Resin composition and molded article using said composition
The resin composition with inorganic acid acceptors addresses the decomposition and corrosion issues of THV resin during melt-molding, enabling use in general-purpose equipment while preserving the transparency and appearance of molded products.
Patent Information
- Application Number
- JP2021563862
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-12-11
- Filing Date
- 2020-11-30
- Publication Date
- 2024-10-02
- Estimated Expiration
- 2040-11-30
AI Technical Summary
THV resin decomposes under high-temperature melt-molding conditions, generating acidic gases that can cause equipment corrosion and impair the appearance of molded products, making it difficult to use in general-purpose molding equipment without special corrosion-resistant measures.
A resin composition containing tetrafluoroethylene-hexafluoropropylene-vinylidene fluoride copolymer and an inorganic acid acceptor, such as metal oxides or hydrotalcite compounds, captures and prevents the spread of acidic gases generated during melt molding, maintaining the transparency and appearance of the molded product.
The resin composition allows for melt-molding using general-purpose equipment without equipment corrosion and maintains the transparency and appearance of the molded product, suppressing clouding and yellowing.
Smart Images

Figure 0007560481000001 
Figure 0007560481000002 
Figure 0007560481000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a resin composition and a molded article using the composition, and more particularly to a tetrafluoroethylene-hexafluoropropylene-vinylidene fluoride copolymer resin composition and a film- or sheet-shaped molded article using the same. [Background technology]
[0002] Tetrafluoroethylene-hexafluoropropylene-vinylidene fluoride copolymers (hereinafter sometimes referred to as "THV resins") are used in hoses and gaskets for transporting chemicals, oils, fuels, etc., because of their excellent chemical resistance, contamination resistance, water repellency, insulation, and low friction. In addition, THV resins can be formed into films by melt molding, so they are used in a variety of applications, such as solar cell component films, release films, and glass interlayer films.
[0003] For example, Patent Document 1 discloses a release film mainly made of THV resin. The document also describes that the above-mentioned film is used as a release film in the semiconductor manufacturing process.
[0004] Furthermore, Patent Document 2 describes a fuel hose in which a THV resin is used in a layer that requires low fuel permeability. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Patent Publication No. 2013-71382 [Patent Document 2] Patent Publication No. 2016-11715 Summary of the Invention [Problem to be solved by the invention]
[0006] However, when THV resin is melt-molded, it decomposes under high temperature conditions, which may easily generate acidic gases, leading to concerns that the components used in the molding equipment may deteriorate or rust. In other words, it is desirable to take special measures against the generation of acidic gases, but it is not desirable to melt-molde THV resin in general-purpose molding equipment that molds general thermoplastic resins without such measures. In addition, as a countermeasure against the above, there are molding equipment with enhanced corrosion resistance, but considering the cost, these measures are not necessarily easy to introduce.
[0007] On the other hand, to suppress the decomposition of the resin during melt processing, heat stabilizers made of organic substances such as antioxidants are sometimes added. However, since the melt processing temperature of THV resin is high, the heat stabilizer may evaporate, or the poor compatibility between THV resin and the heat stabilizer may cause the molded product to become cloudy, damaging the appearance of the molded product. Since THV resin has excellent chemical resistance and contamination resistance, it is expected to be used in applications that require good appearance, such as protective films for products and building materials. For this reason, it is undesirable for the appearance of the molded product to deteriorate due to the effects of additives.
[0008] As described above, there is a demand for the development of a THV resin composition that can be processed using general-purpose molding equipment and that does not impair the appearance of the molded article.
