Bridging frustrated Lewis pairs as a thermal trigger for the reaction of Si-H with epoxides

Bridged frustrated Lewis pairs act as thermal triggers for silyl hydride and epoxide reactions, addressing the limitations of transition metal catalysts and UV-induced systems by providing a stable, one-component system with controlled reaction initiation.

JP7560490B2Active Publication Date: 2024-10-02DOW SILICONES CORP
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2021571830
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-06-04
Filing Date
2020-06-02
Publication Date
2024-10-02
Estimated Expiration
2040-06-02

AI Technical Summary

Technical Problem

Existing chemical reactions between silyl hydrides and epoxides typically require transition metal catalysts and result in rapid reaction rates, limiting their use to two-component systems and necessitating storage in the dark for UV-induced reactions, which are not practical for one-component systems.

Method used

The use of bridged frustrated Lewis pairs (B-FLP) as a thermal trigger, allowing the Lewis acid to be stored stably and released upon heating, catalyzing the reaction between silyl hydrides and epoxides without the need for transition metal catalysts, enabling a one-component system with controlled reaction initiation.

Benefits of technology

B-FLP provides a storage-stable, one-component system that undergoes rapid reaction upon heating, avoiding the need for UV induction and allowing for controlled reaction initiation, enhancing handling and storage stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007560490000001
    Figure 0007560490000001
  • Figure 0007560490000002
    Figure 0007560490000002
  • Figure 0007560490000003
    Figure 0007560490000003
Patent Text Reader

Abstract

The composition contains a mixture of silyl hydrides, epoxides, and bridged frustrated Lewis pairs.
Need to check novelty before this filing date? Find Prior Art

Description

[Background technology]

[0001] FIELD OF THEINVENTION The present invention relates to the use of a bridged frustrated Lewis pair as a thermal trigger for the chemical reaction of silyl hydrides with epoxides. The bridged frustrated Lewis pair dissociates upon heating to release a Lewis acid. The Lewis acid acts as a catalyst for the chemical reaction of silyl hydrides with epoxides.

[0002] Introduction Frustrated Lewis pairs ("FLPs") are a term used to refer to pairs of Lewis acids and Lewis bases where the Lewis acid and Lewis base cannot complex and neutralize each other due to steric congestion. When the Lewis acid and Lewis base of an FLP are mixed, they remain independent of each other rather than mixing and neutralizing each other. In addition, FLPs have been found to indirectly bind to each other in the form of bridged frustrated Lewis pairs ("B-FLPs"), where a bridge molecule binds to both the acid and base of the FLP to form a complex with the bridge molecule between the Lewis acid and the Lewis base. In some cases, the bridge molecule can be cleaved to generate a blocked Lewis acid and a blocked Lewis base, with a portion of the bridge molecule complexed with each of the Lewis acid and Lewis base, blocking further complexation or reaction. Hydrogen (H2) is an example of a bridge molecule that cleaves in this manner upon forming a B-FLP.

[0003] B-FLP has been used to activate bridge molecules for use in chemical reactions. For example, hydrogen (H2) has been used as a bridge molecule in B-FLP to activate hydrogen for use in hydrogenation reactions (see, for example, JACS 2015, 137, 10018-10032), and carbon dioxide has been used as a bridge molecule in B-FLP to activate carbon dioxide for deoxygenation hydrosilylation (see, for example, JACS 2010, 132, 10660-10661). Other molecules used as bridge molecules in B-FLP for use in activation for chemical reactions include nitrous oxide (N2O), sulfur dioxide (SO2), alkenes, and alkynes. See, for example, Angew. Chem. Int. Ed. 2009, 48, 6643-6646; Angew. Chem. Int. Ed. 2015, 54, 6400-6441 and JACS 2015, 137, 10018-10032. Summary of the Invention [Problem to be solved by the invention]

[0004] It would be surprising and useful to discover additional uses for B-FLP, especially if such uses allow for the control of chemical reactions other than those involving cross-linking molecules.

[0005] The present invention provides a surprising and unexpected use of B-FLP as a thermal trigger for the addition reaction of silyl hydrides (Si-H) with epoxide functional groups.

[0006] Addition reactions such as hydrosilylation reactions typically require the presence of a transition metal catalyst. However, it has been discovered that silyl hydride and epoxide functional groups undergo addition reactions in the presence of a Lewis acid catalyst without the need for a transition metal catalyst. Lewis acids are known to catalyze the reaction of silyl hydrides with silyl ethers, known as the Piers-Rubinsztajn ("PR") reaction. However, unlike the PR reaction, the present reaction of silyl hydrides with epoxies does not require a silyl ether, and the present reaction does not produce gaseous by-products as does the PR reaction. The present invention also offers advantages over typical addition reactions because it does not require a transition metal catalyst.

[0007] Similar to the PR reaction, Lewis acid catalyzed addition reactions of silyl hydrides with epoxides may be desirable for curing siloxanes in coatings, adhesives, elastomers, and foaming applications. However, because epoxide / silyl hydride reactions tend to be rapid, their use requires that the reaction system be supplied and stored as a two-part system in which the Lewis acid catalyst keeps the reaction system separate from the Si-H and / or epoxide until reaction is desired. One-component systems are easier to handle and more desirable than two-part systems, so the reaction components can be combined together in a one-part system, but it is desirable that the system does not immediately cure to a gel unless heated to an inducing temperature. Ideally, the one-part system is shelf stable for storage or experiences delayed cure at least at 23° C. for extended handling time, but includes a means to induce the addition reaction on demand to rapidly cure the system.

[0008] Systems of PR reactive materials exist in which a Lewis acid catalyst is complexed with an ultraviolet (UV) light-sensitive blocking agent that prevents the catalyst from undergoing a PR reaction until irradiated with UV light. However, such systems must be stored in the dark for storage stability and exposed to UV light to initiate curing. It may be desirable to avoid the need for storage in the dark and expose to light to induce a reaction in the system.

