Shock absorbing material

The HIPE foam shock absorbing material, with tailored properties, addresses the limitations of conventional technologies by providing stable energy absorption performance across a wide strain range, enhancing its suitability for applications like automobile and construction materials.

JP7560334B2Active Publication Date: 2024-10-02JSP CORP
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2020194659
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-11-24
Publication Date
2024-10-02
Estimated Expiration
2040-11-24

AI Technical Summary

Technical Problem

Conventional HIPE foam technologies either reduce energy absorption per unit weight or exhibit poor energy absorption performance under high strain, making them unsuitable as effective shock absorbers for applications such as automobile materials and construction materials.

Method used

A shock absorbing material composed of HIPE foam with specific properties, including a crosslinked polymer base resin derived from styrene and/or acrylic monomers, glass transition temperature of 60°C or higher, molecular weight between crosslinking points of 3×10³, apparent density between 35 and 100 kg/m³, and a compressive stress ratio of 0.70 to 1.0 at 10% and 50% strain, ensuring stable energy absorption across a wide strain range.

Benefits of technology

The material achieves excellent energy absorption per unit weight with minimal performance variation across varying strains, suitable for applications requiring effective shock absorption.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007560334000007
    Figure 0007560334000007
  • Figure 0007560334000008
    Figure 0007560334000008
  • Figure 0007560334000001
    Figure 0007560334000001
Patent Text Reader

Abstract

To provide an impact absorption material which is excellent in an energy absorption amount per unit weight, and shows little change of energy absorption performance over a wide strain range.SOLUTION: An impact absorption material 2 is composed of an HIPE foam 1. The HIPE foam 1 contains a crosslinked polymer 11 containing a component derived from a styrenic monomer and / or an acrylic monomer as a base material resin. A glass transition temperature of the crosslinked polymer 11 is 60°C or higher. A molecular weight between crosslinking points of the crosslinked polymer 11 is 3×103 or more. Apparent density of the HIPE foam 1 is 35 kg / m3 or more and less than 100 kg / m3. A ratio of 10%-strain compression stress to 50%-strain compression stress at 23°C exceeds 0.70 and 1.0 or less.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an impact absorbing material. [Background technology]

[0002] Conventionally, a method has been known in which a water-in-oil type high internal phase emulsion (i.e., HIPE) is formed by incorporating a high ratio of an aqueous phase made of an aqueous liquid such as water into an organic phase containing a vinyl monomer, a crosslinking agent, an emulsifier, a polymerization initiator, etc., and the organic phase is polymerized in the emulsion to obtain a porous polymer called a HIPE foam, etc. This porous polymer is a polymer that reflects the dispersion form of the organic phase and the aqueous phase in the high internal phase emulsion and the dispersion form of the aqueous phase during polymerization, and has a bubble structure in which many bubbles are uniformly present in the polymer, and also has an open bubble structure in which many through holes are formed to communicate between the bubbles. HIPE foam is expected to be used for applications such as absorbents and separators.

[0003] For example, Patent Document 1 proposes a HIPE foam with adjusted density, glass transition temperature, and toughness index. According to Patent Document 1, such a HIPE foam has excellent toughness and is suitable for products such as wipes. Furthermore, Patent Document 2 proposes an organic porous body (i.e., a HIPE foam) obtained by the so-called HIPE method and having a predetermined cell structure. According to Patent Document 2, such a HIPE foam is used as an adsorbent with high physical strength and excellent adsorption amount and adsorption speed, an ion exchanger with excellent durability against swelling and shrinkage, and a chromatography packing with excellent separation ability. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Special Publication No. 2003-514052 [Patent Document 2] JP 2003-246809 A Summary of the Invention [Problem to be solved by the invention]

[0005] HIPE foam is expected to be applied to shock absorbing materials used to protect objects from external forces in the fields of automobile materials, construction materials, logistics materials, etc. However, when using HIPE foam as a shock absorbing material, the technology of Patent Document 1 may reduce the amount of energy absorbed per unit weight, and the technology of Patent Document 2 may reduce the energy absorption performance under high strain. Therefore, it has not been possible to obtain a HIPE foam suitable as a shock absorbing material with conventional technology.

[0006] The present invention has been made in view of the above background, and aims to provide an impact absorbing material which is excellent in energy absorption amount per unit weight and which exhibits little change in energy absorption performance over a wide range of strain amounts. [Means for solving the problem]

[0007] One aspect of the present invention is an impact absorbing material made of HIPE foam, The HIPE foam has a base resin of a crosslinked polymer containing a component derived from a styrene-based monomer and / or an acrylic monomer, The glass transition temperature of the crosslinked polymer is 60° C. or higher, The molecular weight between crosslinking points of the crosslinked polymer is 3×10 3 That's all. The apparent density of the above HIPE foam is 35kg / m 3 More than 100kg / m 3 is less than The impact absorbing material has a ratio of the compressive stress at 10% strain to the compressive stress at 50% strain of the HIPE foam at 23° C. that is greater than 0.70 and is 1.0 or less. Effect of the Invention

[0008] The impact absorbing material is composed of HIPE foam, and the HIPE foam uses a crosslinked polymer containing a component derived from a styrene monomer and / or an acrylic monomer as a base resin. Furthermore, the apparent density, glass transition temperature, molecular weight between crosslinking points, and ratio of compressive stress at 10% strain to compressive stress at 50% strain are within the above ranges. Therefore, the impact absorbing material has excellent energy absorption per unit weight and little change in energy absorption performance over a wide range of strain. [Brief description of the drawings]

[0009] [Figure 1] Figure 1(a) is a low-vacuum scanning electron microscope photograph (magnification: 500x) of a HIPE foam with an average bubble diameter of 18 μm, Figure 1(b) is a low-vacuum scanning electron microscope photograph (magnification: 500x) of a HIPE foam with an average bubble diameter of 44 μm, and Figure 1(c) is a low-vacuum scanning electron microscope photograph (magnification: 500x) of a HIPE foam with an average bubble diameter of 90 μm. [Diagram 2] FIG. 2 is a schematic diagram of a dynamic mechanical properties measurement (DMA) curve obtained by DMA of a HIPE foam. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] Next, a preferred embodiment of the impact absorbing material will be described. In this specification, when a numerical value or a physical property value is enclosed before and after the symbol "~", the values ​​before and after the symbol are included. When a numerical value or a physical property value is expressed as a lower limit, it means that the value is equal to or greater than the numerical value or physical property value, and when a numerical value or a physical property value is expressed as an upper limit, it means that the value is equal to or less than the numerical value or physical property value. In this specification, mass and weight, mass% and weight%, parts by mass and parts by weight are essentially synonymous.

[0011] [Shock absorbing material] The impact absorbing material is composed of HIPE foam as described above. The impact absorbing material is used for, for example, automobile materials, construction materials, logistics materials, cushioning materials, bedding, etc. The impact absorbing material is suitable for, for example, automobile materials such as tibia pads, door pads, and bumpers. In particular, shock absorbing materials for automotive materials must adequately absorb the large impact that occurs during a collision, etc., and reduce the impact acceleration experienced by occupants. As described below, the above-mentioned HIPE foam is lightweight, has excellent energy absorption per unit weight, and can adequately absorb energy over a wide range of strain amounts, making it highly suitable for use as tibia pads, door pads, and bumpers for vehicles, and is particularly suitable as tibia pads.

[0012] [HIPE Form] HIPE foam is a porous polymer also called PolyHIPE foam, polyHIPE material, high internal phase emulsion porous body, high internal phase emulsion foam, etc., and is obtained by polymerizing monomers in a water-in-oil type high internal phase emulsion in which a high ratio of aqueous phase is contained in an organic phase. High internal phase emulsion is commonly called HIPE. More specifically, HIPE foam is a porous body with an open-cell structure that has many bubbles and uses a crosslinked polymer as the base resin. Since HIPE foam has an open cell structure, it is not easily affected by the so-called air spring, which occurs in foams with closed cell structures, when the HIPE foam is compressed and deformed. In addition, since the HIPE foam has a moderately fragile cell structure, the cell walls are prone to buckling when a relatively large compressive stress is applied. By adjusting the HIPE foam having such properties to the range of physical properties described below, the increase in compressive stress accompanying the increase in strain can be made gentle, and energy can be appropriately absorbed over a wide range of strain.

[0013] HIPE foam is a porous cross-linked polymer obtained by polymerizing a vinyl monomer (specifically, a styrene monomer and / or an acrylic monomer) in the presence of a cross-linking agent in a water-in-oil type high internal phase emulsion in which a high ratio of an aqueous phase is encapsulated in an organic phase. HIPE foam uses a cross-linked polymer containing a component derived from a styrene monomer and / or an acrylic monomer as a base resin, which is obtained by polymerizing a styrene monomer and / or an acrylic monomer in a water-in-oil type high internal phase emulsion. Specifically, HIPE foam contains a component derived from a styrene monomer and / or an acrylic monomer in the polymer skeleton of the cross-linked polymer. Also, HIPE foam is a porous cured material obtained by curing a high internal phase emulsion, and the cell walls can be said to be composed of a crosslinked polymer (e.g., a vinyl-based crosslinked polymer). The cells can also be said to be pores. HIPE foam becomes a polymer (specifically, a porous crosslinked polymer) that reflects the dispersion form of the organic phase and the aqueous phase in the high internal phase emulsion and the dispersion shape of the aqueous phase (i.e., the dispersed phase) during polymerization.