[0009] In order to solve the above-mentioned problems, the present invention aims to provide a resin composition that can be melt-molded using general-purpose molding equipment without impairing the appearance of the molded article, and a molded article using the composition. [Means for solving the problem]
[0010] The present inventors have discovered that, when dispersed in a THV resin, an inorganic acid acceptor can suppress clouding or yellowing when the resin composition is molded, maintaining the transparency of the molded article, and can also capture acidic gases produced by thermal decomposition of the THV resin, preventing the diffusion of the acidic gases, thereby arriving at the present invention. <1> A resin composition comprising a tetrafluoroethylene-hexafluoropropylene-vinylidene fluoride copolymer (A) and an inorganic acid acceptor (B), wherein the content of the inorganic acid acceptor (B) in the resin composition is 0.01 to 0.1 parts by mass per 100 parts by mass of the tetrafluoroethylene-hexafluoropropylene-vinylidene fluoride copolymer (A). <2> The inorganic acid acceptor (B) is at least one selected from the group consisting of metal oxides, metal hydroxides, solid solutions containing a plurality of metal oxides, metal stearates, hydrotalcite-based compounds represented by the following formula (I), and hydrotalcite-like layered compounds exhibiting anion exchange activity. <1> The resin composition according to claim 1. Formula (I):M 2+ 1-x M 3+ x (OH)2A n- x / n mH2O(I) [However, M 2+ , M 3+ represent divalent and trivalent metal ions, respectively, and A n- represents an anion with n valence, 0 <x≦0.33であり、m≧0である。〕 <3> The above <1> or <2> A molded article obtained by molding the resin composition according to claim 1. <4> The above-mentioned which is in a sheet or film form <3> The molded article according to claim 1. Effect of the Invention
[0011] According to the present invention, it is possible to provide a resin composition that can be melt-molded in general-purpose molding equipment without impairing the appearance of the molded article, and a molded article using the composition. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] Hereinafter, the present invention will be described in detail using embodiments, but the present invention is not limited to the embodiments shown below.
[0013] 《THV resin composition》 The resin composition of this embodiment (hereinafter sometimes referred to as "THV resin composition") is a resin composition containing a tetrafluoroethylene-hexafluoropropylene-vinylidene fluoride copolymer (A) (hereinafter sometimes referred to as "THV resin (A)") and an inorganic acid acceptor (B), and the content of the inorganic acid acceptor (B) in the resin composition is 0.01 to 0.1 parts by mass per 100 parts by mass of the tetrafluoroethylene-hexafluoropropylene-vinylidene fluoride copolymer (A).
[0014] The resin composition of this embodiment uses a specific amount of inorganic acid acceptor (B) relative to THV resin (A), thereby capturing acidic gases generated by decomposition of THV resin (A) during melt molding and preventing their diffusion. In addition, unlike organic antioxidants, inorganic acid acceptors are less likely to volatilize even at the processing temperature of THV resin (about 280°C or higher). Therefore, little acidic gas is generated during melt molding, and even when using general-purpose molding equipment for molding general thermoplastic resins, there is little effect on the members in the equipment. In addition, organic antioxidants are poorly compatible with THV resin when mixed with it, and may cause clouding. On the other hand, inorganic acid acceptors are easily dispersed in THV resin, and have a refractive index relatively close to that of resins such as THV. This makes it possible to suppress clouding and yellowing when the resin composition is molded, and when the THV resin is molded into a molded product, the transparency of the THV resin molded product can be maintained without impairing its appearance.
[0015] <Tetrafluoroethylene-hexafluoropropylene-vinylidene fluoride copolymer (A)> The tetrafluoroethylene-hexafluoropropylene-vinylidene fluoride copolymer (A) (THV resin (A)) in this embodiment is a copolymer of tetrafluoroethylene (also known as "tetrafluoroethylene", hereinafter sometimes referred to as "TFE"), hexafluoropropylene (also known as "hexafluoropropylene", hereinafter sometimes referred to as "HFP"), and vinylidene fluoride (hereinafter sometimes referred to as "VDF"). The THV resin (A) is not limited to a copolymer consisting of three monomers, namely, TFE monomer, HFP monomer, and VDF monomer. That is, the THV resin (A) may contain other monomers in addition to the TFE monomer, HFP monomer, and VDF monomer. Examples of the other monomers include (perfluorohexyl)ethylene, (perfluorobutyl)ethylene, (perfluorooctyl)ethylene, and [4-(heptafluoroisopropyl)perfluorobutyl]ethylene, and the THV resin (A) also includes copolymers using these other monomers as the fourth monomer.