[0009] The present invention is a result of the discovery that B-FLP can be used in a silyl hydride / epoxide reaction system as a latent Lewis acid catalyst that is thermally released when heated to an inducing temperature. That is, B-FLP can be combined with a silyl hydride and an epoxide to form a stable one-part reaction system that is storage stable or at least has a delayed reactivity at 23° C., but reacts rapidly upon heating to release the Lewis acid from B-FLP. Upon heating, the Lewis acid dissociates from B-FLP, allowing the Lewis acid to act as a reaction catalyst to initiate the addition reaction of the silyl hydride with the epoxide. Desirably, the compositions of the present invention may be exposed to UV light without inducing the reaction by unblocking the Lewis acid.

[0010] B-FLP was found to be a particularly efficient triggering agent because it is difficult to remix once destroyed. This means that once the Lewis acid is liberated, it continues to catalyze the reaction without being inhibited by the reformation of B-FLP. This is an advantage over Lewis acids directly inhibited with a Lewis base, since the Lewis base remains in solution and can remix with the free Lewis acid to neutralize it. B-FLP requires the reformation of a bridging complex between the Lewis acid and the base, and this reformation is much less likely to occur randomly. This is especially true for labile bridging molecules, such as those that are gaseous and will retreat from the reaction system once B-FLP is destroyed. As a result, the use of B-FLP offers unprecedented control over irreversibly triggering the reaction without forming catalytic inhibitors, since upon sufficient heating to dissociate B-FLP, the acid catalyst is essentially irreversibly released and is expected to catalyze a rapid reaction.

[0011] In a first aspect, the invention is a composition comprising a mixture of a silyl hydride, an epoxide, and a bridged frustrated Lewis pair.

[0012] In a second aspect, the invention is a chemical reaction process comprising the steps of: (a) providing a composition of the first aspect; and (b) heating the composition to a temperature sufficient to dissociate a Lewis acid from a bridged frustrated Lewis pair.

[0013] The present invention is useful for preparing coatings, adhesives, and elastomers. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014] Test methods refer to the most recent test method as of the priority date of this document unless a date is given with the test method number. Reference to a test method includes both a reference to the testing society and the test method number. The following test method abbreviations and identifiers apply herein: ASTM refers to ASTM International, EN refers to European Norm, DIN refers to Deutsches Institut fuer Normung, and ISO refers to the International Organization for Standardization.

[0015] Products identified by trade names refer to compositions available under those trade names from suppliers as of the priority date of this application.

[0016] "Plurality" means two or more. "And / or" means "and, or alternatively." All ranges are inclusive of endpoints unless otherwise indicated. Products identified by trade names refer to compositions available from suppliers under those trade names as of the priority date of this document, unless otherwise indicated herein.

[0017] The compositions of the present invention comprise a mixture of silyl hydrides, epoxides, and crosslinked frustrated Lewis pairs. The compositions are storage stable or at least undergo delayed gelation at 23° C., but are useful as one-part reactive systems when the gel is heated in 2 minutes or less, preferably 1 minute or less, and even more preferably 30 seconds or less. "Delayed gelation" means that gelation takes 3 minutes or more at 23° C. "Storage stable" means that the composition does not gel in 5 hours or less, preferably 10 hours or less, more preferably 15 hours or less, even more preferably 24 hours or less, and even more preferably 1 week or less at 23° C.

[0018] A "silyl hydride" is a molecule that contains a silicon-hydrogen (Si-H) bond and can contain multiple Si-H bonds.

[0019] An "alkyl" is a hydrocarbon group derived from an alkane by removing a hydrogen atom. A "substituted alkyl" is an alkyl having an atom or chemical moiety other than carbon and hydrogen in place of at least one carbon or hydrogen.

[0020] An "aryl" is a group derived from an aromatic hydrocarbon by removing a hydrogen atom. A "substituted aryl" is an aryl that has an atom or chemical moiety other than carbon and hydrogen in place of at least one carbon or hydrogen.

[0021] An "epoxide" contains at least one, and may contain more than one, epoxide functional group, where the "epoxide functionality" (or "epoxide functional group") is a three-membered ring containing two carbon atoms and one oxygen atom.

[0022] A "frustrated Lewis pair," or "FLP," is a system of Lewis acids and Lewis bases in which the Lewis acid and Lewis base are unable to complex and completely neutralize ("block") each other due to steric congestion. FLPs are known in the art and have been characterized in papers such as JACS 2015, 137, 10018-10032 and papers identified therein. Desirably, an FLP is a system of Lewis acids and Lewis bases in which congestion makes complexation and neutralization impossible at 20 degrees Celsius (°C). Although FLPs are known in the art, it can be determined whether any Lewis pair is an FLP by combining equimolar amounts of a Lewis acid and a Lewis base at 20°C in a solvent that dissolves both. If more than 10 mole percent of the Lewis acid and Lewis base remain dissociated, then the Lewis acid and Lewis base can be considered an FLP. The extent of dissociation is determined by any reasonable means, such as nuclear magnetic resonance spectroscopy or, preferably, ion chromatography using a conductivity or photometric detector.

[0023] Upon heating the compositions of the present invention, B-FLP releases a Lewis acid that catalyzes the reaction of epoxides with silyl hydrides to form new siloxy (Si-O) bonds. The composition is heated to a temperature of 80° C. or more, 90° C. or more, 100° C. or more, 110° C. or more, 120° C. or more, 130° C. or more, 140° C. or more, 150° C. or more, 160° C. or more, 170° C. or more, 180° C. or more, 190° C. or more, 200° C. or more, 210° C. or more, while reacting and curing the components in the composition, generally at 300° C. or less, 250° C. or less, 240° C. or less, 230° C. or less, 220° C. or less, 210° C. or less, 200° C. or less, 175° C. or less, 150° C. or less, 140° C. or less, 130° C. or less, 120° C. or less, 110° C. or less, or even 100° C. or less, for 2 minutes or less, preferably 1 minute or less, and even more preferably 30 seconds or less.