[0014] Since HIPE foam is a structure composed of crosslinked polymers, it tends to have low resistance to load and shear (specifically, shear stress and shear stress), and is a relatively brittle polymer. In addition, since the polymer of HIPE foam is difficult to stretch during the manufacturing process, it generally does not easily cause molecular orientation and has little anisotropy. HIPE foam is distinguished from foams that are stretched during manufacturing, such as foams obtained by extrusion foaming using an extruder, and foamed bead moldings obtained by foaming expandable resin particles and molding the foamed beads in a mold.

[0015] [Bubble structure] As described above, the HIPE foam is a porous body having an open-cell structure. As illustrated in Figs. 1(a) to (c), the HIPE foam 1 has a cell structure in which a large number of cells 13 are uniformly present in the porous crosslinked polymer 11 constituting the HIPE foam, and has an open-cell structure in which a large number of through-holes 14 are formed, which penetrate the cell walls 12 and communicate between adjacent cells. In Figs. 1(a) to (c), the cells 13 are portions surrounded by the cell walls 12. The through-holes 14 are holes that penetrate the cell walls 12 and communicate between adjacent cells 13. Specifically, the through-holes 14 are holes that are formed in the cell walls 12 and communicate between adjacent cells 13 with the cell walls 12 in between. The through-holes 14 can also be called pores, micropores, through-windows, or connecting holes.

[0016] In the HIPE foam, the average diameter Φ1 of the bubbles is about 5 to 100 μm, and the average diameter Φ2 of the through holes is about 1 to 30 μm. Since the through holes are holes formed in the bubble walls and communicate between the bubbles, the average diameter Φ2 of the through holes is usually smaller than the average diameter Φ1 of the bubbles. The average diameter Φ1 of the bubbles is the average value of the circle-equivalent diameters of the bubbles, which is the diameter of a perfect circle having the same area as the area of ​​the bubbles in the cross section of the HIPE foam. The average diameter Φ2 of the through holes is the average value of the circle-equivalent diameters of the through holes, which is the diameter of a perfect circle having the same area as the area of ​​the through holes in the cross section of the HIPE foam. The method for measuring the average diameter Φ1 of the bubbles and the average diameter Φ2 of the through holes will be described later, but for example, they are measured by image analysis of the open-cell structure of the HIPE foam.

[0017] The average diameter Φ1 of the bubbles is 20 to 100 μm, the average diameter Φ2 of the through holes is 5 to 20 μm, and the ratio Φ1 / Φ2 of the average diameter Φ1 of the bubbles to the average diameter Φ2 of the through holes is preferably 3 to 5. In this case, it is possible to suppress the cell structure of the HIPE foam from being excessively embrittled, while suppressing the cell structure from being excessively deformed by a load. This further suppresses the deterioration of the energy absorption performance of the impact absorbing material at the time of high strain, and further improves the energy absorption amount per unit weight of the impact absorbing material. From the viewpoint of further improving this effect, the average diameter Φ1 of the bubbles is preferably 25 to 95 μm. Moreover, the average diameter Φ2 of the through holes is preferably 6 to 18 μm, and more preferably 8 to 16 μm. Moreover, the ratio Φ1 / Φ2 is preferably 3.0 to 5.0, more preferably 3.2 to 4.8, and even more preferably 3.4 to 4.6.

[0018] The average bubble size can be controlled by adjusting the droplet size of the aqueous phase (i.e., the dispersed phase) of the high internal phase emulsion in the manufacturing method of the HIPE foam described below. For example, by reducing the droplet size, the bubble size becomes finer, and the average bubble size in the HIPE foam can be easily adjusted to, for example, 100 μm or less.

[0019] The through holes are formed by breaking the oil film due to the volumetric shrinkage of the polymer when the monomer is polymerized in the water-in-oil type high internal phase emulsion in the manufacturing method of HIPE foam described later. The oil film becomes the above-mentioned cell wall as the polymerization and crosslinking proceed. The average diameter of the through holes can be controlled by adjusting the stirring power density, polymerization rate, viscosity of the oil phase, etc. in the manufacturing method of HIPE foam described later. For example, by increasing the stirring power density, the diameter of the through holes becomes fine, and in the HIPE foam, the average diameter of the through holes can be easily adjusted to, for example, 20 μm or less.

[0020] The average number of bubbles per unit area in HIPE foam is 120 / mm 2 More than 2400 pieces / mm 2In this case, it is possible to suppress the cell structure of the HIPE foam from being excessively embrittled and to suppress the cell structure from being excessively deformed by a load. From the viewpoint of further improving this effect, the average number of cells is preferably 150 cells / mm or less. 2 More than 2200 pieces / mm 2 It is preferable that the number of particles is less than 300 / mm 2 More than 2100 pieces / mm 2 More preferably, it is 500 pieces / mm or less. 2 More than 2000 pieces / mm 2 It is even more preferable that: The average number of through holes per unit area in HIPE foam is 700 / mm 2 More than 8000 pieces / mm 2 It is preferable that the number of pieces is 800 pieces / mm or less. 2 More than 7000 pieces / mm 2 In this case, it is easy to cause the cell walls to buckle appropriately, and it is easy to reduce the change in compressive stress due to the amount of strain.

[0021] The method for measuring the average number of bubbles and the average number of through holes per unit area in a HIPE foam is described later, and is measured by image analysis. The average number of bubbles can be controlled by adjusting the droplet diameter of the water phase (i.e., the dispersed phase) of the high internal phase emulsion in the manufacturing method of a HIPE foam described later. For example, by reducing the droplet diameter, the bubble diameter becomes finer and the average number of bubbles increases. The average number of through holes can be controlled by adjusting the stirring power density, polymerization rate, viscosity of the oil phase, etc. in the manufacturing method of a HIPE foam described later. For example, by increasing the stirring power density, the through hole diameter becomes finer and the average number of through holes in the HIPE foam increases.

[0022] [apparent density ρ] The apparent density ρ of HIPE foam is 35 kg / m 3 More than 100kg / m 3It is less than this range. By being in this range, it is possible to obtain a HIPE foam having a certain rigidity and a moderately fragile cell structure. As a result, while a moderately high compressive stress is shown in the region where the strain due to compression is small, the cell walls buckle moderately as the strain due to compression increases, so that the compressive stress at high strain does not become excessively high, and the change in compressive stress due to the amount of strain can be reduced. If the apparent density ρ of the HIPE foam is too low, the rigidity decreases and the amount of energy absorbed per unit weight decreases. From the viewpoint of further improving the energy absorption amount per unit weight of the impact absorbing material, the apparent density ρ of the HIPE foam is set to 38 kg / m 3 It is preferable that the thickness is 40 kg / m or more. 3 It is more preferable that the apparent density ρ of the HIPE foam is 90 kg / m or more. On the other hand, if the apparent density of the HIPE foam is too high, the HIPE foam becomes excessively hard, the compressive load at high strain increases, and the energy absorption performance of the impact absorbing material at high strain decreases. From the viewpoint of further improving the energy absorption performance at high strain and further reducing the weight of the impact absorbing material, the apparent density ρ of the HIPE foam is 90 kg / m or more. 3 It is preferable that the thickness is less than 80 kg / m 3 More preferably, it is 60 kg / m or less. 3 It is even more preferable that:

[0023] The apparent density ρ of a HIPE foam is calculated by dividing the weight by the volume.

[0024] The apparent density ρ of the HIPE foam is adjusted to be within the above range by adjusting the ratio of the total amount of vinyl monomer, crosslinking agent, emulsifier, and polymerization initiator to the amount of aqueous phase (specifically, aqueous liquid) in the manufacturing method of the HIPE foam described below.

[0025] The ratio of the cell wall equivalent thickness t of the HIPE foam to the apparent density ρ of the HIPE foam is 0.0060 μm / [kg / m 3 ] or more, and preferably 0.0065 μm / [kg / m 3] or more, and more preferably 0.0070 μm / [kg / m 3 In this case, it is easier to improve the amount of energy absorbed per unit weight. On the other hand, the above ratio is preferably 0.035 μm / [kg / m] or more. 3 ] or less, and preferably 0.032 μm / [kg / m 3 ] or less, and more preferably 0.030 μm / [kg / m 3 In this case, it is possible to easily suppress the change in compressive stress due to the amount of strain. The cell wall equivalent thickness t of the HIPE foam is calculated by the following formula (α), where d is the average cell diameter of the HIPE foam, X=ρs / ρf, ρs is the density of the base resin, and ρf is the apparent density of the HIPE foam. t=d[(X / (X-1)) 1 / 3 −1] (α) The above formula (α) is the relationship of the volume fraction of the base resin in the HIPE foam (i.e., (ρf-ρg) / (ρs-ρg)=[(d+t) 3 -d 3 ] / (d+t) 3 ) in which the gas density in the cells: ρg is approximated to 0. Using the above formula, the cell wall thickness corresponding to the average cell wall thickness of the HIPE foam can be calculated. From the viewpoint of stably achieving the desired physical properties of the HIPE foam, the cell wall equivalent thickness t of the HIPE foam is preferably 0.3 μm or more and 3 μm or less, and more preferably 0.5 μm or more and 2 μm or less.