[0016] The monomer ratio (molar ratio of the constituent units derived from each monomer) in the copolymerization of TFE monomer, HFP monomer and VDF monomer in the THV resin (A) is not particularly limited, but is preferably within the range of 90 or less for the TFE monomer, 1 or more for the HFP monomer, and 9 or more for the VDF when the ratio of all monomers is taken as 100; more preferably, the ratio of TFE is 60 to 90, the ratio of HFP is 1 to 10, and the ratio of VDF is 9 to 30. When the ratio of TFE monomer is 90 or less, the ratios of HFP monomer and VDF monomer increase relatively, so that the resin becomes more likely to soften, and the melt moldability is improved. When the ratio of TFE monomer is 30 or more, a polytetrafluoroethylene-like structure is formed in a part of the molecular chain, and the chemical resistance, weather resistance, antifouling properties, etc., characteristic of fluororesins are further improved.
[0017] The melting point of the THV resin (A) is not particularly limited, but is preferably from 100°C to 250°C, more preferably from 150°C to 250°C, from the viewpoint of heat resistance. The glass transition temperature of the THV resin (A) is preferably from -10°C to 30°C, more preferably from 0°C to 20°C, from the viewpoint of flexibility when molded into a film or sheet.
[0018] The THV resin (A) may be a THV resin having any TFE / HFP / VDF ratio used alone, or may be a mixture of two or more THV resins having different TFE / HFP / VDF ratios. Furthermore, resins other than the THV resin (A) may be added as necessary within a range that does not impair the transparency of the THV resin composition. Also, a THV resin (A) that is a copolymer of three types of monomers such as TFE / HFP / VDF may be used in combination with a THV resin (A) that is a copolymer of TFE / HFP / VDF / a fourth monomer. Examples of resins other than the THV resin (A) include polychlorotrifluoroethylene (PCTFE), ethylene-tetrafluoroethylene copolymer (ETFE), polyvinyl fluoride (PVF), polyvinylidene fluoride (PVDF), vinylidene fluoride-hexafluoropropylene copolymer, polytetrafluoroethylene (PTFE), polyhexafluoropropylene (PHFP), polyperfluoroalkylvinyl ether (PFA), and ethylene-chlorotrifluoroethylene copolymer (ECTFE). When the other resin is used, the content of the other resin in the THV resin composition is preferably 0.2 parts by mass or less, and more preferably 0.1 parts by mass or less, per 100 parts by mass of the THV resin (A).
[0019] <Inorganic acid acceptor (B)> The THV resin composition of the present embodiment contains a specific amount of an inorganic acid acceptor relative to the THV resin (A). Here, the term "inorganic acid acceptor" refers to an acid acceptor containing an inorganic compound. In other words, the inorganic acid acceptor (B) is a general term for inorganic compounds that can capture acids such as acidic gases by taking in the acids or neutralizing the acids.
[0020] The inorganic acid acceptor (B) is not particularly limited, and can be appropriately selected from known inorganic compounds having an acid receiving function (acid capturing ability). However, the mechanism of acid capture in the inorganic acid acceptor (B) is not particularly limited. Among these inorganic acid acceptors, metal oxides, metal hydroxides, solid solutions containing multiple types of metal oxides, metal stearates, hydrotalcite-type compounds represented by the formula (I) described below, and hydrotalcite-like layered compounds exhibiting anion exchange function are preferred, and metal oxides, solid solutions containing multiple types of metal oxides, hydrotalcite-type compounds represented by the formula (I) described below, and hydrotalcite-like layered compounds exhibiting anion exchange function are particularly preferred.