[0024] The reaction of an epoxide with a silyl hydride is an addition reaction between epoxide functional groups that is generally represented by the following reaction: [ka]

[0025] The compositions of the present invention provide delayed gelation and are desirably storage stable.

[0026] Epoxides An epoxide may be any compound having one or more epoxide functional groups. An epoxide may, for example, contain silicon atoms in the form of one or more siloxane (Si-O-Si) bonds. An epoxide may also be a polysiloxane having multiple siloxane bonds and having one or more epoxide functional groups.

[0027] Polysiloxanes contain multiple siloxane bonds and may be characterized by the siloxy (SiO) groups that make up the polysiloxane. The siloxy groups may be of type M, D, T, or Q. M-type siloxy groups have three groups bonded to the silicon atom, in addition to an oxygen atom shared with another atom bonded to the siloxy group, ≡SiO 1 / 2D-type siloxy groups have two groups bonded to the silicon atom in addition to the two oxygen atoms shared with other atoms bonded to the siloxy group: =SiO 2 / 2 A T-type siloxy group has one group bonded to the silicon atom, -SiO, in addition to the three oxygen atoms shared with other atoms bonded to the siloxy group. 3 / 2 Q-type siloxy groups may be described as SiO in which the silicon atom is bonded to four oxygen atoms that are shared with other atoms bonded to the siloxy group. 4 / 2 The group bonded to the silicon atom is assumed to be a methyl group unless otherwise specified. For example, the group "M" is the same as trimethylsiloxy. "M H " group has two methyl groups and a hydrogen bonded to a siloxy group. Epoxy-functional polysiloxanes generally have organic groups that contain epoxy functionality bonded to silicon atoms of the polysiloxane.

[0028] Examples of suitable polysiloxane epoxides for use in the present invention include any one or any combination or two or more of the following:

[0029] MD a D CEP b M, where subscript a is the average number of D siloxy units and is typically 20 or more, 30 or more, 40 or more, 50 or more, 60 or more, 70 or more, 80 or more, 90 or more, 100 or more, 110 or more, and at the same time, generally 150 or less, 140 or less, 130 or less, 120 or less, and may be 110 or less, 100 or less, 90 or less, 80 or less, and even 70 or less, and subscript b is the average number of D siloxy units per molecule. CEP is the average number of siloxy units, typically having a value of 1 or more, 2 or more, 3 or more, 4 or more, 5 or more, 6 or more, 7 or more, 8 or more, 9 or more, or 10 or more, and at the same time typically having a value of 20 or less, 19 or less, 18 or less, 17 or less, 16 or less, 15 or less, 14 or less, 13 or less, 12 or less, 11 or less, 10 or less, 9 or less, or even 8 or less; D CEPis a D siloxy unit in which one of the methyl groups is replaced with a pendant structure having a cyclic epoxide group, preferably a terminal cyclic epoxide group. For example, D HEP is a D siloxy unit, CEP where one of the methyl groups is replaced with ethyl-cyclohexene oxide. [ka]

[0030] MD a D EP b’ M, where subscript a is the average number of D siloxy units per molecule and is as defined above, and subscript b' is the average number of D siloxy units per molecule. EP is the average number of siloxy units, typically having a value of 1 or more, 2 or more, 3 or more, 4 or more, 5 or more, 6 or more, 7 or more, 8 or more, 9 or more, or 10 or more, and at the same time typically having a value of 20 or less, 19 or less, 18 or less, 17 or less, 16 or less, 15 or less, 14 or less, 13 or less, 12 or less, 11 or less, 10 or less, 9 or less, or even 8 or less; D EP is a D siloxy unit in which one of the methyl groups is replaced with a pendant structure having a linear epoxide group, preferably a terminal epoxide group. EP Examples of units are shown below. [ka]

[0031] M CEP D c M CEP where subscript c is the average number of D siloxy units per molecule and typically has a value of 5 or more, 10 or more, 15 or more, 20 or more, 25 or more, 30 or more, 35 or more, 40 or more, 45 or more, 50 or more, 55 or more, or 60 or more, while typically has a value of 100 or less, 90 or less, 80 or less, 70 or less, 65 or less, or 60 or less; M CEPis an M siloxy unit in which one of the methyl groups is replaced with a cyclic epoxide group, preferably a terminal cyclic epoxide group. For example, M HEP is a M siloxy unit, where one of the methyl groups is replaced with ethyl-cyclohexene oxide. [ka]

[0032] D EP x D c T2, where the subscripts x and c correspond to the average number of moles of corresponding siloxy units per molecule, with the subscript "x" typically having a value of 6 or more, 7 or more, 8 or more, 9 or more, and even 10 or more, but also typically having a value of 20 or less, 19 or less, 18 or less, 17 or less, 16 or less, 15 or less, 14 or less, 13 or less, 12 or less, 11 or less, 10 or less, 9 or less, or even 8 or less, and the subscript "c" typically has a value of 0.01 or less, ... HEP D c M HEP has the value defined above for subscript c; EP is as defined above and forms a cyclic ring with a T terminal group.

[0033] The epoxide may contain linear or cyclic epoxide groups, or both linear and cyclic epoxide groups. A linear epoxide group contains carbon atoms of an epoxide functional group that are not directly bonded to each other to form a three-membered cyclic epoxide functional group, but are not directly or indirectly connected to each other in any other way. A "cyclic epoxide" group contains carbon atoms of an epoxide functional group that are both directly bonded to each other to form a three-membered cyclic epoxide functional group, and are also bonded to each other directly or, more typically, indirectly through another atom in a second bond or chain. For example, the D HEPThe cyclohexene oxide group of the unit is a "cyclic" epoxide because the carbons of the two epoxide functional groups are directly bonded to each other and also indirectly through four other carbons of the six-membered ring. In contrast, the D EP The units contain "linear" epoxides because the carbons of the two epoxide functional groups are only directly bonded to each other in the epoxide functional groups.