[0026] [Glass transition temperature] The glass transition temperature of the crosslinked polymer constituting the HIPE foam is 60°C or higher. This allows the rigidity of the HIPE foam to be increased. This is because the strength of the resin skeleton is improved by increasing the glass transition temperature. If the glass transition temperature is too low, the rigidity decreases and the energy absorption amount per unit weight decreases. In addition, when used in an environment where the ambient temperature is high, the mechanical properties of the impact absorbing material may decrease. From the viewpoint of increasing the rigidity and improving the energy absorption amount per unit weight of the impact absorbing material, the glass transition temperature of the crosslinked polymer constituting the HIPE foam is more preferably 65°C or higher. In addition, from the viewpoint of suppressing the impact absorbing material from becoming excessively brittle, the glass transition temperature of the crosslinked polymer constituting the HIPE foam is preferably 160°C or lower, more preferably 150°C or lower, and even more preferably 130°C or lower.

[0027] The glass transition temperature of the crosslinked polymer that constitutes the HIPE foam is measured by differential scanning calorimetry (DSC) analysis based on JIS K7121:1987. The glass transition temperature is the midpoint glass transition temperature of the DSC curve. The condition of the test specimen is adjusted as follows: (3) The glass transition temperature is measured after a certain heat treatment.

[0028] The glass transition temperature of the crosslinked polymer constituting the HIPE foam is adjusted to be within the above range by adjusting the type and mixing ratio of the vinyl monomer, the type and mixing ratio of the crosslinking agent, etc. in the manufacturing method of the HIPE foam described below.

[0029] [Molecular weight between crosslinking points Mc] The molecular weight Mc between crosslinking points is an index of the degree of crosslinking of the crosslinked polymer constituting the HIPE foam. The molecular weight Mc between crosslinking points of the crosslinked polymer constituting the HIPE foam is 3×10 3This makes it possible to increase the rigidity of the HIPE foam while suppressing excessive embrittlement of the HIPE foam. If the molecular weight between crosslinking points is too small, the degree of crosslinking is too high, which makes the foam more likely to become embrittled and reduces the amount of energy absorbed per unit weight. From the viewpoint of suppressing embrittlement and further improving the amount of energy absorbed per unit weight, the molecular weight between crosslinking points Mc of the crosslinked polymer constituting the HIPE foam is set to 4×10 3 It is preferable that the value is 5×10 or more. 3 More preferably, it is 6×10 3 From the viewpoint of suppressing the decrease in rigidity due to the decrease in the degree of crosslinking of the polymer and further improving the amount of energy absorption per unit weight, the molecular weight Mc between crosslinking points of the crosslinked polymer constituting the HIPE foam is more preferably 2×10 5 It is preferable that the value is less than 1×10 5 It is more preferable that it is 9×10 or less. 4 It is even more preferable that:

[0030] The molecular weight Mc between crosslinking points of the crosslinked polymer that constitutes the HIPE foam is measured as follows. Dynamic mechanical analysis (DMA) is performed on the HIPE foam under the conditions of frequency: 1 Hz, load: 98 mN, and deformation mode: compression. At this time, as the temperature rises, the crosslinked polymer that constitutes the HIPE foam transitions from a glassy state to a rubbery state, so in the DMA curve obtained by plotting temperature on the horizontal axis and storage modulus E' on the vertical axis, the storage modulus E' drops sharply at the glass transition temperature Tg (see Figure 2). After that, the DMA curve shows a plateau region (rubber-like flat section). In this plateau region, E' is proportional to temperature, so the molecular weight Mc between crosslinking points can be calculated from the following formula (I). The unit of the molecular weight Mc between crosslinking points is g / mol. Mc = 2(1 + μ)ρRT / E' (I)

[0031] In formula (I), μ is the Poisson's ratio, μ = 0.5. ρ is the apparent density of the HIPE foam, kg / m3 , R is the gas constant: 8.314 J / K / mol. T and E' are the temperature (unit: K) and storage modulus (unit: Pa) at any point on the rubber-like flat part, respectively. T and E' are values ​​measured on the rubber-like flat part. From the viewpoint of being able to properly calculate the molecular weight Mc between crosslinking points, it is preferable to measure the above E' in the temperature range of Tg+50°C to Tg+80°C (where Tg is the glass transition temperature of the crosslinked polymer constituting the HIPE foam). The Poisson's ratio is a value inherent to a material, and is a value obtained by dividing the strain generated in the vertical direction by the strain generated in the parallel direction when stress is applied to an object, and multiplying this by -1. Theoretically, the Poisson's ratio takes values ​​in the range of -1 to 0.5, and when this value is negative, it means that when it is crushed in the vertical direction, it is also crushed in the horizontal direction. Conversely, when it is positive, it means that when it is crushed in the vertical direction, it stretches in the horizontal direction. Under the measurement conditions for the dynamic viscoelastic analysis described above, the distortion occurring in the cross-linked polymer constituting the HIPE foam is extremely small, and it can be assumed that no change in volume occurs. Therefore, the storage modulus E' and the molecular weight between cross-linking points Mc are calculated under a constant volume condition, i.e., a Poisson's ratio of 0.5.

[0032] The molecular weight Mc between crosslinking points of the crosslinked polymer constituting the HIPE foam can be reduced by adding a crosslinking agent in the manufacturing method of the HIPE foam described below, and is adjusted to the above range by adjusting the type and mixing ratio of the crosslinking agent, the type and mixing ratio of the monomer, etc. described below.

[0033] [σ10 / σ50] Ratio of compressive stress at 10% strain σ10 to compressive stress at 50% strain σ50 The compressive stress at 50% strain σ50 represents the compressive stress at high strain, and the compressive stress at 10% strain σ10 represents the compressive stress at low strain. In the following description, the ratio σ10 / σ50 of the compressive stress at 10% strain σ10 to the compressive stress at 50% strain σ50 is appropriately referred to as the "compressive stress ratio σ10 / σ50". The compressive stress ratio σ10 / σ50 of the HIPE foam at a temperature of 23°C is greater than 0.70 and less than or equal to 1.0. This reduces the change in energy absorption performance over a wide range of strain amounts. If the compressive stress ratio σ10 / σ50 is too low, the compressive load at high strain increases, and the energy absorption performance at high strain decreases. From the viewpoint of further improving the energy absorption performance at high strain, the compressive stress ratio σ10 / σ50 is preferably 0.72 or more, more preferably 0.75 or more. On the other hand, from the viewpoint of suppressing the change in energy absorption performance due to the strain amount while enhancing the energy absorption performance at low strain, the compressive stress ratio σ10 / σ50 is preferably 0.95 or less, more preferably 0.90 or less. The method of measuring the compressive stress at 50% strain σ50 and the compressive stress at 10% strain σ10 will be described in the examples.

[0034] In order to suppress changes in energy absorption performance in areas with small strain amounts, the ratio σ10 / σ30 of the compressive stress σ10 at 10% strain to the compressive stress σ30 at 30% strain is preferably 0.85 or more and 1.0 or less, and more preferably 0.90 or more and 1.0 or less. In order to suppress changes in energy absorption performance over a wider range of strain amounts, the ratio σ10 / σ70 of the compressive stress σ10 at 10% strain to the compressive stress σ70 at 70% strain is preferably 0.35 or more and 0.50 or less.

[0035] The compressive stress ratios such as σ10 / σ50 can be adjusted within the above ranges by adjusting the apparent density of the HIPE foam, the components derived from the monomers that make up the base resin, the type and amount of crosslinking agent used, the average diameter of the through holes, and the ratio of the average diameter of the bubbles to the average diameter of the through holes, etc.

[0036] [Components] The crosslinked polymer constituting the HIPE foam is specifically a polymer of a monofunctional vinyl monomer and a crosslinking agent, and has a component derived from the monofunctional vinyl monomer. In this specification, the vinyl monomer is a styrene monomer, an acrylic monomer, etc. As the vinyl monomer, a styrene monomer and / or an acrylic monomer can be used. It can also be said that the HIPE foam has a crosslinked polymer, which is a polymer or copolymer of a styrene-based monomer and / or an acrylic-based monomer, as a base resin.