[0021] In the resin composition of the present embodiment, by adding a specific amount of the inorganic acid acceptor (B) to the THV resin, it is possible to suppress corrosion and deterioration of the molding equipment caused by acid gas generated by decomposition of the THV resin during melt molding, while maintaining the appearance of the molded product. The inorganic acid acceptor (B) may be used alone or in combination of two or more kinds.
[0022] Examples of the inorganic acid acceptor (B) are not particularly limited, and include the inorganic compounds exemplified below. The inorganic acid acceptor (B) may contain the following inorganic compound as a main component and may also contain impurities. Examples of metal oxides include magnesium oxide and zinc oxide. Examples of metal hydroxides include magnesium hydroxide and barium hydroxide. Examples of the metal stearates include calcium stearate and zinc stearate. An example of a solid solution made of a plurality of metal oxides is a magnesium oxide-aluminum oxide solid solution.
[0023] In the hydrotalcite compound represented by the following formula (I), the divalent metal ion is magnesium ion (Mg 2+ ), zinc ion (Zn 2+) and the trivalent metal ion is aluminum ion (Al 3+ ), iron ion (Fe 3+ ) as an n-valent anion. Examples of n-valent anions include monovalent and divalent anions, and specifically, carbonate ion (CO3 2- ), nitrate ion (NO3 - As such hydrotalcite compounds, a combination of magnesium ions, aluminum ions and carbonate ions is preferred, and examples thereof include hydrotalcites containing magnesium oxide-aluminum oxide as the main components.
[0024] Formula (I):M 2+ 1-x M 3+ x (OH)2A n- x / n mH2O [However, M 2+ , M 3+ represent divalent and trivalent metal ions, respectively, and A n- represents an anion with n valence, 0 <x≦0.33であり、m≧0である。〕
[0025] An example of the hydrotalcite-like layered compound that exhibits an anion exchange function is a layered compound obtained by firing the above-mentioned hydrotalcite containing magnesium oxide-aluminum oxide as the main components.
[0026] The refractive index of the inorganic acid acceptor (B) is preferably 1.9 or less, more preferably 1.6 or less. When the refractive index is 1.6 or less, the difference in refractive index with the THV resin is not large, and clouding of the molded product can be effectively prevented.
[0027] The particle size of the inorganic acid acceptor (B) is not particularly limited, but from the viewpoints of maintaining the transparency of the THV resin molded body, dispersibility of the acid acceptor, and acid scavenging performance, the 50% average particle size is preferably 0.1 μm to 1 μm, and more preferably 0.3 μm to 0.6 μm.
[0028] The method of adding the inorganic acid acceptor (B) to the THV resin composition is not particularly limited, and the inorganic acid acceptor (B) may be added in advance in the granulation process of the THV resin raw material, or the inorganic acid acceptor (B) may be added while melt-mixing the unadded THV resin raw material and the inorganic acid acceptor (B) in the process of producing a sheet (molded product) of the THV resin composition.
[0029] The content of the inorganic acid acceptor (B) in the THV resin composition is 0.01 to 0.1 parts by mass per 100 parts by mass of the THV resin (A). When the content of the inorganic acid acceptor (B) is 0.1 parts by mass or less, the THV resin composition can be prevented from becoming cloudy due to the acid acceptor and from becoming discolored due to thermal deterioration of the acid acceptor. When the content of the inorganic acid acceptor (B) is 0.01% by mass or more, a sufficient acid gas capture effect can be obtained.
[0030] (others) The THV resin composition of the present embodiment may contain a plasticizer, a lubricant, an antistatic agent, an antifogging agent, a dripping agent, a hydrophilic agent, a liquid repellent agent, etc., within a range that does not impair the transparency, color tone, glossiness, heat resistance, weather resistance, etc., or the effects of the present invention in practical terms. Furthermore, these additives may be added when the THV resin composition is kneaded, or may be applied to the surface of a film or sheet (molded product) produced by molding the THV resin composition. Furthermore, a pigment can be added to the THV resin composition of the present embodiment as necessary within a range that does not impair the heat resistance, weather resistance, etc., or the effects of the present invention in practical use.