[0034] Typically, the concentration of epoxide in the composition is 70 weight percent (wt%) or more, 75 wt% or more, 80 wt% or more, 85 wt% or more, or even 90 wt% or more, based on the combined weight of silyl hydride, epoxide, and bridged frustrated Lewis pairs, while at the same time typically is 90 wt% or less, 85 wt% or less, 80 wt% or less, or even 75 wt% or less.

[0035] Silyl hydride Silyl hydrides contain one, preferably two or more Si-H bonds. The Si-H bonds are typically part of polysilanes (molecules containing multiple Si-H bonds) or polysiloxanes. Silyl hydrides containing multiple Si-H bonds are desirable as crosslinkers in the compositions of the present invention because they can react with multiple epoxide groups.

[0036] The silyl hydrides of the present invention may be polymeric. The silyl hydrides may be linear, branched, or contain a combination of linear and branched silyl hydrides. The silyl hydrides may be polysilanes, polysiloxanes, or combinations of polysilanes and polysiloxanes.

[0037] Desirably, the silyl hydride is a polysiloxane molecule having one Si-H bond or two or more Si-H bonds. When the silyl hydride is a polysiloxane, the Si-H bonds are on silicon atoms of M-type or D-type siloxane units. The polysiloxane may be linear or may contain only M-type and D-type units. Alternatively, the polysiloxane may be branched and may be T(-SiO 3 / 2) type and / or Q(SiO 4 / 2 ) type units.

[0038] Examples of suitable silyl hydrides include pentamethyldisiloxane, bis(trimethylsiloxy)methyl-silane, tetramethyldisiloxane, tetramethylcyclotetrasiloxane, DMS-HM15, DMS-H03, DMS-H25, DMS-H31, and DMS-H41 available from Gelest. H Containing poly(dimethylsiloxane) (e.g., MD H 65 M), and hydride-terminated poly(dimethylsiloxane).

[0039] The concentration of silyl hydride is typically sufficient to provide a molar ratio of Si-H groups to epoxide groups that is 0.2 or more, 0.5 or more, 0.7 or more, 0.8 or more, 0.9 or more, 1.0 or more, 1.2 or more, 1.4 or more, 1.6 or more, 1.8 or more, 2.0 or more, 2.2 or more, or even 2.5 or more, while at the same time typically is 5.0 or less, 4.5 or less, 4.0 or less, 3.5 or less, 3.0 or less, 2.8 or less, 2.5 or less, 2.3 or less, 2.0 or less, 1.8 or less, 1.6 or less, 1.4 or less, 1.2 or less, or even 1.0 or less.

[0040] The epoxide or silyl hydride (or both) can function as a crosslinker in the reaction. A crosslinker has at least two reactive groups in one molecule and reacts with two different molecules through these reactive groups to crosslink them together. Increasing the length of the linear chain between the reactive groups in the crosslinker tends to increase the flexibility of the resulting crosslinked product. In contrast, shortening the length of the linear chain between the reactive groups in the crosslinker tends to reduce the flexibility of the resulting crosslinked product. In general, to obtain a more flexible crosslinked product, a linear crosslinker is desired, and the length between the reactive sites is selected to obtain the desired flexibility. To obtain a less flexible crosslinked product, a shorter linear or even branched crosslinker is desired to reduce the flexibility between the crosslinked molecules.

[0041] The silyl hydride may be the same molecule as the epoxide, i.e., a single molecule containing both epoxide and silyl hydride functional groups can provide roles as both a silyl hydride and an epoxide. Alternatively, the silyl hydride may be a different molecule than the epoxide. The silyl hydride may not include an epoxide group. The epoxide may not include a silyl hydride group.

[0042] The compositions (and reaction processes) of the present invention may contain two or more silyl hydrides, two or more epoxides, and / or two or more components that function as both silyl hydrides and siloxanes.

[0043] Typically, the concentration of silyl hydride in the composition is 5% or more, 10% or more, 15% or more, 20% or more, or even 25% or more by weight, based on the combined weight of silyl hydride, epoxide, and bridged frustrated Lewis pairs, while at the same time typically is 30% or less, 25% or less, 20% or less, 15% or less, or even 5% or less by weight.

[0044] Bridged frustrated Lewis pair A bridged frustrated Lewis pair ("B-FLP") is a complex containing an FLP where the Lewis acid and Lewis base of the FLP are both bound to a bridge molecule to form a neutralized complex with the bridge molecule that resides between the Lewis acid and the Lewis base (i.e., "bridged"). As in the case of H2, the bridge molecule can be cleaved with one portion of the bridge molecule blocking the Lewis acid and another portion of the bridge molecule blocking the Lewis base. Alternatively, and preferably, the bridge molecule remains intact and the B-FLP is a stable complex (at least at 23°C) with the bridge molecule simultaneously bound to the Lewis acid of the FLP and the Lewis base of the FLP.