[0037] The crosslinked polymer is preferably composed of a polymer of a vinyl monomer including a styrene monomer and / or an acrylic monomer, and a crosslinking agent. Specifically, the crosslinked polymer preferably has a styrene monomer component and / or an acrylic monomer component in the polymer skeleton, and also has a crosslinking agent component described below. In this case, the balance between the toughness and rigidity of the HIPE foam is better. The styrene monomer component means a structural unit derived from a styrene monomer in the crosslinked polymer, and the acrylic monomer component means a structural unit derived from an acrylic monomer in the crosslinked polymer. From the viewpoint of facilitating the production of an impact absorbing material having desired physical properties, the content of the styrene-based monomer component and / or the acrylic-based monomer component in the crosslinked polymer is preferably 50% by weight or more, more preferably 60% by weight or more, and even more preferably 70% by weight or more. From the same viewpoint, the content of the styrene-based monomer component and / or the acrylic-based monomer component in the crosslinked polymer is preferably 95% by weight or less, and more preferably 90% by weight or less. The content of components derived from monomers other than the styrene-based monomer component, the acrylic monomer component, and the crosslinking agent component in the crosslinked polymer is preferably 20% by weight or less, more preferably 10% by weight or less, and even more preferably 5% by weight or less, relative to 100% by weight of the total of the styrene-based monomer component, the acrylic monomer component, and the crosslinking agent component that constitute the crosslinked polymer.

[0038] Examples of the styrene-based monomer include styrene compounds such as styrene, α-methylstyrene, o-methylstyrene, m-methylstyrene, p-methylstyrene, p-ethylstyrene, 2,4-dimethylstyrene, p-methoxystyrene, pn-butylstyrene, pt-butylstyrene, divinylbenzene, o-chlorostyrene, m-chlorostyrene, p-chlorostyrene, 2,4,6-tribromostyrene, styrenesulfonic acid, and sodium styrenesulfonate. Examples of the acrylic monomer include acrylic esters such as methyl acrylate, ethyl acrylate, propyl acrylate, butyl acrylate, 2-ethylhexyl acrylate, hydroxyethyl acrylate, cyclohexyl acrylate, phenyl acrylate, benzyl acrylate, isobornyl acrylate, dicyclopentanyl acrylate, and adamantyl acrylate; and methacrylic esters such as methyl methacrylate, ethyl methacrylate, propyl methacrylate, butyl methacrylate, 2-ethylhexyl methacrylate, hydroxyethyl methacrylate, hydroxypropyl methacrylate, cyclohexyl methacrylate, phenyl methacrylate, benzyl methacrylate, isobornyl methacrylate, dicyclopentanyl methacrylate, and adamantyl methacrylate. Examples of the acrylic monomer also include acrylamide, methacrylamide, and acrylonitrile.

[0039] The crosslinked polymer may be composed of a copolymer of a vinyl monomer containing methyl methacrylate and a (meth)acrylic acid ester other than methyl methacrylate, and a crosslinking agent, but is preferably composed of a copolymer of a vinyl monomer containing a styrene monomer and a (meth)acrylic acid ester, and a crosslinking agent. In other words, the crosslinked polymer preferably has a styrene monomer and a component (i.e., a structural unit) derived from a (meth)acrylic acid ester in the polymer skeleton. In this case, it is easy to obtain a HIPE foam composed of a crosslinked polymer having desired physical properties. Since the crosslinked polymer is a crosslinked polymer, it has a component (i.e., a structural unit) derived from a crosslinking agent in the polymer skeleton. The (meth)acrylic acid ester is an ester of (meth)acrylic acid and an alcohol, and is preferably an ester of (meth)acrylic acid and an alcohol having 1 to 20 carbon atoms. It is preferable that the crosslinked polymer contains a component derived from a styrene-based monomer and a component derived from a (meth)acrylic acid ester, and the (meth)acrylic acid ester is an ester of (meth)acrylic acid and an alcohol having a carbon number of 1 to 20. In this case, it is easy to obtain a HIPE foam having desired physical properties, and it is easy to adjust the glass transition temperature of the crosslinked polymer to a desired range.

[0040] When the vinyl monomer contains a styrene monomer, the content of styrene in the vinyl monomer is preferably 50% by weight or more, more preferably 60% by weight or more. The weight ratio of the styrene monomer to the (meth)acrylic acid ester is preferably 50:50 to 90:10, more preferably 60:40 to 80:20. In this case, the effects of reducing the production cost and facilitating the adjustment to desired physical properties can be obtained. Incidentally, (meth)acrylic acid means acrylic acid and / or methacrylic acid.

[0041] In addition, from the viewpoint of being able to stably obtain a crosslinked polymer having excellent physical properties and a desired glass transition temperature, the number of carbon atoms in the hydrocarbon group constituting the (meth)acrylic acid ester is preferably 1 to 20, more preferably 2 to 18, even more preferably 3 to 16, and even more preferably 4 to 12. The hydrocarbon group is more preferably a saturated hydrocarbon group. The hydrocarbon group may be either cyclic or noncyclic. Among these, it is preferable to use isobornyl methacrylate and / or butyl acrylate, and it is particularly preferable to use butyl acrylate. For example, when isobornyl methacrylate is used, the glass transition temperature of the crosslinked polymer can be easily increased, and when butyl acrylate is used, the glass transition temperature of the crosslinked polymer can be easily decreased.

[0042] A crosslinked polymer has a crosslinked structure and contains a crosslinking agent component. The crosslinking agent component is a structural unit derived from the crosslinking agent in the crosslinked polymer. The crosslinking agent is a compound that crosslinks (bonds) between the polymer chains that make up the polymer, forming a crosslinked structure in the polymer. As the crosslinking agent, for example, a vinyl-based compound having at least two functional groups selected from vinyl and isopropenyl groups in the molecule is used. When the crosslinked polymer contains a predetermined amount of a crosslinking agent component, the rigidity and toughness of the crosslinked polymer can be increased, and the value of the molecular weight between crosslinking points of the crosslinked polymer can be reduced. The vinyl-based compound also includes a compound containing a vinyl group and / or an isopropenyl group in the structure of the functional group, such as an acryloyl group or a methacryloyl group. From the viewpoint of stably polymerizing the crosslinking agent, the number of functional groups in the vinyl-based compound is preferably 6 or less, more preferably 5 or less, and more preferably 4 or less. In addition, from the viewpoint of making it easier to increase the toughness of the crosslinked polymer, the crosslinking agent preferably has functional groups at least at both ends of the molecule, and more preferably has functional groups only at both ends of the molecule.

[0043] The crosslinked polymer may contain one type of crosslinking agent component produced using one type of crosslinking agent, for example. However, since it is easy to increase the toughness of the crosslinked polymer while increasing the rigidity of the crosslinked polymer, it is preferable to contain a hard crosslinking agent component derived from a hard crosslinking agent having a relatively short molecular chain and a soft crosslinking agent component derived from a soft crosslinking agent having a relatively long molecular chain. In this case, it is easy to adjust the molecular weight Mc between crosslinking points of the crosslinked polymer constituting the HIPE foam, the compressive stress ratio σ10 / σ50 at a temperature of 23°C, etc., within the above range. In addition, excessive embrittlement of the impact absorbing material is easily suppressed, and even when a HIPE foam having a complex shape, such as having a thin portion, is produced, it is possible to suppress the occurrence of chipping in the HIPE foam. The hard crosslinking agent can also be called the first crosslinking agent, and the soft crosslinking agent can also be called the second crosslinking agent.

[0044] The hard crosslinking agent (i.e., the first crosslinking agent) is preferably a vinyl compound having a functional group equivalent of 130 g / mol or less. Since such a hard crosslinking agent has a relatively short molecular chain, it is considered that the mobility of the polymer molecular chain is reduced by copolymerizing with a vinyl monomer. By using a hard crosslinking agent, the rigidity of the HIPE foam is easily increased. From the viewpoint of facilitating the production of the HIPE foam, the lower limit of the functional group equivalent of the hard crosslinking agent is preferably about 30 g / mol, more preferably 40 g / mol, even more preferably 50 g / mol, and even more preferably 60 g / mol. The upper limit of the functional group equivalent of the hard crosslinking agent is preferably 120 g / mol. The functional group equivalent of the hard crosslinking agent means the molar mass of the hard crosslinking agent per functional group.

[0045] The soft crosslinking agent (i.e., the second crosslinking agent) is preferably a vinyl compound having a functional group equivalent of more than 130 g / mol and not more than 5000 g / mol. Since such a soft crosslinking agent has a relatively long molecular chain, it is considered that it can crosslink between polymer molecular chains by copolymerizing with a vinyl monomer without significantly reducing the mobility of the polymer molecular chain. The use of a soft crosslinking agent makes it easy to increase the toughness of the HIPE foam. From the viewpoint of easy handling, the upper limit of the functional group equivalent of the soft crosslinking agent is preferably 3000 g / mol, more preferably 2000 g / mol, and even more preferably 1000 g / mol. The lower limit of the functional group equivalent of the soft crosslinking agent is preferably 150 g / mol, more preferably 180 g / mol, and even more preferably 200 g / mol. The functional group equivalent of the soft crosslinking agent means the molar mass of the soft crosslinking agent per functional group.