[0031] <Method of manufacturing molded body> The THV resin composition of the present embodiment can be molded into various shapes, for example, into a film or sheet. Here, a method for producing a film using the THV resin composition of the present embodiment will be described.
[0032] As a method for producing a film, a known method can be used, for example, a method of molding a resin composition by melt extrusion using an extruder and various T-dies such as a feed block die or a multi-manifold die. As an extruder, a single screw type, a twin screw type, a tandem type, etc. can be generally used, but a single screw type extruder is preferred in terms of preventing the resin from stagnation in the extruder system.
[0033] The screw shape used in the single screw extruder is not particularly limited as long as it is configured not to generate excessive shear heat, but a full-flight screw is more preferable for melt extrusion without applying excessive shear.
[0034] The compression ratio of the screw is preferably in the range of 1.8 to 3.0, more preferably 2.1 to 2.7. If the compression ratio is 1.8 or more, the THV resin is not sufficiently plasticized, and a part of the resin is captured by the screen mesh as unmelted matter, which can prevent the resin pressure from increasing due to clogging, and can also prevent the unmelted matter from being mixed into the sheet as a defect. Furthermore, if the compression ratio is 3.0 or less, it can also prevent the amount of acid gas generated from becoming too large due to excessive shear heat generation.
[0035] The ratio (L / D) of the screw length (L) to the screw (barrel) diameter (D) of the extruder is not particularly limited as long as the extruder has an L / D necessary and sufficient for plasticizing the THV resin, but is preferably 20 to 40, more preferably 25 to 35. When the L / D is 20 or more, the resin can be sufficiently plasticized in the screw region, and it is possible to suppress the generation of unmelted material, which is a defect and is mixed into the sheet. In addition, when the L / D is 40 or less, excessive shear is unlikely to be applied, and an increase in the amount of acid gas generated can be suppressed.
[0036] A breaker plate may be provided between the tip of the screw of the extruder and the T-die. The aperture ratio of the breaker plate is preferably 40 to 60%, more preferably 42 to 58%. By setting the aperture ratio of the breaker plate to 40% or more, it is possible to suppress back pressure on the resin and to suppress retention of the resin in the extruder. In addition, by setting the aperture ratio to 60% or less, it is possible to stably maintain the number of defects in the film low for a long period of time. The opening ratio is based on the portion exposed to the resin flow section of the extruder and means the area of the portion where the resin through holes are formed relative to the total area including the resin through holes.
[0037] The resin penetration diameter of the breaker plate is preferably 3.7 to 7.0 mm. By making the resin penetration diameter 3.7 mm or more, it is possible to suppress back pressure on the resin and suppress retention of the resin in the extruder. Also, by making it 7.0 mm or less, it is possible to stably keep the number of defects in the sheet low for a long period of time.
[0038] The screen mesh arranged on the breaker plate is preferably a combination of two or more screen meshes with different mesh openings. The screen meshes may be used in combination with screen meshes with the same mesh openings. In general, it is preferable to arrange the screen meshes with larger mesh openings and the screen meshes with smaller mesh openings in this order from the upstream side (near the screw) of the resin flow section to the downstream side (opening side of the breaker plate). Furthermore, it is preferable to arrange a mesh with a coarser mesh than the mesh with the smallest mesh opening downstream of the mesh with the smallest mesh opening in order to prevent the mesh from breaking due to resin pressure. Specifically, a coarser screen mesh with a larger mesh opening than the mesh with the smallest mesh opening can be introduced downstream of the screen mesh with the smallest mesh opening. The screen mesh is preferably arranged 10 to 100 mm downstream from the tip of the screw. In the sheet production of the THV resin composition of this embodiment, the minimum mesh opening of the screen mesh is preferably 0.03 to 0.2 mm, more preferably 0.03 to 0.15 mm. By making the minimum mesh opening of the screen mesh 0.03 mm or more, deterioration due to shear heat generation of the resin can be suppressed. In addition, by setting the minimum mesh size of the screen mesh to 0.2 mm or less, it is possible to reduce contamination of the resin and deteriorated raw materials. The screen mesh with large openings serves to remove coarse defects, and the openings are preferably 0.15 to 0.6 mm.
