy, retention of the blowing agent, and foaming property to a high level in a well-balanced manner, there is still room for improvement in the conventional expandable composite resin particles.
[0007] The present invention has been made in consideration of the above background, and aims to provide composite resin foam beads that can give foamed bead moldings that stably exhibit excellent flame retardancy, and expandable composite resin beads that can be produced from the composite resin foam beads and have excellent foaming agent retention and expandability. [Means for solving the problem]
[0008] One aspect of the present invention is an expandable composite resin particle, which comprises a composite resin obtained by impregnating and polymerizing an ethylene-based resin with a styrene-based monomer as a base resin, and which contains a blowing agent and a flame retardant in the base resin, a mass ratio of the component derived from the ethylene-based resin to the component derived from the styrene-based monomer is 50:50 to 5:95; The content of the blowing agent in the expandable composite resin particles is 3 to 10% by mass, The flame retardant is a brominated bisphenol flame retardant, The complex shear viscosity η of the composite resin containing the flame retardant is 500 to 300°C at an angular frequency of 1 rad / s and a temperature of 300°C, as measured based on JIS K 7244-10:2005. 2000 The expandable composite resin particles have a thermal expansion coefficient of 1.0 Pa·s.
[0009] Another aspect of the present invention is a composite resin foam particle obtained by foaming an expandable composite resin particle containing a foaming agent and a flame retardant in a base resin, the composite resin being a base resin obtained by impregnating and polymerizing a styrene monomer into an ethylene resin, the base resin comprising: The flame retardant is a brominated bisphenol flame retardant, a mass ratio of the component derived from the ethylene-based resin to the component derived from the styrene-based monomer is 50:50 to 5:95 by mass ratio; The complex shear viscosity η of the composite resin containing the above flame retardant is 500 to 1000 mmHg, measured at a frequency of 1 rad / s and a temperature of 300°C according to JIS K 7244-10:2005. 2000 The composite resin foam particles have a thermal conductivity of 1.0 Pa·s. Effect of the Invention
[0010] The composite resin foam particles can provide a molded article that stably exhibits excellent flame retardancy. The expandable composite resin particles have excellent foaming agent retention and expandability, and the expandable composite resin particles can provide a molded article that stably exhibits excellent flame retardancy. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] Next, preferred embodiments of the expandable composite resin particles and the composite resin foamed particles will be described. In this specification, when "~" is used with a numerical value or a physical property value before and after it, it is used to include the values before and after it. In addition, parts by mass and parts by weight have substantially the same meaning, mass% and weight% have substantially the same meaning, and mass ppm and weight ppm have substantially the same meaning.
[0012] Expandable composite resin particles (hereinafter referred to as "expandable particles") have a composite resin as a base resin obtained by impregnating and polymerizing an ethylene-based resin with a styrene-based monomer. Such a composite resin contains at least an ethylene-based resin component derived from an ethylene-based resin and a styrene-based resin component derived from a styrene-based monomer. In other words, expandable particles have a composite resin as a base resin containing an ethylene-based resin component and a styrene-based resin component, and contain a blowing agent and a flame retardant in this base resin.
[0013] A composite resin expanded bead (hereinafter referred to as "expanded bead") is a particulate foam whose base resin is a composite resin obtained by impregnating and polymerizing an ethylene-based resin with a styrene-based monomer, and which contains a flame retardant in the base resin. The expanded bead is composed of a composite resin containing at least an ethylene-based resin component and a styrene-based resin component, and has a structure containing a large number of bubbles. The expanded bead can be obtained, for example, by expanding the above-mentioned expandable bead.
[0014] The expanded beads are used, for example, to produce a molded article by expanding the expanded beads in a mold and fusing the expanded beads to each other. Such a molded article is formed by fusing a large number of expanded beads to each other.
[0015] Since the expandable particles and the expanded particles have a composite resin of an ethylene-based resin component and a styrene-based resin component as the base resin as described above, the molded article has both the properties of an ethylene-based resin and the properties of a styrene-based resin. Specifically, by sufficiently fusing the expanded particles, the molded article can have both excellent toughness and excellent rigidity.
[0016] In the expandable particles and the expanded particles, the mass ratio of the component derived from the ethylene resin and the component derived from the styrene monomer is 50:50 to 5:95. Therefore, the ratio of the ethylene resin component and the styrene resin component is good. As a result, the expandable particles have excellent retention of the blowing agent, and therefore transportation and storage in the form of expandable particles are possible. In addition, the expandable particles have excellent expandability and can be expanded at a high ratio. Furthermore, the molded body is lightweight and exhibits excellent rigidity and toughness. From the viewpoint of improving such effects, the mass ratio of the component derived from the ethylene resin and the component derived from the styrene monomer is preferably 40:60 to 6:94, more preferably 30:70 to 8:92, even more preferably 20:80 to 10:90, and particularly preferably 18:82 to 10:90.
[0017] As the ethylene-based resin component, for example, linear low-density polyethylene, branched low-density polyethylene, high-density polyethylene, ethylene-acrylic acid copolymer, ethylene-acrylic acid alkyl ester copolymer, ethylene-methacrylic acid alkyl ester copolymer, ethylene-vinyl acetate copolymer, or a mixture of two or more of these can be used. Among these, it is preferable to use at least linear low-density polyethylene as the ethylene-based resin. In this case, the molded article has better toughness. The linear low-density polyethylene is a copolymer of ethylene and an α-olefin such as 1-butene or 1-hexene, and has a density of about 0.910 g / cm. 3 More than 0.930g / cm 3 means something less than.
[0018] The content of linear low density polyethylene in 100% by mass of the ethylene-based resin is preferably 50% by mass or more from the viewpoint of improving the toughness of the molded article. From the above viewpoint, the content of linear low density polyethylene is more preferably 70% by mass or more, and even more preferably 80% by mass or more, and it is even more preferable that the ethylene-based resin is substantially composed of linear low density polyethylene. Here, the ethylene-based resin is substantially composed of linear low density polyethylene, which means that the content of linear low density polyethylene is more than 95% by mass. Furthermore, from the viewpoint of further increasing the strength of the molded article against bending deformation, the content of the vinyl acetate component in the composite resin is preferably less than 0.2% by mass.
[0019] Among linear low density polyethylenes, linear low density polyethylenes polymerized using a metallocene polymerization catalyst are more preferred. In this case, the toughness of the molded article is further improved. In addition, in this case, the amount of low molecular weight components contained in the expandable particles is reduced, and the fusion strength between the expanded particles of the molded article can be further increased, making it possible to produce a molded article that is less susceptible to cracking. Furthermore, a molded article can be obtained that combines the excellent rigidity of a styrene-based resin and the excellent toughness of an ethylene-based resin at a higher level.
[0020] From the viewpoint of foaming property, the melt mass flow rate (MFR 190°C, load 2.16 kg) of the ethylene resin is preferably 0.5 to 4.0 g / 10 min, more preferably 1.0 to 3.0 g / 10 min. The MFR (190°C, load 2.16 kg) of the ethylene resin is a value measured under condition code D based on JIS K7210 (1999). As a measuring device, a melt indexer (for example, Model L203 manufactured by Takara Kogyo Co., Ltd.) can be used.
[0021] The melting point (Tm) of the ethylene-based resin is preferably 80°C to 115°C. In this case, the ethylene-based resin can be sufficiently impregnated with the styrene-based monomer during the production of the expandable particles, and the suspension system can be prevented from becoming unstable during polymerization. As a result, by using the expandable particles, it is possible to obtain a molded product having both the excellent rigidity of the styrene-based resin and the excellent toughness of the ethylene-based resin at a higher level. From the same viewpoint, the melting point (Tm) of the ethylene-based resin is more preferably 85°C to 110°C. The melting point (Tm) of the ethylene-based resin can be measured by differential scanning calorimetry (DSC) based on JIS K7121 (1987).
[0022] As described above, the composite resin is a resin obtained by impregnating and polymerizing an ethylene-based resin with a styrene-based monomer, and is a resin containing a component derived from an ethylene-based resin and a component derived from a styrene-based monomer. Note that the main component of the component derived from the styrene-based monomer is a styrene-based resin obtained by polymerizing the styrene-based monomer. The composite resin is a concept different from a mixed resin obtained by melt-kneading a polymerized ethylene-based resin and a polymerized styrene-based resin. In this specification, styrene and a monomer copolymerizable with styrene are referred to as a styrene-based monomer. As the styrene-based monomer, styrene may be used alone, or a monomer copolymerizable with styrene may be used in combination with styrene. The styrene-based monomer will be described later.
[0023] Examples of the styrene-based resin component include polystyrene and copolymers containing at least a structural unit derived from styrene. Specific examples include polystyrene, rubber-modified polystyrene, acrylonitrile-butadiene-styrene resin, acrylonitrile-styrene resin, acrylonitrile-ethylene-styrene resin, and mixtures of two or more of these. Among these, preferred are polystyrene and copolymers of styrene and an acrylic monomer such as butyl acrylate. However, it is preferable that the copolymer contains 50% by mass or more of a component derived from styrene.
[0024] The expandable particles and the expanded particles have a composite resin as a base resin as described above, and contain a flame retardant in the base resin (i.e., the composite resin). The flame retardant is a brominated bisphenol-based flame retardant. Examples of the brominated bisphenol-based flame retardant include bisphenol A, bisphenol F, bisphenol S, or brominated derivatives thereof, and more specifically, 2,2-bis(4-(2,3-dibromo-2-methylpropoxy)-3,5-dibromophenyl)propane, bis[3,5-dibromo-4-(2,3-dibromopropoxy)phenyl]sulfone, 2,2-bis(4-(2,3-dibromopropoxy)-3,5-dibromophenyl)propane, etc. are used. One or more of these brominated flame retardants are used. From the viewpoint that even a small amount of addition can easily impart excellent flame retardancy to a molded body, it is preferable to use, among brominated bisphenol-based flame retardants, a brominated bisphenol-based flame retardant having a 2,3-dibromo-2-methylpropyl group and / or a brominated bisphenol-based flame retardant having a 2,3-dibromopropyl group, and it is more preferable to use 2,2-bis(4-(2,3-dibromo-2-methylpropoxy)-3,5-dibromophenyl)propane.