[0045] The Lewis acid is selected from the group consisting of aluminum alkyls, aluminum aryls, arylboranes including triarylboranes (including substituted aryl and triarylboranes such as fluorinated arylboranes including tris(pentafluorophenyl)borane), boron halides, aluminum halides, gallium alkyls, gallium aryls, gallium halides, silium cations, and phosphonium cations. Examples of suitable aluminum alkyls include trimethylaluminum and triethylaluminum. Examples of suitable aluminum aryls include triphenylaluminum and tris-pentafluorophenylaluminum. Examples of triarylboranes include the following formula: [ka] where R is independently selected at each occurrence from H, F, Cl, and CF3. Examples of suitable boron halides include (CH3CH2)2BCl and boron trifluoride. Examples of suitable aluminum halides include aluminum trichloride. Examples of suitable gallium alkyls include trimethylgallium. Examples of suitable gallium aryls include triphenylgallium. Examples of suitable gallium halides include trichlorogallium. Examples of suitable silium cations include (CH3CH2)3Si + X - and Ph3Si + X - Examples of suitable phosphonium cations include FP(C6F5)3 + X - Examples include:

[0046] Lewis bases are the following bases: PR3, P(NR2)3, NR3, N(SiR3) x R 3-x , RC(NR)N, P(NR)R3, guanidine (C(=NR)(NR2)2), amidine (RC(=NR)NR2), phosphazene, and [ka] wherein R is independently at each occurrence selected from the group consisting of hydrogen, alkyl, substituted alkyl, aryl, and substituted aryl. Examples of suitable Lewis bases of structure PR3 include tri(t-butyl)phosphine, tri(cyclohexyl)phosphine, PhP(tBu), (cyclohexyl)P(tBu), nBuP(tBu), Me(tBu), tBuP(i-Pr), P(CH 11 )3, P(iBu)3, and P(n-Bu)3. Examples of suitable Lewis bases of the structure RC(NR)N include 1,5,7-triazabicyclo[4.4.0]dec-5-ene, 7-methyl-1,5,7-triazabicyclo4.4.0dec-5-ene, and 2,3,4,6,7,8,9,10-octahydropyrimidol[1,2-a]azepine (DBU). Examples of suitable guanidines include guanidine, biguanidine, and 1,1-dimethylguanidine. Examples of suitable amidines include diethylamide and diisopropylamide. Examples of suitable phosphazenes include tert-butylimino-tri(pyrrolidino)phosphone, tert-octylimino-tris(dimethylamino)phosphorene, and 2-tert-butylimino-2-diethylamino-1,3-dimethylperhydro-1,3,2-diazaphosphorine. Examples of suitable Lewis basis of the following structure are: [ka] Examples include 1,3-dimesityl-imidazol-4,5-dihydro-2-ylidene, 1,3-bis(2,6-diisopropylphenyl)imidazol-2-ylidene, and 1,3-bis(2,4,6-trimethylphenyl)-4,5-dihydroimidazol-2-ylidene.

[0047] A crosslinking molecule within the broadest scope of the present invention includes any molecule that simultaneously binds and blocks the Lewis acid and Lewis base of the FLP to form a B-FLP. The interaction of the crosslinking molecule with the Lewis acid and Lewis base is such that the Lewis acid and Lewis base are blocked by the crosslinking molecule (or a portion thereof) at 23°C, but at least the Lewis acid is unblocked at a temperature of 120°C or higher, preferably 110°C or higher, more preferably 100°C or higher, even more preferably 90°C or higher, 80°C or higher, or even 70°C or higher, and at the same time, desirably 300°C or lower, 240°C or lower, 220°C or lower, 200°C or lower, 180°C or lower, 160°C or lower, 150°C or lower, 125°C or lower, or even 100°C or lower. Unblocking the Lewis acid of the B-FLP can be demonstrated by the composition of the present invention containing the B-FLP curing in less than 1 / 10 the time required to gel at 23°C.

[0048] Examples of suitable cross-linking molecules include carbon dioxide, hydrogen molecules (H2), nitriles, alkenes, alkynes, ketones, esters, and aldehydes. Desirably, the cross-linking molecules contain 10 or less, preferably 9 or less, and may contain 8 or less, 7 or less, 6 or less, 5 or less, 4 or less, 3 or less, 2 or less, and even 1 or less or 0 carbon atoms, while at the same time, the cross-linking molecules may contain 1 or more, 2 or more, 3 or more, 4 or more, 5 or more, and even 6 or more carbon atoms. As mentioned earlier in this specification, in B-FLP, some cross-linking molecules can be cleaved, with some of the cross-linking molecules blocking Lewis acids and Lewis bases and some of the cross-linking molecules blocking Lewis bases. It is preferred that the cross-linking molecules remain uncleaved while cross-linking the Lewis acids and Lewis bases of the FLP. In that respect, the cross-linking molecules are preferably not H2. More preferably, the cross-linking molecules do not include any molecules that cleave while cross-linking the Lewis acids and Lewis bases of the FLP.

[0049] B-FLP is desirably "stable" in the compositions of the present invention, meaning that it does not dissociate to release a Lewis acid at temperatures below 23° C. B-FLP may be stable at temperatures below 30° C., below 50° C., below 70° C., or even below 80° C. At the same time, B-FLP dissociates at temperatures above 120° C., preferably above 110° C., more preferably above 110° C., above 100° C., above 90° C., and even above 80° C. B-FLP may be stable at temperatures below ... or even above 80° C. 1 H and 31 P, 11 B and / or 27 Dissociation of B-FLP can be determined by examining evidence of free Lewis acid by ion exchange (I) or by the addition of 1,2-dichlorophenyl ether (I) or ...

[0050] One method for preparing B-FLP is by mixing the Lewis acid and Lewis base of FLP together with the crosslinking molecule in a solvent at 23° C. The mixing promotes the formation of B-FLP. B-FLP may be isolated from the solvent, typically by evaporating the solvent or filtering if B-FLP precipitates from the solvent. B-FLP can be stored for long periods at or below 23° C. B-FLP can be mixed with silyl hydride and siloxane to form the composition of the present invention.

[0051] In contrast to typical blocked Lewis acid systems, the Lewis acid of the B-FLP of the present invention is complexed with a Lewis base via a bridging molecule, thus complexing the two molecules. Prior art suggests directly complexing the Lewis acid with a blocking agent that is sensitive to ultraviolet (UV) light, so that upon irradiation with UV light, the blocking agent dissociates from the Lewis acid. The B-FLP of the present invention does not require a UV-sensitive blocking agent and may not include any component that liberates the Lewis acid from the B-FLP upon irradiation with UV light. The B-FLP and compositions of the present invention may not include a photoacid generator or any other component that generates a Lewis acid upon exposure to UV radiation.