[0039] The flow path of the T-die used in film production is not particularly limited in shape as long as the resin does not easily accumulate, but a coat hanger die is an example that can be used suitably. The main types of resin discharge direction are a horizontal direction to the side and a downward direction perpendicular to the horizontal direction, but either type can be used suitably.
[0040] The temperature setting of the extruder for film production varies depending on the type and fluidity of the THV resin, but is preferably 200 to 300° C., more preferably 260 to 290° C., downstream of the extruder. If the temperature is 200° C. or higher, the resin can be sufficiently plasticized, and if the temperature is 300° C. or lower, excessive generation of acid gases due to excessive heating can be suppressed.
[0041] The film extruded from the T-die in this way immediately comes into contact with a cooling roll close to the die and is taken up while being cooled. Since the THV resin partially crystallizes when cooled, when transparency is required, it is preferable to rapidly cool the THV resin from the molten state with a cooling roll before the crystallization proceeds. The shortest distance between the outlet of the T-die and the point where the film contacts the cooling roll is preferably 200 mm or less, more preferably 150 mm or less, and particularly preferably 100 mm or less. If the distance is 200 mm or less, the crystallization of the THV resin proceeds more than necessary, and the transparency of the sheet can be suppressed from decreasing. On the other hand, when design or the like is required, a roll engraved with a design, a geometric pattern, or an embossed roll can be used.
[0042] As a cooling method using a cooling roll, either of the following methods can be used: two rolls with hard surfaces such as hard chrome plating or diamond-like carbon are placed with a gap suitable for obtaining the desired film thickness, and the film-like molten resin is brought into contact with the gap between them while being drawn up for cooling; or the hard-surfaced roll is pressed against a rubber roll such as silicone roll, and the film-like molten resin is brought into contact with the gap between them while being drawn up for cooling.
[0043] The film taken up as described above is passed through appropriate guide rolls without damaging the film surface, slit to a desired width, and then wound up in a sufficiently cooled state onto a paper tube, etc. During the process from being extruded from the die to being wound up onto a paper tube, etc., the film surface may be subjected to a corona treatment, a plasma treatment, or a surface chemical treatment using a chemical agent such as a silane coupling agent, or the like, or the above surface treatment may be performed in a separate process.
[0044] In this specification, a sheet refers to something thicker and a film refers to something thinner, and there is no clear distinction between a "sheet" and a "film."
[0045] 《THV resin molded body》 The THV resin molded article can be suitably used in applications requiring excellent chemical resistance, weather resistance, and design. The THV resin molded article can be used as a film or sheet alone, or as a laminate with other substrates.
[0046] In this specification, the state where the appearance is impaired refers to poor dispersion and cloudiness due to the addition of an excessive amount of the acid acceptor, and brownish coloration due to thermal degradation of the acid acceptor. The above-mentioned cloudiness increases the haze value of the film measured in accordance with JIS K7105, but this value can be adjusted depending on the application by the production method, for example, by providing unevenness to the film surface with an embossed roll. In addition, if the haze value is intentionally adjusted, it is not treated as a defective appearance.
[0047] Furthermore, in applications requiring transparency and design, such as signboard protection films and decorative films, the haze value of the film measured with a haze meter in accordance with JIS K7105 is preferably 5% or less, more preferably 3% or less. When the haze value is 5% or less, sufficient visibility of patterns, designs, etc. arranged under the THV resin composition film can be obtained.