[0025] The 50% decomposition temperature of the brominated bisphenol flame retardant is preferably 280° C. or more and 340° C. or less, more preferably 285° C. or more and 320° C. or less. In this case, the complex shear viscosity of the composite resin is easily adjusted to a desired range in the temperature range in which the thermal decomposition of the composite resin proceeds. This makes it possible to impart more stable and excellent flame retardancy to the molded product without reducing the expandability of the expandable particles or the retention of the blowing agent. The 50% decomposition temperature of the brominated flame retardant can be measured by a thermogravimetric and differential thermogravimetric analyzer (TG / DTA). Specifically, a differential thermal weight loss curve is measured under the following measurement conditions: heating rate: 10°C / min, measurement temperature range: 40°C to 500°C, in a nitrogen atmosphere, sample pan material: Pt, sample mass: 50 mg, and the temperature at which the weight is reduced by 50% in the differential thermal weight loss curve can be determined as the 50% decomposition temperature.
[0026] The complex shear viscosity η of the composite resin containing a brominated bisphenol-based flame retardant is 500 to 5000 Pa·s. When the complex shear viscosity η of the composite resin containing a brominated bisphenol as a flame retardant is in this range, the flame retardancy of the molded body can be improved without decreasing the expandability of the expandable particles. The excellent flame retardancy achieved by using a brominated bisphenol-based flame retardant and having a complex shear viscosity η in the above range is thought to be expressed as follows. Usually, when a molded body is burned, the vicinity of the burning part of the molded body becomes hot, and the resin near the burning part melts. In this case, if the complex shear viscosity is too low, the fluidity of the molten resin is high, so the molten resin falls off the molded body early, and the burning of the molded body is likely to continue. On the other hand, if the complex shear viscosity is within the above range, the fluidity of the molten resin is relatively low, so the molten resin is likely to remain near the burning part of the molded body. As a result, the vicinity of the burning part is likely to be covered with a coating layer formed of a molten resin containing a brominated bisphenol flame retardant. When such a coating layer containing a brominated bisphenol flame retardant is formed, the vicinity of the burning part is shielded from the flame, so that oxygen is effectively blocked near the burning part, and the thermal decomposition of the resin is suppressed, and the amount of flammable gas generated is thought to be reduced. As a result, combined with the effect of the brominated bisphenol flame retardant blended in the composite resin, the molded body becomes less flammable, and it is thought that excellent flame retardancy can be imparted to the molded body. As described above, when the composite resin contains a brominated bisphenol-based flame retardant as a flame retardant and has a complex shear viscosity η of 500 to 5,000 Pa s, the expandable particles maintain excellent expandability while the molded product stably exhibits high flame retardancy that satisfies FMVSS 302, the combustion test standard for automotive interior materials.
[0027] If the complex shear viscosity η is too low, the area near the burning part is not easily covered with the molten resin when the molded body is burned, and the flame retardancy is reduced. On the other hand, if the complex shear viscosity η is too high, the expandability of the expandable particles is deteriorated, and it becomes impossible to expand the particles to a desired bulk expansion ratio, for example, 25 times or more. In addition, when the flame retardant does not contain a brominated bisphenol flame retardant, for example, when a brominated-styrene-butadiene copolymer as described in Patent Document 1 is used as a flame retardant by blending it with the core particles, even if the complex shear viscosity η is within the above range, it may be difficult to stably exhibit high flame retardancy depending on the expansion ratio, the foaming agent composition, etc. In addition, in order to obtain the desired flame retardancy, for example, it becomes necessary to add a large amount of flame retardant, and this may cause a decrease in the moldability of the expanded beads and the bending properties of the molded body. From the viewpoint of stably increasing the flame retardancy, the complex shear viscosity η of the composite resin containing a brominated bisphenol flame retardant is preferably 600 Pa·s or more, more preferably 800 Pa·s or more, even more preferably 900 Pa·s or more, and particularly preferably 1000 Pa·s or more. From the viewpoint of more stably increasing the expandability of the expandable particles and the in-mold moldability of the expanded particles, the complex shear viscosity η is preferably 4000 Pa·s or less, more preferably 3000 Pa·s or less, even more preferably 2500 Pa·s or less, even more preferably 2000 Pa·s or less, and particularly preferably 1800 Pa·s or less.
[0028] The complex shear viscosity η of the composite resin containing a flame retardant is measured based on JIS K 7244-10:2005. The complex shear viscosity η of the composite resin is a value at an angular frequency of 1 rad / s and a temperature of 300°C. The complex shear viscosity η is a value measured by a viscoelasticity measuring device. In such a measurement, the viscosity of the measurement target can be measured at high temperatures with a small load applied to the measurement target, so that the state of the composite resin during combustion can be suitably evaluated by employing the complex shear viscosity η. In addition, the measurement temperature of the complex shear viscosity η, 300°C, is the temperature immediately before the composite resin starts to thermally decompose. This temperature immediately before (i.e., 300°C) is a suitable temperature for evaluating the state of the composite resin during combustion. The complex shear viscosity η of the composite resin containing a flame retardant can be measured by preparing a measurement sample of a predetermined shape using expandable particles, expanded particles, or an expanded particle molded product obtained by molding expanded particles in a mold, and performing a predetermined analysis on the measurement sample using a viscoelasticity measuring device. The measurement sample can be prepared, for example, by performing hot press molding on expandable particles from which the blowing agent has been dispersed, or on expanded particles or an in-mold molded product that has been defoamed as necessary. In addition, when a measurement sample is prepared using any of expandable beads, expanded beads, and expanded bead moldings obtained by molding expanded beads in a mold, the complex shear viscosity η measured for these measurement samples is equivalent.
[0029] The complex shear viscosity η of the composite resin is adjusted to the desired range by adjusting the molecular weight (specifically, the weight average molecular weight Mw) of the styrene resin component, the amount of xylene insoluble matter (i.e., gel) in the composite resin, the mass ratio of the ethylene resin component to the styrene resin component in the composite resin, the type and content of the flame retardant and flame retardant assistant, and the like. For example, with regard to the mass ratio of the ethylene resin component to the styrene resin component in the composite resin, the complex shear viscosity η tends to increase when the mass ratio of the ethylene resin component increases. For example, the complex shear viscosity η tends to increase when the content of the flame retardant and flame retardant assistant is reduced. In addition, the amount of xylene insoluble matter (i.e., gel) in the composite resin can be adjusted, for example, by a combination of polymerization initiators with different hydrogen abstraction capabilities. In addition, the complex shear viscosity η tends to increase by increasing the amount of polymerization initiators with relatively high hydrogen abstraction capabilities.
[0030] The blending amount of the flame retardant is preferably 0.1 to 3 parts by mass relative to 100 parts by mass of the composite resin. In this case, the flame retardancy of the molded body can be stably increased without decreasing the expandability of the expandable particles or the moldability of the expanded particles in the mold. From the viewpoint of stably increasing the flame retardancy of the molded body, the blending amount of the flame retardant is preferably 0.5 parts by mass or more relative to 100 parts by mass of the composite resin, more preferably 0.6 parts by mass or more, even more preferably 0.8 parts by mass or more, and particularly preferably 1.0 parts by mass or more. In addition, from the viewpoint of further increasing the bending strength of the molded body, the blending amount of the flame retardant is preferably 2.8 parts by mass or less relative to 100 parts by mass of the composite resin, more preferably 2.5 parts by mass or less, even more preferably 2.0 parts by mass or less, and particularly preferably 1.8 parts by mass or less. It is preferable that the flame retardant does not substantially contain a brominated styrene-butadiene copolymer. More specifically, the content of the brominated styrene-butadiene copolymer in the flame retardant is preferably 5% by mass or less, more preferably 3% by mass or less, and even more preferably 1% by mass or less. It is particularly preferable that the flame retardant does not contain a brominated styrene-butadiene copolymer.
[0031] The composite resin preferably contains a radical generator having a 10-hour half-life temperature of 150°C or more as a flame retardant auxiliary. In this case, the flame retardancy can be further improved while suppressing the decrease in toughness of the molded body. In addition, even if the amount of VOC (volatile organic compounds) in the expandable particles is reduced by a stripping treatment described later, a molded body having excellent flame retardancy can be obtained. Specific examples of such flame retardant auxiliary include 2,3-dimethyl-2,3-diphenylbutane, poly(1,4-diisopropylbenzene), 1,1,3,3-tetramethylbutyl hydroperoxide, cumene hydroperoxide, and t-butyl hydroperoxide. From the viewpoint of obtaining the above effect more stably, it is preferable to use 2,3-dimethyl-2,3-diphenylbutane or poly(1,4-diisopropylbenzene) as the radical generator, and it is more preferable to use 2,3-dimethyl-2,3-diphenylbutane. The 10-hour half-life temperature is defined as the temperature at which 50% of the amount of a radical generator, such as an organic peroxide, charged in an inert solvent is thermally decomposed in 10 hours. The 10-hour half-life temperature can be the value of the 10-hour half-life temperature listed in the catalog or technical documents issued by the manufacturer of the radical generator, such as an organic peroxide.