[0046] From the viewpoint of further improving the above-mentioned effects, specifically, from the viewpoint of making it easier to increase the toughness and rigidity of the HIPE foam, and particularly from the viewpoint of suppressing excessive embrittlement and further improving the handleability in the impact absorbing material, the functional group equivalent of the soft crosslinking agent is preferably 60 g / mol or more larger than the functional group equivalent of the hard crosslinking agent, more preferably 80 g / mol or more larger, even more preferably 100 g / mol or more larger, and even more preferably 120 g / mol or more larger. In other words, the difference between the functional group equivalent of the soft crosslinking agent and the functional group equivalent of the hard crosslinking agent is 60 g / mol or more, more preferably 80 g / mol or more, even more preferably 100 g / mol or more, and even more preferably 120 g / mol or more. In addition, when two or more kinds of hard crosslinking agents are used, the weight average value of the functional group equivalents of all the hard crosslinking agents is calculated, and this value is taken as the functional group equivalent of the hard crosslinking agent. Similarly, when two or more types of soft crosslinking agents are used, the weight average value of the functional group equivalents of all the soft crosslinking agents is calculated, and this value is regarded as the functional group equivalent of the soft crosslinking agent.

[0047] Examples of vinyl compounds used as hard crosslinking agents include divinylbenzene, butanediol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, and hexanediol di(meth)acrylate. However, the number of functional groups in the hard crosslinking agent is two or more. The functional groups are preferably vinyl and / or isopropenyl. The hard crosslinking agent may be one type or two or more types. That is, the hard crosslinking agent component constituting the crosslinked polymer may be one type or two or more types. From the viewpoint of facilitating the adjustment of the rigidity of the HIPE foam, it is preferable to use divinylbenzene and / or butanediol di(meth)acrylate as the hard crosslinking agent.

[0048] Examples of vinyl compounds used as soft crosslinking agents include nonanediol di(meth)acrylate, decanediol di(meth)acrylate, polyethylene glycol di(meth)acrylate, polypropylene di(meth)acrylate, polytetramethylene glycol di(meth)acrylate, polyglycerin di(meth)acrylate, urethane di(meth)acrylate, epoxy di(meth)acrylate, polyester di(meth)acrylate, and silicone modified with (meth)acrylic at both ends. However, the number of functional groups in the soft crosslinking agent is two or more. The functional groups are preferably vinyl groups and / or isopropenyl groups. The soft crosslinking agent may be one type or two or more types. That is, the soft crosslinking agent component constituting the crosslinked polymer may be one type or two or more types. From the viewpoint of making it easier to adjust the toughness of the HIPE foam, it is preferable to use polyethylene glycol di(meth)acrylate as the soft crosslinking agent. In this case, the polyethylene glycol di(meth)acrylate preferably has 3-23 repeating structural units derived from ethylene glycol.

[0049] Table 1 shows the molecular weights of representative crosslinking agents and the molecular weights per functional group (i.e., functional group equivalents).

[0050] [Table 1]

[0051] When the crosslinked polymer is composed of at least a copolymer of a styrene-based monomer, an acrylic acid ester, and a crosslinking agent, from the viewpoint of easily adjusting the molecular weight Mc between crosslinking points and the compressive stress ratio σ10 / σ50 at a temperature of 23 ° C. to the above range, and from the viewpoint of a better balance between the toughness and rigidity of the HIPE foam, the content of the styrene-based monomer component in the crosslinked polymer is preferably 30 parts by weight or more and 90 parts by weight or less, more preferably 35 parts by weight or more and 80 parts by weight or less, and even more preferably 40 parts by weight or more and 70 parts by weight or less, based on 100 parts by weight of the total of the vinyl-based monomer component and the crosslinking agent component constituting the crosslinked polymer. From the same viewpoint, the content of the (meth)acrylic acid ester component in the crosslinked polymer is preferably 5 parts by weight or more and 50 parts by weight or less, more preferably 10 parts by weight or more and 40 parts by weight or less, and even more preferably 15 parts by weight or more and 35 parts by weight or less, based on 100 parts by weight of the total of the vinyl-based monomer component and the crosslinking agent component constituting the crosslinked polymer. In addition, it is preferable to use styrene as the styrene-based monomer, and the content of styrene in the styrene-based monomer is preferably 50% by weight or more, more preferably 80% by weight or more, and even more preferably 90% by weight or more.

[0052] From the viewpoint of easily adjusting the molecular weight Mc between crosslinking points and the compressive stress ratio σ10 / σ50 at a temperature of 23°C of the crosslinked polymer within the above-mentioned ranges, the content of the crosslinking agent component in the crosslinked polymer (specifically, the total content of the soft-based crosslinking agent component and the hard-based crosslinking agent component) is preferably 5 parts by weight or more and 30 parts by weight or less, and more preferably 7 parts by weight or more and 27 parts by weight or less, relative to 100 parts by weight in total of the vinyl-based monomer component and the crosslinking agent component constituting the crosslinked polymer.

[0053] From the viewpoint of easily increasing the rigidity of the HIPE foam and easily adjusting the molecular weight Mc between crosslinking points and the compressive stress ratio σ10 / σ50 at a temperature of 23 ° C. to the above range, the content of the hard crosslinking agent component in the crosslinked polymer is preferably 1 part by weight or more and 18 parts by weight or less, more preferably 3 parts by weight or more and 17 parts by weight or less, and even more preferably 5 parts by weight or more and 15 parts by weight or less, relative to 100 parts by weight of the total of the vinyl monomer component and the crosslinking agent component constituting the crosslinked polymer. In addition, from the viewpoint of easily adjusting the molecular weight Mc between crosslinking points and the compressive stress ratio σ10 / σ50 at a temperature of 23 ° C. to the above range while suppressing excessive embrittlement of the HIPE foam, the content of the soft crosslinking agent component in the crosslinked polymer is preferably 2 parts by weight or more and 18 parts by weight or less, more preferably 3 parts by weight or more and 10 parts by weight or less, relative to 100 parts by weight of the total of the vinyl monomer component and the crosslinking agent component constituting the crosslinked polymer. From the viewpoint of easily adjusting the molecular weight Mc between crosslinking points and the compressive stress ratio σ10 / σ50 at a temperature of 23°C within the above ranges, the weight ratio of the hard crosslinking agent component to the soft crosslinking agent component is preferably 0.2 or more and 6 or less, more preferably 0.3 or more and 5 or less, even more preferably 1 or more and 4 or less, and particularly preferably 1.2 or more and 3.0 or less.

[0054] [Manufacturing method] HIPE foam is produced by polymerizing a high internal phase emulsion, specifically by polymerizing a water-in-oil type high internal phase emulsion. The organic phase of the water-in-oil type high internal phase emulsion is a continuous phase containing vinyl monomers, crosslinking agents, emulsifiers, polymerization initiators, etc., and the aqueous phase is a dispersed phase containing water such as deionized water. Specifically, HIPE foam can be produced by carrying out an emulsification step, a polymerization step, and a drying step as follows.

[0055] First, an aqueous liquid (aqueous phase) containing water is dropped into an oily liquid (organic phase) containing organic substances such as a vinyl monomer, a crosslinking agent, an emulsifier, and a polymerization initiator while stirring to prepare a water-in-oil type high internal phase emulsion (emulsification step). In the emulsification step, a high internal phase emulsion can be prepared by adding an aqueous liquid to an oily liquid so that the aqueous phase is, for example, three times or more the organic phase in volume ratio. The ratio of the aqueous phase to be contained in the organic phase can be adjusted by the weight ratio of the organic phase to the aqueous phase. The content of the aqueous phase in the high internal phase emulsion is preferably 900 to 2700 parts by weight, more preferably 1000 to 2500 parts by weight, and even more preferably 1100 to 2400 parts by weight, relative to 100 parts by weight of the organic phase. Next, the high internal phase emulsion is heated to polymerize the vinyl monomer, crosslinking agent, etc. in the organic phase to obtain a polymerization product (specifically, a crosslinked polymer containing water) (polymerization step). Thereafter, the polymerization product is dried to obtain a HIPE foam composed of a crosslinked polymer (drying step).

[0056] The stirring speed in the emulsification step is not particularly limited. For example, the stirring power density is 0.1 kW / m 3 ~5kW / m 3 The rate of addition of the aqueous liquid to the oily liquid in the emulsification step is not particularly limited, but may be started by adding the oily liquid and the aqueous liquid to the stirring vessel in advance, or may be added only to the oily liquid in advance and stirred, and then the aqueous liquid may be added to the oily liquid using a pump or the like. The rate of addition of the aqueous liquid in this case is not particularly limited, but may be adjusted within a range of, for example, 10 wt% / min to 1000 wt% / min relative to the oily liquid. The emulsification method is not particularly limited, but may be a batch-type emulsification process in which emulsification is performed using a stirring vessel or a centrifugal shaker equipped with a stirring device, or a continuous-type emulsification process in which the oily liquid and the aqueous liquid are continuously supplied and mixed in a line equipped with a static mixer, mesh, or the like.

[0057] The aqueous phase may contain water such as deionized water, a polymerization initiator, an electrolyte, etc. In the emulsification step, for example, an oily liquid and an aqueous liquid are prepared, and the aqueous liquid is added to the oily liquid under stirring to prepare a high internal phase emulsion. In the emulsification step, additives such as a flame retardant, a flame retardant auxiliary, a light resistance agent, and a colorant may be appropriately blended into the aqueous phase and / or the organic phase.