[0048] In addition, in applications where transparency and design are required, the THV resin composition film has a L * a * b * b in color space * is preferably 2.0 or less, and more preferably 1.0 or less. * If the color exceeds 2.0, the film itself may be macroscopically perceived as yellow.
[0049] For example, the effect of reducing the generation of acidic gases when a sheet-shaped THV resin molded body is produced under high temperatures such as extrusion molding can be confirmed using an apparatus for measuring the concentration of acidic gases at any location. The measuring apparatus is not particularly limited as long as it has sufficient quantitative accuracy. One example of a measuring apparatus that can be used is an acidic gas concentration detector in which an acidic gas absorbent is filled in a glass tube, and a quantitative recovery of gas and its gas concentration can be obtained. In the case of fluororesin, it is preferable to use a gas detector tube for hydrogen fluoride gas.
[0050] <Application> The molded article (for example, a film or sheet) obtained by molding the THV resin composition of the present embodiment can be used, for example, in the following applications. - Wall materials, roof materials, tent materials, membrane materials for buildings - Protective film for signs, road signs, and soundproof barriers - Decorative films, water-repellent films, oil-repellent films, snow-proof films, and ice-proof films used in the interior and exterior parts of automobiles, railway vehicles, aircraft, and ships EXAMPLES
[0051] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples in any way.
[0052] <Raw materials> The raw materials used in the present examples and comparative examples are shown below. (THV resin) 3M "Dyneon THV Resin 815GZ" (melting point 225℃)
[0053] (Inorganic acid acceptor) Magnesium oxide: Kyowa Chemical Industry Co., Ltd. "Kyowamag MF150" Magnesium oxide-aluminum oxide-based solid solution: Kyowa Chemical Industry Co., Ltd. "KW-2200" Hydrotalcite compounds: ADEKA "ADEKA STAB AP-582" Hydrotalcite-type compound: Kyowa Chemical Industry Co., Ltd.'s "DHT-4C" (corresponding to a hydrotalcite-like layered compound that exhibits anion exchange properties)
[0054] (Antioxidants) Phenolic antioxidant: BASF "Irganox1010" Phenolic antioxidant: BASF "Irganox1076" Phenolic antioxidant: Sumitomo Chemical's "Sumilizer GA-80"
[0055] <Example 1> 100 parts by mass of THV resin raw material ("Dyneon THV Resin 815GZ") was premixed with 0.01 parts by mass of magnesium oxide ("Kyowamag MF150"), then the mixture was melt mixed at 280°C using a Toyo Seiki Seisakusho "Labo Plastomill Micro" and pulled up onto a metal cast roll to obtain a glossy film with a thickness of 0.05 mm. The amount of acid gas generated during film preparation and the optical properties of the obtained film were measured and evaluated according to the standards described below. The results are shown in the table below.
[0056] <Examples 2 to 20 and Comparative Examples 1 to 16> Sheets were produced in the same manner as in Example 1, except that the raw materials and the amounts added were changed as shown in Tables 2 to 6. The amount of acid gas generated during film production and the optical properties of the obtained films are also shown in Tables 2 to 6. In Tables 2 to 6, the amount of acid acceptor or antioxidant added indicates the amount of acid acceptor or antioxidant added relative to 100 parts by mass of the THV resin raw material.
[0057] <Film Evaluation> (Measurement of acid gas generation amount) Using a gas sampler (Kitagawa gas sampler AP-20; manufactured by Komyo Rikagaku Kogyo Co., Ltd.) and a hydrogen fluoride gas detector (Kitagawa gas detector No. 156S hydrogen fluoride; manufactured by Komyo Rikagaku Kogyo Co., Ltd.), the amount of acid gas generated was measured i) at a position 10 mm directly above the vent port (degassing hole) provided in the above-mentioned "Labo Plastomill Micro" ("immediately adjacent to the vent port" in the table below), and ii) at a position 1 m away from the lip of the T-die of the same device ("work environment" in the table below).