[0052] The compositions of the present invention typically contain sufficient B-FLP to provide a Lewis acid concentration that is 0.1 parts per million (ppm) or more, 1 ppm or more, 10 ppm or more, 50 ppm or more, 100 ppm or more, 200 ppm or more, 300 ppm or more, 400 ppm or more, 500 ppm or more, 600 ppm or more, 700 ppm or more, 800 ppm or more, 900 ppm or more, 1000 ppm or more, but at the same time, typically 10,000 ppm or less, 5,000 ppm or less, 1,000 ppm or less, based on the combined weight of silyl hydride and epoxide in the composition.

[0053] The compositions of the present invention offer the advantage of a one-component reactive system that is storage stable or at least exhibits delayed cure even when exposed to UV light. Desirably, the stability of the B-FLPs of the present invention is not dependent on (i.e., independent of) exposure to UV light.

[0054] The compositions of the present invention may be free of water, or may comprise water, preferably at a concentration of 1 weight percent (wt%) or less, 0.75 wt% or less, 0.5 wt% or less, 0.25 wt% or less, 0.1 wt% or less, 0.05 wt% or less, or even 0.01 wt% or less, based on the weight of the composition.

[0055] Optional Ingredients The composition of the present invention can consist of a silyl hydride, an epoxide, and B-FLP. Alternatively, the composition of the present invention can include one optional ingredient or a combination of two or more optional ingredients. The optional ingredients are desirably present in a concentration of 50% by weight or less, 40% by weight or less, 30% by weight or less, 20% by weight or less, 10% by weight or less, 5% by weight or less, or even 1% by weight or less based on the weight of the composition.

[0056] Examples of possible optional components include one or a combination of two or more components selected from the group consisting of hydrocarbyl solvents (typically at a concentration of 10% by weight or less, 5% by weight or less, or even 1% by weight or less based on the weight of the composition), pigments such as carbon black or titanium dioxide, fillers such as metal oxides including SiO2 (typically at a concentration of 50% by weight or less based on the weight of the composition), moisture scavengers, optical brighteners, stabilizers (such as antioxidants and UV stabilizers), and corrosion inhibitors. The composition of the present invention may also be free of one or a combination of two or more of such additional components.

[0057] In particular, the composition of the invention may contain up to 1% by weight of water, up to 0.5% by weight of water, relative to the weight of the composition. Desirably, the composition is free of water.

[0058] Chemical Reaction Process The present invention includes a chemical reaction process comprising the steps of (a) providing a composition of the present invention, and (b) heating the composition to a temperature sufficient to dissociate a Lewis acid from B-FLP. Upon heating the composition of the present invention, the Lewis acid is released from B-FLP and catalyzes the reaction of the silyl hydride with the epoxide, as described above. The composition of the present invention can be provided in step (a) by mixing together B-FLP, the silyl hydride, and the epoxide. As described above, the silyl hydride and the epoxide can be the same molecule.

[0059] The chemical reaction process can be carried out in the absence of water or with a concentration of water that is 1 weight percent (wt%) or less, 0.75 wt% or less, 0.5 wt% or less, 0.25 wt% or less, 0.1 wt% or less, 0.05 wt% or less, or even 0.01 wt% or less, based on the weight of the composition provided in step (a).

[0060] The composition has use, for example, as a coating that undergoes a heat-induced curing reaction, or as a reactive composition for molding applications where the fluid is placed in a mold and heated to induce curing to form a molded article. In such applications, the process of the present invention further comprises, after step (a) and before step (b), the composition is applied to a substrate or placed in a mold. EXAMPLES

[0061] Synthesis of B-FLP (1). In a glovebox, place tri(t-butyl)phosphine (200 milligrams (mg), 1.0 millimole (mmol), 1 equivalent (equiv)) and tris-pentafluorophenylborane ("BCF") (500 mg, 1 mmol, 1 equiv) in a Schlenk flask equipped with a magnetic stir bar and dissolve the components in 10 milliliters (mL) of toluene. Seal the Schlenk flask and remove it from the glovebox. Connect the Schlenk flask to a Schlenk line. Stir the contents of the Schlenk flask throughout the next step. Purge the Schlenk line with nitrogen, then bubble carbon dioxide in the line for 2 minutes. Expose the Schlenk flask to the carbon dioxide atmosphere, then replace the flask's cap with a septum. Insert a needle through the septum to create an outlet for carbon dioxide gas and improve carbon dioxide circulation. After 5 minutes, a white solid precipitates from the reaction mixture. Seal the flask and stir at room temperature for an additional hour. Transfer the flask to a glove box. Add 20 mL of hexane and isolate the white solid by filtration through a glass frit. Wash the white solid three times with hexane (10 mL each time). The white solid is B-FLP(1) (540 mg, 71% yield). B-FLP(1) can be stored without decomposition even when exposed to UV light. 1 H, 31 P, and 11 The solid is characterized by B nuclear magnetic resonance spectroscopy (NMR) to confirm the absence of impurities and starting materials. The predicted reaction and structure of B-FLP (1) is as follows: [ka]