[0058] The flame retardant is used to improve the flame retardancy of the HIPE foam. Examples of the flame retardant include organic compounds containing halogen, phosphorus, nitrogen, silicone, etc.; inorganic compounds containing metal hydroxide, phosphorus, nitrogen, etc., and the flame retardant can be used within a range that does not impair the effects of the present invention. When the flame retardant is blended, the blending amount is preferably 5 to 20 parts by weight per 100 parts by weight of the total of the vinyl monomer component and the crosslinking agent component constituting the crosslinked polymer. From the viewpoint of easily imparting excellent flame retardancy even with a small amount of addition, it is preferable to use a brominated bisphenol flame retardant having a 2,3-dibromo-2-methylpropyl group and / or a brominated bisphenol flame retardant having a 2,3-dibromopropyl group, and it is even more preferable to use 2,2-bis(4-(2,3-dibromo-2-methylpropoxy)-3,5-dibromophenyl)propane. In addition, a flame retardant auxiliary can be appropriately blended into the HIPE foam in order to improve the flame retardant efficiency. For example, when a halogen-based flame retardant is used, if a radical generator such as dicumyl peroxide is used as the flame retardant auxiliary, the decomposition of the radical generator promotes the detachment of halogen from the flame retardant, and the flame retardant efficiency can be improved. When a halogen-based flame retardant is used, if an antimony compound such as antimony trioxide is used as the flame retardant auxiliary, the radical trapping effect of the halogen-based flame retardant and the air blocking effect of antimony oxide are combined synergistically, and the flame retardant efficiency can be improved. The flame retardant may be used alone, or two or more flame retardants with different flame retardant mechanisms may be used in combination.

[0059] The polymerization initiator is used to start the polymerization of vinyl monomers. As the polymerization initiator, a radical polymerization initiator can be used. Specifically, dilauroyl peroxide (LPO), di(4-t-butylcyclohexyl)peroxydicarbonate, 1,1,3,3-tetramethylbutylperoxy-2-ethylhexanoate, di(3,5,5-trimethylhexanoyl)peroxide, t-butylperoxypivalerate, t-hexylperoxypivalerate, t-butylperoxyneoheptanoate, t-butylperoxyneodecanoate, t-hexylperoxyneodecanoate, Organic peroxides such as di(2-ethylhexyl)peroxydicarbonate, 1,1,3,3-tetramethylbutylperoxyneodecanoate, and benzoyl peroxide; and azo compounds such as 2,2'-azobisisobutyronitrile, 2,2'azobis(4-methoxy-2,4-dimethylvaleronitrile), 2,2'azobis(4-dimethylvaleronitrile), dimethyl 2,2'azobis(2-methylpropionate), and 2,2'azobis(2-methylbutyronitrile) are used. From the viewpoint of suppressing boiling of water during polymerization, the one-hour half-life temperature of the polymerization initiator is preferably 95°C or less, and more preferably 90°C or less. In addition, from the viewpoint of safety, in order to suppress decomposition of the polymerization initiator at room temperature, the one-hour half-life temperature of the polymerization initiator is preferably 50°C or more, and more preferably 55°C or more. As the polymerization initiator, one or more substances can be used. From the viewpoint of shortening the polymerization time without decreasing the uniformity of the density of the HIPE foam, it is preferable to use a combination of an organic peroxide having a one-hour half-life temperature of 50° C. or more and less than 70° C. and an organic peroxide having a one-hour half-life temperature of 70° C. or more and 90° C. or less. The polymerization initiator can be added to the organic phase and / or the aqueous phase. When the polymerization initiator is added to the aqueous phase, a water-soluble polymerization initiator such as 2,2'azobis(2-(2-imidazolin-2-yl)propane)dihydrochloride, 2,2'azobis(2-methylpropionamidine dihydrochloride, potassium persulfate, ammonium persulfate, etc. may be used. The amount of the polymerization initiator to be added can be, for example, in the range of 0.1 to 5 parts by weight per 100 parts by weight of the total of the vinyl monomer and the crosslinking agent.

[0060] The emulsifier is used for forming and stabilizing a high internal phase emulsion. For example, a surfactant can be used as the emulsifier. Specifically, glycerol esters such as polyglycerol condensed ricinoleate, polyglycerol stearate, polyglycerol oleate, polyglycerol laurate, and polyglycerol myristate; sorbitol esters such as sorbitan oleate, sorbitan stearate, sorbitan laurate, sorbitan laurate, and sorbitan palmitate; ethylene glycol sorbitan esters; ethylene glycol esters; copolymers of polyethylene glycol and polypropylene glycol, and the like, can be used. The amount of the emulsifier to be added can be, for example, in the range of 1 to 30 parts by weight per 100 parts by weight of the total of the vinyl monomer, the crosslinking agent, and the emulsifier.

[0061] The electrolyte is used to impart ionic strength to the aqueous phase and to increase the stability of the emulsion. As the electrolyte, a water-soluble electrolyte can be used. Specifically, calcium chloride, sodium chloride, magnesium chloride, sodium acetate, sodium citrate, sodium sulfate, calcium sulfate, magnesium sulfate, sodium dihydrogen phosphate, disodium hydrogen phosphate, etc. can be used. The amount of the electrolyte added can be, for example, in the range of 0.01 to 10 parts by weight with respect to 100 parts by weight of the aqueous liquid.

[0062] The polymerization temperature in the polymerization step is adjusted depending on, for example, the type of vinyl polymer, the type of polymerization initiator, the type of crosslinking agent, etc. The polymerization temperature is, for example, 50°C to 90°C.

[0063] In the drying process, the crosslinked polymer containing water is dried using an oven, a vacuum dryer, a high-frequency / microwave dryer, or the like. When the drying is completed, the places where water droplets were present in the emulsion before polymerization become bubbles in the polymer after drying, and a porous body can be obtained. Before drying, the crosslinked polymer can be dehydrated by squeezing it using, for example, a press machine. The squeezing can be performed at room temperature (for example, 23°C), but can also be performed at a temperature above the glass transition temperature of the crosslinked polymer that constitutes the HIPE foam. In this case, dehydration by squeezing becomes easier, and the drying time can be shortened. The crosslinked polymer can also be dehydrated by centrifugation. In this case, the drying time is also shortened. EXAMPLES

[0064] Examples and comparative examples of impact absorbing materials are described below. Impact absorbing material 2 is composed of HIPE foam 1 (see Figs. 1(a)-(c)). In this example, the HIPE foams shown in the examples in Tables 2-4 and the comparative examples in Tables 5 and 6 were produced by the following method. Note that the specific aspects of the HIPE foam according to the present invention are not limited to the aspects of the examples shown below, and the configuration can be appropriately changed without departing from the gist of the present invention. Note that "%" in the examples means % by weight.

[0065] [Example 1] First, a 3-L glass container equipped with a stirrer with a torque converter was charged with 44 g of styrene and 25 g of butyl acrylate as vinyl monomers, 16 g of divinylbenzene with a purity of 57% as a hard crosslinking agent (hereinafter referred to as the first crosslinking agent) (9.12 g as divinylbenzene), and 5 g of polyethylene glycol diacrylate (specifically, NK Ester A-400 manufactured by Shin-Nakamura Chemical Co., Ltd. / purity 95%) as a soft crosslinking agent (hereinafter referred to as the second crosslinking agent) (polyethylene glycol diacrylate). The following were added: 4.75 g of acrylate, 10 g of polyglycerol condensed ricinoleate as an emulsifier (specifically, CRS-75 manufactured by Sakamoto Yakuhin Kogyo Co., Ltd.), 0.5 g of dilauroyl peroxide as a polymerization initiator, 5 g of brominated bisphenol A derivative as a brominated flame retardant (specifically, 5 g of SR-130: 2,2-bis(4-(2,3-dibromo-2-methylpropoxy)-3,5-dibromophenyl)propane manufactured by Daiichi Kogyo Seiyaku Co., Ltd.), and 1 g of dicumyl peroxide as a flame retardant aid. These were mixed in a glass container to form an organic phase.

[0066] Stirring power density 1.6kW / m 3 While stirring the organic phase at 4000rpm, 2400g of deionized water was added at a rate of about 450g / min. Stirring was continued for 10 minutes after the addition of deionized water was completed to prepare a water-in-oil (i.e., W / O) high internal phase emulsion. The stirring power density after emulsification was 1.4kW / m 3 The stirring power density (kW / m 3 ) is calculated by calculating the power (kW) from the torque (N m) and rotation speed (rpm) of the mixing device, and the volume of the contents (m 3 ) can be calculated by dividing it by

[0067] Next, the stirring power density was set to 0.1 kW / m 3 The pressure in the glass container was reduced by connecting an aspirator to the container to remove the microbubbles contained in the emulsion. Ten minutes after the start of the reduction in pressure, the stirring was stopped and the pressure in the container was returned to atmospheric pressure.

[0068] The contents of the glass container were filled into a container having a length of about 250 mm, a width of about 180 mm, and a depth of about 90 mm, and polymerized in an oven at 70° C. for about 18 hours to obtain a water-containing HIPE foam. The HIPE foam was removed from the oven and cooled to room temperature.