[0032] In the expandable particles, the mass ratio of the flame retardant assistant to the flame retardant is preferably 0.1 to 1. In this case, the effect of improving the bending strength of the molded article and the flame retardancy of the molded article in a well-balanced manner can be obtained. From the viewpoint of improving this effect, the mass ratio of the flame retardant assistant to the flame retardant is more preferably 0.15 to 0.6, and further preferably 0.2 to 0.5. If the blending amount (by mass) of the flame retardant in the expandable particles is a and the blending amount (by mass) of the flame retardant assistant is b, the mass ratio of the flame retardant assistant to the flame retardant is expressed as b / a. From the same viewpoint, the blending amount of the flame retardant auxiliary is preferably 0.1 to 1 part by mass, more preferably 0.2 to 0.5 parts by mass, and further preferably 0.3 to 0.4 parts by mass, per 100 parts by mass of the composite resin.
[0033] The glass transition temperature of the methyl ethyl ketone soluble matter in the composite resin is preferably 102° C. or higher, more preferably 103° C. or higher, and even more preferably 105° C. or higher. In this case, the mechanical properties of the molded body in a high-temperature environment are improved. The methyl ethyl ketone soluble matter in the composite resin is mainly a styrene-based resin component.
[0034] The glass transition temperature is measured, for example, as follows. Specifically, first, the composite resin (composite resin particles before impregnation with a blowing agent or expandable particles from which the blowing agent has been dispersed) is frozen with liquid nitrogen and frozen and pulverized by an analytical mill (for example, A-11 manufactured by IKA Co., Ltd.). The pulverized material is immersed in methyl ethyl ketone at a temperature of 23°C for a predetermined time, and then the methyl ethyl ketone soluble portion is separated. Next, the methyl ethyl ketone soluble portion is dropped into methanol to obtain a white precipitate, which is then thoroughly dried. Heat flux differential scanning calorimetry is performed on 2 to 4 mg of the obtained methanol insoluble portion using a differential scanning calorimeter (DSC) DSC250 manufactured by TA Instruments Co., Ltd. based on JIS K7121-1987. As the condition adjustment, (3) a certain heat treatment is carried out and then the glass transition temperature is measured. The glass transition temperature Tg of the methyl ethyl ketone soluble matter can be obtained as the midpoint glass transition temperature of the DSC curve obtained under the condition of a heating rate of 20°C / min.
[0035] The mass ratio of the xylene insoluble matter in the composite resin by Soxhlet extraction (i.e., mainly crosslinked polyolefin resin components) is preferably 5 mass% or more, more preferably 6 mass% or more, and even more preferably 8 mass% or more. In this case, a molded product that stably exhibits excellent flame retardancy is more likely to be obtained. On the other hand, the mass ratio of the xylene insoluble matter in the composite resin by Soxhlet extraction is preferably 20 mass% or less, more preferably 18 mass% or less, and even more preferably 16 mass% or less. In this case, the expandability of the expandable particles and the moldability of the expanded particles can be stably increased.
[0036] In the expandable beads, the weight average molecular weight of the styrene resin component is preferably 150,000 to 400,000, more preferably 180,000 to 350,000, and even more preferably 200,000 to 300,000. In this case, the shrinkage of the expanded beads can be further prevented. Furthermore, the fusion property between the expanded beads can be further improved during molding in the mold.
[0037] The expandable particles contain a foaming agent. The content of the foaming agent in the expandable particles is 3 to 10% by mass. By setting the content of the foaming agent in this range, the expandable particles have excellent foaming agent retention and expandability. From the viewpoint of further improving this effect, the content of the foaming agent in the expandable particles is preferably 4 to 9% by mass, and more preferably 5 to 8% by mass.
[0038] As the foaming agent, it is preferable to use an organic physical foaming agent, for example, a saturated hydrocarbon having 3 to 6 carbon atoms. In this case, the foaming agent retention and foaming ability of the expandable particles are excellent. Furthermore, the fusion between the expanded particles in the molded product is further improved. As the saturated hydrocarbon, for example, propane, n-butane, isobutane, cyclobutane, n-pentane, isopentane, neopentane, cyclopentane, n-hexane, cyclohexane, etc. can be used. These foaming agents can be used alone or in a mixture of two or more kinds.
[0039] The foaming agent preferably contains isobutane. The content of isobutane in the foaming agent is preferably 50% by mass or more, more preferably 60% by mass or more, even more preferably 70% by mass or more, and particularly preferably more than 80% by mass. In this case, the expandability of the expandable particles and the retention of the foaming agent can be stably increased, and the decrease in flame retardancy of the molded body caused by the foaming agent can be suppressed. In addition, the expandable particles of the present disclosure contain a brominated bisphenol-based flame retardant as a flame retardant, and the complex shear viscosity η of the composite resin is adjusted to a predetermined range, so that even if the isobutane ratio in the foaming agent is increased as described above, a molded body with excellent flame retardancy can be obtained.
[0040] The content of unreacted styrene-based monomer remaining in the expandable particles is preferably 50 mass ppm or less (including 0). In this case, a molded article having a low content of VOC (volatile organic compounds) and excellent flame retardancy can be obtained, and a molded article that can be suitably used as a vehicle member or a building member can be obtained. The content of unreacted styrene-based monomer in the expandable particles is more preferably less than 30 ppm (including 0), and further preferably 25 ppm or less (including 0). The content of styrene-based monomer in the expandable particles can be reduced to the above range by, for example, performing a stripping treatment. The stripping treatment will be described later, and is an operation in which the composite resin particles are heated in an aqueous medium to extract and remove the VOC components (specifically, the unreacted styrene-based monomer) in the composite resin together with the evaporated water.
[0041] The expandable particles are produced, for example, by carrying out a dispersion step, a modification step, and an impregnation step. In the dispersion step, core particles composed of an ethylene-based resin are dispersed in an aqueous medium. In the modification step, a styrene-based monomer in which a flame retardant is dissolved is added to an aqueous medium, and the core particles are impregnated and polymerized with the styrene-based monomer to obtain composite resin particles in which the composite resin is used as a base resin and the base resin contains a flame retardant. In the impregnation step, the composite resin particles are impregnated with a blowing agent during and / or after polymerization of the composite resin particles.
[0042] The amount of the styrene monomer blended in the modification step relative to 100 parts by mass of the ethylene resin is, for example, from 100 parts by mass to 1900 parts by mass, and particularly preferably from more than 500 parts by mass to 1000 parts by mass.
[0043] The polymerization of the styrene monomer can be carried out in the presence of a polymerization initiator. As the polymerization initiator, an organic peroxide A having a t-butoxy group and a 10-hour half-life temperature of 80 to 120°C and an organic peroxide B having a t-hexyloxy group or a t-amyloxy group and a 10-hour half-life temperature of 80 to 120°C are used, and the ratio of the amount of the organic peroxide A to the total amount of the organic peroxide A and the organic peroxide B is adjusted to, for example, more than 85 mass%. Furthermore, a brominated bisphenol flame retardant is used as a flame retardant, and the amount of the flame retardant is adjusted to, for example, 0.1 to 3 mass parts per 100 mass parts of the total of the ethylene resin and the styrene monomer. In this way, the complex shear viscosity η of the composite resin containing the flame retardant, measured based on JIS K 7244-10:2005 at a frequency of 1 rad / s and a temperature of 300°C, can be adjusted to 500 to 5000 Pa·s. As described above, by adjusting the ratio of the amount of organic peroxide A to the total amount of organic peroxide A and organic peroxide B, whose 10-hour half-life temperatures are in the above-mentioned predetermined range, and by adjusting the amount of the brominated bisphenol-based flame retardant, the complex shear viscosity η of the composite resin can be adjusted to a desired range.
[0044] Each step will be described in detail below. In the dispersion step, the core particles made of the ethylene-based resin are dispersed in an aqueous medium to obtain a dispersion liquid. For example, a suspending agent, a surfactant, a water-soluble polymerization inhibitor, etc. can be added to the aqueous medium. The ethylene-based resin used for the core particles is as described above.
[0045] A dispersion diameter expanding agent can be blended with the core particles. By adding the dispersion diameter expanding agent, for example, the phase consisting of a styrene-based resin component can be enlarged. As the dispersion diameter expanding agent, for example, at least one selected from polystyrene, acrylonitrile-styrene copolymer, rubber-modified polystyrene, ABS resin, and AES resin can be used. An acrylonitrile-styrene copolymer is preferable. Also, the amount of the acrylonitrile component in the acrylonitrile-styrene copolymer is preferably 20 to 40% by mass.
[0046] The core particles may contain various additives as long as they do not impair the effects of the present invention. Examples of additives include the dispersion diameter expanding agent described above, as well as bubble regulators, pigments, slip agents, antistatic agents, and flame retardants. The core particles can be produced by blending additives added as necessary with an ethylene-based resin, melt-kneading the blend, and then granulating the blend. The melt-kneading can be carried out using an extruder. In order to perform uniform kneading, it is preferable to mix the resin components in advance and then extrude them. The resin components can be mixed using a mixer such as a Henschel mixer, ribbon blender, V blender, or Loedige mixer. The melt-kneading can be carried out using a single-screw extruder or a twin-screw extruder with a high dispersion type screw such as a Dulmage type, Madoc type, or Unimelt type.