[0058] (Hayes) The transparency of the resin sheet was judged based on the haze value measured in accordance with JIS K7105 using a haze meter "NDH7000" manufactured by Nippon Denshoku Industries Co., Ltd., and in accordance with the criteria listed in Table 1 below. For the measurement, samples cut out from any five points on the resin sheet were used, and the arithmetic average value was adopted.
[0059] (Color tone: b * ) Using Nippon Denshoku Kogyo Co., Ltd.'s ZE6000, * a * b * b in color space * was measured by the transmission method. * Regarding the color tone of the resin sheet, the performance was evaluated according to the criteria shown in Table 1 below.
[0060] [Table 1]
[0061] [Table 2]
[0062] [Table 3]
[0063] [Table 4]
[0064] [Table 5]
[0065] [Table 6]
[0066] From the results of Examples 1 to 20, it was found that adding the inorganic acid acceptor in the amount shown in the table to the THV resin provided excellent ability to suppress the amount of acid gas generation and did not impair the appearance.
[0067] From the results of Comparative Examples 1, 5, 8 and 11, it was found that when the amount of inorganic acid acceptor added was small, the film appearance was not impaired, but the amount of acid gas generation was insufficient. In addition, it was found that the appearance of the film was impaired when the amount of inorganic acid acceptor added was excessive in Comparative Examples 2 to 3, 6 to 7, 9 to 10, and 12 to 13. Furthermore, it was found that when an antioxidant containing an organic compound was added, the amount added was insufficient to suppress the generation of acidic gas, and the film became cloudy and the optical properties were impaired.
[0068] As described above, the THV resin composition of the present invention can suppress the generation of acid gas during melt molding of the THV resin without impairing the appearance by adding an inorganic acid acceptor. In other words, the THV resin can be melt molded using general-purpose molding equipment, not corrosion-resistant equipment.
[0069] The disclosure of Japanese Patent Application No. 2019-224043, filed on December 11, 2019, is incorporated herein by reference in its entirety. In addition, all publications, patent applications, and technical standards mentioned in the specification are herein incorporated by reference to the same extent as if each individual publication, patent application, and technical standard was specifically and individually indicated to be incorporated by reference.
Claims
1. A resin composition comprising a tetrafluoroethylene-hexafluoropropylene-vinylidene fluoride copolymer (A) and an inorganic acid acceptor (B), wherein the content of the inorganic acid acceptor (B) in the resin composition is 0.01 to 0.075 parts by mass per 100 parts by mass of the tetrafluoroethylene-hexafluoropropylene-vinylidene fluoride copolymer (A).
2. 2. The resin composition according to claim 1, wherein the inorganic acid acceptor (B) is at least one selected from the group consisting of metal oxides, metal hydroxides, solid solutions containing a plurality of metal oxides, metal stearates, hydrotalcite-type compounds represented by the following formula (I), and hydrotalcite-like layered compounds exhibiting anion exchange activity. Formula (I): M 2+ 1-x M 3+ x (OH) 2 A n- x / n ・mH 2 O(I) [However, M 2+ , M. 3+ represent divalent and trivalent metal ions, respectively, A n- represents an anion having a valence of n, 0<x≦0.33, and m≧0.
3. A molded article obtained by molding the resin composition according to claim 1 or 2.
4. The molded article according to claim 3, which is in the form of a sheet or a film.
Citation Information
Patent Citations
Silica-based filler and transparent resin composition containing the same
JP2007084606A
Mold release film
JP2013071382A
Combustion hose
JP2016011715A
Transparent sheet for solar cell, transparent back sheet for solar cell, and solar cell module
JP2016195165A
Fluorine resin composition for wire coating material and wire
JP2017045638A