[0069] After cooling, the HIPE foam was taken out of the container, washed with water, dehydrated, and dried in an oven at 85°C until it reached a constant weight. In this way, a rectangular HIPE foam (specifically, an impact absorbing material) made of a vinyl cross-linked polymer was obtained. The apparent density of this HIPE foam was 41 g / L (i.e., 41 kg / m 3 ) was.

[0070] The composition of the crosslinked polymer is shown in Table 2. The contents of the various components (vinyl monomer and crosslinking agent) in the crosslinked polymer can be calculated from the blending amounts of the various components (in the case of the crosslinking agent, the blending amount excluding impurities) and the total blending amount of the vinyl monomer component and the crosslinking agent component (excluding impurities) at the time of blending. In the tables, the compound names are abbreviated as follows: St: styrene BA: Butyl acrylate IBOMA: Isobornyl methacrylate DVB: Divinylbenzene PEGDA: Polyethylene glycol diacrylate PGPR: Polyglycerol condensed ricinoleate LPO: Dilauryl peroxide LTCP: Di(4-t-butylcyclohexyl) peroxydicarbonate Brominated BPA: Brominated Bisphenol A derivatives DCP: Dicumyl peroxide

[0071] [Examples 2 to 13, Comparative Examples 1 to 8] A HIPE foam was produced in the same manner as in Example 1, except that the charged composition was changed as shown in Tables 2 to 6. In Example 4, the stirring power density when stirring the organic phase was 3.0 kW / m3 After emulsification, the stirring power density was 2.6 kW / m 3 In Example 5, the stirring power density when stirring the organic phase was 0.04 kW / m 3 After emulsification, the stirring power density was 0.03 kW / m 3 In Example 6, the stirring power density when stirring the organic phase was 5.0 kW / m 3 After emulsification, the stirring power density was 4.4kW / m 3 In Example 7, the stirring power density when stirring the organic phase was 0.23 kW / m 3 After emulsification, the stirring power density was 0.20 kW / m 3 In Comparative Example 3, the stirring power density when stirring the organic phase was 7.8 kW / m 3 After emulsification, the stirring power density was 6.9 kW / m 3 In Comparative Example 4, the stirring power density when stirring the organic phase was 0.02 kW / m 3 After emulsification, the stirring power density was 0.01 kW / m 3 In Comparative Example 5, the stirring power density when stirring the organic phase was 0.04 kW / m 3 After emulsification, the stirring power density was 0.03 kW / m 3 It was.

[0072] [evaluation] The following measurements and evaluations were carried out for Examples 1 to 13 and Comparative Examples 1 to 8. The results are shown in Tables 2 to 6.

[0073] (apparent density:ρ) Three test pieces without a skin layer of a specified size (specifically, thickness: 20 mm, width: 25 mm, length: 120 mm) were cut out from the HIPE foam produced as described above so as to include the center of the HIPE foam. Then, the weight and actual dimensions (specifically, volume) of the test pieces were measured. The apparent density of the test pieces was calculated by dividing the weight of the test pieces by the volume, and the arithmetic average value of the apparent densities of the three test pieces was taken as the apparent density ρ of the HIPE foam.

[0074] (Glass transition temperature: Tg) Based on JIS K7121:1987, Tg was calculated by differential scanning calorimetry (i.e., DSC) analysis. As a measuring device, DSC250 manufactured by TA Instruments Japan Co., Ltd. was used. Specifically, first, a test piece of about 2 mg was taken from near the center of the HIPE foam. As a condition adjustment of the test piece, "(3) A case where the glass transition temperature is measured after a certain heat treatment" was adopted. Specifically, the taken test piece was left to stand for 24 hours or more in a constant temperature and humidity room at a temperature of 23°C and a humidity of 50%. Next, the test piece was heated at a heating rate of 10°C / min to a temperature about 30°C higher than the temperature at the end of the glass transition, and was held at this temperature for 10 minutes, and then cooled at a cooling rate of 10°C / min to a temperature about 50°C lower than the glass transition temperature. For example, in the measurement of Tg of the HIPE foam of Example 1, it was heated to 105°C and then cooled to 20°C. After cooling, the temperature was maintained for 10 minutes to stabilize the apparatus, and DSC measurement was performed at a temperature increase rate of 20°C / min up to a temperature about 30°C higher than the temperature at the end of the glass transition, to obtain a DSC curve. The midpoint glass transition temperature was determined from this DSC curve, and this value was taken as the glass transition temperature Tg. The measurement temperature range in Examples 1 to 13 and Comparative Examples 1 to 8 was 0°C to 185°C.

[0075] (Molecular weight between crosslinking points: Mc) Three cubic test pieces with no skin layer, each measuring 10 mm x 10 mm x 10 mm, were cut out from the center of the HIPE foam. Dynamic viscoelastic analysis (DMA) was performed on these three test pieces to measure the storage modulus E' in the temperature range of 0 to 200°C. The measurement device used was a DMA7100 manufactured by Hitachi High-Tech Science Corporation. The measurement conditions were as follows: Deformation mode: Compression ·Temperature: 0~200℃ Heating rate: 5℃ / min Frequency: 1Hz Load: 98mN

[0076] Using the storage modulus E' and temperature T in the rubbery flat portion measured by dynamic viscoelastic analysis of the above three test pieces, the molecular weight between crosslinking points Mc was calculated from the following formula (I). Note that FIG. 2 shows a schematic diagram of a DMA curve of a HIPE foam. The DMA curve is obtained by plotting temperature on the horizontal axis and storage modulus E' on the vertical axis. In the examples, the molecular weight between crosslinking points was calculated from the storage modulus E' at three temperatures randomly selected from the temperature range of Tg+50°C to Tg+80°C, which is the rubbery flat portion of the crosslinked polymer constituting the HIPE foam, and the arithmetic average value of the nine calculated molecular weights between crosslinking points was adopted as the molecular weight between crosslinking points Mc. Note that Tg is the glass transition temperature of the crosslinked polymer constituting the HIPE foam. Mc = 2(1 + μ)ρRT / E' (I) In addition, under the measurement conditions of the above dynamic viscoelastic analysis, the distortion generated in the cross-linked polymer constituting the HIPE foam is extremely small, and it can be assumed that no volume change occurs. Therefore, the storage modulus E' and the molecular weight Mc between cross-linking points were calculated under a constant volume condition, i.e., a Poisson's ratio of 0.5.

[0077] (average bubble diameter) The method for measuring the bubble diameter is as follows. Using a feather blade, samples for observation were cut out from the center of the short side and thickness direction of the rectangular parallelepiped HIPE foam, and from the center of the thickness direction at both ends of the short side. The samples were then observed with a low-vacuum scanning electron microscope (Miniscope (registered trademark) TM3030Plus manufactured by Hitachi High-Tech Science Corporation), and cross-sectional photographs were taken. Representative examples of cross-sectional photographs (magnification: 500 times) of the examples and comparative examples are shown in Figures 1(a) to (c). The detailed observation conditions were as follows. - Sample pretreatment: The sample was treated for electrical conductivity using a metal coating device (MSP-1S from Vacuum Device Co., Ltd.) Au-Pd was used as the target electrode. Magnification: 50x Acceleration voltage: 5kV Observation conditions: Surface (low magnification) Observation mode: Secondary electrons (standard)

[0078] Next, the cross-sectional photographs were analyzed using image processing software (NanoHunter NS2K-Pro from Nano Systems Co., Ltd.) to determine the average bubble diameter of each sample. The average bubble diameter of the HIPE foam was calculated by arithmetically averaging the three average bubble diameters obtained. The detailed analysis procedures and conditions were as follows: (1) Monochrome conversion (2) Smoothing filter (3x3, 8 neighborhoods, number of processes = 1) (3) Density unevenness correction (brighter than background, size = 5) (4) NS binarization (darker than background, clarity = 9, sensitivity = 1, noise removal, density range = 0 to 255) (5) Contraction (8 neighbors, number of processes = 1) (6) Image selection by feature (area) (select only 50~∞μm2, 8 neighbors) (7) Dilation without connections to neighbors (8 neighbors, number of processes = 3) (8) Measurement of circle equivalent diameter (calculated from area, 8 neighbors)

[0079] (average diameter of through holes) Cross-sectional photographs were taken in the same manner as for the bubble diameter, except that the observation magnification was changed to 500x and the observation mode was changed to backscattered electron method (standard). Next, the cross-sectional photographs were analyzed using image processing software (WinROOF2013, manufactured by Mitani Shoji Co., Ltd.) to determine the average through-hole diameter of each sample. The average diameter of the through-holes of the HIPE foam was calculated by arithmetically averaging the three average through-hole diameters obtained. The detailed analysis procedure and conditions were as follows: (1) Monochrome imaging (2) Averaging filter (filter size = 3 × 3, number of times = 1) (3) Automatic binarization (discriminant analysis method, extraction area = dark area, target density range = 0 to 255) (4) Morphology adjustment (dilation, times = 3) (5) Measurement from shape characteristics (measurement items = circle equivalent diameter, number)

[0080] (Average number of bubbles per unit area) The total number of bubbles obtained by measuring the average bubble diameter described above was multiplied by the observation area of ​​the actual SEM image (specifically, 7.68 mm2, 2.4 mm2 by 3.2 mm2 in a 50x magnification image). 2 The number of bubbles per unit area was calculated by dividing the measured value by the area of ​​the sample (the area of ​​the sample), and the average number of bubbles per unit area was calculated by taking the arithmetic mean of the three obtained numbers of bubbles per unit area.