[0047] The addition of a bubble regulator can adjust the bubble diameter of the expanded beads after expansion. Examples of the bubble regulator include organic substances such as higher fatty acid bisamide, higher fatty acid metal salt, and PTFE; and inorganic substances such as talc, silica, zinc borate, alum, and PTFE. When an organic bubble regulator is used, the blending amount is preferably in the range of 0.01 to 2 mass% relative to 100 mass% of the core particles. When an inorganic bubble regulator is used, the blending amount is preferably in the range of 0.1 to 5 mass parts relative to 100 mass% of the core particles. By adjusting the blending amount of the bubble regulator within the above range, the bubble diameter of the expanded beads and the molded product becomes good, the bubbles are less likely to be destroyed during molding in the mold, and the appearance of the molded product becomes better.
[0048] The granulation of the core particles can be carried out by, for example, a strand cut method, an underwater cut method, a hot cut method, etc. Any other method can also be used as long as it can produce core particles having a desired particle size.
[0049] The particle diameter of the core particles is preferably 0.1 mm or more, and more preferably 0.3 mm or more. In this case, the composite resin particles obtained after impregnation and polymerization of the styrene monomer can be made large enough to sufficiently retain the foaming agent. In addition, from the viewpoint of preventing the foamed particles from impairing the filling ability into the mold during in-mold molding, the particle diameter of the core particles is preferably 3.0 mm or less, more preferably 1.5 mm or less, and even more preferably 1.2 mm or less. The particle weight of the core particles is preferably 0.5 mg / piece or less, more preferably 0.4 mg / piece or less, and even more preferably 0.3 mg / piece or less. In this case, even if the amount of styrene monomer impregnated into the core particles increases, the styrene monomer is easily impregnated sufficiently into the inside of the core particles, and uneven impregnation between particles is unlikely to occur, making it easier to stably obtain the desired expandable particles. The particle weight of the core particles is preferably 0.01 mg / piece or more, more preferably 0.05 mg / piece or more, and even more preferably 0.1 mg / piece or more. In this case, coagulation during polymerization can be stably suppressed.
[0050] When an extruder is used to granulate the core particles, the particle size and particle weight of the core particles can be adjusted, for example, by adjusting the amount of resin extruded and the cutting speed of the resin when the resin is extruded and cut through holes having an aperture size within the range of the desired particle size. The particle size of the core particles can be measured, for example, as follows. That is, the core particles are observed using a microscope photograph, and the maximum diameter of each of 200 or more core particles is measured, and the arithmetic average value of the maximum diameters is taken as the particle size of the core particles.
[0051] In the dispersion step, the core particles are dispersed in an aqueous medium to prepare a dispersion liquid. Dispersion of the core particles in the aqueous medium can be carried out, for example, in a closed vessel equipped with a stirrer. The closed vessel is, for example, a pressurized vessel. The aqueous medium can be, for example, a liquid such as deionized water.
[0052] The core particles are preferably dispersed in an aqueous medium together with a suspending agent. As the suspending agent, for example, tricalcium phosphate, hydroxyapatite, magnesium pyrophosphate, magnesium phosphate, aluminum hydroxide, ferric hydroxide, titanium hydroxide, magnesium hydroxide, barium phosphate, calcium carbonate, magnesium carbonate, barium carbonate, calcium sulfate, barium sulfate, talc, kaolin, bentonite, and other fine particle inorganic suspending agents can be used. In addition, for example, organic suspending agents such as polyvinylpyrrolidone, polyvinyl alcohol, ethyl cellulose, and hydroxypropylmethylcellulose can also be used. Tricalcium phosphate, hydroxyapatite, and magnesium pyrophosphate are preferable. As the suspending agent, one type of substance may be used, or two or more types of substances may be used.
[0053] The amount of the suspending agent used is preferably 0.05 to 10 parts by mass in terms of solid content per 100 parts by mass of the aqueous medium of the suspension polymerization system (specifically, all water in the system including water such as the reaction product-containing slurry). More preferably, it is 0.3 to 5 parts by mass. By setting the amount of the suspending agent within the above range, the styrene monomer can be stably suspended, the generation of resin lumps can be prevented, and the particle size distribution of the expandable particles can be suppressed from widening.
[0054] A surfactant can be added to the aqueous medium. As the surfactant, for example, an anionic surfactant, a nonionic surfactant, a cationic surfactant, or an amphoteric surfactant is preferably used. These surfactants can be used alone or in combination. Among these, it is preferable to use an anionic surfactant from the viewpoint of dispersion stability.
[0055] Furthermore, electrolytes made of inorganic salts such as lithium chloride, potassium chloride, sodium chloride, sodium sulfate, sodium nitrate, sodium carbonate, and sodium bicarbonate may be added to the aqueous medium as necessary.
[0056] It is preferable to add a water-soluble polymerization inhibitor to the aqueous medium. In this case, the polymerization of the styrene monomer in the form of microdroplets present in the aqueous medium and the styrene monomer present near the surface of the core particles is suppressed. As a result, the expanded beads have excellent moldability in the mold, and the molded product has excellent mechanical strength such as toughness.
[0057] Examples of the water-soluble polymerization inhibitor that can be used include sodium nitrite, potassium nitrate, ammonium nitrite, L-ascorbic acid, and citric acid. The amount of the water-soluble polymerization inhibitor added is preferably 0.001 to 0.1 parts by mass, and more preferably 0.002 to 0.03 parts by mass, per 100 parts by mass of the aqueous medium (specifically, all water in the system including water such as the reaction product-containing slurry). In this case, the amount of the remaining styrene monomer in the expandable particles can be reduced.
[0058] In the modification step, the core particles are impregnated with a styrene-based monomer in an aqueous medium, and the styrene-based monomer is polymerized. As the styrene-based monomer, for example, styrene can be used. As the styrene-based monomer, a monomer copolymerizable with styrene and styrene can be used in combination. The styrene-based monomer may be one type or two or more types.
[0059] Examples of monomers copolymerizable with styrene include the following styrene derivatives and other vinyl monomers, etc. Examples of styrene derivatives include α-methylstyrene, o-methylstyrene, m-methylstyrene, p-methylstyrene, p-ethylstyrene, 2,4-dimethylstyrene, p-methoxystyrene, pn-butylstyrene, pt-butylstyrene, o-chlorostyrene, m-chlorostyrene, p-chlorostyrene, 2,4,6-tribromostyrene, divinylbenzene, styrenesulfonic acid, and sodium styrenesulfonate.
[0060] Other vinyl monomers include acrylic acid esters, methacrylic acid esters, vinyl compounds containing a hydroxyl group, vinyl compounds containing a nitrile group, organic acid vinyl compounds, olefin compounds, diene compounds, vinyl halide compounds, vinylidene halide compounds, and maleimide compounds.
[0061] From the viewpoint of increasing the foaming property after the foaming agent is impregnated, the styrene-based resin component is preferably polystyrene or a copolymer of styrene and an acrylic acid ester. Examples of the acrylic acid ester include methyl acrylate, ethyl acrylate, propyl acrylate, butyl acrylate, and 2-ethylhexyl acrylate. Among them, the acrylic acid ester is preferably butyl acrylate. The content of the butyl acrylate component in the composite resin is preferably 0.2 to 5 mass % based on the total composite resin, more preferably 0.3 to 3 mass %, and even more preferably 0.5 to 2 mass %.
[0062] The polymerization of the styrene monomer can be carried out in the presence of a polymerization initiator as described above. In this case, crosslinking may occur along with the polymerization of the styrene monomer. A polymerization initiator is used in the polymerization of the styrene monomer, and a crosslinking agent can be used in combination as necessary. When using a polymerization initiator or a crosslinking agent, it is preferable to dissolve the polymerization initiator and the crosslinking agent in the styrene monomer in advance.
[0063] As the polymerization initiator, those used in the suspension polymerization method of styrene-based monomers can be used. For example, those soluble in vinyl monomers such as styrene-based monomers can be used. As the polymerization initiator, as described above, organic peroxide A having a t-butoxy group and a 10-hour half-life temperature of 80 to 120°C and organic peroxide B having a t-hexyloxy group or a t-amyloxy group and a 10-hour half-life temperature of 80 to 120°C can be used. As the organic peroxide A, t-butylperoxy-2-ethylhexyl monocarbonate, t-butylperoxy-2-ethylhexanoate, t-butylperoxy laurate, t-butylperoxy isopropyl monocarbonate, t-butylperoxy benzoate, di-t-butyl peroxide, 1,1-bis(t-butylperoxy)cyclohexane, etc. can be used. As the organic peroxide B, t-hexyl peroxybenzoate, t-hexyl peroxy isopropyl monocarbonate, di-t-hexyl peroxide, etc. can be used. As the organic peroxide B having a t-amyloxy group, for example, t-amyl peroxy isopropyl monocarbonate, t-amyl peroxy-2-ethylhexyl monocarbonate, t-amyl peroxy benzoate, 1,1-bis(t-amyl peroxy)cyclohexane, t-amyl peroxy acetate, etc. can be used. As the polymerization initiator, one type may be used, or two or more types may be used. The polymerization initiator can be used in an amount of, for example, 0.1 to 1.0 part by mass, preferably 0.2 to 0.8 parts by mass, more preferably 0.3 to 0.7 parts by mass, and preferably 0.4 to 0.6 parts by mass, relative to 100 parts by mass of the styrene-based monomer. In this case, the amount of unreacted styrene-based monomer remaining in the expandable particles can be reduced. In addition, while maintaining the expandability of the expandable particles and the moldability of the expanded particles, the complex shear viscosity of the composite resin under specified conditions can be increased, and the flame retardancy of the molded article can be improved.
[0064] As described above, from the viewpoint of easily increasing the complex shear viscosity of the composite resin under predetermined conditions, the ratio of the amount of organic peroxide A to the total amount of organic peroxide A and organic peroxide B is preferably more than 85 mass%, more preferably 86 mass% or more, and even more preferably 90 mass% or more. On the other hand, from the viewpoint of obtaining a molded product having good expandability of the expandable particles, excellent in-mold moldability of the expanded particles, and superior bending strength, the ratio of the amount of organic peroxide A to the total amount of organic peroxide A and organic peroxide B is preferably 98 mass% or less, more preferably 96 mass% or less, and even more preferably 95 mass% or less.