[0062] Synthesis of B-FLP (2). In a glovebox, place tri(cyclohexyl)phosphine (546 milligrams (mg), 1.9 millimoles (mmol), 1 equivalent (equiv)) and tris-pentafluorophenylborane (998 mg, 1.9 mmol, 1 equiv) in a Schlenk flask equipped with a magnetic stir bar and dissolve the components in 10 milliliters (mL) of toluene. Seal the Schlenk flask and remove it from the glovebox. Connect the Schlenk flask to a Schlenk line. Stir the contents of the Schlenk flask throughout the next step. Purge the Schlenk line with nitrogen and then bubble carbon dioxide in the line for 2 min. Expose the Schlenk flask to a carbon dioxide atmosphere and then replace the flask's cap with a septum. Insert a needle through the septum to create an outlet for carbon dioxide gas and improve carbon dioxide circulation. After 5 min, a white solid precipitates from the reaction mixture. Seal the flask and stir at room temperature for an additional 1 h. Move the flask to a glove box. Add 20 mL of hexane and isolate the white solid by filtration through a glass frit. Wash the white solid three times with hexane (10 mL each time). The white solid is B-FLP(2) (1.2 g, 76% yield). B-FLP(2) can be stored without decomposition even when exposed to UV light. 1 H, 31 P, and 11 The solid is characterized by B nuclear magnetic resonance spectroscopy (NMR) to confirm the absence of impurities and starting materials. The predicted reaction and structure of B-FLP (2) is as follows: [ka]

[0063] MD 60.5 D H 7.5Synthesis of M: Add 60 grams of deionized water, 15 grams of heptane, and 0.075 grams of tosylic acid to a three-neck flask equipped with a mechanical stirrer. Add a mixture of 270 grams of dimethyldichlorosilane, 28 grams of methyldichlorosilane, and 15 grams of trimethylchlorosilane dropwise to the reaction solution with stirring over 30 minutes. After stirring for 1 hour at 23°C, the reaction solution is washed three times with 80 milliliters of deionized water, dried with anhydrous sodium sulfate, and filtered through a layer of activated carbon. The volatiles are removed by a rotary evaporator (Rotovap) to obtain the polymerization product MD. 60.5 D H 7.5 Get M.

[0064] MD 60.5 D EP 7.5 Synthesis of M. In a 500 mL 3N dry flask, add 80 g (0.118 mol SiH) of MD 60.5 D H 7.6 M, 2 parts per million (ppm) of Pt (Karstedt catalyst), 60.5 D H 7.6 Add to the weight of M and 70 g of toluene, followed by heating to 80° C. Add 20.2 g (0.177 mol) of AGE (allyl glycidyl ether) dropwise in 30 g of toluene at 80° C. within 30 minutes, then heat the reaction mixture to reflux (at about 110° C.) for 6 hours. 29 Monitoring the sample over time by Si NMR reveals when the reactants are exhausted and the reaction is complete. Once the reaction is complete, the solvent and excess AGE are removed by rotary evaporation to give 90 g of product MD 60.5 D EP 7.5 M is obtained in 96% yield.

[0065] MD 60.5 D HEP 7.5 Synthesis of M: In a 500 mL 3N dry flask, add 110.7 g (0.163 mol SiH) of MD 60.5 D H7.6 M, 2 ppm Pt (Karstedt catalyst), MD 60.5 D H 7.6 Add to the weight of M and 80 g of toluene, followed by heating to 80° C. Add 30.4 g (0.245 mol) of 4-vinyl-cyclohexene oxide dropwise in 30 g of toluene at 80° C. within 30 minutes, then heat the reaction mixture to reflux (at about 110° C.) for 6 hours. 29 Monitoring the sample over time by Si NMR reveals when the reactants are exhausted and the reaction is complete. Once the reaction is complete, the solvent and excess AGE are removed by rotary evaporation to give 127 g of product MD 60.5 D HEP 7.5 M is obtained in 90% yield.

[0066] M HEP D 40 M HEP Synthesis of: In a 500 mL 3N dry flask, add 100 g (0.6464 mol) of M H D 40 M H (commercially available as DMS-HM15 from Gelest), 2 ppm Pt (Karstedt catalyst), 60.5 D H 7.6 Add to the weight of M and 80 mL of toluene, followed by heating to 80° C. Add 12 g (0.0.097 mol) of 4-vinylcyclohexene epoxide dropwise in 20 mL of toluene at 80° C. within 25 minutes, then heat the reaction mixture to reflux (at about 110° C.) for 6 hours. 29 Monitoring the sample over time by Si NMR reveals when the reactants are exhausted and the reaction is complete. Once the reaction is complete, the solvent and excess AGE are removed by rotary evaporation to give 103 g of product M HEP D 40 M HEP is obtained in 95% yield.

[0067] MD 117 D HEP 11.8M. This material is commercially available from Gelest as ECMS-924.

[0068] MD H 65 Synthesis of M: Add 40 grams of deionized (DI) water, 10 grams of heptane, and 0.05 grams of tosylic acid to a three-neck flask equipped with a mechanical stirrer. Add a mixture of 200 grams of methyldichlorosilane and 10 grams of trimethylchlorosilane dropwise to the reaction solution with stirring within 30 minutes. After stirring at 23°C for 1 hour, wash the reaction solution with 50 mL of deionized water three times, dry with anhydrous sodium sulfate, and filter through a layer of activated carbon. Remove the volatiles by rotary evaporator to obtain the polymerization product MD. H 65 Get M.

[0069] Test Method 23°C Gel Time. The composition is prepared, placed in a vial, the vial is sealed, and stored at 23°C. The vial is inverted every minute for the first 10 minutes, then every 10 minutes for the first hour, then every hour for the first 8 hours, then every 24 hours. Gel time at 23°C is the time required for the composition to become viscous enough that it will not flow within 1-2 inversions of the vial. During the test, the composition is exposed to ambient (including ultraviolet) light.

[0070] Heat Set Time. The composition is prepared and coated onto glassine paper as a 125 micrometer thick film. The film is placed in an oven at the specified temperature and monitored every 10 seconds for the first minute, then every minute for the first 10 minutes, then every 10 minutes thereafter to determine when the film is tack-free. The time required to become tack-free is the set time for the temperature to which it is being heated.