[0081] (Average number of through holes per unit area) The total number of through holes obtained by measuring the average diameter of the through holes described above was multiplied by the observation area of ​​the actual SEM image (specifically, the area of ​​76,800 μm, 240 μm long and 320 μm wide, in a 500x observation image). 2 The number of through holes per unit area was calculated by dividing the number of through holes per unit area by the area (area of ​​the sample). The average number of through holes per unit area was calculated by taking the arithmetic average of the three numbers of through holes per unit area obtained.

[0082] (Ratio of cell wall thickness t of HIPE foam to apparent density of HIPE foam) The calculated apparent density of the HIPE foam, the average bubble diameter of the HIPE foam, and the density of the base resin constituting the HIPE foam were substituted into the following formula (α) to calculate the cell wall equivalent thickness t (μm) of the HIPE foam. Note that the density of the base resin in the examples and comparative examples was 1.1×10 3 kg / m 3 In formula (α), d is the average bubble diameter of the HIPE foam, X=ρs / ρf, ρs is the density of the base resin, and ρf is the apparent density of the HIPE foam. t=d[(X / (X-1)) 1 / 3 −1] (α) The calculated cell wall equivalent thickness t (μm) of the HIPE foam was calculated as the apparent density (kg / m 3 ) to obtain the ratio of the cell wall equivalent thickness t of the HIPE foam to the apparent density of the HIPE foam (μm / [kg / m 3 ]) was calculated.

[0083] (Closed bubble rate) Three test pieces without a skin layer measuring 25 mm x 25 mm x 25 mm were cut out from the center of the HIPE foam, and the closed cell ratio of the HIPE foam was measured by the pressure change method (pycnometer method) based on JIS K7138:2006. For the measurement, an air comparison specific gravity meter Model 1000 manufactured by Tokyo Science Co., Ltd. was used. The closed cell ratio of each test piece was calculated by the following formula (II), and the average value of the three test pieces was used. Closed cell ratio [%]=(Vx-W / ρ) / (Va-W / ρ)×100 (II) In formula (II), Vx is the true volume [mL] of the HIPE foam measured by the above method, Va is the apparent volume [mL] of the HIPE foam, W is the sample weight [g], and ρ is the specific gravity [-] of the resin that constitutes the HIPE foam. In the table, a closed cell rate of less than 1% is indicated as "<1," and a rate of more than 95% is indicated as ">95." From the viewpoint of making it easier to suppress changes in compression properties associated with an increase in the amount of strain, the closed cell ratio of the HIPE foam is preferably 10% or less, more preferably 5% or less, even more preferably 3% or less, and particularly preferably less than 1%.

[0084] (Compressive elastic modulus: E, compressive stress at 10% strain: σ10, compressive stress at 50% strain: σ50, etc.) A test piece without a skin layer measuring 25 mm x 50 mm x 50 mm was cut out from the center of the HIPE foam, and a compression test was carried out using this test piece. Specifically, a tabletop precision universal testing machine (specifically, an autograph AGS-10kNX manufactured by Shimadzu Corporation) was used to measure the elastic modulus, the compressive stress at 10% strain σ10, the compressive stress at 50% strain σ50, etc., in accordance with JIS K 6767:1999. In this specification, the compressive stress at x% strain is represented as σx. In addition, since the magnitude of the compressive modulus E is highly dependent on the apparent density ρ, the value of the compressive modulus E / ρ relative to the apparent density was calculated by dividing the compressive modulus by the apparent density. The details of the compression test are as follows. ·Room temperature: 23℃ ·Humidity: 50% - Test piece size: length: 50mm, width: 50mm, thickness: 25mm Compression speed: 10mm / min Compression rate: 0-80%

[0085] (Energy absorption amount EA) The amount of energy absorption is expressed as the area under the load-displacement curve (i.e., the compression waveform). The energy absorption (EA) in the region from 0% strain to 50% strain in the load-displacement curve measured in the compression test was calculated. The energy absorption per unit weight, EA / [V ρ], was calculated from this energy absorption EA, the volume V of the HIPE foam used in the compression test, and the apparent density ρ. From the viewpoint of excellent energy absorption characteristics and reducing the component weight of the impact absorbing material, the energy absorption amount EA / [V ρ] is preferably 1.0 J / g or more, more preferably 1.5 J / g or more, and even more preferably 2.0 J / g or more. Furthermore, from the viewpoint of the impact absorbing material not being too hard and being able to absorb impact appropriately, and also being able to ensure the safety of passengers in the event of a collision when used as an automobile material, the energy absorption amount EA / [V ρ] is preferably 5.0 J / g or less, more preferably 4.0 J / g or less, and even more preferably 3.0 J / g or less.

[0086] (Charpy impact strength: S) Five test pieces without a skin layer, each measuring 4 mm in thickness, 10 mm in width, and 80 mm in length, were cut out from the center of the HIPE foam, and a Charpy impact test was carried out in accordance with JIS K7111:2006 to measure the Charpy impact strength of the test pieces. The measurement was carried out using a Charpy impact tester manufactured by Toyo Seiki Seisakusho Co., Ltd., at a measurement temperature of 23°C and without a notch. The average value of the five points was used. In order to prevent excessive embrittlement of the HIPE foam and to improve its ease of handling as a shock absorbing material, the Charpy impact strength value is set at 100 J / m 2 More preferably, 150 J / m 2 More preferably, it is 200 J / m or more.2 More preferably, it is equal to or greater than this.

[0087] [Table 2]

[0088] [Table 3]

[0089] [Table 4]

[0090] [Table 5]

[0091] [Table 6]

[0092] As can be seen from Tables 2 to 4, the HIPE foams of the examples have excellent energy absorption per unit weight and show little change in energy absorption performance over a wide range of strain. Therefore, the HIPE foams of the examples can be said to be shock absorbing materials with excellent shock absorption performance.

[0093] Comparative Example 1 is an example in which the apparent density was low, and the amount of energy absorbed per unit weight was insufficient.

[0094] Comparative Example 2 is an example in which the apparent density was large, the compressive load at high strain was high, and the energy absorption performance at high strain was reduced.

[0095] Comparative Examples 3 to 5 and 7 are examples in which the compressive stress ratio σ10 / σ50 is small. In these comparative examples, the change in compressive load with the increase in the amount of strain was large. In addition, Comparative Examples 3 and 7 had insufficient energy absorption per unit weight.

[0096] Comparative Example 6 is an example having a low glass transition temperature, and Comparative Example 8 is an example having a low molecular weight between crosslinking points. In both Comparative Examples 6 and 8, the energy absorption amount per unit weight was insufficient. [Explanation of symbols]

[0097] 1 HIPE Form 11 Cross-linked polymers 12 Bubble Wall 13 Bubbles 14 Through hole 2. Shock absorbing material

Claims

1. A shock absorbing material made of HIPE foam, The HIPE foam has a base resin of a crosslinked polymer containing a component derived from a styrene-based monomer and / or an acrylic monomer, The crosslinked polymer has a glass transition temperature of 60° C. or higher, The molecular weight between crosslinking points of the crosslinked polymer is 3×10 3 That's all. The apparent density of the HIPE foam is 35 kg / m 3 More than 100kg / m 3 is less than The impact absorbing material has a ratio of the compressive stress at 10% strain to the compressive stress at 50% strain of the HIPE foam at 23°C that is greater than 0.70 and is 1.0 or less.

2. The HIPE foam has an average bubble diameter of 20 to 100 μm; the average diameter of the through holes penetrating the cell walls of the HIPE foam and communicating between adjacent cells is 5 to 20 μm; 2. The impact absorbing material according to claim 1, wherein the ratio of the average diameter of the bubbles to the average diameter of the through holes is 3 to 5.

3. The average number of bubbles per unit area in the HIPE foam is 120 / mm 2 More than 2400 pieces / mm 2 The impact absorbing material according to claim 1 or 2, wherein:

4. The crosslinked polymer contains a component derived from a styrene-based monomer and a component derived from a (meth)acrylic acid ester, and the (meth)acrylic acid ester is an ester of (meth)acrylic acid and an alcohol having 1 to 20 carbon atoms. The impact absorbing material according to any one of claims 1 to 3.

5. The crosslinked polymer comprises a component derived from a first crosslinking agent having a functional group equivalent of 130 g / mol or less, and a component derived from a second crosslinking agent having a functional group equivalent of more than 130 g / mol and 5000 g / mol or less. The impact absorbing material according to any one of claims 1 to 4.

Citation Information

Patent Citations

  • Absorbent foams made from high internal phase emulsions useful for acquiring and distributing aqueous fluids

    JP1999503177A

  • Organic porous material, manufacturing method for it and organic porous ion exchanger

    JP2003246809A

  • Foam materials obtained from high internal phase emulsions

    JP2003514052A

  • Rapid preparation of foaming materials from high-internal-phase emulsions

    JP2004529212A

  • Production method for foam

    JP2012051984A