[0065] In addition, the crosslinking agent used is one that does not decompose at the polymerization temperature but decomposes at the crosslinking temperature. For example, one whose 10-hour half-life temperature is 5°C to 50°C higher than the polymerization temperature can be used. Specifically, peroxides such as dicumyl peroxide, 2,5-t-butyl perbenzoate, and 1,1-bis-t-butylperoxycyclohexane can be used. One type of crosslinking agent may be used, or two or more types may be used. The amount of the crosslinking agent is preferably 0.1 to 5 parts by mass relative to 100 parts by mass of the styrene monomer. The polymerization initiator and the crosslinking agent may be the same compound.
[0066] A bubble regulator can be added to the styrene monomer. Examples of the bubble regulator include fatty acid monoamide, fatty acid bisamide, talc, silica, polyethylene wax, methylene bisstearic acid, methyl methacrylate copolymer, and silicone. Examples of the fatty acid monoamide include oleic acid amide and stearic acid amide. Examples of the fatty acid bisamide include ethylene bisstearic acid amide.
[0067] Furthermore, to the styrene monomer, a plasticizer, an oil-soluble polymerization inhibitor, a flame retardant, a dye, etc. may be added as necessary within the range not impairing the effects of the present invention.
[0068] When the core particles are impregnated with the styrene monomer and polymerized, the entire amount can be added at once, or it can be added in several batches. When adding in several batches, the styrene monomer can be divided into several monomers such as a first monomer and a second monomer, and these monomers can be added to the aqueous medium at different times and temperatures. By adding in several batches, it is possible to prevent the generation of resin lumps in the modification process.
[0069] In the modification step, the polymerization temperature varies depending on the type of polymerization initiator used, but is preferably 80°C to 130°C.
[0070] In the impregnation step, the foaming agent is impregnated. The foaming agent can be impregnated into the particles during or after the polymerization of the styrene monomer. The foaming agent may be impregnated into both the particles during polymerization and the particles after polymerization. Specifically, the foaming agent is pressed into a container that contains the particles after polymerization during polymerization, and the foaming agent is impregnated into the particles. The foaming agent is as described above.
[0071] The impregnation temperature of the foaming agent is preferably within the range of (Tg-10)°C to (Tg+40)°C, and more preferably within the range of (Tg-5)°C to (Tg+25)°C, where Tg (unit: °C) is the glass transition temperature of the styrene-based resin component. The glass transition temperature (Tg) of the styrene-based resin component can be measured by the method described above.
[0072] After impregnation with the foaming agent, the expandable particles are dehydrated and dried, and the expandable particles can be coated with a surface coating agent as required. Examples of the surface coating agent include zinc stearate, stearate triglyceride, stearate monoglyceride, and hardened castor oil. The amount of the surface coating agent added is preferably 0.01 to 2 parts by mass per 100 parts by mass of the expandable particles.
[0073] The expandable particles can be obtained by heating and expanding the expandable particles with a heating medium. Specifically, the expandable particles can be obtained by introducing a heating medium such as steam into a pre-expansion machine to which the expandable particles have been supplied, and pre-expanding the expandable particles.
[0074] The bulk density of the foam particles is 15 to 50 kg / m 3 In this case, a molded article that is lightweight and has mechanical properties such as toughness and rigidity can be obtained. Even if the expandable particles are expanded to a low bulk density within the above range, the expanded particles and the molded article can exhibit excellent flame retardancy. From the viewpoint of improving such effects, the bulk density of the expanded particles is preferably 16 to 40 kg / m 3 More preferably, it is 18 to 35 kg / m 3 More preferably, it is 20 to 30 kg / m 3 It is particularly preferable that the bulk density of the expanded particles (kg / m 3 ) is calculated by preparing a 1 L measuring cylinder, filling the empty measuring cylinder with expanded particles up to the 1 L mark, measuring the mass (g) of expanded particles per 1 L, and converting the mass into units.
[0075] A molded article can be obtained by molding the expanded beads in a mold. Specifically, a large number of expanded beads are fed into a mold, and a heating medium such as steam is introduced to fuse the expanded beads together. In this manner, a molded article can be obtained. From the same viewpoint as the bulk density of the expanded beads described above, the apparent density of the molded article is 20 to 50 kg / m 3 is preferably 25 to 45 kg / m 3 More preferably, it is 30 to 50 kg / m 3 It is even more preferable that: EXAMPLES
[0076] Example 1 [Creation of core particles] As an ethylene-based resin, a linear low-density polyethylene (Nipolon Z HF210K manufactured by Tosoh Corporation) polymerized using a metallocene polymerization catalyst was prepared. The linear low-density polyethylene is hereinafter referred to as "LLDPE" as appropriate. The melting point Tm of this LLDPE is 103°C. In addition, an acrylonitrile-styrene copolymer (AS-XGS manufactured by Denka Co., Ltd., weight average molecular weight: 109,000, acrylonitrile content: 28% by mass, MFR (200°C, 5kgf): 2.8g / 10min) was prepared as a dispersion diameter expander. In addition, a master batch of an antioxidant (TMB113 manufactured by Toho Co., Ltd., linear low-density polyethylene: 90% by mass, phosphorus-based stabilizer: 6.5% by mass, hindered phenol-based antioxidant: 3.5% by mass) was prepared. Furthermore, a mixed master batch (ethylene bis-stearic acid amide: 10 mass%, zinc 12-hydroxystearate: 3 mass%, linear low-density polyethylene: 87 mass%) of ethylene bis-stearic acid amide (Kaowax EB-FF manufactured by Kao Corporation) as a foam regulator and zinc 12-hydroxystearate (ZS-6 manufactured by Nitto Kasei Kogyo Co., Ltd.) as a lubricant was prepared. Then, 87.7 kg of ethylene resin, 4.7 kg of acrylonitrile-styrene copolymer as a dispersion diameter expander, 0.9 kg of antioxidant master batch, and 6.7 kg of a mixed master batch of air bubble adjuster and lubricant were charged into a Henschel mixer (FM-75E manufactured by Mitsui Miike Chemical Engineering Co., Ltd.) and mixed for 5 minutes. Next, the mixture was melt-kneaded at a barrel temperature of 220 to 250° C. using a single-screw extruder (PMS50-28 manufactured by IKG Corporation) with an inner barrel diameter of 50 mm, and cut into particles by an underwater cutting method to obtain core particles of an average weight of 0.2 mg / piece.
[0077] [Preparation of composite resin particles] 1000g of deionized water and 6.0g of sodium pyrophosphate were placed in a 3L autoclave equipped with a stirrer. Then, 12.9g of magnesium nitrate hexahydrate was added and stirred at room temperature for 30 minutes to prepare magnesium pyrophosphate slurry as a suspension. Next, 2g of sodium alkylsulfonate (10% aqueous solution of Latemul PS manufactured by Kao Corporation) as a surfactant, 0.15g of sodium nitrite as a water-soluble polymerization inhibitor, and 75g of core particles were placed in the autoclave.
[0078] Next, 0.21 g of t-hexyl peroxybenzoate (Perhexyl Z manufactured by NOF Corp.) as a polymerization initiator, 2.50 g of t-butylperoxy-2-ethylhexyl monocarbonate (Perbutyl E manufactured by NOF Corp.), 6.67 g of 2,2-bis(4-(2,3-dibromo-2-methylpropoxy)-3,5-dibromophenyl)propane (SR130 manufactured by Daiichi Kogyo Seiyaku Co., Ltd. (50% decomposition temperature: 294°C)) as a bromine-based flame retardant, and 1.67 g of 2,3-dimethyl-2,3-diphenylbutane (Nofumer BC-90 manufactured by NOF Corp. (10-hour half-life temperature: 210°C)) as a flame retardant aid were dissolved in the first monomer (styrene-based monomer). Then, this dissolved matter was put into the autoclave while stirring at a stirring speed of 500 rpm. A mixed monomer of 70 g of styrene and 5 g of butyl acrylate was used as the first monomer.
[0079] Next, the air in the autoclave was replaced with nitrogen, and then heating was started, and the temperature in the autoclave was raised to 100°C over 1.5 hours. It was further maintained at 100°C for 1 hour. Thereafter, the stirring speed was reduced to 450 rpm, and it was maintained at 100°C for 7.5 hours. One hour after reaching 100°C, 350 g of styrene was added to the autoclave as a second monomer (specifically, a styrene-based monomer) over 5 hours.
[0080] The temperature inside the autoclave was then raised to 125°C over 2 hours and held at 125°C for 5 hours. The autoclave was then cooled over 1 hour, and the composite resin particles were removed. Nitric acid was then added to dissolve the magnesium pyrophosphate adhering to the surface of the composite resin particles. The particles were then dehydrated and washed using a centrifuge, and the moisture adhering to the surface was removed using an airflow dryer.