[0071] Compositions Using Cyclic Epoxides Comparative example (Comp Ex) A MD in a dental cup using a SpeedMixer at 23 °C. 60.5 D HEP 7.5 M.D.H 65 A mixture is formed by mixing MD and 500 ppm (based on the weight of the mixture) of BCF (delivered as a 5 wt % solution in tetrahydrofuran). 60.5 D HEP 7.5 M and MD H 65 The amount of M provides a molar concentration ratio of SiH:EP that is 1.5: 1. The mixture gelled within 1 min after addition of BCF at 23°C.

[0072] Comparative Example A shows that epoxides and silyl hydrides react rapidly in the presence of Lewis acids at 23° C. These are clearly not storage stable reactive compositions.

[0073] Example (Ex) 1: MD 60.5 D HEP +MD H 65 M+B-FLP(1) Comparative Example A is repeated, except that 500 ppm of B-FLP(1) is used instead of 500 ppm of BCF. The composition (Example 1) has a gel time of 20 minutes at 23° C. and a cure time of 0.2 minutes at 95° C. Example 1 shows that B-FLP dramatically delays gelation at 23° C. while providing a rapid cure at 95° C.

[0074] Example 2: MD 117 D HEP 11.8 M+MD H 65 M+B-FLP(1) MD 60.5 D HEP 7.5 MD instead of M 117 D HEP 11.8 Example 1 is repeated except that M is used. The composition (Example 2) has a gel time of 2 hours at 23° C. and a cure time of 0.2 minutes at 95° C. Example 2 shows that B-FLP dramatically delays gelation at 23° C. while providing a rapid cure at 95° C.

[0075] Example 3: M HEP D 40 M HEP +MD H 65 M+B-FLP(1) MD 60.5 D HEP 7.5 M instead of M HEP D 40 M HEP Example 1 is repeated except that B-FLP is used. The composition (Example 3) has a gel time of 3 hours at 23° C. and a cure time of 0.5 minutes at 95° C. Example 3 shows that B-FLP dramatically delays gelation at 23° C. while providing a rapid cure at 95° C.

[0076] Example 4: MD 60.5 D HEP +MD H 65 M+B-FLP(2) Example 1 is repeated, except that B-FLP(2) is used instead of B-FLP(1). The composition (Example 4) has a gel time at 23°C of 4 days, a cure time at 95°C of 60 minutes, and a cure time at 215°C of 2 minutes. Example 4 shows that B-FLP dramatically delays gelation at 23°C while providing a rapid cure at 215°C. Example 4 also shows that different crosslinking groups in B-FLP can tune the temperature at which rapid cure occurs. The crosslinking groups of B-FLP(2) release Lewis acid (BCF) at a higher temperature than the crosslinking groups of B-FLP(1), as evidenced by the need to heat to a higher temperature to achieve rapid cure.

[0077] Example 5: MD 117 D HEP 11.8 M+MD H 65 M+B-FLP(2) Example 2 is repeated, except that B-FLP(2) is used instead of B-FLP(1). The composition (Example 5) has a gel time at 23°C of 4 days, a cure time at 95°C of 60 minutes, and a cure time at 215°C of 8 minutes. Example 5 shows that B-FLP dramatically delays gelation at 23°C while providing a rapid cure at 215°C. Example 5 also shows that different crosslinking groups in B-FLP can tune the temperature at which rapid cure occurs. The crosslinking groups of B-FLP(2) release Lewis acid (BCF) at a higher temperature than the crosslinking groups of B-FLP(1), as evidenced by the need to heat to a higher temperature to achieve rapid cure.

[0078] Compositions using linear epoxides Comparative example B MD 60.5 D HEP 7.5 MD instead of M 60.5 D EP 7.5 Comparative Example A is repeated except using M. The mixture gelled within 45 minutes after addition of BCF at 23°C.

[0079] Comparative Example B shows that a linear epoxide and a silyl hydride react in the presence of a Lewis acid at 23° C., but not as rapidly as the cyclic epoxide material of Comparative Example A, but still reacts within an hour. As a result, Comparative Example B is not considered storage stable.

[0080] Example 6: MD 60.5 D EP +MD H 65 M+B-FLP(1) Comparative Example B is repeated, except that B-FLP(1) is used instead of BCF. The composition (Example 6) has a gel time of 4 days at 23° C., a cure time of 20 minutes at 95° C., and a cure time of 0.5 minutes at 150° C. Example 6 shows that B-FLP dramatically delays gelation at 23° C. while providing a fast cure at 95° C. and an even faster cure at 150° C.

Claims

1. 1. A composition comprising a mixture of a silyl hydride, an epoxide, and a bridged frustrated Lewis pair, comprising: The bridged frustrated Lewis pair is (a) a Lewis acid which is a fluorinated arylborane; (b) a Lewis base selected from the group consisting of molecules having the following structure: PR 3 , where R is independently selected at each occurrence from the group consisting of hydrogen, alkyl, substituted alkyl, aryl, and substituted aryl; (c) a bridging molecule that binds the Lewis acid and the Lewis base, the bridging molecule being carbon dioxide; composition.

2. The composition of claim 1 , wherein the composition is free of transition metals.

3. (a) providing a composition according to claim 1 or 2; (b) heating said composition to a temperature sufficient to dissociate said Lewis acid from said bridged frustrated Lewis pair.

4. 4. The process of claim 3, wherein step (a) comprises mixing together the bridged frustrated Lewis pair, a silyl hydride and an epoxide.

5. 5. The process of claim 3 or 4, wherein after step (a) and before step (b), the composition is applied to a substrate or placed in a mold.

Citation Information

Patent Citations

  • Anionic latent catalyst and resin composition using same

    JP2000234015A

  • Epoxy resin composition for laminated sheet and prepreg and laminated sheet using the same

    JP2001226458A

  • Lewis base-lewis acid complex and method for producing the same

    JP2016074633A

  • Silicone compositions

    US20190031932A1