[0081] [Stripping and foaming agent impregnation] In a 3L autoclave equipped with a stirrer, 1030g of deionized water was put in, 1.03g of calcium phosphate tribasic (manufactured by Taihei Chemical Industry Co., Ltd.) as a suspending agent, 1.03g of disodium alkyl diphenyl ether disulfonate (Pelex SSH 1% aqueous solution manufactured by Kao Corporation) as a surfactant, and 670g of the composite resin particles produced above were put in and stirred at a stirring speed of 400 rpm. Next, the air in the autoclave was replaced with nitrogen, and then heating was started, and the temperature in the autoclave was raised to 130°C over 1 hour and maintained at 130°C for 5 hours. During this time, the vent line of the autoclave was slightly opened, the internal pressure was maintained at 0.12MPa (gauge pressure), and volatile organic compounds (VOCs) such as styrene monomers contained in the composite resin particles were distilled out by steam distillation. After holding for 5 hours, the temperature in the autoclave was cooled to 90°C. When the temperature reached 90°C, the vent line was closed to seal the autoclave, and 10.0 g of pentane (a mixture of about 80% by mass of normal pentane and about 20% by mass of isopentane) and 65.0 g of isobutane were added to the autoclave over about 20 minutes (foaming agent impregnation step). The mixture was kept at 90°C for 3 hours, and then heated to 105°C over 1 hour, and kept at 105°C for 5 hours, and then cooled to 30°C over about 2.5 hours.
[0082] The composite resin particles were then removed from the autoclave, and nitric acid was added to dissolve the tribasic calcium phosphate adhering to the surface of the composite resin particles. The particles were washed with water and dehydrated using a centrifuge, and the water adhering to the surface was removed using an airflow dryer to obtain expandable particles. The mass ratio of the styrene-based monomer and the ethylene-based resin used during production was defined as the mass ratio of the component derived from the styrene-based monomer in the composite resin to the component derived from the ethylene-based resin.
[0083] The resulting expandable granules were then placed in a 30 L normal pressure batch expansion machine, and steam was supplied from the bottom of the expansion machine to expand the granules until the bulk density reached approximately 33 kg / m 3 The bulk density was determined by drying the obtained expanded beads at room temperature for one day, filling a 1-L measuring cylinder with the expanded beads up to the 1-L mark, and measuring the mass (g) of the expanded beads per 1 L.
[0084] Next, using a molding machine (DSM-0705VS manufactured by DABO Corporation), the expanded particles were dried at room temperature for one day after foaming to form a rectangular solid-shaped molded body of 300 mm × 75 mm × 25 mm and a box-shaped molded body of 340 mm × 270 mm × 150 mm with a wall thickness of 25 mm. The obtained molded bodies were dried at 40°C for one day, and then further aged at room temperature for at least one day before being used for various evaluations.
[0085] The expandable particles, expanded particles, and molded bodies obtained as described above were measured for average particle size (d63), foaming agent content, xylene insoluble content (XY gel content), weight average molecular weight Mw of tetrahydrofuran soluble content, glass transition temperature (Tg) of styrene resin component, content R-SM of residual styrene monomer in composite resin particles, shelf bulk density, bead life, complex viscosity η at 300°C, lower limit molding steam pressure MPa (gauge pressure), apparent density, 50% compressive stress σ23 at temperature 23°C, 50% compressive stress σ80 at temperature 80°C, breaking strain, maximum bending stress, and burning rate as follows. The results are shown in Tables 1 to 4. The symbols in the tables have the following meanings. T: 10-hour half-life temperature R-SM: Amount of unreacted styrene monomer remaining in the expandable particles BE: t-Butylperoxy-2-ethylhexyl monocarbonate HZ: t-Hexyl peroxybenzoate SR130: 2,2-bis[4-(2,3-dibromo-2-methylpropoxy)-3,5-dibromophenyl]propane FCP-65CN: Bis[3,5-dibromo-4-(2,3-dibromopropoxy)phenyl]sulfone BC: 2,3-dimethyl-2,3-diphenylbutane E3000: Brominated styrene-butadiene copolymer
[0086] ·Average particle diameter (d63) The average particle size (d63) of the expandable particles was calculated using a dry particle size distribution analyzer (Militrack JPA, manufactured by Nikkiso Co., Ltd.) as the particle size value (d63) at which the weight cumulative particle size value from the minimum particle size reaches 63%.
[0087] Foaming agent content Approximately 1 g of the expandable particles was placed in an aluminum dish and heated in a dryer at 120°C for 4 hours to evaporate the volatile matter (including water and the blowing agent). The amount of volatile matter in the expandable particles was calculated from the weight difference before and after heating. Next, about 0.3 g of the expandable particles was weighed, and the moisture content of the expandable particles was determined using a Karl Fischer moisture meter. The foaming agent content of the expandable particles was calculated by the following formula. Foaming agent content (%) = Volatile content (%) - Water content (%)
[0088] Xylene insoluble matter content (XY gel content) 0.5 g of the expanded particles was placed in a 150 mesh wire bag. Next, about 95 ml of xylene was placed in a 200 ml round bottom flask, and the wire bag was set in a Soxhlet extraction tube to perform Soxhlet extraction. After the extraction was completed, it was cooled to room temperature, the wire net was removed from the extraction tube, and the xylene insolubles were washed together with the wire net with about 400 ml of acetone. After air drying, the xylene insolubles were dried for 4 hours in a dryer at a temperature of 120°C. The ratio of the amount of xylene insolubles (mass) to 0.5 g of expanded particles was expressed as a percentage, and was taken as the content of xylene insolubles, i.e., the XY gel amount (mass%). The xylene insolubles are mainly crosslinked ethylene resin components in the composite resin.
[0089] Weight average molecular weight (Mw) of tetrahydrofuran solubles The expandable particles from which the blowing agent had escaped were frozen with liquid nitrogen and freeze-pulverized to a particle size of 0.5 mm or less using an analytical mill manufactured by IKA Japan Co., Ltd. Approximately 35 mg of the pulverized material was collected and placed in a 10 mL measuring flask. Approximately 10 mL of tetrahydrofuran (THF) was then added and allowed to stand for 24 hours. The tetrahydrofuran insoluble matter was removed using a membrane filter (0.45 μm), and the THF-soluble matter was measured by gel permeation chromatography (GPC) and calibrated with standard polystyrene to determine Mw. The THF-soluble matter in the composite resin was mainly a styrene-based resin component. The measurement conditions were as follows. GPC equipment: Tosoh Corporation HLC-8320GPC EcoSEC Detector: Differential refractometer (RI) Column: Tosoh Corporation TSKguardcolumn SuperH-H x 1 TSK-GEL SuperHM-H x 2 connected in series Column temperature: 40°C, eluent: THF, flow rate: 0.6 ml / min, sample concentration: 0.1 wt%
[0090] Glass transition temperature (Tg) of styrene resin components First, the expandable particles from which the blowing agent had escaped were frozen with liquid nitrogen and frozen and crushed using an analytical mill (e.g., A-11 manufactured by IKA Co., Ltd.). Next, 2.0 g of the crushed expandable particles and 30 mL of methyl ethyl ketone (MEK) were placed in a 100 mL beaker and stirred at room temperature for one day. The MEK solution was filtered, the filtrate was dropped into 100 mL of methanol, and the resulting precipitate was dried at 60 ° C for 24 hours to obtain a styrene-based resin component as a MEK soluble matter. Differential scanning calorimetry was performed on 2 to 4 mg of the obtained styrene-based resin component in accordance with JIS K7121 (1987), and the midpoint glass transition temperature of the DSC curve limited by the condition of a heating rate of 20 ° C / min was obtained, and this was taken as the glass transition temperature (Tg) of the styrene-based resin component. For the differential scanning calorimetry, a 250-type DSC measuring instrument manufactured by TA Instruments Co., Ltd. was used.
[0091] · Content of unreacted styrene in expandable particles (R-SM) The content of unreacted styrene in the expandable particles was measured using a headspace gas chromatograph mass spectrometer. Specifically, standard solutions were prepared so that the styrene concentrations in DMF were 5 ppm by mass, 50 ppm by mass, and 500 ppm by mass. 0.2 g of the standard solution was precisely weighed into a 20 ml vial, and 5 ml of DMF was added and sealed. The gas phase was measured using a gas chromatograph mass spectrometer, and a calibration curve was created from the obtained chromatogram. Next, 0.2 g of the freeze-pulverized expandable particles was precisely weighed into a 20 ml vial, and 5 ml of DMF was added and sealed, and the vial was kept at room temperature for one day. The gas phase was measured using a gas chromatograph mass spectrometer. The content of unreacted styrene in the expandable particles was determined from the obtained chromatogram and the calibration curve created in advance.
[0092] The measurement conditions for gas chromatography mass spectrometry were as follows. Gas chromatograph mass spectrometer: Shimadzu Corporation GCMS-QP2020 Headspace sampler: Shimadzu Corporation HS-20 Capillary column: GL Sciences, Inc., Stabilwax, inner diameter 0.32 mm, length 30 m Headspace sampler incubation conditions: 90℃, 1 hour Column temperature: 50°C x 2 min → (10°C / min) → 90°C → (5°C / min) → 120°C → (20°C / min) → 230°C x 2 min Ion source temperature: 200℃ Carrier gas: Helium, column flow rate 2ml / min Split ratio: 1 / 10
[0093] Bead life, shelf bulk density The expandable particles were left in the open at a temperature of 23°C, and expanded every time a predetermined time elapsed using a shelf-type expansion machine (blowing steam pressure of 3 KPa (gauge pressure), heating time of 270 seconds). The expanded particles obtained were dried at room temperature for one day, and then the bulk density (kg / m 3 ) was measured. From the relationship between the time elapsed from the time the expanded particles were opened and the bulk density of the expanded particles obtained at each elapsed time, it was found that the bulk density was 33 kg / m 3 The time (number of days) required for this to occur was defined as the bead life. In addition, the expandable particles immediately after production were expanded under normal pressure using a shelf type expansion machine (blowing steam pressure 3 KPa (gauge pressure), heating time 270 seconds). This resulted in determining the shelf type bulk density of the expanded particles. Note that the lower the shelf type bulk density value, the better the expandability. Bulk density on shelf: 30kg / m 3 If it is less than 25kg / m, it will have better foaming properties. 3 The foaming properties are further improved if the following is satisfied:
[0094] Complex shear viscosity (η) The obtained expandable particles were dried at 60°C for one day under normal pressure. After drying, 35 g of the expandable particles from which the blowing agent had been dispersed by drying were hot-pressed at 200°C using a hot-press machine (HF-37 manufactured by Shinto Metal Industries Co., Ltd.) equipped with a mold measuring 150 mm in length and 150 mm in width, to produce a flat plate with a thickness of about 1.0 to 1.5 mm. The flat plate was cut to a diameter of 25 mm to prepare a measurement sample. The obtained sample was subjected to dynamic viscoelastic analysis using a rheometer (viscoelasticity measuring device) based on JIS K 7244-10:2005 to determine the complex shear viscosity η at an angular frequency of 1 rad / s and a temperature of 300°C. The complex shear viscosity η was determined 600 seconds after the start of the dynamic viscoelastic analysis. This measurement was performed on three different test samples, and the arithmetic mean of the measured values was calculated. The value was rounded off to the nearest tenth, and this value was regarded as the complex shear viscosity of the composite resin containing the flame retardant.
[0095] The measurement conditions for the complex shear viscosity η are as follows: Rheometer: DISCOVERY HR-2 manufactured by TA Instruments Co., Ltd. Geometry: φ25mm parallel plate Measurement temperature: 300℃ Angular frequency: 1rad / s Distortion: 0.1% Gap: 0.8mm Measurement atmosphere: Nitrogen flow
[0096] -Lower molding steam pressure (MPa (gauge pressure)) This is the minimum steam pressure required in in-mold molding to obtain a molded body with a surface smoothness that can be visually judged to be good and with an internal fusion rate of 80% or more. The molded body was broken, the fracture surface was observed, and the number of foamed beads that had been broken into pieces and the number of foamed beads that had peeled off at the interface were counted. The ratio of foamed beads that had been broken into pieces to the total number of foamed beads that had been broken into pieces and the number of foamed beads that had peeled off at the interface, expressed as a percentage, was taken as the internal fusion rate (%). The lower limit of the molding steam pressure is preferably 0.10 MPa or less, and more preferably 0.08 MPa or less, in which case the expanded beads have excellent moldability in the mold.
[0097] Apparent density Apparent density of the compact (kg / m 3 ) was obtained by measuring the mass of the rectangular parallelepiped molded body, dividing the mass by the volume of the molded body, and converting the mass into units.
[0098] 50% compressive stress Plate-shaped test pieces measuring 50 mm in length, 50 mm in width, and 25 mm in thickness were cut out from the rectangular solid-shaped molded body, and compression tests were performed in accordance with JIS K 7220 (2006). The compressive stress when the compressive strain was 50% was the 50% compressive stress (kPa), and the 50% compressive stress when the test conditions were 23°C was σ23, and the 50% compressive stress when the test conditions were 80°C was σ80. For measurements in an 80°C atmosphere, the measurement sample was left to stand in a dryer at 80°C for 24 hours in advance to condition the measurement sample before measurements were performed.
[0099] ·Strain at break, maximum bending stress A three-point bending test was performed on a molded body measuring 300 mm long x 75 mm wide x 25 mm thick in accordance with JIS K 7221-2:2006 under the conditions of a support distance of 200 mm, a pressure wedge of 10R and a support stand of 10R, and a pressure wedge descent speed of 10 mm / min. The bending strength was measured. A stress-strain curve was obtained from the stress (KPa) and strain (%) obtained by the measurement. From the obtained stress-strain curve, the breaking strain, which is the point at which the molded body broke, and the maximum bending stress, which is the point at which the molded body exhibits the maximum stress, were obtained.
[0100] Burning speed, rate of burning speed 80mm / min A rectangular test piece measuring 340mm x 102mm x 12.7mm was cut out from the bottom plate of the box-shaped molded body. The burning rate (mm / min) was measured in accordance with the combustion test of FMVSS (Federal Motor Vehicle Safety Standards) No. 302. The burning rate was measured for 10 test pieces, and the arithmetic mean of these was taken as the average burning rate. Note that test pieces that self-extinguished in the burning test were evaluated as having a burning rate of 0mm / min. In addition, the percentage of the 10 test pieces with a burning rate of 80 mm / min or less was calculated. The average burning rate is preferably 80 mm / min or less, more preferably 60 mm / min or less, even more preferably 30 mm / min or less, and particularly preferably 0 mm / min (i.e., exhibiting self-extinguishing properties).
[0101] Example 2 In this example, the amount of styrene used as the first monomer in producing the composite resin particles in Example 1 was changed from 70 g to 60 g, the amount of butyl acrylate used was changed from 5 g to 15 g, the amount of t-hexyl peroxybenzoate used was reduced to 0, and the amount of t-butylperoxy-2-ethylhexyl monocarbonate used was changed from 2.50 g to 2.71 g. The amount of 2,2-bis(4-(2,3-dibromo-2-methylpropoxy)-3,5-dibromophenyl)propane used as the bromine-based flame retardant was changed from 6.67 g to 3.8 g, and the amount of 2,3-dimethyl-2,3-diphenylbutane used as the flame retardant auxiliary was changed from 1.67 g to 0.96 g. Except for this, the expandable particles, expanded particles, and molded bodies were produced in the same manner as in Example 1.
[0102] Example 3 In this example, the amount of t-hexyl peroxybenzoate used in producing the composite resin particles in Example 1 was changed from 0.21 g to 0.42 g, the amount of 2,2-bis(4-(2,3-dibromo-2-methylpropoxy)-3,5-dibromophenyl)propane used as a bromine-based flame retardant was changed from 6.67 g to 18 g, and the amount of 2,3-dimethyl-2,3-diphenylbutane used as a flame retardant aid was changed from 1.67 g to 0 g. Except for this, the expandable particles, expanded particles, and molded bodies were produced in the same manner as in Example 1.
[0103] Example 4 In this example, the amount of t-hexyl peroxybenzoate used in producing the composite resin particles in Example 1 was changed from 0.21 g to 0.42 g, and the amount of 2,3-dimethyl-2,3-diphenylbutane used as a flame retardant aid was changed from 1.67 g to 0 g, except that the expandable particles, expanded particles, and molded bodies were produced in the same manner as in Example 1.
[0104] Example 5 In this example, the amount of t-hexyl peroxybenzoate used in producing the composite resin particles in Example 1 was changed from 0.21 g to 0.42 g, and further, the brominated flame retardant was changed from 2,2-bis(4-(2,3-dibromo-2-methylpropoxy)-3,5-dibromophenyl)propane to bis[3,5-dibromo-4-(2,3-dibromopropoxy)phenyl]sulfone (FCP-65CN (50% decomposition temperature: 331°C) manufactured by Suzuhiro Chemical Co., Ltd.). Except for this, the expandable particles, expanded particles, and molded bodies were produced in the same manner as in Example 1.
[0105] Example 6 In this example, the expandable particles, expanded particles, and molded bodies were prepared in the same manner as in Example 1, except that the amount of styrene used as the first monomer in preparing the composite resin particles in Example 1 was changed from 70 g to 75 g, the amount of butyl acrylate used was changed from 5 g to 0 g, and the amount of t-hexyl peroxybenzoate used was changed from 0.21 g to 0.42 g.
[0106] Example 7 In this example, the amount of core particles used in producing the composite resin particles in Example 1 was changed from 75 g to 125 g, the amount of t-hexyl peroxybenzoate used was changed from 0.21 g to 0.42 g, and the amount of styrene used as the first monomer was changed from 70 g to 60 g, and the amount of butyl acrylate used was changed from 5 g to 15 g, except that the expandable particles, expanded particles, and molded bodies were produced in the same manner as in Example 1.
[0107] Example 8 In this example, the amount of 2,2-bis(4-(2,3-dibromo-2-methylpropoxy)-3,5-dibromophenyl)propane used as the bromine-based flame retardant in producing the composite resin particles in Example 1 was changed from 6.67 g to 18 g, and the amount of 2,3-dimethyl-2,3-diphenylbutane used as the flame retardant aid was changed from 1.67 g to 4.5 g, except that the expandable particles, expanded particles, and molded bodies were produced in the same manner as in Example 1.
[0108] Example 9 In this example, the expandable particles, expanded particles, and molded bodies were prepared in the same manner as in Example 1, except that the amount of 2,3-dimethyl-2,3-diphenylbutane used as a flame retardant aid in preparing the composite resin particles in Example 1 was changed from 1.67 g to 6.67 g.
[0109] Example 10 In this example, the expandable particles, expanded particles, and molded bodies were produced in the same manner as in Example 1, except that the amount of LLDPE used to produce the core particles in Example 1 was reduced to 65.8 kg instead of 87.7 kg, and 21.9 kg of ethylene-vinyl acetate copolymer (EVA) (Ultrathene 626, manufactured by Tosoh Corporation) with a vinyl acetate content of 15% by mass was used to produce the core particles.
[0110] Comparative Example 1 In this example, the amount of t-hexyl peroxybenzoate used in producing the composite resin particles in Example 1 was changed from 0.21 g to 1.25 g, the amount of t-butylperoxy-2-ethylhexyl monocarbonate used was changed from 2.50 g to 1.25 g, and the amount of styrene used as the first monomer was changed from 70 g to 75 g, and the amount of butyl acrylate used was changed from 5 g to 0 g. Except for this, the expandable particles, expanded particles, and molded bodies were produced in the same manner as in Example 1.
[0111] Comparative Example 2 In this example, expandable particles were produced in the same manner as in Example 1, except that the amount of t-hexyl peroxybenzoate used in producing the composite resin particles in Example 1 was changed from 0.21 g to 0, the amount of 2,2-bis(4-(2,3-dibromo-2-methylpropoxy)-3,5-dibromophenyl)propane used as a bromine-based flame retardant was changed from 6.67 g to 0 g, and the amount of 2,3-dimethyl-2,3-diphenylbutane used as a flame retardant aid was changed from 1.67 g to 0 g. When the tray bulk density of these expandable particles was measured, the tray bulk density was found to be 40 kg / m 3 Therefore, the molded product was not evaluated further.
[0112] Comparative Example 3 In this example, the amount of LLDPE used in the preparation of the core particles in Example 1 was reduced from 87.7 kg to 65.8 kg, and 21.9 kg of ethylene-vinyl acetate copolymer (EVA) (Ultrathene 626 manufactured by Tosoh Corporation) with a vinyl acetate content of 15% by mass was used to prepare the core particles. Furthermore, the amount of t-hexyl peroxybenzoate used in the preparation of the composite resin particles was changed from 0.21 g to 0 g, the amount of t-butylperoxy-2-ethylhexyl monocarbonate used was changed from 2.50 g to 1.7 g, the amount of 2,2-bis(4-(2,3-dibromo-2-methylpropoxy)-3,5-dibromophenyl)propane used as a bromine-based flame retardant was changed from 6.67 g to 10 g, and the amount of 2,3-dimethyl-2,3-diphenylbutane used as a flame retardant auxiliary was changed from 1.67 g to 0 g. Except for this, expandable particles were prepared in the same manner as in Example 1. When the shelf bulk density of the expandable granules was measured, the shelf bulk density was 40 kg / m 3 Therefore, the molded product was not evaluated further.
[0113] Comparative Example 4 In this example, the core particles used in Example 1 were changed to core particles prepared by the following procedure, the amount of t-butylperoxy-2-ethylhexyl monocarbonate used was changed from 2.5 g to 2.58 g, the amount of t-hexyl peroxybenzoate used was changed from 0.21 g to 0 g, and the amount of 2,3-dimethyl-2,3-diphenylbutane used as a flame retardant auxiliary was changed from 1.67 g to 0 g. Except for this, expandable particles, expanded particles, and molded bodies were prepared in the same manner as in Example 1. [Creation of core particles] As the ethylene-based resin, we prepared a linear low-density polyethylene polymerized using a metallocene polymerization catalyst (Nipolon Z HF210K manufactured by Tosoh Corporation) and an ethylene-vinyl acetate copolymer (EVA) with a vinyl acetate content of 46 mass% (EV45LX manufactured by Dow Mitsui Polychemicals Co., Ltd.). As a dispersion size expander, we prepared an acrylonitrile-styrene copolymer (AS-XGS manufactured by Denka Co., Ltd.). Further, a flame retardant master batch (Nikko Bix Co., Ltd., brominated styrene-butadiene copolymer (Chemtura Corporation, Emerald 3000): 70.03 mass%, TBA-bis (2,3-dibromopropyl ether) (Suzuhiro Chemical Co., Ltd., FCP-680): 12.05 mass%, poly (1,4-diisopropylbenzene) (United Initiator Co., Ltd., CCPIB): 3.50 mass%, cresol novolac type epoxy resin (DIC Corporation, Epicron N-680): 7.21 mass%, and antioxidants (ADEKA CORPORATION, Adeka STAB PEP-36): 0.41 mass% and (Songwon Corporation, Songnox 4425): 6.80 mass%) were prepared. Furthermore, polyethylene wax (Baker Petrolite Co., Ltd., PW1000) was prepared as a lubricant. Then, 66.05 kg of LLDPE and 7.33 kg of EVA as ethylene-based resins, 3.62 kg of acrylonitrile-styrene copolymer as a dispersion diameter expander, 18 kg of a flame retardant master batch, and 5 kg of polyethylene wax were added to a Henschel mixer (FM-75E manufactured by Mitsui Miike Chemical Engineering Co., Ltd.) and mixed for 5 minutes. Next, the mixture was melt-kneaded at a barrel temperature of 180° C. using a single-screw extruder (PMS30-28 manufactured by IKG Corporation) with an inner barrel diameter of 30 mm, and cut by a strand cut method to obtain core particles of an average weight of 0.35 mg / piece.
[0114] [Table 1]
[0115] [Table 2]
[0116] [Table 3]
[0117] [Table 4]
[0118] As can be seen from Tables 1 to 4, the expandable particles of Examples 1 to 10 have a long bead life of 0.5 days (12 hours) or more, are excellent in retaining the blowing agent, and have a shelf bulk density of 40 kg / m 3 It is understood that the molded articles obtained from the expandable particles of Examples 1 to 10 have a low burning rate or exhibit self-extinguishing properties, and also stably exhibit such excellent flame retardancy.
[0119] In addition, as Comparative Examples 5 and 6, expandable beads, expanded beads, and molded articles containing a brominated styrene-butadiene copolymer as a flame retardant were prepared as follows.
[0120] Comparative Example 5 In Comparative Example 5, expandable particles were prepared in the same manner as in Example 2, except that the brominated flame retardant used in the preparation of the composite resin particles in Example 2 was changed from 2,2-bis(4-(2,3-dibromo-2-methylpropoxy)-3,5-dibromophenyl)propane to a brominated styrene-butadiene copolymer. The expandable particles of Comparative Example 5 had a weight average molecular weight of 510,000 and a complex shear viscosity of 2910 Pa s. The tray bulk density of these expandable particles was measured, and the tray bulk density was found to be 27 kg / m 3 The expandability was lower than that of Example 2. When molding was performed in a mold using the produced expanded beads, the lower limit of molding steam pressure was 0.12 MPa, and the moldability in the mold was lower than that of the examples.
[0121] Comparative Example 6 In Comparative Example 6, expandable particles were produced in the same manner as in Comparative Example 5, except that the amount of the brominated styrene-butadiene copolymer used in producing the composite resin particles in Comparative Example 5 was changed from 3.8 g to 6.67 g, and the amount of 2,3-dimethyl-2,3-diphenylbutane used as a flame retardant aid was changed from 0.96 g to 1.67 g. The expandable particles of Comparative Example 6 had a weight average molecular weight of 470,000 and a complex shear viscosity of 3630 Pa s. When the tray bulk density of these expandable particles was measured, the tray bulk density was 34 kg / m 3 The foaming property was decreased compared to the examples.
Claims
1. The expandable composite resin particles include a composite resin obtained by impregnating and polymerizing an ethylene-based resin with a styrene-based monomer as a base resin, and a blowing agent and a flame retardant are contained in the base resin, a mass ratio of the component derived from the ethylene-based resin to the component derived from the styrene-based monomer is 50:50 to 5:95; The content of the blowing agent in the expandable composite resin particles is 3 to 10% by mass, The flame retardant is a brominated bisphenol flame retardant, The expandable composite resin particles have a complex shear viscosity η of 500 to 2000 Pa·s of the composite resin containing the flame retardant, as measured in accordance with JIS K 7244-10:2005 at an angular frequency of 1 rad / s and a temperature of 300° C.
2. The amount of the flame retardant in the expandable composite resin particles is based on 100 parts by mass of the composite resin. The expandable composite resin particles according to claim 1, wherein the content is 0.1 to 3 parts by mass.
3. 3. The expandable composite resin particle according to claim 1, wherein the expandable composite resin particle further contains a flame retardant auxiliary in the base resin, and the flame retardant auxiliary is a radical generator having a 10-hour half-life temperature of 150°C or higher.
4. 4. The expandable composite resin particles according to claim 3, wherein a mass ratio of said flame retardant auxiliary to said flame retardant is 0.1 to 1.
5. The expandable composite resin particles according to any one of claims 1 to 4, wherein a mass ratio of the component derived from the ethylene-based resin to the component derived from the styrene-based monomer is 20:80 to 5:
95.
6. The expandable composite resin particles according to any one of claims 1 to 5, wherein the glass transition temperature of the methyl ethyl ketone soluble matter in the composite resin is 105°C or higher.
7. The expandable composite resin particles according to any one of claims 1 to 6, wherein the ethylene-based resin consists essentially of linear low-density polyethylene.
8. The expandable composite resin particles according to any one of claims 1 to 7, wherein the foaming agent contains isobutane, and the content of isobutane in the foaming agent exceeds 80 mass%.
9. The expandable composite resin particles according to any one of claims 1 to 8, wherein the content of a styrene-based monomer in the expandable composite resin particles is 50 ppm by mass or less.
10. A composite resin foam particle is obtained by foaming an expandable composite resin particle containing a foaming agent and a flame retardant in a base resin, the composite resin being a base resin obtained by impregnating and polymerizing an ethylene resin with a styrene monomer, the expandable composite resin particle containing the foaming agent and the flame retardant in the base resin, The flame retardant is a brominated bisphenol flame retardant, a mass ratio of the component derived from the ethylene-based resin to the component derived from the styrene-based monomer is 50:50 to 5:95 by mass ratio, The composite resin foam particles have a complex shear viscosity η of 500 to 2000 Pa·s at a frequency of 1 rad / s and a temperature of 300° C. as measured in accordance with JIS K 7244-10:2005.
11. The bulk density of the composite resin foam particles is 15 to 50 kg / m 3 The composite resin foam particle according to claim 10,
Citation Information
Patent Citations
Method for producing expandable composite resin particles
JP2016037530A
Expandable composite resin particle
JP2016180038A
Complex resin particle, complex resin foam particle, and complex resin foam particle molded body
JP2018203871A